Rare earth sintered neodymium-iron-boron magnets, their manufacturing method and use of praseodymium hydride
The use of praseodymium hydride in the jet milling process for neodymium-iron-boron magnets addresses the imbalance between coercive force and residual magnetic flux density, achieving cost-effective high-performance magnets without heavy rare earths.
Patent Information
- Application Number
- JP2022189055
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-11-30
- Filing Date
- 2022-11-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-11-28
AI Technical Summary
Existing methods for manufacturing neodymium-iron-boron magnets struggle to balance coercive force and residual magnetic flux density, often requiring heavy rare earth elements that increase costs and degrade performance.
A manufacturing method for rare earth sintered neodymium-iron-boron magnets that uses praseodymium hydride in the jet milling process to create a gradient distribution of praseodymium concentration and controlled grain boundary phase thickness, eliminating heavy rare earths and optimizing magnetic properties.
The method achieves a balanced coercive force and residual magnetic flux density with low temperature coefficients, reducing costs by avoiding heavy rare earths and maintaining high magnetic performance.
Smart Images

Figure 0007586881000005 
Figure 0007586881000001 
Figure 0007586881000002
Abstract
Description
[Technical field]
[0001] The present invention provides rare earth sintered neodymium-iron-boron magnets, their manufacturing methods, and uses of praseodymium hydride. [Background technology]
[0002] With the increasing demand for hybrid cars, electric cars and energy-saving air conditioner compressors, the demand for permanent magnet materials with high coercivity and low temperature coefficient is also increasing. The use of large amounts of heavy rare earth elements can improve the coercivity and temperature coefficient of permanent magnet materials. However, this brings about a significant increase in cost and some sacrifices in remanence and magnetic energy product. The atomic composition of each element is Nd 14.1 Co 1.34 Cu 0.04 Fe bal B 5.84 The alloy sheet was then hydrogen-pulverized into coarse powder with a particle size of 10 to 100 μm, and the coarse powder was then jet-milled in a nitrogen atmosphere to produce fine powder with an average particle size of 3.38 μm. y H x The powder is mixed with fine powder, isostatically pressed under a magnetic field of 1800 kA / m and 300 MPa, and the green body is sintered at 1040-1060 °C for 2 h under vacuum conditions, then gas-cooled and quenched, and then tempered at 900 °C and 500 °C for 2 h, respectively. This method requires the use of heavy rare earth Dy, and D y H x The powder is directly mixed with the fine powder. This method can greatly improve the coercive force of the magnet, but the residual magnetic flux density is reduced too much, resulting in an imbalance between the coercive force and the residual magnetic flux density.
[0003] The temperature coefficient of a magnet can be improved by adding Co and Ni elements, but excessive addition of Co and Ni elements leads to a decrease in magnet performance, and Co and Ni elements are strategic elements and are relatively expensive. CN111696742A contains anisotropic magnet materials (Nd, Pr) x Fe (100-x-y-z) B y M z , auxiliary phase material Pra Ni 100-b A method for producing a high-performance neodymium-iron-boron permanent magnet material without heavy rare earth elements is disclosed, in which a main alloy powder and a rare earth cobalt compound powder are directly mixed and then molded to obtain a high-performance neodymium-iron-boron material without heavy rare earth elements. CN104575899A discloses a method for producing a sintered neodymium-iron-boron magnet in which the main alloy powder and the rare earth cobalt compound powder are directly mixed and then molded to increase the average thickness of the grain boundary phase of the obtained magnet. These methods can improve the coercive force of the magnet, but cannot suppress the decrease in remanence, and cannot balance the coercive force and remanence well. Summary of the Invention
[0004] In one aspect, the present invention provides a (R1, R2)-TBM rare earth sintered neodymium-iron-boron magnet that achieves a good balance between the coercivity and remanence of the rare earth sintered neodymium-iron-boron magnet. Furthermore, the rare earth sintered neodymium-iron-boron magnet of the present invention has a low temperature coefficient of remanence and a low temperature coefficient of coercivity.
[0005] In another aspect, the present invention provides a method for producing (R1, R2)-TBM rare earth sintered NdFeB magnets, which, unlike conventional methods, suppresses the loss of remanence, thereby achieving a good balance between the coercivity and remanence of the rare earth sintered NdFeB magnets.
[0006] In another embodiment, the present invention provides the use of praseodymium hydride.
[0007] In one embodiment, the present invention is a (R1,R2)-TBM rare earth sintered neodymium-iron-boron magnet, comprising: The rare earth sintered neodymium-iron-boron magnet is composed of a sintered body containing main phase crystal grains and a grain boundary phase, The main phase grains are (R1, R2)2T14 B phase, a Pr concentration C1 at an edge of the main phase crystal grain is higher than a Pr concentration C2 at a center of the main phase crystal grain, The R1 concentration of the grain boundary phase is higher than the R1 concentration of the main phase crystal grains, and the average thickness of the grain boundary phase is 20 to 60 nm; R1 is one or more elements selected from Nd and Gd, and Nd accounts for 50 at% or more of the total number of atoms in R1; R2 is the Pr element, T is one or more elements selected from Fe, Co, and Ni, and Co and Ni account for 3 at% or less of the total number of atoms of T; B is the element boron, The present invention provides an (R1,R2)-TBM rare earth sintered neodymium-iron-boron magnet, in which M is one or more elements selected from Al, Cu, Ga, Zn, Bi, Zr, Ti, Nb, V, Mo, and W, and the total number of M atoms is 5 at% or less of the sintered body.
[0008] In the rare earth sintered neodymium-iron-boron magnet according to the present invention, the Pr concentration preferably decreases gradually from the edge of the main phase crystal grain toward the center of the main phase crystal grain.
[0009] In the rare earth sintered neodymium-iron-boron magnet according to the present invention, the Pr concentration C1 at the edge of the main phase crystal grain is preferably 0.25 wt% or more higher than the Pr concentration C2 at the center of the main phase crystal grain.
