Bumper fascia and manufacturing method thereof

The bumper fascia is manufactured using a thermoplastic resin members bonded with an in-situ polymerizable composition primer layer, addressing rigidity and appearance issues while reducing weight and cost.

JP7586199B2Active Publication Date: 2024-11-19RESONAC CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022579307
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-08
Publication Date
2024-11-19
Estimated Expiration
2041-02-08

AI Technical Summary

Technical Problem

Existing bumper fascias face challenges in achieving desired rigidity and appearance while reducing weight, with methods like integrating reinforcing ribs causing sink marks and requiring complex surface treatments, leading to increased costs.

Method used

A bumper fascia composed of a first resin member with a thermoplastic resin material and a second resin member, bonded via a primer layer that includes an in-situ polymerizable composition, allowing for strong welding without complex surface treatments.

Benefits of technology

The solution provides a lightweight bumper fascia with desired rigidity and good appearance, manufactured at lower costs by eliminating sink marks and simplifying the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586199000006
    Figure 0007586199000006
  • Figure 0007586199000007
    Figure 0007586199000007
  • Figure 0007586199000008
    Figure 0007586199000008
Patent Text Reader

Abstract

The present invention provides a bumper fascia that can achieve a desired rigidity even if the weight thereof is reduced and can achieve a favorable appearance, and a method that can be used to manufacture such a bumper fascia at a low cost. A first resin member (1) is a reinforcing rib and / or a bracket, a second resin member (4) is a bumper fascia main body, the first and second resin members are welded to each other, and at least one primer layer is an in-situ polymerization composition layer formed by polymerizing an in-situ polymerization composition over the thermoplastic resin material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a bumper fascia provided on the front and rear of an automobile body, and a method for manufacturing the same. [Background technology]

[0002] In recent years, automobile parts are often made into resin molded products from the viewpoint of reducing product weight and cost. Bumpers, which are always attached to the front and rear of a vehicle body, are no exception, and weight reduction is being achieved by using resin.

[0003] Patent Document 1 (JP Patent Publication 2012-166634 A) discloses a vehicle bumper and a molding method thereof. In this vehicle bumper, the thickness of the bumper center where multiple gates are concentrated during injection molding is set small, while the thickness of the bumper sides is set large to create a different thickness distribution, which is said to achieve both overall weight reduction of the bumper and avoidance of poor appearance due to the occurrence of weld lines. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-166634 A Summary of the Invention [Problem to be solved by the invention]

[0005] When the thickness of the bumper center is reduced, as in the case of the bumper fascia of Patent Document 1, there is a risk that the rigidity originally required of the bumper cannot be realized. In addition, in recent years, there has been a demand for bumpers to not only be lightweight but also to have a good appearance. However, when there is a portion with an extremely thin plate thickness, if a reinforcing rib or the like is integrally molded by injection molding or the like on the inside of the bumper fascia in order to increase the rigidity, there is a risk that an appearance defect called a sink mark will occur on the exterior surface of the bumper fascia due to internal stress caused by the shrinkage of the injection-molded resin when it cools.

[0006] Furthermore, the method of adhering a separately molded reinforcing rib to the inside of the bumper fascia using an adhesive requires multiple processes, such as framing the resin surface, surface preparation such as plasma treatment, primer coating, adhesive application, and adhesive curing, to be carried out on the adhesive surface, which has a complex shape, which is disadvantageous in terms of cost.

[0007] An object of the present disclosure is to provide a bumper fascia that can achieve a desired rigidity even when weight reduction is attempted, and can also achieve a good appearance, and a method for inexpensively manufacturing such a bumper fascia. [Means for solving the problem]

[0008] The present disclosure includes the following aspects.

[0009] [1] A first resin member having a thermoplastic resin material; a second resin member having a thermoplastic resin material; one or more primer layers laminated on at least one of the thermoplastic resin material of the first resin member and the thermoplastic resin material of the second resin member; A bumper fascia comprising: the first resin member is a reinforcing rib and / or a bracket, The second resin member is a bumper fascia main body, the first resin member and the second resin member are welded together via the primer layer, A bumper fascia, wherein at least one of the primer layers is an in-situ polymerized composition layer formed by polymerizing an in-situ polymerized composition on the thermoplastic resin material. [2] The bumper fascia according to [1], wherein the in-situ polymerized composition layer is a layer that is in direct contact with the thermoplastic resin material. [3] The bumper fascia according to any one of [1] and [2], wherein the in-situ polymerized composition contains at least one of the following (1) to (7): (1) Combination of difunctional isocyanate compound and diol (2) Combination of a difunctional isocyanate compound and a difunctional amino compound (3) Combination of a bifunctional isocyanate compound and a bifunctional thiol compound (4) Combination of difunctional epoxy compound and diol (5) Combination of a difunctional epoxy compound and a difunctional carboxy compound (6) Combination of a difunctional epoxy compound and a difunctional thiol compound (7) Monofunctional radical polymerizable monomer [4] The bumper fascia according to either [1] or [2], wherein the in-situ polymerization type composition is a composition containing at least one of the following (1) to (7) and a maleic anhydride-modified polypropylene or a modified polyphenylene ether: (1) Combination of difunctional isocyanate compound and diol (2) Combination of a difunctional isocyanate compound and a difunctional amino compound (3) Combination of a bifunctional isocyanate compound and a bifunctional thiol compound (4) Combination of difunctional epoxy compound and diol (5) Combination of a difunctional epoxy compound and a difunctional carboxy compound (6) Combination of a difunctional epoxy compound and a difunctional thiol compound (7) Monofunctional radical polymerizable monomer [5] The bumper fascia according to either [1] or [2], wherein the in-situ polymerization type composition is a composition containing at least one of the following (1) to (7) and a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material. (1) Combination of difunctional isocyanate compound and diol (2) Combination of a difunctional isocyanate compound and a difunctional amino compound (3) Combination of a bifunctional isocyanate compound and a bifunctional thiol compound (4) Combination of difunctional epoxy compound and diol (5) Combination of a difunctional epoxy compound and a difunctional carboxy compound (6) Combination of a difunctional epoxy compound and a difunctional thiol compound (7) Monofunctional radical polymerizable monomer [6] The bumper fascia according to either [1] or [2], wherein the in-situ polymerization type composition is a composition containing at least one of the following (1) to (7), maleic anhydride-modified polypropylene or modified polyphenylene ether, and a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material. (1) Combination of difunctional isocyanate compound and diol (2) Combination of a difunctional isocyanate compound and a difunctional amino compound (3) Combination of a bifunctional isocyanate compound and a bifunctional thiol compound (4) Combination of difunctional epoxy compound and diol (5) Combination of a difunctional epoxy compound and a difunctional carboxy compound (6) Combination of a difunctional epoxy compound and a difunctional thiol compound (7) Monofunctional radical polymerizable monomer [7] The bumper fascia according to any one of [3] to [6], wherein the in-situ polymerization type composition contains the (4), and the diol of the (4) is a bifunctional phenol compound. [8] The bumper fascia according to any one of [1] and [3] to [7], wherein the primer layer has a curable resin layer formed from a composition containing a curable resin between the in-situ polymerization type composition layer and the thermoplastic resin material. [9] The bumper fascia according to [8], wherein the curable resin is at least one selected from the group consisting of a urethane resin, an epoxy resin, a vinyl ester resin, and an unsaturated polyester resin.

[10] Both the first resin member and the second resin member To The primer layer are stacked. , the first resin member Stacked in The primer layer and the second resin member Stacked in The bumper fascia according to any one of [1] to [9], wherein the primer layer is welded.

[11] A bumper fascia according to any one of [1] to

[10] , wherein a monomer having a maximum content among the monomers constituting the thermoplastic resin constituting the thermoplastic resin material of the second resin member is the same as a monomer having a maximum content among the monomers constituting the thermoplastic resin constituting the thermoplastic resin material of the first resin member, and the content of each of the monomers is 70 mass% or more.

[12] A bumper fascia according to any one of [1] to

[11] , wherein an aspect ratio (height / thickness) of the height and thickness of the first resin member is 5 or more, and a ratio of the height of the first resin member to the thickness of the second resin member is 5 or more.

[13] The bumper fascia according to any one of [1] to

[12] , wherein the thermoplastic resin material of the first resin member or the second resin member contains polypropylene and at least one reinforcing material selected from the group consisting of talc, glass fiber, and carbon fiber, and the first resin member or the second resin member has a tensile strength of 40 MPa or more and a Young's modulus of 3 GPa or more.

[14] The bumper fascia according to any one of [1] to

[12] , wherein the thermoplastic resin material of the first resin member or the second resin member contains polyetherimide and at least one reinforcing material selected from the group consisting of talc, glass fiber, and carbon fiber, and the first resin member or the second resin member has a tensile strength of 90 MPa or more and a Young's modulus of 3 GPa or more.

[15] A method for manufacturing a bumper fascia according to any one of [1] to

[14] , comprising heating the primer layer and welding the first resin member and the second resin member by pressing the first resin member and the second resin member together so that the heated primer layer is interposed between the first resin member and the second resin member. Effect of the Invention

[0010] According to the present disclosure, it is possible to provide a bumper fascia that can achieve a desired rigidity even when weight reduction is attempted, and can also achieve a good appearance, and such a bumper fascia can be manufactured inexpensively. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a front view of a vehicle showing the position of a bumper fascia (a dotted line portion, limited to the front bumper) in the vehicle. [Diagram 2] FIG. 2 is a schematic diagram showing the components of the bumper fascia. [Diagram 3] FIG. 3 is a schematic diagram of the bumper fascia showing a state in which other components are joined to the bumper fascia main body. [Figure 4] FIG. 4 is a schematic cross-sectional view showing a state in which one primer layer is laminated on a thermoplastic resin material in a first resin member of one embodiment. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing a state in which a plurality of primer layers are laminated on a thermoplastic resin material in a first resin member according to another embodiment. [Figure 6]FIG. 6 is a schematic cross-sectional view of the first resin member and the second resin member welded together. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Next, embodiments of the present disclosure will be described below with reference to the drawings.

