Manufacturing method of rare earth magnet
By coating samarium-iron-nitrogen magnetic powder with zinc to a 96% coverage, the method addresses oxidation issues, enabling atmospheric processing and cost-effective production of rare earth magnets with maintained residual magnetization.
Patent Information
- Application Number
- JP2021016023
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-03
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-02-03
AI Technical Summary
The manufacturing of samarium-iron-nitrogen rare earth magnets is challenging due to the easy oxidation of the particle surface, leading to a decrease in magnetic phase and residual magnetization, which necessitates costly vacuum or inert gas atmospheres, increasing equipment complexity and costs.
A method involving the formation of a zinc coating on the surface of samarium-iron-nitrogen magnetic powder with a coverage of 96% or more, allowing compression molding and pressure sintering in the atmosphere, while suppressing oxidation and maintaining residual magnetization.
This method enables the production of rare earth magnets with reduced residual magnetization loss, simplifying the manufacturing process and lowering costs by allowing atmospheric processing, thus reducing the need for complex vacuum or inert gas equipment.
Smart Images

Figure 0007585835000002 
Figure 0007585835000003 
Figure 0007585835000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing rare earth magnets, and in particular to a method for producing samarium-iron-nitrogen based rare earth magnets. [Background technology]
[0002] As high-performance rare earth magnets, samarium-cobalt rare earth magnets and neodymium-iron-boron rare earth magnets have been put to practical use, but in recent years, other rare earth magnets have been considered. For example, Th2Zn 17 Type and Th2Ni 17 A rare earth magnet having a magnetic phase with at least one of the crystal structures of the above types (hereinafter, sometimes referred to as a "samarium-iron-nitrogen rare earth magnet") has been studied. The samarium-iron-nitrogen rare earth magnet is manufactured using a magnetic powder containing samarium, iron, and nitrogen (hereinafter, sometimes referred to as a "samarium-iron-nitrogen magnetic powder").
[0003] Samarium-iron-nitrogen magnetic powder is Th2Zn 17 Type and Th2Ni 17 The magnetic powder contains a magnetic phase having at least one of the following crystal structures. It is believed that this magnetic phase is formed by interstitial nitrogen solid solution in the samarium-iron crystal. Therefore, the nitrogen is easily dissociated and decomposed by heat in the samarium-iron-nitrogen magnetic powder. For this reason, when manufacturing a samarium-iron-nitrogen rare earth magnet (molded body), it is necessary to mold the samarium-iron-nitrogen magnetic powder at a temperature at which the nitrogen in the magnetic phase does not dissociate.
[0004] An example of such a molding method is the method for manufacturing a rare earth magnet disclosed in Patent Document 1. In this manufacturing method, a mixed powder of a samarium-iron-nitrogen magnetic powder and a zinc-containing powder is compression molded in a magnetic field, and the resulting green compact is pressure sintered (including liquid phase sintering).
[0005] When a compact of a mixed powder of samarium-iron-nitrogen magnetic powder and zinc-containing powder is pressure sintered (including liquid phase sintering), the zinc component in the zinc-containing powder diffuses into the surface of the particles of the samarium-iron-nitrogen magnetic powder in a solid or liquid phase, resulting in sintering (solidification).For this reason, in the manufacturing method of a rare earth magnet disclosed in Patent Document 1, the zinc-containing powder has a binder function.
[0006] In the samarium-iron-nitrogen powder, Th2Zn 17 Type and Th2Ni 17 A small amount of Fe that did not form a magnetic phase having at least one of the crystal structures of the above types remains as an α-Fe phase. This α-Fe phase reduces the coercive force. The zinc component in the zinc-containing powder forms an α-Fe phase and a Zn-Fe phase (modifier phase). The Zn-Fe phase (modifier phase) magnetically separates the magnetic phase, improving the coercive force. Thus, the zinc-containing powder has a modifier function in addition to the binder function described above. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2019-186368 A Summary of the Invention [Problem to be solved by the invention]
[0008] The particle surface of the samarium-iron-nitrogen magnetic powder is very susceptible to oxidation. When the particle surface of the samarium-iron-nitrogen magnetic powder is oxidized, the magnetic phase in the samarium-iron-nitrogen magnetic powder is reduced, and the residual magnetization is reduced. For this reason, when manufacturing a samarium-iron-nitrogen rare earth magnet (molded body), the manufacturing process has conventionally been carried out in a vacuum or in an inert gas atmosphere.
[0009] In order to manufacture a samarium-iron-nitrogen rare earth magnet (molded body) in a vacuum or in an inert gas atmosphere, the device used for the manufacture must be enclosed in a container that can ensure airtightness, which makes the device larger and more complicated. Power is required to maintain the vacuum in the container, and inert gas is generally expensive. Therefore, manufacture in a vacuum or in an inert gas atmosphere leads to increased manufacturing costs. In view of these circumstances, the present inventors have discovered a problem that if the decrease in remanence can be suppressed by operating in air even for a part of the process in the manufacture of a samarium-iron-nitrogen rare earth magnet (molded body), the manufacturing process can be simplified and the manufacturing cost can be reduced.
