Method for producing positive electrode active material for non-aqueous electrolyte secondary battery, and molded body

A high-density molded body formation and controlled firing process for lithium-nickel composite oxide addresses productivity and heat conduction issues, achieving faster production and improved battery performance with high crystallinity and efficiency.

JP7586152B2Active Publication Date: 2024-11-19SUMITOMO METAL MINING CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022133091
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-08-24
Publication Date
2024-11-19
Estimated Expiration
2038-03-28

AI Technical Summary

Technical Problem

Existing methods for producing lithium-nickel composite oxide for non-aqueous electrolyte secondary batteries face challenges with low productivity and poor heat conduction, leading to prolonged firing times and reduced yield due to inefficient gas exchange during the firing process.

Method used

A method involving the formation of a high-density molded body with a specific atomic ratio of lithium, nickel, cobalt, and aluminum, fired at controlled temperatures in an oxidizing atmosphere without a binder, and using a plate-like member for improved gas exchange, followed by crushing and washing to enhance crystallinity and productivity.

Benefits of technology

The method achieves a lithium-nickel composite oxide with high crystallinity and improved productivity, allowing for faster firing times and higher yield, resulting in better battery performance with enhanced charge/discharge efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586152000004
    Figure 0007586152000004
  • Figure 0007586152000005
    Figure 0007586152000005
  • Figure 0007586152000006
    Figure 0007586152000006
Patent Text Reader

Abstract

The present invention aims to provide a simple method for producing a positive electrode active material having high crystallinity with higher productivity. SOLUTION: A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery containing a lithium nickel composite oxide includes mixing a nickel composite oxide with a lithium compound to obtain a lithium mixture, and molding the lithium mixture to obtain a positive electrode active material having a density of 1.3 g / cm. 3 and a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, the method comprising: obtaining the above-described molded body; and firing the molded body at 650°C or higher and 850°C or lower in an oxidizing atmosphere.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, and a molded article. [Background technology]

[0002] In recent years, with the widespread use of mobile devices such as mobile phones and laptop computers, there is a strong demand for the development of small, lightweight secondary batteries with high energy density. In addition, in the field of eco-friendly vehicles known as xEVs, there is a shift from hybrid electric vehicles (HEVs) to plug-in hybrid electric vehicles (PHEVs) and battery electric vehicles (BEVs), which require high-capacity secondary batteries. BEVs have a shorter driving distance on a single charge than gasoline-powered vehicles, and there is a demand for high-capacity secondary batteries to improve this.

[0003] As a secondary battery that satisfies such requirements, there is a positive electrode active material for a non-aqueous electrolyte secondary battery, and a representative secondary battery is a lithium ion secondary battery. This lithium ion secondary battery is composed of a negative electrode, a positive electrode, an electrolyte, etc., and the active materials for the negative electrode and the positive electrode are made of materials that can extract and insert lithium.

[0004] Lithium-ion secondary batteries are currently the subject of vigorous research and development. In particular, lithium-ion secondary batteries that use layered or spinel-type lithium metal composite oxides as the positive electrode material are capable of achieving a high voltage of around 4 V, and are therefore being put into practical use as batteries with high energy density.

[0005] The main materials that have been proposed so far are lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), and lithium nickel cobalt manganese composite oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) and lithium manganese composite oxide (LiMn2O4) that uses manganese.

[0006] Among these, lithium nickel composite oxide (LiNiO2) has attracted attention as a material that has high capacity and high output and meets the characteristics required for the positive electrode active material of the secondary batteries of future environmentally friendly automobiles, and demand is rapidly expanding.

[0007] Furthermore, with the recent expansion of demand for XEVs, there is a demand for lower prices, which is driving up the demand for lower costs of secondary batteries, one of the factors that make up the high cost of environmentally friendly vehicles.

[0008] The lithium nickel composite oxide can be obtained by mixing a nickel-containing compound such as a nickel composite hydroxide or a nickel composite oxide with a lithium compound to prepare a lithium mixture (raw material mixture), and then calcining the lithium mixture. The lithium mixture is calcined, for example, at a temperature of about 650°C to 850°C for 3 hours or more. During this calcination process, the lithium compound reacts (sinters) with the nickel-containing compound to obtain a lithium nickel composite oxide having high crystallinity.

[0009] In general, the lithium mixture is calcined by putting the lithium mixture powder in a container such as a sagger and calcining it in a calcination furnace. However, when the powder is calcined in a container, the thermal conductivity is poor and the exchangeability between the generated gas and the reaction gas is also poor, so that in order to produce a lithium nickel composite oxide having high crystallinity, a long heating and reaction time is required, and the total calcination time including these becomes very long.

[0010] Several proposals have been made so far regarding the sintering conditions for efficiently sintering the lithium mixture powder.

[0011] For example, Patent Document 1 discloses a method for firing a mixture (powder) obtained by mixing a nickel composite compound and a lithium compound in a firing vessel, filling the resulting mixture (powder) into the firing vessel and firing the mixture as efficiently as possible by specifying a minimum holding time for which the mixture is held in a specific temperature range relative to the pile amount of the mixture (the thickness of the mixture when placed in the firing vessel) and a range of oxygen concentration, in order to sufficiently diffuse oxygen into the mixture.

[0012] Also disclosed are several methods in which a lithium mixture is granulated to obtain a granulated product or molded to obtain a compact, and then calcined to obtain a lithium nickel composite oxide.

[0013] For example, Patent Document 2 describes a method for producing a LiNiO2-based layered composite oxide, which is characterized in that at least a nickel salt and a lithium salt are mixed in a predetermined amount to prepare a raw material mixture, and the raw material mixture is fired to synthesize LiNiO2, and the raw material mixture is granulated and the granulated material obtained is fired. In addition, an example of Patent Document 2 describes that granulated material of about 0.5 mm in an alumina container is charged into a firing furnace, and then the temperature is raised to 700°C while introducing an oxidizing gas, and the furnace is held for 24 hours to obtain a fired composite material. According to Patent Document 2, the above production method can produce a composite material having a desired crystal structure with good productivity, including in terms of workability.

[0014] Patent Document 3 also describes that a raw material mixture containing a lithium raw material is granulated and formed into a compact, which is then sintered at a temperature of 700°C to 1000°C for 2 to 15 hours in an oxidizing atmosphere to synthesize a lithium composite oxide. 2 It is described that the mixture was molded under a pressure of 1000 MPa to form pellets, and the pellets were fired in a pure oxygen atmosphere at 800°C for 10 hours.

[0015] In addition, in the examples of Patent Document 4, the mixed powder of the raw materials is pressed into a compact with a diameter of 50 mm and a thickness of 5 mm under a pressure of 500 kg / cm. 2It is described in Patent Document 4 that the press molding is performed at 740° C., pieces of an alumina spacer having a thickness of 1 mm are sandwiched between appropriate positions of the pressed compact, and the compact is fired at 740° C. for 10 hours, and then the compact is fired by holding it as it is for 20 hours at 820° C. According to Patent Document 4, press molding is extremely useful in that it shortens the distance of intermolecular movement and promotes crystal growth during firing.

[0016] Patent Document 5 also describes a method of forming a slurry from a raw material containing a lithium compound, spray-drying or freeze-drying the slurry, and then pressing the resulting dried product into a molded product, which is then fired. In the examples of Patent Document 5, a dry gel is compressed to 2 t / cm using a static compressor. 2 It is described that the mixture was pressed into pellets measuring φ14 and 2 mm in thickness, which were then placed in an alumina boat and fired in a tubular furnace in an oxygen atmosphere at 750° C. for 48 hours. [Prior art documents] [Patent documents]

[0017] [Patent Document 1] JP 2011-146309 A [Patent Document 2] JP 2000-072446 A [Patent Document 3] Japanese Patent Application Publication No. 11-135123 [Patent Document 4] Japanese Patent Application Publication No. 06-290780 [Patent Document 5] International Publication No. 98 / 06670 Summary of the Invention [Problem to be solved by the invention]

[0018] However, in the technology described in Patent Document 1, if the amount of mixed powder is increased in order to increase productivity, the time required to heat the mixture is extended, and the replacement of the evolved gas with the reactive gas becomes poor, which lengthens the firing time and limits productivity.

[0019] In addition, in the technique described in Patent Document 2, since the granulated product is packed in a container and fired, heat conduction may not be sufficient. Further, in the case of the powder of the lithium mixture or the granulated product having a particle size of less than 1 mm as described in Patent Document 2, for example, when the flow rate of the atmospheric gas in the firing furnace is increased to improve the firing efficiency, the powder or the granulated product may fly up from the container, resulting in a decrease in the yield.

[0020] Furthermore, in the techniques described in Patent Documents 3 to 5, although a larger molded body is formed and fired, the firing conditions specifically disclosed as examples require a firing time of 10 hours or more, so there is a problem of poor productivity.

[0021] In view of the above problems, an object of the present invention is to provide a simple manufacturing method of a positive electrode active material having higher productivity and high crystallinity, and a molded body that can be suitably used in the manufacturing method.