[0010] In the rare earth sintered neodymium-iron-boron magnet of the present invention, the composition of the sintered body preferably is R1: 28-31 wt%, R2: 0.1-5 wt%, B: 0.6-1.6 wt%, Co: 0.1-3.9 wt%, Cu: 0.05-1.0 wt%, Zr: 0.06-0.25 wt%, Ga: 0.1-0.3 wt%, and the remainder essentially Fe.
[0011] In the rare earth sintered neodymium-iron-boron magnet according to the present invention, the Zr content in the sintered body is preferably 0.1 to 0.16 wt %, and the Ga content is preferably 0.15 to 0.25 wt %.
[0012] The rare earth sintered neodymium-iron-boron magnet according to the present invention preferably does not contain any heavy rare earth elements.
[0013] The rare earth sintered neodymium-iron-boron magnet of the present invention preferably has a residual magnetic flux density of 14.50 kGs or more, an intrinsic coercivity of 14.0 kOe or more, a temperature coefficient of residual magnetic flux density in the range of 20 to 150°C of less than 0.113% / °C, and a temperature coefficient of coercivity in the range of 20 to 150°C of less than 0.573% / °C.
[0014] In another embodiment, the present invention provides a method for producing a composition comprising: (a) A process for obtaining a master alloy sheet by melting R1, T, B and M, which are the raw materials for rare earth sintered neodymium-iron-boron magnets; (b) crushing the master alloy sheet into coarse alloy powder having an average particle size D50 of 20-500 μm; (c) pulverizing the coarse alloy powder with a praseodymium-containing powder by jet milling to obtain a magnetic powder having an average particle size D50 of 1 to 10 μm, the praseodymium-containing powder being a praseodymium hydride or Pr-M alloy powder; (d) pressing the magnetic powder in a magnetic field and subjecting it to hydrostatic isostatic pressing to obtain a green body; (e) subjecting the green body to a vacuum heat treatment and two-stage tempering to obtain a rare earth sintered permanent magnet; The present invention also provides a method for producing the rare earth sintered neodymium-iron-boron magnet, comprising the steps of:
[0015] According to the production method of the present invention, the amount of the praseodymium-containing powder used is preferably 0.1 to 5.0 wt % based on the mass of the coarse alloy powder.
[0016] In another aspect, the present invention relates to a use of praseodymium hydride for improving the balance factor between the residual magnetic flux density and the coercive force of a rare earth sintered neodymium-iron-boron magnet, comprising: pulverizing a coarse alloy powder with praseodymium hydride powder into a magnetic powder by jet milling; and the amount of the praseodymium hydride powder used is 0.1-5.0 wt% based on the mass of the coarse alloy powder; The composition of the alloy coarse powder is R1-TBM, R1 is one or more elements selected from Nd and Gd, and Nd accounts for 50 at% or more of the total number of atoms in R1; T is one or more elements selected from Fe, Co, and Ni, and Co and Ni account for 3 at% or less of the total number of atoms of T; B is the element boron, M is one or more elements selected from Al, Cu, Ga, Zn, Bi, Zr, Ti, Nb, V, Mo and W, and the total number of M atoms is 5 at % or less of the sintered body; The balance coefficient E between the residual magnetic flux density and the coercive force is calculated as follows: E=X2 / X1 X1 = (Br1-Br2) / Br1 X2=(Hcj2-Hcj1) / Hcj1 (Br1 represents the residual magnetic flux density of a rare earth sintered neodymium-iron-boron magnet obtained without adding praseodymium hydride powder in the jet milling process, and is expressed in kGs. Br2 represents the residual magnetic flux density of the rare earth sintered neodymium-iron-boron magnet obtained by adding praseodymium hydride powder in the jet milling process, and is expressed in kGs. Hcj1 represents the coercivity of the rare earth sintered neodymium-iron-boron magnet obtained without adding praseodymium hydride powder in the jet milling process, and is expressed in kOe. Hcj2 represents the coercive force of the rare earth sintered neodymium-iron-boron magnet obtained by adding praseodymium hydride powder in the jet milling process, and is expressed in kOe. The use of praseodymium hydride to improve the balance factor between remanence and coercivity in rare earth sintered neodymium-iron-boron magnets is provided.
[0017] The rare earth sintered neodymium-iron-boron magnet of the present invention has a relatively high coercivity and residual magnetic flux density, achieving a good balance between the two, and further has a relatively low temperature coefficient of residual magnetic flux density and temperature coefficient of coercivity. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a scanning electron microscope photograph of the rare earth sintered neodymium-iron-boron magnet obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will be described in more detail below, but the present invention is not limited thereto.
[0020] In the present invention, the residual magnetic flux density means the numerical value of the magnetic flux density corresponding to the zero magnetic field strength at the saturation magnetic hysteresis line, and is usually expressed as Br or Mr, and its unit is Tesla (T) or Gauss (Gs). 1Gs=0.0001T.
[0021] In the present invention, coercivity, also called intrinsic coercivity, refers to the magnetic field strength when the magnetic field is monotonically decreased from the saturation magnetization state of a magnet to zero, then increased in the reverse direction, and the magnetization strength is decreased to zero along the saturation magnetic hysteresis line, and is usually expressed as Hcj, with the unit being Oersted (Oe) or Angles per meter (A / m). 1 Oe=79.6 A / m. Hcj is the intrinsic coercivity at room temperature.
[0022] In the present invention, the inert gas includes helium gas, neon gas, argon gas, krypton gas, xenon gas, etc. Vacuum refers to the degree of absolute vacuum, and the smaller the value, the higher the degree of vacuum.
[0023] In the present invention, the average particle size D50 refers to the equivalent diameter of the maximum particle when the cumulative distribution in the particle size distribution curve is 50%.
[0024] In the present invention, "at %" refers to atomic percentage.
