Manufacturing method for welded products
The method simplifies aluminum member welding by using laser or electron beam welding with strategic steps to prevent cracks at terminal points and overlapping welds, addressing complexity and applicability issues in conventional methods.
Patent Information
- Application Number
- JP2022080661
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-05-17
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-05-17
AI Technical Summary
Conventional methods for joining aluminum members require preparatory work to form a filler film, which becomes complex when the number of welding locations increases, and friction stir welding becomes difficult to apply under similar conditions.
A method involving laser or electron beam welding with specific steps such as peripheral edge welding, outer termination, outer edge crossing, overlapping welding, and end enclosing to form a welded product with an internal space, preventing cracks at the end of linear welded parts by forming terminal points outside the internal space or overlapping them with additional welds.
Simplifies the welding process, prevents cracks from affecting the internal space of the welded product, and allows for increased welding points without the need for filler metal or friction stir welding, maintaining sealing performance.
Smart Images

Figure 0007586134000001 
Figure 0007586134000002 
Figure 0007586134000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a welded article. [Background technology]
[0002] Conventionally, there have been known methods for joining aluminum members by laser welding. For example, the following Patent Document 1 discloses a method for joining aluminum members, which comprises spraying an Al-Si alloy filler metal onto at least one joining surface of two aluminum members to be joined to form a filler metal coating, and assembling and joining the members by laser welding (paragraph 0005, claim 1, abstract, etc.).
[0003] According to this conventional method for joining aluminum components, when joining components that are highly susceptible to solidification cracking, high-speed welding using a laser is possible without the conventional problem of the welding speed being reduced by the feed rate of the filler metal, and the joining work itself is also simplified (Patent Document 1, paragraph 0016).
[0004] Also, a busbar is known that can be welded to an external terminal of an electronic component without using a filler metal and without causing weld cracks in the busbar. The following Patent Document 2 discloses a busbar in which a plurality of terminals connected to external terminals of an electronic component are made of 1000 series aluminum, a main body connecting these terminals is made of 6000 series aluminum alloy, and the terminals and main body are integrated by friction stir welding (Patent Document 2, paragraph 0009, claim 1, abstract, etc.).
[0005] According to this conventional busbar, the terminal portion connected to the external terminal of the electronic component is made of 1000 series aluminum, and therefore has good weldability, and can be satisfactorily joined without the occurrence of weld cracks even without the use of filler metal when welding the terminal portion to the external terminal of the electronic component. Also, since welding can be performed without the use of filler metal, there is no decrease in conductivity due to the filler metal, and energy loss due to busbar connection can be reduced. Furthermore, since there is no need for associated work such as setting and managing conditions for supplying filler metal, welding workability is good (Patent Document 2, paragraph 0015). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 07-100675 [Patent Document 2] JP 2015-015211 A Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, the conventional method for joining aluminum members requires a preparatory step of spraying an Al-Si alloy filler metal onto the joining surfaces of the members to be joined to form a filler metal coating before assembling the members to be joined and joining them by laser welding. Therefore, if the number of welding points relative to the area of the members to be joined increases, the preparatory step increases and the welding of the members to be joined becomes complicated.
[0008] In addition, as described above, the conventional busbar requires friction stir welding between the portion made of 1000 series aluminum and the portion made of 6000 series aluminum alloy, and application of friction stir welding becomes difficult when the number of welds increases relative to the area of the members to be joined.
[0009] The present disclosure provides a method for manufacturing a welded product that is easy to apply even when the number of welding points is increased, that is simple to weld, and that can prevent the internal space of the welded product from being affected even if a crack occurs at the end point of a linear weld. [Means for solving the problem]
[0010] One aspect of the present disclosure is a method for manufacturing a welded product, which includes a peripheral welding process for forming a weld that surrounds the internal space, and further includes at least one of an outer termination process for forming an end point of the weld outside the weld that surrounds the internal space, an outer edge intersection process for moving a laser for laser welding or an electron beam for electron beam welding from the inside to the outside of the outer edge of the multiple components to form the weld, an overlap welding process for forming another weld that overlaps with the end point of one of the welds, or an end surrounding process for forming the end point of the weld in an area surrounded by the welds that partition the internal space.
