Combustion System

A denitrification catalyst with vanadium oxide and a second metal oxide enhances nitrogen oxide reduction at low temperatures, addressing the limitations of conventional catalysts by achieving efficient denitrification in combustion systems.

JP7587225B2Active Publication Date: 2024-11-20THE CHUGOKU ELECTRIC POWER CO INC +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2019538444
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-03-07
Publication Date
2024-11-20
Estimated Expiration
2039-03-07

AI Technical Summary

Technical Problem

Conventional catalysts for nitrogen oxide reduction in fuel combustion exhaust gas exhibit low activity at low temperatures and are limited by the support of vanadium oxide to less than 1 wt% on titanium oxide, necessitating high operating temperatures and inefficient denitrification.

Method used

A denitrification catalyst comprising vanadium oxide as the main component with 1 wt% to 40 wt% of a second metal oxide, such as Co, W, Mo, Nb, Ce, Sn, or Fe, which enhances nitrogen oxide reduction efficiency even at low temperatures.

Benefits of technology

The catalyst achieves higher denitrification efficiency at temperatures below 200°C, effectively reducing nitrogen oxides in exhaust gas using ammonia as a reducing agent, thereby improving the efficiency and flexibility of combustion systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587225000015
    Figure 0007587225000015
  • Figure 0007587225000016
    Figure 0007587225000016
  • Figure 0007587225000017
    Figure 0007587225000017
Patent Text Reader

Abstract

Provided is a combustion system using a catalyst with a more satisfactory denitration efficiency at low temperatures during a selective catalytic reduction reaction having ammonia as the reductant, compared to prior art techniques. The combustion system is equipped with a combustion device for combusting a fuel, an exhaust route for flowing therethrough an exhaust gas generated by the fuel being combusted in the combustion device, a dust collection device disposed in the exhaust route and collecting the soot present in the exhaust gas, and a denitration device disposed in the exhaust route and eliminating nitrogen oxide from the exhaust gas by means of a denitration catalyst. The denitration device is disposed on the downstream side of the dust collection device in the exhaust route. The denitration catalyst has vanadium oxide as the main component. The denitration catalyst has a second metal oxide content of 1% to 40% by weight. In the denitration catalyst, the second metal is at least one metal element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a combustion system, and more particularly to a combustion system that purifies exhaust gas generated by the combustion of fuel by using a denitration catalyst. [Background technology]

[0002] Nitrogen oxides (NO, NO2, NO3, N2O, N2O3, N2O4, N2O5) are among the pollutants emitted into the atmosphere by fuel combustion. Nitrogen oxides cause acid rain, ozone layer destruction, photochemical smog, and other problems, and have serious effects on the environment and human body, so their treatment is an important issue.

[0003] As a technology for removing the above-mentioned nitrogen oxides, selective catalytic reduction reaction (NH3-SCR) using ammonia (NH3) as a reducing agent is known. As described in Patent Document 1, a catalyst that uses titanium oxide as a carrier and supports vanadium oxide is widely used as a catalyst for selective catalytic reduction reaction. Titanium oxide is considered to be the best carrier because it has low activity against sulfur oxides and is highly stable.

[0004] On the other hand, although vanadium oxide plays a major role in NH3-SCR, it oxidizes SO2 to SO3, so vanadium oxide could not be supported at more than about 1 wt%. Also, in conventional NH3-SCR, a catalyst in which vanadium oxide is supported on a titanium oxide carrier hardly reacts at low temperatures, so it had to be used at high temperatures of 350-400°C. However, in order to increase the freedom in designing devices and equipment that perform NH3-SCR and to improve their efficiency, there was a need to develop a catalyst that exhibits high nitrogen oxide reduction activity even at low temperatures.

[0005] Thereafter, the inventors discovered a zeolite having a vanadium pentoxide content of 43 wt % or more and a BET specific surface area of ​​30 m 2 / g or more and is usable for denitration at 200° C. or less (Patent Document 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2004-275852 A [Patent Document 2] Patent No. 6093101 Summary of the Invention [Problem to be solved by the invention]

[0007] The present inventors conducted extensive research to further improve upon the above-mentioned Patent Document 2, and as a result discovered a DeNOx catalyst that exhibits even better activity in reducing the nitrogen oxides.

[0008] An object of the present invention is to provide a combustion system using a catalyst that has better denitration efficiency at low temperatures compared to the prior art during selective catalytic reduction reaction using ammonia as a reducing agent. [Means for solving the problem]

[0009] The present invention relates to a combustion system comprising a combustion device that combusts fuel, an exhaust passage through which exhaust gas generated by the combustion of the fuel in the combustion device flows, a dust collector that is disposed in the exhaust passage and collects soot in the exhaust gas, and a denitration device that is disposed in the exhaust passage and removes nitrogen oxides from the exhaust gas using a denitration catalyst, wherein the denitration device is disposed downstream of the dust collector in the exhaust passage, the denitration catalyst is a denitration catalyst containing vanadium oxide as a main component, has a content of an oxide of a second metal of 1 wt% or more and 40 wt% or less, and the second metal is a denitration catalyst of at least one metal element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe.

[0010] Moreover, it is preferable that the combustion system further includes an air preheater that is disposed in the exhaust path and recovers heat from the exhaust gas, and the air preheater is disposed upstream of the dust collector.

[0011] The present invention also relates to a combustion system comprising a combustion device that combusts fuel, an exhaust passage through which exhaust gas generated by the combustion of the fuel in the combustion device flows, an air preheater that is disposed in the exhaust passage and recovers heat from the exhaust gas, and a denitration device that is disposed in the exhaust passage and removes nitrogen oxides from the exhaust gas using a denitration catalyst, wherein the denitration device is disposed downstream of the air preheater in the exhaust passage, the denitration catalyst is a denitration catalyst containing vanadium oxide as a main component, has a content of an oxide of a second metal of 1 wt% or more and 40 wt% or less, and the second metal is a denitration catalyst of at least one metallic element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe.

[0012] The present invention also relates to a combustion system comprising an internal combustion engine that combusts fuel, an exhaust passage through which exhaust gas generated by the combustion of the fuel in the internal combustion engine flows, an exhaust heat recovery device that is disposed in the exhaust passage and recovers exhaust heat from the exhaust gas discharged from the internal combustion engine, and a denitration device that is disposed in the exhaust passage and removes nitrogen oxides from the exhaust gas using a denitration catalyst, wherein the denitration device is disposed downstream of the exhaust heat recovery device in the exhaust passage, the denitration catalyst is a denitration catalyst containing vanadium oxide as a main component, has a content of an oxide of a second metal of 1 wt% or more and 40 wt% or less, and the second metal is a denitration catalyst of at least one metallic element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe.

[0013] It is also preferable that the exhaust heat recovery device includes a turbine unit and an exhaust gas economizer, the exhaust gas economizer generates steam using the exhaust gas discharged from the internal combustion engine and the exhaust gas supplied from the turbine unit as heat sources, and the turbine unit generates electricity using the exhaust gas discharged from the internal combustion engine and the steam supplied from the exhaust gas economizer. Effect of the Invention

[0014] The combustion system according to the present invention has a better denitration efficiency at low temperatures in a selective catalytic reduction reaction using ammonia as a reducing agent than the prior art. [Brief description of the drawings]

[0015] [Figure 1] 4 is a graph showing the NO conversion rate of vanadium catalysts containing and not containing a second metal according to each Example. [Diagram 2] 2 is a graph showing NO conversion rates for vanadium catalysts containing cobalt and vanadium catalysts not containing cobalt according to each example. [Diagram 3] 1 is a graph showing powder XRD patterns of vanadium catalysts containing cobalt according to each of the examples and comparative examples. [Figure 4] 1 is a graph showing Raman spectra of vanadium catalysts containing cobalt according to each example. [Figure 5A] 1 is a graph showing XPS spectra in the V2p region of vanadium catalysts containing cobalt according to each of Examples and Comparative Examples. [Figure 5B] 1 is a graph showing XPS spectra in the Co2p region of vanadium catalysts containing cobalt according to each of Examples and Comparative Examples. [Figure 6] 2 is a graph showing NO conversion rates for vanadium catalysts containing and not containing tungsten according to each example. [Figure 7] 1 is a graph showing powder XRD patterns of tungsten-containing vanadium catalysts according to each of Examples and Comparative Examples. [Figure 8] 1 is a graph showing the ratio of tungsten element in tungsten-containing vanadium catalysts according to each of Examples and Comparative Examples. [Figure 9] 2 is a graph showing NO conversion rates of vanadium catalysts containing tungsten and vanadium catalysts not containing tungsten according to an embodiment of the present invention. [Figure 10] 1 is a graph showing powder XRD patterns of tungsten-containing vanadium catalysts according to each of Examples and Comparative Examples. [Figure 11] 1 is a graph showing the ratio of tungsten element in tungsten-containing vanadium catalysts according to each of Examples and Comparative Examples. [Figure 12] 2 is a graph showing NO conversion rates of vanadium catalysts containing tungsten and vanadium catalysts not containing tungsten according to an embodiment of the present invention. [Figure 13] 2 is a graph showing the NO conversion rate of vanadium catalysts containing niobium and vanadium catalysts not containing niobium according to an embodiment of the present invention. [Figure 14] 1 is a graph showing the NO conversion rate of a vanadium catalyst containing carbon and cobalt according to an embodiment of the present invention and a vanadium catalyst according to a comparative example. [Figure 15] FIG. 1 is a diagram showing a configuration of a combustion system according to a first application example of the present invention. [Figure 16] FIG. 11 is a diagram showing the configuration of a combustion system according to a second application example of the present invention. [Figure 17] FIG. 11 is a diagram showing the configuration of a combustion system according to a third application example of the present invention. [Figure 18] FIG. 11 is a diagram showing the configuration of a combustion system according to a fourth application example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, a denitration catalyst according to an embodiment of the present invention will be described.