[0010] The present disclosure has been made to solve the above problems. That is, the purpose of the present disclosure is to provide a method for producing a rare earth magnet that can suppress a decrease in remanent magnetization, significantly simplify the production process, and reduce production costs, even when at least a portion of the production process of a samarium-iron-nitrogen rare earth magnet is carried out in air. [Means for solving the problem]
[0011] The present inventors have conducted intensive research to achieve the above object, and have completed the method for producing a rare earth magnet according to the present disclosure. The method for producing a rare earth magnet according to the present disclosure includes the following aspects. <1> Contains samarium, iron, and nitrogen, and is Th2Zn 17 Type and Th2Ni 17 forming a coating containing zinc on the surface of a magnetic powder particle having a magnetic phase having at least one of the crystal structures of the above types to obtain a coated powder; Compressing the coated powder to obtain a green compact; and Pressurizing and sintering the powder compact; Including, the coverage of the coating with respect to the entire surface of the particles of the coating powder is 96% or more; The formation of the coating and the pressure sintering of the green compact are carried out in a vacuum or an inert gas atmosphere; and The compression molding of the coating powder is carried out in air. A method for manufacturing rare earth magnets. <2> The method for producing a rare earth magnet according to item <1>, further comprising compression molding the coated powder in a magnetic field to obtain the green compact while magnetically orienting the coated powder. 〈3〉 The vacuum is 1×10 absolute pressure. -1 3. The method for producing a rare earth magnet according to claim 1, wherein the thermal expansion coefficient is 0.01 Pa or less. <4> The method for producing a rare earth magnet according to any one of <1> to <3>, further comprising sublimating zinc in a vacuum and depositing zinc on the surfaces of the magnetic powder particles to form the coating. <5> The method for producing a rare earth magnet according to <4>, wherein 20 to 50 mass % of zinc is deposited based on the magnetic powder. <6> The method for producing a rare earth magnet according to <4>, wherein 20 to 30 mass % of zinc is deposited based on the magnetic powder. <7> The method for producing a rare earth magnet according to any one of <1> to <6>, comprising pressure sintering at 350 to 380°C for 1 to 5 minutes while applying a pressure of 100 to 2000 MPa. <8> The method for producing a rare earth magnet according to any one of <1> to <7>, wherein the pressure sintering is carried out in an inert gas atmosphere. Effect of the Invention
[0012] According to the present disclosure, by forming a coating with a predetermined coverage on the particle surfaces of the samarium-iron-nitrogen magnetic powder in advance, it is possible to suppress oxidation of the samarium-iron-nitrogen magnetic powder in the air in a process prior to pressure sintering the coated powder having the coating. This makes it possible to provide a method for manufacturing a rare earth magnet that can suppress a decrease in remanence even if the coated powder is compression molded in the air to obtain a green compact prior to pressure sintering. [Brief description of the drawings]
[0013] [Figure 1A] FIG. 1A is an explanatory diagram that shows a schematic diagram of a situation in which particles of a coating powder exist in the atmosphere. [Figure 1B] FIG. 1B is an explanatory diagram that illustrates a state in which the surface of a particle of a coated powder is oxidized. [Diagram 2] FIG. 2 is an explanatory diagram showing an example of a method for forming a zinc-containing coating on the surface of magnetic powder particles using a rotary kiln. [Diagram 3] FIG. 3 is an explanatory diagram showing an example of a method for forming a zinc-containing coating on the surface of a magnetic powder particle by using a vapor deposition method. [Figure 4] FIG. 4 is an explanatory diagram that illustrates an example of a die and a punch used for powder compaction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, embodiments of the method for producing a rare earth magnet according to the present disclosure will be described in detail. Note that the method for producing a rare earth magnet according to the present disclosure is not limited to the embodiments described below.
[0015] Without being bound by theory, the reason why the method for producing a rare earth magnet disclosed herein can suppress oxidation of samarium-iron-nitrogen magnetic powder (hereinafter sometimes simply referred to as "magnetic powder") in the air in the process prior to pressure sintering will be explained using the drawings.
[0016] Fig. 1A is an explanatory diagram showing a schematic diagram of a situation when a coated powder particle is present in the atmosphere, and Fig. 1B is an explanatory diagram showing a schematic diagram of a situation when the surface of the coated powder particle is oxidized.
[0017] As shown in Fig. 1A, a coating 20 is formed on the surface of the magnetic powder 10 particles, and the magnetic powder 10 particles and the coating 20 constitute the particles of the coated powder 30. Oxygen 40 exists in the atmosphere, but as shown in Fig. 1B, near the surface of the coating 20, the oxygen 40 reacts with zinc in the coating 20 to form an oxide coating 25 containing zinc oxide. This prevents the oxygen 40 from coming into direct contact with the magnetic powder 10 particles.
[0018] A rare earth magnet (green body) is obtained by pressure sintering a green compact obtained by compression molding the coated powder 30. The compression molding of the coated powder is performed in the cold state. The coating 20 suppresses oxidation of the surfaces of the magnetic powder 10 particles in the cold state. This makes it possible to perform the compression molding of the coated powder in the air. Details of "cold" will be described later.
[0019] In order to impart anisotropy to the rare earth magnet (molded body) and improve remanent magnetization, a magnetic field may be applied during compression molding of the coated powder to magnetically orient the particles of the coated powder 30. When forming a powder compact, the coated powder is loaded into a mold and compression molded (cold press). To apply a magnetic field during compression molding, an electromagnetic coil is placed around the mold, but to create a vacuum or inert gas atmosphere inside the mold during compression molding, the device becomes complicated. The fact that compression molding can be performed in the atmosphere allows the device to be simplified, and as a result, the manufacturing method of rare earth magnets can be greatly simplified. Among magnetic powders, samarium-iron-nitrogen magnetic powders have a very large anisotropic magnetic field. For this reason, a large electromagnetic coil is required to orient the samarium-iron-nitrogen magnetic powder. Therefore, to perform powder compression in a vacuum or inert gas atmosphere, the device becomes very large and / or complicated, so compression molding in the atmosphere is particularly advantageous.
[0020] The constituent elements of the method for producing rare earth magnets according to the present disclosure, which was completed based on the findings described above, will now be described.
[0021] <<Manufacturing method of rare earth magnets>> The method for producing a rare earth magnet according to the present disclosure includes a coating step, a compression molding step, and a pressure sintering step. In addition, the compression molding step may optionally include a magnetic field application step. Each step will be described below.
[0022] <Coating process> Contains samarium, iron, and nitrogen, and is Th2Zn 17 Type and Th2Ni 17A coating containing zinc is formed on the surface of a magnetic powder particle having a magnetic phase having at least one of the crystal structures of the above types to obtain a coated powder. The coating containing zinc means a coating containing zinc element, and typically means at least one of a coating containing metallic zinc and a coating containing a zinc alloy. The metallic zinc means unalloyed zinc.
[0023] As mentioned above, it contains samarium, iron, and nitrogen, and is represented by the formula Th2Zn 17 Type and Th2Ni 17 A magnetic powder having a magnetic phase having at least one of the above crystal structures may be simply referred to as a “magnetic powder.” Details of the magnetic powder will be described later.
