Positive electrode active material for lithium ion secondary battery, and lithium ion secondary battery

By coating lithium metal composite oxide particles with tungsten to achieve high surface coverage, the positive electrode active material in lithium ion secondary batteries addresses the challenge of reducing reaction resistance while maintaining high capacity, enhancing battery performance and scalability.

JP7586220B2Active Publication Date: 2024-11-19SUMITOMO METAL MINING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023066401
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-11-19
Estimated Expiration
2038-07-24

AI Technical Summary

Technical Problem

Existing lithium ion secondary batteries face challenges in further reducing positive electrode resistance (reaction resistance) while maintaining high battery capacity, particularly in secondary batteries using solid electrolytes.

Method used

A positive electrode active material is developed by coating lithium metal composite oxide particles with a layer containing tungsten, achieving a tungsten coverage of more than 50 mol% on the particle surface, with a thickness of 10 nm or less, and a tungsten content of 1-4% by mass, using a manufacturing process that includes spraying water in a decarboxylation atmosphere to enhance coverage.

Benefits of technology

The solution results in a positive electrode active material with reduced reaction resistance and maintained high battery capacity, enabling improved output characteristics and industrial scalability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586220000002
    Figure 0007586220000002
  • Figure 0007586220000003
    Figure 0007586220000003
  • Figure 0007586220000004
    Figure 0007586220000004
Patent Text Reader

Abstract

To propose a positive electrode active material for a lithium ion secondary battery, in which the particle surface of lithium metal composite oxide is coated with tungsten at a high coverage, and which can reduce a positive electrode resistance (reaction resistance) to enhance the output characteristic while keeping a high battery capacity.SOLUTION: A positive electrode active material for a lithium ion secondary battery comprises: a particle of lithium metal composite oxide; and tungsten which coats at least part of the surface of the lithium metal composite oxide particle. According to measurement by X-ray photoelectron spectroscopy (XPS) on the positive electrode active material, the content of tungsten on the surface of the particle of the lithium metal composite oxide is over 50 mol% to a total content of all of metal elements, excluding lithium, on the particle surface.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery and a lithium ion secondary battery. [Background technology]

[0002] In recent years, with the widespread use of portable electronic devices such as smartphones and tablet PCs, there has been a strong demand for the development of small, lightweight nonaqueous electrolyte secondary batteries with high energy density, as well as high-output secondary batteries as power sources for electric vehicles such as hybrid electric vehicles, plug-in hybrid electric vehicles, and battery-powered electric vehicles.

[0003] A lithium ion secondary battery, which is a type of non-aqueous electrolyte secondary battery, is a secondary battery that satisfies such requirements. This lithium ion secondary battery is composed of a negative electrode, a positive electrode, an electrolyte, etc., and the active materials used for the negative electrode and the positive electrode are materials that can extract and insert lithium. In addition, as the non-aqueous electrolyte, a non-aqueous electrolyte solution obtained by dissolving a lithium salt, which is a supporting salt, in an organic solvent, or a solid electrolyte that is non-flammable and has ion conductivity is used.

[0004] For example, lithium-ion secondary batteries that use layered or spinel-type lithium metal composite oxides as the positive electrode active material can obtain a voltage of about 4 V. As such batteries have a high energy density, they are currently the subject of active research and development, and some of them are already being put to practical use.

[0005] Positive electrode active materials for lithium ion secondary batteries include, for example, lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel, which is cheaper than cobalt, and lithium nickel cobalt manganese composite oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), lithium manganese composite oxide (LiMn2O4), lithium nickel manganese composite oxide (LiNi0.5 Mn 0.5 Lithium metal composite oxides such as CrO2 have been proposed.

[0006] In order to obtain high output characteristics in a lithium ion secondary battery, it is important to reduce the internal resistance, and for example, there is a demand for reducing the positive electrode resistance (reaction resistance) in the positive electrode. In particular, in an all-solid-state secondary battery using a solid electrolyte, there is a demand for further reduction in the interface resistance between the positive electrode active material and the solid electrolyte in the positive electrode.

[0007] As a technique for reducing the positive electrode resistance (reaction resistance) of a positive electrode active material, for example, several techniques have been proposed in which the positive electrode active material is coated with a layer containing a different element (e.g., tungsten) other than the metal element contained in the lithium metal composite oxide.

[0008] For example, Patent Document 1 proposes a coated active material for use in a battery, which has an active material and a coating layer that coats the active material, and is characterized in that the coating layer is made of a material containing elemental tungsten. According to Patent Document 1, an increase in the interface resistance between the active material and the solid electrolyte material occurs when the two react with each other to generate a high resistance layer at the interface, but it is said that a coated active material that can suppress the increase in interface resistance can be obtained.

[0009] Patent Document 2 proposes a positive electrode active material for non-aqueous electrolyte secondary batteries, which contains a first lithium metal composite oxide and a second compound containing lithium and tungsten, the surface of the primary particles being coated with the second compound, the tungsten content being 0.01% by mass or more and 1.0% by mass or less with respect to the entire positive electrode active material, and the amount of lithium eluted when the positive electrode active material is dispersed in water, as measured by neutralization titration, being 0.01% by mass or more and less than 0.4% by mass with respect to the entire positive electrode active material. According to Patent Document 2, a secondary battery using this positive electrode active material is said to have high output characteristics and charge / discharge capacity.

[0010] Patent Document 3 also proposes a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, which includes a mixing step of mixing lithium nickel composite oxide particles with a lithium-free tungsten compound powder to obtain a tungsten mixture containing lithium nickel composite oxide particles and tungsten compound particles, and a heat treatment step of heat treating the tungsten mixture to disperse tungsten on the primary particle surfaces and form lithium nickel composite oxide particles having a compound containing tungsten and lithium on the primary particle surfaces. According to Patent Document 3, when used as a battery positive electrode material, a positive electrode active material that can achieve high capacity and high output can be obtained.

[0011] Patent Document 4 proposes a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, which includes mixing a calcined powder made of a lithium metal composite oxide, a first compound which is at least one selected from the group consisting of an oxide not containing lithium, an oxide hydrate, and an inorganic acid salt not containing lithium, with water, and drying the mixture obtained by mixing, where the first compound is a compound capable of reacting with lithium ions in the presence of water to form a second compound containing lithium. According to Patent Document 4, it is said that a positive electrode active material can be obtained which can maintain the battery capacity when a secondary battery is constructed, has high output characteristics, and is excellent in charge and discharge cycle characteristics at a high level. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] WO2012 / 105048 publication [Patent Document 2] WO2018 / 043515 publication [Patent Document 3] JP 2017-134996 A [Patent Document 4] WO2017 / 073238 publication Summary of the Invention [Problem to be solved by the invention]

[0013] The above Patent Documents 1 to 4 propose positive electrode active materials in which the positive electrode resistance (reaction resistance) is reduced and the output characteristics are improved by coating with a different element including tungsten. However, in secondary batteries using a lithium metal composite oxide as the positive electrode active material, there is a demand for further reduction in the positive electrode resistance (reaction resistance) while maintaining a high battery capacity.

[0014] The present inventors have conducted extensive research and found that the coverage of tungsten in conventional positive electrode active materials coated with a layer containing tungsten is insufficient. They have also found that by further improving the coverage of tungsten on the surface of lithium metal composite oxide particles, it is possible to further reduce the positive electrode resistance (reaction resistance) while maintaining a high battery capacity.

[0015] In view of the above problems, the present invention aims to provide a positive electrode active material that has a high tungsten coverage and, when used in a positive electrode for a lithium ion secondary battery, can maintain a high battery capacity while significantly reducing the positive electrode resistance (reaction resistance) and providing high output characteristics. It also aims to provide a method for easily and highly productively producing such a positive electrode active material on an industrial scale. [Means for solving the problem]

[0016] According to a first aspect of the present invention, there is provided a positive electrode active material for a lithium ion secondary battery obtained by mixing particles of a lithium metal composite oxide and particles of a compound containing tungsten, the positive electrode active material having lithium metal composite oxide particles and a layer containing tungsten covering at least a part of the surface of the lithium metal composite oxide particles, wherein the content of tungsten on the surface of the lithium metal composite oxide particles as measured using X-ray photoelectron spectroscopy (XPS) exceeds 50 mol % relative to the content of all metal elements other than lithium on the surface of the particles.

