Biaxially oriented films and laminated films
A biaxially stretched film using polyethylene naphthalate and amorphous polyester with controlled hysteresis and residual strain addresses the limitations of existing films, providing enhanced heat resistance and folding durability for flexible display applications.
Patent Information
- Application Number
- JP2021019381
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-02-09
AI Technical Summary
Existing polyester films, such as those made from polyethylene terephthalate (PET) and polyimide, lack sufficient bending resistance and adhesion properties, and their manufacturing processes are inefficient, leading to high costs and poor moldability.
A biaxially stretched film composed of a polyethylene naphthalate resin and an amorphous polyester with controlled hysteresis loss and residual strain, combined with a laminated structure for improved heat resistance and folding durability.
The film exhibits excellent heat resistance and folding durability, suitable for flexible displays, with reduced anisotropy and improved handling properties, making it suitable for applications like foldable displays.
Smart Images

Figure 0007585842000002 
Figure 0007585842000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a biaxially oriented film and a laminated film. [Background technology]
[0002] Polyester has excellent properties such as heat resistance, weather resistance, mechanical strength, transparency, chemical resistance, and gas barrier properties, and is also readily available at a reasonable price, making it a versatile resin that is currently widely used in beverage and food containers and packaging materials, molded products, films, etc. The main polyester resin is polyethylene terephthalate (hereinafter sometimes referred to as "PET"), which has excellent mechanical properties, electrical properties, chemical resistance, etc. and a wide range of applications, but has drawbacks such as poor heat resistance and folding resistance.
[0003] Meanwhile, in recent years, with the trend towards smaller and lighter electronic devices, there has been a trend towards using flexible substrates and flexible printed circuits. In line with this trend, there is also an increasing demand for flexibility in display applications, and there is a strong demand for films that have high heat resistance, excellent recovery properties, and excellent resistance to repeated bending.
[0004] Flexible displays include types such as foldable, bendable, rollable, and stretchable. A typical example of a flexible display comprises a substrate film made of a synthetic resin such as polyimide, and elements such as thin film transistors (TFTs) and organic light-emitting diodes (OLEDs) supported on the substrate film. In addition to the substrate film, optical films with excellent flexibility are used as components for the front panel of a flexible display, base film for touch sensors, and film for protecting the substrate film (hereinafter referred to as lower protective film), etc.
[0005] Thus, in recent years, resin films with excellent flexibility have been studied. For example, Patent Document 1 studies a film made of a cyclic olefin resin that is resistant to repeated bending.
[0006] Patent Document 2 proposes a polyimide film as a film having excellent heat resistance and bending resistance.
[0007] Furthermore, Patent Document 3 proposes a polyethylene naphthalate resin in which the crystallinity is improved without impairing the heat resistance by blending an ethylene oxide adduct of a bisphenol compound or its derivative in the entire alcohol component.
[0008] Furthermore, Patent Document 4 proposes a modified polyester resin in which heat resistance, impact strength, etc. are improved by blending 2,6-naphthalenedicarboxylic acid as the acid component and a bisphenol-based compound and 1,4-cyclohexanedimethanol as the glycol component. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2014-104687 A [Patent Document 2] International Publication No. 2016 / 060213 [Patent Document 3] Japanese Patent Application Publication No. 8-48759 [Patent Document 4] JP 2004-107559 A Summary of the Invention [Problem to be solved by the invention]
[0010] However, the film disclosed in Patent Document 1 has a low level of resistance to repeated folding, and does not satisfy market demands. Furthermore, cyclic olefin resins have poor coating and adhesive properties, making them difficult to laminate with other materials, making them unsuitable for use as materials for flexible displays.
[0011] Furthermore, although the polyimide film described in Patent Document 2 has flex resistance, the production process thereof involves a molding method using a coating of a solvent, which results in problems such as poor productivity and high costs.
[0012] The polyethylene naphthalate resin described in Patent Document 3 is one that has an improved crystallization rate, alleviates problems that occur during drying of the raw material, and improves moldability by blending an ethylene oxide adduct of a bisphenol compound or its derivative in the entire alcohol component. However, since the crystallization rate is too fast, the film formability and stretchability by extrusion molding are deteriorated, and there is a problem that it is not suitable for stretched films.
[0013] The modified polyester resin described in Patent Document 4 exhibits high heat resistance, but on the other hand, the temperature during molding must be set high, which may result in concerns about thermal decomposition and a decrease in moldability and the properties of the material after molding.
[0014] An object of the present invention is to solve the above problems and to provide a biaxially stretched film having excellent heat resistance and folding resistance. [Means for solving the problem]
[0015] The present inventors have conducted extensive research to achieve the above object, and as a result have completed the present invention. In one aspect, the present invention is summarized as follows [1] to
[12] . [1] A biaxially oriented film comprising a polyethylene naphthalate resin (A) and an amorphous polyester (B) having a higher glass transition temperature than the polyethylene naphthalate resin (A), the film having an average hysteresis loss rate of 46.0% or less when subjected to a tensile cycle test up to 5% tensile strain in each of the longitudinal direction (MD) and the transverse direction (TD). [2] The biaxially stretched film according to the above [1], wherein the polyethylene naphthalate resin (A) is a copolymer containing a dicarboxylic acid component (a-1) and a diol component (a-2), and contains 2,6-naphthalenedicarboxylic acid units as the (a-1) component and ethylene glycol units and bisphenol A-ethylene oxide adduct units as the (a-2) component. [3] The biaxially stretched film according to [2] above, wherein the (a-2) component contains 4 mol% or more and 70 mol% or less of the bisphenol A-ethylene oxide adduct units and 30 mol% or more and 96 mol% or less of ethylene glycol units. [4] The biaxially stretched film according to any one of the above [1] to [3], wherein the amorphous polyester (B) is a polyarylate. [5] The biaxially stretched film according to any one of the above [1] to [4], having an average residual strain of 0.900% or less when subjected to a tensile cycle test up to 5% tensile strain in each of the longitudinal direction (MD) and the transverse direction (TD). [6] The biaxially stretched film according to any one of the above [1] to [5], having a glass transition temperature of 75° C. or higher and 150° C. or lower. [7] The biaxially stretched film according to any one of the above [1] to [6], which has a crystalline melting temperature of 220° C. or higher and 300° C. or lower. [8] The biaxially stretched film according to any one of the above [1] to [7], having a thickness of 1 μm or more and 250 μm or less. [9] The biaxially stretched film according to any one of the above [1] to [8], which is for a flexible display.
[10] A laminated film comprising the biaxially stretched film according to any one of the above [1] to [9] and an adhesive layer provided on at least one surface of the biaxially stretched film.
[11] The laminated film according to
[10] above, having a coating layer between the biaxially stretched film and the adhesive layer.
[12] A flexible display comprising the biaxially stretched film according to any one of the above [1] to [9] or the laminated film according to the above
[10] or
[11] . Effect of the Invention
[0016] The biaxially stretched film and laminated film of the present invention have excellent heat resistance and folding resistance. Therefore, the biaxially stretched film and laminated film of the present invention can be suitably used for flexible displays and the like. [Brief description of the drawings]
[0017] [Figure 1] 1 is a profile of a stress-strain curve. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will be described in detail below. However, the present invention is not limited to the embodiments described below.
