Polyester film, laminated polyester film, method for producing polyester film, method for producing laminated polyester film, and method for producing biaxially oriented polyester film
By integrating a polyvinyl alcohol skeleton into the inner layer of polyester films and optimizing manufacturing conditions, the film's transportability and productivity are enhanced, facilitating efficient recovery and reuse.
Patent Information
- Application Number
- JP2021031362
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-03-01
AI Technical Summary
Existing polyester films face issues with transportability and productivity due to tearing during the manufacturing process, which hinders efficient recovery and reuse.
Incorporating a polyvinyl alcohol skeleton into the inner layer of the polyester film, enhancing the interaction between the polyester molecular chains through hydroxyl groups, and using specific manufacturing conditions to improve transportability and reduce tearing during biaxial stretching.
The film exhibits improved transportability and reduced tearing, leading to enhanced productivity and ease of recovery for recycling.
Smart Images

Figure 0007585879000001 
Figure 0007585879000002 
Figure 0007585879000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester film, a laminated polyester film, a method for producing a polyester film, a method for producing a laminated polyester film, and a method for producing a biaxially oriented polyester film. [Background technology]
[0002] While plastics are used in various fields, they are also considered to be a cause of marine pollution such as microplastics, and there is an urgent need to reduce the environmental burden caused by plastics. In addition, in recent years, with the evolution of IoT (Internet of Things), electronic devices such as CPUs and liquid crystal displays mounted on computers and smartphones have rapidly increased, and accordingly, the number of multilayer ceramic capacitors (MLCCs), which are important for driving electronic devices, and polarizing films used in liquid crystal display devices have also explosively increased. A large amount of process film is used to manufacture MLCCs and these films, but the process film after use is generally discarded. In other words, the burden on the environment due to the increase in discarded process films is becoming an issue. In response to this issue, technologies for reusing used process films have been disclosed (Patent Documents 1, 2, and 3). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2012-171276 A [Patent Document 2] Patent No. 4284936 [Patent Document 3] JP 2019-066841 A Summary of the Invention [Problem to be solved by the invention]
[0004] Both films undergo a process of transporting the film in order to recover the polyester film used as the process film. However, in the production process of the polyester film, there is room for further improvement in transportability, that is, in terms of the decrease in productivity and decrease in recoverability due to breakage of the film during the production process.
[0005] Therefore, an object of the present invention is to provide a polyester film, a laminated polyester film, a method for producing a polyester film, a method for producing a laminated polyester film, and a method for producing a biaxially oriented polyester film, which are excellent in transportability. [Means for solving the problem]
[0006] A preferred embodiment of the present invention has the following configuration. [I] When the following measurements were performed using Measurement Method A and Measurement Method B, the wave number was 3300 cm -1 From 3400cm -1 A peak is detected at and the peak intensity is 1.0×10 -3 The polyester film is as described above. (Measurement method A) A method of measuring using a microscopic infrared spectrometer. Equipment: Microscopic infrared spectroscopic analyzer; LUMOS (manufactured by Bruker) Measurement conditions: Light source: Silicon carbide rod heating element (glow bar) Detector: Narrow MCT (HgCdTe) Detection range: 4000~650cm -1 Purge; Nitrogen gas Measurement mode: Transmission method Resolution; 8cm -1 Number of times accumulated: 256 A spectrum is obtained by plotting the absorption intensity against each wave number.
[0007] In the cross section of the polyester film, measurements are taken in a direction perpendicular to the outermost surface of the polyester film, and 10 points are measured evenly in the thickness direction at a depth of 5 μm or more (hereinafter referred to as the inner layer portion) using the above-mentioned device and conditions to obtain a spectrum. The spectrum is then divided by the spectrum of PET (a PET spectrum (measured under the same conditions using #50T60 manufactured by Toray Industries, Inc.) to obtain a spectrum at 1000 cm -1 ~1500cm -1 The spectrum is obtained by dividing the spectrum obtained by measurement by the four basic arithmetic operations so that the peak shapes of the two spectra match as closely as possible.
[0008] Here, at least one of the 10 measurement points was measured, and the divided spectrum was measured at a wave number of 3300 cm -1 From 3400cm -1 If a peak is detected at a wavenumber of 3,300 cm when measured using measurement method A, -1 From 3400cm -1 In addition, at least one of the 10 measurement points has a peak intensity of 1.0×10 -3 If the peak intensity is 1.0×10 or more when measured by measurement method A, -3 Let's say that this is all.
[0009] In addition, for the above-mentioned divided spectrum at a certain measurement point, -1 From 3400cm -1 If two or more peaks are observed, the maximum peak intensity is 1.0×10 -3 or more, the peak intensity detected in the divided spectrum at that measurement point is 1.0×10 -3 Let's say that this is all. (Measurement method B) A method of measuring using an infrared spectrometer. Apparatus: Infrared spectrometer; "Nicolet" (registered trademark) 6700 (manufactured by Thermofisher Scientific) Measurement conditions: Light source: Silicon carbide rod heating element (glow bar) Detector: DTGS (triglycine sulfate) Detection range: 4000~680cm -1 Purge; Nitrogen gas Measurement mode: ATR method (attenuated total reflection measurement method) Single-reflection ATR measurement accessory device (OMNI sampler), ATR crystal: Ge, incident angle: 45° Resolution; 4cm -1 Number of times accumulated: 256 A spectrum is obtained by plotting the absorption intensity against each wave number.
[0010] First, for each of 50 pieces of 4 cm square polyester film, 5 μm is scraped off from one surface of the polyester film using a microtome while observing under a microscope, and then 5 μm is scraped off from the surface of the opposite surface in the same manner to obtain the inner layer of the polyester film.
[0011] The obtained inner layer portion is immersed in hexafluoro-2-propanol (HFIP) and dissolved for 30 minutes under nitrogen atmosphere with stirring at 50° C. The liquid is then cooled to 25° C., and insoluble matter is collected with a PTFE filter (manufactured by ADVANTEC, model number: 13010802). The collected matter is measured with the above-mentioned device and conditions to obtain a spectrum.
[0012] Here, for the spectrum obtained, the wave number is 3300 cm -1 From 3400cm -1 If a peak is detected at a wavenumber of 3,300 cm when measured using measurement method B, -1 From 3400cm -1 In addition, for the spectrum obtained, a peak is detected at a peak intensity of 1.0×10 -3 If the peak intensity is 1.0×10 or more when measured by measurement method B, -3 Let's say that this is all.
