Fuel composition and method for producing same
A fuel composition with controlled properties minimizes sediment formation at high temperatures, addressing storage instability and filter clogging issues in marine fuels.
Patent Information
- Application Number
- JP2020136678
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-13
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-08-13
AI Technical Summary
Existing marine fuel oils face issues with sediment formation, particularly at high temperatures, leading to filter clogging and storage instability, which are not adequately addressed by current methods.
A fuel composition is formulated using specific base materials with controlled sulfur content, kinematic viscosity, and aromatic content, adhering to a predictive formula to minimize sediment formation even at elevated temperatures.
The composition exhibits excellent storage stability, significantly reducing sediment formation even after long-term storage at high temperatures, ensuring engine safety and efficiency.
Smart Images

Figure 0007586667000001 
Figure 0007586667000002 
Figure 0007586667000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a fuel composition and a method for producing the same. [Background technology]
[0002] Marine fuel oil has traditionally been produced from residual oil obtained at oil refineries. For example, fuel oil with adjusted kinetic viscosity and sulfur content is produced by mixing diesel fractions and cracked diesel with a base material mainly consisting of residual oil from a vacuum distillation unit, desulfurized residual oil, and cracked residual oil from a fluid catalytic cracking (FCC) unit (for example, see Patent Document 1 below).
[0003] In recent years, regulations on NOx, SOx and PM emissions from ships have led to the trend toward lowering the sulfur content of marine fuel oil, and from 2020 onwards, low-sulfur fuel oil for general marine use will be required to have a sulfur content of 0.50 mass% or less.
[0004] In addition, the kinetic viscosity of marine fuel oil at 50°C is set at 20mm 2 This is because the kinetic viscosity at the engine inlet is set at 2mm / s, which is the minimum kinetic viscosity set by major engine manufacturers. 2 It is set so that it will not fall below / s. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2020-2339 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, heavy base materials such as residual oil are prone to sedimentation, and if the amount of sediment in fuel oil increases, problems such as clogging of fuel oil filters may occur. In addition, the environment in which fuel oil is stored may be at a temperature higher than room temperature, and fuel oil is required to be less susceptible to sedimentation even in such an environment.
[0007] An object of the present invention is to provide a fuel composition having excellent storage stability and which is less likely to produce sediment even when stored at high temperatures, and a method for producing the same. [Means for solving the problem]
[0008] In order to solve the above problems, the present inventors have conducted extensive research and found that, although Patent Document 1 discloses that the latent sediment in a heavy oil composition is adjusted to a predetermined value or less, even if the latent sediment immediately after production is small, the amount of sediment after long-term storage may not necessarily be sufficiently suppressed. Therefore, the present inventors have devised a calculation formula for predicting the actual sediment of a fuel composition after storage at 60°C for four months from specific properties of the fuel composition by performing a storage stability test at 60°C for four months on a fuel oil composition in which a specific heavy base stock and another specific base stock are blended to adjust the sulfur content and kinematic viscosity. Then, the present inventors have completed the present invention based on this calculation formula.
[0009] That is, one aspect of the present invention is a fuel composition comprising a base material A which is a directly desulfurized heavy oil, and at least one base material B selected from the group consisting of hydrocracked heavy oil, hydrocracked light oil, hydrocracked kerosene, directly desulfurized light oil, hydrodesulfurized light oil, catalytic cracked light oil, thermal cracked light oil, straight run light oil, catalytic cracked kerosene, and straight run kerosene, The sulfur content is 0.5% by mass or less, Kinematic viscosity at 50℃ is 20mm 2 / s or more, The present invention provides a fuel composition, in which the total aromatic content a (volume %) of the fuel composition satisfies the following formula (1): a×(-0.1007s 2+0.065s-0.0107)+(1.2324s 2 -0.6297s+0.4204)≦0.19 …(1) [In formula (1), s represents the potential sediment (mass%) of directly desulfurized heavy oil]
[0010] By satisfying the above-mentioned constitution, the above-mentioned fuel composition can be one that is less likely to generate sediment even when stored at high temperatures, even though it contains a heavy base material. For example, even when stored at 60°C for a long period of four months, the amount of sediment can be sufficiently reduced.
[0011] Directly desulfurized heavy oil has a latent sediment content of 0.20% by mass or less and a kinematic viscosity of 20mm at 50°C. 2 / s or more and an aromatic content of 17.3 to 35.5 mass %, and base material B may have a sulfur content of 0.78 mass % or less.