Means for Solving the Problems

[0022] According to a first aspect of the present invention, there is provided a method for manufacturing a positive electrode active material for a non-aqueous electrolyte secondary battery containing a lithium nickel composite oxide, comprising obtaining a lithium mixture by mixing a nickel composite oxide and a lithium compound, molding the lithium mixture to obtain a molded body having a density of 1.3 g / cm 3 or more, and firing the molded body at 650°C or higher and 850°C or lower in an oxidizing atmosphere, wherein the lithium nickel composite oxide contains lithium (Li), nickel (Ni), cobalt (Co), and aluminum (Al), and the atomic number ratio of each element is Li:Ni:Co:Al = s:(1-x-y):x:y (where 0.93 < s < 1.03, 0.03 ≤ x ≤ 0.10, 0.03 ≤ y ≤ 0.10), and a method for manufacturing a positive electrode active material for a non-aqueous electrolyte secondary battery is provided.

[0023] In addition, the lithium compound is composed of lithium hydroxide having a moisture content of 1.5% or less and total carbon of 1.0% or less, and the molded body may not contain a binder. Further, the density of the molded body is 1.4 g / cm 3The above may be applicable. Also, the maximum value of the distance between two points on the outer shape of the molded body may be 1 mm or more. Further, the firing may be performed by placing the molded body on a plate-like member disposed in a firing furnace. Further, it may include crushing the fired product after firing. Further, it may include washing the fired product after crushing with water and drying it. Further, in the firing, the holding time of the firing temperature may be 3 hours or less. Further, the lithium nickel composite oxide contains lithium (Li), nickel (Ni), cobalt (Co), aluminum (Al), and other element M, and the atomic ratio of each element is Li:Ni:Co:Al:M = s:(1-x-y):x:y:z (where 0.93 < s < 1.03, 0.03 ≤ x ≤ 0.10, 0.03 ≤ y ≤ 0.10, 0 < z ≤ 0.1, and M is an element other than Li, Ni, Co, Al, and O). Further, 5 g of the lithium nickel composite oxide is dispersed in 100 ml of pure water, and the amount of lithium eluted in the supernatant after standing for 10 minutes may be 0.11 mass% or less with respect to the total amount of the lithium nickel composite oxide. Further, the lithium nickel composite oxide may have a lithium site occupancy rate of 97.0% or more at the 3a site obtained from the Rietveld analysis of the X-ray diffraction pattern.

[0024] According to the first aspect of the present invention, it includes nickel (Ni), cobalt (Co), and aluminum (Al), and the molar ratio of each element is represented by Ni:Co:Al = (1-x-y):x:y (0.03 ≤ x ≤ 0.10, 0.03 ≤ y ≤ 0.10). The nickel composite oxide, Lithium hydroxide with a moisture content of 1.5% or less and total carbon of 1.0% or less, and does not contain a binder. The maximum value of the distance between two points on the outer shape is 1 mm or more, and the density is 1.3 g / cm 3 The above, a molded body is provided.

Advantages of the Invention

[0025] According to the present invention, it is possible to provide a simple manufacturing method of a cathode active material with higher productivity and high crystallinity, and a molded body that can be suitably used in the manufacturing method.

Brief Description of the Drawings

[0026] [Figure 1] FIG. 1 is a diagram showing an example of a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery. [Diagram 2] FIG. 2 is a diagram showing an example of a method for producing a nickel composite oxide. [Diagram 3] 3(A) to (D) are diagrams showing an example of a molded body. [Figure 4] FIG. 4(A) is a diagram showing an example of a molded body placed on a plate-like member, and FIG. 4(B) is a diagram showing an example in which a lithium mixture powder is placed in a container (housing). [Diagram 5] FIG. 5 is a diagram showing an example of a treatment process for the lithium-nickel composite oxide after firing. [Figure 6] FIG. 6 shows a secondary battery for evaluation used in the examples. [Figure 7] FIG. 7 is a graph showing the relationship between the density of the compact and the heating rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. However, the present invention is not limited to the embodiment described below. In the drawings, the invention may be represented diagrammatically or at a different scale as appropriate.

[0028] 1. Method for producing positive electrode active material for non-aqueous electrolyte secondary battery This embodiment is a method for manufacturing a positive electrode active material for a non-aqueous electrolyte secondary battery containing a lithium nickel composite oxide (hereinafter, also simply referred to as "positive electrode active material"). The lithium nickel composite oxide has an atomic ratio of lithium (Li), nickel (Ni), cobalt (Co), and aluminum (Al) represented by Li:Ni:Co:Al = s:(1 - x - y):x:y (where 0.93 < s < 1.03, 0.03 ≤ x ≤ 0.10, 0.03 ≤ y ≤ 0.10). Further, the lithium nickel composite oxide (hereinafter, also simply referred to as "composite oxide") has a crystal structure of a layered structure and may contain secondary particles formed by aggregation of primary particles.

[0029] Figure 1 is a diagram showing an example of a method for manufacturing a positive electrode active material according to this embodiment. As shown in Figure 1, the method for manufacturing a positive electrode active material includes, for example, obtaining a lithium mixture containing a nickel composite oxide and a lithium compound (mixing step: step S10), molding the lithium mixture to obtain a molded body (molding step: step S20), and firing the molded body (firing step: step S30). Hereinafter, each step will be described.

[0030] [Mixing step: step S10] First, a nickel composite oxide and a lithium compound are mixed to obtain a lithium mixture (step S10). By using a nickel composite oxide as a raw material in the manufacturing method of this embodiment, a highly crystalline lithium nickel composite oxide can be obtained with high productivity by firing for a very short time. Hereinafter, each raw material used in the mixing step (step S10) will be described.

[0031] (Nickel composite oxide) The nickel composite oxide is an oxide containing nickel, cobalt, and aluminum (hereinafter, also referred to as "nickel cobalt aluminum composite oxide"). Further, the nickel composite oxide may contain another element M in addition to nickel, cobalt, and aluminum, and examples of the other element M include molybdenum, tungsten, silicon, boron, niobium, vanadium, titanium, and the like.

[0032] The nickel composite oxide may contain, for example, nickel (Ni), cobalt (Co), and aluminum (Al), and the atomic ratio (molar ratio) of each element may be expressed as Ni:Co:Al=(1-xy):x:y (0.03≦x≦0.10, 0.03≦y≦0.10). The ratio of each element contained in the nickel composite oxide is inherited to the formed body and the lithium nickel composite oxide. Therefore, the composition of the entire nickel composite oxide can be made the same as the composition of metals other than lithium in the lithium nickel composite oxide to be obtained.

[0033] The nickel composite oxide may contain nickel (Ni), cobalt (Co), aluminum (Al), and another element M, and the atomic ratio (molar ratio) of each element may be expressed as Ni:Co:Al:M=(1-xy):x:y:z (0.03≦x≦0.10, 0.03≦y≦0.10, 0≦z≦0.10, M is an element other than Ni, Co, Al, and O). The element M may be, for example, at least one of molybdenum, tungsten, silicon, boron, niobium, vanadium, and titanium.

[0034] The nickel composite oxide can be obtained, for example, by oxidizing a nickel composite hydroxide used as a precursor of a positive electrode active material. When the nickel composite oxide is used, the amount of water vapor generated during the calcination of the lithium mixture is reduced, the reaction proceeds much more easily, and the calcination time can be significantly shortened. An example of a method for producing the nickel composite oxide is described below. The nickel composite oxide may be obtained by other methods.

[0035] Fig. 2 is a diagram showing an example of a method for producing a nickel composite oxide. For example, as shown in Fig. 2, a nickel composite oxide can be obtained by a method including oxidative roasting (step S2) of a nickel composite hydroxide obtained by crystallization (step S1). The nickel composite hydroxide obtained by crystallization has a uniform composition throughout the particles, and the composition of the finally obtained positive electrode active material is also uniform. The nickel composite oxide may be obtained by a method other than crystallization. Each step of producing a nickel composite oxide will be described below.

[0036] [Crystallization process; Step S1] The nickel composite hydroxide is obtained by supplying a neutralizing agent or the like to an aqueous solution containing a salt containing nickel (Ni salt), a salt containing cobalt (Co salt), and a salt containing aluminum (Al salt) and crystallizing (step S1). As a specific example, the nickel composite hydroxide can be produced by neutralizing an aqueous solution containing a nickel salt, a cobalt salt, and an aluminum salt with an alkaline aqueous solution in the presence of a complexing agent such as an ammonium ion donor while stirring the aqueous solution, thereby carrying out a crystallization reaction. The nickel composite hydroxide obtained by the crystallization method is composed of secondary particles formed by agglomeration of primary particles, and a positive electrode active material obtained by using this nickel composite hydroxide particle as a precursor is also composed of secondary particles formed by agglomeration of primary particles.

[0037] Examples of the metal salts used in preparing the aqueous solution containing the metal salts include sulfates, nitrates, and chlorides of Ni, Co, and Al. The aqueous solution of the metal salts may also contain a salt containing a metal M other than nickel, cobalt, and aluminum.

[0038] The nickel composite hydroxide can contain nickel (Ni), cobalt (Co), and optionally other metals (M), and the molar ratio of each element is preferably expressed as Ni:Co:Al:M=(1-xy):x:y:z (0.03≦x≦0.10, 0.03≦y≦0.10, 0≦z≦0.10). The ratio of each element contained in the nickel composite hydroxide is inherited to the nickel composite oxide, the formed body, and the lithium nickel composite oxide. Therefore, the composition of the entire nickel composite hydroxide can be made similar to the composition of metals other than lithium in the lithium nickel composite oxide to be obtained.

