Soundproofing material and its manufacturing method

The soundproofing material integrates a skin material with open-celled polyurethane foam to enhance sound absorption and maintain structural integrity under pressure, addressing the limitations of existing materials by improving soundproofing and damping while resisting deformation.

JP7587620B2Active Publication Date: 2024-11-20INOAC CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023036880
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-03-09
Publication Date
2024-11-20
Estimated Expiration
2038-12-25

AI Technical Summary

Technical Problem

Existing soundproofing materials for vehicles face challenges in achieving both high soundproofing effectiveness and maintaining shape under load, particularly on the noise emission side, and lack consideration for noise permeability through the carpet material.

Method used

A soundproofing material is designed with a skin material integrally molded on one side of polyurethane foam, where the opposite side is open-celled and impregnated with the foam raw material, ensuring high air permeability and compression hardness, and located between double walls for enhanced sound absorption and vibration damping.

Benefits of technology

The material achieves superior soundproofing and vibration damping properties, maintaining structural integrity under pressure, with improved sound absorption and reduced sinking when subjected to loads, suitable for vehicle floors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587620000001
    Figure 0007587620000001
  • Figure 0007587620000002
    Figure 0007587620000002
  • Figure 0007587620000003
    Figure 0007587620000003
Patent Text Reader

Abstract

To provide a soundproof material having high soundproof property, and being suitable for a floor silencer for a vehicle, and a dash silencer, and a production method thereof.SOLUTION: There is provided a soundproof material 10 in which a skin material 30 is integrally molded to one surface of a polyurethane foam 20, the polyurethane foam 20 is a foam being obtained from a polyurethane foam raw material and is configured so that, an opposite surface of the skin material 30 is an open cell. The skin material 30 has an impregnation layer 34 which is acquired by impregnation of the polyurethane foam raw material and curing, on the integration side with the polyurethane foam. An airflow quantity of the skin material 30 including the impregnation layer 34 on the basis of JIS K 6400-7B method:2012 is 5-80 cc / cm2 / sec.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a soundproofing material and a method for producing the same. [Background technology]

[0002] 2. Description of the Related Art Conventionally, soundproofing materials used as floor silencers or the like placed on the floor of a vehicle include polyurethane foam having a skin material laminated on one side thereof.

[0003] The following Patent Document 1 describes an automobile floor carpet having improved sound absorption and vibration damping properties by integrally forming an impact material made of a skinless urethane resin foam on the back surface of the carpet.

[0004] In addition, the following Patent Document 2 discloses that the breathability of the foam layer is 3.0 ft 3 / min or more, the foam layer hardness is 8kg / 314cm 2 The following polyurethane foam molded products with an integrated skin are described: [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 10-71884 [Patent Document 2] Japanese Patent Application Publication No. 11-5499 Summary of the Invention [Problem to be solved by the invention]

[0006] In Patent Document 1, an airtight film or a thin nonwoven fabric membrane is applied to the back of the carpet to prevent air from passing through, and an impact material made of a skinless urethane resin foam is integrally formed to improve soundproofing.

[0007] The polyurethane foam molded product with an integrated skin in Patent Document 2 is intended to provide good sound insulation in the low and mid-frequency ranges, and while improving the air permeability of the foam layer, it has a hardness of 8 kg / 314 cm. 2 When the skin is molded at an ILD of 25% or less and used in a vehicle, there is a problem that it sinks due to its softness when a load is applied to the skin.

[0008] In addition, both Patent Document 1 and Patent Document 2 consider the soundproofing properties of polyurethane foam, which is the sound source side (e.g., the floor side of a vehicle) where noise is incident, but do not consider the noise permeability of the carpet body or covering material, which is the non-sound source side (e.g., the interior side of a vehicle) where noise is emitted. Furthermore, it was difficult to achieve both with the hardness to maintain the shape when a load is applied.

[0009] The present invention has been made in consideration of the above-mentioned points, and aims to provide a soundproofing material with high soundproofing (sound absorption) effect that is placed between double walls having sound-insulating materials on both sides, and a manufacturing method thereof. [Means for solving the problem]

[0010] The invention of claim 1 relates to a soundproofing material having a skin material integrally molded on one side of a polyurethane foam, the polyurethane foam being a foam obtained from a polyurethane foam raw material, the surface opposite to the skin material being open cell, the skin material having an impregnation layer formed by impregnating and curing the polyurethane foam raw material on the side integral with the polyurethane foam, and the air permeability of the skin material including the impregnation layer based on JIS K6400-7B method: 2012 is 5 to 80 cc / cm. 2 / sec.

