Composite Article Providing Flame Retardancy and Noise Reduction Properties - Patent application

Lightweight reinforced thermoplastic composite articles with a porous core and open cell skin integrate flame retardancy and noise reduction, addressing the dual performance needs in industries by meeting ASTM standards for flame and noise criteria.

JP7587421B2Active Publication Date: 2024-11-20AZDEL INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2020537495
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-03-05
Filing Date
2019-01-04
Publication Date
2024-11-20
Estimated Expiration
2039-01-04

AI Technical Summary

Technical Problem

Existing composite materials used in industries such as building and construction, automotive, and recreational vehicles often lack both flame retardancy and noise reduction properties, necessitating separate treatments for each property.

Method used

Development of lightweight reinforced thermoplastic (LWRT) composite articles with a porous core layer comprising a web of open cell structure made from reinforcing fibers held together by a thermoplastic material, incorporating a flame retardant and an open cell skin for noise reduction, achieving a balance between flame retardancy and noise absorption.

Benefits of technology

The composite articles provide both effective flame retardancy and noise reduction, meeting ASTM standards for flame spread and smoke development while offering noise reduction factors of at least 0.5, enhancing safety and acoustic performance in various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587421000006
    Figure 0007587421000006
  • Figure 0007587421000007
    Figure 0007587421000007
  • Figure 0007587421000008
    Figure 0007587421000008
Patent Text Reader

Abstract

A thermoplastic composite article is described that includes a porous core layer and an open-cell skin disposed on a first surface of the core layer. The composite article has a noise reduction factor of at least 0.5 when tested according to ASTM C423-17, a flame spread index of less than 25, and a smoke development index of less than 150 when tested according to ASTM E84, 2009. [Selected Figure] Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Related Applications This application claims priority to and the benefit of U.S. Provisional Patent Application No. 62 / 614,038, filed January 5, 2018, and U.S. Provisional Patent Application No. 62 / 638,859, filed March 5, 2018, the entire disclosures of each of which are incorporated herein by reference. Certain embodiments described herein relate to composite articles that provide both flame retardant and noise reducing properties. [Background technology]

[0002] Composite materials have a wide range of applications in different industries, such as building and construction, automotive, and recreational vehicles, etc. To be used in these industries, composite materials often need to meet certain performance characteristics. Summary of the Invention

[0003] Certain aspects, embodiments, configurations, and examples of lightweight reinforced thermoplastic (LWRT) composite articles that can provide both flame retardant and noise reducing properties are described. Although certain configurations are described as including certain components, the components may be rearranged, substituted, or otherwise modified to provide articles with desired performance characteristics. In addition, other components, layers, and materials may be used on, in, or with the exemplary components described herein.

[0004] In a first aspect, a thermoplastic composite article is provided that includes a porous core layer comprising an open-celled web comprising a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer comprising a flame retardant and a basis weight of at least 2500 grams per square meter (gsm), e.g., at least 2800 gsm. In some examples, the composite article also includes an open-celled skin disposed on a first surface of the porous core layer, the composite article comprising a noise reduction factor of at least 0.5 when tested by ASTM C423-17, and the composite article comprising a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009.

[0005] In certain embodiments, the flame retardant comprises expandable graphite particles. In some examples, the open cell skin comprises an apertured film having an open surface area of ​​at least 10%, and the composite article comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17.

[0006] In other embodiments, the flame retardant comprises magnesium hydroxide. In some cases, the open cell skin comprises an apertured film having an open surface area of ​​at least 10%, and the composite article comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17.

[0007] In some examples, the thermoplastic material comprises a polyolefin resin. In other examples, the plurality of reinforcing fibers comprises glass fibers. In some embodiments, the composite article includes a decorative layer disposed on the second surface of the porous core layer.

[0008] In other embodiments, the composite article includes a closed cell skin disposed on the second surface of the porous core layer. In some embodiments, the composite article includes a decorative layer disposed on the closed cell skin.

[0009] In another embodiment, the ceiling tile includes a porous core layer and an open cell skin disposed on the porous core layer. For example, the ceiling tile may include a porous core layer including an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm, for example, at least 2800 gsm. The ceiling tile may also include an open cell skin disposed on a first surface of the porous core layer, the ceiling tile including a noise reduction factor of at least 0.5 when tested by ASTM C423-17, and the ceiling tile including a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009.

[0010] In certain embodiments, the open cell skin comprises at least 10% open surface area, and the ceiling tile comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other embodiments, the ceiling tile further comprises a porous decorative layer disposed on the open cell skin. In some examples, the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both. In certain examples, the open cell skin comprises a perforated film having at least 10% open surface area, and the ceiling tile panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some embodiments, the ceiling tile comprises a closed cell skin disposed on a second surface of the porous core layer. In certain cases, the flame retardant is homogeneously dispersed in the porous core layer. In some examples, the thermoplastic material comprises a polyolefin resin. In certain examples, the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both. In some embodiments, the porous core layer further comprises clay.

[0011] In another aspect, a cubicle wall panel sized and arranged to be bonded to another cubicle wall panel is described. For example, the cubicle wall panel may include a porous core layer including an open-cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm, e.g., at least 2800 gsm. The cubicle wall panel may also include an open-cell skin disposed on a first surface of the porous core layer, the cubicle wall panel including a noise reduction factor of at least 0.5 when tested by ASTM C423-17, and the cubicle wall panel including a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009.

[0012] In some examples, the open cell skin comprises an open surface area of ​​at least 10%, and the cubicle wall panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other examples, the cubicle wall panel comprises a porous decorative layer disposed on the open cell skin. In some examples, the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both. In further examples, the open cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the cubicle wall panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some cases, the cubicle wall panel comprises a closed cell skin disposed on a second surface of the porous core layer. In other examples, the flame retardant is homogeneously dispersed in the porous core layer. In some embodiments, the thermoplastic material comprises a polyolefin resin. In certain examples, the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both. In some cases, the porous core layer further comprises clay.

[0013] In an additional embodiment, a structural panel includes a porous core layer, an open cell skin, and a structural substrate bonded to the porous core layer. The porous core layer may include an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm, e.g., at least 2800 gsm. The open cell skin may be bonded to a first surface of the porous core layer. The structural substrate may be bonded to a second surface of the porous core layer, the structural panel including a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the structural panel provides a noise reduction factor of at least 0.85 when tested by ASTM C423-17.

[0014] In certain embodiments, the structural substrate comprises a plywood panel, gypsum board, wood tile, ceramic tile, metal tile, wood panel, concrete panel, concrete board, or brick. In other embodiments, the open cell skin comprises at least 10% open surface area, and the structural panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some examples, the structural panel comprises a porous decorative layer disposed on the open cell skin. In certain examples, the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both. In some examples, the open cell skin comprises a perforated film having at least 10% open surface area, and the structural panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other examples, the structural panel comprises a closed cell skin disposed on the second surface of the porous core layer. In some embodiments, the flame retardant is homogeneously dispersed in the porous core layer. In certain embodiments, the thermoplastic material comprises a polyolefin resin and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both. In some embodiments, the structural panel comprises a second structural panel bonded to the open cell skin, and the second structural panel is a porous structural panel.

[0015] In another embodiment, a wall panel includes a porous core layer, an open cell skin, and a wall substrate. The porous core layer includes an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, and the porous core layer includes a flame retardant and a basis weight of at least 2500 gsm, for example at least 2800 gsm. The open cell skin can be bonded to a first surface of the porous core layer. The wall substrate can be bonded to a second surface of the porous core layer and configured to support the porous core layer when the wall panel is bonded to the wall surface, the wall panel includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the wall panel includes a sound absorption coefficient of at least 0.5 when tested by ASTM C423-17.

[0016] In some examples, the wall substrate does not include cellulose. In other examples, the open cell skin includes an open surface area of ​​at least 10%, and the wall panel includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some examples, the wall panel includes a porous decorative layer disposed on the open cell skin. In certain cases, the flame retardant includes expandable graphite particles, or magnesium hydroxide, or both. In some examples, the open cell skin includes a perforated film having an open surface area of ​​at least 10%, and the wall panel includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17. In other embodiments, the wall panel includes a closed cell skin disposed on the second surface of the porous core layer. In some examples, the flame retardant is homogeneously dispersed in the porous core layer. In certain examples, the thermoplastic material includes a polyolefin resin, and the plurality of reinforcing fibers includes glass fibers, or mineral fibers, or both. In some embodiments, the wall panel includes a second wall panel bonded to an open cell skin, the second wall panel being a porous wall panel.

[0017] In an additional embodiment, the vinyl siding panel includes a flame retardant noise reduction layer and a vinyl substrate. In some examples, the flame retardant noise reduction layer includes a porous core layer including an open-cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm, for example at least 2800 gsm, and an open-cell skin bonded to a first surface of the porous core layer, the flame retardant layer includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the flame retardant layer includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17. The vinyl substrate can be bonded to the first surface of the flame retardant noise reduction layer and can be configured to bond to a non-horizontal surface of a building to hold the vinyl siding panel to the non-horizontal surface of a building.

[0018] In certain embodiments, the vinyl siding panel includes a weather barrier bonded to the second surface of the flame retardant noise reduction layer. In some embodiments, the vinyl substrate includes a nailing flange. In other embodiments, the open cell skin includes at least 10% open surface area, and the vinyl siding includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some embodiments, the flame retardant includes expandable graphite particles, or magnesium hydroxide, or both. In certain embodiments, the open cell skin includes a perforated film having at least 10% open surface area, and the vinyl siding panel includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some embodiments, the vinyl siding panel includes a closed cell skin disposed on the second surface of the porous core layer. In other embodiments, the flame retardant is homogeneously dispersed in the porous core layer. In some cases, the thermoplastic material includes a polyolefin resin, and the plurality of reinforcing fibers includes glass fibers, or mineral fibers, or both. In some embodiments, the vinyl siding panel includes a second vinyl siding panel including a second flame retardant noise reducing layer bonded to a second vinyl substrate, wherein the flame retardant noise reducing layer is configured to lock to the second flame retardant noise reducing layer when the vinyl substrate is bonded to the second vinyl substrate.

[0019] In another embodiment, a roof panel includes a flame retardant noise reduction layer and a roof substrate. The flame retardant noise reduction layer includes a porous core layer including an open-cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm, for example at least 2800 gsm, and an open-cell skin bonded to a first surface of the porous core layer, the flame retardant noise reduction layer includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the flame retardant noise reduction layer includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17. The roof substrate can be bonded to the first surface of the flame retardant noise reduction layer and can be configured to bond to the roof of the residence to hold the roof panel to the roof.

[0020] In certain embodiments, the roof panel includes a weather barrier bonded to the second surface of the flame retardant noise reduction layer. In some embodiments, the roof substrate includes a cellulosic material. In other embodiments, the open cell skin includes at least 10% open surface area, and the roof panel includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some embodiments, the flame retardant includes expandable graphite particles, or magnesium hydroxide, or both. In some embodiments, the open cell skin includes a perforated film having at least 10% open surface area, and the roof panel includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some embodiments, the roof panel includes a closed cell skin disposed on the second surface of the porous core layer. In certain embodiments, the flame retardant is homogeneously dispersed in the porous core layer. In some embodiments, the thermoplastic material includes a polyolefin resin, and the plurality of reinforcing fibers includes glass fibers, or mineral fibers, or both. In some embodiments, the roof panel includes a second roof panel including a second flame-retardant noise-reducing layer bonded to a second roof substrate, and the flame-retardant noise-reducing layer is configured to engage with the second flame-retardant noise-reducing layer when the roof substrate is positioned to overlap the second roof substrate.

[0021] In an additional aspect, the roof shingle includes a flame retardant noise reduction layer and a weatherable shingle substrate. In some examples, the flame retardant noise reduction layer includes a porous core layer including an open-cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm, for example at least 2800 gsm, and an open-cell skin bonded to a first surface of the porous core layer, the flame retardant noise reduction layer includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the flame retardant noise reduction layer includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17. The weatherable shingle substrate can be bonded to the first surface of the flame retardant noise reduction layer and can be configured to bond to a roof panel of a building to provide a weatherable flame retardant noise reduction shingle on the roof panel.

[0022] In some embodiments, the shingle includes a weather barrier bonded to the second surface of the flame retardant noise reduction layer. In some embodiments, the shingle includes asphalt. In other embodiments, the open cell skin includes at least 10% open surface area, and the shingle includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In certain embodiments, the flame retardant includes expandable graphite particles, or magnesium hydroxide, or both. In some embodiments, the open cell skin includes a perforated film having at least 10% open surface area, and the shingle includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some embodiments, the shingle includes a closed cell skin disposed on the second surface of the porous core layer. In certain embodiments, the flame retardant is homogeneously dispersed in the porous core layer. In certain embodiments, the thermoplastic material includes a polyolefin resin, and the plurality of reinforcing fibers includes glass fibers, or mineral fibers, or both. In another embodiment, the shingle includes a second shingle including a second flame-retardant noise-reducing layer bonded to the second weather-resistant shingle, wherein the flame-retardant noise-reducing layer is configured to engage with the second flame-retardant noise-reducing layer when the weather-resistant shingle is positioned to overlap the second weather-resistant shingle.

[0023] In another embodiment, a recreational vehicle interior panel includes a flame retardant sound reduction layer and an interior wall substrate. The flame retardant sound reduction layer includes a porous core layer including an open-cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm, for example at least 2800 gsm, and an open-cell skin bonded to a first surface of the porous core layer. The interior wall substrate can be bonded to a second surface of the porous core layer, the recreational vehicle interior panel includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the recreational interior vehicle panel includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17.

[0024] In some embodiments, the interior wall substrate is configured as a decorative layer. In other embodiments, the open cell skin comprises at least 10% open surface area, and the recreational vehicle interior panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some embodiments, the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both. In certain embodiments, the open cell skin comprises a perforated film having at least 10% open surface area, and the recreational vehicle interior panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other embodiments, the recreational interior vehicle interior panel comprises a closed cell skin disposed on the second surface of the porous core layer. In other embodiments, the flame retardant is homogeneously dispersed in the porous core layer. In some embodiments, the thermoplastic material comprises a polyolefin resin, and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both. In another embodiment, the recreational vehicle interior panel includes a second recreational vehicle interior panel including a second flame retardant noise reducing layer bonded to a second interior wall substrate, the flame retardant noise reducing layer configured to lock onto the second flame retardant noise reducing layer when the interior wall substrate is positioned in vertical overlap with the second interior wall substrate on a first side of the recreational vehicle interior panel. In an additional embodiment, the recreational vehicle interior panel includes a third recreational vehicle interior panel including a third flame retardant noise reducing layer bonded to a third interior wall substrate, the flame retardant noise reducing layer configured to lock onto the third flame retardant noise reducing layer when the interior wall substrate is positioned in vertical overlap with the third interior wall substrate on a second side of the recreational vehicle interior panel.

[0025] In an additional embodiment, a recreational vehicle exterior panel includes a flame retardant sound reduction layer and a weather resistant exterior wall substrate. The flame retardant sound reduction layer includes a porous core layer including an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm, for example at least 2800 gsm, and an open cell skin bonded to a first surface of the porous core layer. The weather resistant exterior wall substrate can be bonded to a second surface of the porous core layer, the recreational vehicle exterior panel includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the recreational exterior vehicle panel includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17.