[0024] In order to suppress oxidation of the magnetic powder, a coating containing zinc is formed on the surface of the magnetic powder particles in a vacuum or in an inert gas atmosphere. The method of forming the coating is not particularly limited as long as the coating is formed in a vacuum or in an inert gas atmosphere, the oxidation of the magnetic powder is suppressed, and a predetermined coverage rate is obtained. During the subsequent pressure sintering process, the coating powder forms a modified phase with the α-Fe phase in the magnetic powder, so that the coating powder may or may not be modified at the stage of the coating process.
[0025] Examples of methods for forming the coating include a method using a rotary kiln, a vapor deposition method, and a kneading method. These methods may be combined. Each of these methods will be briefly described below.
[0026] <Method using a rotary kiln> FIG. 2 is an explanatory diagram showing an example of a method for forming a zinc-containing coating on the surface of magnetic powder particles using a rotary kiln.
[0027] The rotary kiln furnace 100 includes an agitating drum 110. The agitating drum 110 includes a material storage section 120, a rotating shaft 130, and an agitating plate 140. A rotating means (not shown) such as an electric motor is connected to the rotating shaft 130.
[0028] The magnetic powder 10 and the zinc-containing powder 50 are charged into the material storage section 120. The zinc-containing powder 50 will be described later. Thereafter, while the stirring drum 110 is rotating, the material storage section 120 is heated by a heater (not shown).
[0029] When the material storage unit 120 is heated to a temperature lower than the melting point of the zinc-containing powder 50, the zinc component of the zinc-containing powder 50 is solid-phase diffused or vapor-deposited on the surface of the particles of the magnetic powder 10. As a result, a coating containing zinc is formed on the surface of the particles of the samarium-iron-nitrogen magnetic powder.
[0030] When the material storage section 120 is heated to a temperature lower than the melting point of the zinc-containing powder 50, if the material storage section is placed in a vacuum state, the zinc-containing powder 50 sublimes and the zinc component of the zinc-containing powder 50 is deposited. In the case of deposition by sublimation, the zinc vapor reaches every corner of each particle of the magnetic powder 10, and the zinc is uniformly deposited on the surface of the magnetic powder particles to form the coating 20. Therefore, even if the amount of zinc deposition is small, the desired coverage can be obtained. Since zinc does not exhibit magnetism, it is preferable to obtain the desired coverage with a small amount of zinc deposition.
[0031] When zinc is deposited by sublimation, to obtain the desired coverage, it may be 20% by weight or more, 22% by weight or more, or 25% by weight or more, and may be 50% by weight or less, 45% by weight or less, 40% by weight or less, or 30% by weight or less, based on the magnetic powder.
[0032] When depositing zinc in a vacuum, the absolute pressure should be set to 1×10 in order to prevent oxidation of the magnetic powder and to prevent zinc from sublimating. -1 Pa or less, 1×10 -2 Pa or less, 1×10 -3 Pa or less, 1×10 -4 Pa or less, 1×10 -5 Pa or less, 1×10 -6 Pa or less, or 1×10 -7On the other hand, there is no practical problem even if the pressure is not excessively reduced, and as long as the above-mentioned atmospheric pressure is satisfied, the atmospheric pressure may be 1×10 -8 It may be Pa or more.
[0033] If the material storage section 120 is heated to above the melting point of the zinc-containing powder 50, a molten solution of the zinc-containing powder is obtained, and the solution comes into contact with the magnetic raw material powder 150. If the material storage section 120 is cooled in this state, a coating containing zinc is formed on the surface of the magnetic powder particles. When the material storage section 120 is heated to above the melting point of the zinc-containing powder 50, the material storage section 120 is preferably in an inert gas atmosphere. The loading gas atmosphere includes a nitrogen gas atmosphere.
[0034] The operating conditions of the rotary kiln furnace 100 may be appropriately determined so as to obtain a desired coating.
[0035] The heating temperature of the material storage section may be, for example, (T-50)°C or higher, (T-40)°C or higher, (T-30)°C or higher, (T-20)°C or higher, (T-10)°C or higher, or T°C or higher, and may be (T+50)°C or lower, (T+40)°C or lower, (T+30)°C or lower, (T+20)°C or lower, or (T+10)°C or lower, where T is the melting point of the zinc-containing powder. When the zinc-containing powder is a powder containing metallic zinc, T is the melting point of zinc. When the zinc-containing powder is a powder containing a zinc alloy, T is the melting point of the zinc alloy.
[0036] The rotation speed may be, for example, 5 rpm or more, 10 rpm or more, or 20 rpm or more, and may be 200 rpm or less, 100 rpm or less, or 50 rpm or less. The rotation time (film formation time) may be appropriately determined depending on the rotation speed and the processing amount. The rotation time (film formation time) may be, for example, 10 minutes or more, 20 minutes or more, 40 minutes or more, 60 minutes or more, 80 minutes or more, 100 minutes or more, or 120 minutes or more, and may be 240 minutes or less, 180 minutes or less, or 150 minutes or less.
[0037] After the coating 20 is formed on the surface of the particles of the magnetic powder 10, if the particles of the coated powder 30 are bonded to each other, the bonded body may be pulverized. The pulverization method is not particularly limited, and examples thereof include pulverization methods using a ball mill, a jaw crusher, a jet mill, a cutter mill, and combinations of these.
[0038] Vapor Deposition Method FIG. 3 is an explanatory diagram showing an example of a method for forming a zinc-containing coating on the surface of a magnetic powder particle by using a vapor deposition method.
[0039] The magnetic powder 10 is stored in a first container 181, and the zinc-containing powder 50 is stored in a second container 182. The first container 181 is stored in a first heat treatment furnace 171, and the second container 182 is stored in a second heat treatment furnace 172. The first heat treatment furnace 171 and the second heat treatment furnace 172 are connected by a connecting path 173. The first heat treatment furnace 171 and the second heat treatment furnace 172 and the connecting path 173 are airtight, and a vacuum pump 180 is connected to the second heat treatment furnace.