[0017] The content of tungsten in the entire positive electrode active material is preferably more than 1 mass% and not more than 4 mass%. At least a part of the layer containing tungsten preferably has a thickness of 10 nm or less. The lithium metal composite oxide particles preferably contain lithium (Li), nickel (Ni), cobalt (Co), and element M, and the substance amount ratio (molar ratio) of these elements is Li:Ni:Co:M=s:(1-xy):x:y (where 0.95≦s≦1.30, 0≦x≦0.35, 0≦y≦0.35, and M is one or more elements selected from Mn, Mo, V, Mg, Ca, Al, Ti, Cr, Zr, La, Nb, Hf, and Ta).

[0018] According to a second aspect of the present invention, there is provided a method for producing a positive electrode active material for a lithium ion secondary battery, comprising: spraying water onto and mixing with particles of a lithium metal composite oxide in a decarbonation atmosphere to obtain a first mixture; mixing the first mixture with particles of a compound containing tungsten to obtain a second mixture; and drying the second mixture to coat at least a portion of the surface of the lithium metal composite oxide particles with a layer containing tungsten, wherein the lithium metal composite oxide particles obtained after drying have a tungsten content on the surface of the particles that exceeds 50 mol % relative to the content of all metal elements other than lithium on the surface of the particles, as measured by X-ray photoelectron spectroscopy (XPS).

[0019] Moreover, it is preferable that water is mixed in an amount of 2 mass% or more with respect to the entire lithium metal composite oxide particles. It is preferable that the compound containing tungsten is mixed so that the amount of tungsten with respect to the entire lithium metal composite oxide particles is more than 1 mass% and 4 mass% or less. It is preferable that the compound containing tungsten contains tungsten oxide. It is preferable that the lithium metal composite oxide particles contain lithium (Li), nickel (Ni), cobalt (Co), and element M, and the substance amount ratio (molar ratio) of these elements is expressed as Li:Ni:Co:M=s:(1-xy):x:y (where 0.95≦s≦1.30, 0≦x≦0.35, 0≦y≦0.35, and M is one or more elements selected from Mn, Mo, V, Mg, Ca, Al, Ti, Cr, Zr, La, Nb, Hf, and Ta). It is preferable that drying is performed at 50°C or more and 300°C or less.

[0020] According to a third aspect of the present invention, there is provided a lithium ion secondary battery having a positive electrode, a negative electrode, and an electrolyte, in which the positive electrode contains the above-mentioned positive electrode active material. Effect of the Invention

[0021] The positive electrode active material of the present invention has a surface of a lithium metal composite oxide particle covered with tungsten at a very high coverage rate, and in a lithium ion secondary battery using this positive electrode active material in the positive electrode, it is possible to reduce the positive electrode resistance (reaction resistance) while maintaining a high battery capacity, thereby improving the output characteristics. In addition, according to the manufacturing method of the positive electrode active material of the present invention, the above-mentioned positive electrode active material can be easily manufactured on an industrial scale with high productivity. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a diagram illustrating an example of a positive electrode active material according to this embodiment. [Diagram 2] FIG. 2 is a diagram showing an example of a method for producing a positive electrode active material according to this embodiment. [Diagram 3]FIG. 3 is a graph showing the tungsten coverage (mol %) and total carbon amount (mass %) of the positive electrode active materials obtained in the base materials used in the examples, Comparative Example 8, and Comparative Example 9. [Figure 4] FIG. 4 is a graph showing the coverage (mol %) of tungsten for the positive electrode active materials obtained in Comparative Example 6, Comparative Example 7, Example 1, and Example 3. [Diagram 5] FIG. 5 is a graph showing the tungsten coverage (mol %) and initial discharge capacity (relative value) of the positive electrode active materials obtained in Comparative Example 9 and Example 1. [Figure 6] 6(A) and 6(B) are photographic drawings showing backscattered electron images (COMPO images) by SEM of the positive electrode active materials obtained in Comparative Example 9 and Example 1. FIG. [Figure 7] FIG. 7 is a schematic cross-sectional view of a coin-type battery used in the battery evaluation. [Figure 8] FIG. 8 is a schematic explanatory diagram of an example of impedance evaluation measurement and an equivalent circuit used in the analysis. [Figure 9] FIG. 9 is a graph showing the relationship between the tungsten content (mass %) and the tungsten coverage (mol %) of the positive electrode active materials obtained in the examples and comparative examples. [Figure 10] 10(A) and 10(B) are photographic drawings showing backscattered electron images (COMPO images) by SEM of the positive electrode active material (surface and cross section) obtained in Example 1. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, a description will be given of a positive electrode active material for a lithium ion secondary battery (hereinafter also referred to as a "secondary battery") according to an embodiment, a method for producing the same, and a lithium ion secondary battery, with reference to the drawings. Note that the present invention is not limited to the embodiments described below. In addition, in the drawings, in order to make each configuration easier to understand, some parts are emphasized or simplified, and the actual structure or shape, scale, etc. may differ.

[0024] 1.Cathode active material Fig. 1(A) is a schematic diagram showing an example of a positive electrode active material of this embodiment. The positive electrode active material 100 has a lithium metal composite oxide particle 10 and a layer WL containing tungsten. The layer WL containing tungsten covers at least a part of the surface of the lithium metal composite oxide particle 10. Hereinafter, the positive electrode active material according to this embodiment will be described with reference to Fig. 1(A).

[0025] (1) Layer containing tungsten The positive electrode active material 100 has improved lithium ion conductivity and can reduce the positive electrode resistance in the positive electrode of a secondary battery due to the presence of a layer WL containing tungsten W on the surface of the lithium metal composite oxide particle 10. In addition, the positive electrode active material 100 has a high coverage of tungsten (W) on the surface (entire surface of the powder) of the lithium metal composite oxide particle 10, so that the entire particle (powder) is more uniformly coated with tungsten, and when used in the positive electrode of a secondary battery, the positive electrode resistance is reduced and a decrease in battery capacity due to coating with a different element can be suppressed.

[0026] [Tungsten content on particle surface] The tungsten content on the surface of the lithium metal composite oxide particles 10, as measured using X-ray photoelectron spectroscopy (XPS), exceeds 50 mol%, preferably 55 mol% or more, more preferably 60 mol% or more, and even more preferably 65 mol% or more, relative to the content of all metal elements other than lithium on the surface of the particles 10. When the tungsten content is within the above range, the surface of the lithium metal composite oxide particles 10 (the surface of the entire powder) can be more uniformly coated with tungsten (W).

[0027] The upper limit of the tungsten content on the surface of the lithium metal composite oxide particles 10 is not particularly limited, and may be, for example, 90 mol % or less, 80 mol % or less, or 75 mol % or less.

[0028] As a result of intensive research, the present inventors found that the coverage of tungsten is insufficient in a cathode active material having a layer containing tungsten obtained by a conventional manufacturing method, and that, for example, in the manufacturing method used in the comparative example described later, even if the amount of added tungsten is increased, the tungsten content (mol%) on the surface of the lithium metal composite oxide particle 10 is about 30 to 35 mol%, and does not tend to increase beyond that (see Comparative Examples 4 to 6, 8, and 10 in FIG. 9). On the other hand, in the cathode active material 100 according to this embodiment, for example, by using the manufacturing method described later, the tungsten content (mol%) on the surface of the lithium metal composite oxide particle 10 can be set to the above range.

[0029] In addition, when the surface of the lithium metal composite oxide particle 10 is coated with a different element, the battery characteristics such as the battery capacity (e.g., initial charge / discharge capacity) of the secondary battery using the same may be reduced, but in the positive electrode active material 100, the tungsten content (mol%) on the surface of the lithium metal composite oxide particle 10 is set within the above range, thereby making it possible to further reduce the positive electrode resistance (reaction resistance) while maintaining a high battery capacity. Therefore, when the positive electrode active material 100 according to this embodiment is used in the positive electrode of a lithium ion secondary battery (including a non-aqueous electrolyte secondary battery and an all-solid-state secondary battery), the battery characteristics can be improved.