[0039] The crystallization method is not particularly limited, and for example, a continuous crystallization method, a batch method, or the like can be used. The continuous crystallization method is, for example, a method of continuously recovering nickel composite hydroxide overflowing from a reaction vessel, and can easily produce nickel composite hydroxide having the same composition in large quantities. In addition, the nickel composite oxide obtained by the continuous crystallization method has a wide particle size distribution, so that the packing density of a molded body obtained by using this can be improved. The particle size of the nickel composite hydroxide is, for example, 1 μm or more and 50 μm or less.

[0040] The batch method can obtain a nickel composite hydroxide having a more uniform particle size and a narrow particle size distribution. A molded body obtained by using the nickel composite hydroxide obtained by the batch method can react more uniformly with a lithium compound during firing. In addition, the nickel composite hydroxide obtained by the batch method can reduce the inclusion of fine powder, which is one of the causes of deterioration of cycle characteristics and output characteristics when used in a secondary battery.

[0041] [Oxidation roasting: Step S2] Next, the nickel composite hydroxide is subjected to oxidizing roasting (heat treatment) to obtain a nickel composite oxide (step S2). The conditions of the oxidizing roasting are not particularly limited as long as most of the nickel composite hydroxide is converted into the nickel composite oxide, but for example, the temperature of the oxidizing roasting is preferably 600°C or more and 800°C or less. If the temperature of the oxidizing roasting is less than 600°C, moisture may remain in the nickel composite hydroxide (precursor) and oxidation may not proceed sufficiently. On the other hand, if the temperature of the oxidizing roasting exceeds 800°C, the composite oxides may bond together to form coarse particles. In addition, if the temperature of the oxidizing roasting is too high, a lot of energy is used, and from the viewpoint of cost, productivity decreases, which is not industrially appropriate.

[0042] The time of the oxidizing roasting is preferably, for example, 0.5 hours or more and 3.0 hours or less. When the time of the oxidizing roasting is less than 0.5 hours, the oxidation of the nickel composite hydroxide may not proceed sufficiently. On the other hand, when the time of the oxidizing roasting is more than 3.0 hours, the energy cost increases and the productivity decreases, which is not industrially suitable.

[0043] (Lithium compounds) The lithium compound is not particularly limited, and any known lithium compound can be used, such as lithium hydroxide, lithium nitrate, lithium carbonate, lithium acetate, or a mixture thereof. Among these, lithium hydroxide and lithium carbonate are preferably used.

[0044] In addition, the lithium compound is preferably lithium hydroxide from the viewpoint of increasing the reactivity during sintering and shortening the firing time. Depending on the type of lithium compound, it may be necessary to add a binder to bind the particles together during mixing in order to form a molded body with sufficient strength, but when lithium hydroxide is used as the lithium compound, the particles are bound by the properties of lithium hydroxide, so that a binder is not required depending on the molding conditions. When the lithium mixture does not contain a binder, it is possible to further suppress the incorporation of impurities into the positive electrode active material.

[0045] The lithium hydroxide may be a hydrate such as lithium hydroxide monohydrate (LiOH HO) or an anhydrous such as anhydrous lithium hydroxide (LiOH). Of these, anhydrous lithium hydroxide is preferred, and lithium hydroxide with a moisture content of 1.5% or less and a total carbon (total carbon content) of 1.0% or less is more preferred.

[0046] Lithium hydroxide with a moisture content of 1.5% or less and a total carbon content of 1.0% or less can be obtained, for example, by heat treating lithium hydroxide hydrate (LiOH·HO). When such lithium hydroxide is used, the generation of moisture in the firing step (step S30) is suppressed, thereby accelerating the synthesis reaction of the lithium nickel composite oxide and shortening the firing time.

[0047] The moisture content is calculated by vacuum drying the lithium hydroxide to be measured at 200°C for 8 hours, and then measuring the weight before and after vacuum drying, with the moisture content of the obtained lithium hydroxide being set to 0% by mass. The moisture content is the amount including hydration water; for example, lithium hydroxide monohydrate has a moisture content of about 43% by mass. The total carbon (total carbon content) is a value that can be measured by high-frequency combustion-infrared absorption method.

[0048] (Lithium mixture) The nickel composite oxide and the lithium compound are mixed in such a ratio that the ratio (Li / Me ratio) of the total number of atoms (Me) of nickel, cobalt, and aluminum in the nickel composite oxide to the number of lithium atoms (Li) is in the range of more than 0.93 and less than 1.03. If the Li / Me ratio is 0.93 or less, some of the nickel composite oxide may remain unreacted in the firing step (step S30), and sufficient battery performance may not be obtained. On the other hand, if the Li / Me ratio is 1.03 or more, sintering may be promoted in the firing step (step S30), making the fired product hard and difficult to crush, or the particle size and crystallite size of the resulting lithium nickel composite oxide may become too large, and sufficient battery performance may not be obtained.

[0049] Since the required value of the Li / Me ratio varies depending on the configuration of the secondary battery, the value of the Li / Me ratio can be appropriately set within the above range according to the requirement. The value of the Li / Me ratio may be, for example, 0.95 or more and less than 1.03, 1.0 or more and less than 1.03, or more than 1.0 and less than 1.03.

[0050] In addition, since the Li / Me ratio is almost unchanged before and after the firing step (step S30), the Li / Me ratio in the lithium mixture is almost maintained in the lithium nickel composite oxide. Therefore, the mixing ratio of the nickel composite oxide and the lithium compound can be appropriately adjusted so that it is the same as the Li / Me ratio in the lithium nickel composite oxide to be obtained.

[0051] A general mixer can be used to mix the nickel composite oxide and the lithium compound, such as a shaker mixer, a Loedige mixer, a Julia mixer, or a V blender. This mixing should be sufficient so long as the nickel composite oxide is not destroyed. If the mixing is not sufficient, the Li / Me ratio may vary between individual particles, resulting in problems such as insufficient battery characteristics.

[0052] (binder) The lithium mixture may contain a binder. When the lithium mixture contains a binder, the moldability of the lithium mixture is improved, and molded bodies of various shapes can be easily formed. For example, when lithium carbonate is used as the lithium compound, a molded body having sufficient strength can be easily obtained by containing a binder. As the binder, a known binder can be used, for example, polyvinyl alcohol, polyacrylamide, carboxymethyl cellulose, etc. can be used. Among these, it is preferable to use polyvinyl alcohol.

[0053] The content of the binder in the lithium mixture can be, for example, 0.05% by mass or more and 0.2% by mass or less, preferably 0.08% by mass or more and 0.12% by mass or less, based on the total amount of the lithium mixture. When the content of the binder is within the above range, a molded body having an appropriate strength can be produced. When the content of the binder is too high, the adhesive strength of each particle constituting the molded body becomes too strong, and the efficiency of discharging the generated gas generated by the reaction between lithium and nickel composite oxide decreases, or the amount of carbon dioxide gas generated by the decomposition of the binder increases, and the generated gas cannot be discharged inside the molded body, so that the internal pressure of the molded body increases, and the molded body may be crushed.

[0054] The lithium mixture may not contain a binder. For example, when lithium hydroxide is used as the lithium compound, a molded body can be formed only from the nickel composite oxide and lithium hydroxide without using a binder. When no binder is used, the content of impurities (e.g., carbon, etc.) in the obtained lithium nickel composite oxide can be reduced.

[0055] [Formation of molded body: Step S20] The lithium mixture was then molded to a density of 1.3 g / cm 3 The above-mentioned molded body is obtained (Step S20). By molding and densifying in this way, the contact area between the particles of the lithium mixture increases, heat transfer improves, and the gaps between the particles are reduced, which makes it easier to discharge moisture and generated gases in the lithium mixture, and heat and reactive gases are efficiently supplied to the inside of the molded body, allowing efficient firing in a very short time.

[0056] (density of compact) The density of the molded body is preferably 1.3 g / cm 3 More preferably, it is 1.4 g / cm 3 The density of the molded body is 1.3 g / cm 3 If the density is less than 1.4 g / cm3, the strength of the molded product is low and it may crumble during handling. 3If the density is less than 1.0 g / cm, chipping may occur at the corners and edges, resulting in a decrease in yield. On the other hand, there is no particular upper limit to the density of the molded body, and the density may be set to a degree that allows the particle structure of the nickel composite oxide to be maintained, for example, 2.3 g / cm. 3 The density of the compact can be set within the above range by, for example, adjusting the surface pressure during the production of the compact.

[0057] The density of the molded body is, for example, 1.3 g / cm 3 More than 2.0g / cm 3 When the density of the molded body is within the above range, the heat transfer to the inside of the molded body in the firing step (step S30) is very good (see FIG. 7).