[0019] [Biaxially oriented film] A biaxially stretched film according to one embodiment of the present invention (hereinafter, sometimes referred to as "the film") contains a polyethylene naphthalate (hereinafter, sometimes referred to as "PEN")-based resin (A) and an amorphous polyester (B) having a higher glass transition temperature than the polyethylene naphthalate-based resin (A), and is characterized in that the average hysteresis loss rate when subjected to a tensile cycle test up to 5% tensile strain in each of the longitudinal direction (MD) and the transverse direction (TD) is 46.0% or less. Since the present film is a biaxially oriented film, it can be made thin, and since the hysteresis loss is adjusted to within a specific range by using a specific mixed resin material, the film has excellent heat resistance and folding resistance. In the present invention, the machine direction (MD) of the film refers to the direction in which the film travels during the film production process, that is, the winding direction of the film roll. The transverse direction (TD) of the film refers to a direction parallel to the film surface and perpendicular to the longitudinal direction, that is, a direction parallel to the central axis of the roll of the film.
[0020] The present invention was completed based on the discovery that the present film, which has a hysteresis loss rate of a specific value or less, has excellent heat resistance and folding resistance as a display film and is suitable for flexible applications, particularly foldable applications. This film has a low hysteresis loss rate, which is believed to be why it has excellent recovery and folding resistance.
[0021] 1. Physical properties First, the physical properties of the present film will be described.
[0022] (1) Hysteresis loss rate The film has an average hysteresis loss rate of 46.0% or less, preferably 45.0% or less, and more preferably 44.0% or less, when subjected to a tensile cycle test up to 5% tensile strain in each of the machine direction (MD) and the transverse direction (TD) at 23°C. The lower limit is not particularly limited, but is 0.100% or more. By keeping the hysteresis loss rate at 46.0% or less, the restoring force of the film is increased and the bending resistance (folding resistance) of the film is maintained within a practical range.
[0023] Moreover, by taking the hysteresis loss rate as an average value in each of the machine direction (MD) and the transverse direction (TD), it can be used as an index of properties of the entire film. The hysteresis loss rate can be adjusted by the type and content of the resin used, the stretching conditions, and the like. The hysteresis loss rate of the present film can be measured by the method described in the Examples in accordance with JIS K 7312:1996. More specifically, when a stress-strain curve like that shown in Figure 1 is obtained by a tensile cycle test, the ratio of the area enclosed by abcef to the total area (abcda) is defined as the hysteresis loss rate.
[0024] Furthermore, the difference in hysteresis loss rate between the machine direction (MD) and the transverse direction (TD) of the present film at 23° C. is preferably 20.0% or less, more preferably 15.0% or less, and even more preferably 13.0% or less. When the difference in hysteresis loss rate between the machine direction (MD) and the transverse direction (TD) is within the above range, the bending resistance of the film and therefore the anisotropy of various properties of the film become small, so that the film is not restricted by the direction. Therefore, when the film is used as a component or during manufacturing steps such as secondary processing, it is no longer necessary to select a specific direction, which has the advantage of preventing an increase in the workload of workers. In addition, since defects in a specific direction due to anisotropy are unlikely to occur, the film also has excellent handleability. In addition, as a method for reducing the difference in hysteresis loss rate between the machine direction (MD) and the transverse direction (TD), for example, a desired value can be achieved by controlling the stretching ratio in each direction.
[0025] (2) Residual strain The average value of the residual strain when the film is subjected to a tensile cycle test up to 5% tensile strain in each of the machine direction (MD) and the transverse direction (TD) at 23° C. is preferably 0.900% or less, more preferably 0.880% or less, further preferably 0.860% or less, and particularly preferably 0.840% or less. The lower limit is not particularly limited, but is 0.100% or more. By keeping the residual strain at 0.900% or less, the film's restoring force increases, and the film's bending resistance is kept within a practical range. In addition, by taking the residual strain as an average value in both the machine direction (MD) and the transverse direction (TD), it can be used as an index of the film's overall characteristics. The residual strain can be adjusted by adjusting the stretching conditions, etc. The residual strain of the present film can be measured according to JIS K 7312:1996 by the method described in the Examples. More specifically, when a stress-strain curve such as that shown in FIG. 1 is obtained by a tensile cycle test, the value of f is defined as the residual strain.
[0026] Furthermore, the difference in residual strain between the machine direction (MD) and the transverse direction (TD) of the present film at 23°C is preferably 0.900% or less, more preferably 0.700% or less, even more preferably 0.500% or less, and particularly preferably 0.350% or less. By keeping the difference in residual strain between the machine direction (MD) and the transverse direction (TD) within the above range, the film's bending resistance and, in turn, the anisotropy of various film properties are reduced, so there is no restriction due to the film direction. Therefore, when using the film as a component or in the manufacturing process such as secondary processing, there is no need to select a specific direction, which has the advantage of preventing an increase in the workload of workers. In addition, since defects in a specific direction due to anisotropy are unlikely to occur, the film also has excellent handleability.
[0027] (3) Glass transition temperature The glass transition temperature (Tg) of the present film is preferably from 75° C. to 150° C., more preferably from 76° C. to 140° C., and even more preferably from 77° C. to 130° C. If the glass transition temperature (Tg) of the present film is 75° C. or higher, the film will not deform even when used for display purposes, and therefore the film can be said to have excellent heat resistance. On the other hand, if the glass transition temperature (Tg) is 150° C. or lower, the material is also suitable for processability. The glass transition temperature (Tg) of this film is measured using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min according to JIS K7121 (2012).
[0028] (4) Crystal melting temperature The crystalline melting temperature (Tm) of the present film is preferably from 220° C. to 300° C., more preferably from 221° C. to 295° C., even more preferably from 222° C. to 290° C., and particularly preferably from 223° C. to 285° C. If the crystalline melting temperature (Tm) of the present film is within the above range, the present film has an excellent balance between heat resistance and melt extrusion moldability. Here, the crystalline melting temperature (Tm) of the present film is measured in accordance with JIS K7121 (2012) using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min. The crystalline melting temperature (Tm) of the present film can be optimized by adjusting the cooling temperature from the molten state, the stretching ratio, the stretching temperature, and the heat treatment conditions after stretching during the production of the present film.
[0029] (5) Thickness The thickness of the present film is preferably 1 μm or more and 250 μm or less, more preferably 5 μm or more and 200 μm or less. By making it 1 μm or more, the film strength is kept within a practical range. By making it 250 μm or less, folding resistance is easily exhibited. The thickness can be adjusted by film formation and stretching conditions.
[0030] 2. Ingredients Next, the components constituting the present film will be described.