[0026] In some examples, the exterior wall substrate comprises fiberglass or is configured as a metal panel. In other examples, the open cell skin comprises a perforated film having at least 10% open surface area, and the recreational vehicle exterior panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In additional examples, the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both. In other embodiments, the open cell skin comprises a perforated film having at least 10% open surface area, and the recreational vehicle exterior panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some examples, the recreational vehicle exterior panel comprises a closed cell skin disposed on the second surface of the porous core layer. In other examples, the flame retardant is homogeneously dispersed in the porous core layer. In some embodiments, the thermoplastic material comprises a polyolefin resin, and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both. In other examples, the recreational vehicle exterior panel includes a second recreational vehicle exterior panel including a second flame retardant noise reducing layer coupled to a second exterior wall substrate, where the flame retardant noise reducing layer is configured to lock onto the second flame retardant noise reducing layer when the exterior wall substrate is positioned to overlap the second exterior wall substrate on a first side of the recreational vehicle exterior panel. In some examples, the recreational vehicle exterior panel includes a third recreational vehicle exterior panel including a third flame retardant noise reducing layer coupled to a third exterior wall substrate, where the flame retardant noise reducing layer is configured to lock onto the third flame retardant noise reducing layer when the exterior wall substrate is positioned to overlap the third exterior wall substrate on a second side of the recreational vehicle exterior panel.

[0027] In another aspect, an interior building panel including two or three dimensional features is provided. In some examples, the interior building panel includes a porous core layer including an open-cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm, for example at least 2800 gsm, and an open-cell skin disposed on a first surface of the porous core layer, the interior building panel including two or three dimensional features includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17, and the interior building panel including two or three dimensional features includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009.

[0028] In an additional aspect, an interior trim article is described. The interior trim may, for example, include a flame retardant noise reduction layer and an interior trim substrate. The flame retardant noise reduction layer includes a porous core layer including an open-cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm, for example, at least 2800 gsm, and an open-cell skin disposed on a first surface of the porous core layer, the flame retardant noise reduction layer includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17, and the flame retardant noise reduction layer includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009. The interior trim substrate may be bonded to the first surface of the flame retardant noise reduction layer. The interior trim may be, for example, a base molding, a crown molding, a door molding, a chair rail, a window molding, or other interior trim article.

[0029] Additional aspects, configurations, embodiments, examples, and features are described in more detail below. [Brief description of the drawings]

[0030] Certain exemplary configurations of composite articles are described with reference to the figures. [Figure 1] FIG. 1 is a diagram of a composite article including a prepreg or core layer bonded on one surface to an open cell skin according to a particular configuration. [Diagram 2] FIG. 2 is a diagram of a composite article including a prepreg or core layer bonded on one surface to an open cell skin, where different regions of the open cell skin include different porosities or permeabilities according to a particular configuration. [Diagram 3] FIG. 2 is a diagram of a composite article including a prepreg or core layer bonded on one surface to an open cell skin and a second open cell skin bonded to the open cell skin according to a particular configuration. [Figure 4A] FIG. 2 is a diagram of a composite article including a prepreg or core layer bonded on one surface to an open cell skin and including a surface layer disposed on the open cell skin, in accordance with certain embodiments. [Figure 4B] FIG. 2 is a diagram of a composite article including a prepreg or core layer bonded on one surface to an open cell skin, and including a surface layer disposed on the open cell skin and another surface layer disposed on the prepreg or core layer, in accordance with certain embodiments. [Diagram 5] FIG. 2 is a diagram of a composite article including a prepreg or core layer bonded on one surface to an open cell skin and on an opposing surface to a closed cell skin according to certain embodiments. [Figure 6] FIG. 2 is a diagram of a composite article including a prepreg or core layer bonded to an open cell skin on one surface and a surface layer bonded to the prepreg or core layer on an opposing surface, according to some configurations. [Figure 7] FIG. 2 is a diagram of a composite article including a prepreg or core layer bonded on one surface to an open cell skin and on an opposing surface to a closed cell skin, the open cell skin being bonded to a surface layer, according to certain embodiments. [Figure 8] FIG. 2 is a diagram of a composite article including a first prepreg or core layer bonded to a second prepreg or core layer through an open cell skin, according to certain embodiments. [Figure 9] FIG. 2 is a diagram of a composite article including a first prepreg or core layer bonded through an open cell skin to a second prepreg or core layer, and including another open cell skin bonded to one of the prepreg or core layers, according to certain examples. [Figure 10] FIG. 2 is a diagram of a composite article including a first prepreg or core layer bonded to a second prepreg or core layer through an open cell skin and including a closed cell skin bonded to one of the prepreg or core layers according to certain embodiments. [Figure 11] FIG. 1 illustrates ceiling tiles, one of which includes a LWRT article as described herein, according to certain embodiments. [Figure 12] FIG. 2 is a diagram of cubicle panels, one of the panels including an LWRT article described herein, according to certain embodiments. [Figure 13A] In accordance with certain embodiments, structural panels comprising the LWRT articles described herein are [Figure 13B] 1 is a diagram of a structural panel including an LWRT article bonded to a structural substrate, according to certain embodiments. [Figure 14] FIG. 2 is a diagram of a wallboard including a LWRT article as described herein, according to certain embodiments. [Figure 15] FIG. 1 is a diagram of an architectural siding including an LWRT article described herein according to certain embodiments. [Figure 16] FIG. 2 is a diagram of a roof panel including a LWRT article as described herein, according to certain embodiments. [Figure 17] FIG. 2 is a diagram of a roof shingle including an LWRT article described herein, according to certain embodiments. [Figure 18] FIG. 1 is a diagram of an interior recreational vehicle wall including LWRT articles described herein, according to certain embodiments. [Figure 19] FIG. 1 is a diagram of an exterior recreational vehicle wall including a LWRT article as described herein, according to certain embodiments. [Figure 20]1 is a diagram of an interior panel including a LWRT article including two-dimensional features, according to certain embodiments. [Figure 21] 1 is a diagram of an interior trim including an LWRT article including two-dimensional features, according to a particular configuration. [Figure 22] 1 is a graph illustrating sound absorption results for certain tested materials, in accordance with certain embodiments. [Figure 23] 1 is a graph showing acoustic properties measured for Sample A1 and Sample A2 according to certain configurations. [Figure 24] 1 is a graph illustrating the sound absorption performance of Subject B samples, in accordance with certain examples. [Diagram 25] 13 is a graph illustrating the sound absorption performance of Sample B3, in accordance with certain examples. [Figure 26A] 1 is a photograph showing the top side of a test specimen after flammability testing, according to some examples. [Figure 26B] 1 is a photograph showing the underside of a test specimen after flammability testing, according to some examples. [Figure 27] 1 is a bar graph comparing flexural strength measurements of different samples, according to some examples. [Figure 28] 2 is another bar graph comparing flexural strength measurements of different samples, according to some examples.Those of ordinary skill in the art, given the benefit of this disclosure, will recognize that the exemplary representations shown in Figures 1-21 are provided for convenience and to facilitate better understanding.The exact shape, length, width, thickness, geometric arrangement, and overall orientation of the components in the figures may vary depending on the intended use and desired properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] Examples of several configurations of composite articles are described that may include two or more layers bonded together. Although various layers are shown in the figures and described below, the thicknesses, sizes, and geometric arrangements of the different layers need not be the same and may be other thicknesses, sizes, and geometric arrangements than those shown in the figures. Additionally, the exact arrangement or layering of components may be changed, or intermediate layers may exist between the exemplary layers shown in the figures.

[0032] In certain embodiments, the articles described herein generally include a prepreg or core layer bonded to another layer. The prepreg may be a core layer that is not fully formed and may include a material that is processed to form the final core layer. For example, the prepreg may include a thermoplastic material in combination with reinforcing fibers, but may not be fully formed or may exist in a softened state by applying heat. The prepreg may be pressed, compressed, or molded into a desired shape to provide the core layer. Other layers bonded to the prepreg layer may be added before or after the core is fully formed. The other layers may be bonded to the prepreg or core layer using an adhesive, or in some cases, the prepreg or core layer may be bonded directly to the other layers without the use of an adhesive material between the prepreg or core layer and the other layers.

[0033] In certain examples, the prepreg or core layer may be used in lightweight reinforced thermoplastic (LWRT) articles. LWRT may provide certain desirable properties, including but not limited to high stiffness / weight ratio, low part weight, simple and low-cost part molding process, low coefficient of thermal expansion, recyclability, etc. LWRT has a wide range of applications in the automotive industry, including different types of soft trim for both interior and exterior applications. Recreational vehicles, commercial truck trailers, and similar applications represent another category of wide applications of LWRT articles. Ceiling tiles, office panels, cubicle panels, building and construction industries may also use the LWRT articles described herein.

[0034] In some examples, the LWRT articles described herein may provide a desired level of flame retardancy and sound absorption or noise reduction. For example, certain articles described herein may conform to either the FMVSS 302 test or the SAE J369 test standard. These tests are generally equivalent and are used to determine a measurement of the burn rate. Briefly, the test uses a horizontal flame chamber, a fume hood, a tote large enough to handle a test specimen about 12 inches long, a water source, a timer, a lighter, and a ruler. The test specimen size is about 4 inches by about 12 inches, and typically five or more specimens are tested. The adhesive side of the test specimen is typically subjected to a flame. In the FMVSS 302 test, the fume hood is typically open enough to provide an airflow of about 150 cubic feet per minute. In the SAE J369 test, for example, the fume hood may be opened to provide the same airflow or may be fully open. Unless otherwise noted, the FMVSS 302 test may be interchanged with the SAE J369 test. The results of these tests may be classified in several ways, including DNI, SE / 0, SE / NBR, SE / B, B, and RB. DNI refers to materials that do not support burning during or after the 15 second ignition period and / or do not propagate a flame front to the selected distance on either surface. SE / 0 refers to a material that ignites on the surface, but the flame is extinguished before traveling the selected distance. SE / NBR refers to a material that stops burning before burning 60 seconds from the start of the ignition adjustment and does not burn more than about 50 mm from the start of the ignition adjustment. SE / B refers to a primary flame front that travels the selected distance but is extinguished before reaching the second distance. B refers to a material that burns the entire distance. RB refers to a material that burns very quickly and the burn rate cannot be measured. One or more of burn distance, burn time, burn rate, and whether the material is self-extinguishing may also be measured. A specimen may be considered to "conform" or "pass" the FMVSS 302 or SAE J369 test if the flame travels less than about 102 mm per minute. A specimen may fail the test if it burns faster than 102 mm per minute.

[0035] In some configurations described herein, the presence of a flame retardant material in the thermoplastic prepreg or thermoplastic core allows the prepreg or core to provide flame retardancy, at least to some extent. For example, the prepreg or core (and composite articles including the prepreg or core layer) may meet the Class A standard of the ASTM E84 test entitled "Standard Test Method for Surface Burning Characteristics of Building Materials", 2009. The particular flame retardant material selected for use in the core layer may provide the article with an as-formed article that meets the Class A or Class B requirements of ASTM E84, for example, unmolded or, if desired, in a molded article. Class A articles differ from Class B articles in that Class A articles have a flame spread index of about 0-25, while Class B articles have a flame spread index of about 26-75. In some cases, there is enough flame retardant material in the final prepreg or core that the prepreg or core meets Class A standards based on the 2009 ASTM E84 test.

[0036] In certain examples, the LWRT articles described herein may also provide sound absorption or noise reduction in addition to being flame retardant. A variety of different acoustic measurement tests may be performed to evaluate noise reduction, including ASTM C423-17, entitled "Standard Test Method for Sound Absorption and Sound Absorption Coefficients by the Reverberation Room Method." For example, a sound absorption average (SAA) value may be measured based on absorption at a series of frequencies. Similar to the SAA, the Noise Reduction Coefficient (NRC) is also based on a series of frequencies. The Sound Absorption Average (SAA) is defined as a single numerical rating, the average, rounded to the nearest 0.01, of the sound absorption coefficients of a material in 12 1 / 3 octave bands from 200 to 2500 Hz. The Noise Reduction Coefficient (NRC) is defined from previous versions of this same test method as the average of the coefficients at 250, 500, 1000, and 2000 Hz, expressed to the nearest integer multiple of 0.05. The NRC / SAA test also specifies the method of mounting the test specimen, which is described in ASTM E795-16 Type E 400 mounting method.

[0037] In certain configurations of the articles described herein, the articles may provide both flame retardancy and noise reduction. With the benefit of this disclosure, it will be recognized by those skilled in the art that the exact level of flame retardancy and noise reduction may depend on the materials used in the composite article, as well as their placement and orientation relative to the incoming sound waves, and / or potential heat or flame sources. In some cases, referring to FIG. 1, an article 100 is shown that includes a prepreg or core layer 110 bonded to an open-cell skin 120. The skin 120 is disposed on a first surface 112 of the prepreg or core 110. In FIG. 1, the surface 114 may be open and may not include any other layers or materials disposed thereon. As mentioned herein, the skin 120 may be disposed and bonded directly to the prepreg or core layer 110, for example, without the use of adhesive materials, or glues, spot welding or melting or other materials, and instead, techniques may be used to hold the skin 120 to the prepreg or core layer 110.

[0038] In certain examples, the prepreg or core layer 110 may include thermoplastic material and reinforcing fibers, which may be held in place in the general form of a web by the thermoplastic material. The fibers are generally arranged in a random manner without any particular orientation or configuration. In certain examples, the thermoplastic material of the prepreg or core may be present in fiber form, particulate form, resin form, or other suitable form. In some cases, the thermoplastic material used in the prepreg may be present in particulate form, having an average particle size that is substantially the same as the average particle size of the flame retardant material. Without wishing to be bound by any particular scientific theory, by matching the particle sizes of the thermoplastic material and the flame retardant material, enhanced processing of the prepreg or core may be achieved, including, for example, an increased loading of the flame retardant material in the prepreg or core. In some cases, the average particle size of the flame retardant material and the average particle size of the thermoplastic material may vary by about 5% to about 10%, and enhanced processing may still be achieved. In certain configurations, the average particle size of each of the thermoplastic material and the flame retardant material in the prepreg may differ by about 50 microns to about 100 microns. In some configurations, the average particle size of the flame retardant material is at least 50% of the average particle size of the thermoplastic material particles, providing enhanced processing. In other cases, a flame retardant material having an average particle size approximately the same as the average particle size of the thermoplastic material may be present along with a flame retardant material of an average particle size different from the average particle size of the thermoplastic material. Even though the average particle sizes of the flame retardant materials may be different, the chemical composition of the flame retardant materials may be the same or different. In still other configurations, there may be two or more thermoplastic materials with different average particle sizes. If desired, there may be two flame retardant materials with an average particle size that is substantially the same as the average particle size of the thermoplastic material. The two flame retardant materials may be chemically the same or chemically different. Similarly, the thermoplastic materials may be chemically the same (but have different average particle sizes) or chemically different. In certain cases, the virgin or natural thermoplastic material used to produce the prepreg or core may be the same thermoplastic material that is present in the formulated flame retardant material, e.g., a mixture of flame retardant and thermoplastic material.In other cases, the formulated flame retardant material may include two or more thermoplastic materials where one of the thermoplastic materials is the same as the virgin thermoplastic material used to produce the prepreg.

