Welding structure and welding method

The welding method addresses the issue of insufficient stirring and strength in conventional laser welding by specifying the welded portion's width and composition, using nickel and silicon, and adjusting laser beam positioning to enhance stirring and promote austenite formation, thereby preventing cracks and maintaining strength.

JP7587341B2Active Publication Date: 2024-11-20NISSAN MOTOR CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2018019293
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-02-06
Publication Date
2024-11-20
Estimated Expiration
2038-02-06

AI Technical Summary

Technical Problem

Conventional laser welding methods that reduce manufacturing costs by minimizing laser beam condensing diameter suffer from insufficient stirring of molten welding metal components, leading to potential cracks and reduced strength in the welded portion.

Method used

A welding method and structure that specifies the widthwise size of the welded portion, incorporates nickel and silicon, and adjusts the laser beam irradiation position to enhance stirring and composition, promoting austenite formation and reducing viscosity, thereby preventing cracks and maintaining strength.

Benefits of technology

The method effectively suppresses welding distortion, prevents cracks, and maintains strength by ensuring a silicon concentration of 0.9% by mass or more and a width direction size of 3.0 mm or less, along with controlled nickel and carbon concentrations, enhancing the welded joint's integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587341000003
    Figure 0007587341000003
  • Figure 0007587341000004
    Figure 0007587341000004
  • Figure 0007587341000005
    Figure 0007587341000005
Patent Text Reader

Abstract

To provide the welding structure and welding method capable of restraining or preventing occurrence of strain resulting from welding of a welding structure, and capable of restraining or preventing occurrence of crack at a welding part and degradation of strength at the same part.SOLUTION: A welding structure has a cast iron member comprising a cast iron, a steel member comprising a carbon steel or alloy steel, and a welding part joining the cast iron and steel members. The welding part has a magnitude of 3.0 mm or less in its width direction, and includes nickel and silicon. In the welding part, a silicon concentration in an optional portion on the center line of this part is 0.9 mass% or more. A welding method for forming the welding structure comprises a process of feeding a metallic material for nickel-including weld to an abutment part abutting a cast iron member comprising the cast iron with a steel member comprising carbon steel or alloy steel, and irradiating a position shifted from the abutment part to a cast iron member side with a fiber laser beam.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a welded structure and a welding method. [Background technology]

[0002] Conventionally, a welding method capable of reducing manufacturing costs has been proposed (see Patent Document 1). This welding method involves laser welding a first member and a second member while melting a metal material for welding by focusing and irradiating a laser beam onto the butted portion between the first member and the second member. This welding method is characterized in that no groove preparation is performed on the butted portion between the first member and the second member, and the focused diameter of the laser beam is set to φ0.2 mm or less. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2011-161506 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the welding method described in Patent Document 1, it is possible to suppress the occurrence of distortion of the welded product due to welding by reducing the focused diameter of the laser beam. However, in this welding method, the molten components of the welding metal material are not stirred sufficiently in the depth direction of the weld. Therefore, there is a problem that the weld is likely to crack or have a low strength.

[0005] The present invention has been made in consideration of the problems associated with the conventional techniques, and has an object to provide a welded structure and a welding method that can suppress or prevent the occurrence of distortion due to welding in a welded structure, and can suppress or prevent the occurrence of cracks in the welded portion and the decrease in strength of the welded portion. [Means for solving the problem]

[0006] The present inventors have conducted extensive research to achieve the above object, and as a result, have found that the above object can be achieved by specifying the width direction size of the welded portion, the components of the welded portion, etc., and have completed the present invention. Effect of the Invention

[0007] According to the present invention, it is possible to provide a welded structure and a welding method that can suppress or prevent the occurrence of distortion due to welding in a welded structure, and can suppress or prevent the occurrence of cracks in the welded portion and the weakening of the welded portion. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram of a welded structure for explaining the welded structure and the welding method. [Diagram 2] FIG. 2 is a cross-sectional view taken along line aa shown in FIG. 1 before welding. [Diagram 3] FIG. 3 is a view seen from the direction of the arrow b shown in FIG. [Figure 4] FIG. 4 is a cross-sectional view taken along line dd shown in FIG. [Diagram 5] FIG. 5 is a cross-sectional view taken along line aa shown in FIG. 1 after welding. [Figure 6] FIG. 6 is an enlarged cross-sectional view showing a main part of the welded structure according to the embodiment, which corresponds to FIGS. 2 and 5. In FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, a welding structure and a welding method according to an embodiment of the present invention will be described in detail. First, a welding structure according to an embodiment of the present invention will be described in detail. Next, a welding method according to an embodiment of the present invention will be described in detail. After that, an example of a welding structure and a welding method will be described in detail with reference to the drawings.

[0010] <1> Welded construction The welded structure of this embodiment includes a cast iron member made of cast iron, a steel member made of carbon steel or alloy steel, and a welded portion joining the cast iron member and the steel member. The welded portion has a width direction size of 3.0 mm or less. The welded portion contains nickel and silicon. Furthermore, the welded portion has a silicon concentration of 0.9 mass% or more at any position on the center line of the welded portion.

[0011] Here, the cast iron in the cast iron member is not particularly limited, but examples thereof include FCD450, FCD600, FCD700, FCD800, etc., as specified in the Japanese Industrial Standards. Although not particularly limited, it is preferable to use FCD450.

[0012] The carbon steel or alloy steel in the steel member is not particularly limited as long as it has a lower silicon content than cast iron, and examples of the steel include SCr417H, SCr420H, SCM420H, SCM418H, and SNCM420H, which are specified in the Japanese Industrial Standards. Although not particularly limited, it is preferable to use SCM420H.

[0013] The "width direction of the weld" means a direction perpendicular to the "length direction of the weld" and the "depth direction of the weld".