[0011] The invention of claim 2 is characterized in that in claim 1, the skin material is made of a fiber aggregate.

[0012] The invention of claim 3 is characterized in that, in the case of claim 1 or 2, the soundproofing material has a compression hardness of 500 N or more, measured as the load at 50% compression when a sample of 200 mm square x 20 mm thick is compressed to 80% of its thickness in a compression jig of φ80 mm at a test speed of 50 mm / min.

[0013] The invention of claim 4 is characterized in that in any one of claims 1 to 3, the soundproofing material has a reverberation room sound absorption coefficient of 40% or more measured based on JIS A1409.

[0014] The invention of claim 5 is characterized in that in any one of claims 1 to 4, the soundproofing material has a transmission loss of 42.2 dB or more at 1600 Hz measured based on JIS A1441-1:2007.

[0015] The invention of claim 6 is characterized in that in any one of claims 1 to 5, the soundproofing material is located between a double wall having sound insulation materials on both sides.

[0016] The invention of claim 7 relates to a method for producing a soundproofing material in which a skin material is integrally molded on one side of a polyurethane foam by attaching a skin material to a mold surface of either an upper or lower mold of a foam molding mold, injecting a polyurethane foam raw material containing at least a polyol component, a catalyst, a blowing agent, and an isocyanate into the foam molding mold, and foaming the polyurethane foam raw material, the method comprising the steps of: attaching a skin material to a mold surface of either an upper or lower mold of a foam molding mold; injecting a polyurethane foam raw material containing at least a polyol component, a catalyst, a blowing agent, and an isocyanate into the foam molding mold; and foaming the polyurethane foam raw material, the method comprising the steps of: attaching a skin material to a mold surface of either an upper or lower mold of a foam molding mold;2 / sec, and the soundproofing material is characterized in that it has a compression hardness of 500 N or more, measured as the load at 50% compression when a sample of 200 mm square x 20 mm thick is compressed to 80% of its thickness in a φ80 mm compression jig at a test speed of 50 mm / min. Effect of the Invention

[0017] In the soundproofing material of the present invention, the skin side is the non-sound source side, and the polyurethane foam side opposite to the skin side is the sound source side. In the soundproofing material of the present invention, the surface of the polyurethane foam on the sound source side is made of open cells, so that sound from the sound source can easily enter the polyurethane foam, and further, the skin on the non-sound source side (i.e., the sound exit side) has an impregnated layer, and the air permeability of the skin including the impregnated layer based on JIS K6400-7B method: 2012 is 5cc / cm 2 / sec or more, it provides good soundproofing (sound absorption). In addition, by providing slits of 100 mm square or less to the urethane foam alone, it improves adhesion to the soundproofing material, and further improves vibration damping.

[0018] The method for manufacturing soundproofing material of the present invention can produce soundproofing material that has good soundproofing properties (sound absorption properties) and sufficient hardness, and that does not sink much due to pressure, for example, when placed on the floor of a vehicle and pressed by the shoes of a passenger. [Brief description of the drawings]

[0019] [Figure 1] 1 is a cross-sectional view of a soundproofing material according to an embodiment. [Diagram 2] 4 is a cross-sectional view showing a process halfway through in a method for producing a soundproofing material. FIG. [Diagram 3] 4A to 4C are cross-sectional views showing the remaining steps in the method for manufacturing the soundproofing material. [Figure 4] 1 is a table showing the configurations of the examples and the measurement results of the physical properties and soundproofing properties (sound absorption properties). [Diagram 5] 1 is a table showing the configuration of a comparative example and the measurement results of the physical properties and soundproofing (sound absorption). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] An embodiment of the present invention will be described below. A soundproofing material 10 of the embodiment shown in Fig. 1 is made of a laminate in which a skin material 30 is integrally formed on one side of a polyurethane foam 20. The soundproofing material 10 is suitable as a floor silencer or the like placed on the floor of a vehicle as a soundproofing (sound absorbing) material between double walls having sound insulation materials on both sides, and the surface of the polyurethane foam 20 opposite to the skin material 30 is placed on a sound source member such as a vehicle floor as the sound source side. On the other hand, the skin material 30 side of the soundproofing material 10 is the non-sound source side.

