Organic solvent dispersion sol containing conductive stannic oxide particles and method for producing the same
Modified metal oxide particles, with stannic oxide cores coated by antimony or silicon oxide, are dispersed in organic solvents to create a stable, conductive, and transparent coating solution, addressing the limitations of existing technologies in producing effective conductive films.
Patent Information
- Application Number
- JP2024543885
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-04-03
- Filing Date
- 2024-03-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-03-26
AI Technical Summary
Existing technologies do not effectively produce a stable organic solvent-dispersed sol of conductive stannic oxide colloidal particles with high conductivity and refractive index, suitable for use as a transparent conductive coating agent.
The production of modified metal oxide particles, where stannic oxide serves as the core coated with antimony oxide or silicon oxide, dispersed in an organic solvent, utilizing specific particle size relationships and amine solubility to achieve stability and conductivity, with optional surface treatment using silane or phosphoric ester compounds.
The resulting sol provides high conductivity and transparency, enabling the formation of a coating film with specific resistance values, suitable for applications as a coating agent.
Smart Images

Figure 0007586384000001 
Figure 0007586384000002 
Figure 0007586384000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an organic solvent dispersion sol containing conductive stannic oxide colloidal particles (also called modified oxide particles), and a method for producing the same. [Background technology]
[0002] High-purity stannic oxide itself is insulating, but it is known that electronic conductivity appears when it is doped with indium or antimony. It is also known that stannic oxide exhibits electronic conductivity due to oxygen defects. It has been disclosed that these properties of stannic oxide particles can be used as a transparent conductive coating agent, for example, by applying it to a film to obtain a transparent conductive coating (see Patent Document 1).
[0003] In addition, a modified metal oxide sol has been disclosed in which an aqueous sol of stannic oxide containing a water-soluble amine and having an average particle size of 4 to 50 nm is subjected to hydrothermal treatment at a pressure of 0.1 to 40 MPa and a temperature of 100 to 350°C to produce an aqueous sol containing core particles, and then an aqueous sol of composite colloidal particles of diantimony pentoxide and silicon dioxide having an average particle size of 5 nm or less as coating particles, or an aqueous sol of colloidal particles of diantimony pentoxide containing a water-soluble amine and having an average particle size of 1 to 10 nm, is mixed therewith, and the surfaces of the core particles are coated with the coating particles (see Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 35-6616 [Patent Document 2] JP 2006-176392 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention provides an organic solvent sol containing modified metal oxide particles (iii) formed by coating at least one type of metal oxide particle (ii) selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide with stannic oxide (i) as a core, the modified metal oxide particles (iii) having high electrical conductivity and a high refractive index, and being stably dispersed in an organic solvent, the sol is capable of exhibiting transparency, particle refractive index, and coating film resistivity when applied to a substrate as a coating agent. [Means for solving the problem]
[0006] According to a first aspect, the present invention provides a modified metal oxide sol comprising modified metal oxide particles (iii) having an average primary particle size of 1 to 10 nm and coated with at least one kind of metal oxide particles (ii) selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide, the modified metal oxide particles being dispersed in an organic solvent, the average primary particle size satisfying the relationship of core particles (i)≧coated particles (ii), (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide) being 0.005 to 1.0, and the sol comprising an amine (a) having a water solubility of 0.1 g / L or more and an amine (b) having a water solubility of less than 0.1 g / L; As a second aspect, the modified metal oxide sol according to the first aspect, which has an average particle size of 5 to 100 nm as measured by a dynamic light scattering method; As a third aspect, the modified metal oxide sol according to the first aspect or the second aspect, in which the stannic oxide particles (i) serving as the core particles are hydrothermally treated stannic oxide particles; As a fourth aspect, the modified metal oxide sol according to any one of the first to third aspects, in which the stannic oxide particles (i) serving as the core particles have a crystallinity of 60% or more as measured by an X-ray diffraction method. As a fifth aspect, the modified metal oxide sol according to any one of the first to fourth aspects, in which the metal oxide particles (ii) as the coated particles are antimony oxide particles or composite particles of stannic oxide and silicon oxide in a mass ratio of 1:0.1 to 10.0. as a sixth aspect, the modified metal oxide sol according to any one of the first to fifth aspects, in which the amine (a) is contained in the modified metal oxide sol in an amount of 20 to 3,000 ppm; As a seventh aspect, the modified metal oxide sol according to any one of the first to sixth aspects, in which the amine (b) is contained in the modified metal oxide sol in an amount of 1,000 to 30,000 ppm. as an eighth aspect, the modified metal oxide sol according to any one of the first to seventh aspects, in which the amine (a) is a primary amine, a secondary amine, or an amine consisting of a combination thereof; as a ninth aspect, the modified metal oxide sol according to any one of the first to eighth aspects, in which the amine (b) is a tertiary amine; As a tenth aspect, the modified metal oxide sol according to any one of the first to ninth aspects, in which the amine (a) is at least one amine selected from the group consisting of n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, n-butylamine, isobutylamine, di-n-butylamine, and diisobutylamine. As an eleventh aspect, the modified metal oxide sol according to any one of the first to tenth aspects, in which the amine (b) is at least one amine selected from the group consisting of tri-n-butylamine, triisobutylamine, tri-n-pentylamine, and triisopentylamine. According to a twelfth aspect, the modified metal oxide sol according to any one of the first to eleventh aspects, in which a mass ratio of amine (b) / amine (a) is 3.0 to 200. As a thirteenth aspect, the modified metal oxide particles (iii) are represented by formulas (1) to (6): [ka] [ka] [In formula (1), R 1each represents an alkyl group, a halogenated alkyl group, an alkenyl group, an aryl group, or an organic group having a polyether group, an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a ureido group, or a cyano group, and is bonded to a silicon atom by a Si-C bond; R 2 each represents an alkoxy group, an acyloxy group, or a halogen group; a represents an integer of 1 to 3; In formula (2) and formula (3), R 3 and R 5 are each an alkyl group having 1 to 3 carbon atoms or an aryl group having 6 to 30 carbon atoms and bonded to a silicon atom by a Si-C bond, and R 4 and R 6 each represents an alkoxy group, an acyloxy group, or a halogen group; Y represents an alkylene group, an NH group, or an oxygen atom; b is an integer of 1 to 3; c is an integer of 0 or 1; and d is an integer of 1 to 3. In formulas (4) to (6), X1, X2, and X3 each represent an alkylene group having 2 to 20 carbon atoms, f, h, and j each represent an integer from 1 to 100, e, g, and i each represent an integer from 1 to 3, and Y1, Y2, and Y3 each represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, or a (meth)acrylic group. The modified metal oxide sol according to any one of claims 1 to 12, which is coated with at least one coating agent selected from the group consisting of: As a fourteenth aspect, the modified metal oxide sol according to any one of the first to thirteenth aspects, in which the organic solvent is an alcohol, a ketone, an ester, an ether, an amide, a hydrocarbon, a cyano group-containing solvent, a halogen-containing solvent, a sulfonyl group-containing solvent, a carboxyl group-containing solvent, or a mixed solvent thereof. as a fifteenth aspect, the modified metal oxide sol according to the fourteenth aspect, wherein the alcohol is a monohydric alcohol having 1 to 20 carbon atoms or a polyhydric alcohol having 1 to 20 carbon atoms; According to a sixteenth aspect, there is provided an antistatic composition comprising the modified metal oxide particles (iii) in the modified metal oxide sol according to any one of the first to fifteenth aspects. According to a seventeenth aspect, there is provided a composition for an electron transport material, the composition comprising the modified metal oxide particles (iii) in the modified metal oxide sol according to any one of the first to fifteenth aspects. As an 18th aspect, the method comprises the steps (A) to (D) below: Step (A): preparing an aqueous sol of stannic oxide particles (i) containing an amine (a) having a water solubility of 0.1 g / L or more and having an average primary particle size of 4 to 50 nm; Step (B): preparing an aqueous sol of at least one metal oxide particle (ii) having an average primary particle size of 1 to 10 nm and selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide, which contains an amine (a) having a water solubility of 0.1 g / L or more; Step (C): mixing the aqueous sol of stannic oxide obtained in step (A) and the aqueous sol of the modified metal oxide obtained in step (B) in a ratio of (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide) of 0.005 to 1.0 to produce modified metal oxide particles (iii) having an average primary particle size of 1 to 10 nm and coated with at least one kind of metal oxide particles (ii) selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide, using stannic oxide particles (i) having an average primary particle size of 4 to 50 nm as cores, and adding an amine (b) having a water solubility of less than 0.1 g / L; A method for producing an organic solvent sol of modified metal oxide particles according to any one of the first to fifteenth aspects, comprising: step (D): a step of solvent-substituting an aqueous medium of the aqueous sol of the modified metal oxide particles (iii) obtained in step (C) with an alcohol having 1 to 5 carbon atoms; As a 19th aspect, the method for producing an organic solvent sol of modified metal oxide particles (iii) according to the 18th aspect, in which the step (A) is a step (A-1) of adding an amine (a) having a water solubility of 0.1 g / L or more to an aqueous sol of stannic oxide particles (i) having an average primary particle size of 4 to 50 nm, and then subjecting the aqueous sol to a hydrothermal treatment at a pressure of 0.1 to 40 MPa and a temperature of 100 to 350° C. for 0.01 to 100 hours; As a twentieth aspect, after the step (D), a step (E) and / or a step (F): Step (E): adding at least one coating agent selected from the group consisting of formulas (1) to (6) to an organic solvent sol of the modified metal oxide particles (iii) to perform surface treatment of the modified metal oxide particles (iii); A method for producing an organic solvent sol of modified metal oxide particles according to the eighteenth or nineteenth aspect, further comprising the step of: (F) replacing the alcohol in the alcohol solvent sol having 1 to 5 carbon atoms of the modified metal oxide particles (iii) with an alcohol, ketone, ester, ether, amide, hydrocarbon, cyano group-containing solvent, halogen-containing solvent, sulfonyl group-containing solvent, carboxyl group-containing solvent, or a mixture thereof other than that used in the step (D). to provide. Effect of the Invention
[0007] In the present invention, stannic oxide particles (i) serving as core particles and modified metal oxide particles (iii) comprising at least one metal oxide particle selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide as coating particles that coat the surface of the core particles are used. For both the core particles and the coated particles, an aqueous sol in which colloidal metal oxide particles are stably dispersed in an aqueous medium can be used. These aqueous sols can be mixed. For example, an aqueous sol containing modified metal oxide particles (iii) can be obtained by adding an aqueous sol containing coated particles (ii) to an aqueous sol containing core particles (i). In order to stably disperse these aqueous sols in an aqueous medium, it is necessary to contain an amine (a) having a water solubility of 0.1 g / L or more. Both the aqueous sol containing core particles (i) and the aqueous sol containing coated particles (ii) are subjected to cation exchange before or after mixing, and some of them are removed, but the aqueous sol of the mixed modified metal oxide particles (iii) is then replaced from the aqueous medium to an organic solvent to prepare an organic solvent sol of the modified metal oxide particles (iii). In this step, the aqueous medium can be replaced with an organic solvent by the coexistence of an amine (a) having a water solubility of 0.1 g / L or more and an amine (b) having a water solubility of less than 0.1 g / L. This makes it possible to produce an organic solvent sol of modified metal oxide particles (iii) without aggregation. The core particles (i) can also be subjected to hydrothermal treatment. The hydrothermal treatment is carried out, for example, at a pressure of 0.1 to 40 MPa and a temperature of 100 to 350°C for 0.01 to 100 hours. It is desirable that the core particles are stably dispersed in an aqueous medium, and therefore an amine (a) having a water solubility of 0.1 g / L or more is required.
[0008] In the present invention, the modified metal oxide particles (iii) are dispersed in an organic solvent to form a sol. In order to improve the dispersibility of the modified metal oxide particles (iii) in the organic solvent by replacing the aqueous medium with the organic solvent, it is necessary to contain an amine (b) having a water solubility of less than 0.1 g / L. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention is a sol comprising modified metal oxide particles (iii) having an average primary particle size of 1 to 10 nm and coated with at least one kind of metal oxide particles (ii) selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide, which are cores of stannic oxide particles (i) having an average primary particle size of 4 to 50 nm, and the modified metal oxide particles are dispersed in an organic solvent, the average primary particle size satisfying the relationship of core particles (i)≧coated particles (ii), (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide) being 0.005 to 1.0, and the sol comprises an amine (a) having a water solubility of 0.1 g / L or more and an amine (b) having a water solubility of less than 0.1 g / L.
[0010] The method for measuring the solubility of a chemical substance in water is to use the column elution method when the solubility is low, or the flask method when the solubility is high. For example, the measurement method specified in OECD Test Guideline 105 (Solubility in Water) can be used.
[0011] The metal oxide other than stannic oxide refers to a metal oxide whose metal component is other than tin. The average primary particle size of the stannic oxide particles (i) and the metal oxide particles (ii) can be measured by observation with a transmission electron microscope.
[0012] The sol containing the modified metal oxide particles (iii) can be measured by dynamic light scattering, and the average particle size measured by dynamic light scattering is preferably 5 to 100 nm, or 10 to 60 nm, or 10 to 50 nm.
[0013] The stannic oxide particles (i) having an average primary particle size of 4 to 50 nm used as a raw material in the present invention can be prepared as an aqueous sol containing the stannic oxide particles (i). For example, it can be easily produced in the form of a sol of colloidal particles having a particle size of about 4 to 50 nm by methods such as ion exchange, peptization, hydrolysis, and reaction.
[0014] Examples of the ion exchange method include a method of treating a stannic acid salt such as sodium stannate with a hydrogen-type cation exchange resin, or a method of treating a stannic acid salt such as stannic chloride or stannic nitrate with a hydroxide-type anion exchange resin. Examples of the peptization method include a method of neutralizing a stannic acid salt with a base, or neutralizing a stannic acid with hydrochloric acid to obtain a stannic hydroxide gel, which is then washed and peptized with an acid or a base. Examples of the hydrolysis method include a method of hydrolyzing a tin alkoxide, or a method of hydrolyzing a basic stannic chloride salt under heating, followed by removing unnecessary acid. Examples of the reaction method include a method of reacting a metallic tin powder with an acid.
[0015] The aqueous sol containing the raw material stannic oxide particles (i) can also be obtained by reacting metallic tin with aqueous hydrogen peroxide.
[0016] Metallic tin can be used in powder or granular form. For example, metallic tin powder obtained by an atomization method in which an ingot is melted and sprayed to solidify, or flake-shaped metallic tin powder produced by cutting an ingot with a lathe or file can be used.
[0017] A commercially available aqueous solution of 35% by mass of hydrogen peroxide can be used at a desired concentration. For example, an aqueous solution of an organic acid such as oxalic acid with a concentration of 1 to 30% by mass or 5 to 20% by mass is prepared, and hydrogen peroxide and metallic tin are added simultaneously or alternately to the aqueous solution of the organic acid to obtain an aqueous solution of stannic acid. An aqueous solution of an organic acid such as oxalic acid is placed in a reaction vessel equipped with a stirrer, and hydrogen peroxide and metallic tin are added simultaneously or alternately from separate addition ports while stirring. Since the slurry containing aggregates of tin oxide colloid is acidic, it is preferable to use a glass reaction device or a glass-lined (enamel) reaction device as the reaction device used in these steps.