[0031] The present invention is based on the discovery that a film having as its main component a polyester-based mixed resin containing a polyethylene naphthalate-based resin (A), which is a polyester-based resin generally exhibiting a relatively higher yield stress and elastic modulus than polyethylene-based resins and polypropylene-based resins, and an amorphous polyester (B) having a higher glass transition temperature than the polyethylene naphthalate-based resin (A), has excellent bending resistance. Even with polyester resin, which is a material with high yield stress and elastic modulus, if the stress or strain applied due to deformation is large, deformation occurs and unresolved strain remains in the material, which is a problem. However, in the present invention, it has been found that if the hysteresis loss rate of the film is equal to or less than a specific value, the restoring force of the film becomes large and distortion is less likely to occur. Generally, deformation beyond the elastic deformation region causes large strain in the material. However, even if the deformation is within the elastic deformation region, residual strain may remain in the material, leaving traces of deformation such as folds or wrinkles, which may result in poor appearance or affect the material properties themselves. In other words, the smaller the hysteresis loss rate, the higher the recovery from deformation and the smaller the strain remaining in the material. Therefore, even when a deformation within the elastic deformation region or a large strain exceeding the elastic deformation region is applied, deformation marks are unlikely to be left and the material is considered to have excellent deformation resistance. In the present invention, a specific polyester-based mixed resin is used, i.e., a mixed resin containing a polyethylene terephthalate-based resin (A) and an amorphous polyester (B) having a higher glass transition temperature than the resin (A). This makes it possible to keep the hysteresis loss rate of the film below a specific numerical value and to increase the restoring force of the film, thereby suppressing distortion of the material and providing heat resistance.
[0032] <Polyethylene naphthalate resin (A)> The polyethylene naphthalate resin (A) constituting the present film may be a homopolyester or a copolymer polyester, or a blend of a homopolyester and a copolymer polyester. In the case of a homopolyester, it is obtained by polycondensing 2,6-naphthalenedicarboxylic acid as the dicarboxylic acid component (a-1) and ethylene glycol as the diol component (a-2). When a homopolyester is used as the PEN resin, the heat resistance of the biaxially oriented polyester film of the present invention can be further improved.
[0033] On the other hand, in the case of a copolymer polyester, 2,6-naphthalenedicarboxylic acid is an essential component as the dicarboxylic acid component (a-1), and other copolymer components may be added thereto as necessary. Examples of other copolymerization components include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 3,4-furandicarboxylic acid, benzophenone dicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenylether dicarboxylic acid; aliphatic dicarboxylic acids such as cyclohexanedicarboxylic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dimer acid; and oxycarboxylic acids such as p-oxybenzoic acid. Among these, isophthalic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, and 3,4-furandicarboxylic acid are preferred from the viewpoint of moldability. These copolymerization components can be used alone or in combination of two or more. When a copolymer polyester is used as the PEN resin, the folding endurance of the biaxially oriented polyester film of the present invention can be further improved.
[0034] The copolymer polyester contains 2,6-naphthalenedicarboxylic acid units in the dicarboxylic acid component (a-1) at preferably 90 mol % or more, more preferably 92 mol % or more, even more preferably 94 mol % or more, particularly preferably 96 mol % or more, and especially preferably 98 mol % or more, and all of the dicarboxylic acid component (a-1) (100 mol %) may be 2,6-naphthalenedicarboxylic acid. By adjusting the content of the 2,6-naphthalenedicarboxylic acid unit in the dicarboxylic acid component (a-1) to fall within the above numerical range, the glass transition temperature and melting point of the copolymerized polyester are improved, and thus the heat resistance of the present film is improved.
[0035] The copolymer polyester contains, in the dicarboxylic acid component (a-1), preferably 0 mol % or more and 10 mol % or less, more preferably 0 mol % or more and 8 mol % or less, even more preferably 0 mol % or more and 6 mol % or less, particularly preferably 0 mol % or more and 4 mol % or less, and especially preferably 0 mol % or more and 2 mol % or less of other copolymer components. By adjusting the content of the other copolymerization component in the dicarboxylic acid component (a-1) to fall within the above numerical range, the glass transition temperature and melting point of the copolymerized polyester are improved, and thus the heat resistance of the present film is improved.
[0036] As the diol component (a-2), ethylene glycol is an essential component, and other copolymerization components may be used as necessary, such as 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, triethylene glycol, propylene glycol, polyalkylene glycol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, hydroquinone, spiroglycol, 2,2,4,4,-tetramethylcyclobutane-1,3-diol, isosorbide, 1,4-cyclohexanedimethanol, polytetramethylene ether glycol, dimer diol, and bisphenols (bisphenol compounds such as bisphenol A, bisphenol F, or bisphenol S, or derivatives thereof, or ethylene oxide adducts thereof), and among these, 1,4-cyclohexanedimethanol, polytetramethylene ether glycol, dimer diol, and bisphenols are preferred. In particular, from the viewpoint of maintaining the strength of the film, it is preferable to use bisphenols. As the bisphenol, it is preferable to use a bisphenol A-ethylene oxide adduct. These copolymerization components can be used alone or in combination of two or more.
[0037] The copolymer polyester contains ethylene glycol in the diol component (a-2) in an amount of preferably 30 mol % or more and 96 mol % or less, more preferably 40 mol % or more and 95.8 mol % or less, even more preferably 50 mol % or more and 95.6 mol % or less, particularly preferably 60 mol % or more and 95.4 mol % or less, and especially preferably 70 mol % or more and 95.2 mol % or less. By adjusting the content of ethylene glycol in the diol component (a-2) to fall within the above range, the crystallinity of the copolymerized polyester is maintained, and the heat resistance of the present film is improved.
[0038] The copolymer polyester contains another copolymer component in the diol component (a-2) in an amount of preferably 4 mol % or more and 70 mol % or less, more preferably 4.2 mol % or more and 60 mol % or less, even more preferably 4.4 mol % or more and 50 mol % or less, particularly preferably 4.6 mol % or more and 40 mol % or less, and particularly preferably 4.8 mol % or more and 30 mol % or less. By setting the content of other copolymerization components in the diol component (a-2) within the above numerical range, the glass transition temperature and melting point of the copolymerized polyester are improved, and the heat resistance of the present film is improved. In addition, since the crystallinity can be controlled, the crystallization rate can be slowed down, and the extrusion moldability and stretching processability of the film can be improved. In addition, when the content is 70 mol% or less, the melting point does not become too high. Therefore, there is no need to set the molding temperature high, and there is no concern about thermal decomposition.
[0039] The copolymerized polyester constituting the PEN resin (A) is preferably a polyethylene naphthalate copolymer containing a dicarboxylic acid component (a-1) and a diol component (a-2), the component (a-1) containing 2,6-naphthalenedicarboxylic acid units, and the component (a-2) containing ethylene glycol units and bisphenol A-ethylene oxide adduct units.
[0040] The crystalline melting temperature (Tm(A)) of the PEN resin (A) is preferably from 220° C. to 300° C., more preferably from 225° C. to 290° C., even more preferably from 230° C. to 280° C., and particularly preferably from 235° C. to 270° C. If the crystalline melting temperature (Tm(A)) of the PEN resin (A) is within this range, the PEN resin (A) has an excellent balance between heat resistance and melt moldability. The crystalline melting temperature (Tm(A)) of the PEN resin (A) can be measured using a differential scanning calorimeter (DSC) at a heating rate of 10° C. / min in accordance with JIS K7121 (2012).