[0011] The manufacturing method of the welded product according to the one aspect can include at least the outer terminal end step or the outer edge intersection step. The manufacturing method of the welded product according to each aspect can include at least the overlap welding step and the terminal end surrounding step. In the manufacturing method of the welded product according to each aspect, the welded portion may have a straight portion extending linearly and a bent portion formed between the straight portions extending in different directions, and the included angle between the straight portions on both sides of the bent portion may be 90 degrees or more. Effect of the Invention
[0012] According to each of the above aspects of the present disclosure, it is possible to provide a method for manufacturing a welded product that is easy to apply even when the number of welding locations is increased, that is simple to weld, and that can prevent weld cracks that occur at the end points of linear welds from affecting the internal space of the welded product. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a flow diagram illustrating one embodiment of a method for manufacturing a welded article according to the present disclosure. [Diagram 2] 2 is a cross-sectional view showing an example of a welded product manufactured by the method for manufacturing a welded product shown in FIG. 1; [Diagram 3] Bottom view of the welded item in Figure 2. [Figure 4]Top view of the welded item in Figure 2. [Diagram 5] An enlarged view of the weld at part V of the welded product in Figure 4. [Figure 6] 6 is an enlarged view of a welded portion showing a modified example of the welded product in FIG. 5. [Figure 7] FIG. 7 is an enlarged view of the welded portion at part VII of the welded product of FIG. 4 . [Figure 8] 8 is an enlarged view of a welded portion showing a modified example of the welded product in FIG. 7. [Figure 9] FIG. 5 is an enlarged view of the welded portion at part IX of the welded product of FIG. 4 . [Figure 10] 10 is an enlarged view of the weld at part X of the welded product in FIG. 9 . [Figure 11] 8 is an enlarged view of a welded portion showing a modified example of the welded product in FIG. 7. [Figure 12] 10 is an enlarged view of the welded portion at part XII of the welded product of FIG. 9 . [Figure 13] 5 is an enlarged view of the welded portion at part XIII of the welded product of FIG. 4 . DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the method for manufacturing a welded product according to the present disclosure will be described with reference to the drawings. Fig. 1 is a flow diagram showing one embodiment of the method for manufacturing a welded product according to the present disclosure. Fig. 2 is a cross-sectional view showing an example of a welded product 1 manufactured by the method for manufacturing a welded product P of Fig. 1. Fig. 3 is a bottom view of the welded product 1 of Fig. 2. Fig. 4 is a top view of the welded product 1 of Fig. 2. The cross section of the welded product 1 of Fig. 2 is a cross section taken along the center line of the welded product 1 shown in Figs. 3 and 4.
[0015] The manufacturing method P of the welded product of this embodiment is a method of manufacturing a welded product 1 having an internal space 2 by forming a welded portion W by laser welding or electron beam welding a plurality of members. As shown in FIG. 1, the manufacturing method P of the welded product of this embodiment includes a peripheral welding step P1. The manufacturing method P of the welded product of this embodiment also includes, for example, an outer termination step P2 or an outer edge intersection step P3 in addition to the peripheral welding step P1. Furthermore, the manufacturing method P of the welded product of this embodiment includes an overlap welding step P4 and an end surrounding step P5. Note that the manufacturing method P of the welded product of this embodiment may include at least one of the outer termination step P2, the outer edge intersection step P3, the overlap welding step P4, or the end surrounding step P5 in addition to the peripheral welding step P1.
[0016] The welded product 1 manufactured by the welded product manufacturing method P of this embodiment is composed of a plurality of members welded by laser welding or electron beam welding. In the example shown in Figures 2 to 4, the welded product 1 is composed of a plurality of plate-like members. More specifically, the welded product 1 has, for example, a flat lower plate 3 and an upper plate 4 having an uneven shape.
[0017] The welded product 1 has an internal space 2 between a plurality of welded members. In the example shown in Fig. 2, the upper plate 4 has a flat portion 41 in contact with the lower plate 3, and a bulging portion 42 that bulges in the opposite direction to the lower plate 3 to form the internal space 2 between the upper plate 4 and the lower plate 3. More specifically, in this embodiment, the welded product 1 is, for example, a cooler, and the internal space 2 of the welded product 1 is a refrigerant flow path of the cooler. As shown in Fig. 3, the lower plate 3 has a refrigerant inlet 31 and a refrigerant outlet 32.
[0018] As shown in Fig. 4, the bulging portion 42 of the upper plate 4 has a shape corresponding to the shape of the internal space 2 formed between it and the lower plate 3. The internal space 2 of the welded product 1 of this embodiment is, for example, a coolant flow path of a cooler having a plurality of branching and bending portions, and as shown in Fig. 3, a coolant is supplied and discharged through a coolant inlet 31 and a coolant outlet 32 that open in the lower plate 3. As shown in Figs. 2 and 4, the flat portion 41 of the upper plate 4 is welded to the lower plate 3 by laser welding or electron beam welding to form a linear weld W.
[0019] The welded product 1 is not limited to a cooler, and may be a heat exchanger or a tank having a configuration in which a plurality of members are welded together and an internal space 2 surrounded by a linear weld B. The welded product 1 may also be a configuration in which three or more plate-like members are welded together. The material of the plurality of members constituting the welded product 1 is, for example, a metallic material such as a 2000 series (Al-Cu series), 3000 series (Al-Mn series), or 4000 series (Al-Si series) aluminum alloy.
[0020] The method P for manufacturing a welded product of this embodiment is particularly effective when the materials of the members constituting the welded product are aluminum alloys such as 5000 series (Al-Mg series), 6000 series (Al-Mg-Si series), or 7000 series (Al-Zn-Mg light alloy). Each step of the method P for manufacturing a welded product of this embodiment will be described in detail below.
