A perovskite film based on tin dioxide and modified by polymer interface, a preparation method thereof, and a solar cell
By modifying polyvinyl butyral on the SnO2 substrate, the problems of low-coordination Pb2+ defects and poor film formation quality in the CH3NH3PbI3 perovskite solar cell thin film are solved, and the optical performance of the film and the efficiency and stability of the solar cell are improved. .
Patent Information
- Application Number
- CN202111191567.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-10-13
AI Technical Summary
During the preparation process, the CH3NH3PbI3 perovskite solar cell film has defects in the surface low-coordination Pb2+ deep energy level and poor film formation quality, resulting in unfavorable carrier transmission and affecting the photoelectric conversion efficiency and stability.
Using SnO2 as the substrate and modifying the polymer polyvinyl butyral on it, forming a passivation defect of Lewis acid-base adduct, and spin-coated at the SnO2/CH3NH3PbI3 interface through polyvinyl butyral to reduce organic cation volatility and film stress , improve the quality of the film.
The morphology, structure and optical performance of the CH3NH3PbI3 film are improved, the photoelectric conversion efficiency and stability of perovskite solar cells are improved, and the device performance is improved.
Smart Images

Figure CN114141954B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solar cell preparation and relates to a SnO 2 The invention relates to a perovskite film and a solar cell with a polymer interface modified as a substrate, and specifically relates to a method for preparing a perovskite light absorption layer modified with a polymer interface, and especially relates to the interface engineering of the electron transport layer / light absorption layer of a perovskite solar cell. Background Art
[0002] Among renewable energy sources, solar energy is a good choice. As we all know, solar energy has the characteristics of being inexhaustible, requiring no transportation, and low risk, and has great potential in solving the energy crisis and environmental pollution problems facing mankind. Solar cells can effectively convert solar energy into electrical energy and are one of the new energy technologies that are currently receiving much attention. In the development process in recent years, three generations of solar cells have emerged, namely silicon-based solar cells, thin-film solar cells, and emerging solar cells. Among them, perovskite solar cells are one of the emerging solar cells, which have the advantages of high photoelectric conversion efficiency, low cost, simple manufacturing process, and long charge diffusion length. So far, the highest energy conversion efficiency of perovskite solar cells has reached 25.5%, and its rapid development speed has received high attention. CH 3 NH 3 PbI 3 Perovskite solar cells based on CH 3 NH 3 PbI 3 As a light absorbing layer material, its band gap is about 1.4 eV. 3 NH 3 PbI 3 The material has the following excellent properties: broadband absorption, low exciton binding energy, high carrier mobility (25cm 2 / Vs), long carrier lifetime and carrier diffusion length, is one of the most suitable materials for the light absorption layer of perovskite solar cells. 3 NH 3 PbI 3 The following problems exist in the film preparation process: ①CH 3 NH 3 PbI 3 The organic cations and iodide ions on the film surface will volatilize during the annealing process, resulting in the appearance of low-coordinated Pb 2+ The low-coordinated Pb on the film surface 2+It is a deep energy level defect. Deep energy level defects will trap carriers at the heterojunction interface. Defect-bound carriers accumulate at the interface, which will lead to problems such as band bending, energy level arrangement changes, built-in electric field changes, and interface non-radiative recombination. It is not conducive to the separation and injection of carriers during carrier transmission and ultimately destroys the photoelectric conversion efficiency and stability. ②CH 3 NH 3 PbI 3 The film quality is poor, the coverage is low, and the crystallinity is low. Summary of the invention
[0003] The purpose of the present invention is to provide a SnO 2 A perovskite film with a SnO substrate and a polymer interface modified perovskite film and a preparation method thereof, and a solar cell can improve the quality of the perovskite film and enhance the performance of the perovskite solar cell. The core of the invention is a SnO 2 A perovskite film with a substrate and polymer interface modified and a preparation method thereof. The perovskite film prepared by the method can be applied to solar cells to effectively improve device efficiency and stability and promote its commercialization process.
