Laminated film with protective layer

The polarizing film with varying dichroic dye content regions addresses inconsistent visibility correction in organic EL displays, enhancing image clarity and reducing reflections through tailored polarization characteristics.

JP7586643B2Active Publication Date: 2024-11-19SUMITOMO CHEM CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2019551034
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-12-28
Filing Date
2018-10-16
Publication Date
2024-11-19
Estimated Expiration
2038-10-16

AI Technical Summary

Technical Problem

Existing polarizing films for organic EL display devices do not effectively address the issue of varying visibility correction polarization degrees, leading to inconsistent performance in reducing reflections and enhancing image clarity.

Method used

A polarizing film with at least two regions having different visibility correction polarization degrees, achieved by varying the dichroic dye content and alignment in a liquid crystal layer, combined with a base material layer and alignment layer, allowing for tailored polarization characteristics.

Benefits of technology

The film provides enhanced visibility correction and reduced reflections, improving image clarity and camera performance by optimizing polarization across different regions, suitable for use in organic EL display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586643000023
    Figure 0007586643000023
  • Figure 0007586643000024
    Figure 0007586643000024
  • Figure 0007586643000025
    Figure 0007586643000025
Patent Text Reader

Abstract

The polarizing film has a liquid crystal layer containing a liquid crystal compound and at least two regions distinguished by a luminosity-corrected polarization coefficient, the at least two regions having different dichroic dye contents.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing film and a method for producing the same, and more particularly to a polarizing film having a layer containing a liquid crystal compound and a dichroic dye and a method for producing the same. [Background technology]

[0002] Organic EL display devices using organic light-emitting diodes (OLEDs) are not only lighter and thinner than liquid crystal display devices, but also have the advantage of being able to achieve high image quality with a wide viewing angle, fast response speed, and high contrast, and are therefore used in a variety of fields, including smartphones, televisions, and digital cameras. It is known that in organic EL display devices, the anti-reflection performance is improved by using circular polarizers, etc., in order to suppress the deterioration of visibility caused by the reflection of external light.

[0003] As a polarizing film used in such a circular polarizing plate, JP-A-2015-206852 (Patent Document 1) and JP-A-2015-212823 (Patent Document 2) describe a patterned polarizing film in which a patterned liquid crystal cured film is laminated on a substrate. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-206852 A [Patent Document 2] JP 2015-212823 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a novel polarizing film having at least two regions with different luminosity-corrected polarization degrees, and a method for producing the same. [Means for solving the problem]

[0006] The present invention provides a polarizing film and a method for producing the same, as described below. [1] A polarizing film having a liquid crystal layer, the liquid crystal layer includes a liquid crystal compound and has at least two regions that are distinguished by a value of a luminosity-corrected polarization degree; A polarizing film, wherein the at least two regions have different contents of dichroic dye. [2] Further, a base material layer; An orientation layer laminated on at least one side of the substrate layer, The polarizing film according to [1], wherein the liquid crystal layer is laminated on the alignment layer. [3] The polarizing film according to [2], wherein the alignment layer contains a photoalignable polymer. [4] The polarizing film according to any one of [1] to [3], wherein the liquid crystal compound includes a polymerizable liquid crystal compound. [5] The liquid crystal layer has a first region containing a dichroic dye and a second region having a lower content of the dichroic dye than the first region, The luminosity-corrected polarization degree of the first region is 90% or more, The polarizing film according to any one of [1] to [4], wherein the luminous efficiency-corrected polarization degree of the second region is 10% or less. [6] The liquid crystal layer has a first region containing a dichroic dye and a second region having a lower content of the dichroic dye than the first region, The luminous efficiency corrected single transmittance of the first region is 35% or more; The polarizing film according to any one of [1] to [5], wherein the luminous efficiency-corrected single transmittance of the second region is 80% or more. [7] The second region has a circular, elliptical, oblong or polygonal shape in a plan view, When the second region is circular, the diameter is 5 cm or less; When the second region is elliptical or oval, the major axis of the second region is 5 cm or less; The polarizing film according to either [5] or [6], wherein when the second region is a polygon, a diameter of an imaginary circle drawn to inscribe the polygon is 5 cm or less. [8] The polarizing film according to any one of [5] to [7], wherein the first region exhibits a Bragg peak in X-ray diffraction measurement. [9] Further, the electrophotographic film has a base layer, The polarizing film according to any one of [1] to [8], wherein the base layer has a function as a ¼ wavelength plate.

[10] The polarizing film according to any one of [1] to [9], wherein the polarizing film has a length of 10 m or more.

[11] A circularly polarizing plate comprising the polarizing film according to any one of [1] to [8] and

[10] laminated with a retardation layer having a quarter-wave plate function.

[12] A preparation step of preparing a laminated film having a polarizing layer containing a liquid crystal compound and a dichroic dye on at least one side of a base layer; a liquid contacting step of contacting a partial region of the polarizing layer of the laminate film with a liquid that can reduce the content of dichroic dye in the polarizing layer, thereby reducing the content of dichroic dye in the partial region of the polarizing layer.

[13] The liquid contacting step comprises: a protective layer lamination step of laminating a protective layer having a covering region for covering the polarizing layer and an exposure region for exposing the polarizing layer on the polarizing layer of the laminated film prepared in the preparation step, thereby obtaining a laminated film with a protective layer; a bleaching step of contacting the laminate film with the protective layer with a liquid material capable of reducing the content of the dichroic dye in the polarizing layer to obtain a bleached laminate film in which the content of the dichroic dye in a partial region of the polarizing layer is reduced; The method for producing a polarizing film according to

[12] , further comprising a peeling step of peeling the protective layer from the bleached laminate film.

[14] The exposed region of the protective layer has a circular, elliptical, oval, or polygonal shape in a plan view, When the exposed area is circular, the diameter is 5 cm or less; When the exposed area is elliptical or oval, the major axis of the exposed area is 5 cm or less; The method for producing a polarizing film according to

[13] , wherein when the exposed area is a polygon, a diameter of an imaginary circle drawn to inscribe the polygon is 5 cm or less.

[15] The preparation step includes: An orientation layer forming step of forming an orientation layer by applying a composition for forming an orientation layer to one side of the base layer; and a polarizing layer-forming step of forming the polarizing layer by applying a polarizing layer-forming composition containing the liquid crystal compound and the dichroic dye onto a surface of the base layer on which the alignment layer is formed, to form the polarizing layer.

[16] The composition for forming an alignment layer contains a photoalignable polymer, The method for producing a polarized film according to

[15] , wherein the alignment layer forming step comprises irradiating a coating layer for an alignment layer formed by coating the composition for forming an alignment layer with polarized light to form the alignment layer.

[17] The liquid crystal compound is a polymerizable liquid crystal compound, The method for producing a polarizing film according to

[15] or

[16] , wherein the polarizing layer forming step comprises irradiating a coating layer for a polarizing layer formed by coating the composition for forming a polarizing layer with active energy rays to form the polarizing layer.

[18] The method for producing a polarizing film according to any one of

[12] to

[17] , wherein the polarizing film has a length of 10 m or more.

[19] A method for producing a circularly polarizing plate, comprising a retardation layer lamination step of laminating a polarizing film produced by the method for producing a polarizing film according to any one of

[12] to

[18] and a retardation layer having a quarter-wave plate function.

[20] The polarizing film is a long polarizing film having a length of 10 m or more, The retardation layer is a long retardation layer having a length of 10 m or more, The retardation layer lamination step forms a long laminate by laminating the long polarizing film and the long retardation layer, The method for producing a circularly polarizing plate according to

[19] , further comprising a cutting step of cutting the long laminate into sheets. Effect of the Invention

[0007] According to the present invention, it is possible to provide a polarizing film having at least two regions with different luminous efficiency-corrected polarization degrees, and a method for producing the same. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1A is a schematic plan view showing an example of a polarizing film of the present invention, and FIG. 1B is a cross-sectional view taken along the line XX of FIG. [Diagram 2] 1(a) to 1(c) are schematic cross-sectional views illustrating an example of the circularly polarizing plate of the present invention. [Diagram 3] 1(a) to 1(d) are schematic cross-sectional views showing examples of layer structures obtained in each step of the production process for the polarizing film of the present invention. [Figure 4] FIG. 2 is a schematic cross-sectional view showing an example of a liquid contact step in the method for producing the polarizing film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, preferred embodiments of the polarizing film and the manufacturing method thereof of the present invention will be described with reference to the drawings. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.

[0010] <Polarizing film> FIG. 1(a) is a schematic plan view showing an example of the polarizing film of the present invention, and FIG. 1(b) is a cross-sectional view taken along line XX of FIG. 1(a). The polarizing film 1 of this embodiment is a film having a function of light absorption anisotropy, and has a liquid crystal layer 11 containing a liquid crystal compound. The liquid crystal layer 11 has at least two regions that are distinguished by the value of the luminosity-corrected polarization degree (Py), and the at least two regions have different contents of dichroic dyes. The polarizing film 1 has a liquid crystal layer 11, but may further have a base layer 13, an alignment layer 12, other layers, etc. In the polarizing film 1 shown in FIG. 1(b), an example is shown in which the alignment layer 12 and the liquid crystal layer 11 are provided on one side of the base layer 13, but the alignment layer and the liquid crystal layer may be provided on both sides of the base layer 13. The structures of the liquid crystal layers provided on both sides of the base layer 13 may be the same as each other, or may be different from each other.

[0011] The polarizing film 1 may be a long polarizing film having a length of 10 m or more. In this case, the polarizing film 1 may be wound into a roll. The polarizing film may be continuously unwound from the roll and may be laminated with a retardation layer, which will be described later, cut into sheets, or the like. The length of the long polarizing film to be wound into a roll is not particularly limited as long as it is 10 m or more, but may be, for example, 10,000 m or less.

[0012] (Liquid crystal layer) The liquid crystal layer 11 contains a liquid crystal compound, and has a region containing the liquid crystal compound and a dichroic dye. When the polarizing film 1 has polarization characteristics in the plane of the polarizing film 1, it is preferable that the liquid crystal layer 11 has a region in which the dichroic dye and the liquid crystal compound are aligned horizontally to the plane of the polarizing film 1. When the polarizing film 1 has polarization characteristics in the thickness direction of the polarizing film 1, it is preferable that the liquid crystal layer 11 has a region in which the dichroic dye and the liquid crystal compound are aligned horizontally to the plane of the polarizing film 1.

[0013] In the liquid crystal layer 11, a region containing a dichroic dye and a liquid crystal compound, in which the dichroic dye and the liquid crystal compound are aligned horizontally relative to the polarizing film 1 surface, preferably has a dichroic ratio (=A1(λ) / A2(λ)) of the absorbance A1(λ) in the horizontal direction of liquid crystal alignment to the absorbance A2(λ) in the vertical direction in the liquid crystal alignment plane for light with a wavelength of λ nm, of 7 or more, more preferably 20 or more, and even more preferably 30 or more. The higher this value, the more excellent the polarization characteristics in absorption selectivity are. Depending on the type of dichroic dye, when the liquid crystal layer 11 is a nematic liquid crystal phase, the above ratio is about 5 to 10. When the liquid crystal layer 11 is a nematic liquid crystal phase or a smectic liquid crystal phase described later, it can be confirmed that the liquid crystal compound and the dichroic dye are not phase-separated, for example, by observing the surface with various microscopes or measuring the scattering degree with a haze meter.

[0014] 1(a) and 1(b), the liquid crystal layer 11 has a first region 11a and a second region 11b that are distinguished by a luminous-corrected polarization degree (Py) and a dichroic dye content. The polarizing film 1 shown in FIG. 1(a) has two regions each having different luminous-corrected polarization degrees (Py) and different dichroic dye contents, but there may be two or more first regions and two or more second regions, or there may be three or more regions each having different dichroic dye contents.

