Composite active material for secondary battery and secondary battery

A composite active material with silicon particles coated in magnesium silicate and embedded in a silicon dioxide and carbon matrix addresses the inefficiencies in silicon-containing lithium ion batteries, improving initial coulombic efficiency and capacity retention.

JP7586255B2Active Publication Date: 2024-11-19DIC CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023149177
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-10-25
Filing Date
2023-09-14
Publication Date
2024-11-19
Estimated Expiration
2042-08-25

AI Technical Summary

Technical Problem

Conventional lithium ion batteries using silicon-containing active materials suffer from low initial charging/discharging efficiency due to irreversible reactions between lithium and silicon oxide, leading to reduced coulombic efficiency and capacity retention rates, and the dispersion of metal silicates within these materials can inhibit further improvements.

Method used

A composite active material is developed with silicon particles of 150 nm or less, coated with a silicate compound such as magnesium silicate near the surface, and embedded in a matrix phase containing silicon dioxide and carbon, which suppresses the formation of lithium oxide during initial charging.

Benefits of technology

The composite active material enhances initial coulombic efficiency and capacity retention rate by preventing irreversible reactions, maintaining high performance over multiple cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586255000001
    Figure 0007586255000001
  • Figure 0007586255000002
    Figure 0007586255000002
  • Figure 0007586255000003
    Figure 0007586255000003
Patent Text Reader

Abstract

To provide a composite active material for secondary batteries, in which the initial coulomb efficiency and capacitance maintaining rate of a negative electrode active material is improved, and provide a secondary battery using the composite active material for secondary batteries.SOLUTION: A composite active material for secondary batteries according to the present invention, includes: silicon particles with a mean diameter of 150 nm or less; a matrix phase in which the silicon particles are dispersed; and at least one metal silicate compound selected from the group of Li, K, Na, Ca, Mg, and Al, where the silicate compound is present near the front surfaces of the silicon particles. The silicate concentration near the front surfaces of the silicon particles is preferably a concentration higher than that in the matrix phase. Also preferably, silicon dioxide is also present near the front surfaces of the silicon particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite active material for a secondary battery and a secondary battery, and more particularly to a composite active material for a secondary battery and a secondary battery comprising the composite active material for a secondary battery in a negative electrode. [Background technology]

[0002] Non-aqueous electrolyte secondary batteries are used in portable devices, hybrid and electric vehicles, home storage batteries, etc., and are required to have a good balance of multiple properties such as electric capacity, safety, operational stability, etc. As such secondary batteries, various types of lithium ion batteries have been developed and put to practical use, mainly using lithium intercalation compounds as negative electrode active materials that can absorb and release lithium ions between layers between crystal planes during charging and discharging. Furthermore, in recent years, with the miniaturization of various electronic and communication devices and the rapid spread of hybrid vehicles, there is a strong demand for the development of lithium-ion batteries with higher capacity and improved battery characteristics, such as cycle characteristics and discharge rate characteristics, to serve as the driving power source for these devices.

[0003] However, conventional lithium-ion batteries mainly use graphite as the negative electrode active material, and the theoretical specific capacity of graphite-based negative electrode materials places a limit on the development of lithium-ion batteries with higher energy density. Therefore, the development of negative electrode materials using metals such as silicon and tin, which have high theoretical capacity and can absorb and release lithium ions, or alloys with other elements, is being considered. Among these, silicon and silicon-containing active materials, which have a theoretical capacity 10 times higher than that of graphite-based negative electrode materials, have attracted attention. However, silicon-containing active materials are known to have low initial efficiency.

[0004] In order to improve the initial efficiency of the silicon-containing active material, a negative electrode active material containing a Li compound and a silicon-containing active material has been investigated. For example, Patent Document 1 describes a method of doping lithium-doped layered silicon by contacting layered polysilane with a lithium complex solution in which metallic lithium and a polycyclic aromatic compound are dissolved in an organic solvent, and doping the layered polysilane with lithium.

[0005] As silicon oxide doped with Mg, a metal other than Li, Patent Document 2 discloses an anode active material containing silicon particles with a crystal size of 1 to 25 nm and MgSiO3 crystals in silicon oxide, and a silicon compound containing a carbon coating on the surface. Patent Document 3 describes an anode active material having a silicon oxide complex containing silicon oxide and magnesium silicate, and a carbon coating layer containing a carbon-based material located on the surface of the silicon oxide complex. Furthermore, as a silicate compound containing both Li and Mg, Patent Document 4 also considers a negative electrode active material in which silicon compound particles contain a Li compound, a salt of polyacrylic acid or a salt of carboxymethyl cellulose, and a metal salt containing at least one metal selected from Mg and Al. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-202914 A [Patent Document 2] JP 2018-156922 A [Patent Document 3] Special Publication No. 2020-529709 [Patent Document 4] JP 2018-60771 A Summary of the Invention [Problem to be solved by the invention]

[0007] When a silicon-containing active material is used as a negative electrode active material, lithium reacts with silicon oxide present in the silicon-containing active material during initial charging to produce lithium oxide. The lithium oxide produced cannot be reversibly returned to the positive electrode during discharge. It is believed that this irreversible reaction results in the loss of lithium, resulting in a decrease in the initial charge / discharge efficiency. The methods described in the above-mentioned documents 1 to 4 aim to suppress the reaction between lithium and silicon oxide in the initial stage by incorporating Li or Mg into silicon oxide present in the silicon-containing active material, thereby suppressing the decrease in the initial charge-discharge efficiency.

[0008] However, in the negative electrode active materials of the above-mentioned documents 1 to 4, it is believed that a metal silicate compound of Li and / or Mg is dispersed throughout the silicon-containing active material, which is still insufficient for suppressing the reaction between lithium and silicon oxide at the initial stage. Furthermore, since Li and Mg silicates generally have strong water absorption properties, aggregation of the negative electrode active material is likely to occur during preparation of the aqueous slurry for forming the negative electrode film. As a result, the lithium secondary batteries using the negative electrode active materials of Patent Documents 1 to 4 were insufficient in improving the initial coulombic efficiency and capacity retention rate.

[0009] The present inventors have investigated methods for efficiently suppressing the production of lithium oxide during initial charging and discharging, and as a result have discovered a composite active material for secondary batteries that improves the initial Coulombic efficiency and capacity retention rate of the negative electrode active material. That is, the present invention relates to a composite active material for secondary batteries used in lithium ion secondary batteries and a secondary battery containing the composite active material for secondary batteries as a negative electrode active material, and aims to provide a negative electrode active material for secondary batteries that provides a secondary battery excellent in initial coulombic efficiency and capacity retention rate. [Means for solving the problem]

[0010] The present invention has the following aspects. [1] A composite active material for a secondary battery having silicon particles with an average particle diameter of 150 nm or less, a matrix phase in which the silicon particles are dispersed, and a silicate compound of at least one metal selected from the group consisting of Li, K, Na, Ca, Mg, and Al, and having the silicate compound near the surface of the silicon particles. [2] The composite active material for a secondary battery according to [1] above, wherein the silicate concentration near the surface of the silicon particles is higher than the silicate concentration in the matrix phase. [3] The composite active material for a secondary battery according to [1] or [2] above, further having silicon dioxide near the surface of the silicon particles. [4] The composite active material for a secondary battery according to [3] above, wherein the molar ratio of the silicon dioxide is 0.9 or less with the total molar number of the silicate compound and the silicon dioxide being 1. [5] The composite active material for a secondary battery according to any one of [1] to [4] above, wherein the silicate compound is a magnesium silicate compound. [6] The composite active material for a secondary battery according to [5] above, which is a crystalline film having a thickness of 0.2 nm to 10 nm of the magnesium silicate compound near the surface of the silicon particles. [7] The composite active material for a secondary battery according to any one of [1] to [6] above, wherein the matrix phase contains at least a compound represented by SiOxCyNz (where 1 < x < 2, 1 < y < 20, 0 < z < 0.5). [8] The composite active material for a secondary battery according to any one of [1] to [7] above, wherein the silicon particles are flaky crystals and the crystallite size obtained from the peak at 2θ of 28.4° in the X-ray diffraction spectrum is 25 nm or less. [9] With an average particle diameter of 1 μm to 15 μm and a specific surface area of 1 m 2 / g to 30 m 2 / g, the composite active material for a secondary battery according to any one of [1] to [8] above.

[0011] The present invention also has the following aspects.

[10] A secondary battery including the composite active material for a secondary battery according to any one of [1] to [9] above in a negative electrode. Effect of the Invention

[0012] According to the present invention, there is provided a negative electrode active material for a secondary battery which provides a secondary battery excellent in initial coulombic efficiency and capacity retention rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The composite active material for secondary batteries of the present invention (hereinafter also referred to as "the present active material") has silicon particles (hereinafter also referred to as "the present silicon particles") having an average particle size of 150 nm or less, a matrix phase in which the silicon particles are dispersed, and a silicate compound of at least one metal selected from the group consisting of Li, K, Na, Ca, Mg and Al, and has the silicate compound in the vicinity of the surface of the silicon particles. It is believed that a silicon oxide film exists on the surface of silicon particles, and that the generation of lithium oxide due to the reaction between lithium and silicon oxide during initial charging occurs in the vicinity of the silicon oxide. It is believed that the present active material can efficiently suppress the generation of lithium oxide by having a large amount of silicate compound of at least one metal selected from the group consisting of Li, K, Na, Ca, Mg, and Al present in the vicinity of the surface of the silicon particles. As a result, when the present active material is used as a negative electrode active material, it is believed that the initial coulombic efficiency and capacity retention rate of the negative electrode active material are improved.

