Manufacturing method of layered object
The method stabilizes weld bead formation by measuring height deviations and updating correction ratios, addressing the instability caused by local height variations in the base part, thereby ensuring consistent quality in layered object manufacturing.
Patent Information
- Application Number
- JP2021000993
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-01-06
AI Technical Summary
Existing feedback control methods struggle to correct processing conditions when there are local height deviations in the base part, particularly at the start and end portions of the bead, leading to unstable bead stacking during the manufacturing of layered objects.
A method involving a base measurement process to determine height differences, followed by a welding condition setting process and a correction ratio update process to stabilize the formation of weld beads by selecting appropriate correction ratios based on shape characteristics and planned movement positions of the torch.
Enables stable formation of weld beads by adjusting welding conditions in real-time, effectively correcting for various height deviations and ensuring consistent quality of the manufactured object.
Smart Images

Figure 0007586715000001 
Figure 0007586715000002 
Figure 0007586715000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a layered object. [Background technology]
[0002] In recent years, there has been an increasing need for 3D printers as a means of production, and research and development is being conducted for practical use in the aircraft industry, etc., particularly in the case of application to metallic materials. 3D printers that use metallic materials use a heat source such as a laser or arc to melt metal powder or metal wire, and then layer the molten metal to create a model.
[0003] As a technique for forming such objects by welding, Patent Document 1 discloses a technique in which the height of an already formed object is measured by a measuring unit, and the processing conditions when a new object is stacked at the measured position are feedback-controlled according to the measurement results. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6576593 Summary of the Invention [Problem to be solved by the invention]
[0005] Incidentally, in feedback control when stacking beads to form a model, if the height deviation of the base portion is locally larger than expected, normal feedback control may not be able to correct the processing conditions in time, making it difficult to stack the beads stably. For example, at the start and end portions of the bead, the height deviation of the lower bead tends to be large, making it difficult to deal with this with normal feedback control.
[0006] Therefore, an object of the present invention is to provide a method for manufacturing a layered object that is capable of always stably forming a weld bead and manufacturing a good object by appropriately performing feedback control. [Means for solving the problem]
[0007] The present invention comprises the following configurations. A method for manufacturing a layered object, comprising the steps of: laminating a weld bead formed by melting and solidifying a filler material by a torch while moving the torch to form a model; a modeling process for moving the torch to layer the weld bead based on a layering plan that defines a shape of the weld bead obtained from a target shape of the object and a trajectory of the torch for forming the weld bead; In the molding process, a substrate measurement process for measuring a height of the substrate at a planned movement position of the torch when the weld bead is laminated by a shape sensor and acquiring a measured height; a welding condition setting process for determining a planned height of the substrate at the planned movement position of the torch from the lamination plan, determining a difference height by comparing the measured height obtained in the substrate measurement process with the planned height, and setting welding conditions in a feedback correction for reducing the difference height; a correction rate update process for selecting from a plurality of preset correction rates and updating the correction rate in the welding conditions based on the selected correction rate; Execute A method for manufacturing an additively manufactured object. Effect of the Invention
[0008] By appropriately performing feedback control, the present invention can always stably form a weld bead and manufacture a good object. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a schematic diagram illustrating the configuration of a manufacturing system for manufacturing a layered object by a manufacturing method according to an embodiment of the present invention. [Diagram 2] 1A and 1B are schematic side views showing a wall portion on which welding beads are laminated. [Diagram 3] FIG. 2 shows a forming process for forming a wall portion by stacking weld beads, where (A) to (E) are schematic side views of the wall portion. [Figure 4] 1 is a graph showing a correction rate under welding conditions. [Diagram 5] 1A and 1B are diagrams showing the shapes of weld beads, in which (A) is a schematic plan view of a weld bead having a bent portion, and (B) is a schematic plan view of a weld bead having an intersection portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. FIG. 1 is a schematic diagram illustrating the configuration of a manufacturing system 100 for manufacturing a layered object by a manufacturing method according to an embodiment of the present invention. The additive manufacturing system 100 of this configuration includes a welding robot 11, a robot controller 13, a filler metal supply unit 15, a welding power source 19, and a control unit 21.