[0015] 1(a) of the polarizing film 1, the first region 11a contains a liquid crystal compound and a dichroic dye. The second region 11b contains a liquid crystal compound, but may or may not contain a dichroic dye. If the second region 11b contains a dichroic dye, the content of the dichroic dye is preferably lower than the content of the dichroic dye contained in the first region 11a.

[0016] The content of the dichroic dye in the liquid crystal layer 11 is, for example, the maximum absorption wavelength (λ MAX ) can be determined by measuring the absorbance at

[0017] The first region 11a is preferably a region having high polarization characteristics, and for example, the luminous-corrected polarization degree (Py) can be 90% or more, preferably 92% or more, more preferably 95% or more, and usually 100% or less. The first region 11a can also have a luminous-corrected single transmittance (Ty) of, for example, 35% or more, preferably 40% or more, more preferably 44% or more, and usually less than 50%.

[0018] The second region 11b is preferably a low polarization region having a luminosity-corrected polarization degree (Py) lower than that of the first region 11a. The luminosity-corrected polarization degree (Py) of the second region 11b can be, for example, 10% or less, preferably 5% or less, more preferably 1% or less, and may be 0%. The second region 11b also preferably has a luminosity-corrected single transmittance (Ty) higher than that of the first region 11a. The luminosity-corrected single transmittance (Ty) of the second region 11b can be, for example, 80% or more, preferably 85% or more, more preferably 88% or more, and is usually 98% or less.

[0019] The luminosity-corrected polarization degree (Py) and luminosity-corrected single transmittance (Ty) in this specification can be calculated based on the polarization degree and single transmittance measured using a spectrophotometer. For example, the transmittance (T1) in the transmission axis direction (perpendicular to the orientation) and the transmittance (T2) in the absorption axis direction (same orientation direction) in the visible light wavelength range of 380 nm to 780 nm can be measured by a double beam method using a device in which a polarizer-equipped folder is set on a spectrophotometer. The polarization degree and single transmittance in the visible light range can be calculated as the luminosity-corrected single transmittance (Ty) and the luminosity-corrected polarization degree (Py) by calculating the polarization degree and single transmittance at each wavelength using the following formulas (Formula 1) and (Formula 2), and further performing luminosity correction using a 2-degree visual field (C light source) of JIS Z 8701.

[0020] Polarization degree [%] = {(T1-T2) / (T1+T2)} x 100 (Equation 1) Single-body transmittance [%] = (T1 + T2) / 2 (Equation 2)

[0021] The occupied area of ​​the first region 11a and the occupied area of ​​the second region 11b may be appropriately selected according to the characteristics required for the polarizing film 1. The ratio of the total occupied area of ​​the first region 11a and the second region 11b to the surface area of ​​the polarizing film 1 is preferably 90% or more, more preferably 95% or more, and even more preferably 99% or more. The occupied area of ​​the first region 11a is preferably 50% or more, more preferably 70% or more, and even more preferably 80% or more, relative to the total occupied area of ​​the first region 11a and the second region 11b. For example, as shown in FIG. 1(a), the occupied area of ​​the second region 11b may be smaller than the occupied area of ​​the first region 11a, and the first region 11a may be provided so as to surround the second region 11b. In the polarizing film 1 shown in FIG. 1(a), the first region 11a is provided so as to surround one circular second region 11b, but a plurality of second regions 11b may be provided independently.

[0022] The shape of the first region 11a and the shape of the second region 11b are not particularly limited. For example, when the first region 11a is provided so as to surround the second region 11b as shown in FIG. 1(a), the second region 11b can be formed in any shape in a plan view, such as a circle; an ellipse; an oval; a polygon such as a triangle, square, rectangle, or rhombus; a character shape; or a combination of these.

[0023] The second region 11b is preferably circular, elliptical, oval, or polygonal in plan view. When the second region 11b is circular, its diameter is preferably 5 cm or less, more preferably 3 cm or less, and even more preferably 2 cm or less. When the second region 11b is elliptical or oval, its major axis is preferably 5 cm or less, more preferably 3 cm or less, and even more preferably 2 cm or less. When the second region 11b is polygonal, the diameter of a virtual circle drawn so as to inscribe this polygon is preferably 5 cm or less, more preferably 3 cm or less, and even more preferably 2 cm or less. The second region 11b having the above-mentioned shape can be suitably used as a region corresponding to the lens position of a camera provided in a smartphone, tablet, or the like. In addition, in this case, by making the second region 11b a region having a luminous-corrected polarization degree (Py) of 10% or less and a luminous-corrected single transmittance (Ty) of 80% or more, coloring of the second region 11b can be reduced and excellent transparency can be obtained, thereby improving the performance of the camera.

[0024] Furthermore, the first region 11a and the second region 11b may be provided so that their planar shape is linear, band-like, wavy, or the like. In this case, the first region 11a and the second region 11b may be provided in multiple alternating fashion. In this case, the width of the first region 11a and the second region 11b is preferably 1 μm to 10 mm, more preferably 1 μm to 1 mm, and further preferably 1 μm to 100 μm, respectively.

[0025] In addition, when the polarizing film is a long polarizing film, the long polarizing film is usually cut to a predetermined size depending on the application of the polarizing film, etc., and therefore, it is preferable to set the arrangement of the first region 11a and the second region 11b in the long polarizing film so that the first region 11a and the second region 11b are formed at predetermined positions in the polarizing film after cutting. For example, when the polarizing film after cutting is the polarizing film 1 shown in Fig. 1(a), it is preferable to provide a plurality of second regions 11b at predetermined intervals in the length direction and / or width direction of the long polarizing film.

[0026] The thickness of the first region 11a in the liquid crystal layer 11 is preferably 0.5 μm or more, more preferably 1 μm or more, and preferably 5 μm or less, and more preferably 3 μm or less. The thickness of the second region 11b in the liquid crystal layer 11 is preferably the same as that of the first region 11a, and is preferably 0.5 μm or more, more preferably 1 μm or more, and preferably 5 μm or less, and more preferably 3 μm or less. The thickness of the liquid crystal layer 11 can be measured with an interference thickness meter, a laser microscope, a stylus thickness meter, or the like.

[0027] The thickness of the second region 11b may be smaller than that of the first region 11a, but the difference between the thickness of the first region 11a and the thickness of the second region 11b is preferably 2 μm or less, more preferably 1 μm or less, and even more preferably 0.5 μm or less. By making the thicknesses of the first region 11a and the second region 11b of the liquid crystal layer 11 approximately the same and reducing the step between the first region 11a and the second region 11b, defects such as air bubbles being trapped and wrinkles occurring can be suppressed when a retardation layer or other layers (such as a surface protection layer) described later are laminated on the liquid crystal layer 11. In addition, defects such as the formation of rolling marks can be suppressed when the polarizing film 1 having the liquid crystal layer 11 is wound into a roll.

[0028] (liquid crystal compound) A known liquid crystal compound can be used as the liquid crystal compound contained in the liquid crystal layer 11. The type of liquid crystal compound is not particularly limited, and a rod-shaped liquid crystal compound, a discotic liquid crystal compound, or a mixture thereof can be used. In addition, the liquid crystal compound may be a polymer liquid crystal compound, a polymerizable liquid crystal compound, or a mixture thereof.

[0029] As the liquid crystal compound, it is preferable to use a polymerizable liquid crystal compound. By using a polymerizable liquid crystal compound, the hue of the polarizing film can be arbitrarily controlled, and the polarizing film can be significantly thinned. In addition, since the polarizing film can be produced without performing a stretching process, it is possible to obtain a non-stretchable polarizing film that is not relaxed by stretching due to heat.

[0030] The polymerizable liquid crystal compound refers to a compound having a polymerizable group and liquid crystallinity. The polymerizable group means a group involved in a polymerization reaction, and is preferably a photopolymerizable group. Here, the photopolymerizable group refers to a group that can be involved in a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator described later. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, or an oxetanyl group is preferable, and an acryloyloxy group is more preferable. The liquid crystallinity may be a thermotropic liquid crystal or a lyotropic liquid crystal, but when mixed with a dichroic dye as in the liquid crystal layer of the present embodiment, it is preferable to use a thermotropic liquid crystal.

[0031] When the polymerizable liquid crystal compound is a thermotropic liquid crystal, it may be a thermotropic liquid crystal compound exhibiting a nematic liquid crystal phase, or a thermotropic liquid crystal compound exhibiting a smectic liquid crystal phase. When the liquid crystal layer 11 exhibits a polarizing function as a polymer film obtained by a polymerization reaction, the liquid crystal state exhibited by the polymerizable liquid crystal compound is preferably a smectic phase, and more preferably a high-order smectic phase from the viewpoint of high performance. Among them, a high-order smectic liquid crystal compound forming a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, or a smectic L phase is more preferable, and a high-order smectic liquid crystal compound forming a smectic B phase, a smectic F phase, or a smectic I phase is even more preferable. When the liquid crystal layer 11 formed by the polymerizable liquid crystal compound is in these higher-order smectic phases, a region with higher polarization performance can be formed in the liquid crystal layer 11. In addition, in such a region with higher polarization performance, a Bragg peak derived from a higher-order structure such as a hexatic phase or a crystalline phase is obtained in X-ray diffraction measurement. The Bragg peak is a peak derived from a periodic structure of molecular orientation, and a film with a periodic interval of 3 to 6 Å can be obtained. In the polarizing film 1 of the present embodiment, it is preferable that the liquid crystal layer 11 contains a polymer obtained by polymerizing the polymerizable liquid crystal compound in a smectic phase state, since this can impart higher polarization properties to, for example, the first region 11a.

[0032] Whether or not the polymerizable liquid crystal compound exhibits a nematic liquid crystal phase or a smectic liquid crystal phase can be confirmed, for example, as follows. After a coating film is formed by applying a composition for forming a polarizing film to a substrate, the coating film is heated under conditions in which the polymerizable liquid crystal compound does not polymerize, thereby removing the solvent contained in the coating film. Next, the coating film formed on the substrate is heated to an isotropic phase temperature, and gradually cooled to develop a liquid crystal phase, which is then inspected by texture observation using a polarizing microscope, X-ray diffraction measurement, or differential scanning calorimetry.

[0033] Specific examples of such polymerizable liquid crystal compounds include those represented by the following formula (A): U1 -V 1 -W 1 -X 1 -Y 1 -X 2 -Y 2 -X 3 -W 2 -V 2 -U 2 (A) [In formula (A), X 1 , X 2 and X 3 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group, wherein a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. 1 , X 2 and X 3 At least one of these is a 1,4-phenylene group which may have a substituent or a cyclohexane-1,4-diyl group which may have a substituent. Y 1 , Y 2 , W 1 and W 2 are each independently a single bond or a divalent linking group. V 1 and V 2 each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, and -CH2- constituting the alkanediyl group may be replaced by -O-, -S- or NH-. U 1 and U 2 each independently represents a polymerizable group or a hydrogen atom, and at least one of them is a polymerizable group. (hereinafter, may be referred to as compound (A)).

[0034] In compound (A), X 1 , X 2 and X 3At least one of X is an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group. 1 and X 3 is preferably a cyclohexane-1,4-diyl group which may have a substituent, and the cyclohexane-1,4-diyl group is more preferably a trans-cyclohexane-1,4-diyl group. When the cyclohexane-1,4-diyl group structure is contained, smectic liquid crystallinity tends to be easily exhibited. In addition, examples of the optional substituents of the 1,4-phenylene group which may have a substituent and the cyclohexane-1,4-diyl group which may have a substituent include an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, or a butyl group, a cyano group, and a halogen atom such as a chlorine atom or a fluorine atom. It is preferably unsubstituted.