[0025] The object of the present invention is to achieve a good balance between the residual magnetic flux density and the coercive force of a magnet. The formula for calculating the balance coefficient E between the residual magnetic flux density and the coercive force is as follows:
[0026] E=X2 / X1 X1 = (Br1-Br2) / Br1 X2=(Hcj2-Hcj1) / Hcj1 Br1 represents the remanence, in kGs, of a rare earth sintered neodymium-iron-boron magnet obtained without the addition of modifier powder. In some embodiments, Br1 represents the remanence, in kGs, of a rare earth sintered neodymium-iron-boron magnet obtained without the addition of praseodymium hydride powder in the jet milling process.
[0027] Br2 represents the remanence, in kGs, of the rare earth sintered neodymium-iron-boron magnet obtained by adding the modified powder. In some embodiments, Br2 represents the remanence, in kGs, of the rare earth sintered neodymium-iron-boron magnet obtained by adding the praseodymium hydride powder to the jet milling process.
[0028] Hcj1 represents the coercivity of the rare earth sintered neodymium-iron-boron magnet obtained without adding any modifier powder, in kOe. In some embodiments, Hcj1 represents the coercivity of the rare earth sintered neodymium-iron-boron magnet obtained without adding any additive praseodymium hydride powder to the jet milling process, in kOe.
[0029] Hcj2 represents the coercivity of the rare earth sintered neodymium-iron-boron magnet obtained by adding the modified powder, in kOe. In some embodiments, Hcj2 represents the coercivity of the rare earth sintered neodymium-iron-boron magnet obtained by adding the praseodymium hydride powder to the jet milling process, in kOe.
[0030] In the present invention, it has been found that by adding a praseodymium-containing powder to the jet milling process in which the coarse alloy powder is pulverized into fine magnetic powder, the thickness of the grain boundary phase of the resulting magnet can be maintained within a certain range, and the praseodymium exhibits a gradient distribution in the main phase particles, thereby achieving a good balance between the residual magnetic flux density and the coercive force of the magnet. Based on this, the present invention is completed.
[0031] <Rare earth sintered neodymium-iron-boron magnet> The rare earth sintered neodymium-iron-boron magnet according to the present invention has the elemental composition shown in the following formula. (R1,R2)-TBM
[0032] The rare earth sintered neodymium-iron-boron magnet is composed of a sintered body containing main phase crystal grains and grain boundary phase. In some embodiments, the rare earth sintered neodymium-iron-boron magnet is synonymous with the sintered body.
[0033] R1 is one or more selected from Nd and Gd elements. Nd is 50 at% or more of the total number of R1 atoms, preferably, Nd is 80 at% or more of the total number of R1 atoms, more preferably, Nd is 95 at% or more of the total number of R1 atoms. According to one embodiment of the present invention, R1 is Nd.
[0034] R2 is the element Pr.
[0035] T is one or more elements selected from Fe, Co, and Ni. Co and Ni account for 3 at% or less of the total number of atoms of T, preferably Co and Ni account for 2 at% or less of the total number of atoms of T, and more preferably Co and Ni account for 1 to 1.5 at% of the total number of atoms of T. According to one embodiment of the present invention, T is Fe and Co.
[0036] B is elemental boron.
[0037] M is one or more elements selected from Al, Cu, Ga, Zn, Bi, Zr, Ti, Nb, V, Mo, and W. Preferably, M is Cu, Zr, or Ga. The total atomic number of M is 5 at% or less of the sintered body, preferably 4 at% or less, more preferably 3 at% or less, and most preferably 0.1 to 2 at%. According to one embodiment of the present invention, the total atomic number of M is 0.3 to 1 at% of the sintered body.
[0038] The rare earth sintered neodymium-iron-boron magnet according to the present invention has a main phase crystal grain with a (R1, R2)2T 14 The present inventors have found that the Pr concentration C1 at the edge of the main phase crystal grain is higher than the Pr concentration C2 at the center of the main phase crystal grain. The Pr concentration C1 at the edge of the main phase crystal grain is higher than the Pr concentration C2 at the center of the main phase crystal grain by 0.25 wt% or more. Preferably, the Pr concentration C1 at the edge of the main phase crystal grain is higher than the Pr concentration C2 at the center of the main phase crystal grain by 0.40 wt% or more, and more preferably, the Pr concentration C1 at the edge of the main phase crystal grain is higher than the Pr concentration C2 at the center of the main phase crystal grain by 0.50 wt% or more. In some embodiments, the concentration difference (C1-C2) between the Pr concentration C1 at the edge of the main phase crystal grain and the Pr concentration C2 at the center of the main phase crystal grain is in the range of 0.25 to 0.70 wt%, preferably in the range of 0.40 to 0.70 wt%, and more preferably in the range of 0.45 to 0.65 wt%. According to one embodiment of the present invention, the concentration difference (C1-C2) between the Pr concentration C1 at the edge of a main phase crystal grain and the Pr concentration C2 at the center of the main phase crystal grain is 0.53 to 0.57 wt%. If the Pr concentration difference is too small, it is disadvantageous for improving the coercivity, while if the Pr concentration difference is too large, it has a negative effect on the remanence, the temperature coefficient of remanence, and the temperature coefficient of coercivity. A Pr concentration difference in the above range is advantageous for achieving a good balance between the coercivity and remanence of the magnet.
[0039] According to one embodiment of the present invention, the Pr concentration gradually decreases from the edge of the main phase crystal grain to the center of the main phase crystal grain. Therefore, the Pr concentration shows a gradient distribution. This further ensures a good balance between the coercivity and the residual magnetic flux density of the magnet.