[0018] The hydrogen peroxide solution and metallic tin are added to an aqueous solution of an organic acid such as oxalic acid while maintaining the H2O2 / Sn molar ratio of 2 to 3. More specifically, a method of divided addition may be used in which 1 / 3 to 1 / 30 parts by mass of each of the hydrogen peroxide solution and metallic tin to the total parts by mass to be added is separately collected, and a series of steps of adding the hydrogen peroxide solution to an aqueous solution of an organic acid such as oxalic acid, followed by adding metallic tin, and reacting for 2 to 20 minutes is repeated 3 to 30 times.
[0019] Although the reaction is possible even if the H2O2 / Sn molar ratio is slightly more than 3, it is not preferable to exceed it significantly. If the H2O2 / Sn molar ratio is less than 2, the oxidation is insufficient, which is not preferable. The time for adding the hydrogen peroxide solution and the metallic tin can be 0.4 to 10 hours, preferably 0.4 to 5 hours. If the addition time is less than 0.4 hours, the exothermic reaction becomes intense and cannot be controlled, and unreacted metallic tin is likely to remain, which is not preferable. Also, although it may be more than 10 hours, it is not economical and is not preferable.
[0020] The reaction of metallic tin and hydrogen peroxide in an aqueous solution of an organic acid such as oxalic acid is carried out at 30 to 95°C, preferably 40 to 85°C. The reaction between hydrogen peroxide and metallic tin is an oxidation reaction, which is an exothermic reaction, and the decomposition reaction of hydrogen peroxide also occurs at the same time, which is also an exothermic reaction, so care must be taken to control the temperature during the reaction, and cooling can be performed as necessary. The reaction temperature may be less than 30°C, but since it is an exothermic reaction, excessive cooling is required, and the reaction takes too long, which is not economical. A reaction temperature of 95°C or higher is not preferable because it generates coarse colloidal particles.
[0021] This is a process in which excess electrolytes (mainly anions) are removed from the obtained stannic oxide colloid aggregate slurry to peptize the stannic oxide colloid particles and obtain a sol. By removing excess electrolytes, a sol in which the stannic oxide colloid particles are dispersed in a state close to primary particles can be obtained. This washing can be performed by a method of flocculation and settling, followed by decantation of the supernatant, ultrafiltration, ion exchange, etc., but when a large amount of electrolyte is contained, a washing method in which ultrafiltration is performed, followed by water injection, followed by another ultrafiltration (ultrafiltration-water injection-ultrafiltration) is particularly preferred. The average primary particle size of the stannic oxide composite colloid particles obtained by this process is 4 to 50 nm, or 10 to 20 nm (nanometers).
[0022] A process of anion-exchanging the stannic oxide aqueous sol can be added. This anion-exchange treatment makes it possible to obtain a sol that is stable even at high concentrations. For anion-exchange, a commercially available anion-exchange resin can be used, which is used after being prepared into a hydroxyl group type. Anion-exchange can be easily performed by passing the stannic oxide aqueous sol through a column packed with the anion-exchange resin. The liquid passing temperature is preferably 0 to 60°C, and the liquid passing speed is preferably a space velocity SV of 1 to 10 hours.
[0023] Before and / or after the anion exchange treatment, a basic substance can be added to the stannic oxide aqueous sol to improve stability. The basic substance used is preferably an organic base, and for example, an amine (a) having a water solubility of 0.1 g / L or more, 0.1 to 5,000.0 g / L, 0.1 to 3,000.0 g / L, 0.1 to 2,000.0 g / L, 0.5 to 2,000.0 g / L, 1.0 to 2,000.0 g / L, 10.0 to 2,000.0 g / L, or 100 to 1,000.0 g / L can be used.
[0024] The amine (a) can be added at a ratio of 20 to 3,000 ppm or 20 to 1,000 ppm. The amine (a) can be a primary amine, a secondary amine, or an amine consisting of a combination thereof. For example, the amine (a) can be at least one amine selected from the group consisting of n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, n-butylamine, isobutylamine, di-n-butylamine, and diisobutylamine.
[0025] In the present invention, the crystallinity of the stannic oxide particles (i) as the core particles, as measured by an X-ray diffraction method, is preferably 60% or more, or 65% or more and 100% or less, but typically 60 to 95% or 65 to 95% can be used. The crystallinity is preferably 60% or more, but typically 60 to 99% or 60 to 95%.
[0026] In the present invention, the stannic oxide aqueous sol having an SnO2 concentration of 1 to 50 mass% produced by the above method can be used as is, but hydrothermally treated stannic oxide particles can be produced by hydrothermal treatment at 100 to 350°C under pressure for 0.01 to 100 hours. For the hydrothermal treatment, for example, the above stannic oxide aqueous sol is placed in an autoclave and treated at a pressure of 0.1 to 40 MPa (megapascals) and a temperature of 100 to 350°C for 0.01 to 100 hours.
[0027] The medium for these stannic oxide sols may be either water or a hydrophilic organic solvent, but an aqueous sol in which the medium is water is preferred. The pH of the sol should be a value that stabilizes the sol, and is usually about 0.2 to 11.5. As long as the object of the present invention is achieved, the stannic oxide sol may contain any component, such as an alkaline substance, an acidic substance, or an oxycarboxylic acid, for stabilizing the sol. The concentration of the stannic oxide sol used is about 0.5 to 50% by mass in terms of stannic oxide, but the lower this concentration, the better, and is preferably 1 to 30% by mass.
[0028] It is particularly preferable to use an alkaline sol stabilized with an organic base such as the above-mentioned amine as the stannic oxide sol, and the above-mentioned amine is added at 5 to 100° C., preferably room temperature (20° C.) to 60° C. The above-mentioned amine is added to the stannic oxide sol under stirring, and mixing must be carried out thoroughly, preferably for 0.5 to 3 hours.
[0029] The coated particles (ii) used in the present invention can be an aqueous sol of coated particles. The coated particles (ii) can be antimony oxide particles (ii-1) alone, or composite particles (ii-2) of stannic oxide and silicon oxide with a mass ratio of stannic oxide:silicon dioxide=1:0.1 to 10.0.
[0030] The alkylamine-containing antimony pentoxide colloidal particles (ii-1) can be obtained by oxidation method, acid decomposition method, etc. Examples of the acid decomposition method include a method in which an alkali antimonate is reacted with an inorganic acid and then peptized with an amine (JP-A-60-41536, JP-A-61-227918, JP-A-2001-123115), an example of the oxidation method includes a method in which antimony trioxide is oxidized with hydrogen peroxide in the presence of an amine or an alkali metal (JP-B-57-11848, JP-A-59-232921), or a method in which antimony trioxide is oxidized with hydrogen peroxide and then an amine or an alkali metal is added. As the amine, for example, an amine (a) having a water solubility of 0.1 g / L or more can be used. The amine (a) can be added at a ratio of 20 to 3,000 ppm or 20 to 1,000 ppm. The amine (a) may be a primary amine, a secondary amine, or an amine consisting of a combination thereof. For example, the amine (a) may be at least one amine selected from the group consisting of n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, n-butylamine, isobutylamine, di-n-butylamine, and diisobutylamine.
[0031] The alkylamine-containing diantimony pentoxide colloidal particles (ii-1) are fine colloidal particles of diantimony pentoxide, and the particle size thereof is about 1 to 20 nm as an oligomer or primary particle size as determined by electron microscopy. As the amine component, an alkylamine salt such as diisopropylamine is preferred, and the molar ratio of amine / Sb2O5 is 0.02 to 4.00.
[0032] In the above coating, alkylamine-containing silicon dioxide particles can be further added to the amine-containing antimony pentoxide colloidal particles. The composite colloid of antimony pentoxide and silicon dioxide that can be used as the coating sol can be obtained by the following known method (for example, JP-B-50-40119), namely, by mixing an aqueous alkali silicate solution or a silicic acid solution with an aqueous alkali antimonate solution, and then decationizing the mixture with a cation exchange resin.
[0033] As the antimony raw material, preferably, an aqueous solution of potassium antimonate can be used. As the silicon dioxide raw material, sodium silicate, potassium silicate, and activated silicic acid obtained by cation exchange of these can be used. The molar ratio of SiO2 / Sb2O5 is 0.55 to 55. The particle size of the oligomer or the average primary particle is 5 nm or less, preferably 1 to 5 nm, as determined by electron microscope observation.
[0034] The colloidal particles (ii-2) of a composite of stannic oxide and silicon dioxide used in the coating sol of the present invention can be obtained by the method shown below. This is obtained by preparing an aqueous solution containing stannate and silicate in a SiO2 / SnO2 mass ratio of 0.1 to 10, and removing cations present in the resulting aqueous solution. The total concentration of SnO2 and SiO2 contained in this sol is usually 40 mass% or less, practically preferably 2 mass% or more, and preferably 5 to 30 mass%.
[0035] This sol can exist stably without substantially containing an alkaline component. However, it is also possible to stabilize it by containing an alkaline component. The alkaline component can be added at a ratio of 20 to 3,000 ppm or 20 to 1,000 ppm as amine (a). The amine (a) can be a primary amine, a secondary amine, or an amine consisting of a combination thereof. For example, the amine (a) can be at least one amine selected from the group consisting of n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, n-butylamine, isobutylamine, di-n-butylamine, and diisobutylamine. These alkaline components can be contained in an amount of about 30 mass% or less based on the total amount of SnO2 and SiO2. In addition, two or more of these can be mixed and contained. By adding amine (a) at a ratio of 20 to 3,000 ppm, the amine dissolved in the sol is adsorbed to the surface of the modified metal oxide particles, improving the dispersion stability. +
[0036] This sol is a colorless, transparent or slightly colloidal liquid having a pH of 1 to 9. It is stable for at least 3 months at room temperature and for at least 1 month at 60° C., and does not produce any precipitate in the sol, nor does it thicken or gel.
[0037] Examples of the stannate and silicate used in the production of this sol are preferably sodium stannate (Na2SnO3·3H2O) and sodium silicate (water glass). Also usable are those in which stannic acid, silicic acid, etc. are dissolved in an aqueous solution of an alkali metal hydroxide. Examples of the aqueous solution include a method in which each powder of a stannate and a silicate is dissolved in water to prepare an aqueous solution, a method in which an aqueous solution of a stannate and an aqueous solution of a silicate are mixed to prepare an aqueous solution, and a method in which a powder of a stannate and an aqueous solution of a silicate are added to water to prepare an aqueous solution. The aqueous solution of a stannate preferably has an SnO2 concentration of about 0.1 to 30% by mass, but can also be used at a concentration higher than this. The aqueous solution of a silicate preferably has an SiO2 concentration of about 0.1 to 30% by mass, but can also be used at a concentration higher than this.
[0038] The preparation of the aqueous solution is carried out under stirring at room temperature (about 20°C) to 100°C, preferably at room temperature (about 20°C) to about 60°C. The aqueous solution to be mixed preferably has a SiO2 / SnO2 mass ratio of 0.1 to 100. Subsequently, the cations present in the aqueous solution obtained here are removed to obtain an aqueous sol. The decationization treatment can be carried out by contacting with a hydrogen-type ion exchanger or by salting out. The hydrogen-type cation exchanger used here is one that is commonly used, and it is convenient to use a commercially available hydrogen-type cation exchange resin. When the concentration of the sol is low, the concentration of the sol can be increased as desired by subjecting the aqueous sol to a conventional concentration method, such as evaporation or ultrafiltration. Ultrafiltration is particularly preferred. In this concentration, the temperature of the sol is preferably kept at about 100° C. or less, particularly 60° C. or less. Although there is no particular lower limit, the temperature is preferably kept at 10° C. or more, and more preferably at 20° C. or more.
[0039] The modified stannic oxide colloid particles (iii-1) whose surfaces are covered with the amine-containing Sb2O5 colloid particles (ii-1) according to the present invention are negatively charged in the sol. The above stannic oxide particles (i) are positively charged, and the Sb2O5 colloid is negatively charged. Therefore, it is considered that the negatively charged Sb2O5 colloid (ii-1) is electrically attracted around the positively charged stannic oxide colloid particles (i) by mixing, and the Sb2O5 colloid is bonded to the surface of the positively charged colloid particles by chemical bonds, and the surface of the positively charged particles is covered with negatively charged Sb2O5 as the nucleus, thereby generating the modified stannic oxide colloid particles (iii-1).
[0040] When mixing tin oxide colloid particles (i) having an average primary particle diameter of 4 to 50 nm as a core sol with amine-containing Sb2O5 colloid (ii-1) as a coating sol, if the metal oxide of the coating sol is less than 1 part by mass per 100 parts by mass of the metal oxide (SnO2) of the core sol, a stable sol cannot be obtained. This is because, when the amount of Sb2O5 colloid is insufficient, the surface of the tin oxide colloid particles as the core is not sufficiently covered by the colloid particles of this complex, and the resulting colloid particles are likely to aggregate, making the resulting sol unstable. Therefore, the amount of Sb2O5 colloid particles to be mixed may be less than the amount that covers the entire surface of the tin oxide colloid particles, but is equal to or greater than the minimum amount required to produce a sol of stable modified tin oxide particles. When an amount of Sb2O5 colloidal particles used in the above mixing exceeds the amount used for the surface coating, the resulting sol is merely a stable mixed sol of the Sb2O5 colloidal sol and the resulting sol of the modified stannic oxide colloidal particles.
[0041] The stannic oxide colloid particles (i) are positively charged, and the stannic oxide and silicon dioxide complex colloid (ii-2) is negatively charged. Therefore, it is considered that the negatively charged stannic oxide and silicon dioxide complex colloid (ii-2) is electrically attracted around the positively charged stannic oxide colloid particles (i) by mixing, and the stannic oxide and silicon dioxide complex colloid is chemically bonded to the surface of the positively charged colloid particles, and the surface of the positively charged particles is covered with the negatively charged stannic oxide and silicon dioxide complex colloid, thereby generating the modified stannic oxide colloid particles (iii-2).
[0042] When mixing stannic oxide colloid particles (i) having an average primary particle diameter of 4 to 50 nm as a core sol with a composite colloid of stannic oxide and silicon dioxide (ii-2) as a coating sol, if the metal oxide of the coating sol is less than 1 part by mass per 100 parts by mass of the metal oxide (SnO2) of the core sol, a stable sol cannot be obtained. This is because, when the amount of the composite colloid of stannic oxide and silicon dioxide is insufficient, the surface of the stannic oxide colloid particles serving as the core is not sufficiently covered by the colloid particles of the composite, and the resulting colloid particles are likely to aggregate, making the resulting sol unstable. Therefore, the amount of the composite colloid particles of stannic oxide and silicon dioxide to be mixed may be less than the amount that covers the entire surface of the stannic oxide or stannic oxide-zirconium oxide composite colloid particles, but is equal to or greater than the minimum amount required to produce a sol of stable modified stannic oxide colloid particles. When an amount of stannic oxide and silicon dioxide composite colloidal particles used in the above mixing exceeds the amount used for the surface coating, the resulting sol is merely a stable mixed sol of the stannic oxide and silicon dioxide composite colloidal sol and the resulting sol of modified stannic oxide colloidal particles.
[0043] Preferably, to modify the stannic oxide colloidal particles by surface coating, the amount of the stannic oxide and silicon dioxide composite colloid used is 50 parts by mass or less of the metal oxide in the coating sol per 100 parts by mass of the metal oxide (SnO2) in the core sol.