[0014] The silicon particles are composed of zero-valent silicon and have an average particle size of 150 nm or less. Here, the average particle size is the value of D50, which can be measured using a laser diffraction particle size analyzer or the like. D50 can be measured by dynamic light scattering using a laser particle size analyzer or the like. The average particle size of the present silicon particles is the particle size at which the cumulative volume distribution curve is 50% when drawn from the small diameter side in the particle size distribution.

[0015] Silicon particles with a size of over 300 nm become large lumps, and when this active material is used as a negative electrode active material, they tend to pulverize during charging and discharging, which tends to reduce the capacity retention rate of the negative electrode active material. On the other hand, small silicon particles with a size of less than 10 nm are too fine, so the silicon particles tend to aggregate with each other. This may reduce the dispersibility of the silicon particles in the negative electrode active material. In addition, if the silicon particles are too fine, their surface activity energy increases, and there is a tendency for by-products to increase on the surface of the silicon particles during high-temperature sintering of the negative electrode active material. These may lead to a decrease in charge and discharge performance. Therefore, it is preferable that the content of large silicon particles exceeding 300 nm and small silicon particles less than 10 nm in the present silicon particles is as small as possible. From the above viewpoints, the average particle size is preferably 120 nm or less, more preferably 100 nm or less, and is preferably 20 nm or more, more preferably 30 nm or more.

[0016] The present silicon particles can be prepared, for example, by pulverizing a silicon lump into particles having an average particle size within the above range. Examples of the pulverizer used to pulverize the silicon lumps include pulverizers such as a ball mill, a bead mill, a jet mill, etc. The pulverization may be wet pulverization using an organic solvent, and as the organic solvent, for example, alcohols, ketones, etc. can be suitably used, but aromatic hydrocarbon solvents such as toluene, xylene, naphthalene, and methylnaphthalene can also be used. The obtained silicon particles can be classified or the like by controlling the bead mill conditions such as bead particle size, blending ratio, rotation speed or grinding time, thereby making it possible to adjust the average particle size of the silicon particles to the above range.

[0017] The shape of the silicon particles may be any of granular, needle-like, and flake-like as long as it satisfies the above-mentioned average particle size, but flake-like is preferable from the viewpoint of handling.When the silicon particles are flake-like, it is preferable from the viewpoint of initial coulombic efficiency and capacity retention rate that the crystallite size obtained from the peak half-width at 28.4° of 2θ in X-ray diffraction spectrum is 35 nm or less.The crystallite size is more preferably 25 nm or less.

[0018] From the viewpoint of charge / discharge performance when used as a negative electrode active material, the silicon particles preferably have a length in the long axis direction of 70 to 300 nm and a thickness of 15 to 70 nm. From the viewpoint of charge / discharge performance when used as a negative electrode active material, the aspect ratio, which is the ratio of thickness to length, is preferably 0.5 or less. The morphology of the silicon particles can be measured by the average particle size using a dynamic light scattering method, but the sample with the above aspect ratio can be identified more easily and precisely by using an analytical means such as a transmission electron microscope (TEM) or a field emission scanning electron microscope (FE-SEM). In the case of a negative electrode active material containing the secondary battery material of the present invention, the sample can be cut with a focused ion beam (FIB) and the cross section can be observed with FE-SEM, or the sample can be sliced ​​and the state of the silicon particles can be identified by TEM observation. The aspect ratio of the silicon particles is a calculation result based on 50 particles in the main part of the sample within the field of view of the TEM image.

[0019] The silicon particles are dispersed in the matrix phase. Compounds constituting the matrix phase include silicon dioxide and titanium oxide, but compounds containing silicon, oxygen, and carbon are preferred, and compounds containing silicon, oxygen, and carbon are preferred that have a three-dimensional network structure of a silicon-oxygen-carbon skeleton and a structure containing free carbon. Here, free carbon refers to carbon that is not included in the three-dimensional skeleton of silicon-oxygen-carbon. Free carbon includes carbon that exists as a carbon phase, carbon that is bonded to carbon in the carbon phase, and carbon that is bonded to the silicon-oxygen-carbon skeleton and the carbon phase.

[0020] When the compound constituting the matrix phase is a compound containing silicon, oxygen, and carbon, and has a three-dimensional network structure of a silicon-oxygen-carbon skeleton and a structure containing free carbon, the silicon-oxygen-carbon skeleton in the matrix phase has high chemical stability, and the composite structure with the free carbon reduces the electronic transition resistance and facilitates the diffusion of lithium ions. The silicon particles are tightly wrapped in a composite structure of a silicon-oxygen-carbon skeleton and free carbon, preventing direct contact between the silicon particles and the electrolyte. As a result, when the active material is used as a negative electrode, the silicon particles in the negative electrode play a role as a main component for expressing the charge / discharge performance, while chemical reactions between silicon and the electrolyte during charge / discharge are avoided, thereby preventing performance degradation of the silicon particles to the maximum extent possible.

[0021] When the compound that constitutes the matrix phase has a three-dimensional network structure of silicon-oxygen-carbon skeleton and a structure containing free carbon, the electron distribution inside the silicon-oxygen-carbon skeleton changes when lithium ions approach, and electrostatic bonds and coordinate bonds are formed between the silicon-oxygen-carbon skeleton and the lithium ions. Lithium ions are stored in the silicon-oxygen-carbon skeleton through these electrostatic bonds and coordinate bonds. On the other hand, because the coordinate bond energy is relatively low, the lithium ion desorption reaction occurs easily. In other words, it is thought that the silicon-oxygen-carbon skeleton can reversibly cause lithium ion insertion and desorption reactions during charging and discharging.

[0022] When the compound constituting the matrix phase is a compound containing silicon, oxygen, and carbon, the matrix phase preferably contains a compound represented by the following formula (1). SiOxCy (1) In formula (1), x represents the molar ratio of oxygen to silicon, and y represents the molar ratio of carbon to silicon. When the present active material is used in a secondary battery, from the viewpoint of obtaining an advantageous balance between charge / discharge performance and capacity retention rate, 1≦x<2 is preferable, 1≦x≦1.9 is more preferable, and 1≦x≦1.8 is even more preferable. In addition, when this active material is used in a secondary battery, from the viewpoint of the balance between charge-discharge performance and initial Coulomb efficiency, 1 ≦ y ≦ 20 is preferable, and 1.2 ≦ y ≦ 15 is more preferable.

[0023] The compound constituting the matrix phase may contain nitrogen in addition to silicon, oxygen, and carbon. In the method for producing this active material described below, nitrogen can be introduced into the matrix phase because raw materials used, such as phenolic resin, dispersant, polysiloxane compound, other nitrogen compounds, and nitrogen gas used in the firing process, have atomic groups containing nitrogen as functional groups in their molecules. When the matrix phase contains nitrogen, the charge-discharge performance and capacity retention rate tend to be excellent when this active material is used as a negative electrode active material. When the compound constituting the matrix phase is a compound containing silicon, oxygen, carbon, and nitrogen, the matrix phase preferably contains a compound represented by the following formula (2). SiOxCyNz (2) In formula (2), x and y have the same meanings as described above, and z represents the molar ratio of nitrogen to silicon. When the matrix phase contains the compound represented by the formula (2), from the viewpoints of charge-discharge performance and capacity retention rate when this active material is used in a secondary battery, 1 ≦ x ≦ 2, 1 ≦ y ≦ 20, 0 < z ≦ 0.5 are preferable, and 1 ≦ x ≦ 1.9, 1.2 ≦ y ≦ 15, 0 < z ≦ 0.4 are more preferable.

[0024] The above x, y, and z can be obtained by measuring the mass content of each element and then converting it to a molar ratio (atomic ratio). At this time, the content of oxygen and carbon can be quantified by using an inorganic element analyzer, and the content of silicon can be quantified by using an ICP emission spectrometer (ICP-OES). In addition, although the measurement of x, y, and z is preferably carried out by the method described above, it is also possible to perform a local analysis of this active material, obtain a large number of measurement points of the content ratio data obtained thereby, and estimate the content ratio of the entire active material. Examples of local analysis include energy-dispersive X-ray spectroscopy (SEM-EDX) and electron probe microanalyzer (EPMA).