[0040] The R1 concentration A1 of the grain boundary phase is higher than the R1 concentration A2 of the main phase crystal grains. The average thickness L of the grain boundary phase is 20 to 60 nm, preferably 20 to 40 nm, and more preferably 22 to 27 nm. If the thickness of the grain boundary phase is too small, the coercivity of the magnet cannot be significantly improved, and if the thickness of the grain boundary phase is too large, the remanence decreases significantly and the temperature coefficient of remanence and the temperature coefficient of coercivity increase significantly. A grain boundary phase thickness in the above range is advantageous for achieving a good balance between the coercivity and remanence of the magnet.
[0041] The sintered body according to the present invention includes elements such as R1, R2, B, Co, Cu, Zr, Ga, and Fe. In some embodiments, the sintered body according to the present invention consists of R1, R2, B, Co, Cu, Zr, Ga, and Fe.
[0042] Based on the mass of the sintered body, the content of R1 may be 28 to 31 wt%, preferably 28 to 30 wt%, and more preferably 28 to 29 wt%.
[0043] Based on the mass of the sintered body, the content of R2 may be 0.1 to 5 wt%, preferably 1.0 to 3 wt%, more preferably 1.5 to 2.5 wt%, and most preferably 1.7 to 2.0 wt%.
[0044] Based on the mass of the sintered body, the B content may be 0.6 to 1.6 wt%, preferably 0.7 to 1.3 wt%, and more preferably 0.9 to 1.0 wt%.
[0045] Based on the mass of the sintered body, the Co content may be 0.1 to 3.9 wt%, preferably 0.7 to 1.3 wt%, and more preferably 0.9 to 1.0 wt%.
[0046] Based on the mass of the sintered body, the Cu content may be 0.05 to 1.0 wt%, preferably 0.10 to 0.70 wt%, and more preferably 0.12 to 0.20 wt%.
[0047] Based on the mass of the sintered body, the Zr content may be 0.06 to 0.25 wt%, preferably 0.1 to 0.16 wt%, and more preferably 0.13 to 0.15 wt%.
[0048] Based on the mass of the sintered body, the Ga content may be 0.1 to 0.3 wt%, preferably 0.15 to 0.25 wt%, and more preferably 0.18 to 0.20 wt%.
[0049] The balance is Fe.
[0050] Controlling each element within the above range is advantageous in obtaining a rare earth sintered neodymium-iron-boron magnet that achieves a good balance between coercive force and residual magnetic flux density.
[0051] According to one embodiment of the present invention, the rare earth sintered neodymium-iron-boron magnet of the present invention does not contain heavy rare earth elements. The heavy rare earth elements are terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), rubidium (Tm), ytterbium (Yb) and rubidium (Lu). This can reduce the cost and better ensure a good balance between coercivity and residual magnetic flux density.
[0052] The rare earth sintered neodymium-iron-boron magnet according to the present invention has a residual magnetic flux density of 14.50 kGs or more, preferably 14.60 kGs or more, and more preferably 14.65 kGs or more. The residual magnetic flux density may be less than 16.1 kGs, preferably less than 15.8 kGs, and more preferably 15.5 kGs. The intrinsic coercivity is 14.0 kOe or more, preferably 16.3 kOe or more, and more preferably 16.5 kOe or more. The intrinsic coercivity may be less than 29 kOe, preferably less than 25 kOe, and more preferably less than 19 kOe. The residual magnetic flux density temperature coefficient within the temperature range of 20 to 150°C is less than 0.113% / °C, preferably less than 0.110% / °C, and more preferably less than 0.109% / °C. The temperature coefficient of remanence may exceed 0, preferably exceeds 0.05% / °C, more preferably exceeds 0.08% / °C. The temperature coefficient of coercivity within the range of 20 to 150°C is less than 0.573% / °C, preferably less than 0.570% / °C, more preferably less than 0.565% / °C. The temperature coefficient of coercivity exceeds 0, preferably exceeds 0.1% / °C, more preferably exceeds 0.3% / °C.
[0053] The rare earth sintered neodymium-iron-boron magnet according to the present invention may have a balance factor E between remanence and coercivity of 25 or more, preferably 35 or more, and more preferably 39 or more. The balance factor E may be 150 or less, preferably 100 or less, and more preferably 80 or less. The definition of the balance factor E is as described above.
[0054] <Manufacturing method for rare earth sintered neodymium-iron-boron magnets> The method for producing a rare earth sintered neodymium-iron-boron magnet according to the present invention includes (a) a melting step, (b) a crushing step, (c) a jet milling step, (d) a molding step, and (e) a sintering and aging treatment step, which are described in detail below.
[0055] Melting process A mother alloy sheet is obtained by melting a raw material of a rare earth sintered neodymium-iron-boron magnet containing R1, T, B and M. Preferably, the raw material of the rare earth sintered neodymium-iron-boron magnet is composed of R1, T, B and M. R1 is one or more selected from Nd and Gd elements. Nd is 50 at% or more of the total number of atoms of R1, preferably Nd is 80 at% or more of the total number of atoms of R1, and more preferably Nd is 95 at% or more of the total number of atoms of R1. According to one embodiment of the present invention, R1 is Nd. T is one or more selected from Fe, Co and Ni elements. Co and Ni are 3 at% or less of the total number of atoms of T, preferably Co and Ni are 2 at% or less of the total number of atoms of T, and more preferably Co and Ni are 1 to 1.5 at% of the total number of atoms of T. According to one embodiment of the present invention, T is Fe and Co. B is a boron element. M is one or more elements selected from Al, Cu, Ga, Zn, Bi, Zr, Ti, Nb, V, Mo, and W. Preferably, M is Cu, Zr, or Ga. The total atomic number of M is 5 at% or less of the raw material, preferably 4 at% or less, more preferably 3 at% or less, and most preferably 0.1 to 2 at%. According to one embodiment of the present invention, the total atomic number of M is 0.3 to 1 at% of the raw material.