[0044] The sol of the present invention can be prepared by the following steps (A) to (D): Step (A): preparing an aqueous sol of stannic oxide particles (i) containing an amine (a) having a water solubility of 0.1 g / L or more and having an average primary particle size of 4 to 50 nm; Step (B): preparing an aqueous sol of at least one metal oxide particle (ii) having an average primary particle size of 1 to 10 nm and selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide, which contains an amine (a) having a water solubility of 0.1 g / L or more; Step (C): mixing the aqueous sol of stannic oxide obtained in step (A) and the aqueous sol of the modified metal oxide obtained in step (B) in a ratio of (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide) of 0.005 to 1.0 to produce modified metal oxide particles (iii) having an average primary particle size of 1 to 10 nm and coated with at least one kind of metal oxide particles (ii) selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide, using stannic oxide particles (i) having an average primary particle size of 4 to 50 nm as cores, and adding an amine (b) having a water solubility of less than 0.1 g / L; Step (D): replacing the aqueous medium of the aqueous sol of the modified metal oxide particles (iii) obtained in step (C) with an alcohol having 1 to 5 carbon atoms.
[0045] In the present invention, the step (A) can employ a step (A-1) in which an amine (a) having a water solubility of 0.1 g / L or more is added to an aqueous sol of stannic oxide particles (i) having an average primary particle size of 4 to 50 nm, and then the aqueous sol is subjected to a hydrothermal treatment at a pressure of 0.1 to 40 MPa and a temperature of 100 to 350°C for 0.01 to 100 hours.
[0046] In the present invention, the mixing in step (C) of the aqueous sol of stannic oxide particles (i) obtained in step (A) and the aqueous sol of at least one metal oxide particle (ii) selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide obtained in step (B) is preferably carried out in such a manner that the modified metal oxide particles (iii) have a ratio of (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide) of 0.005 to 1.0, or 0.005 to 0.5, or 0.01 to 0.5, or 0.01 to 0.3, or 0.01 to 0.2, or 0.04 to 0.15.
[0047] The amine (b) having a water solubility of less than 0.1 g / L used in the step (C) is an amine having a water solubility of less than 0.1 g / L, 0.00001 g / L or more and less than 0.1 g / L, 0.00002 g / L or more and less than 0.1 g / L, 0.00003 g / L or more and less than 0.1 g / L, 0.00005 g / L or more and less than 0.1 g / L, 0.0001 g / L or more and less than 0.1 g / L, 0.001 g / L or more and less than 0.1 g / L, Examples of tertiary amines include tertiary amines with an average concentration of less than 0.01 g / liter and less than 0.1 g / liter, tertiary amines with an average concentration of 0.00003 g / liter and less than 0.08 g / liter, tertiary amines with an average concentration of 0.00003 g / liter and less than 0.05 g / liter, and tertiary amines with an average concentration of 0.00003 g / liter and less than 0.03 g / liter. For example, at least one amine selected from the group consisting of tri-n-butylamine, triisobutylamine, tri-n-pentylamine, and triisopentylamine can be mentioned. The amine (a) can be contained in the modified metal oxide sol at a ratio of 20 to 3,000 ppm, or 20 to 1,000 ppm. The amine (b) can be contained in the modified metal oxide sol at a ratio of 1,000 to 30,000 ppm, or 1,000 to 10,000 ppm.
[0048] It is considered that the amine (b) having a water solubility of less than 0.1 g / L added in the step (C) is partially adsorbed on the surface of the modified metal oxide particles (iii) in the aqueous sol in the step (C). When the dispersion medium of the sol is replaced from the aqueous medium to an organic solvent in the subsequent step (D), the presence of the amine (b) improves compatibility with the organic solvent, and the modified metal oxide particles (iii) can be dispersed in the organic solvent without aggregation. The amine (b) is transferred from the surface of the modified metal oxide particles (iii) into the organic solvent in the organic solvent. In the organic solvent dispersion sol of the modified metal oxide particles (iii), the amine (a) and the amine (b) can be detected in the dispersion medium. Since the modified metal oxide particles (iii) are sufficiently dispersed in the organic solvent and the sol is stably present, when a coating agent using them is applied to a substrate and cured, the modified metal oxide particles are not unevenly distributed on the substrate, and a high refractive index and good electrical conductivity are obtained. The refractive index of such modified metal oxide particles is preferably in the range of 1.75 to 2.00.
[0049] Examples of the alcohol having 1 to 5 carbon atoms in the above step (D) include methanol, ethanol, n-propanol, i-propanol, n-butanol, and propylene glycol monomethyl ether.
[0050] In the modified metal oxide sol obtained in the present invention, the mass ratio of amine (b) / amine (a) is preferably 3.0-200, or 3.0-100, or 3.0-60.
[0051] In the present invention, step (D) is followed by step (E) and / or step (F): Step (E): adding at least one coating agent selected from the group consisting of formulas (1) to (6) to an organic solvent sol of the modified metal oxide particles (iii) to perform surface treatment of the modified metal oxide particles (iii); Step (F): a step of solvent-substitution of the alcohol in the alcohol solvent sol having 1 to 5 carbon atoms of the modified metal oxide particles (iii) with an alcohol, ketone, ester, ether, amide, hydrocarbon, cyano group-containing solvent, halogen-containing solvent, sulfonyl group-containing solvent, carboxyl group-containing solvent, or a mixture thereof other than that used in step (D) can be added.
[0052] In the coating agent in the above step (E), the formulas (1) to (3) are silane coupling agents, and the formulas (4) to (6) are phosphate compounds. As the coating agent, a silane coupling agent, a phosphate compound, or a combination thereof can be used. For example, step (D) may be followed by step (E), step (D) may be followed by step (F), or step (D) may be followed by step (E) and then step (F).
[0053] The silane compound may be a hydrolysate of at least one silane compound selected from the group consisting of the formulae (1) to (3).
[0054] In formula (1), R 1 each represents an alkyl group, a halogenated alkyl group, an alkenyl group, an aryl group, or an organic group having a polyether group, an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a ureido group, or a cyano group, and is bonded to a silicon atom by a Si-C bond; R 2 represents an alkoxy group, an acyloxy group, or a halogen group, and a represents an integer of 1 to 3.
[0055] In formula (2) and formula (3), R 3 and R 5 are each an alkyl group having 1 to 3 carbon atoms or an aryl group having 6 to 30 carbon atoms and bonded to a silicon atom by a Si-C bond, and R 4 and R 6each represents an alkoxy group, an acyloxy group, or a halogen group; Y represents an alkylene group, an NH group, or an oxygen atom; b is an integer of 1 to 3; c is an integer of 0 or 1; and d is an integer of 1 to 3.
[0056] The alkyl group is an alkyl group having 1 to 18 carbon atoms, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, a cyclopropyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, a cyclobutyl group, a 1-methyl-cyclopropyl group, a 2-methyl-cyclopropyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, a 1-ethyl -n-propyl, cyclopentyl, 1-methyl-cyclobutyl, 2-methyl-cyclobutyl, 3-methyl-cyclobutyl, 1,2-dimethyl-cyclopropyl, 2,3-dimethyl-cyclopropyl, 1-ethyl-cyclopropyl, 2-ethyl-cyclopropyl, n-hexyl, 1-methyl-n-pentyl, 2-methyl-n-pentyl, 3-methyl-n-pentyl, 4-methyl-n-pentyl, 1,1-dimethyl-n-butyl, 1,2-dimethyl-n-butyl, 1,3-dimethyl-n-butyl , 2,2-dimethyl-n-butyl, 2,3-dimethyl-n-butyl, 3,3-dimethyl-n-butyl, 1-ethyl-n-butyl, 2-ethyl-n-butyl, 1,1,2-trimethyl-n-propyl, 1,2,2-trimethyl-n-propyl, 1-ethyl-1-methyl-n-propyl, 1-ethyl-2-methyl-n-propyl, cyclohexyl, 1-methyl-cyclopentyl, 2-methyl-cyclopentyl, 3-methyl-cyclopentyl, 1-ethyl-cyclobutyl, 2-ethyl-cyclobutyl cyclopropyl, 3-ethyl-cyclobutyl, 1,2-dimethyl-cyclobutyl, 1,3-dimethyl-cyclobutyl, 2,2-dimethyl-cyclobutyl, 2,3-dimethyl-cyclobutyl, 2,4-dimethyl-cyclobutyl, 3,3-dimethyl-cyclobutyl, 1-n-propyl-cyclopropyl, 2-n-propyl-cyclopropyl, 1-i-propyl-cyclopropyl, 2-i-propyl-cyclopropyl, 1,2,2-trimethyl-cyclopropyl, 1,2,3-trimethyl-cyclopropyl, 2,2,Examples of the cyclopropyl group include, but are not limited to, 3-trimethyl-cyclopropyl group, 1-ethyl-2-methyl-cyclopropyl group, 2-ethyl-1-methyl-cyclopropyl group, 2-ethyl-2-methyl-cyclopropyl group, 2-ethyl-3-methyl-cyclopropyl group, hexyl group, heptyl group, octyl group, nonyl group, decyl group, undecyl group, dodecyl group, tridecyl group, tetradecyl group, pentadecyl group, hexadecyl group, heptadecyl group, and octadecyl group.
[0057] Examples of the alkylene group include alkylene groups derived from the above-mentioned alkyl groups.
[0058] The aryl group is an aryl group having 6 to 30 carbon atoms, and examples thereof include a phenyl group, a naphthyl group, an anthracenyl group, and a pyrenyl group.
[0059] The alkenyl group is an alkenyl group having 2 to 10 carbon atoms, and examples of the alkenyl group include ethenyl group, 1-propenyl group, 2-propenyl group, 1-methyl-1-ethenyl group, 1-butenyl group, 2-butenyl group, 3-butenyl group, 2-methyl-1-propenyl group, 2-methyl-2-propenyl group, 1-ethylethenyl group, 1-methyl-1-propenyl group, 1-methyl-2-propenyl group, 1-pentenyl group, 2-pentenyl group, 3-pentenyl group, 4-pentenyl group, 1-n-propylethenyl group, 1-methyl-1-butenyl group, 1-methyl-2-butenyl group, 1-methyl-3-butenyl group, 2-ethyl-2-propenyl group, 2-methyl-1-butenyl group, 2-methyl-2-butenyl group, 2-methyl-3-butenyl group, 3 Examples of the aryl group include, but are not limited to, 1-methyl-1-butenyl group, 3-methyl-2-butenyl group, 3-methyl-3-butenyl group, 1,1-dimethyl-2-propenyl group, 1-i-propylethenyl group, 1,2-dimethyl-1-propenyl group, 1,2-dimethyl-2-propenyl group, 1-cyclopentenyl group, 2-cyclopentenyl group, 3-cyclopentenyl group, 1-hexenyl group, 2-hexenyl group, 3-hexenyl group, 4-hexenyl group, 5-hexenyl group, 1-methyl-1-pentenyl group, 1-methyl-2-pentenyl group, 1-methyl-3-pentenyl group, 1-methyl-4-pentenyl group, 1-n-butylethenyl group, 2-methyl-1-pentenyl group, and 2-methyl-2-pentenyl group.
[0060] The alkoxy group includes an alkoxy group having 1 to 10 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, an n-butoxy group, an i-butoxy group, an s-butoxy group, a t-butoxy group, an n-pentyloxy group, a 1-methyl-n-butoxy group, a 2-methyl-n-butoxy group, a 3-methyl-n-butoxy group, a 1,1-dimethyl-n-propoxy group, a 1,2-dimethyl-n-propoxy group, a 2,2-dimethyl-n-propoxy group, a 1-ethyl-n-propoxy group, and an n-hexyloxy group, but is not limited to these.
[0061] Examples of the acyloxy group having 2 to 10 carbon atoms include, but are not limited to, a methylcarbonyloxy group, an ethylcarbonyloxy group, an n-propylcarbonyloxy group, an i-propylcarbonyloxy group, an n-butylcarbonyloxy group, an i-butylcarbonyloxy group, an s-butylcarbonyloxy group, a t-butylcarbonyloxy group, an n-pentylcarbonyloxy group, a 1-methyl-n-butylcarbonyloxy group, a 2-methyl-n-butylcarbonyloxy group, a 3-methyl-n-butylcarbonyloxy group, a 1,1-dimethyl-n-propylcarbonyloxy group, a 1,2-dimethyl-n-propylcarbonyloxy group, a 2,2-dimethyl-n-propylcarbonyloxy group, a 1-ethyl-n-propylcarbonyloxy group, an n-hexylcarbonyloxy group, a 1-methyl-n-pentylcarbonyloxy group, and a 2-methyl-n-pentylcarbonyloxy group.
[0062] The halogen group includes fluorine, chlorine, bromine, iodine, and the like.
[0063] An example of the organic group having a polyether group is a polyetherpropyl group having an alkoxy group, such as (CH3O)3SiC3H6(OC2H4)nOCH3. n can be in the range of 1 to 100 or 1 to 10.
[0064] Examples of the organic group having an epoxy group include a 2-(3,4-epoxycyclohexyl)ethyl group and a 3-glycidoxypropyl group.
[0065] The above-mentioned (meth)acryloyl group refers to both an acryloyl group and a methacryloyl group. Examples of organic groups having a (meth)acryloyl group include a 3-methacryloxypropyl group and a 3-acryloxypropyl group.
[0066] An example of the organic group having a mercapto group is a 3-mercaptopropyl group.
[0067] Examples of organic groups having an amino group include a 2-aminoethyl group, a 3-aminopropyl group, an N-2-(aminoethyl)-3-aminopropyl group, an N-(1,3-dimethyl-butylidene)aminopropyl group, an N-phenyl-3-aminopropyl group, and an N-(vinylbenzyl)-2-aminoethyl-3-aminopropyl group.
[0068] An example of the organic group having a ureido group is a 3-ureidopropyl group.
[0069] An example of the organic group having a cyano group is a 3-cyanopropyl group.
[0070] The above formulas (2) and (3) are preferably compounds capable of forming trimethylsilyl groups on the surface of silica particles. Examples of such compounds include the following.
[0071] [ka]
[0072] In the above formula, R 12 is an alkoxy group, and examples thereof include a methoxy group and an ethoxy group. As the silane compound, for example, a silane compound manufactured by Shin-Etsu Chemical Co., Ltd. can be used.
[0073] This is a process in which the silane compound reacts with the hydroxyl group on the surface of the modified metal oxide particle (iii), for example, the silanol group in the case of silica particles, to coat the surface of the silica particle with the silane compound through siloxane bonds. The reaction temperature can be from 20°C to the boiling point of the dispersion medium, for example, in the range of 20°C to 100°C. The reaction time can be about 0.1 to 6 hours.
[0074] The silane compound is used in such a manner that the number of silicon atoms in the silane compound is 0.1 / nm as a coating amount on the surface of the modified metal oxide particle (iii). 2 ~6.0 pieces / nm 2The surface of the silica particles can be coated by adding a silane compound corresponding to the coating amount of (iii) to the sol of the modified metal oxide particles.
[0075] Water is necessary for the hydrolysis of the silane compound, but the water remaining in the solvent when the aqueous medium is replaced with an organic solvent can be used. For example, water present at 0.01 to 1 mass % can be used. The hydrolysis can be performed with or without a catalyst.
[0076] The phosphate compound may be at least one phosphate compound selected from the group consisting of the formulae (4) to (6).
[0077] In formulas (4) to (6), X1, X2, and X3 each represent an alkylene group having 2 to 20 carbon atoms, f, h, and j each represent an integer of 1 to 100, e, g, and i each represent an integer of 1 to 3, and Y1, Y2, and Y3 each represent a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or a (meth)acrylic group.
[0078] As the phosphate ester, polyoxyethylene alkyl ether phosphate ester can be preferably used, for example, the phosphate ester in which the terminal alkyl group (Y1) in the above formula (4) is an alkyl group having 6 to 10 carbon atoms or 12 to 15 carbon atoms can be used. Examples of these products that can be used include products manufactured by Toho Chemical Industry Co., Ltd., trade names of Phosphanol RA-600 and RS-610.