[0030] The tungsten content (mol %) is one of the indicators showing the coverage of the tungsten-containing layer WL on the surface of the lithium metal composite oxide particle 10. Therefore, in this specification, the tungsten content (mol %) on the surface of the lithium metal composite oxide particle 10 is also simply referred to as the "tungsten coverage (mol %)."

[0031] In this specification, the tungsten content (mol %) on the surface of the lithium metal composite oxide particle 10 is a value obtained from the intensity (area) ratio of peaks derived from each metal element in the XPS spectrum obtained when the lithium metal composite oxide particle 10 is measured by X-ray photoelectron spectroscopy (XPS) using an X-ray photoelectron spectrometer (ESCALAB220i-XL, manufactured by VG-Scientific) with an Al target, an Al-Kα X-ray source, a voltage of 10 kV, and a current of 15 mA.

[0032] [Tungsten content in the entire positive electrode active material] The content of tungsten in the entire positive electrode active material 100 is not particularly limited and can be appropriately adjusted depending on the characteristics (particle size, particle structure, etc.) of the lithium metal composite oxide particles 10, but is, for example, more than 1 mass% to 4 mass% or less, preferably more than 1 mass% to 2 mass% or less, and more preferably 1.2 mass% to 2 mass% or less. When the content of tungsten in the entire positive electrode active material 100 is within the above range, it is possible to achieve both a high tungsten coverage (mol%) and a reduction in battery capacity when the positive electrode active material 100 is used in a secondary battery.

[0033] When the tungsten content is within the above range, the surface of the lithium metal composite oxide particles 10 (the surface of the entire powder) can be more uniformly covered with tungsten, and the decrease in the battery capacity (e.g., initial charge / discharge capacity, etc.) can be suppressed. The tungsten (W) content in the positive electrode active material (whole) can be measured by inductively coupled plasma (ICP) emission spectroscopy (ICP method).

[0034] [Thickness of tungsten-containing layer] At least a part of the tungsten-containing layer WL may have a thickness of 10 nm or less, may have a thickness of 5 nm or less, or may have a thickness of 1 nm or less. When the thickness of the tungsten-containing layer WL is within the above range, the entire surface of the lithium metal composite oxide particle 10 can be more uniformly covered with tungsten, and the deterioration of battery characteristics such as battery capacity due to the covering of the tungsten-containing layer WL can be more suppressed (for example, see FIG. 10(B)).

[0035] The thickness of the tungsten-containing layer WL can be determined from the results of a backscattered electron image (COMPO image) obtained by a scanning electron microscope (SEM), STEM, SEM-EDS, or the like, and can be determined, for example, by the method described in the Examples.

[0036] As long as the coverage (mol %) of tungsten is within the above-mentioned range, the tungsten-containing layer WL does not need to cover the entire surface of the lithium metal composite oxide particle 10, and may cover a portion of the surface of the lithium metal composite oxide particle 10. When the cross sections of 10 or more randomly selected lithium metal composite oxide particles 10 are observed using a backscattered electron image (COMPO image) by SEM, the average thickness of the tungsten-containing layer WL may be 10 nm or less, or may be 5 nm or less.

[0037] The form of tungsten in the tungsten-containing layer WL is not particularly limited, and may be, for example, a compound containing lithium and tungsten, or lithium tungstate. For example, when using a manufacturing method for the positive electrode active material 100 described later, the compound containing tungsten reacts with lithium present on the surface of the lithium metal composite oxide particle (base material) to form lithium tungstate, thereby reducing the amount of excess lithium on the surface of the resulting lithium metal composite oxide particle 10. The form of tungsten can be confirmed, for example, by X-ray diffraction (XRD).

[0038] [Lithium metal composite oxide particles] FIG. 1(B) is a schematic diagram showing an example of a lithium metal composite oxide particle 10. The lithium metal composite oxide particle 10 is composed of secondary particles 2 formed by agglomeration of a plurality of primary particles 1. The shape of the secondary particles 2 is not particularly limited, and may have a structure such as a solid structure, a hollow structure, or a porous structure. The lithium metal composite oxide particle 10 may include not only the secondary particles 2 but also a small number of single primary particles 1. The lithium metal composite oxide particle 10 may be an oxide containing lithium and a metal other than lithium, and preferably has a layered crystal structure of a hexagonal system. The layer WL containing tungsten described above may be formed on the surface of the secondary particles 2, or may be formed on the surface of the primary particles 1 inside the secondary particles 2.

[0039] [Composition of positive electrode active material] The positive electrode active material 100 may contain, for example, lithium (Li), nickel (Ni), cobalt (Co), and element M, and the substance amount ratio (molar ratio) of these elements may be expressed as Li:Ni:Co:M=s:(1-xy):x:y (where 0.95≦s≦1.3, 0≦x≦0.35, 0≦y≦0.35, and M is one or more elements selected from Mn, Mo, V, Mg, Ca, Al, Ti, Cr, Zr, La, Nb, Hf, and Ta). When the positive electrode active material 100 has the above composition, it can obtain high battery capacity and excellent output characteristics when used in the positive electrode of a secondary battery. The content of each element can be measured by an ICP method.

[0040] Nickel (Ni) is an element that contributes to increasing the potential and capacity of a secondary battery. In the above molar ratio, the value of (1-xy) indicating the Ni content is, for example, 0.3 or more, preferably 0.6 or more, more preferably 0.65 or more and 0.99 or less, and even more preferably 0.8 or more and 0.95 or less. When the value of (1-xy) exceeds 0.6, a high battery capacity can be obtained.

[0041] Cobalt (Co) is an element that contributes to improving charge-discharge cycle characteristics. In the above molar ratio, the value of x, which indicates the content of Co, is 0 to 0.35, preferably 0.05 to 0.35, more preferably 0.1 to 0.3. When the value of x is 0.05 or more, the charge-discharge cycle characteristics are improved.

[0042] M, which indicates an additive element, is at least one element selected from Mn, Mo, V, Mg, Ca, Al, Ti, Cr, Zr, La, Nb, Hf, and Ta. In the above molar ratio, the value of y, which indicates the content of M, is 0 or more and 0.35 or less, and when y is greater than 0, the thermal stability, output characteristics, cycle characteristics, and the like can be improved. In addition, M preferably contains Al. When M contains Al and the content of Al in the above molar ratio is y1 and the content of M other than Al is y2 (where y1+y2=y), the value of y1 is preferably 0.01 or more and 0.1 or less. In addition, the value of y2 may be 0 or more and 0.1 or less, or may be 0.

[0043] In the above molar ratio, the value of s indicating the lithium content is preferably 0.95 or more and 1.3 or less, more preferably 1.0 or more and 1.10 or less, and may be more than 1.0 and 1.10 or less. When the value of s is less than 0.95, the site that lithium should occupy in the crystal of the lithium metal composite oxide particle 10 is occupied by other elements, and the charge / discharge capacity of the secondary battery may decrease. On the other hand, when the value of s exceeds 1.3, an excess amount of lithium compound that does not contribute to charge / discharge is present other than the lithium nickel composite oxide particle 10 and the compound containing lithium and tungsten, and the positive electrode resistance (reaction resistance) may increase or the charge / discharge capacity may decrease.

[0044] The positive electrode active material 100 has a composition other than tungsten represented by the general formula (1): Li s Ni 1-x-y Co x M y O 2+α(In the general formula (1), 0.95≦s≦1.30, 0≦x≦0.35, 0≦y≦0.35, 0≦α≦0.5, and M is one or more elements selected from Mn, Mo, V, Mg, Ca, Al, Ti, Cr, Zr, La, Nb, Hf, and Ta). In the general formula (1), the preferred range of each element can be the same as the molar ratio described above.