[0004] The technical solution of the present invention is:
[0005] A SnO 2 CH 3 NH 3 PbI 3 The method for preparing perovskite thin film is to first prepare SnO with conductive glass as the substrate. 2 film, and then on the conductive glass / SnO 2 The substrate is modified with polymer polyvinyl butyral, and CH 3 NH 3 PbI 3 A perovskite film is prepared and the obtained product is applied to a solar cell. A typical preparation method of the film may include the following steps, wherein the parameters are all preferred values:
[0006] (1) Conductive glass was ultrasonically treated with acetone, anhydrous ethanol, and deionized water for 20 min, then dried with nitrogen, and then treated with ultraviolet ozone in a UV irradiator for 30 min. 2 The colloidal dispersion is spin-coated onto the conductive glass treated with UV ozone, and the spin coating is performed at a speed of 2500 to 5000 r / min for 10 to 60 seconds. The process is repeated 3 to 6 times, and then annealed at 100 to 200 ° C for 15 to 60 minutes to obtain SnO based on the conductive glass. 2 film.
[0007] (2) Add solid polyvinyl butyral to isopropanol solvent, heat at 80-100°C and stir with magnetic force for 20-40 min until completely dissolved. Take a volume of 100-200 μl polyvinyl butyral solution with a mass concentration of 0.5-2 mg / ml and spin coat it on the SnO substrate. 2 The spin coating speed is 2000-4000 r / min and the spin coating time is 20-40 s. Then, the conductive glass / SnO is obtained by annealing at 70-90°C for 1-10 min on a constant temperature heating table. 2 / PVB film.
[0008] (3) Weigh an appropriate amount of PbI 2 Dissolve in a mixed solvent of dimethyl sulfoxide and N,N-dimethylformamide in a volume ratio of 1:8 to 1:11, and heat and stir at 60°C to 90°C for 15 to 45 minutes with a constant temperature heating magnetic stirrer until dissolved to obtain a PbI with a molar concentration of 0.5 to 1.5 mol / L. 2 The precursor solution was then filtered through a polytetrafluoroethylene filter. A volume of 130-170 μl of PbI 2 The solution is spin-coated onto the conductive glass / SnO prepared in step (2) which has been treated with UV ozone. 2 / PVB film, the spin coating speed is 2000~4000r / min, and the spin coating time is 30~60s. Then anneal at 60~90℃ for 20~60min. Weigh an appropriate amount of methylammonium iodide and dissolve it in isopropanol solution. Stir magnetically at 20℃~40℃ for 20~60min to obtain a methylammonium iodide solution with a mass concentration of 5~10mg / mL. Spin-coated PbI 2 The device was immersed in methylammonium iodide solution for 1 to 3 minutes, and then washed with isopropanol for 40 to 60 seconds. After being taken out, the excess liquid was dried. Then, the conductive glass / SnO was annealed at 70 to 100°C for 1 to 10 minutes. 2 / PVB / CH 3 NH 3 PbI 3 film.
[0009] After the film is prepared, it can be applied to perovskite solar cells, that is, the above steps can be followed as follows:
[0010] (4) Use a pipette to transfer 60 μL of Spiro-OMeTAD cobalt-based spin coating solution to the conductive glass / SnO prepared in step (3) adsorbed on the vacuum chuck. 2 / PVB / CH 3 NH 3 PbI 3 The conductive glass / SnO film was obtained by spin coating at 3000r / min for 30s.2 / PVB / CH 3 NH 3 PbI 3 The thin film is a cobalt-doped Spiro-OMeTAD hole transport layer on the substrate.
[0011] (5) In high vacuum (5×10 -5 Pa) in conductive glass / SnO 2 / PVB / CH 3 NH 3 PbI 3 A 80nm thick gold (Au) layer was thermally evaporated on the Spiro-OMeTAD substrate as the cathode to obtain a conductive glass / SnO 2 / PVB / CH 3 NH 3 PbI 3 / Spiro-OMeTAD / Au perovskite solar cells.
[0012] The polymer polyvinyl butyral (PVB) is a Lewis base molecule. 2+ It can be regarded as a Lewis acid and can be effectively passivated by Lewis base molecules containing lone pair electrons N, O, and S. Therefore, the introduction of polymer polyvinyl butyral can be used to transfer the under-coordinated Pb 2+ A pair of non-bonding electrons is provided to form Lewis acid-base adducts, thereby passivating defects, reducing interface non-radiative recombination losses, and improving energy conversion efficiency. Since the glass transition temperature of polyvinyl butyral is low (66-84°C), and the annealing temperature of the perovskite layer is often higher than this temperature, the polyvinyl butyral layer remains soft and glassy during the preparation of the perovskite layer. This allows the perovskite to properly release the film stress during the growth stage, resulting in a better quality film.
