Adhesion film forming material, pattern forming method, and adhesion film forming method

The adhesive film forming material with specific resin units and a thermal acid generator addresses the pattern collapse issue in semiconductor manufacturing by enhancing adhesion and etching resistance, enabling precise pattern transfer in multilayer resist processes.

JP7586797B2Active Publication Date: 2024-11-19SHIN ETSU CHEMICAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021153704
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-22
Publication Date
2024-11-19
Estimated Expiration
2041-09-22

AI Technical Summary

Technical Problem

The challenge in semiconductor manufacturing is the collapse of fine patterns during the dry etching process due to the decrease in photoresist film thickness and resolution performance, leading to inadequate pattern transfer and weak etching resistance, especially with the advent of advanced lithography techniques like ArF immersion lithography and EUV lithography.

Method used

An adhesive film forming material is developed, comprising a resin with specific structural units and a thermal acid generator, which forms an adhesive film between a silicon-containing intermediate film and a resist upper layer film, enhancing adhesion and suppressing pattern collapse.

Benefits of technology

The adhesive film material improves pattern transfer precision by preventing fine pattern collapse and adjusting pattern shape, exposure sensitivity, and etching resistance, suitable for multilayer resist processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586797000074
    Figure 0007586797000074
  • Figure 0007586797000075
    Figure 0007586797000075
  • Figure 0007586797000001
    Figure 0007586797000001
Patent Text Reader

Abstract

To provide: an adhesion film forming material with which an adhesion film having high adhesion property to a resist upper layer film, having an effect of suppressing fall-down of a fine pattern, and being capable of forming an excellent pattern shape can be imparted; a pattern forming method using the material; and a forming method of the adhesion film, in a fine patterning process by a multilayer resist method in a semiconductor device manufacturing process.SOLUTION: An adhesion film forming material is for an adhesion film formed between a silicon-containing intermediate film and a resist upper layer film and includes (A) a resin having, on a resin side chain terminal, a structural unit with two phenolic hydroxy groups and a (meth)acrylic structural unit with an epoxy group or an oxetane group on the side chain terminal, (B) a thermal acid generator, and (C) an organic solvent, wherein in the component (A), a mole fraction of the structural unit of the epoxy group or the oxetane group is 30% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesion film-forming material, a pattern forming method using the adhesion film-forming material, and a method for forming an adhesion film using the adhesion film-forming material. [Background technology]

[0002] As LSIs become more highly integrated and faster, pattern dimensions are becoming finer. Lithography technology has achieved the formation of fine patterns by shortening the wavelength of light sources and appropriately selecting resist compositions to match them, in line with this miniaturization. The core of this technology is a positive photoresist composition used in a single layer. This single-layer positive photoresist composition has a skeleton in the resist resin that is resistant to dry etching using chlorine- or fluorine-based gas plasma, and has a resist mechanism that dissolves the exposed parts, so that the exposed parts are dissolved to form a pattern, and the remaining resist pattern is used as an etching mask to dry etch the substrate to which the photoresist composition has been applied.

[0003] However, if the thickness of the photoresist film used is kept the same and the pattern width is made smaller, the resolution of the photoresist film decreases, and if the photoresist film is developed into a pattern using a developer, the aspect ratio becomes too large, resulting in pattern collapse. For this reason, the thickness of the photoresist film has been made thinner as the pattern becomes finer.

[0004] On the other hand, in the processing of the substrate to be processed, a method is used in which the substrate to be processed is processed by dry etching using a photoresist film on which a pattern is usually formed as an etching mask, but in reality, there is no dry etching method that can obtain complete etching selectivity between the photoresist film and the substrate to be processed, so that the photoresist film is also damaged during the processing of the substrate to be processed, and the photoresist film collapses during the processing of the substrate to be processed, making it impossible to accurately transfer the resist pattern to the substrate to be processed. Therefore, with the miniaturization of patterns, photoresist compositions have been required to have high dry etching resistance. In addition, as the exposure wavelength becomes shorter, the resin used in the photoresist composition is required to have low light absorption at the exposure wavelength, so that in response to the change to i-line, KrF, and ArF, novolac resins, polyhydroxystyrene, and resins with aliphatic polycyclic skeletons have been used. However, in reality, the etching speed under the above dry etching conditions has become fast, and recent photoresist compositions with high resolution tend to have weak etching resistance.

[0005] For this reason, it has become necessary to dry etch the substrate to be processed using a thinner photoresist film with a weaker etching resistance, and securing the materials and processes for this processing step has become an urgent need.

[0006] One method for solving such problems is the multi-layer resist method, in which an intermediate film having a different etching selectivity from the photoresist film (i.e., resist top layer film) is interposed between the resist top layer film and the substrate to be processed, and after a pattern is obtained in the resist top layer film, the pattern is transferred to the intermediate film by dry etching using the resist top layer film pattern as a dry etching mask, and the pattern is further transferred to the substrate to be processed by dry etching using the intermediate film as a dry etching mask.

[0007] One of the multilayer resist methods is a three-layer resist method that can be performed using a general resist composition used in a single-layer resist method. In this three-layer resist method, for example, an organic film made of novolac or the like is formed on a substrate to be processed as a resist underlayer film, a silicon-containing film is formed thereon as a silicon-containing resist intermediate film, and a normal organic photoresist film is formed thereon as a resist upper layer film. For dry etching with fluorine-based gas plasma, the organic resist upper layer film has a good etching selectivity to the silicon-containing resist intermediate film, so the resist upper layer film pattern is transferred to the silicon-containing resist intermediate film by using dry etching with fluorine-based gas plasma. Furthermore, for etching with oxygen gas or hydrogen gas, the silicon-containing resist intermediate film can have a good etching selectivity to the resist underlayer film, so the silicon-containing resist intermediate film pattern is transferred to the resist underlayer film by etching with oxygen gas or hydrogen gas. According to this method, even if a photoresist composition is used that is difficult to form a pattern with a sufficient film thickness for directly processing a substrate to be processed, or a photoresist composition that does not have sufficient dry etching resistance for processing a substrate, if a pattern can be transferred to a silicon-containing film (silicon-containing resist intermediate film), it is possible to obtain a pattern of an organic film (resist underlayer film) made of novolak or the like that has sufficient dry etching resistance for processing.

[0008] On the other hand, in recent years, the appearance of ArF immersion lithography, EUV lithography, etc. has made it possible to form finer patterns, but on the other hand, because the contact area between the ultra-fine pattern and the substrate is small, collapse is extremely likely to occur, and suppressing pattern collapse is a major issue. Recently, it is said that the interaction at the interface between the resist top layer film and the resist underlayer film in a fine pattern affects pattern collapse, and there is a need to improve the performance of the resist underlayer film.

[0009] In order to suppress pattern collapse, materials have been reported that improve adhesion to the resist upper layer film by using a resist underlayer film containing a polar functional group such as a lactone structure or a urea structure (Patent Documents 1 and 2). However, in the current situation where finer pattern formation is required, it cannot be said that these materials have sufficient pattern collapse suppression performance. Furthermore, a resist underlayer film that combines a resin containing a phenolic hydroxyl group and a compound having a vinyl ether group has been reported, but its thermosetting property is not sufficient (Patent Document 3). For the above reasons, a material with higher pattern collapse suppression performance and adhesion is required. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] International Publication No. 2003 / 017002 [Patent Document 2] International Publication No. 2018 / 143359 [Patent Document 3] Patent No. 5708938 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been made in consideration of the above circumstances, and has an object to provide an adhesion film forming material that provides an adhesion film that has high adhesion to an overlying resist film, has an effect of preventing a fine pattern from collapsing, and is capable of forming a good pattern shape, in a fine patterning process using a multilayer resist method in a semiconductor device manufacturing process, a pattern formation method using the material, and a method for forming the adhesion film. [Means for solving the problem]

[0012] In order to solve the above problems, the present invention provides An adhesion film forming material for an adhesion film formed between a silicon-containing intermediate film and a resist top layer film, (A) a resin having structural units represented by the following general formula (1) and the following general formula (2), (B) a thermal acid generator; and (C) Organic solvent and The component (A) has a molar fraction of structural units represented by the following general formula (1) of 5% or more, and a molar fraction of structural units represented by the following general formula (2) of 30% or more. [ka] (In the formula, R1 is a hydrogen atom or a methyl group, L1 is a single bond, a divalent organic group containing -C(=O)O-, or a divalent organic group containing -C(=O)NR2-. R2 is a hydrogen atom, or a linear or branched alkyl group having 1 to 3 carbon atoms.) [ka] (In the formula, R3 is a hydrogen atom or a methyl group, and R4 is a group selected from the following formulae (2-1) to (2-3).) [ka] (In the above formula, the dashed lines represent bonds.)

[0013] Such an adhesive film-forming material can form an adhesive film that has high adhesion to the resist upper layer film, has the effect of preventing the fine pattern from collapsing, and gives a good pattern shape.

[0014] Furthermore, in the present invention, the general formula (1) is preferably represented by the following general formula (3). [ka] (In the formula, R1 and R2 are the same as above. L2 is a single bond or an alkylene group having 1 to 2 carbon atoms, and a hydrogen atom of the alkylene group may be substituted with a hydroxyl group, and a methylene group constituting the alkylene group may be substituted with a carbonyl group.)

[0015] The introduction of such a catechol structural unit containing an amide bond can improve adhesion not only to the resist top layer but also to the silicon-containing intermediate layer, thereby enhancing the effect of preventing collapse of the fine pattern.

[0016] In the present invention, the silicon-containing intermediate film is preferably a silicon-containing resist intermediate film or an inorganic hard mask intermediate film.

[0017] In the present invention, such an interlayer film can be suitably used as the silicon-containing interlayer film.