[0045] [Volume average particle size] The size of the positive electrode active material 100 is not particularly limited, but the volume average particle size (MV) is preferably about 1 μm or more and 30 μm or less, and more preferably 5 μm or more and 20 μm or less. The volume average particle size (MV) can be calculated, for example, from the integrated volume measured by a laser light diffraction scattering type particle size distribution analyzer.

[0046] [Particle size variation index] The positive electrode active material 100 may have a particle size variation index [(D90-D10) / MV] of, for example, 0.65 or more, or 0.70 or more. When the variation index of the positive electrode active material 100 is in the above range, fine particles and coarse particles are appropriately mixed in, and the packing property of the particles of the positive electrode active material 100 in the positive electrode can be improved while suppressing the deterioration of the cycle characteristics and output characteristics of the obtained secondary battery. The upper limit of [(D90-D10) / MV] is not particularly limited, but from the viewpoint of suppressing the excessive mixing of fine particles or coarse particles in the positive electrode active material 100, the variation index of the composite hydroxide is preferably 1.2 or less, more preferably 1.0 or less.

[0047] In the above [(D90-D10) / MV], D10 means the particle size at which the cumulative volume of the number of particles at each particle size, calculated from the smallest particle size, is 10% of the total volume of all particles, and D90 means the particle size at which the cumulative volume of the number of particles, calculated from the smallest particle size, is 90% of the total volume of all particles. MV, D90, and D10 can be measured using a laser light diffraction / scattering particle size analyzer.

[0048] The method for producing the positive electrode active material 100 is not particularly limited as long as the above-mentioned properties can be obtained, but it is preferable to use the method for producing the positive electrode active material described below.

[0049] 2. Manufacturing method of positive electrode active material Fig. 2 is a diagram showing an example of a method for producing a positive electrode active material for a lithium ion secondary battery according to this embodiment (hereinafter, also referred to as a "method for producing a positive electrode active material"). As shown in Fig. 2, the above-mentioned positive electrode active material 100 can be easily produced on an industrial scale with high productivity by the method for producing a positive electrode active material according to this embodiment. Note that Fig. 2 shows an example of the method for producing a positive electrode active material, and the method is not limited to this method.

[0050] The method for producing the positive electrode active material 100 includes the steps of spraying water onto and mixing lithium metal composite oxide particles (base material) in a decarbonation atmosphere to obtain a first mixture (step S10), mixing the first mixture with particles of a compound containing tungsten to obtain a second mixture (step S20), and drying the second mixture to coat at least a portion of the surface of the lithium metal composite oxide particles 10 with a layer WL containing tungsten (step S30). Each step will be described below with reference to FIG. 2.

[0051] [Step S10] First, in a decarbonation atmosphere, water is sprayed onto and mixed with lithium metal composite oxide particles (base material) to obtain a first mixture (step S10). The lithium metal composite oxide particles used as the base material are also referred to as "lithium metal composite oxide particles 10a" below. As described below, it is believed that lithium present on the surface of the lithium metal composite oxide particles 10a reacts with a compound containing tungsten to obtain lithium metal composite oxide particles 10 having a layer WL containing tungsten formed thereon.

[0052] (Water spray atmosphere) In the manufacturing method according to the present embodiment, the coverage of tungsten can be significantly improved by using a decarbonated atmosphere when spraying and mixing water. Hereinafter, the effect of the atmosphere when spraying water on the coverage (mol%) of tungsten on the surface of the lithium metal composite oxide particle 10 will be described with reference to FIG. 3. Note that each example in FIG. 3 shows the base material used in the examples and the positive electrode active materials obtained in Comparative Example 8 and Comparative Example 9, which will be described later.

[0053] The bar graph in FIG. 3 is a graph showing the coverage (mol %) of tungsten in each example, and the line graph in FIG. 3 is a graph showing the total carbon amount (TC amount) contained in the entire positive electrode active material in each example.

[0054] As shown in FIG. 3, in positive electrode active materials obtained by coating tungsten under the same conditions except for the atmosphere when spraying and mixing water, the positive electrode active material obtained by spraying water in a decarbonation atmosphere (Comparative Example 9) has a significantly higher tungsten coverage (mol %) than the positive electrode active material obtained by spraying water in an air atmosphere (Comparative Example 8).

[0055] Moreover, in the positive electrode active material obtained by spraying water in an air atmosphere (Comparative Example 8), the amount of TC contained in the positive electrode active material 100 is increased compared to the lithium metal composite oxide used as the base material (left side of the graph in FIG. 3) and the positive electrode active material obtained by spraying water in a decarbonated atmosphere (Comparative Example 9).

[0056] Although the details of the reasons for these are unclear, for example, when water is sprayed in an atmospheric environment, carbon dioxide (CO2) contained in the air reacts with lithium present on the surface of the lithium metal composite oxide particles (base material) to form carbonate, which inhibits the formation of a tungsten-containing layer WL in the entire lithium metal composite oxide particle (entire powder), resulting in a decrease in the tungsten coverage (mol%) and an increase in the TC amount.

[0057] The decarbonation atmosphere refers to an atmosphere in which the content of carbon dioxide gas (CO2) is reduced below that of the air atmosphere, and for example, the content of carbon dioxide gas (CO2) may be less than 100 ppm by volume, 50 ppm by volume or less, 20 ppm by volume or less, or 10 ppm by volume or less. The lower limit of the content of carbon dioxide gas (CO2) in the decarbonation atmosphere is not particularly limited, and may be 0 ppm by volume or more.

[0058] The decarbonation atmosphere is not particularly limited in terms of the content of components other than carbon dioxide, and any atmosphere can be used. For example, air with a reduced carbon dioxide content (decarbonated air), an inert gas atmosphere, an oxygen atmosphere, etc. may be used, and it is preferable to use decarbonated air.

[0059] (Amount of water to be sprayed) The amount of water sprayed onto the lithium metal composite oxide particles 10a is not particularly limited, but from the viewpoint of sufficiently forming the tungsten-containing layer WL, the amount of water is preferably 2 mass % or more, more preferably 3 mass % or more, and even more preferably 4 mass % or more, relative to the lithium metal composite oxide particles 10a.

[0060] Fig. 4 is a graph showing the coverage (mol%) of tungsten in each example where the amount of sprayed water was changed. The examples in Fig. 4 show the positive electrode active materials obtained in Comparative Example 6, Comparative Example 7, Example 1, and Example 3, which will be described later.

[0061] As shown in FIG. 4, in positive electrode active materials obtained by coating tungsten under the same conditions except for changing the amount of water sprayed, the positive electrode active material obtained by spraying 8% water by mass (Comparative Example 7, Example 3) tends to have a higher tungsten coverage (mol %) than the positive electrode active material obtained by spraying 4% water by mass (Comparative Example 6, Example 1).

[0062] The upper limit of the amount of water to be sprayed is not particularly limited and can be appropriately adjusted depending on the particle shape of the lithium metal composite oxide particles 10a used as the base material, and may be, for example, 20 mass % or less, or 10 mass % or less.

[0063] (Water spraying and other mixing conditions) The water to be sprayed may be in a mist state, for example, or may be in a mist state with an average size of 100 μm or less. The device for spraying and mixing the water may be any device that can obtain a uniform mixture, and various mixers such as a shaker mixer, a stirring mixer, and a rocking mixer may be used depending on the amount of water to be added.

[0064] (Lithium metal composite oxide particles) The composition of the lithium metal composite oxide particles 10a used as the base material is not particularly limited, and may be, for example, within the same range as the composition of the above-mentioned positive electrode active material 100. The preferred ranges of each element contained in the lithium metal composite oxide particles 10a are the same as the composition of the above-mentioned positive electrode active material 100, and therefore will not be described here.

[0065] The method for producing the lithium metal composite oxide particles 10a is not particularly limited, but for example, they may be produced by crystallization. When produced by crystallization, the lithium metal composite oxide particles 10a having a relatively uniform composition can be obtained. For example, when the lithium metal composite oxide particles 10a having a high nickel content are used as the positive electrode active material 100, they may be washed with water before use. However, in the method for producing the positive electrode active material according to this embodiment, the lithium metal composite oxide particles 10a having a high nickel content can be used as the base material without washing with water.

