- Current Assignee / Owner
- Priority Date
- 2019-11-27
- Filing Date
- 2020-11-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-11-25
AI Technical Summary
Conventional resin compositions for flexible printed wiring boards fail to maintain sufficient conductivity and adhesiveness after long-term storage in high-temperature, high-humidity environments, leading to issues in bonding and insulation reliability.
A resin composition comprising a polyester polyurethane resin with a molecular weight per urethane bond of 200 to 8,000, combined with an epoxy resin, which enhances adhesion and conductivity even after prolonged exposure to harsh conditions.
The composition provides a cured product with excellent conductivity and adhesiveness, maintaining high adhesive strength and insulation reliability even after 1,000 hours in a 60°C, 95% RH environment, with improved initial and post-soldering adhesion and stability.
Smart Images

Figure 0007586092000001 
Figure 0007586092000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester polyurethane resin composition which has high adhesion to polyimide films and metals, and when cured has heat resistance and moist heat resistance, and is excellent in liquid stability and processability, and is an effective member for producing a printed wiring board, in particular a flexible printed wiring board or a multilayer printed wiring board by a build-up method.Furthermore, the present invention relates to a bonding film in which the resin composition is applied to a release film, a laminate with a resin composition layer in which the resin composition is applied to a base film, a laminate having a layer formed by curing the resin composition, a flexible copper-clad laminate or a flexible flat cable, and an electromagnetic wave shielding film which is applied to a flexible printed wiring board or the like and is suitably used for shielding electromagnetic noise generated from an electric circuit. [Background technology]
[0002] Flexible printed wiring boards are capable of three-dimensional and high-density mounting even in a limited space, and therefore their applications are expanding. In recent years, with the miniaturization and weight reduction of electronic devices, products related to flexible printed wiring boards have become more diverse and the demand for them has increased. Such related products include flexible copper-clad laminates in which copper foil is bonded to a polyimide film, flexible printed wiring boards in which an electronic circuit is formed on a flexible copper-clad laminate, flexible printed wiring boards with reinforcement plates in which a flexible printed wiring board and a reinforcement plate are bonded together, flexible copper-clad laminates or multilayer boards in which flexible printed wiring boards are stacked and bonded, and the like. For example, when manufacturing a flexible copper-clad laminate, an adhesive is usually used to bond the polyimide film and the copper foil.
[0003] As a conventional adhesive composition or a conventional laminate, the methods described in Patent Documents 1 to 3 are known. Patent Document 1 describes a halogen-free flame-retardant adhesive composition comprising (A) a solvent-soluble polyamide resin that is solid at 25°C, (B) a phenoxy resin, (C) an epoxy resin that does not contain halogen atoms, and (D) a phosphorus-based flame retardant having a structure represented by the following general formula (1), wherein the epoxy resin (C) is an epoxy resin having three or more epoxy groups in one molecule, the content of the phenoxy resin (B) is 100 to 450 parts by mass per 100 parts by mass of the polyamide resin (A), the content of the epoxy resin (C) is 1 to 60 parts by mass per 100 parts by mass of the total of the polyamide resin (A) and the phenoxy resin (B), and the content of the phosphorus-based flame retardant (D) is 5 to 100 parts by mass per 100 parts by mass of the polyamide resin (A) and the phenoxy resin (B).
[0004] Patent Document 2 describes a laminate comprising a polyester polymer (a) containing two or more carboxyl groups in the molecule, a number average molecular weight of 5,000 to 100,000, and a molecular weight per carboxyl group of 1,500 to 10,000, an epoxy resin (b) containing two or more epoxy groups in the molecule, and an epoxy resin curing accelerator (c), the curable resin composition being capable of retaining thermoplasticity for five months or more at 5°C, laminated on at least one surface of a polyimide film, a polyester film, or a metal foil, and a laminate in which the curable resin composition of the laminate is cured and laminated on a metal foil (including a metal circuit).
[0005] In addition, Patent Document 3 describes a method for producing a carboxyl group-containing polymer having an acid value (unit: equivalent / 10 6 g) is 100 or more and 1000 or less, and the number average molecular weight is 5.0 × 10 3 Above 1.0×10 5The document describes a resin composition for adhesives, which comprises a polyurethane resin (a) having a glass transition temperature of -10°C or more and 70°C or less, an epoxy resin (b) containing nitrogen atoms, and an epoxy resin (c) having a dicyclopentadiene skeleton, wherein the blending ratio of the resin (b) is 0.1 mass % or more and 20 mass % or less of the total epoxy resins contained in the resin composition. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 5846290 [Patent Document 2] JP 2005-125724 A [Patent Document 3] JP 2010-84005 A Summary of the Invention [Problem to be solved by the invention]
[0007] The problem to be solved by the present invention is to provide a resin composition which gives a cured product having excellent electrical conductivity and adhesiveness even after long-term (1,000 hours) storage in a high-temperature, high-humidity environment (60°C, 95% RH). Another problem to be solved by the present invention is to provide a laminate having a resin composition layer, a laminate, a flexible copper-clad laminate, a flexible flat cable, or an electromagnetic wave shielding film, which uses the resin composition. [Means for solving the problem]
[0008] Means for solving the above problems include the following aspects. <1> A resin composition comprising a polyester polyurethane resin (A) and an epoxy resin (B), wherein the polyester polyurethane resin (A) has a molecular weight of 200 to 8,000 per urethane bond. <2> The diol component constituting the polyester polyurethane resin (A) contains a diol having a side chain. <1> The resin composition according to claim 1. <3> The polyester polyurethane resin (A) contains a polyester polyurethane resin having a polyester structure and a number average molecular weight of 8,000 to 30,000. <1> or <2> The resin composition according to claim 1. <4> The number average molecular weight of the polyester polyurethane resin (A) is 10,000 to 80,000. <1> ~ <3> 10. The resin composition according to claim 9 . <5> The acid value of the polyester polyurethane resin (A) is 0.1 mgKOH / g to 20 mgKOH / g. <1> ~ <4> 10. The resin composition according to claim 9 . <6> The glass transition temperature of the polyester polyurethane resin (A) is 30°C to 150°C. <1> ~ <5> 10. The resin composition according to claim 9 . <7> The content of the epoxy resin (B) is 1 part by mass to 30 parts by mass with respect to 100 parts by mass of the polyester polyurethane resin (A). <1> ~ <6> 10. The resin composition according to claim 9 . <8> The epoxy resin (B) contains a bisphenol novolac type epoxy resin. <1> ~ <7> 10. The resin composition according to claim 9 . <9> <1> ~ <8> a resin composition layer comprising the resin composition according to any one of the above items 1 to 5, a B-stage resin composition layer formed by partially curing the resin composition, or a cured layer formed by curing the resin composition, and a substrate film in contact with at least one surface of the resin composition layer, the B-stage resin composition layer, or the cured layer. <10> <1> ~ <8> 13. A laminate comprising a cured layer obtained by curing the resin composition according to any one of the above items. <11> Copper foil and <1> ~ <8> 13. A flexible copper-clad laminate comprising a cured layer obtained by curing the resin composition according to any one of claims 1 to 12, and a substrate. <12> Copper wiring, <1> ~ <8> 13. A flexible flat cable comprising: a cured layer formed by curing the resin composition according to any one of claims 1 to 12; and a covering material. <13> <1> ~ <8> 1. An electromagnetic wave shielding film having a resin composition layer made of the resin composition according to any one of claims 1 to 9, a B-stage resin composition layer obtained by partially curing the resin composition, or a cured layer obtained by curing the resin composition. Effect of the Invention
[0009] According to the present invention, it is possible to provide a resin composition which gives a cured product having excellent electrical conductivity and adhesiveness even after long-term (1,000 hours) storage in a high-temperature, high-humidity environment (60°C, 95% RH). Furthermore, according to the present invention, it is possible to provide a laminate having a resin composition layer, a laminate, a flexible copper-clad laminate, a flexible flat cable, or an electromagnetic wave shielding film using the resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following description of the constituent elements may be based on a representative embodiment of the present invention, but the present invention is not limited to such an embodiment. In this specification, the word "to" is used to mean that the numerical values before and after it are included as the lower limit and upper limit. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples. In the present invention, when a plurality of substances corresponding to each component are present in the composition, the amount of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. In the present invention, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. In the present invention, "mass %" and "weight %" are synonymous, and "parts by mass" and "parts by weight" are synonymous. Also, in the present invention, a combination of two or more preferred embodiments is a more preferred embodiment. In addition, in this specification, "(meth)acrylic" refers to both or either of acrylic and methacrylic. In the present disclosure, the term "main chain" refers to the relatively longest bond chain in the molecule of the polymer compound that constitutes the resin, and the term "side chain" refers to a carbon chain branching off from the main chain. Furthermore, in some of the compounds in this specification, the hydrocarbon chain may be represented by a simplified structural formula in which the symbols for carbon (C) and hydrogen (H) are omitted. The present invention will be described in detail below.
[0011] (Resin composition) The resin composition of the present invention contains a polyester polyurethane resin (A) and an epoxy resin (B), and the polyester polyurethane resin (A) has a molecular weight of 200 to 8,000 per urethane bond. The resin composition of the present invention can be suitably used as an adhesive composition, more suitably used as an adhesive composition for bonding polyimide or metal, and particularly suitably used as an adhesive composition for bonding polyimide and metal.