[0012] Another aspect of the present invention provides a method for producing a fuel composition. The method for producing the fuel composition includes mixing a base material A which is a directly desulfurized heavy oil, and at least one base material B selected from the group consisting of hydrocracked heavy oil, hydrocracked light oil, hydrocracked kerosene, directly desulfurized light oil, hydrocracked light oil, catalytically cracked light oil, thermally cracked light oil, straight-run light oil, catalytically cracked kerosene, and straight-run kerosene, so that the total aromatic content a (volume %) of the fuel composition satisfies the following formula (1), the sulfur content of the fuel composition is 0.5 mass% or less, and the kinetic viscosity of the fuel composition at 50°C is 20 mm 2 Mix so that the ratio is / s or higher. a×(-0.1007s 2 +0.065s-0.0107)+(1.2324s 2 -0.6297s+0.4204)≦0.19 …(1) [In formula (1), s represents the potential sediment (mass%) of directly desulfurized heavy oil.]
[0013] According to the above-mentioned method for producing a fuel composition, it is possible to produce a fuel composition that is excellent in storage stability and is less likely to produce sediment even when stored at high temperatures.
[0014] In the above-mentioned method for producing a fuel composition, the directly desulfurized heavy oil has a latent sediment content of 0.20 mass% or less and a kinematic viscosity at 50°C of 20 mm 2 / s or more and an aromatic content of 17.3 to 35.5 mass %, and base material B may have a sulfur content of 0.78 mass % or less. Effect of the Invention
[0015] According to the present invention, it is possible to provide a fuel composition having excellent storage stability in which sedimentation is unlikely to occur even when stored at high temperatures (in particular, having long-term storage stability in which the amount of sedimentation is sufficiently suppressed even after the lapse of four months), and a method for producing the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferred embodiments of the present invention will now be described in detail.
[0017] <Fuel composition> The fuel composition of the present embodiment includes a base material A which is a direct desulfurized heavy oil, and at least one base material B selected from the group consisting of hydrocracked heavy oil, hydrocracked light oil, hydrocracked kerosene, direct desulfurized light oil, hydrodesulfurized light oil, catalytically cracked light oil, thermally cracked light oil, straight-run light oil, catalytically cracked kerosene, and straight-run kerosene.
[0018] Directly desulfurized heavy oil is a heavy fraction obtained by desulfurizing atmospheric or vacuum residual oil. For example, desulfurized bottom oil obtained from a Residue Hydrodesulfurizing plant (RDS) can be used.
[0019] From the viewpoint of making it easier for the composition to meet the sulfur content regulation value, the directly desulfurized heavy oil may have a sulfur content of 0.6 mass % or less, 0.1 to 0.55 mass %, or 0.15 to 0.55 mass %.
[0020] In this specification, the sulfur content refers to a value measured in accordance with JIS K2541-4 "Crude petroleum and petroleum products-Determination of sulfur content, Part 4: Radioisotope excitation method."
[0021] From the viewpoint of easily ensuring long-term storage stability of up to 4 months, the directly desulfurized heavy oil may have a latent sediment content of 0.0 to 0.20 mass%, 0.0 to 0.17 mass%, or 0.0 to 0.12 mass%.
[0022] In this specification, potential sediment means the value measured in accordance with ISO 10307-2 (2009).
[0023] In order to ensure sufficient heating value, the density of directly desulfurized heavy oil at 15°C is set to 0.9001 to 0.9423 g / cm 3 0.9107 to 0.9391 g / cm 3 0.9213 to 0.9359 g / cm 3 may be also possible.
[0024] In this specification, density at 15°C refers to a value measured in accordance with JIS K 2249 "Crude petroleum and petroleum products - Density test method and density, mass and volume conversion table".
[0025] In order to easily secure a desirable kinetic viscosity as the final composition, the directly desulfurized heavy oil has a kinetic viscosity at 50°C of 20.0 to 874 mmHg. 2 / s, 30.0~874mm 2 / s, 33.6~874mm 2 / s may also be used.
[0026] In this specification, the kinematic viscosity at 50°C means a value measured in accordance with JIS K 2283 "Crude oil and petroleum products - Test method for kinematic viscosity and calculation method for viscosity index".
[0027] From the viewpoint of suppressing sediment formation and making it easier to ensure long-term storage stability, the directly desulfurized heavy oil may have an aromatic content of 17 to 40 mass%, 17.3 to 35.5 mass%, 20.0 to 35.0 mass%, or 23.0 to 32.0 mass%.
