Polyimide precursor composition and polyimide film

A polyimide precursor composition with specific tetracarboxylic dianhydride and diamine components, combined with an imidazole compound, addresses thermal decomposition and expansion issues, providing a polyimide film with high thermal resistance, low expansion, and reduced haze for flexible electronic devices.

JP7586281B2Active Publication Date: 2024-11-19UBE CORPORATION
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023500928
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-07-02
Filing Date
2022-02-17
Publication Date
2024-11-19
Estimated Expiration
2042-02-17

AI Technical Summary

Technical Problem

Existing polyimide films lack sufficient thermal decomposition resistance, high thermal expansion coefficients, and optical transparency, making them unsuitable for high-temperature processing in flexible electronic devices, and they also suffer from storage stability issues and high haze values.

Method used

A polyimide precursor composition comprising specific tetracarboxylic dianhydride and diamine components, with a structure represented by general formula (I), and the inclusion of an imidazole compound, which results in a polyimide film with improved thermal decomposition resistance, low thermal expansion, high transparency, and reduced haze, along with enhanced storage stability.

Benefits of technology

The polyimide film exhibits a 5% weight loss temperature of 515°C or higher, a linear thermal expansion coefficient of 20 ppm/K or less, and a haze value of less than 1.0%, while maintaining excellent mechanical properties and optical clarity, suitable for flexible electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586281000001
    Figure 0007586281000001
  • Figure 0007586281000002
    Figure 0007586281000002
  • Figure 0007586281000003
    Figure 0007586281000003
Patent Text Reader

Abstract

Provided are: a precursor composition which can produce a polyimide film with excellent light transmittance, excellent mechanical properties, an excellent coefficient of linear thermal expansion and excellent resistance to thermal decomposition; and a polyimide film obtained from said precursor composition. The polyimide precursor composition contains: a polyimide precursor with a repeating unit represented by formula (I); an imidazole compound in an amount in the range of 0.01 to 2 moles in relation to 1 mole of the repeating unit of the polyimide precursor; and a solvent. (I) In general formula I, 70 mol.% or more of X1 is a structure represented by formula (1-1), and 70 mol.% or more of Y1 is a structure represented by formula (D-1) and / or (D-2).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyimide precursor composition that is suitably used for electronic device applications such as substrates for flexible devices, and a polyimide film having improved resistance to thermal decomposition. [Background technology]

[0002] Polyimide films have been widely used in fields such as electric and electronic devices and semiconductors due to their excellent heat resistance, chemical resistance, mechanical strength, electrical properties, and dimensional stability. Meanwhile, in recent years, with the advent of an advanced information society, the development of optical materials such as optical fibers and optical waveguides in the optical communications field, and liquid crystal alignment films and protective films for color filters in the display device field has progressed. In particular, in the display device field, there has been active research into lightweight and flexible plastic substrates as an alternative to glass substrates, and the development of displays that can be bent or rolled.

[0003] Displays such as liquid crystal displays and organic electroluminescence displays use semiconductor elements such as TFTs to drive each pixel. This requires heat resistance and dimensional stability in the substrate. Polyimide film is promising as a substrate for displays because it has excellent heat resistance, chemical resistance, mechanical strength, electrical properties, and dimensional stability.

[0004] Polyimide is generally colored yellowish brown, which limits its use in transparent devices such as backlit liquid crystal displays. However, in recent years, polyimide films with excellent optical transparency as well as mechanical and thermal properties have been developed, raising expectations for their use as substrates for displays (see Patent Documents 1 to 3).

[0005] Patent Documents 4 to 8 disclose polyimide films obtained from a monomer component containing a tetracarboxylic dianhydride having two norbornane rings (bicyclo[2.2.1]heptane rings) bonded by a single bond. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2012 / 011590 [Patent Document 2] International Publication No. 2013 / 179727 [Patent Document 3] International Publication No. 2014 / 038715 [Patent Document 4] International Publication No. 2017 / 030019 [Patent Document 5] International Publication No. 2019 / 163703 [Patent Document 6] JP 2018-44180 A [Patent Document 7] International Publication No. 2018 / 051888 [Patent Document 8] JP 2019-137828 A Summary of the Invention [Problem to be solved by the invention]

[0007] Known examples of TFTs (thin film transistors) include amorphous silicon TFTs (a-Si TFTs), low-temperature polysilicon TFTs (LTPS TFTs), high-temperature polysilicon TFTs, and oxide TFTs. Even amorphous silicon TFTs, which can be formed at relatively low temperatures, require a film formation temperature of 300°C to 400°C. In particular, high-temperature film formation is advantageous for forming a semiconductor layer with high charge mobility. However, if the thermal decomposition resistance of the polyimide film is insufficient, for example, in the TFT formation process, outgassing due to the decomposition of polyimide may cause swelling between the polyimide film and the barrier film, or may contaminate the manufacturing equipment. As a substrate for flexible electronic devices, a material that is stable at high temperatures, that is, a film that has excellent thermal decomposition resistance at process temperatures and generates very little gas, is preferable. From the viewpoint of process margin, a film with a high thermal decomposition (initiation) temperature is also preferable.

[0008] In addition, since heating and cooling (cooling down) are repeated during the manufacturing process of flexible electronic devices, a polyimide film with excellent thermal properties, such as a sufficiently small coefficient of linear thermal expansion (CTE), is preferable as a substrate for flexible electronic devices.

[0009] The above Patent Documents 4 to 8 state that the object is to provide a polyimide having excellent light transmittance and heat resistance. There is no disclosure of a polyimide film that has a sufficiently small linear thermal expansion coefficient and high thermal decomposition resistance while having light transmittance and mechanical properties in a satisfactory range. For example, Patent Document 6 evaluates heat resistance by glass transition temperature (Tg), but does not disclose a polyimide film having excellent thermal decomposition resistance. Therefore, there is a strong demand for the realization of a polyimide film having excellent thermal decomposition resistance that is optimal, for example, as a substrate for flexible electronic devices. As a result of intensive research by the present inventors, we have found a composition that gives a polyimide with high heat resistance as a combination of an appropriate tetracarboxylic acid component, including a tetracarboxylic dianhydride having two norbornane rings bonded by a single bond, and an appropriate diamine component. However, it was found that the haze value of the film produced from this was high and the film was cloudy, making it unsuitable for use as an optical substrate for displays and the like. Furthermore, as a result of the research conducted by the present inventors, it was found that a polyimide precursor solution which gives a highly heat-resistant polyimide has a problem of poor storage stability and a decrease in fluidity during storage.

[0010] The present invention has been made in consideration of the problems in the related art, and an object of the present invention is to provide a precursor composition from which a polyimide film having a sufficiently small coefficient of linear thermal expansion, excellent light transmission and mechanical properties, and particularly excellent resistance to thermal decomposition, can be produced, and a polyimide film obtained from the precursor composition. Another object of the present invention is to provide a polyimide precursor composition capable of producing a polyimide film having a small haze value and little turbidity, preferably in addition to the above-mentioned properties, and a polyimide film obtained from the precursor composition. Another object of the present invention is to provide a polyimide precursor composition which is capable of producing a polyimide film preferably having the above-mentioned properties and which has excellent storage stability. [Means for solving the problem]

[0011] The main disclosures of this application can be summarized as follows: 1. A polyimide precursor having a repeating unit represented by the following general formula (I): at least one imidazole compound contained in an amount ranging from more than 0.01 moles to 2 moles or less per mole of the repeating unit of the polyimide precursor; and solvent A polyimide precursor composition comprising:

[0012] [ka] (In the general formula I, X1 is a tetravalent aliphatic group or aromatic group, Y1 is a divalent aliphatic group or aromatic group, R1 and R2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms, provided that 70 mol % or more of X1 is a group represented by the formula (1-1):

[0013] [ka] wherein 70 mol % or more of Y1 is represented by formula (D-1) and / or (D-2):

[0014] [ka] It is a structure represented by the following formula:

[0015] 2. The polyimide precursor composition according to item 1 above, wherein the imidazole compound is at least one selected from the group consisting of 1,2-dimethylimidazole, 1-methylimidazole, 2-methylimidazole, 2-phenylimidazole, imidazole and benzimidazole.

[0016] 3. The polyimide precursor composition according to item 1 or 2, wherein 90 mol % or more of X1 are the structure represented by formula (1-1).

[0017] 4. The polyimide precursor composition according to any one of items 1 to 3, wherein a polyimide film obtained from the polyimide precursor composition exhibits a 5% weight loss temperature of 515° C. or higher.

[0018] 5. The polyimide precursor composition according to any one of items 1 to 4 above, wherein a polyimide film obtained from the polyimide precursor composition has a linear thermal expansion coefficient of 20 ppm / K or less.

[0019] 6. The polyimide precursor composition according to any one of items 1 to 5 above, wherein a polyimide film having a thickness of 10 μm obtained from the polyimide precursor composition has a haze value of less than 1.0%.

[0020] 7. The polyimide precursor composition according to any one of items 1 to 6, which maintains its fluidity when stored in a sealed state at 23° C. for 10 days.

[0021] 8. A polyimide film obtained from the polyimide precursor composition according to any one of items 1 to 7 above.

[0022] 9. A polyimide film obtained from the polyimide precursor composition according to any one of items 1 to 7 above; Substrate and A polyimide film / substrate laminate comprising:

[0023] 10. The laminate according to item 9, wherein the base material is a glass substrate.

[0024] 11. (a) a step of applying the polyimide precursor composition according to any one of items 1 to 7 onto a substrate; and (b) a step of heat-treating the polyimide precursor on the substrate and laminating a polyimide film on the substrate; A method for producing a polyimide film / substrate laminate having the above structure.