[0025] In addition to the silicon particles and the matrix phase, the active material has a silicate compound of at least one metal selected from the group consisting of Li, K, Na, Ca, Mg and Al (hereinafter also referred to as "the silicate compound") near the surface of the silicon particles. A silicate compound is generally a compound containing an anion having a structure in which one or more silicon atoms are at the center and electronegative ligands surround the silicon atom, and the present silicate compound is a salt of at least one metal selected from the group consisting of Li, K, Na, Ca, Mg, and Al and a compound containing the above anion. The compound containing the anion is orthosilicate ion (SiO4 4- ), metasilicate ion (SiO3 2- ), pyrosilicate ion (SiO7 6- ), cyclic silicate ion (Si3O9 6- or SiO 18 12- ) and other silicate ions are known. The silicate compound is preferably a silicate compound which is a salt of metasilicate ion and at least one metal selected from the group consisting of Li, K, Na, Ca, Mg, and Al. Among the metals, Li or Mg is preferred. The silicate compound has at least one metal selected from the group consisting of Li, K, Na, Ca, Mg and Al, and may have two or more of these metals. When it has two or more metals, one silicate ion may have multiple metals, or it may be a mixture of silicate compounds having different metals. In addition, the silicate compound may have other metals as long as it has at least one metal selected from the group consisting of Li, K, Na, Ca, Mg and Al. The silicate compound is preferably a lithium silicate compound or a magnesium silicate compound, more preferably lithium metasilicate (Li2SiO3) or magnesium metasilicate (MgSiO3), and particularly preferably magnesium metasilicate (MgSiO3).

[0026] The present active material has the present silicate compound in the vicinity of the surface of the present silicon particle. That is, the present silicate compound may be directly chemically or physically attached to the surface of the present silicon particle, and the present silicate compound may be present in the vicinity of the surface of the present silicon particle. Note that the vicinity of the surface of the present silicon particle is, for example, within 10 nm, preferably within 5 nm from the surface. From the viewpoint of efficiently suppressing the generation of lithium oxide, it is preferable that the silicate compound be present in large amounts near the surface of the silicon particles, and it is more preferable that 50 mass% or more of the total mass of the silicate compound contained in the active material be present near the surface, and it is even more preferable that 60 mass% or more be present near the surface. The presence of this silicate compound near the surface of this silicon particle can be confirmed by a high-resolution transmission electron microscope (hereinafter, also referred to as "HR-TEM"). In detail, the sample can be sliced ​​using a focused ion beam (FIB) and confirmed by HR-TEM observation.

[0027] In addition, the concentration (silicate concentration) of the silicate compound in the vicinity of the surface of the silicon particle is preferably higher than the concentration (silicate concentration) of the compound constituting the matrix phase. The vicinity of the surface is as described above, and the concentration (silicate concentration) of the silicate compound in the vicinity of the surface of the silicon particle is the concentration of the silicate compound in the above range. For example, the concentration (silicate concentration) of the silicate compound in the vicinity of the surface is the mass per unit volume of the silicate compound in the above range.

[0028] When the silicate compound is in a crystalline state, the lattice structure of the crystallites of the silicate compound is observed in the HR-TEM measurement. Therefore, the concentration of the silicate compound in the vicinity of the surface of the silicon particle is the ratio of the area of ​​the lattice structure attributed to the crystallites of the silicate compound per unit area to the area of ​​the entire field of view in a 1,000,000 times magnification of the HR-TEM, and is calculated by the following formula: Area ratio = area of ​​lattice structure attributed to crystallites / area of ​​total field of view This area ratio is calculated using the average value of five or more different fields of view. In addition, by using STEM-EDS (Scanning Transmission Electron Microscope Energy-Dispersive-Spectroscopy), the concentrations of Mg, Si, and O elements present near silicon particles can be detected in a mapping image. The concentration of silicate compounds can be determined by combining the Mg, Si, and O elements.

[0029] The concentration (silicate concentration) of the silicate compound near the surface is preferably twice, and more preferably three times, the concentration (silicate concentration) of the compound constituting the matrix phase, and it is even more preferable that the silicon particles are coated with the silicate compound. Furthermore, when the concentrations of the silicate compound and the compound constituting the matrix phase are compared within the area near the surface of the silicon particle using HR-TEM, the area of ​​the lattice structure of the silicate compound crystallites near the surface of the silicate compound is preferably at least twice, and more preferably at least three times, the area of ​​the crystal lattice structure of the compound constituting the matrix phase per unit area of ​​the observation field. When the silicate compound is a magnesium silicate compound, it is preferable that the magnesium silicate compound is a crystalline film and covers at least a part of the surface of the silicon particles. When the magnesium silicate compound covers at least a part of the surface of the silicon particles, the coverage is more preferably 50% or more, particularly preferably 80% or more. When the magnesium silicate compound covers at least a part of the silicon particles, the thickness of the crystalline film is preferably 0.2 nm to 10 nm, more preferably 1 nm to 8 nm. The coverage and the thickness of the crystalline film can be measured by the HR-TEM. The coverage can be determined from the ratio of the amount of silicon particles to the amount of the magnesium silicate compound.

[0030] It is preferable that the present active material contains silicon dioxide in the vicinity of the surface of the present silicon particle in addition to the present silicate compound, from the viewpoint of achieving an excellent balance between the initial coulombic efficiency and the capacity retention rate. When the active material has silicon dioxide, the silicate compound and silicon dioxide are present near the surface of the silicon particles. The molar ratio of the silicate compound to silicon dioxide is preferably 0.9 or less, more preferably 0.5 or less, when the total molar number of the silicate compound and silicon dioxide is 1. The molar ratio of the silicate compound to silicon dioxide is preferably 0.05 or more, more preferably 0.1 or more, when the total molar number of the silicate compound and silicon dioxide is 1.

[0031] When the active material has silicon dioxide, the surface of the silicon particles is preferably coated with a silicon dioxide film, which is an oxide film of silicon.When the surface of the silicon particles is coated with a silicon dioxide film, the silicate compound is preferably present on the surface of the silicon dioxide film.When the silicate compound is a crystalline film of a magnesium silicate compound, the silicon dioxide film that coats the silicon particles is preferably further coated with a crystalline film of a magnesium silicate compound.

[0032] The average particle size of the present active material having the present silicon particles, the matrix phase, and the present silicate compound in the vicinity of the surface of the present silicon particles is preferably 1 μm to 15 μm, more preferably 2 μm to 8 μm. The average particle size is the D50 value as above, and is measured by the same method as above. If the average particle size is too small, the specific surface area increases significantly, and when the active material is used in a secondary battery, the amount of solid-phase interface electrolyte decomposition product (hereinafter, also referred to as "SEI") generated during charging and discharging increases, which may reduce the reversible charge / discharge capacity per unit volume. If the average particle size is too large, there is a risk of the active material peeling off from the current collector during electrode film production.

[0033] The specific surface area of ​​this active material is 1m 2 / g to 30m 2 / g is preferred, and 2m 2 / g to 15m 2 / g is more preferable. When the specific surface area is within the above range, the amount of solvent absorbed during electrode preparation can be appropriately maintained, and the amount of binder used to maintain binding properties can also be appropriately maintained. The specific surface area is a value determined by the BET method, and can be determined by nitrogen gas adsorption measurement, for example, using a specific surface area measurement device.

[0034] The average particle size of this active material is 1 to 15 μm, and the specific surface area is 1 m 2 / g to 30m 2 The average particle size of the active material is preferably 2 μm to 8 μm and the specific surface area is preferably 2 m 2 / g to 15m 2 / g is particularly preferred.

[0035] The active material may contain other necessary third components in addition to those mentioned above. The surface of the active material may be coated with a coating material, which is preferably a material that is expected to have electronic conductivity, lithium ion conductivity, and the effect of inhibiting decomposition of the electrolyte.

[0036] When the surface of the active material is coated with the coating material, the average thickness of the coating layer is preferably 10 nm or more and 300 nm or less. The average thickness is more preferably 20 nm or more and 200 nm or less. When the active material has a coating layer of the average thickness, the silicon particles exposed on the surface of the active material can be protected, and when the active material is used as a negative electrode active material, the chemical stability and thermal stability of the negative electrode active material are improved. As a result, the deterioration of the charge and discharge performance of the secondary battery can be further suppressed. In addition, when the surface of the present active material is coated with the coating material, the content of the coating material is preferably 1 to 30 mass%, more preferably 3 to 25 mass%, based on the total amount of the present active material being 100 mass%, from the viewpoint of improving the chemical stability and thermal stability of the negative electrode active material. The total amount of the present active material is the total amount of the present silicon particles, the matrix phase, the present silicate compound, and the coating material that constitute the present active material. When the matrix phase contains nitrogen, the total amount includes nitrogen.

[0037] The coating material includes electron conductive materials such as carbon, titanium, nickel, etc. Among these, from the viewpoint of improving the chemical stability and thermal stability of the negative electrode active material, carbon is preferred, and low crystalline carbon is more preferred. When the coating material is low-crystalline carbon, the average thickness of the coating layer is preferably 10 nm to 300 nm, or the content of low-crystalline carbon is preferably 1 to 30 mass % relative to 100 mass % of the total amount of the active material.

[0038] Since the present active material is excellent in charge / discharge capacity, initial efficiency, and capacity retention rate, a secondary battery using the present active material as a battery negative electrode exhibits good charge / discharge characteristics. Specifically, a slurry containing the active material, an organic binder, and other components such as a conductive assistant, if necessary, can be applied to a copper foil collector in the form of a thin film to form a negative electrode. A carbon material such as graphite can also be added to the slurry to form a negative electrode. Examples of the carbon material include natural graphite, artificial graphite, and amorphous carbon such as hard carbon or soft carbon.