[0040] After the insides of the first heat treatment furnace 171, the second heat treatment furnace 172 and the connecting passage 173 are depressurized by the vacuum pump 180, these insides are heated. Then, zinc-containing vapor is generated from the zinc-containing powder 50 stored in the second container 182. The zinc-containing vapor moves from the inside of the second container 182 to the inside of the first container 181, as shown by the solid line arrow in FIG.
[0041] The zinc-containing vapor that has moved to the inside of the first container 181 is cooled and forms (deposits) a coating 20 on the surface of the particles of the magnetic powder 10. The vicinity of the interface between the thus obtained coating 20 and the surface of the particles of the magnetic powder 10 is substantially not modified.
[0042] By making the first container 181 a rotary container, it can be made to function like a kiln, and it is possible to further increase the coverage of the coating 20 formed on the surface of the magnetic powder 10. The coverage will be described later.
[0043] The conditions for forming the coating 20 by the method shown in FIG. 3 may be appropriately determined so as to obtain a desired coating.
[0044] The temperature of the first heat treatment furnace (heating temperature of the samarium-iron-nitrogen magnetic powder) may be, for example, 120°C or more, 140°C or more, 160°C or more, 180°C or more, 200°C or more, or 220°C or more, and may be 410°C or less, 400°C or less, 380°C or less, 360°C or less, 340°C or less, 320°C or less, 300°C or less, 280°C or less, or 260°C or less.
[0045] The temperature of the second heat treatment furnace (heating temperature of the zinc-containing powder 50), when the melting point of the zinc-containing powder 50 is T, may be, for example, (T-30) ° C. or more, (T-20) ° C. or more, (T-10) ° C. or more, T ° C. or more, (T+20) ° C. or more, (T+40) ° C. or more, (T+60) ° C. or more, (T+80) ° C. or more, (T+100) ° C. or more, or (T+120) ° C. or more, and may be (T+200) ° C. or less, (T+180) ° C. or less, (T+160) ° C. or less, or (T+140) ° C. or less. In addition, when the zinc-containing powder is a powder containing metal zinc, T is the melting point of zinc. In addition, when the zinc-containing powder is a powder containing a zinc alloy, T is the melting point of the zinc alloy. The second container 182 may store a bulk material containing zinc. However, from the viewpoint of quickly melting the charge in the second container 182 and generating vapor containing zinc from the molten liquid, it is preferable to store a powder containing zinc in the second container 182.
[0046] The first heat treatment furnace and the second heat treatment furnace are set to a reduced pressure atmosphere in order to promote the generation of vapor containing zinc and to prevent oxidation of the magnetic powder 10, the zinc-containing powder 50, the coating 20, etc. The atmospheric pressure is, for example, 1×10 absolute pressure. -1 Pa or less, 1×10 -2 Pa or less, 1×10 -3 Pa or less, 1×10 -4 Pa or less, 1×10 -5 Pa or less, 1×10 -6 Pa or less, or 1×10 -7On the other hand, there is no practical problem even if the pressure is not excessively reduced, and as long as the above-mentioned atmospheric pressure is satisfied, the atmospheric pressure may be 1×10 -8 Pa or more. When the temperature of the second heat treatment furnace is set to be less than T° C. within the above-mentioned temperature range, it is preferable to make the atmospheric pressure as low as possible within the above-mentioned range so that the zinc-containing powder 50 can easily sublimate.
[0047] When the first container 181 is a rotating container, the rotation speed may be, for example, 5 rpm or more, 10 rpm or more, or 20 rpm or more, and may be 200 rpm or less, 100 rpm or less, or 50 rpm or less.
[0048] In the deposition method, after forming the zinc-containing coating 20 on the surface of the magnetic powder 10 particles, if the particles of the coated powder 30 are bonded to each other, the bonded body may be pulverized. The pulverization method is not particularly limited, and examples thereof include pulverization methods using a ball mill, a jaw crusher, a jet mill, a cutter mill, and combinations of these.
[0049] <Kneading method> Compared with magnetic powder, powder containing zinc is very soft. Therefore, when magnetic powder and powder containing zinc are kneaded, the particles of the powder containing zinc are deformed, and the deformed material (material containing zinc) adheres to the outer circumference of the particles of the magnetic powder to form a coating. There is no particular restriction on the kneading method as long as a desired coverage is obtained. From the viewpoint of deforming the particles of the powder containing zinc, it is preferable to knead using, for example, a ball mill, an attritor, a Muller wheel mixer, Mechanofusion, and Nobilta (registered trademark), etc. These may be used in combination.
[0050] In the kneading method, after forming a zinc-containing coating on the surface of the magnetic powder particles, if the coated powder particles are bonded to each other, the bonded body may be pulverized. The pulverization method is not particularly limited, and examples thereof include pulverization methods using a ball mill, a jaw crusher, a jet mill, a cutter mill, and combinations thereof.
[0051] <Coverage rate> As described above, in the method of manufacturing rare earth magnets disclosed herein, the coating formed on the surface of the magnetic powder particles allows compaction of the coated powder in air. If the coverage is 96% or more, 97% or more, 98% or more, or 99% or more, oxidation of the magnetic particles in the coated powder can be suppressed, and the decrease in remanence can be suppressed to a substantially negligible range. The higher the coverage, the better, with 100% being ideal.
[0052] The coverage rate is the percentage of the coating relative to the entire surface of the coated powder particles. The coverage rate (%) is calculated as follows.
[0053] X-ray photoelectron spectroscopy (XPS) is used to obtain composition information on the constituent elements of the magnetic powder and the coating for the coating powder. Then, the coverage rate (%) is calculated using the following formula.
[0054] Coverage rate (%) = (total of composition information for each of the constituent elements of the coating) / {(total of composition information for each of the constituent elements of the magnetic powder) + (total of composition information for each of the constituent elements of the coating)}) x 100
[0055] For example, when the magnetic powder is composed of Sm, Fe, and N, the sum of the composition information for each of the constituent elements of the magnetic powder means the sum of the composition information for each of Sm, Fe, and N. Also, when the coating is, for example, metallic zinc, the sum of the composition information for each of the constituent elements of the coating means the composition information for Zn. When the coating is, for example, a zinc alloy, the sum of the composition information for each of the constituent elements of the coating means the sum of the composition information for Zn and each of the alloying elements. When the zinc alloy is, for example, a Zn-Al alloy, the sum of the composition information for each of the constituent elements of the coating means the sum of the composition information for Zn and Al.