[0025] 12. The method according to item 11, wherein the base material is a glass substrate.

[0026] 13. (a) A step of applying the polyimide precursor composition according to any one of items 1 to 7 onto a substrate; (b) heat-treating the polyimide precursor on the substrate to produce a polyimide film / substrate laminate in which a polyimide film is laminated on the substrate; (c) forming at least one layer selected from a conductive layer and a semiconductor layer on the polyimide film of the laminate; and (d) peeling the polyimide film from the substrate A method for producing a flexible electronic device comprising the steps of:

[0027] 14. The method according to item 13, wherein the substrate is a glass substrate. Effect of the Invention

[0028] According to the present invention, it is possible to provide a polyimide precursor composition capable of producing a polyimide film having a sufficiently small linear thermal expansion coefficient and excellent light transmittance, mechanical properties and thermal decomposition resistance, and a polyimide film obtained from the precursor composition. Furthermore, according to one embodiment of the present invention, it is possible to provide a polyimide precursor composition capable of producing a polyimide film having a small haze value and little turbidity, in addition to the above-mentioned properties, and a polyimide film obtained from the precursor composition. Furthermore, according to one embodiment of the present invention, in addition to being able to produce a polyimide film preferably having the above-mentioned properties, it is also possible to provide a polyimide precursor composition having excellent storage stability.

[0029] According to another aspect of the present invention, there are provided a polyimide film and a polyimide film / substrate laminate obtained by using the polyimide precursor composition. According to another aspect of the present invention, there are provided a method for producing a flexible electronic device using the polyimide precursor composition, and a flexible electronic device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] In this application, the term "flexible (electronic) device" means that the device itself is flexible, and the device is usually completed by forming a semiconductor layer (such as transistors and diodes as elements) on a substrate. The "flexible (electronic) device" is distinguished from devices such as COF (Chip On Film) in which a "hard" semiconductor element such as an IC chip is mounted on a conventional FPC (flexible printed circuit board). However, there is no problem in mounting a "hard" semiconductor element such as an IC chip on a flexible substrate or electrically connecting the same to the flexible substrate to operate or control the "flexible (electronic) device" of this application. Suitable flexible (electronic) devices include display devices such as liquid crystal displays, organic EL displays, and electronic paper, solar cells, and light-receiving devices such as CMOS.

[0031] The polyimide precursor composition of the present invention will be described below, followed by a description of a method for producing a flexible electronic device.

[0032] <<Polyimide precursor composition>> The polyimide precursor composition for forming a polyimide film contains a polyimide precursor, an imidazole compound, and a solvent, both of which are dissolved in the solvent.

[0033] The polyimide precursor is represented by the following general formula (I):

[0034] [ka] (In general formula I, X1 is a tetravalent aliphatic or aromatic group, Y1 is a divalent aliphatic or aromatic group, and R1 and R2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms.) Particularly preferred is a polyamic acid in which R1 and R2 are hydrogen atoms. When X1 and Y1 are aliphatic groups, the aliphatic groups are preferably groups having an alicyclic structure.

[0035] Of all the repeating units in the polyimide precursor, preferably 70 mol % or more of X1 is a structure represented by the following formula (1-1), i.e., a structure derived from 2,2'-binorbornane-5,5',6,6'-tetracarboxylic dianhydride (hereinafter abbreviated as BNBDA as necessary).

[0036] [ka]

[0037] Of all the repeating units in the polyimide precursor, preferably 70 mol % or more of Y1 are structures represented by the following formulas (D-1) and / or (D-2), i.e., structures derived from 4,4'-diaminobenzanilide (abbreviated as DABAN if necessary).

[0038] [ka]

[0039] By using a composition containing such a polyimide precursor, it is possible to produce a polyimide film that has a sufficiently small coefficient of linear thermal expansion, excellent light transmission and mechanical properties, and in addition, particularly excellent resistance to thermal decomposition.

[0040] The polyimide precursor will be explained with reference to the monomers (tetracarboxylic acid component, diamine component, other components) that provide X1 and Y1 in the general formula (I), and then the production method will be explained.

[0041] In this specification, the tetracarboxylic acid component includes tetracarboxylic acids, tetracarboxylic dianhydrides, other tetracarboxylic acid silyl esters, tetracarboxylic acid esters, tetracarboxylic acid chlorides, and other tetracarboxylic acid derivatives used as raw materials for producing polyimide. Although not particularly limited, it is convenient to use tetracarboxylic dianhydrides in production. In the following description, an example using tetracarboxylic dianhydride as the tetracarboxylic acid component will be described. The diamine component is a diamine compound having two amino groups (-NH2) used as a raw material for producing polyimide.

[0042] In this specification, the polyimide film means both a film formed on a (carrier) substrate and present in the laminate, and a film after peeling off the substrate. Also, the material constituting the polyimide film, that is, the material obtained by heat-treating (imidizing) the polyimide precursor composition, may be referred to as the "polyimide material".

[0043] <X1 and Tetracarboxylic Acid Component> As described above, in all repeating units in the polyimide precursor, X1 preferably has a structure represented by the formula (1-1) in an amount of 70 mol% or more, more preferably 80 mol% or more, still more preferably 90 mol% or more, and most preferably 95 mol% or more (100 mol% is also very preferable). The tetracarboxylic dianhydride that gives the structure of the formula (1-1) as X1 is 2,2'-bionorbornane-5,5',6,6'-tetracarboxylic dianhydride (BNBDA).

[0044] In the present invention, X1 may contain a tetravalent aliphatic group or aromatic group other than the structure represented by formula (1-1) (abbreviated as "other X1") in an amount within a range that does not impair the effects of the present invention. That is, the tetracarboxylic acid component may contain other tetracarboxylic acid derivatives in addition to BNBDA in an amount within a range that does not impair the effects of the present invention. The amount of other tetracarboxylic acid derivatives is 30 mol% or less (preferably less than 30 mol%), more preferably 20 mol% or less (preferably less than 20 mol%), and even more preferably 10 mol% or less (preferably less than 10 mol%) (0 mol% is also preferable) relative to 100 mol% of the tetracarboxylic acid component.

[0045] When "another X1" is a tetravalent group having an aromatic ring, it is preferably a tetravalent group having an aromatic ring having 6 to 40 carbon atoms.

[0046] Examples of the tetravalent group having an aromatic ring include the following.

[0047] [ka] (In the formula, Z1 is a direct bond or the following divalent group:

[0048] [ka] In the formula, Z2 is a divalent organic group, Z 3、 Z4 is independently an amide bond, an ester bond, or a carbonyl bond, and Z5 is an organic group containing an aromatic ring.

[0049] Specific examples of Z2 include aliphatic hydrocarbon groups having 2 to 24 carbon atoms and aromatic hydrocarbon groups having 6 to 24 carbon atoms.

[0050] Specific examples of Z5 include aromatic hydrocarbon groups having 6 to 24 carbon atoms.

[0051] As the tetravalent group having an aromatic ring, the following are particularly preferred since they can provide a polyimide film having both high heat resistance and high light transmittance.

[0052] [ka] (In the formula, Z1 is a direct bond or a hexafluoroisopropylidene bond.)

[0053] Here, Z1 is more preferably a direct bond, since this allows the resulting polyimide film to have high heat resistance, high light transmittance, and a low linear thermal expansion coefficient all at the same time.

[0054] In addition, as a preferred group, in the above formula (9), Z1 is the following formula (3A):

[0055] [ka] Examples of such compounds include compounds having a fluorenyl-containing group represented by the formula: 11 and Z 12 are each independently, preferably the same, a single bond or a divalent organic group. 11 and Z 12 As the group, an organic group containing an aromatic ring is preferable, for example, a group represented by the formula (3A1):

[0056] [ka] (Z 13 and Z 14 are each independently a single bond, -COO-, -OCO- or -O-, where Z 14 When attached to a fluorenyl group, Z 13 is -COO-, -OCO- or -O- and Z 14 is preferably a single bond; R 91 is an alkyl group having 1 to 4 carbon atoms or a phenyl group, preferably methyl, and n is an integer of 0 to 4, preferably 1. The structure represented by the following formula is preferred.

[0057] Examples of tetracarboxylic acid components that provide repeating units of general formula (I) in which X1 is a tetravalent group having an aromatic ring include 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic acid, pyromellitic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, and the like. Examples of the tetracarboxylic acid component that provides the repeating unit of general formula (I) in which X1 is a tetravalent group having an aromatic ring containing a fluorine atom include 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane and its derivatives such as tetracarboxylic acid dianhydride, tetracarboxylic acid silyl ester, tetracarboxylic acid ester, and tetracarboxylic acid chloride. Further, a preferred compound is (9H-fluorene-9,9-diyl)bis(2-methyl-4,1-phenylene)bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylate). The tetracarboxylic acid component may be used alone or in combination of two or more kinds.

[0058] When "other X1" is a tetravalent group having an alicyclic structure, it is preferably a tetravalent group having an alicyclic structure having 4 to 40 carbon atoms, and more preferably has at least one aliphatic 4- to 12-membered ring, more preferably an aliphatic 4-membered ring or an aliphatic 6-membered ring. Preferable tetravalent groups having an aliphatic 4-membered ring or an aliphatic 6-membered ring include the following.