[0039] For example, the present active material and a binder, which is an organic binding material, are kneaded together with a solvent using a dispersing device such as a stirrer, a ball mill, a super sand mill, or a pressure kneader to prepare a negative electrode material slurry, which is then applied to a current collector to form a negative electrode layer. Alternatively, the negative electrode material can be obtained by forming a paste-like negative electrode material slurry into a sheet, pellet, or other shape and integrating it with a current collector.

[0040] Examples of the organic binder include styrene-butadiene rubber copolymers (hereinafter also referred to as "SBR"); ethylenically unsaturated carboxylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, (meth)acrylonitrile, and hydroxyethyl (meth)acrylate, and unsaturated carboxylic acid copolymers such as (meth)acrylic copolymers composed of ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, fumaric acid, and maleic acid; and polymer compounds such as polyvinylidene fluoride, polyethylene oxide, polyepichlorohydrin, polyphosphazene, polyacrylonitrile, polyimide, polyamideimide, and carboxymethylcellulose (hereinafter also referred to as "CMC").

[0041] Depending on their physical properties, these organic binders may be dispersed or dissolved in water, or dissolved in an organic solvent such as N-methyl-2-pyrrolidone (NMP), etc. The content of the organic binder in the negative electrode layer of the lithium ion secondary battery negative electrode is preferably 1 mass % to 30 mass %, more preferably 2 mass % to 20 mass %, and even more preferably 3 mass % to 15 mass %.

[0042] When the content of the organic binder is 1% by mass or more, the adhesion is better and the destruction of the negative electrode structure due to the expansion or contraction during charging and discharging is more suppressed, whereas when the content is 30% by mass or less, the increase in the electrode resistance is more suppressed. Within this range, the present active material has high chemical stability and can employ an aqueous binder, making it easy to handle in practical applications.

[0043] In addition, the negative electrode material slurry may be mixed with a conductive assistant as necessary. Examples of the conductive assistant include carbon black, graphite, acetylene black, and oxides and nitrides that exhibit conductivity. The amount of the conductive assistant used may be about 1% by mass to 15% by mass with respect to the negative electrode active material of the present invention.

[0044] The material and shape of the current collector may be, for example, a strip of copper, nickel, titanium, stainless steel, etc. in the form of foil, perforated foil, mesh, etc. Also, porous materials such as porous metal (foamed metal) and carbon paper can be used.

[0045] Examples of the method for applying the negative electrode material slurry to the current collector include metal mask printing, electrostatic coating, dip coating, spray coating, roll coating, doctor blade, gravure coating, screen printing, etc. After application, it is preferable to perform a rolling treatment using a flat plate press, a calendar roll, etc., as necessary.

[0046] The negative electrode material slurry may be formed into a sheet or pellet shape, and this may be integrated with the current collector by, for example, rolling, pressing, or a combination of these.

[0047] The negative electrode layer formed on the current collector or the negative electrode layer integrated with the current collector is preferably heat-treated according to the organic binder used. For example, when a water-based styrene-butadiene rubber copolymer (SBR) is used, the heat treatment may be performed at 100 to 130°C, and when an organic binder having a polyimide or polyamideimide as the main skeleton is used, the heat treatment is preferably performed at 150 to 450°C.

[0048] This heat treatment removes the solvent, hardens the binder, and increases the strength, improving the adhesion between the particles and between the particles and the current collector. It is preferable to carry out these heat treatments in an inert atmosphere such as helium, argon, or nitrogen, or in a vacuum atmosphere, in order to prevent oxidation of the current collector during the treatment.

[0049] In addition, it is preferable to subject the negative electrode to pressure treatment after the heat treatment. In the negative electrode using this active material, the electrode density is 1 g / cm 3 from 1.8 g / cm 3 and preferably 1.1 g / cm 3 to 1.7 g / cm 3More preferably, it is 1.2 g / cm 3 from 1.6 g / cm 3 It is more preferable that the electrode density is higher. The higher the electrode density, the more the adhesion and the volumetric capacity density of the electrode tend to improve. On the other hand, if the electrode density is too high, the voids in the electrode are reduced, which weakens the effect of suppressing the volumetric expansion of silicon and the like, and the capacity retention rate may decrease. Therefore, the optimal range of the electrode density is selected.

[0050] The secondary battery of the present invention contains the present active material in the negative electrode. As the secondary battery having a negative electrode containing the present active material, non-aqueous electrolyte secondary batteries and solid electrolyte secondary batteries are preferable, and the present active material exerts excellent performance particularly when used as the negative electrode of a non-aqueous electrolyte secondary battery.

[0051] When the secondary battery of the present invention is used as a wet electrolyte secondary battery, for example, the secondary battery of the present invention can be constructed by disposing a positive electrode and a negative electrode containing the negative electrode active material of the present invention opposite each other via a separator and injecting an electrolyte solution.

[0052] The positive electrode can be obtained by forming a positive electrode layer on the surface of a current collector in the same manner as the negative electrode. In this case, the current collector can be a strip of a metal or alloy such as aluminum, titanium, or stainless steel in the form of a foil, a perforated foil, a mesh, or the like.

[0053] There are no particular limitations on the positive electrode material used in the positive electrode layer. When preparing a lithium ion secondary battery among non-aqueous electrolyte secondary batteries, for example, a metal compound, metal oxide, metal sulfide, or conductive polymer material capable of doping or intercalating lithium ions may be used. For example, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2), and composite oxides thereof (LiCoxNiyMnzO2, x+y+z=1), lithium manganese spinel (LiMn2O4), lithium vanadium compounds, V2O5, V6O 13, VO2, MnO2, TiO2, MoV2O8, TiS2, V2S5, VS2, MoS2, MoS3, Cr3O8, Cr2O5, olivine-type LiMPO4 (wherein M is Co, Ni, Mn, or Fe), conductive polymers such as polyacetylene, polyaniline, polypyrrole, polythiophene, polyacene, porous carbon, etc. can be used alone or in combination.

[0054] As the separator, for example, a nonwoven fabric, cloth, microporous film, or a combination thereof, mainly composed of polyolefin such as polyethylene or polypropylene can be used. Note that if the positive electrode and the negative electrode of the nonaqueous electrolyte secondary battery to be produced are not in direct contact with each other, there is no need to use a separator.

[0055] As the electrolyte, for example, a so-called organic electrolyte can be used in which a lithium salt such as LiClO4, LiPF6, LiAsF6, LiBF4, or LiSO3CF3 is dissolved in a non-aqueous solvent such as ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, cyclopentanone, sulfolane, 3-methylsulfolane, 2,4-dimethylsulfolane, 3-methyl-1,3-oxazolidin-2-one, γ-butyrolactone, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, butyl methyl carbonate, ethyl propyl carbonate, butyl ethyl carbonate, dipropyl carbonate, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, methyl acetate, or ethyl acetate, or a mixture of two or more components.

[0056] The structure of the secondary battery of the present invention is not particularly limited, but usually, the positive electrode, the negative electrode, and a separator provided as necessary are wound into a flat spiral shape to form a wound electrode plate group, or these are stacked in a flat plate shape to form a stacked electrode plate group, and these electrode plate groups are sealed in an exterior body. Note that the half cells used in the examples of the present invention are configured so that the negative electrode is mainly made of the present active material, and a simple evaluation is performed using metallic lithium as the counter electrode, in order to more clearly compare the cycle characteristics of the active material itself.

[0057] The secondary battery using the present active material is not particularly limited, but is used as a paper type battery, a button type battery, a coin type battery, a laminated type battery, a cylindrical type battery, a square type battery, etc. The above-mentioned negative electrode active material of the present invention can also be applied to electrochemical devices in general that use the insertion and desorption of lithium ions as a charge / discharge mechanism, such as hybrid capacitors and solid lithium secondary batteries.

[0058] The present active material can be produced, for example, by a method including the following steps 1 to 4. Note that the following steps illustrate a method in which a polysiloxane compound and a carbon source resin are used as the silicon-containing compound that forms the matrix phase, but the method is not limited to these steps. Step 1: A slurry of wet-milled silicon (zero valence) is mixed with an aggregate containing a polysiloxane compound and a carbon source resin to obtain a suspension. Step 2: A salt of at least one metal selected from the group consisting of Li, K, Na, Ca, Mg and Al is added to the obtained suspension, mixed, and then the solvent is removed to obtain a precursor. Step 3: The precursor obtained in step 2 is calcined in an inert atmosphere at a maximum temperature within the range of 1000° C. to 1180° C. to obtain a calcined product. Step 4: The fired product obtained in step 3 is pulverized to obtain the active material.

[0059] Each step will be described below. <Process 1> (Silicon (0 valence) slurry) The wet-milled silicon (0-valent) slurry used in step 1 can be prepared by using an organic solvent and pulverizing silicon particles in a wet powder pulverizer. A dispersant may be used to promote pulverization of silicon particles in the organic solvent. The wet pulverizer is not particularly limited, and examples thereof include a roller mill, a high-speed rotary pulverizer, a container-driven mill, and a bead mill. In wet grinding, it is preferable to grind the silicon particles until they reach the particle size of the present silicon particles.