[0041] The glass transition temperature (Tg(A)) of the PEN resin (A) is preferably from 75° C. to 150° C., more preferably from 77° C. to 145° C., and even more preferably from 80° C. to 140° C. If the glass transition temperature (Tg(A)) of the PEN resin (A) is within this range, the balance between heat resistance and melt moldability is excellent.
[0042] <Amorphous polyester (B)> The amorphous polyester (B) constituting the present film is an amorphous polyester having a higher glass transition temperature (Tg) than the PEN-based resin (A), and is a component that mainly imparts heat resistance to the PEN-based resin (A), which is the component that mainly contributes to folding resistance.
[0043] In general, the heat resistance of a resin composition can be improved by increasing the glass transition temperature (Tg). By mixing the amorphous polyester (B) having a higher glass transition temperature (Tg) than the PEN resin (A), a resin composition having a higher glass transition temperature (Tg) than the PEN resin (A) alone can be obtained, and a film having excellent heat resistance can be obtained. Furthermore, by adding the amorphous polyester (B), the crystallinity of the PEN resin (A) itself can be alleviated, breakage during stretching can be suppressed, and handling properties during processing can be improved.
[0044] The amorphous polyester (B) has, for example, a structure obtained by polycondensation of at least three or more dicarboxylic acid components and diol components. Examples of the dicarboxylic acid component include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 3,4-furandicarboxylic acid, benzophenonedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid; aliphatic dicarboxylic acids such as cyclohexanedicarboxylic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dimer acid; and oxycarboxylic acids such as p-oxybenzoic acid. Examples of the diol component include ethylene glycol, diethylene glycol, propylene glycol, 1,2-propanediol, 1,3-butanediol, 1,4-butanediol, 1,4-cyclohexanedimethanol, 1,5-pentanediol, neopentyl glycol, polytetramethylene ether glycol, dimer diol, polyalkylene glycol, 2,2-bis(4'-β-hydroxyethoxyphenyl)propane, isosorbite, spiroglycol, and bisphenols (bisphenol compounds such as bisphenol A, bisphenol F, bisphenol S, and bisphenol TMC, or derivatives thereof, or ethylene oxide adducts thereof). Among the amorphous polyesters (B), from the viewpoint of folding endurance, amorphous copolyesters containing at least one diol component selected from 1,4-cyclohexanedimethanol, polytetramethylene ether glycol, dimer diol, and bisphenols are preferred. Furthermore, from the viewpoint of achieving both heat resistance and folding resistance, wholly aromatic polyesters are more preferred, and among them, polyarylates (hereinafter sometimes referred to as "PAR") are even more preferred.
[0045] The PAR is a polycondensation product of a dicarboxylic acid component and a dihydric phenol component. The dicarboxylic acid component constituting the PAR is not particularly limited as long as it is a divalent aromatic carboxylic acid, and is preferably a mixture of a terephthalic acid component and an isophthalic acid component. The mixing ratio (molar ratio) of the terephthalic acid component and the isophthalic acid component is preferably terephthalic acid / isophthalic acid=99 / 1 to 1 / 99, more preferably 90 / 10 to 10 / 90, further preferably 80 / 20 to 20 / 80, particularly preferably 70 / 30 to 30 / 70, and particularly preferably 60 / 40 to 40 / 60. When the mixture ratio of terephthalic acid and isophthalic acid as the dicarboxylic acid components is within the above range, the PAR has excellent heat resistance and melt moldability.
[0046] The PAR may be copolymerized with an acid component other than terephthalic acid and isophthalic acid as the dicarboxylic acid component. Specifically, aromatic dicarboxylic acids such as phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, benzophenone dicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenylether dicarboxylic acid are preferred. In order not to impair the heat resistance of the PAR resin, the copolymerization ratio of acid components other than terephthalic acid and isophthalic acid is preferably less than 10 mol %.
[0047] The dihydric phenol component constituting the PAR is not particularly limited as long as it is a dihydric phenol, but it is preferable that the PAR contains either a bisphenol A (2,2-bis(4-hydroxyphenyl)propane) component or a bisphenol TMC (1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane) component, or both bisphenol A and bisphenol TMC. In general, the inclusion of bisphenol A gives PAR excellent melt moldability (fluidity). On the other hand, the inclusion of bisphenol TMC components increases the glass transition temperature, resulting in a PAR with excellent heat resistance. When it is desired to balance the melt moldability and heat resistance, it is preferable to use both the bisphenol A component and the bisphenol TMC component. In this case, the ratio (mol %) of the bisphenol A component to the bisphenol TMC component, bisphenol A / bisphenol TMC, is preferably 99 / 1 to 1 / 99, more preferably 90 / 10 to 10 / 90, further preferably 80 / 20 to 20 / 80, particularly preferably 70 / 30 to 30 / 70, and particularly preferably 60 / 40 to 40 / 60. By setting the ratio of the bisphenol A component and the bisphenol TMC component within this range, a PAR having an excellent balance between heat resistance and melt moldability can be obtained.
[0048] The PAR may be copolymerized with bisphenols other than bisphenol A and bisphenol TMC as the dihydric phenol component. Specifically, bisphenol AP (1,1-bis(4-hydroxyphenyl)-1-phenylethane), bisphenol AF (2,2-bis(4-hydroxyphenyl)hexafluoropropane), bisphenol B (2,2-bis(4-hydroxyphenyl)butane), bisphenol BP (bis(4-hydroxyphenyl)diphenylmethane), bisphenol C (2,2-bis(3-methyl-4-hydroxyphenyl)propane), bisphenol E (1,1-bis(4-hydroxyphenyl)ethane), bisphenol F (bis(4-hydroxyphenyl)methane), bisphenol Examples of such bisphenols include phenol G (2,2-bis(4-hydroxy-3-isopropylphenyl)propane), bisphenol M (1,3-bis(2-(4-hydroxyphenyl)-2-propyl)benzene), bisphenol S (bis(4-hydroxyphenyl)sulfone), bisphenol P (1,4-bis(2-(4-hydroxyphenyl)-2-propyl)benzene), bisphenol PH (5,5'-(1-methylethylidene)-bis[1,1'-(bisphenyl)-2-ol]propane), and bisphenol Z (1,1-bis(4-hydroxyphenyl)cyclohexane). In order not to impair the heat resistance of PAR, the copolymerization ratio of the above compound is preferably less than 10 mol %.
[0049] In order to enhance compatibility with the PEN resin (A), it is preferable to select a mixture of a terephthalic acid component and an isophthalic acid component as the dicarboxylic acid component, and a bisphenol A component, a bisphenol TMC component, or a mixture of bisphenol A and bisphenol TMC as the dihydric phenol component.