[0013] In addition, the spectrum obtained above has a wave number of 3300 cm -1 From 3400cm -1 If two or more peaks are observed, the maximum peak intensity is 1.0×10 -3 or more, the peak intensity detected in the obtained spectrum is 1.0×10 -3 Let's say that this is all. [II] In the measurement method B, the wave number is 3300 cm -1 From 3400cm -1 A peak is detected at and the peak intensity is 1.0×10 -3 The polyester film according to [I], wherein an organic component insoluble in HFIP is contained in an inner layer portion of the polyester film in an amount of 10 ppm to 1000 ppm by mass. [III] In the measurement method B, the wave number is 3300 cm -1 From 3400cm -1 A peak is detected at and the peak intensity is 1.0×10 -3 The polyester film according to [I] or [II], wherein the HFIP-insoluble organic component has a polyethylene terephthalate skeleton. [IV] The polyester film according to any one of [I] to [III], wherein the outermost layer of the polyester film contains a component having a polyvinyl alcohol skeleton. [V] A laminated polyester film having a layer X mainly composed of a resin having a polyvinyl alcohol skeleton on at least one surface of the polyester film according to any one of [I] to [IV]. [VI] The laminated polyester film according to [V], which has the polyester film, the layer X, and a release layer Y in this order. [VII] The laminated polyester film according to [VI], which has the polyester film, the layer X, the release layer Y, and the functional layer Z in this order. [VIII] and [VII], a method for producing a laminated polyester film, comprising a step of peeling off the functional layer Z from the laminated polyester film. [IX] and [VI], a method for producing a polyester film, comprising a step of simultaneously removing layer X and release layer Y from the laminated polyester film. [X] [VII] A method for producing a polyester film, comprising the steps of peeling off a functional layer Z from the laminated polyester film and simultaneously removing a layer X and a release layer Y, in this order. A method for producing a polyester film, comprising laminating a release layer Y on layer X of the laminated polyester film described in [XI][V], providing a functional layer Z on the release layer Y, peeling off the functional layer Z, and then removing layer X and the release layer Y. [XII] [A method for producing a polyester film, comprising a step of molding a polyester film using a composition obtained by melting a polyester film obtained by removing a part of layer X from the laminated polyester film according to any one of [V] to [VII]. [XIII] A method for producing a biaxially oriented polyester film, comprising the steps of melting a polyester and a component having a polyvinyl alcohol skeleton and forming the polyester into a film. Effect of the Invention
[0014] According to the present invention, it is possible to provide a polyester film, a laminated polyester film, a method for producing a polyester film, a method for producing a laminated polyester film, and a method for producing a biaxially oriented polyester film, all of which are excellent in transportability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention will be described in detail below with reference to specific examples.
[0016] The present invention relates to a polyester film. The polyester in the present invention is composed of a dicarboxylic acid component and a diol component. In this specification, the term "component" refers to the smallest unit obtainable by hydrolysis of a polyester. Examples of the dicarboxylic acid component constituting such a polyester include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid, or ester derivatives thereof.
[0017] Examples of diol components constituting such polyesters include aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,2-butanediol, and 1,3-butanediol, alicyclic diols such as cyclohexanedimethanol and spiroglycol, and a combination of a plurality of the above-mentioned diols. Among these, from the viewpoint of mechanical properties and transparency, polyesters in which polyethylene terephthalate (PET), polyethylene-2,6-naphthalenedicarboxylate (PEN), and a portion of the dicarboxylic acid component of PET is copolymerized with isophthalic acid or naphthalenedicarboxylic acid, and a portion of the diol component of PET is copolymerized with cyclohexanedimethanol, spiroglycol, or diethylene glycol are preferably used.
[0018] From the viewpoint of mechanical strength and chemical resistance, the polyester of the present invention is preferably composed mainly of polyethylene terephthalate (PET) consisting of terephthalic acid and ethylene glycol. The term "main component" means that polyethylene terephthalate accounts for 90 mol % or more of 100 mol % of polyester constituents.
[0019] A preferred embodiment of the polyester film of the present invention is a film having a wavelength of 3,300 cm when measured by the following measurement method A and measurement method B. -1From 3400cm -1 A peak is detected at and the peak intensity is 1.0×10 -3 The polyester film is as described above. (Measurement method A) A method of measuring using a microscopic infrared spectrometer. Equipment: Microscopic infrared spectroscopic analyzer; LUMOS (manufactured by Bruker) Measurement conditions: Light source: Silicon carbide rod heating element (glow bar) Detector: Narrow MCT (HgCdTe) Detection range: 4000~650cm -1 Purge; Nitrogen gas Measurement mode: Transmission method Resolution; 8cm -1 Number of times accumulated: 256 A spectrum is obtained by plotting the absorption intensity against each wave number.
[0020] In the cross section of the polyester film, measurements are taken in a direction perpendicular to the outermost surface of the polyester film, and 10 points are measured evenly in the thickness direction at a depth of 5 μm or more (hereinafter referred to as the inner layer portion) using the above-mentioned device and conditions to obtain a spectrum. The spectrum is then divided by the spectrum of PET (a PET spectrum (measured under the same conditions using #50T60 manufactured by Toray Industries, Inc.) to obtain a spectrum at 1000 cm -1 ~1500cm -1 The spectrum is obtained by dividing the spectrum obtained by measurement by the four basic arithmetic operations so that the peak shapes of the two spectra match as closely as possible.
[0021] Here, at least one of the 10 measurement points was measured, and the divided spectrum was measured at a wave number of 3300 cm -1 From 3400cm -1 If a peak is detected at a wavenumber of 3,300 cm when measured using measurement method A, -1 From 3400cm -1In addition, at least one of the 10 measurement points has a peak intensity of 1.0×10 -3 If the peak intensity is 1.0×10 or more when measured by measurement method A, -3 Let's say that this is all.
[0022] In addition, for the above-mentioned divided spectrum at a certain measurement point, -1 From 3400cm -1 If two or more peaks are observed, the maximum peak intensity is 1.0×10 -3 or more, the peak intensity detected in the divided spectrum at that measurement point is 1.0×10 -3 Let's say that this is all. (Measurement method B) A method of measuring using an infrared spectrometer. Apparatus: Infrared spectrometer; "Nicolet" (registered trademark) 6700 (manufactured by Thermofisher Scientific) Measurement conditions: Light source: Silicon carbide rod heating element (glow bar) Detector: DTGS (triglycine sulfate) Detection range: 4000~680cm -1 Purge; Nitrogen gas Measurement mode: ATR method (attenuated total reflection measurement method) Single-reflection ATR measurement accessory device (OMNI sampler), ATR crystal: Ge, incident angle: 45° Resolution; 4cm -1 Number of times accumulated: 256 A spectrum is obtained by plotting the absorption intensity against each wave number.
[0023] First, for each of 50 pieces of 4 cm square polyester film, 5 μm is scraped off from one surface of the polyester film using a microtome while observing under a microscope, and then 5 μm is scraped off from the surface of the opposite surface in the same manner to obtain the inner layer of the polyester film.
[0024] The obtained inner layer portion is immersed in hexafluoro-2-propanol (HFIP) and dissolved for 30 minutes under nitrogen atmosphere with stirring at 50° C. The liquid is then cooled to 25° C., and insoluble matter is collected with a PTFE filter (manufactured by ADVANTEC, model number: 13010802). The collected matter is measured with the above-mentioned device and conditions to obtain a spectrum.
[0025] Here, for the spectrum obtained, the wave number is 3300 cm -1 From 3400cm -1 If a peak is detected at a wavenumber of 3,300 cm when measured using measurement method B, -1 From 3400cm -1 In addition, for the spectrum obtained, a peak is detected at a peak intensity of 1.0×10 -3 If the peak intensity is 1.0×10 or more when measured by measurement method B, -3 Let's say that this is all.
[0026] In addition, the spectrum obtained above has a wave number of 3300 cm -1 From 3400cm -1 If two or more peaks are observed, the maximum peak intensity is 1.0×10 -3 or more, the peak intensity detected in the obtained spectrum is 1.0×10 -3 Let's say that this is all.
[0027] If the amount of sample collected is so large that it is not possible to measure the entire amount in one measurement, measurements are made for every 0.1 mg of sample collected, and the spectrum obtained in at least one of these measurements is measured at a wavenumber of 3300 cm -1 From 3400cm -1 If a peak is detected at a wavenumber of 3,300 cm when measured using measurement method B, -1 From 3400cm -1 In addition, for the spectrum obtained in the at least one measurement, the detected peak intensity is 1.0×10 -3If the peak intensity is 1.0×10 or more when measured by measurement method B, -3 Let's say that this is all.