[0056] The raw material of the rare earth sintered neodymium-iron-boron magnet according to the present invention includes elements such as R1, B, Co, Cu, Zr, Ga, and Fe. In some embodiments, the raw material of the rare earth sintered neodymium-iron-boron magnet according to the present invention is composed of R1, B, Co, Cu, Zr, Ga, and Fe. Based on the mass of the raw material of the rare earth sintered neodymium-iron-boron magnet, the content of R1 may be 28 to 31 wt%, preferably 28 to 30 wt%, and more preferably 28 to 29 wt%. The content of B may be 0.6 to 1.6 wt%, preferably 0.7 to 1.3 wt%, and more preferably 0.9 to 1.0 wt%. The content of Co may be 0.1 to 3.9 wt%, preferably 0.7 to 1.3 wt%, and more preferably 0.9 to 1.0 wt%. The Cu content may be 0.05 to 1.0 wt%, preferably 0.10 to 0.70 wt%, and more preferably 0.12 to 0.20 wt%. The Zr content may be 0.06 to 0.25 wt%, preferably 0.1 to 0.16 wt%, and more preferably 0.13 to 0.15 wt%. The Ga content may be 0.1 to 0.3 wt%, preferably 0.15 to 0.25 wt%, and more preferably 0.18 to 0.20 wt%, with the remainder being Fe. According to one embodiment of the present invention, the raw material for the rare earth sintered neodymium-iron-boron magnet of the present invention may not contain a heavy rare earth element. The heavy rare earth elements are terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), rubidium (Tm), ytterbium (Yb) and rubidium (Lu).
[0057] The raw materials are mixed according to the composition of the rare earth sintered neodymium-iron-boron magnet. In some embodiments, the raw materials consist of Nd, B, Co, Cu, Zr, Ga, and Fe. The Nd content may be 28-31 wt%, preferably 28-30 wt%, and more preferably 28-29 wt%. The B content may be 0.6-1.6 wt%, preferably 0.7-1.3 wt%, and more preferably 0.9-1.0 wt%. The Co content may be 0.1-3.9 wt%, preferably 0.7-1.3 wt%, and more preferably 0.9-1.0 wt%. The Cu content may be 0.05-1.0 wt%, preferably 0.10-0.70 wt%, and more preferably 0.12-0.20 wt%. The Zr content may be 0.06 to 0.25 wt%, preferably 0.1 to 0.16 wt%, and more preferably 0.13 to 0.15 wt%. The Ga content may be 0.1 to 0.3 wt%, preferably 0.15 to 0.25 wt%, and more preferably 0.18 to 0.20 wt%, and the remainder is Fe.
[0058] The melting may be carried out in a vacuum melting furnace. The average thickness of the obtained master alloy sheet may be 0.05 to 1.00 mm, preferably 0.1 to 0.8 mm, and more preferably 0.2 to 0.5 mm.
[0059] Crushing process The mother alloy sheet is crushed into coarse alloy powder. The average particle size D50 of the coarse alloy powder is 20 to 500 μm, preferably 50 to 300 μm, and more preferably 80 to 150 μm. The coarse alloy powder can be obtained by adopting a method called hydrogen crushing, for example, the mother alloy sheet may be subjected to hydrogen absorption and dehydrogenation treatment in a hydrogen crushing furnace to form coarse alloy powder.
[0060] Jet Milling Process In the traditional jet milling process, the coarse alloy powder is directly ground into fine alloy powder. In the present invention, the praseodymium-containing powder is added to the jet milling process to facilitate at least a portion of the fine alloy powder being coated with the praseodymium-containing powder. The coarse alloy powder and the praseodymium-containing powder are ground into magnetic powder by jet milling. The magnetic powder has an average particle size D50 of 1-10 μm, preferably 2-7 μm, and more preferably 3-5 μm.
[0061] The praseodymium-containing powder according to the present invention may be praseodymium hydride or Pr-M alloy powder. In the Pr-M alloy powder, M is one or more elements selected from Al, Cu, Ga, Zn, Bi, Zr, Ti, Nb, V, Mo and W. Preferably, M is Cu, Zr and Ga. The Pr-M alloy powder is not a Pr-Ni alloy powder or a Pr-Co alloy powder. These two types of alloy powders are expensive, but are not significantly effective in improving the balance between the residual magnetic flux density and the coercive force of the magnet, and are even inferior to the Pr-M alloy powder of the present invention.
[0062] According to one embodiment of the present invention, the praseodymium-containing powder is a praseodymium hydride powder. Such a powder is not only inexpensive and easy to obtain, but also has a very significant effect of improving the balance between the residual magnetic flux density and the coercive force of a magnet. Such a technical effect is unexpected.
[0063] According to another embodiment of the present invention, the Pr-M alloy powder is a Pr-Cu alloy powder, in which Pr is 50 at% or more, preferably 60 at% or more, and more preferably 65 to 75 at%.
[0064] The amount of the praseodymium-containing powder used is 0.1 to 5.0 wt %, preferably 1.0 to 4.0 wt %, and more preferably 1.5 to 2.5 wt %, based on the mass of the coarse alloy powder.
[0065] The jet milling process may be carried out in a nitrogen atmosphere.
[0066] Molding process The magnetic powder is pressed in a magnetic field and then subjected to hydrostatic isostatic pressing to obtain a green body.
[0067] The molding step may be performed by pressing in a molding press, preferably under nitrogen protection.
[0068] The magnetic field strength is greater than 1.0T, preferably greater than 1.5T, more preferably greater than 1.7T.
[0069] The density of the green body is 2.5 to 5.5 g / cm 3 and preferably 3.5 to 5.0 g / cm 3 and more preferably 4.0 to 4.5 g / cm 3 It is.
[0070] Sintering and aging process The green body is subjected to vacuum heat treatment and two-stage tempering treatment to obtain a rare earth sintered permanent magnet.
[0071] The vacuum conditions of the vacuum heat treatment mean that the absolute vacuum is less than 0.5 Pa, preferably less than 0.3 Pa, and more preferably less than 0.1 Pa. The heat treatment temperature may be 850 to 1300° C., preferably 950 to 1200° C., and more preferably 1000 to 1100° C. The heat treatment time may be 2 to 10 hours, preferably 3 to 8 hours, and more preferably 4 to 7 hours.