[0012] The present inventors have found that conventional resin compositions, when cured, do not have sufficient electrical conductivity and adhesion after long-term storage in a high-temperature, high-humidity environment. As a result of intensive research, the present inventors have found that it is possible to provide a resin composition which contains a polyester polyurethane resin (A) and an epoxy resin (B), in which the molecular weight per urethane bond in the polyester polyurethane resin (A) is 200 to 8,000, and in which these two resins act in a synergistic manner and complement each other, thereby producing a cured product which has excellent electrical conductivity and adhesion even after long-term storage in a high-temperature, high-humidity environment, although the detailed mechanism is unknown.
[0013] In addition, the resin composition of the present invention contains a polyester polyurethane resin (A) and an epoxy resin (B). Since the molecular weight per urethane bond in the polyester polyurethane resin (A) is 200 to 8,000, the resin composition is excellent in initial or post-soldering adhesion, and initial or post-soldering conductivity. In particular, the resin composition of the present invention contains a polyester polyurethane resin (A) and an epoxy resin (B). Since the molecular weight per urethane bond in the polyester polyurethane resin (A) is 200 to 8,000, the resin composition has high adhesive strength to polyimide and metal, excellent appearance after solder formation, excellent heat resistance, and excellent insulation reliability.
[0014] In this specification, "polyester polyurethane resin (A)" and the like are also referred to as "component (A)" and the like.
[0015] <Polyester polyurethane resin (A)> The resin composition of the present invention contains a polyester polyurethane resin (A), and the polyester polyurethane resin (A) has a molecular weight of 200 to 8,000 per urethane bond. The polyester polyurethane resin (A) may be any resin having two or more ester bonds and two or more urethane bonds, but is preferably a resin having a polyester chain and two or more urethane bonds. In addition, the polyester polyurethane resin (A) is preferably a resin obtained by reacting at least a polyester polyol, a polyisocyanate, and a chain extender as raw materials, and more preferably a resin obtained by reacting at least a polyester polyol, a polyisocyanate, and a diol compound.
[0016] The molecular weight per urethane bond in the polyester polyurethane resin (A) is 200 to 8,000, and from the viewpoints of electrical conductivity and heat resistance, it is preferably 250 to 5,000, more preferably 300 to 2,000, even more preferably 500 to 1,500, and particularly preferably 700 to 1,000. The molecular weight per urethane bond in the polyester polyurethane resin (A) of the present invention is determined by dividing the number average molecular weight Mn of the polyester polyurethane resin (A) by the average number of urethane bonds in the polyester polyurethane resin (A).
[0017] The polyester portion in the polyester polyurethane resin (A) is preferably formed from an acid component and an alcohol component. The acid component is preferably a polycarboxylic acid compound, more preferably a dicarboxylic acid compound. In addition, a sulfocarboxylic acid compound or the like can also be used as the acid component. Furthermore, an aromatic acid is preferably used as the acid component. As the alcohol component, a polyhydric alcohol compound is preferable, and a diol compound is more preferable. The polyester portion may be formed from a hydroxycarboxylic acid compound. When the total amount of all acid components constituting the polyester portion of the polyester polyurethane resin (A) is taken as 100 mol %, from the viewpoints of adhesion, heat resistance, and moist heat resistance, aromatic acids preferably account for 30 mol % or more of the total acid components, more preferably 45 mol % or more, and particularly preferably 60 mol % or more.
[0018] Examples of aromatic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, biphenyldicarboxylic acid, and 5-hydroxyisophthalic acid. In addition, aromatic dicarboxylic acids having a sulfonic acid group or a sulfonic acid group such as sulfoterephthalic acid, 5-sulfoisophthalic acid, 4-sulfophthalic acid, 4-sulfonaphthalene-2,7-dicarboxylic acid, 5-(4-sulfophenoxy)isophthalic acid, sulfoterephthalic acid, and / or their metal salts and ammonium salts, and aromatic oxycarboxylic acids such as p-hydroxybenzoic acid, p-hydroxyphenylpropionic acid, p-hydroxyphenylacetic acid, 6-hydroxy-2-naphthoic acid, and 4,4-bis(p-hydroxyphenyl)valeric acid can be mentioned. Among these, from the viewpoint of adhesiveness, it is preferable that the acid component contains terephthalic acid and / or isophthalic acid, and terephthalic acid and / or isophthalic acid are particularly preferable. Furthermore, the acid component may be a derivative of an acid compound such as an ester during resin synthesis.
[0019] Examples of other acid components include alicyclic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,2-cyclohexanedicarboxylic acid and their acid anhydrides, and aliphatic dicarboxylic acids such as succinic acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, and dimer acid.
[0020] On the other hand, preferred examples of the polyhydric alcohol component include an aliphatic diol compound, an alicyclic diol compound, an aromatic diol compound, and an ether bond-containing diol compound. Examples of the aliphatic diol compound include ethylene glycol, 1,2-propylene diol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, 2-butyl-2-ethyl-1,3-propanediol, hydroxypivalic acid neopentyl glycol ester, dimethylol heptane, and 2,2,4-trimethyl-1,3-pentanediol. Examples of the alicyclic diol compound include 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, tricyclodecanediol, tricyclodecanedimethylol, spiroglycol, hydrogenated bisphenol A, and ethylene oxide and propylene oxide adducts of hydrogenated bisphenol A. Examples of aromatic diol compounds include glycols obtained by adding 1 to several moles of ethylene oxide or propylene oxide to two phenolic hydroxyl groups of bisphenols, such as paraxylene glycol, metaxylene glycol, ortho-xylene glycol, 1,4-phenylene glycol, an ethylene oxide adduct of 1,4-phenylene glycol, bisphenol A, an ethylene oxide adduct of bisphenol A, and a propylene oxide adduct of bisphenol A. Examples of the ether bond-containing diol compound include diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, neopentyl glycol ethylene oxide adduct, and neopentyl glycol propylene oxide adduct. Among these diols, diols having a side chain such as neopentyl glycol and 2-butyl-2-ethyl-1,3-propanediol are preferred for reasons of compatibility with epoxy resins and solution stability. That is, the diol component constituting the polyester polyurethane resin (A) preferably contains a diol having a side chain from the viewpoints of compatibility with epoxy resins and the like and solution stability. Among them, from the viewpoints of compatibility with epoxy resins, solution stability, and electrical conductivity, it is more preferable that the chain extender constituting the polyester polyurethane resin (A) contains a diol having a side chain. That is, from the viewpoints of compatibility with epoxy resins, solution stability, and electrical conductivity, it is more preferable that the polyester polyurethane resin (A) is a resin obtained by reacting at least a polyester polyol, a polyisocyanate, and a diol having a side chain as raw materials.
[0021] In addition, hydroxycarboxylic acid compounds having a hydroxy group and a carboxy group in their molecular structure can also be used as polyester raw materials, and examples of such compounds include 5-hydroxyisophthalic acid, p-hydroxybenzoic acid, p-hydroxyphenethyl alcohol, p-hydroxyphenylpropionic acid, p-hydroxyphenylacetic acid, 6-hydroxy-2-naphthoic acid, and 4,4-bis(p-hydroxyphenyl)valeric acid.
[0022] As a component constituting the polyester portion of the polyester polyurethane resin (A), about 0.1 mol % to 5 mol % of trifunctional or higher polycarboxylic acids and / or polyols may be copolymerized with respect to the total acid components or total polyhydric alcohol components constituting the polyester portion, if necessary, for the purpose of introducing a branched skeleton. In particular, when a cured layer is obtained by reacting with a curing agent, the introduction of a branched skeleton increases the terminal group concentration (reaction points) of the resin, and a cured layer with high crosslink density can be obtained. In this case, examples of polycarboxylic acids having three or more functional groups include trimellitic acid, trimesic acid, ethylene glycol bis(anhydrotrimellitate), glycerol tris(anhydrotrimellitate), trimellitic anhydride, pyromellitic anhydride (PMDA), oxydiphthalic dianhydride (ODPA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 3,3',4,4'-diphenyltetracarboxylic dianhydride (BPDA), 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (DSDA), 4,4'-(hexafluoroisopropylidene)diphthalic dianhydride (6FDA), 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride (BSAA), and the like. On the other hand, examples of polyols having three or more functional groups include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and the like. When a trifunctional or higher functional polycarboxylic acid and / or polyol is used, it is preferable to copolymerize it in an amount of preferably 0.1 mol % to 5 mol %, more preferably 0.1 mol % to 3 mol %, based on the total acid components or total polyhydric alcohol components.