[0021] As shown in Fig. 1, when the manufacturing method P of the welded product of this embodiment is started, for example, a periphery welding step P1 is performed. In the periphery welding step P1, a weld W surrounding an internal space 2 is formed. More specifically, as shown in Fig. 2, an upper plate 4 is placed on a lower plate 3, and a flat portion 41 of the upper plate 4 and the lower plate 3 are overlapped. Then, the periphery of a bulging portion 42 of the upper plate 4 that forms the internal space 2 between the lower plate 3 and the upper plate 4 is continuously welded by laser welding or electron beam welding, and as shown in Fig. 4, a periphery weld W1 is formed as a weld W that continuously surrounds the entire periphery of the bulging portion 42.
[0022] The circumferential weld W1 has a plurality of straight portions W13 that extend linearly along the outer edge of the upper plate 4, and a plurality of bent portions W14 that are formed between the straight portions W13, W13 that extend in different directions. In the example shown in Fig. 4, each bent portion W14 is formed in an arc shape, and the included angle between the straight portions W13, W13 on both sides of each bent portion W14 is 90 degrees.
[0023] As an example, the conditions for laser welding a lower sheet 3 and an upper sheet 4 made of a 6000 series aluminum alloy (A6061-T6) with a thickness of 0.8 mm can be a laser spot diameter of 0.6 mm, a laser output of 2.8 kW, and a laser scanning speed of 5 m / min. Note that these conditions are merely examples, and it goes without saying that the conditions will vary depending on the welding method, the thickness and material of the parts to be welded, etc. In the case of laser welding, for example, a continuous wave (CW) method can be used, but it is not limited to the CW method as long as it is a method that can form a continuous linear weld W.
[0024] Fig. 5 is an enlarged view of the welded portion W in the V portion of the welded product 1 in Fig. 4. As shown in Fig. 4 and Fig. 5, in the peripheral welding process P1, welding of the lower plate 3 and the upper plate 4 is started from an arbitrary point on the peripheral portion of the upper plate 4 where the lower plate 3 and the flat portion 41 of the upper plate 4 overlap, such as the lower left corner of the upper plate 4, to form a start point W11 of the welded portion W. Then, from the start point W11, the welded portion W is formed linearly on the peripheral portion of the upper plate 4 along one side edge, such as the left side edge of the upper plate 4, and further formed linearly along the other side edge of the upper plate 4, to form the welded portion W around the entire periphery of the upper plate 4.
[0025] Finally, as shown in Fig. 5, a weld W is formed that intersects with the weld W formed along one side edge of the upper plate 4 where welding has started, forming a circumferential weld W1 that surrounds the entire circumference of the internal space 2 formed between the bulging portion 42 of the upper plate 4 and the lower plate 3. This ends the circumferential welding process P1, and the outer termination process P2 is performed immediately after. In the outer termination process P2, as shown in Fig. 5, the weld W that intersects with the initially formed weld W is continuously extended to form an end point W12 of the weld W outside the frame-shaped circumferential weld W1, which is the weld W that surrounds the internal space 2.
[0026] For example, when the members constituting the welded product 1 are 5000, 6000, 7000, or other aluminum alloys, cracks are likely to occur at the end point W12 of the weld W. This is thought to be because, since there is no subsequent weld W at the end point W12 of the weld W, molten metal is not supplied from subsequent parts when the molten metal solidifies, and the stress acting on the end point W12 when the molten metal solidifies is greater than that on other parts.
[0027] Even if a crack occurs at the end point W12 of the weld W, by performing the outer termination process P2 to form the end point W12 of the weld W outside the frame-shaped circumferential weld W1, which is the weld W that surrounds the internal space 2, it is possible to prevent the crack from affecting the internal space 2 of the welded product 1. In other words, since the circumferential weld W1 surrounding the internal space 2 ensures the sealability of the periphery of the internal space 2, even if a crack occurs at the end point W12 of the weld W outside the circumferential weld W1, the sealability of the periphery of the internal space 2 is not reduced.
[0028] Fig. 6 is an enlarged view of a welded portion W showing a modified example of the welded product 1 of Fig. 5. As shown in Fig. 1, in the manufacturing method P of the welded product of this embodiment, after the circumferential welding process P1, an outer edge intersection process P3 may be performed instead of the outer termination process P2. The outer edge intersection process P3 can be performed directly and continuously after the circumferential welding process P1 for forming the circumferential weld W1 that surrounds the entire circumference of the internal space 2, for example, in the same manner as the outer termination process P2 shown in Fig. 5.
[0029] 6, in the outer edge intersection process P3, a laser for laser welding or an electron beam for electron beam welding is moved from the inside to the outside of the outer edges of the upper plate 4 and the lower plate 3, which are the multiple members constituting the welded product 1, to form a welded part W. As a result, an end point W12 of the welded part W is not formed on the peripheral parts of the upper plate 4 and the lower plate 3, which are the members constituting the welded product 1.