[0018] In the present invention, it is preferable that the composition further contains, as the photoacid generator (D), one or more compounds represented by the following general formula (4). [ka] (In the formula, R5, R6, and R7 each independently represent a linear alkyl group or alkenyl group having 1 to 10 carbon atoms, which may be substituted with a heteroatom or may have a heteroatom interposed therebetween, or an aryl group or aralkyl group having 6 to 21 carbon atoms, which may be substituted with a heteroatom or may have a heteroatom interposed therebetween. Any two of R5, R6, and R7 may be bonded to each other to form a ring together with the sulfur atom in the formula. Y - represents either the following general formula (5) or the following general formula (6). [ka] [ka] (In the formula, R8 and R9 are each independently a monovalent hydrocarbon group containing an aliphatic ring structure having 3 to 40 carbon atoms which may be substituted with or interrupted by a heteroatom.)

[0019] Such an adhesive film-forming material has the effect of preventing collapse of a fine pattern, and also allows appropriate adjustment of the pattern shape, exposure sensitivity, etc. of the resist upper layer film.

[0020] In this case, the general formula (5) is preferably represented by the following general formula (7). [ka] (In the formula, R 10 R represents a hydrogen atom or a trifluoromethyl group. 11 represents a monovalent hydrocarbon group containing an aliphatic ring structure having 3 to 35 carbon atoms, which may be substituted with a heteroatom or which may be interrupted by a heteroatom.

[0021] Such an adhesive film-forming material has sufficient acidity, and allows for appropriate adjustment of acid diffusion, and may also be effective in reducing residues derived from the upper layer film of the resist.

[0022] In the present invention, the weight average molecular weight of the (A) resin is preferably 1,000 to 30,000.

[0023] An adhesive film-forming material containing a resin having such a weight-average molecular weight range has excellent film-forming properties, and can suppress the generation of sublimates during heat curing, thereby suppressing contamination of the device due to the sublimates. Also, the occurrence of coating defects can be suppressed.

[0024] In the present invention, it is preferable that the composition further contains at least one selected from the group consisting of (E) a surfactant, (F) a crosslinking agent, (G) a plasticizer, and (H) a dye.

[0025] The presence or absence / selection of these various additives makes it possible to fine-tune the performance in accordance with customer requirements, such as film-forming properties, embedding properties, optical properties, and reduction of sublimation products, which is preferable from a practical standpoint.

[0026] In addition, in the present invention, A method for forming a pattern on a workpiece substrate, comprising the steps of: (I-1) forming a resist underlayer film on the substrate; (I-2) forming a silicon-containing resist intermediate film on the resist underlayer film; (I-3) on the silicon-containing resist intermediate film, The above A step of forming an adhesive film by applying an adhesive film-forming material and then performing a heat treatment; (I-4) forming a resist top layer film on the adhesion film using a photoresist material; (I-5) a step of forming a pattern on the resist upper layer film by pattern-exposing the resist upper layer film and then developing the resist upper layer film with a developer; (I-6) a step of transferring the pattern to the adhesion film by dry etching using the resist upper layer film on which the pattern has been formed as a mask; (I-7) a step of transferring the pattern to the silicon-containing resist intermediate film by dry etching using the adhesion film on which the pattern has been formed as a mask; (I-8) a step of transferring a pattern to the resist underlayer film by dry etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; and (I-9) a step of transferring the pattern to the substrate by dry etching using the resist underlayer film to which the pattern has been transferred as a mask; The present invention provides a pattern forming method comprising the steps of:

[0027] In addition, in the present invention, A method for forming a pattern on a workpiece substrate, comprising the steps of: (II-1) forming a resist underlayer film on the substrate; (II-2) forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the resist underlayer film; (II-3) On the inorganic hard mask intermediate film, The above A step of forming an adhesive film by applying an adhesive film-forming material and then performing a heat treatment; (II-4) forming a resist top layer film on the adhesion film using a photoresist material; (II-5) a step of forming a pattern on the resist upper layer film by pattern-exposing the resist upper layer film and then developing the resist upper layer film with a developer; (II-6) a step of transferring the pattern to the adhesion film by dry etching using the resist upper layer film on which the pattern is formed as a mask; (II-7) a step of transferring the pattern to the inorganic hard mask intermediate film by dry etching using the adhesive film on which the pattern is formed as a mask; (II-8) a step of transferring a pattern to the resist underlayer film by dry etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; and (II-9) a step of transferring the pattern to the substrate by dry etching using the resist underlayer film to which the pattern has been transferred as a mask; The present invention provides a pattern forming method comprising the steps of:

[0028] In this way, the adhesion film-forming material of the present invention can be suitably used in various pattern formation methods, such as a four-layer resist process in which the above-mentioned adhesion film is formed on a silicon-containing intermediate film (silicon-containing resist intermediate film, inorganic hard mask intermediate film). In these pattern formation methods, the formation of an adhesion film can effectively reduce pattern collapse, and is suitable for photolithography of a resist upper layer film.

[0029] In this case, it is preferable that the inorganic hard mask intermediate film is formed by a CVD method or an ALD method.

[0030] In the present invention, the method for forming a circuit pattern on the resist upper layer film is preferably photolithography with a wavelength of 10 nm or more and 300 nm or less, direct writing with an electron beam, nanoimprinting, or a combination of these.

[0031] In the present invention, the developing method is preferably alkaline developing or developing with an organic solvent.

[0032] In the present invention, by using the above-mentioned pattern formation method, the pattern can be formed satisfactorily and efficiently.

[0033] In addition, in the present invention, it is preferable to use, as the substrate to be processed, a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.

[0034] In this case, the metal is preferably silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.

[0035] According to the pattern forming method of the present invention, the above-mentioned substrate to be processed can be processed as described above to form a pattern.

[0036] The present invention also provides a method for forming an adhesion film that functions as an adhesion layer used in the manufacturing process of a semiconductor device, which comprises spin-coating the above-mentioned adhesion film-forming material on a substrate to be processed, and heat-treating the substrate coated with the adhesion film-forming material at a temperature of 100°C or higher and 300°C or lower for 10 to 600 seconds to form a hardened film.

[0037] The present invention also provides a method for forming an adhesion film that functions as an adhesion layer used in the manufacturing process of a semiconductor device, which comprises spin-coating the above-mentioned adhesion film-forming material on a substrate to be processed, and heat-treating the substrate coated with the adhesion film-forming material in an atmosphere having an oxygen concentration of 0.1% or more and 21% or less to form a hardened film.

[0038] By using such a method, the crosslinking reaction during the formation of the adhesive film can be promoted, and mixing with the resist upper layer film can be more effectively suppressed. In addition, by appropriately adjusting the heat treatment temperature, time, and oxygen concentration within the above ranges, it is possible to obtain an effect of suppressing the collapse of the pattern of the adhesive film suitable for the application, and to obtain the pattern shape adjustment property of the resist upper layer film.

[0039] The present invention also provides a method for forming an adhesion film that functions as an adhesion layer used in the manufacturing process of a semiconductor device, which comprises spin-coating the above-mentioned adhesion film-forming material on a substrate to be processed, and heat-treating the substrate coated with the adhesion film-forming material in an atmosphere with an oxygen concentration of less than 0.1%, thereby forming a hardened film.

[0040] This method is useful because it promotes the crosslinking reaction during the formation of the adhesion film and more highly suppresses intermixing with the overlying film without causing deterioration of the substrate to be processed, even if the substrate contains a material that is unstable when heated in an oxygen atmosphere. Effect of the Invention

[0041] As described above, the present invention can provide an adhesive film-forming material that has high adhesion to the resist top layer film and has a fine pattern collapse suppressing effect. In addition, this adhesive film-forming material has high adhesion and has a fine pattern collapse suppressing effect, and can appropriately adjust the pattern shape and exposure sensitivity of the resist top layer film. Therefore, it is extremely useful in a multi-layer resist process, such as a four-layer resist process in which the adhesive film is formed on a silicon-containing intermediate film. In addition, the adhesive film forming method of the present invention can form an adhesive film that is sufficiently cured on the substrate to be processed and has high adhesion to the resist top layer film. In addition, the pattern forming method of the present invention can form a fine pattern on the substrate to be processed with high precision in the multi-layer resist process. [Brief description of the drawings]

[0042] [Figure 1]FIG. 2 is an explanatory diagram of an example of a pattern forming method using a four-layer resist process of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram showing a method for measuring adhesion in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] As described above, in the fine patterning process using the multilayer resist method in the semiconductor device manufacturing process, there has been a demand for an adhesion film forming material that has high adhesion to an overlying resist film and has an effect of preventing the collapse of a fine pattern, a pattern formation method using said material, and a method for forming an adhesion film.

[0044] As a result of intensive research into the above-mentioned problems, the present inventors have been searching for an adhesion film-forming material that has high adhesion to a resist upper layer film by forming an adhesion film in multilayer lithography and has an effect of suppressing collapse of a fine pattern, and a pattern formation method using the material. As a result, the inventors have found that an adhesion film-forming material mainly composed of a resin having a specific terminal structure, a pattern formation method using the material, and a method for forming an adhesion film are very effective, and have completed the present invention.

[0045] That is, the present invention provides: An adhesion film forming material for an adhesion film formed between a silicon-containing intermediate film and a resist top layer film, (A) a resin having structural units represented by the following general formula (1) and the following general formula (2), (B) a thermal acid generator; and (C) Organic solvent and The component (A) is an adhesion film-forming material in which the molar fraction of structural units represented by the following general formula (1) is 5% or more, and the molar fraction of structural units represented by the following general formula (2) is 30% or more. [ka] (In the formula, R1 is a hydrogen atom or a methyl group, L1 is a single bond, a divalent organic group containing -C(=O)O-, or a divalent organic group containing -C(=O)NR2-. R2 is a hydrogen atom, or a linear or branched alkyl group having 1 to 3 carbon atoms.) [ka] (In the formula, R3 is a hydrogen atom or a methyl group, and R4 is a group selected from the following formulae (2-1) to (2-3).) [ka] (In the above formula, the dashed lines represent bonds.)

[0046] The present invention will be described in detail below, but the present invention is not limited thereto.