[0013] In this disclosure, bonding means connecting two objects together, and adhesion and welding are subordinate concepts. Adhesion means joining two adherends (objects to be bonded) together using an organic material such as tape or adhesive (curable resin, thermoplastic resin, etc.). Welding means melting the surface of the adherend, such as thermoplastic resin, by heat, and joining the two by entanglement and crystallization caused by molecular diffusion through contact pressure and cooling.

[0014] In this disclosure, "(meth)acrylic" means acrylic or methacrylic, and "(meth)acrylate" means acrylate or methacrylate.

[0015] [Bumper fascia] 1 is a front view of a vehicle showing the position of a bumper fascia 10 (the dotted line portion, limited to the front bumper) in the vehicle. The bumper fascia is the part that is located on the outermost side of the vehicle body among the parts that make up the bumper, and is the part (outer panel) that can be seen as part of the vehicle exterior.

[0016] Fig. 2 is a schematic diagram showing each component of the bumper fascia 10, and Fig. 3 is a schematic diagram of the bumper fascia showing the state in which other components are joined to the bumper fascia main body 12. In both of these figures, the bumper fascia main body 12 shows the surface inside the vehicle body. As shown in these figures, the bumper fascia 10 includes the bumper fascia main body 12, a reinforcing rib 14 for reinforcing a thin-walled central portion of the bumper fascia main body 12, and brackets 16 that are joined to both outer portions of the bumper fascia main body 12 and that house sensors and the like for detecting obstacles in front of the vehicle.

[0017] The reinforcing rib 14 need not be excessively heavy, and for example, as shown in Figures 2 and 3, includes a stem 14a extending along the longitudinal direction of the bumper fascia main body 12, and a plurality of branch portions 14b extending on both sides of the stem 14a and spaced equally apart in the longitudinal direction of the stem 14a. The presence of the reinforcing rib 14 makes it possible to achieve the desired rigidity for the bumper fascia 10, even if the central portion of the bumper fascia main body 12 is thin-walled.

[0018] Hereinafter, the reinforcing rib 14 and / or the bracket 16 will also be referred to as the "first resin member 1," and the bumper fascia main body 12 will also be referred to as the "second resin member 4."

[0019] [First resin member 1] The first resin member 1 of one embodiment is a laminate having a thermoplastic resin material 2 and one or more primer layers 3 laminated on the thermoplastic resin material, as shown in Fig. 4. In Fig. 4, at least one of the primer layers 3 is an in situ polymerized composition layer 3a formed by polymerizing an in situ polymerized composition on the thermoplastic resin material 2.

[0020] In the present disclosure, the in situ polymerization type composition means a composition that forms a thermoplastic structure, i.e., a linear polymer structure, by a combination of specific bifunctional compounds undergoing a polyaddition reaction in the presence of a catalyst on site, i.e., on various materials, or by a radical polymerization reaction of specific monofunctional monomers. Unlike a curable resin that forms a three-dimensional network due to a crosslinked structure upon polymerization, the in situ polymerization type composition does not form a three-dimensional network due to a crosslinked structure and has thermoplasticity.

[0021] The in-situ polymerization type composition layer 3a is preferably a layer formed from a composition containing an in-situ polymerization type phenoxy resin. The in-situ polymerization type phenoxy resin is also called a thermoplastic epoxy resin, an in-situ curing type phenoxy resin, an in-situ curing type epoxy resin, etc., and forms a thermoplastic structure, i.e., a linear polymer structure, by polyaddition reaction of a bifunctional epoxy resin and a bifunctional phenol compound in the presence of a catalyst.

[0022] In this disclosure, the primer layer 3 refers to a layer that is interposed between the thermoplastic resin material 2 of the first resin member 1 and the thermoplastic resin material of the second resin member 4, which is the other object to be joined, and improves the bonding strength between the thermoplastic resin material 2 of the first resin member 1 and the thermoplastic resin material of the second resin member 4, when the thermoplastic resin material 2 of the first resin member 1 and the second resin member 4, which is the other object to be joined, are joined together to obtain a bumper fascia 10 (resin-resin bonded body), as shown in FIG. 6 described later.

[0023] According to the present disclosure, when the second resin member 4 has a thermoplastic resin material made of the same type of thermoplastic resin as the thermoplastic resin constituting the thermoplastic resin material 2, the first resin member 1 and the second resin member 4 can be firmly welded together. When the second resin member 4 has a thermoplastic resin material made of a different type of thermoplastic resin from the thermoplastic resin constituting the thermoplastic resin material 2, the SP values ​​of the thermoplastic resin material 2 of the first resin member 1 and the thermoplastic resin material of the second resin member 4 are generally often far apart, but according to the present disclosure, such different types of thermoplastic resin materials can also be firmly welded together.

[0024] In this disclosure, "same type of thermoplastic resin" means a thermoplastic resin in which the monomers constituting the thermoplastic resin are the same and the contents of the monomers are 70% by mass or more. "Different types of thermoplastic resin" means a thermoplastic resin other than "same type of thermoplastic resin", specifically, a thermoplastic resin that does not have a common monomer, a thermoplastic resin in which the monomers constituting the thermoplastic resin are different in the maximum content, or a thermoplastic resin in which the monomers constituting the maximum content are the same and at least one of the monomers constituting the maximum content is less than 70% by mass.

[0025] <Thermoplastic resin material 2> The thermoplastic resin constituting the thermoplastic resin material 2 is not particularly limited.

[0026] As a thermoplastic resin, for example, polypropylene (PP, SP value: 8.0 (J / cm 3 ) 1 / 2 ), Polyamide 6 (PA6, SP value: 12.7 to 13.6 (J / cm 3 ) 1 / 2 ), Polyamide 66 (PA66, SP value: 13.6 (J / cm 3 ) 1 / 2 ), polyimide (PI), modified polyphenylene ether (m-PPE), polyphenylene sulfide (PPS, SP value: 19.8 (J / cm 3 ) 1 / 2 ), polyetherimide (PEI), polycarbonate (PC, SP value: 9.7 (J / cm 3 ) 1 / 2 ), Polybutylene terephthalate (PBT, SP value: 20.5 (J / cm 3 ) 1 / 2 ) etc.

[0027] In this disclosure, the solubility parameter (SP value) is a value (δ) that provides a numerical prediction of the degree of interaction between materials, defined by the regular solution theory introduced by Hildebrand.

[0028] Various methods for calculating the SP value have been proposed. For example, the SP value can be calculated using the following formula (1) according to the method proposed by Fedors (Polym. Eng. Sci. 1974, Vol. 14, p. 147). δ = (ΣE coh / ΣV) 1 / 2 (1) where δ is the solubility parameter (J 0.5 / cm 1.5 ), E coh is the cohesive energy density (J / mol), V is the molar volume (cm 3 / mol), and Σ means that the values ​​given for each atomic group are summed up for all the atomic groups that make up the monomer. coh The values ​​of and V are given, for example, in Table 7.3 of “Properties of Polymers, Third completely revised edition.”

[0029] The thermoplastic resin material 2 may further include at least one selected from the group consisting of fillers and fibers. For example, the thermoplastic resin material 2 may be a high-rigidity type including the above-mentioned thermoplastic resin and at least one reinforcing material selected from the group consisting of talc, glass fiber, and carbon fiber. In an embodiment in which the thermoplastic resin is polypropylene, an example of the talc-containing polypropylene is manufactured by SunAllomer Co., Ltd. under the product name TRC104N, an example of the glass fiber-containing polypropylene is manufactured by Daicel Miraize Co., Ltd. under the product name PP-GF40-01 F02, and an example of the carbon fiber-containing polypropylene is manufactured by Daicel Miraize Co., Ltd. under the product name PP-CF40-11 F008.

[0030] The glass fiber-containing thermoplastic resin material is a type of glass fiber reinforced resin (GFRP), and the carbon fiber-containing thermoplastic resin material is a type of carbon fiber reinforced resin (CFRP). The thermoplastic resin material containing reinforcing fibers such as glass fiber and carbon fiber may be in the form of a molded body such as a sheet molding compound (SMC) or a bulk molding compound (BMC). SMC is a sheet-like molded body obtained by impregnating a resin composition containing a thermoplastic resin, a low shrinkage agent, a filler, etc., into reinforcing fibers such as glass fiber and carbon fiber.

[0031] <Primer layer 3> The primer layer 3 is laminated on the thermoplastic resin material 2 .

[0032] [In-situ polymerizable composition layer 3a] At least one layer of the primer layer 3 is an in-situ polymerizable composition layer 3 a formed by polymerizing an in-situ polymerizable composition on the thermoplastic resin material 2 .

[0033] The in-situ polymerization type composition layer 3a can be obtained by applying an in-situ polymerization type composition dissolved in a solvent to the surface of the thermoplastic resin material 2, penetrating the in-situ polymerization type composition into the surface layer of the thermoplastic resin material 2 swollen by the penetration of the solvent, volatilizing the solvent, and polymerizing the in-situ polymerization type composition. The in-situ polymerization type composition layer 3a can also be obtained by applying an emulsion containing the in-situ polymerization type composition or a powder coating containing the in-situ polymerization type composition onto the thermoplastic resin material 2, and polymerizing the in-situ polymerization type composition on the thermoplastic resin material 2. The in-situ polymerization type composition layer 3a can also be obtained by applying an in-situ polymerization type composition dissolved in a solvent onto a release film so that the film has a thickness of 1 to 100 μm after drying, leaving it in an environment of room temperature to 40 ° C. while volatilizing the solvent, slightly proceeding the reaction to B stage, placing the surface of the obtained film opposite to the release film on the thermoplastic resin material 2, peeling off the release film from the B staged film, and then performing a heating reaction at 40 to 150 ° C. for 1 to 30 minutes to polymerize the B staged film.