[0059] [ka] (In the formula, R 31 ~R 38 R is independently a direct bond or a divalent organic group. 41 ~R 47 , and R 71 ~R 73 R each independently represents one selected from the group consisting of groups represented by the formulas: -CH2-, -CH=CH-, -CH2CH2-, -O-, and -S-. 48 is an organic group containing an aromatic ring or an alicyclic structure.

[0060] R 31 , R 32 , R 33 , R 34 , R 35 , R 36 , R 37 , R 38 Specific examples of the bond include a direct bond, an aliphatic hydrocarbon group having 1 to 6 carbon atoms, an oxygen atom (-O-), a sulfur atom (-S-), a carbonyl bond, an ester bond, and an amide bond.

[0061] R 48 Examples of the organic group containing an aromatic ring include the following.

[0062] [ka] (Wherein, W1 is a direct bond or a divalent organic group, n 11 ~n 13 each independently represents an integer of 0 to 4; R 51 , R 52 , R 53 are each independently an alkyl group having 1 to 6 carbon atoms, a halogen group, a hydroxyl group, a carboxyl group, or a trifluoromethyl group.

[0063] Specific examples of W1 include a direct bond, a divalent group represented by the following formula (5), and a divalent group represented by the following formula (6).

[0064] [ka] (R in Equation (6) 61 ~R 68 each independently represents a direct bond or a divalent group represented by the formula (5).

[0065] As the tetravalent group having an alicyclic structure, the following are particularly preferred since they can provide the resulting polyimide with high heat resistance, high light transmittance, and a low linear thermal expansion coefficient.

[0066] [ka]

[0067] Examples of tetracarboxylic acid components which provide the repeating unit of formula (I) in which X1 is a tetravalent group having an alicyclic structure include 1,2,3,4-cyclobutanetetracarboxylic acid, isopropylidenediphenoxybisphthalic acid, cyclohexane-1,2,4,5-tetracarboxylic acid, [1,1'-bi(cyclohexane)]-3,3',4,4'-tetracarboxylic acid, [1,1'-bi(cyclohexane)]-2,3,3',4'-tetracarboxylic acid, [1,1'-bi(cyclohexane)]-2,2',3,3'-tetracarboxylic acid, 4,4'-methylenebis(cyclohexane-1,2-dicarboxylic acid), 4,4'-(propane-2,2-diyl)bis(cyclohexane-1,2-dicarboxylic acid), 4,4'-oxybis(cyclohexane-1,2-dicarboxylic acid), 4,4'-thiobis(cyclohexane-1,2-dicarboxylic acid), 4,4'-sulfonylbis( cyclohexane-1,2-dicarboxylic acid), 4,4'-(dimethylsilanediyl)bis(cyclohexane-1,2-dicarboxylic acid), 4,4'-(tetrafluoropropane-2,2-diyl)bis(cyclohexane-1,2-dicarboxylic acid), octahydropentalene-1,3,4,6-tetracarboxylic acid, bicyclo[2.2.1]heptane-2,3,5,6-tetracarboxylic acid, 6-(carboxymethyl)bicyclo[2. 2.1]heptane-2,3,5-tricarboxylic acid, bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic acid, bicyclo[2.2.2]oct-5-ene-2,3,7,8-tetracarboxylic acid, tricyclo[4.2.2.02,5]decane-3,4,7,8-tetracarboxylic acid, tricyclo[4.2.2.02,5]dec-7-ene-3,4,9,10-tetracarboxylic acid, 9-oxatricyclo[4.2.1.02,5]Nonane-3,4,7,8-tetracarboxylic acid, norbornane-2-spiro-α-cyclopentanone-α'-spiro-2''-norbornane 5,5'',6,6''-tetracarboxylic acid, (4arH,8acH)-decahydro-1t,4t:5c,8c-dimethanonaphthalene-2c,3c,6c,7c-tetracarboxylic acid, (4arH,8acH)-decahydro-1t,4t:5c,8c-dimethanonaphthalene-2t,3t,6c,7c-tetracarboxylic acid, decahydro-1,4-ethano-5,8-methanonaphthalene-2,3,6,7-tetracarboxylic acid, tetradecahydro-1,4:5,8:9,10-trimethanoanthracene-2,3,6,7-tetracarboxylic acid, and derivatives thereof such as tetracarboxylic dianhydrides, tetracarboxylic acid silyl esters, tetracarboxylic acid esters, and tetracarboxylic acid chlorides. The tetracarboxylic acid component may be used alone or in combination of two or more kinds.

[0068] <Y1 and diamine component> As described above, in all repeating units in the polyimide precursor, Y1 preferably has a structure represented by formula (D-1) and / or (D-2) in an amount of 70 mol% or more, more preferably 80 mol% or more, still more preferably 90 mol% or more (100 mol% is also preferable), and is a structure represented by formula (D-1) and / or (D-2). The diamine compound that gives the structure of formula (D-1) or formula (D-2) as Y1 is 4,4'-diaminobenzanilide (abbreviation: DABAN).

[0069] In the present invention, Y1 may contain a divalent aliphatic group or aromatic group (abbreviated as "other Y1") other than the structures represented by formulae (D-1) and (D-2) in an amount that does not impair the effects of the present invention. That is, the diamine component may contain other diamine compounds in addition to DABAN in an amount that does not impair the effects of the present invention. The amount of other diamine compounds is 30 mol% or less (preferably less than 30 mol%), more preferably 20 mol% or less (preferably less than 20 mol%), and even more preferably 10 mol% or less (preferably less than 10 mol%) (0 mol% is also preferred) relative to 100 mol% of the diamine component.

[0070] In a preferred embodiment of the present invention, the ratio of the structure of formula (D-1) and / or (D-2) in Y1 is less than 100 mol %. In this case, the other Y1 is a structure of formula (G-1):

[0071] [ka] (In the formula, m represents 0 to 3, n1 and n2 each independently represent an integer of 0 to 4, B1 and B2 each independently represent one selected from the group consisting of an alkyl group having 1 to 6 carbon atoms, a halogen group, or a fluoroalkyl group having 1 to 6 carbon atoms, and X each independently represent one selected from the group consisting of a direct bond, or a group represented by the formula: -NHCO-, -CONH-, -COO-, -OCO-, except for the formulas (D-1) and (D-2).) It is preferable that the compound contains a structure represented by the following formula:

[0072] m is preferably 0, 1 or 2, n1 and n2 are preferably 0 or 1, and B1 and B2 are preferably a methyl group or a trifluoromethyl group. For example, there are structures where m=0 and n1=0, where m=1 and X is a direct bond or -COO-, -OCO-, and n1=n2=0 or 1, and where m=2 and X is a direct bond or -COO-, -OCO-. Particularly preferred structures are those where m=1 and X is a direct bond.

[0073] The structure of formula (G-1) is preferably contained in a proportion of more than 0 mol% and not more than 30 mol%, more preferably more than 5 mol% and not more than 30 mol% of Y1. By containing the structure of formula (G-1), mechanical properties such as breaking strength and optical properties can be improved. The structure of formula (G-1) includes the structures of formula (B-1) and / or (B-2):

[0074] [ka] Examples of the structure include those represented by the following formula: Furthermore, as Y1, "other Y1" other than those represented by formula (D-1), formula (D-2) and formula (G-1) may be contained in a proportion of 10 mol % or less (0 mol % is also preferred).

[0075] When "other Y1" other than that of formula (G-1) is a divalent group having an aromatic ring, it is preferably a divalent group having an aromatic ring having 6 to 40 carbon atoms, more preferably 6 to 20 carbon atoms.

[0076] Examples of the divalent group having an aromatic ring include the following, except for those included in formula (G-1).

[0077] [ka] (Wherein, W1 is a direct bond or a divalent organic group, n 11 ~n 13 each independently represents an integer of 0 to 4; R 51 , R 52 , R 53 are each independently an alkyl group having 1 to 6 carbon atoms, a halogen group, a hydroxyl group, a carboxyl group, or a trifluoromethyl group.

[0078] Specific examples of W1 include a direct bond, a divalent group represented by the following formula (5), and a divalent group represented by the following formula (6).

[0079] [ka]

[0080] [ka] (R in Equation (6) 61 ~R 68 each independently represents a direct bond or a divalent group represented by the formula (5).

[0081] Here, it is particularly preferable that W1 is a direct bond or one selected from the group consisting of groups represented by the formulae: -NHCO-, -CONH-, -COO-, and -OCO-, because the resulting polyimide can have high heat resistance, high light transmittance, and a low linear thermal expansion coefficient at the same time. 61 ~R 68 is particularly preferably any one of a direct bond or a divalent group represented by the formula (6), which is one selected from the group consisting of groups represented by the formulas: -NHCO-, -CONH-, -COO-, and -OCO-. However, when -NHCO- or -CONH- is selected, "other Y1" is selected so as to be different from formula (D-1) or formula (D-2).

[0082] In addition, as a preferred group, in the above formula (4), W1 is the following formula (3B):

[0083] [ka] Examples of such compounds include compounds having a fluorenyl-containing group represented by the formula: 11 and Z 12 are each independently, preferably the same, a single bond or a divalent organic group. 11 and Z 12 As the group, an organic group containing an aromatic ring is preferable, for example, a group represented by the formula (3B1):

[0084] [ka] (Z 13 and Z 14are each independently a single bond, -COO-, -OCO- or -O-, where Z 14 When attached to a fluorenyl group, Z 13 is -COO-, -OCO- or -O- and Z 14 is preferably a single bond; R 91 is an alkyl group having 1 to 4 carbon atoms or a phenyl group, preferably phenyl, and n is an integer of 0 to 4, preferably 1. The structure represented by the following formula is preferred.