[0047] [Adhesive film forming materials] The present invention provides an adhesion film-forming material that provides an adhesion film formed between a silicon-containing intermediate film and a resist upper layer film, the adhesion film-forming material comprising (A) a resin having structural units represented by the following general formulas (1) and (2), (B) a thermal acid generator, and (C) an organic solvent, wherein in the (A) component, the molar fraction of the structural unit represented by the following general formula (1) is 5% or more, and the molar fraction of the structural unit represented by the following general formula (2) is 30% or more. [ka] (In the formula, R1 is a hydrogen atom or a methyl group, L1 is a single bond, a divalent organic group containing -C(=O)O-, or a divalent organic group containing -C(=O)NR2-. R2 is a hydrogen atom, or a linear or branched alkyl group having 1 to 3 carbon atoms.) [ka] (In the formula, R3 is a hydrogen atom or a methyl group, and R4 is a group selected from the following formulae (2-1) to (2-3).) [ka] (In the above formula, the dashed lines represent bonds.)

[0048] In the adhesive film-forming material of the present invention, the (A) resin may be used alone or in combination of two or more. Furthermore, the adhesive film-forming material may contain components other than the components (A) to (C). Each component will be described below.

[0049] [(A) Resin] The (A) resin contained in the adhesion film-forming material of the present invention has structural units represented by the following general formula (1) and the following general formula (2), and in the (A) component, the molar fraction of the structural unit represented by the following general formula (1) is 5% or more, and the molar fraction of the structural unit represented by the following general formula (2) is 30% or more. [ka] (In the formula, R1 is a hydrogen atom or a methyl group, L1 is a single bond, a divalent organic group containing -C(=O)O-, or a divalent organic group containing -C(=O)NR2-. R2 is a hydrogen atom, or a linear or branched alkyl group having 1 to 3 carbon atoms.) [ka] (In the formula, R3 is a hydrogen atom or a methyl group, and R4 is a group selected from the following formulae (2-1) to (2-3).) [ka] (In the above formula, the dashed lines represent bonds.)

[0050] The structural unit represented by the above general formula (1) functions as an adhesive group, and specifically, it is believed that the catechol group terminal structure interacts with the silicon-containing intermediate film and the resist top layer film through hydrogen bonding or other interactions, thereby improving adhesion.

[0051] Specific examples of L1 in the above general formula (1) other than a single bond include the following. [ka]

[0052] [ka] (In the formula, the dashed lines represent bonds.)

[0053] The structural unit represented by the above general formula (1) is preferably a structure represented by the following general formula (3). [ka] (In the formula, R1 and R2 are the same as above. L2 is a single bond or an alkylene group having 1 to 2 carbon atoms, and a hydrogen atom of the alkylene group may be substituted with a hydroxyl group, and a methylene group constituting the alkylene group may be substituted with a carbonyl group.)

[0054] Specific examples of the structural unit represented by the above general formula (3) include the following: Among these, from the viewpoints of adhesion and ease of raw material availability, it is particularly preferable that L2 is an alkylene group having 2 carbon atoms (ethylene group).

[0055] [ka]

[0056] The structural unit represented by the above general formula (2) functions as a crosslinking group. As shown in the diagram below, the interaction of the hydroxyl group generated by the ring-opening reaction that occurs during curing of the epoxy or oxetane structure allows the resin to be cured without impairing the adhesion to the resist top layer and the silicon-containing intermediate film.

[0057] [ka] (R3 is the same as above.)

[0058] Specific examples of the structural unit represented by the above general formula (2) include the following. [ka] (R3 is the same as above.)

[0059] In addition, the (A) resin contained in the adhesion film forming material of the present invention has structural units represented by the above general formula (1) and the above general formula (2) in its structural units, and the structural units represented by the above general formula (1) or the above general formula (2) can be used singly or in combination of two or more kinds.

[0060] By combining multiple structural units, it is possible to improve adhesion and prevent fine patterns from collapsing, as well as to appropriately adjust the pattern shape and exposure sensitivity of the resist upper layer film. and This becomes possible.

[0061] Furthermore, in the present invention, the molar fraction of the structural unit represented by the above general formula (1) in the (A) resin is 5% or more, preferably 5% to 50%, more preferably 5% to 30%, and even more preferably 10% to 30%. The molar fraction of the structural unit represented by the above general formula (2) is 30% or more, preferably 30% to 95%, more preferably 40% to 90%, and even more preferably 50% to 90%. Combining structural units within such a range makes it possible to impart adhesion while maintaining curability.

[0062] In addition, when the molar fractions of the structural units represented by the above general formula (1) and the above general formula (2) do not total 100%, the resin (A) contains other structural units. In that case, the other structural units include α,β-unsaturated carboxylic acid esters such as other acrylic acid esters, other methacrylic acid esters, other acrylic acid amides, other methacrylic acid amides, crotonate esters, maleate esters, and itaconic acid esters; α,β-unsaturated carboxylic acids such as methacrylic acid, acrylic acid, maleate, and itaconic acid; acrylonitrile; methacrylonitrile; α,β-unsaturated lactones such as 5,5-dimethyl-3-methylene-2-oxotetrahydrofuran; norbornene derivatives, tetracyclo[4.4.0.1 2,5 .1 7,10 Any of structural units derived from cyclic olefins such as ]dodecene derivatives; α,β-unsaturated carboxylic anhydrides such as maleic anhydride and itaconic anhydride; allyl ethers; vinyl ethers; vinyl esters; and vinyl silanes can be used in combination.

[0063] By using an adhesion film-forming material containing such a resin in the formation of a multilayer resist film applied to fine processing in the manufacturing process of a semiconductor device or the like, it is possible to provide an adhesion film-forming material that has high adhesion to an overlying resist film and has the effect of preventing collapse of a fine pattern, and which can be easily manufactured, a method for forming an adhesion film, and a method for forming a pattern.

[0064] The resin can be synthesized by polymerizing each monomer protected by a protecting group as necessary by a known method, and then carrying out a deprotection reaction as necessary. The polymerization reaction is not particularly limited, but is preferably radical polymerization or anionic polymerization. For these methods, JP-A-2004-115630 can be referred to.

[0065] The resin preferably has a weight average molecular weight (Mw) of 1,000 to 30,000, more preferably 5,000 to 25,000, and even more preferably 5,000 to 15,000. If Mw is 1,000 or more, the resin has excellent film-forming properties, and can suppress the generation of sublimates during heat curing, thereby suppressing contamination of the device due to the sublimates. On the other hand, if Mw is 30,000 or less, the resin can suppress poor coating properties and coating defects due to insufficient solubility in a solvent. The resin also preferably has a molecular weight distribution (Mw / Mn) of 1.0 to 3.0, and more preferably 1.0 to 2.5. In the present invention, Mw and molecular weight distribution are values ​​measured in terms of polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent.

[0066] [(B) Thermal acid generator] In the adhesive film-forming material of the present invention, a thermal acid generator (B) is added in order to promote the crosslinking reaction by heat.

[0067] The thermal acid generator (B) that can be used in the adhesive film-forming material of the present invention is Examples include general formula (8).

[0068] [ka] (In the formula, K - R represents a non-nucleophilic counter ion. 12 , R 13 , R 14 , R 15 each represents a hydrogen atom or a linear, branched or cyclic alkyl group, alkenyl group, oxoalkyl group or oxoalkenyl group having 1 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group or aryloxoalkyl group having 7 to 12 carbon atoms, and some or all of the hydrogen atoms of these groups may be substituted with an alkoxy group or the like. 12 and R 13 , R 12 and R 13 and R 14 may form a ring, and when a ring is formed, R12 and R 13 and R 12 and R 13 and R 14 represents an alkylene group having 3 to 10 carbon atoms, or a heteroaromatic ring having a nitrogen atom in the ring.

[0069] Above, R 12 , R 13 , R 14 , R 15may be the same or different, and specifically, the alkyl group includes a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclopropylmethyl group, a 4-methylcyclohexyl group, a cyclohexylmethyl group, a norbornyl group, and an adamantyl group. The alkenyl group includes a vinyl group, an allyl group, a propenyl group, a butenyl group, a hexenyl group, and a cyclohexenyl group. The oxoalkyl group includes a 2-oxocyclopentyl group, a 2-oxocyclohexyl group, and the like, and examples of the oxopropyl group, a 2-cyclopentyl-2-oxoethyl group, a 2-cyclohexyl-2-oxoethyl group, and a 2-(4-methylcyclohexyl)-2-oxoethyl group. Examples of the oxoalkenyl group include a 2-oxo-4-cyclohexenyl group and a 2-oxo-4-propenyl group. Examples of the aryl group include a phenyl group, a naphthyl group, and the like; alkoxyphenyl groups such as a p-methoxyphenyl group, a m-methoxyphenyl group, an o-methoxyphenyl group, an ethoxyphenyl group, a p-tert-butoxyphenyl group, and a m-tert-butoxyphenyl group; alkylphenyl groups such as a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, an ethylphenyl group, a 4-tert-butylphenyl group, a 4-butylphenyl group, and a dimethylphenyl group; alkylnaphthyl groups such as a methylnaphthyl group and an ethylnaphthyl group; alkoxynaphthyl groups such as a methoxynaphthyl group and an ethoxynaphthyl group; dialkylnaphthyl groups such as a dimethylnaphthyl group and a diethylnaphthyl group; and dialkoxynaphthyl groups such as a dimethoxynaphthyl group and a diethoxynaphthyl group. Examples of the aralkyl group include a benzyl group, a phenylethyl group, a phenethyl group, etc. Examples of the aryloxoalkyl group include a 2-aryl-2-oxoethyl group such as a 2-phenyl-2-oxoethyl group, a 2-(1-naphthyl)-2-oxoethyl group, and a 2-(2-naphthyl)-2-oxoethyl group.