[0050] The glass transition temperature (Tg) of the amorphous polyester (B) is preferably 80°C or more and 350°C or less, more preferably 100°C or more and 340°C or less, even more preferably 120°C or more and 330°C or less, particularly preferably 140°C or more and 320°C or less, and especially preferably 160°C or more and 300°C or less. When the glass transition temperature (Tg) of the amorphous polyester (B) falls within the above range, the glass transition temperature of the biaxially stretched film of the present invention falls within a suitable range, and a film having excellent heat resistance and formability can be obtained.
[0051] The difference in glass transition temperature (Tg) between the PEN resin (A) and the amorphous polyester (B) is preferably 5°C or more, more preferably 20°C or more, even more preferably 35°C or more, particularly preferably 50°C or more, and especially preferably 65°C or more. When the difference in glass transition temperature between the PEN resin (A) and the amorphous polyester (B) is within the above range, the glass transition temperature of the biaxially stretched film of the present invention falls within a suitable range, and a film having excellent heat resistance and formability can be obtained. The upper limit of the difference in glass transition temperature (Tg) between the PEN resin (A) and the amorphous polyester (B) is not particularly limited, but is usually 100° C. or less, and preferably 90° C. or less.
[0052] From the viewpoint of achieving both heat resistance and folding resistance, the content of the amorphous polyester (B) is preferably 1 part by mass or more and 50 parts by mass or less, more preferably 3 parts by mass or more and 48 parts by mass or less, even more preferably 5 parts by mass or more and 46 parts by mass or less, and particularly preferably 10 parts by mass or more and 44 parts by mass or less, per 100 parts by mass of the PEN-based resin (A). When the content of the amorphous polyester (B) in the present film is 1 part by mass or more, the crystallization rate can be slowed down, and therefore the stretching processability when the film is stretched can be improved. On the other hand, when the content of the amorphous polyester (B) is 50 parts by mass or less, the crystallinity of the film is maintained, and the heat resistance of the obtained film is sufficient.
[0053] In the present invention, the present film can be allowed to contain other resins than the PEN resin (A) and the amorphous polyester (B) as long as the effects of the present invention are not impaired. Examples of the other resins include polystyrene-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, chlorinated polyethylene-based resins, polyester-based resins other than the above (A) and (B), polycarbonate-based resins, polyamide-based resins, polyacetal-based resins, acrylic-based resins, ethylene-vinyl acetate copolymers, polymethylpentene-based resins, polyvinyl alcohol-based resins, cyclic olefin-based resins, polylactic acid-based resins, polybutylene succinate-based resins, polyacrylonitrile-based resins, polyethylene oxide-based resins, cellulose-based resins, polyimide-based resins, polyurethane-based resins, polyphenylene sulfide-based resins, polyphenylene ether-based resins, polyvinyl acetal-based resins, polybutadiene-based resins, polybutene-based resins, polyamideimide-based resins, polyamide bismaleimide-based resins, polyetherimide-based resins, polyetheretherketone-based resins, polyetherketone-based resins, polyethersulfone-based resins, polyketone-based resins, polysulfone-based resins, aramid-based resins, and fluorine-based resins.
[0054] Among these, polycarbonate-based resins are preferred. The melt moldability of the PAR is improved by mixing the polycarbonate-based resin. That is, since PAR and polycarbonate are compatible with each other, the glass transition temperature of the PAR can be lowered while maintaining the transparency and mechanical properties by mixing the PAR with polycarbonate, and as a result, the melt moldability can be improved. When PAR and polycarbonate are mixed, the mixing ratio (mass ratio) of PAR / polycarbonate is preferably 99 / 1 to 50 / 50, more preferably 98 / 2 to 60 / 40, further preferably 97 / 3 to 70 / 30, and particularly preferably 96 / 4 to 80 / 20. When the mixing ratio of PAR and polycarbonate is within this range, the melt moldability can be improved while maintaining the heat resistance of PAR.
[0055] The present film may contain particles for the main purpose of imparting easy slippage and preventing scratches during each process. The type of particles to be added is not particularly limited as long as it is a particle capable of imparting easy slippage, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenolic resin, epoxy resin, and benzoguanamine resin. Furthermore, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the production process of a polymer such as polyester can also be used.
[0056] The film may also contain additives that are generally used as appropriate, such as recycled resins resulting from trimming losses such as edges, pigments such as titanium oxide and carbon black, flame retardants, weathering stabilizers, heat stabilizers, antistatic agents, melt viscosity improvers, crosslinking agents, lubricants, nucleating agents, plasticizers, antioxidants, antioxidants, light stabilizers, ultraviolet absorbers, neutralizing agents, antifogging agents, antiblocking agents, slip agents, and colorants, which are added for the purpose of improving and adjusting moldability, productivity, and various physical properties of the porous film.
[0057] 3. Manufacturing method Next, a method for producing the present film will be described.
[0058] A method for producing the biaxially stretched film of the present invention will be described below. However, the following description is one example of the method for producing the present film, and the present film is not limited to films produced by this production method.
[0059] The method for producing the film according to one embodiment of the present invention comprises forming a resin composition containing the PEN resin (A) and the amorphous polyester (B) into a film and biaxially stretching the film.
[0060] The method of kneading the PEN resin (A), the amorphous polyester (B), other resins, and additives to obtain a resin composition is not particularly limited, but in order to obtain the resin composition as simply as possible, it is preferable to produce it by melt kneading using an extruder. In order to uniformly mix the raw materials constituting the resin composition, it is preferable to melt knead using a co-rotating twin screw extruder. The kneading temperature must be equal to or higher than the glass transition temperature (Tg) of all polymers used, and for crystalline resins, equal to or higher than the crystalline melting temperature (Tm) of the polymer. The higher the kneading temperature is, the easier it is for a part of the polymer to undergo an ester exchange reaction and the compatibility is improved, but if the kneading temperature is higher than necessary, the resin will decompose, which is not preferable. For this reason, the kneading temperature is preferably 255°C or higher and 340°C or lower, more preferably 260°C or higher and 330°C or lower, even more preferably 270°C or higher and 320°C or lower, and particularly preferably 280°C or higher and 310°C or lower. If the kneading temperature is within this range, the compatibility and melt moldability can be improved without causing decomposition of the polymer.
[0061] The obtained resin composition can be molded into a biaxially stretched film by a general molding method such as extrusion molding, injection molding, blow molding, vacuum molding, pressure molding, press molding, etc. In each molding method, the apparatus and processing conditions are not particularly limited. The present film is preferably produced, for example, by the following method.
[0062] From the resin composition obtained by mixing, a substantially amorphous and unoriented film (hereinafter, sometimes referred to as "unstretched film") is produced by an extrusion method. For the production of this unstretched film, for example, an extrusion method can be adopted in which the above-mentioned raw materials are melted by an extruder, extruded from a flat die or annular die, and then quenched to form a flat or annular unstretched film. In this case, a laminated structure using multiple extruders may be used in some cases.