[0058] Furthermore, as described below, when crushing (step S40, see FIG. 5) after firing (step S30), if the density of the molded body is too high, the crushability after firing may be poor and the particle size distribution may become broad. Therefore, from the viewpoint of achieving both reactivity in the firing step (step S30) and crushability in the crushing step (step S40), the density of the molded body is preferably 1.4 g / cm. 3 More than 1.7g / cm 3 More preferably, it is 1.4 g / cm or less. 3 More than 1.6g / cm 3 or less, more preferably 1.4 g / cm 3 More than 1.5g / cm 3 The following is the result.

[0059] (Shape of Molded Product) Fig. 3 is a diagram showing an example of a molded body used in this embodiment. The shape of the molded body 10 is not particularly limited, and may be a briquette, pellet, tablet, plate, sphere, or the like. For example, as shown in Fig. 3(A) to Fig. 3(C), it may be approximately cylindrical or approximately elliptical, or as shown in Fig. 3(D), it may be plate-like. From the viewpoint of productivity, the shape of the molded body 10 is preferably plate-like, which has a high filling property in a firing device.

[0060] (Size of molded product) The size of the molded body is not particularly limited, and may be within a range in which the molded body can be formed. For example, when the maximum value of the distance between two points on the outer shape of the molded body is 1 mm or more, the yield in the manufacturing process of the molded body can be 90% or more. The upper limit of the size of the molded body is not particularly limited, and can be appropriately selected according to the shape inside the firing furnace. From the viewpoint of improving the handleability and productivity, the molded body preferably has a maximum value of the distance between two points on the outer shape of 10 mm or more and 1000 mm or less, more preferably 50 mm or more and 500 mm or less, and even more preferably 100 mm or more and 500 mm or less. In addition, as shown in the examples described later, molded bodies in which the distance between two points on the outer shape of the molded body is within the range of 100 mm or more and 500 mm or less have the same high thermal conductivity, so from the viewpoint of further improving the productivity, the maximum value of the distance between two points on the outer shape of the molded body may be 350 mm or more and 500 mm or less.

[0061] For example, as shown in FIG. 3(D), when the molded body 10 is plate-shaped, the thickness (t) of the molded body 10 is preferably 5 mm or more and 200 mm or less, more preferably 10 mm or more and 100 mm or less. The area of ​​the cross section perpendicular to the thickness direction of the molded body 10 is, for example, 10 mm 2 More than 1000mm 2 It may be less than 100 mm 2 More than 10000mm 2 It may be the following.

[0062] The apparatus for producing the compact is not particularly limited, and may be any apparatus capable of pressurizing the lithium mixture, such as a granulator, tablet press, briquette machine, press, etc. For example, when producing a plate-shaped compact having long and short sides of 10 mm to 100 mm and a thickness of 5 mm to 200 mm, it is preferable to use a hydraulic press.

[0063] The surface pressure during molding (step S20) is appropriately adjusted depending on the composition of the lithium mixture, the powder characteristics of the raw material, the shape of the molded body, etc. For example, when obtaining a plate-shaped molded body, the surface pressure during molding is 100 kg / cm 2 More than 2000kg / cm 2 or less, 150 kg / cm 2 More than 1500kg / cm 2 If the lithium mixture does not contain a binder, the surface pressure may be 200 kg / cm 2 It may be more than that.

[0064] [Firing: Step S30] Next, the obtained molded body is fired in an oxygen atmosphere at 650°C to 850°C (firing step, step S30). By firing the molded body, the nickel composite oxide reacts with the lithium compound to produce a lithium nickel composite oxide. By firing the above-mentioned molded body at the above temperature, it is possible to obtain a lithium nickel composite oxide (positive electrode active material) having high crystallinity equal to or higher than that of conventional materials in a time much shorter than that of conventional firing.

[0065] The firing conditions are not particularly limited as long as the nickel composite oxide in the compact reacts with the lithium compound to form the lithium nickel composite oxide. For example, it is preferable to gradually increase the temperature from room temperature and hold it at a temperature range of 650°C to 850°C for 3 hours or less. If the firing temperature is less than 650°C, lithium diffusion may not be sufficient, unreacted lithium compound particles may remain, or the crystal structure of the lithium nickel composite oxide may not be fully aligned, so that the secondary battery using the obtained positive electrode active material may not have sufficient battery characteristics. On the other hand, if the firing temperature is more than 850°C, intense sintering may occur between the lithium nickel composite oxide particles and abnormal grain growth may occur, resulting in a decrease in the specific surface area. In addition, the specific surface area of ​​the positive electrode active material may decrease, causing the resistance of the positive electrode in the secondary battery to increase and the battery capacity to decrease. The firing temperature can be appropriately adjusted according to the composition and shape of the compact, and may be 700°C to 800°C, or 730°C to 770°C.

[0066] The time for which the molded body is held at the above firing temperature (hereinafter also referred to as "holding time") is not particularly limited as long as a lithium nickel composite oxide having high crystallinity is formed, but is, for example, 5 hours or less, preferably 3 hours or less, more preferably 2.5 hours or less, and may be less than 2.5 hours. The shorter the firing time, the higher the productivity. The lower limit of the firing time is, for example, 1 hour or more, and may be 2 hours or more.

[0067] The temperature rise rate at the center of the molded article is not particularly limited and is, for example, 4° C. / min or more, and preferably 5° C. / min or more. The temperature rise rate at the center of the molded article can be measured by inserting a thermocouple into the center of the molded article.

[0068] The atmosphere during firing is preferably an oxidizing atmosphere having an oxygen concentration equal to or higher than that of the air atmosphere, more preferably an atmosphere having an oxygen concentration of 80% by volume or more, and may be 100% by volume. That is, firing is preferably carried out in an oxygen stream. If the oxygen concentration of the atmosphere during firing is less than 80% by volume, it may be impossible to supply the amount of oxygen necessary for the reaction between the nickel composite oxide and the lithium compound, and the lithium nickel composite oxide may not be sufficiently formed.

[0069] The firing furnace is not particularly limited, and may be any furnace capable of heating in an oxygen stream, such as a vertical furnace, a rotary hearth furnace, a roller hearth kiln, etc. Among these, it is preferable to use a roller hearth kiln from the viewpoint of capital investment and running costs.

[0070] Fig. 4(A) is a diagram showing a state in which a molded body 10 is placed on a plate-like member 1 during firing, and Fig. 4(B) is a diagram showing a state in which a lithium mixture powder 20 is placed in a container 2 during firing. Conventionally, when firing a lithium mixture powder 20 or a granulated material, the powder or granulated material is placed in a container 2 such as a sagger and fired, as shown in Fig. 4(B).

[0071] During firing, the molded body 10 may be placed in a container 2 as in the past, but the molded body 10 may be placed directly on a plate-like member 1 (e.g., a setter) arranged in a firing furnace without using the container 2. The setter is a member (furnace material) with which the molded body comes into contact in the firing furnace, and is preferably a plate-like member 1 such as a shelf or a floor plate on which the molded body can be placed, as shown in FIG. 4(A). When the plate-like member 1 is used without using the container 2, the contact area between the molded body 10 and the atmospheric gas can be increased, which can further promote the reaction between the precursor and the lithium compound, and the amount of raw material input into the firing furnace can be further increased.

[0072] FIG. 5 is a diagram showing an example of a process for treating the lithium nickel composite oxide obtained after calcination. As shown in FIG. 5, the method for producing a positive electrode active material according to this embodiment may include crushing the lithium nickel composite oxide (calcined product) obtained after the calcination process (step S30) to obtain a crushed product (powders of lithium nickel composite oxide) (crushing process: step S40), washing the crushed product with water and filtering it (water washing process: step S50), and drying the washed lithium nickel composite oxide (drying process: step S60). The method for producing a positive electrode active material according to this embodiment may not include the above-mentioned crushing (step S40), water washing (step S50), and drying process (step S60), or may include at least one of these three processes. Each process will be described below.

[0073] [Crushing process: Step S40] The lithium nickel composite oxide (calcined product) obtained after the calcination (step S30) may be further crushed (step S40). By crushing, secondary particles of the lithium nickel composite oxide in which aggregation or slight sintering has occurred can be separated from each other, and the average particle size and particle size distribution of the obtained positive electrode active material can be adjusted to a suitable range. In addition, when the molded body is fired, the obtained fired product maintains the shape at the time of molding, so it is preferable to crush it (step S40). Note that crushing refers to an operation of applying mechanical energy to aggregates consisting of multiple secondary particles generated by sintering necking between secondary particles during firing, separating them without destroying the secondary particles themselves, and loosening the aggregates.

[0074] As a crushing method, known means can be used, for example, a pin mill, a hammer mill, a crusher with a classification function, etc. In this case, it is preferable to adjust the crushing force within an appropriate range so as not to destroy the secondary particles. [Water washing process: Step S50] Next, the crushed material obtained may be washed with water (step S50). By washing the lithium nickel composite oxide (crushed material) with water, excess lithium and impurities on the surface of the lithium nickel composite oxide particles are removed, and a positive electrode active material for a non-aqueous electrolyte secondary battery having a higher capacity and higher thermal stability can be obtained. Here, the washing method is not particularly limited, and a known technique can be used.

[0075] As a method of washing with water, for example, the lithium nickel composite oxide (crushed material) is put into water to make a slurry, and the slurry is preferably stirred so that excess lithium on the particle surfaces of the lithium nickel composite oxide is sufficiently removed. After stirring, the slurry is separated into solid and liquid, and dried (step S60) as described later to obtain the lithium nickel composite oxide.