[0034] For powder paint, the B-staged film can be crushed and layered on the thermoplastic resin material 2 to a thickness of 1 to 100 μm, and can be used as a powder paint primer as is. For emulsion, the powder paint primer can be post-emulsified using an emulsifier, and then applied on the thermoplastic resin material 2 to a thickness of 1 to 100 μm, and can be used as an emulsified (water-based) primer.

[0035] The in situ polymerization type composition layer 3a preferably contains 50 to 100 mass %, and more preferably contains 70 to 100 mass %, of an in situ polymerization type resin produced by polymerizing an in situ polymerization type composition.

[0036] The in situ polymerization type composition preferably contains at least one of the following (1) to (7), more preferably contains the following (4), and further preferably contains a combination of a difunctional epoxy resin and a difunctional phenol compound. (1) Combination of difunctional isocyanate compound and diol (2) Combination of a difunctional isocyanate compound and a difunctional amino compound (3) Combination of a bifunctional isocyanate compound and a bifunctional thiol compound (4) Combination of difunctional epoxy compound and diol (5) Combination of a difunctional epoxy compound and a difunctional carboxy compound (6) Combination of a difunctional epoxy compound and a difunctional thiol compound (7) Monofunctional radical polymerizable monomer

[0037] The blending ratio of the bifunctional isocyanate compound and the diol in (1) is set so that the molar equivalent ratio of isocyanate groups to hydroxyl groups is preferably 0.7 to 1.5, more preferably 0.8 to 1.4, and even more preferably 0.9 to 1.3.

[0038] The blending ratio of the bifunctional isocyanate compound and the bifunctional amino compound in (2) is set so that the molar equivalent ratio of the isocyanate group to the amino group is preferably 0.7 to 1.5, more preferably 0.8 to 1.4, and even more preferably 0.9 to 1.3.

[0039] The blending ratio of the bifunctional isocyanate compound and the bifunctional thiol compound in (3) is preferably set so that the molar equivalent ratio of the isocyanate group to the thiol group is 0.7 to 1.5, more preferably 0.8 to 1.4, and even more preferably 0.9 to 1.3.

[0040] The mixing ratio of the bifunctional epoxy compound and the diol in (4) is set so that the molar equivalent ratio of epoxy groups to hydroxyl groups is preferably 0.7 to 1.5, more preferably 0.8 to 1.4, and even more preferably 0.9 to 1.3.

[0041] The blending ratio of the bifunctional epoxy compound and the bifunctional carboxy compound in (5) is preferably set so that the molar equivalent ratio of epoxy groups to carboxy groups is 0.7 to 1.5, more preferably 0.8 to 1.4, and even more preferably 0.9 to 1.3.

[0042] The blend ratio of the bifunctional epoxy compound and the bifunctional thiol compound in (6) is preferably set so that the molar equivalent ratio of epoxy groups to thiol groups is 0.7 to 1.5, more preferably 0.8 to 1.4, and even more preferably 0.9 to 1.3.

[0043] Examples of the in situ polymerization type composition include the following in situ polymerization type compositions (A) to (D). In-situ polymerization type composition (A): A composition containing at least one of the above (1) to (7). In-situ polymerization type composition (B): A composition containing at least one of the above (1) to (7) and maleic anhydride-modified polypropylene or modified polyphenylene ether. In-situ polymerization type composition (C): A composition containing at least one of the above (1) to (7) and a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2. In-situ polymerization type composition (D): A composition containing at least one of the above (1) to (7), maleic anhydride modified polypropylene or modified polyphenylene ether, and a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2.

[0044] The in-situ polymerization type composition layer 3a is laminated as the primer layer 3 on the thermoplastic resin material 2, so that the thermoplastic resin material 2 can be firmly welded to the same kind of thermoplastic resin material or to a different kind of thermoplastic resin material. In particular, it is preferable that the in-situ polymerization type composition layer 3a is a layer that is in direct contact with the thermoplastic resin material 2.

[0045] As the in situ polymerization type composition, it is preferable to select a composition containing the same or similar thermoplastic resin as the thermoplastic resin constituting the thermoplastic resin material 2. For example, when the thermoplastic resin material 2 is a polyolefin, stronger welding can be achieved by using an in situ polymerization type composition containing a maleic anhydride modified polyolefin. When the thermoplastic resin material 2 is a modified polyphenylene ether, stronger welding can be achieved by using an in situ polymerization type composition containing a modified polyphenylene ether.

[0046] The primer layer 3 may be composed of multiple layers including the in situ polymerized composition layer 3a. When the primer layer 3 is composed of multiple layers, it is preferable to laminate the layers so that the essential in situ polymerized composition layer 3a is the outermost surface on the side opposite to the thermoplastic resin material 2. In this case, the in situ polymerized composition is polymerized not on the surface of the thermoplastic resin material 2 but on the surface of the layer directly below the in situ polymerized composition layer 3a.

[0047] (In-situ polymerizable composition layer A) The in situ polymerizable composition layer A is formed from a polymer of the in situ polymerizable composition (A).

[0048] The in-situ polymerization type composition layer A can be obtained by subjecting a composition containing at least one of the above (1) to (6) to a polyaddition reaction in the presence of a catalyst. As a catalyst for the polyaddition reaction, for example, tertiary amines such as triethylamine and 2,4,6-tris(dimethylaminomethyl)phenol, and phosphorus-based compounds such as triphenylphosphine are preferably used. The polyaddition reaction is preferably carried out by heating at room temperature to 200° C. for 5 to 120 minutes, depending on the composition of the composition.

[0049] Specifically, the in situ polymerization type composition layer A can be formed by dissolving a composition containing at least one of the above (1) to (6) in a solvent, applying the solution onto the thermoplastic resin material 2, appropriately volatilizing the solvent, and then heating to carry out a polyaddition reaction, thereby forming a more strongly bonded in situ polymerization type composition layer. The in situ polymerization type composition layer A can also be formed by placing a film of a composition containing at least one of the above (1) to (6) in a B-stage on the thermoplastic resin material 2, and heating the film to carry out a polyaddition reaction.

[0050] The in-situ polymerization type composition layer A can also be obtained by subjecting a composition containing the monofunctional radically polymerizable monomer (7) to a radical polymerization reaction. The radical polymerization reaction is preferably carried out by heating at room temperature to 200°C for 5 to 90 minutes, depending on the composition of the composition. In the case of photocuring, the polymerization reaction is carried out by irradiating ultraviolet light or visible light.

[0051] Specifically, the in situ polymerization type composition layer A can be formed by dissolving a composition containing the monofunctional radical polymerizable monomer of (7) in a solvent, applying the solution on the thermoplastic resin material 2, and then heating or irradiating with light to cause a radical polymerization reaction, thereby forming a more strongly bonded in situ polymerization type composition layer. The in situ polymerization type composition layer A can also be formed by placing a film of a B-staged composition containing the monofunctional radical polymerizable monomer of (7) on the thermoplastic resin material 2, and heating or irradiating the film with light to cause a radical polymerization reaction.

[0052] (Difunctional isocyanate compound) The bifunctional isocyanate compound is a compound having two isocyanato groups, and examples thereof include diisocyanate compounds such as hexamethylene diisocyanate, tetramethylene diisocyanate, dimer acid diisocyanate, 2,4- or 2,6-tolylene diisocyanate (TDI) or a mixture thereof, p-phenylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate (MDI), etc. From the viewpoint of the strength of the primer, the bifunctional isocyanate compound is preferably TDI or MDI.

[0053] (Diol) The diol is a compound having two hydroxy groups, and examples thereof include aliphatic glycols such as ethylene glycol, propylene glycol, diethylene glycol, and 1,6-hexanediol, and bisphenols such as bisphenol A, bisphenol F, and bisphenol S. From the viewpoint of the toughness of the primer, the diol is preferably propylene glycol or diethylene glycol.

[0054] (Bifunctional amino compounds) The bifunctional amino compound is a compound having two amino groups, and examples thereof include bifunctional aliphatic diamines and aromatic diamines. Examples of aliphatic diamines include ethylenediamine, 1,2-propanediamine, 1,3-propanediamine, 1,4-diaminobutane, 1,6-hexamethylenediamine, 2,5-dimethyl-2,5-hexanediamine, 2,2,4-trimethylhexamethylenediamine, isophoronediamine, bis(4-amino-3-methylcyclohexyl)methane, 1,3-diaminocyclohexane, and N-aminoethylpiperazine. Examples of aromatic diamines include diaminodiphenylmethane and diaminodiphenylpropane. From the viewpoint of the toughness of the primer, the bifunctional amino compound is preferably 1,3-propanediamine, 1,4-diaminobutane, or 1,6-hexamethylenediamine.

[0055] (Bifunctional thiol compounds) The bifunctional thiol compound is a compound having two mercapto groups in the molecule, and an example of the bifunctional secondary thiol compound is 1,4-bis(3-mercaptobutyryloxy)butane (for example, "KarenzMT (registered trademark) BD1" manufactured by Showa Denko K.K.).

[0056] (Difunctional epoxy compound) The bifunctional epoxy compound is a compound having two epoxy groups in one molecule, and examples thereof include aromatic epoxy resins such as bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, biphenol type epoxy resin, and naphthalene type bifunctional epoxy resin, and aliphatic epoxy compounds such as 1,6-hexanediol diglycidyl ether.

[0057] The bifunctional epoxy compounds may be used alone or in combination of two or more kinds.