[0021] The polyurethane foam 20 is a foam obtained from a polyurethane foam raw material, and a surface 21 (a surface on the sound source side) opposite to the skin material 30 has open cells. The surface 21 of the polyurethane foam 20 opposite to the skin material 30 (the surface on the sound source side) may be slit to adhere to a sound-proofing material and improve vibration-damping properties. The shape of the slits is not limited, and examples include a lattice-like or parallel cut line.

[0022] In addition, the polyurethane foam 20 has a density (JIS K7222:2005) of 30 to 95 kg / m 3 The thickness is preferably 1 to 40 mm. If the density of the polyurethane foam 20 is too low, the hardness will be low, and if the density is too high, the soundproofing material 10 will be heavy. If the polyurethane foam 20 is too thin, the raw material cannot be filled and the soundproofing material 10 will not be able to be molded, and if the polyurethane foam 20 is too thick, the soundproofing material 10 will be bulky and heavy.

[0023] The polyurethane foam raw material contains at least a polyol component, a catalyst, a blowing agent, and an isocyanate, and the polyol component contains a polymer polyol.

[0024] The polyol component comprises a polyether polyol and a polymer polyol. Examples of the polyether polyol include polyhydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, neopentyl glycol, glycerin, pentaerythritol, trimethylolpropane, sorbitol, and sucrose, and polyether polyols in which an alkylene oxide such as ethylene oxide or propylene oxide is added to the polyhydric alcohol.

[0025] The polyether polyol is preferably a polyether polyol having a functionality of 2 to 8, a hydroxyl value of 20 to 168 mgKOH / g, and a number average molecular weight of 168 to 20000. The ethylene oxide content (EO ratio) of the polyether polyol is preferably 5 to 90%. The ethylene oxide content (EO ratio) of the polyether polyol is the content of ethylene oxide units when the total amount of one raw material composition unit is taken as 100% by weight.

[0026] The polymer polyol is obtained by polymerizing an ethylenically inactive compound in a polyether polyol. By including the polymer polyol in the polyol component, the effect of improving the breathability and hardness can be obtained. The polymer polyol preferably has a functionality of 3 to 8, a hydroxyl value of 20 to 60 mgKOH / g, and a number average molecular weight of 2000 to 8000. The ethylene oxide content (EO rate) of the polymer polyol is preferably 3 to 50%. The ethylene oxide content (EO rate) of the polymer polyol is the content of ethylene oxide units when the total amount of one raw material composition unit is taken as 100% by weight. The weight proportion of the polymer polyol in the polyol component is preferably from 20 to 100%, more preferably from 50 to 100%, with the remainder being polyether polyol.

[0027] The catalyst may be one known for use in polyurethane foams. Examples of the catalyst include amine catalysts such as triethylamine, triethylenediamine, diethanolamine, dimethylaminomorpholine, N-ethylmorpholine, tetramethylguanidine, and imidazole-based compounds, tin catalysts such as stannous octoate and dibutyltin dilaurate, and metal catalysts (also called organometallic catalysts) such as phenylmercury propionate and lead octenate. A combination of multiple catalysts may be used. The general amount of catalyst is about 0.2 to 4 parts by weight, preferably 1 to 3 parts by weight, per 100 parts by weight of the polyol component.

[0028] The foaming agent is not particularly limited, but water is preferred. The amount of water used as the foaming agent is preferably about 2 to 10 parts by weight, more preferably 3 to 7 parts by weight, based on 100 parts by weight of the polyol component.

[0029] The isocyanate may be any of aromatic, alicyclic, and aliphatic isocyanates, and may be a bifunctional isocyanate having two isocyanate groups in one molecule, or a trifunctional or higher isocyanate having three or more isocyanate groups in one molecule, and these may be used alone or in combination.