[0017] The denitration catalyst of the present invention is a denitration catalyst mainly composed of vanadium oxide, in which the content of an oxide of a second metal is 1 wt% or more and 40 wt% or less, and the second metal is at least one metal element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe. Such a denitration catalyst can exhibit a high denitration effect even in a low temperature environment, compared to conventionally used denitration catalysts such as vanadium / titanium catalysts.

[0018] First, the denitration catalyst of the present invention is mainly composed of vanadium oxide, which includes vanadium oxide (II) (VO), vanadium trioxide (III) (VO), vanadium tetroxide (IV) (VO), and vanadium pentoxide (V) (VO), and during the denitration reaction, the V element of vanadium pentoxide (VO) may be in the pentavalent, tetravalent, trivalent, or divalent form. The vanadium oxide is the main component of the denitration catalyst of the present invention, and may contain other substances within the range that does not impair the effects of the present invention, but it is preferable that the vanadium oxide is present in the denitration catalyst of the present invention in an amount of 50 wt% or more calculated as vanadium pentoxide, and more preferably, the vanadium oxide is present in the denitration catalyst of the present invention in an amount of 60 wt% or more calculated as vanadium pentoxide.

[0019] Secondly, the denitration catalyst of the present invention has a content of the second metal oxide of 1 wt% or more and 40 wt% or less, and by containing such an oxide of the second metal, it can exhibit a high denitration effect even in a low temperature environment, compared to conventional denitration catalysts such as vanadium / titanium catalysts. When impurities are introduced into the denitration catalyst of the present invention, amorphous parts are generated in the denitration catalyst, so that the crystal structure is not continuous, and the lines and faces in the crystal lattice are distorted, thereby exhibiting a high denitration effect, and it is presumed that the more the oxide of the second metal is present as an impurity, the higher the denitration effect will be.

[0020] In an embodiment of the present invention, in a selective catalytic reduction reaction using a denitration catalyst having a cobalt oxide content of 1 wt% to 10 wt% as the second metal oxide at a reaction temperature of 200°C or less, a NO conversion rate of 79% to 100% was observed in the absence of moisture, and a NO conversion rate of 38% to 90% was observed in the presence of moisture. On the other hand, in a selective catalytic reduction reaction at 200°C or less using a denitrification catalyst with a 0 wt% cobalt oxide content as the second metal oxide, a NO conversion rate of 76% was observed in the absence of moisture, and only 32% in the presence of moisture.

[0021] In addition, in a selective catalytic reduction reaction using a denitration catalyst with a tungsten oxide content of 12 wt% to 38 wt% as the second metal oxide at a reaction temperature of 200°C or less, a NO conversion rate of 83% to 96% was observed in the absence of moisture, and a NO conversion rate of 50% to 55% was observed in the presence of moisture. On the other hand, in a selective catalytic reduction reaction at 200°C or less using a denitrification catalyst with a tungsten oxide content of 0 wt% as the second metal oxide, a NO conversion rate of 76% was observed in the absence of moisture, and only 32% in the presence of moisture. In addition, in a selective catalytic reduction reaction at 200°C or less using a denitrification catalyst with a tungsten oxide content of 62 wt% to 100 wt% as the second metal oxide, the NO conversion rate was only 3 to 69% in the absence of moisture, and 0% to 29% in the presence of moisture.

[0022] In addition, in a selective catalytic reduction reaction using a denitration catalyst with a niobium oxide content of 2 wt% to 16 wt% as the second metal oxide, a NO conversion rate of 76 wt% to 97% was observed in the absence of moisture, and a NO conversion rate of 32% to 73% was observed in the presence of moisture.

[0023] In the above description, the content of the second metal oxide in the denitration catalyst of the present invention is 1 wt% or more and 40 wt% or less, but it is preferably 3 wt% or more and 38 wt% or less. The content of the second metal oxide is more preferably 3 wt% or more and 10 wt% or less. The content of the second metal oxide is more preferably 5 wt% or more and 10 wt% or less. The content of the second metal oxide is more preferably 5 wt% or more and 8 wt% or less. The content of the second metal oxide is more preferably 6 wt% or more and 8 wt% or less. The content of the second metal oxide is more preferably 6 wt% or more and 7 wt% or less.

[0024] Third, the second metal is at least one metal element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe. This disrupts the crystal structure of vanadium oxide and increases Lewis acidity. In particular, Co, Mo, Ce, Sn, Ni, and Fe promote the redox cycle of V2O5. Among these elements, Co is known to have strong oxidizing power. W, Mo, and Nb all function as solid acids and provide adsorption sites for ammonia, allowing ammonia to efficiently come into contact with and react with NO.

[0025] In an embodiment of the present invention, in a selective catalytic reduction reaction using a denitration catalyst containing 3.1 wt% cobalt oxide as the second metal oxide at a reaction temperature of 200°C or less, a NO conversion rate of 94.6% was observed in the absence of moisture, and a NO conversion rate of 69.4% was observed in the presence of moisture. In addition, in an embodiment of the present invention, in a selective catalytic reduction reaction using a denitration catalyst containing 8.4 wt% tungsten oxide as the second metal oxide at a reaction temperature of 200°C or less, a NO conversion rate of 92% was observed in the absence of moisture, and a NO conversion rate of 64% was observed in the presence of moisture. In addition, in an embodiment of the present invention, in a selective catalytic reduction reaction using a denitration catalyst containing 5.4 wt% molybdenum oxide as the second metal oxide at a reaction temperature of 200°C or less, a NO conversion rate of 97% was observed in the absence of moisture, and a NO conversion rate of 62% was observed in the presence of moisture. In addition, in an embodiment of the present invention, in a selective catalytic reduction reaction using a denitration catalyst containing 5.0 wt% niobium oxide as the second metal oxide at a reaction temperature of 200°C or less, a NO conversion rate of 96.7% was observed in the absence of moisture, and a NO conversion rate of 61.7% was observed in the presence of moisture. In addition, in an embodiment of the present invention, in a selective catalytic reduction reaction using a denitration catalyst containing 6.4 wt% cesium oxide as the second metal oxide at a reaction temperature of 200°C or less, a NO conversion rate of 89.8% was observed in the absence of moisture, and a NO conversion rate of 52.9% was observed in the presence of moisture. In addition, in an embodiment of the present invention, in a selective catalytic reduction reaction using a denitration catalyst containing 5.6 wt% tin oxide as the second metal oxide at a reaction temperature of 200°C or less, a NO conversion rate of 88.1% was observed in the absence of moisture, and a NO conversion rate of 45.5% was observed in the presence of moisture. In addition, in an embodiment of the present invention, in a selective catalytic reduction reaction using a denitration catalyst containing 2.9 wt% nickel oxide as the second metal oxide at a reaction temperature of 200°C or less, a NO conversion rate of 81.9% was observed in the absence of moisture, and a NO conversion rate of 37.9% was observed in the presence of moisture. In addition, in an embodiment of the present invention, in a selective catalytic reduction reaction using a denitration catalyst having an iron oxide content of 3.1 wt% as the second metal oxide at a reaction temperature of 200°C or less, a NO conversion rate of 74.5% was observed in the absence of moisture, and a NO conversion rate of 33.9% was observed in the presence of moisture. On the other hand, in a selective catalytic reduction reaction at 200°C or less using a denitrification catalyst that did not contain an oxide of the second metal, a NO conversion rate of 75.5% was observed in the absence of moisture, and only 32% in the presence of moisture.

[0026] In addition, the denitration catalyst of the present invention is preferably used for denitration at 300°C or less. This is because the calcination temperature of the denitration catalyst of the present invention is 300°C. On the other hand, in the examples described later, the denitration catalyst of the present invention exhibited a high denitration effect in a selective catalytic reduction reaction at a reaction temperature of 200°C or less, so the denitration catalyst of the present invention can be used for denitration at 200°C or less. Since oxidation of SO2 to SO3 does not occur at 200°C or less, as found in the above Patent Document 2, oxidation of SO2 to SO3 does not occur during the selective catalytic reduction reaction.

[0027] In the above description, the denitration catalyst of the present invention is preferably used for denitration at 300° C. or less, but it may be preferably used for denitration at 200° C. or less, more preferably for denitration at a reaction temperature of 100-200° C. More preferably, it may be used for denitration at a reaction temperature of 160-200° C. Alternatively, it may be used for denitration at a reaction temperature of 80-150° C.

[0028] Moreover, it is preferable that the denitration catalyst of the present invention further contains carbon. In particular, it is preferable that the carbon content is 0.05 wt% or more. More preferably, the carbon content may be 0.07 wt% or more. Even more preferably, the carbon content may be 0.11 wt% or more. Even more preferably, the carbon content may be 0.12 wt% or more. Even more preferably, the carbon content may be 0.14 wt% or more. Even more preferably, the carbon content may be 0.16 wt% or more. Even more preferably, the carbon content may be 0.17 wt% or more. Even more preferably, the carbon content may be 0.70 wt% or more. By containing carbon, it is possible to exhibit a high denitration effect even in a low temperature environment, compared to conventional denitration catalysts such as vanadium / titanium catalysts. When impurities are introduced into the denitration catalyst of the present invention, amorphous parts are generated in the denitration catalyst, causing the crystal structure to be discontinuous, and the lines and faces in the crystal lattice are distorted, thereby exhibiting a high denitration effect. It is presumed that the presence of carbon as an impurity results in the high denitration effect.

[0029] Hereinafter, a method for producing a denitration catalyst containing vanadium oxide as a main component, in which the content of an oxide of a second metal is 1 wt% or more and 40 wt% or less, and the second metal is at least one metallic element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe, will be described.