[0014] Moreover, the "width direction size of the weld" refers to the width direction length of the weld at the end face formed by the laser beam irradiated end face of the cast iron member and the laser beam irradiated end face of the steel member. For example, X in FIG. 5 indicates the width direction size of the weld. When assuming such a face, fine irregularities on the surface of the weld may be ignored. The end face formed by the laser beam irradiated end face of the cast iron member and the laser beam irradiated end face of the steel member may be referred to as the "surface of the weld structure."

[0015] Furthermore, the "center line of the weld" means a line parallel to the depth direction of the weld that halves the length of a bisector of the weld that halves the distance from the surface of the welded structure to the deepest position of the weld.

[0016] The silicon concentration can be measured, for example, by an X-ray fluorescence analyzer or an electron probe microanalyzer (EPMA). The nickel concentration and carbon concentration, which will be described later, can also be measured in the same manner as above.

[0017] Although not particularly limited, the silicon concentration and nickel concentration are preferably measured by a fluorescent X-ray analyzer (measurement conditions are, for example, voltage: 50 kV, current: 200 μA, and live time: 100 sec.) Furthermore, although not particularly limited, the carbon concentration is preferably measured by an electron probe microanalyzer (EPMA) (measurement conditions are, for example, voltage: 10 kV, current: 70 nA, and spot analysis area: φ0.05 to 0.5 μm.).

[0018] As the X-ray fluorescence analyzer, for example, a micro-area micro X-ray fluorescence analyzer (M4 TRANDO, manufactured by Bruker) can be used. Also, as the electron probe microanalyzer (EPMA), for example, an electron probe microanalyzer (EPMA) (EPMA-1600, manufactured by Shimadzu Corporation) can be used.

[0019] As described above, the welded structure of this embodiment has a cast iron member made of cast iron, a steel member made of carbon steel or alloy steel, and a predetermined welded portion that joins the cast iron member and the steel member. The predetermined welded portion has a widthwise size of 3.0 mm or less, contains nickel and silicon, and has a silicon concentration of 0.9 mass% or more at any point on the center line of the welded portion. Therefore, it is possible to suppress or prevent the occurrence of distortion caused by welding of the welded structure, and to suppress or prevent the occurrence of cracks in the welded portion and the weakening of the welded portion.

[0020] If the width of the welded portion exceeds 3.0 mm, distortion due to welding of the welded structure is likely to occur. From the viewpoint of suppressing or preventing the occurrence of distortion due to welding of the welded structure, the smaller the width of the welded portion, the more preferable. Although not particularly limited, the width of the welded portion is preferably 2.0 mm or less, more preferably 1.0 mm or less, and even more preferably 0.5 mm or less.

[0021] On the other hand, as long as the occurrence of cracks in the welded portion and the weakening of the welded portion can be suppressed or prevented, there is no particular limitation, but the width direction size of the welded portion is preferably 0.1 mm or more, more preferably 0.2 mm or more, and even more preferably 0.3 mm or more.

[0022] The lower limit of the width of the weld can be set appropriately according to the width of the weld set according to the required performance, but is not limited thereto. The lower limit of the width of the weld can be set appropriately according to the distance from the butt joint to the position where the fiber laser beam is irradiated (welding point offset amount) when the fiber laser beam is irradiated to a position shifted from the butt joint toward the cast iron member in a welding method described in detail later. Although not particularly limited, when the width of the weld is set to 0.1 mm, it is preferable that the distance from the butt joint to the position where the fiber laser beam is irradiated (welding point offset amount) is 50 μm or less.

[0023] Furthermore, if nickel and silicon are not contained, cracks are likely to occur in the welded joints and the strength of the welded joints is likely to decrease.

[0024] Furthermore, when the silicon concentration at any point on the center line of the weld is less than 0.9 mass%, cracks are likely to occur at the weld and the strength of the weld is likely to decrease. From the viewpoint of suppressing or preventing cracks and the strength of the weld, the higher the silicon concentration at any point on the center line of the weld, the more preferable it is. Although not particularly limited, the silicon concentration at any point on the center line of the weld is preferably 1.1 mass% or more.

[0025] On the other hand, as long as the occurrence of cracks in the welded portion and the weakening of the welded portion can be suppressed or prevented, there are no particular limitations, but the silicon concentration at any location on the center line of the welded portion is preferably 4.0 mass% or less, more preferably 3.0 mass% or less, and even more preferably 2.0 mass% or less.

[0026] The upper limit of the silicon concentration at any point on the center line of the weld can be set appropriately depending on, for example, the cast iron member used, but is not limited thereto. The upper limit of the silicon concentration at any point on the center line of the weld can be set appropriately depending on, for example, the distance from the butt joint to the position where the fiber laser beam is irradiated (welding point offset amount) when the fiber laser beam is irradiated to a position shifted from the butt joint toward the cast iron member in a welding method described in detail later.

[0027] At present, we believe that the above-mentioned effects have been achieved for the following reasons.

[0028] When welding a cast iron member made of cast iron and a steel member made of carbon steel or alloy steel, a nickel-containing welding metal material is supplied to the butt joint where the cast iron member and the steel member are butted together. When a fiber laser beam is irradiated to a position shifted from the butt joint toward the cast iron member while the nickel-containing welding metal material is being supplied, the width of the welded portion formed can be reduced to 3.0 mm or less. As a result, the occurrence of distortion due to welding in the welded structure can be suppressed or prevented.

[0029] In addition, when welding a cast iron member made of cast iron and a steel member made of carbon steel or alloy steel, a nickel-containing welding metal material is supplied to the butt joint where the cast iron member and the steel member are butted together. Then, when a fiber laser beam is irradiated to a position shifted from the butt joint toward the cast iron member while the nickel-containing welding metal material is being supplied, silicon components from the cast iron member are dissolved in components of the nickel-containing welding metal material supplied to the butt joint.