[0030] For example, bifunctional isocyanates include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, xylylene diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'- Examples of the isocyanate include aromatic isocyanates such as biphenylene diisocyanate, alicyclic isocyanates such as cyclohexane-1,4-diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, and methylcyclohexane diisocyanate, and aliphatic isocyanates such as butane-1,4-diisocyanate, hexamethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, and lysine isocyanate.

[0031] Examples of trifunctional or higher isocyanates include 1-methylbenzene-2,4,6-triisocyanate, 1,3,5-trimethylbenzene-2,4,6-triisocyanate, biphenyl-2,4,4'-triisocyanate, diphenylmethane-2,4,4'-triisocyanate, methyldiphenylmethane-4,6,4'-triisocyanate, 4,4'-dimethyldiphenylmethane-2,2',5,5'tetraisocyanate, triphenylmethane-4,4',4"-triisocyanate, polymeric MDI, and the like. Other urethane prepolymers can also be used. The isocyanate is, Each of them is not limited to one type, and may be one or more types. For example, one type of aliphatic isocyanate and two types of aromatic isocyanate may be used, or two types of aromatic isocyanate and urethane prepolymer may be used, or three or more types of isocyanate may be used. The isocyanate index is preferably 90 to 130, more preferably 95 to 120. The isocyanate index is an index used in the field of polyurethane, and is a numerical value that represents the equivalent ratio of the isocyanate group of the isocyanate to the active hydrogen group in the raw material (for example, the active hydrogen group contained in the hydroxyl group of polyols and the active hydrogen group of water as a blowing agent, etc.) expressed as a percentage.

[0032] The polyol component may optionally contain a foam stabilizer and additives. The foam stabilizer may be any foam stabilizer that is used in polyurethane foam, including silicone foam stabilizers, fluorine-containing compound foam stabilizers, and known surfactants. The amount of foam stabilizer is preferably 0 to 2 parts by weight per 100 parts by weight of the polyol component.

[0033] Examples of the additives include a linking agent, a crosslinking agent, a pigment, a filler, a flame retardant, an antioxidant, and an ultraviolet absorbing agent. Examples of the opening agent include polyether polyols with a high EO addition ratio, polyethylene glycols, and silicone foam stabilizers that increase air permeability (having foam breaking properties). When a opening agent is used, the amount of the opening agent is preferably 0.5 to 20 parts by weight per 100 parts by weight of polyol. The opening agent is not limited to one type, and two or more types may be used. Examples of the crosslinking agent include glycerin, trimethylolpropane, 1,2,4-butanetriol, 2-methyl-2,3,4-butanetriol, triethanolamine, pentaerythritol, etc., and one or more of them may be used in combination. Preferred crosslinking agents include glycerin, pentaerythritol, diethanolamine, etc., which have 2 to 4 functional groups, a molecular weight of 92 to 136, and a hydroxyl value of 1066 to 1826 mgKOH / g. The amount of the crosslinking agent is preferably 1 to 6 parts by weight based on 100 parts by weight of the polyol component. The crosslinking agent may have an ethylene oxide content (EO ratio) of more than 0%. For example, ethylenediamine-based (functional group number: 4, molecular weight: 280, hydroxyl value 800 mg KOH / g, EO ratio 40%), trimethylolpropane-based (functional group: 3, molecular weight: 183, hydroxyl value 920 mg KOH / g, EO ratio 50%), etc.

[0034] Examples of the pigment include carbon black and titanium oxide. Examples of the filler include graphite, alumina, and melamine.

[0035] Specific examples of the flame retardant include halogenated diphenyl ethers such as degabromdiphenyl ether and octabromdiphenyl ether, halogen compounds such as halogenated polycarbonates, inorganic compounds such as antimony trioxide, antimony tetraoxide, antimony pentoxide, sodium pyroantimonate, and aluminum hydroxide, triazine ring-containing compounds, metal hydroxides, phosphate flame retardants, condensed phosphate flame retardants, phosphate flame retardants, inorganic phosphorus flame retardants, dialkylphosphinates, silicone flame retardants, metal oxides, boric acid compounds, and expandable graphite.

[0036] Examples of the antioxidant include naphthylamines, diphenylamines, p-phenyldiamines, quinolines, hydroquinone derivatives, monophenols, thiobisphenols, hindered phenols, and phosphites.