[0030] The method for producing the above-mentioned DeNOx catalyst includes a step of calcining a mixture of a vanadate, a chelate compound, and a compound of a second metal. As the vanadate, for example, ammonium vanadate, magnesium vanadate, strontium vanadate, barium vanadate, zinc vanadate, lead vanadate, lithium vanadate, etc. may be used. In addition, examples of chelating compounds that may be used include those having multiple carboxyl groups, such as oxalic acid and citric acid, those having multiple amino groups, such as acetylacetonate and ethylenediamine, and those having multiple hydroxyl groups, such as ethylene glycol. The compound of the second metal may be a chelate complex, a hydrate, an ammonium compound, or a phosphate compound. The chelate complex may be, for example, a complex of oxalic acid or citric acid. The hydrate may be, for example, (NH4) 10 W 12 O 41 5H2O and H3PW 12 O 40 ·nH2O. The ammonium compound may be, for example, (NH4) 10 W 12 O 41 5H2O. Examples of phosphate compounds include H3PW 12 O 40 ·nH2O may be used.

[0031] The mixture preferably further contains ethylene glycol.

[0032] The denitration catalysts produced by these methods can exhibit a high denitration effect even in a low-temperature environment, compared to conventional denitration catalysts such as vanadium / titanium catalysts. When impurities are introduced into the denitration catalyst of the present invention, amorphous parts are generated in the denitration catalyst, causing the crystal structure to be discontinuous, and the lines and faces in the crystal lattice are distorted, thereby exhibiting a high denitration effect. It is presumed that the more carbon present as an impurity, the higher the denitration effect.

[0033] In an embodiment of the present invention, a denitration catalyst produced by a method of calcining a mixture of ammonium vanadate, oxalic acid, and an oxalate complex of a second metal exhibited a NO conversion rate of 74.5 to 100% in the absence of moisture, and a NO conversion rate of 33.9 to 90% in the presence of moisture. In addition, the denitrification catalyst produced by the method in which the above mixture further contained ethylene glycol showed a NO conversion rate of 100% in the absence of moisture and a NO conversion rate of 89% in the presence of moisture. On the other hand, a denitration catalyst produced by a method not including such a step, for example, a denitration catalyst produced by a method in which ammonium vanadate and oxalic acid are mixed but no oxide of a second metal is mixed and then calcined, showed a NO conversion rate of only 76% in the absence of moisture and a NO conversion rate of only 32% in the presence of moisture.

[0034] Moreover, the above-mentioned firing is preferably carried out at a temperature of 270° C. or less. When the denitration catalyst according to this embodiment is produced, it is calcined at a temperature of 270°C or lower, which is lower than the usual temperature of 300°C, and this causes localized disorder in the structure of the vanadium pentoxide crystals contained in the denitration catalyst, enabling it to exhibit a high denitration effect, and it is presumed that a particularly high denitration effect is exhibited due to the appearance of sites in the vanadium pentoxide crystal structure where oxygen atoms are deficient. The "sites where oxygen atoms are deficient" are also referred to as "oxygen deficiency sites."

[0035] The denitration catalyst prepared in this manner is a denitration catalyst mainly composed of vanadium oxide, the content of the oxide of a second metal is 1 wt% or more and 40 wt% or less, and the second metal is at least one metallic element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe.

[0036] The present invention is not limited to the above-described embodiment, and includes modifications and improvements within the scope of the present invention that can achieve the object of the present invention. EXAMPLES

[0037] EXAMPLES The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0038] <1 Vanadium catalyst containing various metals as the second metal> <1.1 Examples and Comparative Examples>

[0039] [Example 1] A precursor complex was synthesized by dissolving 4.96g (42.4mmol) of ammonium vanadate (NH4VO3) and 11.5g (127.6mmol) of oxalic acid ((COOH)2) in pure water. To this precursor complex, an oxalic acid complex of the second metal, cobalt (Co), was added so that the cobalt (Co) was 3.5mol% in terms of metal atoms, that is, the Co3O4 was 3.1wt% in terms of metal oxide. The obtained vanadium-heterometal complex mixture was fired twice in an electric furnace at 300℃ for 4 hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing cobalt (Co).

[0040] [Example 2] A precursor complex was synthesized by dissolving 4.96g (42.4mmol) of ammonium vanadate (NH4VO3) and 11.5g (127.6mmol) of oxalic acid ((COOH)2) in pure water. To this precursor complex, an oxalic acid complex of the second metal, tungsten (W), was added so that tungsten (W) was 3.5mol% in terms of metal atoms, that is, WO3 was 8.4wt% in terms of metal oxide. The obtained vanadium-heterometal complex mixture was fired twice in an electric furnace at a temperature of 300℃ for 4 hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing tungsten (W).

[0041] [Example 3] A precursor complex was synthesized by dissolving 4.96g (42.4mmol) of ammonium vanadate (NH4VO3) and 11.5g (127.6mmol) of oxalic acid ((COOH)2) in pure water. To this precursor complex, an oxalic acid complex of the second metal, molybdenum (Mo), was added so that the molybdenum (Mo) content was 3.5mol% in terms of metal atoms, i.e., the MoO3 content was 5.4wt% in terms of metal oxide. The resulting vanadium-heterometal complex mixture was fired twice in an electric furnace at 300℃ for 4 hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing molybdenum (Mo).

[0042] [Example 4] A precursor complex was synthesized by dissolving 4.96g (42.4mmol) of ammonium vanadate (NH4VO3) and 11.5g (127.6mmol) of oxalic acid ((COOH)2) in pure water. To this precursor complex, an oxalic acid complex of the second metal, niobium (Nb), was added so that the metal atom equivalent of niobium (Nb) was 3.5mol%, that is, the metal oxide equivalent of Nb2O5 was 5.0wt%. The obtained vanadium-heterometal complex mixture was fired twice in an electric furnace at 300℃ for 4 hours to obtain a denitrification catalyst of vanadium pentoxide (V2O5) containing niobium (Nb).

[0043] [Example 5] A precursor complex was synthesized by dissolving 4.96g (42.4mmol) of ammonium vanadate (NH4VO3) and 11.5g (127.6mmol) of oxalic acid ((COOH)2) in pure water. To this precursor complex, an oxalic acid complex of the second metal, cesium (Ce), was added so that the metal atom amount of cesium (Ce) was 3.5mol%, that is, the metal oxide amount of CeO2 was 6.4wt%. The obtained vanadium-heterometal complex mixture was fired twice in an electric furnace at 300℃ for 4 hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing cesium (Ce).

[0044] [Example 6] A precursor complex was synthesized by dissolving 4.96g (42.4mmol) of ammonium vanadate (NH4VO3) and 11.5g (127.6mmol) of oxalic acid ((COOH)2) in pure water. To this precursor complex, an oxalic acid complex of tin (Sn), the second metal, was added so that tin (Sn) was 3.5mol% in terms of metal atoms, that is, SnO2 was 5.6wt% in terms of metal oxide. The obtained vanadium-heterometal complex mixture was fired twice in an electric furnace at a temperature of 300℃ for 4 hours to obtain a denitrification catalyst of vanadium pentoxide (V2O5) containing tin (Sn).

[0045] [Example 7] A precursor complex was synthesized by dissolving 4.96g (42.4mmol) of ammonium vanadate (NH4VO3) and 11.5g (127.6mmol) of oxalic acid ((COOH)2) in pure water. To this precursor complex, 0.113g of nickel (Ni) as nickel carbonate, the second metal, was added so that the nickel (Ni) was 3.5mol% in terms of metal atoms, that is, NiO was 2.9wt% in terms of metal oxide. The obtained vanadium-heterometal complex mixture was fired twice in an electric furnace at a temperature of 300℃ for 4 hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing nickel (Ni).

[0046] [Example 8] A precursor complex was synthesized by dissolving 4.96g (42.4mmol) of ammonium vanadate (NH4VO3) and 11.5g (127.6mmol) of oxalic acid ((COOH)2) in pure water. To this precursor complex, an oxalic acid complex of the second metal, iron (Fe), was added so that the iron (Fe) was 3.5mol% in terms of metal atoms, that is, the Fe2O3 was 3.1wt% in terms of metal oxide. The obtained vanadium-heterometal complex mixture was fired twice in an electric furnace at a temperature of 300℃ for 4 hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing iron (Fe).

[0047] [Comparative Example 1] A precursor complex was synthesized by dissolving 4.96g (42.4mmol) of ammonium vanadate (NH4VO3) and 11.5g (127.6mmol) of oxalic acid ((COOH)2) in pure water. This precursor complex was calcined twice for 4 hours at 300℃ in an electric furnace to obtain a vanadium pentoxide (V2O5) denitrification catalyst that does not contain a second metal.

[0048] <1.2 Evaluation> <1.2.1 NO conversion rate> The NH3-SCR reaction was carried out using a fixed-bed flow-type catalytic reactor at a reaction temperature of 150°C under the conditions in Table 1 below. NO in the gas that passed through the catalyst layer was analyzed using a Jasco FT-IR-4700.

[0049] [Table 1]

[0050] The NO conversion rate was calculated by the following formula (1). in is the NO concentration at the reactor inlet, NO out is the NO concentration at the reactor outlet.

number

[0051] (Measurement results) Table 2 shows the NO conversion rates for each vanadium pentoxide catalyst in both the absence and presence of moisture. Figure 1 is a graph of Table 2. [Table 2]

[0052] In both the case where moisture is not present and the case where moisture is present, the denitration catalysts of the Examples generally exhibited higher NO conversion rates than the denitration catalysts of the Comparative Examples. In particular, the denitration catalysts obtained by adding cobalt, tungsten, molybdenum, and niobium to ammonium vanadate and then calcining the mixture exhibited high NO conversion rates. Among these, Example 3 (molybdenum added) exhibited the highest NO conversion rate in the case where moisture is not present, and Example 1 (cobalt added) exhibited the highest NO conversion rate in the case where moisture is present.

[0053] <2 Vanadium catalyst containing cobalt as the second metal> <2.1 Examples>

[0054] As described above, in the vanadium catalysts of Examples 1 to 8, in the case where moisture coexists, Example 1 (cobalt added) showed the highest NO conversion rate, so the vanadium catalysts of the following Examples were produced by changing the amount of cobalt added.