[0070] Also, R 12 , R 13 , R14 , R 15 Examples of the heteroaromatic ring having a nitrogen atom in the ring include imidazole derivatives (e.g., imidazole, 4-methylimidazole, 4-methyl-2-phenylimidazole, etc.), pyrazole derivatives, furazan derivatives, pyrroline derivatives (e.g., pyrroline, 2-methyl-1-pyrroline, etc.), pyrrolidine derivatives (e.g., pyrrolidine, N-methylpyrrolidine, pyrrolidinone, N-methylpyrrolidone, etc.), imidazoline derivatives, imidazolidine derivatives, pyridine derivatives (e.g., pyridine, methylpyridine, ethylpyridine, propylpyridine, butylpyridine, 4-(1-butylpentyl)pyridine, dimethylpyridine, trimethylpyridine, triethylpyridine, phenylpyridine, 3-methyl-2-phenylpyridine, 4-tert-butylpyridine, diphenylpyridine, benzylpyridine, methoxypyridine, butoxypyridine, dimethoxypyridine, 1-methyl-2-pyridone, Examples include 4-pyrrolidinopyridine, 1-methyl-4-phenylpyridine, 2-(1-ethylpropyl)pyridine, aminopyridine, dimethylaminopyridine, etc.), pyridazine derivatives, pyrimidine derivatives, pyrazine derivatives, pyrazoline derivatives, pyrazolidine derivatives, piperidine derivatives, piperazine derivatives, morpholine derivatives, indole derivatives, isoindole derivatives, 1H-indazole derivatives, indoline derivatives, quinoline derivatives (e.g., quinoline, 3-quinolinecarbonitrile, etc.), isoquinoline derivatives, cinnoline derivatives, quinazoline derivatives, quinoxaline derivatives, phthalazine derivatives, purine derivatives, pteridine derivatives, carbazole derivatives, phenanthridine derivatives, acridine derivatives, phenazine derivatives, 1,10-phenanthroline derivatives, adenine derivatives, adenosine derivatives, guanine derivatives, guanosine derivatives, uracil derivatives, uridine derivatives, and the like.

[0071] Above, K. -Examples of the non-nucleophilic counter ion include halide ions such as chloride ion and bromide ion; fluoroalkyl sulfonates such as triflate, 1,1,1-trifluoroethanesulfonate, and nonafluorobutanesulfonate; aryl sulfonates such as tosylate, benzenesulfonate, 4-fluorobenzenesulfonate, and 1,2,3,4,5-pentafluorobenzenesulfonate; alkyl sulfonates such as mesylate and butanesulfonate; imide acids such as bis(trifluoromethylsulfonyl)imide, bis(perfluoroethylsulfonyl)imide, and bis(perfluorobutylsulfonyl)imide; methide acids such as tris(trifluoromethylsulfonyl)methide and tris(perfluoroethylsulfonyl)methide; and sulfonates substituted with fluoro at the α-position as shown in the following general formula (9) and sulfonates substituted with fluoro at the α- and β-positions as shown in the following general formula (10).

[0072] [ka] [ka] (In the above general formula (9), R 16 is a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, an acyl group, an alkenyl group having 2 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aryloxy group. 17 is a hydrogen atom, a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms.

[0073] Specific examples of the above-mentioned thermal acid generator include the following. [ka]

[0074] The above thermal acid generators can be used alone or in combination of two or more.

[0075] The amount of the thermal acid generator added is preferably 0.05 to 50 parts by mass, more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the above-described (A) resin. If the amount is 0.05 parts by mass or more, the amount of acid generated is small and there is little risk of the crosslinking reaction becoming insufficient, while if the amount is 50 parts by mass or less, there is little risk of the mixing phenomenon occurring due to the acid migrating to the upper resist layer.

[0076] [(C) Organic solvent] The organic solvent (C) contained in the adhesive film forming material used in the adhesive film forming method of the present invention is not particularly limited as long as it dissolves the above-mentioned (A) resin, (B) thermal acid generator, (D) photoacid generator (if present), and other additives. Specifically, solvents having a boiling point of less than 180°C, such as those described in paragraphs

[0091] to

[0092] of JP-A-2007-199653, can be used. Among them, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, 2-heptanone, cyclopentanone, cyclohexanone, and mixtures of two or more of these are preferably used.

[0077] The amount of the organic solvent to be added is desirably adjusted depending on the set thickness of the adhesive film, but is usually within the range of 100 to 50,000 parts by mass per 100 parts by mass of the above-described (A) resin.

[0078] Such an adhesion film-forming material can be applied by spin coating, and since it contains the above-mentioned (A) resin, it has high adhesion to the resist overcoat film, and serves as an adhesion film-forming composition for forming an adhesion film that has the effect of preventing the collapse of a fine pattern.

[0079] [(D) Photoacid generator] The adhesive film-forming material of the present invention preferably contains a photoacid generator as component (D). The photoacid generator is preferably one represented by the following general formula (4). [ka] (In the formula, R5, R6, and R7 each independently represent a linear alkyl group or alkenyl group having 1 to 10 carbon atoms, which may be substituted with a heteroatom or may have a heteroatom interposed therebetween, or an aryl group or aralkyl group having 6 to 21 carbon atoms, which may be substituted with a heteroatom or may have a heteroatom interposed therebetween. Any two of R5, R6, and R7 may be bonded to each other to form a ring together with the sulfur atom in the formula. Y - represents either the following general formula (5) or the following general formula (6). [ka] [ka] (In the formula, R8 and R9 are each independently a monovalent hydrocarbon group containing an aliphatic ring structure having 3 to 40 carbon atoms which may be substituted with or interrupted by a heteroatom.)

[0080] In this case, it is more preferable that the above general formula (5) is represented by the following general formula (7). [ka] (In the formula, R 10 R represents a hydrogen atom or a trifluoromethyl group. 11 represents a monovalent hydrocarbon group containing an aliphatic ring structure having 3 to 35 carbon atoms, which may be substituted with a heteroatom or which may be interrupted by a heteroatom.

[0081] R5, R6, and R7 in the above general formula (4) each independently represent a linear alkyl group or alkenyl group having 1 to 10 carbon atoms, which may be substituted with a heteroatom or which may have a heteroatom interposed therebetween, or a branched or cyclic alkyl group or alkenyl group having 3 to 10 carbon atoms, which may be substituted with a heteroatom or which may have a heteroatom interposed therebetween, or an aryl group or aralkyl group having 6 to 21 carbon atoms, which may be substituted with a heteroatom or which may have a heteroatom interposed therebetween. Specific examples of the alkyl group include alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, a cyclopropyl group, a cyclopentyl group, a cyclohexyl group, a cyclopropylmethyl group, a 4-methylcyclohexyl group, a cyclohexylmethyl group, a norbornyl group, and an adamantyl group; alkenyl groups such as a vinyl group, an allyl group, a propenyl group, a butenyl group, a hexenyl group, and a cyclohexenyl group; aryl groups such as a phenyl group, a naphthyl group, and a thienyl group; and aralkyl groups such as a benzyl group, a 1-phenylethyl group, and a 2-phenylethyl group, with an aryl group being preferred. In addition, some of the hydrogen atoms of these groups may be replaced with heteroatoms such as oxygen atoms, sulfur atoms, nitrogen atoms, and halogen atoms, or heteroatoms such as oxygen atoms, sulfur atoms, and nitrogen atoms may be present, resulting in the formation or interposition of a hydroxy group, cyano group, carbonyl group, ether bond, ester bond, sulfonate ester bond, carbonate bond, lactone ring, sultone ring, carboxylic acid anhydride, haloalkyl group, etc. In addition, any two of R5, R6, and R7 may be bonded to each other to form a ring together with the sulfur atom in the formula.

[0082] R5, R6, R7 and S in the above general formula (4) +Specific examples of the partial structure represented by the formula (I) include triphenylsulfonium, 4-hydroxyphenyldiphenylsulfonium, bis(4-hydroxyphenyl)phenylsulfonium, tris(4-hydroxyphenyl)sulfonium, 4-tert-butoxyphenyldiphenylsulfonium, bis(4-tert-butoxyphenyl)phenylsulfonium, tris(4-tert-butoxyphenyl)sulfonium, 3-tert-butoxyphenyldiphenylsulfonium, bis(3-tert-butoxyphenyl)phenylsulfonium, ylsulfonium, tris(3-tert-butoxyphenyl)sulfonium, 3,4-di-tert-butoxyphenyl diphenylsulfonium, bis(3,4-di-tert-butoxyphenyl)phenylsulfonium, tris(3,4-di-tert-butoxyphenyl)sulfonium, diphenyl(4-thiophenoxyphenyl)sulfonium, 4-tert-butoxycarbonylmethyloxyphenyl diphenylsulfonium, tris(4-tert-butoxycarbonylmethyloxyphenyl)sulfonium, (4-tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, tris(4-dimethylaminophenyl)sulfonium, 2-naphthyldiphenylsulfonium, (4-hydroxy-3,5-dimethylphenyl)diphenylsulfonium, (4-n-hexyloxy-3,5-dimethylphenyl)diphenylsulfonium, dimethyl(2-naphthyl)sulfonium, 4-hydroxyphenyldimethylsulfonium, 4-methoxyphenyldimethylsulfonium, trimethylsulfonium, 2-oxo Examples of such sulfonium compounds include cyclohexylcyclohexylmethylsulfonium, trinaphthylsulfonium, tribenzylsulfonium, diphenylmethylsulfonium, dimethylphenylsulfonium, 2-oxo-2-phenylethylthiacyclopentanium, diphenyl-2-thienylsulfonium, 4-n-butoxynaphthyl-1-thiacyclopentanium, 2-n-butoxynaphthyl-1-thiacyclopentanium, 4-methoxynaphthyl-1-thiacyclopentanium, and 2-methoxynaphthyl-1-thiacyclopentanium.More preferred are triphenylsulfonium, 4-tert-butylphenyldiphenylsulfonium, 4-tert-butoxyphenyldiphenylsulfonium, tris(4-tert-butylphenyl)sulfonium, tris(4-tert-butoxyphenyl)sulfonium, dimethylphenylsulfonium, and the like.

[0083] Further examples include those represented by the following structures.

[0084] [ka]

[0085] In addition, Y in the above general formula (4) - is either the above general formula (5) or the above general formula (6), but is not limited thereto. In the above general formula (5) or the above general formula (6), R8 and R9 each independently represent a monovalent hydrocarbon group containing an aliphatic ring structure having 3 to 40 carbon atoms which may be substituted with a heteroatom and may be interrupted by a heteroatom, and are preferably a 1-norbornyl group, a 1-adamantyl group, a 2-adamantyl group, or a 4-oxo-1-adamantyl group.