[0023] The polyester portion of the polyester polyurethane resin (A) may be subjected to acid addition in an amount of about 0.1 mol % to 10 mol % based on the total acid components or polyhydric alcohol components constituting the polyester portion for the purpose of introducing a carboxy group as necessary. When a monocarboxylic acid, dicarboxylic acid, or polyfunctional carboxylic acid compound is used for acid addition, a decrease in molecular weight occurs due to ester exchange, so it is preferable to use an acid anhydride. Examples of acid anhydrides that can be used include succinic anhydride, maleic anhydride, orthophthalic acid, 2,5-norbornene dicarboxylic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride (PMDA), oxydiphthalic dianhydride (ODPA), 3,3',4,4'-benzophenone tetracarboxylic dianhydride (BTDA), 3,3',4,4'-diphenyl tetracarboxylic dianhydride (BPDA), 3,3',4,4'-diphenyl sulfone tetracarboxylic dianhydride (DSDA), 4,4'-(hexafluoroisopropylidene) diphthalic dianhydride (6FDA), and 2,2'-bis[(dicarboxyphenoxy)phenyl]propane dianhydride (BSAA). Acid addition can be carried out directly in bulk after polyester polycondensation, or by dissolving the polyester and then adding the acid. The reaction in bulk is fast, but adding a large amount of acid can cause gelation, and the reaction is carried out at high temperatures, so care must be taken to prevent oxidation by blocking oxygen gas. On the other hand, acid addition in solution is slow, but can stably introduce a large amount of carboxyl groups.
[0024] The polyisocyanate used in the production of the polyester polyurethane resin (A) may be one of diisocyanates, their dimers (uretdione), their trimers (isocyanurates, triol adducts, biuret), etc., or a mixture of two or more of them. For example, the diisocyanate component may be 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, p-phenylene diisocyanate, diphenylmethane diisocyanate, m-phenylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, tetramethylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 1,5-naphthalene ...4-tolylene diisocyanate, p-phenylene diisocyanate, diphenylmethane diisocyanate, m-phenylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, tetramethylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 1,5-naphthalene diisocyanate, 2,6-tolylene diisocyanate, p-phenylene diisocyanate, diphenylmethane diisocyanate, m-phenylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, tetramethylene diisocyanate, 3, Examples of the diisocyanates include 2,6-naphthalene diisocyanate, 4,4'-diisocyanate diphenyl ether, m-xylylene diisocyanate, 1,3-diisocyanate methylcyclohexane, 1,4-diisocyanate methylcyclohexane, 4,4'-diisocyanate cyclohexane, 4,4'-diisocyanate cyclohexylmethane, isophorone diisocyanate, dimer acid diisocyanate, and norbornene diisocyanate. Among these, from the viewpoint of transparency, aliphatic or alicyclic diisocyanates are preferred. Furthermore, hexamethylene diisocyanate and isophorone diisocyanate are particularly preferred for ease of availability and economic reasons.
[0025] In producing the polyester polyurethane resin (A), a chain extender may be used, if necessary. Examples of chain extenders include the diol compounds already described as components of the polyester portion, and compounds having one carboxy group and two hydroxy groups, such as 2,2-bis(hydroxymethyl)propionic acid and 2,2-bis(hydroxymethyl)butyric acid. Among these, as the chain extender, from the viewpoint of electrical conductivity, a diol compound is preferable, a diol compound having a side chain is more preferable, and a diol compound having a branched chain is particularly preferable. That is, from the viewpoint of electrical conductivity, the diol component constituting the polyester polyurethane resin (A) preferably contains a diol having a side chain, and particularly preferably contains a diol compound having a branched chain. From the viewpoint of electrical conductivity, the diol compound having a side chain preferably contains at least one compound selected from the group consisting of neopentyl glycol, 2-butyl-2-ethyl-1,3-propanediol, and 2,2-bis(hydroxymethyl)propionic acid, and particularly preferably contains at least one compound selected from the group consisting of neopentyl glycol and 2-butyl-2-ethyl-1,3-propanediol and 2,2-bis(hydroxymethyl)propionic acid.
[0026] The method for producing the polyester polyurethane resin (A) is not particularly limited, and a known method can be used. For example, the polyester polyol and the polyisocyanate, and if necessary, the chain extender, may be charged in a reaction vessel all at once, or may be charged in portions. In any case, the ratio of the functional group of the isocyanate group / hydroxy group is preferably 0.9 or more and 1.1 or less, more preferably 0.98 or more and 1.02 or less, and particularly preferably 1, with respect to the total hydroxyl value of the polyester polyol and the chain extender in the system and the total isocyanate group of the polyisocyanate. This reaction can be produced by reacting in the presence or absence of a solvent inert to the isocyanate group. Examples of the solvent include ester solvents (ethyl acetate, butyl acetate, ethyl butyrate, etc.), ether solvents (dioxane, tetrahydrofuran, diethyl ether, etc.), ketone solvents (cyclohexanone, methyl ethyl ketone, methyl isobutyl ketone, etc.), aromatic hydrocarbon solvents (benzene, toluene, xylene, etc.), and mixed solvents thereof, and from the viewpoint of reducing the environmental load, ethyl acetate and / or methyl ethyl ketone are preferred. The reaction apparatus is not limited to a reaction vessel equipped with a stirrer, and a mixing and kneading apparatus such as a kneader or a twin-screw extruder can also be used.
[0027] In order to promote the urethane reaction, catalysts used in ordinary urethane reactions can be used, such as tin-based catalysts (trimethyltin laurate, dimethyltin dilaurate, trimethyltin hydroxide, dimethyltin dihydroxide, stannous octoate, etc.), lead-based catalysts (red oleate, red-2-ethylhexoate, etc.), and amine-based catalysts (triethylamine, tributylamine, morpholine, diazabicyclooctane, diazabicycloundecene, etc.).
[0028] From the viewpoints of adhesion, electrical conductivity, and heat resistance, the glass transition temperature (Tg) of the polyester portion in the polyester polyurethane resin (A) is preferably 40°C to 150°C, more preferably 45°C to 120°C, even more preferably 50°C to 90°C, and particularly preferably 60°C to 70°C. From the viewpoints of adhesion, conductivity, and heat resistance, the glass transition temperature (Tg) of the polyester polyurethane resin (A) is preferably 30°C to 150°C, more preferably 40°C to 140°C, and particularly preferably 50°C to 120°C.
[0029] From the viewpoints of electrical conductivity and heat resistance, the number average molecular weight (Mn) of the polyester polyurethane resin (A) is preferably from 5,000 to 100,000, more preferably from 10,000 to 80,000, further preferably from 20,000 to 60,000, and particularly preferably from 25,000 to 50,000. In the present invention, the number average molecular weight (Mn) and weight average molecular weight (Mw) of the resin can be obtained by gel permeation chromatography (GPC).
[0030] From the viewpoints of adhesion and conductivity, the acid value of the polyester polyurethane resin (A) is preferably 0 mgKOH / g to 50 mgKOH / g, more preferably 0.1 mgKOH / g to 20 mgKOH / g, further preferably 0.1 mgKOH / g to 5 mgKOH / g, and particularly preferably 1.0 mgKOH / g to 5.0 mgKOH / g. From the viewpoint of heat resistance, the acid value of the polyester polyurethane resin (A) is preferably 20 mgKOH / g or less, and particularly preferably 5 mgKOH / g or less. In the present invention, the acid value of a resin is measured by neutralizing a sample with a potassium hydroxide benzyl alcohol solution using a phenolphthalein solution as an indicator to determine the acid value.
[0031] Furthermore, from the viewpoints of adhesion, electrical conductivity, and heat resistance, the polyester polyurethane resin (A) preferably contains a polyester polyurethane resin having a polyester structure with a number average molecular weight of 1,000 to 50,000, more preferably contains a polyester polyurethane resin having a polyester structure with a number average molecular weight of 2,000 to 40,000, even more preferably contains a polyester polyurethane resin having a polyester structure with a number average molecular weight of 3,000 to 30,000, and particularly preferably contains a polyester polyurethane resin having a polyester structure with a number average molecular weight of 8,000 to 30,000.
[0032] The resin composition of the present invention may contain one type of polyester polyurethane resin (A) alone, or may contain two or more types. From the viewpoints of adhesion, electrical conductivity, and heat resistance, the content of the polyester polyurethane resin (A) is preferably 30% by mass to 99% by mass, more preferably 50% by mass to 95% by mass, and particularly preferably 70% by mass to 90% by mass, based on the total amount of resin solids excluding the filler component in the resin composition. The resin solids excluding the filler components refer to the resin components (such as the polyester polyurethane resin (A) and the epoxy resin (B)) which are non-volatile components excluding the organic filler, metal filler, and inorganic filler other than the metal filler described below, and the curing accelerator described below. The resin components and the curing accelerator may be solid or liquid at room temperature (25°C). Furthermore, from the viewpoints of adhesion, conductivity, and heat resistance, the content of the polyester polyurethane resin (A) in the resin composition of the present invention is preferably 10% by mass to 70% by mass based on the total amount of resin solids excluding the filler component.