[0030] 5, it is formed inside the outer edges of the upper plate 4 and the lower plate 3 which are members constituting the welded product 1. That is, there is a portion where the weld W is not formed between the end point W12 of the weld W and the outer edge of the upper plate 4. In this case, as described above, cracks are likely to occur at the end point W12 of the weld W.
[0031] In contrast, in the outer edge intersecting process P3, as shown in Fig. 6, the weld W is formed so as to intersect with the outer edges of the upper plate 4 and the lower plate 3 which are members constituting the welded product 1, and an end point W12 of the weld W is not formed on the peripheral parts of the upper plate 4 and the lower plate 3. In the example shown in Fig. 6, the outer edge of an auxiliary plate AP made of the same material as the upper plate 4 and the lower plate 3 is butted against the outer edges of the upper plate 4 and the lower plate 3 which constitute the welded product 1.
[0032] In this state, the laser for laser welding or the electron beam for electron beam welding is moved from the inside to the outside of the outer edges of the upper plate 4 and the lower plate 3, continuously forming a weld W from the upper plate 4 and the lower plate 3 to the auxiliary plate AP, and an end point W12 of the weld W is formed on the auxiliary plate AP. As a result, the portion of the weld W that intersects with the outer edges of the upper plate 4 and the lower plate 3 is supplied with molten metal from the subsequent weld W formed on the auxiliary plate AP, preventing cracks. After that, the weld W is cut at the outer edges of the upper plate 4 and the lower plate 3.
[0033] In addition, the outer edge intersection process P3 does not need to use the auxiliary plate AP. In this case, when the laser of laser welding or the electron beam of electron beam welding is moved from the inside to the outside of the outer edges of the upper plate 4 and the lower plate 3, which are members constituting the welded product 1, the outer edges of the upper plate 4 and the lower plate 3 melt and solidify to form a welded part W. The end of this welded part W is different from the end point part W12 shown in FIG. 5, and there is no part between the outer edges of the lower plate 3 and the upper plate 4 where the welded part W of the lower plate 3 and the upper plate 4 is not formed. Therefore, the end of the welded part W solidifies while shrinking inward from the outer edges of the upper plate 4 and the lower plate 3, thereby reducing the stress acting during solidification and preventing cracks.
[0034] In the manufacturing method P of the welded product of this embodiment, the outer termination step P2 and the outer edge intersection step P3 include, for example, a step of forming a flow passage forming weld W2 described below. The flow passage forming weld W2 is a part of the weld W shown in Fig. 4 and extends from the inside to the outside of the peripheral weld W1 surrounding the internal space 2. The flow passage forming weld W2 partitions the internal space 2 of the welded product 1 and forms a refrigerant flow passage in the internal space 2, as shown in Fig. 2, for example.
[0035] Fig. 7 is an enlarged view of the welded portion W at part VII of the welded product 1 in Fig. 4. In the example shown in Fig. 4, the flat portion 41 of the upper plate 4 has an L-shaped peninsula portion extending from the peripheral portion toward the center of the upper plate 4. In the step of forming the flow passage forming weld W2 in the outer end process P2, welding is started from the tip of the peninsula portion of the flat portion 41 of the upper plate 4, and the flow passage forming weld W2 extending linearly from the starting point W21 is formed.
[0036] 7, an end point W22 of the flow passage forming weld W2 is formed outside the circumferential weld W1, which is the weld W that surrounds the internal space 2. This provides the same effect as the process of forming the end point W12 of the circumferential weld W1 outside the circumferential weld W1 that surrounds the internal space 2 in the outer termination process P2 described above.
[0037] Fig. 8 is an enlarged view of a welded portion W showing a modified example of the welded product 1 in Fig. 7. In the step of forming the flow passage weld W2 in the outer edge crossing step P3, similar to the outer termination step P2 described above, welding is started from the tip of the peninsula-shaped portion of the flat portion 41 of the upper plate 4, and the flow passage weld W2 extending linearly from the starting point W21 is formed.
[0038] Then, as shown in Fig. 8, the laser for laser welding or the electron beam for electron beam welding is moved from the inside to the outside of the outer edges of the upper plate 4 and the lower plate 3, which are multiple members constituting the welded product 1, to form a flow passage forming weld W2 that intersects with the outer edges of the upper plate 4 and the lower plate 3. In the example shown in Fig. 8, like the example shown in Fig. 6 described above, an auxiliary plate AP is used, but the outer edge intersecting process P3 for forming the flow passage forming weld W2 can also be performed without using the auxiliary plate AP.
[0039] As shown in Fig. 4, the flow passage weld W2, which is a part of the weld W, has a plurality of straight portions W23 extending linearly and one or a plurality of bent portions W24 formed between the straight portions W23, W23 extending in different directions. In the example shown in Fig. 4, each bent portion W24 is formed in an arc shape, and the included angle between the straight portions W23, W23 on both sides of each bent portion W24 is an obtuse angle equal to or greater than 90 degrees.