[0063] Next, the unstretched film is stretched in the longitudinal direction (MD) of the film and in the transverse direction (TD) perpendicular to the MD, usually by 1.1 to 6.0 times in at least one direction, preferably by 1.1 to 6.0 times in each of the longitudinal and transverse directions, in terms of the stretching effect, film strength, etc.
[0064] As the method of biaxial stretching, any of the conventionally known stretching methods such as tenter-type sequential biaxial stretching, tenter-type simultaneous biaxial stretching, and tubular-type simultaneous biaxial stretching can be used. For example, in the case of the tenter-type sequential biaxial stretching method, the unstretched film is heated to a temperature range of Tg to Tg+50°C, where Tg is the glass transition temperature of the resin composition, and stretched in the longitudinal direction by 1.1 to 6.0 times using a roll-type longitudinal stretching machine, and then stretched in the transverse direction by 1.1 to 6.0 times within a temperature range of Tg to Tg+50°C using a tenter-type transverse stretching machine. In addition, in the case of the tenter-type simultaneous biaxial stretching method or the tubular-type simultaneous biaxial stretching method, for example, the film can be produced by simultaneously stretching in the longitudinal and transverse directions by 1.1 to 6.0 times in the temperature range of Tg to Tg+50°C.
[0065] The biaxially stretched film stretched by the above method is subsequently heat-set. By heat-setting, dimensional stability at room temperature can be imparted. In this case, the treatment temperature is preferably selected in the range of the crystalline melting temperature Tm-1 to Tm-120°C of the resin composition. If the heat-setting temperature is within the above range, heat-setting is sufficiently performed, stress during stretching is alleviated, sufficient heat resistance and mechanical properties are obtained, and an excellent film without problems such as breakage or whitening of the film surface can be obtained.
[0066] In the present invention, in order to relieve the stress of crystallization shrinkage due to heat setting, it is preferable to perform relaxation in the width direction during heat setting by 0 to 15%, preferably 1 to 10%. Since the relaxation is performed sufficiently and the film is relaxed uniformly in the width direction, the shrinkage rate in the width direction becomes uniform, and a film with excellent dimensional stability at room temperature is obtained. In addition, since the relaxation is performed in accordance with the shrinkage of the film, there is no sagging of the film, no fluttering in the tenter, and no breakage of the film.
[0067] [Uses of this film] The biaxially stretched film of the present invention has excellent heat resistance and folding resistance, and can be used as an optical film, a packaging film, various protective films, and the like. Among them, from the viewpoint of folding resistance, it is preferably used for flexible displays. Specifically, it is preferably used as a display component such as a front panel, a base film for a touch sensor, or a lower protective film, and is particularly preferably used as a lower protective film. The lower protective film is a film that protects the back side of a display device. In addition, the display is particularly preferably a foldable display. The display may be used in a mobile phone, a smartphone, a digital camera, a personal computer, etc. The type of display is not particularly limited, and may be any of a liquid crystal display, a plasma display, an organic electroluminescence display, etc., or may be a touch panel type display. As the display, an organic electroluminescence display is preferable.
[0068] [Laminated film] The laminated film of the present invention comprises the biaxially stretched film and an adhesive layer on at least one surface of the biaxially stretched film. The laminate is preferably used as a component of the display and laminated with another member via the adhesive layer.Furthermore, it is preferable to form a flexible display having a configuration in which another member is bonded to the laminate via the adhesive layer.
[0069] <Adhesive layer> The adhesive for forming the adhesive layer may be an acrylic adhesive, a urethane adhesive, a synthetic rubber adhesive, a natural rubber adhesive, a silicone adhesive, a polyester adhesive, a vinyl alkyl ether adhesive, an epoxy adhesive, etc., and among these, an acrylic adhesive, a urethane adhesive, and a silicone adhesive are preferred. As long as the optical properties are not affected, two or more types of materials may be mixed and used, or two or more layers may be used. The pressure-sensitive adhesive may be of any of an emulsion type, a solvent type, or a solventless type, and may be of any of a crosslinked type or a non-crosslinked type. Furthermore, particles such as fillers and additives can also be added.
[0070] The (meth)acrylic resin (base polymer) constituting the acrylic pressure-sensitive adhesive preferably includes, for example, a polymer or copolymer having one or more types of (meth)acrylic acid esters as monomers, such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate. It is preferable to copolymerize a polar monomer into the base polymer. Examples of the polar monomer include monomers having a carboxyl group, a hydroxyl group, an amide group, an amino group, an epoxy group, etc., such as (meth)acrylic acid, 2-hydroxypropyl (meth)acrylate, hydroxyethyl (meth)acrylate, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, and glycidyl (meth)acrylate.
[0071] The pressure-sensitive adhesive composition may contain only the base polymer, but usually contains a crosslinking agent. Examples of the crosslinking agent include divalent or higher metal ions, polyamine compounds, polyepoxy compounds, and polyisocyanate compounds, among which polyisocyanate compounds are preferred.
[0072] The urethane-based adhesive is preferably made of a urethane-based polymer, which is an adhesive polymer obtained by reacting a polyol with a polyisocyanate compound. Examples of the polyol include polyether polyol, polyester polyol, polycarbonate polyol, and polycaprolactone polyol. Examples of the polyisocyanate compound include diphenylmethane diisocyanate, tolylene diisocyanate, and hexamethylene diisocyanate.
[0073] As the silicone-based adhesive, preferably, an adhesive obtained by blending or agglomerating a silicone-based polymer, which is an adhesive polymer, can be used. Examples of the silicone-based adhesive include addition reaction curing type silicone-based adhesives and peroxide curing type silicone-based adhesives. The addition reaction curing type silicone-based adhesive is preferred because it does not use peroxide and does not generate decomposition products. The curing reaction of the addition reaction curing type silicone adhesive can be, for example, a reaction in which a polyalkyl hydrogen siloxane composition used to obtain a polyalkyl silicone adhesive is cured with a platinum catalyst.
[0074] The adhesive layer can be formed by applying the above-mentioned adhesive to a polyester film. Alternatively, the adhesive may be applied to a release sheet, and the adhesive layer formed on another substrate such as a release sheet may be transferred to the polyester film to form the adhesive layer on the polyester film. The adhesive can be applied by any method, including a comma coater, knife coater, die coater, gravure coater, and Meyer bar coater, without any particular limitation, and can be appropriately selected depending on the viscosity and film thickness.
[0075] The method for curing the adhesive layer can be appropriately selected from methods using energy rays such as ultraviolet rays and electron beams, and heat.
[0076] <Coating layer> In the laminated film of the present invention, a coating layer can be provided between the adhesive layer and the biaxially stretched film. The presence of the coating layer imparts various functions to the laminated film. Functions of the coating layer include hard coat properties, antistatic properties, peelability, easy adhesion, printability, UV protection properties, infrared blocking properties, gas barrier properties, etc. The coating layer may be formed by in-line coating, which treats the film surface during the stretching process, or by off-line coating, which applies the coating outside the system onto a film that has already been produced, or both may be used in combination.