[0028] In addition, in the measurement method A, the wave number is 3300 cm -1 From 3400cm -1 A peak is detected at and the peak intensity is 1.0×10 -3 If the measurement method B is more than 3300 cm, it is said to meet condition A. -1 From 3400cm -1 A peak is detected at and the peak intensity is 1.0×10 -3 If the above conditions are met, then condition B is said to be met, and so on.
[0029] Wave number 3300cm -1 From 3400cm -1 Since the peaks detected in are mainly attributable to components having hydroxyl groups, when the condition A and / or condition B is met, the components interact with the polyester molecular chains, and as a result, when the film is conveyed under tension at a temperature near the glass transition point of the polyester film, for example, at a temperature of about 80°C to 150°C, or when the film is conveyed under tension in contact with a liquid (water or organic solvent) heated to that temperature, the film shrinkage and expansion are suppressed, improving conveyability. Also, by the same mechanism, film breakage is suppressed during biaxial stretching, improving productivity.
[0030] The reason for the improved transportability is presumed to be as follows. Hydroxyl groups generally have electric polarization due to differences in the electronegativity of elements. In addition, polyesters also have carboxyl groups, and therefore generally have electric polarization due to differences in the electronegativity of elements. Even between polyester molecular chains, there is interaction due to polarization caused by differences in electronegativity, but it is believed that the inclusion of a component having a hydroxyl group further strengthens the interaction between molecular chains via the component, and the effect can be obtained at the above-mentioned specific temperature and conditions.
[0031] A preferred means for achieving condition A or B is to add a component having a polyvinyl alcohol skeleton to the inner layer of the polyester film.
[0032] The component having a polyvinyl alcohol skeleton has a molecular structure represented by chemical formula (1).
[0033] [ka]
[0034] Here, a is 1 or more and b is 0 or more.
[0035] Methods for obtaining a polyester film that satisfies condition A and / or condition B include a method of melting a polyester and a component having a polyvinyl alcohol skeleton and forming a film. Specifically, when obtaining a polyester film by melt film formation, preferred methods include a method in which a component having a polyvinyl alcohol skeleton is added when melting polyester pellets as a raw material, a method in which a laminated polyester film, the surface of which has been coated with a component having a polyvinyl alcohol skeleton, is melted again to obtain a polyester film using the obtained raw material, and a method in which a film, the surface of which has been coated with a component having a polyvinyl alcohol skeleton, is mixed with polyester pellets and then melted to obtain a polyester film, but are not particularly limited thereto.
[0036] The component having the polyvinyl alcohol skeleton may be polyvinyl alcohol or a polyvinyl alcohol-based resin such as copolymerized polyvinyl alcohol. Preferred examples of copolymerized polyvinyl alcohol include vinyl alcohol-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, vinyl alcohol-(meth)acrylic acid-(meth)acrylic acid alkyl copolymer, vinyl alcohol-isoprene sulfonic acid copolymer, vinyl alcohol-vinyl pyrrolidone copolymer, and polyvinyl alcohol-based resin having a specific modified group in the side chain as shown in the chemical formula (2) described below.
[0037] From the viewpoint of heat resistance and dispersibility, the degree of polymerization of the polyvinyl alcohol-based resin is preferably 1000 or less, more preferably 500 or less. In order to efficiently obtain the above-mentioned interaction, the degree of saponification reflecting the amount of hydroxyl groups in the polyvinyl alcohol-based resin is preferably 80 or more, particularly preferably 85 or more. Among the above-mentioned methods for obtaining a polyester film that satisfies condition A and / or condition B, a method in which at least 0.001% by mass of polyvinyl alcohol having a degree of saponification of 80 or more is contained in 100% by mass of the inner layer portion can be mentioned as an example.
[0038] In addition, from the viewpoint of strengthening the interaction between the component having a polyvinyl alcohol skeleton and the polyester molecular chain and further improving the transportability of the film, it is more preferable to use a polyvinyl alcohol-based resin having a specific modifying group in the side chain of polyvinyl alcohol, as shown in chemical formula (2).
[0039] [ka]
[0040] Here, Q is at least one selected from the group consisting of 1,2-ethanediol group, acetoacetyl group, sulfonic acid group, sulfonate group, carboxyl group, carboxyl group, amino group, and ammonium group, c and e are 1 or more, and d is 0 or more.
[0041] This embodiment is preferable because a component having a polyvinyl alcohol skeleton and a polyester molecular chain are chemically bonded during melt extrusion, and transportability is improved. The mechanism is assumed to be as follows. It is considered that the action of highly polar carboxylate, sulfonate, ammonium base, etc. causes depolymerization of the ester bonds in the polyester molecular chain, resulting in acid and alcohol ends of the polyester, which in turn causes polycondensation of the acid ends of the polyester and the hydroxyl groups of the polyvinyl alcohol, resulting in chemical bonds.
[0042] From the viewpoint of manufacturability, when the total amount of hydroxyl groups, acetoxy groups, and functional group Q in the polyvinyl alcohol resin is taken as 100 mol %, the content of functional group Q is preferably 1 mol % or more and 10 mol % or less.
[0043] In order to efficiently disperse the component having a polyvinyl alcohol skeleton in the polyester film, the shear rate in the melting step is preferably 10 sec -1 More than 250sec -1 Less than 25 seconds, preferably -1 Over 180sec -1 From the viewpoint of generating chemical bonds between the component having a polyvinyl alcohol skeleton and the polyester molecular chain during melt extrusion, the extrusion temperature is preferably 260° C. to 300° C., more preferably 270° C. to 290° C. The melting time is preferably 30 seconds to 600 seconds, more preferably 60 seconds to 300 seconds.
[0044] As described above, a preferred embodiment of the polyester film of the present invention is a polyester film that satisfies the following condition A and / or condition B. When the polyester film satisfies condition A, the polyester film preferably has a wavelength of 2800 cm in the spectrum obtained under condition A. -1 From 3000cm -1 It has a peak at wavenumber 2800 cm -1 From 3000cm -1Peak intensity / wave number 3000cm -1 From 3400cm -1 It is more preferable that the peak intensity at the wave number of 2800 cm is 0.05 or more and 2.0 or less. -1 From 3000cm -1 The peak at the wavenumber of 2800 cm represents the stretching vibration of aliphatic hydrocarbons. When obtaining the polyester film of the present invention, the peak at the wavenumber of 2800 cm is obtained by using a polyvinyl alcohol resin having aliphatic hydrocarbons. -1 From 3000cm -1 It is possible to set the peak intensity in a preferred range.
[0045] When a polyester film containing a component having a polyvinyl alcohol skeleton is obtained by melt film formation, in order to efficiently express the interaction between the component having a polyvinyl alcohol skeleton and the polyester molecular chain, it is preferable that the content of a compound having an isocyanate group or an oxazoline group, which crosslinks compounds via a hydroxyl group by reacting with the hydroxyl group, that is, a so-called crosslinking agent, is 0.01% by mass or less in 100% by mass of the raw material of the polyester film. By making the content of the crosslinking agent 0.01% by mass or less, the components having a polyvinyl alcohol skeleton are crosslinked with each other, and the interaction between the component having a polyvinyl alcohol skeleton and the polyester molecular chain is reduced. Note that the crosslinking agent does not include the dicarboxylic acid component of polyester.
[0046] It is more preferable that the polyester film of the present invention satisfies the above-mentioned condition B. Since an organic component that is insoluble in HFIP, which is a parent solvent for polyester films such as PET, exists in the film with a certain shape, it can not only interact with polyester molecular chains but also function as a lubricant.
[0047] An example of a method that satisfies the above-mentioned condition B is a method in which a component having a polyvinyl alcohol skeleton is chemically bonded to a polyester molecular chain during melt extrusion, and a preferred example of such a method is the method of kneading at the above-mentioned temperature and time.