[0011] The welding robot 11 is an articulated robot, and a torch 23 is supported on the tip shaft. The position and posture of the torch 23 can be set arbitrarily in three dimensions within the range of the degrees of freedom of the robot arm. The torch 23 holds the filler material (welding wire) M, which is continuously supplied from a filler material supply unit 15, in a state where it protrudes from the tip of the torch. The tip shaft of the welding robot 11 is provided with the torch 23 and a shape sensor 25.
[0012] The torch 23 has a shield nozzle (not shown) through which a shielding gas is supplied to the welded portion. The arc welding method may be either a consumable electrode type such as shielded metal arc welding or carbon dioxide gas arc welding, or a non-consumable electrode type such as TIG welding or plasma arc welding, and is appropriately selected depending on the additive manufacturing object to be produced.
[0013] For example, in the case of a consumable electrode type, a contact tip is disposed inside the shield nozzle, and a filler material M to which a melting current is supplied is held by the contact tip. The torch 23 holds the filler material M and generates an arc from the tip of the filler material M in a shielding gas atmosphere. The filler material M is fed to the torch 23 by a feeding mechanism (not shown) attached to a robot arm or the like. Then, as the torch 23 moves, the continuously fed filler material M is melted and solidified, and a weld bead 29, which is a molten and solidified body of the filler material M, is formed on the base plate 27.
[0014] The base plate 27 is made of a metal plate such as a steel plate, and is basically larger than the bottom surface (the surface of the lowest layer) of the layered object W. The base plate 27 is not limited to a plate shape, and may be a base of other shapes such as a block or rod shape.
[0015] The heat source for melting the filler material M is not limited to the above-mentioned arc. For example, other types of heat sources may be used, such as a heating method using both an arc and a laser, a heating method using plasma, or a heating method using an electron beam or a laser. When heating with an electron beam or a laser, the amount of heat can be controlled more precisely, and the state of the weld bead can be more appropriately maintained, which contributes to further improving the quality of the additive manufacturing product.
[0016] Any commercially available welding wire can be used as the filler metal M. For example, wires specified in MAG and MIG welding solid wires for mild steel, high tensile steel and low temperature steel (JIS Z 3312), arc welding flux-cored wires for mild steel, high tensile steel and low temperature steel (JIS Z 3313), etc. can be used.
[0017] An active metal such as titanium can be used as the filler metal M. In that case, it is necessary to place the weld in a shielding gas atmosphere to prevent oxidation and nitridation due to reaction with the atmosphere during welding.
[0018] The shape sensor 25 is provided in parallel with the torch 23 and moves together with the torch 23. This shape sensor 25 is a sensor that measures the shape of a portion that will be a base when forming the weld bead B. As the shape sensor 25, for example, a laser sensor that acquires reflected light of an irradiated laser beam as height data is used. Note that as the shape sensor 25, a camera for three-dimensional shape measurement may also be used.
[0019] The robot controller 13 receives instructions from the control unit 21 to drive each part of the welding robot 11 and controls the output of the welding power source 19 as necessary.
[0020] The control unit 21 is configured with a computer device equipped with a CPU, memory, storage, etc., and executes a drive program prepared in advance or a drive program created under desired conditions to drive each part such as the welding robot 11. This causes the torch 23 to move in accordance with the drive program, and multiple layers of weld beads 29 are stacked on a base plate 27 based on the created stacking plan, thereby forming a multi-layered laminated object W. A database 17 is also connected to the control unit 21. This database 17 stores in advance data on multiple correction ratios under welding conditions at the time of feedback correction.
[0021] Next, a case where the layered object W is manufactured by the manufacturing system 100 will be described. Fig. 2 is a schematic side view of a layered object formed by laminating linear weld beads 29 on a base plate 27 to form a wall portion Wo. Fig. 3 is a process diagram showing a forming process of forming the wall portion Wo by laminating the weld beads 29.
[0022] As shown in Fig. 2A, when forming this wall portion Wo, one end (the left end in Fig. 2A) is set as the starting end, and torch 23 is moved from this starting end to start forming a weld bead 29, and torch 23 is then moved to the other end (the right end in Fig. 2A) to finish forming the weld bead 29. Then, the formation of this linear weld bead 29 is repeated to form wall portion Wo in which a plurality of linear weld beads 29 are layered. At this time, control unit 21 measures the shape of the base using shape sensor 25 arranged alongside torch 23, and performs feedback correction to correct the welding conditions based on the measurement results.