[0058] Specific examples include Mitsubishi Chemical Corporation's "jER (registered trademark) 828," "jER (registered trademark) 834," "jER (registered trademark) 1001," "jER (registered trademark) 1004," and "jER (registered trademark) YX-4000." Other bifunctional epoxy compounds with special structures can also be used.

[0059] (Bifunctional carboxy compound) The bifunctional carboxy compound is a compound having two carboxy groups, and examples thereof include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, maleic acid, fumaric acid, isophthalic acid, terephthalic acid, etc. From the viewpoint of the strength or toughness of the primer, the bifunctional carboxy compound is preferably isophthalic acid, terephthalic acid, or adipic acid.

[0060] (Monofunctional radical polymerizable monomer) The monofunctional radical polymerizable monomer is a monomer having one ethylenically unsaturated bond. For example, styrene monomer, α-, o-, m- or p-alkyl, nitro, cyano, amide or ester derivatives of styrene, chlorostyrene, vinyltoluene, divinylbenzene and other styrene-based monomers; and (meth)acrylic acid esters such as ethyl (meth)acrylate, methyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, dodecyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofuryl (meth)acrylate, acetoacetoxyethyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, phenoxyethyl (meth)acrylate, and glycidyl (meth)acrylate. The monofunctional radical polymerizable monomer may be used alone or in combination of two or more. From the viewpoint of strength or toughness of the primer, the monofunctional radical polymerizable monomer is preferably styrene, methyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, phenoxyethyl (meth)acrylate, or a combination of two or more of these.

[0061] In order to sufficiently advance the radical polymerization reaction and form a desired in-situ polymerization type composition layer, a solvent and, if necessary, an additive such as a colorant may be contained. In this case, it is preferable that the monofunctional radical polymerizable monomer is the main component among the components contained in the radical polymerizable composition other than the solvent. The main component means that the content of the monofunctional radical polymerizable monomer is 50 to 100 mass %. The content is preferably 60 mass % or more, more preferably 80 mass % or more.

[0062] As the polymerization initiator for the radical polymerization reaction, for example, a known organic peroxide, a photoinitiator, etc. may be suitably used. A room temperature radical polymerization initiator in which an organic peroxide is combined with a cobalt metal salt or an amine may be used. As the organic peroxide, those classified as ketone peroxide, peroxyketal, hydroperoxide, diallyl peroxide, diacyl peroxide, peroxy ester, or peroxydicarbonate may be used. As the photoinitiator, it is desirable to use one that can initiate polymerization within the wavelength range from ultraviolet light to visible light.

[0063] The radical polymerization reaction is preferably carried out by heating at room temperature to 200° C. for 5 to 90 minutes, depending on the type of reactive compound, etc. In the case of photocuring, the polymerization reaction is carried out by irradiating with ultraviolet light or visible light. Specifically, after the composition is applied, the composition is heated or irradiated with light to carry out the radical polymerization reaction, whereby an in-situ polymerization type composition layer can be formed from the radical polymerizable compound.

[0064] (In-situ polymerizable composition layer B) The in situ polymerizable composition layer B is formed from a polymer of the in situ polymerizable composition (B).

[0065] The in-situ polymerization type composition layer B can be obtained by polyaddition reaction of at least one of the above (1) to (6) in the presence of a catalyst in a solution of maleic anhydride modified polypropylene or modified polyphenylene ether. As a catalyst for the polyaddition reaction, for example, tertiary amines such as triethylamine and 2,4,6-tris(dimethylaminomethyl)phenol, and phosphorus compounds such as triphenylphosphine are preferably used. The polyaddition reaction is preferably carried out by heating at room temperature to 200°C for 5 to 120 minutes, depending on the composition of the composition.

[0066] Specifically, the in-situ polymerization type composition layer B can be formed by dissolving in a solvent a composition containing at least one of the above (1) to (6) and applying the solution onto the thermoplastic resin material 2, then volatilizing the solvent appropriately, and then heating to carry out a polyaddition reaction. The in-situ polymerization type composition layer B can also be formed by placing a film of a mixture of maleic anhydride modified polypropylene or modified polyphenylene ether and a composition containing at least one of the above (1) to (6) in a B-stage on the thermoplastic resin material 2, and heating the film to carry out a polyaddition reaction.

[0067] The in-situ polymerization type composition layer B can also be obtained by subjecting a composition containing the monofunctional radically polymerizable monomer (7) to a radical polymerization reaction in a solution of maleic anhydride-modified polypropylene or modified polyphenylene ether. The radical polymerization reaction is preferably carried out by heating at room temperature to 200°C for 5 to 90 minutes, depending on the composition of the composition. In the case of photocuring, the polymerization reaction is carried out by irradiating ultraviolet light or visible light.

[0068] Specifically, the in situ polymerization type composition layer B can be formed by dissolving in a solvent a composition containing maleic anhydride-modified polypropylene or modified polyphenylene ether and the monofunctional radical polymerizable monomer of (7) above, applying the solution onto the thermoplastic resin material 2, and then heating or irradiating with light to cause a radical polymerization reaction. The in situ polymerization type composition layer B can also be formed by placing a film of a B-stage mixture of maleic anhydride-modified polypropylene or modified polyphenylene ether and the composition containing the monofunctional radical polymerizable monomer of (7) above on the thermoplastic resin material 2, and heating or irradiating the film to cause a radical polymerization reaction.

[0069] (Maleic anhydride modified polypropylene) The maleic anhydride-modified polypropylene is a polypropylene graft-modified with maleic anhydride. Examples of the polypropylene include Kayabrid 002PP, 002PP-NW, 003PP, and 003PP-NW manufactured by Kayaku Akzo Co., Ltd., and Modic series manufactured by Mitsubishi Chemical Corporation. SCONA TPPP2112GA, TPPP8112GA, or TPPP9212GA manufactured by BYK Co., Ltd. may be used in combination as a polypropylene additive functionalized with maleic anhydride.

[0070] (Modified polyphenylene ether) The modified polyphenylene ether may be a known one, which is a blend of polyphenylene ether with polystyrene, polyamide, polyphenylene sulfide, polypropylene, etc., and examples thereof include NORYL series (PPS / PS): 731, 7310, 731F, 7310F manufactured by SABIC, ZYLON series (PPE / PS, PP / PPE, PA / PPE, PPS / PPE, PPA / PPE) manufactured by Asahi Kasei Chemicals Corporation, Epiace series and Lemalloy series (PPE / PS, PPE / PA) manufactured by Mitsubishi Engineering Plastics Corporation, etc.

[0071] The total amount of the (1) to (7) used when obtaining the in situ polymerization type composition layer B is preferably 5 to 100 parts by mass, more preferably 5 to 60 parts by mass, and even more preferably 20 to 40 parts by mass, relative to 100 parts by mass of the maleic anhydride modified polypropylene or modified polyphenylene ether.

[0072] (In-situ polymerizable composition layer C) The in situ polymerizable composition layer C is formed from a polymer of the in situ polymerizable composition (C).

[0073] The in-situ polymerization type composition layer C can be obtained by subjecting at least one of the above (1) to (6) to a polyaddition reaction in the presence of a catalyst in a solution containing a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2. As a catalyst for the polyaddition reaction, for example, tertiary amines such as triethylamine and 2,4,6-tris(dimethylaminomethyl)phenol, and phosphorus-based compounds such as triphenylphosphine are preferably used. The polyaddition reaction is preferably performed by heating at room temperature to 200°C for 5 to 120 minutes, depending on the composition of the composition.

[0074] Specifically, the in situ polymerization type composition layer C can be formed by dissolving in a solvent a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2 and a composition containing at least one of the above (1) to (6), applying the solution onto the thermoplastic resin material 2, volatilizing the solvent as appropriate, and then heating to carry out a polyaddition reaction. The in situ polymerization type composition layer C can also be formed by placing a film of a mixture of a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2 and a composition containing at least one of the above (1) to (6) in a B-stage on the thermoplastic resin material 2, and heating the film to carry out a polyaddition reaction.

[0075] The in-situ polymerization type composition layer C can also be obtained by subjecting a composition containing the monofunctional radically polymerizable monomer of (7) to a radical polymerization reaction in a solution containing a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2. The radical polymerization reaction is preferably carried out by heating at room temperature to 200°C for 5 to 90 minutes, depending on the composition of the composition. In the case of photocuring, the polymerization reaction is carried out by irradiating ultraviolet light or visible light.

[0076] Specifically, the in situ polymerization type composition layer C can be formed by dissolving in a solvent a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2 and a composition containing the monofunctional radical polymerizable monomer of (7) above, and then applying the solution to the thermoplastic resin material 2, and then heating or irradiating with light to cause a radical polymerization reaction. The in situ polymerization type composition layer C can also be formed by placing a film of a mixture of a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2 and a composition containing the monofunctional radical polymerizable monomer of (7) above, which has been B-staged, on the thermoplastic resin material 2, and heating or irradiating the film to cause a radical polymerization reaction.

[0077] (In-situ polymerizable composition layer D) The in-situ polymerizable composition layer D is formed from a polymer of the in-situ polymerizable composition (D).

[0078] The in-situ polymerization type composition layer D can be obtained by polyaddition reacting at least one of the above (1) to (6) in the presence of a catalyst in a solution of maleic anhydride-modified polypropylene or modified polyphenylene ether, and then mixing with a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2. It can also be obtained by polyaddition reacting at least one of the above (1) to (6) in the presence of a catalyst in a solution containing a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2, and then mixing with maleic anhydride-modified polypropylene or modified polyphenylene ether. It can also be obtained by polyaddition reacting at least one of the above (1) to (6) in the presence of a catalyst with maleic anhydride-modified polypropylene or modified polyphenylene ether, a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2, and a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2. As a catalyst for the polyaddition reaction, for example, tertiary amines such as triethylamine and 2,4,6-tris(dimethylaminomethyl)phenol, and phosphorus-based compounds such as triphenylphosphine are preferably used. The polyaddition reaction is preferably carried out by heating at room temperature to 200° C. for 5 to 120 minutes, although this depends on the composition of the composition.