[0013] The present invention spin-coats polyvinyl butyral on SnO 2 / CH 3 NH 3 PbI 3 interface. The introduction of polymer polyvinyl butyral can reduce CH 3 NH 3 PbI 3 The organic cations evaporate during the annealing process, and polyvinyl butyral can transfer to the under-coordinated Pb 2+ Provide a pair of non-bonding electrons to form Lewis acid-base adducts, thereby passivating defects. The low glass transition temperature of polyvinyl butyral can properly release the film stress during the perovskite growth stage to obtain a better quality film. The research results show that the SnO 2 / CH 3 NH3 PbI 3 Interface modification improves CH 3 NH 3 PbI 3 The morphology, structure, optical properties, stability of the film and the performance of the corresponding solar cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 CH 3 NH 3 PbI 3 Field emission scanning electron microscopy images of perovskite (abbreviated as PVK in the figure) films: (a) unmodified with polyvinyl butyral; (b) modified with polyvinyl butyral (PVB).
[0015] Figure 2 CH without PVB modification and with PVB modification 3 NH 3 PbI 3 XRD diffraction pattern of perovskite (PVK) thin film.
[0016] Figure 3 CH without PVB modification and with PVB modification 3 NH 3 PbI 3 UV-visible absorption spectra of perovskite (PVK) thin films.
[0017] Figure 4 CH without PVB modification and with PVB modification 3 NH 3 PbI 3 The optical performance stability of perovskite (PVK) films stored in air for 0 to 20 hours.
[0018] Figure 5 CH without PVB interface modification and with PVB interface modification 3 NH 3 PbI 3 JV characteristic curve of perovskite (PVK) solar cell. DETAILED DESCRIPTION
[0019] The present invention will be described in detail below with reference to specific embodiments.
[0020] Example 1
[0021] (1) The FTO conductive glass was ultrasonically treated with acetone, anhydrous ethanol, and deionized water for 20 min, then dried with nitrogen, and then treated with ultraviolet ozone in a UV irradiator for 30 min. 2The colloidal dispersion was spin-coated onto the FTO conductive glass treated with UV ozone at a speed of 2500 r / min for 20 s. The process was repeated 3 times and then annealed at 100 °C for 25 min to obtain SnO based on FTO conductive glass. 2 film.
[0022] (2) Add solid polyvinyl butyral to isopropanol solvent and heat at 80°C with magnetic stirring for 20 min until it is completely dissolved. Take a volume of 100 μl and a mass concentration of 0.5 mg / ml polyvinyl butyral solution and spin coat it on the SnO substrate. 2 The spin coating speed was 2500r / min and the spin coating time was 30s. Then, the FTO / SnO was obtained by annealing at 70°C for 10min on a constant temperature heating table. 2 / PVB film.
[0023] (3) Weigh an appropriate amount of PbI 2 Dissolve in a mixed solvent of dimethyl sulfoxide and N,N-dimethylformamide in a volume ratio of 1:9, and heat and stir at 70°C for 25 min with a constant temperature heating magnetic stirrer until dissolved to obtain PbI with a molar concentration of 0.5 mol / L 2 The precursor solution was then filtered through a polytetrafluoroethylene filter. A volume of 140 μl of PbI 2 The solution was spin-coated onto the FTO / SnO prepared in step (2) after UV-ozone treatment. 2 / PVB film, the spin coating speed is 2500r / min, the spin coating time is 40s. Then anneal at 70℃ for 30min. Weigh an appropriate amount of methylammonium iodide and dissolve it in isopropanol solution. Stir magnetically at 25℃ for 25min to obtain a methylammonium iodide solution with a mass concentration of 6mg / mL. Spin-coated PbI 2 The device was immersed in methylammonium iodide solution for 2 minutes, and then washed with isopropanol for 40 seconds, and the excess liquid was dried. Then annealed at 85°C for 5 minutes to obtain FTO / SnO 2 / PVB / CH 3 NH 3 PbI 3 film.