[0055] [Example 9] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, cobalt (Co), was added so that the metal oxide equivalent was 1 wt% Co3O4. The resulting vanadium-cobalt complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing cobalt (Co).

[0056] [Example 10] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, cobalt (Co), was added so that the metal oxide equivalent was 3 wt% Co3O4. The resulting vanadium-cobalt complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing cobalt (Co).

[0057] [Example 11] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, cobalt (Co), was added so that the metal oxide equivalent was 5 wt% Co3O4. The resulting vanadium-cobalt complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing cobalt (Co).

[0058] [Example 12] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, cobalt (Co), was added so that the metal oxide equivalent was 6 wt% Co3O4. The resulting vanadium-cobalt complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing cobalt (Co).

[0059] [Example 13] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, cobalt (Co), was added so that the metal oxide equivalent was 7 wt% Co3O4. The resulting vanadium-cobalt complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing cobalt (Co).

[0060] [Example 14] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, cobalt (Co), was added so that the metal oxide equivalent was 8 wt% Co3O4. The resulting vanadium-cobalt complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing cobalt (Co).

[0061] [Example 15] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex, which is the precursor of the second metal, cobalt (Co), was added so that the metal oxide equivalent was 10 wt% Co3O4. The resulting vanadium-cobalt complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing cobalt (Co).

[0062] The following Table 3 shows the amounts of precursors charged when cobalt was introduced in Examples 9 to 15. [Table 3] <2.2 Evaluation> <2.2.1 NO conversion rate> (Measurement method) Under the conditions in Table 1 above, the NH3-SCR reaction was carried out using a fixed-bed flow-type catalytic reactor at a reaction temperature of 150°C. NO in the gas that passed through the catalyst layer was analyzed using a Jasco FT-IR-4700. The NO conversion rate was calculated according to the above formula (1).

[0063] (Measurement results) Table 4 shows the NO conversion rates for each vanadium oxide catalyst in both the absence and presence of moisture. Figure 2 is a graph of Table 4. [Table 4]

[0064] In both the absence and presence of moisture, the denitration catalysts of the Examples all exhibited higher NO conversion rates than the denitration catalysts of the Comparative Examples. In particular, in the absence of moisture, Example 12 (6 wt%) and Example 13 (7 wt%) exhibited the highest NO conversion rates, while in the presence of moisture, Example 14 (8 wt%) exhibited the highest NO conversion rate.

[0065] <2.2.2 Powder X-ray diffraction> (Diffraction method) Powder X-ray diffraction was performed using Cu-Kα on a Rigaku smart lab.

[0066] (Diffraction results) FIG. 3 shows powder XRD (X-Ray Diffraction) patterns of Example 9 (1 wt%), Example 10 (3 wt%), Example 12 (6 wt%), Example 15 (10 wt%), and Comparative Example 1 (None: 0 wt%). It was shown that the stable phase V2O5 exists as the main component, and with increasing Co addition, the Co3O4 phase also appears.

[0067] <2.2.3 Raman spectrum> (Measurement method) In order to analyze the crystal structure of each vanadium pentoxide catalyst, the Raman spectrum was measured by Raman spectroscopy. More specifically, a small amount of each catalyst sample was placed on a slide glass, and the Raman spectrum was measured using a Raman spectrometer. The measuring device used was a JASCO NRS-4100 Raman spectrophotometer.

[0068] (Measurement results) Figure 4 shows the Raman spectrum of each catalyst. It was shown that increasing the amount of Co added disrupts the crystal structure of V2O5, weakening the pattern intensity.

[0069] <2.2.4 X-ray photoelectron spectrum (XPS) measurement> (Measurement method) X-ray photoelectron spectrum (XPS: X-Ray Photoelectron Spectrum) was measured to analyze the electronic state of Example 9 (1 wt%), Example 10 (3 wt%), Example 12 (6 wt%), Example 15 (10 wt%), and Comparative Example 1 (None: 0 wt%). More specifically, the powder sample of the catalyst of each Example and Comparative Example was fixed to a sample holder using carbon tape, and the X-ray photoelectron spectrum was measured. The measurement device used was a JPS-9010MX photoelectron spectrometer manufactured by JEOL Ltd.

[0070] (Measurement results) FIG. 5A shows the XPS spectrum in the V2p region. FIG. 5B shows the XPS spectrum in the Co2p region. When the amount of Co added is increased, the V 4+ and Co 2+ It was shown that the components increased.

[0071] <3 Vanadium catalyst containing tungsten as the second metal> <3.1 Examples> As described above, in the vanadium catalysts of Examples 1 to 8, Example 2 (tungsten added) showed the second highest NO conversion rate when moisture coexisted, so the vanadium catalysts of the following Examples were produced by changing the amount of tungsten added. In addition to simply changing the amount of tungsten added, as described later, the vanadium catalysts of the following Examples were produced by using K2WO4 and H3PW as precursors. 12 O 40 In each case where nH2O was used, the amount of tungsten added was changed.

[0072] [Example 16] To a mixture of ammonium vanadate (NH4VO3), 43.9 mmol of K2WO4, and 20 ml of pure water, 11.9 g (131.7 mmol) of oxalic acid ((COOH)2) was added, and the mixture was stirred at room temperature for 10 minutes, and then at 70°C for 12 hours. This precursor sample was calcined at 300°C for 4 hours to obtain a vanadium pentoxide (V2O5) denitration catalyst containing tungsten (W). The amount of ammonium vanadate used as a raw material was adjusted so that the total weight ratio of WO3 in the resulting denitration catalyst was 4.9 wt%.

[0073] [Example 17] To a mixture of ammonium vanadate (NH4VO3), 43.9 mmol of K2WO4, and 20 ml of pure water, 11.9 g (131.7 mmol) of oxalic acid ((COOH)2) was added, and the mixture was stirred at room temperature for 10 minutes, and then at 70°C for 12 hours. This precursor sample was calcined at 300°C for 4 hours to obtain a vanadium pentoxide (V2O5) denitration catalyst containing tungsten (W). The amount of ammonium vanadate used as a raw material was adjusted so that the total weight ratio of WO3 in the resulting denitration catalyst was 11.8 wt%.

[0074] [Example 18] 11.9g (131.7mmol) of oxalic acid was added to a mixture of ammonium vanadate (NH4VO3), 43.9mmol of K2WO4, and 20ml of pure water, and the mixture was stirred at room temperature for 10 minutes, and then at 70℃ for 12 hours. This precursor sample was calcined at 300℃ for 4 hours to obtain a vanadium pentoxide (V2O5) denitration catalyst containing tungsten (W). The amount of ammonium vanadate used as a raw material was adjusted so that the total weight ratio of WO3 in the denitration catalyst produced was 22.1wt%.

[0075] [Comparative Example 2] To a mixture of ammonium vanadate (NH4VO3), 43.9 mmol of K2WO4, and 20 ml of pure water, 11.9 g (131.7 mmol) of oxalic acid ((COOH)2) was added, and the mixture was stirred at room temperature for 10 minutes, and then stirred at 70°C for 12 hours. This precursor sample was calcined at 300°C for 4 hours to obtain a vanadium pentoxide (V2O5) denitration catalyst containing tungsten (W). The amount of ammonium vanadate used as a raw material was adjusted so that the total weight ratio of WO3 in the denitration catalyst produced was approximately 100 wt%.

[0076] The following Table 5 shows the amounts of precursors charged when tungsten was introduced in Examples 16 to 18 and Comparative Example 2. [Table 5]

[0077] [Example 19] Ammonium vanadate (NH4VO3) and H3PW 12 O 40 To a mixture of 1.5 nH2O and 20 ml of pure water, 11.9 g (131.7 mmol) of oxalic acid ((COOH)2) was added, and the mixture was stirred at room temperature for 10 minutes, and then stirred at 70°C for 12 hours. This precursor sample was calcined at 300°C for 4 hours to obtain a vanadium pentoxide (V2O5) denitration catalyst containing tungsten (W). The raw materials ammonium vanadate and H3PW were adjusted so that the total weight ratio of WO3 in the denitration catalyst produced was 38.4 wt%. 12 O 40 -Adjusted the amount of nH2O.

[0078] [Comparative Example 3] Ammonium vanadate (NH4VO3) and H3PW 12 O 40To a mixture of 1.5 nH2O and 20 ml of pure water, 11.9 g (131.7 mmol) of oxalic acid ((COOH)2) was added, and the mixture was stirred at room temperature for 10 minutes, and then at 70°C for 12 hours. This precursor sample was calcined at 300°C for 4 hours to obtain a vanadium pentoxide (V2O5) denitration catalyst containing tungsten (W). The raw materials, ammonium vanadate and H3PW, were adjusted so that the total weight ratio of WO3 in the denitration catalyst produced was 61.7 wt%. 12 O 40 -Adjusted the amount of nH2O.

[0079] [Comparative Example 4] Ammonium vanadate (NH4VO3) and H3PW 12 O 40 To a mixture of 1.5 nH2O and 20 ml of pure water, 11.9 g (131.7 mmol) of oxalic acid ((COOH)2) was added, and the mixture was stirred at room temperature for 10 minutes, and then stirred at 70°C for 12 hours. This precursor sample was calcined at 300°C for 4 hours to obtain a vanadium pentoxide (V2O5) denitration catalyst containing tungsten (W). The raw materials ammonium vanadate and H3PW were adjusted so that the total weight ratio of WO3 in the denitration catalyst produced was 77.3 wt%. 12 O 40 -Adjusted the amount of nH2O.