[0072] The primary tempering temperature may be 600 to 1050°C, preferably 700 to 1000°C, and more preferably 800 to 950°C. The primary tempering time may be 1 to 6 hours, preferably 2 to 5 hours, and more preferably 3 to 4 hours. The primary tempering is performed under vacuum conditions. The vacuum conditions mean that the absolute vacuum is less than 0.5 Pa, preferably less than 0.3 Pa, and more preferably less than 0.1 Pa.
[0073] The secondary tempering temperature may be 300 to 700°C, preferably 400 to 600°C, and more preferably 450 to 550°C. The secondary tempering time may be 3 to 10 hours, preferably 4 to 8 hours, and more preferably 5 to 7 hours. The secondary tempering is performed under vacuum conditions. The vacuum conditions mean that the absolute vacuum is less than 0.5 Pa, preferably less than 0.3 Pa, and more preferably less than 0.1 Pa.
[0074] <Use of praseodymium hydride> The present invention provides the use of praseodymium hydride to improve the balance factor between remanence and coercivity of rare earth sintered neodymium-iron-boron magnets. The balance factor between remanence and coercivity can be expressed as E and is calculated by the following formula:
[0075] E=X2 / X1 X1 = (Br1-Br2) / Br1 X2=(Hcj2-Hcj1) / Hcj1 Br1 represents the residual magnetic flux density of the rare earth sintered neodymium-iron-boron magnet obtained without adding praseodymium hydride powder in the jet milling process, and is expressed in kGs. Br2 represents the residual magnetic flux density of the rare earth sintered neodymium-iron-boron magnet obtained by adding praseodymium hydride powder in the jet milling process, and is expressed in kGs. Hcj1 represents the coercivity of the rare earth sintered neodymium-iron-boron magnet obtained without adding praseodymium hydride powder in the jet milling process, and is expressed in kOe. Hcj2 represents the coercivity of the rare earth sintered neodymium-iron-boron magnet obtained by adding praseodymium hydride powder in the jet milling process, and is expressed in kOe.
[0076] The balance factor E between the residual magnetic flux density and the coercive force of the rare earth sintered neodymium-iron-boron magnet according to the present invention may be 25 or more, preferably 35 or more, and more preferably 39 or more. The balance factor E may be 150 or less, preferably 100 or less, and more preferably 80 or less.
[0077] In the use according to the present invention, the alloy coarse powder and the praseodymium hydride powder are pulverized into coarse powder by jet milling. Based on the mass of the alloy coarse powder, the amount of the praseodymium hydride powder used is 0.1-5.0 wt%, preferably 1.0-4.0 wt%, and more preferably 2.0-3.0 wt%. In addition to the jet milling process, the use according to the present invention may further include a melting process, a crushing process, a molding process, and a sintering and aging treatment process. The specific process conditions are as described above.
[0078] The composition of the alloy coarse powder according to the present invention has R1-TBM, and is preferably R1-TBM.
[0079] R1 is one or more selected from Nd and Gd elements. Nd is 50 at% or more of the total number of R1 atoms, preferably Nd is 80 at% or more of the total number of R1 atoms, more preferably Nd is 95 at% or more of the total number of R1 atoms. According to one embodiment of the present invention, R1 is Nd.
[0080] T is one or more elements selected from Fe, Co, and Ni. Co and Ni account for 3 at% or less of the total number of atoms of T, preferably Co and Ni account for 2 at% or less of the total number of atoms of T, and more preferably Co and Ni account for 1 to 1.5 at% of the total number of atoms of T. According to one embodiment of the present invention, T is Fe and Co.
[0081] B is elemental boron.
[0082] M is one or more elements selected from Al, Cu, Ga, Zn, Bi, Zr, Ti, Nb, V, Mo, and W. Preferably, M is Cu, Zr, and Ga. The total atomic number of M is 5 at% or less, preferably 4 at% or less, more preferably 3 at% or less, and most preferably 0.1 to 2 at% of the alloy coarse powder. According to one embodiment of the present invention, the total atomic number of M is 0.3 to 1 at% of the alloy coarse powder.
[0083] The alloy coarse powder according to the present invention includes elements such as R1, B, Co, Cu, Zr, Ga, and Fe. In some embodiments, the alloy coarse powder according to the present invention is composed of R1, B, Co, Cu, Zr, Ga, and Fe. Based on the mass of the alloy coarse powder, the content of R1 may be 28-31 wt%, preferably 28-30 wt%, and more preferably 28-29 wt%. The content of B may be 0.6-1.6 wt%, preferably 0.7-1.3 wt%, and more preferably 0.9-1.0 wt%. The content of Co may be 0.1-3.9 wt%, preferably 0.7-1.3 wt%, and more preferably 0.9-1.0 wt%. The content of Cu may be 0.05-1.0 wt%, preferably 0.10-0.70 wt%, and more preferably 0.12-0.20 wt%. The content of Zr may be 0.06 to 0.25 wt%, preferably 0.1 to 0.16 wt%, and more preferably 0.13 to 0.15 wt%. The content of Ga may be 0.1 to 0.3 wt%, preferably 0.15 to 0.25 wt%, and more preferably 0.18 to 0.20 wt%. The balance is Fe. According to one embodiment of the present invention, the alloy coarse powder according to the present invention does not contain a heavy rare earth element. The heavy rare earth elements are terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), rubidium (Tm), ytterbium (Yb), and rubidium (Lu).