[0037] Examples of the ultraviolet absorber include 2-hydroxybenzophenones such as 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-octoxybenzophenone, and 5,5'-methylenebis(2-hydroxy-4-methoxybenzophenone); 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, and 2-(2'-hydroxy-3',5'- 2-(2'-hydroxyphenyl)benzotriazoles such as 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-dicumylphenyl)benzotriazole, 2,2'-methylenebis(4-tert-octyl-6-(benzotriazolyl)phenol), 2-(2'-hydroxy-3'-tert-butyl-5'-carboxyphenyl)benzotriazole; phenyl Benzoates such as ricinate, resorcinol monobenzoate, 2,4-ditert-butylphenyl-3,5-ditert-butyl-4-hydroxybenzoate, 2,4-ditert-amylphenyl-3,5-ditert-butyl-4-hydroxybenzoate, hexadecyl-3,5-ditert-butyl-4-hydroxybenzoate; substituted oxanilides such as 2-ethyl-2'-ethoxyoxanilide, 2-ethoxy-4'-dodecyloxanilide; ethyl-α-cyano-β,β-diphenylacrylate, methyl cyanoacrylates such as aryl-2-cyano-3-methyl-3-(p-methoxyphenyl)acrylate; and triaryltriazines such as 2-(2-hydroxy-4-octoxyphenyl)-4,6-bis(2,4-di-tert-butylphenyl)-s-triazine, 2-(2-hydroxy-4-methoxyphenyl)-4,6-diphenyl-s-triazine, and 2-(2-hydroxy-4-propoxy-5-methylphenyl)-4,6-bis(2,4-di-tert-butylphenyl)-s-triazine.

[0038] The EO ratio of the polyurethane foam is preferably 7 to 15%, more preferably 8 to 13%. If the EO ratio of the polyurethane foam is too low or too high, the soundproofing (sound absorption) properties of the soundproofing material will decrease.

[0039] Here, the method for measuring the EO ratio of polyurethane foam is to place only the polyurethane foam in a Soxhlet extractor (weight of polyurethane foam put in is A (g)), wash with a solvent (acetone) at 68-72°C for 8 hours, dry, and then decompose with alkali. After that, extract only the polyol component (weight of the extracted component is B (g)), and evaluate a part of it by matrix-assisted laser time-of-flight mass spectrometry (manufactured by JEOL). Calculate the EO ratio for each molecular weight (EO ratio for each molecular weight (= EO N number (theoretical value) × number of each molecular weight ÷ total number)), and let the sum be C. The method for calculating the EO ratio of polyurethane foam is as follows. EO ratio of polyurethane foam = [B x C] / [A] x 100 However, the molecular weight is calculated to be 800 or more.

[0040] The skin material 30 may be a fiber aggregate such as nonwoven fabric or felt, with felt being particularly preferred from the standpoint of light weight and soundproofing (sound absorption). The skin material of this embodiment is made of a two-layer nonwoven fabric sheet consisting of a first layer 31 and a second layer 33. The first layer 31 faces away from the polyurethane foam 20, while the second layer 33 faces the polyurethane foam 20.

[0041] Either the first layer 31 or the second layer 33 is made of a fiber having a diameter of 2 to 4d and has a basis weight of 90 g / m 2 More than 90g / m 2 More than 500g / m 2 The other layer has a basis weight of 100 g / m 2 More than 100g / m 2 More than 500g / m 2When the skin 30 is constructed in this manner, one of the layers is densely packed with fine fibers, so that the viscous polyurethane foam raw material is less likely to seep out of the skin 30. One of the two layers contains an acrylic ester resin at 35 g / m 2 More than 35g / m 2 More than 100g / m 2 The layer impregnated with the acrylic ester resin has spaces between the fibers filled with the acrylic ester resin, making it difficult for the polyurethane foam raw material to pass through the skin material 30, and making it even more difficult for the polyurethane foam raw material to seep out. The acrylic ester resin can be impregnated into the skin material 30 by applying an emulsion of the acrylic ester resin to the surface of the skin material 30, or by scattering acrylic ester resin powder on the surface of the skin material 30 and applying a heated roller or hot air to the surface.