[0035] Y 1 and Y 2 are each independently a single bond, -CH2CH2-, -CH2O-, -COO-, -OCO-, -N=N-, -CR a =CR b -, -C≡C- or CR a =N- is preferred, R a and R b each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 and Y 2 is more preferably -CH2CH2-, -COO-, -OCO- or a single bond, 1 , X 2 and X 3 When none of Y contains a cyclohexane-1,4-diyl group, 1 and Y 2 It is more preferable that Y are different from each other in the bonding method. 1 and Y 2 When the bonding modes are different from each other, smectic liquid crystallinity tends to be easily exhibited.

[0036] W 1 and W 2are preferably, independently of each other, a single bond, -O-, -S-, -COO- or -OCO-, and more preferably, are, independently of each other, a single bond or -O-.

[0037] V 1 and V 2 Examples of the alkanediyl group having 1 to 20 carbon atoms represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,14-diyl group, and an icosane-1,20-diyl group. 1 and V 2 is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably a linear alkanediyl group having 6 to 12 carbon atoms. By using a linear alkanediyl group having 6 to 12 carbon atoms, crystallinity is improved and smectic liquid crystallinity tends to be easily exhibited.

[0038] Examples of the substituent that the optionally substituted alkanediyl group having 1 to 20 carbon atoms may have include a cyano group and a halogen atom such as a chlorine atom or a fluorine atom. The alkanediyl group is preferably unsubstituted, and more preferably an unsubstituted and linear alkanediyl group.

[0039] U 1 and U 2 Preferably, both of are polymerizable groups, and more preferably, both are photopolymerizable groups. A polymerizable liquid crystal compound having a photopolymerizable group can be polymerized under a lower temperature condition than a thermally polymerizable group, and is therefore advantageous in that a polymer of the polymerizable liquid crystal compound can be formed in a state of high order.

[0040] U 1 and U 2The polymerizable groups represented by may be different from each other, but are preferably the same. Examples of the polymerizable group include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group, or an oxetanyl group is preferred, and a methacryloyloxy group or an acryloyloxy group is more preferred.

[0041] Examples of such polymerizable liquid crystal compounds include the following.

[0042] [ka]

[0043] [ka]

[0044] [ka]

[0045] [ka]

[0046] Among the above-listed compounds, at least one selected from the group consisting of compounds represented by formula (1-2), formula (1-3), formula (1-4), formula (1-6), formula (1-7), formula (1-8), formula (1-13), formula (1-14) and formula (1-15) is preferred.

[0047] The exemplified compounds (A) can be used alone or in combination in the liquid crystal layer 11. When two or more polymerizable liquid crystal compounds are combined, it is preferable that at least one of them is compound (A), and more preferable that two or more of them are compound (A). By combining two or more polymerizable liquid crystal compounds, liquid crystallinity may be temporarily maintained even at a temperature below the liquid crystal-crystal phase transition temperature. When two types of polymerizable liquid crystal compounds are combined, the mixing ratio is usually 1:99 to 50:50, preferably 5:95 to 50:50, and more preferably 10:90 to 50:50.

[0048] Compound (A) can be produced by known methods, for example, as described in Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996) or Japanese Patent No. 4719156.

[0049] The content of the polymerizable liquid crystal compound in the liquid crystal layer 11 is usually 50 to 99.5 parts by mass, preferably 60 to 99 parts by mass, more preferably 70 to 98 parts by mass, and further preferably 80 to 97 parts by mass, based on 100 parts by mass of the solid content of the liquid crystal layer 11. If the content of the polymerizable liquid crystal compound is within the above range, the alignment tends to be high. Here, the solid content refers to the total amount of components excluding the solvent from the composition for forming the polarizing layer described later.

[0050] (dichroic dye) A dichroic dye is a dye that has different absorbance in the long axis direction of the molecule and absorbance in the short axis direction. A dichroic dye is a dye that exhibits dichroism when oriented together with a liquid crystal compound, and the dichroic dye itself may be polymerizable or may have liquid crystal properties. Dichroic dyes include those that have the property of absorbing visible light. RukoPreferably, the dichroic dye has a maximum absorption wavelength (λMAX) in the range of 380 to 680 nm. Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes, among which azo dyes are preferred. Examples of azo dyes include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes, and preferably bisazo dyes or trisazo dyes. The dichroic dyes may be used alone or in combination of two or more kinds, but in order to obtain absorption over the entire visible light range, it is preferable to combine three or more kinds of dichroic dyes, and more preferably to combine three or more kinds of azo dyes.

[0051] Examples of the azo dye include a dye represented by the formula (I) T 1 -A 1 (-N=NA 2 ) p -N=NA 3 -T 2 (I) [In formula (I), A 1 , A 2 and A 3 each independently represents a 1,4-phenylene group which may have a substituent, a naphthalene-1,4-diyl group, or a divalent heterocyclic group which may have a substituent; T 1 and T 2 are each independently an electron-withdrawing group or an electron-releasing group, and are positioned at substantially 180° with respect to the azo bond plane. p represents an integer of 0 to 4. When p is 2 or more, each A 2 may be the same or different. The -N=N- bond may be replaced with a -C=C-, -COO-, -NHCO- or -N=CH- bond as long as the compound exhibits absorption in the visible region. (hereinafter, may be referred to as "compound (I)").

[0052] A 1 , A 2 and A 3In the above, the 1,4-phenylene group, the naphthalene-1,4-diyl group, and the divalent heterocyclic group may have any of the following substituents: an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, or a butyl group; an alkoxy group having 1 to 4 carbon atoms, such as a methoxy group, an ethoxy group, or a butoxy group; a fluorinated alkyl group having 1 to 4 carbon atoms, such as a trifluoromethyl group; a cyano group; a nitro group; a halogen atom, such as a chlorine atom or a fluorine atom; and a substituted or unsubstituted amino group, such as an amino group, a diethylamino group, or a pyrrolidino group (the substituted amino group means an amino group having one or two alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. The unsubstituted amino group is -NH2.). Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, and a hexyl group. Examples of the alkanediyl group having 2 to 8 carbon atoms include an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, and an octane-1,8-diyl group. In order to include the compound (I) in a highly ordered liquid crystal structure such as a smectic liquid crystal, A 1 , A 2 and A 3 are each independently preferably unsubstituted, a 1,4-phenylene group in which hydrogen is substituted with a methyl group or a methoxy group, or a divalent heterocyclic group, and p is preferably 0 or 1. In particular, it is preferable that p is 1 and 1 , A 2 and A 3 It is more preferable that at least two of the above three structures are 1,4-phenylene groups in terms of both ease of molecular synthesis and high performance.

[0053] Examples of the divalent heterocyclic group include groups in which two hydrogen atoms have been removed from quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, and benzoxazole. 2When is a divalent heterocyclic group, a structure in which the molecular bond angle is substantially 180° is preferred, and specifically, a benzothiazole, benzimidazole, or benzoxazole structure in which two five-membered rings are condensed is more preferred.

[0054] T 1 and T 2 are each independently an electron-withdrawing group or an electron-releasing group, and preferably have different structures; T 1 is an electron withdrawing group and T 2 is an electron releasing group, or T 1 is an electron releasing group and T 2 More preferably, T is an electron withdrawing group. 1 and T 2 are preferably, independently, an alkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, an amino group having one or two alkyl groups having 1 to 6 carbon atoms, an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms, or a trifluoromethyl group, and among these, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, an amino group having one or two alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms is preferred, since a structure having a smaller excluded volume of the molecule is required for inclusion in a highly ordered liquid crystal structure such as a smectic liquid crystal.

[0055] Examples of such azo dyes include the following:

[0056] [ka]

[0057] [ka]

[0058] [In formulas (2-1) to (2-6), B 1~B 20 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the definitions of the substituted amino group and the unsubstituted amino group are as described above), a chlorine atom, or a trifluoromethyl group. 2 , B 6 , B 9 , B 14 , B 18 , B 19 is preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom. n1 to n4 each independently represent an integer of 0 to 3. If n1 is 2 or more, multiple B 2 may be the same or different, If n2 is 2 or more, multiple B 6 may be the same or different, If n3 is 2 or more, multiple B 9 may be the same or different, If n4 is 2 or more, multiple B 14 may be the same or different.

[0059] The anthraquinone dye is preferably a compound represented by formula (2-7).

[0060] [ka]

[0061] [In formula (2-7), R 1 ~R 8 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]

[0062] The oxazine dye is preferably a compound represented by formula (2-8).

[0063] [ka]

[0064] [In formula (2-8), R 9 ~R 15 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]

[0065] The acridine dye is preferably a compound represented by formula (2-9).

[0066] [ka]

[0067] [In formula (2-9), R 16 ~R 23 are each independently a hydrogen atom, -R x , -NH2, -NHR x , -NR x 2, -SR x or a halogen atom. R x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]

[0068] R in formula (2-7), formula (2-8) and formula (2-9) x Examples of the alkyl group having 1 to 4 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and examples of the aryl group having 6 to 12 carbon atoms include a phenyl group, a toluyl group, a xylyl group, and a naphthyl group.

[0069] As the cyanine dye, the compounds represented by formula (2-10) and formula (2-11) are preferred.

[0070] [ka]

[0071] [In formula (2-10), D 1 and D. 2 each independently represents a group represented by any one of formulas (2-10a) to (2-10d).

[0072] [ka] n5 represents an integer from 1 to 3.

[0073] [ka]

[0074] [In formula (2-11), D 3 and D. 4 each independently represents a group represented by any one of formulas (2-11a) to (2-11h). [ka] n6 represents an integer from 1 to 3.

[0075] In terms of obtaining good light absorption characteristics, the content of the dichroic dye (the ratio of the total amount when multiple types are included) is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, and even more preferably 3 to 15 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound in a region having high polarization characteristics such as a luminous-corrected polarization degree (Py) of 90% or more, such as the first region 11a of the liquid crystal layer 11. If the content of the dichroic dye is less than this range, light absorption becomes insufficient and sufficient polarization performance cannot be obtained, and if it is more than this range, the alignment of the liquid crystal molecules may be hindered. In a region having low polarization characteristics such as a luminous-corrected polarization degree (Py) of 10% or less, such as the second region 11b of the liquid crystal layer 11, the content is preferably 0 to 20 parts by mass, more preferably 0 to 10 parts by mass, and even more preferably 0 to 5 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound.

[0076] (base material layer) The polarizing film 1 may have a base layer 13. The base layer 13 can be used to support the alignment layer 12 and the polarizing layer 21 described later when producing the polarizing film 1, as described later, and can also be used to support the liquid crystal layer 11 of the polarizing film 1.

[0077] The substrate layer 13 may be a glass substrate or a resin substrate, but is preferably a resin substrate. In addition, in order to continuously produce the polarizing film 1, it is more preferable that the substrate layer 13 is a long resin substrate that is wound in a roll and then unwound. The resin substrate is preferably a substrate having translucency that allows visible light to pass through. Here, translucency refers to a luminosity-corrected single transmittance of 80% or more for light in the wavelength range of 380 to 780 nm.

[0078] The thickness of the substrate layer 13 is preferably thin in terms of the mass being practically manageable, but if it is too thin, the strength decreases and the processability tends to be poor. The thickness of the substrate layer 13 is usually 5 μm to 300 μm, and preferably 20 μm to 200 μm. The substrate layer 13 may be provided so as to be peelable, and may be peelable from the polarizing film 1 after, for example, the liquid crystal layer 11 of the polarizing film 1 is bonded to a member constituting a display device or a retardation layer described later. This provides the effect of further reducing the thickness of the polarizing film 1.

[0079] Examples of resins constituting the resin substrate include polyolefins such as polyethylene and polypropylene; cyclic olefin resins such as norbornene-based polymers; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide and polyphenylene oxide; and the like.

[0080] Examples of commercially available cellulose ester resin substrates include "FUJITAC FILM" (manufactured by Fuji Photo Film Co., Ltd.); "KC8UX2M", "KC8UY" and "KC4UY" (all manufactured by Konica Minolta Opto, Inc.).