[0086] Furthermore, it is preferable that the general formula (5) is represented by the general formula (7). 10 R represents a hydrogen atom or a trifluoromethyl group, and is preferably a trifluoromethyl group. 11 represents a monovalent hydrocarbon group containing an aliphatic ring structure having 3 to 35 carbon atoms which may be substituted with or interrupted by a heteroatom, and is preferably a 1-norbornyl group, a 1-adamantyl group, a 2-adamantyl group, or a 4-oxo-1-adamantyl group.

[0087] Specific examples of Y- represented by the above general formulas (5), (6) and (7) include, but are not limited to, the following:

[0088] [ka]

[0089] [ka]

[0090] [ka]

[0091] [ka]

[0092] [ka]

[0093] [ka]

[0094] [ka]

[0095] [ka]

[0096] The above (D) photoacid generator can be used alone or in combination of two or more to appropriately adjust the pattern shape, exposure sensitivity, etc. of the resist upper layer film. When the (D) photoacid generator is added, the amount added is preferably 0.5 to 20 parts by mass, more preferably 1 to 15 parts by mass, per 100 parts by mass of the above (A) resin. When the (D) photoacid generator is added in an amount within the above range, the resolution is good, and there is no risk of problems with foreign matter that may cause defects after resist development or during peeling.

[0097] [Other additives] In addition to the above-mentioned components (A) to (D), the adhesive film-forming material of the present invention may further contain one or more of the following: (E) a surfactant, (F) a crosslinking agent, (G) a plasticizer, and (H) a dye. Each component will be described below.

[0098] [(E) Surfactant] To the adhesive film forming material of the present invention, a surfactant (E) can be added to improve the coating property in spin coating. For example, the surfactants described in

[0142] to

[0147] of JP-A-2009-269953 can be used. When a surfactant is added, the amount of the surfactant added is preferably 0.001 to 20 parts by mass, more preferably 0.01 to 10 parts by mass, based on 100 parts by mass of the resin (A).

[0099] [(F) Crosslinking agent] In addition, in order to enhance the curing property and further suppress intermixing with the resist upper layer film, a crosslinking agent (F) may be added to the adhesive film forming material of the present invention. The crosslinking agent is not particularly limited, and various known crosslinking agents can be widely used. Examples include melamine-based crosslinking agents, glycoluril-based crosslinking agents, benzoguanamine-based crosslinking agents, urea-based crosslinking agents, β-hydroxyalkylamide-based crosslinking agents, isocyanurate-based crosslinking agents, aziridine-based crosslinking agents, oxazoline-based crosslinking agents, epoxy-based crosslinking agents, and phenol-based crosslinking agents (polynuclear phenol-based crosslinking agents).

[0100] The (F) crosslinking agent can be used alone or in combination of two or more, and the amount of the crosslinking agent added is preferably 5 to 50 parts by mass, more preferably 10 to 40 parts by mass, relative to 100 parts by mass of the (A) resin. If the amount added is 5 parts by mass or more, sufficient curability is exhibited and intermixing with the resist upper layer film can be suppressed. On the other hand, if the amount added is 50 parts by mass or less, there is no risk of deterioration of adhesion due to a low ratio of the (A) resin in the composition.

[0101] Specific examples of the melamine-based crosslinking agent include hexamethoxymethylated melamine, hexabutoxymethylated melamine, alkoxy and / or hydroxyl-substituted derivatives thereof, and partial self-condensates thereof. Specific examples of the glycoluril-based crosslinking agent include tetramethoxymethylated glycoluril, tetrabutoxymethylated glycoluril, alkoxy and / or hydroxyl-substituted derivatives thereof, and partial self-condensates thereof. Specific examples of the benzoguanamine-based crosslinking agent include tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, alkoxy and / or hydroxyl-substituted derivatives thereof, and partial self-condensates thereof. Specific examples of the urea-based crosslinking agent include dimethoxymethylated dimethoxyethyleneurea, alkoxy and / or hydroxyl-substituted derivatives thereof, and partial self-condensates thereof. Specific examples of the β-hydroxyalkylamide-based crosslinking agent include N,N,N',N'-tetra(2-hydroxyethyl)adipic acid amide. Specific examples of the isocyanurate crosslinking agent include triglycidyl isocyanurate and triallyl isocyanurate.Specific examples of the aziridine crosslinking agent include 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate]. Specific examples of the oxazoline-based crosslinking agent include 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tertbutyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymer.Specific examples of epoxy crosslinking agents include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether.

[0102] Specific examples of polynuclear phenol-based crosslinking agents include compounds represented by the following general formula (12). [ka] (In the formula, Q is a single bond or a q-valent hydrocarbon group having 1 to 20 carbon atoms. R 18 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. q is an integer of 1 to 5.

[0103] Q is a single bond or a q-valent hydrocarbon group having 1 to 20 carbon atoms. q is an integer of 1 to 5, and is more preferably 2 or 3. Specific examples of Q include methane, ethane, propane, butane, isobutane, pentane, cyclopentane, hexane, cyclohexane, methylpentane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, benzene, toluene, xylene, ethylbenzene, ethylisopropylbenzene, diisopropylbenzene, methylnaphthalene, ethylnaphthalene, and eicosane. R 18 is a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. Specific examples of the alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a pentyl group, an isopentyl group, a hexyl group, an octyl group, an ethylhexyl group, a decyl group, and an eicosanyl group, and a hydrogen atom or a methyl group is preferable.

[0104] Specific examples of the compound represented by the above general formula (12) include the following compounds. Among these, from the viewpoint of improving the curability and thickness uniformity of the adhesive film, hexamethoxymethylated products of triphenolmethane, triphenolethane, 1,1,1-tris(4-hydroxyphenyl)ethane, and tris(4-hydroxyphenyl)-1-ethyl-4-isopropylbenzene are preferred.

[0105] [ka]

[0106] [ka]

[0107] [(G) Plasticizer] A plasticizer can be added to the adhesive film forming material of the present invention. The plasticizer is not particularly limited, and various known plasticizers can be widely used. Examples include low molecular weight compounds such as phthalates, adipic esters, phosphates, trimellitates, and citrates, and polymers such as polyethers, polyesters, and polyacetal polymers described in JP-A-2013-253227. When a plasticizer is added, the amount of the plasticizer is preferably 5 to 500 parts by mass, more preferably 10 to 200 parts by mass, relative to 100 parts by mass of the (A) resin.

[0108] [(H)Dye] In addition, a dye can be added to the adhesive film forming material of the present invention in order to further improve the resolution during patterning in multilayer lithography. The dye is not particularly limited as long as it is a compound that has a suitable absorption at the exposure wavelength, and various known compounds can be widely used. Examples include benzenes, naphthalenes, anthracenes, phenanthrenes, pyrenes, isocyanuric acids, and triazines. When a dye is added, the amount of the dye is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, based on 100 parts by mass of the (A) resin.

[0109] Furthermore, the adhesion film forming material of the present invention is extremely useful as an adhesion film material for multi-layer resist processes such as a four-layer resist process using a resist underlayer film and a silicon-containing intermediate film.

[0110] The silicon-containing intermediate film can be a silicon-containing resist intermediate film or an inorganic hard mask intermediate film according to the pattern forming method described later. The inorganic hard mask intermediate film is preferably selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film.

[0111] [Method of forming adhesive film] The present invention provides a method for forming an adhesion film that has high adhesion to an overlying resist film and has an effect of preventing collapse of a fine pattern in a fine patterning process using a multilayer resist method in a semiconductor device manufacturing process, using the above-mentioned adhesion film forming material.

[0112] In the method for forming an adhesive film of the present invention, the above-mentioned adhesive film forming material is coated on a substrate to be processed by a spin coating (spin coating) method or the like. After spin coating, the organic solvent is evaporated, and baking (heat treatment) is performed to promote a crosslinking reaction in order to prevent intermixing with the resist upper layer film or the silicon-containing intermediate film. The baking is preferably performed at 100°C or higher and 300°C or lower for 10 to 600 seconds, more preferably at 200°C or higher and 250°C or lower for 10 to 300 seconds. Considering the damage to the adhesive film and the influence on the deformation of the wafer, the upper limit of the heating temperature in the wafer process of lithography is preferably 300°C or lower, more preferably 250°C or lower.

[0113] In addition, in the method for forming an adhesion film of the present invention, the adhesion film forming material of the present invention is coated on a substrate to be processed by the spin coating method or the like as described above, and the adhesion film forming material is baked in an atmosphere with an oxygen concentration of 0.1% to 21% to harden the adhesion film, thereby forming the adhesion film. By baking the adhesion film forming material of the present invention in such an oxygen atmosphere, a sufficiently hardened film can be obtained.

[0114] The atmosphere during baking may be air or may contain an inert gas such as N2, Ar, or He. In this case, the atmosphere may have an oxygen concentration of less than 0.1%. The baking temperature and the like may be the same as above. Even if the substrate to be processed contains a material that is unstable when heated in an oxygen atmosphere, the crosslinking reaction during the formation of the adhesive film can be promoted without causing deterioration of the substrate to be processed.

[0115] [Pattern formation method] In the present invention, the following two methods are provided as a pattern formation method by a four-layer resist process using the above-mentioned adhesive film-forming material.

[0116] The first method is to first A method for forming a pattern on a workpiece substrate, comprising at least (I-1) forming a resist underlayer film on a substrate to be processed using an organic film material; (I-2) forming a silicon-containing intermediate film (silicon-containing resist intermediate film) on the resist underlayer film using a resist intermediate layer material containing silicon atoms; (I-3) applying the adhesion film-forming material of the present invention onto the silicon-containing resist intermediate film, and then heat-treating the coating to form an adhesion film; (I-4) forming a resist upper layer film on the adhesion film using a resist upper layer film material (photoresist material) composed of a photoresist composition to form a multi-layer resist film; (I-5) exposing the pattern circuit region of the resist upper layer film (pattern exposure) and then developing it with a developer to form a pattern on the resist upper layer film; (I-6) dry-etching the adhesive film using the resist upper layer film on which the pattern has been formed as an etching mask to transfer the pattern to the adhesive film; (I-7) dry-etching the silicon-containing resist intermediate film using the adhesion film on which the pattern is formed as an etching mask to transfer the pattern to the silicon-containing resist intermediate film; (I-8) dry-etching the resist underlayer film using the silicon-containing resist intermediate film on which the pattern has been formed as an etching mask to transfer the pattern to the resist underlayer film; (I-9) Further, there is provided a pattern forming method, which comprises dry etching the substrate to be processed using the resist underlayer film on which the pattern is formed as an etching mask to transfer the pattern to the substrate to be processed.

