Thermally conductive polyurethane composition

A novel isocyanate composition with specific thermally conductive fillers addresses the challenges of high thermal conductivity and low viscosity in two-component PU adhesives, ensuring stable mixing ratios and easy processing.

JP7586940B2Active Publication Date: 2024-11-19DOW GLOBAL TECHNOLOGIES LLC +1
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2022576136
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-29
Publication Date
2024-11-19
Estimated Expiration
2040-06-29

AI Technical Summary

Technical Problem

Two-component polyurethane (PU) adhesives face challenges in achieving high thermal conductivity while maintaining low viscosity and processability, and incorporating thermally conductive fillers is hindered by moisture sensitivity and the need for precise mixing ratios, which complicates manufacturing.

Method used

A novel isocyanate composition containing specific thermally conductive fillers, such as spherical metal oxide particles and surface-treated metal oxide particles, with controlled mixing ratios, allowing for high thermal conductivity and low viscosity, suitable for use in two-part polyurethane adhesive formulations.

Benefits of technology

The composition achieves thermal conductivity of 2.73 W/mK or higher with a viscosity of 230 Pa.s or less, enabling easy processing and use of conventional equipment, while maintaining storage stability and consistent mixing ratios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586940000001
    Figure 0007586940000001
  • Figure 0007586940000002
    Figure 0007586940000002
  • Figure 0007586940000003
    Figure 0007586940000003
Patent Text Reader

Abstract

The composition comprising the isocyanate composition comprising a polyisocyanate and a specific thermally conductive filler composition (C) may further be part of a two-component curable composition comprising an isocyanate composition and a polyol composition, and having low viscosity when mixed and providing high thermal conductivity when cured.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention is a two-component thermally conductive polyurethane composition and a process for preparing the same.

[0002] Introduction Two-component polyurethane (PU) adhesives or gap fillers, including a polyol component and an isocyanate component, are becoming important in industry, but still suffer from limitations such as insufficient thermal conductivity. For example, some applications, such as gap fillers for battery packs, require high thermal conductivity of at least 2.73 watts per meter per Kelvin (W / mK), preferably 3.0 W / mK or higher, as measured according to ISO 22007-2. For example, there are challenges to improve thermal conductivity while maintaining flowability and processability, including manufacturing equipment.

[0003] Although the incorporation of sufficient amounts of thermally conductive fillers into conventional two-component PU adhesives can reach the thermal conductivity requirements listed above, it is difficult to achieve a formulation viscosity of 230 Pascal seconds (Pa.s) at room temperature (23±2 degrees Celsius (°C)) when measured within 30 minutes of mixing the two components of the adhesive together, while also achieving the viscosity of the resulting highly filled system. Thus, it is difficult for a two-component PU composition to reach the required high thermal conductivity while maintaining a low viscosity for easy processability and application.

[0004] Furthermore, due to the sensitivity of isocyanates to moisture from the filler, only limited types and amounts of fillers can be introduced into the isocyanate portion, e.g., typical thermally conductive fillers such as amorphous alumina cannot be included in the isocyanate component of a two-component polyurethane adhesive. These issues not only limit the total amount of thermally conductive fillers that can be included in a two-component PU adhesive, but also make it difficult to provide a consistent mix ratio for the two components, i.e., a volumetric mix ratio of 0.95:1 to 1.05:1. Mix ratios outside of this mix ratio (e.g., 30:1) result in unequal flow rates of the two components, resulting in poor performance and requiring special equipment design to mix each component. It is further desirable to be able to produce two-component PU compositions using existing manufacturing equipment.

[0005] It would be desirable to find an isocyanate composition that can be used in two-part polyurethane adhesive formulations that contain thermally conductive fillers but without the problems mentioned above. Summary of the Invention

[0006] The present invention solves the problem of finding an isocyanate composition that can be used in two-part polyurethane adhesive formulations that contain thermally conductive fillers but without the problems mentioned above.

[0007] The present invention provides a novel composition comprising an isocyanate composition comprising a polyisocyanate and a specific thermally conductive filler composition (C). The composition of the present invention is storage stable as shown by the isocyanate composition having a viscosity variation of 50% or less after storage for 24 hours at 50°C under a nitrogen atmosphere. The isocyanate composition of the present invention is particularly suitable as a two-component curable composition further comprising a polyol composition. The two-component curable composition comprises two components: a polyol composition as component A and an isocyanate composition as component B. The two-component curable composition has a viscosity of 230 Pascal seconds (Pa·s) or less at room temperature (23±2°C) when measured within 30 minutes after mixing the two components. The two-component curable composition also provides a polyurethane material, when cured, having a thermal conductivity of 2.73 Watts per meter per Kelvin (W / mK) or more, or 3.0 W / mK or more. Furthermore, the volume mixing ratio of component A and component B of the curable composition can be controlled between 0.95:1 and 1.05:1, so that the two-component curable composition can be prepared using existing manufacturing equipment. The above properties are measured according to the test methods described in the Examples section below.

[0008] In a first aspect, the present invention provides a composition comprising an isocyanate composition comprising a polyisocyanate and a thermally conductive filler composition (C), the thermally conductive filler composition comprising: (c1) spherical metal oxide particles having an average particle size of 20 micrometers (μm) or more; (c2) surface-treated metal oxide particles having an average particle size of more than 1 μm to 10 μm, which are treated with an alkoxysilane; (c3) an additional thermally conductive filler selected from the group consisting of metal oxide particles having an average particle size of 1 μm or less, a thermally conductive filler other than metal oxide particles having a thermal conductivity of 40 W / mK or more, or a mixture thereof.

[0009] In a second aspect, the present invention provides a process for preparing the composition of the first aspect, the process comprising mixing the components of the thermally conductive filler composition (C) with a polyisocyanate and, optionally, with a polyol composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] "Polyol" refers to any compound that contains two or more hydroxyl (OH) groups.

[0011] "Thermally conductive filler" refers to any filler that exhibits a thermal conductivity of 10 W / mK or greater when measured according to ASTM D5470-17.

[0012] In this specification, the "aspect ratio" refers to the minimum diameter (D min ) maximum diameter (D max ) to the ratio (D min / D max The aspect ratio can be measured according to the test method described in the Examples section below.

[0013] The composition of the present invention includes an isocyanate composition comprising one or more polyisocyanates and a thermally conductive filler composition (C). "Polyisocyanate" refers to any compound containing two or more isocyanate groups. The polyisocyanate may include monomeric diisocyanates, polymeric isocyanates, isocyanate prepolymers, or mixtures thereof. The polyisocyanate may be aromatic, aliphatic, araliphatic, or cycloaliphatic polyisocyanates, or mixtures thereof. The preferred polyisocyanates are aromatic polyisocyanates. Aromatic polyisocyanates refer to compounds having at least one isocyanate group attached to an aromatic carbon atom. The polyisocyanates in the isocyanate composition can have an average isocyanate functionality of 2.0 or greater, 2.1 or greater, 2.2 or greater, or even 2.3 or greater, and at the same time 4.0 or less, 3.8 or less, 3.5 or less, 3.2 or less, 3.0 or less, 2.8 or less, or even 2.7 or less.

[0014] The isocyanate composition of the present invention may include one or more monomeric polyisocyanates. Examples of suitable monomeric diisocyanates include diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HDI), tetramethylene-1,4-diisocyanate, cyclohexane-1,4-diisocyanate, hexahydrotolylene diisocyanate, 1-methoxyphenyl-2,4-diisocyanate, diphenylmethane-4,4'-diisocyanate, diphenylmethane-2,4'-diisocyanate, 4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-diphenyl diisocyanate, and 3,3'-dimethyldiphenylpropane-4,4'-diisocyanate, their isomers, or their mixtures. The preferred monomeric diisocyanate is MDI.