[0081] Examples of commercially available cyclic olefin resins include "Topas" (registered trademark) (manufactured by Ticona, Germany), "Arton" (registered trademark) (manufactured by JSR Corporation), "ZEONOR" (registered trademark), "ZEONEX" (registered trademark) (all manufactured by Zeon Corporation), and "Apel" (registered trademark) (manufactured by Mitsui Chemicals, Inc.). Such cyclic olefin resins can be formed into a film by known means such as a solvent casting method or a melt extrusion method to form a resin substrate. A resin substrate made of a commercially available cyclic olefin resin can also be used. Examples of commercially available resin substrates made of a cyclic olefin resin include "S-Cina" (registered trademark), "SCA40" (registered trademark) (all manufactured by Sekisui Chemical Co., Ltd.), "ZEONOR Film" (registered trademark) (manufactured by Optes Co., Ltd.), and "Arton Film" (registered trademark) (manufactured by JSR Corporation).

[0082] The base layer 13 may have a single-layer structure or a multi-layer structure of two or more layers. When the base layer 13 has a multi-layer structure, the layers may be made of the same material or different materials.

[0083] The base layer 13 may also have a quarter-wave plate function. By the base layer 13 having the quarter-wave plate function, a polarizing film having the function of a circular polarizing plate can be obtained by combining the base layer 13 with the liquid crystal layer 11. This makes it possible to obtain a circular polarizing plate without laminating a retardation layer having a quarter-wave plate function to the polarizing film 1 separately from the base layer 13. In addition, when the base layer 13 has a multi-layer structure, a circular polarizing plate can be obtained by using a layer having a half-wave plate function and a layer having a quarter-wave plate function laminated together, and laminating the liquid crystal layer 11 on the layer having the half-wave plate function. Alternatively, when the base layer 13 has a multi-layer structure, a circular polarizing plate can also be obtained by using a layer having a quarter-wave plate function with reverse wavelength dispersion and a layer having a positive C-plate function laminated together.

[0084] (Alignment layer) The polarizing film 1 may have an alignment layer 12 on a substrate layer 13, and the alignment layer 12 is disposed between the substrate layer 13 and the liquid crystal layer 11. The alignment layer 12 can have an alignment regulating force that aligns the liquid crystal compound in the liquid crystal layer 11 laminated thereon in a desired direction.

[0085] The alignment layer 12 facilitates the alignment of the liquid crystal compound. The state of liquid crystal alignment, such as horizontal alignment, vertical alignment, hybrid alignment, and tilt alignment, varies depending on the properties of the alignment layer 12 and the liquid crystal compound, and the combination can be selected arbitrarily. For example, if the alignment layer 12 is a material that exhibits horizontal alignment as an alignment control force, the liquid crystal compound can form a horizontal alignment or a hybrid alignment, and if the alignment layer 12 is a material that exhibits vertical alignment, the liquid crystal compound can form a vertical alignment or a tilt alignment. The expressions horizontal, vertical, and the like refer to the direction of the long axis of the aligned liquid crystal compound when the polarizing film 1 plane is used as a reference. For example, vertical alignment means that the long axis of the aligned polymerizable liquid crystal is in a direction perpendicular to the polarizing film 1 plane. The vertical here means 90°±20° to the polarizing film 1 plane. Since the polarizing film 1 preferably has the polarization characteristics of the polarizing film 1 plane, the alignment layer 12 is preferably formed using a material that exhibits horizontal alignment.

[0086] The alignment regulating force of the alignment layer 12 can be arbitrarily adjusted by the surface state or rubbing conditions when the alignment layer 12 is made of an alignment polymer, and can be arbitrarily adjusted by the polarized light irradiation conditions, etc. In addition, the liquid crystal alignment can be controlled by selecting the physical properties, such as the surface tension and liquid crystallinity, of the polymerizable liquid crystal compound.

[0087] The thickness of the alignment layer 12 is usually 10 nm to 5000 nm, preferably 10 nm to 1000 nm, and more preferably 30 nm to 300 nm. The alignment layer 12 formed between the substrate layer 13 and the liquid crystal layer 11 is preferably insoluble in a solvent used when forming the liquid crystal layer 11 on the alignment layer 12, and is preferably heat resistant to removal of the solvent and heat treatment for aligning the liquid crystal.

[0088] Examples of the alignment layer 12 include an alignment film made of an oriented polymer, a photo-alignment film, a groove alignment film, etc. When the base layer 13 is unwound from a roll of a long resin base material, the alignment layer 12 is preferably a photo-alignment film because the alignment direction can be easily controlled.

[0089] Examples of the oriented polymer include polyamides and gelatins having an amide bond in the molecule, polyimides having an imide bond in the molecule, and their hydrolyzates such as polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinylpyrrolidone, polyacrylic acid, and polyacrylic acid esters. Among these, polyvinyl alcohol is preferred. These oriented polymers may be used alone or in combination of two or more.

[0090] An alignment film made of an alignment polymer can usually be obtained by applying a composition in which an alignment polymer is dissolved in a solvent (hereinafter sometimes referred to as an "alignment polymer composition") to a substrate layer 13 and removing the solvent, or by applying an alignment polymer composition to a substrate layer 13, removing the solvent, and rubbing (rubbing method).

[0091] Examples of the solvent used in the oriented polymer composition include water; alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, or propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, or ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, or methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, or heptane; aromatic hydrocarbon solvents such as toluene or xylene, and nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran or dimethoxyethane; and chlorine-substituted hydrocarbon solvents such as chloroform or chlorobenzene. These solvents may be used alone or in combination of two or more.

[0092] The content of the orienting polymer in the orienting polymer composition may be within a range in which the orienting polymer can be completely dissolved in the solvent, and is preferably 0.1 to 20 mass %, more preferably 0.1 to 10 mass %, calculated as solid content relative to the solution.

[0093] As the oriented polymer composition, a commercially available alignment film material may be used as it is. Examples of commercially available alignment film materials include Sunever (registered trademark) (manufactured by Nissan Chemical Industries, Ltd.) and Optomer (registered trademark) (manufactured by JSR Corporation).

[0094] Examples of a method for applying the oriented polymer composition to the substrate layer 13 include known methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography. When the polarizing film 1 is produced by a roll-to-roll continuous production method, the application method can usually be a printing method such as gravure coating, die coating, or flexography.

[0095] The solvent contained in the oriented polymer composition is removed to form a dry coating of the oriented polymer. Methods for removing the solvent include natural drying, ventilation drying, heat drying, and reduced pressure drying. The dried coating is then brought into contact with a rotating rubbing roll wrapped with a rubbing cloth to form the orientation layer 12.

[0096] The photo-alignment film can be obtained by irradiating polarized light (preferably polarized UV) onto a coating layer for an alignment layer formed by coating a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter, sometimes referred to as a "photo-alignment film-forming composition") on a base layer 13. The photo-alignment film is more preferable in that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the polarized light to be irradiated.

[0097] The photoreactive group refers to a group that generates liquid crystal alignment ability by irradiation with light. Specifically, it is a group that generates a photoreaction that is the origin of liquid crystal alignment ability, such as molecular alignment induction or isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction, which occurs by irradiation with light. Among the photoreactive groups, those that cause a dimerization reaction or a photocrosslinking reaction are preferred in terms of excellent alignment ability. As the photoreactive group that can generate the above-mentioned reaction, those having an unsaturated bond, particularly a double bond, are preferred, and groups having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond) are more preferred.

[0098] Examples of photoreactive groups having a C=C bond include vinyl groups, polyene groups, stilbene groups, stilbazolyl groups, stilbazolium groups, chalcone groups, and cinnamoyl groups. From the viewpoint of easy control of reactivity and expression of alignment control force during photoalignment, chalcone groups and cinnamoyl groups are preferred. Examples of photoreactive groups having a C=N bond include groups having a structure such as aromatic Schiff bases or aromatic hydrazones. Examples of photoreactive groups having an N=N bond include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, formazan groups, and groups having azoxybenzene as a basic structure. Examples of photoreactive groups having a C=O bond include benzophenone groups, coumarin groups, anthraquinone groups, and maleimide groups. These groups may have a substituent such as an alkyl group, an alkoxy group, an aryl group, an allyloxy group, a cyano group, an alkoxycarbonyl group, a hydroxyl group, a sulfonic acid group, or a halogenated alkyl group.

[0099] The solvent for the composition for forming a photo-alignment film is preferably one that dissolves the polymer and monomer having a photoreactive group, and examples of the solvent include the solvents exemplified above as the solvent for the alignment polymer composition.

[0100] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted depending on the type of the polymer or monomer having a photoreactive group and the thickness of the photo-alignment film to be produced, but is preferably 0.2 mass% or more, and more preferably in the range of 0.3 to 10 mass%. In addition, polymer materials such as polyvinyl alcohol and polyimide and photosensitizers may be contained within a range that does not significantly impair the properties of the photo-alignment film.

[0101] The method for applying the composition for forming a photo-alignment film to the substrate layer 13 may be the same as the method for applying the above-mentioned oriented polymer composition to the substrate layer 13. The method for removing the solvent from the applied composition for forming a photo-alignment film may be the same as the method for removing the solvent from the oriented polymer composition.

[0102] The polarized light irradiation may be performed directly from the dried film obtained by removing the solvent from the composition for forming a photo-aligned film coated on the substrate layer 13, or may be performed from the substrate layer 13 side so that the polarized light transmitted through the substrate layer 13 is irradiated onto the dried film. In addition, it is particularly preferable that the polarized light used for the polarized light irradiation is substantially parallel light. The wavelength of the polarized light to be irradiated is preferably in a wavelength range in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength of 250 to 400 nm is particularly preferable. Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, and ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, or metal halide lamps are more preferable. These lamps are preferable because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. Polarized light can be irradiated by passing light from the light source through an appropriate polarizer. As such a polarizer, a polarizing filter, a polarizing prism such as a Glan-Thompson or Glan-Taylor type polarizer, or a wire grid type polarizer can be used.

[0103] If masking is performed during rubbing or polarized light irradiation, a plurality of regions (patterns) in which the liquid crystal alignment directions are different can be formed.

[0104] A groove alignment film is a film that has a concave-convex pattern or multiple grooves on the film surface. When liquid crystal molecules are placed on a film that has multiple equally spaced linear grooves, the liquid crystal molecules are oriented in the direction along the grooves.

[0105] Methods for obtaining a groove alignment film include a method of forming a concave-convex pattern by exposing a photosensitive polyimide film surface through an exposure mask having slits in a pattern shape, followed by development and rinsing, a method of forming a layer of UV-curable resin before curing on a plate-shaped master having grooves on the surface, transferring the resin layer to a substrate and curing it, a method of pressing a roll-shaped master having a plurality of grooves against a film of UV-curable resin before curing formed on a substrate to form concave-convex patterns, and then curing the film, etc. Specific examples of the method include the methods described in JP-A-6-34976 and JP-A-2011-242743.

[0106] In order to obtain an alignment with little alignment disturbance, the width of the convex portions of the groove alignment film is preferably 0.05 μm to 5 μm, the width of the concave portions is preferably 0.1 μm to 5 μm, and the depth of the unevenness is preferably 2 μm or less, more preferably 0.01 μm to 1 μm or less.

[0107] (Other layers) The polarizing film 1 may have layers other than the substrate layer 13 and the alignment layer 12. For example, a surface protective layer for protecting the surface of the liquid crystal layer 11 may be provided on the surface of the liquid crystal layer 11 opposite to the substrate layer 13. In addition, when the substrate layer 13 is peeled off before use, a surface protective layer may be provided on the surface of the liquid crystal layer 11 from which the substrate layer 13 has been peeled off. The surface protective layer may have a single layer structure or a multilayer structure. When the surface protective layer has a multilayer structure, the layers may be formed from the same material or from different materials.