[0040] In the manufacturing method P of a welded product of this embodiment, after the outer terminal end step P2 or the outer edge intersection step P3 for forming the flow passage forming weld W2 is completed, for example, an overlap welding step P4 and a terminal end surrounding step P5 are performed as shown in Fig. 1. The overlap welding step P4 includes, for example, a first overlap welding step P41 and a second overlap welding step P42, and the terminal end surrounding step P5 includes, for example, a first terminal end surrounding step P51 and a second terminal end surrounding step P52.
[0041] In the first overlap welding process P41 and the first end surrounding process P51, a flow path forming weld W3, which is part of the weld W, is formed, and in the second overlap welding process P42 and the second end surrounding process P52, a flow path forming weld W4, which is part of the weld W, is formed. The flow path forming welds W3, W4 join the island-shaped flat portion 41 surrounded by the bulge 42 of the upper plate 4 to the lower plate 3, as shown in Fig. 4, and define the internal space 2 between the bulge 42 of the upper plate 4 and the lower plate 3, thereby forming a refrigerant flow path in the welded product 1.
[0042] Fig. 9 is an enlarged view of the welded portion W at part IX of the welded product 1 in Fig. 4. The flow path forming welded portion W3 which is the welded portion W has, for example, a first portion W31, a second portion W32, a third portion W33, and a fourth portion W34 which are welded portions W, and partitions the internal space 2 of the welded product 1 to form a refrigerant flow path in the welded product 1 as shown in Fig. 2.
[0043] The first portion W31 has a starting point W311 at one tip of a three-pronged flat portion 41, and has an ending point W312 just before the central tip of the three-pronged flat portion 41. The first portion W31 also has a plurality of straight portions W313 extending linearly and a plurality of bent portions W314 formed between the straight portions W313, W313 extending in different directions, and the included angle between the straight portions W313, W313 on both sides of each bent portion W314 is 90 degrees.
[0044] The second portion W32 has a starting point W321 at the base opposite to the three tips of the flat portion 41 having a three-pronged fork shape. The second portion W32 extends linearly from the starting point W321 between one end and the center of the base of the trifurcated flat portion 41 to the other end of the base, is bent in a direction perpendicular to the base at the other end of the base, and has an end point W322 just before one of the three tips of the trifurcated flat portion 41. The second portion W32 also has two straight line portions W323 that extend linearly and one arc-shaped bent portion W324 formed between the two straight line portions W323 that extend in different directions, and the included angle between the straight line portions W323, W323 on both sides of the bent portion W324 is 90 degrees.
[0045] The third portion W33 has a starting point W331 at the tip opposite to the tip where the starting point W311 of the first portion W31 is formed, out of the two tips at both ends of the trifurcated flat portion 41, and has an ending point W332 short of the central tip of the trifurcated flat portion 41. The third portion W33 also has a plurality of straight portions W333 extending linearly and a plurality of bent portions W334 formed between two straight portions W333, W333 extending in different directions, and the included angle between the straight portions W333, W333 on both sides of the bent portion W334 is 90 degrees.
[0046] The fourth portion W34 has a starting point 341 at the central tip of the trifurcated flat portion 41, extends in a straight line toward the base of the trifurcated flat portion 41, and has an ending point W342 at the central portion of the base of the flat portion 41 extending in a direction perpendicular to the fourth portion W34.
[0047] Fig. 10 is an enlarged view of the weld W at part X of the welded product in Fig. 9. In the first overlap welding process P41 for forming the flow passage weld W3, as shown in Fig. 9 and Fig. 10, first, the first portion W31 is formed to form the end point W312, and then the second portion W32 is formed to form the end point W322. Next, as shown in Fig. 9 and Fig. 10, the end point W322 of the second portion W32, which is one weld W, and the third portion W33, which is another weld W overlapping the end point W312 of the first portion W31, which is one weld W, are formed.
[0048] Finally, a fourth portion W34 is formed, which has a start portion W341 at the central tip of the trifurcated flat portion 41 and overlaps the end portions W332, W312 of the third portion W33 and the first portion W31, respectively. Here, the third portion W33 and the first portion W31 are each one of the welded portions W, and the fourth portion W34 is another welded portion W that overlaps the end portions W332, W312 of the respective welded portions W.
[0049] In this manner, in the first overlap welding process P41, the third portion W33 or the fourth portion W34 is formed as another weld W overlapping the end points W312, W322, and W332 of the first portion W31, the second portion W32, and the second portion W32, which are the weld W. This allows cracks that have occurred in the end points W312, W322, and W332 to be repaired by the third portion W33 or the fourth portion W34 formed to overlap the end points W312, W322, and W332.
[0050] Fig. 11 is an enlarged view of a welded portion W showing a modified example of the welded product 1 of Fig. 7. In the example shown in Fig. 7, after the circumferential welding step P1 is performed to form the circumferential welded portion W1, the outer termination step P2 is performed to form the flow passage formation welded portion W2. In contrast, in the example shown in Fig. 11, the circumferential welding step P1 is performed in parallel with the overlap welding step P4.