[0033] <Epoxy resin (B)> The resin composition of the present invention contains an epoxy resin (B). The epoxy resin (B) is a component that imparts adhesiveness and heat resistance to the cured portion after adhesion. The epoxy resin (B) in the present invention includes not only high molecular weight compounds having an epoxy group, but also low molecular weight compounds having an epoxy group. The number of epoxy groups in the epoxy resin (B) is preferably 2 or more. Examples of the epoxy resin (B) include glycidyl esters such as orthophthalic acid diglycidyl ester, isophthalic acid diglycidyl ester, terephthalic acid diglycidyl ester, p-hydroxybenzoic acid diglycidyl ester, tetrahydrophthalic acid diglycidyl ester, succinic acid diglycidyl ester, adipic acid diglycidyl ester, sebacic acid diglycidyl ester, and trimellitic acid triglycidyl ester; diglycidyl ether of bisphenol A and its oligomers, ethylene glycol diglycidyl ether, and propylene glycol diglycidyl ether. glycidyl ethers such as 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, pentaerythritol tetraglycidyl ether, tetraphenylglycidyl ether ethane, triphenylglycidyl ether ethane, polyglycidyl ether of sorbitol, and polyglycerol polyglycidyl ether; and novolac epoxy resins such as phenol novolac epoxy resin, o-cresol novolac epoxy resin, and bisphenol A novolac epoxy resin. In addition, brominated bisphenol A type epoxy resins, phosphorus-containing epoxy resins, dicyclopentadiene skeleton-containing epoxy resins, naphthalene skeleton-containing epoxy resins, anthracene type epoxy resins, tertiary butyl catechol type epoxy resins, biphenyl type epoxy resins, and bisphenol S type epoxy resins that have been imparted with flame retardancy can also be used. Among these, from the viewpoints of adhesion and heat resistance, the epoxy resin (B) preferably contains a bisphenol type epoxy resin and / or a novolac type epoxy resin, and more preferably contains a bisphenol type epoxy resin and a phenol novolac type epoxy resin.
[0034] In the present invention, in order to achieve high heat resistance after curing, it is preferable that the epoxy resin (B) contains a compound having three or more epoxy groups in one molecule. When such a compound is used, the crosslinking reactivity with the polyester polyurethane resin (A) becomes higher than when an epoxy resin having two epoxy groups is used, and sufficient heat resistance is obtained. From the viewpoint of heat resistance, the content of the compound having three or more epoxy groups in one molecule in the epoxy resin (B) is preferably 15 mass % or more, more preferably 20 mass % or more, and particularly preferably 25 mass % or more, based on the total mass of the epoxy resin (B).
[0035] The resin composition of the present invention may contain one type of epoxy resin (B) alone, or may contain two or more types of epoxy resin (B). From the viewpoints of adhesion, conductivity, and heat resistance, the content of the epoxy resin (B) is preferably 0.5 parts by mass to 60 parts by mass, more preferably 1 part by mass to 30 parts by mass, and particularly preferably 3 parts by mass to 25 parts by mass, per 100 parts by mass of the polyester polyurethane resin (A).
[0036] <Organic filler> The resin composition of the present invention preferably contains an organic filler from the viewpoints of the elongation property, electrical conductivity, and moist heat resistance of the resulting cured product. Examples of the organic filler include (meth)acrylic resin particles, polybutadiene particles, nylon particles, polyolefin particles, polyester particles, polycarbonate particles, polyvinyl alcohol particles, polyvinyl ether particles, polyvinyl butyral particles, silicone rubber particles, polyurethane particles, phenolic resin particles, and polytetrafluoroethylene particles. The present inventors have found that when an organic filler is mixed with a polyester polyurethane resin (A) and an epoxy resin (B), the compatibility of these resins is further improved. Furthermore, from the viewpoint of further improving the compatibility and liquid stability of these resins, silicone particles, polybutadiene particles, (meth)acrylic resin particles, or polyurethane particles are particularly preferred as the organic filler. From the viewpoint of electrical conductivity, (meth)acrylic resin particles or polyurethane particles are preferred.
[0037] The average particle size of the organic filler is not particularly limited, but from the viewpoints of coatability and coat thickness adjustment, it is preferably 0.5 μm to 50 μm, and more preferably 1 μm to 30 μm.
[0038] The resin composition of the present invention may contain one type of organic filler alone, or may contain two or more types of organic fillers. From the viewpoints of adhesion, conductivity, and curability, the content of the organic filler in the resin composition is preferably 1 part by mass to 50 parts by mass, more preferably 5 parts by mass to 40 parts by mass, and particularly preferably 10 parts by mass to 20 parts by mass, per 100 parts by mass of the total amount of resin solids excluding the filler component.
[0039] <Metal filler> From the viewpoints of electrical conductivity and heat resistance, the resin composition of the present invention preferably contains a metal filler. From the viewpoints of electrical conductivity and heat resistance, the metal filler is preferably an electrically conductive filler, and more preferably a metal particle made of an electrically conductive metal such as gold, platinum, silver, copper, or nickel, or an alloy thereof. In addition, from the viewpoint of cost reduction, particles having a core of metal or resin, and a coating layer formed of a highly conductive material, rather than particles of a single composition, are also preferable. The core is preferably made of at least one material selected from the group consisting of nickel, silica, copper, and resin, and more preferably made of an electrically conductive metal or an alloy thereof. The coating layer is preferably a layer made of a material having excellent electrical conductivity, and is preferably a layer made of an electrically conductive metal or a conductive polymer. Examples of conductive metals include gold, platinum, silver, tin, manganese, and indium, as well as alloys thereof. Examples of conductive polymers include polyaniline and polyacetylene. Among these, silver is preferred in terms of electrical conductivity.
[0040] From the viewpoints of cost and electrical conductivity, the particles consisting of a core and a coating layer preferably have the coating layer in a ratio of 1 part by mass to 40 parts by mass, and more preferably 5 parts by mass to 30 parts by mass, per 100 parts by mass of the core.
[0041] The particles consisting of the core and the coating layer are preferably particles in which the coating layer completely covers the core. However, in reality, there are cases where a part of the core is exposed. Even in such cases, if 70% or more of the core surface area is covered with a conductive material, the conductivity is easily maintained.
[0042] The shape of the metal filler is not limited as long as the desired electrical conductivity is obtained. Specifically, for example, a spherical, flake, leaf, dendritic, plate, needle, rod, or grape shape is preferable.
[0043] From the viewpoints of electrical conductivity and storage stability, the average particle size of the metal filler is preferably from 1 μm to 100 μm, more preferably from 3 μm to 50 μm, and particularly preferably from 4 μm to 15 μm. The average particle size of the particles in this disclosure is the D50 average particle size obtained by measuring each conductive fine particle powder with a tornado dry powder sample module using a laser diffraction / scattering particle size distribution analyzer LS 13320 (manufactured by Beckman Coulter, Inc.), and the average particle size of the particle diameter at which the cumulative value of the particles is 50% is used. The refractive index was set to 1.6. The average particle size of the metal filler can also be determined by averaging about 20 randomly selected particles in an enlarged image (approximately 1,000 to 10,000 times) taken with an electron microscope. In this case, the average particle size is also preferably 1 μm to 100 μm, more preferably 3 μm to 50 μm. In addition, when the metal filler has a long axis direction and a short axis direction (e.g., rod-shaped particles), the average particle size is calculated based on the length in the long axis direction.
[0044] The resin composition of the present invention may contain one type of metal filler alone, or may contain two or more types of metal fillers. From the viewpoints of electrical conductivity, heat resistance, and storage stability, the content of the metal filler in the resin composition is preferably 1 part by mass to 500 parts by mass, more preferably 10 parts by mass to 350 parts by mass, and particularly preferably 10 parts by mass to 50 parts by mass, per 100 parts by mass of the total amount of resin solids excluding the filler component.
[0045] The resin composition of the present invention may contain additives other than the above-mentioned components. Other additives may include thermoplastic resins other than those mentioned above, tackifiers, flame retardants, curing agents, curing accelerators, coupling agents, heat aging inhibitors, leveling agents, defoamers, inorganic fillers, solvents, and the like, to the extent that they do not affect the functions of the resin composition.
[0046] Examples of the other thermoplastic resins include phenoxy resins, polyester resins, polycarbonate resins, polyphenylene oxide resins, polyurethane resins, polyacetal resins, polyethylene-based resins, polypropylene-based resins, polyvinyl-based resins, etc. These thermoplastic resins may be used alone or in combination of two or more.
[0047] Examples of the tackifier include coumarone-indene resin, terpene resin, terpene-phenol resin, rosin resin, pt-butylphenol-acetylene resin, phenol-formaldehyde resin, xylene-formaldehyde resin, petroleum-based hydrocarbon resin, hydrogenated hydrocarbon resin, turpentine-based resin, etc. These tackifiers may be used alone or in combination of two or more.
[0048] The flame retardant may be either an organic flame retardant or an inorganic flame retardant. Examples of organic flame retardants include phosphorus-based flame retardants such as melamine phosphate, melamine polyphosphate, guanidine phosphate, guanidine polyphosphate, ammonium phosphate, ammonium polyphosphate, ammonium amido phosphate, ammonium amido polyphosphate, carbamate phosphate, carbamate polyphosphate, aluminum trisdiethylphosphinate, aluminum trismethylethylphosphinate, aluminum trisdiphenylphosphinate, zinc bisdiethylphosphinate, zinc bismethylethylphosphinate, zinc bisdiphenylphosphinate, titanyl bisdiethylphosphinate, titanium tetrakisdiethylphosphinate, titanyl bismethylethylphosphinate, titanium tetrakismethylethylphosphinate, titanyl bisdiphenylphosphinate, and titanium tetrakisdiphenylphosphinate; nitrogen-based flame retardants such as triazine-based compounds such as melamine, melam, and melamine cyanurate, cyanuric acid compounds, isocyanuric acid compounds, triazole-based compounds, tetrazole compounds, diazo compounds, and urea; and silicon-based flame retardants such as silicone compounds and silane compounds. Examples of inorganic flame retardants include metal hydroxides such as aluminum hydroxide, magnesium hydroxide, zirconium hydroxide, barium hydroxide, and calcium hydroxide; metal oxides such as tin oxide, aluminum oxide, magnesium oxide, zirconium oxide, zinc oxide, molybdenum oxide, and nickel oxide; zinc carbonate, magnesium carbonate, calcium carbonate, barium carbonate, zinc borate, and hydrated glass. These flame retardants may be used alone or in combination of two or more.