[0056] For example, the composition information for Zn means the mass of Zn present, which is obtained by measuring the XPS spectrum of the coated particle and determining the peak intensity of the obtained XPS spectrum. In the case where the magnetic powder is composed of, for example, Sm, Fe, and N, and the coating is, for example, metallic zinc, the coverage (%) is calculated as follows: Coverage rate (%) = (abundant mass of Zn) / (abundant masses of Sm, Fe, N, and Zn) × 100
[0057] <Compression molding process> The coated powder is compressed under atmospheric pressure to obtain a green compact. In the manufacturing method of the rare earth magnet disclosed herein, since the coated powder has a predetermined coverage, the oxidation of the magnetic powder can be suppressed even if the coated powder is compressed under atmospheric pressure. There is no particular limitation on the compression molding method. For example, a method using a metal mold equipped with a die and a punch can be mentioned. FIG. 4 is an explanatory diagram showing a schematic example of a metal mold used for powder compaction. The die 200 has a cavity 210, and the punch 220 slides inside the cavity. The coated powder is stored in the cavity 210 of the die 200, and the punch 220 is moved to compact the coated powder. When the coated powder is compressed while applying a magnetic field, an electromagnetic coil 250 may be arranged as shown in FIG. 4. In addition, when the same die 200 and punch 220 are used for powder compaction and pressure sintering, a heater 240 for heating may be arranged.
[0058] From the viewpoint of increasing the density of the rare earth magnet (molded body), it is preferable to apply a high pressure during compression molding, as long as it does not damage the die 200 and punch 220. The pressure during compression molding may be, for example, 10 MPa or more, 50 MPa or more, 100 MPa or more, 200 MPa or more, 250 MPa or more, or 300 MPa or more, and may be 5000 MPa or less, 4000 MPa or less, 3000 MPa or less, 2000 MPa or less, 1000 MPa or less, 500 MPa or less, 400 MPa or less, or 350 MPa or less. There is no particular limit to the pressure application time, and it may be 0.2 minutes or more, 0.4 minutes or more, 0.6 minutes or more, 0.8 minutes or more, or 1 minute or more, and may be 5 minutes or less, 3 minutes or less, or 2 minutes or less.
[0059] When the coating powder is compressed in the cold state, a green compact is obtained. "Cold" means a temperature at which sintering (solidification) of the coating powder does not substantially start. The temperature at which sintering (solidification) starts means a temperature at which the zinc component in the zinc-containing powder starts solid-phase or liquid-phase diffusion to the surface of the magnetic powder particles. The temperature at which the coating powder is compressed may be, for example, 0°C or higher, 10°C or higher, 20°C or higher, 30°C or higher, or 40°C or higher, and may be 100°C or lower, 80°C or lower, 60°C or lower, or 50°C or lower. Typically, the coating powder is compressed at room temperature.
[0060] <Magnetic field application process> The coating powder may be compression molded in a magnetic field. In this case, a magnetic field is applied to the coating powder. This allows the coating powder to be magnetically oriented during compression, and makes it possible to impart anisotropy to the rare earth magnet (sintered body). There are no particular limitations on the direction in which the magnetic field is applied, but typically the magnetic field is applied in a direction approximately perpendicular to the compression molding direction of the coating powder.
[0061] There is no particular limitation on the method of applying the magnetic field. For example, the method of applying the magnetic field includes a method of charging the coating powder into a container and applying a magnetic field to the coating powder. The container is not particularly limited as long as a magnetic field can be applied to the inside of the container, and for example, a die and a punch for compression molding the coating powder can be used as the container. When applying the magnetic field, a magnetic field generating device can be installed on the outer periphery of the container. In addition, when the magnetic field to be applied is strong, for example, a magnetizing device can also be used.
[0062] The magnitude of the magnetic field to be applied may be, for example, 100 kA / m or more, 150 kA / m or more, 160 kA / m or more, 300 kA / m or more, 500 kA / m or more, 1000 kA / m, or 1500 km / A or more, and may be 4000 kA / m or less, 3000 kA / m or less, 2500 kA / m or less, or 2000 kA / m or less. Methods for applying a magnetic field include a method of applying a static magnetic field using an electromagnet and a method of applying a pulse magnetic field using an alternating current.
[0063] <Pressure sintering process> The coated powder is pressure sintered in a vacuum or in an inert gas atmosphere. By using a vacuum or inert gas atmosphere, oxidation of the magnetic powder and the like is suppressed. From the viewpoint of suppressing oxidation, an inert gas atmosphere is preferable. The inert gas atmosphere includes a nitrogen gas atmosphere.
[0064] When pressure sintering is performed in a vacuum, the atmospheric pressure is, for example, 1×10 -1 Pa or less, 1×10 -2 Pa or less, 1×10 -3 Pa or less, 1×10 -4 Pa or less, 1×10 -5 Pa or less, 1×10 -6 Pa or less, or 1×10 -7 On the other hand, there is no practical problem even if the pressure is not excessively reduced, and as long as the above-mentioned atmospheric pressure is satisfied, the atmospheric pressure may be 1×10 -8 During pressure sintering, the magnetic powder is easily oxidized due to the high temperature and pressure. -5 Pa or less, 1×10 -6 Pa or less, or 1×10 -7 Pa or less is preferable.
[0065] The conditions such as temperature, pressure and time during pressure sintering may be appropriately determined so that nitrogen in the magnetic phase of the magnetic powder is not dissociated and the coated powder undergoes solid-phase sintering or liquid-phase sintering.
[0066] The pressure sintering temperature may be, for example, 350° C. or more, 360° C. or more, or 370° C. or more, and may be 500° C. or less, 480° C. or less, 460° C. or less, 440° C. or less, 420° C. or less, 400° C. or less, or 380° C. or less. From the viewpoint of preventing excessive progress of the modification, the pressure sintering temperature is preferably 380° C. or less.