[0084] According to one embodiment of the present invention, the alloy coarse powder may be composed of Nd, B, Co, Cu, Zr, Ga and Fe. The Nd content may be 28-31wt%, preferably 28-30wt%, more preferably 28-29wt%. The B content may be 0.6-1.6wt%, preferably 0.7-1.3wt%, more preferably 0.9-1.0wt%. The Co content may be 0.1-3.9wt%, preferably 0.7-1.3wt%, more preferably 0.9-1.0wt%. The Cu content may be 0.05-1.0wt%, preferably 0.10-0.70wt%, more preferably 0.12-0.20wt%. The Zr content may be 0.06 to 0.25 wt%, preferably 0.1 to 0.16 wt%, and more preferably 0.13 to 0.15 wt%. The Ga content may be 0.1 to 0.3 wt%, preferably 0.15 to 0.25 wt%, and more preferably 0.18 to 0.20 wt%, and the remainder is Fe.
[0085] In the jet milling step, the raw material containing the alloy coarse powder and the praseodymium hydride powder is pulverized into a magnetic powder by jet milling. The magnetic powder may have an average particle size D50 of 1 to 10 μm, preferably 2 to 7 μm, and more preferably 3 to 5 μm. The jet milling step may be performed in a nitrogen atmosphere.
[0086] Example 1 Melting process: The raw materials were mixed in the following composition (mass percentage): Nd 29.0%, B 1.0%, Co 1.0%, Cu 0.15%, Zr 0.15%, Ga 0.2%, and the balance Fe. The raw materials were melted in a vacuum smelting rapid solidification furnace to produce an alloy sheet with an average thickness of 0.3 mm.
[0087] Hydrogen crushing process: The alloy sheet was subjected to hydrogen absorption and dehydrogenation treatment in a hydrogen crushing furnace to produce coarse alloy powder with an average particle size D50 of 100 μm.
[0088] Jet milling process: 2.0 wt% of praseodymium hydride powder was added to the alloy coarse powder and mixed uniformly. The mixture was then pulverized into magnetic powder with an average particle size D50 of 4.0 μm by jet milling using nitrogen gas as a medium.
[0089] Molding process: The magnetic powder is applied to a nitrogen-protected molding press, oriented by applying a 1.8 T magnetic field, and molded into a green body, with a density of 4.3 g / cm 3 It was.
[0090] Sintering and aging treatment process: The green body was placed into a vacuum sintering furnace with an absolute vacuum of less than 0.1 Pa and sintered at 1,070°C for 5 hours to obtain a sintered magnet. The sintered magnet was then subjected to a first-stage tempering process at 900°C for 3 hours and a second-stage tempering process at 500°C for 5 hours under an absolute vacuum of less than 0.1 Pa to obtain a rare earth sintered neodymium-iron-boron magnet.
[0091] The rare earth sintered neodymium-iron-boron magnet was machined into a sample pillar of D10 x 10 mm, and the magnetic properties of the magnet were measured at room temperature and 150°C using a BH tester. The temperature coefficient α of the residual magnetic flux density and the temperature coefficient β of the coercivity were also calculated within the range of 20 to 150°C.
[0092] The rare earth sintered neodymium-iron-boron magnet was observed for microstructure with a sigma 500 field emission scanning electron microscope (see FIG. 1), and composition analysis was performed with an EDS detector.
[0093] Tables 1 and 2 show the average thickness L of the grain boundary phase, the Pr concentration difference (C1-C2) between the main phase crystal grain edge and the main phase crystal grain center, and magnetic performance parameters of the rare earth sintered neodymium-iron-boron magnet.
[0094] Examples 2-3 and Comparative Examples 1-2 In the jet milling process, the amount of praseodymium hydride powder used was changed, and the other processes were the same as in Example 1. The average thickness L of the grain boundary phase, the Pr concentration difference (C1-C2) between the main phase crystal grain edge and the main phase crystal grain center, and magnetic performance parameters of the rare earth sintered neodymium-iron-boron magnet are shown in Tables 1 and 2.
[0095] Example 4 In the jet milling process, 3.0%wt of Pr68Cu32 alloy was added, and other processes were the same as in Example 1. The average thickness L of the grain boundary phase, the Pr concentration difference (C1-C2) between the main phase crystal grain edge and the main phase crystal grain center of the rare earth sintered neodymium-iron-boron magnet, and the magnetic performance parameters are shown in Tables 1 and 2.
[0096] Comparative Example 3 In the melting process, the raw materials were blended according to mass percent of Nd 29.0%, Pr 2.0%, B 1.0%, Co 1.0%, Cu 0.15%, Zr 0.15%, Ga 0.2%, and the balance Fe, and in the jet milling process, no praseodymium hydride powder was added, and the other processes were the same as in Example 1. The average thickness L of the grain boundary phase, the Pr concentration difference (C1-C2) between the main phase crystal grain edge and the main phase crystal grain center, and the magnetic performance parameters of the rare earth sintered neodymium-iron-boron magnet are shown in Tables 1 and 2.
[0097] TIFF0007586881000001.tif72170
[0098] Comparative Examples 4 to 9 Sintered neodymium-iron-boron magnets were manufactured according to Examples 1 to 6 of CN111696742A. The average thickness L of the grain boundary phase, the Pr concentration difference (C1-C2) between the main phase crystal grain edge and the main phase crystal grain center, and magnetic performance parameters of the rare earth sintered neodymium-iron-boron magnets are shown in Table 2.
[0099] Comparative Examples 10 to 13 Sintered neodymium-iron-boron magnets were manufactured according to Examples 1 to 4 of CN104575899A. The average thickness L of the grain boundary phase, the Pr concentration difference (C1-C2) between the main phase crystal grain edge and the main phase crystal grain center, and magnetic performance parameters of the rare earth sintered neodymium-iron-boron magnets are shown in Table 2.
[0100] TIFF0007586881000002.tif224170TIFF0007586881000003.tif40170Note: Br1 represents the residual magnetic flux density of the rare earth sintered neodymium-iron-boron magnet obtained without adding any modifying powder, in kGs; Br2 represents the residual magnetic flux density of the rare earth sintered neodymium-iron-boron magnet obtained with adding any modifying powder, in kGs; Hcj1 represents the coercive force of the rare earth sintered neodymium-iron-boron magnet obtained without adding any modifying powder, in kOe; Hcj2 represents the coercive force of the rare earth sintered neodymium-iron-boron magnet obtained with adding any modifying powder, in kOe.