[0049] The curing agent is a component for forming a crosslinked structure by reaction with the epoxy resin (B), and examples thereof include amine-based curing agents such as aliphatic diamines, aliphatic polyamines, cyclic aliphatic diamines, and aromatic diamines, polyamidoamine-based curing agents, acid-based curing agents such as aliphatic polycarboxylic acids, alicyclic polycarboxylic acids, aromatic polycarboxylic acids, and acid anhydrides thereof, basic active hydrogen-based curing agents such as dicyandiamide and organic acid dihydrazides, polymercaptan-based curing agents, novolac resin-based curing agents, urea resin-based curing agents, and melamine resin-based curing agents. These curing agents may be used alone or in combination of two or more.
[0050] Examples of the aliphatic diamine curing agent include ethylenediamine, 1,3-diaminopropane, 1,4-diaminobutane, hexamethylenediamine, polymethylenediamine, polyetherdiamine, 2,5-dimethylhexamethylenediamine, and trimethylhexamethylenediamine.
[0051] Examples of the aliphatic polyamine curing agent include diethylenetriamine, iminobis(hexamethylene)triamine, trihexatetramine, tetraethylenepentamine, aminoethylethanolamine, tri(methylamino)hexane, dimethylaminopropylamine, diethylaminopropylamine, and methyliminobispropylamine.
[0052] Examples of cyclic aliphatic diamine curing agents include benzenediamine, isophoronediamine, bis(4-amino-3-methyldicyclohexyl)methane, diaminodicyclohexylmethane, bis(aminomethyl)cyclohexane, N-ethylaminopiperazine, 3,9-bis(3-aminopropyl)2,4,8,10-tetraoxaspiro[5.5]undecane, and hydrogenated metaxylylenediamine.
[0053] Examples of the aromatic diamine curing agent include metaphenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, diaminodiethyldiphenylmethane, and metaxylylenediamine.
[0054] Examples of the aliphatic polyvalent carboxylic acid-based hardener and the acid anhydride-based hardener include succinic acid, adipic acid, dodecenyl succinic anhydride, polyadipic anhydride, polyazelaic anhydride, and polysebacic anhydride.
[0055] Examples of alicyclic polyvalent carboxylic acid curing agents and acid anhydride curing agents include methyltetrahydrophthalic acid, methylhexahydrophthalic acid, methylhimic acid, hexahydrophthalic acid, tetrahydrophthalic acid, trialkyltetrahydrophthalic acid, methylcyclodicarboxylic acid, and acid anhydrides thereof.
[0056] Examples of aromatic polyvalent carboxylic acid-based curing agents and acid anhydride-based curing agents include phthalic acid, trimellitic acid, pyromellitic acid, benzophenone tetracarboxylic acid, ethylene glycol glycol bistrimellitic acid, glycerol tristrimellitic acid, and acid anhydrides thereof.
[0057] Examples of the polymercaptan-based curing agent include mercapto-modified epoxy resins and mercaptopropionic acid esters.
[0058] Examples of the novolac-based hardener include a phenol novolac-based hardener and a cresol novolac-based hardener.
[0059] When the resin composition of the present invention contains the curing agent, the content of the curing agent is set so that the functional group equivalent thereof is preferably in the range of 0.2 to 2.5 molar equivalents, more preferably in the range of 0.4 to 2.0 molar equivalents, relative to 1 molar equivalent of the epoxy group of the epoxy resin (B), from the viewpoints of adhesiveness and heat resistance.
[0060] The curing accelerator is a component used for the purpose of accelerating the reaction of the epoxy resin (B), and examples of the curing accelerator that can be used include tertiary amine curing accelerators, tertiary amine salt curing accelerators, and imidazole curing accelerators. These curing accelerators may be used alone or in combination of two or more.
[0061] Examples of the tertiary amine curing accelerator include benzyldimethylamine, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, tetramethylguanidine, triethanolamine, N,N'-dimethylpiperazine, triethylenediamine, and 1,8-diazabicyclo[5.4.0]undecene.
[0062] Examples of the tertiary amine salt curing accelerator include the formate, octylate, p-toluenesulfonate, o-phthalate, phenol salt, and phenol novolac resin salt of 1,8-diazabicyclo[5.4.0]undecene; and the formate, octylate, p-toluenesulfonate, o-phthalate, phenol salt, and phenol novolac resin salt of 1,5-diazabicyclo[4.3.0]nonene.
[0063] Imidazole-based curing accelerators include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-methyl-4-ethylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'- undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and the like.
[0064] When the resin composition of the present invention contains a curing accelerator, the content of the curing accelerator is preferably 1 to 10 parts by mass, and more preferably 2 to 5 parts by mass, per 100 parts by mass of the epoxy resin (B) from the viewpoints of adhesion and heat resistance.
[0065] Examples of the coupling agent include silane-based coupling agents such as vinyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatepropyltriethoxysilane, and imidazolesilane; titanate-based coupling agents; aluminate-based coupling agents; and zirconium-based coupling agents. These may be used alone or in combination of two or more.
[0066] Examples of the heat aging inhibitor include phenol-based antioxidants such as 2,6-di-tert-butyl-4-methylphenol, n-octadecyl-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate, and tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane; sulfur-based antioxidants such as dilauryl-3,3'-thiodipropionate and dimyristyl-3,3'-dithiopropionate; and phosphorus-based antioxidants such as trisnonylphenyl phosphite and tris(2,4-di-tert-butylphenyl)phosphite. These may be used alone or in combination of two or more.
[0067] Examples of the inorganic filler include powders made of calcium carbonate, titanium oxide, aluminum oxide, zinc oxide, carbon black, talc, silica, etc. These may be used alone or in combination of two or more.
[0068] The resin composition of the present invention can be prepared by mixing the polyester polyurethane resin (A) and the epoxy resin (B), and, if necessary, other components. Since the resin composition of the present invention is preferably used in the state of a solution or dispersion, it preferably contains a solvent. Examples of the solvent include alcohols such as methanol, ethanol, isopropyl alcohol, n-propyl alcohol, isobutyl alcohol, n-butyl alcohol, benzyl alcohol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, diethylene glycol monomethyl ether, and diacetone alcohol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl amyl ketone, cyclohexanone, and isophorone; aromatic hydrocarbons such as toluene, xylene, ethylbenzene, and mesitylene; esters such as methyl acetate, ethyl acetate, ethylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; and aliphatic hydrocarbons such as hexane, heptane, cyclohexane, and methylcyclohexane. These solvents may be used alone or in combination of two or more. When the resin composition of the present invention is a solution or dispersion containing a solvent, coating on an adherend and formation of a resin composition layer can be smoothly performed, and a resin composition layer of a desired thickness can be easily obtained.
[0069] When the resin composition of the present invention contains a solvent, from the viewpoint of workability including film-forming property, the solvent is used so that the solid content concentration is preferably in the range of 3 mass % to 80 mass %, more preferably 10 mass % to 50 mass %.
[0070] Suitable adherends for the resin composition of the present invention are objects made of polymeric materials such as polyimide resins, polyether ether ketone resins, polyphenylene sulfide resins, aramid resins, and liquid crystal polymers; and metal materials such as copper, aluminum, and stainless steel. The shape of the adherend is not particularly limited. Two members made of the same material or different materials as the adherend can be bonded together with the resin composition of the present invention to produce an integrated composite. In addition, products having a resin composition layer with adhesive properties, such as the following coverlay films and bonding sheets, can be produced.
[0071] (Laminate with Resin Composition Layer, and Laminate) The laminate with a resin composition layer of the present invention is a laminate having a resin composition layer made of the resin composition of the present invention, a B-stage resin composition layer obtained by partially curing the resin composition of the present invention, or a cured layer obtained by curing the resin composition of the present invention (hereinafter collectively referred to as "each resin composition layer"). Of these, a laminate having the B-stage resin composition layer or the cured layer is preferred. The laminate with a resin composition layer of the present invention preferably includes each resin composition layer and a substrate film in contact with at least one surface of each of the resin composition layers. In the present invention, the resin composition layer being in the B stage refers to a semi-cured state in which a part of the resin composition layer has begun to cure, and the curing of the resin composition layer can be further promoted by heating or the like. When a resin composition containing a solvent is used, the resin composition layer made of the resin composition of the present invention is preferably a layer obtained by removing at least a part of the solvent from the resin composition of the present invention. The laminate of the present invention is a laminate having a cured layer formed by curing a resin composition comprising the resin composition of the present invention, and preferably includes a cured layer formed by curing the resin composition of the present invention and a substrate in contact with at least one surface of the cured layer.