[0030] Generally, the silicon content (mass%) of a cast iron member is higher than the silicon content (mass%) of a steel member. Therefore, when a fiber laser beam is irradiated at a position shifted toward the cast iron member, a larger amount of silicon can be effectively dissolved in the components of the nickel-containing welding metal material, compared to when a fiber beam is irradiated at a position shifted toward the steel member.

[0031] This reduces the viscosity and surface tension of the molten components of the nickel-containing welding metallic material, promotes stirring of the molten components of the nickel-containing welding metallic material in the depth direction of the weld to be formed, and supplies the components of the nickel-containing welding metallic material to the depth of the weld. As a result, it is possible to suppress or prevent the occurrence of cracks in the weld and the weakening of the weld.

[0032] In addition, the viscosity and surface tension of the molten components of the nickel-containing welding metal material are reduced, and the stirring of the molten components of the nickel-containing welding metal material is promoted in the depth direction of the welded portion to be formed. This suppresses the formation of martensite, which is a brittle structure, in the welded portion, and promotes the formation of austenite, which is a ductile structure. As a result, it can be considered that the occurrence of cracks in the welded portion and the weakening of the welded portion are suppressed or prevented. The correlation between the carbon content of the welded portion and austenite is predicted from the Schaeffler phase diagram.

[0033] However, it goes without saying that even if the above-mentioned effects are obtained for reasons other than those mentioned above, they are still included in the scope of the present invention.

[0034] Although not particularly limited, it is preferable that the weld has a silicon concentration of 1.1 mass% or more at any location on the center line of the weld, and that the average value of the silicon concentration (average silicon concentration) on the center line of the weld is 1.5 mass% or more.

[0035] Here, the average silicon concentration on the center line of the weld is calculated by dividing the length of the center line of the weld into 10 or more equal lengths, measuring the silicon concentration of each divided region, and calculating the average value using the silicon concentration of each divided region. When dividing the center line of the weld into equal lengths, there is no particular limitation as long as a reasonable average value can be calculated, but it is preferable to divide it into 10 or more, and more preferable to divide it into 15 or more. When dividing the center line of the weld into equal lengths, there is no particular limitation on the upper limit of the number of divisions as long as a reasonable average value can be calculated, and for example, it is preferable to divide it into 30 or less, and more preferable to divide it into 25 or less. In particular, it is preferable to divide it into 20.

[0036] As described above, by forming a welded structure having a weld in which the silicon concentration at any location on the center line of the weld is 1.1 mass% or more and the average value of the silicon concentration (average silicon concentration) on the center line of the weld is 1.5 mass% or more, it is possible to further suppress or prevent the occurrence of cracks in the weld and the weakening of the weld.

[0037] In addition, although not particularly limited, the nickel concentration of the weld at any point on the center line of the weld is preferably 0.5 mass% or more and 40 mass% or less. From the viewpoint of cost reduction, although not particularly limited, the nickel concentration at any point on the center line of the weld is more preferably 30 mass% or less, further preferably 20 mass% or less, and particularly preferably 10 mass% or less. When a low-cost nickel-containing welding metal material with a nickel content of about 10 mass% is applied, it is possible to make the maximum nickel concentration 5 mass% or less by controlling the position where the fiber laser beam is irradiated. In addition, at that time, it is also possible to make the minimum nickel concentration 0.50 mass%.

[0038] In a welding method in which silicon components from a cast iron member are dissolved into the components of a nickel-containing welding metal material to reduce the viscosity and surface tension of the nickel-containing welding metal material, there is an advantage that the desired effects can be obtained even when using an inexpensive nickel-containing welding metal material with a nickel content of about 10 mass%.

[0039] The nickel in the weld is usually derived from the nickel-containing metal material for welding, but is not limited thereto, and may be derived from cast iron or steel members. The upper limit of the nickel concentration is usually measured at the position where the fiber laser beam is irradiated (welding point), and the lower limit of the nickel concentration is usually measured at the deepest position of the weld.

[0040] As described above, by forming a welded structure having a weld in which the nickel concentration at any location on the center line of the weld is 0.5 mass % or more and 40 mass % or less, it is possible to suppress or prevent the occurrence of distortion due to welding in the welded structure, and to suppress or prevent the occurrence of cracks in the weld and the weakening of the weld.

[0041] Furthermore, although not particularly limited, when the weld is defined as divided regions by dividing the length of the center line of the weld into 10 or more equal lengths, it is preferable that the nickel concentration ratio of the divided region with the minimum nickel concentration to the divided region with the maximum nickel concentration on the center line is 0.1 or more.

[0042] As described above, when the divided regions are defined so as to divide the length of the center line of the weld into 10 or more equal lengths, by using a joint structure having a weld in which the nickel concentration ratio of the divided region with the minimum nickel concentration on the center line to the divided region with the maximum nickel concentration is 0.1 or more, it is possible to further suppress or prevent the occurrence of cracks in the weld and the weakening of the weld.

[0043] In addition, the nickel concentration ratio of the minimum nickel concentration region to the maximum nickel concentration region is an index showing that the nickel component derived from the nickel-containing welding metal material is supplied deep into the weld and local concentration is suppressed, which shows that the nickel-containing welding metal material is being effectively utilized.

[0044] The upper limit of the nickel concentration ratio of the divided area of ​​the minimum nickel concentration to the divided area of ​​the maximum nickel concentration is theoretically 1 when the maximum nickel concentration and the minimum nickel concentration are the same. The maximum nickel concentration is usually measured at the position (weld point) where the fiber laser beam is irradiated, and the minimum nickel concentration is usually measured at the deepest position of the weld.

[0045] Although not particularly limited, when the weld is defined as divided regions by dividing the length of the center line of the weld into 10 or more equal lengths, the carbon concentration of each divided region is measured, and the average value (average carbon concentration) calculated using the measured carbon concentrations of each divided region is preferably 1.0 mass% or more, more preferably 1.5 mass% or more, even more preferably 2.0 mass% or more, and particularly preferably 2.4 mass% or more.