[0108] <Circular polarizing plate> 2(a) to 2(c) are schematic cross-sectional views showing an example of the circular polarizer of the present invention. The polarizing film 1 shown in FIG. 1(b) can be made into the circular polarizers 5a and 5b shown in FIG. 2(a) and 2(b) by laminating a retardation layer 15 having a ¼ wavelength plate function. The retardation layer 15 may be laminated on the liquid crystal layer 11 side of the polarizing film 1 (FIG. 2(a)), or on the base layer 13 side (FIG. 2(b)). In addition, the circular polarizer 5a shown in FIG. 2(a) from which the base layer 13 has been peeled off can be used as the circular polarizer 5c (FIG. 2(c)). In this case, the alignment layer 12 may be peeled off together with the base layer 13.

[0109] The circular polarizing plate may be a laminate of the polarizing film 1 and a multilayered retardation layer. In this case, a retardation layer in which a layer having a 1 / 2 wavelength plate function and a layer having a 1 / 4 wavelength plate function are laminated can be used as the multilayered retardation layer, and a circular polarizing plate can be obtained by laminating the layer having the 1 / 2 wavelength plate function of the multilayered retardation layer and the polarizing film 1. Alternatively, a circular polarizing plate can be obtained by using a retardation layer in which a layer having a 1 / 4 wavelength plate function with reverse wavelength dispersion and a layer having a positive C plate function are laminated as the multilayered retardation layer.

[0110] Furthermore, a layer having a function as a retardation layer may be used as the base layer 13 of the polarizing film 1, and a retardation layer may be further laminated thereon to form a circular polarizing plate. In this case, the functions of the base layer 13 and the retardation layer as a retardation layer may be selected according to the lamination positions of the base layer 13 and the retardation layer in the circular polarizing plate.

[0111] The polarizing film and the retardation layer can be laminated via an adhesive layer using a known pressure-sensitive adhesive or adhesive.

[0112] <Polarizing Film Manufacturing Method (First Manufacturing Method)> 3(a) to (d) are schematic cross-sectional views showing layer structures obtained in each step of the manufacturing process of the polarizing film 1 shown in FIG. 1(b). The first manufacturing method of the polarizing film 1 includes the following steps: a preparation step of preparing a laminated film 62 (FIG. 3(b)) having a polarizing layer 21 containing a liquid crystal compound and a dichroic dye on at least one side of a base layer 13; The method includes a liquid contacting process for reducing the content of dichroic dye in a portion of the polarizing layer 21 of the laminate film 62 by contacting the portion of the polarizing layer 21 with a liquid that can reduce the content of dichroic dye in the polarizing layer 21.

[0113] The liquid contacting step includes a protective layer laminating step of laminating a protective layer 35 having a covering region 35a for covering the polarizing layer 21 and an exposed region 35b for exposing the polarizing layer 21 on the polarizing layer 21 of the laminated film 62 to obtain a laminated film 63 with a protective layer (FIG. 3(c)). a bleaching step of bringing the laminate film 63 with the protective layer into contact with a liquid material capable of reducing the content of the dichroic dye in the polarizing layer 21 to obtain a bleached laminate film 64 ( FIG. 3( d )) in which the content of the dichroic dye in a partial region of the polarizing layer 21 is reduced; The method includes a peeling step of peeling the protective layer 35 from this bleached laminate film 64, whereby the polarizing film 1 shown in FIG. 1(b) can be produced.

[0114] (preparation process) The laminated film 62 prepared in the preparation step is not particularly limited as long as it has a polarizing layer 21 on at least one side of the base layer 13, but is preferably one in which an alignment layer 12 and a polarizing layer 21 are laminated in this order on the base layer 13, as shown in Fig. 3(b). Such a laminated film 62 can be manufactured through an alignment layer formation step in which an alignment layer-forming composition is applied to one side of the base layer 13 to form an alignment layer 12 to obtain a base layer with an alignment layer 61 (Fig. 3(a)), and a polarizing layer formation step in which a polarizing layer-forming composition is applied to the surface of the base layer with an alignment layer 61 on the side on which the alignment layer 12 is formed to form the polarizing layer 21.

[0115] In the alignment layer forming step, the substrate layer 13 may be subjected to a surface treatment before the alignment layer forming composition is applied. Examples of the surface treatment method include corona treatment, plasma treatment, laser treatment, ozone treatment, saponification treatment, flame treatment, application of a coupling agent, and primer treatment. As the alignment layer forming composition, the above-mentioned alignment polymer composition, photo-alignment film forming composition, and composition containing a resin material for forming a groove alignment film can be used. The method of forming an alignment layer using each composition is also as described above. For example, when the alignment layer forming composition contains a photo-alignment polymer, the alignment layer forming step can form an alignment layer having an alignment regulating force in a predetermined direction by irradiating the alignment layer coating layer formed by applying the alignment layer forming composition with polarized light.

[0116] The composition for forming the polarizing layer is a composition containing a liquid crystal compound and a dichroic dye, and preferably contains a solvent and a polymerization initiator, and may contain a sensitizer, a polymerization inhibitor, a leveling agent, a reactive additive, etc. As the liquid crystal compound and the dichroic dye, those described above can be used, and as the solvent, polymerization initiator, sensitizer, polymerization inhibitor, leveling agent, and reactive additive, those described below can be used.

[0117] Examples of methods for applying the composition for forming a polarizing layer include extrusion coating, direct gravure coating, reverse gravure coating, CAP coating, slit coating, microgravure, die coating, and inkjet coating. Examples of methods for applying the composition using a coater such as a dip coater, a bar coater, or a spin coater are also included. Among these, when applying continuously in a roll-to-roll format, the microgravure, inkjet, slit coating, and die coating methods are preferred, and when applying to a sheet of substrate such as glass, the spin coating method, which has high uniformity, is preferred. When applying in a roll-to-roll format, the composition for forming an alignment film or the like is applied to the substrate layer 13 to form an alignment layer 12, and the composition for forming a polarizing layer can be applied continuously on the resulting alignment layer 12.

[0118] When the polarizing layer 21 is formed by coating the composition for forming a polarizing layer, the solvent is removed from the applied composition for forming a polarizing layer to form a coating layer for the polarizing layer. The method for removing the solvent can be the same as the method for removing the solvent from the orientable polymer composition, and examples of the method include natural drying, ventilation drying, heat drying, reduced pressure drying, and combinations of these. Of these, natural drying or heat drying is preferred. The drying temperature is preferably in the range of 0 to 200°C, more preferably in the range of 20 to 150°C, and even more preferably in the range of 50 to 130°C. The drying time is preferably 10 seconds to 10 minutes, and more preferably 30 seconds to 5 minutes.

[0119] When the liquid crystal compound contained in the composition for forming a polarizing layer is a polymerizable liquid crystal compound, it is preferable to irradiate the coating layer for the polarizing layer formed in the polarizing layer forming step with active energy rays to photopolymerize the polymerizable liquid crystal compound and form the polarizing layer 21 as a polymer layer of the polymerizable liquid crystal compound. The active energy rays to be irradiated are appropriately selected according to the type of polymerizable liquid crystal compound contained in the coating layer for the polarizing layer (particularly, the type of photopolymerizable functional group possessed by the polymerizable liquid crystal compound), the type of photopolymerization initiator if included, and the amount thereof. Specifically, one or more types of light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α rays, β rays, and γ rays can be mentioned. Among them, ultraviolet light is preferable in terms of ease of controlling the progress of the polymerization reaction and the fact that photopolymerization devices widely used in this field can be used, and it is preferable to select the type of polymerizable liquid crystal compound so that it can be photopolymerized by ultraviolet light.

[0120] Examples of light sources for active energy rays include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, xenon lamps, halogen lamps, carbon arc lamps, tungsten lamps, gallium lamps, excimer lasers, LED light sources emitting light in the wavelength range of 380 to 440 nm, chemical lamps, black light lamps, microwave-excited mercury lamps, and metal halide lamps.

[0121] The irradiation intensity of active energy rays is usually 10 mW / cm 2 ~3000mW / cm 2 The irradiation intensity of the active energy rays is preferably an intensity in a wavelength region effective for activating a cationic polymerization initiator or a radical polymerization initiator. The time for irradiating the active energy rays is usually 0.1 seconds to 10 minutes, preferably 0.1 seconds to 5 minutes, more preferably 0.1 seconds to 3 minutes, and further preferably 0.1 seconds to 1 minute. When irradiating once or multiple times with such an irradiation intensity of the active energy rays, the integrated light amount is 10 mJ / cm 2 ~3000mJ / cm 2 , preferably 50 mJ / cm 2 ~2,000mJ / cm 2 , more preferably 100 mJ / cm 2 ~1000mJ / cm 2 If the accumulated light amount is less than this range, the polymerizable liquid crystal compound may not be sufficiently cured, and good transferability may not be obtained. Conversely, if the accumulated light amount is more than this range, the polarizing layer may be colored.

[0122] (solvent) The polarizing layer forming composition may contain a solvent. In general, polymerizable liquid crystal compounds have high viscosity, so when a polymerizable liquid crystal compound is used as the liquid crystal compound, the polarizing layer forming composition containing a solvent is used to facilitate coating, and as a result, the polarizing layer is easily formed. The solvent is preferably one that can completely dissolve the polymerizable liquid crystal compound and the dichroic dye, and is preferably a solvent that is inactive to the polymerization reaction of the polymerizable liquid crystal compound.

[0123] Examples of the solvent include alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, ethylene glycol methyl ether, ethylene glycol butyl ether, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-heptanone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene; nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorine-containing solvents such as chloroform and chlorobenzene; dimethylacetamide, dimethylformamide, and the like. M Examples of the solvent include amide-based solvents such as amide, N-methyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, etc. These solvents may be used alone or in combination of two or more kinds.

[0124] The content of the solvent contained in the composition for forming a polarizing layer is preferably 50 to 98% by mass with respect to the total amount of the composition for forming a polarizing layer. In other words, the content of solids in the composition for forming a polarizing layer is preferably 2 to 50% by mass. When the content of solids is 50% by mass or less, the viscosity of the composition for forming a polarizing layer is low, so that the thickness of the polarizing layer 21 becomes approximately uniform and unevenness in the polarizing layer 21 tends to be less likely to occur. The content of solids can be determined in consideration of the thickness of the polarizing layer 21 to be manufactured.

[0125] (Polymerization initiator) The composition for forming the polarizing layer may contain a polymerization initiator. The polymerization initiator can be used when a polymerizable liquid crystal compound is used as the liquid crystal compound, and is a compound capable of initiating a polymerization reaction of the polymerizable liquid crystal compound, etc. As the polymerization initiator, a photopolymerization initiator that generates active radicals by the action of light is preferable from the viewpoint of not depending on the phase state of the thermotropic liquid crystal.

[0126] Examples of the polymerization initiator include a benzoin compound, a benzophenone compound, an alkylphenone compound, an acylphosphine oxide compound, a triazine compound, an iodonium salt, or a sulfonium salt.

[0127] Examples of the benzoin compound include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.

[0128] Examples of the benzophenone compound include benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.

[0129] Examples of the alkylphenone compound include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethane-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.

[0130] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.

[0131] Examples of the triazine compound include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethenyl]-1,3,5-triazine. 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine are examples thereof.

[0132] As the polymerization initiator, a commercially available one can also be used. Examples of commercially available polymerization initiators include Irgacure (registered trademark) 907, 184, 651, 819, 250, 369, 379, 127, 754, OXE01, OXE02, or OXE03 (manufactured by Chiba Specialty Chemicals Co., Ltd.); Seikuol (registered trademark) BZ, Z, or BEE (manufactured by Seiko Chemical Co., Ltd.); Kayacure (registered trademark) BP100 or UVI-6992 (manufactured by Dow Chemical Co., Ltd.); Adeka Optomer SP-152, N-1717, N-1919, SP-170, Adeka Arcles NCI-831, Adeka Arcles NCI-930 (manufactured by ADEKA Corporation); TAZ-A or TAZ-PP (manufactured by Nippon SiberHegner Co., Ltd.); and TAZ-104 (manufactured by Sanwa Chemical Co., Ltd.). The composition for forming a polarizing layer may contain one type of polymerization initiator, or two or more types of polymerization initiators may be mixed together in accordance with the light source.