[0015] The isocyanate composition of the present invention may include one or more isocyanate-terminated prepolymers. The isocyanate-terminated prepolymer may be any prepolymer prepared by the reaction of one or more polyols with a stoichiometric excess of one or more polyisocyanates. The isocyanate-terminated prepolymer may include a polyether backbone and an isocyanate moiety. The isocyanate-terminated prepolymer may have an isocyanate content of 5% by weight or more, 6% by weight or more, 8% by weight or more, or even 10% by weight or more, and at the same time 30% by weight or less, 25% by weight or less, 20% by weight or less, or even 15% by weight or less, based on the total weight of the isocyanate-terminated prepolymer. The isocyanate (NCO) content herein is measured according to ASTM D5155-19. The isocyanates used to prepare the isocyanate-terminated prepolymer include the monomeric diisocyanates described above, their isomers, their polymeric derivatives, or mixtures thereof. The preferred isocyanate is diphenylmethane diisocyanate (MDI), its polymeric derivatives, or mixtures thereof. The MDI used to prepare the isocyanate-terminated prepolymer can be 4,4'-, 2,4'-, or 2,2'-diphenylmethane diisocyanate, or mixtures thereof. Mixtures of 2,4'-diphenylmethane diisocyanate and 4,4'-diphenylmethane diisocyanate may also be used.The polyol used to prepare the isocyanate-terminated prepolymer can be any polyol known in the art, including, for example, ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butenediol, 1,4-butynediol, 1,5-pentanediol, neopentyl-glycol, bis(hydroxy-methyl)cyclohexane, such as 1,4-bis(hydroxymethyl)cyclohexane, 2-methylpropane-1,3-diol, methylpentanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, dibutylene glycol, polybutylene glycol, polyoxyethylene glycol, polyoxypropylene glycol, polyoxypropylene-polyoxyethylene glycol, or mixtures thereof. Preferred polyols are the polyether polyols described in the polyol composition section above.

[0016] The isocyanate composition of the present invention may also include polymeric derivatives of the above monomeric diisocyanates, such as polymeric methylene diphenyl diisocyanate ("polymeric MDI"). The polymeric MDI may be a mixture of diphenylmethane diisocyanate and polyphenylene polymethylene polyisocyanate. The polymeric MDI useful in the present invention may contain 2.5 to 3.5 isocyanate groups per molecule and have an isocyanate equivalent weight of 130 to 150 or 132 to 140. Suitable commercially available polymeric MDI products may include, for example, PAPI™ 27 and PAPI 32 polymeric MDI, both available from The Dow Chemical Company (PAPI is a trademark of The Dow Chemical Company).

[0017] The thermally conductive filler composition (C) useful in the present invention comprises three different thermally conductive fillers: (c1), (c2), and (c3).

[0018] The thermally conductive filler (c1) is a spherical metal oxide particle. The spherical particle refers to a particle having an aspect ratio of 0.8 or more, for example, 0.81 or more, 0.82 or more, 0.85 or more, 0.86 or more, 0.88 or more, 0.89 or more, 0.9 or more, 0.9 or more, 0.91 or more, 0.92 or more, 0.93 or more, 0.94 or more, or more than 0.95 to 1.0, preferably more than 0.9. The spherical metal oxide particle is desirably selected from aluminum oxide particles, magnesium oxide particles, zinc oxide particles, and mixtures thereof. Preferred spherical metal oxide particles are aluminum oxide particles, magnesium oxide particles, or mixtures thereof. The spherical metal oxide particles (c1) may optionally be surface-treated with an alkyltrialkoxysilane, including, for example, those used to prepare the surface-treated metal oxide particles (c2) described below.

[0019] The spherical metal oxide particles (c1) useful in the present invention have an average particle size of 20 μm or more. In the present invention, "average particle size" refers to the D50 particle size measured according to the test method described in the Examples section below. The spherical metal oxide particles (c1) have an average particle size (D50) of 20 μm or more, 22 μm or more, 25 μm or more, 28 μm or more, 30 μm or more, 32 μm or more, or even 35 μm or more, and at the same time, typically 60 μm or less, 58 μm or less, 55 μm or less, 52 μm or less, 50 μm or less, 48 ​​μm or less, 45 μm or less, 42 μm or less, or even 40 μm or less. The spherical metal oxide particles (c1) may be present in the isocyanate composition in an amount of 20% by weight or more, 22% by weight or more, 25% by weight or more, 28% by weight or more, 30% by weight or more, 32% by weight or more, 35% by weight or more, 38% by weight or more, 40% by weight or more, 42% by weight or more, 45% by weight or more, 48% by weight or more, 50% by weight or more, 52% by weight or more, 55% by weight or more, or even 58% by weight or more, and at the same time, typically in an amount of 90% by weight or less, 88% by weight or less, 85% by weight or less, 82% by weight or less, 80% by weight or less, 78% by weight or less, 75% by weight or less, 72% by weight or less, 70% by weight or less, or even 68% by weight or less, based on the weight of the isocyanate composition.

[0020] (c2) The thermally conductive filler is a metal oxide particle surface-treated with one or more alkoxysilanes, i.e., a metal oxide particle surface-treated with one or more alkoxysilanes. The surface-treated metal oxide particles (c2) after mixing with an aromatic isocyanate have a 1232 cm -1 band (absorbance of -C=O in the complex) at 2300 cm -1 The isocyanate may contain a complex resulting from reaction and / or interaction of NCO groups in the isocyanate with functional groups on the surface of the metal oxide, such as an NCO-O-metal oxide complex, at a concentration that is at least 50% lower than the concentration of the same complex formed by mixing the untreated metal oxide with the same isocyanate, as shown by a peak height ratio of at least 50% reduction in the peak height ratio of the band (absorbance of free -NCO groups in the isocyanate) relative to such peak height ratio in the infrared spectrum of a mixture of the untreated metal oxide with the same isocyanate. The peak height ratio is determined by the test method described in the Examples section below.

[0021] The surface-treated metal oxide particles (c2) useful in the present invention have an average particle size (D50) of 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, 5 μm or less, 4 μm or less, 3 μm or less, or even 2.5 μm or less, and at the same time, more than 1 μm, or typically 1.1 μm or more, 1.2 μm or more, 1.3 μm or more, 1.4 μm or more, 1.5 μm or more, 1.6 μm or more, 1.7 μm or more, 1.8 μm or more, 1.9 μm or more, or even 2.0 μm or more. The surface-treated metal oxide particles (c2) are typically non-spherical. Non-spherical particles refer to particles with an aspect ratio of less than 0.8, for example, 0.7 or less, 0.6 or less, 0.5 or less, or even 0.4 or less.

[0022] Alkoxysilanes useful for forming surface-treated metal oxide particles (c2) are those that can react with functional groups (e.g., -OH groups) on the metal oxide (untreated) to form covalent bonds such as -MO-Si-C- (where M is the metal in the metal oxide). Alkoxysilanes useful for forming surface-treated metal oxides (i.e., alkoxysilanes used to treat the metal oxide) can include alkyltrialkoxysilanes, alkyldialkoxysilanes, vinyltrialkoxysilanes, vinyldialkoxysilanes, or mixtures thereof, preferably alkyltrialkoxysilanes. Alkoxysilanes are those that are capable of reacting with functional groups (e.g., -OH groups) on the metal oxide (untreated) to form covalent bonds such as -MO-Si-C- (where M is the metal in the metal oxide). Alkoxysilanes useful for forming surface-treated metal oxides (i.e., alkoxysilanes used to treat the metal oxide) can include alkyltrialkoxysilanes, alkyldialkoxysilanes, vinyltrialkoxysilanes, vinyldialkoxysilanes, or mixtures thereof, preferably alkyltrialkoxysilanes. Alkoxysilanes can be selected from the group consisting of R 1 Si(OR 2 )3 or R 1 R 3 Si(OR 2 )2(wherein, R 1 may be an alkyl or alkylene group having 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, and each R 2 is independently methyl, ethyl, or a combination thereof; R 3may be an alkyl group having 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms). Specific examples of alkoxysilanes used in the preparation of the surface-treated metal oxide particles (c2) include methyltrimethoxysilane, n-decyltrimethoxysilane, ethyltrimethoxysilane, methyltris(methoxyethoxy)silane, pentyltrimethoxysilane, hexyltrimethoxysilane, and octyltrimethoxysilane; vinyltrimethoxysilane, vinyltriethoxysilane, and vinylmethyldimethoxysilane; or mixtures thereof. The surface-treated metal oxide particles (c2) may be surface-treated aluminum oxide particles, surface-treated zinc oxide particles, or mixtures thereof. The surface-treated metal oxide particles (c2) may be present in the isocyanate composition in an amount of 10% by weight or more, 12% by weight or more, 15% by weight or more, 17% by weight or more, 19% by weight or more, or even 20% by weight or more, and at the same time 40% by weight or less, 38% by weight or less, 35% by weight or less, 32% by weight or less, 30% by weight or less, 28% by weight or less, or even 25% by weight or less, based on the weight of the isocyanate composition.