[0028] In this specification, the aromatic content of directly desulfurized heavy oil means a value measured in accordance with JPI-5S-22-83 "Composition analysis method of asphalt by column chromatography method".
[0029] The directly desulfurized heavy oil may have a CCAI of 780-810, 785-805, or 788-800, from the viewpoint of making it easier to ensure combustibility.
[0030] In this specification, CCAI means a value calculated by the following formula. CCAI=D-140.7log{log(V+0.85)}-80.6 where D is density (kg / m 3 @15℃), V is kinetic viscosity (mm 2 / s@50℃).
[0031] The directly desulfurized heavy oil may be used alone or in combination of two or more. When the base material A is made of two or more directly desulfurized heavy oils, it is sufficient that the base material A has the above-mentioned properties.
[0032] From the viewpoint of making it easier to ensure the required kinetic viscosity of the final composition, the content of base material A in the fuel composition may be 50 to 99% by volume, 55 to 95% by volume, or 55 to 90% by volume based on the total amount of the fuel composition.
[0033] Next, the base material B will be described.
[0034] Hydrocracked heavy oil is a heavy oil fraction obtained by supplying vacuum gas oil obtained by vacuum distillation of atmospheric residual oil to a hydrocracker. For example, a hydrocracker can be used that can carry out a process in which heavy distillate oil is desulfurized in a desulfurization unit, and the heavy oil is decomposed into naphtha (gasoline), kerosene, and gas oil fractions using hydrogen under high temperature and pressure using a catalyst.
[0035] Hydrocracked gas oil is the gas oil fraction obtained in the above process.
[0036] Hydrocracked kerosene is the kerosene fraction obtained in the above process.
[0037] Directly desulfurized diesel fuel is a diesel fraction obtained by desulfurizing atmospheric residue or vacuum residue. For example, diesel fuel obtained from a direct desulfurization unit can be used.
[0038] Catalytically cracked diesel and catalytically cracked kerosene are middle distillates (kerosene fractions) obtained by selectively cracking desulfurized vacuum diesel and residual oil with a cracking catalyst. For example, middle distillates (kerosene fractions) obtained from FCC (Fluid Catalytic Cracking) units that produce gasoline, kerosene, diesel, etc. from heavy oil can be used.
[0039] Thermal cracking diesel is a diesel fraction obtained by cracking the residual oil of an atmospheric distillation unit or a vacuum distillation unit. For example, a diesel fraction obtained from a delayed coker, which is a unit for cracking residual oil, can be used. Delayed cokers include a system in which residual oil is rapidly heated in a heating furnace coil, subjected to a liquid-phase thermal cracking reaction in a batch drum, and a distillate oil is produced, which is then desulfurized to reduce sulfur.
[0040] Straight-run diesel and straight-run kerosene are middle distillates (kerosene fractions) obtained by distillation separation of crude oil.
[0041] From the viewpoint of making it easier for the composition to satisfy the sulfur content regulation value, the base material B may have a sulfur content of 1.5 mass% or less, 0.78 mass% or less, 0.0 to 0.5 mass%, or 0.0 to 0.38 mass%.
[0042] In order to ensure sufficient heat generation, the density of the base material B at 15°C is set to 0.8279 to 0.9500 g / cm 3 0.8300 to 0.9500 g / cm 30.8700 to 0.9500 g / cm 3 may be also possible.
[0043] Base material B has a kinetic viscosity at 50°C of 1.640 to 35.70 mmHg, from the viewpoint of making it easier for the final fuel composition obtained by mixing with base material A to satisfy the required kinetic viscosity range. 2 / s, 1.65 to 31.00 mm 2 / s, 1.650~27.77mm 2 / s may also be used.
[0044] The aromatic content of the base material B may be 9.0 to 85.0% by volume, 10.0 to 82.0% by volume, or 10.0 to 79.0% by volume.
[0045] In this specification, the aromatic content of the base material B means the value measured by JPI-5S-49 "Petroleum products - Hydrocarbon type test method - High performance liquid chromatography method. However, hydrocracked heavy oil is measured according to JPI-5S-22-83 "Asphalt composition analysis method by column chromatography method". When the base material B contains hydrocracked heavy oil with aromatic content Ar1 (mass%), the aromatic content (volume%) of the base material B is calculated by approximating Ar1 (mass%) = Ar1 (volume%).
[0046] The base material B may have a CCAI of 775-903, 780-845, or 789-845 from the viewpoint of combustibility.