[0067] The pressure sintering pressure may be, for example, 200 MPa or more, 300 MPa or more, 400 MPa or more, 500 MPa, 600 MPa or more, 700 MPa or more, or 900 MPa or more, and may be 2000 MPa or less, 1500 MPa or less, or 1000 MPa or less.
[0068] The pressure sintering time may be, for example, 1 minute or more, 2 minutes or more, or 3 minutes or more, and may be 120 minutes or less, 60 minutes or less, 30 minutes or less, 10 minutes or less, or 5 minutes or less. From the viewpoint of not excessively progressing the modification, the pressure sintering time is preferably 5 minutes or less.
[0069] As long as the above-mentioned points are satisfied, there is no particular limitation on the method of pressure sintering. As the pressure sintering method, for example, a method using a die and a punch can be mentioned.
[0070] Next, the magnetic powder and coating composition will be described.
[0071] <Magnetic powder> The magnetic powder used in the method for producing a rare earth magnet of the present disclosure contains samarium, iron, and nitrogen, and is 17 Type and Th2Ni 17 The magnetic phase has at least one of the following crystal structures: TbCu7 type, TbCu8 type, and TbCu1 type. The magnetic phase has the above-mentioned crystal structure, and the like. Here, Th is thorium, Zn is zinc, Ni is nickel, Tb is terbium, and Cu is copper.
[0072] In the magnetic powder, for example, the composition formula (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 N h The rare earth magnet obtained by the manufacturing method of the present disclosure (hereinafter, sometimes referred to as the "result") exhibits magnetic properties due to the magnetic phase in the magnetic powder. Note that i, j, and h are molar ratios. Note that Sm is samarium, Fe is iron, Co is cobalt, and N is nitrogen.
[0073] The magnetic phase in the magnetic powder may contain R within a range that does not impair the effect of the manufacturing method of the present disclosure and the magnetic properties of the product. Such a range is represented by i in the above composition formula. i may be, for example, 0 or more, 0.10 or more, or 0.20 or more, and 0.50 or less, 0.40 or less, or 0.30 or less. R is one or more selected from rare earth elements other than samarium, yttrium, and zirconium. In this specification, the rare earth elements are scandium, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, eurobium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and ruthenium.
[0074] (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 N h For example, Sm2(Fe (1-j) Co j ) 17 N h The Sm position is substituted with R, but this is not limited to this. For example, Sm2(Fe (1-j) Co j ) 17 N h A part of R may be interstitially arranged in the
[0075] The magnetic phase in the magnetic powder may contain Co within a range that does not impair the effect of the manufacturing method for rare earth magnet of the present disclosure and the magnetic properties of the resulting product. Such a range is represented by j in the above composition formula. j may be 0 or more, 0.10 or more, or 0.20 or more, and may be 0.52 or less, 0.40 or less, or 0.30 or less.
[0076] (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 N h For example, (Sm (1-i) R i )2Fe 17 Nh Co is substituted for the Fe position in, but this is not limited to this. For example, (Sm (1-i) R i )2Fe 17 N h A part of Co may be interstitially arranged in the GaN layer.
[0077] The magnetic phase in the magnetic powder is (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 The presence of interstitial N in the crystal grains represented by the formula (I) contributes to the development and improvement of magnetic properties.
[0078] (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 N h For h, h can be 1.5 to 4.5, but typically, (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 N3. h may be 1.8 or more, 2.0 or more, or 2.5 or more, and may be 4.2 or less, 4.0 or less, or 3.5 or less. (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 N h For the whole (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 The content of N3 is preferably 70 mass% or more, more preferably 80 mass% or more, and even more preferably 90 mass% or more. (1-i) R i )2(Fe (1-j) Co j ) 17 N h All of this (Sm (1-i) R i )2(Fe (1-j) Co j ) 17It doesn't have to be N3. (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 N h For the whole (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 The content of N3 may be 99% by mass or less, 98% by mass or less, or 97% by mass or less.
[0079] The magnetic powder is (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 N h In addition to the magnetic phase represented by the formula (I), oxygen and M may be added to the extent that they do not substantially impair the effect of the method for producing a rare earth magnet of the present disclosure and the magnetic properties of the resulting product. 1 In order to ensure the magnetic properties of the product, the total amount of the magnetic powder (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 N h The content of the magnetic phase represented by may be 80 mass% or more, 85 mass% or more, or 90 mass% or more. On the other hand, the content of the magnetic phase represented by (Sm (1-i) R i )2(Fe (1-j) Co j ) 17 N h There is no practical problem even if the content of the magnetic phase represented by the formula (Sm) is not excessively high. Therefore, the content may be 99% by mass or less, 98% by mass or less, or 97% by mass or less. (1-i) R i )2(Fe (1-j) Co j ) 17 N h The remainder of the magnetic phase represented by the formula is oxygen and M 1 The content of M 1 A portion of may be present in the magnetic phase in an interstitial and / or substitutional form.
[0080] The above mentioned M 1 Examples of the impurity elements include one or more elements selected from the group consisting of gallium, titanium, chromium, zinc, manganese, vanadium, molybdenum, tungsten, silicon, rhenium, copper, aluminum, calcium, boron, nickel, and carbon. The unavoidable impurity elements refer to impurity elements whose inclusion is unavoidable when manufacturing magnetic powders, etc., or whose avoidance would lead to a significant increase in manufacturing costs. These elements may be present in the above-mentioned magnetic phases as substitutional and / or interstitial types, or may be present in phases other than the above-mentioned magnetic phases. Alternatively, they may be present in the grain boundaries of these phases.
[0081] There is no particular restriction on the particle size of the magnetic powder, so long as the resulting product has the desired magnetic properties and does not impair the effects of the method for producing a rare earth magnet of the present disclosure. 50 For example, D may be 1 μm or more, 2 μm or more, 3 μm or more, 4 μm or more, 5 μm or more, 6 μm or more, 7 μm or more, 8 μm or more, or 9 μm or more, and may be 20 μm or less, 19 μm or less, 18 μm or less, 17 μm or less, 16 μm or less, 15 μm or less, 14 μm or less, 13 μm or less, 12 μm or less, 11 μm or less, or 10 μm or less. 50 means the median diameter. Also, D of the magnetic powder 50 is measured, for example, by a dry laser diffraction / scattering method.