[0039] In certain embodiments, the prepreg or core 110 generally includes a significant amount of open cell structure such that void space is present in the prepreg. For example, the prepreg or core 110 may include 0-30%, 10-40%, 20-50%, 30-60%, 40-70%, 50-80%, 60-90%, 0-40%, 0-50%, 0-60%, 0-70%, 0-80%, 0-90%, 10-50%, 10-60%, 10-70%, 10-80%, 10-90%, 10-95%, 20-60%, 20-70%, 20-80%, 20-95%, 20-95%, 20-10 ... The prepreg may include a void content or porosity of 0%, 20-90%, 20-95%, 30-70%, 30-80%, 30-90%, 30-95%, 40-80%, 40-90%, 40-95%, 50-90%, 50-95%, 60-95%, 70-80%, 70-90%, 70-95%, 80-90%, 80-95%, or any exemplary value within these exemplary ranges. In some cases, the prepreg is comprised of a porosity or void content of greater than 0%, e.g., up to about 95% that is not fully consolidated. Unless otherwise indicated, references to a prepreg or core that includes a particular void content or porosity are based on the total volume of the prepreg or core, and not necessarily the total volume of the prepreg or core plus any other materials or layers bonded to the prepreg or core.

[0040] In certain embodiments, the high porosity present in the prepreg allows for the trapping of sound waves within the open structure of the prepreg or core layer, and the flame retardant material may be trapped within the pores or voids. For example, the flame retardant material may be present in the void space in a non-covalent manner. The presence of the flame retardant material in the void space may provide enhanced flame retardancy, and the presence of the void space may generally act to absorb and / or deflect sound waves within the prepreg or core 110. The flame retardant material may also be coated on the surface of the prepreg to provide enhanced flame retardancy.

[0041] In certain embodiments, the thermoplastic material of the prepreg or core 110 may at least partially comprise one or more of polyethylene, polypropylene, polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachlorate, and polyvinyl chloride (plasticized and unplasticized), as well as blends of these materials with each other or with other polymeric materials. Other suitable thermoplastics include, but are not limited to, polyarylene ethers, polycarbonates, polyester carbonates, thermoplastic polyesters, polyimides, polyetherimides, polyamides, acrylonitrile-butyl acrylate-styrene polymers, amorphous nylons, polyarylene ether ketones, polyphenylene sulfides, polyarylsulfones, polyethersulfones, liquid crystal polymers, poly(1,4 phenylene) compounds commercially known as PARMAX®, high heat polycarbonates such as Bayer's APEC® PC, high temperature nylons, and silicones, as well as alloys and blends of these materials with each other or with other polymeric materials. The virgin thermoplastic material used to form the prepreg or core 110 may be used in powder form, resin form, rosin form, fiber form, or other suitable form. Exemplary thermoplastic materials in various forms are described herein, for example, in U.S. Patent Application Publication Nos. 2013 / 0244528 and 2012 / 0065283. The exact amount of thermoplastic material present in the prepreg or core 110 may vary, with exemplary amounts ranging from about 20% to about 80% by weight.

[0042] In certain examples, the reinforcing fibers of the prepreg or core 110 described herein may include glass fibers, carbon fibers, graphite fibers, synthetic organic fibers, particularly high modulus organic fibers such as para- and meta-aramid fibers, nylon fibers, polyester fibers, or any high melt flow index resin suitable for use as fibers, natural fibers such as hemp, sisal, jute, flax, coir, kenaf, and cellulosic fibers, mineral fibers such as basalt, mineral wool (e.g., rock wool or slag wool), wollastonite, alumina silica, and the like, or mixtures thereof, metal fibers, metallized natural and / or synthetic fibers, ceramic fibers, yarn fibers, or mixtures thereof. In some cases, one type of reinforcing fiber may be used with mineral fibers, such as, for example, fibers formed by spinning or drawing molten minerals. Exemplary mineral fibers include, but are not limited to, mineral wool fibers, glass wool fibers, stone wool fibers, and ceramic wool fibers. In some embodiments, any of the aforementioned fibers may be chemically treated prior to use to provide the fibers with desired functional groups or to impart other physical properties, e.g., they may be chemically treated so that they may react with a thermoplastic material, a flame retardant material, or both. Alternatively, a flame retardant material may react with the thermoplastic material of the prepreg or core 110 to provide a derivatized thermoplastic material that is then mixed with the fibers. The total fiber content in the prepreg or core 110 may be from about 20% to about 90% by weight of the prepreg, more specifically, from about 30% to about 70% by weight of the prepreg. Typically, the fiber content of a composite article including the prepreg or core 110 varies between about 20% to about 90% by weight of the composite, more specifically, from about 30% to about 80% by weight, e.g., from about 40% to about 70% by weight. The particular size and / or orientation of the fibers used may depend, at least in part, on the polymeric material used and / or the desired properties of the resulting prepreg. Suitable additional fiber types, fiber sizes, and amounts will be readily selected by the person of ordinary skill in the art, given the benefit of this disclosure.In one non-limiting example, the fibers dispersed in the thermoplastic material to provide the prepreg generally have a diameter greater than about 5 microns, more specifically, between about 5 microns and about 22 microns, and a length between about 5 mm and about 200 mm. More specifically, the fiber diameter can be between about microns and about 22 microns, and the fiber length can be between about 5 mm and about 75 mm. In some configurations, the flame retardant material can be present in fibrous form. For example, the prepreg or core 110 can include a thermoplastic material, a reinforcing fiber, and a fiber comprising a flame retardant material, such as a fiber comprising an EG material or an inorganic flame retardant material. The flame retardant fiber can include any one or more of the flame retardant materials described herein. For example, polypropylene fibers compounded with a hydroxide material extruded and cut into fibers using a suitable die or other device, or an EG material mixed with polypropylene fibers compounded with a hydroxide material extruded and cut into fibers using a suitable die or other device.

[0043] In some configurations, the prepreg or core 110 may be substantially halogen-free or halogen-free prepreg to meet regulations regarding hazardous materials requirements for a particular application. In other cases, the prepreg may include halogenated flame retardants (which may be present in the flame retardant material or may be additionally added to the flame retardant material), such as halogenated flame retardants including one or more of F, Cl, Br, I, and At, or compounds containing such halogens, such as tetrabromobisphenol-A polycarbonate, or monohalo-, dihalo-, trihalo-, or tetrahalo-polycarbonates. In some cases, the thermoplastic materials used in the prepreg and core may include one or more halogens to impart some degree of flame retardancy without the addition of another flame retardant. For example, the thermoplastic materials may be halogenated in addition to the flame retardant material being present, or virgin thermoplastic materials may be halogenated and used on their own. When a halogenated flame retardant is present, it is desirably present in a flame retardant amount that may vary depending on other components present. For example, the halogenated flame retardant present in addition to the flame retardant material may be present at about 0.1 weight percent to about 15 weight percent (based on the weight of the prepreg), more specifically, about 1 weight percent to about 13 weight percent, for example, about 5 weight percent to about 13 weight percent. If desired, two different halogenated flame retardants may be added to the prepreg. In other cases, a non-halogenated flame retardant may be added, such as a flame retardant containing one or more of N, P, As, Sb, Bi, S, Se, and Te. In some embodiments, the non-halogenated flame retardant may include a phosphorus-containing material, thus making the prepreg more environmentally friendly. When a non-halogenated or substantially halogen-free flame retardant is present, it is desirably present in a flame retardant amount that may vary depending on other components present.For example, the substantially halogen-free flame retardant may be present at about 0.1 weight percent to about 15 weight percent (based on the weight of the prepreg), more specifically, about 1 weight percent to about 13 weight percent, such as about 5 weight percent to about 13 weight percent, based on the weight of the prepreg. If desired, two different substantially halogen-free flame retardants may be added to the prepreg. In certain cases, the prepregs described herein may include one or more halogenated flame retardants in combination with one or more substantially halogen-free flame retardants. When two different flame retardants are present, the combination of the two flame retardants may be present in an amount of flame retardant that may vary depending on other components present. For example, the total weight of the flame retardants present may be about 0.1 weight percent to about 20 weight percent (based on the weight of the prepreg or core), more specifically, about 1 weight percent to about 15 weight percent, such as about 2 weight percent to about 14 weight percent, based on the weight of the prepreg or core. The flame retardants used in the prepregs or cores described herein may be added to the mixture containing the thermoplastic material and fibers (prior to placement of the mixture on a wire screen or other processing component) or may be added after the prepregs or cores are formed.

[0044] In other configurations as described herein and above, the composite article may include flame retardant material such that the composite article complies with ASTM E84 or SAE J369 methods (revised November 2007). This test method is referred to as the SAE Flammability Test or SAE Self-Extinguishing Test in certain cases herein and in the claims. In some examples, less than 10 weight percent of flame retardant material, less than 9 weight percent of flame retardant material, less than 8 weight percent of flame retardant material, less than 7 weight percent of flame retardant material, less than 6 weight percent of flame retardant material, or even less than 5 weight percent of flame retardant material may be present in the prepreg or core layer such that the composite article complies with or passes the non-oil-immersed and oil-immersed SAE flammability tests.

[0045] In certain embodiments, the flame retardant may include many different materials, including organic and inorganic flame retardant materials. In certain examples, expandable graphite materials may be used in the prepreg or core 110 and may include one or more graphene-based materials that are typically present in laminated molecular layers. Without wishing to be bound by any particular theory, in addition to providing lofting functionality, the expandable graphite material may also provide some degree of flame retardancy. In some embodiments, there is sufficient expandable graphite material, e.g., a flame retardant amount of expandable graphite material, in the prepreg or core 110 such that the prepreg or core 110 meets the 2009 ASTM E84 test or the 1991 Federal Motor Vehicle Safety Standard 302 (FMVSS 302) flammability test (which are generally equivalent to the 1989 ISO 3795 and 2004 ASTM D5132). Such amounts of flame retardant allow for the construction of a prepreg or core 110 that is substantially free of external flame retardants. The exact type of expandable graphite material used in the prepreg may depend on many factors, including, for example, the desired lofting temperature, the desired flame retardancy, the desired acoustic performance, and the like. Exemplary commercially available expandable graphite materials are available from Nyacol Nano Technologies, Inc. (Ashland, MA), including, for example, grades 35, 200, 249, 250, 251, KP251, and 351 expandable graphite materials. Additional expandable graphite materials may be purchased commercially from Graftech International (Lakewood, OH). While not wishing to be bound by any particular reaction, expandable graphite materials may generally be produced by acidifying graphite ore. Acidification results in an intercalation process in which, for example, sulfuric acid acts as an intercalator. The solution may then be neutralized to provide a series of layers of sheets of hexagonal carbon-carbon bonded material. The layers are generally flat and interact with additional hexagonal carbon-carbon layers to provide a layered sheet structure.The layered sheet structure may be held together through covalent bonds or electrostatic interactions (or both) between the sheets. Heating the expandable graphite material in the thermoplastic prepreg or core 110 described herein may result in an increase in interlayer separation and, consequently, an increase in prepreg thickness. If desired, the expandable graphite material may be oxidized using a suitable oxidizing agent to form graphene oxide. As referred to herein, the expandable graphite material may exist in many forms, including flake form, particulate form, or other forms. In some cases, the expandable graphite material may exist in particulate form and may, for example, include an average particle size of at least 300 microns.

[0046] In certain configurations, the flame retardant may include an inorganic material or an inorganic salt. For example, restrictions on hazardous substances (RoHS) may make it desirable to select a flame retardant material as an inorganic salt that is substantially free (or free) of halides. In some embodiments, the flame retardant material may include a group II metal or a group III metal in combination with one or more anions. For example, the flame retardant material may include beryllium, calcium, magnesium, or other group II metal salts. In some embodiments, the group II metal of the flame retardant material may be present as a hydroxide material. For example, the flame retardant material may be present as beryllium hydroxide, calcium hydroxide, magnesium hydroxide (MDH), or other group II metal hydroxides. In other cases, the flame retardant material may include aluminum, gallium, indium, or other group III metal salts. In some embodiments, the group III metal salt of the flame retardant material may be present as a hydroxide material. For example, the flame retardant material may be present as aluminum hydroxide (ATH), or gallium hydroxide, or other group III metal hydroxides. In other configurations, the inorganic material present as the flame retardant material may include one or more transition metal salts that may function as a flame retardant material. For example, a transition metal that may form a divalent cation in solution may be combined with one or more anions and used as a flame retardant. In some cases, to avoid outgassing of toxic gases when the prepreg or core is burned, the transition metal salt may be present in a non-halide form, e.g., not as a fluoride, chloride, bromide or iodide salt. In certain configurations, the transition metal salt may be present, for example, as a hydroxide.

[0047] The exact amount of flame retardant material used in the prepreg and core may vary depending on the other materials present, but the flame retardant material is usually present in a weight percent less than the major amount of the prepreg or core, e.g., the flame retardant material is usually present in 50 weight percent or less based on the weight of the prepreg or core. In certain cases, the flame retardant material is present in more than a small amount to provide flame retardancy to the prepreg or core. For example, the flame retardant material may be present in 30 weight percent or more, 35 weight percent or more, 40 weight percent or more, or even 45 weight percent or more based on the weight of the prepreg or core. For example, the flame retardant material:other material ratio may vary from 1:1, 2:13:1, 4:1:5:1, 1:5, 1:4, 1:3, or 1:2.

[0048] Depending on the particular process used to produce the prepreg or core, the flame retardant material may be ground, filtered, sized, or otherwise processed prior to addition to the other materials in the prepreg or core. In some cases where thermoplastic particles are used in the prepreg or core, the average particle size of the flame retardant material may be about the same as the average particle size of the thermoplastic material. In other configurations, the average particle size of the flame retardant material may be smaller or larger than the average particle size of the thermoplastic material particles used in the prepreg or core.

[0049] In certain configurations, a porous prepreg or core may be produced that includes one or more thermoplastic materials and a plurality of fibers that together provide an open cell structure, e.g., void space. In some configurations, a flame retardant material, e.g., EG material, Group II metal salt, Group III metal salt, etc., may be introduced into the void space in such a manner that the flame retardant material resides (at least partially) within the void space formed by the intersection of fibers, which may be held in place by the thermoplastic material. In some cases, the thermoplastic material and / or fibers may be selected such that they are generally inert or non-reactive with the flame retardant material. In some examples, the flame retardant material may not be covalently bonded to the thermoplastic material and / or fibers, but there may be an association between any charged flame retardant material and the thermoplastic material of the porous prepreg. For example, weak interactions, such as van der Waals interactions or electrostatic interactions, may occur between the flame retardant material and other components of the prepreg or core.

[0050] In certain embodiments, the open cell skin 120 generally includes a sufficient amount of open surface area to allow sound waves to enter the prepreg or core 110. The open structure may be within the film itself, for example, by a network of crosslinked material in the film, or may be provided by treating the film using a suitable method that increases the open surface area of ​​the film, including creating perforations, slits, holes, apertures, punches, or other structures. In some examples, the open cell skin includes at least 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15% or more open surface area (based on the overall surface area of ​​the skin). In some cases, the open surface area of ​​the skin is selected to provide the desired noise reduction factor, but is not so open that it lacks the proper structure to function as a film.