[0085] Another preferred group is a compound represented by the above formula (4) in which W1 is a phenylene group, that is, a terphenyldiamine compound, and particularly preferred is a compound in which all bonds are para-bonded.

[0086] As another preferred group, in the above formula (4), W1 is R 61 and R 62 is a 2,2-propylidene group.

[0087] As yet another preferred group, in the above formula (4), W1 is represented by the following formula (3B2):

[0088] [ka] Examples of the compound include compounds represented by the following formula:

[0089] Examples of diamine components that provide repeating units of general formula (I) in which Y1 is a divalent group having an aromatic ring include p-phenylenediamine, m-phenylenediamine, benzidine, 3,3'-diamino-biphenyl, 2,2'-bis(trifluoromethyl)benzidine, 3,3'-bis(trifluoromethyl)benzidine, m-tolidine, 3,4'-diaminobenzanilide, N,N'-bis(4-aminophenyl)terephthalamide, N,N'-p-phenylenebis(p-aminobenzamide), and 4-aminophenoxy-4-diaminobenzoate. , bis(4-aminophenyl)terephthalate, biphenyl-4,4'-dicarboxylic acid bis(4-aminophenyl)ester, p-phenylenebis(p-aminobenzoate), bis(4-aminophenyl)-[1,1'-biphenyl]-4,4'-dicarboxylate, [1,1'-biphenyl]-4,4'-diylbis(4-aminobenzoate), 4,4'-oxydianiline, 3,4'-oxydianiline, 3,3'-oxydianiline, p-methylenebis(phenylenediamine), 1,3-bis(4-aminophenoxy)benzene, 1, 3-bis(3-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 2,2-bis(4-(4-aminophenoxy)phenyl)hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, bis(4-aminophenyl)sulfone, 3,3'-bis(trifluoromethyl)benzidine, 3,3'-bis((aminophenoxy)phenyl)propane, 2,2'-bis(3-amino-4 -hydroxyphenyl)hexafluoropropane, bis(4-(4-aminophenoxy)diphenyl)sulfone, bis(4-(3-aminophenoxy)diphenyl)sulfone, octafluorobenzidine, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dichloro-4,4'-diaminobiphenyl, 3,3'-difluoro-4,4'-diaminobiphenyl, 2,4-bis(4-aminoanilino)-6-amino-1,3,5-triazine, 2,4-bis(4-aminoanilino)-6-methylamino-1,3,5-triazine, 2,Examples of the diamine component that provides the repeating unit of the general formula (I) in which Y1 is a divalent group having an aromatic ring containing a fluorine atom include 2,2'-bis(trifluoromethyl)benzidine, 3,3'-bis(trifluoromethyl)benzidine, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, and 2,2'-bis(3-amino-4-hydroxyphenyl)hexafluoropropane. Additionally, preferred diamine compounds include 9,9-bis(4-aminophenyl)fluorene, 4,4'-(((9H-fluorene-9,9-diyl)bis([1,1'-biphenyl]-5,2-diyl))bis(oxy))diamine, [1,1':4',1"-terphenyl]-4,4"-diamine, and 4,4'-([1,1'-binaphthalene]-2,2'-diylbis(oxy))diamine. The diamine components may be used alone or in combination.

[0090] When "other Y1" is a divalent group having an alicyclic structure, it is preferably a divalent group having an alicyclic structure having 4 to 40 carbon atoms, and further preferably has at least one aliphatic 4- to 12-membered ring, more preferably aliphatic 6-membered ring.

[0091] Examples of the divalent group having an alicyclic structure include the following.

[0092] [ka] (In the formula, V1 and V2 each independently represent a direct bond or a divalent organic group, n 21 ~n 26 each independently represents an integer of 0 to 4; R 81 ~R 86 are each independently an alkyl group having 1 to 6 carbon atoms, a halogen group, a hydroxyl group, a carboxyl group, or a trifluoromethyl group, and R91 , R 92 , R 93 are each independently one selected from the group consisting of groups represented by the formula: -CH2-, -CH=CH-, -CH2CH2-, -O-, and -S-.

[0093] Specific examples of V1 and V2 include a direct bond and a divalent group represented by the above formula (5).

[0094] As the divalent group having an alicyclic structure, the following are particularly preferred since they can provide a polyimide having both high heat resistance and a low linear thermal expansion coefficient.

[0095] [ka] Among the divalent groups having an alicyclic structure, the following are preferred:

[0096] [ka]

[0097] Examples of diamine components that provide repeating units of general formula (I) in which Y1 is a divalent group having an alicyclic structure include 1,4-diaminocyclohexane, 1,4-diamino-2-methylcyclohexane, 1,4-diamino-2-ethylcyclohexane, 1,4-diamino-2-n-propylcyclohexane, 1,4-diamino-2-isopropylcyclohexane, 1,4-diamino-2-n-butylcyclohexane, 1,4-diamino-2-isobutylcyclohexane, 1,4-diamino-2-sec-butylcyclohexane, 1,4-diamino-2-tert-butylcyclohexane, 1,2-diaminocyclohexane, 1,3-diaminocyclobutane, 1, Examples of the diamine component include 4-bis(aminomethyl)cyclohexane, 1,3-bis(aminomethyl)cyclohexane, diaminobicycloheptane, diaminomethylbicycloheptane, diaminooxybicycloheptane, diaminomethyloxybicycloheptane, isophoronediamine, diaminotricyclodecane, diaminomethyltricyclodecane, bis(aminocyclohexyl)methane, bis(aminocyclohexyl)isopropylidene, 6,6'-bis(3-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane, and 6,6'-bis(4-aminophenoxy)-3,3,3',3'-tetramethyl-1,1'-spirobiindane. The diamine component may be used alone or in combination of multiple types.

[0098] As the tetracarboxylic acid component and diamine component that give the repeating unit represented by the general formula (I), any of aliphatic tetracarboxylic acids other than alicyclic (particularly dianhydrides) and / or aliphatic diamines can be used, and the content thereof is preferably less than 30 mol%, more preferably less than 20 mol%, and even more preferably less than 10 mol% (including 0%) relative to 100 mol% in total of the tetracarboxylic acid component and the diamine component.

[0099] By incorporating a structure represented by formula (4) as "other Y1" and a diamine compound such as p-phenylenediamine, 3,3'-bis(trifluoromethyl)benzidine, m-tolidine, 4,4'-bis(4-aminophenoxy)biphenyl, diaminodiphenyl ether, etc. as a specific compound, the light transmittance and other physical properties of the resulting polyimide film may be improved. In addition, by incorporating a structure represented by formula (3B) as "other Y1" and a diamine compound such as 9,9-bis(4-aminophenyl)fluorene, etc. as a specific compound, the Tg may be improved and the phase difference (retardation) in the film thickness direction may be reduced.

[0100] The polyimide precursor can be produced from the above tetracarboxylic acid component and diamine component. The polyimide precursor used in the present invention (a polyimide precursor containing at least one repeating unit represented by the above formula (I)) can be produced according to the chemical structures of R1 and R2. 1) Polyamic acid (R1 and R2 are hydrogen), 2) Polyamic acid ester (at least a part of R1 and R2 is an alkyl group), 3) 4) Polyamic acid silyl ester (at least a part of R1 and R2 is an alkylsilyl group), The polyimide precursors can be easily produced according to the following production methods for each of the above categories. However, the production methods for the polyimide precursors used in the present invention are not limited to the following production methods.

[0101] 1) Polyamic acid The polyimide precursor can be suitably obtained as a polyimide precursor solution by reacting a tetracarboxylic dianhydride as a tetracarboxylic acid component and a diamine component in approximately equal moles in a solvent, preferably at a molar ratio of the diamine component to the tetracarboxylic acid component [the number of moles of the diamine component / the number of moles of the tetracarboxylic acid component] of 0.90 to 1.10, more preferably 0.95 to 1.05, while suppressing imidization at a relatively low temperature, for example, 120° C. or lower.

[0102] Although not limited thereto, more specifically, a polyimide precursor is obtained by dissolving a diamine in an organic solvent or water, gradually adding a tetracarboxylic dianhydride to the solution while stirring, and stirring the solution at 0 to 120°C, preferably 5 to 80°C, for 1 to 72 hours. When reacting at 80°C or higher, the molecular weight varies depending on the temperature history during polymerization, and imidization proceeds due to heat, so that the polyimide precursor may not be stably produced. The order of addition of the diamine and the tetracarboxylic dianhydride in the above production method is preferred because the molecular weight of the polyimide precursor is easily increased. In addition, the order of addition of the diamine and the tetracarboxylic dianhydride in the above production method can be reversed, which is preferred because it reduces precipitates. When water is used as a solvent, it is preferred to add an imidazole such as 1,2-dimethylimidazole or a base such as triethylamine, preferably in an amount of 0.8 times or more equivalent to the carboxyl group of the polyamic acid (polyimide precursor) to be produced.

[0103] 2) Polyamic acid ester Tetracarboxylic dianhydride is reacted with any alcohol to obtain a diester dicarboxylic acid, which is then reacted with a chlorinating agent (such as thionyl chloride or oxalyl chloride) to obtain a diester dicarboxylic acid chloride. The diester dicarboxylic acid chloride and diamine are stirred at -20 to 120°C, preferably at -5 to 80°C, for 1 to 72 hours to obtain a polyimide precursor. When reacting at 80°C or higher, the molecular weight varies depending on the temperature history during polymerization, and imidization proceeds due to heat, so that the polyimide precursor may not be stably produced. In addition, a polyimide precursor can be easily obtained by dehydrating and condensing a diester dicarboxylic acid and a diamine using a phosphorus-based condensing agent or a carbodiimide condensing agent.