[0117] As the silicon-containing resist intermediate film in the above four-layer resist process, a polysilsesquioxane-based intermediate film is also preferably used. By imparting an anti-reflection effect to the silicon-containing resist intermediate film, reflection can be suppressed. In particular, for 193 nm exposure, if a material containing many aromatic groups and having high substrate etching resistance is used as the resist underlayer film, the k value becomes high and the substrate reflection becomes high, but by suppressing reflection with the silicon-containing resist intermediate film, the substrate reflection can be reduced to 0.5% or less. As the silicon-containing resist intermediate film having an anti-reflection effect, anthracene is preferably used for 248 nm and 157 nm exposure, and polysilsesquioxane is preferably used for 193 nm exposure, which is pendant with a light-absorbing group having a phenyl group or a silicon-silicon bond and crosslinked with acid or heat.

[0118] In this case, the formation of the silicon-containing resist intermediate film by spin coating is easier and more cost-effective than the CVD method.

[0119] In the second method, an inorganic hard mask intermediate film may be formed as the silicon-containing intermediate film. In this case, A method for forming a pattern on a workpiece substrate, comprising at least (II-1) forming a resist underlayer film on a substrate to be processed using an organic film material; (II-2) forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the resist underlayer film; (II-3) applying the adhesion film forming material of the present invention onto the inorganic hard mask intermediate film, and then heat-treating the material to form an adhesion film; (II-4) forming a resist upper layer film on the adhesion film using a resist upper layer film material (photoresist material) consisting of a photoresist composition; (II-5) exposing the pattern circuit region of the resist upper layer film (pattern exposure) and then developing it with a developer to form a pattern on the resist upper layer film; (II-6) Using the resist upper layer film on which the pattern has been formed as an etching mask, the adhesive film is dry-etched to transfer the adhesive film pattern; (II-7) dry-etching the inorganic hard mask intermediate film using the adhesion film on which the pattern is formed as an etching mask to transfer the pattern to the inorganic hard mask intermediate film; (II-8) dry-etching the resist underlayer film using the inorganic hard mask intermediate film on which the pattern has been formed as an etching mask to transfer the pattern to the resist underlayer film; (II-9) Furthermore, the pattern can be transferred to the substrate to be processed by dry etching the substrate using the resist underlayer film on which the pattern has been formed as an etching mask.

[0120] The resist underlayer film is not particularly limited, and any known one can be used. For example, the resist underlayer film material is coated on the substrate to be processed using a spin coating method or the like. After spin coating, the solvent is evaporated, and baking is performed to promote the crosslinking reaction in order to prevent mixing with the silicon-containing intermediate film. Baking is performed at a temperature range of 100°C to 600°C, for 10 to 600 seconds, preferably 10 to 300 seconds. At a baking temperature of 100°C or higher, curing proceeds sufficiently and mixing with the upper layer film or intermediate film does not occur. If the baking temperature is 600°C or lower, the thermal decomposition of the base resin can be suppressed, the film thickness does not decrease, and the film surface becomes uniform. The thickness of the resist underlayer film is appropriately selected, but it is preferably 2 to 20,000 nm, particularly 50 to 15,000 nm.

[0121] As described above, when forming an inorganic hard mask intermediate film on a resist underlayer film, a silicon oxide film, a silicon nitride film, and a silicon oxide nitride film (SiON film) can be formed by a CVD method, an ALD method, or the like. For example, a method for forming a silicon nitride film is described in JP-A-2002-334869 and WO-A-2004 / 066377. The thickness of the inorganic hard mask intermediate film is preferably 5 to 200 nm, more preferably 10 to 100 nm. In addition, as the inorganic hard mask intermediate film, a SiON film, which has a high effect as an anti-reflection film, is most preferably used. Since the substrate temperature during the formation of the SiON film is 300 to 500°C, the resist underlayer film needs to withstand a temperature of 300 to 500°C.

[0122] The resist upper layer film in the above four-layer resist process may be either positive or negative, and may be the same as a commonly used photoresist composition. After spin-coating the photoresist composition, pre-baking is performed, preferably at 60 to 180°C for 10 to 300 seconds. Thereafter, exposure is performed according to a conventional method, followed by post-exposure baking (PEB) and development to obtain a resist upper layer film pattern. The thickness of the resist upper layer film is not particularly limited, but is preferably 30 to 500 nm, and more preferably 50 to 400 nm.

[0123] A circuit pattern (resist upper layer film pattern) is formed on the resist upper layer film. In forming the circuit pattern, it is preferable to form the circuit pattern by lithography using light having a wavelength of 10 nm or more and 300 nm or less, direct drawing with an electron beam, nanoimprinting, or a combination of these.

[0124] Examples of the exposure light include high-energy rays having a wavelength of 300 nm or less, specifically far ultraviolet rays, KrF excimer laser light (248 nm), ArF excimer laser light (193 nm), F2 laser light (157 nm), Kr2 laser light (146 nm), Ar2 laser light (126 nm), soft X-rays (EUV) of 3 to 20 nm, electron beams (EB), ion beams, X-rays, etc. In particular, it is preferable to use ArF excimer laser light (193 nm), soft X-rays (EUV) of 3 to 20 nm, and electron beams (EB), which are exposure lights for processing ultrafine patterns.

[0125] In the development method during the formation of the circuit pattern, it is preferable to develop the circuit pattern with an alkali developer or an organic solvent.

[0126] Next, etching is performed using the resist top layer film pattern as a mask. In the four-layer resist process, the adhesion film is etched using an oxygen-based gas with the resist top layer film pattern as a mask. This forms an adhesion film pattern.

[0127] Next, etching is performed using the obtained adhesive film pattern as a mask. The etching of the silicon-containing resist intermediate film or the inorganic hard mask intermediate film is performed using the adhesive film pattern as a mask with a fluorocarbon-based gas. In this way, a silicon-containing resist intermediate film pattern or an inorganic hard mask intermediate film pattern is formed.

[0128] The etching of the adhesion film may be carried out prior to and consecutively with the etching of the silicon-containing intermediate film, or the etching of the silicon-containing intermediate film may be carried out after etching only the adhesion film, for example by changing the etching apparatus.

[0129] Next, the resist underlayer film is etched using the obtained silicon-containing resist intermediate film pattern or inorganic hard mask intermediate film pattern as a mask.

[0130] The next step, etching of the substrate to be processed, can also be done by standard methods; for example, if the substrate to be processed is a SiO2, SiN, or silica-based low dielectric constant insulating film, etching is done mainly with fluorocarbon gases, and for p-Si, Al, or W, etching is done mainly with chlorine- or bromine-based gases. When etching the substrate with fluorocarbon gases, the silicon-containing intermediate film pattern in the four-layer resist process is peeled off at the same time as the substrate is processed. When etching the substrate with chlorine- or bromine-based gases, the silicon-containing intermediate film pattern must be peeled off by separate dry etching using fluorocarbon gases after substrate processing.

[0131] The substrate to be processed is not particularly limited, and may be a semiconductor device substrate, or a semiconductor device substrate on which any of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film is formed. As the metal, silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof may be used.

[0132] Specifically, substrates such as Si, α-Si, p-Si, SiO2, SiN, SiON, W, TiN, Al, etc., and substrates on which a layer to be processed is formed, etc. are used. As the layer to be processed, various low-k films such as Si, SiO2, SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si, etc. and their stopper films are used, and can be formed to a thickness of usually 50 to 10,000 nm, particularly 100 to 5,000 nm. When forming a layer to be processed, the substrate and the layer to be processed are made of different materials.

[0133] An example of a four-layer resist process is specifically shown below with reference to Fig. 1. In the four-layer resist process, as shown in Fig. 1(A), a resist underlayer film 3 is formed using an organic film material on a processable layer 2 laminated on a substrate 1, and then a silicon-containing intermediate film 4 is formed thereon, an adhesion film 5 is formed thereon using the adhesion film-forming material of the present invention, and a resist upper layer film 6 is formed thereon.

[0134] Next, as shown in FIG. 1(B), the exposed portion (required portion) 7 of the resist upper layer film is exposed, and PEB and development are performed to form a resist upper layer film pattern 6a (FIG. 1(C)). Using the obtained resist upper layer film pattern 6a as a mask, the adhesion film 5 is etched using an O2-based gas to form an adhesion film pattern 5a. (FIG. 1(D)). Using the obtained adhesion film pattern 5a as a mask, the silicon-containing intermediate film 4 is etched using a CF-based gas to form a silicon-containing intermediate film pattern 4a (FIG. 1(E)). After removing the adhesion film pattern 5a, using the obtained silicon-containing intermediate film pattern 4a as a mask, the resist underlayer film 3 is etched using an O2-based gas to form a resist underlayer film pattern 3a (FIG. 1(F)). Furthermore, after removing the silicon-containing intermediate film pattern 4a, the processed layer 2 is etched using the resist underlayer film pattern 3a as a mask to form a pattern 2a (FIG. 1(G)).

[0135] As described above, the pattern forming method of the present invention makes it possible to form a fine pattern on a substrate to be processed with high precision in a multi-layer resist process. EXAMPLES

[0136] The present invention will be described in more detail below with reference to synthesis examples, examples, and comparative examples, but the present invention is not limited thereto. The molecular weight was measured by the following method. The weight average molecular weight (Mw) and number average molecular weight (Mn) in terms of polystyrene were determined by gel permeation chromatography (GPC) using tetrahydrofuran as an eluent (solvent), and the polydispersity (Mw / Mn) was determined.