[0080] [Comparative Example 5] Ammonium vanadate (NH4VO3) and H3PW 12 O 40 To a mixture of 1.5 nH2O and 20 ml of pure water, 11.9 g (131.7 mmol) of oxalic acid ((COOH)2) was added, and the mixture was stirred at room temperature for 10 minutes, and then at 70°C for 12 hours. This precursor sample was calcined at 300°C for 4 hours to obtain a vanadium pentoxide (V2O5) denitration catalyst containing tungsten (W). The raw materials, ammonium vanadate and H3PW, were adjusted so that the total weight ratio of WO3 in the denitration catalyst produced was 84.4 wt%. 12 O 40 -Adjusted the amount of nH2O.

[0081] [Comparative Example 6] Ammonium vanadate (NH4VO3) and H3PW 12 O 40 To a mixture of 1.5 nH2O and 20 ml of pure water, 11.9 g (131.7 mmol) of oxalic acid ((COOH)2) was added, and the mixture was stirred at room temperature for 10 minutes, and then stirred at 70°C for 12 hours. This precursor sample was calcined at 300°C for 4 hours to obtain a vanadium pentoxide (V2O5) denitration catalyst containing tungsten (W). The raw materials ammonium vanadate and H3PW were adjusted so that the total weight ratio of WO3 in the denitration catalyst produced was approximately 100 wt%. 12 O 40 -Adjusted the amount of nH2O.

[0082] The following Table 6 shows the amounts of precursors charged when tungsten was introduced in Example 19 and Comparative Examples 3 to 6. [Table 6] <3.2 Evaluation> <3.2.1 Overview> Under the conditions in Table 1 above, the NH3-SCR reaction was carried out using a fixed-bed flow-type catalytic reactor at a reaction temperature of approximately 150° C. The NO in the gas that passed through the catalyst layer was analyzed using a Jasco FT-IR-4700. The NO conversion rate was calculated according to the above formula (1).

[0083] (Measurement results) Table 7 shows the NO conversion rates for each vanadium pentoxide catalyst in the absence and presence of moisture. Figure 6 is a graph of Table 7. [Table 7]

[0084] In both the cases where moisture is not present and where moisture is present, compared to Comparative Example 1, in which the tungsten content is 0 wt%, and Comparative Examples 2 to 5 and 7, in which the tungsten content is 39 wt% to 100 wt%, it was shown that adding tungsten in an amount between 10 and 38 wt% is generally effective.

[0085] Below, we will discuss the cases where K2WO4 and H3PW are used as precursors. 12 O 40 For each of the cases where nHO was used, elemental analysis was carried out by powder X-ray diffraction and SEM-EDS, and the NO conversion rate for each tungsten content was graphed.

[0086] <3.2.2 When K2WO4 is used as a precursor> <3.2.2.1 Powder X-ray diffraction and elemental analysis> (Measurement method) Powder X-ray diffraction was performed using Cu-Kα on a Rigaku smart lab. Elemental analysis was also performed using SEM-EDS.

[0087] (Measurement results) FIG. 7 shows the powder XRD patterns of Example 16 (4.9 wt%), Example 17 (11.8 wt%), Example 18 (22.1 wt%), Comparative Example 1 (0 wt%), and Comparative Example 2 (100 wt%). FIG. 8 also shows the ratio (%) of tungsten element when the horizontal axis represents mol% of K2WO4.

[0088] Figures 7 and 8 show that by increasing the amount of K2WO4, the crystal phase changed from triclinic V4O7 (12 wt%) to monoclinic WO3 (100 wt%), and the ratio of tungsten atoms in the catalyst increased proportionally.

[0089] <3.2.2.2 NO conversion rate> (Measurement results) Table 8 shows the NO conversion rates for each vanadium pentoxide catalyst in the absence and presence of moisture. Figure 9 is a graph of Table 6. [Table 8]

[0090] As can be seen from Table 8 and Figure 9, the catalytic activity was maximum (96.3%) with triclinic V4O7 (22.1 wt%). In addition, excessive K2WO4 caused a decrease in catalytic activity, and there was no catalytic activity when the tungsten content was 100 wt%.

[0091] 3.2.3 H3PW as a precursor 12 O 40 When using nH2O> <3.2.3.1 Powder X-ray diffraction and elemental analysis> (Measurement method) Powder X-ray diffraction was performed using Cu-Kα on a Rigaku smart lab. Elemental analysis was also performed using SEM-EDS.

[0092] (Measurement results) FIG. 10 shows the powder XRD patterns of Example 19 (38.4 wt%), Comparative Example 4 (61.7 wt%), Comparative Example 5 (77.3 wt%), Comparative Example 6 (84.4 wt%), and Comparative Example 7 (100 wt%). In addition, in Fig. 11, the horizontal axis is H3PW 12 O 40 This indicates the percentage of tungsten element in mol% of nH2O.

[0093] From Figures 10 and 11, H3PW 12 O 40 By increasing the amount of nH2O, H3PW 12 O 40 It was shown that the diffraction peak due to nH2O becomes larger and that the tungsten content becomes high even with a relatively small amount of the material.

[0094] <3.2.3.2 NO conversion rate> (Measurement results) Table 9 shows the NO conversion rates for each vanadium pentoxide catalyst in both the absence and presence of moisture. Figure 12 is a graph of Table 9. [Table 9]

[0095] As can be seen from Table 9 and Figure 12, H3PW 12 O 40 When nH2O was used as the precursor, the catalytic activity was maximized (82.9%) at a tungsten content of 38.4 wt%, but the vanadium catalyst with a tungsten content of 22.1 wt% using K2WO4 as the precursor had higher catalytic activity.

[0096] <4 Vanadium catalyst containing niobium as the second metal> <4.1 Examples>

[0097] As described above, in the vanadium catalysts of Examples 1 to 8, in the absence of moisture, Example 4 (niobium added) showed the second highest NO conversion rate, and even in the presence of moisture, it showed a relatively high NO conversion rate. Therefore, by changing the amount of niobium added, the vanadium catalysts according to the following Examples were produced.

[0098] [Example 20] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, niobium (Nb), was added so that the metal oxide equivalent was 1.8 wt% Nb2O5. The resulting vanadium-niobium complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing niobium (Nb).

[0099] [Example 21] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, niobium (Nb), was added so that the metal oxide equivalent was 5.2 wt% Nb2O5. The resulting vanadium-niobium complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing niobium (Nb).

[0100] [Example 22] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, niobium (Nb), was added so that the metal oxide equivalent was 8.5 wt% Nb2O5. The resulting vanadium-cobalt complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing cobalt (Co).

[0101] [Example 23] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, niobium (Nb), was added so that the metal oxide equivalent was 11.7 wt% Nb2O5. The resulting vanadium-niobium complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing niobium (Nb).

[0102] [Example 24] Ammonium vanadate (NH4VO3) and oxalic acid ((COOH)2) were dissolved in pure water to synthesize a precursor complex. To this precursor complex, an oxalic acid complex of the second metal, niobium (Nb), was added so that the metal oxide equivalent was 16.2 wt% Nb2O5. The resulting vanadium-niobium complex mixture was fired twice in an electric furnace at 300°C for four hours to obtain a vanadium pentoxide (V2O5) denitrification catalyst containing niobium (Nb).

[0103] The following Table 10 shows the amounts of precursors charged when niobium was introduced in Examples 20 to 24. [Table 10] <4.2 Evaluation> <4.2.1 NO conversion rate> (Measurement method) Under the conditions in Table 1 above, the NH3-SCR reaction was carried out using a fixed-bed flow-type catalytic reactor at a reaction temperature of 150°C. NO in the gas that passed through the catalyst layer was analyzed using a Jasco FT-IR-4700. The NO conversion rate was calculated according to the above formula (1).

[0104] (Measurement results) Table 11 shows the NO conversion rates for each vanadium oxide catalyst in both the absence and presence of moisture. Figure 13 is a graph of Table 11. [Table 11]

[0105] In both the absence and presence of moisture, the denitration catalysts of the Examples all exhibited higher NO conversion rates than the denitration catalysts of the Comparative Examples. In particular, in the absence of moisture, Example 22 (9 wt%) exhibited the highest NO conversion rate, and in the presence of moisture, Example 21 (5 wt%) exhibited the highest NO conversion rate.

[0106] <5 Vanadium catalyst containing carbon and cobalt as the second metal and calcined at low temperature> <5.1 Examples and Comparative Examples> [Example 25] Ammonium vanadate (NH4VO3) and oxalic acid were dissolved in pure water to synthesize a precursor complex. Ethylene glycol and an oxalic acid complex, which is a precursor of the second metal, cobalt (Co), were added to this precursor complex so that the metal oxide equivalent of Co3O4 was 6 wt%. The resulting catalyst framework was fired in an electric furnace at 270°C for 2 hours to obtain a vanadium oxide denitration catalyst containing carbon and cobalt (Co). The following Table 12 shows the amounts of precursors charged when cobalt was introduced in Example 25. [Table 12]

[0107] <5.2 Evaluation> <5.2.1 Carbon content> (Measurement method) When measuring the carbon content of each vanadium pentoxide catalyst, the carbon content was quantified by elemental analysis of C (carbon), H (hydrogen), and N (nitrogen). More specifically, each denitrification catalyst was completely combusted and decomposed in a high-temperature reaction tube inside an Exeter Analytical CE-440F, and the main constituent elements C, H, and N were converted to CO2, H2O, and N2, and these three components were then quantified sequentially using three thermal conductivity detectors to measure the contents of C, H, and N in the constituent elements.

[0108] (Measurement results) The carbon content in the vanadium catalyst of Example 25 was 0.70 wt %.

[0109] <5.2.2 NO conversion rate> (Measurement method) Under the conditions in Table 1 above, the NH3-SCR reaction was carried out using a fixed-bed flow-type catalytic reactor at a reaction temperature of 150°C. NO in the gas that passed through the catalyst layer was analyzed using a Jasco FT-IR-4700. The NO conversion rate was calculated according to the above formula (1).

[0110] (Measurement results) Table 13 shows the NO conversion rates in the absence and presence of moisture for each of the vanadium pentoxide catalysts of Comparative Example 1, Example 12, and Example 25. Figure 14 is a graph of Table 13. [Table 13]

[0111] The DeNOx catalyst of Example 25 exhibited the highest NO conversion rate both in the absence and presence of moisture.