[0024] (4) Use a pipette to transfer 60 μL of Spiro-OMeTAD cobalt-based spin coating solution to the FTO / SnO prepared in step (3) adsorbed on the vacuum chuck. 2 / PVB / CH 3 NH 3 PbI 3 The FTO / SnO film was obtained by spin coating at 3000 r / min for 30 seconds. 2 / PVB / CH 3NH 3 PbI 3 The thin film is a cobalt-doped Spiro-OMeTAD hole transport layer on the substrate.
[0025] (5) In high vacuum (5×10 -5 Pa) in FTO / SnO 2 / PVB / CH 3 NH 3 PbI 3 A 80 nm thick gold (Au) layer was thermally evaporated on the Spiro-OMeTAD substrate as the cathode to obtain a structure of FTO / SnO 2 / PVB / CH 3 NH 3 PbI 3 / Spiro-OMeTAD / Au perovskite solar cells.
[0026] In this example, the polyvinyl butyral is 15.0-18.0 mPa.s, butyraldehyde base is 70%-75%, and other specifications of PVB are also feasible; the specifications of the FTO conductive glass are 20mm*25mm, the square resistance is 14Ω, and the transmittance is ≥90%. Other types of conductive glass are also feasible.
[0027] The present invention will be specifically described below in conjunction with the accompanying drawings:
[0028] Attached Figure 1 CH 3 NH 3 PbI 3 Perovskite film and polyvinyl butyral modified CH 3 NH 3 PbI 3 SEM image of perovskite film. As can be seen from the figure, unmodified CH 3 NH 3 PbI 3 The surface of the perovskite film has many voids, the grain size is small and uneven, and the crystallinity is poor. However, the perovskite film based on polyvinyl butyral has significantly fewer voids on the film surface, the grains of the perovskite film are significantly larger, the film is more dense, flat and uniform, and the crystallinity is significantly improved. This high-quality, high-flatness film is conducive to the transmission of carriers between grains and between grains and perovskite layers and interfaces. These changes can effectively improve the photoelectric properties of perovskites.
[0029] Attached Figure 2 CH 3 NH 3 PbI 3 Perovskite film and polyvinyl butyral modified CH3 NH 3 PbI 3 XRD pattern of perovskite film. The results show that after modification with polyvinyl butyral, the corresponding CH 3 NH 3 PbI 3 The XRD diffraction peak intensity of perovskite is improved. The results show that after polyvinyl butyral modification, the crystallinity of perovskite film is improved, which is beneficial to improve its photoelectric properties.
[0030] Attached Figure 3 CH 3 NH 3 PbI 3 Perovskite film and polyvinyl butyral modified CH 3 NH 3 PbI 3 UV-visible absorption spectra of perovskite films. The results show that polyvinyl butyral modification can improve CH 3 NH 3 PbI 3 The absorbance of perovskite film in the wavelength range of 500nm-900nm is reduced and its absorption edge is red-shifted, which improves CH 3 NH 3 PbI 3 Light absorption properties of perovskite films.
[0031] Attached Figure 4 The UV-visible absorption spectra of the perovskite film without polyvinyl butyral modification and the perovskite film modified with polyvinyl butyral were tested by UV-visible absorption spectrum immediately after preparation and again after exposure to air for 20 hours. Figure 4 It can be seen that the absorbance of the perovskite film modified with polyvinyl butyral in the wavelength range of 500nm-900nm is higher than that of the perovskite film control group without polyvinyl butyral modification. And after being exposed to air for 20 hours, the absorbance of the perovskite film modified with polyvinyl butyral in the wavelength range of 500nm-900nm did not change much, while the absorbance of the control group in the wavelength range of 500nm-900nm decreased significantly after being exposed to air for 20 hours. Figure 4 It can be seen that the modification of polyvinyl butyral can inhibit the decomposition of perovskite film in the air, and the modification of polyvinyl butyral makes the perovskite film have better stability.