[0077] [Flexible display] The flexible display of the present invention comprises the biaxially stretched film or laminated film described above. The biaxially stretched film and laminated film of the present invention have excellent heat resistance and folding resistance. Therefore, the flexible display of the present invention also has excellent heat resistance and folding resistance, and has high performance as a foldable display device, a bendable display device, a rollable display device, or a stretchable display device. EXAMPLES
[0078] The following examples are given, but the present invention is not limited to these in any way.
[0079] [Evaluation method] (1) Hysteresis loss rate In accordance with JIS K 7312:1996, the average hysteresis loss rate at 23°C was determined by the following method. The measuring device used was a tensile tester (Shimadzu Corporation tensile tester AG-1kNXplus). The test specimen was a rectangle cut from the film with a length of 100 mm in the measurement direction and a width of 10 mm. The test specimen was chucked at both ends in the length direction with a chuck distance of 50 mm, raised to a strain of 5% at a crosshead speed of 0.5 mm / min, and then lowered to the initial position at the same speed to obtain a stress-strain curve from one cycle of tensile cycle testing. The stress-strain curve had a profile as shown in Figure 1, and the hysteresis loss rate was calculated from the obtained stress-strain curve using the area A1 (abcda) of the curve obtained during the upward movement and the area A2 (abcef) which is the difference between the area A1 and the area of the curve obtained during the downward movement, using the following formula 1. The test was performed three times, and the average value was calculated. The above tensile cycle test was performed in the longitudinal direction (MD) and the transverse direction (TD) of the film, respectively, and the average value was calculated. Hysteresis loss rate = (A2 / A1) x 100 (Formula 1)
[0080] (2) Residual strain In accordance with JIS K 7312:1996, the average value of residual strain at 23°C was determined by the following method. The measuring device used was a tensile testing machine (AG-1kNXplus tensile testing machine manufactured by Shimadzu Corporation). As the test piece, a rectangle with a length of 100 mm and a width of 10 mm in the measuring direction was cut out from this film. Both ends of the test piece in the length direction were chucked with a chuck distance of 50 mm, and after raising the strain to 5% at a crosshead speed of 0.5 mm / min, the strain at the point where the stress disappeared was taken as the residual strain from the stress-strain curve obtained from one cycle of tensile cycle test in which it was lowered to the initial position at the same speed. The test was measured three times and the average value was obtained. The above tensile cycle test was carried out in the longitudinal direction (MD) and the width direction (TD) of the film respectively, and the average value was obtained.
[0081] (3) Glass transition temperature For the obtained film, using Diamond DSC (manufactured by PerkinElmer Japan), in accordance with JIS K7121 (2012), after raising the temperature to the melting temperature once at a heating rate of 10 °C / min, the temperature was then lowered at a heating rate of 10 °C / min, and the glass transition temperature in the heating process at a heating rate of 10 °C / min was measured.
[0082] (4) Crystal melting temperature For the obtained film, using Diamond DSC (manufactured by PerkinElmer Japan), in accordance with JIS K7121 (2012), the crystal melting temperature in the heating process at a heating rate of 10 °C / min was measured.
[0083] [Materials used] <PEN-based resin (A)> As PEN-based resin (A)-1, dicarboxylic acid component (a-1): 2,6-naphthalenedicarboxylic acid = 100 mol%, diol component (a-2): ethylene glycol = 90 mol%, bisphenol A-ethylene oxide adduct = 10 mol% was used. The Tg of the PEN-based resin (A)-1 was 116 °C. As PEN-based resin (A)-2, dicarboxylic acid component (a-1): 2,6-naphthalenedicarboxylic acid = 100 mol%, diol component (a-2): ethylene glycol = 100 mol%, and the Tg of the PEN-based resin (A)-2 was 119 °C.
[0084] <Amorphous polyester (B)> As the amorphous polyester (B), PAR was used, in which the carboxylic acid component was terephthalic acid / isophthalic acid (molar ratio)=50 / 50, and the bisphenol component was 100 mol % of bisphenol A. The Tg of the amorphous polyester (B) was 193° C.
[0085] [PET film (C)] As the PET film (C), a biaxially stretched PET film having a thickness of 50 μm was used.
[0086] Example 1 Pellet-form (B) was added at a ratio of 10% by mass to 90% by mass of pellet-form (A)-1 (11 parts by mass of (B) per 100 parts by mass of (A)-1), dry-blended, and then melt-kneaded in a Φ40 mm twin-screw extruder set at 290°C. The mixture was extruded as a film from a T-die with a gap of 1.0 mm, taken up by a cast roll at 120°C, and cooled and solidified to obtain a film-like material with a thickness of approximately 460 μm. The obtained cast film was then passed through a longitudinal stretching machine, heated by an IR heater (temperature near the IR heater was about 181°C), and stretched 2.8 times in the machine direction (MD). The obtained longitudinally stretched film was then passed through a transverse stretching machine (tenter) and stretched 3.7 times in the width direction (TD) at a preheat temperature of 120°C, a stretching temperature of 127°C, and a heat setting temperature of 190°C, after which the film was relaxed by 3% in the tenter. The results of measurements of the obtained film are shown in Table 1.
[0087] Example 2 Pellet-form (B) was added in a ratio of 20% by mass to 80% by mass of pellet-form (A)-1 (25 parts by mass of (B) per 100 parts by mass of (A)-1), and then dry-blended. A film-like material having a thickness of approximately 460 μm was obtained in the same manner as in Example 1. The obtained cast film was then passed through a longitudinal stretching machine, heated by an IR heater (temperature near the IR heater was about 190°C), and stretched 2.8 times in the machine direction (MD). The obtained longitudinally stretched film was then passed through a transverse stretching machine (tenter) and stretched 3.7 times in the width direction (TD) at a preheating temperature of 130°C, a stretching temperature of 135°C, and a heat setting temperature of 190°C, after which the film was relaxed by 3% in the tenter. The results of measurements of the obtained film are shown in Table 1.
[0088] Example 3 A film-like material having a thickness of approximately 460 μm was obtained in the same manner as in Example 1, except that pellet-like (B) was added in a ratio of 10 mass% to 90 mass% of pellet-like (A)-2 (11 mass parts of (B) per 100 mass parts of (A)-2), dry blended, and then the temperature of the cast roll was set to 121° C. The obtained cast film was then passed through a longitudinal stretching machine, heated by an IR heater (temperature near the IR heater was about 197°C), and stretched 2.8 times in the machine direction (MD). The obtained longitudinally stretched film was then passed through a transverse stretching machine (tenter) and stretched 3.6 times in the width direction (TD) at a preheating temperature of 130°C, a stretching temperature of 135°C, and a heat setting temperature of 205°C, after which the film was relaxed by 3% in the tenter. The results of measurements of the obtained film are shown in Table 1.