[0079] Examples of the alkylene group having 2 to 20 carbon atoms include alkylene groups derived from the above-mentioned alkyl groups, and examples of the alkenyl group having 2 to 20 carbon atoms and the aryl group having 6 to 30 carbon atoms include those mentioned above.
[0080] The amount of the phosphate ester compound coated on the surface of the modified metal oxide particle (iii) is such that the number of phosphorus atoms in the phosphate ester compound is 0.1 / nm 2 ~6.0 pieces / nm 2 The surface of the modified metal oxide particles can be coated by adding a phosphoric acid ester compound corresponding to the coating amount of the above to the sol of the modified metal oxide particles (iii).
[0081] In the present invention, the following step (F) can be added after step (D). Step (F): A step of replacing the alcohol of the alcohol solvent sol having 1 to 5 carbon atoms of the modified metal oxide particles (iii) obtained in step (D) with an alcohol, ketone, ester, ether, amide, hydrocarbon, cyano group-containing solvent, halogen-containing solvent, sulfonyl group-containing solvent, carboxyl group-containing solvent, or a mixed solvent thereof other than that used in step (D).
[0082] The alcohol other than that used in step (D) that can be used in step (F) is a monohydric alcohol having 1 to 20 or 1 to 10 carbon atoms, or a polyhydric alcohol having 1 to 20 or 1 to 10 carbon atoms. Examples of the monohydric alcohol include methanol, ethanol, n-propanol, i-propanol, n-butanol, propylene glycol monomethyl ether, isobutanol, n-pentanol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, 1-octanol, 1-nonanol, 1-decanol, benzyl alcohol, 2-phenoxyethanol, 2-benzyloxyethanol, and tetrahydrofurfuryl alcohol. Examples of the polyhydric alcohol include ethylene glycol, propylene glycol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, 1,3-butanediol, and 2,3-butanediol.
[0083] As the ketone, an aliphatic ketone can be preferably used as a ketone having 1 to 20 carbon atoms or 1 to 10 carbon atoms. Examples thereof include acetone, methyl ethyl ketone, diethyl ketone, methyl propyl ketone, methyl isobutyl ketone, methyl amyl ketone, cyclohexanone, methyl cyclopentanone, isophorone, 4-hydroxy-4-methyl-2-pentanone, methyl-n-propyl ketone, methyl-n-butyl ketone, methyl-n-amyl ketone, 2-heptanone, and acetylacetone.
[0084] As the ester, an aliphatic ester having 1 to 20 carbon atoms or an ester having 1 to 10 carbon atoms can be preferably used. For example, methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl acrylate, ethyl acrylate, propyl acrylate, dimethyl maleate, diethyl maleate, dipropyl maleate, dimethyl adipate, diethyl adipate, dipropyl adipate, propylene glycol monomethyl ether acetate, methyl benzoate, ethyl benzoate, butyl benzoate, dimethyl phthalate, dibutyl maleate, diethyl oxalate, dibutyl oxalate, hexyl acetate, benzyl acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, diethyl maleate, diethyl fumarate, dipropylene glycol methyl ether acetate, 1,3-butylene glycol diacetate, propylene glycol diacetate, 1,6-Hexanediol diacetate, triacetin, gamma-butyrolactone, ethylene carbonate, propylene carbonate, methyl cellosolve acetate, ethyl cellosolve acetate, diethyl cellosolve acetate, phenyl cellosolve acetate, n-butyl acetate, isobutyl acetate, methyl lactate, ethyl lactate, methyl hydroxyacetate, ethyl hydroxyacetate, butyl hydroxyacetate, methoxymethyl acetate, methoxyethyl acetate, methoxybutyl acetate, ethoxymethyl acetate, ethoxyethyl acetate, methyl 3-hydroxypropionate, ethyl 3-hydroxypropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, methyl 2-hydroxypropionate, Cypropionate, ethyl 2-hydroxypropionate, propyl 2-hydroxypropionate, methyl 2-methoxypropionate, ethyl 2-methoxypropionate, ethyl 2-ethoxypropionate, methyl 2-ethoxypropionate, methyl 2-hydroxy-2-methylpropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 2-methoxy-2-methylpropionate, ethyl 2-ethoxy-2-methylpropionate, 2-hydroxyethylpropionate, 2-hydroxy-2-methylethylpropionate, hydroxyethyl acetate, methyl 2-hydroxy-3-methylbutanoate, ethyl pyruvate, methyl ethyl carbitol, diethyl carbitol, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, etc.,
[0085] As the ether, an aliphatic ether can be preferably used as an ether having 1 to 20 carbon atoms or 1 to 10 carbon atoms. Examples thereof include dimethyl ether, ethyl methyl ether, diethyl ether, tetrahydrofuran, 1,4-dioxane, anisole, 4-methoxytoluene, diethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol monophenyl ether, triethylene glycol monomethyl ether, dipropylene glycol monomethyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether, tripropylene glycol monomethyl ether, 2-(2-isobutoxyethoxy)ethanol, and benzyl ethyl ether.
[0086] Examples of the amides include amides having 1 to 20 carbon atoms or amides having 1 to 10 carbon atoms, such as dimethylacetamide, dimethylformamide, N-methylpyrrolidone, N-ethylpyrrolidone, N,N-dimethylisobutylamide, 1,3-dimethyl-2-imidazolidinone, N-methylformamide, N-methylformanilide, and N-methylacetamide.
[0087] Examples of the hydrocarbon include paraffinic hydrocarbons, naphthenic hydrocarbons, aromatic hydrocarbons, and mixtures thereof having 6 to 18 or 6 to 40 carbon atoms. Examples of n-paraffins include n-hexane, n-heptane, n-octane, n-nonane, and n-decane. Examples of i-paraffins include i-octane, i-nonane, and i-decane. Examples of aromatic hydrocarbons include toluene, xylene, tetralin, cyclohexylbenzene, and decylbenzene.
[0088] Examples of the cyano group-containing solvent include acetonitrile and 3-methoxypropionitrile.
[0089] Examples of halogen-containing solvents include chloroform and chlorobenzene.
[0090] The sulfonyl group-containing solvent may, for example, be dimethyl sulfoxide.
[0091] Examples of the carboxyl group-containing solvent include formic acid, acetic acid, acrylic acid, methacrylic acid, oleic acid, linoleic acid, linolenic acid, lactic acid, and caproic acid.
[0092] In the present invention, in step (D), the surface of the modified metal oxide particles (iii) can be coated with a silane compound.
[0093] In the present invention, a film-forming composition is obtained which contains the organic solvent sol of the modified metal oxide particles (iii) and an organic resin.
[0094] The organic resin is a film-forming composition obtained by selecting and mixing a thermosetting or photosetting resin, and can be made into a cured product by including a curing agent such as an amine-based curing agent, an acid anhydride-based curing agent, a radical generator-based curing agent (thermal radical generator, photoradical generator), or an acid generator-based curing agent (thermal acid generator, photoacid generator).
[0095] The present composition can form a cured product by applying or filling a film-forming composition containing an organic resin and a curing agent to a substrate and then heating, irradiating with light, or a combination thereof. The organic resin (curable resin) can be a resin having a functional group such as an epoxy group or a (meth)acryloyl group, or an isocyanate-based resin. For example, a photocurable polyfunctional acrylate can be preferably used.
[0096] Examples of the polyfunctional acrylate include polyfunctional acrylates having difunctional, trifunctional, tetrafunctional or higher functional groups in the molecule, such as neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. These multifunctional acrylates may also be described below.
[0097] [ka]
[0098] [ka]
[0099] [ka]
[0100] [ka]
[0101] The film-forming composition of the present invention may contain a surfactant (leveling agent).
[0102] The surfactant (leveling agent) may be an anionic surfactant, a cationic surfactant, an amphoteric surfactant, a nonionic surfactant, or a silicone surfactant. The surfactant (leveling agent) may be added in an amount of 0.01 to 5 phr or 0.01 to 1 phr relative to the organic resin.
[0103] Anionic surfactants for use in the present invention include sodium and potassium salts of fatty acids, alkylbenzene sulfonates, higher alcohol sulfates, polyoxyethylene alkyl ether sulfates, α-sulfofatty acid esters, α-olefin sulfonates, monoalkyl phosphates, and alkanesulfonates.
[0104] For example, alkylbenzenesulfonates include sodium salts, potassium salts and lithium salts, such as sodium C10-C16 alkylbenzenesulfonate, C10-C16 alkylbenzenesulfonic acid, and sodium alkylnaphthalenesulfonate.
[0105] Examples of higher alcohol sulfates include sodium dodecyl sulfate (sodium lauryl sulfate) having 12 carbon atoms, triethanolamine lauryl sulfate, and triethanolammonium lauryl sulfate.
[0106] Examples of polyoxyethylene alkyl ether sulfates include sodium polyoxyethylene styrenated phenyl ether sulfate, ammonium polyoxyethylene styrenated phenyl ether sulfate, sodium polyoxyethylene decyl ether sulfate, ammonium polyoxyethylene decyl ether sulfate, sodium polyoxyethylene lauryl ether sulfate, ammonium polyoxyethylene lauryl ether sulfate, sodium polyoxyethylene tridecyl ether sulfate, and sodium polyoxyethylene oleyl cetyl ether sulfate. The α-olefin sulfonate salts include sodium α-olefin sulfonate.
[0107] Examples of the alkane sulfonate include sodium 2-ethylhexyl sulfate.
[0108] Examples of the cationic surfactant that can be used in the present invention include alkyl trimethyl ammonium salts, dialkyl dimethyl ammonium salts, alkyl dimethyl benzyl ammonium salts, and amine salt-based agents.
[0109] Alkyltrimethylammonium salts are quaternary ammonium salts that have a chloride ion or a bromide ion as a counterion. Examples include dodecyltrimethylammonium chloride, cetyltrimethylammonium chloride, coconut alkyltrimethylammonium chloride, and alkyl(C16-18)trimethylammonium chloride.
[0110] Dialkyldimethylammonium salts have two lipophilic main chains and two methyl groups. Examples include bis(hydrogenated tallow)dimethylammonium chloride. Examples include didecyldimethylammonium chloride, dicoconucleic acid alkyldimethylammonium chloride, dihydrogenated tallow alkyldimethylammonium chloride, and dialkyl(C14-18)dimethylammonium chloride.
[0111] Alkyl dimethyl benzyl ammonium salts are quaternary ammonium salts with one lipophilic main chain, two methyl groups, and a benzyl group, and examples of these include benzauconium chloride. For example, alkyl (C8-18) dimethyl benzyl ammonium chloride is included.
[0112] Amine salt agents include those in which the hydrogen atom of ammonia is replaced with one or more hydrocarbon groups, such as N-methylbishydroxyethylamine fatty acid ester hydrochloride.
[0113] The amphoteric surfactants used in the present invention include N-alkyl-β-alanine type alkylamino fatty acid salts, alkylcarboxybetaine type alkylbetaines, and N,N-dimethyldodecylamine oxide type alkylamine oxides, examples of which include lauryl betaine, stearyl betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, and lauryl dimethylamine oxide.
[0114] The nonionic surfactant used in the present invention is selected from polyoxyethylene alkyl ethers, polyoxyethylene alkylphenol ethers, alkyl glucosides, polyoxyethylene fatty acid esters, sucrose fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and fatty acid alkanolamides. For example, examples of polyoxyethylene alkyl ethers include polyoxyethylene dodecyl ether (polyoxyethylene lauryl ether), polyoxyalkylene lauryl ether, polyoxyethylene tridecyl ether, polyoxyalkylene tridecyl ether, polyoxyethylene myristyl ether, polyoxyethylene cetyl ether, polyoxyethylene oleyl ether, polyoxyethylene stearyl ether, polyoxyethylene behenyl ether, polyoxyethylene-2-ethylhexyl ether, and polyoxyethylene isodecyl ether.
[0115] Examples of polyoxyethylene alkylphenol ethers include polyoxyethylene styrenated phenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene distyrenated phenyl ether, and polyoxyethylene tribenzyl phenyl ether.
[0116] The alkyl glucoside includes decyl glucoside and lauryl glucoside.
[0117] Examples of polyoxyethylene fatty acid esters include polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyethylene monooleate, polyethylene glycol distearate, polyethylene glycol dioleate, and polypropylene glycol dioleate.
[0118] Examples of sorbitan fatty acid esters include sorbitan monocaprylate, sorbitan monolaurate, sorbitan monomyristate, sorbitan monopalmitate, sorbitan monostearate, sorbitan distearate, sorbitan tristearate, sorbitan monooleate, sorbitan trioleate, sorbitan monosesquioleate, and ethylene oxide adducts thereof.
[0119] Examples of polyoxyethylene sorbitan fatty acid esters include polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan tristearate, polyoxyethylene sorbitan monooleate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan triisostearate.
[0120] Examples of fatty acid alkanolamides include coconut oil fatty acid diethanolamide, beef tallow fatty acid diethanolamide, lauric acid diethanolamide, and oleic acid diethanolamide.
[0121] Further examples include polyoxyalkyl ethers or polyoxyalkyl glycols such as polyoxyethylene polyoxypropylene glycol, polyoxyethylene fatty acid esters, polyoxyethylene hydrogenated castor oil ether, sorbitan fatty acid ester alkyl ethers, alkyl polyglucosides, sorbitan monooleate, and sucrose fatty acid esters.
[0122] Silicone-based surfactants can be used. Silicone-based surfactants are compounds having a repeating unit containing a siloxane bond in the main chain. The weight-average molecular weight of the silicone-based surfactants can be in the range of 500 to 50,000. These may be modified silicone-based surfactants, and examples of such surfactants include structures in which an organic group is introduced into the side chain and / or end of a polysiloxane. Examples of the organic group include amino groups, epoxy groups, alicyclic epoxy groups, carbinol groups, mercapto groups, carboxyl groups, aliphatic ester groups, aliphatic amide groups, and polyether groups. Examples of silicone-based surfactants include those under the trade names of Toray Silicone DC3PA, Toray Silicone SH7PA, Toray Silicone DC11PA, Toray Silicone SH21PA, Toray Silicone SH28PA, Toray Silicone SH29PA, Toray Silicone SH30PA, and Toray Silicone SH8400 (all manufactured by Toray Dow Corning Co., Ltd.), Silwet Examples of suitable polyether-modified silicones include L-77, L-7280, L-7001, L-7002, L-7200, L-7210, L-7220, L-7230, L7500, L-7600, L-7602, L-7604, L-7605, L-7622, L-7657, L-8500, and L-8610 (all manufactured by Momentive Performance Materials, Inc.), KP-341, KF-6001, and KF-6002 (all manufactured by Shin-Etsu Silicone Co., Ltd.), BYK307, BYK323, and BYK330 (all manufactured by BYK-Chemie Co., Ltd.). For example, the trade name L-7001 (manufactured by DOWSIL Co., Ltd.) can be suitably used as the polyether-modified silicone.
[0123] In the present invention, a film-forming composition containing the above organic solvent sol and an organic resin is obtained. The film-forming composition can be obtained by removing the organic solvent from the organic solvent sol to form a film-forming composition containing modified metal oxide particles (iii) and an organic resin.
[0124] In the case of the thermosetting coating composition, the heat curing agent can be added in the range of 0.01 to 50 phr or 0.01 to 10 phr to the resin containing a functional group such as an epoxy group or a (meth)acryloyl group, and for example, the heat curing agent can be contained in a ratio of 0.5 to 1.5 equivalents, preferably 0.8 to 1.2 equivalents to the functional group such as an epoxy group or a (meth)acryloyl group. The equivalent of the heat curing agent to the curable resin is represented by the equivalent ratio of the heat curing agent to the functional group.