[0051] More specifically, first, similarly to the outer termination process P2 described above, a flow passage forming weld W2 is formed from the tip of a peninsula-shaped flat portion 41 extending in an L-shape from the peripheral portion to the center of the upper plate 4 shown in Fig. 4 toward the peripheral portion of the upper plate 4, and an end point W22 is formed on the flat portion 41 at the peripheral portion of the upper plate 4. At this time, the end point W22 of the flow passage forming weld W2 is formed at a position overlapping the peripheral weld W1 formed by the peripheral welding process P1 performed after the formation of the end point W22.
[0052] Next, the above-mentioned circumferential welding step P1 is performed to form a circumferential weld W1 that surrounds the internal space of the welded product 1. At this time, as shown in Fig. 11, the circumferential weld W1 is formed to overlap an end point W22 of a flow passage weld W2 formed on a flat portion 41 of the periphery of the upper plate 4. As a result, even if a crack occurs at the end point W22 of the flow passage weld W2, the crack at the end point W22 of the flow passage weld W2 can be repaired by forming the circumferential weld W1 to overlap.
[0053] 9, in the first overlap welding process P41 for forming the flow passage formation weld W3, when a fourth portion W34 overlapping an end point W332 of the third portion W33 and an end point W312 of the first portion W31 is formed, the first overlap welding process P41 ends. In the manufacturing method P for a welded product of this embodiment, when the first overlap welding process P41 ends, a first end surrounding process P51 is performed immediately thereafter.
[0054] Fig. 12 is an enlarged view of the welded portion W at part XII of the welded product 1 in Fig. 9. In the first end surrounding process P51, an end point W342 of the fourth portion W34 is formed in a region surrounded by the first portion W31, the second portion W32, and the third portion W33 of the flow passage forming weld W3, which is the welded portion W that defines the internal space 2 of the welded product 1.
[0055] More specifically, in this first end surrounding process P51, the fourth portion W34, which is started to be welded from the central tip portion of the trifurcated flat portion 41 of the upper plate 4 in the first overlap welding process P41, is continuously formed toward the base portion of the trifurcated flat portion 41. Then, the end point W342 of the fourth portion W34 is formed in the area surrounded by the first portion W31, the second portion W32, and the third portion W33 at the base portion of the trifurcated flat portion 41. With the above, the first end surrounding process P51 is completed.
[0056] In this manner, in the end surrounding step P5, an end point W342 of the fourth portion W34 of the welded portion W is formed in an area surrounded by the first portion W31, the second portion W32, and the third portion W33 of the welded portion W that define the internal space 2 of the welded product 1. This prevents a crack from affecting the internal space 2 of the welded product 1 even if a crack occurs in the end point W342. As shown in FIG. 1, in the manufacturing method P of a welded product of this embodiment, a second overlap welding step P42 and a second end surrounding step P52 are then performed.
[0057] Fig. 13 is an enlarged view of the welded portion W in part XIII of the welded product in Fig. 4. In the second overlap welding process P42 and the second end surrounding process P52, a flow passage forming welded portion W4 shown in Fig. 4 and Fig. 13 is formed. The flow passage forming welded portion W4, which is the welded portion W, has, for example, a first portion W41, a second portion W42, and a third portion W43, which are also the welded portion W, and defines an internal space 2 formed between the bulging portion 42 of the upper plate 4 and the lower plate 3, thereby forming a refrigerant flow passage in the welded product 1.
[0058] The first portion W41 has a starting point W411 formed at one end of the elongated flat portion 41, and an end point W412 formed at the other end of the flat portion 41. The first portion W41 also has a straight portion W413a extending linearly from the starting point W411 toward the end point W412, a straight portion W413b extending linearly in a different direction from the straight portion W413a, and a straight portion W413c extending linearly in a different direction from the straight portion W413b.
[0059] The first portion W41 has a bent portion W414a between the straight portion W413a and the straight portion W413b, and a bent portion W414b between the straight portion W413b and the straight portion W413c. The included angle between the straight portion W413a on both sides of the bent portion W414a and the straight portion W413b, and the included angle between the straight portion W413b on both sides of the bent portion W414b and the straight portion W413c are both obtuse angles of 90 degrees or more.
[0060] The second portion W42 has a starting point W421 formed at an end of the elongated flat portion 41 opposite to the end where the starting point W411 of the first portion W41 is formed, and an end point W422 formed at the end of the flat portion 41 opposite to the end point W421 closer to the center of the flat portion 41 than the starting point W411 of the first portion W41. The second portion W42 has a straight line portion W423a extending linearly from the starting point W421 to the end point W422, a straight line portion W423b extending linearly in a direction different from the straight line portion W423a, and a straight line portion W423c extending linearly in a direction different from the straight line portion W423b.
[0061] The second portion W42 has a bent portion W424a between the straight portion W423a and the straight portion W423b, and a bent portion W424b between the straight portion W423b and the straight portion W423c. The included angle between the straight portion W423a on both sides of the bent portion W424a and the straight portion W423b, and the included angle between the straight portion W423b on both sides of the bent portion W424b and the straight portion W423c are both obtuse angles of 90 degrees or more.