[0032] Attached Figure 5 The JV characteristic curves of the perovskite solar cells modified with polyvinyl butyral and the unmodified perovskite solar cells are shown in Table 1. Figure 5 Related perovskite solar cell photovoltaic parameter table. Figure 5 It can be seen that the perovskite solar cell with polyvinyl butyral modified light absorption layer / electron transport layer has improved in various photovoltaic parameters. The photoelectric conversion efficiency of the perovskite solar cell modified with polyvinyl butyral reached 10.12%, the open circuit voltage reached 1.08V, and the short circuit current reached 14.80mA·cm -2 , the filling factor is 0.64, compared with CH 3 NH 3 PbI 3 The efficiency of perovskite solar cells increased by 1.02%, a relative improvement of 11.21%.
[0033] Table 1 Photovoltaic parameters of perovskite solar cells
[0034]
[0035] The present invention modifies SnO by polyvinyl butyral 2 / CH 3 NH 3 PbI 3 The perovskite film was prepared at the interface, reducing CH 3 NH 3 PbI 3 The organic cations in the film volatilize during the annealing process and passivate the low-coordinated Pb 2+ , reducing CH 3 NH 3 PbI 3 Defects of perovskite films. Polyvinyl butyral is spin-coated on SnO 2 On the substrate, CH 3 NH 3 PbI 3 The perovskite film can properly release the film stress during the growth stage to obtain a better quality film, thereby improving device performance.
[0036] Example 2
[0037] (1) The FTO conductive glass was ultrasonically treated with acetone, anhydrous ethanol, and deionized water for 20 min, then dried with nitrogen, and then treated with ultraviolet ozone in a UV irradiator for 30 min. A volume of 200 μL and a mass percentage concentration of 5 wt% SnO 2 The colloidal dispersion was spin-coated onto the FTO conductive glass treated with UV ozone at a speed of 4000 r / min for 30 s. The process was repeated 6 times and then annealed at 180 °C for 40 min to obtain SnO based on FTO conductive glass. 2 film.
[0038] (2) Add solid polyvinyl butyral to isopropanol solvent and heat at 90°C with magnetic stirring for 30 min until it is completely dissolved. Take a volume of 180 μl and a mass concentration of 1.5 mg / ml polyvinyl butyral solution and spin coat it on the SnO substrate. 2 The spin coating speed was 3500r / min and the spin coating time was 20s. Then, the FTO / SnO was obtained by annealing at 90°C for 5min on a constant temperature heating table. 2 / PVB film.
[0039] (3) Weigh an appropriate amount of PbI 2 Dissolve in a mixed solvent of dimethyl sulfoxide and N,N-dimethylformamide in a volume ratio of 1:10, and heat and stir at 80°C for 20 min with a constant temperature heating magnetic stirrer until dissolved to obtain PbI with a molar concentration of 1 mol / L 2 The precursor solution was then filtered through a polytetrafluoroethylene filter. A volume of 160 μl of PbI 2 The solution was spin-coated onto the FTO / SnO prepared in step (2) after UV-ozone treatment. 2 / PVB film, the spin coating speed is 4000r / min, the spin coating time is 30s. Then anneal at 80℃ for 20min. Weigh an appropriate amount of methylammonium iodide and dissolve it in isopropanol solution. Stir it magnetically at 30℃ for 20min to obtain a methylammonium iodide solution with a mass concentration of 5-10mg / mL. Spin-coat PbI 2 The device was immersed in methylammonium iodide solution for 1 to 3 minutes, and then washed with isopropanol for 40 to 60 seconds. After being taken out, the excess liquid was dried. Then, the device was annealed at 70 to 100°C for 1 to 10 minutes to obtain FTO / SnO 2 / PVB / CH 3 NH 3 PbI 3 film.
[0040] (4) Use a pipette to transfer 60 μL of Spiro-OMeTAD cobalt-based spin coating solution to the FTO / SnO prepared in step (3) adsorbed on the vacuum chuck. 2 / PVB / CH 3 NH 3 PbI 3 The FTO / SnO film was obtained by spin coating at 3000 r / min for 30 seconds. 2 / PVB / CH 3 NH 3 PbI 3 The thin film is a cobalt-doped Spiro-OMeTAD hole transport layer on the substrate.
[0041] (5) In high vacuum (5×10 -5Pa) in FTO / SnO 2 / PVB / CH 3 NH 3 PbI 3 A 80 nm thick gold (Au) layer was thermally evaporated on the Spiro-OMeTAD substrate as the cathode to obtain a structure of FTO / SnO 2 / PVB / CH 3 NH 3 PbI 3 / Spiro-OMeTAD / Au perovskite solar cells.