[0023] Incidentally, as shown in Fig. 2B, when the torch 23 is moved from the starting end to the ending end to form the weld bead 29, the formation of the weld bead 29 by the torch 23 is stable in the intermediate portion between the starting end and the ending end of the weld bead 29. Therefore, in the intermediate region Am, it is possible to form a shape with few irregularities that conforms to the target shape based on the lamination plan. As a result, in the intermediate region Am where it is possible to form the weld bead to a stable thickness, it is possible to handle it with normal feedback correction.
[0024] In contrast, in the starting region As and the terminal region Ae, the thickness of the weld bead 29 formed tends to be unstable. Specifically, in the starting region As, the weld bead 29 tends to become thicker and bulge, while in the terminal region Ae, the weld bead 29 tends to become thinner and sag. Therefore, in the starting region As and the terminal region Ae, where the thickness is unstable, normal feedback correction may not be able to correct in time.
[0025] In this case, in order to accommodate the starting region As and the ending region Ae, the correction rate of the welding conditions in the feedback correction can be increased; however, in the intermediate region Am where the weld bead 29 can be stably formed, abrupt correction would result in larger unevenness.
[0026] For this reason, in the manufacturing method according to this embodiment, the following feedback correction is performed in the manufacturing process in which the weld beads 29 are layered.
[0027] (Substrate measurement processing) The height of the base at the planned movement position of the torch 23 when depositing the weld bead 29 is measured by the shape sensor 25. Then, the measured height Hr, which is the height of the base measured by this shape sensor 25, is obtained.
[0028] (Welding condition setting process) The planned height Hp of the base at the planned movement position of the torch 23 is obtained from the lamination plan, and the measured height Hr obtained in the base measurement process is compared with the planned height Hp to obtain the differential height ΔH (ΔH = Hr - Hp), and the welding conditions are set so as to reduce the differential height ΔH.
[0029] (Correction rate update process) A correction ratio is selected from a plurality of correction ratios set in advance according to the shape characteristics of the planned movement position of the torch 23. The plurality of correction ratios are determined in advance, for example, by experiments or the like, in order to stably form the weld bead 29 for various shape characteristics, and are stored in the database 17. Then, based on the selected correction ratio, the correction ratio in the welding conditions (for example, the ratio of increase / decrease in the welding speed with respect to the differential height ΔH) is updated. For example, in a portion where the thickness is unstable, such as the start end region As or the end end region Ae when forming the wall portion Wo, a correction ratio corresponding to the shape characteristics of these portions is selected and retrieved from the database 17, and the correction ratio in the welding conditions is updated to the selected correction ratio. In addition, in this correction ratio update process, if the planned movement position of the torch 23 has shape characteristics that do not require the correction ratio of the welding conditions to be updated, the correction ratio is not selected, and the correction ratio in the welding conditions set in the welding condition setting process is maintained. For example, in a portion where the thickness is stable, such as the middle region Am when forming the wall portion Wo, the correction ratio in the welding conditions set in the welding condition setting process is maintained.
[0030] Next, an example of feedback correction in the molding process when molding the wall portion Wo will be described. Fig. 4 is a graph showing the correction ratio in the welding conditions. Fig. 5 is a schematic plan view showing the shape of a weld bead 29.
[0031] (Starting area As) 3A, the shape sensor 25 arranged next to the torch 23 is placed at the starting portion of the base U of the formed body WA on which a weld bead 29 has already been deposited, and the shape sensor 25 and the torch 23 are moved along the formed body WA. Then, the height of the starting region As of the base U of the formed body WA is measured by the shape sensor 25, and the measured height Hr is obtained (base measurement process).
[0032] The control unit 21 obtains the planned height Hp of the base U from the lamination plan, and compares the planned height Hp with the measured height Hr acquired by the shape sensor 25. Then, the control unit 21 obtains a differential height ΔH (ΔH=Hr−Hp) between the measured height Hr and the planned height Hp, and sets the welding conditions so as to reduce the differential height ΔH (welding condition setting process).
[0033] Here, FIG. 4 shows the correction rate between the differential height ΔH and the welding speed in feedback correction, and the control unit 21 sets, for example, the welding conditions for the correction rate Fa (solid line in FIG. 4) during normal feedback correction.