[0125] Examples of the heat curing agent include phenol resins, amine-based curing agents, polyamide resins, imidazoles, polymercaptans, acid anhydrides, heat radical generators, heat acid generators, etc. In particular, radical generator-based curing agents, acid anhydride-based curing agents, and amine-based curing agents are preferred.
[0126] Even if these thermosetting agents are solid, they can be used by dissolving them in a solvent. However, evaporation of the solvent reduces the density of the cured product and creates pores, resulting in reduced strength and reduced water resistance. Therefore, it is preferable for the curing agent itself to be liquid at room temperature and normal pressure.
[0127] Examples of the phenol resin include phenol novolac resin and cresol novolac resin.
[0128] Examples of the amine curing agent include piperidine, N,N-dimethylpiperazine, triethylenediamine, 2,4,6-tris(dimethylaminomethyl)phenol, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, N-aminoethylpiperazine, di(1-methyl-2-aminocyclohexyl)methane, menthenediamine, isophoronediamine, diaminodicyclohexylmethane, 1,3-diaminomethylcyclohexane, xylylenediamine, metaphenylenediamine, diaminodiphenylmethane, diaminodiphenylsulfone, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and diethyltoluenediamine. Of these, liquid diethylenetriamine, triethylenetetramine, tetraethylenepentamine, diethylaminopropylamine, N-aminoethylpiperazine, di(1-methyl-2-aminocyclohexyl)methane, menthenediamine, isophoronediamine, diaminodicyclohexylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, diethyltoluenediamine, etc. can be preferably used.
[0129] The polyamide resin is produced by condensation of dimer acid and polyamine, and is a polyamide amine having a primary amine and a secondary amine in the molecule.
[0130] Examples of the imidazoles include 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and epoxy imidazole adduct.
[0131] The polymercaptan is, for example, one having a mercaptan group at the end of a polypropylene glycol chain or one having a mercaptan group at the end of a polyethylene glycol chain, and is preferably in a liquid form.
[0132] As the acid anhydride curing agent, the anhydride of the compound having a plurality of carboxyl groups in one molecule is preferable.As these acid anhydride curing agents, phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenone tetracarboxylic anhydride, ethylene glycol bis trimellitate, glycerol tris trimellitate, maleic anhydride, tetrahydrophthalic anhydride, methyl tetrahydrophthalic anhydride, endomethylene tetrahydrophthalic anhydride, methyl endomethylene tetrahydrophthalic anhydride, methyl butenyl tetrahydrophthalic anhydride, dodecenyl succinic anhydride, hexahydrophthalic anhydride, methyl hexahydrophthalic anhydride, succinic anhydride, methylcyclohexene dicarboxylic anhydride, chlorendic anhydride, etc. can be mentioned.
[0133] Examples of the thermal acid generator include sulfonium salts and phosphonium salts, and sulfonium salts are preferably used. For example, the following compounds can be mentioned.
[0134] [ka]
[0135] R may be an alkyl group having 1 to 12 carbon atoms or an aryl group having 6 to 20 carbon atoms, and is particularly preferably an alkyl group having 1 to 12 carbon atoms.
[0136] Among these, methyltetrahydrophthalic anhydride, methyl-5-norbornene-2,3-dicarboxylic anhydride (methylnadic anhydride, methylhimic anhydride), hydrogenated methylnadic anhydride, methylbutenyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, methylhexahydrophthalic anhydride, and a mixture of methylhexahydrophthalic anhydride and hexahydrophthalic anhydride, which are liquid at room temperature and normal pressure, are preferred. These liquid acid anhydrides have a viscosity of about 10 to 1,000 mPa s when measured at 25°C.
[0137] Examples of the thermal radical generator include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methylpropionate)dimethyl, 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, tert-butyl hydroperoxide, cumene hydroperoxide, di-tert-butyl peroxide, dicumyl peroxide, and benzoyl peroxide. These can be obtained from Tokyo Chemical Industry Co., Ltd.
[0138] In addition, when obtaining the above-mentioned cured product, a curing assistant may be used in combination as appropriate. Examples of the curing assistant include organic phosphorus compounds such as triphenylphosphine and tributylphosphine, quaternary phosphonium salts such as ethyltriphenylphosphonium bromide and methyltriphenylphosphonium diethyl phosphate, and quaternary ammonium salts such as 1,8-diazabicyclo(5,4,0)undecane-7-ene, salts of 1,8-diazabicyclo(5,4,0)undecane-7-ene and octylic acid, zinc octylate, and tetrabutylammonium bromide. These curing assistants can be contained in a ratio of 0.001 to 0.1 parts by mass relative to 1 part by mass of the curing agent.
[0139] The composition is a thermosetting varnish obtained by mixing a resin, a curing agent, and optionally a curing aid. The mixing can be carried out in a reaction vessel using a stirring blade or a kneader. The mixing is carried out by a hot mixing method at a temperature of 60 to 100°C for 0.5 to 1 hour.
[0140] The obtained curable film-forming composition is a thermosetting coating composition, and has a suitable viscosity for use as, for example, a liquid sealant. The liquid thermosetting film-forming composition can be prepared to any viscosity, and can be partially sealed at any location for use as a transparent sealant for LEDs, etc., by casting, potting, dispenser, printing, etc. The liquid thermosetting composition is directly mounted on an LED, etc., in the liquid state, by the above-mentioned method, and then dried and cured to obtain a cured epoxy resin body.
[0141] The thermosetting film-forming composition (thermosetting coating composition) is applied to a substrate and heated at a temperature of 80 to 200° C. to obtain a cured product.
[0142] In the case of the photocurable resin composition in the above-mentioned film-forming composition, a photocuring agent (photoradical generator, photoacid generator) can be added in the range of 0.01 to 50 phr or 0.01 to 10 phr to a resin containing a functional group such as an epoxy group or a (meth)acryloyl group, and for example, the photocuring agent (photoradical generator, photoacid generator) can be contained in a ratio of 0.5 to 1.5 equivalents, preferably 0.8 to 1.2 equivalents, to a functional group such as an epoxy group or a (meth)acryloyl group. The equivalent of the photocuring agent to the curable resin is represented by the equivalent ratio of the photocuring agent to the functional group.
[0143] The photoradical generator is not particularly limited as long as it generates radicals directly or indirectly upon irradiation with light.
[0144] Examples of photoradical generators include photoradical polymerization initiators, such as imidazole compounds, diazo compounds, bisimidazole compounds, N-arylglycine compounds, organic azide compounds, titanocene compounds, aluminate compounds, organic peroxides, N-alkoxypyridinium salt compounds, and thioxanthone compounds. Examples of azide compounds include p-azidobenzaldehyde, p-azidoacetophenone, p-azidobenzoic acid, p-azidobenzalacetophenone, 4,4'-diazidochalcone, 4,4'-diazidodiphenyl sulfide, and 2,6-bis(4'-azidobenzal)-4-methylcyclohexanone. Examples of the diazo compound include 1-diazo-2,5-diethoxy-4-p-tolylmercaptobenzene borofluoride, 1-diazo-4-N,N-dimethylaminobenzene chloride, and 1-diazo-4-N,N-diethylaminobenzene borofluoride. Examples of the bisimidazole compound include 2,2'-bis(o-chlorophenyl)-4,5,4',5'-tetrakis(3,4,5-trimethoxyphenyl)-1,2'-bisimidazole, and 2,2'-bis(o-chlorophenyl)-4,5,4',5'-tetraphenyl-1,2'-bisimidazole.Titanocene compounds include dicyclopentadienyl-titanium-dichloride, dicyclopentadienyl-titanium-bisphenyl, dicyclopentadienyl-titanium-bis(2,3,4,5,6-pentafluorophenyl), dicyclopentadienyl-titanium-bis(2,3,5,6-tetrafluorophenyl), dicyclopentadienyl-titanium-bis(2,4,6-trifluorophenyl), dicyclopentadienyl-titanium-bis(2,6-difluorophenyl), dicyclopentadienyl Examples of such aryl groups include dicyclopentadienyl-titanium-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl), dicyclopentadienyl-titanium-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl), dicyclopentadienyl-titanium-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl), and dicyclopentadienyl-titanium-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl).
[0145] Further examples of photoradical generators include 1,3-di(tert-butyldioxycarbonyl)benzophenone, 3,3',4,4'-tetrakis(tert-butyldioxycarbonyl)benzophenone, 3-phenyl-5-isoxazolone, 2-mercaptobenzimidazole, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone.
[0146] These photoradical polymerization agents are available, for example, under the trade name Irgacure TPO (the component is 2,4,6-trimethylbenzoyldiphenylphosphine oxide) (c1-1-1) manufactured by BASF, under the trade name Omnirad819 (the component is bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide) (c1-1-2) manufactured by IGM RESINS, and under the trade name Irgacure 184 (the component is 1-hydroxycyclohexyl phenyl ketone) (c1-1-3) manufactured by IGM RESINS.
[0147] [ka]
[0148] The photoacid generator is not particularly limited as long as it generates an acid directly or indirectly by irradiation with light.Specific examples of the photoacid generator include triazine compounds, acetophenone derivative compounds, disulfone compounds, diazomethane compounds, sulfonic acid derivative compounds, onium salts such as iodonium salts, sulfonium salts, phosphonium salts, and selenium salts, metallocene complexes, and iron arene complexes.
[0149] The onium salt used as the photoacid generator includes, as an iodonium salt, for example, diphenyliodonium chloride, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium mesylate, diphenyliodonium tosylate, diphenyliodonium bromide, diphenyliodonium tetrafluoroborate, diphenyliodonium hexafluoroantimonate, diphenyliodonium hexafluoroarsenate, bis(p-tert-butylphenyl)iodonium hexafluorophosphate, bis(p-tert-butylphenyl)iodonium mesylate, bis(p-tert-butylphenyl)iodonium tosylate, bis(p-tert-butylphenyl)iodonium trifluoromethanesulfonate, bis(p-tert-butylphenyl)iodonium trifluoromethanesulfonate, )iodonium tetrafluoroborate, bis(p-tert-butylphenyl)iodonium chloride, bis(p-chlorophenyl)iodonium chloride, bis(p-chlorophenyl)iodonium tetrafluoroborate, further bis(alkylphenyl)iodonium salts such as bis(4-t-butylphenyl)iodonium hexafluorophosphate, alkoxycarbonylalkoxy-trialkylaryliodonium salts (e.g., 4-[(1-ethoxycarbonyl-ethoxy)phenyl]-(2,4,6-trimethylphenyl)-iodonium hexafluorophosphate, etc.), bis(alkoxyaryl)iodonium salts (e.g., bis(alkoxyphenyl)iodonium salts such as (4-methoxyphenyl)phenyliodonium hexafluoroantimonate, etc.).
[0150] Examples of the sulfonium salt include triphenylsulfonium salts such as triphenylsulfonium chloride, triphenylsulfonium bromide, tri(p-methoxyphenyl)sulfonium tetrafluoroborate, tri(p-methoxyphenyl)sulfonium hexafluorophosphonate, tri(p-ethoxyphenyl)sulfonium tetrafluoroborate, triphenylsulfonium triflate, triphenylsulfonium hexafluoroantimonate, and triphenylsulfonium hexafluorophosphate; and sulfonium salts such as (4-phenylthiophenyl)diphenylsulfonium hexafluoroantimonate, (4-phenylthiophenyl)diphenylsulfonium hexafluorophosphate, bis[4-(diphenylsulfonio)phenyl]sulfide-bis-hexafluoroantimonate, bis[4-(diphenylsulfonio)phenyl]sulfide-bis-hexafluorophosphate, and (4-methoxyphenyl)diphenylsulfonium hexafluoroantimonate.
[0151] Examples of the phosphonium salt include triphenylphosphonium chloride, triphenylphosphonium bromide, tri(p-methoxyphenyl)phosphonium tetrafluoroborate, tri(p-methoxyphenyl)phosphonium hexafluorophosphonate, tri(p-ethoxyphenyl)phosphonium tetrafluoroborate, 4-chlorobenzenediazonium hexafluorophosphate, and benzyltriphenylphosphonium hexafluoroantimonate.
[0152] Examples include selenium salts such as triphenylselenium hexafluorophosphate, and metallocene complexes such as (η5 or η6-isopropylbenzene)(η5-cyclopentadienyl)iron(II) hexafluorophosphate.
[0153] In addition, the following compounds can also be used as the photoacid generator.
[0154] [ka]
[0155] [ka]
[0156] [ka]
[0157] [ka]
[0158] [ka]
[0159] [ka]
[0160] [ka]
[0161] [ka]
[0162] [ka]
[0163] As the photoacid generator, sulfonium salt compounds and iodonium salt compounds are preferred. The anion species thereof is CF3SO3 - , C4F9SO3 - , C8F 17 SO3 - , camphorsulfonate anion, tosylate anion, BF4 - , PF6 - , AsF6 -and SbF6 - In particular, anion species such as phosphorus hexafluoride and antimony hexafluoride, which exhibit strong acidity, are preferred.
[0164] The film-forming composition of the present invention may contain conventional additives as necessary. Examples of such additives include pigments, colorants, thickeners, sensitizers, defoamers, coating improvers, lubricants, stabilizers (antioxidants, heat stabilizers, light resistance stabilizers, etc.), plasticizers, dissolution promoters, fillers, antistatic agents, etc. These additives may be used alone or in combination of two or more.
[0165] Examples of methods for applying the coating composition of the present invention include flow coating, spin coating, spray coating, screen printing, casting, bar coating, curtain coating, roll coating, gravure coating, dipping, and slit coating.
[0166] In the present invention, the photo-coating composition (film-forming composition) can be applied onto a substrate and cured by light irradiation, or can be heated before or after light irradiation.
[0167] The thickness of the coating film can be selected from the range of about 0.01 μm to 10 mm depending on the application of the cured product; for example, when used as a photoresist, it can be about 0.05 to 10 μm (particularly 0.1 to 5 μm), when used as a printed wiring board, it can be about 5 μm to 5 mm (particularly 100 μm to 1 mm), and when used as an optical thin film, it can be about 0.1 to 100 μm (particularly 0.3 to 50 μm).
[0168] When a transparent coating is obtained, the coating can have a visible light transmittance of 80% or more, or 90% or more, typically 90 to 96%.
[0169] When a photoacid generator is used, the light to be irradiated or exposed to may be, for example, gamma rays, X-rays, ultraviolet rays, visible light, etc., and is usually visible light or ultraviolet rays, particularly ultraviolet rays. The wavelength of the light is, for example, about 150 to 800 nm, preferably about 150 to 600 nm, and more preferably about 150 to 400 nm. The amount of irradiation light varies depending on the thickness of the coating film, but is, for example, 2 to 20,000 mJ / cm. 2 , preferably 5 to 5,000 mJ / cm 2 The light source can be selected according to the type of light to be exposed, and for example, in the case of ultraviolet light, a low pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a deuterium lamp, a halogen lamp, or laser light (helium-cadmium laser, excimer laser, etc.) can be used. Such light irradiation causes the curing reaction of the composition to proceed.
[0170] When a thermal acid generator is used or when a photoacid generator is used, the coating film is heated as necessary after light irradiation, for example, at 60 to 350° C., preferably about 100 to 300° C. The heating time can be selected within a range of 3 seconds or more (for example, about 3 seconds to 5 hours), for example, 5 seconds to 2 hours, preferably about 20 seconds to 30 minutes, and usually about 1 minute to 3 hours (for example, about 5 minutes to 2.5 hours).