[0060] The organic solvent used in the wet method is an organic solvent that does not chemically react with silicon, such as ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and diisobutyl ketone; alcohols such as ethanol, methanol, normal propyl alcohol, and isopropyl alcohol; and aromatics such as benzene, toluene, and xylene.

[0061] The type of dispersant includes aqueous and non-aqueous dispersants. In order to suppress excessive oxidation on the surface of the silicon particles, it is preferable to use a non-aqueous dispersant. The type of non-aqueous dispersant includes polymer types such as polyethers, polyalkylene polyamines, and polycarboxylic acid partial alkyl esters, low molecular types such as polyhydric alcohol esters and alkyl polyamines, and inorganic types such as polyphosphates. The concentration of silicon in the silicon (0-valent) slurry is not particularly limited, but when the solvent and, if necessary, a dispersant are included, the total amount of the dispersant and silicon is 100 mass%, and the amount of silicon is preferably in the range of 5 mass% to 40 mass%, more preferably 10 mass% to 30 mass%.

[0062] (Polysiloxane compound) The polysiloxane compound used in step 1 is a resin containing at least one of a polycarbosilane structure, a polysilazane structure, a polysilane structure, and a polysiloxane structure. It may be a resin containing only these structures, or a composite resin having at least one of these structures as a segment and chemically bonded to another polymer segment. The form of the composite may be graft copolymerization, block copolymerization, random copolymerization, alternating copolymerization, etc. For example, there is a composite resin having a graft structure in which a polysiloxane segment is chemically bonded to the side chain of a polymer segment, and a composite resin having a block structure in which a polysiloxane segment is chemically bonded to the end of a polymer segment.

[0063] The polysiloxane segment preferably has a structural unit represented by the following general formula (S-1) and / or the following general formula (S-2): In particular, the polysiloxane compound more preferably has a carboxy group, an epoxy group, an amino group, or a polyether group on the side chain or terminal of the siloxane bond (Si-O-Si) main skeleton.

[0064] [ka]

[0065] [ka] (In the above general formulas (S-1) and (S-2), R 1 R represents an aromatic hydrocarbon group, an alkyl group, an epoxy group, a carboxy group, or the like, which may have a substituent. 2 and R 3 respectively represent an alkyl group, a cycloalkyl group, an aryl group or an aralkyl group, an epoxy group, a carboxy group, etc.)

[0066] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 1,2-dimethylpropyl group, a 1-ethylpropyl group, a hexyl group, an isohexyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 2,2-dimethylbutyl group, a 1-ethylbutyl group, a 1,1,2-trimethylpropyl group, a 1,2,2-trimethylpropyl group, a 1-ethyl-2-methylpropyl group, a 1-ethyl-1-methylpropyl group, etc. Examples of the cycloalkyl group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, etc.

[0067] Examples of the aryl group include a phenyl group, a naphthyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 4-vinylphenyl group, and a 3-isopropylphenyl group.

[0068] Examples of the aralkyl group include a benzyl group, a diphenylmethyl group, and a naphthylmethyl group.

[0069] Examples of polymer segments other than the polysiloxane segment contained in the polysiloxane compound include vinyl polymer segments such as acrylic polymers, fluoroolefin polymers, vinyl ester polymers, aromatic vinyl polymers, and polyolefin polymers, as well as polymer segments such as polyurethane polymer segments, polyester polymer segments, and polyether polymer segments. Among these, vinyl polymer segments are preferred.

[0070] The polysiloxane compound may be a composite resin in which a polysiloxane segment and a polymer segment are bonded in a structure represented by the following structural formula (S-3), or may have a three-dimensional network polysiloxane structure.

[0071] [ka]

[0072] (In the formula, the carbon atom is a carbon atom constituting a polymer segment, and the two silicon atoms are silicon atoms constituting a polysiloxane segment).

[0073] The polysiloxane segment of the polysiloxane compound may have a functional group capable of reacting by heating, such as a polymerizable double bond, in the polysiloxane segment. By subjecting the polysiloxane compound to heat treatment before thermal decomposition, a crosslinking reaction progresses and the compound is solidified, which makes it easy to carry out the thermal decomposition treatment.

[0074] Examples of the polymerizable double bond include a vinyl group and a (meth)acryloyl group. The number of polymerizable double bonds in the polysiloxane segment is preferably 2 or more, more preferably 3 to 200, and even more preferably 3 to 50. In addition, by using a composite resin having 2 or more polymerizable double bonds as the polysiloxane compound, the crosslinking reaction can be easily promoted.

[0075] The polysiloxane segment may have a silanol group and / or a hydrolyzable silyl group. Examples of the hydrolyzable group in the hydrolyzable silyl group include a halogen atom, an alkoxy group, a substituted alkoxy group, an acyloxy group, a phenoxy group, a mercapto group, an amino group, an amide group, an aminooxy group, an iminoxy group, and an alkenyloxy group. The hydrolyzable silyl group becomes a silanol group by hydrolysis of these groups. In parallel with the thermosetting reaction, a hydrolysis condensation reaction proceeds between the hydroxyl group in the silanol group and the hydrolyzable group in the hydrolyzable silyl group, thereby obtaining a solid polysiloxane compound.

[0076] The silanol group in the present invention is a silicon-containing group having a hydroxyl group directly bonded to a silicon atom. The hydrolyzable silyl group in the present invention is a silicon-containing group having a hydrolyzable group directly bonded to a silicon atom, and specifically includes, for example, a group represented by the following general formula (S-4).

[0077] [ka]

[0078] (In the formula, R 4 R represents a monovalent organic group such as an alkyl group, an aryl group, or an aralkyl group. 5 is a halogen atom, an alkoxy group, an acyloxy group, an allyloxy group, a mercapto group, an amino group, an amido group, an aminooxy group, an iminoxy group, or an alkenyloxy group, and b is an integer of 0 to 2.

[0079] Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, an isopentyl group, a neopentyl group, a tert-pentyl group, a 1-methylbutyl group, a 2-methylbutyl group, a 1,2-dimethylpropyl group, a 1-ethylpropyl group, a hexyl group, an isohexyl group, a 1-methylpentyl group, a 2-methylpentyl group, a 3-methylpentyl group, a 1,1-dimethylbutyl group, a 1,2-dimethylbutyl group, a 2,2-dimethylbutyl group, a 1-ethylbutyl group, a 1,1,2-trimethylpropyl group, a 1,2,2-trimethylpropyl group, a 1-ethyl-2-methylpropyl group, and a 1-ethyl-1-methylpropyl group.

[0080] Examples of the aryl group include a phenyl group, a naphthyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 4-vinylphenyl group, and a 3-isopropylphenyl group.

[0081] Examples of the aralkyl group include a benzyl group, a diphenylmethyl group, and a naphthylmethyl group.

[0082] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0083] Examples of the alkoxy group include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, and a tert-butoxy group.

[0084] Examples of the acyloxy group include a formyloxy group, an acetoxy group, a propanoyloxy group, a butanoyloxy group, a pivaloyloxy group, a pentanoyloxy group, a phenylacetoxy group, an acetoacetoxy group, a benzoyloxy group, and a naphthoyloxy group.

[0085] Examples of the allyloxy group include a phenyloxy group and a naphthyloxy group.

[0086] Examples of the alkenyloxy group include a vinyloxy group, an allyloxy group, a 1-propenyloxy group, an isopropenyloxy group, a 2-butenyloxy group, a 3-butenyloxy group, a 2-pentenyloxy group, a 3-methyl-3-butenyloxy group, and a 2-hexenyloxy group.

[0087] Examples of the polysiloxane segment having the structural unit represented by the general formula (S-1) and / or the general formula (S-2) include those having the following structures.

[0088] [ka]

[0089] [ka]

[0090] [ka]

[0091] The polymer segment may have various functional groups as necessary within the scope of not impairing the effects of the present invention. Examples of such functional groups include a carboxyl group, a blocked carboxyl group, a carboxylic anhydride group, a tertiary amino group, a hydroxyl group, a blocked hydroxyl group, a cyclocarbonate group, an epoxy group, a carbonyl group, a primary amide group, a secondary amide group, a carbamate group, and a functional group represented by the following structural formula (S-5).

[0092] [ka]

[0093] The polymer segment may also have a polymerizable double bond such as a vinyl group or a (meth)acryloyl group.

[0094] The polysiloxane compound is preferably produced, for example, by the following methods (1) to (3).

[0095] (1) A method in which a polymer segment containing a silanol group and / or a hydrolyzable silyl group is prepared in advance as a raw material for the polymer segment, and this polymer segment is mixed with a silane compound having both a silanol group and / or a hydrolyzable silyl group and a polymerizable double bond, followed by a hydrolysis and condensation reaction.