[0133] The content of the polymerization initiator in the composition for forming the polarizing layer can be appropriately adjusted depending on the type and amount of the polymerizable liquid crystal compound, but is usually 0.1 to 30 parts by mass, preferably 0.5 to 10 parts by mass, and more preferably 0.5 to 8 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the polymerization initiator is within the above range, polymerization can be carried out without disturbing the alignment of the polymerizable liquid crystal compound.

[0134] (sensitizer) The polarizing layer forming composition may contain a sensitizer. The sensitizer can be suitably used when a polymerizable liquid crystal compound is used as the liquid crystal compound, and when a polymerizable liquid crystal compound having a photopolymerizable group is used, the sensitizer is preferably a photosensitizer. Examples of the sensitizer include xanthone compounds such as xanthone and thioxanthone (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.); anthracene compounds such as anthracene and an alkoxy group-containing anthracene (e.g., dibutoxyanthracene, etc.); phenothiazine, rubrene, etc.

[0135] When the composition for forming a polarizing layer contains a sensitizer, the polymerization reaction of the polymerizable liquid crystal compound contained in the composition for forming a polarizing layer can be further accelerated. The amount of the sensitizer used is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and even more preferably 0.5 to 3 parts by mass, relative to 100 parts by mass of the content of the polymerizable liquid crystal compound.

[0136] (Polymerization inhibitor) The composition for forming the polarizing layer may contain a polymerization inhibitor from the viewpoint of stably proceeding with the polymerization reaction. The polymerization inhibitor can be suitably used when a polymerizable liquid crystal compound is used as the liquid crystal compound, and the polymerization inhibitor can control the degree of progress of the polymerization reaction of the polymerizable liquid crystal compound.

[0137] Examples of the polymerization inhibitor include radical scavengers such as hydroquinone, alkoxy group-containing hydroquinone, alkoxy group-containing catechol (e.g., butylcatechol, etc.), pyrogallol, and 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenols; β-naphthylamines, and β-naphthols.

[0138] When the composition for forming a polarizing layer contains a polymerization inhibitor, the content of the polymerization inhibitor is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 5 parts by mass, and further preferably 0.5 to 3 parts by mass, relative to 100 parts by mass of the content of the polymerizable liquid crystal compound. When the content of the polymerization inhibitor is within the above range, polymerization can be carried out without disturbing the alignment of the polymerizable liquid crystal compound.

[0139] (Leveling agent) The composition for forming a polarizing layer may contain a leveling agent. The leveling agent is an additive having a function of adjusting the fluidity of the composition and making the film obtained by applying the composition flatter, and examples of the leveling agent include organic modified silicone oil-based, polyacrylate-based, and perfluoroalkyl-based leveling agents. Specifically, DC3PA, SH7PA, DC11PA, SH28PA, SH29PA, SH30PA, ST80PA, ST86PA, SH8400, SH8700, FZ2123 (all manufactured by Dow Corning Toray Co., Ltd.), KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001 (all manufactured by Shin-Etsu Chemical Co., Ltd.), TSF400, TSF401, TSF410, TSF4300, TSF4440, TSF4445, TSF-4446, TSF4452, TSF4460 (all manufactured by Momentive Performance Materials Co., Ltd.) Japan LLC), Fluorinert (registered trademark) FC-72, FC-40, FC-43, FC-3283 (all manufactured by Sumitomo 3M Limited), Megafac (registered trademark) R-08, R-30, R-90, F-410, F-411, F-443, F-445, F-470, F-477, F-479, F-482, F-483 (all manufactured by DIC Corporation), F-top (trade name) EF301, EF303, EF351, EF352 (all manufactured by Mitsubishi Materials Electronics Co., Ltd.), Surflon (registered trademark) S-381, S-382, S-383, S-393, SC-101, SC-105, KH-40, SA-100 (all manufactured by AGC Seimi Chemical Co., Ltd.), trade names E1830, E5844 (manufactured by Daikin Fine Chemical Research Institute Co., Ltd.), BM-1000, BM-1100, BYK-352, BYK-353 or BYK-361N (all trade names: manufactured by BM Chemie Co., Ltd.), etc. Among them, polyacrylate-based leveling agents or perfluoroalkyl-based leveling agents are preferred.

[0140] When the composition for forming a polarizing layer contains a leveling agent, the amount is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the liquid crystal compound. When the amount of the leveling agent is within the above range, the liquid crystal compound is easily aligned horizontally, and the obtained polarizing layer tends to be smoother. When the amount of the leveling agent relative to the liquid crystal compound exceeds the above range, the obtained polarizing layer tends to be easily uneven. The composition for forming a polarizing layer may contain two or more types of leveling agents.

[0141] (Reactive Additives) The composition for forming a polarizing layer may contain a reactive additive. The reactive additive preferably has a carbon-carbon unsaturated bond and an active hydrogen reactive group in its molecule. The "active hydrogen reactive group" here means a group reactive to a group having active hydrogen such as a carboxyl group (-COOH), a hydroxyl group (-OH), or an amino group (-NH2), and representative examples thereof include a glycidyl group, an oxazoline group, a carbodiimide group, an aziridine group, an imide group, an isocyanate group, a thioisocyanate group, and a maleic anhydride group. The number of carbon-carbon unsaturated bonds or active hydrogen reactive groups contained in the reactive additive is usually 1 to 20, and preferably 1 to 10.

[0142] In the reactive additive, it is preferable that at least two active hydrogen reactive groups are present, and in this case, the multiple active hydrogen reactive groups present may be the same or different.

[0143] The carbon-carbon unsaturated bond of the reactive additive may be a carbon-carbon double bond, a carbon-carbon triple bond, or a combination thereof, but is preferably a carbon-carbon double bond. Among them, the reactive additive preferably contains a carbon-carbon unsaturated bond as a vinyl group and / or a (meth)acrylic group. Furthermore, the reactive additive is preferably one in which the active hydrogen reactive group is at least one selected from the group consisting of an epoxy group, a glycidyl group, and an isocyanate group, and more preferably a reactive additive having an acrylic group and an isocyanate group.

[0144] Specific examples of reactive additives include compounds having a (meth)acrylic group and an epoxy group, such as methacryloxyglycidyl ether and acryloxyglycidyl ether; compounds having a (meth)acrylic group and an oxetane group, such as oxetane acrylate and oxetane methacrylate; compounds having a (meth)acrylic group and a lactone group, such as lactone acrylate and lactone methacrylate; compounds having a vinyl group and an oxazoline group, such as vinyl oxazoline and isopropenyl oxazoline; oligomers of compounds having a (meth)acrylic group and an isocyanate group, such as isocyanatomethyl acrylate, isocyanatomethyl methacrylate, 2-isocyanatoethyl acrylate, or 2-isocyanatoethyl methacrylate. In addition, compounds having a vinyl group or a vinylene group and an acid anhydride, such as methacrylic anhydride, acrylic anhydride, maleic anhydride, or vinyl maleic anhydride, can be mentioned. Among these, methacryloxyglycidyl ether, acryloxyglycidyl ether, isocyanatomethyl acrylate, isocyanatomethyl methacrylate, vinyloxazoline, 2-isocyanatoethyl acrylate, 2-isocyanatoethyl methacrylate, or oligomers thereof are preferred, and isocyanatomethyl acrylate, 2-isocyanatoethyl acrylate, or oligomers thereof are particularly preferred.

[0145] Specifically, a compound represented by the following formula (Y) is preferred.

[0146] [ka]

[0147] [In formula (Y), n represents an integer of 1 to 10, and R 1’ represents a divalent aliphatic or alicyclic hydrocarbon group having 2 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 5 to 20 carbon atoms. 2’ is -NH- on one side and >NC(=O)-R on the other side. 3’ R 3’ represents a hydroxyl group or a group having a carbon-carbon unsaturated bond. R in formula (Y) 3’ At least one R 3’ is a group having a carbon-carbon unsaturated bond.

[0148] Among the reactive additives represented by the formula (Y), a compound represented by the following formula (YY) (hereinafter, sometimes referred to as compound (YY)) is particularly preferred (n has the same meaning as above).

[0149] [ka]

[0150] Compound (YY) may be a commercially available product, either as is or after purification as necessary. Commercially available products include, for example, Laromer (registered trademark) LR-9000 (manufactured by BASF).

[0151] When the composition for forming a polarizing layer contains a reactive additive, the content of the reactive additive is usually 0.01 to 10 parts by mass, and preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the liquid crystal compound.

[0152] (Protective layer lamination process) In the protective layer lamination step, as shown in FIG. 3(c), a protective layer 35 having a covering region 35a for covering the polarizing layer 21 and an exposed region 35b for exposing the polarizing layer 21 is laminated on the polarizing layer 21 of the laminate film 62 prepared in the preparation step. This allows a laminate film 63 with a protective layer to be obtained. The exposed region 35b can be, for example, an opening of the protective layer 35. The covering region 35a can prevent a liquid material that can reduce the content of the dichroic dye in the polarizing layer 21, which will be described later, from contacting the laminate film 63 with the protective layer. On the other hand, the exposed region 35b of the protective layer 35 allows the liquid material to come into contact with the polarizing layer 21.

[0153] As described later, when the polarizing layer 21 comes into contact with a liquid, the liquid penetrates into the polarizing layer 21 and causes the dichroic dye to lose its function as a dye. difference It is preferable to form the exposed region 35b in accordance with the region where the exposed region 35b is to be exposed. For example, when manufacturing the polarizing film 1 shown in Fig. 1(a) and (b), it is preferable to determine the shape of the exposed region 35b in accordance with the shape of the second region 11b. For example, if the planar shape of the second region 11b is a circle, an ellipse, an oval, a polygon such as a triangle, a square, a rectangle, or a diamond, a line, a stripe, a wave shape, or the like, the exposed region 35b may be formed in accordance with these shapes.

[0154] For example, when exposed area 35b is circular, its diameter is preferably 5 cm or less, more preferably 3 cm or less, and even more preferably 2 cm or less. When exposed area 35b is elliptical or oval, its major axis is preferably 5 cm or less, more preferably 3 cm or less, and even more preferably 2 cm or less. When exposed area 35b is polygonal, the diameter of an imaginary circle inscribed in this polygon is preferably 5 cm or less, more preferably 3 cm or less, and even more preferably 2 cm or less. As described later, since the liquid permeates into the liquid crystal layer, the size of exposed area 35b may be formed to be slightly smaller than the second area 11b.

[0155] Moreover, it is preferable that the covering region 35a of the protective layer 35 is formed to correspond to a region in the polarizing layer 21 where the content of the dichroic dye is not to be reduced. For example, when manufacturing the polarizing film 1 shown in Figures 1(a) and (b), it is preferable to determine the shape of the covering region 35a in accordance with the shape of the first region 11a.

[0156] A sheet-like substrate having an area to be exposed area 35b formed thereon can be used as protective layer 35. The area to be exposed area 35b can be formed by a method of mechanically punching out a predetermined portion of the sheet-like substrate using punching, a cutting plotter, a water jet, or the like, or by a method of removing a predetermined portion of the sheet-like substrate by laser ablation, chemical dissolution, or the like.

[0157] The sheet-like substrate for forming the protective layer 35 is not particularly limited as long as it is insoluble in a liquid when it is brought into contact with a liquid that can reduce the content of the dichroic dye in the liquid crystal layer described later, and has durability against removal of the liquid and against UV irradiation performed after contact with the liquid. The sheet-like substrate for forming the protective layer 35 can be formed, for example, using the same material as the substrate layer 13 described above, and is preferably formed using a resin substrate, and more preferably uses a polyester resin such as polyethylene terephthalate that is easy to suppress deformation of the region (e.g., opening) that becomes the exposed region 35b of the protective layer 35.