[0076] As for the slurry concentration, it is preferable to add 0.5 to 2 parts by mass of the lithium nickel composite oxide (crushed material) per 1 part by mass of water. If the amount of the crushed material added per 1 part by mass of water is more than 2 parts by mass, the viscosity becomes very high and stirring becomes difficult, and the alkalinity (pH) in the liquid is high, so that the dissolution rate of the attached matter slows down due to the equilibrium relationship, and even if peeling occurs, separation from the powder becomes difficult. On the other hand, if the amount of the crushed material added per 1 part by mass of water is less than 0.5 parts by mass, the slurry is too dilute, so that the amount of lithium elution is large, and lithium is also released from the crystal lattice of the lithium nickel composite oxide (crushed material), making the crystals more likely to collapse, and the high pH aqueous solution (slurry) absorbs carbon dioxide gas in the air, and lithium carbonate may be reprecipitated on the surface of the lithium nickel composite oxide.

[0077] The washing liquid used in the water washing step (step S50) is not particularly limited, and may be, for example, water. When water is used, for example, water with a measured electrical conductivity of less than 10 μS / cm is preferred, and water with a measured electrical conductivity of 1 μS / cm or less is more preferred. When water with a measured electrical conductivity of less than 10 μS / cm is used, the deterioration of battery performance due to adhesion of impurities to the positive electrode active material can be further suppressed.

[0078] When the slurry is subjected to solid-liquid separation, it is preferable that the amount of water remaining on the surface of the lithium nickel composite oxide particles is small. If the amount of water remaining is large, lithium dissolved in the liquid (slurry) may be reprecipitated, and the amount of lithium present on the surface of the lithium nickel composite oxide after drying (step S60) may increase. For solid-liquid separation, a commonly used centrifuge, filter press, etc. may be used.

[0079] [Drying process: Step S60] After washing with water (step S50), the lithium nickel composite oxide (positive electrode active material) may be obtained by drying (step S60). The drying conditions are not particularly limited as long as at least a portion of the moisture in the lithium nickel composite oxide is removed. The drying step (step S60) is preferably carried out at a predetermined temperature, for example, by using a dryer that can control the lithium nickel composite oxide (powder) after filtration (solid-liquid separation) under a gas atmosphere that does not contain compound components containing carbon and sulfur, or under a vacuum atmosphere.

[0080] The drying temperature is preferably 80° C. or higher and 550° C. or lower, and more preferably 120° C. or higher and 350° C. or lower. When the drying temperature is 80° C. or higher, the positive electrode active material after water washing (step S50) can be quickly dried, and the occurrence of a gradient in lithium concentration between the particle surface and the particle interior can be suppressed. On the other hand, when the drying temperature exceeds 550° C., the crystal structure near the surface of the lithium nickel composite oxide, which is expected to be very close to the stoichiometric ratio or to be in a state close to a charged state with some lithium desorbed, may collapse, which may lead to a deterioration in the battery characteristics of the secondary battery.

[0081] Moreover, the drying temperature is more preferably 120° C. or higher and 350° C. or lower from the viewpoints of productivity and heat energy costs.

[0082] [Characteristics of the positive electrode active material] By the method for producing a positive electrode active material according to the above-described embodiment, a lithium nickel composite oxide (positive electrode active material) excellent in crystallinity can be obtained with high productivity in a very short firing time. Hereinafter, the characteristics of the lithium nickel composite oxide (positive electrode active material) obtained by the production method according to this embodiment will be described.

[0083] (Composition) The lithium nickel composite oxide contains lithium (Li), nickel (Ni), cobalt (Co), and aluminum (Al), and the molar ratio of each metal element is Li:Ni:Co:Al = s:(1 - x - y):x:y (where 0.93 < s < 1.03, 0.03 ≤ x ≤ 0.10, 0.03 ≤ y ≤ 0.10).

[0084] Further, the lithium nickel composite oxide contains lithium (Li), nickel (Ni), cobalt (Co), aluminum (Al), and another element M, and the atomic ratio of each element is Li:Ni:Co:Al:M = s:(1 - x - y):x:y:z (where 0.93 < s < 1.03, 0.03 ≤ x ≤ 0.10, 0.03 ≤ y ≤ 0.10, 0 < z ≤ 0.1, and M is an element other than Li, Ni, Co, Al, and O).

[0085] Further, the lithium nickel composite oxide has a hexagonal crystal structure having a layered structure. For example, the general formula (1): Li s Ni 1-xーy Co x Al y M z O 2+α (However, in formula (1), 0.93 < s < 1.03, 0.03 ≤ x ≤ 0.10, 0.03 ≤ y ≤ 0.10, 0 ≤ z ≤ 0.10, -0.5 ≤ α ≤ 0.5, and M is at least one element selected from Mn, V, Mo, Nb, Ti, and W.) may be represented. Further, the element M may be, for example, at least one of molybdenum, tungsten, silicon, boron, niobium, vanadium, and titanium.

[0086] (Lithium site occupancy) The lithium nickel composite oxide has a lithium site occupancy of 95% or more, preferably 96% or more, more preferably 97% or more, and may be 98% or more, of the 3a site, which is a lithium-dominated layer, obtained by Rietveld analysis of an X-ray diffraction pattern, for example. When the lithium site occupancy is within the above range, the sintering reaction between the precursor and the lithium compound is sufficiently carried out in the firing step (step S30), and the lithium nickel composite oxide has high crystallinity. When a lithium nickel composite oxide with high crystallinity is used as a positive electrode active material for a secondary battery, it exhibits excellent battery characteristics (high battery capacity, etc.).

[0087] (amount of dissolved lithium) The lithium nickel composite oxide has an amount of lithium eluted into water when the lithium nickel composite oxide is dispersed in water (amount of eluted lithium) of, for example, 0.11% by mass or less, preferably 0.10% by mass or less, and more preferably 0.05% by mass or less, based on the total amount of the lithium nickel composite oxide. The amount of eluted lithium can be measured by neutralization titration. When a water washing step (step S50) is performed, the amount of eluted lithium is a value measured using the lithium nickel composite oxide obtained after water washing (step S50) and drying (step S60).

[0088] The eluted lithium is considered to originate from unreacted lithium compounds present on the particle surface of the lithium nickel composite oxide (positive electrode active material) and excess lithium present in the crystals. That is, the amount of eluted lithium can be used as an index showing the remaining amount of unreacted lithium compounds derived from the raw material, and it can be said that the smaller the amount of eluted lithium, the smaller the remaining amount of unreacted lithium compounds, and the more the sintering reaction between the precursor and the lithium compounds has progressed. In addition, the smaller the amount of eluted lithium, the more the gelation of the positive electrode composite paste can be suppressed.

[0089] The amount of eluted lithium is a value calculated by dispersing 15 g of lithium nickel composite oxide in 75 ml of pure water, leaving it to stand for 10 minutes, diluting 10 ml of the supernatant with 50 ml of pure water, and measuring the amount of lithium eluted in the water (amount of eluted lithium) by neutralization titration by adding 1 mol / L hydrochloric acid.

[0090] (Initial charge / discharge efficiency) In a 2032-type coin cell CBA (see FIG. 6) for evaluation, which is produced using a lithium nickel composite oxide as a positive electrode active material, the initial charge-discharge efficiency (initial discharge capacity / initial charge capacity) is, for example, 85% or more, preferably 89% or more, and more preferably 89.5% or more. When the initial charge-discharge efficiency is within the above range, it indicates that the sintering reaction between the precursor and the lithium compound is sufficiently carried out in the firing step (step S30), and that the lithium nickel composite oxide has high crystallinity. The initial discharge capacity efficiency was measured by leaving the coin cell CBA used in the examples for about 24 hours after production, and after the open circuit voltage OCV (Open Circuit Voltage) stabilized, applying a current density of 0.1 mA / cm to the positive electrode. 2 The capacity was measured when the battery was charged to a cut-off voltage of 4.3 V, then allowed to rest for one hour, and then discharged to a cut-off voltage of 3.0 V.

[0091] 2. Molded body The molded body according to the present embodiment includes a nickel composite oxide and lithium hydroxide. The molded body according to the present embodiment can be suitably used as a positive electrode active material for a secondary battery by sintering the molded body to form a lithium nickel composite oxide.

[0092] The nickel composite oxide contains nickel (Ni), cobalt (Co), and aluminum (Al), and the molar ratio of each element is expressed as Ni:Co:Al=(1-xy):x:y (0.03≦x≦0.10, 0.03≦y≦0.10). The composition and characteristics of the nickel composite oxide are similar to the metal elements contained in the nickel composite oxide in the above-mentioned method for producing a positive electrode active material, and therefore will not be described here.

[0093] The lithium hydroxide preferably has a moisture content of 1.5% or less and a total carbon content of 1.0% or less. When the moisture content is 1.5% or less, the amount of moisture generated during firing is reduced, and the reaction between the nickel composite oxide and the lithium compound can proceed efficiently. In addition, lithium hydroxide may react with carbon dioxide in the air to form lithium carbonate, for example, and when the total carbon content is within the above range, a positive electrode active material with a reduced amount of impurities can be obtained.