[0051] In some cases, the material used in the open cell skin may be a polyolefin, a copolymer including a polyolefin, a polyamide, a copolymer including a polyamide, or a combination thereof. The exact basis weight of the open cell skin or film may vary from about 10 gsm to about 150 gsm, for example, about 70 to 120 gsm, or about 80 to 110 gsm, or about 85 to 100 gsm, although the open cell skin or film may be lighter or heavier depending on the exact open surface area present. In some cases, the open cell skin may take the form of an open cell film, an open cell scrim, an open cell flim (film + scrim), or other open cell layer. For example, the open cell skin may include an open cell polyethylene film, an open cell polypropylene film, or an open cell polyamide film, or a combination thereof.

[0052] In certain embodiments, as referred to herein, the open cell skin and prepreg or core may together provide both flame retardant and noise reducing properties. For example, when used together, the open cell skin and prepreg or core layers may provide an article having a noise reduction factor of at least 0.5 when tested by ASTM C423-17, a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009. In other configurations, the open cell skin and prepreg or core layers may together provide an article having a noise reduction factor of at least 0.65 when tested by ASTM C423-17, a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009. In some examples, the open cell skin and prepreg or core layers can together provide an article having a noise reduction factor of at least 0.75 when tested by ASTM C423-17, and a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009. In additional examples, the open cell skin and prepreg or core layers can together provide an article having a noise reduction factor of at least 0.85 when tested by ASTM C423-17, and a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009. In other examples, the open cell skin and prepreg or core layers can together provide an article having a noise reduction factor of at least 0.85 when tested by ASTM C423-17, and a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009. In some examples, the open cell skin and prepreg or core layers may together provide an article having a Noise Reduction Factor of at least 0.88 or 0.9 when tested by ASTM C423-17, and a Flame Spread Index of less than 25 and a Smoke Development Index of less than 150 when tested by ASTM E84, 2009.

[0053] In certain embodiments, the open cell skin need not have the same porosity or structure across the entire flat surface of the film. With reference to FIG. 2, article 200 includes a prepreg or core layer 210 and an open cell skin 220 disposed on the surface of layer 210. Open cell skin 220 includes region 222 having a first open surface area and regions 224, 226 having a different surface area than region 222. The open surface areas of regions 224, 226 do not have to be the same, but may be the same. In some cases, the open surface area of ​​regions 224, 226 is greater than the open surface area of ​​region 222, while in other cases, the open surface area of ​​regions 224, 226 is less than the open surface area of ​​region 222. For example, if the composite article is used as a cubicle panel, ceiling tile, or wall construction, the edge regions of the article may not need to provide the same noise reduction coefficient as the center portion of the article. In other cases, it may be desirable to vary the open surface area across the flat surface of the skin 220 to provide different noise reduction coefficients at different frequencies. For example, if the article is configured for use in a movie theater ceiling tile, it may be desirable to configure the skin 220 to include different noise coefficient reductions in different areas such that the skin 220 provides variable noise reduction properties. The prepreg or core layer 210 may include any of those components described in connection with the prepreg or core layer 110, and is generally configured as a "heavy" layer having an areal weight of at least 2000gsm, or at least 2100gsm, or at least 2200gsm, or at least 2300gsm, or at least 2400gsm, or at least 2500gsm. For example, the prepreg or core layer 210 may include one or more thermoplastic materials, flame retardant materials, and reinforcing fibers randomly arranged in the prepreg or core layer 210.

[0054] In other examples, two or more different open cell skins may be layered on the core layer. With reference to FIG. 3, a composite article 300 includes a prepreg or core layer 300, a first open cell skin 320 disposed on the prepreg or core layer 320, and a second open cell skin 330 disposed on the first open cell skin 320. In some cases, the first skin 320 may include a larger open surface area than the second skin 330, while in other cases, the first skin 320 may include a smaller open surface area than the second skin 330. If desired, the skins 320, 330 may be melted or bonded together to provide a single composite skin layer prior to placing the skins 320, 330 on the prepreg or core layer 310. Additionally, if desired, three or more skin layers may be bonded together. In some examples, the outermost skin may have the largest open surface area, allowing sound waves to enter the layered skin structure, and the skin closer to the prepreg or core layer 320 may have a smaller open surface area than the outer film layer. This exemplary skin arrangement may allow for capture or more sound waves in the layered skin structure and prepreg or core layer 310 than if only a single skin layer were used. The prepreg or core layer 310 may include any of those components described in connection with the prepreg or core layer 110, and is generally configured as a "heavy" prepreg or core layer having an areal weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm. For example, the prepreg or core layer 310 may include one or more thermoplastic materials, flame retardant materials, and reinforcing fibers randomly arranged in the prepreg or core layer 310.

[0055] In some configurations, one or more non-film layers may be bonded to the open cell skin. With reference to Figure 4, article 400 includes a prepreg or core layer 410 and an open cell skin 420 disposed on the prepreg or core layer 410. A surface layer 440 or skin is disposed on the open cell skin 420. As mentioned in more detail below, surface layer 440 can take many different configurations and is desirably porous or open to allow sound waves to enter composite article 400 through surface layer 440 and into skin 420 and core layer 410.

[0056] Layer 440 may include, for example, a scrim (e.g., a fiber-based scrim), a foil, a woven fabric, a nonwoven fabric, or may be present as an inorganic coating, an organic coating, or a thermosetting coating disposed on the prepreg or on core 410. In other cases, layer 440 may include a limiting oxygen index greater than about 22 as measured by ISO 4589, 1996. When a fiber-based scrim is present as (or as part of) layer 440, the fiber-based scrim may include at least one of glass fibers, aramid fibers, graphite fibers, carbon fibers, inorganic mineral fibers, metal fibers, metallized synthetic fibers, and metallized inorganic fibers. When a thermosetting coating is present as (or as part of) layer 440, the coating may include at least one of unsaturated polyurethanes, vinyl esters, phenolics, and epoxies. If an inorganic coating is present as (or as part of) layer 440, the inorganic coating may include minerals containing cations selected from Ca, Mg, Ba, Si, Zn, Ti, and Al, or may include at least one of gypsum, calcium carbonate, and mortar. If a nonwoven fabric is present as (or as part of) layer 440, the nonwoven fabric may include thermoplastic materials, thermosetting binders, inorganic fibers, metal fibers, metallized inorganic fibers, and metallized synthetic fibers.

[0057] Optionally, a second surface layer or skin may be present on the opposite surface of the core layer 410. For example, referring to FIG. 4B, a second surface layer 460 is disposed on the opposite surface of the prepreg or core layer 410 to provide a composite article 450. The second surface layer 460 may be the same as or different from the surface layer 440, and may be any one or more of those materials described in connection with the surface layer 440. The prepreg or core layer 410 may include any of those components described in connection with the prepreg or core layer 110, and is generally configured as a "heavy" prepreg or core layer having an areal weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm. For example, the prepreg or core layer 410 may include one or more thermoplastic materials, flame retardant materials, and reinforcing fibers randomly arranged in the prepreg or core layer 410.

[0058] In certain configurations, the composite articles described herein may include one or more closed cell skins. With reference to FIG. 5, a composite article 500 includes a prepreg or core layer 510 bonded to an open cell skin 520 on a first surface 512 and bonded to a closed cell skin 530 at a second surface 514. Without wishing to be bound by any particular theory, sound waves may enter the article 500 through the open cell skin 520 and into the core layer 510. The closed cell skin 530 may act to reflect the sound waves back to the core layer 510 and skin 520, absorbing the sound waves. Sound waves incident on the closed cell skin 530 may generally be reflected such that they do not pass through the article 500. By constructing article 500 with both open cell skin 520 and closed cell skin 530, sound waves can be absorbed through one surface and reflected by another surface, providing an increased noise reduction factor using article 500. Open cell skin 520 can be any of those films described above in connection with film layer 120.

[0059] The closed cell skin 530 generally includes a smaller open surface area than the open cell skin 520, and may include a heavier areal weight (for comparable thickness) compared to the areal weight of the open cell display 520. In some embodiments, even if the skin 530 is a closed cell skin, the skin 530 may allow for the transmission of water vapor through the article 500 to reduce the possibility of mold growth and / or allow water migration from one side of the article 500 to the other side of the article 500. The exact open surface area of ​​the closed cell skin 530 may vary, for example, from about 0% to less than 10%, such as from 1 to 9%, or from 2 to 8%, or from 3 to 7%, or from 4 to 6%, or less than 5% open area. When open cell and closed cell skins are used together, the open surface area of ​​the closed cell skin may be at least 50% less than the open cell skin, or may be at least 75%, 80%, 85%, or 90% less than the open cell skin. In some embodiments, the closed cell skin may be configured as a closed cell film, closed cell scrim, closed cell flim, or other closed cell layers and materials.

[0060] While the exact materials and configurations used for the closed cell skin 530 can vary, exemplary materials include, but are not limited to, polyethylene skins such as closed cell polyethylene films, polypropylene skins such as closed cell polypropylene films, polyamide skins such as closed cell polyamide films, or combinations thereof. In some examples, the closed cell skin 530 can be similar to the open cell skin 520 and can include the same materials such as, for example, polyolefin and polyamide materials, but the open cell skin 520 can include perforations or holes to increase the overall porosity or permeability of the skin 520 to allow sound waves to pass through the skin 520 into the underlying core layer 500. For example, the same film material can be used on both sides of the core layer, but the film on one surface of the core layer can be treated to provide perforations or openings before (or after) placing the film on the surface of the core layer. The prepreg or core layer 510 may include any of those components described in connection with the prepreg or core layer 110, and is generally configured as a "heavy" prepreg or core layer having an areal weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm. For example, the prepreg or core layer 510 may include one or more thermoplastic materials, flame retardant materials, and reinforcing fibers randomly arranged in the prepreg or core layer 510.

[0061] In certain examples, the composite articles described herein may include one or more surface layers on an opposite surface of the core layer than where the open cell film is present. With reference to FIG. 6, a composite article 600 includes a prepreg or core layer 610 bonded to an open cell skin 620 on a first surface 612 and bonded to a surface layer 650 at a second surface 614. The surface layer 650 may be any of those surface layers or skins described in connection with the surface layer 440 above. If desired, the surface layer may also include a closed cell skin disposed on one or more surfaces. The open cell skin 620 may be any of those skins described above in connection with the skin layer 120, e.g., an open cell film, an open cell scrim, an open cell flim, etc. The prepreg or core layer 610 may include any of those components described in connection with the prepreg or core layer 110, and is generally configured as a "heavy" prepreg or core layer having an areal weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm. For example, the prepreg or core layer 610 may include one or more thermoplastic materials, flame retardant materials, and reinforcing fibers randomly arranged in the prepreg or core layer 610.

[0062] In a particular embodiment, referring to Figure 7, an article 700 may include a prepreg or core layer 710, an open cell skin 720 disposed on a first surface 712 of the layer 710, a closed cell skin 730 disposed on another surface 714 of the layer 710, and a surface layer 750 disposed on the open cell skin 720. The open cell skin 720 may be any of those films described above in connection with the open cell skin 120, e.g., an open cell film, an open cell scrim, an open cell flim, etc. The closed cell skin 730 may be any of those films described above in connection with the closed cell film 530, e.g., a closed cell film, a closed cell scrim, a closed cell flim, etc. The prepreg or core layer 710 may include any of those components described in connection with the prepreg or core layer 110, and is generally configured as a "heavy" prepreg or core layer having an areal weight of at least 2500 gsm. For example, the prepreg or core layer 710 may include one or more thermoplastic materials, flame retardant materials, and reinforcing fibers randomly arranged in the prepreg or core layer 710 .

[0063] In certain configurations, the open cell skin may be bonded to multiple prepreg or core layers. For example, referring to FIG. 8, a composite article 800 includes a first core layer 810 and a second core layer 815 separated by an open cell skin 820. The prepreg or core layers 810, 815 may be the same or different. In some cases, the layers 810, 815 may generally include the same material but have different areal weights. For example, the weight of the prepreg or core layer 810 may be greater or less than the weight of the prepreg or core layer 815. The layers 810, 815 may independently include any of those components described in connection with the prepreg or core layer 110. For example, one or both of the layers 810, 815 may be configured as a "heavy" prepreg or core layer having an areal weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm. In some cases, each of the prepreg or core layers 810, 615 may include one or more thermoplastic materials, flame retardant materials, and reinforcing fibers randomly arranged in the prepreg or core layer 810, 815. The thermoplastic materials, reinforcing fibers, and flame retardants need not be the same in the different prepreg or core layers 810, 815. If desired, the sum of the weights of the two layers 810, 815 may be at least 2500 gsm, with each layer contributing some weight to the total weight, but the layers 810, 815 need not be the same weight. Open cell skin 820 can be any of those open cell skins described in connection with open cell skin 120, e.g., open cell film, open cell scrim, open cell flim, etc. Although not shown, one or more surface layers can be bonded to core layer 810, core layer 815, or both, as desired.

[0064] In certain examples, an open cell skin may be bonded to multiple prepreg or core layers that are bonded to another open cell film. For example, referring to FIG. 9, a composite article 900 includes a first core layer 910 and a second core layer 915 separated by an open cell skin 920. The core layer 915 includes a second open cell skin 925 disposed on a surface thereof. In some cases, the layers 910, 915 may generally include the same material but have different areal weights. For example, the weight of the prepreg or core layer 910 may be greater or less than the weight of the prepreg or core layer 915. The layers 910, 915 may independently include any of those components described in connection with the prepreg or core layer 110. For example, one or both of the layers 910, 915 may be configured as a "heavy" prepreg or core layer having an areal weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm. In some examples, the prepreg or core layer 910, 915 may include one or more thermoplastic materials, flame retardant materials, and reinforcing fibers randomly arranged in each of the prepreg or core layers 910, 915. The thermoplastic materials, reinforcing fibers, and flame retardants need not be the same in each of the layers 910, 915. If desired, the sum of the weights of the two layers 910, 915 may be at least 2500 gsm, with each layer contributing some weight to the total weight, but the layers 910, 915 need not be the same weight. Each of the open cell skins 920, 925 can independently be any of those open cell skins described in connection with the open cell skin 120, e.g., open cell film, open cell scrim, open cell flim, etc. Each of the open cell skins 920, 925 can also be the same or different. In some examples, the open surface area of ​​the skin 925 can be greater than the open surface area of ​​the skin 920, allowing sound waves to penetrate the article 900. Additionally, the thicknesses of the skins 920, 925 can be the same or different.In some cases, skins 920, 925 may be produced from the same epidermis, but skin 925 may have an increased number of perforations or pores as compared to the numerous perforations or pores present in skin 920. Although not shown, one or more surface layers may be bonded to skin 925, core layer 910, or both, as desired.