[0112] <6 Application Examples> <6.1 Combustion system> <6.1.1 First Combustion System> A first application example of the present invention will be described below with reference to the drawings. Fig. 15 is a diagram showing the configuration of a combustion system 1 according to a first application example. The combustion system 1 is a combustion system that uses pulverized coal as fuel. As shown in Fig. 15, the combustion system 1 is assumed to be a thermal power generation system as an example, and includes a boiler 10 as a combustion device, a coal pulverizer 20, an exhaust passage L1, an air preheater 30, a gas heater 40 as a heat recovery device, a dust collector 50, an induced draft fan 60, a desulfurization device 70, a gas heater 80 as a heater, a denitrification device 90, and a chimney 100.

[0113] The boiler 10 burns pulverized coal as fuel together with air. In the boiler 10, exhaust gas is generated by burning the pulverized coal. The combustion of the pulverized coal produces coal ash such as clinker ash and fly ash. The clinker ash produced in the boiler 10 is discharged to a clinker hopper 11 disposed below the boiler 10 and then transported to a coal ash recovery silo (not shown).

[0114] The boiler 10 is formed generally in an inverted U-shape. Exhaust gas generated in the boiler 10 moves in the inverted U-shape along the shape of the boiler 10. The temperature of the exhaust gas near the exhaust gas outlet of the boiler 10 is, for example, 300 to 400°C.

[0115] The coal pulverizer 20 pulverizes coal supplied from a coal bunker (not shown) into fine particles to form pulverized coal. The coal pulverizer 20 preheats and dries the pulverized coal by mixing the pulverized coal with air. The pulverized coal formed in the coal pulverizer 20 is supplied to the boiler 10 by blowing air onto it.

[0116] The exhaust passage L1 has an upstream side connected to the boiler 10. The exhaust passage L1 is a flow path through which exhaust gas generated in the boiler 10 flows.

[0117] The air preheater 30 is disposed in the exhaust passage L1. The air preheater 30 exchanges heat between the exhaust gas and the combustion air sent from a forced draft fan (not shown) to recover heat from the exhaust gas. The combustion air is heated in the air preheater 30 and then supplied to the boiler 10.

[0118] The gas heater 40 is disposed in the exhaust passage L1 downstream of the air preheater 30. The gas heater 40 is supplied with the exhaust gas whose heat has been recovered in the air preheater 30. The gas heater 40 further recovers heat from the exhaust gas.

[0119] The dust collector 50 is disposed downstream of the gas heater 40 in the exhaust passage L1. The dust collector 50 is supplied with exhaust gas whose heat has been recovered in the gas heater 40. The dust collector 50 is a device that collects soot such as coal ash (fly ash) in the exhaust gas by applying a voltage to electrodes. The fly ash collected in the dust collector 50 is transported to a coal ash recovery silo (not shown). The temperature of the exhaust gas in the dust collector 50 is, for example, 80 to 120°C.

[0120] The induced draft fan 60 is disposed in the exhaust passage L1 downstream of the dust collector 50. The induced draft fan 60 takes in the exhaust gas from which fly ash has been removed in the dust collector 50 from the primary side and sends it out to the secondary side.

[0121] The desulfurizer 70 is disposed downstream of the induced draft fan 60 in the exhaust passage L1. The desulfurizer 70 is supplied with the exhaust gas sent out from the induced draft fan 60. The desulfurizer 70 removes sulfur oxides from the exhaust gas. In detail, the desulfurizer 70 sprays a mixed liquid of limestone and water (limestone slurry) onto the exhaust gas, thereby causing the sulfur oxides contained in the exhaust gas to be absorbed into the mixed liquid, thereby removing the sulfur oxides from the exhaust gas. The temperature of the exhaust gas in the desulfurizer 70 is, for example, 50 to 120°C.

[0122] The gas heater 80 is disposed downstream of the desulfurizer 70 in the exhaust passage L1. Exhaust gas from which sulfur oxides have been removed in the desulfurizer 70 is supplied to the gas heater 80. The gas heater 80 heats the exhaust gas. The gas heater 40 and the gas heater 80 may be configured as a gas-gas heater that performs heat exchange between the exhaust gas flowing between the air preheater 30 and the dust collector 50 in the exhaust passage L1 and the exhaust gas flowing between the desulfurizer 70 and a denitrification device 90 described later. In particular, the gas heater 80 heats the exhaust gas to a temperature suitable for the denitration reaction in the downstream denitration device 90 .

[0123] The denitration device 90 is disposed downstream of the gas heater 80 in the exhaust passage L1. Exhaust gas heated in the gas heater 80 is supplied to the denitration device 90. The denitration device 90 removes nitrogen oxides from the exhaust gas by a denitration catalyst. The denitration device 90 uses a denitration catalyst containing vanadium oxide as a main component, in which the content of the oxide of a second metal is 1 wt% or more and 40 wt% or less, and the second metal is at least one metal element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe. The temperature of the exhaust gas in the denitration device 90 is, for example, 130 to 200°C.

[0124] In the denitration device 90, nitrogen oxides are removed from the exhaust gas by selective catalytic reduction. According to the selective catalytic reduction, nitrogen and water are produced from the nitrogen oxides by using a reducing agent and the above-mentioned denitration catalyst, so that the nitrogen oxides can be efficiently removed from the exhaust gas. The reducing agent used in the selective catalytic reduction includes at least one of ammonia and urea. When ammonia is used as the reducing agent, the ammonia may be in any state such as ammonia gas, liquid ammonia, or an aqueous ammonia solution.

[0125] More specifically, the denitration device 90 may be configured to inject ammonia gas into the introduced exhaust gas, and then bring the resulting mixed gas into contact with a denitration catalyst.

[0126] For this reason, the denitration device 90 may include, for example, one or more stages of denitration catalyst layers, and the denitration catalyst layers may include a plurality of casings, a plurality of honeycomb catalysts housed in the plurality of casings, and sealing members.

[0127] More specifically, the casing may be made of a rectangular cylindrical metal member with one end and the other end open, and may be arranged so that the open ends face the exhaust gas flow path in the denitration reactor, that is, so that the exhaust gas flows through the inside of the casing. Also, a plurality of casings may be arranged by being connected in an abutting state so as to block the exhaust gas flow path.

[0128] The honeycomb catalyst may be formed in an elongated shape (rectangular parallelepiped shape) with a plurality of exhaust gas circulation holes extending in the longitudinal direction, and may be arranged so that the extension direction of the exhaust gas circulation holes is along the exhaust gas flow path.

[0129] The chimney 100 is connected to the downstream side of the exhaust passage L1. Exhaust gas from which nitrogen oxides have been removed in the denitrification device 90 is introduced into the chimney 100. The exhaust gas introduced into the chimney 100 is heated by the gas heater 80, and is therefore effectively discharged from the top of the chimney 100 due to the chimney effect. In addition, heating the exhaust gas in the gas heater 80 can prevent water vapor from condensing above the chimney 100 and causing white smoke. The temperature of the exhaust gas near the outlet of the chimney 100 is, for example, 110°C.

[0130] <6.1.2 Secondary Combustion System> 16 is a diagram showing the configuration of a combustion system 1A according to a second application example. The combustion system 1A is a combustion system that uses pulverized coal as fuel, similar to the combustion system 1. In the combustion system 1A, the same components as those in the combustion system 1 are designated by the same reference numerals, and the description of their functions will be omitted.

[0131] The combustion system 1A differs from the combustion system 1 in that a denitration device 90 is installed immediately after the dust collector 50. Furthermore, downstream of the denitration device 90, an induced draft fan 60, a desulfurization device 70, and a gas heater 80 are provided in this order from upstream to downstream.

[0132] The gas heater 80 in the combustion system 1 heats the exhaust gas to a temperature suitable for the denitration reaction in the downstream denitration device 90. On the other hand, the gas heater 80 in the combustion system 1A heats the exhaust gas to a temperature suitable for diffusion from the downstream chimney 100.

[0133] By installing the denitration device 90 immediately after the dust collector 50, it is not necessary to provide a gas heater upstream of the denitration device 90, and the temperature of the exhaust gas in the denitration device 90 can be set to 130 to 200°C.

[0134] <6.1.3 Third Combustion System> 17 is a diagram showing the configuration of a combustion system 1B according to a third application example. Unlike the combustion systems 1 and 1A, the combustion system 1B is a combustion system that uses natural gas as fuel. In the combustion system 1B, the same components as those in the combustion system 1 and the combustion system 1A are designated by the same reference numerals, and the description of their functions is omitted.

[0135] 17, the combustion system 1B includes a boiler 10 as a combustion device, a natural gas vaporizer 15, an exhaust passage L1, an air preheater 30, a denitration device 90, an induced draft fan 60, and a chimney 100. On the other hand, the combustion system 1B does not include a dust collector and a desulfurization device as essential components.

[0136] The vaporizer 15 vaporizes the natural gas supplied from an LNG tank (not shown) and supplies the gas to the boiler 10. When vaporizing the gas, a method using seawater (open rack type) may be used, a method using hot water produced by a gas burner for heating (submerged combustion type) may be used, or a method using an intermediate medium for performing heat exchange in several stages may be used.

[0137] The denitration device 90 is disposed downstream of the air preheater 30 in the exhaust passage L1. Exhaust gas cooled in the air preheater 30 is supplied to the denitration device 90. The denitration device 90 removes nitrogen oxides from the exhaust gas by a denitration catalyst. The temperature of the exhaust gas in the denitration device 90 is, for example, 130 to 200°C.