[0137] The polymers (A1) to (A8) and the comparative polymers (R1) to (R9) used as the resin (A) for the adhesive film-forming material were synthesized using the monomers (B1) to (B12) shown below. [ka]

[0138] [Synthesis Example 1] Synthesis of polymer (A1) 37.5 g of propylene glycol monomethyl ether acetate (PGMEA) was heated and stirred at 80°C under a nitrogen atmosphere. To this, a mixture of 7.22 g of (B1), 42.78 g of (B6), and 82.5 g of PGMEA, and a mixture of 4.07 g of dimethyl 2,2-azobis(2-methylpropionate) and 30.0 g of PGMEA were added simultaneously and separately over a period of 2 hours. After further heating and stirring for 24 hours, the mixture was cooled to room temperature to obtain a PGMEA solution of the target polymer (A1). Analysis showed that the weight average molecular weight (Mw) of the polymer (A1) was 14,300 and the dispersity (Mw / Mn) was 1.95. [ka]

[0139] [Synthesis Examples 2 to 17] Synthesis of Polymers (A2) to (A8) and Comparative Polymers (R1) to (R9) Except for changing the type and molar ratio of the raw material monomers used according to the structure of each polymer, the following polymers (A2) to (A8) and comparative polymers (R1) to (R9) were obtained as products by the method according to Synthesis Example 1. The weight average molecular weight (Mw) and dispersity (Mw / Mn) determined by GPC are also shown.

[0140] [ka]

[0141] [ka]

[0142] Preparation of adhesive film forming materials (AL-1 to 14, comparative AL-1 to 9) The adhesive film-forming materials and comparative materials were prepared using the above polymers (A1) to (A8) and the above comparative polymers (R1) to (R9), thermal acid generators (T1) to (T3), photoacid generators (P1) to (P3), and crosslinker (X1). The adhesive film-forming materials (AL-1 to 14, comparative AL-1 to 9) were prepared by dissolving the materials in the ratios shown in Table 1 using propylene glycol monomethyl ether acetate (PGMEA) containing 0.1 mass% PF636 (manufactured by OMNOVA) and filtering through a 0.1 μm fluororesin filter.

[0143] (Thermal acid generator) [ka]

[0144] (Photoacid generator) [ka]

[0145] (Crosslinking agent) [ka]

[0146] [Table 1]

[0147] Example 1 Solvent Resistance Evaluation (Examples 1-1 to 1-14, Comparative Examples 1-1 to 1-9) The adhesive film forming materials (AL-1 to 14, Comparative AL-1 to 9) prepared above were applied onto a silicon substrate, baked at 220°C for 60 seconds, the film thickness was measured, PGMEA solvent was dispensed onto it, left for 30 seconds, spin-dried, baked at 100°C for 60 seconds to evaporate the PGMEA solvent, the film thickness was measured again, and the difference in film thickness before and after PGMEA treatment was calculated to evaluate the solvent resistance. The results are shown in Table 2.

[0148] [Table 2]

[0149] As shown in Table 2, in Examples 1-1 to 1-14 using the adhesion film-forming material (AL-1 to 14) of the present invention, it is found that the film thickness is hardly reduced by the solvent treatment and a film with good solvent resistance is obtained. On the other hand, it is found that sufficient solvent resistance cannot be secured in Comparative Example 1-6, which does not have the structural unit represented by the above general formula (2) that contributes to crosslinking, and Comparative Example 1-7, which has a small amount of the structural unit. In addition, in Comparative Example 1-8, which has a small introduction rate of the structural unit represented by the above general formula (1), the residual film rate tends to be slightly low.

[0150] Example 2 Adhesion Test (Examples 2-1 to 2-14, Comparative Examples 2-1 to 2-9) The above adhesive film forming materials (AL-1 to 14, Comparative AL-1 to 9) were applied onto a SiO2 wafer substrate and baked for 60 seconds at 220°C in air using a hot plate to form an adhesive film with a thickness of 200 nm. The wafer with the adhesive film was cut into a 1 x 1 cm square, and aluminum pins with epoxy adhesive were attached to the cut wafers using a special tool. The aluminum pins were then attached to the substrate by heating at 150°C for 1 hour in an oven. After cooling to room temperature, the initial adhesion was evaluated by resistance using a thin film adhesion strength measuring device (Sebastian Five-A).

[0151] Figure 2 shows an explanatory diagram of the adhesion measurement method. In Figure 2, 8 is the silicon wafer (substrate), 9 is the cured film, 10 is an aluminum pin with adhesive, 11 is the support base, 12 is the grip, and 13 indicates the tensile direction. The adhesion strength is the average value of 12 measurements, and the higher the value, the stronger the adhesion of the adhesive film to the substrate. The adhesion was evaluated by comparing the obtained values. The results are shown in Table 3.

[0152] [Table 3]

[0153] As shown in Table 3, Examples 2-1 to 2-14 using the adhesive film-forming material of the present invention (AL-1 to 14) have a structure similar to that of Comparative Examples 2-1 to 2-14, which have a structure having one hydroxyl group and a structure represented by the general formula (1) above. - It can be seen that the adhesion is superior to that of Comparative Example 2-5. It can also be seen that Comparative Example 2-8, which uses Comparative Example AL-8, which has a small amount of the structural unit represented by the general formula (1), does not exhibit sufficient adhesion. It can also be seen from the results of Comparative Examples 2-6 and 2-7, which use Comparative Examples AL-6 and 7, that the structural unit represented by the general formula (2) also contributes to improving adhesion. Furthermore, Comparative Example AL-9 uses a crosslinking agent, so the curing method is different, but it can be seen that the adhesion is low despite the large number of hydroxyl groups contained in the polymer. From these results, it can be seen that the structural units represented by the general formulas (1) and (2) of the present invention can be effectively used to improve adhesion by combining them in an appropriate ratio.

[0154] Example 3 Pattern formation test (Examples 3-1 to 3-14, Comparative Examples 3-1 to 3-7) On a silicon wafer substrate, spin-on carbon ODL-301 (carbon content 88% by mass) manufactured by Shin-Etsu Chemical Co., Ltd. was applied and baked at 350°C for 60 seconds to form a resist underlayer film with a thickness of 200 nm. A CVD-SiON hard mask intermediate film was formed thereon, and the above-mentioned adhesion film forming materials (AL-1 to 14, Comparative AL-1 to 5, 8, 9) were further applied and baked at 220°C for 60 seconds to form an adhesion film with a thickness of 20 nm, and a single layer resist for ArF of the resist upper layer film material was applied thereon and baked at 105°C for 60 seconds to form a resist upper layer film with a thickness of 100 nm. An immersion protective film material (TC-1) was applied on the resist upper layer film and baked at 90°C for 60 seconds to form a protective film with a thickness of 50 nm. As for Comparative AL-6 and 7, as in the results of Example 1, the solvent resistance could not be ensured, so the resist upper layer film could not be applied, and therefore the pattern formation test could not be performed.

[0155] The resist top layer material (ArF single layer resist) was prepared by dissolving a polymer (PRP-A1), an acid generator (PAG1), and a basic compound (Amine1) in a solvent containing 0.1 mass% FC-430 (Sumitomo 3M Limited) in the proportions shown in Table 4 and filtering the solution through a 0.1 μm fluororesin filter.

[0156] [Table 4]

[0157] Resist polymer: PRP-A1 Molecular weight (Mw)=7,800 Dispersity (Mw / Mn)=1.88 [ka]

[0158] Acid generator: PAG1 [ka]

[0159] Basic compound: Amine1 [ka]

[0160] The immersion protective film material (TC-1) was prepared by dissolving the protective film polymer (PP1) in an organic solvent in the ratio shown in Table 5, and filtering the solution through a 0.1 μm fluorine resin filter.

[0161] [Table 5]

[0162] Protective film polymer: PP1 Molecular weight (Mw)=8,800 Dispersity (Mw / Mn)=1.69 [ka]

[0163] Next, the pattern was exposed using an ArF immersion exposure tool (Nikon Corporation; NSR-S610C, NA 1.30, σ 0.98 / 0.65, 35-degree dipole s-polarized illumination, 6% halftone phase shift mask), baked at 100°C for 60 seconds (PEB), and developed with a 2.38% by mass tetramethylammonium hydroxide (TMAH) aqueous solution for 30 seconds to obtain a 40 nm 1:1 line and space pattern. The cross-sectional shape and pattern roughness of this pattern were observed using an electron microscope. In addition, the minimum dimension at which the lines could be resolved without collapsing when the line dimensions were narrowed by increasing the exposure dose was determined, and this was taken as the collapse limit (nm). The smaller the value, the higher the collapse resistance, which is preferable.

[0164] The cross-sectional shape of the obtained pattern was evaluated using an electron microscope (S-4700) manufactured by Hitachi, Ltd., and the pattern roughness was evaluated using an electron microscope (CG4000) manufactured by Hitachi High-Technologies Corp. The results are shown in Table 6.

[0165] [Table 6]

[0166] As shown in Table 6, Examples 3-1 to 3-14 using the adhesion film-forming material of the present invention (AL-1 to 14) show superior collapse suppression performance compared to Comparative Examples 3-1 to 3-7, and it is understood that finer pattern formation is possible. Furthermore, it is understood that by appropriately adjusting the photoacid generator as in Examples 3-9 to 3-14, pattern roughness can be improved more than Examples 3-1, 2, 4, and 6 to 8 that do not contain a photoacid generator. On the other hand, Comparative Examples 3-1 to 3-7, which do not contain a sufficient amount of the structural unit contained in the adhesion film-forming material of the present invention and have low adhesion, show low pattern collapse suppression performance, and in Comparative Example 3-7, which is cured only by the action of a crosslinking agent by adding a crosslinking agent unlike the present invention, deterioration of the cross-sectional shape of the pattern was also observed.

[0167] From the above, the adhesion film forming material of the present invention has high adhesion to the resist overlying film and has the effect of preventing the collapse of a fine pattern, and is therefore extremely useful as an adhesion film material for use in a multilayer resist method. Furthermore, the pattern forming method of the present invention using this material makes it possible to form a fine pattern on a substrate to be processed with high precision.