[0048] The content of the HFIP-insoluble organic component in the inner layer of the polyester film of the present invention is preferably 10 ppm or more and 1000 ppm or less by mass. By having a content of 10 ppm or more, sufficient interaction with the polyester molecular chain can be obtained. By having a content of 1000 ppm or less, it is possible to prevent the organic component from precipitating as a foreign matter in the film and becoming a starting point for film breakage.
[0049] The HFIP-insoluble organic component in the present invention more preferably has a polyethylene terephthalate (PET) skeleton. When a component having a polyvinyl alcohol skeleton is bonded to a PET molecular chain, it becomes insoluble in HFIP, and it is considered that the HFIP-insoluble component has a polyethylene terephthalate skeleton. When the HFIP-insoluble organic component has a PET skeleton, the HFIP-insoluble organic component interacts more with the PET molecular chain in the polyester film, so that the effect of the present invention is more easily obtained.
[0050] Whether the HFIP-insoluble organic component has a PET skeleton can be confirmed by the method described in the Examples.
[0051] In the polyester film of the present invention, it is also preferred that the outermost layer of the polyester film contains a component having a polyvinyl alcohol skeleton. In this embodiment, when coating is used as a means for making the layer X or other layers in contact with the polyester film of the present invention, the transportability is improved in the step of drying the solvent used in forming the layer X or other layers, so that the occurrence of defects in the formation of the layer X or other layers can be suppressed.
[0052] Having a component having a polyvinyl alcohol skeleton in the outermost layer of a polyester film means that the outermost layer of the polyester film is measured in accordance with conditions A and B and is found to fall under condition A and / or condition B. The outermost layer refers to a region from at least one surface of the polyester film to a depth of 5 μm in the thickness direction.
[0053] The polyester film of the present invention is preferably a biaxially oriented polyester film in terms of productivity, transportability, and handleability. Biaxial orientation can be confirmed by the Young's modulus of the film, and refers to measuring the Young's modulus (Emd) in the machine direction (MD) of the film and the Young's modulus (Etd) in the direction perpendicular thereto, and the Emd / Etd is 0.6 to 1.7. When the direction of the film is unknown, the direction of the film is defined as 0°, and the Young's modulus is measured while shifting the angle by 30°, and the maximum / minimum value is 1.0 to 1.7.
[0054] Next, a preferred embodiment of the method for producing the polyester film of the present invention will be described below.
[0055] In the method for producing the polyester film of the present invention, a method (melt casting method) can be used in which dried raw materials are heated and melted in an extruder as necessary, and extruded from a die onto a cooled casting drum to process into a sheet. When extruding onto the casting drum, the raw materials are cooled to a surface temperature of 20°C to 60°C and then cooled and solidified by static electricity to produce an unstretched sheet. The temperature of the casting drum is more preferably 20°C to 40°C, and even more preferably 20°C to 30°C.
[0056] The raw material used here may be one obtained by adding a component having a polyvinyl alcohol skeleton to polyester pellets, one obtained by remelting a laminated polyester film in which a component having a polyvinyl alcohol skeleton has been applied to the surface of the polyester film, or one obtained by mixing a film in which a component having a polyvinyl alcohol skeleton has been applied to the surface of a polyester film with polyester pellets.
[0057] Next, it is preferable to biaxially stretch the unstretched sheet at a temperature T1n (°C) that satisfies the following formula (i), by 3.6 times or more in the longitudinal direction (MD) of the film, by 3.9 times or more in the transverse direction (TD) of the film, and by an area stretching ratio of 14.0 times to 20.0 times. (i)Tg(℃)≦T1n(℃)≦Tg+40(℃) Tg: Glass transition temperature of polyester film (℃) The method of stretching the film in the longitudinal direction is preferably a method using a speed difference between rolls. In this case, it is also a preferred embodiment to stretch the film in a plurality of sections while fixing the film with nip rolls to prevent the film from slipping.
[0058] The polyester film of the present invention is biaxially oriented by biaxial stretching, whereby the component having a polyvinyl alcohol skeleton can move within the film and interact most stably with the polyester molecular chains.
[0059] Next, the biaxially stretched film or biaxially oriented film is heat-set for 1 second to 30 seconds at a temperature (Th0 (°C)) that satisfies the following formula (ii), and then uniformly cooled slowly to room temperature to obtain a polyester film. (ii)Tmf-35(℃)≦Th0(℃)≦Tmf(℃) Tmf: Melting point of the film (℃) By obtaining a biaxially oriented film under the condition (ii), it is possible to impart an appropriate orientation to the film and improve the handling properties of the film.
[0060] Next, a preferred embodiment of the laminated polyester film of the present invention will be described below.
[0061] The laminated polyester film of the present invention preferably has a layer X containing, as a main component, a resin having a polyvinyl alcohol skeleton on at least one surface of the polyester film of the present invention.
[0062] A resin having a polyvinyl alcohol skeleton is a resin having a molecular structure represented by chemical formula (3).
[0063] [ka]
[0064] Here, f is 1 or more and g is 0 or more.
[0065] As the resin having a polyvinyl alcohol skeleton, the above-mentioned polyvinyl alcohol-based resins can be suitably used.
[0066] The layer X mainly composed of a resin having a polyvinyl alcohol skeleton means that the layer X contains 90% by mass or more of the resin having a polyvinyl alcohol skeleton in 100% by mass of all components of the layer X, more preferably 95% by mass or more.
[0067] Since the resin having a polyvinyl alcohol skeleton is hydrophilic, this embodiment makes it possible to remove, using water, the layer X mainly composed of the resin having a polyvinyl alcohol skeleton, and other layers laminated in contact with the layer X. Furthermore, since the layer X has a skeleton similar to that of the component having a polyvinyl alcohol skeleton contained in the polyester film of the present invention, the polyester film of the present invention can be produced by removing a part of the layer X from the laminated polyester film and using the resulting film as part of the raw material, as described below, and recycling is easy.
[0068] The method for coating the layer X can be a general coating method such as gravure coating, Mayer bar coating, air knife coating, doctor knife coating, etc. In particular, from the viewpoint of the film-forming properties of the layer X, an in-line coating method is preferably used in which the raw material of the layer X is coated on the surface of the polyester film after uniaxial stretching in the longitudinal direction, and the polyester film is stretched in the width direction and the layer X is formed at the same time.
[0069] The thickness of the layer X is preferably 50 nm or more and 1000 nm or less. If the thickness is less than 50 nm, the water absorbency of the layer X may not be fully exhibited, and the removability may be poor. If the thickness exceeds 1000 nm, blocking may occur, and the handling properties may be deteriorated.
[0070] The laminated polyester film of the present invention preferably has a polyester film, the layer X, and the release layer Y in this order. This embodiment allows the film to be used as a release film, and also allows the polyester film to be obtained by removing the layer X and the release layer Y after use as a release film, and the film can be recycled by using it as a part of the raw material.
[0071] The above-mentioned laminated polyester film can be prepared by applying a coating solution containing the raw material components of the release layer Y to the laminated polyester film containing the layer X obtained by the above-mentioned method using a general coating method such as gravure coating, Mayer bar coating, air knife coating, doctor knife coating, etc.
[0072] Here, the release layer Y is preferably a layer containing, as a main component, one or more components selected from a silicone compound, a compound having a long-chain alkyl group (having 10 or more carbon atoms), and a compound having fluorine. Among them, from the viewpoint of coatability onto the layer X, silicone having a dimethylsiloxane as a main skeleton can be preferably used.