[0023] (c3) The thermally conductive filler is one or more additional thermally conductive fillers selected from one or a combination of more than one of the following two types of thermally conductive fillers: (c3-a) metal oxide particles having an average particle size of 1 μm or less, and (c3-b) non-metal oxide particles (i.e., other than metal oxide particles) thermally conductive fillers having a thermal conductivity of 40 W / mK or more. The metal oxide particles (c3-a) have an average particle size (D50) of 1 μm or less, 0.9 μm or less, 0.8 μm or less, 0.7 μm or less, 0.6 μm or less, 0.5 μm or less, 0.4 μm or less, 0.3 μm or less, or even 0.25 μm or less, while typically having an average particle size (D50) of 0.1 μm or more, 0.11 μm or more, 0.12 μm or more, 0.13 μm or more, 0.14 μm or more, or even 0.15 μm or more. The thermally conductive filler (c3-b) may comprise any one or more of any combination of particles selected from metal nitride particles, non-metal nitride particles, or mixtures thereof. The thermally conductive filler (c3-b) has a thermal conductivity of 40 W / mK or more, 41 W / mK or more, 42 W / mK or more, 43 W / mK or more, 44 W / mK or more, 45 W / mK or more, and at the same time typically 300 W / mK or less, 250 W / mK or less, 240 W / mK or less, 230 W / mK or less, 220 W / mK or less, 210 W / mK or less, 200 W / mK or less, 80 W / mK or less, 79 W / mK or less, 78 W / mK or less, 75 W / mK or less, 72 W / mK or less, or even 70 W / mK or less. Preferably, the thermal conductivity of the thermally conductive filler (c3-b) is less than 80 W / mK. Thermal conductivity can be measured according to the test method described in the Examples section below. The thermally conductive filler (c3-b) can have an average particle size (D50) of 1 μm or more, 2 μm or more, 3 μm or more, 4 μm or more, 5 μm or more, 6 μm or more, 7 μm or more, 8 μm or more, 9 μm or more, or even 10 μm or more, while typically 50 μm or less, 48 ​​μm or less, 45 μm or less, 42 μm or less, 40 μm or less, 38 μm or less, 35 μm or less, 32 μm or less, or even 30 μm or less. The additional thermally conductive filler (c3) can include any one or any combination of more than one of particles selected from aluminum nitride (AlN) particles, zinc oxide (ZnO) particles, and boron nitride (BN) particles.Preferred additional thermally conductive fillers (c3) are zinc oxide particles, boron nitride particles, or a mixture thereof.

[0024] The additional thermally conductive filler (c3) may be present in the isocyanate composition in an amount of 1.5% by weight or more, 1.6% by weight or more, 1.7% by weight or more, 1.75% by weight or more, 2% by weight or more, 3% by weight or more, 4% by weight or more, 5% by weight or more, 5.5% by weight or more, 5.8% by weight or more, 6% by weight or more, 6.2% by weight or more, 6.5% by weight or more, 6.8% by weight or more, or even 7% by weight or more, based on the weight of the isocyanate composition, while typically being present in an amount of 12% by weight or less, 11.5% by weight or less, 11% by weight or less, 10.5% by weight or less, 10% by weight or less, 9% by weight or less, or even 8% by weight or less. For example, the zinc oxide particles can be present in an amount of zero or more, 5.5 or more, 5.8 or more, 6 or more, 6.2 or more, 6.5 or more, 6.8 or more, or even 7 or more by weight, based on the weight of the isocyanate composition, while typically being present in an amount of 12 or less, 11.5 or less, 11 or less, 10.5 or less, or even 10 or less by weight. The boron nitride particles may be present in an amount of zero or more, 1.5 or more, 1.6 or more, 1.65 or more, 1.7 or more, 1.75 or more, 1.8 or more, 1.85 or more, 1.9 or more, 1.95 or more by weight, based on the weight of the isocyanate composition, while typically being present in an amount of 4 or less, 3.5 or less, 3.0 or less, 2.5 or less, 2.4 or less, 2.2 or less, 2.1 or less, or even 2.0 or less by weight.

[0025] The isocyanate composition useful in the present invention may further comprise a thermally conductive filler (c4) different from (c1), (c2), and (c3). The thermally conductive filler (c4) is an untreated metal oxide particle having an average particle size (D50) of more than 1 μm and less than 20 μm, for example, 18 μm or less, 15 μm or less, 12 μm or less, 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, 5 μm or less, 4 μm or less, 3 μm or less, or even 2.5 μm or less, and at the same time more than 1.0 μm, or typically 1.1 μm or more, 1.2 μm or more, 1.3 μm or more, 1.4 μm or more, 1.5 μm or more, 1.6 μm or more, or even 1.7 μm or more. By "untreated" it is meant that the filler does not contain a surface treatment agent. Preferably, the untreated metal oxide particles (c4) have an average particle size of less than 10 μm. The untreated metal oxide particles (c4) may be spherical particles, non-spherical particles, or a combination thereof. Preferably, the untreated metal oxide particles (c4) are untreated aluminum oxide particles, more preferably non-spherical untreated aluminum oxide particles. The isocyanate composition may contain the untreated metal oxide particles (c4) in an amount of zero to 4 wt.%, for example, 3.8 wt.% or less, 3.5 wt.% or less, 3.2 wt.% or less, 3 wt.% or less, 2.5 wt.% or less, 2 wt.% or less, 1.5 wt.% or less, 1 wt.% or less, or even 0.5 wt.% or less, based on the weight of the isocyanate composition. Preferably, the thermally conductive filler in the isocyanate composition consists of (c1), (c2), and (c3).

[0026] The total concentration of the thermally conductive filler in the isocyanate composition can be greater than 87% by weight, for example, 87.5% by weight or more, 88% by weight or more, 88.5% by weight or more, or even 89% by weight or more, and at the same time 92% by weight or less, 91.5% by weight or less, 91% by weight or less, 90.5% by weight or less, 90% by weight or less, or even 89.5% by weight or less, based on the total weight of the isocyanate composition. The isocyanate composition is storage stable, as indicated by a viscosity change of 50% or less or 45% or less after storage for 24 hours at 50° C. under a nitrogen atmosphere, especially when the isocyanate composition contains a total amount of thermally conductive filler of more than 87% of the isocyanate composition. The infrared spectrum of the isocyanate composition has a 1232 cm IR spectrum of 0.17 or less, 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, or even 0.12 or less. -1 Band at 2300cm -1 The peak height ratio for the band in the above can be shown. The band for determining the peak height ratio is as defined in the above section on surface-treated metal oxide particles (c2). The viscosity variation and peak height ratio are determined by the test methods described in the following section on examples.

[0027] The composition of the present invention may be a two-component curable composition further comprising a polyol composition. The two-component curable composition comprises a polyol composition as component A (also referred to as A part or A side) and an isocyanate composition as component B (also referred to as B part or B side). The polyol composition useful in the present invention comprises one or more polyether polyols. The polyether polyols in the polyol composition may have an average functionality of greater than 2.0 (>2.0). The average functionality refers to the average number of hydroxyl groups per molecule, i.e., the total moles of OH groups divided by the total moles of polyether polyols. The polyether polyols may have an average functionality of 2.1 or more, 2.2 or more, 2.3 or more, 2.4 or more, or even 2.5 or more, and at the same time 4.0 or less, 3.9 or less, 3.8 or less, 3.7 or less, 3.6 or less, 3.5 or less, 3.4 or less, 3.2 or less, 3.1 or less, 3.0 or less, 2.9 or less, 2.8 or less, or even 2.7 or less.