[0047] From the viewpoint of making it easier for the final fuel composition obtained by mixing base material B with base material A to satisfy the required kinematic viscosity range, the content of base material B in the fuel composition may be 1.0 to 50.0% by volume, 5.0 to 45.0% by volume, or 10.0 to 45.0% by volume based on the total amount of the fuel composition.
[0048] The total content of base material A and base material B in the fuel composition may be 80% by volume or more, or may be 100% by volume, based on the total amount of the fuel composition.
[0049] In order to satisfy the sulfur content regulations for fuel compositions, the fuel composition of this embodiment has a sulfur content of 0.5 mass % or less, or may be 0.49 mass % or less, or may be 0.48 mass % or less.
[0050] In order to avoid damage to the engine, the fuel composition of the present embodiment has a kinetic viscosity of 20 mm at 50°C. 2 / s or more, 20.0 to 250.0 mm 2 / s, 20.0 to 216.0 mm 2 / s may also be used.
[0051] Incidentally, conventional marine fuel oils produced mainly from residual oils have been heated to about 120°C before use, but some coastal ships are unable to control the heating temperature to 120°C or lower. The fuel composition of the present embodiment has the above-mentioned kinetic viscosity, and therefore, even in such ships, it is possible to maintain a kinetic viscosity of 2mm even when heated to a temperature of 120°C or higher, as in the past. 2 / s or higher, thus avoiding damage to the engine.
[0052] In the fuel composition of the present embodiment, the total aromatic content a (vol %) of the fuel composition can satisfy the following formula (1). a×(-0.1007s 2 +0.065s-0.0107)+(1.2324s 2 -0.6297s+0.4204)≦0.19 …(1) [In formula (1), s represents the potential sediment (mass%) of directly desulfurized heavy oil]
[0053] The total aromatic content a (volume %) of a fuel composition containing directly desulfurized heavy oil with aromatic content Ar (mass %) is calculated by approximating Ar (mass %) = Ar (volume %). When the fuel composition contains hydrocracked heavy oil, the total aromatic content a (volume %) of the fuel composition is calculated in the same manner.
[0054] In this embodiment, the storage stability index Y calculated from the following formulas (A) to (C) may be 0.19 or less, may be 0.00 to 0.18, or may be 0.0 to 0.17. Y = B(s) a + C(s) …(A) B(s)=-0.1007s 2 +0.065s-0.0107 …(B) C(s)=1.2324s 2 -0.6297s+0.4204 …(C) In the above formula, a represents the total aromatic content (volume %) of the fuel composition, and s represents the latent sediment content (mass %) of the directly desulfurized heavy oil.
[0055] Furthermore, from the viewpoint of suppressing sediment formation and making it easier to ensure long-term storage stability, the fuel composition of this embodiment may have a total aromatic content of 21.5 to 70% by volume, 22.0 to 50.0% by volume, or 23.1 to 41.6% by volume.
[0056] The fuel composition of the present embodiment may have a CCAI of 771-836, 784-832, or 796-827 from the viewpoint of combustibility.
[0057] The fuel composition of the present embodiment can be used as a fuel oil for internal combustion engines for ships and the like, and as a fuel oil for boilers in the electric power, chemical, and pulp and paper industries, etc.
[0058] In addition, the fuel composition of this embodiment can be used as a heavy oil composition equivalent to C heavy oil.
[0059] <Method of producing fuel composition> The method for producing a fuel composition of the present embodiment includes mixing a base material A which is a directly desulfurized heavy oil and at least one base material B selected from the group consisting of hydrocracked heavy oil, hydrocracked light oil, hydrocracked kerosene, directly desulfurized light oil, hydrodesulfurized light oil, catalytically cracked light oil, thermally cracked light oil, straight-run light oil, catalytically cracked kerosene, and straight-run kerosene, and producing a fuel composition having a total aromatic content a (volume %) which satisfies the following formula (1), a sulfur content of the fuel composition is 0.5 mass% or less, and a kinetic viscosity of the fuel composition at 50°C is 20 mm 2 A process is included to mix the components so that the content is equal to or greater than 1 / s. a×(-0.1007s 2 +0.065s-0.0107)+(1.2324s 2 -0.6297s+0.4204)≦0.19 …(1) [In formula (1), s represents the potential sediment (mass%) of directly desulfurized heavy oil.]