[0073] The thickness of the release layer Y is preferably 10 nm to 1000 nm. If it is less than 10 nm, the release function of the release layer Y may not be exhibited, and if it exceeds 1000 nm, the film-forming property may be poor.
[0074] Furthermore, a functional layer Z can be laminated on the release layer Y side of the laminated polyester film obtained by laminating a layer X and a release layer Y on the polyester film of the present invention. The functional layer Z is not particularly limited, but it is preferably a layer that is peeled off from the release layer Y, such as a ceramic green sheet used in MLCC production, or an adhesive for transferring to an adherend. When a ceramic green sheet is used as the functional layer Z, silicone having dimethylsiloxane as the main skeleton is preferably used as the release layer Y from the viewpoint of peelability. By using the laminated polyester film obtained by laminating a layer X and a release layer Y on the polyester film of the present invention as a release film for the MLCC production process, the ceramic green sheet can be peeled off without affecting the physical properties of the ceramic green sheet, and the sheet can be used for ceramic production, and the release film can be easily recycled.
[0075] A laminated polyester film of the present invention having layer X and release layer Y laminated thereon can be obtained by peeling off the functional layer Z from a film obtained by laminating layer X, release layer Y, and functional layer Z in this order on the polyester film of the present invention. By using this method, a laminated polyester film having layer X and release layer Y laminated thereon can be obtained without using the energy required for melt film formation or the energy required for coating and drying. Methods for peeling off the functional layer Z include, but are not limited to, a method of peeling off using an adhesive roll or a method of suctioning and peeling off only the functional layer Z.
[0076] Here, another preferred embodiment of the method for producing the polyester film of the present invention will be described.
[0077] As a method for producing the polyester film of the present invention, a preferred embodiment can be carried out in which the layer X and the release layer Y are simultaneously removed from the laminated polyester in which the layer X and the release layer Y are laminated on the polyester film of the present invention, and the polyester film of the present invention is obtained again. By adopting this embodiment, it is possible to save energy required for newly performing melt casting to obtain a polyester film.
[0078] Next, the process of removing the layer X and the release layer Y will be described.
[0079] Since the resin having a polyvinyl alcohol skeleton, which is the main component of layer X, is generally water-absorbent, washing with water is a preferred embodiment. In order to increase the water-absorbency of the resin having a polyvinyl alcohol skeleton, which is the main component of layer X, it is preferable to have a highly hydrophilic modified group contained in the side chain of the resin. Examples of highly hydrophilic modified groups include those with strong polarity such as carboxylate groups, carboxylate groups, sulfonate groups, and sulfonic acid groups. In addition, when the total amount of hydroxyl groups and acetoxy groups and the amount of modified groups in the resin having a polyvinyl alcohol skeleton is 100 mol%, the content of the modified group is preferably 1 mol% or more and 10 mol% or less.
[0080] The method of washing with water preferably includes a step of unwinding the laminated polyester film, a step of supplying hot water to the surface of the unwound laminated polyester film to peel off the surface laminated part such as layer X from the laminated polyester film, and a step of winding up the polyester film after peeling. The temperature of the hot water is preferably 50°C or higher and 150°C or lower. If the temperature is less than 50°C, sufficient cleaning properties may not be obtained. If the temperature exceeds 150°C, the glass transition temperature of the polyester film may be exceeded, and the film may not be transported. The time during which the water contacts the surface of the laminated polyester film is 5 seconds or more, preferably 10 seconds or more, and more preferably 30 seconds or more. From the viewpoint of productivity, the time is preferably 600 seconds or less. The step of supplying hot water to the surface of the unwound laminated polyester film is preferably performed in a water tank to cover the entire laminated polyester film, or a method of pressurizing heated water and spraying it onto the film.
[0081] The speed at which the film is conveyed is preferably 5 m / min or more, more preferably 10 m / min or more, and even more preferably 20 m / min or more and 100 m / min or less. When conveying the laminated polyester film provided with the layer X and the release layer Y in the step of removing the layer X and the release layer Y, it is also important to apply tension to the laminated polyester film. By applying tension, the surface of the laminated polyester film is stretched, and the mobility of the layer X and the release layer Y is improved, so that the washability can be improved. The tension is 5 N / m or more and 100 N / m or less, more preferably 20 N / m or more and 80 N / m or less, and even more preferably 30 N / m or more and 50 N / m or less. If it is less than 5 N / m, the surface of the laminated polyester film may not be stretched, and the washability may be poor. If it exceeds 100 N / m, the film may wrinkle, the surface may have poor stretchability, and the washability may be poor.
[0082] By using the polyester film of the present invention, when the film is washed by the above-mentioned method, the transportability of the film is improved, and as a result, it becomes possible to transport the film while applying a certain tension and removing the layer X and the release layer Y, which is preferable because the cleanability is improved.
[0083] In addition, the polyester film can be recycled and used by obtaining the polyester film in the following cycle. Specifically, the layer X is laminated on at least one side of the polyester film of the present invention by the above-mentioned method, a release layer Y is further laminated on the layer X, a functional layer Z is provided on the release layer Y, and then the layer X and the release layer Y are simultaneously removed from the laminated polyester film obtained by peeling the functional layer Z from the release layer Y. In addition, the polyester film after simultaneously removing the layer X and the release layer Y is melted as it is or together with other PET raw materials or a resin having a polyvinyl alcohol skeleton, and molded into a film to obtain a polyester film. By melting once and forming a film, a polyester film with good quality such as grade can be obtained while being recycled.
[0084] As a recycling method, a polyester film can be preferably obtained by melting a polyester film obtained by removing a part of the layer X from the laminated polyester film, and molding the polyester film using the composition obtained. By leaving a part of the layer X, a component having a polyvinyl alcohol skeleton can be introduced into the polyester film without a step of adding a component having a polyvinyl alcohol skeleton to the melt-cast polyester film, and productivity is good. The amount of the layer X to be removed is preferably 90% or more by mass, more preferably 95% or more, from the viewpoint of setting the amount of the component having a polyvinyl alcohol skeleton to be contained in an appropriate range.
[0085] [Method of evaluating characteristics] A. (Measurement method A) A method of measuring using a microscopic infrared spectrometer. Equipment: Microscopic infrared spectroscopic analyzer; LUMOS (manufactured by Bruker) Measurement conditions: Light source: Silicon carbide rod heating element (glow bar) Detector: Narrow MCT (HgCdTe) Detection range: 4000~650cm -1 Purge; Nitrogen gas Measurement mode: Transmission method Resolution; 8cm -1 Number of times accumulated: 256 A spectrum is obtained by plotting the absorption intensity against each wave number.
[0086] In the cross section of the polyester film, measurements are taken in a direction perpendicular to the outermost surface of the polyester film, and 10 points are measured evenly in the thickness direction at a depth of 5 μm or more (hereinafter referred to as the inner layer portion) using the above-mentioned device and conditions to obtain a spectrum. The spectrum is then divided by the spectrum of PET (a PET spectrum (measured under the same conditions using #50T60 manufactured by Toray Industries, Inc.) to obtain a spectrum at 1000 cm -1 ~1500cm -1The spectrum is obtained by dividing the spectrum obtained by measurement by the four basic arithmetic operations so that the peak shapes of the two spectra match as closely as possible.
[0087] Here, the wave number 3300 cm obtained by measuring each point -1 From 3400cm -1 The peak intensity of the peak detected at is measured at 10 points and the minimum value is obtained.