[0171] Furthermore, when forming a pattern or an image (for example, when manufacturing a printed wiring board or the like), the coating film formed on the substrate may be pattern-exposed, and this pattern exposure may be performed by scanning with laser light or by irradiating light through a photomask. A pattern or an image can be formed by developing (or dissolving) the non-irradiated area (unexposed part) generated by such pattern exposure with a developer.
[0172] The developer may be an aqueous alkaline solution or an organic solvent.
[0173] Examples of the alkaline aqueous solution include aqueous solutions of alkali metal hydroxides such as potassium hydroxide, sodium hydroxide, potassium carbonate, and sodium carbonate; aqueous solutions of quaternary ammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline; and aqueous solutions of amines such as ethanolamine, propylamine, and ethylenediamine.
[0174] The alkaline developer is generally an aqueous solution of 10% by mass or less, and preferably an aqueous solution of 0.1 to 3.0% by mass, etc. Furthermore, alcohols and surfactants can be added to the developer, and each of these is preferably 0.05 to 10 parts by mass relative to 100 parts by mass of the developer.
[0175] Of these, an aqueous solution of 0.1 to 2.38 mass % tetramethylammonium hydroxide can be used.
[0176] In addition, the organic solvent used as the developer can be a general organic solvent, such as acetone, acetonitrile, toluene, dimethylformamide, methanol, ethanol, isopropanol, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, propylene glycol butyl ether, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, propylene glycol butyl ether acetate, ethyl lactate, cyclohexanone, etc. These can be used alone or as a mixture of two or more. In particular, propylene glycol methyl ether, propylene glycol methyl ether acetate, ethyl lactate, etc. can be preferably used.
[0177] In the present invention, an adhesion promoter can be added for the purpose of improving adhesion to the substrate after development. These adhesion promoters include chlorosilanes such as trimethylchlorosilane, dimethylvinylchlorosilane, methyldiphenylchlorosilane, and chloromethyldimethylchlorosilane, alkoxysilanes such as trimethylmethoxysilane, dimethyldiethoxysilane, methyldimethoxysilane, dimethylvinylethoxysilane, diphenyldimethoxysilane, and phenyltriethoxysilane, silazanes such as hexamethyldisilazane, N,N'-bis(trimethylsilyl)urea, dimethyltrimethylsilylamine, and trimethylsilylimidazole, vinyltrichlorosilane, 3-chloropropyltrimethoxysilane, 3-chloropropyltrimethoxysilane, and 3-chloropropyltrimethoxysilane. silanes such as 3-aminopropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-(N-piperidinyl)propyltrimethoxysilane, heterocyclic compounds such as benzotriazole, benzimidazole, indazole, imidazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, urazole, thiouracil, mercaptoimidazole, mercaptopyrimidine, urea such as 1,1-dimethylurea, 1,3-dimethylurea, or thiourea compounds. The adhesion promoters may be used alone or in combination of two or more. The amount of these adhesion promoters added is usually 18% by mass or less, preferably 0.0008 to 9% by mass, more preferably 0.04 to 9% by mass, based on the solid content.
[0178] The present invention may contain a sensitizer. Examples of sensitizers that can be used include anthracene, phenothiazene, perylene, thioxanthone, and benzophenone thioxanthone. Examples of sensitizing dyes include thiopyrylium salt dyes, merocyanine dyes, quinoline dyes, styrylquinoline dyes, ketocoumarin dyes, thioxanthene dyes, xanthene dyes, oxonol dyes, cyanine dyes, rhodamine dyes, and pyrylium salt dyes. Anthracene sensitizers are particularly preferred, and when used in combination with a cationic curing catalyst (radiation-sensitive cationic polymerization initiator), they dramatically improve sensitivity and also have a radical polymerization initiation function, and in the hybrid type in which the cationic curing system of the present invention and the radical curing system are used in combination, the catalyst species can be simplified. Specific examples of anthracene compounds that are effective include dibutoxyanthracene and dipropoxyanthraquinone. The amount of the sensitizer added is 0.01 to 20% by mass, preferably 0.01 to 10% by mass, based on the solid content.
[0179] The composition of the present invention can be photocured or thermally cured using a photoradical generator, a thermal radical generator, a photoacid generator, or a thermal acid generator. When a photoacid generator or a thermal acid generator is used, for example, commonly used epoxy curing agents (e.g., amines and acid anhydrides) are not used, or even if they are used, the content of these agents is extremely small, so that the storage stability of the composition is improved.
[0180] The above composition has been found to be applicable to photocationic polymerization. It has a higher curing speed than conventional liquid epoxy compounds (e.g., alicyclic epoxy compounds having an epoxycyclohexyl ring). Because of the fast curing speed, it is possible to reduce the amount of acid generator added and to use weak acid generators. Reducing the amount of acid generator is important for preventing metal corrosion, as active acid species may remain even after UV irradiation. Because of the fast curing speed, thick film curing is possible.
[0181] Curing by UV irradiation can be applied to materials (equipment) that are sensitive to heat. In the present invention, an antistatic composition can be produced containing the modified metal oxide particles (iii) in the modified metal oxide sol. In addition, in the present invention, a composition for an electron transport material can be produced which contains the modified metal oxide particles (iii) in the modified metal oxide sol. A coating agent in which the amount of modified metal oxide particles (iii) derived from the modified metal oxide sol is mixed in an amount of 300 phr with respect to a resin varnish serving as a binder component is applied to a substrate so that the coating film after drying has a thickness of 1.0 μm. When a voltage of 1,000 V is applied, the coating exhibits a surface resistance value of 10 to 500 giga Ω / □. EXAMPLES
[0182] The physical properties of the sol (dispersion) were determined by the following measuring methods.
[0183] [Average primary particle size] The particles were photographed using a transmission electron microscope (manufactured by JEOL Ltd., product name JEM-F200), and the average value of the primary particle diameters of 500 randomly selected particles equivalent to a circle was taken as the average primary particle diameter.
[0184] [Average particle size by dynamic light scattering (dynamic light scattering particle size)] The sol was diluted with a dispersion solvent, and the parameters of the solvent were used to perform measurement using a dynamic light scattering measurement device (manufactured by Malvern Instruments Ltd., trade name: Zetasizer).
[0185] [Stability] After storing the dispersion at 50°C for one week, samples in which the particle size measured by dynamic light scattering (DLS) was less than 1.2 times that before the storage test were marked with an "O" (good), and samples in which the particle size measured by dynamic light scattering (DLS) had changed by 1.2 times or more compared to that before the storage test were marked with an "X".
[0186] [Measurement of Amine Amount] The amount of amine in the sol obtained in the examples and comparative examples was measured by the following procedures 1) to 3). 1) Preparation of standard samples for calibration curve Standard samples of isopropylamine and diisopropylamine were prepared by diluting with 3 mM nitric acid to concentrations of 10 ppm, 100 ppm, and 1000 ppm, respectively. Standard samples of tri-n-pentylamine were prepared by diluting with 3 mM nitric acid containing 20% by mass of acetonitrile so that the tri-n-pentylamine concentrations were 100 ppm, 1,000 ppm, and 1% by mass. 2) Preparation of samples for quantifying the amount of amine in the sols obtained in the examples and comparative examples The sol obtained in the examples and comparative examples was diluted with pure water so that the concentration of colloidal particles was 3% by mass. 0.2 mL of 1 M nitric acid was added to 8.5 g of the diluted sol, and the mixture was left to stand at room temperature for 24 hours to peel off the amine adsorbed on the particle surface from the particle surface. The obtained solution was then centrifuged using a centrifugal ultrafiltration filter unit with a molecular weight cutoff of 10,000 Da to recover the filtrate. The recovered filtrate was diluted 10 times with pure water to prepare a sample for quantifying the amount of amine in the sol obtained in the examples and comparative examples. 3) Calculation of the amount of amine in the sol obtained in the examples and comparative examples The samples prepared in 1) and 2) were measured using an ion chromatograph (Metrohm Compact IC 761, manufactured by Metrohm Japan Co., Ltd.). A calibration curve was created by plotting the peak integral intensity of the standard samples of isopropylamine, diisopropylamine, and tri-n-pentylamine prepared in 1) against the respective amine concentrations. The amount of amine contained in the sample prepared in 2) was calculated using the created calibration curve.
[0187] [Measurement of Crystallinity] The crystallinity of the modified metal oxide particles in the sol obtained in the Examples and Comparative Examples was measured by the following procedures 1) to 3). 1) X-ray diffraction measurement of modified metal oxide particles in the sol obtained in the examples and comparative examples The sol in which the modified metal oxide particles obtained in the examples were dispersed was vacuum dried at 60° C. for 1 hour. The obtained dried powder was placed in a mortar and crushed with a pestle. The crushed particles were mixed with tungsten powder (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., containing 99.9% by mass or more of tungsten) in a mass ratio of 50:50. The X-ray diffraction of the mixed powder was measured using an X-ray diffractometer (manufactured by Rigaku Corporation, product name MiniFlex600). 2) X-ray diffraction measurement of tin(IV) oxide standard sample Tin(IV) oxide powder (Kanto Chemical Co., Ltd., containing 99.0% or more by mass as SnO2) and tungsten powder (FUJIFILM Wako Pure Chemical Industries, Ltd., containing 99.9% or more by mass as tungsten) were mixed in a mass ratio of 50:50. X-ray diffraction of the mixed powder was measured using an X-ray diffractometer (Rigaku Corporation, product name MiniFlex600). 3) Calculation of crystallinity The sum of the integrated peak intensities of the tin(IV) oxide (110), (101), (200), (211), and (220) peaks contained in the modified metal oxide particles measured in 1) is A S1 , and tungsten (110) peak integrated intensity A W1 Next, the sum A of the integrated peak intensities of the tin(IV) oxide (110), (101), (200), (211), and (220) measured in 2) was calculated. S2 , and tungsten (110) peak integrated intensity A W2 The crystallinity of the modified metal oxide particles obtained in the examples and comparative examples was calculated from the following formula. Crystallinity=(A S1 / A W1 ) / (A S2 / A W2 )
[0188] [Measurement of refractive index] The refractive index of the modified metal oxide in the sol obtained in the Examples and Comparative Examples was measured by the following procedures 1) to 3). 1) Preparation of varnish containing methanol-dispersed sol of modified metal oxide 20.00 g of 3-glycidoxypropyltrimethoxysilane (manufactured by Momentive, product name SILQUEST A-187T) was weighed into a plastic container, 18.57 g of methanol and 4.57 g of 0.01N hydrochloric acid solution were added thereto, and the mixture was stirred at room temperature for 5 hours. 6.00 g of a methanol solution (10% by mass Al(acac)3) of aluminum 2,4-pentanedionate (Al(acac)3) prepared in advance was added as a curing agent, and the mixture was stirred for 10 minutes to prepare a partial hydrolyzate of 3-glycidoxypropyltrimethoxysilane (concentration: 43% by mass). The prepared partial hydrolysate of 3-glycidoxypropyltrimethoxysilane, modified metal oxide dispersion sol, water, methanol, and 0.25 g of a methanol solution (10 mass% L-7604) of a leveling agent (DOWSIL product name L-7604) were weighed into a brown bottle so that the total amount was 25.00 g, the final solvent composition was the sum of water / solvents other than water = 1 / 4 by mass, and the amount of modified metal oxide in the methanol dispersion sol was 50 phr, 100 phr, and 150 phr, and the mixture was stirred at room temperature for 30 minutes to prepare a varnish containing modified metal oxide methanol dispersion sol (solid concentration was 10.0 mass%, amount of modified metal oxide: 50 phr, 100 phr, and 150 phr). 2) Preparation of particle-containing membrane Approximately 0.5 mL of the modified metal oxide methanol dispersion sol-blended varnish obtained in 1) was dropped onto a UV-O3-treated Si substrate, and coated with a spin coater (Mikasa Co., Ltd., product name Opticoat MS-B100) so that the film thickness after coating was 1.0 μm. After that, it was baked on a hot plate at 80°C for 5 minutes, and heat-treated in an oven at 120°C for 1 hour to prepare a particle-blended film (particle blend amount: 50 phr, 100 phr, 150 phr). 3) Measurement of the refractive index of a film containing particles and calculation of the refractive index of the particles The refractive index of the particle-blended films obtained in 2) (particle blend amounts: 50 phr, 100 phr, 150 phr) was measured using an ellipsometer (product name: Multi-angle Spectroscopic Ellipsometer VASE, manufactured by J.A. Woollam Japan, Inc.). The refractive index of a film containing no particles, which was prepared in the same manner using only the partial hydrolysate of 3-glycidoxypropyltrimethoxysilane, was also measured. The measured refractive index of the blended film was plotted against the particle blend amount, and the refractive index of the particles was calculated by extrapolating so that the particle blend amount was 100 mass%.
[0189] [Measurement of resistivity value] The resistivity of the films containing the particles obtained in the examples and comparative examples was measured by the following procedures 1) to 3). 1) Preparation of varnish containing modified metal oxide dispersion sol 37.50 g of 3-glycidoxypropyltrimethoxysilane (manufactured by Momentive, product name SILQUEST A-187T) was weighed into a plastic container, 8.57 g of 0.01N hydrochloric acid solution was added thereto, and the mixture was stirred at room temperature for 24 hours. 4.61 g of the resulting solution was weighed into a plastic container, 0.23 g of aluminum 2,4-pentanedionate (Al(acac)3) was added as a curing agent, and 0.50 g of a methanol solution (10 mass% L-7604) of a leveling agent (Dowsil product name L-7604) was added. Next, the modified metal oxide dispersion sol obtained in the examples and comparative examples, water, and methanol were added so that the final solvent composition was water / solvent other than water = 1 / 4 by mass, and the amount of modified metal oxide was 300 phr, and the mixture was stirred at room temperature for 24 hours to prepare a varnish containing modified metal oxide dispersion sol (solid concentration: 15.0 mass%, amount of modified metal oxide: 300 phr). 2) Preparation of particle-containing membrane Approximately 1 mL of the modified metal oxide dispersion sol-containing varnish obtained in 1) was dropped onto a quartz substrate treated with UV-O3, and coated with a tabletop wire bar coater (manufactured by MST Corporation, product name PM-9050MC) so that the film thickness after drying would be 1.0 μm. After that, it was baked on a hot plate at 80°C for 15 minutes, and then heat-treated in an oven at 120°C for 2 hours to prepare a particle-containing film. 3) Measurement of resistivity of particle-mixed film The surface resistance of the particle-blended film (particle blending amount: 300 phr) obtained in 2) was measured with a resistivity meter (Mitsubishi Chemical Corporation, product name Hiresta-UP MCP-HT450) under conditions of a voltage of 1,000 V and a time of 10 seconds. The unit is Ω / □ (ohms per square).