[0094] As described above, the molded body according to the present embodiment does not include a binder. As described above, the molded body contains lithium hydroxide having a moisture content of 1.5% or less and a total carbon content of 1.0% or less as a raw material, so that the molded body can have sufficient strength even without a binder. In addition, when the molded body does not contain a binder, a positive electrode active material with a reduced amount of impurities can be obtained.

[0095] In addition, the molded article according to this embodiment has a maximum distance between two points on the outer shape of 1 mm or more and a density of 1.3 g / cm 3 The preferred ranges for the shape and density of the molded body are the same as those for the molded body in the above-mentioned method for producing a positive electrode active material, and therefore description thereof will be omitted.

[0096] 3.Nonaqueous electrolyte secondary battery The method for producing a non-aqueous electrolyte secondary battery according to this embodiment (hereinafter also referred to as "method for producing a secondary battery") includes obtaining a non-aqueous electrolyte secondary battery using a positive electrode, a negative electrode, and a non-aqueous electrolyte, and the positive electrode is obtained using the positive electrode active material obtained by the above-mentioned production method. The secondary battery obtained by the production method according to this embodiment may include, for example, a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte solution, or may include a positive electrode, a negative electrode, and a solid electrolyte. The secondary battery may also be composed of the same components as a known lithium ion secondary battery.

[0097] Hereinafter, as an example of the method for producing a secondary battery according to this embodiment, each constituent material of a secondary battery using a non-aqueous electrolyte solution and the method for producing the same will be described. Note that the embodiment described below is merely an example, and the method for producing a secondary battery can be carried out in a form in which various modifications and improvements have been made based on the embodiment described in this specification and on the knowledge of those skilled in the art. In addition, the use of the secondary battery obtained by the production method according to this embodiment is not particularly limited.

[0098] (positive electrode) The positive electrode contains the above-mentioned positive electrode active material. The positive electrode can be manufactured, for example, as follows. Note that the method for manufacturing the positive electrode is not limited to the following example, and other methods may be used.

[0099] First, the positive electrode active material, conductive material, and binder are mixed, and activated carbon and a solvent for viscosity adjustment, etc. are added as necessary, and the mixture is kneaded to prepare a positive electrode composite paste. Note that the constituent materials of the positive electrode composite paste are not particularly limited, and materials equivalent to known positive electrode composite pastes may be used.

[0100] The mixing ratio of each material in the positive electrode composite paste is not particularly limited and is adjusted appropriately according to the required performance of the secondary battery. The mixing ratio of the materials can be in the same range as that of the positive electrode composite paste of a known secondary battery, and for example, when the total mass of the solid content of the positive electrode composite excluding the solvent is 100 parts by mass, the content of the positive electrode active material may be 60 parts by mass or more and 95 parts by mass or less, the content of the conductive material may be 1 part by mass or more and 20 parts by mass or less, and the content of the binder may be 1 part by mass or more and 20 parts by mass or less.

[0101] As the conductive agent, for example, graphite (natural graphite, artificial graphite, expanded graphite, etc.), acetylene black, Ketjen black, and other carbon black-based materials can be used.

[0102] The binder serves to bind the active material particles together, and examples of the binder that can be used include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene butadiene, cellulose-based resin, and polyacrylic acid.

[0103] If necessary, a solvent for dispersing the positive electrode active material, conductive material, and activated carbon and dissolving the binder (binding agent) may be added to the positive electrode mixture paste. Specifically, an organic solvent such as N-methyl-2-pyrrolidone (NMP) may be used as the solvent. Activated carbon may be added to the positive electrode mixture in order to increase the electric double layer capacity.

[0104] Next, the obtained positive electrode composite paste is applied to the surface of a current collector made of, for example, aluminum foil, dried, and the solvent is removed to prepare a sheet-shaped positive electrode. If necessary, pressure may be applied by a roll press or the like to increase the electrode density. The sheet-shaped positive electrode can be cut to an appropriate size according to the desired battery and used to prepare the battery.

[0105] (Negative electrode) The negative electrode may be made of metallic lithium, a lithium alloy, etc. The negative electrode may be made by mixing a binder with a negative electrode active material capable of absorbing and desorbing lithium ions, adding an appropriate solvent to the negative electrode mixture to make a paste, applying the paste to the surface of a metal foil current collector such as copper, drying the paste, and compressing the paste to increase the electrode density as necessary.

[0106] As the negative electrode active material, for example, natural graphite, artificial graphite, a calcined organic compound such as phenolic resin, or a powder of a carbon material such as coke can be used. As the negative electrode binder, a fluorine-containing resin such as PVDF can be used, as in the positive electrode. As the solvent for dispersing these active materials and binders, an organic solvent such as N-methyl-2-pyrrolidone can be used.

[0107] (Separator) A separator is sandwiched between the positive electrode and the negative electrode. The separator separates the positive electrode and the negative electrode and retains the electrolyte. A thin membrane made of polyethylene, polypropylene, or the like and having many minute pores can be used as the separator.

[0108] (Non-aqueous electrolyte) The non-aqueous electrolyte solution is a solution of a lithium salt as a supporting salt dissolved in an organic solvent. The organic solvent may be selected from cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and trifluoropropylene carbonate, chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate, ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane, sulfur compounds such as ethyl methyl sulfone and butane sultone, and phosphorus compounds such as triethyl phosphate and trioctyl phosphate, either alone or in combination.

[0109] The supporting salt may be LiPF6, LiBF4, LiClO4, LiAsF6, LiN(CF3SO2)2, or a composite salt thereof. Furthermore, the non-aqueous electrolyte may contain a radical scavenger, a surfactant, a flame retardant, or the like.

[0110] (Battery shape and configuration) The shape of the nonaqueous electrolyte secondary battery of this embodiment, which is composed of the positive electrode, negative electrode, and nonaqueous electrolyte described above, can be various, such as a cylindrical type, a laminated type, etc. Regardless of the shape, the positive electrode and the negative electrode are laminated via a separator to form an electrode body, the obtained electrode body is impregnated with a nonaqueous electrolyte solution, and the positive electrode current collector and the positive electrode terminal leading to the outside, and the negative electrode current collector and the negative electrode terminal leading to the outside are connected using a current collector lead or the like, and the battery case is sealed to complete the nonaqueous electrolyte secondary battery. In addition, when a solid electrolyte is used, the solid electrolyte may also serve as a separator. EXAMPLES

[0111] Hereinafter, the present invention will be specifically described using examples, but the present invention is not limited by these examples. The performance (stability of the paste, initial discharge capacity, positive electrode resistance, discharge capacity retention rate) of the positive electrode active material obtained by this embodiment, the positive electrode composite paste using this positive electrode active material, and the non-aqueous electrolyte secondary battery was measured. In this embodiment, each sample of special grade reagents manufactured by Wako Pure Chemical Industries, Ltd. was used for the production of the composite hydroxide, the positive electrode active material, and the secondary battery.

[0112] [Production and evaluation of secondary batteries for evaluation] A 2032-type coin-type battery CBA (see FIG. 6) was produced by the following method, and the battery characteristics of the positive electrode active material were evaluated.

[0113] (Making coin-cell batteries) 52.5 mg of the positive electrode active material, 15 mg of acetylene black, and 7.5 mg of polytetrafluoroethylene resin (PTFE) were mixed and pressed at a pressure of 100 MPa to produce a positive electrode PE (electrode for evaluation) with a diameter of 11 mm and a thickness of 100 μm. The produced positive electrode PE was dried in a vacuum dryer at 120 ° C for 12 hours. The dried positive electrode PE, negative electrode NE, separator SE, and electrolyte were used to produce a coin-type battery CBA shown in Figure 6 in a glove box in an Ar atmosphere with a dew point controlled at -80 ° C.

[0114] The negative electrode NE was a negative electrode sheet in which graphite powder with an average particle size of about 20 μm and polyvinylidene fluoride were applied to copper foil, punched into a disk shape with a diameter of 14 mm, and the electrolyte was an equal mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) (manufactured by Toyama Pharmaceutical Co., Ltd.) with 1M LiPF6 as the supporting electrolyte. A polyethylene porous film with a thickness of 25 μm was used for the separator SE. The coin-type battery CBA had a gasket GA and a wave washer WW, and was assembled into a coin-type battery with a positive electrode can PC and a negative electrode can NC.

[0115] (Initial discharge capacity) The initial discharge capacity was measured by leaving the coin cell CBA for about 24 hours after production, and after the open circuit voltage OCV (Open Circuit Voltage) had stabilized, applying a current density of 0.1 mA / cm to the positive electrode. 2 The battery was charged to a cut-off voltage of 4.3 V, and after one hour of rest, the capacity at which the battery was discharged to a cut-off voltage of 3.0 V was defined as the initial discharge capacity.

[0116] [Lithium dissolution titration] 15 g of the obtained lithium nickel composite oxide (positive electrode active material) was dispersed in 75 ml of pure water and then allowed to stand for 10 minutes. 10 ml of the supernatant was diluted with 50 ml of pure water, and the amount of lithium dissolved in the water (amount of dissolved lithium) was measured by neutralization titration by adding 1 mol / L hydrochloric acid.