[0158] The protective layer 35 preferably has an adhesive layer for bonding to the polarizing layer 21. Since the protective layer 35 is peeled off as described below, the adhesive layer is preferably peelable from the polarizing layer 21. The thickness of the protective layer 35 is usually 20 μm or more, preferably 30 μm or more, and usually 250 μm or less, preferably 200 μm or less.

[0159] (Decolorization process) In the bleaching step, the laminate film 63 with the protective layer obtained in the protective layer lamination step is brought into contact with a liquid material capable of reducing the content of the dichroic dye in the polarizing layer 21, thereby obtaining a bleached laminate film 64 in which the content of the dichroic dye is reduced in a partial region of the polarizing layer 21 (FIG. 3(d)). The protective layer 35 of the laminate film 63 with the protective layer has a covering region 35a for covering the polarizing layer 21 and an exposed region 35b for exposing the polarizing layer 21, so that the liquid material can come into contact with the polarizing layer 21 in the exposed region 35b. This can reduce the content of the dichroic dye in the region of the polarizing layer 21 that comes into contact with the liquid material.

[0160] The laminated film 63 with the protective layer can be brought into contact with the liquid by immersing the laminated film 63 with the protective layer in the liquid, or by applying, spraying, or dropping the liquid onto the laminated film 63 with the protective layer. It is preferable to immerse the laminated film 63 with the protective layer in the liquid. As a result, the liquid comes into contact with the surface of the polarizing layer 21 exposed from the exposed region 35b of the protective layer 35, and penetrates into the polarizing layer 21. Although the details are not clear, it is considered that the liquid that penetrates into the polarizing layer 21 decomposes the dichroic dye in the polarizing layer 21 or reacts with the dichroic dye, thereby causing the dichroic dye to lose its function as a dye. As a result, a second region 11b, which is a region having a lower content of dichroic dye than other regions, is formed in a part of the polarizing layer 21, and a decolorized laminated film 64 (FIG. 3(d)) having a liquid crystal layer 11 can be obtained.

[0161] In the area of ​​the surface of the polarizing layer 21 covered by the covered area 35a of the protective layer 35, the polarizing layer 21 does not come into direct contact with the liquid, so the liquid is less likely to penetrate into the polarizing layer 21 and the dichroic dye is less likely to disappear. In contrast, in the area of ​​the polarizing layer 21 exposed from the exposed area 35b of the protective layer 35, the polarizing layer 21 comes into direct contact with the liquid, so the liquid is more likely to penetrate into the polarizing layer 21 and the dichroic dye is more likely to disappear. Therefore, in the bleached laminate film 64 shown in FIG. 3(d), a liquid crystal layer 11 having a second region 11b that is a low polarization region having a lower content of dichroic dye than other regions can be formed in the area of ​​the polarizing layer 21 corresponding to the exposed area 35b.

[0162] In this way, by using the laminate film 63 with a protective layer in which the exposed region 35b of the protective layer 35 is disposed in a region of the polarizing layer 21 where it is desired to reduce the content of the dichroic dye, it is possible to form a liquid crystal layer 11 with a reduced content of the dichroic dye in a desired position of the polarizing layer 21. However, since the liquid penetrates into the polarizing layer 21 and causes the function of the dichroic dye to disappear, it is preferable to adjust the thickness of the protective layer 35, the size of the exposed region 35b, the concentration of the liquid, the immersion time of the laminate film with a protective layer in the liquid, the amount of the liquid applied, sprayed or dropped onto the laminate film 63 with a protective layer, and the like, so that the liquid does not penetrate into a region where it is not necessary to reduce the content of the dichroic dye and reduce the content of the dichroic dye.

[0163] The liquid material capable of reducing the content of the dichroic dye in the polarizing layer 21 is not particularly limited as long as it can reduce the content of the dichroic dye, and for example, peroxides (hydrogen peroxide, sodium percarbonate, etc.), chlorine compounds (sodium hypochlorite, etc.), acids (sulfuric acid, nitric acid, hexafluorophosphoric acid), alkalis (sodium hydroxide, potassium hydroxide), etc. can be appropriately used. Among these, acids such as sulfuric acid, nitric acid, and hexafluorophosphoric acid are preferred. These liquid materials may be used alone or in combination.

[0164] The contact conditions for contacting the protective layer-attached laminate film 63 with the liquid may be appropriately selected depending on the thickness of the polarizing layer 21 and the range in which the content of the dichroic dye is to be reduced. The concentration of the liquid is, for example, preferably 20 to 80 mass %, and more preferably 30 to 70 mass %. The temperature of the liquid is preferably 50 to 150°C, and more preferably 80 to 120°C.

[0165] The decolorization step is preferably performed by bringing the protective layer-attached laminate film 63 into contact with a liquid to form a region in part of the polarizing layer 21 having a lower content of dichroic dye than other regions, and then performing a first washing step to wash away the liquid. The first washing step can be performed using water or an organic solvent such as alcohol.

[0166] (Peeling process) In the peeling step, the protective layer 35 is peeled off from the bleached laminate film 64 obtained in the bleaching step. This results in a polarizing film 1 (FIGS. 1(a) and (b)) in which the second region 11b, which is a region having a lower content of dichroic dye than the other regions, is formed in a part of the liquid crystal layer 11.

[0167] The polarizing film 1 shown in Fig. 1(b) can also be used after peeling off the substrate layer 13. In this case, the alignment layer 12 may also be peeled off together with the substrate layer 13. For example, the substrate layer 13 can also be peeled off after the liquid crystal layer 11 of the polarizing film 1 is attached to a member constituting a display device, a retardation layer, or the like.

[0168] (Method for continuously producing polarizing film) The polarizing film 1 can be manufactured continuously, preferably in a roll-to-roll format. In this case, a laminate film wound in a roll shape is prepared in the preparation step, and the laminate film is transported while being unwound, and the protective layer lamination step, the bleaching step, and the peeling step are continuously performed. In the protective layer lamination step, the protective layer wound in a roll shape is transported while being unwound, and the protective layer is bonded to the laminate film to obtain a laminate film with a protective layer. In the bleaching step, the laminate film with a protective layer is passed through a liquid bath filled with a liquid while being continuously transported, or a liquid is applied, sprayed, or dropped onto the laminate film with a protective layer while being continuously transported, to obtain a bleached laminate film. In the peeling step, the protective layer is continuously peeled off from the bleached laminate film, and the polarizing film is wound into a roll to form a rolled body. The polarizing film continuously manufactured as described above can have a length of, for example, 10 m or more.

[0169] When the preparation process includes an alignment layer forming step, the substrate layer wound in a roll shape may be conveyed while being unwound, and the alignment layer may be formed by continuously applying the alignment layer forming composition to the substrate layer using a coating device.When the preparation process includes a polarizing layer forming step, the substrate layer with the alignment layer may be conveyed continuously, and the polarizing layer may be formed by applying the polarizing layer forming composition to the surface of the substrate layer with the alignment layer on which the alignment layer is formed.

[0170] In the polarizing film 1 manufactured by this first manufacturing method, the difference in thickness between the first region 11a and the second region 11b can be made small, for example, to 2 μm or less, and therefore a polarizing film 1 without any steps can be obtained. As a result, even if another film is attached onto the polarizing layer 21 with an adhesive or the like, the other film can be laminated without trapping air bubbles.

[0171] <Polarizing Film Manufacturing Method (Second Manufacturing Method)> The polarizing film 1 can be produced by the second production method described below, in addition to the first production method described above. Fig. 4 is a schematic cross-sectional view showing an example of a liquid contact step in the production method of the polarizing film 1 shown in Fig. 1(b). The second production method of the polarizing film 1 includes the steps of: a preparation step of preparing a laminated film 62 (FIG. 3(b)) having a polarizing layer 21 containing a liquid crystal compound and a dichroic dye on at least one side of a base layer 13; and a liquid contacting step (FIG. 4) of reducing the content of dichroic dye in a partial region of the polarizing layer 21 of the laminate film 62 by contacting the partial region with a liquid that can reduce the content of dichroic dye in the polarizing layer 21, thereby making it possible to produce the polarizing film 1 shown in FIGS. 1(a) and (b).

[0172] The preparation step in the second manufacturing method is the same as the preparation step in the first manufacturing method described above with reference to Figures 3(a) and (b). Through this preparation step, a laminated film 62 having a polarizing layer 21 is prepared.

[0173] In the second manufacturing method, a partial region of the polarizing layer 21 on the laminated film 62 is brought into contact with a liquid (FIG. 4). The liquid used at this time is capable of reducing the content of the dichroic dye in the partial region of the polarizing layer 21, and the same liquid as that used in the bleaching step in the first manufacturing method described above can be used. As a method for bringing the liquid into contact with the partial region of the polarizing layer 21, for example, as shown in FIG. 4, a so-called inkjet method in which the liquid is dropped and applied to the partial region can be mentioned. By bringing the polarizing layer 21 into contact with the liquid, the liquid permeates the partial region of the polarizing layer 21, reducing the content of the dichroic dye and forming a low polarization region.

[0174] The second manufacturing method preferably includes a second washing step of washing away the liquid on the polarizing layer 21 after contacting the polarizing layer 21 with the liquid. The second washing step can be performed using the same organic solvent, such as water or alcohol, used in the first washing step in the first manufacturing method. This makes it possible to obtain the polarizing film 1 shown in FIG. 1(b).

[0175] In the second manufacturing method, as in the first manufacturing method, the polarizing film 1 can be continuously manufactured, for example, by a roll-to-roll method. In this case, a laminated film wound into a roll is prepared in the preparation step, and the laminated film is transported while being unwound, and the liquid contact step is continuously performed. In the liquid contact step, a liquid is applied dropwise to the laminated film while it is continuously transported to obtain a polarizing film, and the obtained polarizing film is wound into a roll to form a rolled body. The polarizing film continuously manufactured as described above can have a length of, for example, 10 m or more.

[0176] When the preparation process includes an alignment layer forming step, the substrate layer wound in a roll shape may be conveyed while being unwound, and the alignment layer may be formed by continuously applying the alignment layer forming composition to the substrate layer using a coating device.When the preparation process includes a polarizing layer forming step, the substrate layer with the alignment layer may be conveyed continuously, and the polarizing layer may be formed by applying the polarizing layer forming composition to the surface of the substrate layer with the alignment layer on which the alignment layer is formed.

[0177] This second manufacturing method also makes it possible to reduce the difference in thickness between the first region 11a and the second region 11b to, for example, 2 μm or less, and obtain a polarizing film 1 without any steps. This makes it possible to laminate another film on the polarizing layer 21 with an adhesive or the like without trapping air bubbles.

[0178] <Method of manufacturing circularly polarizing plate> The circular polarizing plate can be manufactured by laminating the polarizing film 1 and the retardation layer. As described above, when the polarizing film is a continuously manufactured long polarizing film having a length of 10 m or more, it is preferable to use a long retardation layer having a length of 10 m or more as the retardation layer, and to laminate the long polarizing film and the long retardation layer while continuously transporting both to form a long laminate. At this time, it is preferable to coat at least one of the long polarizing film and the long retardation layer with a pressure-sensitive adhesive or adhesive to laminate both.

[0179] The method for producing a circularly polarizing plate may include a step of cutting a long laminate obtained by laminating a long polarizing film and a long retardation layer into sheets of a predetermined size so that the polarizing film can be attached to a display device or the like of a predetermined size. In the cutting step, it is preferable to cut the long laminate in at least one of the length direction and width direction of the long laminate. In this case, it is preferable to determine the cutting position in the long laminate so that the second region 11b of the liquid crystal layer 11 is located at a predetermined position in the cut sheet. EXAMPLES

[0180] The present invention will be described in more detail with reference to examples, although the present invention is not limited to these examples.