[0079] Specifically, the in-situ polymerization type composition layer D can be formed by dissolving maleic anhydride-modified polypropylene or modified polyphenylene ether, a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2, and a composition containing at least one of the above (1) to (6) in a solvent, applying the solution onto the thermoplastic resin material 2, volatilizing the solvent appropriately, and then heating to carry out a polyaddition reaction. The in-situ polymerization type composition layer D can also be formed by placing a film obtained by B-stage a mixture of maleic anhydride-modified polypropylene or modified polyphenylene ether, a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2, and a composition containing at least one of the above (1) to (6) on the thermoplastic resin material 2, and heating the film to carry out a polyaddition reaction.

[0080] The in-situ polymerization type composition layer D can also be obtained by subjecting a composition containing the monofunctional radically polymerizable monomer (7) to a radical polymerization reaction in a solution containing maleic anhydride modified polypropylene or modified polyphenylene ether and a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2. The radical polymerization reaction is preferably carried out by heating at room temperature to 200°C for 5 to 90 minutes, depending on the composition of the composition. In the case of photocuring, the polymerization reaction is carried out by irradiating ultraviolet light or visible light.

[0081] Specifically, the in-situ polymerization type composition layer D can be formed by dissolving maleic anhydride-modified polypropylene or modified polyphenylene ether, a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2, and a composition containing the monofunctional radical polymerizable monomer (7) in a solvent, applying the solution onto the thermoplastic resin material 2, and then heating or irradiating with light to cause a radical polymerization reaction. The in-situ polymerization type composition layer D can also be formed by placing a film of a mixture of maleic anhydride-modified polypropylene or modified polyphenylene ether, a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material 2, and a composition containing the monofunctional radical polymerizable monomer (7) in a B-stage on the thermoplastic resin material 2, and heating or irradiating the film to cause a radical polymerization reaction.

[0082] In addition, the manner of reaction occurring when forming the in situ polymerization type composition layer is diverse, such as the reaction of maleic anhydride-modified polypropylene or modified polyphenylene ether with a bifunctional epoxy resin, the reaction of maleic anhydride-modified polypropylene or modified polyphenylene ether with a bifunctional phenol compound, etc., and it is not possible to comprehensively express specific embodiments based on the combinations thereof. Therefore, it can be said that it is impossible or impractical to directly specify the in situ polymerization type composition layer by its structure or properties.

[0083] [Curable resin layer 3b] When the primer layer 3 is composed of multiple layers including the in-situ polymerization type composition layer 3a, as shown in FIG. 5, the primer layer 3 can also include a curable resin layer 3b formed from a composition containing a curable resin between the in-situ polymerization type composition layer 3a and the thermoplastic resin material 2.

[0084] The composition containing the curable resin may contain a solvent and, if necessary, an additive such as a colorant, in order to sufficiently advance the curing reaction of the curable resin and form a desired curable resin layer. In this case, it is preferable that the curable resin is the main component among the components contained in the composition other than the solvent. The main component means that the content of the curable resin is 40 to 100 mass%. The content is preferably 60 mass% or more, more preferably 70 mass% or more, and even more preferably 80 mass% or more.

[0085] Examples of the curable resin include urethane resin, epoxy resin, vinyl ester resin, and unsaturated polyester resin.

[0086] The curable resin layer 3b may be formed of one of these resins, or may be formed by mixing two or more of them. The curable resin layer 3b may be composed of multiple layers, and each layer may be formed of a composition containing a different type of curable resin.

[0087] The coating method for forming the curable resin layer 3b from the composition containing the curable resin monomer is not particularly limited, but examples thereof include a spray coating method and a dipping method.

[0088] In the present disclosure, the term "curable resin" broadly refers to a resin that is cured by crosslinking, and is not limited to a heat-curable type, but also includes a room temperature curable type and a light-curable type. The light-curable type can be cured in a short time by irradiation with visible light or ultraviolet light. The light-curable type may be used in combination with a heat-curable type and / or a room temperature curable type. Examples of the light-curable type include vinyl ester resins such as "Lipoxy (registered trademark) LC-760" and "Lipoxy (registered trademark) LC-720" manufactured by Showa Denko K.K.

[0089] (urethane resin) The urethane resin is usually a resin obtained by reacting an isocyanato group of an isocyanate compound with a hydroxyl group of a polyol compound, and is preferably a urethane resin that corresponds to the definition of "a coating material containing 10% by weight or more of polyisocyanate as a non-volatile component of a vehicle" in ASTM D16. The urethane resin may be of one-component type or two-component type.

[0090] Examples of one-component urethane resins include oil-modified types (cured by oxidative polymerization of unsaturated fatty acid groups), moisture-cured types (cured by reaction of isocyanato groups with water in the air), block types (cured by reaction of hydroxyl groups with isocyanato groups regenerated by dissociation of a blocking agent by heating), and lacquer types (cured by evaporation of a solvent and drying). Among these, moisture-cured one-component urethane resins are preferably used from the viewpoint of ease of handling. Specific examples include "UM-50P" manufactured by Showa Denko K.K.

[0091] Examples of two-component urethane resins include catalyst-curing types (which cure when an isocyanato group reacts with water in the air in the presence of a catalyst) and polyol-curing types (which cure when an isocyanato group reacts with a hydroxyl group of a polyol compound).

[0092] Examples of the polyol compound in the polyol curing type include polyester polyol, polyether polyol, and phenol resin.

[0093] Examples of the isocyanate compound having an isocyanato group in the polyol curing type include aliphatic isocyanates such as hexamethylene diisocyanate (HDI), tetramethylene diisocyanate, and dimer acid diisocyanate; aromatic isocyanates such as 2,4- or 2,6-tolylene diisocyanate (TDI) or a mixture thereof, p-phenylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate (MDI) or a polynuclear mixture thereof, namely polymeric MDI; and alicyclic isocyanates such as isophorone diisocyanate (IPDI).

[0094] The compounding ratio of the polyol compound to the isocyanate compound in the polyol-curing two-component urethane resin is preferably such that the molar equivalent ratio of hydroxyl group / isocyanato group is in the range of 0.7 to 1.5.

[0095] Examples of urethanization catalysts used in the two-component urethane resin include amine-based catalysts such as triethylenediamine, tetramethylguanidine, N,N,N',N'-tetramethylhexane-1,6-diamine, dimethyletheramine, N,N,N',N'',N''-pentamethyldipropylene-triamine, N-methylmorpholine, bis(2-dimethylaminoethyl)ether, dimethylaminoethoxyethanol, and triethylamine; and organotin-based catalysts such as dibutyltin diacetate, dibutyltin dilaurate, dibutyltin thiocarboxylate, and dibutyltin dimaleate.

[0096] In the polyol curing type, it is generally preferable that the urethane catalyst be blended in an amount of 0.01 to 10 parts by mass per 100 parts by mass of the polyol compound.

[0097] (Epoxy resin) The epoxy resin is a resin having at least two epoxy groups in one molecule. Examples of the prepolymer of the epoxy resin before curing include ether-based bisphenol-type epoxy resin, novolac-type epoxy resin, polyphenol-type epoxy resin, aliphatic-type epoxy resin, ester-based aromatic epoxy resin, cyclic aliphatic epoxy resin, and ether-ester-based epoxy resin. Among these, bisphenol A-type epoxy resin is preferably used. The epoxy resin may be used alone or in combination of two or more kinds.

[0098] Specific examples of bisphenol A type epoxy resins include "jER (registered trademark) 828" and "jER (registered trademark) 1001" manufactured by Mitsubishi Chemical Corporation.

[0099] Specific examples of novolac type epoxy resins include "DEN (registered trademark) 438 (registered trademark)" manufactured by The Dow Chemical Company.

[0100] Examples of the curing agent used for the epoxy resin include known curing agents such as aliphatic amines, aromatic amines, acid anhydrides, phenolic resins, thiols, imidazoles, cationic catalysts, etc. By using the curing agent in combination with a long-chain aliphatic amine and / or thiols, a curable resin layer having a large elongation rate and excellent impact resistance can be formed.

[0101] Specific examples of the thiols include the same compounds as those exemplified as thiol compounds for forming a functional group-containing layer described later. Among these, pentaerythritol tetrakis(3-mercaptobutyrate) (for example, Karenz MT (registered trademark) PE1 manufactured by Showa Denko K.K.) is preferred from the viewpoint of the elongation rate and impact resistance of the curable resin layer.

[0102] (Vinyl ester resin) The vinyl ester resin is a compound obtained by dissolving a vinyl ester compound in a polymerizable monomer (such as styrene). It is also called an epoxy (meth)acrylate resin, but in the present disclosure, the vinyl ester resin also includes a urethane (meth)acrylate resin.

[0103] As the vinyl ester resin, for example, those described in "Polyester Resin Handbook" (published by Nikkan Kogyo Shimbun, 1988) and "Paint Terminology Dictionary" (published by Shikizai Kyokai, 1993) can be used. Specific examples include "Lipoxy (registered trademark) R-802", "Lipoxy (registered trademark) R-804", and "Lipoxy (registered trademark) R-806" manufactured by Showa Denko K.K.

[0104] The urethane (meth)acrylate resin may be, for example, a radical polymerizable unsaturated group-containing oligomer obtained by reacting an isocyanate compound with a polyol compound, followed by a hydroxyl group-containing (meth)acrylic monomer (and optionally a hydroxyl group-containing allyl ether monomer). Specific examples include "Lipoxy (registered trademark) R-6545" manufactured by Showa Denko K.K.