[0117] Example 1 A nickel composite hydroxide with a composition ratio of Ni:Co:Al = 88:9:3 was oxidized and roasted in a rotary kiln to obtain a nickel composite oxide, which was then mixed with lithium hydroxide with a moisture content of 1.5% or less and a total carbon content of 1.0% or less so that the Li / Me ratio was 1.03 to produce a lithium mixture. 290 g of the lithium mixture powder thus produced was placed in a 100 mm x 100 mm mold and pressed with a hydraulic press at a molding surface pressure of 290 kg / cm. 2 The molded product was pressed at 100° C. to produce a 20 mm thick molded product (maximum distance between two points on the outer shape: 143 mm). The density of the molded product was 1.45 g / cm 3 The produced compact was rapidly heated from room temperature to 760°C in a 90% oxygen atmosphere, and the heating rate at the center of the compact was measured and found to be 6.48°C / min.

[0118] Example 2 A nickel composite hydroxide with a composition ratio of Ni:Co:Al = 88:9:3 was oxidized and roasted in a rotary kiln to obtain a nickel composite oxide, which was then mixed with lithium hydroxide with a moisture content of 1.5% or less and a total carbon content of 1.0% or less so that the Li / Me ratio was 1.03 to produce a lithium mixture. 9135 g of the lithium mixture powder thus produced was placed in a 300 mm x 300 mm mold and pressed with a hydraulic press at a molding surface pressure of 300 kg / cm. 2The molded product was pressed at 430 mm in thickness and had a density of 1.45 g / cm. 3 The produced compact was rapidly heated from room temperature to 760°C in a 90% oxygen atmosphere, and the heating rate at the center of the compact was measured and found to be 6.01°C / min.

[0119] Example 3 A nickel composite hydroxide with a composition ratio of Ni:Co:Al = 88:9:3 was oxidized and roasted in a rotary kiln to obtain a nickel composite oxide, which was mixed with lithium hydroxide with a moisture content of 1.5% or less and a total carbon content of 1.0% or less so that the Li / Me ratio was 1.03 to produce a lithium mixture. 13,705 g of the lithium mixture powder thus produced was placed in a 300 mm x 300 mm mold and pressed with a hydraulic press at a molding surface pressure of 300 kg / cm. 2 The molded product was pressed at 437 mm in thickness and had a density of 1.45 g / cm. 3 The produced compact was rapidly heated from room temperature to 760°C in a 90% oxygen atmosphere, and the heating rate at the center of the compact was measured and found to be 5.68°C / min.

[0120] Comparative Example 1 A nickel composite oxide with a composition ratio of Ni:Co:Al = 88:9:3 was oxidized and roasted in a rotary kiln, and this nickel composite oxide was mixed with lithium hydroxide with a moisture content of 1.5% or less and a total carbon content of 1.0% or less so that the Li / Me ratio was 1.03 to produce a lithium mixture. 200g of the lithium mixture powder produced was placed in a 100mm x 100mm sagger (height of mound: approximately 20mm) and rapidly heated from room temperature to 760°C in a 90% oxygen atmosphere. The heating rate at the center of the compact was measured and found to be 5.62°C / min.

[0121] Comparative Example 2 A nickel composite oxide with a composition ratio of Ni:Co:Al=88:9:3 was oxidized and roasted in a rotary kiln, and this nickel composite oxide was mixed with lithium hydroxide with a moisture content of 1.5% or less and a total carbon content of 1.0% or less so that the Li / Me ratio was 1.03 to produce a lithium mixture. 9,450g of the lithium mixture powder produced was placed in a 300mm x 300mm sagger (height of mound: approximately 105mm) and rapidly heated from room temperature to 760°C in a 90% oxygen atmosphere. The heating rate at the center of the lithium mixture powder was measured and found to be 2.60°C / min.

[0122] [Table 1]

[0123] (Evaluation result 1) Table 1 shows the evaluation results of Examples 1 to 3 and Comparative Examples 1 and 2. From these evaluation results, it was found that by forming the lithium mixture powder into a compact, the heat transfer property is improved, and therefore, for the same thickness (pile height), the compact has a faster temperature rise rate despite the greater amount (weight) of the lithium mixture.

[0124] Example 4 The amount of lithium powder mixture was 8255g, and the molding pressure was 200kg / cm 2 A lithium mixture molded body was produced and sintered in the same manner as in Example 2, except that the furnace temperature was set to 6.00° C. / min and the furnace temperature increase rate was set to 6.00° C. / min. The lithium mixture molded body had a thickness of 70 mm and a density of 1.31 g / cm. 3 The temperature rise rate at the center of the compact was 5.08°C / min. However, about 20% of the compacts were cracked during handling after compaction.

[0125] Example 5 The amount of lithium powder mixture was 10140g, and the molding pressure was 500kg / cm 2 A lithium mixture molded body was produced and sintered in the same manner as in Example 2, except that the furnace temperature was set to 6.00° C. / min and the furnace temperature increase rate was set to 6.00° C. / min. The lithium mixture molded body had a thickness of 70 mm and a density of 1.61 g / cm.3 The temperature rise rate at the center of the compact was 5.05° C. / min. No cracks were found during handling after compaction.

[0126] Example 6 The amount of lithium powder mixture was 10900g, and the molding pressure was 750kg / cm 2 A lithium mixture molded body was produced and sintered in the same manner as in Example 2, except that the furnace temperature was set to 6.00° C. / min and the furnace temperature increase rate was set to 6.00° C. / min. The lithium mixture molded body had a thickness of 70 mm and a density of 1.73 g / cm. 3 The temperature rise rate at the center of the compact was 5.05° C. / min. No cracks were found during handling after compaction.

[0127] Example 7 The amount of lithium powder mixture was 11530g, and the molding pressure was 1000kg / cm 2 A lithium mixture molded body was produced and sintered in the same manner as in Example 2, except that the furnace temperature was set to 6.00° C. / min and the furnace temperature increase rate was set to 6.00° C. / min. The lithium mixture molded body had a thickness of 70 mm and a density of 1.83 g / cm. 3 The temperature rise rate at the center of the compact was 5.07°C / min. No cracks were found during handling after compaction.

[0128] Example 8 The amount of lithium mixture powder was 12050g, and the molding pressure was 1500kg / cm 2 A lithium mixture molded body was produced and sintered in the same manner as in Example 2, except that the furnace temperature was set to 6.00° C. / min and the furnace temperature increase rate was set to 6.00° C. / min. The lithium mixture molded body had a thickness of 70 mm and a density of 1.91 g / cm. 3 The temperature rise rate at the center of the molded body was 5.04° C. / min. No cracks were found during handling after molding.

[0129] Comparative Example 3 The amount of lithium powder mixture was 7980g, and the molding pressure was 100kg / cm 2A lithium mixture molded body was produced in the same manner as in Example 2, except that the temperature in the furnace was changed to 6.00° C. / min and the heating rate of the furnace was changed to 6.00° C. / min. However, the lithium mixture molded body was hardly solidified and could not be molded.

[0130] [Table 2]

[0131] (Evaluation result 2) Table 2 shows the evaluation results of Examples 4 to 8 and Comparative Examples 2 and 3. Fig. 7 is a graph showing the relationship between density and heating rate for these Examples and Comparative Example 2. From the results of Comparative Example 3, it can be seen that in the case of a molded body containing a nickel composite oxide having the above composition ratio and lithium hydroxide (water content of 1.5% or less, total carbon of 1.0% or less) and no binder, the density was 1.3 g / cm 3 It was shown that if the density is not more than this, a molded body having sufficient strength cannot be formed. Also, from the results of Examples 4 to 8, the heat transferability did not change much depending on the density of the molded body (see FIG. 7).