[0028] The polyether polyols useful in the present invention may contain one or more alkylene oxide units in the polyether polyol backbone. The alkylene oxide units may be ethylene oxide, propylene oxide, or a combination thereof. The polyether polyol may be a polyoxypropylene polyol, a polyoxyethylene polyol, a propylene oxide / ethylene oxide copolymer polyol, an ethylene oxide-capped polyether polyol, or a mixture thereof. Polyether polyols are, for example, water, organic dicarboxylic acids such as succinic acid, adipic acid, phthalic acid, terephthalic acid; or polyhydric alcohols (such as dihydric to pentahydric alcohols or dialkylene glycols), such as ethanediol, 1,2- and 1,3-propanediol, diethylene glycol, dipropylene glycol, 1,4-butanediol, 1,6-hexanediol, glycerol, trimethylolpropane, pentaerythritol, sorbitol, and sucrose, or blends thereof; linear and cyclic amine compounds which may also contain tertiary amines, such as ethanoldiamine, triethanolamine, ... The polyether polyols may be initiated with ethylene oxide-capped polyols, such as phenyl diamine, toluene diamine, various isomers of toluene diamine, methyldiphenylamine, aminoethylpiperazine, ethylenediamine, N-methyl-1,2-ethanediamine, N-methyl-1,3-propanediamine, N,N-dimethyl-1,3-diaminopropane, N,N-dimethylethanolamine, diethylenetriamine, bis-3-aminopropylmethylamine, aniline, aminoethylethanolamine, 3,3-diamino-N-methylpropylamine, N,N-dimethyldipropylenetriamine, aminopropylimidazole, and mixtures thereof; or combinations of at least two of these. The preparation of ethylene oxide-capped polyether polyols is well known in the art and generally involves the polymerization of propylene oxide using a hydroxyl or amine-containing initiator, followed by capping with ethylene oxide.

[0029] The polyether polyols useful in the present invention may have an average hydroxyl number of 5 to 500 milligrams of potassium hydroxide per gram of sample (mg KOH / g) or 50 to 400 mg KOH / g according to ASTM D4274-16. The polyether polyols may have an average equivalent weight of 140 or more, 200 or more, 300 or more, 400 or more, or even 500 or more, and at the same time 8,000 or less, 4,000 or less, 3,000 or less, 2,000 or less, or even 1,000 or less. Equivalent weight is the weight of polyol per reactive site. Equivalent weight is calculated by 56000 / (OH number (mg KOH / g)).

[0030] Polyether polyols useful in the present invention may include glycerol propoxylated polyether polyols, propylene glycol-initiated homopolymer polyols, or mixtures thereof. Examples include VORANOL™ CP450 polyol (VORANOL is a trademark of The Dow Chemical Company) and VORANOL 1000LM polyol, both available from The Dow Chemical Company.

[0031] Polyol compositions useful in the present invention may comprise polyether polyols in an amount of 20 wt% or more, 25 wt% or more, 30 wt% or more, 35 wt% or more, 40 wt% or more, 45 wt% or more, or even 50 wt% or more, and at the same time 100 wt% or less, 90 wt% or less, 85 wt% or less, 80 wt% or less, 75 wt% or less, 70 wt% or less, 65 wt% or less, or even 60 wt% or less, based on the total weight of polyols in the polyol composition.

[0032] The polyol composition useful in the present invention may comprise one or more polyester polyols. The polyester polyol may be an aromatic polyester polyol. The polyester polyol may be a reaction product of a polycarboxylic acid or anhydride thereof with a polyhydric alcohol. The polycarboxylic acid or anhydride may be aliphatic, cycloaliphatic, aromatic, and / or heterocyclic. Examples of suitable polycarboxylic acids and anhydrides thereof may include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, fumaric acid, glutaconic acid, α-hydromuconic acid, β-hydromuconic acid, α-butyl-α-ethyl-glutaric acid, α,β-diethylsuccinic acid, isophthalic acid, terephthalic acid, hemimellitic acid, and 1,4-cyclohexane-dicarboxylic acid; anhydrides thereof, such as phthalic anhydride; or mixtures thereof. The polyhydric alcohol may be aliphatic or aromatic. Examples of suitable polyhydric alcohols include ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 1,5-pentanediol, 1,4-pentanediol, 1,3-pentanediol, 1,6-hexanediol, 1,8-octanediol, neopentyl glycol, cyclohexanedimethanol, 1,7-heptanediol, glycerol, 1,1,1-trimethylolpropane, 1,1,1-trimethylolethane, hexane-1,2,6-triol, α-methyl glucoside, pentaerythritol, quinitol, mannitol, sorbitol, sucrose, methyl glucoside, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, dibutylene glycol, or blends thereof. Also included are compounds derived from phenol such as bisphenol A, bis(4,4'-hydroxyphenyl)sulfide, and 2,2-(4,4'-hydroxyphenyl)propane, commonly known as bis-(4,4'-hydroxyphenyl)sulfone.The polyester polyols may also include hybrid polyester polyols, such as the reaction product of a polyester polyol with an alkoxylating agent, such as propylene oxide. Examples of suitable hybrid polyester polyols include the reaction product of phthalic anhydride, a polyhydric alcohol, such as diethylene glycol, and propylene oxide.

[0033] Polyol compositions useful in the present invention may comprise polyester polyols in an amount of zero or more, 0.1 or more, 0.5 or more, 1 or more, 1.5 or more, 2 or more, 3 or more, 4 or more, 5 or more, or even 6 or more, and at the same time 20 or less, 18 or less, 15 or less, 12 or less, 10 or less, or even 8 or less, by weight, based on the total weight of polyols in the polyol composition.

[0034] The polyol compositions useful in the present invention may include one or more natural vegetable oil polyols, derivatives thereof, or mixtures thereof, including, for example, castor oil, which may be present in an amount of zero or more, 5 or more, 10 or more, 15 or more, or even 20 or more by weight, and at the same time, 50 or less, 45 or less, 40 or less, 35 or less, or even 30 or less by weight, based on the total weight of the polyols in the polyol composition.

[0035] The polyol composition useful in the present invention may include one or more chain extenders having two isocyanate-reactive groups and a hydrocarbon backbone. The chain extenders typically have a molecular weight of 200 grams per mole (g / mol) or less, for example, 80 to 120 g / mol. In this specification, "isocyanate-reactive group" includes any active hydrogen-containing moiety such as -OH and -SH. The backbone may further include one or more heteroatoms. The heteroatoms in the backbone may be oxygen, sulfur, or mixtures thereof. The chain extenders may include diols, particularly straight or branched chain diols having 9 or fewer carbon atoms. Examples of suitable chain extenders include ethanediol, propanediol, butanediol, hexanediol, heptanediol, octanediol, neopentyl glycol, or mixtures thereof. The chain extender may be present in an amount of zero or more, 1 or more, 2 or more, 3 or more, or even 5 or more by weight, and at the same time 20 or less, 18 or less, 15 or less, 12 or less, or even 10% or less by weight, based on the total weight of the polyols in the polyol composition.

[0036] Polyol compositions useful in the present invention may contain one or more polyoxyalkylene polyamines having two or more amines per polyamine, two to four amines per polyamine, or two to three amines per polyamine, such as the JEFFAMINE amine-terminated polyethers available from Huntsman Corporation. The polyoxyalkylene polyamines may be present in an amount of zero or more, 5 or more, or even 10 or more by weight, and simultaneously 40 or less, 30 or less, or even 20 or less by weight, based on the total weight of the polyol composition excluding thermally conductive filler.