[0034] Next, the control unit 21 performs a correction rate update process to update the correction rate in the welding conditions. Specifically, since the start end region As is an area with shape characteristics with a large amount of change in height, a correction rate Fb (dotted line in FIG. 4) corresponding to the shape characteristics of the start end region As is selected from a plurality of correction rates set for each shape characteristic stored in the database 17. Then, the correction rate Fa in the welding conditions is updated to the selected correction rate Fb. This correction rate Fb is a rate of change in the welding speed with respect to the differential height ΔH that is larger than the correction rate Fa, and by updating to this correction rate Fb, it becomes possible to quickly change the welding speed with respect to the differential height ΔH in the feedback correction.
[0035] 3B, the shape sensor 25 and the torch 23 are moved along the formed body WA toward the terminal end side, and the torch 23 deposits a weld bead 29 on the starting end region As of the base U. At this time, feedback correction is performed using a correction ratio Fb that can quickly change the welding speed in response to the differential height ΔH. Therefore, the height of the weld bead 29 formed by the torch 23 can be quickly corrected in response to a large shape change of the differential height ΔH.
[0036] (middle area Am) When the torch 23 is forming the weld bead 29 in the starting end region As, the shape sensor 25 juxtaposed to the torch 23 continues to measure the height of the intermediate region Am of the base U (base measurement process). Then, the measured height Hr is compared with the planned height Hp to obtain a differential height ΔH (ΔH=Hr-Hp), and the welding conditions are set to, for example, a correction rate Fa (solid line in FIG. 4) during normal feedback correction so as to reduce the differential height ΔH (welding condition setting process).
[0037] Next, control unit 21 performs a correction ratio update process to update the correction ratio in the welding conditions. Here, since intermediate region Am is a region with stable shape characteristics in which the amount of change in height is relatively small, control unit 21 does not select a correction ratio from database 17 in the correction ratio update process, but maintains the correction ratio Fa (solid line in FIG. 4) in the welding conditions set in the welding condition setting process.
[0038] 3C, the shape sensor 25 and the torch 23 are moved along the formed body WA toward the terminal end, and the torch 23 deposits a weld bead 29 in the intermediate region Am of the base U. At this time, feedback correction is performed using a correction ratio Fa that changes the welding speed gradually with respect to the differential height ΔH. Therefore, the height of the weld bead 29 formed by the torch 23 can be smoothly corrected in response to a small change in shape of the differential height ΔH.
[0039] (Terminal area Ae) 3D, when the shape sensor 25 reaches the terminal region Ae in the base U of the shaped body WA, the shape sensor 25 measures the height of the terminal region Ae and obtains the measured height Hr (base measurement process). Then, the measured height Hr is compared with the planned height Hp of the base U from the lamination plan to obtain the differential height ΔH (ΔH=Hr-Hp), and the welding conditions are set to a correction ratio Fa (solid line in FIG. 4) so as to reduce the differential height ΔH (welding condition setting process).
[0040] Next, the control unit 21 performs a correction ratio update process to update the correction ratio in the welding conditions. Specifically, since the terminal area Ae is an area with shape characteristics with a large amount of change in height, the control unit 21 selects a correction ratio Fb (dotted line in FIG. 4) corresponding to the shape characteristics of the terminal area Ae from a plurality of correction ratios set for each shape characteristic stored in the database 17, and updates the correction ratio Fa in the welding conditions to the selected correction ratio Fb. Here, the correction ratio corresponding to the shape characteristics of the terminal area Ae is set to the correction ratio Fb corresponding to the shape characteristics of the starting area As. The correction ratios corresponding to the shape characteristics of the starting area As and the terminal area Ae may be different from each other.
[0041] As shown in Fig. 3(E) , the torch 23 that has reached the terminal end area Ae deposits a weld bead 29 in the terminal end area Ae. At this time, feedback correction is performed using a correction rate Fb that can quickly change the welding speed in response to the differential height ΔH. Therefore, the height of the weld bead 29 formed by the torch 23 can be quickly corrected in response to a large shape change in the differential height ΔH.
[0042] As described above, according to the manufacturing method of the additive manufacturing object of this embodiment, the correction rate of the welding conditions in the feedback correction that reduces the height difference ΔH between the planned height Hp based on the lamination plan and the actually measured height Hr is updated to a correction rate selected from a plurality of correction rates that are set and prepared in advance. This makes it possible to stably form the weld bead 29 by performing feedback correction with a correction rate appropriately selected for various cases of height deviation.