[0089] Example 4 A film-like material having a thickness of approximately 460 μm was obtained in the same manner as in Example 1, except that pellet-like (B) was added in a ratio of 20 mass% to pellet-like (A)-2 (25 mass parts of (B) per 100 mass parts of (A)-1), dry blended, and then the temperature of the cast roll was set to 125° C. The obtained cast film was then passed through a longitudinal stretching machine, heated by an IR heater (temperature near the IR heater was about 207°C), and stretched 2.6 times in the machine direction (MD). The obtained longitudinally stretched film was then passed through a transverse stretching machine (tenter) and stretched 3.7 times in the width direction (TD) at a preheating temperature of 135°C, a stretching temperature of 140°C, and a heat setting temperature of 205°C, after which the film was relaxed by 3% in the tenter. The results of measurements of the obtained film are shown in Table 1.
[0090] Comparative Example 1 The biaxially stretched PET film (C) was evaluated, and the results are shown in Table 1.
[0091] Comparative Example 2 Pelletized (A)-2 was extruded using a Φ44 mm twin-screw extruder (set to 300°C) and rapidly cooled and solidified on a cooling roll with a surface temperature set to 50°C using an electrostatic adhesion method to obtain a cast film. The obtained cast film was then passed through a longitudinal stretching machine and stretched 3.0 times in the machine direction (MD) at a stretching temperature of 133° C. The obtained longitudinally stretched film was then passed through a transverse stretching machine (tenter) and stretched 3.7 times in the width direction (TD) at a preheating temperature of 115° C., a stretching temperature of 130° C., and a heat setting temperature of 210° C., after which the film was relaxed by 1.5% in the tenter. The results of measurements of the obtained film are shown in Table 1.
[0092] Comparative Example 3 A film-like material having a thickness of about 460 μm was obtained in the same manner as in Example 1, except that pellet-shaped (A)-1 was used, the cast roll was set at 110° C., and the extruder temperature was set at 285° C. The obtained cast film was then passed through a longitudinal stretching machine, heated by an IR heater (temperature near the IR heater was about 160°C), and stretched 2.8 times in the machine direction (MD). The obtained longitudinally stretched film was then passed through a transverse stretching machine (tenter) and stretched 4.1 times in the width direction (TD) at a preheating temperature of 125°C, a stretching temperature of 130°C, and a heat setting temperature of 170°C, after which the film was relaxed by 3% in the tenter. The results of measurements of the obtained film are shown in Table 1.
[0093] [Table 1]
[0094] As shown in the above examples, the films of Examples 1 to 4 have high glass transition temperatures (Tg) and crystalline melting temperatures (Tm), and are excellent in heat resistance. Moreover, the films of Examples 1 to 4 have clearly lower hysteresis loss rates and residual strain values than those of Comparative Examples 1 to 3, and can be said to have greater recovery and superior folding resistance. [Industrial Applicability]
[0095] The biaxially stretched film and laminated film of the present invention have excellent heat resistance and folding resistance, and therefore can be suitably used as an optical film, particularly for flexible displays. Therefore, the embodiments of the present disclosure are useful for flexible displays, such as foldable displays, bendable displays, rollable displays, and stretchable displays, that utilize the advantages of flexible display panels that can be folded, bent, or rolled.
Claims
1. The polyethylene naphthalate resin (A) and the amorphous polyester (B) having a glass transition temperature higher than that of the polyethylene naphthalate resin (A), The average hysteresis loss rate when a tensile cycle test was performed up to 5% tensile strain in each of the machine direction (MD) and the transverse direction (TD) is 46.0% or less; the polyethylene naphthalate resin (A) is a copolymer containing a dicarboxylic acid component (a-1) and a diol component (a-2); The component (a-1) contains a 2,6-naphthalenedicarboxylic acid unit, A biaxially stretched film comprising ethylene glycol units and bisphenol A-ethylene oxide adduct units as the component (a-2).
2. A polyethylene naphthalate resin (A) and an amorphous polyester (B) having a glass transition temperature higher than that of the polyethylene naphthalate resin (A), The average hysteresis loss rate when a tensile cycle test was performed up to 5% tensile strain in each of the machine direction (MD) and the transverse direction (TD) is 46.0% or less; the polyethylene naphthalate resin (A) is a copolymer containing a dicarboxylic acid component (a-1) and a diol component (a-2); The component (a-1) contains a 2,6-naphthalenedicarboxylic acid unit, A biaxially stretched film for flexible displays, comprising ethylene glycol units and bisphenol A-ethylene oxide adduct units as the component (a-2).
3. A polyethylene naphthalate resin (A) and an amorphous polyester (B) having a glass transition temperature higher than that of the polyethylene naphthalate resin (A), The average hysteresis loss rate when a tensile cycle test was performed up to 5% tensile strain in each of the machine direction (MD) and the transverse direction (TD) is 46.0% or less; the polyethylene naphthalate resin (A) is a copolymer containing a dicarboxylic acid component (a-1) and a diol component (a-2); The component (a-1) contains a 2,6-naphthalenedicarboxylic acid unit, The (a-2) component contains ethylene glycol units and bisphenol A-ethylene oxide adduct units, A biaxially stretched film, wherein the content of the amorphous polyester (B) is 1 part by mass or more and 50 parts by mass or less per 100 parts by mass of the polyethylene naphthalate-based resin (A).
4. The biaxially stretched film according to any one of claims 1 to 3, wherein the component (a-2) contains 4 mol% or more and 50 mol% or less of the bisphenol A-ethylene oxide adduct unit and 50 mol% or more and 96 mol% or less of ethylene glycol unit.
5. The biaxially stretched film according to any one of claims 1 to 4, wherein the amorphous polyester (B) is a polyarylate.
6. A biaxially stretched film described in any one of claims 1, 2, 4 and 5, wherein the content of the amorphous polyester (B) is 1 part by mass or more and 50 parts by mass or less per 100 parts by mass of the polyethylene naphthalate resin (A).
7. The biaxially stretched film according to any one of claims 1 to 6, wherein the average residual strain when subjected to a tensile cycle test up to 5% tensile strain in each of the machine direction (MD) and the transverse direction (TD) is 0.900% or less.
8. The biaxially stretched film according to any one of claims 1 to 7, having a glass transition temperature of 75°C or more and 150°C or less.
9. The biaxially stretched film according to any one of claims 1 to 8, having a crystalline melting temperature of 220°C or more and 300°C or less.
10. The biaxially stretched film according to any one of claims 1 to 9, having a thickness of 1 µm or more and 250 µm or less.
11. The biaxially stretched film according to any one of claims 1 and 3 to 10, which is for a flexible display.
12. A laminated film comprising the biaxially stretched film according to any one of claims 1 to 11 and an adhesive layer provided on at least one surface of the biaxially stretched film.
13. The laminated film according to claim 12 , further comprising a coating layer between the biaxially oriented film and the adhesive layer.
14. A flexible display comprising the biaxially stretched film according to any one of claims 1 to 11 or the laminate film according to claim 12 or 13.
Citation Information
Patent Citations
Silver halide photographic sensitive material
JP1994332108A
Polyethylene naphthalate resin
JP1996048759A
Polyethylene naphthalate copolymer and its production
JP1998204165A
Modified polyester resin and molded product composed of the same resin
JP2004107559A
Biaxial oriented film for electric insulation
JP2013131323A