[0065] In some configurations, an open cell skin may be bonded to multiple prepreg or core layers that are bonded to another open cell film and a closed cell film. For example, referring to FIG. 10, a composite article 1000 includes a first core layer 1010 and a second core layer 1015 separated by an open cell skin 1020. A closed cell skin 1030 is bonded to an opposing surface of the core layer 1010. In some cases, the layers 1010, 1015 may generally include the same material but include different areal weights. For example, the weight of the prepreg or core layer 1010 may be greater or less than the weight of the prepreg or core layer 1015. The layers 1010, 1015 may independently include any of those components described in connection with the prepreg or core layer 110. For example, one or both of the layers 1010, 1015 may be configured as a "heavy" prepreg or core layer having an areal weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm. In some cases, the prepreg or core layer 1010 may include one or more thermoplastic materials, flame retardant materials, and reinforcing fibers randomly arranged in the prepreg or core layer 1010. The thermoplastic materials, reinforcing fibers, and flame retardants in the layers 1010, 1015 do not have to be the same. If desired, the sum of the weights of the two layers 1010, 1015 may be at least 2500 gsm, with each layer contributing some weight to the total weight, but the layers 1010, 1015 do not have to be the same weight. The open cell skin 1020 can be any of those open cell skins described in connection with the open cell skin 120, e.g., open cell film, open cell scrim, open cell flim, etc. The closed cell skin 1030 can be any of those closed cell skins described in connection with the closed cell film 530, e.g., closed cell film, closed cell scrim, closed cell flim, etc. Although not shown, one or more surface layers can be bonded to the core layer 1015, the closed cell skin 1030, or both, as desired.

[0066] Additional layers such as decorative layers, textured layers, colored layers, etc. may also be present in the composite articles described herein. For example, the decorative layer may be formed from a thermoplastic film, such as, for example, polyvinyl chloride, polyolefin, thermoplastic polyester, thermoplastic elastomer, etc. The decorative layer may also be a multi-layer structure including a foam core formed from, for example, polypropylene, polyethylene, polyvinyl chloride, polyurethane, etc. Fabrics may be adhered to the foam core, such as natural and synthetic fibers, organic fiber nonwovens after needle punching or the like, brushed fabrics, knit goods, flock fabrics, or woven fabrics made from other such materials. Fabrics may also be bonded to the foam core with thermoplastic adhesives, including pressure sensitive adhesives and hot melt adhesives such as polyamides, modified polyolefins, urethanes, and polyolefins. The decorative layer may also be produced using spunbond, heat bond, spunlace, melt blown, wet laid processes, and / or dry laid processes. Insulation layers may also be bonded to one or more surfaces of the articles described herein, and the insulation layers may be open or closed, as appropriate, e.g., open-cell or closed-cell foam.

[0067] In certain embodiments, any one or more of the articles described herein, such as those described in connection with Figures 1-10, may be configured as ceiling tiles that absorb sound and provide flame retardancy. Referring to Figure 11, a grid of ceiling tiles 1100 is shown that includes a support structure 1102, 1103, 1104, and 1105 with a plurality of ceiling tiles, such as tiles 1110, arranged in the grid formed by the support structure. As referred to herein, the open cell skin of the ceiling tile is typically oriented toward the noise source to allow for noise absorption. In some cases, for example, when it is desired to reduce noise from a room, the open cell skin of the ceiling tile faces the interior of the room, while in other cases, for example, when it is desired to reduce noise from a ceiling mounted and suspended HVAC device, the open cell skin of the ceiling tile faces away from the interior of the room.

[0068] In some embodiments, the ceiling tile includes a porous core layer including an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and an area weight or basis weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm, and an open-celled skin disposed on a first surface of the porous core layer, the ceiling tile includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17, and the ceiling tile includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009. For example, the open-celled skin includes an open surface area of ​​at least 10%. Optionally, the ceiling tile includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some examples, the ceiling tile may include an open cell skin, such as a porous decorative layer disposed on a fabric, cloth, or other layer. In certain cases, the flame retardant in the ceiling tile includes expandable graphite particles, or magnesium hydroxide, or both. In some examples, the open cell skin includes a perforated film having an open surface area of ​​at least 10%, and the ceiling tile panel includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In certain cases, the ceiling tile may also include a closed cell skin disposed on a second surface of the porous core layer. In further examples, the flame retardant may be homogenously dispersed in the porous core layer. In some examples, the thermoplastic material includes a polyolefin resin. In certain embodiments, the plurality of reinforcing fibers includes glass fibers, or mineral fibers, or both. In some cases, the porous core layer of the ceiling tile further includes clay.

[0069] In certain embodiments, any one or more of the articles described herein, such as those described in connection with FIGS. 1-10, may be configured as a cubicle panel that absorbs sound and provides flame retardancy. Referring to FIG. 12, a top view of a cubicle 1200 is shown, including side panels 1210, 1230, and a center panel 1230. Any one or more of the panels 1210-1230 may include one of the LWRT articles described herein. As referred to herein, the open cell skin of the cubicle panel is typically oriented toward the noise source to allow for noise absorption. In some cases, e.g., when it is desired to reduce noise from within the cubicle, the open cell skin of the cubicle panel faces the interior of the cubicle space, while in other cases, e.g., when it is desired to reduce noise from outside the cubicle, the open cell skin of the cubicle panel faces away from the interior of the cubicle space. If desired, two or more cubicle panels may be sandwiched together with one open cell skin facing the interior of the cubicle space and the other open cell skin facing outward from the interior of the cubicle space.

[0070] In some examples, a cubicle wall panel is sized and arranged to be bonded to another cubicle wall panel, the porous core layer comprising an open cell structured web comprising a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer comprising a flame retardant and an area weight or basis weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm, and an open cell skin disposed on a first surface of the porous core layer, the cubicle wall panel comprising a noise reduction factor of at least 0.5 when tested by ASTM C423-17, the cubicle wall panel comprising a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009. In some cases, the open cell skin comprises at least 10% open surface area. The cubicle wall panel may include a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other cases, the cubicle wall panel includes a porous decorative layer disposed on an open cell skin. In further examples, the flame retardant in the cubicle wall panel includes expandable graphite particles, or magnesium hydroxide, or both. In some configurations, the open cell skin includes a perforated film having an open surface area of ​​at least 10%, and the cubicle wall panel includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other cases, the cubicle wall panel includes a closed cell skin disposed on a second surface of the porous core layer. In some examples, the flame retardant is homogeneously dispersed in the porous core layer. In other examples, the thermoplastic material includes a polyolefin resin. In certain embodiments, the plurality of reinforcing fibers includes glass fibers, or mineral fibers, or both. In some cases, in some examples, the porous core layer of the cubicle wall panel further includes clay.

[0071] In certain embodiments, any one or more of the articles described herein, such as those described in connection with FIGS. 1-10, may be configured as a structural panel that absorbs sound and provides fire retardancy. The structural panel may be used, for example, as subflooring, wall covering, roof covering, as structural support for cabinets, countertops, etc., as stair treads, as a replacement for plywood and other applications. If desired, the structural panel may be bonded to another substrate, such as, for example, plywood, oriented strand board, or other architectural panels commonly used in residential and commercial environments. Referring to FIG. 13A, a top view of a structural panel 1310 is shown. The panel 1310 may include any one of the LWRT articles described herein. As referred to herein, the open cell skin of the structural panel is typically oriented toward the noise source to allow for noise absorption. In some cases, e.g., when reducing noise from within a room, the open cell skin of the structural panel faces the interior of the room, while in other cases, e.g., when reducing noise from outside the room, the open cell skin of the structural panel faces away from the interior of the room. If desired, two or more structural panels can be sandwiched with one open cell skin facing the interior of the room and the open cell skin of the other structural panel facing away from the interior of the room.

[0072] In some cases, the structural panel may also include a structural substrate 1320. For example, the structural panel may include a porous core layer including an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and an areal weight or basis weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm, an open cell skin bonded onto a first surface of the porous core layer, and a structural substrate 1320 bonded onto a second surface of the porous core layer, the structural panel including a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the structural panel provides a noise reduction factor of at least 0.85 when tested by ASTM C423-17. The exact nature of the structural substrate 1320 may vary and may include, but is not limited to, plywood, gypsum board, wood planks, wood tiles, cement board, oriented strand board, polymer or vinyl or plastic panels, and the like. In some examples, the structural substrate includes plywood panels, gypsum board, wood tiles, ceramic tiles, metal tiles, wood panels, concrete panels, concrete boards, or bricks. In other examples, the open cell skin includes an open surface area of ​​at least 10%. Optionally, the structural panel may include a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some cases, the structural panel may include a porous decorative layer disposed on the open cell skin. In other examples, the flame retardant includes expandable graphite particles, or magnesium hydroxide, or both. In some examples, the open cell skin includes a perforated film having an open surface area of ​​at least 10% and the structural panel includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some embodiments, the structural panel includes a closed cell skin disposed on the second surface of the porous core layer. In other embodiments, the flame retardant is homogeneously dispersed in the porous core layer.In some embodiments, the thermoplastic material comprises a polyolefin resin and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.Optionally, the structural panel may further comprise a second structural panel bonded to the open cell skin, the second structural panel being a porous structural panel.

[0073] In certain cases, any one or more of the articles described herein, such as those described in connection with FIGS. 1-10, may be configured as a wallboard or wall panel that absorbs sound and provides fire retardancy. The wall panel may be used, for example, to cover studs or structural members of a building, to cover ceiling joists or trusses, etc. If desired, the wall panel may be bonded to another substrate, such as, for example, tile, wood panel, gypsum, concrete backing board, or other wall panel substrates commonly used in residential and commercial environments. Referring to FIG. 14, a side view of a wall panel 1400 is shown. The panel 1400 may include any one of the LWRT articles described herein. As referred to herein, the open cell skin of the wall panel is typically oriented toward the noise source to enable noise absorption. In some cases, e.g., when reducing noise from within a room, the open cell skin of the wall panel faces the interior of the room, while in other cases, e.g., when reducing noise from outside the room, the open cell skin of the wall panel faces away from the interior of the room. If desired, two or more wall panels may be sandwiched together with one open cell skin facing the interior of the room and the other wall panel's open cell skin facing away from the interior of the room.

[0074] In some cases, the wall panel 1400 includes a porous core layer 1410 including an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a fire retardant and an areal weight or basis weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm. The wall panel 1400 may also include an open cell skin 1420 bonded to a first surface of the porous core layer 1410. As mentioned herein, any wall substrate may be bonded to the second surface of the porous core layer 1410 and configured to support the porous core layer 1410 when the wall panel 1400 is bonded to a wall surface, the wall panel including a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the wall panel 1400 including a sound absorption coefficient of at least 0.5 when tested by ASTM C423-17.

[0075] In some embodiments, the wall substrate does not include cellulose. In other embodiments, the open cell skin 1420 includes an open surface area of ​​at least 10% and the wall panel 1400 includes a noise reduction coefficient of at least 0.85 when tested by ASTM C423-17. In certain configurations, the wall panel 1400 further includes a porous decorative layer disposed on the open cell skin 1420. In other embodiments, the flame retardant includes expandable graphite particles, or magnesium hydroxide, or both.

[0076] In certain examples, the open cell skin 1420 comprises a perforated film having an open surface area of ​​at least 10%, and the wall panel comprises a noise reduction factor of at least 0.5 when tested by ASTM C423-17. In some embodiments, the wall panel may comprise a closed cell skin disposed on the second surface of the porous core layer. In other cases, the flame retardant is homogeneously dispersed in the porous core layer. In some examples, the thermoplastic material comprises a polyolefin resin, and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both. In certain embodiments, a second wall panel may be bonded to the open cell skin 1420, and the second wall panel is a porous wall panel.

[0077] In certain cases, any one or more of the articles described herein, such as those described in connection with FIGS. 1-10, may be configured as siding attached to a building, such as a residential or commercial building, that absorbs sound and provides fire retardancy. The siding may be used, for example, to cover house wrap, cladding, or other materials commonly used on the exterior surface of the building. If desired, the siding may be bonded to another substrate, such as, for example, vinyl, concrete board, wood siding, brick, or other substrates commonly placed on the exterior of a building. Referring to FIG. 15, a side view of a siding panel 1500 is shown. The panel 1500 may include any one of the LWRT articles described herein. As referred to herein, the open cell skin of the siding is typically oriented toward the noise source to allow for noise absorption. In some cases, e.g., when reducing noise from within the building, the open cell skin of the siding faces the interior of the building, while in other cases, e.g., when reducing noise from the exterior of the building, the open cell skin of the siding faces away from the interior of the building. If desired, two or more siding panels may be sandwiched together with one open cell skin facing the interior of the building and the other open cell skin of the wall panel facing away from the interior of the building.

[0078] In some examples, the siding can be comprised of a flame retardant noise reduction layer that can be bonded to a substrate 1530. For example, the flame retardant noise reduction layer can include a porous core layer 1510 including an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and an areal weight or basis weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm, and an open cell skin 1520 bonded onto a first surface of the porous core layer, the flame retardant layer including a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the flame retardant layer including a noise reduction factor of at least 0.5 when tested by ASTM C423-17. The substrate 1530 may be constructed of many different materials including, but not limited to, vinyl, wood, brick, concrete, etc. For example, a vinyl substrate may be bonded to a first surface of a flame retardant noise reducing layer and the siding may be configured to bond to a non-horizontal surface of a building to hold the siding panel to the non-horizontal surface of the building.

[0079] In some cases, the siding panel further includes a weather barrier, e.g., house wrap, membrane, etc., bonded to the second surface of the flame retardant noise reducing layer. In some embodiments, the substrate includes a nailing flange that allows for bonding of the siding to the side of a building.

[0080] In certain embodiments, the open cell skin of the siding panel comprises at least 10% open surface area and the siding comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17.. In other embodiments, the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both.

[0081] In some cases, the open cell skin of the siding panel comprises a perforated film having an open surface area of ​​at least 10%, and the siding panel comprises a sound reduction factor of at least 0.85 when tested by ASTM C423-17. In other examples, the siding panel further comprises a closed cell skin disposed on a second surface of the porous core layer. In some examples, the flame retardant is homogenously dispersed in the porous core layer. In other examples, the thermoplastic material comprises a polyolefin resin, and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both. In some examples, the siding panel may further comprise a second siding panel comprising a second flame retardant sound reduction layer bonded to a second substrate, the flame retardant sound reduction layer being configured to interlock with the second flame retardant sound reduction layer when the substrate is bonded to the second vinyl substrate, and where the two siding panels may interlock horizontally with one another, there may be, for example, a butt joint, a lap joint, or the like.

[0082] In certain cases, any one or more of the articles described herein, such as those described in connection with FIGS. 1-10, may be configured as a roof panel attached to a building, such as a residential or commercial building, that absorbs sound and provides fire retardancy. The roof panel may be used, for example, to cover an attic, to attach to a roof truss, or to cover a flat roof commonly present on commercial buildings. If desired, the roof panel may be bonded to another substrate, such as, for example, oriented strand board, plywood, or solar panels, that are attached to the roof and function to cover the roof. Referring to FIG. 16, a perspective view of a roof panel 1610 attached to a house 1600 is shown. The roof panel 1610 may include any one of the LWRT articles described herein. As referred to herein, the open cell skin of the roof panel is typically oriented toward the noise source to allow for noise absorption. In some cases, e.g., when reducing noise from within the attic, the open cell skin of the roof panel faces the attic interior, while in other cases, e.g., when reducing noise from outside the building, the open cell skin of the roof panel faces away from the attic interior. If desired, two or more roof panels can be sandwiched with one open cell skin facing the building interior and the other open cell skin facing away from the building interior.