[0043] For example, by setting the correction rate to be small at positions where there is an average and gradual height deviation and setting the correction rate to be large for localized and large height deviations, the weld bead 29 can be stably formed in an appropriate control mode according to the shape characteristics of the forming portion of the weld bead 29.
[0044] The correction ratio is not limited to being set in advance in multiple proportions corresponding to the shape characteristics. Multiple correction ratios may be set in advance in accordance with positions designated based on a stacking plan. Examples of the designated positions include positions that are prone to local fluctuations in the frame, the filling portion within the frame, the corners of the frame, and the overhanging portion.
[0045] For example, as shown in FIG. 5A, the lamination height of the weld bead 29 tends to vary locally at a bent portion 51 when the weld bead 29 is bent and laminated, and as shown in FIG. 5B, at an intersection 53 when the weld bead 29 is laminated and crossed. Therefore, these bent portions 51 and intersections 53 are designated as designated positions, and a correction ratio corresponding to the designated positions is set. Then, when the weld bead 29 is formed, at the designated positions consisting of the bent portions 51 and intersections 53, a correction ratio corresponding to the designated positions is selected, and the correction ratio in the welding conditions for feedback correction is updated to the selected correction ratio. This makes it possible to form the weld bead 29 while responding to sudden height variations at designated positions such as the bent portions 51 and intersections 53.
[0046] Also, a base profile may be obtained from the measurement result of the shape sensor 25 on the front side in the moving direction of the torch 23, and the shape characteristics of the planned moving position of the torch 23 may be obtained in real time from this base profile and a target profile obtained from the lamination plan. Then, in the correction ratio update process, a correction ratio corresponding to the shape characteristics obtained during the molding may be selected from a plurality of correction ratios set in advance, and the correction ratio in the welding conditions may be updated based on the selected correction ratio.
[0047] In this way, when forming the weld bead 29, the shape of the base can be sensed in real time, and the weld bead 29 can be stably formed in an appropriate control mode even in the case of unexpected large height deviations or localized unevenness.
[0048] In the above embodiment, the correction rate of the welding speed with respect to the differential height ΔH is used as a parameter in the feedback correction. However, the parameter of the correction rate with respect to the differential height ΔH is not limited to the welding speed, and may be the feed speed of the filler metal M or the heat input for generating an arc.
[0049] For example, when the feed speed of the filler metal M is used as a parameter, the height of the weld bead 29 can be increased by increasing the feed speed, and the height of the weld bead 29 can be decreased by decreasing the feed speed. When the heat input is used as a parameter, the height of the weld bead 29 can be decreased by increasing the heat input, and the height of the weld bead 29 can be increased by decreasing the heat input.
[0050] In the above embodiment, the case where shape sensor 25 is provided in parallel with torch 23 has been exemplified, but shape sensor 25 does not necessarily have to be provided in parallel with torch 23. For example, a robot that moves shape sensor 25 may be provided separately from welding robot 11, and this robot may be used to measure the shape of the base on the forward side in the movement direction of torch 23 that forms weld bead 29.
[0051] As such, the present invention is not limited to the above-described embodiments, and the present invention also contemplates mutual combinations of the various components of the embodiments, as well as modifications and applications by those skilled in the art based on the descriptions in the specification and well-known technologies, and these are included in the scope of protection sought.
[0052] As described above, the present specification discloses the following: (1) A method for manufacturing an additive manufacturing object, comprising the steps of: laminating a weld bead formed by melting and solidifying a filler metal by a torch while moving the torch to form an object; a modeling process for moving the torch to layer the weld bead based on a layering plan that defines a shape of the weld bead obtained from a target shape of the object and a trajectory of the torch for forming the weld bead; In the molding process, a substrate measurement process for measuring a height of the substrate at a planned movement position of the torch when the weld bead is laminated by a shape sensor and acquiring a measured height; a welding condition setting process for determining a planned height of the substrate at the planned movement position of the torch from the lamination plan, determining a difference height by comparing the measured height obtained in the substrate measurement process with the planned height, and setting welding conditions in a feedback correction for reducing the difference height; a correction rate update process for selecting from a plurality of preset correction rates and updating the correction rate in the welding conditions based on the selected correction rate; A manufacturing method for an additive manufacturing object, comprising: According to this method for manufacturing a layered object, the correction rate of the welding conditions in the feedback correction for reducing the height difference between the planned height based on the lamination plan and the actually measured height is updated to a correction rate selected from a plurality of correction rates that are set and prepared in advance. This makes it possible to stably form a weld bead by performing feedback correction with a correction rate appropriately selected for various cases of height deviation.