[0060] The above process is Step S1 of measuring the latent sediment (mass%), aromatic content (mass%), sulfur content and kinematic viscosity at 50 ° C. of the base material A before blending; Step S2 of measuring the aromatic content (volume%), sulfur content, and kinematic viscosity at 50 ° C. of the base material B before blending; From the potential sediment s (mass%) obtained in step S1 and the above formula (1), the lower limit a of the total aromatic content a (volume%) of the fuel composition is determined. min Step S3 of calculating Based on the aromatic content (mass%), sulfur content, and kinetic viscosity at 50°C of the base material A obtained in step S1, and the aromatic content (volume%), sulfur content, and kinetic viscosity at 50°C of the base material B obtained in step S2, the sulfur content of the fuel composition is 0.5 mass% or less, the kinetic viscosity at 50°C is 20 mm 2 / s or more, and the total aromatic content a (volume %) is less than the lower limit a min Step S4: Setting the blending ratio of the base material A and the base material B so as to satisfy the above; may include.
[0061] The base material A and the base material B can be the same as the base material A and the base material B in the fuel composition described above.
[0062] In addition, in the above step S4, the blending ratio of the base material A and the base material B may be set so that the storage stability index Y calculated from the total aromatic content a (volume %) of the fuel composition and the latent sediment s (mass %) of the directly desulfurized heavy oil and the above formulas (A) to (C) is 0.19 or less, 0.00 to 0.18, or 0.00 to 0.17.
[0063] The total aromatic content a (volume %) satisfies the above formula (1), the sulfur content is 0.5 mass% or less, and the kinetic viscosity at 50 °C is 20 mm 2 From the viewpoint of efficiently producing a fuel composition having a viscosity of 100 / s or more, the base material A has a latent sediment content of 0.20 mass% or less and a kinematic viscosity at 50°C of 20.0 mm 2 / s or more, the aromatic content is 17.3 to 35.5 mass %, and the base material B has a sulfur content of 0.78 mass % or less. EXAMPLES
[0064] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0065] <Production of fuel oil composition> (Examples 1 to 13, Comparative Example 1) Fuel compositions were obtained by mixing the base materials shown in Tables 1 and 2 in the blending ratios (volume %) shown in Tables 3 and 4. The properties shown in Tables 1 to 4 were measured as follows.
[0066] Sediment potential: Measured according to ISO 10307-2(2009).
[0067] Sulfur content: Measured in accordance with JIS K2541-4 "Crude oil and petroleum products-Determination of sulfur content, Part 4: Radiation excitation method."
[0068] Density (15°C): Measured in accordance with JIS K 2249 "Crude oil and petroleum products - Density test method and density, mass and volume conversion table."
[0069] Kinematic viscosity (50°C): Measured in accordance with JIS K 2283 "Crude oil and petroleum products - Kinematic viscosity test method and viscosity index calculation method".
[0070] Aromatic content of base material: For directly desulfurized heavy oil and hydrocracked heavy oil, the aromatic content (mass%) was measured according to JPI-5S-22-83 "Composition analysis method of asphalt by column chromatography" and this value was used as volume %. For other base materials, the aromatic content (volume %) was measured using JPI-5S-49 "Petroleum products - Hydrocarbon type test method - High performance liquid chromatography method."
[0071] Total aromatic content a: A weighted average value based on the aromatic content of each base material obtained above and the blending ratio of each base material was calculated, and this was taken as the total aromatic content a.
[0072] CCAI: Calculated using the following formula. CCAI=D-140.7log{log(V+0.85)}-80.6 where D is density (kg / m 3 @15℃), V is kinetic viscosity (mm 2 / s@50℃).
[0073] For the resulting fuel compositions, the storage stability index Y calculated from the following formulas (A) to (C) is shown in the table. Y = B(s) a + C(s) …(A) B(s)=-0.1007s 2 +0.065s-0.0107 …(B) C(s)=1.2324s 2 -0.6297s+0.4204 …(C) In the above formula, a represents the total aromatic content (volume %) of the fuel composition, and s represents the latent sediment content (mass %) of the directly desulfurized heavy oil.
[0074] <Storage stability of fuel composition> The fuel compositions were stored at 60°C for 4 months, and the actual sediment content of the fuel compositions after storage was measured in accordance with ISO 10307-1 (2009).
[0075] [Table 1]
[0076] [Table 2]
[0077] [Table 3]
[0078] [Table 4]
[0079] The fuel compositions of Examples 1 to 13, which were formulated so as to have a storage stability index Y of 0.19 or less, had actual sediment of 0.002 to 0.19 mass % after storage at 60°C for 4 months, demonstrating excellent storage stability.