[0072] The laminate with a resin composition layer of the present invention and the laminate of the present invention preferably have a substrate, and more preferably have each resin composition layer made of the resin composition of the present invention on the substrate. The substrate is not particularly limited, and any known substrate can be used. The substrate is preferably a film-like substrate (substrate film). The substrate film is preferably a resin film, more preferably a polyimide film or an aramid film, and particularly preferably a polyimide film. The polyimide film or aramid film is not particularly limited as long as it has electrical insulation properties, and may be a film made of only a polyimide resin or an aramid resin, or a film containing the resin and an additive, and the side on which the resin composition layer is formed may be subjected to a surface treatment. Moreover, a peelable film can also be used as the base film. The thickness of the substrate is not particularly limited, but is preferably 3 μm to 125 μm. The thickness of the resin composition layer is preferably from 5 μm to 50 μm, and more preferably from 10 μm to 40 μm.
[0073] As a method for producing a laminate with a resin composition layer of the present invention, for example, the resin composition of the present invention containing a solvent is applied to the surface of a base film such as a polyimide film to form a resin composition layer, and then at least a portion of the solvent is removed from the resin composition layer to produce a laminate having a resin composition layer. Furthermore, during the process of removing the solvent, a portion of the resin composition layer begins to harden, thereby producing a laminate having a resin composition layer in a B-stage state. The drying temperature when removing the solvent is preferably from 40°C to 250°C, and more preferably from 70°C to 170°C. The drying is carried out by passing the laminate coated with the resin composition through a furnace in which hot air drying, far infrared heating, high frequency induction heating, or the like is performed. The laminate with a resin composition layer of the present invention may further have a release film on the surface of each resin composition layer for storage or the like, if necessary. The release film may be a known film such as a polyethylene terephthalate film, a polyethylene film, a polypropylene film, silicone release treated paper, a polyolefin resin coated paper, a polymethylpentene (TPX) film, or a fluorine-based resin film.
[0074] The thickness of the B-stage resin composition layer is preferably 3 μm to 100 μm, more preferably 5 μm to 70 μm, further preferably 5 μm to 50 μm, and particularly preferably 10 μm to 40 μm. The thickness of the base film and each resin composition layer is selected depending on the application, but the base film tends to be thinner in order to improve electrical properties. The preferred thickness of the base film is the same as the preferred thickness of the base material described above. In the laminate with a resin composition layer of the present invention, the ratio (A / B) of the thickness (A) of each resin composition layer to the thickness (B) of the base film is preferably 1 or more and 10 or less, and more preferably 1 or more and 5 or less. Furthermore, it is preferable that the thickness of each resin composition layer is thicker than the thickness of the base film.
[0075] As a method for producing the laminate of the present invention, for example, the resin composition of the present invention containing a solvent is applied to the surface of a substrate film, and then dried in the same manner as in the case of the laminate with a resin composition layer of the present invention, and then the surface of the formed resin composition layer is brought into surface contact with an adherend, and lamination, for example, thermal lamination is performed at 80° C. to 150° C. Next, this laminate (substrate film / resin composition layer / adherend) is heated and pressed, and further the resin composition layer is cured by after-curing to form a cured layer. The conditions for the thermocompression bonding are not particularly limited as long as the bonding is possible, but are preferably 150°C to 200°C, 1 MPa to 3 MPa pressure, and 1 minute to 60 minutes. The conditions for the aftercure are not particularly limited, but are preferably 100°C to 200°C, 30 minutes to 4 hours. The thickness of the cured layer is preferably from 3 μm to 100 μm, more preferably from 5 μm to 70 μm, further preferably from 5 μm to 50 μm, and particularly preferably from 10 μm to 40 μm. The adherend is not particularly limited, and examples thereof include those mentioned above. Among them, metal adherends are preferred, copper foil or plated copper foil is more preferred, and gold-plated copper foil is particularly preferred. The shape and size of the adherend are not particularly limited, and any known shape and size can be used.
[0076] One embodiment of the laminate of the present invention is a flexible copper-clad laminate. That is, the flexible copper-clad laminate of the present invention is preferably a flexible copper-clad laminate comprising a copper foil, a cured layer obtained by curing the resin composition of the present invention, and a substrate, more preferably a flexible copper-clad laminate comprising at least a copper foil, a cured layer obtained by curing the resin composition of the present invention, and a substrate, and particularly preferably a flexible copper-clad laminate comprising at least a copper foil, a cured layer obtained by curing the resin composition of the present invention, and a polyimide film or an aramid film. In the flexible copper-clad laminate of the present invention, the cured layer and the copper foil may be formed on both sides of the substrate, for example, a polyimide film or an aramid film. Since the resin composition of the present invention has excellent adhesion to an article containing copper, the flexible copper-clad laminate of the present invention has excellent stability as an integrated product. As the substrate in the flexible copper-clad laminate of the present invention, those mentioned above in relation to the laminate are preferably used.
[0077] The configuration of the polyimide film or aramid film is the same as that of the polyimide film or aramid film in the laminate of the present invention described above. The thickness of the hardened layer is not particularly limited, but is preferably from 3 μm to 50 μm, and more preferably from 10 μm to 40 μm. The copper foil is not particularly limited, and electrolytic copper foil, rolled copper foil, etc. can be used. Additionally, the copper foil may be plated with known metals or alloys such as gold or silver.
[0078] Another embodiment of the laminate of the present invention is a flexible flat cable. In other words, the flexible flat cable of the present invention is preferably a flexible flat cable comprising a copper wiring, a cured layer obtained by curing the resin composition of the present invention, and a coating material, and more preferably a flexible flat cable comprising a copper wiring, a cured layer obtained by curing the resin composition of the present invention, and a coating material, with the cured layer being between the copper wiring and the coating material. Since the resin composition of the present invention has excellent adhesion to articles containing copper, the flexible flat cable of the present invention has excellent stability as an integrated product. The thickness, length, and cross-sectional shape of the copper wiring are not particularly limited and may be appropriately selected as desired. Among them, a copper wiring having a rectangular parallelepiped cross section is preferable. The material for the covering material is not particularly limited as long as it is an insulating material, but is preferably a resin, more preferably a thermoplastic resin. Specific examples of the material for the covering material include polyester resin, polyimide resin, polyphenylene sulfide resin, and the like. Preferred examples of the polyester resin include polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polybutylene naphthalate, polytrimethylene terephthalate, and polytrimethylene naphthalate. Furthermore, there are no particular limitations on the thickness, length, cross-sectional shape, and other configurations of the covering material, and these can be appropriately selected as desired. The thickness of the hardened layer is not particularly limited, but is preferably from 3 μm to 50 μm, and more preferably from 10 μm to 40 μm.
[0079] The method for producing the flexible flat cable of the present invention is not particularly limited, but a preferred example is a method in which a laminate is produced in the form of resin film / resin composition layer / copper wiring / resin composition layer / another resin film, the laminate is thermocompression-bonded at 80° C. to 150° C., and the resin composition layer is hardened by after-curing. The after-curing conditions can be, for example, 100° C. to 200° C. and 30 minutes to 4 hours. The thickness of the resin film is not particularly limited, but may be from 9 μm to 50 μm.
[0080] Examples of the laminate with a resin composition layer of the present invention include a bonding film, a coverlay film, and an electromagnetic wave shielding film.
[0081] -Bonding film- The bonding film of the present invention has a layer made of the resin composition of the present invention, or a B-stage resin composition layer formed by partially curing the resin composition of the present invention, of which the B-stage resin composition layer is preferred. The bonding film of the present invention preferably includes a release film in contact with at least one surface of the resin composition layer or the B-stage resin composition layer. The bonding film of the present invention may have an embodiment in which a resin composition layer is provided between two release films. As the release film, known films as described above are used. The release film preferably has a thickness of 20 μm to 100 μm. The thickness of the resin composition layer is preferably from 3 μm to 100 μm, and more preferably from 10 μm to 60 μm.
[0082] A preferred method for producing the bonding sheet of the present invention is, for example, to coat the surface of a release film with the resin composition of the present invention containing a solvent, and then drying in the same manner as in the case of the laminate with a resin composition layer of the present invention described above.
[0083] -Coverlay film- The coverlay film of the present invention has each resin composition layer of the present invention, and among these, a B-stage resin composition layer or a cured layer is preferred. The coverlay film of the present invention preferably has a base film other than a release film such as a polyimide film or an aramid film in contact with at least one surface of each resin composition layer. The coverlay film of the present invention may be in an embodiment in which a release film is provided on the side of each resin composition layer opposite the substrate film side. As the base film, known films as described above are used. The thickness of the base film is preferably 3 μm to 125 μm. The thickness of the resin composition layer is preferably from 3 μm to 100 μm, and more preferably from 10 μm to 60 μm.
[0084] A preferred method for producing the coverlay film of the present invention is, for example, to coat the surface of a base film with the resin composition of the present invention containing a solvent, and then drying the coated film in the same manner as in the case of the laminate with the resin composition layer of the present invention described above.