[0083] In some embodiments, the roof panel includes a flame retardant noise reduction layer bonded to the roof substrate. In certain embodiments, the flame retardant noise reduction layer includes a porous core layer including an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and an areal weight or basis weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm, and an open cell skin bonded to a first surface of the porous core layer, the flame retardant noise reduction layer includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the flame retardant noise reduction layer includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17. The roof panel may also include a roof substrate bonded to the first surface of the flame retardant noise reduction layer and configured to bond to the roof of the building to retain the roof panel thereon.

[0084] In some examples, the roof panel may include a weather barrier bonded to the second surface of the flame retardant noise reduction layer, such as, for example, a membrane, house wrap, tar paper, plastic film, etc. In other cases, the roof substrate includes a cellulosic material. In some examples, the open cell skin includes at least 10% open surface area, and the roof panel includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other examples, the flame retardant includes expandable graphite particles, or magnesium hydroxide, or both. In some examples, the open cell skin includes a perforated film having at least 10% open surface area, and the roof panel includes a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other examples, the roof panel includes a closed cell skin disposed on the second surface of the porous core layer. In some cases, the flame retardant is homogeneously dispersed in the porous core layer. In other examples, the thermoplastic material includes a polyolefin resin, and the plurality of reinforcing fibers includes glass fibers, or mineral fibers, or both. In certain cases, the roof panel includes a second roof panel including a second flame-retardant noise-reducing layer bonded to a second roof substrate, and the flame-retardant noise-reducing layer is configured to engage with the second flame-retardant noise-reducing layer when the roof substrate is positioned to overlap the second roof substrate.

[0085] In certain configurations, any one or more of the articles described herein, such as those described in connection with FIGS. 1-10, may be configured as a roof shingle attached to a building, such as a residential or commercial building, that absorbs sound and provides fire retardancy. The roof shingle may be used, for example, to cover roofs commonly present on residential and commercial buildings. If desired, the roof shingle may be bonded to another substrate, such as, for example, asphalt, ceramic, clay tile, aluminum, copper, wood such as cedar, and other materials commonly found or used as roof shingles. Referring to FIG. 17, an exploded view of a roof shingle 1700 is shown. The roof panel 1700 may include any one of the LWRT articles described herein. As referred to herein, the open cell skin of the roof shingle is typically oriented toward the noise source to allow for noise absorption. In some cases, e.g., to reduce noise from within the attic, the open cell skin of the shingle faces the attic interior, while in other cases, e.g., to reduce noise from outside the building, the open cell skin of the shingle faces away from the attic interior. If desired, two or more shingles can be sandwiched with one open cell skin facing the building interior and the open cell skin of the other roof panel facing away from the building interior.

[0086] In certain examples, the roof panel 1700 includes a fire retardant noise reduction layer, the fire retardant noise reduction layer includes a porous core layer 1710 including an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a fire retardant agent and an areal weight or basis weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm, and an open cell skin 1720 bonded onto a first surface of the porous core layer, the fire retardant noise reduction layer includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the fire retardant noise reduction layer includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17. The weatherable shingle substrate 1730 may be bonded to a first surface of the flame retardant noise reducing layer and may be configured to be bonded to a roof panel of a building to provide a weather resistant, flame retardant, noise reducing shingle on the roof panel.

[0087] In certain cases, a weather barrier is bonded to the second surface of the flame retardant noise reduction layer. In other examples, the shingle comprises asphalt. In some examples, the open cell skin comprises at least 10% open surface area, and the shingle comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In certain examples, the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both. In other examples, the open cell skin comprises a perforated film having at least 10% open surface area, and the shingle comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some cases, the shingle comprises a closed cell skin disposed on the second surface of the porous core layer. In other examples, the flame retardant is homogeneously dispersed in the porous core layer. In certain embodiments, the thermoplastic material comprises a polyolefin resin, and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both. In some embodiments, the shingle includes a second shingle including a second flame-retardant noise-reducing layer bonded to the second weather-resistant shingle, and the flame-retardant noise-reducing layer is configured to engage with the second flame-retardant noise-reducing layer when the weather-resistant shingle is positioned to overlap the second weather-resistant shingle.

[0088] In certain configurations, any one or more of the articles described herein, such as those described in connection with FIGS. 1-10, may be configured as interior panels or walls of a recreational vehicle (RV) that absorb sound and provide flame retardancy. The panels or walls may be used, for example, to cover a skeleton structure on the interior side of the recreational vehicle and may be bonded to foam or other insulating material between the interior and exterior of the recreational vehicle. If desired, the RV interior panels may be bonded to another substrate, such as, for example, fabric, plastic, tile, etc. Referring to FIG. 18, a side view of a recreational vehicle 1800 is shown. The interior panel 1800 may include any one of the LWRT articles described herein. As referred to herein, the open cell skin of the interior panel is typically oriented toward the noise source to allow for noise absorption. In some cases, e.g., when reducing noise from inside the RV, the open cell skin of the interior panel faces the interior of the RV 1800, while in other cases, e.g., when reducing noise from outside the RV 1800, the open cell skin of the RV panel faces away from the interior of the RV 1800. If desired, two or more RV panels can be sandwiched with one open cell skin facing the interior of the RV and the open cell skin of the other RV panel facing outward from the interior of the RV.

[0089] In certain examples, the RV interior panel includes a flame retardant sound reduction layer, the flame retardant sound reduction layer includes a porous core layer including an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and an areal weight or basis weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm, and an open cell skin bonded onto a first surface of the porous core layer. In other cases, the RV interior panel includes an interior wall substrate bonded onto a second surface of the porous core layer, the recreational vehicle interior panel includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the recreational interior vehicle panel includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17. In some examples, the interior wall substrate is configured as a decorative layer, such as fabric, plastic, tile, wood, and the like. In some cases, the open cell skin comprises at least 10% open surface area, and the recreational vehicle interior panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other cases, the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both. In some examples, the open cell skin comprises a perforated film having at least 10% open surface area, and the recreational vehicle interior panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other examples, the RV interior panel comprises a closed cell skin disposed on the second surface of the porous core layer. In certain examples, the flame retardant is homogeneously dispersed in the porous core layer. In some embodiments, the thermoplastic material comprises a polyolefin resin, and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.In additional cases, the RV panel includes a second RV interior panel including a second flame retardant noise reducing layer bonded to a second interior wall substrate, the flame retardant noise reducing layer configured to lock onto the second flame retardant noise reducing layer when the interior wall substrate is positioned to vertically overlap the second interior wall substrate on a first side of the RV interior panel. Optionally, the RV panel can include a third RV interior panel including a third flame retardant noise reducing layer bonded to a third interior wall substrate, the flame retardant noise reducing layer configured to lock onto the third flame retardant noise reducing layer when the interior wall substrate is positioned to vertically overlap the third interior wall substrate on a second side of the recreational vehicle interior panel.

[0090] In certain configurations, any one or more of the articles described herein, such as those described in connection with FIGS. 1-10, may be configured as an exterior panel or wall of a recreational vehicle (RV) that absorbs sound and provides flame retardancy. The panel or wall may be used, for example, to cover a skeleton structure on the exterior side of the recreational vehicle and may be bonded to foam or other insulating material between the interior and exterior of the recreational vehicle. If desired, the RV exterior panel may be bonded to another substrate, such as, for example, metal, fiberglass, etc. Referring to FIG. 19, a side view of a recreational vehicle 1900 including an exterior panel 1910 is shown, which may be configured as any one of the LWRT articles described herein. As referred to herein, the open cell skin of the exterior panel is typically oriented toward the noise source to enable noise absorption. In some cases, e.g., when reducing noise from inside the RV, the open cell skin of the exterior panel faces the interior of the RV 1900, while in other cases, e.g., when reducing noise from outside the RV 1900, the open cell skin of the RV panel faces away from the interior of the RV 1900. If desired, two or more RV panels can be sandwiched with one open cell skin facing the interior of the RV and the open cell skin of the other RV panel facing outward from the interior of the RV.

[0091] In some examples, the RV exterior panel includes a flame retardant sound reduction layer, the flame retardant sound reduction layer includes a porous core layer including an open cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and an area weight or basis weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm, and an open cell skin bonded on a first surface of the porous core layer. The RV exterior panel may also include a weather resistant exterior wall substrate bonded to a second surface of the porous core layer, the recreational vehicle exterior panel includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009, and the recreational exterior vehicle panel includes a sound reduction factor of at least 0.5 when tested by ASTM C423-17.

[0092] In certain configurations, the exterior wall substrate comprises fiberglass or is configured as a metal panel. In some embodiments, the open cell skin comprises a perforated film having at least 10% open surface area, and the recreational vehicle exterior panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In other embodiments, the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both. In certain embodiments, the open cell skin comprises a perforated film having at least 10% open surface area, and the recreational vehicle exterior panel comprises a noise reduction factor of at least 0.85 when tested by ASTM C423-17. In some embodiments, the RV exterior panel comprises a closed cell skin disposed on the second surface of the porous core layer. In certain cases, the flame retardant is homogeneously dispersed in the porous core layer. In some embodiments, the thermoplastic material comprises a polyolefin resin, and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both. In another embodiment, the RV panel includes a second RV exterior panel including a flame retardant noise reducing layer coupled to a second exterior wall substrate, the flame retardant noise reducing layer configured to lock onto the second flame retardant noise reducing layer when the exterior wall substrate is positioned to overlap the second exterior wall substrate on a first side of the recreational vehicle exterior panel. In an additional embodiment, the RV exterior panel includes a third recreational vehicle exterior panel including a third flame retardant noise reducing layer coupled to a third exterior wall substrate, the flame retardant noise reducing layer configured to lock onto the third flame retardant noise reducing layer when the exterior wall substrate is positioned to overlap the third exterior wall substrate on a second side of the recreational vehicle exterior panel.

[0093] In certain configurations, any one or more of the articles described herein, such as those described in connection with Figures 1-10, can be configured as interior panels that absorb sound and provide fire retardancy. For example, interior architectural panels that include two-dimensional or three-dimensional features can be produced. The interior building panel includes a porous core layer comprising an open cell structured web comprising a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer comprising a flame retardant and an areal weight or basis weight of at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm, and an open cell skin disposed on a first surface of the porous core layer, the interior building panel includes two or three dimensional features including a noise reduction factor of at least 0.5 when tested by ASTM C423-17, and the interior building panel includes two or three dimensional features including a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009. Referring to this specification and referring to Figure 20, there is shown an interior panel 2000 that includes two-dimensional features including indentations 2010 and raised surfaces 2020. The ability of the panel to provide complex shapes and surfaces is a substantial attribute. Such shapes and multi-dimensional features can be molded into desired shapes and used for interior applications including decorative wall panels.

[0094] In some embodiments, the same configuration can be used for interior trim applications. For example, an interior trim including a flame retardant noise reduction layer and an interior trim substrate can be used. The flame retardant noise reduction layer can include a porous core layer including an open-cell structured web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and an area weight or basis weight of at least 2000gsm, or at least 2100gsm, or at least 2200gsm, or at least 2300gsm, or at least 2400gsm, or at least 2500gsm, and an open-cell skin disposed on a first surface of the porous core layer, the flame retardant noise reduction layer includes a noise reduction factor of at least 0.5 when tested by ASTM C423-17, and the flame retardant noise reduction layer includes a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009. The interior trim substrate may be bonded to the first surface of the flame retardant noise reducing layer and may include wood, PVC, vinyl, plastic, leather, or other materials. A side view of a trim piece that may be used as a baseboard trim is shown in FIG. 21. The trim piece 2100 includes a trim substrate 2120 bonded to a flame retardant noise reducing layer 2110. The trim piece 2100 may be nailed or otherwise attached to a stud or wallboard as desired. The substrate 2120 faces outward and is visible within the room. The trim piece 2100 may be curved or take on a two- or three-dimensional shape as desired.

[0095] In certain examples, the prepreg or core of the articles described herein may be prepared using woven or nonwoven fabrics generally made of chopped glass fibers, thermoplastic materials, flame retardant materials, open cell films, and / or glass fibers, or thermoplastic fibers such as, for example, polypropylene (PP), polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polycarbonate (PC), blends of PC / PBT, or blends of PC / PET. In some embodiments, PP, PBT, PET, PC / PET blends, or PC / PBT blends may be used as the thermoplastic materials. To produce the prepreg or core, the thermoplastic materials, reinforcing materials, flame retardant material(s), and / or other additives may be added or metered into a dispersed foam contained in an open-top mixing tank equipped with an impeller. Without wishing to be bound by any particular theory, the presence of air pockets trapped in the foam may aid in the dispersion of the glass fibers, thermoplastic materials, and flame retardant materials. In some examples, the dispersed mixture of glass and resin may be pumped through a dispersion manifold to a headbox located above the wire section of the paper machine. The dispersed mixture may then be fed to a moving wire screen using a vacuum to continuously produce a uniform fibrous wet web, and then the foam, but not the glass fiber, the flame retardant material, or the thermoplastic, may be removed. The wet web may be passed through a dryer at a suitable temperature to reduce the moisture content and melt or soften the thermoplastic material. As the hot web exits the dryer, a surface layer, such as, for example, an open-cell film, may be laminated onto the web by passing the web of glass fiber, the flame retardant material, the thermoplastic material, and the open-cell film through the nip of a set of heated rollers. Optionally, additional layers, such as, for example, closed-cell film, nonwoven and / or woven layers, surface layers, may also be attached to one or both sides of the web along with the open-cell film to facilitate handling of the resulting composite. The composite may then be passed through tension rolls and subsequently cut (cut) to the desired size for later formation into the final product article.Further information regarding the preparation of such complexes, including suitable materials and processing conditions used to form such complexes, is described, for example, in U.S. Pat. Nos. 6,923,494, 4,978,489, 4,944,843, 4,964,935, 4,734,321, 5,053,449, 4,925,615, 5,609,966, and U.S. Patent Application Publication Nos. US2005 / 0082881, US2005 / 0228108, US2005 / 0217932, US2005 / 0215698, US2005 / 0164023, and US2005 / 0161865.

[0096] In certain cases, a method of producing a composite article includes combining a thermoplastic material, a reinforcing fiber, and a flame retardant material in a mixture to form an agitated aqueous foam. The foam is placed on a wire support and the water is drained to form a web or open-cell structure including the thermoplastic material, the fiber, and the flame retardant material. In some cases, the web is then heated to a first temperature that exceeds the melting temperature of the thermoplastic material. In some cases, pressure may then be applied to the web, for example using a nip roller or other device, to provide a thermoplastic composite sheet including the flame retardant material dispersed in the web. An open-cell film may then be placed over the formed prepreg or core, optionally with heating, to bond the open-cell film to the prepreg or core.