[0080] In addition, in the fuel compositions of Examples 1 to 13, the actual sediment is equal to or less than the storage stability index Y, and according to the present invention, by producing a fuel oil composition in which the total aromatic content is adjusted according to the latent sediment of the directly desulfurized heavy oil, it becomes possible to predict and manage the storage stability of the resulting fuel composition. It is known that CCAI represents the aromaticity of a fuel oil. However, Comparative Example 1, which has a CCAI equivalent to that of Examples 3 and 7 but has a storage stability index Y of 0.232 calculated based on the latent sediment s and the total aromatic content a, has more actual sediment than Examples 3 and 7, and it can be said that the storage stability index Y according to the present invention is superior to CCAI in terms of management to suppress the generation of sediment.
Claims
1. Base material A is a directly desulfurized heavy oil; At least one base material B selected from the group consisting of hydrocracked heavy oil, hydrocracked light oil, hydrocracked kerosene, direct desulfurized light oil, hydrodesulfurized light oil, catalytic cracked light oil, thermal cracked light oil, straight run light oil, catalytic cracked kerosene, and straight run kerosene; A fuel composition comprising: The sulfur content is 0.5% by mass or less, Kinematic viscosity at 50°C is 20mm 2 / s or more, The total aromatic content a (vol %) of the fuel composition satisfies the following formula (1), A fuel composition having a storage stability index Y calculated from the following formulas (A) to (C) of 0.00 to 0.18: a×(-0.1007s 2 +0.065s-0.0107)+(1.2324s 2 -0.6297s+0.4204)≦0.19…(1) [In formula (1), s represents the potential sediment (mass%) of the directly desulfurized heavy oil.] Y=B(s)・a+C(s)...(A) B(s)=-0.1007s 2 +0.065s-0.0107...(B) C(s)=1.2324s 2 -0.6297s+0.4204...(C) [In the formulas (A) to (C), a represents the total aromatic content (volume %) of the fuel composition, and s represents the latent sediment (mass %) of the directly desulfurized heavy oil.]
2. The directly desulfurized heavy oil has a latent sediment content of 0.20 mass% or less and a kinematic viscosity at 50°C of 20.0 mm 2 / s or more, and the aromatic content is 17.3 to 35.5 mass%, 2. The fuel composition according to claim 1, wherein the base material B has a sulfur content of 0.78 mass% or less.
3. 1. A method for producing a fuel composition, comprising the steps of: A base material A which is a directly desulfurized heavy oil, and at least one base material B selected from the group consisting of hydrocracked heavy oil, hydrocracked light oil, hydrocracked kerosene, directly desulfurized light oil, hydrodesulfurized light oil, catalytic cracked light oil, thermal cracked light oil, straight run light oil, catalytic cracked kerosene, and straight run kerosene, The total aromatic content a (vol %) of the fuel composition satisfies the following formula (1), The storage stability index Y calculated from the following formulas (A) to (C) is 0.00 to 0.18, the sulfur content of the fuel composition is 0.5 mass% or less, and the kinematic viscosity of the fuel composition at 50°C is 20 mm 2 3. A method for producing a fuel composition comprising blending the fuel composition so that the content of each component is equal to or greater than 100% by mass. a×(-0.1007s 2 +0.065s-0.0107)+(1.2324s 2 -0.6297s+0.4204)≦0.19…(1) [In formula (1), s represents the potential sediment (mass%) of the directly desulfurized heavy oil.] Y=B(s)・a+C(s)...(A) B(s)=-0.1007s 2 +0.065s-0.0107...(B) C(s)=1.2324s 2 -0.6297s+0.4204...(C) [In the formulas (A) to (C), a represents the total aromatic content (volume %) of the fuel composition, and s represents the latent sediment (mass %) of the directly desulfurized heavy oil.]
4. The directly desulfurized heavy oil has a latent sediment content of 0.20 mass% or less and a kinematic viscosity at 50°C of 20.0 mm 2 / s or more, and the aromatic content is 17.3 to 35.5 mass%, The method for producing a fuel composition according to claim 3 , wherein the base material B has a sulfur content of 0.78 mass % or less.
Citation Information
Patent Citations
Fuel oil composition and method for producing the same
JP2018165365A
Heavy oil composition and producing method for heavy oil composition
JP2019214696A
Heavy oil composition and manufacturing method of heavy oil composition
JP2020002339A
Heavy oil composition and production method of heavy oil composition