[0105] The vinyl ester resin can be cured by radical polymerization through heating in the presence of a catalyst such as an organic peroxide.

[0106] The organic peroxide is not particularly limited, but examples thereof include ketone peroxides, peroxyketals, hydroperoxides, diallyl peroxides, diacyl peroxides, peroxy esters, peroxydicarbonates, etc. By combining these with a cobalt metal salt or the like, curing at room temperature is also possible.

[0107] The cobalt metal salt is not particularly limited, but examples thereof include cobalt naphthenate, cobalt octylate, cobalt hydroxide, etc. Among these, cobalt naphthenate and cobalt octylate are preferred.

[0108] (Unsaturated polyester resin) The unsaturated polyester resin is prepared by dissolving a condensation product (unsaturated polyester) obtained by an esterification reaction between a polyol compound and an unsaturated polybasic acid (and, if necessary, a saturated polybasic acid) in a polymerizable monomer (e.g., styrene, etc.).

[0109] As the unsaturated polyester resin, those described in "Polyester Resin Handbook" (published by Nikkan Kogyo Shimbun, 1988) and "Paint Terminology Dictionary" (published by Shikizai Kyokai, 1993) can be used. Specific examples include "Rigolac (registered trademark)" manufactured by Showa Denko K.K.

[0110] The unsaturated polyester resin can be cured by radical polymerization through heating in the presence of a catalyst, similar to that of the vinyl ester resin.

[0111] [Function of primer layer 3] The primer layer 3 is formed on the surface of the thermoplastic resin material 2 or on the surface and a surface layer of the thermoplastic resin material 2 .

[0112] The primer layer 3 on the surface of the thermoplastic resin material 2 means a layer formed by dissolving the composition for forming the primer layer 3 in a solvent and applying the solution to the surface of the thermoplastic resin material 2, and then volatilizing the solvent on the surface of the thermoplastic resin material 2.

[0113] The primer layer 3 on the surface of the thermoplastic resin material 2 means a layer formed by dissolving the composition forming the primer layer 3 in a solvent and applying the solution to the surface of the thermoplastic resin material 2, allowing the composition forming the primer layer 3 to penetrate into the surface of the thermoplastic resin material 2 which has swelled due to the penetration of the solvent, and then evaporating the solvent.

[0114] The primer layer 3 can provide excellent bonding to the second resin member 4, which is the object to be bonded. It is also possible to obtain a first resin member 1 that can maintain the bonding property over a long period of time, such as several months. In addition, the primer layer 3 protects the surface of the thermoplastic resin material 2, and can suppress deterioration such as adhesion of dirt and oxidation.

[0115] [Second resin member 4] The thermoplastic resin constituting the thermoplastic resin material of the second resin member 4 may be the same as or different from the thermoplastic resin constituting the thermoplastic resin material 2 of the first resin member 1. From the viewpoint of strong welding, it is preferable that these thermoplastic resins are the same type.

[0116] When two thermoplastic resin materials are to be joined, even if the thermoplastic resin constituting one thermoplastic resin material and the thermoplastic resin constituting the other thermoplastic resin material are the same type, if one or both of the thermoplastic resins contain fillers or fibers or are blends with other thermoplastic resins, the bonding strength between the two thermoplastic resin materials may be insufficient according to the conventional technology. According to the present disclosure, even in these cases, the first resin member 1 and the second resin member 4 can be firmly welded together via the primer layer 3 (contained in the first resin member 1).

[0117] When the thermoplastic resin constituting the thermoplastic resin material 2 of the first resin member 1 and the thermoplastic resin constituting the thermoplastic resin material of the second resin member 4 are of the same type, the proportion of the monomer that occupies the maximum content among the monomers constituting the thermoplastic resins is 70 mass% or more in each case, preferably 70 to 100 mass%, more preferably 80 to 100 mass%, and even more preferably 85 to 100 mass%.

[0118] When the thermoplastic resin material 2 of the first resin member 1 and / or the thermoplastic resin material of the second resin member 4 contains at least one selected from the group consisting of fillers and fibers, the content thereof is preferably 5 to 50 mass%, more preferably 5 to 40 mass%, and even more preferably 5 to 30 mass%. When the content is within the above range, the bonding strength between the first resin member 1 and the second resin member 4 can be increased.

[0119] When the thermoplastic resin constituting the thermoplastic resin material 2 of the first resin member 1 and / or the thermoplastic resin constituting the thermoplastic resin material of the second resin member 4 is a blend of a main thermoplastic resin and a secondary thermoplastic resin, the content of the secondary thermoplastic resin is preferably 5 to 40 mass%, more preferably 5 to 30 mass%, and even more preferably 5 to 20 mass%. When the content is within the above range, the bonding strength between the first resin member 1 and the second resin member 4 can be increased.

[0120] The content can be calculated by the following formula. Content rate (mass%)=[B / (A+B)]×100 (In the formula, A is the mass (g) of the main thermoplastic resin among the thermoplastic resin constituting the thermoplastic resin material 2 of the first resin member 1 and / or the thermoplastic resin constituting the thermoplastic resin material of the second resin member 4, and B is the mass (g) of the secondary thermoplastic resin among the thermoplastic resin constituting the thermoplastic resin material 2 of the first resin member 1 and / or the thermoplastic resin constituting the thermoplastic resin material of the second resin member 4.)

[0121] According to the present disclosure, even if the thermoplastic resin constituting the thermoplastic resin material of the second resin member 4 and the thermoplastic resin constituting the thermoplastic resin material 2 of the first resin member 1 are different types, the second resin member 4 and the first resin member 1 can be firmly welded together. Furthermore, even if the SP value of the thermoplastic resin constituting the thermoplastic resin material of the second resin member 4 and the SP value of the thermoplastic resin constituting the thermoplastic resin material 2 of the first resin member 1 are different from each other, the second resin member 4 and the first resin member 1 can be firmly welded together.

[0122] [Bumper fascia 10 (resin-resin bonded body)] Fig. 6 is a schematic cross-sectional view of the first resin member 1 and the second resin member 4 welded together, and is a diagram showing, for example, the circled portion A in Fig. 3. The bumper fascia 10 (resin-resin bonded body) is formed by welding the first resin member 1 and the second resin member 4 together via the primer layer 3 (contained in the first resin member 1).

[0123] As shown in FIG. 6, in the bumper fascia 10, the thermoplastic resin material of the bumper fascia main body 4 (12) is welded to the thermoplastic resin material 2 of the reinforcing rib 1 (14) and the thermoplastic resin material 2 of the bracket 1 (16) via a primer layer 3 (included in the reinforcing rib 1 and the bracket 1).

[0124] As described above, the presence of the reinforcing rib 14(1) allows the bumper fascia 10 to achieve the desired rigidity even if the central portion of the bumper fascia main body 12(4) is thinned. Furthermore, since the bumper fascia 10 of this embodiment is manufactured by the above-mentioned method (i.e., joining via the primer layer (3)) without injection molding the reinforcing rib 14(1) and the like into the bumper fascia main body 4(12), there is no appearance defect called sink mark on the exterior surface of the obtained bumper fascia 10. Furthermore, unlike the case where a reinforcing rib molded separately is bonded to the inside of the bumper fascia using an adhesive, the bumper fascia 10 of this embodiment is manufactured by the above-mentioned method without going through multiple steps (frame treatment of the resin surface, surface treatment such as plasma treatment, primer coating, adhesive application, adhesive curing, etc.), and therefore can be manufactured at low cost.

[0125] As described above, in this embodiment, it is possible to provide a bumper fascia that can achieve a desired rigidity even when weight reduction is attempted, and that can achieve a good appearance, and it is also possible to manufacture such a bumper fascia at low cost.

[0126] In one embodiment, the aspect ratio (height / thickness) of the height to thickness of the first resin member 1 is 5 or more, and the ratio of the height of the first resin member 1 to the thickness of the second resin member 4 is 5 or more.

[0127] It is preferable that the thermoplastic resin material of the first resin member 1 or the second resin member 4 contains polypropylene and at least one reinforcing material selected from the group consisting of talc, glass fiber, and carbon fiber, and that the first resin member 1 or the second resin member 4 has a tensile strength of 40 MPa or more and a Young's modulus of 3 GPa or more.

[0128] It is preferable that the thermoplastic resin material of the first resin member 1 or the second resin member 4 contains polyetherimide and at least one reinforcing material selected from the group consisting of talc, glass fiber, and carbon fiber, and that the first resin member 1 or the second resin member 4 has a tensile strength of 90 MPa or more and a Young's modulus of 3 GPa or more.

[0129] The thickness (thickness after drying) of the primer layer 3 depends on the materials of the first resin member 1 and the second resin member 4 and the contact area of ​​the joint, but from the viewpoint of obtaining excellent joint strength, it is preferably 1 μm to 500 μm, more preferably 3 μm to 100 μm, and even more preferably 5 μm to 70 μm. The thickness (thickness after drying) of the in-situ polymerization composition layer 3a is preferably 1 to 60 μm. When the primer layer 3 is a multi-layered layer, the thickness (thickness after drying) of the primer layer 3 is the total thickness of each layer.

[0130] Methods for manufacturing the bumper fascia 10 (resin-resin joint) include a method in which the second resin member 4 is welded to the primer layer 3 of the first resin member 1 by at least one method selected from the group consisting of ultrasonic welding, vibration welding, electromagnetic induction, high frequency, laser, hot plate welding, and hot press, and a method in which a thermoplastic resin material of the second resin member 4 is molded by injection molding onto the primer layer 3 of the first resin member 1.