[0096] (2) A method in which a polymer segment containing a silanol group and / or a hydrolyzable silyl group is prepared in advance as a raw material for the polymer segment. A polysiloxane is also prepared in advance by subjecting a silane compound having both a silanol group and / or a hydrolyzable silyl group and a polymerizable double bond to a hydrolysis and condensation reaction. The polymer segment and the polysiloxane are then mixed together to carry out a hydrolysis and condensation reaction.

[0097] (3) A method in which the polymer segment, a silane compound having a silanol group and / or a hydrolyzable silyl group, and a polymerizable double bond, and a polysiloxane are mixed together to carry out a hydrolysis and condensation reaction. A polysiloxane compound can be obtained by the above method. Examples of polysiloxane compounds include the Ceranate (registered trademark) series (organic / inorganic hybrid coating resin; manufactured by DIC Corporation) and the Compocelan SQ series (silsesquioxane hybrid; manufactured by Arakawa Chemical Industries, Ltd.).

[0098] (Carbon source resin) The carbon source resin used in the step 1 is preferably a synthetic resin or natural chemical raw material that has good miscibility with polysiloxane compounds, is carbonized by high-temperature baking in an inert atmosphere, and has aromatic functional groups.

[0099] Examples of synthetic resins include thermoplastic resins such as polyvinyl alcohol and polyacrylic acid, and thermosetting resins such as phenol resins and furan resins. Examples of natural chemical raw materials include heavy oils, particularly tar pitches, such as coal tar, light tar oil, medium tar oil, heavy tar oil, naphthalene oil, anthracene oil, coal tar pitch, pitch oil, mesophase pitch, oxygen-crosslinked petroleum pitch, and heavy oil. From the viewpoints of cheap availability and removal of impurities, the use of phenol resins is more preferable.

[0100] In particular, in step 1, the carbon source resin is preferably a resin containing an aromatic hydrocarbon moiety, and the resin containing an aromatic hydrocarbon moiety is preferably a phenolic resin, an epoxy resin, or a thermosetting resin, and the phenolic resin is preferably a resol type. Examples of phenolic resins include SUMILITE resin series (resole type phenolic resins, manufactured by Sumitomo Bakelite Co., Ltd.).

[0101] <Process 2> The salt of at least one metal selected from the group consisting of Li, K, Na, Ca, Mg, and Al (hereinafter referred to as "the metal salt") used in step 2 includes halides such as fluorides, chlorides, and bromides, hydroxides, carbonates, and the like of these metals. The metal salt may be a salt of two or more metals, one salt may have more than one metal, or it may be a mixture of salts having different metals. There is no particular restriction on the amount of the metal salt added when the metal salt is added to the suspension obtained in step 1, but the molar ratio of the amount of the metal salt compound added to the total amount of silicon particles is preferably 0.01 to 0.4. The mixing method includes a method in which the metal salt is dissolved in an organic solvent and added to the suspension and mixed when it is soluble in an organic solvent. When it is insoluble in an organic solvent, the metal salt particles are dispersed in an organic solvent and then added to the suspension and mixed. From the viewpoint of improving the dispersion effect, the metal salt is preferably nanoparticles having an average particle size of 100 nm or less. The organic solvent can be preferably alcohols, ketones, etc., but aromatic hydrocarbon solvents such as toluene, xylene, naphthalene, and methylnaphthalene can also be used.

[0102] (Precursor) The suspension obtained in step 1 is mixed uniformly with the present metal salt, stirred, and then the mixture is desolvated and dried to obtain a precursor of the present active material (hereinafter also referred to as "precursor"). The aggregate containing the polysiloxane compound and the carbon source resin is preferably in a state in which the polysiloxane compound and the carbon source resin are uniformly mixed. The mixing is carried out using a device having the functions of dispersion and mixing. Examples include a stirrer, an ultrasonic mixer, and a premix disperser. In the process of desolvation and drying for the purpose of distilling off the organic solvent, a dryer, a reduced pressure dryer, a spray dryer, and the like can be used.

[0103] The precursor preferably contains 3% by mass to 50% by mass of the present silicon particles which are silicon (0 valence), 15% by mass to 85% by mass of the solid content of the polysiloxane compound, and 3% by mass to 70% by mass of the solid content of the carbon source resin, and more preferably contains 8% by mass to 40% by mass of the present silicon particles, 20% by mass to 70% by mass of the solid content of the polysiloxane compound, and 3% by mass to 60% by mass of the solid content of the carbon source resin.

[0104] By uniformly dispersing the metal salt in the suspension in step 2, the molecules of the metal salt can be brought into sufficient contact with the silicon particles. When silicon oxide is present on the surface or in the vicinity of the silicon particles, the molecules of the metal salt can be brought into sufficient contact with the silicon particles under conditions in which the molecules of the metal salt and the silicon particles undergo a solid-phase reaction, so that the silicate compound can be present near the surface of the silicon particles. In order to make the concentration of the silicate compound near the surface of the silicon particles higher than the concentration of the compound that constitutes the matrix phase, it is important to improve the contact state between the metal salt and the silicon particles. In addition, the molecules of the present metal salt can be attached to the vicinity of the surface of the present silicon particles by surface modification using an organic additive. The molecular structure of the organic additive is not particularly limited, but it is sufficient that it can form a physical or chemical bond with the dispersant present on the surface of the present silicon particles. The physical or chemical bond can be an electrostatic action, a hydrogen bond, an intermolecular van der Waals force, an ionic bond, a covalent bond, or the like. During high-temperature firing, the molecules of the present metal salt undergo a solid-phase reaction with silicon oxide on the surface of the present silicon particles, so that the surface of the present silicon particles can be coated with the present silicate compound.

[0105] <Process 3> In step 3, the precursor obtained in step 2 is baked in an inert atmosphere at a maximum temperature of 900°C to 1200°C to completely decompose the thermally decomposable organic components, and the other main components are baked into a baked product suitable for the present active material by precisely controlling the baking conditions. Specifically, the raw material polysiloxane compound and carbon source resin are converted into a silicon-oxygen-carbon skeleton and free carbon by the energy of the high-temperature treatment.

[0106] The firing is performed according to a firing program that is determined by the heating rate, the holding time at a constant temperature, etc. The maximum temperature is the highest temperature that is set, and it strongly affects the structure and performance of the fired product, which is the composite active material for secondary batteries. In the present invention, by setting the maximum temperature to 900°C to 1200°C, the microstructure of the active material for secondary batteries that retains the chemical bond state of silicon and carbon can be precisely controlled, and oxidation of the silicon particles due to firing at an excessively high temperature can be avoided, thereby obtaining better charge / discharge characteristics.

[0107] The calcination method is not particularly limited, but it is sufficient to use a reaction device having a heating function in an inert atmosphere, and treatment can be performed by a continuous method or a batch method. The calcination device can be appropriately selected from a fluidized bed reaction furnace, a rotary furnace, a vertical moving bed reaction furnace, a tunnel furnace, a batch furnace, a rotary kiln, etc. depending on the purpose.

[0108] <Step 4> Step 4 is a step of obtaining the active material by pulverizing the fired product obtained in step 3 and classifying it as necessary. The pulverization may be performed in one step until the particle size reaches the desired particle size, or may be performed in several steps. For example, when preparing an active material of about 10 μm from a fired product of lumps or aggregates of 10 mm or more, the material is coarsely pulverized with a jaw crusher, roll crusher, etc., and then pulverized into particles of about 1 mm, to about 100 μm with a glow mill, ball mill, etc., and to about 10 μm with a bead mill, jet mill, etc. The particles produced by pulverization may contain coarse particles, and classification is performed to remove them or to remove fine powder and adjust the particle size distribution. The classifier used is a wind classifier, a wet classifier, etc., depending on the purpose, but when removing coarse particles, a classification method that passes through a sieve is preferable because it can reliably achieve the purpose. In addition, if the precursor mixture is controlled to a shape near the target particle size by spray drying or the like before firing, and fired in that shape, it is possible to omit the pulverization step.

[0109] When the silicon particles have silicon dioxide, the surface of the silicon particles can be oxidized to form a silicon dioxide film during the process of removing the solvent and drying in step 2 and during the process of step 3.

[0110] As described above, when the present active material is used as the negative electrode active material of a secondary battery, it gives a secondary battery excellent in initial coulombic efficiency and capacity retention rate. The present active material can be used as a negative electrode by the above-mentioned method to produce a secondary battery having the negative electrode. Although the present active material and the secondary battery containing the present active material in the negative electrode have been described above, the present invention is not limited to the configurations of the above-mentioned embodiments. In the present active material and the secondary battery containing the present active material in the negative electrode, any other configuration may be added to the configuration of the above embodiment, or any other configuration that exerts the same function may be substituted. EXAMPLES

[0111] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. In addition, the half-cell used in the examples of the present invention has a negative electrode mainly made of the silicon-containing active material of the present invention, and a simple evaluation is performed using metallic lithium as the counter electrode, in order to more clearly compare the cycle characteristics of the active material itself.