[0082] As long as the magnetic powder satisfies the above description, there is no particular limitation on the manufacturing method thereof, and a commercially available product may be used. As a manufacturing method of the magnetic powder, for example, a method of manufacturing a samarium-iron alloy powder from samarium oxide and iron powder by a reduction diffusion method, and performing a heat treatment at 600°C or less in an atmosphere of a mixed gas of nitrogen and hydrogen, nitrogen gas, ammonia gas, or the like to obtain a samarium-iron-nitrogen magnetic powder, etc., can be mentioned. Alternatively, for example, a method of manufacturing a samarium-iron alloy by a melting method, coarsely crushing the alloy to obtain coarsely crushed particles, nitriding the resulting particles, and further crushing the particles until they reach a desired particle size can be mentioned. For example, a dry jet mill, a dry ball mill, a wet ball mill, or a wet bead mill can be used for the crushing. These methods may also be used in combination.
[0083] <Coating composition> The coating has both a binder function and a property-modifying function. The coating has a binder function, which allows a sintered body to be obtained at a low temperature at which the nitrogen in the magnetic phase does not dissociate. In addition, the coating forms a modifying phase, mainly with the α-Fe phase, in the magnetic powder, thereby suppressing a decrease in coercivity. The coating having such a function contains zinc. The modifying phase is considered to be a zinc-iron phase (Zn-Fe phase). Examples of zinc-iron phases include Γ phase, Γ1 phase, δ 1k Phase, δ 1p phase, and zeta phase.
[0084] Examples of coatings having the above-mentioned functions include coatings containing metallic zinc, coatings containing zinc alloys, and coatings containing metallic zinc and zinc alloys. Metallic zinc means unalloyed zinc. The purity of the metallic zinc coating may be 95.0% by mass or more, 98.0% by mass or more, 99.0% by mass or more, or 99.9% by mass or more.
[0085] When the coating is formed by the rotary kiln method and / or the kneading method, for example, a powder containing metallic zinc powder and / or a powder containing a zinc alloy is used. In particular, when a powder containing metallic zinc powder is used, metallic zinc powder produced by a hydrogen plasma reaction method (HPMR method) is used, but is not limited thereto. Metallic zinc powder produced by a hydrogen plasma reaction method has a very low oxygen content, and is advantageous in absorbing oxygen contained in a magnetic material and improving magnetic properties, particularly coercive force. From this viewpoint, when a powder containing zinc is used in the coating step, the oxygen content is preferably 5.0 mass% or less, more preferably 3.0 mass%, and even more preferably 1.0 mass% or less, based on the entire zinc-containing powder. On the other hand, extremely reducing the oxygen content of the zinc-containing powder leads to an increase in manufacturing costs. For this reason, the oxygen content of the zinc-containing powder may be 0.1 mass% or more, 0.2 mass% or more, or 0.3 mass% or more, based on the entire zinc-containing powder.
[0086] In the above explanation, for example, "powder containing metallic zinc" means that it may contain substances that are inevitably contained other than the metallic zinc powder. The content of the unavoidable impurities is preferably 5 mass% or less with respect to the entire powder containing metallic zinc. Incidentally, the unavoidable impurities are substances that are inevitably contained when producing the metallic zinc powder, and are typically oxides. What has been explained here also applies to powders other than the powder containing metallic zinc.
[0087] Zinc alloy Zinc-M 2 Expressed as M 2 is preferably an element that alloys with zinc to lower the melting point (melting start temperature) of the zinc alloy below the melting point of zinc, and an unavoidable impurity element. This facilitates pressure sintering at a lower temperature, and can suppress excessive modification caused by reaction of the magnetic phase with the zinc component other than the α-Fe phase during pressure sintering.
[0088] The melting point of the zinc alloy is lowered below that of zinc.2 As for zinc and M 2 These elements form eutectic alloys with M. 2 The elements that are typically used are tin, magnesium, and aluminum, as well as combinations thereof. The melting point lowering effect of these elements and elements that do not impair the properties of the resulting product are also included in the M 2 The unavoidable impurity elements refer to impurity elements, such as impurities contained in raw materials, whose inclusion cannot be avoided, or whose avoidance would result in a significant increase in production costs.
[0089] Zinc-M 2 In the zinc alloy represented by the formula 2 The ratio (molar ratio) of M to the entire zinc alloy may be appropriately determined so that the pressure sintering temperature is appropriate. 2 The ratio (molar ratio) may be, for example, 0.02 or more, 0.05 or more, 0.10 or more, or 0.20 or more, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less.
[0090] Among zinc alloys, a typical zinc-aluminum alloy will be further described. The zinc-aluminum alloy may contain 8 to 90 atomic % of zinc and 2 to 10 atomic % of aluminum. Alternatively, the zinc-aluminum alloy may contain 2 to 10 atomic % of aluminum, with the remainder being zinc and unavoidable impurities.
[0091] There is no particular restriction on the particle size of the metallic zinc powder and / or zinc alloy powder used in the rotary kiln method and the kneading method, but by making the particle size finer than that of the magnetic powder, it becomes easier to improve the coverage rate even if the amount of metallic zinc powder and / or zinc alloy powder is small. The particle size of the metallic zinc powder and / or zinc alloy powder is D 50The particle size (median diameter) may be, for example, more than 0.1 μm, 0.5 μm or more, 1 μm or more, or 2 μm or more, and may be 12 μm or less, 11 μm or less, 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, 5 μm or less, or 4 μm or less. The particle size of the zinc metal powder and / or zinc alloy powder is measured, for example, by a dry laser diffraction / scattering method or the like. EXAMPLES
[0092] The method for producing a rare earth magnet according to the present disclosure will be described in more detail below with reference to examples and comparative examples. Note that the method for producing a rare earth magnet according to the present disclosure is not limited to the conditions used in the following examples.
[0093] <Sample preparation> The rare earth magnet samples were prepared as follows.