[0062] The third portion W43 has a start portion W431 formed at one end of the elongated flat portion 41 at a position closer to the longitudinal edge than the start portion W411 of the first portion W41, and an end portion W432 formed in the longitudinal center of the flat portion 41. The end portion W432 of the third portion W43 is formed in a region surrounded by the first portion W41 and the second portion W42 of the flow passage forming weld W4 that partitions the internal space 2 of the welded product 1.
[0063] The third portion W43 has a straight portion W433a extending in a straight line from the starting point W431 to the ending point W432, and a straight portion W433b extending in a straight line in a direction different from the straight portion W433a. The third portion W43 has a bent portion W434 between the straight portion W433a and the straight portion W433b. The included angle between the straight portion W433a on both sides of the bent portion W434 and the straight portion W433b is an obtuse angle of 90 degrees or more.
[0064] In the second overlap welding process P42, first, a first portion W41 of the flow passage forming weld W4 is formed on the elongated island-shaped flat portion 41 of the upper plate 4. Next, a second portion W42 is formed as another weld W overlapping an end point W412 of the first portion W41, which is one weld W. Finally, a third portion W43 is formed as another weld W overlapping an end point W422 of the second portion W42, which is one weld W.
[0065] In this way, in the second overlap welding process P42, by forming a second portion W42 overlapping the end portion W412 of the first portion W41 and a third portion W43 overlapping the end portion W422 of the second portion W42, even if cracks occur in the end portions W412, W422, the cracks can be repaired.
[0066] In the manufacturing method P of the welded product of this embodiment, when the second overlap welding step P42 is completed, the second end surrounding step P52 is performed immediately after. In the second end surrounding step P52, an end point W432 of the third portion W43 is formed in the area surrounded by the first portion W41 and the second portion W42 of the flow passage forming weld W4, which is the weld W that defines the internal space 2 of the welded product 1. In this way, the second end surrounding step P52 is completed, and the manufacturing method P of the welded product shown in FIG. 1 is completed.
[0067] In this manner, in the end surrounding step P5, the end point W432 of the third portion W43 is formed in the area surrounded by the first portion W41 and the second portion W42, which are the welded portion W that partition the internal space 2 of the welded product 1. This prevents a crack from affecting the internal space 2 of the welded product 1 even if a crack occurs in the end point W432.
[0068] As described above, the manufacturing method P of the welded product of this embodiment is a method for manufacturing a welded product 1 having an internal space 2 by forming a welded portion W by welding a plurality of members by laser welding or electron beam welding. The manufacturing method P of the welded product of this embodiment includes a peripheral welding step P1 for forming a welded portion W surrounding the internal space 2. The manufacturing method P of the welded product of this embodiment further includes at least one of an outer termination step P2, an outer edge intersection step P3, an overlap welding step P4, and an end surrounding step P5. In the outer termination step P2, as shown in Figs. 5 and 7, end points W12 and W22 of the welded portion W are formed on the outside of the welded portion W surrounding the internal space 2. In the outer edge intersection step P3, as shown in Figs. 6 and 8, the laser of the laser welding or the electron beam of the electron beam welding is moved from the inside to the outside of the outer edge of the plurality of members constituting the welded product 1 to form the welded portion W. In the overlap welding process P4, as shown in Fig. 10, a third portion W33, a fourth portion W34, etc., which are other welded portions W that overlap an end portion W312, etc., of one welded portion W, are formed. In the end surrounding process P5, as shown in Figs. 12 and 13, end portions W342, W432 of the welded portions W are formed in an area surrounded by the first portion W31, etc., which are welded portions W that define the internal space 2.
[0069] With this configuration, the manufacturing method P of the welded product of this embodiment does not require a preparation work for forming a filler metal coating as in the conventional joining method of aluminum members described above, and the welding can be simplified. In addition, the manufacturing method P of the welded product of this embodiment does not require friction stir welding as in the conventional bus bar described above, so it is easy to apply even if the number of welds relative to the area of the members constituting the welded product 1 increases. In addition, by forming the end points W12, W22 of the welded part W on the outside of the welded part W surrounding the internal space 2 of the welded product 1 by the outer end process P2, it is possible to prevent cracks from affecting the internal space 2 of the welded product 1 even if they occur at the end points W12, W22 of the linear welded part W. In addition, as shown in FIG. 6 or FIG. 8, by not forming the end points W12, W22 of the welded part W on the members constituting the welded product 1 by the outer edge intersection process P3, it is possible to prevent cracks from affecting the internal space 2 of the welded product 1 even if they occur at the end points W12, W22 of the welded part W. 10 and 13, by forming another weld W overlapping the end points W312, W322, W332, W412, and W422 of the weld W by the overlap welding process P4, it is possible to repair the cracks that have occurred in the end points W312, W322, W332, W412, and W422. Therefore, it is possible to prevent the cracks that have occurred in the end points W312, W322, W332, W412, and W422 from affecting the internal space 2 of the welded product 1. Also, as shown in FIG. 12 and 13, by forming the end points W342 and W432 of the weld W in the area surrounded by the weld W that divides the internal space 2 by the end surrounding process P5, it is possible to prevent the cracks that have occurred in the end points W342 and W432 from affecting the internal space 2 of the welded product 1.