[0104] The polyimide precursor obtained by this method is stable, and therefore can be purified by reprecipitation or other methods by adding a solvent such as water or alcohol.

[0105] 3) Polyamic acid silyl ester (indirect method) A diamine is reacted with a silylation agent in advance to obtain a silylated diamine. If necessary, the silylated diamine is purified by distillation or the like. The silylated diamine is dissolved in a dehydrated solvent, and a tetracarboxylic dianhydride is gradually added while stirring. The mixture is stirred at 0 to 120°C, preferably 5 to 80°C, for 1 to 72 hours to obtain a polyimide precursor. If the reaction is carried out at 80°C or higher, the molecular weight varies depending on the temperature history during polymerization, and imidization proceeds due to heat, so that the polyimide precursor may not be stably produced.

[0106] 4) Polyamic acid silyl ester (direct method) A polyimide precursor is obtained by mixing the polyamic acid solution obtained by method 1) with a silylating agent and stirring for 1 to 72 hours at 0 to 120° C., preferably 5 to 80° C. If the reaction is carried out at 80° C. or higher, the molecular weight varies depending on the temperature history during polymerization, and imidization proceeds due to heat, so that the polyimide precursor may not be stably produced.

[0107] In the methods 3) and 4), it is preferable to use a silylating agent that does not contain chlorine, since there is no need to purify the silylated polyamic acid or the resulting polyimide. Examples of silylating agents that do not contain chlorine atoms include N,O-bis(trimethylsilyl)trifluoroacetamide, N,O-bis(trimethylsilyl)acetamide, and hexamethyldisilazane. N,O-bis(trimethylsilyl)acetamide and hexamethyldisilazane are particularly preferred because they do not contain fluorine atoms and are low cost.

[0108] In the silylation reaction of the diamine in method 3), an amine catalyst such as pyridine, piperidine, or triethylamine can be used to accelerate the reaction. This catalyst can be used as it is as a polymerization catalyst for the polyimide precursor.

[0109] The solvent used in preparing the polyimide precursor is preferably water or an aprotic solvent such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, or dimethyl sulfoxide, and is not particularly limited in structure since any type of solvent can be used without problems as long as it dissolves the raw material monomer components and the resulting polyimide precursor. As the solvent, water, amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and N-ethyl-2-pyrrolidone, cyclic ester solvents such as γ-butyrolactone, γ-valerolactone, δ-valerolactone, γ-caprolactone, ε-caprolactone, and α-methyl-γ-butyrolactone, carbonate solvents such as ethylene carbonate and propylene carbonate, glycol solvents such as triethylene glycol, phenol solvents such as m-cresol, p-cresol, 3-chlorophenol, and 4-chlorophenol, acetophenone, 1,3-dimethyl-2-imidazolidinone, sulfolane, and dimethyl sulfoxide are preferably used. In addition, other common organic solvents, such as phenol, o-cresol, butyl acetate, ethyl acetate, isobutyl acetate, propylene glycol methyl acetate, ethyl cellosolve, butyl cellosolve, 2-methyl cellosolve acetate, ethyl cellosolve acetate, butyl cellosolve acetate, tetrahydrofuran, dimethoxyethane, diethoxyethane, dibutyl ether, diethylene glycol dimethyl ether, methyl isobutyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, methyl ethyl ketone, acetone, butanol, ethanol, xylene, toluene, chlorobenzene, turpentine, mineral spirits, petroleum naphtha solvents, etc., can also be used. A combination of multiple solvents can also be used.

[0110] In the production of the polyimide precursor, although there are no particular limitations, the monomer and the solvent are charged at a concentration such that the solids concentration of the polyimide precursor (polyimide equivalent mass concentration) is, for example, 5 to 45 mass % and the reaction is carried out.

[0111] The logarithmic viscosity of the polyimide precursor is not particularly limited, but it is preferable that the logarithmic viscosity in an N-methyl-2-pyrrolidone solution having a concentration of 0.5 g / dL at 30° C. is 0.2 dL / g or more, more preferably 0.3 dL / g or more, and particularly preferably 0.4 dL / g or more. When the logarithmic viscosity is 0.2 dL / g or more, the molecular weight of the polyimide precursor is high, and the mechanical strength and heat resistance of the obtained polyimide are excellent.

[0112] <Imidazole compounds> The polyimide precursor composition contains at least one kind of imidazole compound. The imidazole compound is not particularly limited as long as it is a compound having an imidazole skeleton, and examples thereof include 1,2-dimethylimidazole, 1-methylimidazole, 2-methylimidazole, 2-phenylimidazole, imidazole, and benzimidazole. From the viewpoint of storage stability of the polyimide precursor composition, 2-phenylimidazole and benzimidazole are preferred. The imidazole compound may be used in combination with a plurality of compounds.

[0113] The content of the imidazole compound in the polyimide precursor composition can be appropriately selected in consideration of the balance between the effect of addition and the stability of the polyimide precursor composition. The amount of the imidazole compound is preferably more than 0.01 moles to 2 moles or less per mole of the repeating unit of the polyimide precursor. The addition of the imidazole compound is effective in improving the light transmittance, the linear thermal expansion coefficient and / or the mechanical properties, while if the content of the imidazole compound is too high, the storage stability of the polyimide precursor composition may be deteriorated.

[0114] The content of the imidazole compound is more preferably 0.02 mol or more, even more preferably 0.025 mol or more, even more preferably 0.05 mol or more, and more preferably 1.5 mol or less, even more preferably 1.2 mol or less, even more preferably 1.0 mol or less, even more preferably 0.8 mol or less, and most preferably 0.6 mol or less, relative to 1 mol of the repeating unit.

[0115] In addition, in the course of intensive research by the present inventors, when a film was formed from a solution containing a polyimide precursor having a repeating unit represented by general formula (I) and not containing an imidazole compound, it was found that the film had a large haze value and was turbid, making it unsuitable for use as an optical substrate for displays, etc. When a film was produced from the polyimide precursor composition of the present invention containing an imidazole compound, it had a small haze value and was excellent in transparency (no turbidity), making it suitable for use as an optical electronic device substrate for displays, etc., among flexible electronic devices.

[0116] In this respect, the present application also discloses a method for improving the haze value of a polyimide film obtained from a polyimide precursor solution containing a polyimide precursor whose repeating unit is represented by the above general formula (I) and a solvent, the method comprising the step of adding at least one imidazole compound in an amount of more than 0.01 mol and not more than 2 mol per mol of the repeating unit of the polyimide precursor.

[0117] Furthermore, as a finding obtained during intensive research by the present inventor, it was found that a solution of a polyimide precursor having a repeating unit represented by general formula (I) (not containing an imidazole compound) has poor storage stability and its fluidity decreases during storage. In contrast, the polyimide precursor composition of the present invention to which an imidazole compound is added has excellent storage stability, and is particularly advantageous in terms of transportation, distribution and inventory storage. When an imidazole compound is not contained, a composition in which the storage stability is likely to decrease is one in which the polyimide equivalent mass concentration (solid concentration) is high. This effect can be clearly confirmed, particularly when applied to a solution having a solid concentration of 10 mass% or more, preferably 15 mass% or more. In addition, a composition in which this effect is particularly effective is a composition in which the proportion of formula (1-1) in X1 of general formula (I) is large, and / or a composition in which the proportion of formula (D-1) and / or (D-2) in Y1 is large. In particular, a significant effect is observed in a composition in which the proportion of formula (1-1) in X1 is 80% or more, preferably 90% or more, and the proportion of formula (D-1) and / or (D-2) in Y1 is 80% or more, preferably 90% or more.

[0118] From this viewpoint, the present application also discloses a method for improving the storage stability of a polyimide precursor solution that contains a polyimide precursor whose repeating unit is represented by the above general formula (I) and a solvent and has poor storage stability, by including at least one imidazole compound in an amount of more than 0.01 mol and 2 mol or less per mol of the repeating unit of the polyimide precursor.

[0119] <Formulation of polyimide precursor composition> The polyimide precursor composition used in the present invention contains at least one polyimide precursor, at least one of the above-mentioned imidazole compounds, and a solvent.

[0120] As the solvent, the above-mentioned solvents described as the solvent used when preparing the polyimide precursor can be used. Usually, the solvent used when preparing the polyimide precursor can be used as it is, that is, as the polyimide precursor solution, but it may be used after dilution or concentration as necessary. The imidazole compound is dissolved and exists in the polyimide precursor composition. The concentration of the polyimide precursor is not particularly limited, but is usually 5 to 45 mass% in terms of polyimide equivalent mass concentration (solid content concentration). Here, the polyimide equivalent mass is the mass when all the repeating units are completely imidized.

[0121] The viscosity (rotational viscosity) of the polyimide precursor composition of the present invention is not particularly limited, but is measured using an E-type rotational viscometer at a temperature of 25° C. and a shear rate of 20 sec -1 The rotational viscosity measured by is preferably 0.01 to 1000 Pa·sec, more preferably 0.1 to 100 Pa·sec. Thixotropy can also be imparted as necessary. With a viscosity in the above range, the composition is easy to handle when coating or forming a film, and repellency is suppressed, resulting in excellent leveling properties, making it possible to obtain a good coating film.

[0122] The polyimide precursor composition of the present invention may, if necessary, ,acid It may contain antioxidants, UV absorbers, fillers (inorganic particles such as silica), dyes, pigments, coupling agents such as silane coupling agents, primers, flame retardants, defoamers, leveling agents, rheology control agents (flow aids), etc.