[0037] The polyol composition useful in the present invention may comprise any one or any combination of the following thermally conductive fillers: spherical metal oxide particles (c1), surface-treated metal oxide particles (c2), additional thermally conductive fillers (c3), and untreated metal oxide particles (c4). The polyol composition may comprise (c1), (c2) and (c3), and optionally (c4). Alternatively, the polyol composition may comprise (c1), (c3) and (c4), such as non-spherical untreated metal oxide particles, and optionally (c2). The thermally conductive filler in the polyol composition may be the same as or different from the thermally conductive filler in the isocyanate composition. The polyol composition may comprise the spherical metal oxide particles (c1) in an amount of zero or more, 20 or more, 22 or more, 25 or more, 28 or more, 30 or more, 32 or more, 35 or more, 38 or more, 40 or more, 42 or more, 45 or more, 48 or more, 50 or more, 52 or more, 55 or more, or even 58 or more by weight, and at the same time 90 or less, 88 or less, 85 or less, 82 or less, 80 or less, 78 or less, 75 or less, 72 or less, 70 or less, or even 68 or less by weight, based on the weight of the polyol composition. The polyol composition may comprise the surface-treated metal oxide particles (c2) in an amount of zero or more, 5 wt.%, 10 wt.%, 12 wt.%, 15 wt.%, 17 wt.%, 19 wt.%, or even 20 wt.% or more, and at the same time 40 wt.%, 38 wt.%, 35 wt.%, 32 wt.%, 30 wt.%, 28 wt.%, or even 25 wt.%, based on the weight of the polyol composition.The polyol composition may comprise an additional thermally conductive filler (c3) in an amount of 1.5 wt.-% or more, 1.6 wt.-% or more, 1.7 wt.-% or more, 1.75 wt.-% or more, 2 wt.-% or more, 3 wt.-% or more, 4 wt.-% or more, 5 wt.-% or more, 5.5 wt.-% or more, 5.8 wt.-% or more, 6 wt.-% or more, 6.2 wt.-% or more, 6.5 wt.-% or more, 6.8 wt.-% or even 7 wt.-% or less, based on the weight of the polyol composition, while typically being present in an amount of 12 wt.-% or less, 11.5 wt.-% or less, 11 wt.-% or less, 10.5 wt.-% or less, 10 wt.-% or less, 9 wt.-% or less, or even 8 wt.-% or less. The polyol composition may comprise as additional thermally conductive filler (c3) zinc oxide particles in an amount of greater than or equal to zero, greater than or equal to 5.5 wt.-%, greater than or equal to 5.8 wt.-%, greater than or equal to 6 wt.-%, greater than or equal to 6.2 wt.-%, greater than or equal to 6.5 wt.-%, greater than or equal to 6.8 wt.-%, or even greater than or equal to 7 wt.-%, and at the same time less than or equal to 12 wt.-%, less than or equal to 11.5 wt.-%, less than or equal to 11 wt.-%, less than or equal to 10.5 wt.-%, or even less than or equal to 10 wt.-%, based on the weight of the polyol composition. The polyol composition may comprise as additional thermally conductive filler (c3) boron nitride particles in an amount of greater than or equal to zero, greater than or equal to 1.5 wt.%, greater than or equal to 1.6 wt.%, greater than or equal to 1.65 wt.%, greater than or equal to 1.7 wt.%, greater than or equal to 1.75 wt.%, greater than or equal to 1.8 wt.%, greater than or equal to 1.85 wt.%, greater than or equal to 1.9 wt.%, greater than or equal to 1.95 wt.%, and at the same time less than or equal to 4 wt.%, less than or equal to 3.5 wt.%, less than or equal to 3.0 wt.%, less than or equal to 2.5 wt.%, less than or equal to 2.4 wt.%, less than or equal to 2.2 wt.%, less than or equal to 2.1 wt.%, or even less than or equal to 2.0 wt.%, based on the weight of the polyol composition. The polyol composition may comprise untreated metal oxide particles (c4) in an amount of zero or more, 5 wt.-% or more, 10 wt.-% or more, 12 wt.-% or more, 15 wt.-% or more, or even 20 wt.-% or more, and at the same time 40 wt.-% or less, 38 wt.-% or less, 35 wt.-% or less, 32 wt.-% or less, or even 30 wt.-% or less, based on the weight of the polyol composition.

[0038] The two-component curable composition of the present invention comprises a total amount of thermally conductive fillers of more than 87 wt.%, such as 87.5 wt.% or more, 88 wt.% or more, 88.5 wt.% or more, or even 89 wt.% or more, and at the same time 92 wt.% or less, 91.5 wt.% or less, 91 wt.% or less, 90.5 wt.% or less, 90 wt.% or less, or even 89.5 wt.% or less, based on the total weight of the two-component curable composition. For example, the two-component curable composition may comprise a total amount of spherical metal oxide particles (c1) of 20% by weight or more, 22% by weight or more, 25% by weight or more, 28% by weight or more, 30% by weight or more, 32% by weight or more, 35% by weight or more, 38% by weight or more, 40% by weight or more, 42% by weight or more, 45% by weight or more, 48% by weight or more, 50% by weight or more, 52% by weight or more, 55% by weight or more, or even 58% by weight or more, and at the same time 90% by weight or less, 88% by weight or less, 85% by weight or less, 82% by weight or less, 80% by weight or less, 78% by weight or less, 75% by weight or less, 72% by weight or less, 70% by weight or less, or even 68% by weight or less, based on the total weight of the two-component curable composition. The two-component curable composition may comprise a total amount of surface-treated metal oxide particles (c2) of 10 wt.-%, 12 wt.-%, 15 wt.-%, 17 wt.-%, 19 wt.-%, or even 20 wt.-% or more, and at the same time 40 wt.-%, 38 wt.-%, 35 wt.-%, 32 wt.-%, 30 wt.-%, 28 wt.-%, or even 25 wt.-%, based on the total weight of the two-component curable composition.

[0039] The additional thermally conductive filler (c3) may be present in the two-component curable composition in an amount sufficient to provide the desired viscosity and satisfactory thermal conductivity as defined above, for example in a total amount of 1.5 wt.-% or more, 1.6 wt.-% or more, 1.7 wt.-% or more, 1.75 wt.-% or more, 2 wt.-% or more, 3 wt.-% or more, 4 wt.-% or more, 5 wt.-% or more, 5.5 wt.-% or more, 5.8 wt.-% or more, 6 wt.-% or more, 6.2 wt.-% or more, 6.5 wt.-% or more, 6.8 wt.-% or more, or even 7 wt.-% or more, and at the same time typically in a total amount of 12 wt.-% or less, 11.5 wt.-% or less, 11 wt.-% or less, 10.5 wt.-% or less, 10 wt.-% or less, 9 wt.-% or less, or even 8 wt.-% or less, based on the total weight of the two-component curable composition. If the additional thermally conductive filler (c3) comprises zinc oxide particles, the total concentration of zinc oxide particles in the two-component curable composition can be 5.5 wt.-% or more, 5.8 wt.-% or more, 6 wt.-% or more, 6.2 wt.-% or more, 6.5 wt.-% or more, 6.8 wt.-% or more, or even 7 wt.-% or more, and at the same time 12 wt.-% or less, 11.5 wt.-% or less, 11 wt.-% or less, 10.5 wt.-% or less, or even 10 wt.-% or less, based on the total weight of the two-component curable composition. When the additional thermally conductive filler (c3) comprises boron nitride particles, the total concentration of the boron nitride particles in the two-component curable composition can be 1.5 wt.% or more, for example 1.6 wt.% or more, 1.65 wt.% or more, 1.7 wt.% or more, 1.75 wt.% or more, 1.8 wt.% or more, 1.85 wt.% or more, 1.9 wt.% or more, 1.95 wt.% or more, and at the same time 4 wt.% or less, 3.5 wt.% or less, 3.0 wt.% or less, 2.5 wt.% or less, 2.4 wt.% or less, 2.2 wt.% or less, 2.1 wt.% or less, or 2.0 wt.% or less, based on the total weight of the two-component curable composition.

[0040] The two-component curable composition of the present invention may comprise a total amount of untreated metal oxide particles (c4) of greater than or equal to zero, greater than or equal to 5 wt.-%, greater than or equal to 10 wt.-%, greater than or equal to 12 wt.-%, greater than or equal to 15 wt.-%, or even greater than or equal to 20 wt.-%, and at the same time less than or equal to 40 wt.-%, less than or equal to 38 wt.-%, less than or equal to 35 wt.-%, less than or equal to 32 wt.-%, or even less than or equal to 30 wt.-%, based on the weight of the two-component curable composition.

[0041] In the two-component curable composition, the weight ratio of the total thermally conductive filler in the polyol composition to the total thermally conductive filler in the isocyanate composition may be zero or more, or may be in the range of 0.90 to 1.20, such as 0.91 or more, 0.92 or more, 0.93 or more, 0.94 or more, 0.95 or more, 0.96 or more, 0.97 or more, 0.98 or more, 0.99 or more, or even 1.0 or more, and at the same time 1.18 or less, 1.15 or less, 1.12 or less, 1.10 or less, 1.08 or less, 1.05 or less, 1.04 or less, 1.03 or less, 1.02 or less, or even 1.01 or less. Such weight ratio of the thermally conductive filler in the two components of the curable composition allows the volume ratio of the polyol component to the polyisocyanate component to be prepared in the range of 0.95 to 1.05, and allows the curable composition to be prepared by using conventional processing equipment to mix the two components, i.e., the polyol composition and the isocyanate composition. Thus, the mixing equipment for preparing each component of the curable composition can be the same size without special equipment design to reach other mixing ratios required by conventional two-component curable polyurethane compositions. The weight ratio of the total filler in the polyol composition to the total filler in the isocyanate composition can be the same as the weight ratio described above, i.e., the weight ratio of the total thermally conductive filler in the two components of the curable composition.