[0138] The downstream side of the exhaust passage L1 is connected to the chimney 100. Exhaust gas from which nitrogen oxides have been removed in the denitration device 90 is introduced into the chimney 100. Since the temperature of the exhaust gas in the denitration device 90 is, for example, 130 to 200°C, the exhaust gas introduced into the chimney 100 is effectively discharged from the top of the chimney 100 due to the chimney effect. The temperature of the exhaust gas near the outlet of the chimney 100 is, for example, 110°C.

[0139] By disposing the denitration device 90 downstream of the air preheater 30, the temperature of the exhaust gas that is denitrified by the denitration catalyst is lowered, making it possible to reduce deterioration of the denitration catalyst.

[0140] <6.1.4 Fourth Combustion System> Fig. 18 is a diagram showing the configuration of a combustion system 1C according to a fourth application example. As shown in Fig. 18, the combustion system 1C is a combustion system used for propulsion of a ship, and includes a fuel supply device 110, an internal combustion engine 120 as a combustion device, a dust collector 130, an exhaust heat recovery device 140, a denitration device 150, a chimney 160, an assist motor 170, a fuel line R1, exhaust lines R2 and R3, a steam line R4, and an electric power line R5.

[0141] The fuel supply device 110 supplies fuel to the internal combustion engine 120 through a fuel path R1. As the fuel, for example, petroleum-based fuel such as light oil or heavy oil can be used.

[0142] The fuel passage R1 is connected at its upstream side to the fuel supply device 110 and at its downstream side to the internal combustion engine 120. The fuel passage R1 is a flow path through which fuel is transported from the fuel supply device 110 to the internal combustion engine 120.

[0143] The internal combustion engine 120 combusts petroleum-based fuel together with air. In the internal combustion engine 120, exhaust gas is generated by the combustion of the petroleum-based fuel. The generated exhaust gas is discharged to the dust collector 130 via an exhaust passage R2. Note that the internal combustion engine 120 may be, for example, a two-stroke low-speed diesel engine used in large ships, a four-stroke medium-speed diesel engine used in ferries, or a four-stroke high-speed diesel engine used in high-speed boats and small ships.

[0144] The exhaust passage R2 has an upstream side connected to the internal combustion engine 120. The exhaust passage R2 is a flow path through which exhaust gas generated in the internal combustion engine 120 flows.

[0145] The dust collector 130 is disposed downstream of the internal combustion engine 120 in the exhaust passage R2, and is supplied with exhaust gas discharged from the internal combustion engine 120. The dust collector 130 is a device that collects dust in the exhaust gas. As a method for collecting dust, for example, a method in which a voltage is applied to an electrode to charge the dust and the dust is collected using Coulomb force may be used. Alternatively, a method in which a dust absorbing liquid is supplied to a venturi section, the dust absorbing liquid is atomized by the high-speed exhaust gas in the venturi section, and the dust is collected by gas-liquid contact may be used, as in the method performed by a venturi scrubber.

[0146] The exhaust heat recovery device 140 is disposed downstream of the dust collector 130 in the exhaust passage, and is supplied with exhaust gas from which soot and dust has been removed by the dust collector 130. The exhaust heat recovery device 140 recovers exhaust heat from the exhaust gas supplied from the dust collector 130. More specifically, the exhaust heat recovery device 140 includes a turbine device 141 and an exhaust gas economizer 145.

[0147] The turbine device 141 includes a gas turbine 142, a steam turbine 143, and a generator 144. The gas turbine 142 and the generator 144, and the steam turbine 143 and the generator 144 are connected to each other. The gas turbine 142 is driven by exhaust gas supplied from the dust collector 130 via an exhaust path R3. When the gas turbine 142 is driven, the generator 144 connected to the gas turbine 142 is also driven in conjunction to generate power. The steam turbine 143 is driven by steam supplied from an exhaust gas economizer 145 described later via a steam path R4. When the steam turbine 143 is driven, the generator 144 connected to the steam turbine 143 is also driven in conjunction to generate power. The power generated by the generator 144 is supplied to the boosting motor 170 via a power path R5.

[0148] The exhaust gas economizer 145 generates steam from water stored in a water tank (not shown) or the like, using the exhaust gas supplied from the dust collector 130 via an exhaust passage R2 and the exhaust gas supplied from the gas turbine 142 via an exhaust passage R3 as heat sources. The steam generated by the exhaust gas economizer 145 is supplied to the steam turbine 143 via a steam passage R4.

[0149] The exhaust path R3 is an exhaust path different from the exhaust path R2, and is connected to the dust collector 130 on the upstream side and to the exhaust gas economizer 145 on the downstream side, and passes through the gas turbine 142 on the way. The exhaust path R3 is a flow path that flows the exhaust gas supplied from the dust collector 130 to the exhaust gas economizer 145 via the gas turbine 142.

[0150] The steam path R4 is connected at its upstream side to the exhaust gas economizer 145 and at its downstream side to the steam turbine 143. The steam path R4 is a flow path through which steam generated in the exhaust gas economizer 145 flows.

[0151] The upstream side of the electric power path R5 is connected to the generator 144, and the downstream side is connected to the assist motor 170. The electric power path is a flow path through which the electric power generated by the generator 144 flows.

[0152] The denitration device 150 is disposed downstream of the exhaust heat recovery device 140 in the exhaust passage R2, and is supplied with exhaust gas from which exhaust heat has been recovered. The denitration device 150 removes nitrogen oxides from the exhaust gas by a denitration catalyst. The denitration device 150 uses a denitration catalyst containing vanadium oxide as a main component, in which the content of the oxide of a second metal is 1 wt% or more and 40 wt% or less, and the second metal is at least one metal element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe. Since the denitration device 150 is disposed downstream of the exhaust heat recovery device 140, the temperature of the exhaust gas in the denitration device 150 is, for example, 130 to 200°C.

[0153] In the denitration device 150, nitrogen oxides are removed from the exhaust gas by selective catalytic reduction. According to the selective catalytic reduction, nitrogen and water are produced from the nitrogen oxides by a reducing agent and a denitration catalyst, so that the nitrogen oxides can be efficiently removed from the exhaust gas. The reducing agent used in the selective catalytic reduction includes at least one of ammonia and urea. When ammonia is used as the reducing agent, the ammonia may be in any state such as ammonia gas, liquid ammonia, or an aqueous ammonia solution.

[0154] More specifically, the denitration device 150 may be configured to inject ammonia gas into the introduced exhaust gas and then bring the mixed gas into contact with a denitration catalyst.

[0155] The chimney 160 is connected to the downstream side of the exhaust passage R2. Exhaust gas from which nitrogen oxides have been removed in the denitrification device 150 is introduced into the chimney 160. Since the temperature of the exhaust gas in the denitrification device 150 is, for example, 130 to 200°C, the exhaust gas introduced into the chimney 160 is effectively discharged from the upper part of the chimney 160 due to the chimney effect. In addition, it is possible to prevent water vapor from condensing above the chimney 160 and generating white smoke. The temperature of the exhaust gas near the outlet of the chimney 160 is, for example, 110°C.

[0156] The assist motor 170 is installed downstream of the generator 144 on the power path R5, and is driven to assist the rotation around the propeller shaft of the internal combustion engine 120. Electric power is supplied to the assist motor 170 from the generator 144 via the power path R5, and the assist motor 170 is driven to assist the power generated by the internal combustion engine 120 by using this electric power.

[0157] <6.1.5 Fifth Combustion System> As a fifth application example (not shown), a denitration catalyst mainly composed of vanadium oxide, in which the content of an oxide of a second metal is 1 wt% to 40 wt%, and the second metal is at least one metal element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe, may be used in a denitration device provided in a combustion system for incinerating food waste, etc. In a denitration device provided in the downstream of a boiler for burning food waste, the temperature of the exhaust gas may be 150°C or lower, but the denitration catalyst described above can be used for denitration at a reaction temperature of 80-150°C, and is therefore useful for such a combustion system.

[0158] <6.2 Denitrification catalyst made by coating catalytic components on a substrate> The above-mentioned denitration catalyst is basically in powder form, but as disclosed in, for example, JP 2005-199108 A, a honeycomb-type catalyst in which a honeycomb-shaped substrate is coated with a catalytic component may be used in flue gas denitration devices installed in thermal power plants. In the present invention, as a sixth application example, the above-mentioned denitration catalyst can be coated as a catalytic component on a substrate.

[0159] Any substrate can be used as the substrate as long as it does not deform at temperatures of 200° C. or higher. For example, ceramic, pottery, or metal such as titanium may be used as the substrate. Alternatively, ceramic fiber paper, glass fiber paper, flame-retardant paper, activated carbon paper, deodorizing paper, honeycomb filter nonwoven fabric, felt, or corrugated honeycomb filter made of a plastic sheet may be used as the substrate. Alternatively, the catalyst component of the present invention may be further coated on a new catalyst or a used catalyst. The substrate may be of any shape, such as a plate, pellet, fluid, cylinder, star, ring, extrusion, sphere, flake, pastille, rib extrusion, or rib ring. For example, a corrugated honeycomb filter may be of any shape, such as a block, rotor, oblique, irregular block, rectangular, or mini pleat.

[0160] <6.3 Block-shaped denitrification catalyst> Furthermore, for example, as described in JP 2017-32215 A, a catalyst block such as a honeycomb catalyst may be used in a denitration device installed in a coal-fired power generation facility. As a seventh application example of the present invention, it is also possible to manufacture a catalyst block containing the above-mentioned denitration catalyst as a catalyst component.

[0161] Specifically, the powdered denitration catalyst is mixed with 1 to 50 wt% of a binder, such as CMC (carboxymethyl cellulose) or PVA (polyvinyl alcohol), and kneaded, extruded with a molding machine such as an extrusion granulator or vacuum extruder, or pressed, dried, and then fired to produce a catalyst block. Note that, since the binder is burned off during firing, the weight ratio of the denitration catalyst in the fired catalyst block is 100 wt%.

[0162] In addition, it is possible to produce a catalyst block by further mixing, for example, titanium, molybdenum, tungsten, and / or compounds thereof (especially oxides), or silica with the above-mentioned powdered denitrification catalyst, kneading the mixture, and extruding it.