[0123] The polyimide precursor composition can be prepared by adding an imidazole compound or a solution of an imidazole compound to the polyimide precursor solution obtained by the above-mentioned method and mixing them. The tetracarboxylic acid component and the diamine component may be reacted in the presence of the imidazole compound.

[0124] <<Uses of polyimide precursor composition and film properties>> The polyimide precursor composition of the present invention can be used to produce polyimide and polyimide film. The production method is not particularly limited, and any known imidization method can be suitably applied. The form of the obtained polyimide can be suitably exemplified as a film, a laminate of a polyimide film and another substrate, a coating film, a powder, beads, a molded product, a foam, etc.

[0125] Although it depends on the application, the thickness of the polyimide film is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 5 μm or more, and for example, 250 μm or less, preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less.

[0126] The polyimide film of the present invention is excellent in light transparency, mechanical properties, thermal properties, and heat resistance. Here, "heat resistance" refers to phase change (indicated by glass transition temperature, melting temperature, etc.) and thermal decomposition (indicated by weight loss). Since the two are different phenomena, there is no direct relationship between them. The polyimide and polyimide film of the present invention are excellent in both glass transition temperature (Tg) and thermal decomposition resistance, and are particularly excellent in thermal decomposition resistance compared to conventional polyimides.

[0127] The thermal decomposition resistance of a polyimide film (or a polyimide constituting the polyimide film) can be evaluated based on the properties required for the manufacturing process of flexible electronic devices and the like. For example, it can be evaluated by the 5% weight loss temperature of the polyimide film. The 5% weight loss temperature is preferably 515°C or higher, more preferably 517°C or higher, and even more preferably 520°C or higher. If the 5% weight loss temperature is in the "preferred range", it is recognized as a material with clearly improved thermal decomposition resistance, if it is in the "even more preferred range", it is recognized as a material with significantly improved thermal decomposition resistance, and if it is in the "even more preferred range", it is recognized as a material with significantly improved thermal decomposition resistance. Even if the 5% weight loss temperature is improved by just 2 or 3°C, the process margin is improved, which is advantageous for the stable manufacturing of flexible electronic devices.

[0128] In addition, when contamination due to outgassing is a particular problem, it is also preferable to evaluate the thermal decomposition resistance of the polyimide film (or the polyimide constituting the polyimide film) based on stricter criteria such as the 0.5% weight loss temperature of the polyimide film. The 0.5% weight loss temperature is preferably 482°C or higher, more preferably 484°C or higher, and even more preferably 489°C or higher.

[0129] The thermal decomposition resistance of a polyimide film (or the polyimide constituting the polyimide film) can also be evaluated by the weight loss rate when the film is held at a certain high temperature for a certain period of time. For example, the film can be held in an inert atmosphere at a suitable temperature selected from the range of 400°C to 420°C for a suitable period of time selected from 2 to 6 hours, and the weight loss rate can be calculated.

[0130] The polyimide film of the present invention has an extremely low coefficient of linear thermal expansion. In one embodiment of the present invention, the coefficient of linear thermal expansion (CTE) of the polyimide film from 150° C. to 250° C., measured on a film having a thickness of 10 μm, is preferably 20 ppm / K or less, more preferably less than 20 ppm, even more preferably 15 ppm / K or less, even more preferably 11 ppm / K or less, and most preferably 10 ppm / K or less.

[0131] In one embodiment of the present invention, the glass transition temperature (Tg) of the polyimide film (or the polyimide constituting the polyimide film) is preferably 390°C or higher, more preferably 400°C or higher, even more preferably 410°C or higher, even more preferably 415°C or higher, even more preferably 420°C or higher, even more preferably 425°C or higher, even more preferably 430°C or higher, even more preferably 435°C or higher, and most preferably 440°C or higher.

[0132] In one embodiment of the present invention, when measured on a film having a thickness of 10 μm, the 400 nm light transmittance of the polyimide film is preferably 70% or more, more preferably 73% or more, more preferably 75% or more, and even more preferably 80% or more. When measured on a film having a thickness of 10 μm, the yellowness index (YI) of the polyimide film is preferably 6.0 or less, more preferably 5.0 or less, even more preferably 4.0 or less, even more preferably 3.2 or less, even more preferably 3.0 or less, and most preferably 2.7 or less. Usually, 0 or more is preferable.

[0133] In one embodiment of the present invention, the haze value of the polyimide film is preferably less than 1.0%, more preferably 0.8% or less, and even more preferably 0.7% or less, when measured on a film having a thickness of 10 μm. For example, if the haze value exceeds 1%, the film becomes cloudy to the naked eye, making it unsuitable for optical applications.

[0134] Here, optical properties will be described. The 400 nm light transmittance can be used as an index for estimating and evaluating the degree of yellowness and transparency of a film. For example, wholly aromatic polyimide films such as Upilex-S (Upilex is a registered trademark of Ube Industries) and Kapton (registered trademark) are generally colored yellowish brown. This is because they absorb wavelengths of 380 nm to 500 nm (violet to blue light) in the visible light range. When a colorless, highly transparent polyimide film is desired as in the present application, the higher the 400 nm light transmittance, the more preferable it is.

[0135] Yellowness index (YI) is calculated from a color system (e.g., tristimulus values ​​of X, Y, and Z) converted from the transmitted wavelength (transmittance), with ideal white having a yellowness index of 0, and a hue shift from white in the yellow direction being a positive value, and a hue shift in the blue direction being a negative value. Therefore, for a polyimide film, the closer the yellowness index value is to 0, the better. Note that yellowness index is an index showing the relative relationship of tristimulus values, so that even if the 400 nm light transmittance is low, if the transmittances in other visible light regions are similarly low, the yellowness index will not be high, and therefore it is not a value that indicates the transparency of the film.

[0136] Haze (cloudiness) is an index used to evaluate the degree of "cloudiness, turbidity" of a film, and indicates the ratio of transmitted scattered light to the total light transmitted through the film (transmitted scattered light / total transmitted light x 100). A receiver that matches the standard visual curve is used. The smaller the haze value of a film, the better, and when the haze value exceeds 1%, the cloudiness can be recognized visually.

[0137] In this application, the total light transmittance (or total light transmittance) represents the average transmittance in the entire visible light region (380 nm to 780 nm). On the other hand, in haze measurement, the transmittance (ratio) of light rays including all parallel and diffuse components transmitted through the film (sample) is also called "total light transmittance", so it may be confused. Haze measurement uses a D65 light source (average daylight) and a light receiver matched to the standard spectral luminous curve V(λ) (equal to the color matching function y(λ)), so the weighting of the region with a peak near 555 nm is large, and the transmittance near a wavelength of 400 nm hardly contributes to the "total light transmittance". Therefore, it should be noted that the "total light transmittance" measured with a haze meter does not indicate the transmittance of the entire visible light region, unlike the total light transmittance (or total light transmittance) in this application.

[0138] Furthermore, in one embodiment of the present invention, the breaking elongation of the polyimide film is preferably 4% or more, more preferably 7% or more, when measured on a film having a thickness of 10 μm.

[0139] In another preferred embodiment of the present invention, the breaking strength of the polyimide film is preferably 150 MPa or more, more preferably 170 MPa or more, even more preferably 180 MPa or more, even more preferably 200 MPa or more, and even more preferably 210 MPa or more. The breaking strength may be, for example, a value obtained from a film having a thickness of about 5 to 100 μm.

[0140] It is particularly preferable that the polyimide film has the above-mentioned preferable properties simultaneously.

[0141] The polyimide film can be produced by a known method. A typical method is to cast a polyimide precursor composition onto a substrate, and then heat imidize the composition on the substrate to obtain a polyimide film. This method will be described later in relation to the production of a polyimide film / substrate laminate. Alternatively, the polyimide precursor composition can be cast onto a substrate, heated and dried to produce a self-supporting film, and then the self-supporting film can be peeled off from the substrate, and the film can be held, for example, by a tenter and heat imidized in a state in which degassing is possible from both sides of the film to obtain a polyimide film.

[0142] <<Manufacturing of polyimide film / substrate laminates and flexible electronic devices>> A polyimide film / substrate laminate can be produced using the polyimide precursor composition of the present invention. The polyimide film / substrate laminate can be produced by (a) applying the polyimide precursor composition onto a substrate, and (b) heat-treating the polyimide precursor on the substrate to produce a laminate (polyimide film / substrate laminate) in which a polyimide film is laminated on the substrate. The method for producing a flexible electronic device of the present invention uses the polyimide film / substrate laminate produced in the steps (a) and (b) and includes further steps, namely (c) forming at least one layer selected from a conductive layer and a semiconductor layer on the polyimide film of the laminate, and (d) peeling the substrate from the polyimide film.

[0143] First, in step (a), a polyimide precursor composition is cast onto a substrate, and a polyimide film is formed by imidization and removal of the solvent through a heat treatment, thereby obtaining a laminate of the substrate and the polyimide film (polyimide film / substrate laminate).

[0144] As the substrate, a heat-resistant material is used, for example, a plate- or sheet-shaped substrate such as a ceramic material (glass, alumina, etc.), a metal material (iron, stainless steel, copper, aluminum, etc.), a semiconductor material (silicon, compound semiconductor, etc.), or a film- or sheet-shaped substrate such as a heat-resistant plastic material (polyimide, etc.). In general, a flat and smooth plate-shaped substrate is preferred, and generally, glass substrates such as soda-lime glass, borosilicate glass, alkali-free glass, sapphire glass, etc., semiconductor (including compound semiconductor) substrates such as silicon, GaAs, InP, GaN, etc., and metal substrates such as iron, stainless steel, copper, aluminum, etc. are used.