[0112] Synthesis Example 1: Preparation of silicon particles Zirconia beads with a particle size of 0.1 mm to 0.2 mm and 100 ml of methyl ethyl ketone solvent (MEK) were placed in a 150 ml container of a small bead mill device at a filling rate of 60%. Silicon powder (commercially available) with an average particle size of 5 μm and a cationic dispersant liquid (BYK Japan Co., Ltd.: BYK145) were then placed in the container, and wet milling was performed using a bead mill under the conditions shown in Table 1 to obtain a dark brown liquid silicon slurry with a solid concentration of 30 mass%. The morphology and size of the silicon pulverized product were confirmed by TEM observation, and they were designated Si1, Si2, Si3, Si4, and Si5, as shown in Table 1.

[0113] [Table 1]

[0114] Synthesis Example 2: Preparation of polysiloxane compound (Synthesis of methyltrimethoxysilane condensate (a1)) A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet was charged with 1,421 parts by mass of methyltrimethoxysilane (hereinafter abbreviated as "MTMS") and heated to 60° C. Next, a mixture of 0.17 parts by mass of isopropyl acid phosphate ("Phoslex A-3" manufactured by SC Organic Chemical Co., Ltd.) and 207 parts by mass of deionized water was dropped into the reaction vessel over a period of 5 minutes, and the mixture was stirred at a temperature of 80° C. for 4 hours to carry out a hydrolysis condensation reaction. The condensate obtained by the hydrolysis and condensation reaction was distilled at a temperature of 40 to 60°C and under a reduced pressure of 40 to 1.3 kPa. The phrase "under a reduced pressure of 40 to 1.3 kPa" means that the reduced pressure condition at the start of methanol distillation is 40 kPa, and the pressure is finally reduced to 1.3 kPa. The same applies to the following description. By removing the methanol and water produced during the reaction, 1,000 parts by mass of a liquid containing a condensate (a1) of MTMS having a number average molecular weight of 1,000 to 5,000 was obtained. The active ingredient of the obtained liquid was 70% by mass. The effective component is calculated by dividing the theoretical yield (parts by mass) when all methoxy groups of a silane monomer such as MTMS undergo a condensation reaction by the actual yield (parts by mass) after the condensation reaction, i.e., [theoretical yield (parts by mass) when all methoxy groups of a silane monomer undergo a condensation reaction / actual yield (parts by mass) after the condensation reaction].

[0115] (Production of Curable Resin Composition (1)) A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet was charged with 150 parts by mass of butanol (hereinafter also referred to as "BuOH"), 105 parts by mass of phenyltrimethoxysilane (hereinafter also referred to as "PTMS"), and 277 parts by mass of dimethyldimethoxysilane (hereinafter also referred to as "DMDMS"), and the temperature was raised to 80°C. Next, at the same temperature, a mixture containing 21 parts by mass of methyl methacrylate (hereinafter also referred to as "MMA"), 4 parts by mass of butyl methacrylate (hereinafter also referred to as "BMA"), 3 parts by mass of butyric acid (hereinafter also referred to as "BA"), 2 parts by mass of methacryloyloxypropyltrimethoxysilane (hereinafter also referred to as "MPTS"), 3 parts by mass of BuOH and 0.6 parts by mass of butylperoxy-2-ethylhexanoate (hereinafter also referred to as "TBPEH") was dropped into the reaction vessel over 6 hours. After the dropwise addition was completed, the mixture was further reacted at the same temperature for 20 hours to obtain an organic solvent solution of a vinyl polymer (a2-1) having a number average molecular weight of 10,000 and having a hydrolyzable silyl group.

[0116] Next, a mixture of 0.04 parts by mass of isopropyl acid phosphate ("Phoslex A-3" manufactured by SC Organic Chemical Co., Ltd.) and 112 parts by mass of deionized water was added dropwise over a period of 5 minutes, and the mixture was stirred at the same temperature for a further 10 hours to cause a hydrolysis condensation reaction, thereby obtaining a liquid containing a composite resin in which a hydrolyzable silyl group having a vinyl polymer (a2-1) and a hydrolyzable silyl group and a silanol group having a polysiloxane derived from the PTMS and DMDMS were bonded together. Next, 472 parts by mass of the MTMS condensate (a1) obtained in Synthesis Example 2 and 80 parts by mass of deionized water were added to this liquid, and the mixture was stirred at the same temperature for 10 hours to cause a hydrolysis condensation reaction, and the produced methanol and water were removed by distillation under the same conditions as in Synthesis Example 1. Next, 250 parts by mass of BuOH was added to obtain 1,000 parts by mass of a curable resin composition (1) with a non-volatile content of 60.1% by mass.

[0117] (Production of Curable Resin Composition (2)) A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, a cooling tube, and a nitrogen gas inlet was charged with 150 parts by mass of BuOH, 249 parts by mass of PTMS, and 263 parts by mass of DMDMS, and the temperature was raised to 80°C. Next, at the same temperature, a mixture containing 18 parts by mass of MMA, 14 parts by mass of BMA, 7 parts by mass of BA, 1 part by mass of acrylic acid (hereinafter also referred to as "AA"), 2 parts by mass of MPTS, 6 parts by mass of BuOH, and 0.9 parts by mass of TBPEH was dropped into the reaction vessel over 5 hours. After the dropwise addition was completed, the mixture was further reacted at the same temperature for 10 hours to obtain an organic solvent solution of vinyl polymers (a2-2) having hydrolyzable silyl groups and number average molecular weights of 20 and 100.

[0118] Next, a mixture of 0.05 parts by mass of isopropyl acid phosphate ("Phoslex A-3" manufactured by SC Organic Chemical Co., Ltd.) and 147 parts by mass of deionized water was added dropwise over a period of 5 minutes, and the mixture was stirred at the same temperature for a further 10 hours to cause a hydrolysis condensation reaction, thereby obtaining a liquid containing a composite resin in which a hydrolyzable silyl group having a vinyl polymer (a2-2) is bonded to a hydrolyzable silyl group and a silanol group having a polysiloxane derived from the PTMS and DMDMS. Next, 76 parts by mass of 3-glycidoxypropyltrimethoxysilane, 231 parts by mass of the MTMS condensate (a1) obtained in Synthesis Example 2, and 56 parts by mass of deionized water were added to this liquid, and the mixture was stirred at the same temperature for 15 hours to cause a hydrolysis and condensation reaction, and the produced methanol and water were removed by distillation under the same conditions as in Synthesis Example 1. Next, 250 parts by mass of BuOH was added, and 1,000 parts by mass of a curable resin composition (2) with a non-volatile content of 60.0% by mass was obtained.

[0119] Example 1 The polysiloxane resin (curable resin composition (1)) with an average molecular weight of 3500 prepared in Synthesis Example 2 and the phenolic resin with an average molecular weight of 3000 were added in a resin solid weight ratio of 45 / 55, and the silicon slurry of Si3 obtained in Synthesis Example 1 and an appropriate amount of methyl ethyl ketone solvent were added so that the silicon particle content in the product after high-temperature firing would be 50 mass%, and thoroughly mixed in a stirrer. As a result, a mixed suspension of a resin containing silicon particles with a solid concentration of 10 mass% was obtained. The amount of Mg relative to the amount of silicon particles was 100%. 2+ MgCl2 was added as a raw material to the mixed suspension of the silicon particle-containing resin so that the molar ratio of MgCl2 was 2.5 / 100. After thorough mixing, the solvent was removed in a 120°C oil bath under nitrogen flow conditions.

[0120] The mixture was then dried at 110°C for 10 hours under reduced pressure using a vacuum dryer, and finally sintered at 1100°C for 4 hours in a nitrogen atmosphere to obtain black solid composite particles. The mixture was pulverized using a planetary ball mill to produce active material composite particles. The obtained active material composite particles had a D50 of about 5.5 μm and a specific surface area of ​​3.6 m 2 The value was calculated by the Scherrer equation based on the half-width of the diffraction peak (2θ=28.4°) attributable to the silicon (111) crystal plane from the results of powder X-ray diffraction (XRD) using Cu-Kα radiation. The silicon crystallite size was 21 nm. 29Si-NMR (JEOL RESONANCE) spectrum measurement showed that the area ratio of the peak at around -85 ppm attributed to the MgSiO3 structure and the peak at around -110 ppm attributed to the SiO2 structure was 10 / 90. HR-TEM (High-Resolution Transmission Electron Microscopy) observation results showed that the thickness of the MgSiO3 layer on the silicon particle surface was approximately 0.8 nm, and that no lattice structure of crystals resembling MgSiO3 was present in the matrix phase away from the silicon particles. In addition, the results of energy dispersive X-ray spectroscopy (EDS) showed that the elemental composition ratio of the matrix phase after removing the amount of added silicon particles was SiO 1.7 C 5.6 N 0.1 It was.