[0101] As can be seen from Tables 1 and 2, in the present invention, the alloy coarse powder is pulverized into magnetic powder by jet milling with praseodymium-containing powder, and then through processes such as molding and sintering, a rare earth sintered neodymium-iron-boron magnet is obtained, which allows the magnet to have both remanence and coercivity, achieving a perfect balance between the two, with a balance factor of 25 or more. In this case, the Pr concentration C1 at the edge of the main phase crystal grain is 0.25 wt% or more higher than the Pr concentration C2 at the center of the main phase crystal grain, and the average thickness of the grain boundary phase is 20 to 60 nm. When an appropriate amount of praseodymium hydride powder is used, the balance factor between remanence and coercivity is high, at 35 or more (see Example 1).
[0102] As can be seen from Table 3, the magnets of Comparative Examples 1 to 13 fail to simultaneously satisfy the following conditions: (1) The Pr concentration C1 at the edge of the main phase crystal grain is 0.25 wt% or more higher than the Pr concentration C2 at the center of the main phase crystal grain, and (2) The average thickness of the grain boundary phase is 20 to 60 nm.
[0103] As can be seen from Table 2, in Comparative Example 1, the praseodymium hydride powder was not added, and the residual magnetic flux density and coercive force were relatively low. In Comparative Example 2, the amount of praseodymium hydride powder used was too much, and the residual magnetic flux density was reduced too much, so the balance factor was relatively low. In Comparative Example 3, even though Pr was added in the raw material mixing process, the coercive force was not significantly improved, and the balance factor was relatively low. In Comparative Examples 4 to 9, PrNi alloy powder was directly mixed with fine magnetic powder, and the coercive force was significantly improved, but the residual magnetic flux density was too low, so the balance factor was less than 20. In Comparative Examples 11 and 12, (PrNd)Co alloy powder was directly mixed with fine magnetic powder, and the coercive force could be improved, but the residual magnetic flux density was too low, so the balance factor was 10 or less. In Comparative Examples 10 and 13, DyCo or TbCo alloy powder was directly mixed with fine magnetic powder, and the coercive force was obviously improved, but the residual magnetic flux density was further reduced, and the balance factor was very low.
[0104] TIFF0007586881000004.tif116170
[0105] The present invention is not limited to the above-described embodiments, and all modifications, improvements, substitutions, etc. that may occur to those skilled in the art are included in the scope of the present invention, provided that they do not deviate from the spirit of the present invention.
Claims
1. (R1, R2)-TBM rare earth sintered neodymium-iron-boron magnet, The rare earth sintered neodymium-iron-boron magnet is composed of a sintered body containing main phase crystal grains and a grain boundary phase, The main phase crystal grains are (R1, R2) 2 T 14 B phase, and the Pr concentration at the edge of the main phase crystal grain is C 1 is the Pr concentration C at the center of the main phase crystal grain 2 Higher, The R1 concentration of the grain boundary phase is higher than the R1 concentration of the main phase crystal grains, and the average thickness of the grain boundary phase is 20 to 40 nm; R1 is one or more elements selected from Nd and Gd, and Nd accounts for 50 at % or more of the total number of atoms of R1; R2 is a Pr element; T is one or more elements selected from Fe, Co, and Ni, and Co and Ni account for 3 at % or less of the total number of atoms of T; B is elemental boron; M is one or more elements selected from Al, Cu, Ga, Zn, Bi, Zr, Ti, Nb, V, Mo and W, and the total atomic number of M is 5 at % or less of the sintered body; The composition of the sintered body is R1: 28 to 31 wt%, R2: 0.1 to 5 wt%, B: 0.6 to 1.6 wt%, Co: 0.1 to 3.9 wt%, Cu: 0.05 to 1.0 wt%, Zr: 0.06 to 0.25 wt%, Ga: 0.1 to 0.3 wt%, and the balance is substantially Fe; The rare earth sintered neodymium-iron-boron magnet has a residual magnetic flux density of 14.50 kGs or more, an intrinsic coercive force of 14.0 kOe or more, a temperature coefficient of residual magnetic flux density within the range of 20 to 150°C of less than 0.113% / °C, and a temperature coefficient of coercive force within the range of 20 to 150°C of less than 0.573% / °C. The (R1, R2)-TBM rare earth sintered neodymium-iron-boron magnet is characterized by the above.
2. 2. The rare earth sintered neodymium-iron-boron magnet according to claim 1, wherein the Pr concentration gradually decreases from the edge of the main phase crystal grain toward the center of the main phase crystal grain.
3. The Pr concentration C at the edge of the main phase crystal grain 1 is the Pr concentration C at the center of the main phase crystal grain 2 2. The rare earth sintered neodymium-iron-boron magnet according to claim 1, wherein the content of the magnetron is at least 0.25 wt % higher than the content of the magnetron.
4. 2. The rare earth sintered neodymium-iron-boron magnet according to claim 1, characterized in that the Zr content in the sintered body is 0.1 to 0.16 wt %, and the Ga content is 0.15 to 0.25 wt %.
5. 5. The rare earth sintered neodymium-iron-boron magnet according to claim 1, which contains no heavy rare earth elements.
Citation Information
Patent Citations
R-t-b-based sintered magnet and method for producing the same
JP2014130888A
Rare earth-(iron, cobalt)-boron based sintered magnet, and method for manufacturing the same
JP2018082040A
R-t-b based permanent magnet
JP2021158342A
R-t-b-based alloy powder and method for producing same, and r-t-b-based sintered magnet and method for producing same
WO2015146888A1
R-t-b sintered magnet
WO2018034264A1