Claims
1. A perovskite film based on SnO2 and modified by a polymer interface, characterized in that: The film is a structure obtained by preparing a layer of polyvinyl butyral (PVB) on a substrate containing a planar structure SnO2 layer, and then preparing a CH3NH3PbI3 film on the substrate; the film is prepared by the following method: (1) The conductive glass is ultrasonically treated with acetone, anhydrous ethanol, and deionized water, and then dried with nitrogen. After ultraviolet ozone treatment, the SnO2 colloidal dispersion is spin-coated onto the treated conductive glass. This process is repeated several times, and then annealed to obtain a SnO2 thin film on the conductive glass substrate. (2) Using the sample prepared in step (1) as a substrate, adding PVB solid into isopropanol solvent, heating and stirring until completely dissolved to obtain a PVB solution, spin coating the solution onto the substrate, and annealing to obtain a conductive glass / SnO2 / PVB film; (3) Using the sample prepared in step (2) as a substrate, a CH3NH3PbI3 thin film is prepared thereon by a two-step method to obtain a perovskite thin film with SnO2 as a substrate and polymer interface modification, namely, conductive glass / SnO2 / PVB / CH3NH3PbI3.
2. The perovskite film based on SnO2 and modified with a polymer interface according to claim 1, characterized in that: The mass percentage concentration of the SnO2 colloidal dispersion described in step (1) is 1wt%~5wt%, the spin coating speed is 2500~5000r / min, the spin coating time is 10 s~60 s, the process is repeated 3 to 6 times, the annealing temperature is 100~200℃, and the annealing time is 15~60 min.
3. The perovskite film based on SnO2 and modified by polymer interface according to claim 1, characterized in that: The heating and stirring in step (2) has a heating temperature of 80-100° C., a stirring time of 20-40 min, and a mass concentration of the PVB solution of 0.5-2 mg / ml.
4. The perovskite film based on SnO2 and modified by polymer interface according to claim 1, characterized in that: In step (2), the PVB solution is spin-coated at a speed of 2000 to 4000 revolutions per minute, the spin-coating time is 20 to 40 seconds, the annealing temperature is 70 to 90° C., and the annealing time is 1 to 10 minutes.
5. The perovskite film based on SnO2 and modified by polymer interface according to claim 1, characterized in that: The step (3) specifically includes: 1) PbI2 is dissolved in a mixed solvent of N, N-dimethylformamide and dimethyl sulfoxide, heated and stirred until completely dissolved to obtain a PbI2 precursor solution, the solution is filtered and spin-coated onto the surface of the conductive glass / SnO2 / PVB film treated with UV ozone, immersed in isopropanol for 1-10 minutes, taken out and dried to remove excess liquid, and annealed; 2) Dissolve methylammonium iodide in isopropanol solution, stir at room temperature to obtain a methylammonium iodide solution with a mass concentration of 5-10 mg / mL, immerse the film obtained in 1) in the methylammonium iodide solution to react for 1-3 minutes, remove the film and then spin off excess liquid, anneal it, and obtain a conductive glass / SnO2 / PVB / CH3NH3PbI3 film.
6. The perovskite film based on SnO2 and modified with a polymer interface according to claim 5, characterized in that: 1) The heating and stirring described in the above method is that the heating temperature is 60°C to 90°C and the stirring time is 15 to 45 minutes; the concentration of the PbI2 precursor solution is 0.5 to 1.5 mol / L, the volume ratio of dimethyl sulfoxide to N,N-dimethylformamide is 1:8 to 1:11; the spin coating speed is 2000 to 4000 r / min and the spin coating time is 30 to 60 seconds.
7. The perovskite film based on SnO2 and modified by polymer interface according to claim 5, characterized in that: 1) The annealing temperature is 60-90°C and the annealing time is 20-60min.
8. The perovskite film based on SnO2 and modified with a polymer interface according to claim 5, characterized in that: 2) The annealing temperature is 70-100°C and the annealing time is 1-10 minutes.
9. A CH3NH3PbI3 perovskite solar cell, characterized in that: Based on the perovskite film as described in any one of claims 1 to 8, a hole transport layer is prepared on the perovskite film, and then an electrode is prepared to obtain a perovskite solar cell device.