[0053] (2) The method for manufacturing an additively molded object described in (1), wherein the multiple correction ratios are set in accordance with shape characteristics of the location where the weld bead is to be laminated. According to this method for manufacturing an additive manufacturing object, for example, the correction rate is set small at positions where there is an average and gradual height deviation, and the correction rate is set large for localized and large height deviations, thereby making it possible to stably form a weld bead in an appropriate control mode according to the shape characteristics of the forming portion of the weld bead.
[0054] (3) The method for manufacturing an additively molded object according to (2), wherein the multiple correction ratios are set in advance according to shape characteristics at positions specified based on the stacking plan. According to this method for manufacturing a layered object, it is possible to stably form a weld bead in an appropriate control mode according to a position that can be known in advance based on a layering plan.
[0055] (4) In the method for manufacturing an additively molded object described in (2), the correction ratio update process determines a base profile from the measurement results of the shape sensor, determines shape characteristics of the planned movement position of the torch from the base profile and a target profile determined from the stacking plan, selects from a plurality of correction ratios set in advance according to the shape characteristics, and updates the correction ratio in the welding conditions based on the selected correction ratio. According to this method for manufacturing an additive manufacturing object, the shape characteristics of the planned movement position of the torch are calculated in real time from the base profile and the target profile, and a correction ratio is selected according to the shape characteristics. In other words, while sensing the base shape in real time, it is possible to stably form a weld bead in an appropriate control mode even for unexpected large height deviations or localized unevenness. [Explanation of symbols]
[0056] 23. Torch 29 Weld bead 25 Shape Sensor Fa,Fb correction ratio ΔH Differential height M filler metal U Base W Laminated Model
Claims
1. A method for manufacturing a layered object, comprising the steps of: laminating a weld bead formed by melting and solidifying a filler material by a torch while moving the torch to form a model; a modeling process for layering the weld bead by moving the torch from a starting point to a terminal point based on a layering plan that defines a shape of the weld bead obtained from a target shape of the object and a trajectory of the torch for forming the weld bead; In the molding process, a substrate measurement process for measuring a height of the substrate at a planned movement position of the torch when the weld bead is laminated by a shape sensor and acquiring a measured height; a welding condition setting process for determining a planned height of the substrate at the planned movement position of the torch from the lamination plan, determining a difference height by comparing the measured height obtained in the substrate measurement process with the planned height, and setting welding conditions in a feedback correction for reducing the difference height; a correction rate update process for selecting from a plurality of correction rates previously set corresponding to shape characteristics of a location where a weld bead is to be deposited, and updating the correction rate in the welding conditions based on the selected correction rate; In addition to carrying out the above, When the planned movement position of the torch is a start end region where the weld bead is to be laminated, a correction rate corresponding to the shape characteristic of the start end region is selected from a plurality of correction rates set for each of the shape characteristics in order to change the welding speed, and the welding conditions are updated; When the planned movement position of the torch is a terminal region where the weld bead is to be deposited, a correction rate corresponding to a shape characteristic of the terminal region is selected from the plurality of correction rates, and the welding conditions are updated; When the planned movement position of the torch is an intermediate region between the start end region and the end end region, the correction rate is not selected and the set welding conditions are maintained. A method for manufacturing an additively manufactured object.
2. At least one of a bent portion when the weld bead is bent and laminated and an intersection portion when the weld bead is crossed and laminated is set as a designated position as a planned movement position of a torch, and the correction ratio corresponding to the designated position is set in advance. The method for producing a layered object according to claim 1 .
3. The plurality of correction ratios are preset according to shape characteristics at positions designated based on the stacking plan. The method for producing a layered object according to claim 2 .
4. The correction rate update process obtains a base profile from the measurement result of the shape sensor, obtains a shape characteristic of a planned movement position of the torch from the base profile and a target profile obtained from the lamination plan, selects from a plurality of the correction rates set in advance according to the shape characteristic, and updates the correction rate in the welding conditions based on the selected correction rate. The method for producing a layered object according to claim 2 .
Citation Information
Patent Citations
Additive manufacturing equipment
JP6576593B1
JPP6765569B