[0168] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0169] 1...substrate, 2...processed layer, 2a...pattern (pattern formed on the processed layer), 3...resist underlayer film, 3a...resist underlayer film pattern, 4...silicon-containing intermediate film, 4a...silicon-containing intermediate film pattern, 5...adhesive film, 5a...adhesive film pattern, 6: resist upper layer film; 6a: resist upper layer film pattern; 7: exposed portion; 8...silicon wafer; 9...hardened film; 10...aluminum pin with adhesive; 11...support base; 12...grip; 13...pulling direction.

Claims

1. An adhesion film forming material for an adhesion film formed between a silicon-containing intermediate film and a resist top layer film, (A) a resin having structural units represented by the following general formula (3) and the following general formula (2): (B) a thermal acid generator; and (C) Organic solvent and An adhesion film-forming material, characterized in that in the component (A), the molar fraction of the structural unit represented by the following general formula (3) is 5% or more, and the molar fraction of the structural unit represented by the following general formula (2) is 30% or more. 【Chemistry 1】 (In the formula, R 1 is a hydrogen atom or a methyl group, R 2 is a hydrogen atom or a linear or branched alkyl group having 1 to 3 carbon atoms, L 2 is a single bond or an alkylene group having 1 to 2 carbon atoms, and a hydrogen atom of the alkylene group may be substituted with a hydroxyl group, and a methylene group constituting the alkylene group may be substituted with a carbonyl group.) 【Chemistry 2】 (In the formula, R 3 is a hydrogen atom or a methyl group, R 4 is a group selected from the following formulas (2-1) to (2-3). 【Chemistry 3】 (In the above formula, the dashed lines represent bonds.)

2. 2. The adhesion film forming material according to claim 1, wherein the silicon-containing intermediate film is a silicon-containing resist intermediate film or an inorganic hard mask intermediate film.

3. 3. The adhesive film forming material according to claim 1, further comprising one or more compounds represented by the following general formula (4) as a photoacid generator (D): 【Chemistry 4】 (In the formula, R 5 , R 6 and R 7 each independently represents a linear alkyl or alkenyl group having 1 to 10 carbon atoms, which may be substituted with a heteroatom or may have a heteroatom interposed therebetween, or a branched or cyclic alkyl or alkenyl group having 3 to 10 carbon atoms, which may be substituted with a heteroatom or may have a heteroatom interposed therebetween, or an aryl or aralkyl group having 6 to 21 carbon atoms, which may be substituted with a heteroatom or may have a heteroatom interposed therebetween. 5 , R 6 and R 7 Any two of may be bonded to each other to form a ring together with the sulfur atom in the formula. - represents either the following general formula (5) or the following general formula (6). 【Chemistry 5】 【Chemistry 6】 (In the formula, R 8 and R 9 are mutually independent and represent a monovalent hydrocarbon group containing an aliphatic ring structure having 3 to 40 carbon atoms which may be substituted with or may be interrupted by a heteroatom.

4. 4. The adhesive film forming material according to claim 3, wherein the general formula (5) is represented by the following general formula (7): 【Chemistry 7】 (In the formula, R 10 R represents a hydrogen atom or a trifluoromethyl group. 11 represents a monovalent hydrocarbon group containing an aliphatic ring structure having 3 to 35 carbon atoms, which may be substituted with a heteroatom or may be interrupted by a heteroatom.

5. 5. The adhesive film forming material according to claim 1, wherein the weight average molecular weight of the resin (A) is 1,000 to 30,000.

6. The adhesion film forming material according to any one of claims 1 to 5, further comprising at least one selected from the group consisting of (E) a surfactant, (F) a crosslinking agent, (G) a plasticizer, and (H) a dye.

7. A method for forming a pattern on a workpiece substrate, comprising the steps of: (I-1) forming a resist underlayer film on the substrate; (I-2) forming a silicon-containing resist intermediate film on the resist underlayer film; (I-3) a step of applying an adhesion film-forming material onto the silicon-containing resist intermediate film, followed by heat treatment to form an adhesion film; (I-4) forming a resist top layer film on the adhesion film using a photoresist material; (I-5) a step of forming a pattern on the resist upper layer film by pattern-exposing the resist upper layer film and then developing the resist upper layer film with a developer; (I-6) a step of transferring the pattern to the adhesion film by dry etching using the resist upper layer film on which the pattern has been formed as a mask; (I-7) a step of transferring the pattern to the silicon-containing resist intermediate film by dry etching using the adhesion film on which the pattern has been formed as a mask; (I-8) a step of transferring a pattern to the resist underlayer film by dry etching using the silicon-containing resist intermediate film to which the pattern has been transferred as a mask; and (I-9) a step of transferring the pattern to the substrate by dry etching using the resist underlayer film to which the pattern has been transferred as a mask; A pattern forming method comprising the steps of: The adhesion film forming material is (A) a resin having structural units represented by the following general formula (1) and the following general formula (2), (B) a thermal acid generator; and (C) Organic solvent and A method for forming a pattern, wherein in the component (A), a molar fraction of a structural unit represented by the following general formula (1) is 5% or more, and a molar fraction of a structural unit represented by the following general formula (2) is 30% or more: 【Chemistry 8】 (In the formula, R 1 is a hydrogen atom or a methyl group, L 1 is a single bond, a divalent organic group containing -C(=O)O-, or a divalent organic group containing -C(=O)NR 2 -. R 2 is a hydrogen atom, or a linear or branched alkyl group having 1 to 3 carbon atoms.) 【Chemistry 9】 (In the formula, R 3 is a hydrogen atom or a methyl group, and R 4 is a group selected from the following formulae (2-1) to (2-3).) 【Chemistry 10】 (In the above formula, the dashed lines represent bonds.)

8. A method for forming a pattern on a workpiece substrate, comprising the steps of: (II-1) forming a resist underlayer film on the substrate; (II-2) forming an inorganic hard mask intermediate film selected from a silicon oxide film, a silicon nitride film, and a silicon oxynitride film on the resist underlayer film; (II-3) A step of forming an adhesion film by applying an adhesion film forming material onto the inorganic hard mask intermediate film and then heat-treating the material; (II-4) forming a resist top layer film on the adhesion film using a photoresist material; (II-5) a step of forming a pattern on the resist upper layer film by pattern-exposing the resist upper layer film and then developing the resist upper layer film with a developer; (II-6) A step of transferring the pattern to the adhesion film by dry etching using the resist upper layer film on which the pattern is formed as a mask; (II-7) A step of transferring the pattern to the inorganic hard mask intermediate film by dry etching using the adhesion film on which the pattern is formed as a mask; (II-8) A step of transferring a pattern to the resist underlayer film by dry etching using the inorganic hard mask intermediate film to which the pattern has been transferred as a mask; and (II-9) a step of transferring the pattern to the substrate by dry etching using the resist underlayer film to which the pattern has been transferred as a mask; A pattern forming method comprising the steps of: The adhesion film forming material is (A) a resin having structural units represented by the following general formula (1) and the following general formula (2), (B) a thermal acid generator; and (C) Organic solvent and A method for forming a pattern, wherein in the component (A), a molar fraction of a structural unit represented by the following general formula (1) is 5% or more, and a molar fraction of a structural unit represented by the following general formula (2) is 30% or more: 【Chemistry 11】 (In the formula, R 1 is a hydrogen atom or a methyl group, L 1 is a single bond, a divalent organic group containing -C(=O)O-, or a divalent organic group containing -C(=O)NR 2 -. R 2 is a hydrogen atom, or a linear or branched alkyl group having 1 to 3 carbon atoms.) 【Chemistry 12】 (In the formula, R 3 is a hydrogen atom or a methyl group, and R 4 is a group selected from the following formulae (2-1) to (2-3).) 【Chemistry 13】 (In the above formula, the dashed lines represent bonds.)

9. 9. The pattern forming method according to claim 8, wherein the inorganic hard mask intermediate film is formed by a CVD method or an ALD method.

10. 10. The method for forming a pattern according to claim 7, wherein a method for forming a circuit pattern on the resist upper layer film is performed by using photolithography having a wavelength of 10 nm or more and 300 nm or less, direct writing using an electron beam, nanoimprinting, or a combination thereof.

11. 11. The method for forming a pattern according to claim 7, wherein the development is carried out using an alkali development or an organic solvent.

12. 12. The pattern forming method according to claim 7, wherein the workpiece substrate is a semiconductor device substrate, or a semiconductor device substrate having any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film formed thereon.

13. 13. The pattern formation method according to claim 12, wherein the metal is silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.

14. A method for forming an adhesion film that functions as an adhesion layer used in a manufacturing process of a semiconductor device, comprising spin-coating an adhesion film-forming material according to any one of claims 1 to 6 on a substrate to be processed, and heat-treating the substrate coated with the adhesion film-forming material at a temperature of 100°C or higher and 300°C or lower for 10 to 600 seconds to form a hardened film.

15. A method for forming an adhesion film that functions as an adhesion layer used in the manufacturing process of a semiconductor device, comprising spin-coating an adhesion film-forming material according to any one of claims 1 to 6 onto a substrate to be processed, and heat-treating the substrate coated with the adhesion film-forming material in an atmosphere having an oxygen concentration of 0.1% or more and 21% or less to form a hardened film.

16. A method for forming an adhesion film that functions as an adhesion layer used in the manufacturing process of a semiconductor device, comprising spin-coating an adhesion film-forming material according to any one of claims 1 to 6 onto a substrate to be processed, and heat-treating the substrate coated with the adhesion film-forming material in an atmosphere with an oxygen concentration of less than 0.1%, thereby forming a hardened film.

Citation Information

Patent Citations

  • Tape end detecting circuit of magnetic recorder and reproducer

    JP1982008938A

  • Monomer, polymer compound, resist material and pattern formation method

    JP2016117878A

  • Coating composition for use with overcoated photoresist

    JP2017107185A

  • Coating-type composition for forming organic film, patterning process, polymer, and method for manufacturing polymer

    JP2021138851A

  • Composition for forming antireflective film for use in lithography

    WO2003017002A1