[0066] In addition, since the particle properties of the lithium metal composite oxide particles 10a used as the base material are also inherited in the positive electrode active material 100, the particle size and particle size variation index of the lithium metal composite oxide particles 10a can be made similar to the particle size and particle size variation index of the desired positive electrode active material 100.

[0067] [Step S20] Next, the first mixture is mixed with particles of a compound containing tungsten to obtain a second mixture (step S20). In the manufacturing method according to the present embodiment, after the lithium metal composite oxide particles 10a are mixed with water (step S10), the compound containing tungsten is mixed (step S20), thereby improving the coverage (mol%) of tungsten and providing a high battery capacity when used in a secondary battery.

[0068] (Mixing order) The bar graph in Fig. 5 is a graph showing the coverage (mol%) of tungsten in each example, and the line graph in Fig. 5 is a graph showing the initial discharge capacity (relative value) in each example. Hereinafter, with reference to Fig. 5, the influence on the coverage (mol%) of tungsten when the order of mixing the lithium metal composite oxide particles 10a with water and a tungsten-containing compound is changed will be described. Note that the samples in Fig. 5 use the positive electrode active material 100 obtained in Comparative Example 9 and Example 1 described below.

[0069] As shown in FIG. 5, when tungsten (1.5 mass%) was coated under the same conditions except for changing the order of mixing water and the compound containing tungsten, the case in which water was mixed first and then the compound containing tungsten (Example 1) had a higher tungsten coverage (mol %) and a higher initial discharge capacity than the case in which the compound containing tungsten was mixed first and then water was mixed (Comparative Example 6).

[0070] 6(A) and 6(B) are SEM backscattered electron images of the positive electrode active materials obtained in the above examples (Comparative Example 9 and Example 1). In FIG. 6(A) and FIG. 6(B), the white parts (bright parts) are considered to represent tungsten (heavy element). As shown in FIG. 6(A) and FIG. 6(B), the positive electrode active material has less white parts and is more uniformly coated with tungsten when the compound containing tungsten is mixed with water and then mixed with water (Example 1) than when the compound containing tungsten is mixed with water and then mixed with water (Comparative Example 9), although the tungsten content in the positive electrode active material is about the same.

[0071] Although the details of the reason for this are unclear, it is believed that, for example, by mixing water before the compound containing tungsten, the reactivity between the lithium metal composite oxide particles 10a and the compound containing tungsten is improved, and tungsten is uniformly coated on the entire surface (entire powder) of the lithium metal composite oxide particles 10.

[0072] (Particles of compounds containing tungsten) The particles of the compound containing tungsten are preferably a solid-state compound capable of reacting with lithium, and the particles of the compound containing tungsten are preferably free of lithium.

[0073] Examples of compounds containing tungsten include tungsten oxide, tungstic acid, and ammonium tungstate. Among these, at least one of tungsten oxide and tungstic acid is preferred, and tungsten oxide is more preferred. The compounds containing tungsten may be used alone or in combination of two or more.

[0074] The amount of the particles of the compound containing tungsten is not particularly limited and can be appropriately adjusted so as to obtain the above-mentioned positive electrode active material 100. For example, the amount of tungsten may be more than 1 mass% and not more than 4 mass% based on the total amount of the lithium metal composite oxide particles 10a, preferably more than 1 mass% and not more than 2 mass%, more preferably 1.2 mass% or more and not more than 2 mass%. The amount of the particles of the compound containing tungsten may be set by, for example, performing a preliminary test in advance to confirm the amount of the compound containing tungsten that can obtain the positive electrode active material 100.

[0075] [Step S30] Next, the second mixture is dried to cover at least a part of the surface of the lithium metal composite oxide particle 10a with a layer WL containing tungsten (step S30). In step S30, while removing moisture, lithium present on the surface of the lithium metal composite oxide particle 10a reacts with the compound containing tungsten to form the layer WL containing tungsten.

[0076] The drying temperature is not particularly limited as long as it is a temperature at which at least a portion of the moisture can be removed and a layer WL containing tungsten can be formed, and is, for example, from 50° C. to 300° C., preferably from 80° C. to 250° C., and more preferably from 90° C. to 200° C. When the drying temperature is within the above range, the reaction between the lithium present on the surface of the lithium metal composite oxide particles 10a and the compound containing tungsten can be sufficiently advanced, and tungsten can be sufficiently dispersed on the surface of the obtained lithium metal composite oxide particles 10.

[0077] The drying time is not particularly limited, but is, for example, from 5 hours to 72 hours, preferably from 10 hours to 48 hours, and more preferably from 15 hours to 25 hours.

[0078] Furthermore, from the viewpoint of dispersing tungsten more thoroughly on the surface of the resulting lithium metal composite oxide particles 10, the drying may be performed in at least two stages. For example, a first drying step may involve drying at a temperature of 50° C. or more and 200° C. or less for a period of 5 hours or more and 24 hours or less, and a second drying step may involve drying at a temperature of 50° C. or more and 250° C. or less, which is a temperature higher than that of the first drying step, for a period of 5 hours or more and 24 hours or less.

[0079] In addition, from the viewpoint of suppressing the reaction between moisture or carbon dioxide gas (CO2) in the atmosphere and unreacted lithium compound remaining on the surface of the lithium metal composite oxide particles 10a, the atmosphere during drying is preferably a decarbonated atmosphere (e.g., decarbonated air), an inert gas atmosphere, or a vacuum atmosphere, and a vacuum atmosphere is more preferable.

[0080] In addition, the pressure of the atmosphere during drying is not particularly limited, but is preferably lower than atmospheric pressure, and is preferably 1 atm or less. If the pressure is higher than 1 atm, the water content of the positive electrode active material 100 may not be reduced sufficiently.

[0081] [Characteristics of the positive electrode active material] In the method for producing a positive electrode active material according to this embodiment, the positive electrode active material 100 obtained preferably has the following properties.

[0082] (total carbon) The total carbon amount (TC amount) contained in the positive electrode active material 100 may be 0.07% by mass or less, or may be 0.065% by mass or less, based on the entire positive electrode active material 100. When the total carbon amount (TC amount) is within the above range, it indicates that the formation of carbonates on the surfaces of the lithium metal composite oxide particles 10 is suppressed. In addition, the TC amount contained in the positive electrode active material 100 is preferably 0.9 to 1.1 times the TC amount contained in the lithium metal composite oxide particles 10a used as the base material.

[0083] (Initial discharge capacity) The positive electrode active material 100 has an initial discharge capacity (initial discharge capacity of the positive electrode active material 100 / initial discharge capacity of the base material) of the lithium metal composite oxide particles 10 (i.e., the positive electrode active material 100) coated with a layer WL containing tungsten, when used as a positive electrode active material of a 2032-type coin battery, preferably 0.9 times or more, more preferably 0.95 times or more, compared to the initial discharge capacity of the lithium metal composite oxide particles 10a (i.e., the base material) before spraying water, when used as a positive electrode active material of a 2032-type coin battery. The upper limit of (initial discharge capacity of the positive electrode active material 100 / initial discharge capacity of the base material) is not particularly limited, but may be, for example, 1.1 times or less, or 1.05 times or less.

[0084] The 2032 type coin battery can be produced by the method described later in the Examples, and the initial discharge capacity (mAh / g) can be evaluated by the method described later in the Examples.

[0085] (Reaction resistance) For example, the positive electrode resistance (SOC20%) of the lithium metal composite oxide particles 10a (i.e., the base material) before spraying water is used as the positive electrode active material of a 2032-type coin battery, and the positive electrode resistance (SOC20%) of the lithium metal composite oxide particles 10 (i.e., the positive electrode active material 100) coated with a layer WL containing tungsten is used as the positive electrode active material of a 2032-type coin battery (positive electrode resistance of the positive electrode active material 100 / positive electrode resistance of the base material) is preferably 0.7 times or less, more preferably 0.65 times or less, and even more preferably 0.6 times or less. The lower limit of (positive electrode resistance of the positive electrode active material 100 / positive electrode resistance of the base material) is not particularly limited, but may be 0.3 times or more, or may be 0.4 times or more.