[0190] [Qualitative and quantitative determination of stannic oxide and other metal oxides] The particles obtained in the Examples and Comparative Examples were qualitatively and quantitatively measured for stannic oxide and other metal oxides contained in the blend by the following procedures 1) to 3). 1) X-ray fluorescence analysis of standard samples Tin(IV) oxide powder (Kanto Chemical Co., Ltd., containing 99.0% by mass or more as SnO2), antimony(V) oxide powder (Sigma-Aldrich, containing 99.9% by mass or more as Sb2O5), and silica powder (Nissan Chemical Co., Ltd., product name ST-XS, vacuum dried at 60°C for 1 hour, and the obtained dried powder was placed in a mortar and crushed with a pestle) were mixed in a mass ratio of SnO2 / Sb2O5 / SiO2=1 / 1 / 1. The obtained powder was measured using a fluorescent X-ray analyzer (Rigaku Co., Ltd., product name Supermini200). Peak integrated intensity A derived from tin(IV) oxide Sn1 , the integrated intensity A of the peak due to antimony (V) oxide Sb1 , and the integrated intensity A of the peak derived from silica Si1 was calculated. 2) X-ray fluorescence analysis of modified metal oxides in the sols obtained in the examples and comparative examples The sols in which the modified metal oxides were dispersed obtained in the Examples and Comparative Examples were vacuum dried at 60° C. for 1 hour. The obtained dried powder was placed in a mortar and crushed with a pestle. The crushed particles were measured using a fluorescent X-ray analyzer (manufactured by Rigaku Corporation, product name Supermini200). 3) Qualitative and quantitative analysis of stannic oxide and other metal oxides If the peak wavelength of the fluorescent X-ray measured in 2) was the same as the peak wavelength of the standard sample measured in 1), it was determined that the sample contained a metal oxide originating from that peak wavelength. Next, the peak integrated intensity A of the fluorescent X-ray measured in 2) originating from tin (IV) oxide was Sn2 , the integrated intensity A of the peak due to antimony (V) oxide Sb2 , and the integrated intensity A of the peak derived from silica Si2 The amounts of stannic oxide and other metal oxides contained in the modified metal oxides obtained in the Examples and Comparative Examples were determined using the following calculation formula. Stannic oxide content = (A Sn2 / A Sn1 ) / A TOTAL Antimony oxide (V) content = (A Sb2 / A Sb1 ) / A TOTAL Silica content = (A Si2 / A Si1 ) / A TOTAL Here, A TOTAL =(A Sn2 / A Sn1 )+(A Sb2 / A Sb1 )+(A Si2 / A Si1 )
[0191] (Reference Example 1) Preparation of stannic oxide composite oxide colloidal particles (i) as cores 37.5 kg of oxalic acid ((COOH)2·2H2O) was dissolved in 363 kg of pure water, which was heated to 70°C with stirring, and 170 kg of 35% hydrogen peroxide and 75 kg of metallic tin were added. The hydrogen peroxide and metallic tin were added alternately. First, 10 kg of 35% hydrogen peroxide was added, followed by 5 kg of metallic tin. This operation was repeated after waiting for the reaction to finish (5-10 minutes). After the entire amount had been added, an additional 10 kg of 35% hydrogen peroxide was added. The addition took 3 hours, and after the addition was finished, the mixture was heated at 95°C for an additional hour to finish the reaction. 231 kg of 35% hydrogen peroxide and 52 kg of pure water were added to 629 kg of the obtained sol, and the mixture was diluted to 10 mass% SnO2 and 8.0 molar ratio of H2O2 / (COOH)2 relative to the oxalic acid at the time of preparation, and aged at 95°C for 5 hours. This operation decomposed the contained oxalic acid into carbon dioxide and water by reaction with hydrogen peroxide. After cooling the obtained stannic oxide slurry to about 40°C, 2.7 kg of isopropylamine (water solubility 1,000g / L, quoted from data listed in Chemical Book. This can be found on the website at the following URL: https: / / www.chemicalbook.com / ProductList_En.aspx?kwd=isopropylamine) was added, and the mixture was peptized. The mixture was then passed through and circulated in a catalyst tower filled with about 15L of platinum-based catalyst (N-220 (manufactured by Süd-Chemie Catalyst Co., Ltd.)) to decompose the excess hydrogen peroxide. The solution was circulated at a flow rate of about 30 L / min for 5 hours, and then passed through a column packed with anion exchange resin, after which it was concentrated by ultrafiltration. The obtained sol was a water-dispersed sol of stannic oxide colloidal particles (i), with a pH of 11.0, an SnO2 concentration of 10.0 mass%, and a primary particle diameter of 10-15 nm as observed by a transmission electron microscope.
[0192] (Reference Example 2) Preparation of silicon dioxide-stannic oxide composite oxide colloidal particles (ii-2) to be used as the coating material 77.2 g of JIS No. 3 sodium silicate (containing 29.8% by mass in terms of SiO2) was dissolved in 668.8 g of pure water, and then 20.9 g of sodium stannate NaSnO3·H2O (containing 55.1% by mass in terms of SnO2) was dissolved. The resulting aqueous solution was passed through a column filled with hydrogen-type cation exchange resin. Next, 7.2 g of diisopropylamine (water solubility 100 g / L, cited from data listed in Chemical Book. This can be found on the website at the following URL: https: / / www.chemicalbook.com / ProductList_En.aspx?kwd=108-18-9) was added to the resulting aqueous dispersion sol. The resulting sol was an aqueous dispersion sol of silicon dioxide-stannic oxide composite oxide colloidal particles (ii-2), with a pH of 8.0, a total metal oxide concentration (SnO2 and SnO2) of 2.5% by mass, and a primary particle diameter of 1 to 4 nm as observed by a transmission electron microscope.
[0193] (Reference Example 3) Preparation of antimony pentoxide colloidal particles (ii-1) to be used as coating material 12.5 kg of antimony trioxide (containing 99.5% by mass as Sb2O3), 66.0 kg of pure water, and 12.5 kg of potassium hydroxide (containing 95% by mass as KOH) were added to a 100 L vessel, and 8.4 kg of 35% hydrogen peroxide was gradually added under stirring. 17.6 kg of the resulting aqueous solution of potassium antimonate was diluted to 2.2% by mass and passed through a column filled with hydrogen cation exchange resin. 0.25 kg of diisopropylamine was added to the solution of antimonic acid after ion exchange under stirring. The resulting sol was a water-dispersed sol of antimony pentoxide colloidal particles (ii-1), with a pH of 10.8, an Sb2O5 concentration of 1.5% by mass, and a primary particle diameter of 1 to 10 nm as observed by a transmission electron microscope.
[0194] (Production Example 1) Preparation of stannic oxide colloidal particles coated with silicon dioxide-stannic oxide composite oxide (iii-2-1) The aqueous dispersion sol of alkaline stannic oxide colloidal particles (i) prepared in Reference Example 1 was continuously subjected to hydrothermal treatment at a treatment temperature of 310°C, a treatment pressure of 20 MPa, and an average flow rate of 0.6 L / min. Next, under stirring, 400 g of aqueous dispersion sol of silicon dioxide-stannic oxide composite oxide colloidal particles (ii-2) prepared in Reference Example 2 (10 g of total metal oxide concentration (SnO2 and SnO2), 10 mass% relative to the core particles) was added to 1,000 g of the aqueous dispersion sol of alkaline stannic oxide colloidal particles obtained (100 g as SnO2), and then aged at 95°C for 2 hours to obtain an aqueous dispersion sol of stannic oxide colloidal particles (iii-2-1) coated with silicon dioxide-stannic oxide composite oxide. Next, the aqueous dispersion sol obtained was passed through a column packed with a hydrogen cation exchange resin. To the obtained water-dispersed sol, 3.5 g of tri-n-pentylamine (water solubility 0.02 g / L, quoted from the data listed on the Ambeed website. This can be found on the website at the following URL: https: / / www.ambeed.com / products / 621-77-2.html) was added, and the mixture was concentrated by ultrafiltration. The obtained sol was a water-dispersed sol of stannic oxide colloidal particles (iii-2-1) coated with silicon dioxide-stannic oxide composite oxide, with a pH of 5.5, a total metal oxide (SnO2 and SiO2) concentration of 30.5 mass%, an average particle size (dynamic light scattering particle size) of 19 nm measured by dynamic light scattering (DLS), and (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide) = 0.065.
[0195] (Production Example 2) Preparation of stannic oxide colloidal particles coated with silicon dioxide-stannic oxide composite oxide (iii-2-2) A sol was prepared in the same manner as in Production Example 1, except that the amount of the water-dispersed sol of silicon dioxide-stannic oxide composite oxide colloidal particles added was changed to 800 g (20 g as the total metal oxide concentration (SnO2 and SnO2), 20 mass% relative to the core particles). The obtained sol was a water-dispersed sol of stannic oxide colloidal particles (iii-2-2) coated with silicon dioxide-stannic oxide composite oxide, and had a pH of 5.5, a total metal oxide (SnO2 and SiO2) concentration of 30.5 mass%, an average particle size (dynamic light scattering particle size) of 25 nm measured by dynamic light scattering (DLS), and (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide)=0.125.
[0196] (Production Example 3) Preparation of stannic oxide colloidal particles coated with antimony pentoxide colloidal particles (iii-1-1) The aqueous dispersion sol of alkaline stannic oxide colloidal particles (i) prepared in Reference Example 1 was continuously subjected to hydrothermal treatment at a treatment temperature of 310°C, a treatment pressure of 20 MPa, and an average flow rate of 0.6 L / min. Next, under stirring, 400 g (6.0 g as Sb2O5, 5.0 mass% relative to the core particles) of the aqueous dispersion sol of antimony pentoxide colloidal particles (ii-1) prepared in Reference Example 3 was added to 1,200 g (120 g as SnO2) of the aqueous dispersion sol of alkaline stannic oxide colloidal particles obtained, and then aged at 95°C for 2 hours to obtain an aqueous dispersion sol of stannic oxide colloidal particles (iii-1-1) coated with antimony pentoxide colloidal particles. Next, the aqueous dispersion sol obtained was passed through a column filled with a hydrogen cation exchange resin. 3.8 g of tri-n-pentylamine was added to the aqueous dispersion sol obtained, and the mixture was concentrated by ultrafiltration membrane method. The obtained sol was a water-dispersed sol of stannic oxide colloidal particles (iii-1-1) coated with antimony pentoxide colloidal particles, with a pH of 4.2, a total metal oxide (SnO2 and Sb2O5) concentration of 20.5 mass%, an average particle size measured by dynamic light scattering (DLS) (dynamic light scattering particle size) of 20 nm, and (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide)=0.05.
[0197] (Production Example 4) Preparation of stannic oxide colloidal particles coated with silicon dioxide-stannic oxide composite oxide (iii-2-3) A sol was prepared in the same manner as in Production Example 1, except that the hydrothermal treatment temperature was changed to 240° C. and the treatment pressure was changed to 7.0 MPa. The obtained sol was a water-dispersed sol of stannic oxide colloidal particles (iii-2-3) coated with silicon dioxide-stannic oxide composite oxide, and had a pH of 5.5, a total metal oxide (SnO2 and SiO2) concentration of 30.5 mass%, an average particle size (dynamic light scattering particle size) of 23 nm measured by dynamic light scattering (DLS), and (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide)=0.125.
[0198] (Production Example 5) Preparation of stannic oxide colloidal particles coated with silicon dioxide-stannic oxide composite oxide (iii-2-4) A sol was prepared in the same manner as in Production Example 1, except that the hydrothermal treatment temperature was changed to 150° C. and the treatment pressure was changed to 1.0 MPa. The obtained sol was a water-dispersed sol of stannic oxide colloidal particles (iii-2-4) coated with silicon dioxide-stannic oxide composite oxide, and had a pH of 5.5, a total metal oxide (SnO2 and SiO2) concentration of 30.5 mass%, an average particle size (dynamic light scattering particle size) of 21 nm measured by dynamic light scattering (DLS), and (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide)=0.125.
[0199] (Production Example 6) Preparation of stannic oxide colloidal particles coated with silicon dioxide-stannic oxide composite oxide (iii-2-5) A sol was prepared in the same manner as in Production Example 1, except that the hydrothermal treatment was not performed. The obtained sol was a water-dispersed sol of stannic oxide colloidal particles (iii-2-5) coated with silicon dioxide-stannic oxide composite oxide, and had a pH of 5.5, a total metal oxide (SnO2 and SiO2) concentration of 30.5 mass%, an average particle size (dynamic light scattering particle size) of 20 nm measured by dynamic light scattering (DLS), and (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide)=0.125.
[0200] (Comparative Production Example 1) Preparation of stannic oxide colloidal particles (iii-3) coated with silicon dioxide-stannic oxide composite oxide A sol was prepared in the same manner as in Production Example 1, except that tri-n-pentylamine was not added in Production Example 1. The obtained sol was a water-dispersed sol of stannic oxide colloidal particles (iii-3) coated with silicon dioxide-stannic oxide composite oxide, and had a pH of 4.2, a total metal oxide (SnO2 and SiO2) concentration of 20.5 mass%, an average particle size (dynamic light scattering particle size) of 28 nm measured by dynamic light scattering (DLS), and (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide)=0.125.
[0201] Example 1 100 g of the water-dispersed sol of stannic oxide colloidal particles (iii-2-1) coated with silicon dioxide-stannic oxide composite oxide obtained in Production Example 1 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of stannic oxide colloidal particles (iii-2-1) coated with silicon dioxide-stannic oxide composite oxide. The obtained sol had a pH of 4.7 (diluted with the same mass of water as methanol), a total metal oxide (SnO2 and SiO2) concentration of 20.5 mass%, an average particle size (dynamic light scattering particle size) of 16 nm as measured by dynamic light scattering (DLS), a sol stability test result of "Good", the amount of tri-n-pentylamine remaining in the methanol dispersion sol of particle (iii-2-1) was 3,900 ppm, the amount of diisopropylamine was 180 ppm, and the amount of isopropylamine was 24 ppm, the crystallinity of core particle (i) was 92%, the refractive index of particle (iii-2-1) was 1.91, and the specific resistance of the coating film containing particle (iii-2-1) was 1.1 x 10 11 The mass ratio of amine (b) / amine (a) was 19.1.
[0202] Example 2 100 g of the water-dispersed sol of stannic oxide colloidal particles (iii-2-2) coated with silicon dioxide-stannic oxide composite oxide obtained in Production Example 2 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of stannic oxide colloidal particles (iii-2-2) coated with silicon dioxide-stannic oxide composite oxide. The obtained sol had a pH of 4.8 (diluted with the same mass of water as methanol), a total metal oxide (SnO2 and SiO2) concentration of 20.5 mass%, an average particle size (dynamic light scattering particle size) of 21 nm as measured by dynamic light scattering (DLS), a sol stability test result of "good", the amount of tri-n-pentylamine remaining in the methanol dispersion sol of particle (iii-2-2) was 4,200 ppm, the amount of diisopropylamine was 190 ppm, and the amount of isopropylamine was 22 ppm, the crystallinity of core particle (i) was 91%, the refractive index of particle (iii-2-2) was 1.87, and the specific resistance of the coating film containing particle (iii-2-2) was 1.9 × 10 11 The mass ratio of amine (b) / amine (a) was 19.8.
[0203] Example 3 100 g of the water-dispersed sol of stannic oxide colloidal particles (iii-1-1) coated with silicon dioxide-stannic oxide composite oxide obtained in Production Example 3 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of stannic oxide colloidal particles (iii-1-1) coated with silicon dioxide-stannic oxide composite oxide. The obtained sol had a pH of 5.2 (diluted with the same mass of water as methanol), a total metal oxide (SnO2 and Sb2O5) concentration of 30.5 mass%, an average particle size (dynamic light scattering particle size) of 16 nm as measured by dynamic light scattering (DLS), a sol stability test result of "good", the amount of tri-n-pentylamine remaining in the methanol dispersion sol of particle (iii-1-1) was 1500 ppm, the amount of diisopropylamine remaining in the methanol dispersion sol of particle (iii-1-1) was 40 ppm, the crystallinity of core particle (i) was 92%, the refractive index of particle (iii-1-1) was 1.93, and the resistivity of the coating film containing particle (iii-1-1) was 6.1 × 10 10 The mass ratio of amine (b) / amine (a) was 37.5.