[0070] Furthermore, the manufacturing method P of the welded product of this embodiment includes at least an outer termination step P2 or an outer edge intersection step P3. With this configuration, the manufacturing method P of the welded product of this embodiment can form a peripheral weld W1 surrounding an internal space 2 on the peripheral part of the upper plate 4 as a weld W in the welded product 1, as shown in Fig. 4. Also, with this configuration, a flow path forming weld W2 that partitions the internal space 2 and forms a coolant flow path in the welded product 1 can be formed in a peninsula-shaped flat part 41 extending from the peripheral part to the center of the upper plate 4.
[0071] Furthermore, the manufacturing method P of the welded product of this embodiment includes at least an overlap welding step P4 and an end surrounding step P5. With this configuration, the manufacturing method P of the welded product of this embodiment can form, as welds W, flow path forming welds W3 and flow path forming welds W4 that define the internal space 2 and form a refrigerant flow path in the welded product 1 in the island-shaped flat portion 41 surrounded by the bulging portion 42 of the upper plate 4, as shown in Fig. 4.
[0072] In the manufacturing method P of the welded product of this embodiment, the circumferential weld W1 of the weld W has, for example, a straight portion W13 extending linearly and a bent portion W14 formed between the straight portions W13, W13 extending in different directions. The angle between the straight portions W13, W13 on both sides of the bent portion W14 is 90 degrees or more. With this configuration, the manufacturing method P of the welded product of this embodiment can reduce the thermal stress acting on the weld W from the non-welded portion of the upper plate 4 and the lower plate 3 between the straight portions W13, W13 extending in different directions, and prevent cracks from occurring in the weld W. The same is true for the flow passage weld W2, the flow passage weld W3, and the flow passage weld W4 other than the circumferential weld W1 of the weld W.
[0073] As described above, according to this embodiment, it is possible to provide a manufacturing method P for a welded product that is easy to apply even when the number of welding points is increased, that involves simple welding, and that can prevent weld cracks that occur at the end point W12 of the linear weld W, etc., from affecting the internal space 2 of the welded product 1.
[0074] The above describes in detail an embodiment of the method for manufacturing a welded product according to the present disclosure using the drawings. However, the specific configuration is not limited to this embodiment, and even if there are design changes and the like within the scope of the gist of the present disclosure, they are included in the present disclosure. [Explanation of symbols]
[0075] 1 Welded parts 2. Interior space 3 Lower plate (component) 4 Upper plate (component) P Manufacturing method of welded products P1 Circumferential welding process P2 Outer end process P3 Outer edge intersection process P4 Duplicate welding process P5 End enclosing process W Welding W1 Circumferential weld (weld) W12 End W13 Straight section W14 Bend W2 Flow passage weld (weld) W22 End W23 Straight section W24 Bend W3 Flow passage weld (weld) W312 End W313 Straight section W314 Bent part W322 End W323 Straight section W324 Bent part W332 End W333 Straight section W334 Bent part W342 End W4 Flow passage weld (weld) W412 End W413a Straight section W413b Straight section W413c Straight section W414a bent part W414b Bend part W422 End W423a Straight section W423b Straight section W423c Straight section W424a Bend part W424b Bent part W432 End W433a Straight section W433b Straight section W434 Bend
Claims
1. A method for manufacturing a welded product comprising the steps of: welding a plurality of members by laser welding or electron beam welding to form a welded portion and manufacturing a welded product having an internal space, the method comprising the steps of: a peripheral welding step of forming the weld surrounding the internal space; A method for manufacturing a welded product, further comprising at least the overlap welding process and the end surrounding process, among an outer termination process of forming an end point of the weld outside the weld surrounding the internal space, an outer edge intersection process of forming the weld by moving the laser of the laser welding or the electron beam of the electron beam welding from the inside to the outside of the outer edge of the multiple components to form the weld, an overlap welding process of forming another weld overlapping the end point of one of the welds, and an end surrounding process of forming the end point of the weld in an area surrounded by the welds that partition the internal space.
2. The welded portion has a straight portion extending linearly and a bent portion formed between the straight portions extending in different directions, 2. The method for manufacturing a welded product according to claim 1, wherein an included angle between the straight portions on both sides of the bent portion is 90 degrees or more.
Citation Information
Patent Citations
Welding method and laser sealing method for battery
CN1986139A
Butt welding method for aluminum thin plate
JP1987286680A
Method for joining aluminum member by laser beam welding
JP1995100675A
Manufacture of rectangular battery
JP1999167904A
Welded structure, process and equipment for welding
JP2003290951A