[0042] Surprisingly, it has been found that the weight ratio of the thermally conductive filler having an average particle size of 20 μm or more to the thermally conductive filler having an average particle size of 10 μm or less in the two-component curable composition or in each of the polyol composition and the isocyanate composition ("the weight ratio of large fillers to small fillers") can be within a certain range, and can significantly improve the flowability of the two-component curable composition without compromising the thermal conductivity properties.For example, the weight ratio of the large (more than 20 micrometers) filler to the small (10 micrometers or less) filler in the curable composition or in each of the polyol composition and the isocyanate composition can be 2.0 or more, for example, 2.05 or more, 2.1 or more, 2.2 or more, 2.3 or more, 2.4 or more, or even 2.45 or more, and at the same time, can be 4.0 or less, 3.9 or less, 3.8 or less, 3.7 or less, or even 3.6 or less. The weight ratio of the spherical metal oxide particles (c1) to the surface-treated metal oxide particles (c2) in the thermally conductive filler composition (C) can be in the same range as the weight ratio of the larger filler to the smaller filler, for example, in the range of 2.0 to 4.0. Significantly improved flowability herein refers to a viscosity at room temperature of 150 Pa.s or less, for example, 140 Pa.s or less, 130 Pa.s or less, 120 Pa.s or less, 110 Pa.s or less, 100 Pa.s or less, 90 Pa.s or less, or even 80 Pa.s or less, when measured within 30 minutes after mixing the two components of the curable composition according to the test method described in the Examples section below.

[0043] The two-component curable composition of the present invention may include one or more organosilanes, which are useful for adjusting the viscosity without impairing the cured strength of the curable composition. The cured strength of the two-component curable composition may be 0.5 megapascals (MPa) or more, 0.6 MPa or more, or even 0.7 MPa or more, as determined according to the test method described in the Examples section below. The organosilane may be present in the polyol composition and / or the isocyanate composition. The organosilane may include a silane having the formula RSi(OR2)3 or RR3Si(OR2)2, where R is an organic group, preferably an alkyl group having 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, which may optionally contain functional organic groups, such as, for example, mercapto, epoxy, acrylic, and methacrylic; or a silyl-terminated dimethylsiloxane group having the structure Me3SiO(SiMe2O)n--, where n may be an integer from 1 to 10 or 1 to 4; each R2 may independently be methyl, ethyl, or a combination thereof, and R3 may be an alkyl group having 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms. The organosilane may include one or more alkyltrialkoxysilanes, such as alkyltrimethoxysilanes, epoxy-functional alkoxysilanes, or mixtures thereof.

[0044] Suitable organosilanes useful in the present invention include, for example, alkyltrialkoxysilanes such as n-decyltrimethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, pentyltrimethoxysilane, hexyltrimethoxysilane, octyltrimethoxysilane, and methyltris(methoxyethoxy)silane; (meth)acrylic-functional alkoxysilanes such as 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, and 3-methacryloxypropyldimethylmethoxysilane; 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethylmethyldimethoxysilane, 4-oxiranylbutyritirnetoxysilane, 5-methylbutyritirnetoxysilane, 6-methylbutyritirnetoxysilane, 7-methylbutyritirnetoxysilane, 8-methylbutyritirnetoxysilane, 9-methylbutyritirnetoxysilane, 10-methylbutyritirnetoxysilane, 11-methylbutyritirnetoxysilane, 12-methylbutyritirnetoxysilane, 13-methylbutyritirnetoxysilane, 14-methylbutyritirnetoxysilane, 15-methylbutyritirnetoxysilane, 16-methylbutyritirnetoxysilane, 17-methylbutyritirnetoxysilane, 18-methylbutyritirnetoxysilane, 19-methylbutyritirnetoxysilane, 20-methylbutyritirnetoxysilane, 21-methylbutyritirnetoxysilane, 22-methylbutyritirnetoxysilane, 23-methylbutyritirnetoxysilane, 24-methylbutyritirnetoxysilane, 25-methylbutyritirnetoxysil silane, epoxy-functional alkoxysilanes such as 4-oxiranylbutyitriethoxysilane, 4-oxiranyibutylmethyldimethoxysilane, 8-oxiranyloctyltrimethoxysilane, 8-oxiranyloctyltriethoxysilane, and 8-oxiranyloctylmethyidimethoxysilane; mercapto-functional alkoxysilanes such as 3-mercaptopropyltrimethoxysilane and 3-mercaptopropylmethyidimethoxysilane; or mixtures thereof. Preferred organosilanes include n-decyltrimethoxysilane, glycidoxypropyltrimethoxysilane, or mixtures thereof.

[0045] The two-component curable composition of the present invention may comprise organosilane in an amount of zero to 20 wt.%, for example, 5 wt.% or more, 6.5 wt.% or more, 7 wt.% or more, 8 wt.% or more, 9 wt.% or more, 10 wt.% or more, 11 wt.% or more, or even 12 wt.% or more, and at the same time 20 wt.% or less, 19 wt.% or less, 18 wt.% or less, 17 wt.% or less, 16 wt.% or less, 15 wt.% or less, or even 14 wt.% or less, based on the total weight of the two-component curable composition.

[0046] The two-component curable composition of the present invention may include one or more catalysts for the reaction of isocyanate functional groups with isocyanate reactive groups. The catalyst may be present in the polyol composition, the isocyanate composition, or both. The catalyst may be any one or any combination of more than one selected from organotin compounds, metal alkanoates, tertiary amines, and diazabicyclo compounds. Examples of suitable organotin catalysts include alkyl tin oxides such as dibutyltin oxide, stannous alkanoates such as stannous octoate, dialkyl tin carboxylates, and tin mercaptides. Preferred organotin catalysts are dialkyl tin dicarboxylates or dialkyl tin dimercaptides. Examples of suitable metal alkanoates include bismuth octoate, bismuth neodecanoate, or mixtures thereof. Examples of suitable tertiary amines include dimorpholinodialkyl ethers, di((dialkylmorpholino)alkyl)ethers such as (di-(2-(3,5-dimethyl-morpholino)ethyl)ether), bis-(2-dimethylaminoethyl)ether, triethylenediamine, pentamethyldiethylenetriamine, N,N-dimethylcyclohexylamine, N,N-dimethylpiperazine, 4-methoxyethylmorpholine, N-methylmorpholine, N-ethylmorpholine, or mixtures thereof. The catalyst may be present in an amount of 0.006% to 5.0% by weight, 0.01% to 2.0% by weight, or 0.02% to 1.0% by weight, based on the total weight of the two-component curable composition.

[0047] In addition to the above components, the two-component curable composition of the present invention may further include one or more of the following additives: fillers other than thermally conductive fillers, pigments, adhesion promoters, plasticizers, stabilizers such as UV stabilizers, flame retardants, and antioxidants. These additives may be present in the polyol composition and / or the isocyanate composition in a total amount of zero to 10 wt%, 0.1 wt% to 5 wt%, or 0.5 wt% to 1 wt%, based on the total weight of the two-component curable composition.

[0048] The two-component curable compositions useful in the present invention have good processability as indicated by low viscosity at room temperature, for example, 230 Pa.s or less, 210 Pa.s or less, 200 Pa.s or less, 190 Pa.s or less, 180 Pa.s or less, 170 Pa.s or less, 160 Pa.s or less, 150 Pa.s or less, or even 140 Pa.s or less at room temperature. Preferably, the two-component curable composition has a viscosity of 150 Pa.s or less at room temperature. Viscosity herein is measured within 30 minutes after mixing the polyol and polyisocyanate components (components A and B) of the curable composition according to the test method described in the Examples section. The two-component curable composition is thermally conductive and upon curing forms a polyurethane material (i.e., the cured composition) with high thermal conductivity. In the present invention, "high thermal conductivity" means a thermal conductivity of 2.73 W / mK or greater, preferably 3.0 W / mK or greater, when measured according to the test methods described in the Examples section below.

[0049] The present invention also relates to a process for preparing the compositions of the present invention, which comprises mixing a polyisocyanate with a thermally conductive filler (C).