[0046] On the other hand, as long as the occurrence of cracks in the welded portion and the weakening of the welded portion can be suppressed or prevented, there is no particular limitation, but the average carbon concentration (average carbon concentration) is preferably 4.0 mass% or less, more preferably 3.6 mass% or less, and even more preferably 3.2 mass% or less.

[0047] As described above, when the divided regions are defined so as to divide the length of the center line of the weld into 10 or more equal lengths, the carbon concentration of each divided region is measured, and a weld structure is formed having a weld in which the average value (average carbon concentration) calculated using the measured carbon concentrations of each divided region is 1.0 mass% or more, thereby making it possible to suppress or prevent the occurrence of cracks in the weld and the weakening of the weld.

[0048] In addition, although not particularly limited, the welded portion preferably has a ratio of the size of the welded portion in the depth direction to the size of the welded portion in the width direction (aspect ratio (Y / X)) of 4 or more. In addition, X in FIG. 5 indicates the size of the welded portion in the width direction, and Y in FIG. 5 indicates the size of the welded portion in the depth direction. From the viewpoint of suppressing or preventing the occurrence of distortion due to welding of the welded structure and suppressing or preventing the occurrence of cracks in the welded portion and the weakening of the welded portion, the larger the ratio of the size of the welded portion in the depth direction to the size of the welded portion in the width direction (aspect ratio (Y / X)), the more preferable. Although not particularly limited, the ratio of the size of the welded portion in the depth direction to the size of the welded portion in the width direction (aspect ratio (Y / X)) is more preferably 8 or more, and even more preferably 12 or more. In addition, the upper limit value of the ratio of the size of the welded portion in the depth direction to the size of the welded portion in the width direction (aspect ratio (Y / X)) at present is about 16.

[0049] As described above, by forming a welded structure having a weld in which the ratio of the depth of the weld to the width of the weld is 4 or more, distortion caused by welding can be further suppressed or prevented, cracking in the weld can be further suppressed or prevented, and a decrease in the strength of the weld can be further suppressed or prevented.

[0050] Furthermore, although not particularly limited, the ratio of the components derived from the cast iron member to the sum of the components derived from the cast iron member and the components derived from the steel member in the welded portion is preferably more than 0.50, more preferably 0.60 or more, and even more preferably 0.75 or more. From the viewpoint of reliable formation of the welded portion, the upper limit of the ratio of the components derived from the cast iron member to the sum of the components derived from the cast iron member and the components derived from the steel member is preferably 0.99 or less.

[0051] Here, the "ratio of the components originating from the cast iron member to the total of the components originating from the cast iron member and the steel member" can be calculated based on the deviation between the center line of the butt joint and the welded part when the butt joint between the cast iron member and the steel member can be observed even after welding. Also, when the butt joint between the cast iron member and the steel member cannot be observed after welding, the above ratio can be calculated from the composition ratio of the components of the cast iron member, the steel member and the welded part by analyzing them.

[0052] As described above, the ratio of the components derived from the cast iron material to the total of the components derived from the cast iron member and the components derived from the steel member is preferably more than 0.5, more preferably 0.6 or more, and even more preferably 0.75 or more, so that the silicon concentration and carbon concentration in the welded portion can be increased. This reduces the viscosity and surface tension of the molten components of the nickel-containing welding metal material, promotes stirring of the molten components of the nickel-containing welding metal material in the depth direction of the welded portion to be formed, and supplies the components of the nickel-containing welding metal material to the depth of the welded portion. In addition, the formation of martensite, which is a brittle structure, is suppressed in the welded portion, and the formation of austenite, which is a ductile structure, is promoted. As a result, the occurrence of cracks in the welded portion and the weakening of the welded portion can be suppressed or prevented.

[0053] Although not particularly limited, it is preferable that the cast iron member be a differential case and the steel member be a ring gear.

[0054] By forming a welded structure having a differential case made of cast iron members, a ring gear made of steel members, and the above-mentioned welded portion, it is possible to suppress or prevent the occurrence of distortion due to welding of the welded structure, as well as suppress or prevent the occurrence of cracks in the welded portion and the weakening of the welded portion. In addition, since the differential case and the ring gear are joined by welding, there is no need to join them using bolts, there is no need to form a flange on the differential case, and it is possible to thin the ring gear, so it is possible to realize a lightweight welded structure in which the differential case and the ring gear are welded.

[0055] <2> Welding method The welding method of the present embodiment is one form of a welding method for forming a welded structure of the present invention, and includes the steps of supplying a nickel-containing welding metallic material to a butt joint between a cast iron member made of cast iron and a steel member made of carbon steel or alloy steel, and irradiating a fiber laser beam to a position shifted from the butt joint toward the cast iron member.

[0056] Here, the cast iron member made of cast iron and the steel member made of carbon steel or alloy steel are equivalent to those described in the above embodiment.

[0057] In addition, the nickel-containing welding metal material is not particularly limited, but may be, for example, a nickel-containing welding wire. From the viewpoint of cost reduction, the nickel content of the nickel-containing welding wire is preferably as low as possible. For example, a nickel-containing welding wire having a nickel content of 10% by mass or less is preferable from the viewpoint of reducing material costs and manufacturing costs. However, it is not limited thereto, and for example, a nickel content of more than 10% by mass and 97% by mass or less may be applied. The nickel-containing welding wire is not particularly limited, but may be, for example, Y308, Y310, etc., as specified in the Japanese Industrial Standards. It is preferable to apply Y308, although it is not particularly limited thereto.

[0058] Furthermore, the fiber laser welding machine that irradiates the fiber laser beam is not particularly limited as long as it can form the above-mentioned welded portion, and any conventionally known fiber laser welding machine can be used.