[0094] Example 1 Using the apparatus shown in Figure 2, a coating containing zinc was formed on the surface of the magnetic powder particles to obtain a coated powder. 50 The powder used had a diameter of 3.16 μm. The zinc-containing powder used was zinc metal powder manufactured by Kamite Co., Ltd. This zinc metal powder was 50 The particle size was 0.5 μm, and the oxygen content was 1000 mass ppm or less. The oxygen content was measured by an infrared absorption method. The amount of the metal zinc powder used (blended amount) was 30 mass % based on the magnetic powder.
[0095] Regarding the operating conditions of the equipment (rotary kiln) shown in Figure 2, the temperature inside the furnace is 410°C, and the absolute pressure inside the furnace is 1×10 -2 The pressure was below 1 Pa. The rotary kiln was rotated at 6 rpm for 100 minutes.
[0096] 1 g of the coated powder prepared as described above was placed in a cavity of a 7 mm square cemented carbide die, and compressed at 300 MPa in air using a hydraulic press to obtain a green compact. No magnetic field was applied during compression molding.
[0097] The green compact prepared as described above was subjected to pressure sintering in an argon gas atmosphere (97000 Pa). The pressure sintering temperature was 380° C., the pressure sintering pressure was 300 MPa, and the pressure sintering time was 5 minutes.
[0098] Example 2 A sample of Example 2 was prepared in the same manner as Example 1, except that the amount of zinc metal powder used (blended amount) was 20 mass % based on the magnetic powder.
[0099] Comparative Example 1 A sample of Comparative Example 1 was prepared in the same manner as in Example 1, except that pressure sintering was carried out in air.
[0100] Comparative Example 2 A sample of Comparative Example 2 was prepared in the same manner as in Example 1, except that the amount (blended amount) of the metallic zinc powder used was 15 mass % based on the magnetic powder.
[0101] Comparative Example 3 A sample of Comparative Example 3 was prepared in the same manner as in Example 1, except that no coating was formed on the magnetic powder.
[0102] <Reference example 1> A sample of Reference Example 1 was prepared in the same manner as in Example 1, except that the coated powder was compression molded in an argon gas atmosphere to obtain a green compact.
[0103] <Reference example 2> A sample of Reference Example 2 was prepared in the same manner as in Example 1, except that the coated powder was not compression molded or pressure sintered. That is, the sample of Reference Example 2 is a sample of the coated powder of Example 1 as it is.
[0104] "evaluation" The coverage of the coated powder was measured by the above-mentioned X-ray photoelectron spectroscopy (XPS) method. The residual magnetization was also measured by a vibrating sample magnetometer (VSM). The maximum applied magnetic field during the measurement was 2.0 T.
[0105] The results are shown in Table 1.
[0106] [Table 1]
[0107] In Examples 1 and 2, which used coated powders having a coating rate of 96% or more, it was confirmed that the same residual magnetization was obtained as in Reference Example 1, in which compression molding (compression) was performed in an inert gas atmosphere, even when compression molding (compression) was performed in the atmosphere. In contrast, in Comparative Example 2, which had a coating rate of less than 96%, and Comparative Example 3, which had no coating (0% coverage), it was confirmed that the residual magnetization was reduced when compression molding (compression) was performed in the atmosphere. It was also confirmed that the residual magnetization was reduced when pressure sintering was performed in the atmosphere, even when the coverage was 100%. Furthermore, it was confirmed that Reference Example 1, in which all steps were performed in a vacuum or inert gas atmosphere, had a residual magnetization almost equivalent to that of Reference Example 2, in which the coated powder was used as is.
[0108] These results confirmed the effectiveness of the manufacturing method for rare earth magnets of the present disclosure. [Explanation of symbols]
[0109] 10 magnetic powder 20 Coating 25 Oxide film 30 Coating Powder 40 Oxygen 50 Zinc-containing powder 100 Rotary Kiln Furnace 110 Mixing drum 120 Material Storage Section 130 Rotational Axis 140 Stirring plate 171 No. 1 Heat Treatment Furnace 172 No. 2 heat treatment furnace 173 Connecting road 180 Vacuum Pump 181 1st container 182 Second container 200 Dice 210 Cavity 220 Punch 240 Heater 250 Electromagnetic Coil
Claims
1. Contains samarium, iron, and nitrogen; Th 2 Zinc 17 Type and Th 2 Ni 17 forming a coating containing zinc on the surface of a magnetic powder particle having a magnetic phase having at least one of the crystal structures of the above types to obtain a coated powder; Compressing the coated powder to obtain a green compact; and Pressurizing and sintering the powder compact; Including, The magnetic powder and the zinc-containing powder were charged into a rotary kiln, and the mixture was heated at an absolute pressure of 1×10 -8 Pa or more, 1×10 -1 The pressure inside the furnace is reduced to Pa or less, and the temperature inside the furnace is maintained at (T-30)°C or more and less than T°C, where T°C is the melting point of the zinc-containing powder, while the furnace body is rotated to sublimate zinc from the zinc-containing powder, and 20 to 30 mass% of zinc based on the magnetic powder is deposited on the surfaces of the particles of the magnetic powder, so that the coverage of the coating with respect to the entire surface of the particles of the coated powder is 96% or more, The formation of the coating and the pressure sintering of the green compact are carried out in a vacuum or an inert gas atmosphere; The pressure sintering is carried out at 350 to 380° C. for 1 to 5 minutes while applying a pressure of 100 to 300 MPa; The compression molding of the coating powder is carried out in air at room temperature; and The rotary kiln includes a stirring drum having a stirring plate therein. A method for manufacturing rare earth magnets.
2. The method for producing a rare earth magnet according to claim 1 , wherein the coated powder is compression-molded in a magnetic field to obtain the green compact while magnetically orienting the coated powder.
3. The method for producing a rare earth magnet according to claim 1 or 2, wherein the pressure sintering is carried out in an inert gas atmosphere.
Citation Information
Patent Citations
Surface rust prevention and performance improving treatment of magnetic material
JP2001254168A
Anisotropic rare earth bonded magnet and its manufacturing method
JP2003168602A
Method of producing rare earth magnet
JP2019012796A
Manufacturing method of rare-earth magnet and manufacturing installation for use therein
JP2019186368A