[0086] The 2032 type coin battery can be produced by the method described in the Examples below, and the positive electrode resistance (reaction resistance, Ω) can be evaluated by the method described in the Examples below.

[0087] 3. Lithium-ion secondary battery The lithium ion secondary battery (hereinafter also referred to as "secondary battery") according to this embodiment includes a positive electrode containing the above-mentioned positive electrode active material 100, a negative electrode, and an electrolyte. The lithium ion secondary battery can be configured with the same components as conventionally known lithium ion secondary batteries, and may be, for example, a non-aqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte. The secondary battery may also be, for example, an all-solid-state secondary battery including a positive electrode, a negative electrode, and a solid electrolyte. Each component will be described below.

[0088] It should be noted that the embodiments described below are merely illustrative, and the lithium ion secondary battery according to the present embodiment can be embodied in various forms that are modified and improved based on the knowledge of those skilled in the art based on the embodiments described in this specification. In addition, the lithium ion secondary battery according to the present embodiment is not particularly limited in its application.

[0089] (positive electrode) The method for producing the positive electrode is not particularly limited, but for example, the positive electrode may be produced as follows.

[0090] First, the positive electrode active material 100, the conductive material, and the binder are mixed, and activated carbon and a solvent for viscosity adjustment, etc. are added as necessary, and the mixture is kneaded to prepare a positive electrode composite paste. At that time, the mixing ratio of each in the positive electrode composite paste can be appropriately adjusted according to the performance of the secondary battery to be targeted. For example, when the solid content of the positive electrode composite excluding the solvent is 100 parts by mass, the content of the positive electrode active material 100 may be 60 parts by mass or more and 95 parts by mass or less, the content of the conductive material may be 1 part by mass or more and 20 parts by mass or less, and the content of the binder may be 1 part by mass or more and 20 parts by mass or less.

[0091] The conductive material is not particularly limited, and for example, graphite (natural graphite, artificial graphite, expanded graphite, etc.) and carbon black-based materials such as acetylene black and ketjen black can be used.

[0092] The binder serves to bind the active material particles together and is not particularly limited, but examples of the binder that can be used include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene butadiene, cellulose-based resin, polyacrylic acid, and the like.

[0093] If necessary, a solvent for dispersing the positive electrode active material, the conductive material, and the activated carbon and dissolving the binder may be added to the positive electrode mixture. Specifically, an organic solvent such as N-methyl-2-pyrrolidone may be used as the solvent. Activated carbon may also be added to the positive electrode mixture in order to increase the electric double layer capacity.

[0094] The obtained positive electrode composite paste is applied to the surface of a current collector made of, for example, aluminum foil, and dried to evaporate the solvent. If necessary, pressure may be applied by a roll press or the like to increase the electrode density. In this way, a sheet-shaped positive electrode can be produced. The sheet-shaped positive electrode can be cut to an appropriate size according to the intended battery and used to produce the battery. The method for producing the positive electrode is not limited to the above method, and other methods may be used.

[0095] (Negative electrode) For the negative electrode, metallic lithium or a lithium alloy may be used. Alternatively, a negative electrode active material capable of absorbing and desorbing lithium ions may be mixed with a binder, and an appropriate solvent may be added to form a paste of the negative electrode mixture, which is then applied to the surface of a metal foil collector such as copper, dried, and compressed as necessary to increase the electrode density.

[0096] As the negative electrode active material, for example, natural graphite, artificial graphite, phenol resin, or other organic compound sintered body, and powder of carbon material such as coke can be used. In this case, as with the positive electrode, fluororesin such as PVDF can be used as the negative electrode binder, and organic solvents such as N-methyl-2-pyrrolidone can be used as the solvent for dispersing these active materials and binders. In addition to the organic binders such as PVDF, aqueous binders such as styrene butadiene rubber may also be used as the binder. The aqueous binder may also use carboxymethylcellulose (CMC) as a viscosity modifier. For example, an aqueous binder that uses styrene butadiene latex as the main additive and CMC as a viscosity modifier can increase the binding force with a small amount.

[0097] (Separator) A separator is placed between the positive electrode and the negative electrode as necessary. The separator separates the positive electrode and the negative electrode and retains the electrolyte. A thin membrane such as polyethylene or polypropylene having many minute pores can be used as the separator.

[0098] (Non-aqueous electrolyte) A non-aqueous electrolyte can be used as the non-aqueous electrolyte. For example, the non-aqueous electrolyte may be a solution in which a lithium salt as a supporting salt is dissolved in an organic solvent. Alternatively, the non-aqueous electrolyte may be a solution in which a lithium salt is dissolved in an ionic liquid. The ionic liquid refers to a salt that is composed of cations and anions other than lithium ions and is liquid even at room temperature.

[0099] The organic solvent may be one selected from cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and trifluoropropylene carbonate; chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane; sulfur compounds such as ethyl methyl sulfone and butane sultone; and phosphorus compounds such as triethyl phosphate and trioctyl phosphate. These may be used alone or in combination of two or more.

[0100] The supporting salt may be LiPF6, LiBF4, LiClO4, LiAsF6, LiN(CF3SO2)2, or a composite salt thereof. Furthermore, the non-aqueous electrolyte may contain a radical scavenger, a surfactant, a flame retardant, and the like.

[0101] In addition, when the lithium ion secondary battery is an all-solid-state secondary battery, a solid electrolyte may be used as the non-aqueous electrolyte. The solid electrolyte has a property of being able to withstand high voltage. Examples of the solid electrolyte include inorganic solid electrolytes and organic solid electrolytes.

[0102] As the inorganic solid electrolyte, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, or the like is used.

[0103] The oxide-based solid electrolyte is not particularly limited, and any oxide-based solid electrolyte that contains oxygen (O) and has lithium ion conductivity and electronic insulation can be used. Examples of oxide-based solid electrolytes include lithium phosphate (Li3PO4), Li3PO4N X , LiBON X , LiNbO3, LiTaO3, Li2SiO3, Li4SiO4-Li3PO4, Li4SiO4-Li3VO4, Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3-ZnO, Li 1+X Al X Ti 2-X (PO4)3(0≦X≦1), Li 1+XAl X Ge 2-X (PO4)3(0≦X≦1), LiTi2(PO4)3, Li 3X La 2 / 3-X TiO3(0≦X≦2 / 3), Li5La3Ta2O 12 , Li7La3Zr2O 12 , Li6BaLa2Ta2O 12 , Li 3.6 S 0.6 P 0.4 Examples include O4.

[0104] The sulfide-based solid electrolyte is not particularly limited, and any electrolyte that contains sulfur (S) and has lithium ion conductivity and electronic insulation can be used. Examples of sulfide-based solid electrolytes include Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, LiI-Li2S-P2O5, and LiI-Li3PO4-P2S5.

[0105] As the inorganic solid electrolyte, materials other than those mentioned above may be used, for example, Li3N, LiI, Li3N-LiI-LiOH, etc. may be used.

[0106] The organic solid electrolyte is not particularly limited as long as it is a polymeric compound exhibiting ion conductivity, and for example, polyethylene oxide, polypropylene oxide, and copolymers thereof can be used. The organic solid electrolyte may also contain a supporting salt (lithium salt). When a solid electrolyte is used, the solid electrolyte may also be mixed into the positive electrode material in order to ensure contact between the electrolyte and the positive electrode active material 100.

[0107] (Battery shape and configuration) The lithium ion secondary battery according to the present embodiment, which is configured with the positive electrode, negative electrode, separator, and nonaqueous electrolyte solution described above, or the positive electrode, negative electrode, and solid electrolyte, can be formed into various shapes, such as a cylindrical shape or a laminated shape.