[0059] As described above, the welding method of the present embodiment includes a step of supplying a nickel-containing welding metal material to a butt joint between a cast iron member made of cast iron and a steel member made of carbon steel or alloy steel, and irradiating a fiber laser beam to a position shifted from the butt joint toward the cast iron member. This suppresses or prevents the occurrence of distortion in the welded structure due to welding, and makes it possible to form a welded structure in which the occurrence of cracks in the welded portion and the weakening of the welded portion are suppressed or prevented.

[0060] Although not particularly limited, in the welding method of this embodiment, the irradiation position of the fiber laser beam is shifted to the cast iron member side with a high silicon content (mass %) to actively dissolve the silicon component into the components of the nickel-containing welding metal material. This reduces the viscosity and surface tension of the nickel-containing welding metal material, and promotes the formation of austenite in the welded part even if the nickel-containing welding metal material has a low nickel content. As a result, it is possible to effectively suppress or prevent cracks in the welded part while suppressing manufacturing costs.

[0061] Although not particularly limited, it is preferable to set the position where the fiber laser beam is irradiated to a position shifted from the butted portion toward the cast iron member by 50 μm or more.

[0062] As described above, by setting the position at which the fiber laser beam is irradiated to a position shifted by 50 μm or more from the butt joint toward the cast iron member, the occurrence of distortion due to welding in the welded structure can be suppressed or prevented, and a welded structure can be formed in which the occurrence of cracks in the welded portion and the weakening of the welded portion are suppressed or prevented.

[0063] From the viewpoint of forming a welded structure in which the occurrence of cracks in the welded portion and the decrease in strength of the welded portion are suppressed or prevented, the greater the distance from the butt joint to the position where the fiber laser beam is irradiated (welding point offset amount), the more preferable. For example, the distance from the butt joint to the position where the fiber laser beam is irradiated (welding point offset amount) is more preferably 100 μm or more, and even more preferably 150 μm or more. On the other hand, while there are no particular limitations as long as the occurrence of distortion due to welding in the welded structure is suppressed or prevented, the distance from the butt joint to the position where the fiber laser beam is irradiated (welding point offset amount) is preferably 1.5 mm or less, more preferably 1.0 mm or less, even more preferably 500 μm or less, and particularly preferably 200 μm or less.

[0064] <3> Hereinafter, the welded structure and the welding method will be described in detail with reference to the drawings. Although the case where the differential case and the ring gear are welded is illustrated, the present invention is not limited to this. Also, the dimensional ratios of the drawings cited below are exaggerated for the convenience of explanation and may differ from the actual ratios.

[0065] FIG. 1 is a schematic diagram of a welded structure for explaining a welded structure and a welding method. As shown in FIG. 1, the welded structure 10 has a differential case 12 and a ring gear 14. After welding, which will be described in detail later, a welded portion derived from the differential case 12, the ring gear 14, and the nickel-containing welding wire W is formed at a butt joint A where the differential case 12 and the ring gear 14 are butted together. In other words, after welding, the welded structure 10 has the differential case 12, the ring gear 14, and a welded portion that joins the differential case 12 and the ring gear 14.

[0066] Here, the differential case 12 is formed of a cast iron member made of cast iron as described above, and the ring gear 14 is formed of a steel member made of carbon steel or alloy steel as described above.

[0067] A nickel-containing welding wire W is supplied to the butt joint A between the differential case 12 and the ring gear 14, and a fiber laser beam B is irradiated to form a welded joint between the differential case 12 and the ring gear 14, thereby welding the differential case 12 and the ring gear 14. The butt joint A is formed by butting together circumferential portions 121, 141 that are coaxially arranged on the differential case 12 and the ring gear 14.

[0068] The fiber laser beam B is emitted from a nozzle N disposed in the vicinity of the butted portion A. The nozzle N may include a gas flow path (not shown) and may blow out a shielding gas such as argon (Ar) or nitrogen (N2).

[0069] Here, Fig. 2 is a cross-sectional view taken along line aa in Fig. 1 before welding. Fig. 3 is a view seen from the direction of arrow b in Fig. 1. Fig. 4 is a cross-sectional view taken along line dd in Fig. 3. Fig. 5 is a cross-sectional view taken along line aa in Fig. 1 after welding. Note that X in Fig. 5 indicates the size of the weld in the width direction, and Y in Fig. 5 indicates the size of the weld in the depth direction. Also, the same components are denoted by the same reference symbols to avoid redundant explanations.

[0070] As shown in Fig. 2, the differential case 12 has a protrusion 123 that protrudes in a direction along the rotation axis. The ring gear 14 has a hole 143 into which the protrusion 123 fits. The differential case 12 and the ring gear 14 are connected by fitting the protrusion 123 into the hole 143. The differential case 12 is connected to a rotary drive device including a motor and the like. The ring gear 14 rotates integrally with the differential case 12. The nozzle N is fixed.

[0071] During welding, the emission position and emission direction of the fiber laser beam B remain fixed, while the differential case 12 and the ring gear 14 rotate in the circumferential direction indicated by the arrow c, as shown in Fig. 3 (and Fig. 1). The differential case 12 and the ring gear 14 are welded while the irradiation position of the fiber laser beam B moves relatively in the circumferential direction of the circumferential portions 121, 141. The differential case 12 and the ring gear 14 are welded around the entire circumference of the circumferential portions 121, 141.

[0072] The nickel-containing welding wire W is supplied by a wire feeding mechanism that feeds out the nickel-containing welding wire W from a wire reel around which the nickel-containing welding wire W is wound. The nickel-containing welding wire W is sequentially supplied in accordance with the rotation of the differential case 12 and the ring gear 14.

[0073] The irradiation position of the fiber laser beam B and its vicinity are photographed by an imaging device C such as a CCD camera. During welding, an operator checks the image photographed by the imaging device C on a display device such as a liquid crystal display. The differential case 12 and the ring gear 14 are welded while the irradiation position of the fiber laser beam B is monitored.