[0145] As the substrate, a glass substrate is particularly preferred. Flat, smooth, and large-area glass substrates have been developed and are easily available. The thickness of a plate-like substrate such as a glass substrate is not limited, but from the viewpoint of ease of handling, it is, for example, 20 μm to 4 mm, and preferably 100 μm to 2 mm. The size of the plate-like substrate is not particularly limited, but one side (the long side in the case of a rectangle) is, for example, about 100 mm to about 4000 mm, preferably about 200 mm to about 3000 mm, and more preferably about 300 mm to about 2500 mm.

[0146] The substrates such as glass substrates may have an inorganic thin film (for example, a silicon oxide film) or a resin thin film formed on the surface.

[0147] The method for casting the polyimide precursor composition onto the substrate is not particularly limited, and examples thereof include conventionally known methods such as slit coating, die coating, blade coating, spray coating, inkjet coating, nozzle coating, spin coating, screen printing, bar coater, and electrodeposition.

[0148] In step (b), the polyimide precursor composition is heat-treated on the substrate to convert it into a polyimide film, thereby obtaining a polyimide film / substrate laminate. The heat treatment conditions are not particularly limited, but for example, after drying at a temperature range of 50°C to 150°C, the maximum heating temperature is, for example, 150°C to 600°C, preferably 200°C to 550°C, more preferably 250°C to 500°C.

[0149] The thickness of the polyimide film is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 5 μm or more. If the thickness is less than 1 μm, the polyimide film cannot maintain sufficient mechanical strength, and may be destroyed due to inability to withstand stress when used, for example, as a flexible electronic device substrate. The thickness of the polyimide film is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 20 μm or less. If the thickness of the polyimide film is too thick, it may be difficult to thin the flexible device. In order to make the polyimide film thinner while maintaining sufficient resistance as a flexible device, the thickness of the polyimide film is preferably 2 to 50 μm.

[0150] In the present invention, it is preferable that the polyimide film / substrate laminate has little warpage. Details of the measurement are described in Japanese Patent No. 6798633. In one embodiment, when the properties of the polyimide film are evaluated based on the residual stress between the polyimide film and the silicon substrate in a polyimide film / silicon substrate (wafer) laminate, the residual stress is preferably less than 27 MPa. However, the polyimide film is assumed to be kept at 23°C in a dry state.

[0151] The polyimide film in the polyimide film / substrate laminate may have a second layer such as a resin film or an inorganic film on the surface. That is, after forming a polyimide film on a substrate, a second layer may be laminated to form a flexible electronic device substrate. It is preferable to have at least an inorganic film, and it is particularly preferable to have one that functions as a barrier layer against water vapor, oxygen (air), etc. As the water vapor barrier layer, for example, silicon nitride (SiNx ), silicon oxide (SiO x ), silicon oxynitride (SiO x N y Examples of the inorganic film include inorganic films containing an inorganic material selected from the group consisting of metal oxides, metal nitrides, and metal oxynitrides, such as aluminum oxide (Al2O3), titanium oxide (TiO2), and zirconium oxide (ZrO2). Generally, known methods for forming these thin films include physical vapor deposition methods such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition methods (chemical vapor deposition methods) such as plasma CVD and catalytic chemical vapor deposition (Cat-CVD). This second layer can also be a multi-layer structure.

[0152] When the second layer is a multi-layer structure, it is also possible to combine a resin film and an inorganic film. For example, a three-layer structure of a barrier layer / polyimide layer / barrier layer may be formed on the polyimide film in a polyimide film / substrate laminate.

[0153] In step (c), at least one layer selected from a conductive layer and a semiconductor layer is formed on a polyimide film (including a polyimide film having a second layer such as an inorganic film laminated on its surface) using the polyimide / substrate laminate obtained in step (b). These layers may be formed directly on the polyimide film (including a polyimide film having a second layer laminated on its surface) or may be formed indirectly on top of other layers required for the device.

[0154] The conductive layer and / or the semiconductor layer are selected from appropriate conductive layers and (inorganic, organic) semiconductor layers according to the elements and circuits required for the target electronic device. When at least one of the conductive layer and the semiconductor layer is formed in the step (c) of the present invention, it is also preferable to form at least one of the conductive layer and the semiconductor layer on a polyimide film having an inorganic film formed thereon.

[0155] The conductive layer and the semiconductor layer include both those formed on the entire surface of the polyimide film and those formed on a part of the polyimide film. In the present invention, the process may proceed to the step (d) immediately after the step (c), or the process may proceed to the step (d) after forming at least one layer selected from the conductive layer and the semiconductor layer in the step (c) and then forming a device structure.

[0156] When manufacturing a TFT liquid crystal display device as a flexible device, for example, metal wiring, amorphous silicon or polysilicon TFT, and transparent pixel electrodes are formed on a polyimide film having an inorganic film formed on the entire surface as necessary. The TFT includes, for example, a gate metal layer, a semiconductor layer such as an amorphous silicon film, a gate insulating layer, and wiring connected to the pixel electrode. On top of this, a structure required for the liquid crystal display can be further formed by a known method. Also, a transparent electrode and a color filter may be formed on the polyimide film.

[0157] When an organic EL display is produced, for example, a polyimide film having an inorganic film formed over the entire surface as required may be coated with a transparent electrode, a light-emitting layer, a hole transport layer, an electron transport layer, and the like, and further with a TFT as required.

[0158] Since the polyimide film preferred in the present invention is excellent in various properties such as heat resistance and toughness, there are no particular limitations on the method for forming circuits, elements and other structures required for devices.

[0159] Next, in step (d), the substrate and the polyimide film are peeled off by a mechanical peeling method in which the substrate is physically peeled off by applying an external force, or by a so-called laser peeling method in which the substrate is peeled off by irradiating the substrate with a laser beam.

[0160] After the base material is peeled off, the (semi-)finished product is made of the polyimide film as a substrate, and the structures or parts required for the device are further formed or incorporated into the product to complete the device.

[0161] As a different method for producing a flexible electronic device, after producing a polyimide film / substrate laminate by the above-mentioned step (b), the polyimide film can be peeled off, and at least one layer selected from a conductive layer and a semiconductor layer and a necessary structure can be formed on the polyimide film as in the above-mentioned step (c), to produce a (semi-)finished product having the polyimide film as a substrate. EXAMPLES

[0162] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0163] In the following examples, evaluations were carried out in the following manner.

[0164] <Evaluation of polyimide film> [400nm light transmittance, total light transmittance] The light transmittance of a polyimide film having a thickness of about 10 μm was measured at 400 nm using a UV-Visible Spectrophotometer / V-650DS (manufactured by JASCO Corporation). The total light transmittance is the average of the transmittance from 380 nm to 780 nm. [Yellowness (YI)] The YI of the polyimide film was measured using a UV-Visible Spectrophotometer / V-650DS (manufactured by JASCO Corporation) in accordance with the standard of ASTEM E313. The light source was D65 and the viewing angle was 2°.

[0165] [Elastic modulus, elongation at break, strength at break] A polyimide film with a thickness of approximately 10 μm was punched into a dumbbell shape according to the IEC 450 standard to prepare a test piece, and the initial elastic modulus, breaking elongation, and breaking strength were measured using an ORIENTEC TENSILON with a chuck length of 30 mm and a tensile speed of 2 mm / min.

[0166] [Coefficient of linear thermal expansion (CTE), glass transition temperature (Tg)] A polyimide film with a thickness of approximately 10 μm was cut into a strip with a width of 4 mm to prepare a test piece, and the test piece was heated to 500°C using a TMA / SS6100 (manufactured by SII Nano Technology Co., Ltd.) with a chuck length of 15 mm, a load of 2 g, and a heating rate of 20°C / min. The linear thermal expansion coefficient from 150°C to 250°C was calculated from the obtained TMA curve. The glass transition temperature (Tg) was also calculated from the inflection point.

[0167] [5% weight loss temperature, 0.5% weight loss temperature] A polyimide film with a thickness of approximately 10 μm was used as a test piece, and the temperature was raised from 25°C to 600°C at a rate of 10°C / min in a nitrogen stream using a calorimeter measuring device (Q5000IR) manufactured by TA Instruments. From the obtained weight curve, the 5% weight loss temperature and the 0.5% weight loss temperature were calculated, with the weight at 150°C being 100%.

[0168] [Haze] The haze of a polyimide film having a thickness of about 10 μm and a size of 5 cm square was measured using a turbidity meter / NDH2000 (manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with the JIS K7136 standard.

[0169] [Fluidity and storage stability of polyimide precursor composition and polyimide precursor solution] About 20 mL of the polyimide precursor composition was placed in a 50 mL sample bottle, the atmosphere was replaced with nitrogen, and the bottle was sealed. The bottle was stored at 23° C., and the fluidity was confirmed after 10 days and 30 days. ○ A sealed container in which the solution moves when tilted by 90 degrees or more is If the solution does not move when the sealed container is tilted by 90 degrees or more, then it is considered an × It was rated as follows:

[0170] <Ingredients> The abbreviations, purities, etc. of the raw materials used in each of the following examples are as follows.