[0088] B. (Measurement method B) A method of measuring using an infrared spectrometer. Apparatus: Infrared spectrometer; "Nicolet" (registered trademark) 6700 (manufactured by Thermofisher Scientific) Measurement conditions: Light source: Silicon carbide rod heating element (glow bar) Detector: DTGS (triglycine sulfate) Detection range: 4000~680cm -1 Purge; Nitrogen gas Measurement mode: ATR method (attenuated total reflection measurement method) Single-reflection ATR measurement accessory device (OMNI sampler), ATR crystal: Ge, incident angle: 45° Resolution; 4cm -1 Number of times accumulated: 256 A spectrum is obtained by plotting the absorption intensity against each wave number.
[0089] First, for each of 50 pieces of 4 cm square polyester film, 5 μm is scraped off from one surface of the polyester film using a microtome while observing under a microscope, and then 5 μm is scraped off from the surface of the opposite surface in the same manner to obtain the inner layer of the polyester film.
[0090] The obtained inner layer portion is immersed in hexafluoro-2-propanol (HFIP) and dissolved for 30 minutes under nitrogen atmosphere with stirring at 50° C. The liquid is then cooled to 25° C., and insoluble matter is collected with a PTFE filter (manufactured by ADVANTEC, model number: 13010802). The collected matter is measured with the above-mentioned device and conditions to obtain a spectrum.
[0091] Here, for the spectrum obtained, the wave number is 3300 cm -1 From 3400cm -1 The peak intensity is calculated at
[0092] C. Thickness of each layer The thickness of each layer of the polyester film and laminated polyester film is measured by the following method. The cross section of the film is cut out with a microtome in a direction parallel to the width direction of the film. The cross section is observed with a scanning electron microscope at a magnification of 5000 times, and the thickness of each layer is measured.
[0093] D. Method for identifying components with PET skeleton (infrared spectroscopy) Apparatus: Infrared spectrometer; “Nicolet” (registered trademark) 6700 (manufactured by Thermofisher Scientific) ·Conditions: Light source: Silicon carbide rod heating element (glow bar) Detector: DTGS (triglycine sulfate) Detection range: 4000~680cm -1 Purge: Nitrogen gas Measurement mode: ATR method (attenuated total reflection measurement method) Single-reflection ATR measurement accessory device (OMNI sampler), ATR crystal: Ge, incident angle: 45° Resolution: 4cm -1 Number of times of accumulation: 256 A spectrum is obtained by plotting the absorption intensity against each wave number.
[0094] First, 5 μm of the polyester film is removed from one surface using a microtome while observing under a microscope, and then 5 μm is removed from the other surface in the same manner to obtain the inner layer of the polyester film.
[0095] The obtained inner layer portion is immersed in hexafluoro-2-propanol (HFIP) and dissolved for 30 minutes while stirring at 50°C under a nitrogen atmosphere. The liquid is then cooled to 25°C, and insoluble matter is collected using a PTFE filter (manufactured by ADVANTEC, model number: 13010802). The collected matter is measured using the above-mentioned device and conditions to obtain a spectrum. The obtained spectrum is analyzed at a wave number of 1090 cm. -1 From 1110cm -1 A peak was detected at a peak intensity of 1.0×10 -3 That is all.
[0096] When two or more peaks are observed, the intensity of the strongest peak is used.
[0097] E. Amount of HFIP-insoluble organic components in the inner layer (ppm) First, 5 μm is scraped off from one surface of the polyester film using a microtome while observing under a microscope. In the same manner, 5 μm is scraped off from the surface of the opposite surface to obtain the inner layer of the polyester film. The mass of the obtained inner layer is weighed and designated as m0.
[0098] The obtained inner layer part is immersed in hexafluoro-2-propanol (HFIP) and dissolved for 30 minutes while stirring at 50°C under a nitrogen atmosphere. After that, the liquid temperature is cooled to 25°C, and insoluble matter is collected with a PTFE filter (manufactured by ADVANTEC, model number: 13010802). The collected matter is dried under vacuum at 80°C, cooled to 25°C, and the mass is measured and designated as m1. Next, the sample is placed on a sample boat made of quartz glass with a known mass, and heated in a cylindrical electric furnace preheated to 320°C under a nitrogen atmosphere for 45 minutes to incinerate the target composition. After cooling the sample boat for 10 minutes under a nitrogen atmosphere, it is transferred to a desiccator and cooled to room temperature, and the mass is weighed and designated as m2. After subtracting m2 from m1, divide by m0 and display as ppm.
[0099] F. Amount of HFIP-insoluble organic components in the outermost layer (ppm) First, 5 μm is scraped off from one surface of the polyester film using a microtome while observing under a microscope. In the same manner, 5 μm is scraped off from the surface of the opposite surface, and the resultant is weighed and the mass of the outermost surface portion is defined as m3.
[0100] The obtained inner layer is immersed in hexafluoro-2-propanol (HFIP) and dissolved for 30 minutes under nitrogen atmosphere at 50°C while stirring. The liquid is then cooled to 25°C, and insoluble matter is collected with a PTFE filter (manufactured by ADVANTEC, model number: 13010802). The collected matter is dried under vacuum at 80°C, cooled to 25°C, and the mass is measured and designated as m4. Next, the sample is placed on a sample boat made of quartz glass with a known mass, and heated in a cylindrical electric furnace preheated to 320°C under a nitrogen atmosphere for 45 minutes to incinerate the desired composition. The sample boat is allowed to cool for 10 minutes under a nitrogen atmosphere, then transferred to a desiccator and allowed to cool to room temperature, and the mass is weighed and designated as m5. After subtracting m5 from m4, the result is divided by m3 and expressed as ppm.
[0101] G. Water contact angle (°) The measurement is performed using the following method using a contact angle meter DM500 manufactured by Kyowa Interface Science Co., Ltd. and the attached analysis software FAMAS. In an atmosphere of 23°C and 65% RH, the time when the water droplet contacts the sample surface is set as 0 seconds, and an image of the droplet is taken 1 second later, and the contact angle is measured from the image. The measurement is performed 5 times at different locations, and the average value is calculated.
[0102] H. Film transportability The transportability of the film is judged by the shape of the roll after transport. The film is wound up at a winding speed of 30 m / min with a width of 300 mm and a length of 500 m, and the state of the wound roll is observed to judge. After unwinding the film, it is passed through a water bath at 80°C for 10 seconds, then dried in a drying oven heated to 150°C for 10 seconds, and then wound up. The judgment method is to measure the occurrence of horizontal wrinkles on the wound roll. One revolution of the roll is taken from the roll, and the ratio of horizontal wrinkles that have occurred on the film is calculated. The ratio (%) of horizontal wrinkles is calculated by [(total length of horizontal wrinkles connected in the width direction of the film in the length direction of the film, i.e. total width of horizontal wrinkles) / (length of one revolution of the roll)]×100. Toner is sprayed on the unwound film to observe the horizontal wrinkles. The evaluation is based on the average value per roll when five or more rolls are wound, and is judged as follows.
[0103] A: Horizontal wrinkle occurrence rate is less than 5% B: Horizontal wrinkle occurrence rate: 5% to less than 10% C: Horizontal wrinkle occurrence rate is 10% or more.
[0104] I. Amount (%) of layer X remaining on polyester film after layer X and release layer Y are peeled off The laminated polyester film sample is cut into 20 pieces each measuring 200 mm square, dried at 50°C for 30 minutes, cooled to 25°C, and the mass is measured and designated as B(0). The film is immersed entirely in a water bath at 80°C, and layer X is dissolved in water for 3 hours while being vibrated with ultrasonic waves. The film is then removed and washed in another water bath at 80°C in the same manner for 30 minutes. The film is then wiped to remove moisture, dried at 50°C for 30 minutes, cooled to 25°C, and the mass is measured and designated as B(1).