[0074] As shown in Fig. 4, the irradiation position of the fiber laser beam B is shifted from the butt joint A toward the differential case 12, which is a cast iron member having a relatively high silicon content (mass %) out of the differential case 12, which is a cast iron member, and the ring gear 14, which is a steel member. Therefore, as shown in Fig. 5, the weld 16 formed by melting the differential case 12, the ring gear 14, and the nickel-containing welding wire W by irradiation with the fiber laser beam B is positioned away from the butt joint A toward the differential case 12.

[0075] By welding while monitoring the irradiation position of the fiber laser beam B, the irradiation position does not deviate toward the ring gear side, and the fiber laser beam B is reliably irradiated to a position shifted toward the differential case 12. Therefore, the entire annular weld 16 formed around the rotating shaft is formed shifted toward the differential case 12, which is a cast iron member with a high silicon content (mass %). This effectively suppresses cracking throughout the entire weld 16, ensuring reliable joining of the members.

[0076] Unlike the above-mentioned welding method, when the differential case 12 and the ring gear 14 are fixed without rotating and the emission position and emission direction of the fiber laser beam B and the supply position of the nickel-containing welding wire W are changed while welding in the circumferential direction, a drive device for moving the nozzle N and the nickel-containing welding wire W, etc., and a control device for controlling them are required. Therefore, the welding device may become complicated. On the other hand, in the above-mentioned welding method, the differential case 12 and the ring gear 14 are welded by rotating them in the circumferential direction while fixing the emission position and emission method of the fiber laser beam B, so that a large-scale device such as that used for welding by moving the fiber laser beam B is not required, and a simple welding device can be used. EXAMPLES

[0077] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0078] (Examples 1 to 4, Comparative Examples 1 to 5) Fig. 6 is an enlarged cross-sectional view showing a main part of the welded structure of the example corresponding to Fig. 2 and Fig. 5. As shown in Fig. 6, the differential case 22 and the ring gear 24, which form annular gaps 221, 241 around the rotation axis between the members when they are butted against each other, were actually welded to form the welded structure 20. In the example, the components other than the gaps 221, 241 are substantially similar to those of the above-mentioned embodiment.

[0079] Here, the differential case 22 was made of spheroidal graphite cast iron, FCD450, as specified by the Japanese Industrial Standards. In the differential case 22, the carburized layer on the welded surface forming the butt joint A was removed to form a groove as shown in FIG.

[0080] The ring gear 24 is made of SCM420H, a case-hardened steel specified by the Japanese Industrial Standards. The ring gear is carburized.

[0081] Furthermore, nickel-containing welding wire made of Y308 specified in the Japanese Industrial Standards was used as the nickel-containing welding wire W. The nickel-containing welding wire had a nickel content of 10 mass% and a diameter of φ0.6 mm. During welding, the nickel-containing welding wire was fed at a feed rate of 7 m / min.

[0082] At each of a plurality of irradiation positions (butt joint A is 0, the cast iron member side is (+), and the steel member side is (-), and set at -200 μm to +200 μm) set by shifting the position along the rotation axis of the differential case 22 and the ring gear 24, nitrogen (N2) as a shielding gas was blown out, and a fiber laser beam B (output: 3800 to 4200 W, spot diameter: φ0.2 mm, defocus: -2 mm (however, the inner direction of the material is (-))) was irradiated at a welding speed of 5 m / min to form a welded portion 26, and the differential case 22 and the ring gear 24 were joined. In other words, a welded structure having the differential case 22, the ring gear 24, and the predetermined welded portion 26 formed by melting the differential case 22, the ring gear 24, and the nickel-containing welding wire W by a predetermined irradiation of the fiber laser beam B was formed.

[0083] Some specifications of each example are shown in Table 1.

[0084] [Table 1]

[0085] In addition, the "beam irradiation position" in Table 1 is the distance from the butt joint A between the differential case 22 and the ring gear 24 in the direction along the rotation axis. When the beam irradiation position is positive (+), the beam irradiation position is located on the differential case 22 side from the butt joint A. For example, when the beam irradiation position is +200 μm, this means that the fiber laser beam B is irradiated to a position shifted 200 μm from the butt joint A to the differential case 22 side in the direction along the rotation axis. On the other hand, when the beam irradiation position is negative (-), the beam irradiation position is located on the ring gear 24 side from the butt joint A. For example, when the beam irradiation position is -200 μm, this means that the fiber laser beam B is irradiated to a position shifted 200 μm from the butt joint A to the ring gear 24 side in the direction along the rotation axis.

[0086] In addition, the "width of the weld (X)" in Table 1 is the length of the weld along the width of the weld on the surface of the welded structure in a cross section of the weld perpendicular to the length of the weld and parallel to the depth of the weld. X in Figure 5 indicates the width of the weld.

[0087] Furthermore, the "depth of the weld (Y)" in Table 1 is the length of the weld in the depth direction from the surface of the welded structure to the deepest position of the weld in a cross section of the weld perpendicular to the length of the weld and parallel to the depth of the weld. Note that Y in Figure 5 indicates the depth of the weld.

[0088] Additionally, the "aspect ratio (Y / X)" in Table 1 is the ratio of the depth of the weld to the width of the weld.

[0089] Furthermore, the "average carbon concentration" in Table 1 is the arithmetic average value obtained by dividing the length of the center line of the weld into 20 equal-length divided regions and measuring the carbon concentration on the center line of each divided region using an electron probe microanalyzer (EPMA) (manufactured by Shimadzu Corporation, EPMA-1600) (measurement conditions: voltage: 10 kV, current: 70 nA, spot analysis region: φ0.05 to 0.5 μm).

[0090] In addition, the "minimum silicon concentration" in Table 1 is the minimum value of each silicon concentration obtained by dividing the length of the center line of the weld into 20 equal lengths and measuring the silicon concentration on the center line of each divided area using a micro-area micro X-ray fluorescence analyzer (M4 TRANDO, manufactured by Bruker) (measurement conditions: voltage: 50 kV, current: 200 μA, live time: 100 sec).