[0108] When a non-aqueous electrolyte solution is used as the non-aqueous electrolyte, a positive electrode and a negative electrode are laminated with a separator interposed therebetween to form an electrode body, the obtained electrode body is impregnated with a non-aqueous electrolyte solution, and the positive electrode current collector and a positive electrode terminal connected to the outside, and the negative electrode current collector and a negative electrode terminal connected to the outside are connected using a current collecting lead or the like, and the battery is sealed in a battery case to complete a lithium ion secondary battery. EXAMPLES

[0109] The present invention will be specifically described below using examples, but the present invention is not limited to these examples. The characteristics of the positive electrode active material and secondary battery obtained by this embodiment were evaluated by the following method. In this example, each sample of special grade reagents manufactured by Wako Pure Chemical Industries, Ltd. was used to prepare the positive electrode active material and secondary battery.

[0110] [composition] The composition of the base material and the positive electrode active material, and the tungsten content were measured by dissolving the base material and the positive electrode active material in acid and then using an ICP emission spectrometer (Shimadzu Corporation, ICPS-8100).

[0111] [Total carbon content] The total carbon amount (TC amount) of the base material and the positive electrode active material was measured using a carbon-sulfur analyzer (CS-600 manufactured by LECO Corporation).

[0112] [Tungsten coverage (mol%)] Using an X-ray photoelectron spectrometer (VG-Scientific, ESCALAB220i-XL) with an Al target, an Al-Kα X-ray source, a voltage of 10 kV, and a current of 15 mA, the XPS spectra of tungsten, nickel, and cobalt on the surface of the lithium metal composite oxide particles were measured, and the tungsten coverage (the tungsten content on the surface of the lithium metal composite oxide particles) was calculated from the ratio of their peak intensities.

[0113] [Thickness of tungsten-containing layer WL (nm)] The particle surface and cross section of the positive electrode active material were observed using a Schottky field emission type scanning electron microscope SEM-EDS, JSM-7001F (manufactured by JEOL Ltd.). The thickness of the tungsten-containing layer WL was measured by observing a cross-section sample processed with a cross-section polisher (CP) [manufactured by JEOL Ltd., product number: SM-09010], drawing two straight lines perpendicular to each other at the approximate center of the cross section of each lithium metal composite oxide particle, measuring the thickness of the tungsten-containing layer WL at four points where these two straight lines intersect, and calculating the average thickness of the tungsten-containing layer WL from the values ​​for 10 particles (n=40).

[0114] [Manufacturing and evaluation of secondary batteries] A method for producing a secondary battery and a method for evaluating battery characteristics will be described below.

[0115] (Secondary battery manufacturing) 52.5 mg of positive electrode active material, 15 mg of acetylene black, and 7.5 mg of polytetrafluoroethylene resin (PTFE) were mixed and pressed under a pressure of 100 MPa to a diameter of 11 mm and a thickness of 100 μm. The mixture was then dried in a vacuum dryer at 120°C for 12 hours to prepare a positive electrode PE (electrode for evaluation).

[0116] Next, a 2032-type coin-type battery CBA (see FIG. 7) was produced using this positive electrode PE in a glove box in an Ar atmosphere with a dew point controlled at -80°C. A lithium metal with a diameter of 17 mm and a thickness of 1 mm was used for the negative electrode NE of this coin-type battery CBA, and an equal mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) with 1M LiClO4 as the supporting electrolyte (manufactured by Toyama Pharmaceutical Co., Ltd.) was used for the electrolyte. A polyethylene porous film with a thickness of 25 μm was used for the separator SE. As shown in FIG. 7, the coin-type battery CBA has a gasket GA and is assembled into a coin-shaped battery by a positive electrode can PC and a negative electrode can NC.

[0117] (Initial discharge capacity) After making the coin cell CBA, leave it for about 24 hours. After the open circuit voltage OCV stabilizes, apply a current density of 0.1 mA / cm to the positive electrode. 2 The capacity when the battery was charged to a cutoff voltage of 4.3 V was defined as the initial charge capacity, and the capacity when the battery was discharged to a cutoff voltage of 3.0 V after a 1-hour rest was defined as the initial discharge capacity. The value obtained by dividing the initial discharge capacity by the initial charge capacity was defined as the initial charge / discharge efficiency (initial discharge capacity / initial charge capacity).

[0118] (Positive electrode resistance) The coin cell CBA was left for about 24 hours after preparation, and after the open circuit voltage OCV stabilized, the current density to the positive electrode was increased to 0.1 mA / cm. 2 The battery was charged at 100 V until the cut-off voltage reached 4.3 V, and after a 1-hour pause, discharged until the cut-off voltage reached 3.0 V. The coin-type battery CBA was then charged to potentials equivalent to SOC 20% and SOC 80%, and the positive electrode resistance (reaction resistance) was calculated by the AC impedance method using a frequency response analyzer and a potentiogalvanostat (Solartron, 1255B).

[0119] The calculation method for the positive electrode resistance (reaction resistance) is explained below. First, when the coin cell CBA is measured by the AC impedance method using a frequency response analyzer and a potentiogalvanostat, a Nyquist plot as shown in Figure 8 is obtained. This Nyquist plot is expressed as the sum of the characteristic curves showing the solution resistance, the negative electrode resistance and its capacity, and the positive electrode resistance and its capacity, so a fitting calculation was performed using an equivalent circuit based on this Nyquist plot to calculate the value of the positive electrode resistance (reaction resistance).

[0120] Example 1 Lithium metal oxide (Li 1.025 Ni 0.82 Co 0.15 Al 0.03O2, average grain size (MV): 12.3 μm, [(D90-D10) / MV]: 0.82, no water washing) was used as the base material. The total carbon content (TC content) of the base material was 0.064 mass%.

[0121] In a decarbonated atmosphere (decarbonated air), the lithium metal composite oxide (base material) was stirred and mixed while 4% by mass of water was sprayed onto the entire lithium metal composite oxide (base material) particles (step S10).Tungsten oxide (WO3) was then added in an amount such that the tungsten in the tungsten oxide was 1.5% by mass with respect to the entire lithium metal composite oxide particles, and mixed (step S20).

[0122] Thereafter, the cathode active material was obtained by drying in a vacuum atmosphere at 100°C for 12 hours and then at 190°C for 10 hours. The tungsten (W) content, tungsten coverage (mol%), and the like of the obtained cathode active material were evaluated by the above-mentioned methods. In addition, a coin-type battery CBA was produced using the obtained cathode active material, and the battery characteristics were evaluated. These evaluation results are shown in Table 1. In addition, the total carbon content (TC content) of the cathode active material obtained in Example 1 was 0.064 mass%.

[0123] Example 2 A positive electrode active material was obtained and evaluated in the same manner as in Example 1. The amount of tungsten contained in the obtained positive electrode active material was 1.3 mass % based on the total mass of the positive electrode active material. The evaluation results are shown in Table 1.

[0124] Example 3 A positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that the amount of water sprayed was 8 mass % based on the total amount of the lithium metal composite oxide particles. The evaluation results are shown in Table 1.

[0125] Comparative Example 1 A positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that the amount of water sprayed was 8 mass% based on the total amount of lithium metal composite oxide particles, and the amount of tungsten oxide mixed was 1 mass% based on the total amount of lithium metal composite oxide particles. The evaluation results are shown in Table 1.

[0126] Comparative Example 2 A positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that the amount of water sprayed was 10 mass% based on the total amount of the lithium metal composite oxide particles, and the amount of tungsten oxide mixed was an amount such that tungsten in the tungsten oxide was 0.5 mass% based on the total amount of the lithium metal composite oxide particles. The evaluation results are shown in Table 1.

[0127] Comparative Example 3 A positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that the amount of water sprayed was 8% by mass relative to the entire lithium metal composite oxide particles, and the amount of tungsten oxide added was an amount such that tungsten in the tungsten oxide was 1% by mass relative to the entire lithium metal composite oxide particles. The evaluation results are shown in Table 1.

[0128] Comparative Example 4 After mixing the lithium metal composite oxide (base material) and tungsten oxide, water was sprayed onto the mixture (steps S10 and S20 were performed in the reverse order to that of Example 1), and the water spraying was performed under an air atmosphere, and the amount of tungsten oxide added was set to an amount such that tungsten in the tungsten oxide was 0.2 mass% relative to the entire lithium metal composite oxide particles. A positive electrode active material was obtained and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0129] Comparative Example 5 A positive electrode active material was obtained and evaluated in the same manner as in Comparative Example 4, except that the amount of tungsten oxide added was set to an amount such that tungsten in the tungsten oxide was 0.5% by mass relative to the entire lithium metal composite oxide particles. The evaluation results are shown in Table 1.