[0085] -Electromagnetic wave shielding film- The electromagnetic wave shielding film of the present invention has each of the resin composition layers described above, and among these, the B-stage resin composition layer or the cured layer is preferred. The electromagnetic wave shielding film of the present invention may also have a base film (including a release film) in contact with at least one surface of each resin composition layer. Moreover, the electromagnetic wave shielding film of the present invention preferably has each resin composition layer and a protective layer. The protective layer is not particularly limited as long as it is a layer made of an insulating resin composition, and any known layer can be used. The protective layer may also use the resin component used in the resin composition of the present invention. Furthermore, the protective layer may be formed of two or more layers having different compositions and hardness. Furthermore, the protective layer may contain, as necessary, a curing accelerator, a tackifier, an antioxidant, a pigment, a dye, a plasticizer, an ultraviolet absorber, an antifoaming agent, a leveling agent, a filler, a flame retardant, a viscosity adjuster, an antiblocking agent, and the like.
[0086] The thickness of each resin composition layer in the electromagnetic wave shielding film of the present invention is not particularly limited, but from the viewpoints of electrical conductivity and connectivity with a ground circuit, it is preferably 3 μm to 30 μm.
[0087] Next, a specific embodiment of the method for producing the electromagnetic wave shielding film of the present invention will be described. For example, a method can be mentioned in which a resin composition for a protective layer is coated and dried on one side of a peelable film to form a protective layer, and then the resin composition of the present invention is coated and dried on the protective layer to form a resin composition layer. By the production method as exemplified above, it is possible to obtain an electromagnetic wave shielding film having a laminated structure of each resin composition layer / protective layer / peelable film.
[0088] The resin composition layer and the protective layer can be provided by a conventionally known coating method, such as a gravure coating method, a kiss coating method, a die coating method, a lip coating method, a comma coating method, a blade coating method, a roll coating method, a knife coating method, a spray coating method, a bar coating method, a spin coating method, or a dip coating method.
[0089] The electromagnetic wave shielding film of the present invention can be adhered to a printed wiring board by, for example, heat pressing. Each resin composition layer becomes soft when heated and flows into the ground part provided on the printed wiring board when pressurized. This electrically connects the ground circuit and the conductive adhesive, thereby enhancing the shielding effect. EXAMPLES
[0090] The present invention will be specifically described below based on examples. Note that the present invention is not limited to these examples. In the following, "parts" and "%" mean "parts by mass" and "% by mass", respectively, unless otherwise specified.
[0091] 1.Raw materials 1-1. Polyester polyurethane resin (A) The polyesters used were either commercially available products or synthetic products. The commercially available products used were ARONMELT PES-360HVXM30 and ARONMELT PES-310S30 manufactured by Toagosei Co., Ltd. The number average molecular weight of PES-360HVXM30 was 20,000 and the glass transition temperature was 65°C. The number average molecular weight of PES-310S30 was 20,000 and the glass transition temperature was 8°C.
[0092] <Synthesis of polyester (PES-1)> A flask equipped with a stirrer, a nitrogen inlet tube, a distillation tube, and a thermometer was charged with 201 parts by mass of dimethyl terephthalate, 86 parts by mass of ethylene glycol, 140 parts by mass of neopentyl glycol, 0.9 parts by mass of trimethylolpropane, and 0.22 parts by mass of zinc acetate as a catalyst. The temperature was raised while introducing nitrogen, and methanol was distilled off at 150°C to 180°C. Then, 183 parts by mass of isophthalic acid, 0.6 parts by mass of trimethylolpropane, and 0.12 parts by mass of antimony trioxide were added, and water was distilled off at 180°C to 210°C. Subsequently, the pressure was gradually reduced, and the reaction was continued at 230°C and a reduced pressure of 200 Pa for 6 hours. The obtained polyester resin A had a number average molecular weight of 7,000 and a glass transition point of 60° C. The monomer composition by NMR analysis was terephthalic acid / isophthalic acid / ethylene glycol / neopentyl glycol=48 / 52 / 43 / 56 in molar ratio. 180 parts by mass of the synthesized polyester resin was taken, and 378 parts by mass of toluene and 42 parts by mass of methyl isobutyl ketone were added to prepare a polyester solution.
[0093] <Preparation of polyester polyurethane resins a1 to a9> The polyester polyurethane resins a1 to a9 obtained by the following method were used.
[0094] (1) Preparation of polyester polyurethane resin a1 In a flask equipped with a stirrer, a reflux dehydration device, and a distillation tube, 600 parts by mass of PES-360HVXM30, 100 parts by mass of toluene, and 20 parts by mass of neopentyl glycol were charged. After raising the temperature to 120°C to distill off 100 parts by mass of a solvent containing water, the temperature was lowered to 105°C, and 0.4 parts by mass of 2,2-bis(hydroxymethyl)propionic acid was charged and dissolved. Then, 34 parts by mass of hexamethylene diisocyanate was added, and 30 minutes later, 0.2 parts by mass of dibutyltin dilaurate was added. After continuing the reaction for 6 hours, a solution of polyester polyurethane resin a1 was obtained in which the solid content concentration was adjusted to 30% by dilution with toluene / 2-propanol. The number average molecular weight of polyester polyurethane resin a1 was 36,000, and the acid value was 2 mgKOH / g.
[0095] (2) Preparation of polyester polyurethane resins a2 to a9> Polyester polyurethane resins a2 to a9 were each prepared in the same manner as polyester polyurethane resin a1, except that the polyester, diol, and diisocyanate listed in Table 1 were each changed to the mass parts listed in Table 1.
[0096] [Table 1]
[0097] 1-2.Epoxy resin (B) The following commercially available products were used: (1) Epoxy resin B1 Bisphenol A novolac epoxy resin "EPICLON N-865" (product name) manufactured by DIC Corporation (2) Epoxy resin B2 Mitsubishi Chemical Corporation's bisphenol A epoxy resin "jER 1055" (product name)
[0098] 1-3.Flame retardants Clariant aluminum dimethylphosphinate "Exolit OP935" (product name)
[0099] 1-4. Curing accelerator Imidazole-based curing accelerator "Curesol C11-Z" (product name) manufactured by Shikoku Chemical Industry Co., Ltd.
[0100] 1-5.Solvent A mixed solvent of toluene, methyl isobutyl ketone, and 2-propanol (mass ratio = 100:20:20)
[0101] (Examples 1 to 8 and Comparative Examples 1 and 2) The raw materials listed in Table 2 were added to a flask equipped with a stirrer in the mass ratios listed in Table 2, and stirred for 6 hours at 60°C to dissolve component (A), component (B), and the curing accelerator in the solvent and disperse the flame retardant, thereby producing a liquid adhesive composition (resin composition). Then, using all of these liquid adhesive compositions, coverlay films, bonding sheets, and adhesion test pieces A, B, and C were produced, and the following evaluations (i) to (vi) were performed.
[0102] (1) Preparation of coverlay film The liquid adhesive composition was roll-coated on the surface of a 25 μm thick polyimide film so that the thickness after drying would be 15 μm, and then dried at 120° C. for 2 minutes to obtain a coverlay film having an adhesive layer.
[0103] (2) Preparation of adhesive test piece A A rolled copper foil with a thickness of 35 μm manufactured by Fukuda Metal Foil and Powder Co., Ltd. was prepared. The mirror surface was then placed on the adhesive layer surface of the coverlay film, and lamination was performed under conditions of 150° C., 0.3 MPa, and 1 m / min. The resulting laminate (polyimide film / adhesive layer / copper foil) was heated and pressed for 5 minutes under conditions of 150° C. and 3 MPa, and then further after-cured in an oven at 160° C. for 2 hours to obtain an adhesion test piece A.
[0104] (3) Preparation of adhesive test piece B The coating (adhesive layer) of the above coverlay film was brought into surface contact with the entire surface of a substrate having a comb-shaped test pattern (line width 100 μm, line spacing 100 μm), and heated and pressed in an oven at 150°C and a pressure of 3 MPa for 5 minutes, after which it was further after-cured in an oven at 160°C for 2 hours to produce test piece B for evaluating insulation reliability.
[0105] (4) Preparation of bonding sheet A 35 μm-thick release polyethylene terephthalate (PET) film was prepared. A mixture of the liquid adhesive composition and copper powder "FCC-115A" manufactured by Fukuda Metal Foil and Powder Co., Ltd., was mixed so that the mixture accounted for 15 mass % of the total resin solid content. The mixture was roll-coated on the surface of the film to a thickness of 25 μm after drying, and dried at 140° C. for 2 minutes to obtain a bonding sheet having an adhesive layer.
[0106] (5) Preparation of adhesive test piece C A flexible printed wiring board was prepared, which had a copper circuit pattern formed on the surface of a 300 μm thick nickel-plated SUS304 plate and a 25 μm thick polyimide film, and a 37.5 μm thick coverlay film with a 1 mm diameter through hole was laminated on the circuit pattern. First, the nickel-plated surface of the SUS304 plate was placed in contact with the adhesive layer surface of the bonding sheet, and lamination was performed under conditions of 150°C, 0.3 MPa, and 1 m / min to obtain a laminate (SUS plate / adhesive layer / release PET film). The release PET film was then peeled off, and the exposed surface of the adhesive layer was heated and pressed to a flexible printed wiring board (a wiring board in which a copper foil circuit was formed on a 25 μm thick polyimide, and a 37.5 μm thick coverlay film with a 1 mm diameter through hole was laminated on the copper foil circuit) at 150°C and 3 MPa for 5 minutes, and then after-cured in an oven at 160°C for 2 hours to produce adhesive test piece C (SUS plate / adhesive layer / flexible printed wiring board).