[0091] Furthermore, the "average silicon concentration" in Table 1 is the arithmetic average value obtained by dividing the length of the center line of the weld into 20 equal-length divided regions and measuring the silicon concentration on the center line of each divided region using a micro-area micro X-ray fluorescence analyzer (M4 TRANDO, manufactured by Bruker) (measurement conditions: voltage: 50 kV, current: 200 μA, live time: 100 sec).

[0092] In addition, the "maximum nickel concentration" and "minimum nickel concentration" in Table 1 are the maximum and minimum values ​​of each nickel concentration obtained by dividing the length of the center line of the weld into 20 equal lengths and measuring the nickel concentration on the center line of each divided area using a micro-area micro X-ray fluorescence analyzer (M4 TRANDO, manufactured by Bruker) (measurement conditions: voltage: 50 kV, current: 200 μA, live time: 100 sec).

[0093] Furthermore, the "nickel concentration ratio" in Table 1 is the ratio of the minimum nickel concentration to the maximum nickel concentration.

[0094] Also, the "cast iron component origin component ratio" in Table 1 was calculated based on the deviation between the center line of the butt joint and the weld joint. For example, when there is no deviation between the center line of the butt joint and the weld joint, the cast iron component origin component ratio is 0.5, and when the center line of the weld joint is deviated toward the cast iron member side from the butt joint, the cast iron component origin component ratio is over 0.5. The steel component origin component ratio can be calculated as 1 - (cast iron component origin component ratio).

[0095] [Performance evaluation] The welded structures of the above examples were observed, measured, and evaluated for cracks in the welded joints, average hardness of the welded joints, and strength of the welded joints in the following manner. The results are shown in Table 2.

[0096] [Table 2]

[0097] (Weld cracks) The cross section of the welded part of each example of the welded structure was observed using an optical microscope (Leica, DMI5000M, magnification: 100 to 500 times) to evaluate the presence or absence of cracks, etc. In Table 2, "No" in the "Cracks in Welded Part" section means that no cracks were observed, "Yes" means that cracks were observed, and "Yes (Micro)" means that cracks were observed, but the observed cracks were microscopic.

[0098] (Average hardness of welded parts) The average hardness of the welded portion of each example was measured and evaluated. The average hardness of the welded portion was determined by dividing the length of the center line of the welded portion into 20 equal lengths in the cross section of the welded portion of each example, and measuring the Vickers hardness on the center line of each divided area in accordance with the Vickers hardness test method (JIS Z 2244-2009) in the Japanese Industrial Standards at a test load of 300 gf, and the arithmetic average value obtained from each Vickers hardness was obtained.

[0099] (Weld strength) The welded structure of each example was subjected to a four-point bending test (test conditions: lower support distance: 55 mm, upper support distance: 10 mm, and push-in speed: 2 mm / min) using a precision universal testing machine (Shimadzu Corporation, Autograph AG-X), and the fracture state was observed to evaluate the strength. In Table 2, "x" in the "Weld Strength" section means that the weld fractured without base material fracture, which is the fracture of the base material such as cast iron or steel, "○" means that base material fracture occurred more frequently before the weld fractured, and "◎" means that base material fracture (cast iron member side) occurred without the weld fracture.

[0100] From Tables 1 and 2, it can be seen that Examples 1 to 4 within the scope of the present invention can suppress or prevent the occurrence of cracks in the welded parts and the weakening of the welded parts, compared with Comparative Examples 1 to 5 outside the present invention. Furthermore, as a result of visual observation, Examples 1 to 4 suppressed or prevented the occurrence of distortion due to welding in the welded structure.

[0101] The reason for this is believed to be that by shifting the irradiation position and irradiating the fiber laser beam to the differential case side formed of a cast iron member made of cast iron and a cast iron member made of carbon steel or alloy steel with a relatively high silicon content, a weld having the following characteristics (1) to (3) was formed.

[0102] (1) The weld shall have a width of 3.0 mm or less. (2) The weld contains nickel and silicon. (3) The weld has a silicon concentration of 0.9 mass percent or more at any location on the center line of the weld.

[0103] Furthermore, the reason why Examples 2 to 4 are able to suppress or prevent the occurrence of cracks and the weakening of the welded joints compared to Example 1 and Comparative Examples 1 to 5 is thought to be because, as described above, by irradiating the fiber laser beam onto the differential case side, a welded joint having the following characteristic (4) in addition to the characteristics (1) to (3) above is formed.

[0104] (4) The weld has a silicon concentration of 1.1 mass% or more at any location on the center line of the weld, and the average silicon concentration on the center line of the weld (average silicon concentration) is 1.5 mass% or more.

[0105] Furthermore, since the welded parts have an average silicon concentration of 1.5 mass% or more, it can be seen that the silicon component has effectively dissolved into the differential case side, which is made of cast iron material.

[0106] Furthermore, the reason why Examples 1 to 4 are able to suppress or prevent the occurrence of cracks and the weakening of the welded parts compared to Comparative Examples 1 to 5 is thought to be that by irradiating the fiber laser beam to the differential case side in the same manner as described above, a welded part having the following characteristic (5) in addition to the characteristics (1) to (3) or (1) to (4) above is formed.

[0107] (5) The weld has a nickel concentration of 0.5% by mass or more and 40% by mass or less at any location on the center line of the weld.

[0108] Furthermore, the reason why Examples 2 to 4 are able to suppress or prevent the occurrence of cracks and the weakening of the welded parts compared to Example 1 and Comparative Examples 1 to 5 is thought to be because, by irradiating the fiber laser beam to the differential case side in the same manner as described above, a welded part having the following characteristic (6) in addition to any one of the characteristics (1) to (3), (1) to (4), or (1) to (5) above is formed.