[0097] In certain cases, a method of producing a composite article includes combining a mixture of a thermoplastic material, a reinforcing fiber, and one or more of (1) an EG material, (2) a Group II or Group III metal hydroxide (such as MDH or ATH) in a mixture to form an agitated aqueous foam. The foam is placed on a wire support and the water is drained to form a web or open-cell structure including the thermoplastic material, the fiber, and the EG material / Group II or Group III metal hydroxide material. In some cases, the web is then heated to a first temperature above the melting temperature of the thermoplastic material. Optionally, the core may be compressed before fully forming. In some cases, pressure may then be applied to the web, for example using a nip roller or other device, to provide a thermoplastic composite sheet including a flame-retardant material from the EG material / Group II or Group III metal hydroxide material dispersed in the web. An open-cell film may then be placed over the formed prepreg or core, optionally with heating, to bond the open-cell film to the prepreg or core.

[0098] In some embodiments, a composite article includes a thermoplastic fiber reinforced porous core layer and an open cell film disposed on at least one surface of the porous core layer, the porous core layer including a web formed from a plurality of reinforcing fibers, a flame retardant material, and a thermoplastic material, the composite article including an amount of the flame retardant material effective to meet Class A requirements when tested by ASTM E84, 2009, and provide a Noise Reduction Coefficient (NRC) of at least 0.50 when tested by ASTM C423-17. More specifically, the NRC can be at least 0.50 when tested by ASTM C423-17.

[0099] The composite article may be used in a variety of settings, including, but not limited to, office furniture, seating, and the like. In some cases, the thermoplastic material includes a polyolefin, the reinforcing fibers include glass fibers, and the flame retardant material includes a Group II metal hydroxide or an EG material or both. In other examples, the glass fibers are present at about 30 to 60 weight percent, the flame retardant material is present at about 30 to about 50 weight percent, and the remainder of the core layer includes a thermoplastic material. The areal weight of the core is desirably at least 2000 gsm, or at least 2100 gsm, or at least 2200 gsm, or at least 2300 gsm, or at least 2400 gsm, or at least 2500 gsm or more to enhance sound absorption. In some cases, an adhesive layer may be present between the core layer and the open cell film. In certain embodiments, the article may include a second skin layer disposed on an opposite surface of the core layer.

[0100] To further demonstrate some of the novel and useful aspects of the technology described herein, certain specific examples are described.

[0101] Example 1 The LWRT sheets were produced using a wet-laid process. They were polyolefin-based, e.g., polypropylene-based, and reinforced using chopped glass fibers. Polypropylene resin and glass fibers were mixed in water and stirred into a uniform suspension. The suspension was deposited onto a forming wire and the water was removed to form a web comprising polypropylene resin and glass fibers. Further processing by heat melting the resin forms a solid composite core after the web is cooled under pressure to a temperature below the melting point of the resin.

[0102] Example 2 LWRT sheets were formed similarly to those produced in Example 1, except that a flame retardant was added to the resin and chopped glass fiber mixture. Two different flame retardant materials were used, including expandable graphite (EG) and magnesium hydroxide (MDH). Both grades meet Class A requirements when tested by the ASTM E84 method, and one grade meets SE-0 requirements when tested by the SAE J369 method.

[0103] Example 3 Various materials were added to the core formed from Example 2 after the web was formed and before the final core was formed. The materials were applied to both sides of the web. Tables 1 and 2 list the various materials and additives present in certain tested LWRT articles. [Table 1] [Table 2]

[0104] Lofting is a property of the LWRT core that allows for the thermoformability of the LWRT material. When the LWRT sheet is heated to a temperature above the melting point of the resin, the glass fibers in the LWRT sheet can return to a freestanding state, resulting in an increase in the thickness of the composite sheet. The lofted LWRT can be further molded to the desired thickness for the end use application. The LWRT material was tested both with and without the thermoforming process. Taking a flat 1200gsm panel as an example, the LWRT material could be heated in an oven set at 204°C for 4 minutes and then compressed to the desired thickness by cold pressing.

[0105] Example 4 Physical properties including areal density, ash content, thickness at production and lofting thickness were measured using disks with a diameter of 99 mm. Two test standards were followed to test the acoustic performance. Both groups of materials were evaluated according to ASTM E1050, and the materials in Group A of Table 1 were also tested according to ASTM C423-17 method for potential use in building and construction applications. Flammability tests were performed according to SAE J369 and ASTM E84 methods. SAE J369 is more common in automotive applications, while the performance tested by ASTM E84 method provides a deeper insight into the performance expected by the office furniture and building and construction industries. In addition, the flexural strength of the materials was also tested according to ASTM D790 or ISO 178 methods.

[0106] Table 3 lists the measured physical properties of the various tested materials. [Table 3]

[0107] The acoustic properties of the Control A material were measured using ASTM E1050. Figure 22 is a graph showing the sound absorption results. The acoustic properties of Sample A1 and Sample A2 were also measured. Figure 23 is a graph showing the results. The materials were tested both with and without the thermoforming process. Without any surface lamination or only a lightweight scrim, the absorption coefficient shows no dependence on the thermoforming process for the standard LWRT or MDH formulations. The difference in the material before and after the thermoforming process for Sample A2 is consistent with the small surface open area changes during the thermoforming process. In general, the sound absorption performance is more determined by a combination of the material thickness, areal density, and the open structure of the surface material.

[0108] Control B and Sample B3 were also considered for use in automotive applications where more complex part geometries are typically required, necessitating a thermoforming process. The sound absorption performance of Control B and Sample B3 was tested without thermoforming and with thermoforming at 4mm and 6mm, as shown in Figures 24 and 25. Unlike the standard LWRT and MDH versions of LWRT, the EG grade LWRT exhibits a different relationship between molding thickness and absorption coefficient. It is generally believed that higher absorption coefficients are achieved when LWRT materials are molded thicker, and that porosity at least partially determines the sound absorption performance of LWRT materials. However, the non-thermoformed EG grade material exhibited a higher sound absorption coefficient than the same material when molded to a thickness of 4mm. This result is believed to be due to the layered structure of EG improving the sound absorption of the material. The thermoforming process may cause a level of EG expansion in the heating process, which causes the material molded at 4mm to exhibit lower acoustic performance than the material having a thickness of about 3.6mm before thermoforming. It should also be noted that significantly higher acoustic performance is achieved at higher frequencies, such as above 4000 Hz.

[0109] Example 5 The Noise Reduction Coefficient (NRC) and Sound Absorption Average (SAA) values ​​of samples A1 and A2 were tested for potential applications in the building and construction industry and are summarized in Table 4. [Table 4]

[0110] In the ASTM C423-17 test, the samples have different surface materials facing the sound source. Sample A1 had a lightweight scrim surface layer that was considered a large open surface laminate. In contrast, the perforated film used in Sample A2 had only about 10% open area. Samples A1 and A2 exhibited the same level of acoustic performance. Therefore, it is believed that a film with about 10% open surface area would be suitable to achieve the same level of acoustic performance as an open structure lightweight scrim.

[0111] Example 6 The flammability performance of samples A1, A2, A3, B1, and B2 were tested using the ASTM E84 test standard. The ASTM E84 standard requires Class A performance to have a Flame Spread Index (FSI) of 25 or less and a Smoke Development Index (SDI) of 450 or less. The materials were tested without a thermoforming process. All the materials tested meet the Class A requirements as shown in Table 5. [Table 5]

[0112] Flammability was more dependent on the substrate formulation, and the surface material only had a minor effect on performance. Between the two formulations, EG was considered the more effective FR additive, while MDH offers more color options if required by the end-use application.

[0113] Example 7 Control B and Sample B3 were also tested to the SAE J369 method after thermoforming so that these materials could be used in automotive applications. Sample B3 demonstrated self-extinguishing capabilities. The molded material exhibits SE-0 level performance as molded and after 10 minutes of immersion in motor oil. Figures 26A (top) and 26B (bottom) show examples of the specimens after flammability testing. The specimens were first immersed in 5W30 engine oil for 10 minutes and then drained vertically for 20 minutes. The specimen was ignited from the end rich in engine oil. It self-extinguished and only minor damage occurred at the ignited end as shown in Figures 26A and 26B.

[0114] Example 8 The flexural strength measurements of Control A and Sample A3 are compared in Figure 27, while Figure 28 compares the flexural strength measurements of Control B, Sample B1, and Sample B2. The materials were tested in both the machine direction (MD) and cross direction (CD). The mechanical strength of the LWRT is more determined by the glass fiber and the resin. Both types of additives are generally considered to reduce the mechanical strength of the composite. Since EG is a more effective FR additive, the flexural strength is less affected with the EG version of the LWRT, which may be a result of the lower loading level of the additive.

[0115] When introducing elements of the embodiments disclosed herein, the articles "a," "an," "the," and "said" are intended to mean that there are one or more elements. The terms "including" and "having" are intended to be open-ended and mean that there may be additional elements other than the listed elements. Those skilled in the art will recognize, given the benefit of this disclosure, that various components of the embodiments may be interchanged or substituted for various components in other embodiments.

[0116] While particular aspects, configurations, examples and embodiments have been described above, those of ordinary skill in the art, given the benefit of this disclosure, will recognize that additions, substitutions, modifications and variations of the disclosed exemplary aspects, configurations, examples and embodiments are possible. Yet another aspect of the present invention may be as follows. [1] A thermoplastic composite article, a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; and an open cell skin disposed on a first surface of the porous core layer, wherein the composite article has a noise reduction factor of at least 0.5 when tested according to ASTM C423-17, and wherein the composite article has a flame spread index of less than 25 and a smoke development index of less than 150 when tested according to ASTM E84, 2009. [2] The thermoplastic composite article according to [1], wherein the flame retardant comprises expandable graphite particles. [3] The thermoplastic composite article according to [2], wherein the open-cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the composite article has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17. [4] The thermoplastic composite article according to [1], wherein the flame retardant comprises magnesium hydroxide. [5] The thermoplastic composite article according to [4], wherein the open-cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the composite article has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17. [6] The thermoplastic composite article according to [3] or [5], wherein the thermoplastic material comprises a polyolefin resin. [7] The thermoplastic composite article according to [6], wherein the plurality of reinforcing fibers comprises glass fibers. [8] The thermoplastic composite article described in [7], further comprising a decorative layer disposed on the second surface of the porous core layer. [9] The thermoplastic composite article according to [7], further comprising a closed cell skin disposed on a second surface of the porous core layer.

[10] The thermoplastic composite article according to [8], further comprising a decorative layer disposed on the closed cell skin.

[11] A ceiling tile comprising: a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; and an open cell skin disposed on the first surface of the porous core layer, wherein the ceiling tile has a noise reduction factor of at least 0.5 when tested in accordance with ASTM C423-17, and wherein the ceiling tile has a flame spread index of less than 25 and a smoke development index of less than 150 when tested in accordance with ASTM E84, 2009.

[12] The ceiling tile of

[11] , wherein the open cell skin has an open surface area of ​​at least 10% and the ceiling tile has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[13] The ceiling tile according to

[12] , further comprising a porous decorative layer disposed on the open-cell skin.

[14] The ceiling tile according to

[13] , wherein the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both.

[15] The ceiling tile of

[14] , wherein the open-cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the ceiling tile panel has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[16] The ceiling tile of

[15] , further comprising a closed cell skin disposed on the second surface of the porous core layer.

[17] The ceiling tile according to

[16] , wherein the flame retardant is homogeneously dispersed in the porous core layer.

[18] The ceiling tile described in

[17] , wherein the thermoplastic material comprises a polyolefin resin.

[19] The ceiling tile of

[18] , wherein the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.

[20] The ceiling tile described in

[18] , wherein the porous core layer further comprises clay.

[21] A cubicle wall panel sized and arranged to be joined to another cubicle wall panel, comprising: a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; and an open cell skin disposed on a first surface of the porous core layer, wherein the cubicle wall panel has a noise reduction factor of at least 0.5 when tested in accordance with ASTM C423-17, and wherein the cubicle wall panel has a flame spread index of less than 25 and a smoke development index of less than 150 when tested in accordance with ASTM E84, 2009.

[22] The cubicle wall panel of

[21] , wherein the open cell skin has an open surface area of ​​at least 10% and the cubicle wall panel has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[23] The cubicle wall panel according to

[22] , further comprising a porous decorative layer disposed on the open-cell skin.

[24] The cubicle wall panel according to

[23] , wherein the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both.

[25] The cubicle wall panel of

[24] , wherein the open cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the cubicle wall panel has a noise reduction coefficient of at least 0.85 when tested by ASTM C423-17.

[26] The cubicle wall panel of

[25] , further comprising a closed cell skin disposed on a second surface of the porous core layer.

[27] The cubicle wall panel according to

[26] , wherein the flame retardant is homogeneously dispersed in the porous core layer.

[28] The cubicle wall panel according to

[27] , wherein the thermoplastic material comprises a polyolefin resin.

[29] The cubicle wall panel of

[28] , wherein the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.

[30] The cubicle wall panel according to

[28] , wherein the porous core layer further comprises clay.

[31] A structural panel comprising: a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; an open cell skin bonded to a first surface of the porous core layer; a structural substrate bonded to a second surface of the porous core layer, wherein the structural panel has a flame spread index of less than 25 and a smoke development index of less than 150 when tested in accordance with ASTM E84, 2009, and provides a noise reduction factor of at least 0.85 when tested in accordance with ASTM C423-17.

[32] The structural panel according to

[31] , wherein the structural substrate comprises a plywood panel, a gypsum board, a wood tile, a ceramic tile, a metal tile, a wood panel, a concrete panel, a concrete board, or a brick.

[33] The structural panel of

[32] , wherein the open cell skin has an open surface area of ​​at least 10% and the structural panel has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[34] The structural panel according to

[33] , further comprising a porous decorative layer disposed on the open-cell skin.

[35] The structural panel according to

[33] , wherein the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both.

[36] The structural panel of

[35] , wherein the open cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the structural panel has a noise reduction coefficient of at least 0.85 when tested by ASTM C423-17.

[37] The structural panel of

[36] , further comprising a closed cell skin disposed on a second surface of the porous core layer.

[38] The structural panel described in

[37] , wherein the flame retardant is homogeneously dispersed in the porous core layer.

[39] The structural panel of

[38] , wherein the thermoplastic material comprises a polyolefin resin and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.

[40] The structural panel of

[39] , further comprising a second structural panel bonded to the open cell skin, the second structural panel being a porous structural panel.

[41] A wall panel comprising: a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; an open cell skin bonded to a first surface of the porous core layer; and a wall substrate bonded to a second surface of the porous core layer and configured to support the porous core layer when the wall panel is bonded to a wall surface, wherein the wall panel has a flame spread index of less than 25 and a smoke development index of less than 150 when tested in accordance with ASTM E84, 2009, and a sound absorption coefficient of at least 0.5 when tested in accordance with ASTM C423-17.

[42] The wall panel according to

[41] , wherein the wall substrate does not contain cellulose.

[43] The wall panel of

[42] , wherein the open cell skin has an open surface area of ​​at least 10% and the wall panel has a noise reduction coefficient of at least 0.85 when tested by ASTM C423-17.

[44] The wall panel according to

[43] , further comprising a porous decorative layer disposed on the open-cell skin.

[45] The wall panel according to

[43] , wherein the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both.