[0131] From the viewpoints of reducing the demands on the manufacturing equipment, simplifying the manufacturing process, and allowing freedom in designing the resin member, it is advantageous to manufacture the bumper fascia 10 (resin-resin bonded body) by a heat press method. Specifically, the bumper fascia 10 (resin-resin bonded body) can be manufactured by heating the primer layer 3 and pressing the first resin member 1 and the second resin member 4 together so that the heated primer layer 3 is interposed between the first resin member 1 and the second resin member 4. The heating temperature of the primer layer during heating depends on the melting point and softening point of the resin to be bonded, and is preferably 100°C to 350°C. For example, when the resin is nylon 6, the heating temperature is preferably 230°C. In addition, the heating temperature of a primer layer having a melting point is preferably set to the melting point ±5°C, and the heating temperature of a primer layer having a softening point is preferably set to the softening point ±15°C. The pressure during pressing is preferably 0.01 MPa to 10 MPa.

[0132] In another embodiment, the second resin member 4, rather than the first resin member 1, may have one or more primer layers laminated to the thermoplastic resin material. The primer layer 3' of the second resin member 4 may be the same as the primer layer 3 described above. In this embodiment, the first resin member 1 and the second resin member 4 can be welded together by replacing the above-mentioned "first resin member 1" with the "second resin member 4" in this embodiment, and replacing the above-mentioned "second resin member 4" with the "first resin member 1" in this embodiment.

[0133] In yet another embodiment, both the first resin member 1 and the second resin member 4 To The above-mentioned primer layers 3, 3' are stacked. , first resin member 1 Stacked in Primer layer 3 and second resin member 4 Stacked inThe primer layer 3' is welded to the first resin member 1. In this embodiment, the thermoplastic resin constituting the thermoplastic resin material 2 of the first resin member 1 and the thermoplastic resin constituting the thermoplastic resin material of the second resin member 4 may be the same or different. In this embodiment, the bumper fascia 10 (resin-resin bonded body) is produced by welding the first resin member 1 to the primer layer 3' using at least one method selected from the group consisting of ultrasonic welding, vibration welding, electromagnetic induction, high frequency, laser, and heat pressing, preferably heat pressing. Stacked in Primer layer 3 and second resin member 4 Stacked in The primer layer 3' can be welded to the substrate 2.

[0134] Although several embodiments of the present invention have been described, the present invention is not limited to the above-described embodiments and can be modified in various ways without departing from the gist of the present invention. EXAMPLES

[0135] Experimental and comparative test examples related to the present invention are shown below, but the present invention is not limited to the experimental examples below.

[0136] <Thermoplastic resin material for test specimens> Using an injection molding machine (SE100V manufactured by Sumitomo Heavy Industries, Ltd.) under the conditions shown in Table 1 below, thermoplastic resin test pieces (width 10 mm, length 45 mm, thickness 3 mm) for tensile tests were obtained: talc-containing PP resin, glass fiber-containing PA6 resin, glass fiber-containing PA66 resin, m-PPE resin, PPS resin, PEI resin, PC resin, and glass fiber-containing PBT resin.

[0137] [Table 1]

[0138] <Preparation of test specimens: Test Examples 1 to 3 and Comparative Test Example 1> (Preparation of in situ polymerizable composition-1 for forming primer layer) A bifunctional epoxy resin (jER (registered trademark) 1001 manufactured by Mitsubishi Chemical Corporation) (bisphenol A type epoxy resin, molecular weight approximately 900): 100 g, bisphenol S: 6.2 g, and triethylamine: 0.4 g were dissolved in toluene (197 g) to obtain an in-situ polymerization type composition-1 (an in-situ polymerization type thermoplastic epoxy resin composition).

[0139] (Formation of primer layer) Next, the in-situ polymerization composition-1 was sprayed onto one surface of the thermoplastic resin material for the test piece, PBT, PC, PEI, or PPS, so that the thickness after drying was 80 μm. The solvent (toluene) was evaporated by leaving it in the air at room temperature for 30 minutes, and then the mixture was left in a furnace at 150 ° C for 30 minutes to carry out a polyaddition reaction, and then cooled to room temperature to obtain test pieces PBT-1, PC-1, PEI-1, and PPS-1 having a thermoplastic epoxy resin as a primer layer.

[0140] Hereinafter, the surface of the test piece on which the primer layer is formed is referred to as the primer surface, and the surface on which the primer layer is not formed is referred to as the primer-free surface. In addition, in the following Tables 2 to 4 and 6, the surface with the primer layer is indicated as (present), and the surface without the primer layer is indicated as (absent).

[0141] <Test Example 1> (Welding) The primer surface of PPS-1 and the primer surface of PEI-1 were overlapped with each other so that the joint had an overlap length of 5 mm and width of 10 mm, and then ultrasonically welded using an ultrasonic welding machine SONOPET-JII430T-M (28.5 KHz) manufactured by Seidensha Electronics Co., Ltd. to obtain a test piece 1 (resin-resin joint). Here, the joint refers to the part where the thermoplastic resin materials for the test piece were overlapped.

[0142] (tensile shear strength) After leaving test piece 1 at room temperature for one day, a tensile shear strength test was performed in accordance with ISO19095 1-4 using a tensile testing machine (Shimadzu Corporation's universal testing machine Autograph "AG-IS", load cell 10kN, tensile speed 10mm / min, temperature 23℃, 50%RH) to measure the bonding strength. The measurement results are shown in Table 2 below.

[0143] <Test Example 2> (Welding) The primer surface of PBT-1 and the primer surface of PC-1 were ultrasonically welded together in the same manner as in Experimental Test Example 1 to obtain a test piece 2 (resin-resin bonded body).

[0144] (tensile shear strength) A tensile shear strength test was carried out on the test piece 2 in the same manner as in the practical test example 1. The measurement results are shown in Table 2 below.

[0145] <Test Example 3> (Welding) The primer surface of PBT-1 and the primer-free surface of PC-1 were ultrasonically welded together in the same manner as in Experimental Test Example 1 to obtain a test piece 3 (resin-resin bonded body).

[0146] (tensile shear strength) A tensile shear strength test was carried out on the test piece 3 in the same manner as in the practical test example 1. The measurement results are shown in Table 2 below.

[0147] <Test Example 4> (Welding) The primer surface of PBT-1 and the primer-free surface of PPS-1 were ultrasonically welded together in the same manner as in Experimental Test Example 1 to obtain a test piece 4 (resin-resin bonded body).

[0148] (tensile shear strength) A tensile shear strength test was carried out on the test piece 4 in the same manner as in the practical test example 1. The measurement results are shown in Table 2 below.

[0149] <Comparative Test Example 1> An attempt was made to ultrasonically weld the primer-free surface of PBT-1 and the primer-free surface of PPS-1 in the same manner as in Experimental Test 1, but welding was not possible.

[0150] [Table 2]

[0151] <Preparation of test specimens: Experimental test examples 5 to 7 and comparative test examples 2 to 3> (Preparation of in situ polymerizable composition-2 for forming primer layer) Diphenylmethane diisocyanate (Millionate MT manufactured by Tosoh Corporation): 100 g, propylene glycol: 54.7 g, and 4,4'-diaminodiphenylmethane: 15.8 g were dissolved in 287 g of acetone to obtain an in situ polymerization type composition-2 (in situ polymerization type urethane resin composition).

[0152] (Formation of primer layer) Next, the in-situ polymerization composition-2 was sprayed onto one surface of the thermoplastic resin material for the test specimen, PA6, PA66, PBT, or PC, so that the thickness after drying was 90 μm. The solvent (acetone) was evaporated by leaving it in the air at room temperature for 30 minutes, and then the mixture was left in a furnace at 150 ° C. for 30 minutes to carry out a polyaddition reaction, and then cooled to room temperature to obtain test specimens PA6-1, PA66-1, PBT-2, and PC-2 with a urethane resin as a primer layer.

[0153] <Test Example 5> (Welding) The primer surface of PA6-1 and the primer surface of PBT-2 were overlapped with each other so that the joint had an overlap length of 5 mm and a width of 10 mm, and then ultrasonically welded using an ultrasonic welding machine SONOPET-JII430T-M (28.5 KHz) manufactured by Seidensha Electronics Co., Ltd. to obtain test piece 5 (resin-resin joint).

[0154] (tensile shear strength) A tensile shear strength test was performed on the test piece 5 in the same manner as in Example Test 1 to measure the bonding strength. The measurement results are shown in Table 3 below.

[0155] <Test Examples 6 and 7> In the same manner as in Example Test 5, test pieces were prepared and tensile shear strength tests were carried out in the combinations shown in Table 3 below. The results are shown in Table 3 below.

[0156] <Comparative Test Example 2> An attempt was made to ultrasonically weld the primer-free surface of PA6-1 and the primer-free surface of PBT-2 in the same manner as in Test Example 5, but welding was not possible.

[0157] <Comparative Test Example 3> An attempt was made to ultrasonically weld the primer-free surface of PA66-1 and the primer-free surface of PC-2 in the same manner as in Test Example 5, but welding was not possible.

[0158] [Table 3]

[0159] <Test pieces: Test examples 8 to 10 and comparative test examples 4 to 5> (Preparation of in situ polymerizable composition-3 for forming primer layer) 5 g of maleic anhydride-modified polypropylene (Modic (registered trademark) ER321P manufactured by Mitsubishi Chemical Corporation), 1.01 g of epoxy resin (jER (registered trademark) 1001 manufactured by Mitsubishi Chemical Corporation), and 0.24 g of bisphenol A were dissolved in 95 g of hot xylene, and then 0.006 g of 2,4,6-tris(dimethylaminomethyl)phenol was added and the mixture was quenched to obtain in situ polymerization type composition-3 (in situ polymerization type maleic anhydride-containing epoxy resin composition).