[0181] [Luminous sensitivity-corrected polarization degree (Py) and luminous sensitivity-corrected transmittance (Ty)] (Preparation of evaluation samples) The compositions for forming an alignment layer and the compositions for forming a polarizing layer used in each of the Examples, Comparative Examples, and Reference Examples were prepared. The same films as those used as the base layers in each of the Examples, Comparative Examples, and Reference Examples were cut into 40 mm x 40 mm pieces and prepared as base layers for evaluation samples. Using these, evaluation samples were obtained by carrying out the same procedures as in the manufacture of the polarizing films in each of the Examples, Comparative Examples, and Reference Examples, except that in Examples 1, 2, Comparative Examples, and Reference Examples, no protective layer was used, and in Example 3, the entire surface of the polarizing layer was brought into contact with the solution instead of dropping the solution partially onto the polarizing layer.

[0182] (Luminous sensitivity-corrected polarization degree (Py) and luminous sensitivity-corrected transmittance (Ty)) The luminosity-corrected single transmittance (Ty) and luminosity-corrected polarization degree (Py) of the evaluation sample were calculated by the following procedure. The transmittance (T1) in the transmission axis direction and the transmittance (T2) in the absorption axis direction were measured by the double beam method using a spectrophotometer (Shimadzu Corporation UV-3150) equipped with a folder with a polarizer in a wavelength range of 380 nm to 780 nm. The reference side of the folder was equipped with a mesh that cuts the amount of light by 50%. The transmittance and polarization degree at each wavelength were calculated using the following (Equation 1) and (Equation 2), and luminosity correction was performed using a 2-degree visual field (C light source) of JIS Z 8701, and the luminosity-corrected transmittance (Ty) and luminosity-corrected polarization degree (Py) were calculated. Polarization degree [%] = {(T1-T2) / (T1+T2)} x 100 (Equation 1) Single-body transmittance [%] = (T1 + T2) / 2 (Equation 2)

[0183] Example 1 (Production of composition for forming alignment layer) The following components were mixed, and the resulting mixture was stirred at 80° C. for 1 hour to obtain a composition for forming an alignment layer, which is a composition for forming a photoalignment film. -2 parts of polymer having the photoreactive group shown below [ka] Solvent: o-xylene 98 parts

[0184] (Production of composition for forming polarizing layer) A composition for forming a polarizing layer was obtained by mixing the following components and stirring for 1 hour at 80° C. The azo-based dye described in the examples of JP-A-2013-101328 was used as the dichroic dye. 75 parts of a polymerizable liquid crystal compound represented by formula (1-6) [ka] 25 parts of a polymerizable liquid crystal compound represented by formula (1-7) [ka] 2.8 parts of the dichroic dye (1) shown below [ka] 2.8 parts of the dichroic dye (2) shown below [ka] 2.8 parts of the dichroic dye (3) shown below [ka] 6 parts of the polymerization initiator shown below 2-Dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Chiba Specialty Chemicals) 1.2 parts of the leveling agent shown below Polyacrylate compound (BYK-361N; manufactured by BYK-Chemie) 250 parts of the following solvent Cyclopentanone

[0185] (Manufacture of polarizing film) A triacetyl cellulose film (KC4UY-TAC manufactured by Konica Minolta, thickness 40 μm) serving as a base layer was cut into a size of 20 × 20 mm, and its surface was subjected to a corona treatment (AGF-B10 manufactured by Kasuga Electric Co., Ltd.). The composition for forming an alignment layer was applied to the corona-treated film surface using a bar coater, and then dried for 1 minute in a drying oven set at 120°C to obtain a coating layer for the alignment layer. Polarized UV was irradiated onto the coating layer for the alignment layer using a polarized UV irradiation device (SPOT CURE SP-7 manufactured by Ushio Inc.) at 50 mJ / cm. 2An alignment layer was formed by irradiating the film with an integrated light amount (based on 313 nm). A composition for forming a polarizing layer was applied onto the obtained alignment layer using a bar coater, and then dried for 1 minute in a drying oven set at 110°C. Thereafter, ultraviolet light was irradiated using a high-pressure mercury lamp (Unicur VB-15201BY-A, manufactured by Ushio Inc.) (under a nitrogen atmosphere, wavelength: 365 nm, integrated light amount at wavelength 365 nm: 1000 mJ / cm2). 2 ) to obtain a polarizing layer in which the liquid crystal compound and the dichroic dye were oriented. A protective layer (AY-638 manufactured by Fujimori Kogyo Co., Ltd., a 15 μm thick adhesive layer provided on a 38 μm thick polyester film) was laminated on the polarizing layer, in which holes were made with a hole punch to form openings, and then the layer was immersed in a 50 wt % solution of diphenyl 4-thiophenoxyphenylsulfonium hexafluorophosphate (CPI-100P manufactured by San-Apro Co., Ltd.) in propylene carbonate at 120° C. for 60 seconds. The protective layer was then peeled off to obtain a polarizing film.

[0186] When the appearance of the obtained polarizing film was visually observed, a circular area (low polarization area) where no polarizing layer was present was clearly confirmed, and it was found that a polarizing film having a polarizing area and a low polarization area was obtained. In addition, an evaluation sample was prepared using the above-mentioned procedure, and its luminous efficiency-corrected transmittance (Ty) and luminous efficiency-corrected polarization degree (Py) were calculated. The results are shown in Table 1.

[0187] Example 2 A polarizing film was obtained in the same manner as in Example 1, except that instead of using a triacetyl cellulose film as the base layer, a hard-coated film was used on the surface of a 1 / 4 wavelength plate (ZEONORFILM, Zeon Corporation, in-plane retardation value Ro: 138 nm), which is a uniaxially stretched film of a cyclic olefin resin, and laminated so that the slow axis and the absorption axis of the polarizing layer are 45°. In addition, an evaluation sample was prepared according to the above procedure, and its luminous efficiency-corrected transmittance (Ty) and luminous efficiency-corrected polarization degree (Py) were calculated. The results are shown in Table 1.

[0188] Example 3 A polarizing film was obtained in the same manner as in Example 1, except that instead of laminating a protective layer in which an opening was formed by making a hole with a hole punch, a 50 wt% solution of diphenyl 4-thiophenoxyphenylsulfonium hexafluorophosphate (manufactured by San-Apro Co., Ltd., CPI-100P) in propylene carbonate was dropped partially onto the polarizing layer using a dropper. In addition, an evaluation sample was prepared using the above-mentioned procedure, and its luminous efficiency-corrected transmittance (Ty) and luminous efficiency-corrected polarization degree (Py) were calculated. The results are shown in Table 1.

[0189] Comparative Example A polarizing film was obtained in the same manner as in Example 1, except that methanol was used at room temperature instead of a 50 wt% solution of diphenyl 4-thiophenoxyphenylsulfonium hexafluorophosphate (manufactured by San-Apro Co., Ltd., CPI-100P) in propylene carbonate. When the appearance of the obtained polarizing film was visually observed, no area without a polarizing layer was confirmed, and it was found that a polarizing film having a polarizing area and a low polarization area was not obtained. In addition, an evaluation sample was prepared according to the above procedure, and its luminous efficiency-corrected transmittance (Ty) and luminous efficiency-corrected polarization degree (Py) were calculated. The results are shown in Table 1.

[0190] [Reference example] A polarizing film was obtained in the same manner as in Example 1, except that a 50 wt% solution of diphenyl 4-thiophenoxyphenylsulfonium hexafluorophosphate (manufactured by San-Apro Co., Ltd., CPI-100P) in propylene carbonate was not used. When the appearance of the obtained polarizing film was visually observed, no area in which a polarizing layer was absent could be confirmed, and it was found that a polarizing film having a polarizing area and a low polarization area was not obtained. In addition, an evaluation sample was prepared according to the above procedure, and its luminous efficiency-corrected transmittance (Ty) and luminous efficiency-corrected polarization degree (Py) were calculated. The results are shown in Table 1.

[0191] In addition, the values ​​of the luminous-corrected transmittance (Ty) and luminous-corrected polarization degree (Py) measured in each of the examples, comparative examples, and reference examples shown in Table 1 include the values ​​of the luminous-corrected transmittance (Ty) and luminous-corrected polarization degree (Py) of the base material layer. However, since the luminous-corrected transmittance (Ty) of the base material layer alone is 92%, and the luminous-corrected polarization degree (Py) of the base material layer is 0%, it is considered that if the base material layer is excluded from each of the examples, comparative examples, and reference examples shown in Table 1, the luminous-corrected transmittance (Ty) value will be larger than the value shown in Table 1, and the luminous-corrected polarization degree (Py) value will be the same as the value shown in Table 1.

[0192] [Table 1] [Explanation of symbols]

[0193] 1 polarizing film, 5a to 5c circular polarizing plates, 11 liquid crystal layer, 11a first region, 11b second region, 12 alignment layer, 13 base layer, 15 retardation layer, 21 polarizing layer, 35 protective layer, 35a covered region, 35b exposed region, 61 base layer with alignment layer, 62 laminate film, 63 laminate film with protective layer, 64 bleached laminate film.

Claims

1. A laminated film with a protective layer, the laminated film having a base layer, a liquid crystal layer laminated on at least one side of the base layer, and a protective layer peelably laminated on the liquid crystal layer, The liquid crystal layer is Including a liquid crystal compound, The optical element has at least two regions that are distinguished by the value of the luminosity-corrected polarization degree and have different contents of a dichroic dye, the first region containing a dichroic dye and the second region having a lower content of the dichroic dye than the first region, in the same plane; the liquid crystal compound is a thermotropic liquid crystal, The difference between the thickness of the first region and the thickness of the second region is 0.5 μm or less; The protective layer has a covering region for covering the first region and an exposing region for exposing the second region.

2. The laminated film with the protective layer further has an orientation layer laminated on at least one side of the base layer, The laminate film with a protective layer according to claim 1 , wherein the liquid crystal layer is laminated on the alignment layer.

3. The laminated film with a protective layer according to claim 2 , wherein the orientation layer comprises a photo-orientable polymer.

4. The laminate film with a protective layer according to any one of claims 1 to 3, wherein the base layer has a quarter wave plate function.

5. 5. The laminate film with a protective layer according to claim 1, wherein the liquid crystal compound contains a polymer of a polymerizable liquid crystal compound.

6. The luminosity-corrected polarization degree of the first region is 90% or more, 6. The laminate film with a protective layer according to claim 1, wherein the luminous efficiency corrected polarization degree of the second region is 10% or less.

7. The luminosity-corrected single transmittance of the first region is 35% or more; The laminate film with a protective layer according to any one of claims 1 to 6, wherein the luminous efficiency-corrected single transmittance of the second region is 80% or more.

8. The second region has a circular, elliptical, oval, or polygonal shape in a plan view, When the second region is circular, the diameter of the second region is 5 cm or less; When the second region is elliptical or oval, the major axis of the second region is 5 cm or less; The laminate film with a protective layer according to any one of claims 1 to 7, wherein when the second region is a polygon, a diameter of an imaginary circle drawn to inscribe the polygon is 5 cm or less.

9. The laminate film with a protective layer according to any one of claims 1 to 8, wherein the first region exhibits a Bragg peak in X-ray diffraction measurement.

Citation Information

Patent Citations

  • Security product, article with security information, forgery discrimination method, and method for manufacturing security product

    JP2001256531A

  • Viewing angle control element and image display device using same

    JP2005221756A

  • Dichroic dye for polarizing film, polarizing film composition containing the same, method for producing highly durable polarizing plate using the same, and polarizing plate produced by the same

    JP2009538957A

  • Light absorption anisotropic film, production method thereof, and liquid crystal display device using the same

    JP2011237513A

  • Optical laminate and manufacturing method of optical laminate

    JP2013167835A