[0204] Example 4 100 g of the water-dispersed sol of stannic oxide colloidal particles (iii-2-3) coated with silicon dioxide-stannic oxide composite oxide obtained in Production Example 4 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of stannic oxide colloidal particles (iii-2-3) coated with silicon dioxide-stannic oxide composite oxide. The obtained sol had a pH of 5.1 (diluted with the same mass of water as methanol), a total metal oxide (SnO2 and SiO2) concentration of 30.5 mass%, an average particle size (dynamic light scattering particle size) of 19 nm as measured by dynamic light scattering (DLS), a sol stability test result of "good", the amount of tri-n-pentylamine remaining in the methanol dispersion sol of particle (iii-2-3) was 3,900 ppm, the amount of diisopropylamine was 180 ppm, and the amount of isopropylamine was 41 ppm, the crystallinity of core particle (i) was 85%, the refractive index of particle (iii-2-3) was 1.85, and the resistivity of the coating film containing particle (iii-2-3) was 4.3 × 10 11 The mass ratio of amine (b) / amine (a) was 17.6.
[0205] Example 5 100 g of the water-dispersed sol of stannic oxide colloidal particles (iii-2-4) coated with silicon dioxide-stannic oxide composite oxide obtained in Production Example 5 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of stannic oxide colloidal particles (iii-2-4) coated with silicon dioxide-stannic oxide composite oxide. The obtained sol had a pH of 5.2 (diluted with the same mass of water as methanol), a total metal oxide (SnO2 and SiO2) concentration of 30.5 mass%, an average particle size (dynamic light scattering particle size) of 19 nm as measured by dynamic light scattering (DLS), a sol stability test result of "good", the amount of tri-n-pentylamine remaining in the methanol dispersion sol of particle (iii-2-4) was 4,000 ppm, the amount of diisopropylamine was 160 ppm, and the amount of isopropylamine was 93 ppm, the crystallinity of core particle (i) was 77%, the refractive index of particle (iii-2-4) was 1.83, and the resistivity of the coating film containing particle (iii-2-4) was 8.3 × 10 11 The mass ratio of amine (b) / amine (a) was 15.8.
[0206] Example 6 100 g of the water-dispersed sol of stannic oxide colloidal particles (iii-2-5) coated with silicon dioxide-stannic oxide composite oxide obtained in Production Example 6 was replaced with methanol using a rotary evaporator to obtain a methanol-dispersed sol of stannic oxide colloidal particles (iii-2-5) coated with silicon dioxide-stannic oxide composite oxide. The obtained sol had a pH of 4.7 (diluted with the same mass of water as methanol), a total metal oxide (SnO2 and SiO2) concentration of 30.5 mass%, an average particle size (dynamic light scattering particle size) of 21 nm as measured by dynamic light scattering (DLS), a sol stability test result of "good", the amount of tri-n-pentylamine remaining in the methanol dispersion sol of particle (iii-2-5) was 3,500 ppm, the amount of diisopropylamine was 140 ppm, and the amount of isopropylamine was 160 ppm, the crystallinity of core particle (i) was 68%, the refractive index of particle (iii-2-5) was 1.81, and the specific resistance of the coating film containing particle (iii-2-5) was 1.2 × 10 12 The mass ratio of amine (b) / amine (a) was 11.7.
[0207] Example 7 100 g of the water-dispersed sol of stannic oxide colloidal particles (iii-2-2) coated with silicon dioxide-stannic oxide composite oxide obtained in Production Example 2 was replaced with ethanol using a rotary evaporator to obtain an ethanol-dispersed sol of stannic oxide colloidal particles (iii-2-2) coated with silicon dioxide-stannic oxide composite oxide. The obtained sol had a pH of 5.0 (diluted with the same mass of water as the ethanol), a total metal oxide (SnO2 and SiO2) concentration of 20.5 mass%, an average particle size (dynamic light scattering particle size) of 22 nm as measured by dynamic light scattering (DLS), a sol stability test result of "Good", the amount of tri-n-pentylamine remaining in the ethanol dispersion sol of particle (iii-2-2) was 4,400 ppm, the amount of diisopropylamine remaining in the ethanol dispersion sol of particle (iii-2-2) was 180 ppm, and the amount of isopropylamine remaining in the ethanol dispersion sol of particle (iii-2-2) was 19 ppm, the degree of crystallinity of core particle (i) was 91%, the refractive index of particle (iii-2-2) was 1.87, and the specific resistance of the coating film containing particle (iii-2-2) was 2.6 × 10 11 The mass ratio of amine (b) / amine (a) was 22.1.
[0208] Example 8 100 g of the water-dispersed sol of stannic oxide colloidal particles (iii-2-2) coated with silicon dioxide-stannic oxide composite oxide obtained in Production Example 2 was replaced with 2-propanol using a rotary evaporator to obtain a 2-propanol-dispersed sol of stannic oxide colloidal particles (iii-2-2) coated with silicon dioxide-stannic oxide composite oxide. The obtained sol had a pH of 5.2 (diluted with the same mass of water as 2-propanol), a total metal oxide (SnO2 and SiO2) concentration of 15.0 mass%, an average particle size (dynamic light scattering particle size) of 22 nm as measured by dynamic light scattering (DLS), a sol stability test result of "Good", the amount of tri-n-pentylamine remaining in the 2-propanol dispersion sol of particle (iii-2-2) was 4,800 ppm, the amount of diisopropylamine remaining in the 2-propanol dispersion sol of particle (iii-2-2) was 170 ppm, and the amount of isopropylamine remaining in the 2-propanol dispersion sol of particle (iii-2-2) was 19 ppm, the degree of crystallinity of core particle (i) was 92%, the refractive index of particle (iii-2-2) was 1.87, and the specific resistance of the coating film containing particle (iii-2-2) was 2.3 × 10 11 The mass ratio of amine (b) / amine (a) was 25.4.
[0209] Example 9 14.6 g of the water-dispersed sol of stannic oxide colloidal particles (iii-1-1) coated with antimony pentoxide colloidal particles obtained in Production Example 3 was replaced with ethanol using a rotary evaporator to obtain 20.0 g of an ethanol-dispersed sol of stannic oxide colloidal particles (iii-1-1) coated with antimony pentoxide colloidal particles with a total metal oxide (SnO2 and SiO2) concentration of 15.0 mass%. 1.00 g of polyoxyethylene alkyl ether phosphate (manufactured by Toho Chemical Industry Co., Ltd.: RS-710) diluted with ethanol to a mass ratio of 30% as a surface modifier was added to the obtained sol under stirring, and the particles were surface-modified by refluxing at 90°C for 5 hours. 12.0 g of propylene glycol monomethyl ether was added to the obtained surface-modified ethanol dispersion sol, and the ethanol was evaporated using a rotary evaporator to obtain 15.0 g of a propylene glycol monomethyl ether dispersion sol of stannic oxide colloidal particles (iii-1-1) coated with antimony pentoxide colloidal particles. The obtained sol had a pH of 4.7 (diluted with the same mass of water as methanol), a total metal oxide (SnO2 and SiO2) concentration of 20.0 mass%, an average particle size (dynamic light scattering particle size) of 25 nm as measured by dynamic light scattering (DLS), a sol stability test result of "Good", the amount of tri-n-pentylamine remaining in the propylene glycol monomethyl ether dispersion sol of particle (iii-1-1) was 4,900 ppm, the amount of diisopropylamine was 240 ppm, and the amount of isopropylamine was 25 ppm, the degree of crystallinity of core particle (i) was 92%, the refractive index of particle (iii-1-1) was 1.91, and the specific resistance of the coating film containing particle (iii-1-1) was 8.0 × 10 11 The mass ratio of amine (b) / amine (a) was 18.5.
[0210] Comparative Example 1 100 g of an aqueous dispersion sol of the stannic oxide colloidal particles (iii-3) coated with silicon dioxide-stannic oxide composite oxide obtained in Comparative Production Example 1 was replaced with methanol using a rotary evaporator, and the sol thickened and gelled during the replacement.
[0211] Comparative Example 2 A sol was prepared in the same manner as in Reference Example 1, except that isopropylamine was not added during the preparation of the stannic oxide composite oxide colloidal particles (i) serving as the cores in Reference Example 1. The stannic oxide slurry was not peptized, and a water-dispersed sol could not be obtained. [Industrial Applicability]
[0212] The modified metal oxide particles of the present invention have high electrical conductivity and a high refractive index, and because they are stably dispersed in an organic solvent, it is possible to provide the above-mentioned sol that, when applied to a substrate as a coating agent, has transparency, a high particle refractive index, and a good coating film resistivity.
Claims
1. A sol comprising modified metal oxide particles (iii) having an average primary particle size of 1 to 10 nm and coated with at least one metal oxide particle (ii) selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide, the modified metal oxide particles being dispersed in an organic solvent, the average primary particle size satisfying the relationship of core particles (i)≧coated particles (ii), the (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide) being 0.005 to 1.0, and the sol comprising an amine (a) having a water solubility of 0.1 g / L or more, and an amine (b) having a water solubility of less than 0.1 g / L.
2. 2. The modified metal oxide sol according to claim 1, wherein the average particle size, as measured by dynamic light scattering, is 5 to 100 nm.
3. 2. The modified metal oxide sol according to claim 1, wherein the stannic oxide particles (i) serving as core particles are hydrothermally treated stannic oxide particles.
4. 2. The modified metal oxide sol according to claim 1, wherein the stannic oxide particles (i) serving as the core particles have a crystallinity of 60% or more as determined by an X-ray diffraction method.
5. 2. The modified metal oxide sol according to claim 1, wherein the metal oxide particles (ii) as the coated particles are antimony oxide particles or composite particles of stannic oxide and silicon oxide in a mass ratio of 1:0.1 to 10.
0.
6. 2. The modified metal oxide sol according to claim 1, wherein the amine (a) is contained in the modified metal oxide sol in an amount of 20 to 3,000 ppm.
7. 2. The modified metal oxide sol according to claim 1, wherein the amine (b) is contained in the modified metal oxide sol in an amount of 1,000 to 30,000 ppm.
8. 2. The modified metal oxide sol according to claim 1, wherein the amine (a) is a primary amine, a secondary amine, or a combination thereof.
9. 2. The modified metal oxide sol according to claim 1, wherein the amine (b) is a tertiary amine.
10. 2. The modified metal oxide sol according to claim 1, wherein the amine (a) is at least one amine selected from the group consisting of n-propylamine, di-n-propylamine, isopropylamine, diisopropylamine, n-butylamine, isobutylamine, di-n-butylamine, and diisobutylamine.
11. 2. The modified metal oxide sol according to claim 1, wherein the amine (b) is at least one amine selected from the group consisting of tri-n-butylamine, triisobutylamine, tri-n-pentylamine, and triisopentylamine.
12. 2. The modified metal oxide sol according to claim 1, wherein the mass ratio of amine (b) / amine (a) is 3.0 to 200.
13. The modified metal oxide particles (iii) are represented by the formulas (1) to (6): 【Chemistry 1】 【Chemistry 2】 [In formula (1), R 1 each represents an alkyl group, a halogenated alkyl group, an alkenyl group, an aryl group, or an organic group having a polyether group, an epoxy group, a (meth)acryloyl group, a mercapto group, an amino group, a ureido group, or a cyano group, and is bonded to a silicon atom by a Si-C bond; R 2 each represents an alkoxy group, an acyloxy group, or a halogen group; a represents an integer of 1 to 3; In formula (2) and formula (3), R 3 and R 5 are each an alkyl group having 1 to 3 carbon atoms or an aryl group having 6 to 30 carbon atoms and bonded to a silicon atom by a Si—C bond, R 4 and R 6 each represents an alkoxy group, an acyloxy group, or a halogen group; Y represents an alkylene group, an NH group, or an oxygen atom; b is an integer of 1 to 3; c is an integer of 0 or 1; and d is an integer of 1 to 3. In formulas (4) to (6), X 1 , X 2 , and X 3 each represents an alkylene group having 2 to 20 carbon atoms; f, h, and j each represent an integer of 1 to 100; e, g, and i each represent an integer of 1 to 3; Y 1 , Y 2 , and Y 3 each represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or a (meth)acrylic group.
2. The modified metal oxide sol according to claim 1, which is coated with at least one coating agent selected from the group consisting of:
14. 2. The modified metal oxide sol according to claim 1, wherein the organic solvent is an alcohol, a ketone, an ester, an ether, an amide, a hydrocarbon, a cyano group-containing solvent, a halogen-containing solvent, a sulfonyl group-containing solvent, a carboxyl group-containing solvent, or a mixture thereof.
15. 15. The modified metal oxide sol according to claim 14, wherein the alcohol is a monohydric alcohol having 1 to 20 carbon atoms or a polyhydric alcohol having 1 to 20 carbon atoms.
16. 16. An antistatic composition comprising modified metal oxide particles (iii) in the modified metal oxide sol according to any one of claims 1 to 15.
17. A composition for an electron transport material, comprising the modified metal oxide particles (iii) in the modified metal oxide sol according to claim 1 .
18. The following steps (A) to (D): Step (A): preparing an aqueous sol of stannic oxide particles (i) containing an amine (a) having a water solubility of 0.1 g / L or more and having an average primary particle size of 4 to 50 nm; Step (B): preparing an aqueous sol of at least one metal oxide particle (ii) having an average primary particle size of 1 to 10 nm and selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide, which contains an amine (a) having a water solubility of 0.1 g / L or more; Step (C): mixing the aqueous sol of stannic oxide obtained in step (A) and the aqueous sol of the modified metal oxide obtained in step (B) in a ratio of (total mass of metal oxides other than stannic oxide) / (mass of stannic oxide) of 0.005 to 1.0 to produce modified metal oxide particles (iii) having an average primary particle size of 1 to 10 nm and coated with at least one kind of metal oxide particles (ii) selected from the group consisting of antimony oxide, stannic oxide, and silicon oxide, using stannic oxide particles (i) having an average primary particle size of 4 to 50 nm as cores, and adding an amine (b) having a water solubility of less than 0.1 g / L; 16. A method for producing an organic solvent sol of modified metal oxide particles according to any one of claims 1 to 15, comprising: step (D): a step of solvent-substituting an aqueous medium of the aqueous sol of the modified metal oxide particles (iii) obtained in step (C) with an alcohol having 1 to 5 carbon atoms.
19. The method for producing an organic solvent sol of modified metal oxide particles (iii) according to claim 18, wherein the step (A) is a step (A-1) in which an amine (a) having a water solubility of 0.1 g / L or more is added to an aqueous sol of stannic oxide particles (i) having an average primary particle size of 4 to 50 nm, and then the aqueous sol is subjected to a hydrothermal treatment at a pressure of 0.1 to 40 MPa and a temperature of 100 to 350° C. for 0.01 to 100 hours.
20. Step (D) is followed by step (E) and / or step (F): Step (E): adding at least one coating agent selected from the group consisting of formulas (1) to (6) to an organic solvent sol of the modified metal oxide particles (iii) to perform surface treatment of the modified metal oxide particles (iii); The method for producing an organic solvent sol of modified metal oxide particles according to claim 18, further comprising the step (F): of replacing the alcohol in the alcohol solvent sol having 1 to 5 carbon atoms of the modified metal oxide particles (iii) with an alcohol other than that used in the step (D), a ketone, an ester, an ether, an amide, a hydrocarbon, a cyano group-containing solvent, a halogen-containing solvent, a sulfonyl group-containing solvent, a carboxyl group-containing solvent, or a mixed solvent thereof.
Citation Information
Patent Citations
Modified metal oxide sol and its production
JP1997080203A
Stroboscopic device
JP2004014329A
Modified stannic oxide-zirconium oxide composite sol, and method for preparing it
JP2005296940A
Process for producing modified stannic oxide sol and stannic oxide / zirconium oxide composite sol
JP2006176392A
Conductive tin oxide sol and process for producing the same
JP2008050253A