[0171] [Diamine component] DABAN: 4,4'-diaminobenzanilide PPD: p-phenylenediamine BAPB: 4,4'-bis(4-aminophenoxy)biphenyl TFMB: 2,2'-bis(trifluoromethyl)benzidine m-TD: m-tolidine 4,4-ODA: 4,4'-diaminodiphenyl ether

[0172] [Tetracarboxylic acid component] BNBDA: 2,2'-binorbornane-5,5',6,6'-tetracarboxylic dianhydride CpODA: Norbornane-2-spiro-α-cyclopentanone-α'-spiro-2”-norbornane-5,5”,6,6”-tetracarboxylic dianhydride PMDA-H: Cyclohexanetetracarboxylic dianhydride

[0173] [Imidazole compounds] 2-Pz: 2-phenylimidazole 1,2-DMz: 1,2-dimethylimidazole z: Imidazole Bz: Benzimidazole 2-Mz: 2-methylimidazole

[0174] [solvent] NMP: N-methyl-2-pyrrolidone

[0175] Table 1-1 shows the structural formulae of the tetracarboxylic acid component and the diamine component, and Table 1-2 shows the structural formulae of the imidazole compound.

[0176] [Table 1-1]

[0177] [Table 1-2]

[0178] <Example 1> [Preparation of polyimide precursor composition] 2.27g (0.010 mol) of DABAN was placed in a reaction vessel purged with nitrogen gas, and 32.11g of N-methyl-2-pyrrolidone was added in an amount such that the total mass of the charged monomers (total of diamine components and carboxylic acid components) was 16% by mass, and the mixture was stirred at 50°C for 1 hour. 3.34g (0.010 mol) of BNBDA was gradually added to this solution. The mixture was stirred at 70°C for 4 hours to obtain a uniform and viscous polyimide precursor solution.

[0179] 2-phenylimidazole as an imidazole compound was dissolved in 4 times the mass of N-methyl-2-pyrrolidone to obtain a uniform solution with a solid concentration of 20 mass% of 2-phenylimidazole. The imidazole compound solution was mixed with the polyimide precursor solution synthesized above so that the amount of the imidazole compound was 0.5 moles per mole of the repeating unit of the polyimide precursor, and the mixture was stirred at room temperature for 3 hours to obtain a uniform and viscous polyimide precursor composition.

[0180] [Production of polyimide film] A 6-inch Corning Eagle-XG (registered trademark) (500 μm thick) was used as the glass substrate. The polyimide precursor composition was applied onto the glass substrate by a spin coater, and the composition was heated from room temperature to 440° C. on the glass substrate in a nitrogen atmosphere (oxygen concentration 200 ppm or less) to thermally imidize the composition, thereby obtaining a polyimide film / substrate laminate. The laminate was immersed in water at 40° C. (for example, in the range of 20° C. to 100° C.) to peel the polyimide film from the glass substrate, and after drying, the properties of the polyimide film were evaluated. The thickness of the polyimide film was about 10 μm. The evaluation results are shown in Table 2.

[0181] <Examples 2 to 26> A polyimide precursor composition was obtained in the same manner as in Example 1, except that the tetracarboxylic acid component, diamine component, and imidazole compound in Example 1 were changed to the compounds and amounts (molar ratios) shown in Tables 2 to 4, and the amic acid concentration was adjusted as shown in the tables. Thereafter, a polyimide film was produced in the same manner as in Example 1, and the film properties were evaluated.

[0182] <Comparative Examples 1 to 16> For the comparative examples, the tetracarboxylic acid component, diamine component, and imidazole compound were changed to the compounds and amounts (molar ratios) shown in Tables 5 and 6, and the amic acid concentration was adjusted as shown in the tables, but polyimide precursor compositions were obtained in the same manner as in Example 1. Thereafter, the film properties were evaluated in the same manner as in Example 1. Comparative examples with blanks in the additive column indicate that no imidazole compound was added.

[0183] <Film properties of Examples and Comparative Examples> Comparative Examples 1, 2, and 5 to 14 are precursor compositions to which no imidazole compound was added. The compositions of the corresponding Examples to which imidazole was added had improved haze values, 400 nm light transmittance, and linear thermal expansion coefficients, compared to these Comparative Examples.

[0184] Comparative Example 3 (CpODA / DABAN+imidazole compound) has the same composition as Example 1, etc., except that the tetracarboxylic acid component is changed to CpODA. The polyimide film obtained in Comparative Example 3 has excellent heat resistance in addition to optical properties such as transparency, but the polyimide film obtained in the examples of the present invention has optical properties equivalent to those of Comparative Example 3, while having a 0.5% weight loss temperature and a 5% weight loss temperature that exceed those of Comparative Example 3. Therefore, it was confirmed that the polyimide film obtained in the present invention has extremely excellent thermal decomposition resistance. In addition, the haze value of the polyimide film obtained in Comparative Example 16 is small at 0.3%, which shows that the composition of CpODA / DABAN does not have a haze problem regardless of whether or not an imidazole compound is added (Comparative Example 3 and Comparative Example 16). Therefore, it was confirmed that the haze problem is a problem specific to the composition mainly composed of BNBDA / DABAN.

[0185] Comparative Example 4 is a comparative example in which the amount of PMDA-H in the tetracarboxylic acid component was increased and the amount of BNBDA was reduced to 60% of the tetracarboxylic acid component in Example 16. A decrease in heat resistance was observed.

[0186] <Storage Stability of Polyimide Precursor Composition> The fluidity and storage stability tests were carried out on the polyimide precursor compositions of the Examples and Comparative Examples. The polyimide precursor compositions of the Examples maintained fluidity after both 10 and 30 days, and had excellent storage stability. On the other hand, the polyimide precursor solution of the Comparative Examples, to which imidazole was not added, had poor storage stability due to a decrease in fluidity during storage, as shown in Table 7. In addition, as in Comparative Example 15, the storage stability also decreases when the amount of the imidazole compound added is too large. In addition, Comparative Examples 3 and 16 are polyimide precursor compositions using CpODA as the tetracarboxylic acid component, but the storage stability was good even without the addition of the imidazole compound. This shows that storage stability is a particular problem when BNBDA is used.

[0187] [Table 2]

[0188] [Table 3]

[0189] [Table 4]

[0190] [Table 5]

[0191] [Table 6]

[0192] [Table 7] [Industrial Applicability]

[0193] The present invention can be suitably applied to the manufacture of flexible electronic devices, for example, display devices such as liquid crystal displays, organic EL displays, and electronic paper, and light-receiving devices such as solar cells and CMOS.

Claims

1. A polyimide precursor having a repeating unit represented by the following general formula (I): at least one imidazole compound contained in an amount ranging from more than 0.01 moles to 2 moles or less per mole of the repeating unit of the polyimide precursor; and solvent and wherein the polyimide precursor composition for thermal imidization does not contain a chemical imidizing agent. 【Chemistry 1】 (In general formula I, X 1 is a tetravalent aliphatic or aromatic group; Y 1 is a divalent aliphatic or aromatic group, R 1 and R 2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an alkylsilyl group having 3 to 9 carbon atoms, provided that X 1 70 mol % or more of the formula (1-1): 【Chemistry 2】 The structure represented by Y 1 70 mol % or more of the formula (D-1) and / or (D-2): 【Chemistry 3】 The structure is represented by the following formula:

2. 2. The polyimide precursor composition according to claim 1, wherein the imidazole compound is at least one selected from the group consisting of 1,2-dimethylimidazole, 1-methylimidazole, 2-methylimidazole, 2-phenylimidazole, imidazole and benzimidazole.

3. X 1 3. The polyimide precursor composition according to claim 1, wherein 90 mol % or more of the structure represented by formula (1-1) is

4. 4. The polyimide precursor composition according to claim 1, wherein a polyimide film obtained from the polyimide precursor composition has a 5% weight loss temperature of 515° C. or higher.

5. 5. The polyimide precursor composition according to claim 1, wherein a polyimide film obtained from the polyimide precursor composition has a linear thermal expansion coefficient of 20 ppm / K or less.

6. 6. The polyimide precursor composition according to claim 1, wherein a polyimide film having a thickness of 10 μm obtained from the polyimide precursor composition has a haze value of less than 1.0%.

7. 7. The polyimide precursor composition according to claim 1, which maintains fluidity when stored in a sealed state at 23° C. for 10 days.

8. A polyimide film obtained from the polyimide precursor composition according to any one of claims 1 to 7.

9. A polyimide film obtained from the polyimide precursor composition according to any one of claims 1 to 7; Substrate and A polyimide film / substrate laminate comprising:

10. The laminate according to claim 9 , wherein the substrate is a glass substrate.

11. (a) applying the polyimide precursor composition according to any one of claims 1 to 7 onto a substrate; and (b) a step of heat-treating the polyimide precursor on the substrate and laminating a polyimide film on the substrate; A method for producing a polyimide film / substrate laminate having the above structure.

12. The method according to claim 11 , wherein the substrate is a glass substrate.

13. (a) applying the polyimide precursor composition according to any one of claims 1 to 7 onto a substrate; (b) heat-treating the polyimide precursor on the substrate to produce a polyimide film / substrate laminate in which a polyimide film is laminated on the substrate; (c) forming at least one layer selected from a conductive layer and a semiconductor layer on the polyimide film of the laminate; and (d) peeling the polyimide film from the substrate A method for producing a flexible electronic device comprising the steps of:

14. The method according to claim 13, wherein the substrate is a glass substrate.

Citation Information

Patent Citations

  • Chemical ring closure of polyamic acid

    JP1985015426A

  • Liquid crystal display element

    JP1986267030A

  • Polyimide resin composition and polyimide varnish

    JP2018044180A

  • Polyimide, varnish and polyimide film

    JP2019137828A

  • Polyimide precursor, polyimide, and materials to be used in producing same