[0160] (Preparation of in situ polymerizable composition-4 for forming primer layer) 3.77 g of modified polyphenylene ether (NOLYL731 manufactured by SABIC), 1.0 g of bifunctional epoxy resin (jER (registered trademark) 1001 manufactured by Mitsubishi Chemical Corporation), and 0.22 g of bisphenol A were dissolved in 95 g of hot xylene, and then 0.005 g of 2,4,6-tris(dimethylaminomethyl)phenol was added and the mixture was quenched to obtain in situ polymerization type composition-4 (in situ polymerization type modified polyphenylene ether-containing epoxy resin composition).

[0161] (Formation of primer layer) Next, the in-situ polymerization composition-3 was sprayed onto one surface of the thermoplastic resin material for the test specimen, PP (talc 30% by mass) or PBT, so that the thickness after drying was 80 μm. The solvent (xylene) was evaporated by leaving it in the air at room temperature for 30 minutes, and then the mixture was left in a furnace at 150° C. for 30 minutes to carry out a polyaddition reaction, and then cooled to room temperature to obtain test specimens PP-1 and PBT-3, each having a primer layer made of a thermoplastic epoxy resin containing maleic anhydride.

[0162] Next, the in-situ polymerization composition-4 was sprayed onto one surface of the thermoplastic resin material m-PPE for the test piece so that the thickness after drying was 80 μm. After leaving it in the air at room temperature for 30 minutes to volatilize the solvent (xylene), it was left in a furnace at 150 ° C for 30 minutes to carry out a polyaddition reaction, and then cooled to room temperature to obtain a test piece m-PPE-1 with a modified polyphenylene ether-containing epoxy resin as a primer layer.

[0163] <Test Example 8> (Welding) The primer surface of PP-1 and the primer surface of m-PPE-1 were overlapped with each other so that the joint had an overlap length of 5 mm and a width of 10 mm, and then ultrasonically welded using an ultrasonic welding machine SONOPET-JII430T-M (28.5 KHz) manufactured by Seidensha Electronics Co., Ltd. to obtain test piece 8 (resin-resin joint).

[0164] (tensile shear strength) The test piece 8 was subjected to a tensile shear strength test in the same manner as in Example Test 1 to measure the bonding strength. The measurement results are shown in Table 4 below.

[0165] <Test Examples 9 and 10> In the same manner as in Example Test 8, test pieces were prepared and tensile shear strength tests were carried out in the combinations shown in Table 4 below. The results are shown in Table 4 below.

[0166] <Comparative Test Example 4> An attempt was made to ultrasonically weld the primer-free surface of PP-1 and the primer-free surface of PBT-3 in the same manner as in Test Example 8, but welding was not possible.

[0167] <Comparative Test Example 5> An attempt was made to ultrasonically weld the primer-free surface of m-PPE-1 to one surface (primer-free surface) of the PC thermoplastic resin material for the test piece in the same manner as in Test Example 8, but welding was not possible.

[0168] [Table 4]

[0169] <Test piece: Test example 11> Primed thermoplastic resin materials PC-1, PBT-1, PEI-1, PPS-1, PA6-1, PA66-1, m-PPE-1, or PP-1 were inserted into an injection molding die, and the different thermoplastic resins listed in Table 5 were injection molded onto the primer surface under the same conditions as in Table 1, to obtain test pieces (8 types) with an overlap of 5 mm in length and 10 mm in width between the primer surface and the injection-molded thermoplastic resin.

[0170] (tensile shear strength) A tensile shear strength test was carried out on each test piece in the same manner as in Experimental Test Example 1. The measurement results are shown in Table 5 below.

[0171] [Table 5] [Industrial Applicability]

[0172] The present invention can be used for a bumper fascia and a manufacturing method thereof. [Explanation of symbols]

[0173] 1 First resin member 2 Thermoplastic resin material 3 Primer layer 3a In-situ polymerizable composition layer 3b Curable resin layer 4 Second resin member 10 Bumper fascia (resin-resin bonded body) 12 Bumper fascia body 14 Reinforcing rib 14a Executive 14b Branch 16 Bracket A Circled part

Claims

1. a first resin member having a thermoplastic resin material; a second resin member having a thermoplastic resin material; one or more primer layers laminated on at least one of the thermoplastic resin material of the first resin member and the thermoplastic resin material of the second resin member; A bumper fascia comprising: the first resin member is a reinforcing rib and / or a bracket, the second resin member is a bumper fascia main body, the first resin member and the second resin member are welded together via the primer layer, At least one of the primer layers is an in-situ polymerized composition layer formed by polymerizing an in-situ polymerized composition on the thermoplastic resin material.

2. 2. The bumper fascia of claim 1, wherein said in-situ polymerized composition layer is the layer directly in contact with said thermoplastic resin material.

3. The bumper fascia according to claim 1 or 2, wherein the in-situ polymerized composition contains at least one of the following (1) to (7): (1) Combination of a bifunctional isocyanate compound and a diol (2) Combination of a bifunctional isocyanate compound and a bifunctional amino compound (3) Combination of a bifunctional isocyanate compound and a bifunctional thiol compound (4) Combination of bifunctional epoxy compound and diol (5) Combination of a difunctional epoxy compound and a difunctional carboxy compound (6) Combination of a difunctional epoxy compound and a difunctional thiol compound (7) Monofunctional radically polymerizable monomer

4. The in-situ polymerization type composition is a composition containing at least one of the following (1) to (7) and maleic anhydride modified polypropylene or modified polyphenylene ether. Bumper fascia according to any one of claims 1 to 2. (1) Combination of a bifunctional isocyanate compound and a diol (2) Combination of a bifunctional isocyanate compound and a bifunctional amino compound (3) Combination of a bifunctional isocyanate compound and a bifunctional thiol compound (4) Combination of bifunctional epoxy compound and diol (5) Combination of a difunctional epoxy compound and a difunctional carboxy compound (6) Combination of a difunctional epoxy compound and a difunctional thiol compound (7) Monofunctional radically polymerizable monomer

5. The in-situ polymerization type composition is a composition containing at least one of the following (1) to (7) and a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material. Bumper fascia according to any one of claims 1 and 2. (1) Combination of a bifunctional isocyanate compound and a diol (2) Combination of a bifunctional isocyanate compound and a bifunctional amino compound (3) Combination of a bifunctional isocyanate compound and a bifunctional thiol compound (4) Combination of bifunctional epoxy compound and diol (5) Combination of a difunctional epoxy compound and a difunctional carboxy compound (6) Combination of a difunctional epoxy compound and a difunctional thiol compound (7) Monofunctional radically polymerizable monomer

6. The in-situ polymerization type composition is a composition containing at least one of the following (1) to (7), maleic anhydride-modified polypropylene or modified polyphenylene ether, and a thermoplastic resin different from the thermoplastic resin constituting the thermoplastic resin material. Bumper fascia according to any one of claims 1 and 2. (1) Combination of a bifunctional isocyanate compound and a diol (2) Combination of a bifunctional isocyanate compound and a bifunctional amino compound (3) Combination of a bifunctional isocyanate compound and a bifunctional thiol compound (4) Combination of bifunctional epoxy compound and diol (5) Combination of a difunctional epoxy compound and a difunctional carboxy compound (6) Combination of a difunctional epoxy compound and a difunctional thiol compound (7) Monofunctional radically polymerizable monomer

7. The bumper fascia according to any one of claims 3 to 6, wherein the in-situ polymerization type composition contains the (4), and the diol of the (4) is a difunctional phenol compound.

8. The bumper fascia according to any one of claims 1, 3 to 7, wherein the primer layer has a curable resin layer formed between the in-situ polymerization composition layer and the thermoplastic resin material from a composition containing a curable resin.

9. 9. The bumper fascia of claim 8, wherein the curable resin is at least one selected from the group consisting of a urethane resin, an epoxy resin, a vinyl ester resin, and an unsaturated polyester resin.

10. The primer layer is laminated on both the first resin member and the second resin member, and the primer layer laminated on the first resin member and the primer layer laminated on the second resin member are welded to each other. The bumper fascia according to any one of claims 1 to 9.

11. The bumper fascia according to any one of claims 1 to 10, wherein a monomer occupying the maximum content among monomers constituting the thermoplastic resin constituting the thermoplastic resin material of the second resin member is the same as a monomer occupying the maximum content among monomers constituting the thermoplastic resin constituting the thermoplastic resin material of the first resin member, and the content of each of the monomers is 70 mass% or more.

12. The aspect ratio (height / thickness) of the height and thickness of the first resin member is 5 or more, and the ratio of the height of the first resin member to the thickness of the second resin member is 5 or more. Bumper fascia according to any one of claims 1 to 11.

13. The thermoplastic resin material of the first resin member or the second resin member contains polypropylene and at least one reinforcing material selected from the group consisting of talc, glass fiber, and carbon fiber, and the first resin member or the second resin member has a tensile strength of 40 MPa or more and a Young's modulus of 3 GPa or more. The bumper fascia according to any one of claims 1 to 12.

14. The thermoplastic resin material of the first resin member or the second resin member contains polyetherimide and at least one reinforcing material selected from the group consisting of talc, glass fiber, and carbon fiber, and the first resin member or the second resin member has a tensile strength of 90 MPa or more and a Young's modulus of 3 GPa or more. The bumper fascia according to any one of claims 1 to 12.

15. 15. A method for manufacturing a bumper fascia according to any one of claims 1 to 14, comprising heating the primer layer and welding the first resin member and the second resin member by pressing the first resin member and the second resin member together so that the heated primer layer is interposed between the first resin member and the second resin member.

Citation Information

Patent Citations

  • JP1987153160U

  • Thermoplastic resin composite, and composite structure thereof as well as monolithically molded article by using it

    JP2007254718A

  • Vehicle bumper, and molding method thereof

    JP2012166634A

  • Crash box and production method of the same

    JP2020199899A

  • Composite multilayer body and metal-polyolefin bonded body

    WO2020256038A1