[46] The wall panel of

[45] , wherein the open cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the wall panel has a noise reduction coefficient of at least 0.5 when tested by ASTM C423-17.

[47] The wall panel of

[46] , further comprising a closed cell skin disposed on a second surface of the porous core layer.

[48] ​​The wall panel according to

[47] , wherein the flame retardant is homogeneously dispersed in the porous core layer.

[49] The wall panel of

[48] , wherein the thermoplastic material comprises a polyolefin resin and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.

[50] The wall panel of

[49] , further comprising a second wall panel bonded to the open cell skin, the second wall panel being a porous wall panel.

[51] A vinyl siding panel comprising: A flame-retardant noise reduction layer, a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; an open cell skin bonded to a first surface of the porous core layer, wherein the flame retardant layer has a flame spread index of less than 25 and a smoke development index of less than 150 when tested according to ASTM E84, 2009, and a noise reduction factor of at least 0.5 when tested according to ASTM C423-17; a vinyl substrate bonded to a first surface of the flame retardant noise reduction layer and configured to bond to a non-horizontal surface of a building to hold the vinyl siding panel to the non-horizontal surface of a building.

[52] The vinyl siding panel of

[51] , further comprising a weather barrier bonded to a second surface of the flame retardant noise reduction layer.

[53] The vinyl siding panel according to

[51] , wherein the vinyl substrate includes a nailing flange.

[54] The vinyl siding panel according to

[53] , wherein the open cell skin has an open surface area of ​​at least 10% and the vinyl siding has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[55] The vinyl siding panel according to

[54] , wherein the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both.

[56] The vinyl siding panel of

[55] , wherein the open cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the vinyl siding panel has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[57] The vinyl siding panel of

[56] , further comprising a closed cell skin disposed on a second surface of the porous core layer.

[58] The vinyl siding panel according to

[57] , wherein the flame retardant is homogeneously dispersed in the porous core layer.

[59] The vinyl siding panel of

[58] , wherein the thermoplastic material comprises a polyolefin resin and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.

[60] The vinyl siding panel of

[59] further comprising a second vinyl siding panel including a second flame retardant noise reducing layer bonded to a second vinyl substrate, wherein the flame retardant noise reducing layer is configured to engage with the second flame retardant noise reducing layer when the vinyl substrate is bonded to the second vinyl substrate.

[61] A roof panel comprising: A flame-retardant noise reduction layer, a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; an open cell skin bonded to a first surface of the porous core layer, wherein the flame retardant noise reduction layer has a flame spread index of less than 25 and a smoke development index of less than 150 when tested in accordance with ASTM E84, 2009, and a noise reduction factor of at least 0.5 when tested in accordance with ASTM C423-17; a roof substrate bonded to a first surface of the flame retardant noise reduction layer and configured to bond to a roof of a building to retain the roof panel to the roof.

[62] The roof panel of

[61] , further comprising a weather barrier bonded to a second surface of the flame-retardant noise reduction layer.

[63] The roof panel according to

[61] , wherein the roof substrate comprises a cellulosic material.

[64] The roof panel of

[63] , wherein the open cell skin has an open surface area of ​​at least 10% and the roof panel has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[65] The roof panel according to

[64] , wherein the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both.

[66] The roof panel of

[65] , wherein the open cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the roof panel has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[67] The roof panel of

[66] , further comprising a closed cell skin disposed on a second surface of the porous core layer.

[68] The roof panel according to

[67] , wherein the flame retardant is homogeneously dispersed in the porous core layer.

[69] The roof panel according to

[68] , wherein the thermoplastic material comprises a polyolefin resin and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.

[70] The roof panel of

[69] , further comprising a second roof panel including a second flame-retardant noise-reducing layer bonded to a second roof substrate, wherein the flame-retardant noise-reducing layer is configured to engage with the second flame-retardant noise-reducing layer when the roof substrate is positioned to overlap the second roof substrate.

[71] A roof shingle, A flame-retardant noise reduction layer, a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; an open cell skin bonded to a first surface of the porous core layer, wherein the flame retardant noise reduction layer has a flame spread index of less than 25 and a smoke development index of less than 150 when tested in accordance with ASTM E84, 2009, and a noise reduction factor of at least 0.5 when tested in accordance with ASTM C423-17; a weatherable shingle substrate bonded to a first surface of the flame retardant noise reducing layer and configured to bond to a roof panel of a building to provide a weatherable, flame retardant, noise reducing shingle over the roof panel.

[72] The roof panel of

[71] , further comprising a weather barrier bonded to a second surface of the flame retardant noise reduction layer.

[73] The roofing sheet according to

[71] , wherein the roofing sheet comprises asphalt.

[74] The roof shingle of

[73] , wherein the open cell skin has an open surface area of ​​at least 10%, and the shingle has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[75] The roofing sheet according to

[74] , wherein the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both.

[76] The roof shingle of

[75] , wherein the open-cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the shingle has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[77] The roof shingle of

[76] , further comprising a closed cell skin disposed on a second surface of the porous core layer.

[78] The roof panel according to

[77] , wherein the flame retardant is homogeneously dispersed in the porous core layer.

[79] The roof panel according to

[78] , wherein the thermoplastic material comprises a polyolefin resin and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.

[80] The roof shingle of

[79] , further comprising a second weather-resistant shingle including a second flame-retardant noise-reducing layer bonded to the second weather-resistant shingle, wherein the flame-retardant noise-reducing layer is configured to engage with the second flame-retardant noise-reducing layer when the weather-resistant shingle is positioned to overlap the second weather-resistant shingle.

[81] A recreational vehicle interior panel, comprising: A flame-retardant sound-reducing layer, a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; an open cell skin bonded to a first surface of the porous core layer; an interior wall substrate bonded to a second surface of the porous core layer, wherein the recreational vehicle interior panel has a flame spread index of less than 25 and a smoke developed index of less than 150 when tested in accordance with ASTM E84, 2009, and a noise reduction factor of at least 0.5 when tested in accordance with ASTM C423-17.

[82] The recreational vehicle interior panel described in

[81] , wherein the interior wall substrate is configured as a decorative layer.

[83] The recreational vehicle interior panel of

[82] , wherein the open cell skin has an open surface area of ​​at least 10%, and the recreational vehicle interior panel has a noise reduction coefficient of at least 0.85 when tested according to ASTM C423-17.

[84] The recreational vehicle interior panel according to

[83] , wherein the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both.

[85] The recreational vehicle interior panel of

[84] , wherein the open-cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the recreational vehicle interior panel has a noise reduction coefficient of at least 0.85 when tested by ASTM C423-17.

[86] The recreational vehicle interior panel of

[85] , further comprising a closed cell skin disposed on a second surface of the porous core layer.

[87] The recreational vehicle interior panel according to

[86] , wherein the flame retardant is homogeneously dispersed in the porous core layer.

[88] The recreational vehicle interior panel of

[87] , wherein the thermoplastic material comprises a polyolefin resin and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.

[89] The recreational vehicle interior panel of

[88] further comprising a second recreational vehicle interior panel including a second flame retardant noise reducing layer bonded to a second interior wall substrate, wherein the flame retardant noise reducing layer is configured to engage with the second flame retardant noise reducing layer when the interior wall substrate is positioned to vertically overlap the second interior wall substrate on a first side of the recreational vehicle interior panel.

[90] The recreational vehicle interior panel of

[89] further comprising a third recreational vehicle interior panel including a third flame retardant noise reducing layer bonded to a third interior wall substrate, wherein the flame retardant noise reducing layer is configured to engage with the third flame retardant noise reducing layer when the interior wall substrate is positioned to vertically overlap the third interior wall substrate on a second side of the recreational vehicle interior panel.

[91] A recreational vehicle exterior panel comprising: A flame-retardant sound-reducing layer, a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; an open cell skin bonded to a first surface of the porous core layer; a weather resistant exterior wall substrate bonded to a second surface of the porous core layer, wherein the recreational vehicle exterior panel has a flame spread index of less than 25 and a smoke developed index of less than 150 when tested in accordance with ASTM E84, 2009, and a sound reduction factor of at least 0.5 when tested in accordance with ASTM C423-17.

[92] The recreational vehicle exterior panel of

[91] , wherein the exterior wall substrate comprises fiberglass or is configured as a metal panel.

[93] The recreational vehicle exterior panel of

[92] , wherein the open cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the recreational vehicle exterior panel has a noise reduction coefficient of at least 0.85 when tested by ASTM C423-17.

[94] The recreational vehicle exterior panel according to

[93] , wherein the flame retardant comprises expandable graphite particles, or magnesium hydroxide, or both.

[95] The recreational vehicle exterior panel of

[94] , wherein the open cell skin comprises a perforated film having an open surface area of ​​at least 10%, and the recreational vehicle exterior panel has a noise reduction coefficient of at least 0.85 when tested by ASTM C423-17.

[96] The recreational vehicle exterior panel of

[95] , further comprising a closed cell skin disposed on a second surface of the porous core layer.

[97] The recreational vehicle exterior panel of

[96] , wherein the flame retardant is homogeneously dispersed in the porous core layer.

[98] The recreational vehicle exterior panel of

[97] , wherein the thermoplastic material comprises a polyolefin resin and the plurality of reinforcing fibers comprises glass fibers, or mineral fibers, or both.

[99] The recreational vehicle exterior panel of

[98] further comprising a second recreational vehicle exterior panel including a second flame retardant noise reducing layer bonded to a second exterior wall substrate, wherein the flame retardant noise reducing layer is configured to engage with the second flame retardant noise reducing layer when the exterior wall substrate is positioned to overlap the second exterior wall substrate on a first side of the recreational vehicle exterior panel.

[100] The recreational vehicle exterior panel of

[99] further comprising a third recreational vehicle exterior panel including a third flame retardant noise reducing layer bonded to a third exterior wall substrate, wherein the flame retardant noise reducing layer is configured to engage with the third flame retardant noise reducing layer when the exterior wall substrate is positioned to overlap the third exterior wall substrate on a second side of the recreational vehicle exterior panel.

[101] An interior architectural panel having two-dimensional or three-dimensional features, a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; and an open cell skin disposed on a first surface of the porous core layer, wherein the interior building panel having two or three dimensional features has a noise reduction coefficient of at least 0.5 when tested in accordance with ASTM C423-17, and the interior building panel having two or three dimensional features has a flame spread index of less than 25 and a smoke development index of less than 150 when tested in accordance with ASTM E84, 2009.

[102] An interior trim article, comprising: A flame-retardant noise reduction layer, a porous core layer comprising an open-celled web including a random arrangement of a plurality of reinforcing fibers held together by a thermoplastic material, the porous core layer including a flame retardant and a basis weight of at least 2500 gsm; an open cell skin disposed on a first surface of the porous core layer, the flame retardant noise reduction layer having a noise reduction factor of at least 0.5 when tested according to ASTM C423-17, and the flame retardant noise reduction layer having a flame spread index of less than 25 and a smoke development index of less than 150 when tested according to ASTM E84, 2009; an interior trim substrate bonded to a first surface of the flame retardant noise reduction layer.

Claims

1. 1. A thermoplastic composite article comprising: a porous core layer comprising an open-celled web comprising a random arrangement of a plurality of reinforcing glass fibers held together by a thermoplastic polyolefin resin material, said porous core layer comprising a flame retardant present at 30% to 50% by weight, based on the weight of the porous core layer, to provide flame retardancy to said composite article, said flame retardant comprising magnesium hydroxide or aluminum hydroxide as a flame retardant entrapped in the open cell structure of the web, said porous core layer comprising a basis weight of at least 2500 gsm, and wherein the thermoplastic polyolefin resin material is present in the porous core layer at 20% to 80% by weight; an open-cell, perforated film disposed on the first surface of the porous core layer, the open-cell, perforated film having an open surface area of ​​at least 5%, the open-cell, perforated film comprising one or more of polyethylene or polypropylene or polyamide; 1. A thermoplastic composite article, wherein the composite article has a noise reduction coefficient of at least 0.85 when tested by ASTM C423-17, and wherein the composite article has a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009.

2. 10. The thermoplastic composite article of claim 1, wherein the open cell, perforated film comprises at least 10% open surface area, and the open cell thermoplastic film has a basis weight of 70-120 gsm.

3. The thermoplastic composite article of claim 1 , wherein the open-celled, perforated film has an open surface area of ​​at least 10%.

4. The thermoplastic composite article of claim 3 , wherein the thermoplastic polyolefin resin material comprises polypropylene.

5. 5. The thermoplastic composite article of claim 4, wherein said plurality of reinforcing glass fibers is present at 30% to 70% by weight.

6. The thermoplastic composite article of claim 5 , further comprising a decorative layer disposed on the second surface of the porous core layer.

7. The thermoplastic composite article of claim 5 , further comprising a closed cell skin disposed on a second surface of said porous core layer.

8. The thermoplastic composite article of claim 6 , further comprising a decorative layer disposed on said closed cell skin.

9. A ceiling tile comprising: a porous core layer comprising an open-celled web comprising a random arrangement of a plurality of reinforcing glass fibers held together by a thermoplastic polyolefin resin material, said porous core layer comprising a flame retardant present at 30% to 50% by weight, based on the weight of the porous core layer, to provide flame retardancy to said ceiling tile, said flame retardant comprising magnesium hydroxide or aluminum hydroxide as a flame retardant trapped within the pores of the web, said porous core layer comprising a basis weight of at least 2500 gsm, and wherein the thermoplastic polyolefin resin material is present in the porous core layer at 20% to 80% by weight; an open-cell, perforated film disposed on the first surface of the porous core layer, the open-cell, perforated film having an open surface area of ​​at least 5%, the open-cell, perforated film comprising one or more of polyethylene or polypropylene or polyamide; A ceiling tile having a noise reduction factor of at least 0.85 when tested by ASTM C423-17, and a flame spread index of less than 25 and a smoke development index of less than 150 when tested by ASTM E84, 2009.

10. 10. The ceiling tile of claim 9, wherein said open cell perforated film has an open surface area of ​​at least 10% and a basis weight of said open cell perforated film is between 70 and 120 gsm.

11. 11. The ceiling tile of claim 10, further comprising a porous decorative layer disposed on said open cell skin.

12. 10. The ceiling tile of claim 9, wherein said open cell perforated film has an open surface area of ​​at least 10%.

13. 13. The ceiling tile of claim 12, further comprising a closed cell skin disposed on the second surface of the porous core layer.

14. 14. The ceiling tile of claim 13, wherein said fire retardant is homogeneously dispersed in said porous core layer.

15. 15. The ceiling tile of claim 14, wherein said thermoplastic polyolefin resin material comprises polypropylene.

16. 16. The ceiling tile of claim 15, wherein said plurality of reinforcing glass fibers is present at 30% to 70% by weight.

17. 16. The ceiling tile of claim 15, wherein the porous core layer further comprises clay.

18. The thermoplastic composite article of claim 1, wherein the thermoplastic polyolefin resin material is polypropylene and the porous core layer includes a scrim on a second surface of the porous core layer.

Citation Information

Patent Citations

  • Acoustic prepregs, cores and composite articles and methods of using them

    US20170129145A1

  • Prepregs, cores and composite articles including synergistic and compounded flame retardant materials

    US20170225429A1