[0132] Example 9 The furnace was heated from room temperature (25°C) to 760°C at a heating rate of 6.00°C / min, and the temperature of the center of the compact was kept at 760°C for 3 hours, after which the temperature was lowered. The heating rate of the center of the compact was 5.06°C / min (heating time was about 2.4 hours). The total firing time was 5.4 hours. After firing, the compact was crushed, washed with water, filtered, and dried, and the crystallite size and Li site occupancy of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0133] Example 10 The furnace was heated from room temperature (25°C) to 760°C at a heating rate of 6.00°C / min, and the temperature of the center of the compact was kept at 760°C for 2.5 hours, after which the temperature was lowered. The heating rate of the center of the compact was 5.06°C / min (heating time was about 2.4 hours). The total firing time was 4.9 hours. After firing, the compact was crushed, washed with water, filtered, and dried, and the crystallite size and Li site occupancy of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0134] Example 11 The furnace was heated from room temperature (25°C) to 760°C at a heating rate of 6.00°C / min, and the temperature of the center of the compact was kept at 760°C for 2.0 hours, after which the temperature was lowered. The heating rate of the center of the compact was 5.07°C / min (heating time was about 2.4 hours). The total firing time was 4.4 hours. After firing, the compact was crushed, washed with water, filtered, and dried, and the crystallite size and Li site occupancy of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0135] Example 12 Nickel composite oxide obtained by oxidizing and roasting nickel composite hydroxide having a composition ratio of Ni:Co:Al=91:4.5:4.5 in a rotary kiln and lithium hydroxide having a moisture content of 1.5% or less and a total carbon content of 1.0% or less were mixed so that the Li / Me ratio was 1.02, and the firing was performed in the same manner as in Example 9, except that the firing temperature was set to 745°C. The temperature rise rate at the center of the molded body was 5.06°C / min (heat rise time was about 2.4 hours). The total firing time was 5.4 hours. After firing, the molded body was crushed, washed with water, filtered, and dried, and the crystallite size and Li site occupancy rate of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0136] (Example 13) Nickel composite oxide obtained by oxidizing and roasting nickel composite hydroxide having a composition ratio of Ni:Co:Al=91:4.5:4.5 in a rotary kiln and lithium hydroxide having a moisture content of 1.5% or less and a total carbon content of 1.0% or less were mixed so that the Li / Me ratio was 1.02, and the firing was performed in the same manner as in Example 10, except that the holding temperature for firing was 745°C. The temperature rise rate at the center of the molded body was 5.06°C / min (heat rise time was about 2.4 hours). The total firing time was 4.9 hours. After firing, the molded body was crushed, washed with water, filtered, and dried, and the crystallite size and Li site occupancy rate of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0137] Example 14 Nickel composite oxide obtained by oxidizing and roasting nickel composite hydroxide having a composition ratio of Ni:Co:Al=91:4.5:4.5 in a rotary kiln and lithium hydroxide having a moisture content of 1.5% or less and a total carbon content of 1.0% or less were mixed so that the Li / Me ratio was 1.02, and the firing was performed in the same manner as in Example 11, except that the firing temperature was set to 745°C. The temperature rise rate at the center of the molded body was 5.05°C / min (heat rise time was about 2.4 hours). The total firing time was 4.4 hours. After firing, the molded body was crushed, washed with water, filtered, and dried, and the crystallite size and Li site occupancy rate of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0138] Comparative Example 4 The furnace was heated from room temperature (25°C) to 760°C at a heating rate of 6.00°C / min, and the temperature of the center of the compact was kept at 760°C for 1.5 hours, after which the temperature was lowered. The heating rate of the center of the compact was 5.07°C / min (heating time was about 2.4 hours). The total firing time was 3.9 hours. After firing, the compact was crushed, washed with water, filtered, and dried, and the crystallite size and Li site occupancy of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0139] Comparative Example 5 The furnace was heated from room temperature (25°C) to 745°C at a heating rate of 6.00°C / min, and the temperature of the center of the compact was kept at 745°C for 1.5 hours, after which the temperature was lowered. The heating rate of the center of the compact was 5.06°C / min (heating time was about 2.4 hours). The total firing time was 3.9 hours. After firing, the compact was crushed, washed with water, filtered, and dried, and the crystallite size and Li site occupancy of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0140] Comparative Example 6 9450g of the lithium mixture powder was placed in a 300mm x 300mm sagger (height of mound was about 105mm), and the furnace was heated from room temperature (25°C) to 760°C at a heating rate of 6.00°C / min, and the temperature of the center of the lithium mixture powder was kept at 760°C for 3 hours, and then the temperature was lowered. The heating rate of the center of the lithium mixture powder was 2.60°C / min (heating time was about 4.7 hours). The total firing time was 7.7 hours. After firing, the obtained lithium nickel composite oxide powder was pulverized, washed with water, filtered, and dried, and the crystallite size and Li site occupancy of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0141] Comparative Example 7 Firing was performed in the same manner as in Comparative Example 6, except that the temperature of the center of the lithium mixture powder was kept at 760°C for 2.5 hours. The temperature rise rate of the center of the lithium mixture powder was 2.60°C / min (heat rise time was about 4.7 hours). The total firing time was 7.2 hours. After firing, the obtained lithium nickel composite oxide powder was pulverized, washed with water, filtered, and dried, and the crystallite size and Li site occupancy rate of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin battery.

[0142] Comparative Example 8 9450g of the lithium mixture powder was placed in a 300mm x 300mm sagger (height of mound was about 105mm), and the furnace was heated from room temperature (25°C) to 745°C at a heating rate of 6.00°C / min, and the temperature of the center of the lithium mixture powder was kept at 745°C for 3 hours, and then the temperature was lowered. The heating rate of the center of the lithium mixture powder was 2.60°C / min (heating time was about 4.6 hours). The total firing time was 7.6 hours. After firing, the obtained lithium nickel composite oxide powder was pulverized, washed with water, filtered, and dried, and the crystallite size and Li site occupancy of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0143] Comparative Example 9 Firing was performed in the same manner as in Comparative Example 8, except that the temperature of the center of the lithium mixture powder was kept at 745°C for 2.5 hours. The temperature rise rate of the center of the lithium mixture powder was 2.61°C / min (heat rise time was about 4.6 hours). The total firing time was 7.1 hours. After firing, the obtained lithium nickel composite oxide powder was pulverized, washed with water, filtered, and dried, and the crystallite size and Li site occupancy rate of the dried powder were measured using X-ray diffraction. The results are shown in Table 1. Table 1 also shows the results of the battery characteristic evaluation using a coin-type battery.

[0144] [Table 3]

[0145] (Evaluation result 3) The lithium nickel composite oxide obtained in the examples has a sufficiently large crystallite diameter, a high lithium site occupancy rate, and a reduced amount of eluted lithium, and is shown to have a high crystallinity due to the progress of the sintering reaction. In addition, it has been shown that a secondary battery using the lithium nickel composite oxide obtained in the examples as a positive electrode active material has a very high initial charge / discharge capacity and initial discharge efficiency. From the above, it is clear that according to the manufacturing method of this embodiment, by forming the lithium mixture into a high-density molded body, the amount of raw material input per unit volume is increased, and a lithium nickel composite oxide (positive electrode active material) having high crystallinity can be obtained by a short firing time, and the productivity is greatly improved.

[0146] The technical scope of the present invention is not limited to the aspects described in the above-mentioned embodiments. One or more of the requirements described in the above-mentioned embodiments may be omitted. The requirements described in the above-mentioned embodiments may be combined as appropriate. In addition, to the extent permitted by law, the disclosures of all documents cited in the above-mentioned embodiments are incorporated by reference and are included as part of the description in this text. [Explanation of symbols]

[0147] 1...Plate-shaped member 2…Container 10...Molded body 20...Lithium mixture powder t: thickness of molded body CBA…Coin cell battery NC: Negative electrode can NE: Negative electrode PC…Positive electrode can PE: Positive electrode SE…Separator GA…Gasket WW…Wave washer

Claims

1. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, comprising: Mixing a nickel composite oxide with a lithium compound to obtain a lithium mixture; The lithium mixture was molded by pressing without spraying water to a density of 1.3 g / cm 3 obtaining a molded product having a density of 2.0 g / cm 3 or more and 2.0 g / cm 3 or less; Firing the molded body at 650° C. or more and 850° C. or less in an oxidizing atmosphere; The lithium nickel composite oxide contains lithium (Li), nickel (Ni), cobalt (Co), and aluminum (Al), and the atomic ratio of each element is expressed as Li:Ni:Co:Al=s:(1-x-y):x:y (where 0.93<s<1.03, 0.03≦x≦0.10, and 0.03≦y≦0.10).

2. The lithium compound is composed of lithium hydroxide having a moisture content of 1.5% or less and a total carbon content of 1.0% or less, The molded body does not contain a binder. The method for producing the positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 .

3. The density of the molded body is 1.4 g / cm 3 The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein

4. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 3, wherein the maximum value of a distance between two points on the outer shape of the molded body is 1 mm or more.

5. 5. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, wherein the firing is performed by placing the molded body on a plate-like member placed in a firing furnace.

6. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 5, further comprising crushing the fired product after the firing.

7. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 6, further comprising washing the fired product with water and drying the fired product.

8. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 7, wherein the firing temperature is maintained for 3 hours or less during the firing.

9. The lithium nickel composite oxide contains lithium (Li), nickel (Ni), cobalt (Co), aluminum (Al), and another element M, and the atomic ratio of each element is expressed as Li:Ni:Co:Al:M=s:(1-xy):x:y:z (where 0.93<s<1.03, 0.03≦x≦0.10, 0.03≦y≦0.10, 0<z≦0.1, and M is an element other than Li, Ni, Co, Al, and O). The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 8.

10. 10. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 9, wherein 5 g of the lithium nickel composite oxide is dispersed in 100 ml of pure water, and the amount of lithium eluted into a supernatant after standing for 10 minutes is 0.11 mass% or less with respect to the total amount of the lithium nickel composite oxide.

11. The lithium nickel composite oxide has a lithium site occupancy rate of 97.0% or more at 3a sites obtained by Rietveld analysis of an X-ray diffraction pattern.

Citation Information

Patent Citations

  • Positive electrode material for lithium secondary battery and its synthesis and evaluation, and lithium secondary battery and its manufacture

    JP1994290780A

  • Positive active material for lithium secondary battery and secondary battery using the same

    JP1999135123A

  • Production of linio2-based laminar multiple oxide

    JP2000072446A

  • Firing apparatus for lithium-metal multicomponent oxide and firing method of the same

    JP2000203947A

  • Positive electrode active material and lithium secondary battery using it

    JP2000323143A