[0130] Comparative Example 6 A positive electrode active material was obtained and evaluated in the same manner as in Comparative Example 4, except that the amount of tungsten oxide added was set to an amount such that tungsten in the tungsten oxide was 1 mass % relative to the entire lithium metal composite oxide particles. The evaluation results are shown in Table 1.

[0131] Comparative Example 7 A positive electrode active material was obtained and evaluated in the same manner as in Comparative Example 4, except that the amount of water sprayed was 8% by mass relative to the entire lithium metal composite oxide particles, and the amount of tungsten oxide added was an amount such that tungsten in the tungsten oxide was 1% by mass relative to the entire lithium metal composite oxide particles. The evaluation results are shown in Table 1.

[0132] Comparative Example 8 A positive electrode active material was obtained and evaluated in the same manner as in Comparative Example 4, except that the amount of tungsten oxide added was set to an amount such that tungsten in the tungsten oxide was 1.5 mass% relative to the entire lithium metal composite oxide particles. The evaluation results are shown in Table 1.

[0133] Comparative Example 9 A positive electrode active material was obtained and evaluated in the same manner as in Example 1, except that the lithium metal composite oxide (base material) and tungsten oxide were mixed and then water was sprayed onto the resulting mixture (steps S10 and S20 were performed in the reverse order to that in Example 1). The evaluation results are shown in Table 1.

[0134] Comparative Example 10 A positive electrode active material was obtained and evaluated in the same manner as in Comparative Example 4, except that the amount of tungsten oxide added was set to an amount such that tungsten in the tungsten oxide was 2 mass% relative to the entire lithium metal composite oxide particles. The evaluation results are shown in Table 1.

[0135] [Table 1]

[0136] (Evaluation Results) As shown in Table 1, the positive electrode active material obtained in the examples had a tungsten coverage (mol%) of more than 50 mol%, indicating that tungsten was more uniformly coated over the entire positive electrode active material. In addition, it was shown that the secondary battery using the positive electrode active material of the examples had the same initial charge / discharge capacity and initial charge / discharge efficiency as the lithium metal composite oxide used as the base material, and also had a low positive electrode resistance (reaction resistance).

[0137] As shown in FIGS. 10(A) and 10(B), when the positive electrode active material obtained in Example 1 was observed using a scanning electron microscope (SEM) backscattered electron image, it was confirmed that a layer WL containing tungsten and having a thickness of 10 nm or less was formed on the surface of the lithium metal composite oxide particles.

[0138] FIG. 9 is a graph showing the relationship between the tungsten content (mass %) and the tungsten coverage (mol %) of the positive electrode active materials obtained in the Examples and Comparative Examples (note that FIG. 9 only shows the Examples and Comparative Examples produced under similar conditions except for the tungsten content (mass %) in the positive electrode active material). As shown in FIG. 9, the positive electrode active materials obtained in Comparative Examples 1 to 3 had a tungsten content of 0.5 to 1 mass %, and a tungsten coverage of 50 mol % or less. In addition, the positive electrode resistance also tended to be higher than that of the Examples.

[0139] In Comparative Examples 4 to 8 and 10, the lithium metal composite oxide (base material) and tungsten oxide (0.2 mass% to 2 mass%) were mixed, and then water was sprayed onto the mixture (steps S10 and S20 were performed in the reverse order to Example 1), and water was sprayed under air atmosphere, and the positive electrode active materials obtained in these Comparative Examples had a low tungsten coverage of 32 mol% or less. As shown in Fig. 9, the positive electrode active material of Comparative Example 10, in which the amount of tungsten oxide added (2 mass%) was increased, also had a low tungsten coverage of 31 mol%, and the initial charge / discharge capacity was also significantly reduced.

[0140] As shown in FIG. 4, when Comparative Example 6 in which the amount of water sprayed was 4 mass % relative to the lithium metal composite oxide was compared with Comparative Example 7 in which the amount of water sprayed was 8 mass % relative to the lithium metal composite oxide, the positive electrode active material obtained in Comparative Example 7 had a higher tungsten coverage (mol %).

[0141] In addition, the positive electrode active material obtained in Comparative Example 9 was produced in the same manner as in Example 1 (spraying water in a decarbonated atmosphere) except that, as described above, steps S10 and S20 were performed in the reverse order to those in Example 1. As shown in FIG. 3, the positive electrode active material obtained in Comparative Example 9 showed a very high tungsten coverage compared to other Comparative Examples, but the tungsten coverage was 50 mol % or less. [Industrial Applicability]

[0142] The positive electrode active material according to the present invention has a very high coverage (mol%) of tungsten, and therefore when used as a positive electrode material for a lithium ion secondary battery, it has a high battery capacity and can improve output characteristics by reducing the positive electrode resistance (reaction resistance). Therefore, the positive electrode active material according to the present invention can be suitably used as a positive electrode active material for lithium ion secondary batteries (non-aqueous electrolyte secondary batteries, all-solid-state secondary batteries, etc.) used as power sources for hybrid vehicles and electric vehicles in particular. [Explanation of symbols]

[0143] 100...Cathode active material 1…Primary particle 2…Secondary particles 10...Lithium metal composite oxide particles 10a...Lithium metal composite oxide particles (base material) WL: Layer containing tungsten CBA…Coin cell battery PE: Positive electrode NE: Negative electrode GA…Gasket PE: Positive electrode NE: Negative electrode SE…Separator

Claims

1. A positive electrode active material obtained by mixing particles of a lithium metal composite oxide and particles of a compound containing tungsten, The present invention relates to a lithium metal composite oxide particle and a layer containing tungsten that covers at least a part of the surface of the lithium metal composite oxide particle, the content of tungsten on the surface of the lithium metal composite oxide particles, as measured by X-ray photoelectron spectroscopy (XPS), exceeds 50 mol % relative to the content of all metal elements other than lithium on the surface of the particles; The tungsten content of the positive electrode active material is more than 1 mass% and not more than 4 mass%. Positive electrode active material for lithium-ion secondary batteries.

2. 2. The positive electrode active material for a lithium ion secondary battery according to claim 1, wherein at least a portion of the layer containing tungsten has a thickness of 10 nm or less.

3. 3. The positive electrode active material for a lithium ion secondary battery according to claim 1, comprising lithium (Li), nickel (Ni), cobalt (Co), and an element M, wherein a substance amount ratio (molar ratio) of these elements is Li:Ni:Co:M=s:(1-x-y):x:y, where 0.95≦s≦1.30, 0≦x≦0.35, 0≦y≦0.35, and M is one or more elements selected from Mn, Mo, V, Mg, Ca, Al, Ti, Cr, Zr, La, Nb, Hf, and Ta.

4. The positive electrode active material for a lithium ion secondary battery according to claim 3, wherein the (1-x-y) is 0.6 or more.

5. The positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 4, wherein at least a portion of the layer containing tungsten has a thickness of 1 nm or less.

6. The positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 5, wherein the average thickness of the layer containing tungsten is 10 nm or less.

7. A lithium ion secondary battery comprising a positive electrode, a negative electrode, and an electrolyte, the positive electrode including the positive electrode active material according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Positive electrode active material for nonaqueous electrolyte secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery arranged by use of positive electrode active material

    JP2017063003A

  • Positive electrode active material for nonaqueous electrolyte secondary battery and method of producing the same, and nonaqueous electrolyte secondary battery including the positive electrode active material

    JP2017134996A

  • Coated active material, battery, and method for producing coated active material

    WO2012105048A1

  • Positive electrode active material for nonaqueous electrolyte secondary batteries, method for producing same, positive electrode mixture paste for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery

    WO2017073238A1

  • Positive electrode active substance for non-aqueous electrolyte secondary battery and method for producing same, positive electrode mixture paste for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery

    WO2018043515A1