[0105] The remaining amount (%) of layer X relative to the polyester film is calculated using (B(0)-B(1)) / B(0) x 100. EXAMPLES
[0106] The present invention will be described below with reference to examples, but the present invention is not necessarily limited to these.
[0107] [Production of PET-1] Terephthalic acid and ethylene glycol were polymerized in the usual manner using antimony trioxide and magnesium acetate tetrahydrate as catalysts to obtain melt-polymerized PET. The resulting melt-polymerized PET had a glass transition temperature of 81°C, a melting point of 255°C, an intrinsic viscosity of 0.65, and a terminal carboxyl group content of 20eq. / t. [PVA-1] "GOHSENOL" (registered trademark) GL-05 manufactured by Mitsubishi Chemical Corporation was used. [PVA-2] PVA having a degree of saponification of 88, an average degree of polymerization of 500, and 1 mol % of sodium sulfonate in the side chain was prepared with reference to the patent document JP-A-9-227627. [PVA-3] PVA having a degree of saponification of 88, an average degree of polymerization of 1000, and 1 mol % of sodium carboxylate in the side chain was prepared with reference to Patent Document JP-A-2008-291120. [Preparation of Coating A] 100 parts by mass of an addition reaction type silicone resin release agent (manufactured by Dow Corning Toray Silicones Co., Ltd., product name "LTC" (registered trademark) 750A) and 2 parts by mass of a platinum catalyst (manufactured by Dow Corning Toray Silicones Co., Ltd., product name SRX212) were mixed in toluene as a solvent to give a solids content of 5 mass%, thereby obtaining Coating A.
[0108] [Preparation of Coating Agent B] Coating Agent B was obtained by dissolving PVA-2 in water to a concentration of 4% by mass.
[0109] [Preparation of dielectric paste] Glass beads with a number average particle size of 2 mm were added to 100 parts by mass of barium titanate (manufactured by Fuji Titanium Kogyo Co., Ltd., product name HPBT-1), 10 parts by mass of polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd., product name BL-1), 5 parts by mass of dibutyl phthalate, and 60 parts by mass of toluene-ethanol (mass ratio 30:30), and the mixture was mixed and dispersed in a jet mill for 20 hours, and then filtered to prepare a paste-like dielectric paste.
[0110] Example 1 99.999 parts by weight of PET-1 and 0.001 parts by weight of PVA-1 were mixed and fed into an extruder equipped with a vent hole while reducing the pressure to 100 torr or less. The mixture was then heated at 280°C with a shear rate of 20 sec -1 The sheet was melted at 200°C for 100 seconds and extruded through a die onto a casting drum with a surface temperature of 25°C to produce an unstretched sheet. The sheet was then preheated with a heated roll group, stretched 3.8 times in the longitudinal direction (MD direction) at a temperature of 90°C, and then cooled with a roll group at a temperature of 25°C to obtain a uniaxially stretched film. The film was then stretched 4.3 times in the width direction (TD direction) perpendicular to the longitudinal direction in a heating zone at a temperature of 100°C in a tenter while both ends of the film were held with clips. The film was then heat-set for 10 seconds at a temperature of 235°C in a heat treatment zone in the tenter. The film was then uniformly cooled in a cooling zone, and wound up to obtain a polyester film. The properties of the obtained polyester film were as shown in the table. In addition, in the method for distinguishing components having a polyvinyl alcohol skeleton (microscopic infrared spectroscopy), the measured value was 1×10 -3 Therefore, it is shown as "-" in the table.
[0111] The obtained polyester film contained a component having a polyvinyl alcohol skeleton in the inner layer of the film and met condition B, and therefore was a film with excellent transportability.
[0112] (Examples 2-4 and 6) A polyester film was obtained in the same manner as in Example 1, except that the amount and type of polyvinyl alcohol added were changed as shown in the table. The properties of the obtained polyester film are shown in the table. As the amount of the component having a polyvinyl alcohol skeleton increased, the transportability improved. In Example 4, which used PVA having sodium sulfonate in the side chain, the transportability was particularly good.
[0113] Example 5 Two extruders, A and B, were prepared. The same raw materials as in Example 4 were melted in the extruder B in the same manner as in Example 4. Only PET-1 was fed into the other extruder A while reducing the pressure to 10 torr, and the mixture was heated at 280°C with a shear rate of 20 sec. -1 The resin was melted for 100 seconds at 200° C. The resin was fed into two extruders and melted, and then introduced into a lamination device so that the thickness of layer A after stretching would be 5 μm. The flows were joined to form an A / B / A structure, and a polyester film was obtained in the same manner as in Example 4. The properties of the obtained polyester film are shown in the table. The obtained polyester film contained a component having a polyvinyl alcohol skeleton in the inner layer portion and met conditions A and B, and therefore was a film with excellent transportability.
[0114] (Reference example 1) 99.95 parts by weight of PET-1 and 0.05 parts by weight of PVA-2 were mixed and fed into an extruder equipped with a vent hole while reducing the pressure to 10 torr. The mixture was then heated at 280°C with a shear rate of 20 sec. -1The sheet was melted at 25°C for 100 seconds and extruded through a die onto a casting drum with a surface temperature of 25°C to produce an unstretched sheet. The sheet was then preheated with a heated roll group, stretched 3.8 times in the longitudinal direction (MD direction) at a temperature of 90°C, and then cooled with a roll group at a temperature of 25°C to obtain a uniaxially stretched film. Coating agent B was applied to the obtained uniaxially stretched film by a bar coating method so that the coating thickness after drying and stretching would be 100 nm, and then, while holding both ends of the film with clips, the film was stretched 4.3 times in the width direction (TD direction) perpendicular to the longitudinal direction in a heating zone at a temperature of 100°C in a tenter. Further, the film was heat-set for 10 seconds at a temperature of 230°C in a heat treatment zone in the tenter. The film was then uniformly cooled slowly in a cooling zone, and taken up to obtain a laminated polyester film in which layer X was laminated to a thickness of 100 nm.
[0115] On the layer X of the obtained laminated polyester film, the coating material A was applied by gravure coating to form a release layer Y so as to have a thickness of 100 nm after drying, thereby obtaining a laminated polyester film.
[0116] A dielectric paste was applied to the obtained laminated polyester film by a die coating method so that the thickness after drying would be 1.0 μm as the functional layer Z. Then, the functional layer Z was released from the obtained laminate, and a film roll of the laminated polyester film from which the functional layer Z had been peeled was obtained. The film roll was introduced into a water washing device equipped with an unwinding and winding device, and washed with water at 100° C. for 2 minutes under a tension of 30 N / m, and the polyester film from which the layer X and the release layer Y had been removed was collected.
[0117] The contact angle of water on the film surface of the polyester film of Example 4 was 72°, while the contact angle of water on the layer X side surface of the recovered polyester film was 55°, indicating hydrophilicity, suggesting that a portion of layer X remained in the recovered polyester film. The remaining amount was measured, and was found to be mass of layer X / mass of recovered polyester film=0.07%.
[0118] Example 7 The polyester film recovered in Reference Example 1 was cut into flakes, and 20 parts by mass of the flakes were mixed with 80 parts by mass of PET-1 to obtain a polyester film in the same manner as in Example 1, except that no PVA-1 was added. The properties of the obtained film are shown in the table. Since the film contained a component having a polyvinyl alcohol skeleton and met conditions A and B, it was a film with excellent transportability.
[0119] Example 8 The polyester film recovered in Reference Example 1 was cut into flakes, and 20 parts by mass of the flakes were mixed with 79.97 parts by mass of PET-1 and 0.03 parts by mass of PVA-2 to obtain a polyester film in the same manner as in Example 1, except that no PVA-1 was added. The properties of the obtained film are shown in the table. The film contained a component having a polyvinyl alcohol skeleton and met conditions A and B, and therefore had excellent transportability.