[0050] The present invention also provides a process for preparing a two-component curable composition, comprising mixing a polyol composition with an isocyanate composition and optionally the above-mentioned components to form a curable composition. The polyol composition and the isocyanate composition may be combined such that the molar ratio of isocyanate groups to isocyanate-reactive groups may range from 0.95:1 to 1.1:1, 0.96:1 to 1.05:1, or 1:1 to 1.02:1. At the same time, the volume ratio of the polyol composition to the isocyanate composition in the curable composition may be controlled within the range of 0.95:1 to 1.05:1, 0.96:1 to 1.04:1, 0.97:1 to 1.03:1, 0.98:1 to 1.02:1, or 0.99:1 to 1.01:1, or at a ratio of 1:1. Such volume ratios (i.e., consistent mix ratios) indicate that the two-component curable compositions can be prepared using existing processing equipment for conventional two-component polyurethane compositions. The weight ratio of the total thermally conductive filler in the polyol composition to the total thermally conductive filler in the isocyanate composition can be within the ranges described above, preferably within the range of 0.95 to 1.05.

[0051] The two components of the curable composition are reactive with each other and have adhesive properties when they are in contact or mixed during application, undergo a curing reaction, and the reaction product of the two components is a cured product that can bond certain substrates together. The two-component curable composition is useful as a gap filler or adhesive for electric vehicles. The two-component curable composition is particularly suitable for filling the space between plastic metal or glass for housing, support, or framework and liquid crystal display elements such as liquid crystal projectors, liquid crystal televisions, liquid crystal displays, or other liquid crystal devices; as a filling material between plastic or glass for housing, support, or framework and fluorescent display tubes; and as a filling material between power battery cells and plastic metal or glass for housing, support, or framework. The high thermal conductivity described above makes the curable composition useful in the present invention particularly suitable for use as a gap filler or adhesive for electric vehicle applications, such as the assembly of energy storage devices.

[0052] The present invention also provides a method of bonding a first substrate to a second substrate. The method includes (i) mixing an isocyanate composition with a polyol composition to form a two-component curable composition, (ii) applying the two-component curable composition to the surface of at least one of the substrates, (iii) contacting the two substrates with the curable composition present therebetween, and (iv) curing the curable composition. The two substrates useful in the present invention may be the same or different. One of the two substrates may be plastic, metal, alloy, glass, or a composite material. The surface of the substrate may be surface treated prior to application of the composition of the present invention. Any known surface treatment means that increases the number of polar groups present on the surface of a substrate, such as a plastic, may be used, including corona discharge and chemical etching. Generally, the two-component curable composition is applied at ambient temperature (e.g., 23-35°C) in the presence of atmospheric moisture. The curable composition after curing forms a durable bond between the substrates. Curing of the curable composition may be performed at ambient temperature or at elevated temperature (e.g., up to 80°C). Curing of the curable composition may be further accelerated by applying convection heat, infrared radiation, induction heating, microwave heating, and / or by increasing the amount of moisture in the atmosphere, such as by using a humidity chamber. EXAMPLES

[0053] Certain embodiments of the present invention will now be described in the following examples in which all parts and percentages are by weight unless otherwise specified. The following materials are used in the examples: DAM-40K spherical alumina (Al2O3) filler, available from Denka Company Limited, has a D50 particle size of 40 μm, an aspect ratio of greater than 0.9, and a thermal conductivity of 30 w / mk. DAM-40K surface treated spherical alumina filler treated with silane, available from Denka Company Limited, has a D50 particle size of 40 μm, an aspect ratio of greater than 0.9, and a thermal conductivity of 30 W / mk. MARTOXID™ TM2320 alkoxysilane pretreated alumina filler available from Huber Company has a D50 particle size of 2 μm, an aspect ratio of less than 0.8, and a thermal conductivity of 30 W / mK (MARTOXID is a trademark of Martinswerk GmbH). The P662SB alumina filler, available from Alteo Co., has a D50 particle size of 1.7 μm, an aspect ratio of less than 0.8, and a thermal conductivity of 30 W / mk. Zinc oxide (ZnO) filler available from ALCAN Co. has a D50 particle size of 0.2 μm and a thermal conductivity of 45 W / mK. BN PW-30 boron nitride (BN) filler available from Zibo Jonye Tech Ceramic Co. has a D50 particle size of 20 μm and a thermal conductivity of 70 W / mK. Castor oil, available from Fisher Aldrich, is an oil-based polyol. 1,4-butanediol (BDO), available from Fisher Aldrich, is used as the chain extender. STEPANPOL™ PDP-70 hybrid polyol, available from Stephan, is an ester modified difunctional polyether polyol (OH number: 70 mg KOH / g) (STEPANPOL is a trademark of the Stepan Company). Molecular sieves 3 Å are available from Grace.

[0054] All of the following materials are available from The Dow Chemical Company. VORANOL™ CP450 polyol is a glycerin propoxylated multifunctional polyether polyol with functionality 3 and OH number: 380 mg KOH / g. VORANOL 1000LM polyol is a difunctional polyether polyol with an OH content of 2.0 mmol / g. DOWSIL™ Z-6040 silane is glycidoxypropyltrimethoxysilane. DOWSIL Z-6210 silane is n-decyltrimethoxysilane. VORANOL 1045K isocyanate prepolymer, polyether-MDI prepolymer (NCO content: 10-12 wt%, functionality: 2). ISONATE™ 50 O,P'Pure MDI (MDI-50) is diphenylmethane diisocyanate. PAPI™ 27 isocyanate is a polymeric MDI with an equivalent weight of 137 g / mol and a functionality of 2.7. DOWSIL, ISONATE, and PAPI are all trademarks of The Dow Chemical Company.

[0055] In the examples and in determining the properties and characteristics described herein, the following standard analytical equipment and methods are used.

[0056] Thermal Conductivity Thermal conductivity is determined according to ISO 22007-2. The two-component polyurethane composition was cured in an oven at 50°C for 24 hours to form a cured sample. The thermal conductivity of the cured sample was measured by a Hot Disk 5465 equipped with a 3.189mm Kapton sensor (heat power: 350mW, time: 5 seconds, variation compensation enabled, using fine-tuned analysis, and 50-150 plot). Each sample was evaluated three times and the average thermal conductivity was calculated.

[0057] Average particle size and aspect ratio of filler The average particle size, ie, D50 particle size, and aspect ratio of the filler are determined using a Beckman Coulter laser diffraction particle size analyzer (Model LS 13 320) by averaging the particle sizes of 1,500 particles.

[0058] Viscosity test of two-component curable compositions Test The two components of the two-component curable composition (i.e., Part A and Part B) were mixed for 30 seconds using a SpeedMixer DAC 600.2 VAC provided by FlackTek Inc. (at 2,000 revolutions per minute (rpm) under vacuum (20 kilopascals)). The viscosity of the resulting mixture was measured within 30 minutes after mixing. The viscosity of the sample was determined using an ARES G2 using 25 millimeter (mm) parallel plates with a 0.6 mm gap. The flow sweep was performed from 0.01 to 10 s. -1 At room temperature for 1 s -1 The viscosity at that point was recorded.

[0059] Curing strength test The test two-component polyurethane compositions were allowed to cure for at least 72 hours at room temperature. The resulting cured samples were cut into Type 1A test specimens and evaluated for tensile strength according to the International Organization for Standardization ISO 527 standard (current as of the priority date of this document).

[0060] Density and volume ratio measurements The density of the test formulation was measured using a 37 milliliter (mL) standard density cup (PhysiTest 14001 supplied by EPK Co.) according to the International Organization for Standardization ISO 2811 standard (current as of the priority date of this document). The weight of the empty density cup was recorded in grams as W1. The test formulation was then filled into the cup and the filled weight was recorded in grams as W2. Density (g / mL) is calculated as follows: Density=(W2-W1) / 37. The volume ratio of part A to part B is determined by the following formula: Volume ratio (A / B) = density of part B / density of part A.

[0061] Viscosity Variation and Reflectance Fourier Transform Infrared (FTIR) Spectroscopy of Isocyanate Compositions Filler-containing isocyanate compositions were prepared by thoroughly mixing the filler with PAPI 27 polymeric MDI using a speed mixer at 2,000 rpm for 2 minutes at a filler loading of 20% to 50% by weight based on the weight of the isocyanate. The viscosity of the resulting isocyanate composition was measured and recorded as "viscosity (t0)". The isocyanate composition was then purged with nitrogen and stored in a 50°C oven for 24 hours, when the viscosity of the isocyanate composition was measured and recorded as "viscosity (t24)", followed by centrifugation at 4,000 rpm for 30 minutes to remove the liquid on top. The resulting sediment was measured using a reflectance FTIR (Perkin Elmer Spectrum 100) to obtain an IR absorption spectrum. The IR spectrum was measured at 1232 cm -1 Absorbance peak height at 2300 cm -1 The ratio of absorbance at t0 to the peak height was calculated. Viscosity variation was calculated by viscosity(t0) / viscosity(t24). The viscosity of the sample was determined using an ARES G2 using 25 millimeter (mm) parallel plates with a 0.6 mm gap. The flow sweep was performed from 0.01 to 10 s. -1 At room temperature for 1 s -1 The viscosity at that point was recorded.