[0163] The catalyst block may have any shape, such as a plate, pellet, fluid, cylinder, star, ring, extrusion, sphere, flake, honeycomb, pastille, rib extrusion, rib ring, etc. Also, for example, the honeycomb surface of a honeycomb catalyst block may be polygonal, such as triangular, rectangular, pentagonal, hexagonal, or circular.

[0164] <6.4 Other uses> As uses of the above denitration catalysts, 6.1 describes the combustion system, 6.2 describes the denitration catalyst formed by coating a substrate with catalytic components, and 6.3 describes the block-shaped denitration catalyst. However, the uses of denitration catalysts are not limited to these. For example, although 6.1.1 and 6.1.2 describe a combustion system fueled by pulverized coal, and 6.1.3 describes a combustion system fueled by natural gas, the above-mentioned denitrification catalyst may be used in a combustion system that uses petroleum or biomass fuel instead of pulverized coal or natural gas. Also, although 6.1.4 describes a combustion system used for propelling ships, the above-mentioned denitrification catalyst may be used in a combustion system used for propelling automobiles instead of ships.

[0165] According to the combustion system according to the above application example, the following effects are achieved. (1) As described above, in the combustion system 1 according to the above application example, the denitration device 90 is disposed downstream of the dust collector 50 in the exhaust passage L1 through which exhaust gas generated in the boiler (combustion device) 10 flows. Furthermore, in the above embodiment, the denitration device 90 uses a denitration catalyst containing vanadium oxide as a main component, in which the content of the oxide of a second metal is 1 wt % or more and 40 wt % or less, and the second metal is at least one metal element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe. By using the above-described denitration catalyst, the combustion system 1 according to the above-described embodiment can exhibit an effect of achieving higher denitration efficiency at low temperatures compared to the conventional technology during selective catalytic reduction reaction at 200°C or lower using ammonia as a reducing agent.

[0166] (2) The combustion system 1A according to the above-described application example further includes the air preheater 30 that recovers heat from the exhaust gas, and the air preheater 30 is disposed upstream of the dust collector 50. The exhaust gas from which heat has been recovered by the air preheater 30 is supplied to the dust collector 50, thereby suppressing the load on the dust collector 50 due to the heat of the exhaust gas. In addition, since the denitrification device 90 is not disposed upstream of the air preheater 30, which is usually disposed near the boiler (combustion device) 10 in the exhaust passage L1, clogging of the air preheater 30 due to ammonium sulfate generated by the reaction of ammonia with the S component in the exhaust gas does not occur. As a result, the combustion system 1A has low operating costs.

[0167] (3) In the combustion system 1B according to the above application example, the denitration device 90 is disposed downstream of the air preheater 30 in the exhaust passage L1 through which exhaust gas generated in the boiler (combustion device) 10 flows. Furthermore, in the above embodiment, the denitration device 90 uses a denitration catalyst containing vanadium oxide as a main component, in which the content of the oxide of a second metal is 1 wt % or more and 40 wt % or less, and the second metal is at least one metal element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe. By using the above-mentioned denitration catalyst, the combustion system 1A according to the above-mentioned embodiment can achieve an effect of achieving higher denitration efficiency at low temperatures compared to the conventional technology during selective catalytic reduction reaction at 200° C. or less using ammonia as a reducing agent. This also makes it possible to dispose the denitration device 90 downstream of the air preheater 30, thereby lowering the temperature of the exhaust gas denitrified by the denitration catalyst and reducing deterioration of the denitration catalyst. In addition, in the combustion system 1B in the above embodiment, the dust collector and the desulfurization device are not essential components. Therefore, by simplifying the configuration of the combustion system 1B, it is possible to reduce installation costs.

[0168] (4) The combustion system 1C according to the above application example is a combustion system 1C including an exhaust passage R2 through which exhaust gas generated by the combustion of fuel in the internal combustion engine 120 flows, an exhaust heat recovery device 140 that is disposed in the exhaust passage R2 and recovers exhaust heat from the exhaust gas discharged from the internal combustion engine 120, and a denitration device 150 that is disposed in the exhaust passage R2 and removes nitrogen oxides from the exhaust gas using a denitration catalyst, wherein the denitration device 150 is disposed downstream of the exhaust heat recovery device 140 in the exhaust passage R2, the denitration catalyst is a denitration catalyst mainly composed of vanadium oxide, the content of the oxide of a second metal is 1 wt% or more and 40 wt% or less, and the second metal is a denitration catalyst of at least one metal element selected from the group consisting of Co, W, Mo, Nb, Ce, Sn, Ni, and Fe. By using the above-mentioned denitration catalyst, the combustion system 1C according to the above embodiment can achieve a higher denitration efficiency at low temperatures in a selective catalytic reduction reaction at 200°C or less using ammonia as a reducing agent, as compared to the conventional technology, and can arrange the denitration device downstream of the exhaust heat recovery device. Furthermore, it is not essential to heat the exhaust gas immediately before introducing it into the denitration device 150. This prevents the denitration catalyst from being exposed to high temperatures, reducing the deterioration of the denitration catalyst and reducing the operating cost of the combustion system 1C. In addition, the combustion system 1C of the above embodiment can be made compact because a heater for heating the exhaust gas is not essential, which makes it possible to install a combustion system with a denitration device in a small space such as a ship.

[0169] (5) As described above, the exhaust heat recovery device 140 is equipped with the turbine device 141 and the exhaust gas economizer 145. The exhaust gas economizer 145 generates steam using the exhaust gas discharged from the internal combustion engine 120 and the exhaust gas supplied from the turbine device 141 as heat sources. It is preferable that the turbine device 141 generates power using the exhaust gas discharged from the internal combustion engine 120 and the steam supplied from the exhaust gas economizer 145. The exhaust heat recovery device 140 in the above embodiment includes the turbine device 141 and the exhaust gas economizer 145, and thereby makes it possible to more effectively utilize the thermal energy generated by the combustion of fuel in the internal combustion engine 120. [Explanation of symbols]

[0170] 1, 1A, 1B, 1C Combustion Systems 10. Boiler 15. Carburetor 30 Air preheater 50 Electrostatic Precipitator 90 150 Denitration equipment 100 160 Chimney 110 Fuel supply system 120 Internal Combustion Engine 130 Dust collector 140 Waste heat recovery device 141 Turbine Equipment 145 Exhaust Gas Economizer 170 Boosting motor

Claims

1. A combustion device that burns fuel; an exhaust passage through which exhaust gas generated by combustion of the fuel in the combustion device flows; A dust collector disposed in the exhaust passage and configured to collect dust in the exhaust gas; A denitration device that is disposed in the exhaust passage and removes nitrogen oxides from the exhaust gas by a selective catalytic reduction reaction using ammonia as a reducing agent using a denitration catalyst, the denitration device is disposed downstream of the dust collector in the exhaust path, % or more and an oxide of a second metal, the second metal being Co, W or Nb; when the second metal is Co, the content of the oxide of the second metal is 1 wt % or more and 10 wt % or less; when the second metal is W, the content of the oxide of the second metal is 12 wt % or more and 38 wt % or less; and when the second metal is Nb, the content of the oxide of the second metal is 2 wt % or more and 16 wt % or less.

2. The combustion system further includes an air preheater disposed in the exhaust path and configured to recover heat from the exhaust gas; The combustion system of claim 1 , wherein the air preheater is disposed upstream of the dust collector.

3. A combustion device that burns fuel; an exhaust passage through which exhaust gas generated by combustion of the fuel in the combustion device flows; an air preheater disposed in the exhaust passage and configured to recover heat from the exhaust gas; A denitration device that is disposed in the exhaust passage and removes nitrogen oxides from the exhaust gas by a selective catalytic reduction reaction using ammonia as a reducing agent using a denitration catalyst, The denitration device is disposed downstream of the air preheater in the exhaust path, % or more and an oxide of a second metal, the second metal being Co, W or Nb; when the second metal is Co, the content of the oxide of the second metal is 1 wt % or more and 10 wt % or less; when the second metal is W, the content of the oxide of the second metal is 12 wt % or more and 38 wt % or less; and when the second metal is Nb, the content of the oxide of the second metal is 2 wt % or more and 16 wt % or less.

4. An internal combustion engine that burns fuel; an exhaust passage through which exhaust gas generated by combustion of the fuel in the internal combustion engine flows; an exhaust heat recovery device that is disposed in the exhaust passage and recovers exhaust heat from exhaust gas discharged from the internal combustion engine; A combustion system including a denitration device disposed in the exhaust passage and configured to remove nitrogen oxides from the exhaust gas by a selective catalytic reduction reaction using ammonia as a reducing agent using a denitration catalyst, the denitration device is disposed downstream of the exhaust heat recovery device in the exhaust path, % or more and an oxide of a second metal, the second metal being Co, W or Nb; when the second metal is Co, the content of the oxide of the second metal is 1 wt % or more and 10 wt % or less; when the second metal is W, the content of the oxide of the second metal is 12 wt % or more and 38 wt % or less; and when the second metal is Nb, the content of the oxide of the second metal is 2 wt % or more and 16 wt % or less.

5. The exhaust heat recovery device includes a turbine device and an exhaust gas economizer, The exhaust gas economizer generates steam using the exhaust gas discharged from the internal combustion engine and the exhaust gas supplied from the turbine device as heat sources, The combustion system of claim 4 , wherein the turbine device generates electricity using exhaust gas discharged from the internal combustion engine and steam provided from the exhaust gas economizer.

Citation Information

Patent Citations

  • Method of disposing exhaust gas

    JP1980121826A

  • Apparatus for preventing rotor of steam turbine from temperature rise

    JP1985093101A

  • Optical indicating device

    JP1989010202A

  • Treatment of stack gas of fluidized-bed boiler

    JP2000024453A

  • Stack gas denitrification catalyst and method for producing the same

    JP2004275852A