[0107] (i) Peel adhesion strength To evaluate the adhesiveness, the 180° peel strength (N / mm) was measured when peeling the copper foil of each adhesive test piece A from the polyimide film at a temperature of 23°C and a tensile speed of 50 mm / min in accordance with JIS C 6481 (1996) "Test Method for Copper-Clad Laminates for Printed Wiring Boards." The width of the adhesive test piece during measurement was 10 mm. As a result, peel strengths of 0.5 N / mm or more were indicated as "A," those of 0.35 N / mm or more but less than 0.5 N / mm as "B," and those less than 0.35 N / mm as "C."
[0108] (ii) Peel adhesion strength after long-term wet heat test In order to evaluate the adhesiveness of the adhesive test piece A after 1,000 hours under an atmosphere of 60°C and 95% RH, the 180° peel strength (N / mm) was measured when peeling the copper foil of each adhesive test piece A from the polyimide film at a temperature of 23°C and a tensile speed of 50 mm / min according to JIS C 6481 (1996) "Test Method for Copper-Clad Laminates for Printed Wiring Boards". The width of the adhesive test piece during the measurement was 10 mm. As a result, the peel strength reduction rate compared to the initial value was expressed as "A" for less than 15%, "B" for 15% to 30%, "C" for 30% to 50%, and "D" for 50% or more.
[0109] (iii) Solder heat resistance (appearance when soldered and peel strength after soldering) The test was conducted in accordance with JIS C 6481 (1996) under the following conditions. The above-mentioned adhesive test piece A was floated in a solder bath at 260°C for 60 seconds with the polyimide film side facing up, and the adhesive layer was visually evaluated for the presence or absence of appearance abnormalities such as blistering, peeling, etc. As a result, those that showed no appearance abnormalities such as blistering or peeling were rated as "A", those that showed slight appearance abnormalities such as blistering or peeling were rated as "B", and those that showed appearance abnormalities such as blistering or peeling were rated as "C". Furthermore, the test pieces removed from the solder bath were measured for 180° peel strength (N / cm) at 23°C when peeling the polyimide film from the copper foil in accordance with JIS C 6481 (1996). The width of the adhesive test piece during measurement was 10 mm, and the pulling speed was 50 mm / min. The results were graded as follows: "A" for a peel strength reduction rate of less than 15% compared to the initial value, "B" for a peel strength reduction rate of 15% or more but less than 30%, "C" for a peel strength reduction rate of 30% or more but less than 50%, and "D" for a peel strength reduction rate of 50% or more.
[0110] (iv) Insulation reliability A DC voltage of 50 V was applied to the adhesive test piece B for 1000 hours in an atmosphere of 85° C. temperature and 85% RH humidity. Thereafter, the resistance between the patterns was measured, and the insulation reliability was judged according to the following criteria. A resistance value of 10 or higher that can be judged to have sufficient insulation reliability for practical use is 10 or higher. 7 Ω or more is "A", and resistance value is 10 7 Anything less than Ω was indicated as "F".
[0111] (v) Conductivity (connection resistance) The connection resistance between the SUS plate and the copper foil circuit of the flexible printed wiring board of the above adhesive test piece C (SUS plate / adhesive layer / flexible printed wiring board) was measured with a resistance meter. The connection resistance was then marked as "A" if it was less than 0.5Ω, "B" if it was between 0.5Ω and 1Ω, "C" if it was between 1Ω and 3Ω, and "D" if it was more than 3Ω.
[0112] (vi) Conductivity (connection resistance) after soldering The above-mentioned adhesive test piece C was floated in a solder bath at 260°C for 60 seconds. After that, the connection resistance between the SUS plate of the adhesive test piece C taken out of the solder bath and the copper foil circuit of the flexible printed wiring board was measured with a resistance meter. The connection resistance values were as follows: less than 0.5Ω "A", 0.5Ω to 1Ω "B", 1Ω to 3Ω "C", and over 3Ω "D".
[0113] (vii) After long-term reliability test of electrical conductivity (connection resistance) The above adhesive test piece C was left in a thermo-hygrostat at 60°C and 95% RH for 1,000 hours. After that, the connection resistance between the SUS plate of adhesive test piece B and the copper foil circuit of the flexible printed wiring board was measured with a resistance meter. The connection resistance was then marked as "A" if it was less than 0.5 Ω, "B" if it was 0.5 Ω or more but less than 1 Ω, "C" if it was 1 Ω or more but less than 3 Ω, and "D" if it was more than 3 Ω.
[0114] (viii) Storage stability of the adhesive composition The adhesive compositions of Examples 1 to 8 or Comparative Examples 1 or 2 having the compositions shown in Table 1 were each placed in a glass bottle, sealed, and stored at 5° C. for a predetermined time, and the crystallinity of the composition was observed. After storage for the predetermined time, evaluation was performed according to the following evaluation criteria based on the storage time until gelation or liquid separation of the adhesive composition was confirmed. <Evaluation criteria> A: More than a week F: Less than 1 week
[0115] [Table 2]
[0116] As is clear from the results shown in Table 2, the resin compositions of Examples 1 to 8 gave cured products (adhesives) with excellent electrical conductivity and adhesion, even after long-term storage in a high-temperature, high-humidity environment, compared to the resin compositions of Comparative Examples 1 and 2. Furthermore, as is clear from the results shown in Table 2, the resin compositions of Examples 1 to 8 are excellent in initial and post-solder adhesion, excellent in appearance after solder formation, excellent in insulation reliability, and excellent in storage stability.
[0117] The disclosure of Japanese Patent Application No. 2019-214475, filed on November 27, 2019, is incorporated herein by reference in its entirety. All publications, patent applications, and technical standards mentioned in this specification are herein incorporated by reference to the same extent as if each individual publication, patent application, or technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A polyester polyurethane resin (A), An epoxy resin (B); Contains a metal filler, The molecular weight per urethane bond in the polyester polyurethane resin (A) is 200 to 8,000, The acid value of the polyester polyurethane resin (A) is 0.1 mgKOH / g to 3.0 mgKOH / g, An adhesive resin composition, wherein the molecular weight per urethane bond in the polyester polyurethane resin (A) is a value obtained by dividing the number average molecular weight Mn of the polyester polyurethane resin (A) by the average number of urethane bonds contained in the polyester polyurethane resin (A).
2. An adhesive resin composition as described in claim 1, wherein the diol component constituting the polyester polyurethane resin (A) includes a diol having a side chain.
3. An adhesive resin composition described in claim 1 or claim 2, wherein the polyester polyurethane resin (A) comprises a polyester polyurethane resin having a polyester structure with a number average molecular weight of 8,000 to 30,000.
4. An adhesive resin composition described in any one of claims 1 to 3, wherein the number average molecular weight of the polyester polyurethane resin (A) is 10,000 to 80,000.
5. An adhesive resin composition described in any one of claims 1 to 4, wherein the glass transition temperature of the polyester polyurethane resin (A) is 30°C to 150°C.
6. An adhesive resin composition described in any one of claims 1 to 5, wherein the content of the epoxy resin (B) is 1 part by mass to 30 parts by mass per 100 parts by mass of the polyester polyurethane resin (A).
7. An adhesive resin composition described in any one of claims 1 to 6, wherein the epoxy resin (B) comprises a bisphenol novolac type epoxy resin.
8. An adhesive resin composition layer comprising the adhesive resin composition according to any one of claims 1 to 7, a B-stage adhesive resin composition layer obtained by partially curing the adhesive resin composition, or a cured layer obtained by curing the adhesive resin composition; a base film in contact with at least one surface of the adhesive resin composition layer, the B-stage adhesive resin composition layer, or the cured layer; A laminate having an adhesive resin composition layer.
9. A cured layer formed by curing the adhesive resin composition according to any one of claims 1 to 7. Laminate.
10. Copper foil and A cured layer obtained by curing the adhesive resin composition according to any one of claims 1 to 7; A substrate. Flexible copper clad laminate.
11. Copper wiring, A cured layer obtained by curing the adhesive resin composition according to any one of claims 1 to 7; and a covering material. Flexible flat cable.
12. The adhesive resin composition according to any one of claims 1 to 7 has an adhesive resin composition layer, a B-stage adhesive resin composition layer obtained by partially curing the adhesive resin composition, or a cured layer obtained by curing the adhesive resin composition. Electromagnetic wave shielding film.
Citation Information
Patent Citations
Sea-bottom pipeline laying method using marine rail system
JP1983046290A
Epoxy resin composition
JP1989090216A
Laminate
JP2005125724A
Thermosetting resin composition, thermoplastic resin solution, film-forming material and cured product of these
JP2007154134A
Resin composition for adhesive, adhesive and adhesive sheet containing the same, and printed circuit board containing the adhesive sheet as adhesive layer
JP2010084005A