[0120] Comparative Example 1 A polyester film was obtained in the same manner as in Example 1, except that only PET-1 was used and no PVA-1 was added. Since the film did not have a polyvinyl alcohol skeleton, it did not satisfy conditions A and B and had poor transportability.
[0121] Comparative Example 2 A uniaxially stretched film was obtained in the same manner as in Example 1, except that the raw materials and stretching conditions were changed as shown in the table. The film did not satisfy conditions A and B and had poor transportability.
[0122] [Table 1]
[0123] [Table 2]
[0124] [Table 3]
[0125] [Table 4]
[0126] [Table 5] [Industrial Applicability]
[0127] The polyester film of the present invention has excellent transportability, and therefore can be used in various industrial material applications and can improve the recovery of the film after use.
Claims
1. A composition containing a component having a polyvinyl alcohol skeleton, which, when measured by the following measurement method A and measurement method B, has a wave number of 3,300 cm in measurement method A and / or measurement method B. -1 From 3400 cm -1 A peak was detected at and the peak intensity was 1.0×10 -3 The biaxially oriented polyester film is as described above. (Measurement Method A) A method of measuring using a microscopic infrared spectrometer. Device : Microscopic infrared spectroscopic analyzer: LUMOS (manufactured by Bruker) Measurement conditions: Light source: Silicon carbide rod heating element (glow bar) Detector: Narrow MCT (HgCdTe) Detection wave number range: 4000 to 650 cm -1 purge; Nitrogen gas Measurement mode: Transmission method Decomposition energy: 8cm -1 Number of times of accumulation: 256 A spectrum is obtained by plotting the absorption intensity against each wave number. In the cross section of the polyester film, measurements are made at 10 points evenly spaced in the thickness direction, at least 5 μm inside (hereinafter referred to as the inner layer portion) measured in the vertical direction relative to the outermost surface of the polyester film, using the above-mentioned device and conditions to obtain a spectrum. The spectrum is then divided by the PET spectrum (a PET spectrum (measured under the same conditions using #50T60 manufactured by Toray Industries, Inc.)) to obtain a spectrum at 1000 cm. -1 ~1500cm -1 The spectrum is obtained by dividing the spectrum obtained by measurement by the four basic arithmetic operations so that the peak shapes of the above match as closely as possible. Here, at least one of the 10 measurement points was measured, and the divided spectrum had a wave number of 3300 cm -1 From 3400 cm -1 If a peak is detected at a wave number of 3,300 cm when measured by measurement method A, -1 From 3400 cm -1 In addition, at least one of the 10 measurement points has a peak intensity of 1.0×10 -3 If the peak intensity is 1.0×10 or more when measured by measurement method A, -3 Let's say that this is all. In addition, for the divided spectrum at a certain measurement point, -1 From 3400 cm -1 When two or more peaks are observed, the maximum peak intensity is 1.0×10 -3 or more, the peak intensity detected in the divided spectrum at that measurement point is 1.0×10 -3 Let's say that this is all. (Measurement Method B) A method of measuring using an infrared spectrometer. Apparatus: Infrared spectroscopic analyzer; "Nicolet" (registered trademark) 6700 (manufactured by Thermofisher Scientific) Measurement conditions: Light source: Silicon carbide rod heating element (glow bar) Detector: DTGS (triglycine sulfate) Detection wave number range: 4000 to 680 cm -1 Purge: Nitrogen gas Measurement mode: ATR method (attenuated total reflection measurement method) Single reflection type ATR measurement accessory (OMNI sampler), ATR crystal: Ge, incident angle: 45° Decomposition energy: 4cm -1 Number of times of accumulation: 256 A spectrum is obtained by plotting the absorption intensity against each wave number. First, 50 pieces of 4 cm square polyester film are each scraped off 5 μm from one surface layer using a microtome while observing under a microscope, and then 5 μm is scraped off from the other surface in the same manner to obtain the inner layer portion of the polyester film. The obtained inner layer portion is immersed in hexafluoro-2-propanol (HFIP) and dissolved for 30 minutes with stirring at 50° C. in a nitrogen atmosphere. The liquid is then cooled to 25° C., and insoluble matter is collected with a PTFE filter (manufactured by ADVANTEC Corporation, model number: 13010802). The collected matter is measured with the above-mentioned device and conditions to obtain a spectrum. Here, the spectrum obtained is at a wave number of 3300 cm -1 From 3400 cm -1 If a peak is detected at a wave number of 3,300 cm when measured by measurement method B, -1 From 3400 cm -1 In addition, for the spectrum obtained, a peak is detected at a peak intensity of 1.0×10 -3 If the peak intensity is 1.0×10 or more when measured by measurement method B, -3 Let's say that this is all. In addition, the spectrum obtained above has a wave number of 3300 cm -1 From 3400 cm -1 When two or more peaks are observed, the maximum peak intensity is 1.0×10 -3 or more, the peak intensity detected in the obtained spectrum is 1.0×10 -3 Let's say that this is all.
2. A biaxially oriented polyester film as described in claim 1, wherein the content of the component having the polyvinyl alcohol skeleton is 0.001 to 0.05 mass %.
3. In the measurement method B, the wave number is 3300 cm -1 From 3400 cm -1 A peak was detected at and the peak intensity was 1.0×10 -3 3. The biaxially oriented polyester film according to claim 1, wherein the inner layer of the polyester film contains 10 ppm to 1000 ppm of an organic component insoluble in HFIP by mass.
4. In the measurement method B, the wave number is 3300 cm -1 From 3400 cm -1 A peak was detected at and the peak intensity was 1.0×10 -3 The biaxially oriented polyester film according to any one of claims 1 to 3, wherein the HFIP-insoluble organic component has a polyethylene terephthalate skeleton.
5. 5. The biaxially oriented polyester film according to claim 1, wherein the outermost layer of the polyester film contains a component having a polyvinyl alcohol skeleton.
6. 6. A laminated polyester film having a layer X mainly composed of a resin having a polyvinyl alcohol skeleton on at least one surface of the biaxially oriented polyester film according to claim 1.
7. The laminated polyester film according to claim 6 , comprising the polyester film, the layer X, and a release layer Y in this order.
8. The laminated polyester film according to claim 7 , comprising the polyester film, the layer X, the release layer Y, and the functional layer Z in this order.
9. A method for producing a laminated polyester film, comprising a step of peeling off the functional layer Z from the laminated polyester film according to claim 8.
10. A method for producing a polyester film, comprising the step of simultaneously removing the layer X and the release layer Y from the laminated polyester film according to claim 7.
11. A method for producing a polyester film, comprising the steps of peeling off the functional layer Z and simultaneously removing the layer X and the release layer Y from the laminated polyester film according to claim 8, in that order.
12. A method for producing a polyester film, comprising laminating a release layer Y on the layer X of the laminated polyester film according to claim 6, providing a functional layer Z on the release layer Y, peeling off the functional layer Z, and then removing the layer X and the release layer Y.
13. A method for producing a polyester film, comprising a step of melting a polyester film obtained by removing a part of the layer X from the laminated polyester film according to any one of claims 6 to 8, and molding the polyester film using a composition obtained by melting the polyester film.
Citation Information
Patent Citations
Resin composition and film excellent in water resistance and gas barrier properties
JP1995276576A
Anti-icing film
JP2003113254A
Release film
JP2008142960A
Apparatus and method for forming thermoplastic resin film
JP2012171276A
Single-layer or multi-layer tubular food packaging film capable of smoking and air-drying, and method for producing the same.
JP2012516786A