[0109] (6) When the length of the center line of the weld is divided into 20 equal parts, the nickel concentration ratio of the area with the minimum nickel concentration to the area with the maximum nickel concentration on the center line is 0.1 or more.

[0110] In addition, since the nickel concentration ratio is 0.1 or more, it is understood that the silicon component dissolves into the components of the nickel-containing welding wire, the viscosity and surface tension of the molten components of the nickel-containing welding wire decrease, and the stirring of the molten components of the nickel-containing welding wire is promoted in the depth direction of the weld that is formed.

[0111] Furthermore, the reason why Examples 1 to 4 are able to suppress or prevent the occurrence of cracks and the weakening of the welds compared to Comparative Examples 1 to 5 is thought to be because, by irradiating the fiber laser beam to the differential case side in the same manner as described above, a weld is formed that has the following characteristic (7) in addition to any one of the characteristics (1) to (3), (1) to (4), (1) to (5), or (1) to (6) above.

[0112] (7) The ratio of the depth of the weld to the width of the weld is 4 or more.

[0113] Furthermore, the reason why Examples 1 to 4 are able to suppress or prevent the occurrence of cracks and the weakening of the welded parts compared to Comparative Examples 1 to 5 is thought to be because, by irradiating the fiber laser beam to the differential case side in the same manner as described above, a welded part having the following characteristic (8) or (9) in addition to any one of the characteristics (1) to (3), (1) to (4), (1) to (5), (1) to (6), or (1) to (7) above was formed.

[0114] (8) The ratio of components derived from cast iron members to the sum of components derived from cast iron members and components derived from steel members in the welded portion is greater than 0.50. (9) The ratio of components derived from cast iron members to the sum of components derived from cast iron members and components derived from steel members of the welded parts is 0.60 or more.

[0115] In addition, the reason why Examples 1 to 4, especially Examples 2 to 4, can suppress or prevent the occurrence of cracks and the weakening of the welded parts compared to Comparative Examples 1 to 5 is that, by irradiating the fiber laser beam to the differential case side as described above, in addition to any one of the above characteristics (1) to (3), (1) to (4), (1) to (5), (1) to (6), (1) to (7), or (1) to (7), (8), or (9), a welded part having the following characteristic (10) is formed.

[0116] (10) When the length of the center line of the weld is divided into 20 divided regions of equal length, the carbon concentration of each divided region is measured, and the average value (average carbon concentration) calculated using the measured carbon concentrations of each divided region is preferably 1.0 mass% or more, more preferably 1.5 mass% or more, even more preferably 2.0 mass% or more, and particularly preferably 2.4 mass% or more.

[0117] Furthermore, the reason why Examples 2 to 4 are able to suppress or prevent the occurrence of cracks in the welded parts and the weakening of the welded parts compared to Example 1 and Comparative Examples 1 to 5 is thought to be because the amount of austenite contained in the welded parts is increased.

[0118] In other words, when the average hardness of the weld is 600HV or more, the weld contains more brittle martensite than ductile austenite. On the other hand, when the average hardness of the weld is less than 600HV, the weld contains more ductile austenite than brittle martensite. Therefore, it is thought that the increased austenite content in the sprayed part effectively prevents cracking of the weld.

[0119] Furthermore, compared to Comparative Examples 1 to 5, the reason why Examples 1 to 4, especially Examples 2 to 4, are able to suppress or prevent the occurrence of cracks in the welded parts and the weakening of the welded parts is thought to be because the fiber laser beam was irradiated with a shift of 50 μm or more, preferably 100 μm or more, to the differential case side formed of a cast iron member made of cast iron and a cast iron member made of carbon steel or alloy steel having a relatively high silicon content, thereby forming a welded part having the above characteristics (1) to (3).

[0120] Thus, comparing Examples 2 to 4 with Example 1, it can be seen that when welding by irradiating a fiber laser beam, it is more preferable to shift the beam irradiation position by 100 μm or more from the ring gear side, which is made of a steel member made of carbon steel or alloy steel, to the differential case side, which is made of a cast iron member made of cast iron.

[0121] Although the present invention has been described above with reference to some embodiments and examples, the present invention is not limited to these, and various modifications are possible within the scope of the claims. [Explanation of symbols]

[0122] 10,20 Welded structure 12,22 Differential case (cast iron parts) 14,24 Ring gear (steel member) 16,26 Welding 121,141 Circumference 123 Protrusion 143 holes 221,241 Gap A Butt joint B Fiber laser beam C. Imaging Device N Nozzle W Nickel-containing welding wire (nickel-containing welding metal material)

Claims

1. A welding method for forming a welded structure having a cast iron member made of cast iron, a steel member made of carbon steel or alloy steel, and a welded part joining the cast iron member and the steel member, comprising: The weld has a width direction dimension of 3.0 mm or less, and the weld contains nickel and silicon; The weld has a silicon concentration of 0.9% by mass or more and 2.0% by mass or less at any site on a center line of the weld, and an average carbon concentration of the weld is 2.0% by mass or more and 3.2% by mass or less, A welding method comprising the steps of: supplying a nickel-containing welding metal material to a butt joint between the cast iron member and the steel member; and irradiating a fiber laser beam to a position shifted from the butt joint toward the cast iron member.

2. The welding method described in Claim 1, characterized in that the position at which the fiber laser beam is irradiated is a position shifted by 50 μm or more from the butt joint toward the cast iron member.

Citation Information

Patent Citations

  • Method and device for laser tack welding in billet joining

    JP1996290276A

  • Welding method

    JP2011161506A

  • Weld zone of spheroidal graphite cast iron with each other or spheroidal graphite cast iron and steel, welding material used for the welding and heat treatment of the weld zone

    JP2017074602A

  • Welding method and welded product

    JP2017225993A

  • Welding alloy and method

    US4426426A