[0062] Polyurethane compositions of Examples (Ex) 1 to 10 and Comparative Examples (Comp) 1 to 3 Preparation of Resin Mixture A: All materials in Resin Mixture A listed in Table 1-1 were added to a vial ("Vial A") and mixed at 2,000 rpm for 3 minutes using a SpeedMixer (Flektex Inc) to obtain Resin Mixture A. Vial A was then sealed.

[0063] Preparation of Resin Mixture B: All materials in Resin Mixture B listed in Table 1-2 were added to a separate vial ("Vial B") and mixed at 2,000 rpm for 3 minutes using a SpeedMixer to obtain Resin Mixture B. Vial B was then sealed.

[0064] According to the polyurethane composition shown in Tables 2-1 and 2-2, the thermally conductive filler of part A was added to resin mixture A and mixed under vacuum using a SpeedMixer at 2,000 rpm for 5 minutes to obtain part A. Vial A was then sealed. The thermally conductive filler of part B was added to resin mixture B and mixed under vacuum using a SpeedMixer at 2,000 rpm for 5 minutes to obtain part B. Vial B was then sealed. The obtained parts A and B were cooled to room temperature and then mixed under vacuum using a SpeedMixer at 2,000 rpm for 2 minutes in another vial to obtain a polyurethane composition, which was then sealed in the vial. The obtained polyurethane composition was evaluated for thermal conductivity and cured strength properties according to the test methods described above, and the results are shown in Tables 2-1 and 2-2.

[0065] As shown in Table 2-1, all of the polyurethane compositions of Examples 1-10 desirably had low viscosity (≦230 Pa·s) while providing thermal conductivity of 2.73 W / mK or greater. Of Examples 1-10, the polyurethane compositions of Examples 1-6 and 8-9 exhibited a better balance of high thermal conductivity (≧3.0 W / mK) and low viscosity (≦150 Pa·s at room temperature) compared to Example 7, which has a filler weight ratio of (c1) / (c2) of 0.975, or Example 10, which has a lower BN content. Furthermore, the polyurethane compositions of Examples 1-10 also have a part A / part B volume ratio in the range of 0.95-1.05 and can be handled using conventional polyurethane processing equipment. In contrast, as shown in Table 2-2, the polyurethane composition of Comparative Example 1, which has a total filler loading of 87 wt % (based on the total weight of the polyurethane composition), had poorer thermal conductivity. The polyurethane composition of Comparative Example 2, which does not contain ZnO and BN, had poorer thermal conductivity. The polyurethane composition of Comparative Example 3, in which P662SB untreated Al2O3 was used instead of TM2320 pretreated Al2O3, undesirably exhibited high viscosity.

[0066] [Table 1]

[0067] [Table 2]

[0068] [Table 3] * Abs: absolute value

[0069] [Table 4]

[0070] Isocyanate compositions with various loadings of fillers were prepared by mixing the fillers with aromatic polyisocyanate (pMDI), and the viscosity change and peak change in the IR spectrum after storage at 50°C for 24 hours were evaluated according to the above-mentioned test method. The results are shown in Table 3. -1 The height of the peak at 1232 cm in the IR spectrum corresponds to the amount of free NCO groups. -1 The peak height at 1232 cm corresponds to the amount of complex formed by the NCO groups and the filler. Only the precipitate was used for IR spectroscopy, so the peak height ratio (1232 cm -1 / 2300cm -1 ) represents the proportion of isocyanate groups reacted with the filler in the isocyanate residues (unreacted NCO groups) absorbed by the filler. As shown in Table 3, all of isocyanate compositions 1 to 6 containing an aromatic polyisocyanate and a filler containing BN, pretreated Al2O3, and / or ZnO had a higher IR peak ratio (1232 cm) than isocyanate composition 7 containing untreated Al2O3. -1 / 2300cm -1 ) (e.g., 0.12 or less) and showed less viscosity fluctuation and less reaction between the filler and the polyisocyanate.

[0071] [Table 5]

Claims

1. A two-component curable composition comprising an isocyanate composition and a polyol composition, The isocyanate composition contains a polyisocyanate and a thermally conductive filler composition (C), The thermally conductive filler composition comprises: (c1) spherical metal oxide particles having an average particle size of 20 μm or more; (c2) surface-treated metal oxide particles having an average particle size of more than 1 μm to 10 μm, the surface-treated metal oxide particles being treated with an alkoxysilane; (c3) an additional thermally conductive filler selected from the group consisting of metal oxide particles having an average particle size of 1 μm or less, a thermally conductive filler having a thermal conductivity of 40 W / mK or more and being other than metal oxide particles, or a mixture thereof; Including, the polyol composition comprises one or more polyether polyols having an average functionality greater than 2.0; A two-component curable composition, wherein the total concentration of thermally conductive fillers in said curable composition is greater than 87 wt%, based on the total weight of said curable composition.

2. 10. The composition of claim 1, wherein the total concentration of thermally conductive fillers in the isocyanate composition is greater than 87 weight percent, based on the weight of the isocyanate composition.

3. 3. The composition of claim 1 or 2, wherein the surface-treated metal oxide particles (c2) are treated with an alkyltrialkoxysilane, an alkyldialkoxysilane, a vinyltrialkoxysilane, a vinyldialkoxysilane, or a mixture thereof.

4. The composition according to any one of claims 1 to 3, wherein the surface-treated metal oxide particles (c2) are surface-treated aluminum oxide particles.

5. The composition according to any one of claims 1 to 4, wherein the weight ratio of the spherical metal oxide particles (c1) to the surface-treated metal oxide particles (c2) in the thermally conductive filler composition (C) is in the range of 2.0 to 4.

0.

6. The composition according to any one of claims 1 to 5, wherein the additional thermally conductive filler (c3) comprises zinc oxide particles, boron nitride particles, or a mixture thereof.

7. 7. The composition of any one of claims 1 to 6, wherein the polyol composition comprises one or more of the following thermally conductive fillers: the spherical metal oxide particles (c1), the surface-treated metal oxide particles (c2), the additional thermally conductive filler (c3), and (c4) untreated metal oxide particles having an average particle size of more than 1 μm and less than 20 μm.

8. The composition according to any one of claims 1 to 7, wherein the zinc oxide particles as the additional thermally conductive filler (c3) are present in the curable composition in a total amount of 5.5 wt.-% or more, based on the total weight of the curable composition.

9. The composition according to any one of claims 1 to 7, wherein the boron nitride particles as the additional thermally conductive filler (c3) are present in the curable composition in a total amount of 1.5 wt% or more, based on the total weight of the curable composition.

10. 8. The composition of any one of claims 1 to 7, wherein the two-component curable composition further comprises 6.5 wt% to 20 wt% of an alkyltrialkoxysilane, an epoxy-functional alkoxysilane, or a mixture thereof, based on the total weight of the curable composition.

11. The composition of any one of claims 1 to 7, wherein the volume ratio of the polyol composition to the isocyanate composition is from 0.95 to 1.

05.

12. 8. The composition of claim 1, wherein the weight ratio of total thermally conductive fillers in the polyol composition to total thermally conductive fillers in the isocyanate composition is in the range of 0.95 to 1.

05.

13. The composition of any one of claims 1 to 12, wherein the isocyanate composition comprises an aromatic polyisocyanate.

14. 14. A process for preparing the composition of any one of claims 1 to 13, comprising mixing the components of the thermally conductive filler composition (C) with the polyisocyanate and with a polyol composition.

Citation Information

Patent Citations

  • Closed isocyanate coupling agent and application thereof

    CN103819498A

  • Low volatility low oil permeability thermally conductive silicone grease filler and preparing method thereof

    CN108003625A

  • Preparation method of heat-conducting material

    CN110684170A

  • Polyurethane-based graphite-orientation-type heat-conducting interface material

    CN110684340A

  • Two-component polyurethane adhesive for adhering power batteries and preparation method of two-component polyurethane adhesive

    CN111019587A