[0121] A slurry was prepared by mixing 80 parts by mass of the above-obtained active material composite particles, 10 parts by mass of acetylene black as a conductive assistant, and 10 parts by mass of a mixture of CMC and SBR as a binder. The obtained slurry was formed into a film on a copper foil. After drying under reduced pressure at 110°C, a coin-type lithium-ion battery was fabricated as a half cell with a Li metal foil as a counter electrode. The charge and discharge characteristics of the fabricated half cell were evaluated using a secondary battery charge and discharge tester (manufactured by Hokuto Co., Ltd.). The cutoff voltage range was 0.005 to 1.5 V. The charge and discharge measurement results showed that the initial discharge capacity was 1545 mAh / g and the initial coulombic efficiency was 85%. For the evaluation of the full cell, a positive electrode film was prepared using a single-layer sheet using LiCoO2 as the positive electrode active material and aluminum foil as the current collector, and a negative electrode film was prepared by mixing graphite powder and active material powder with a discharge capacity design value of 450mAh / g. A non-aqueous electrolyte solution was used in which lithium hexafluorophosphate was dissolved at a concentration of 1mol / L in a mixture of ethylene carbonate and diethyl carbonate at a volume ratio of 1 / 1, and a laminated lithium ion secondary battery was prepared using a 30μm thick polyethylene microporous film as a separator. The laminated lithium ion secondary battery was charged at a constant current of 1.2mA (0.25c based on the positive electrode) at room temperature until the voltage of the test cell reached 4.2V, and after reaching 4.2V, the current was reduced to keep the cell voltage at 4.2V and the discharge capacity was calculated. The capacity retention rate after 100 cycles at 45℃ was 91%. The results are shown in Table 2.

[0122] Examples 2 to 5 Mg per silicon particle 2+ MgCl2 was added as a raw material to the mixed suspension of the silicon particle-containing resin so that the molar ratio of MgCl2 / Si was 4.0 / 100 (Example 2), 5.5 / 100 (Example 3), 7.5 / 100 (Example 4), and 12 / 100 (Example 5), respectively. The other conditions were the same as in Example 1 to obtain active material composite particles. A secondary battery was evaluated using a negative electrode active material containing the obtained active material composite particles. The results are shown in Table 2.

[0123] Example 6 The precursor preparation conditions were the same as in Example 5, and the firing temperature was set to 1180° C. to obtain active material composite particles. A secondary battery using a negative electrode active material containing the obtained active material composite particles was evaluated. The results are shown in Table 2.

[0124] Examples 7 to 8 LiCl was used as the raw material for the silicate compound instead of MgCl2. +LiCl was added to the silicon particle-containing resin mixed suspension with a molar ratio of 10 / 100 (Example 7) and 24 / 100 (Example 8), respectively, and the firing temperature was set to 1000°C. Other conditions were the same as in Example 1 to obtain active material composite particles. A secondary battery was evaluated using a negative electrode active material containing the obtained active material composite particles. The results are shown in Table 2.

[0125] Examples 9 to 11 A polysiloxane resin (curable resin composition (2)) having an average molecular weight of 3500 prepared in the same manner as in Synthesis Example 2 and a phenolic resin having an average molecular weight of 3000 were used in a weight ratio of 10 / 90 (Example 9), 20 / 80 (Example 10), and 80 / 20 (Example 11) of resin solids. The amount of MgCl2 added was the same as in Example 4, with respect to the amount of silicon particles. 2+ The MgCl2 raw material was added to the mixed suspension of the silicon particle-containing resin so that the molar ratio of MgCl2 / Si was 7.5 / 100. The other conditions were the same as in Example 1 to obtain active material composite particles. A secondary battery was evaluated using a negative electrode active material containing the obtained active material composite particles. The results are shown in Table 2.

[0126] Examples 12 to 14 The silicon particles in the mixed suspension of the silicon particle-containing resin described in Example 1 were replaced with the silicon particles Si4 (Example 12), Si2 (Example 13), and Si1 (Example 14) obtained in Synthesis Example 1, and the other conditions were the same as in Example 1 to obtain active material composite particles. A secondary battery using a negative electrode active material containing the obtained active material composite particles was evaluated. The results are shown in Table 2.

[0127] Example 15 The amount of MgCl2 added was calculated based on the amount of silicon particles. 2+ Active material composite particles were obtained in the same manner as in Example 4, except that the molar ratio of ZnO / Si was 2.0 / 100. A secondary battery using a negative electrode active material containing the obtained active material composite particles was evaluated. The results are shown in Table 2.

[0128] Example 16 A mixed suspension of silicon particle-containing resin was prepared using commercially available silicon particles (manufactured by Alfa Aesar, 50 nm) and pitch (carbon source) so that the silicon particle content would be 50% by weight after high-temperature firing. Other conditions were the same as in Example 1 to obtain active material composite particles. A secondary battery was evaluated using a negative electrode active material containing the obtained active material composite particles. The results are shown in Table 2.

[0129] Comparative Example 1 Li as silicate compound + or Mg 2+ The other conditions were the same as in Example 1, except that no compound was added, and the dried precursor was prepared and then calcined at 1100°C for 4 hours in a nitrogen atmosphere to obtain an active material powder. The active material powder had a D50 of about 5.4 μm and a specific surface area of ​​4.1 m 2 The charge / discharge measurement results were a half-cell charge / discharge capacity of 1935 mAh / g, a discharge capacity of 1587 mAh / g, an initial efficiency of 80.1%, and a capacity retention rate of 90% after 100 cycles in a full cell at 45°C.

[0130] Comparative Example 2 A precursor was prepared by using the silicon particles Si5 of Synthesis Example 1 in the mixed suspension of the silicon particle-containing resin. Other conditions were the same as in Example 1 to obtain active material composite particles. A secondary battery was evaluated using a negative electrode active material containing the obtained active material composite particles. The results are shown in Table 2.

[0131] [Table 2]

[0132] [Evaluation method] In Table 2, the evaluation methods are as follows. D50: Measured using a laser diffraction particle size distribution analyzer (Malvern Panalytical, Mastersizer 3000). Specific surface area: Measured by the BET method using a specific surface area measuring device (BELSORP-mini, manufactured by BELJAPAN) based on nitrogen adsorption measurement. 29Si-NMR: JNM-ECA600 manufactured by JEOL RESONANCE was used.

[0133] Battery characteristic evaluation: Battery characteristics were measured using a secondary battery charge / discharge tester (manufactured by Hokuto Denko Corporation). The charge / discharge characteristics were evaluated under the set conditions of constant current / constant voltage charge / constant current discharge, with a room temperature of 25°C, a cutoff voltage range of 0.005 to 1.5V, and a charge / discharge rate of 0.1C (1st to 3rd times) and 0.2C (after 4th cycle). When switching between charge and discharge, the battery was left in an open circuit for 30 minutes. The initial coulombic efficiency and cycle characteristics (which in this application refers to the capacity retention rate at 100 cycles) were calculated as follows: Initial (coulombic) efficiency (%) = initial discharge capacity (mAh / g) / initial charge capacity (mAh / g) Capacity retention rate (%@100th) = 100th discharge capacity (mAh / g) / initial discharge capacity (mAh / g)

[0134] As is clear from the above results, when the present active material is used as a negative electrode active material, the initial coulombic efficiency is 83% or more, the capacity retention rate is 85% or more, and these secondary battery properties are generally high, and the balance of these properties is excellent. Furthermore, a secondary battery containing the present active material as a negative electrode active material has excellent battery properties.

Claims

1. The silicon particles have an average particle size of 150 nm or less, a matrix phase in which the silicon particles are dispersed, and a silicate compound of at least one metal selected from the group consisting of Li, K, Na, Ca, Mg, and Al; The silicate compound is present in the vicinity of the surface of the silicon particle, The matrix phase at least contains a compound represented by SiOxCyNz (where 1≦x≦2, 1≦y≦20, 0≦z≦0.5). A composite active material for secondary batteries.

2. 2. The composite active material for a secondary battery according to claim 1, wherein the silicate concentration in the vicinity of the surface of the silicon particle is higher than the silicate concentration in the matrix phase.

3. 3. The composite active material for a secondary battery according to claim 1, further comprising silicon dioxide in the vicinity of the surface of the silicon particles.

4. 4. The composite active material for a secondary battery according to claim 3, wherein a molar ratio of said silicon dioxide is 0.9 or less, based on a total molar number of said silicate compound and said silicon dioxide being 1.

5. 3. The composite active material for a secondary battery according to claim 1, wherein the silicate compound is a magnesium silicate compound.

6. 6. The composite active material for a secondary battery according to claim 5, wherein the magnesium silicate compound in the vicinity of the surface of the silicon particle is a crystalline film having a thickness of 0.2 nm to 10 nm.

7. 3. The composite active material for a secondary battery according to claim 1, wherein the silicon particles are in the form of flake crystals, and the crystallite size obtained from the peak at 2θ of 28.4° in an X-ray diffraction spectrum is 25 nm or less.

8. Average particle size is 1 to 15 μm, specific surface area is 1 m 2 / g to 30m 23. The composite active material for a secondary battery according to claim 1, wherein the Mo content is 1 / g.

9. A secondary battery comprising the composite active material for secondary batteries according to claim 1 or 2 in a negative electrode.

Citation Information

Patent Citations

  • Nonaqueous electrolyte battery and negative active material

    JP2007059213A

  • Negative electrode active material, mixing negative electrode active material, and method of manufacturing negative electrode active material

    JP2018060771A

  • Silicon composite oxide for lithium secondary battery negative electrode material and production method thereof

    JP2018156922A

  • Fine particle, method for producing the same, and lithium ion secondary battery