[0042] By adjusting the basis weight of the first layer 31 and the second layer 33 and the impregnation of the acrylic ester resin, the air permeability based on JIS K6400-7B method: 2012 of the skin material 30 including the impregnated layer 34 is set to 5 to 80 cc / cm. 2 The air permeability of the skin material 30 including the impregnated layer 34 based on JIS K6400-7B method: 2012 can be set to 5 to 80 cc / cm 2 / sec, the soundproofing (sound absorption) properties of the soundproofing material 10 can be improved.

[0043] In a more preferred embodiment of the skin 30, the second layer 33 on the polyurethane foam 20 side is made of fibers with a fiber diameter of 2 to 4d and a basis weight of 90 g / m 2 The above composition, and the acrylic ester resin is 35 g / m 2 When the skin material 30 is constructed in this manner, the second layer 33 that comes into contact with the polyurethane foam raw material during the production of the soundproofing material 10 is densely packed with fine fibers, and the acrylic ester resin is impregnated at 35 g / m 2Since the polyurethane foam raw material is impregnated to the extent that the polyurethane foam 20 is impregnated to the inner wall of the second layer 33, the amount of the polyurethane foam raw material that is impregnated (seeps) into the second layer 33 is limited. Therefore, the impregnated layer 34 formed by the impregnation and hardening of the polyurethane foam raw material in the portion of the second layer 33 in contact with the polyurethane foam 20 becomes thin or coarse, and the breathability of the second layer 33 can be ensured.

[0044] The basis weight of the first layer 31 on the opposite side to the polyurethane foam 20 is 100 g / m 2 By doing so, it is possible to effectively prevent the first layer 31 from being impregnated with the raw material for the urethane foam, and ensure the breathability of the skin material 30. Furthermore, it is preferable to improve the abrasion resistance of the surface of the first layer 31 by making the fiber diameter 5d or more. The first layer 31 and the second layer 33 are integrated together by adhesion or needle punching.

[0045] The soundproofing material 10 has a compression hardness of preferably 500 N or more, more preferably 650 to 1200 N, as measured by the load at 50% compression when a sample of 200 mm square x 20 mm thick is compressed to 80% of its thickness in a compression jig of φ80 mm at a test speed of 50 mm / min. If the compression hardness of the soundproofing material 10 is too low, for example, when the upper surface of the soundproofing material 10 is pressed by the foot of a passenger, the pressed portion sinks, making it difficult to walk or making the passenger's posture unstable.

[0046] A manufacturing method of the soundproofing material 10 will be described with reference to Fig. 2. The soundproofing material 10 is manufactured by molding using a metal mold 40. The metal mold 40 is composed of a lower mold 41 and an upper mold 43, and the skin 30 is attached to either the lower mold 41 or the upper mold 43. The skin 30 is attached so that the first layer 31 faces the mold surface of one of the molds and the second layer 33 faces inside the mold. When the skin 30 is attached to the upper mold 43, a locking means consisting of a locking pin or the like for removably holding the skin 30 is provided on the mold surface of the upper mold 43. In the illustrated example, the skin material 30 is attached to the mold surface of the upper mold 43 as shown in FIG. 2 (2-1).

[0047] Before attaching the skin material 30 to the surface of the mold 40, a release agent 38 is applied to the surface of the mold 40. The release agent 38 preferably contains a linear hydrocarbon wax in order to facilitate the formation of open cells on the surface of the polyurethane foam 20 on the sound source side. Examples of linear hydrocarbon wax include paraffin wax, Fischer-Tropsch wax, and Sasol wax. Solvent-based release agents dispersed in an organic solvent, and water-based release agents dispersed in water using an emulsifier can be used.

[0048] A mold release agent 38 is applied to the surface of the mold 40, and the skin 30 is attached. Then, as shown in FIG. 2 (2-2), polyurethane foam raw material 20a is mixed and injected into the mold 40, and the mold is closed to cause the polyurethane foam raw material 20a to foam in the molding space between the second layer 33 of the skin 30 and the surface of the lower part 41 of the mold 40.

[0049] The polyurethane foam raw material 20a injected into the mold 40 fills the molding space between the second layer 33 of the skin material 30 and the mold surface of the lower part of the mold 40 by foaming, and forms the polyurethane foam 20 integrally with the skin material 30, as shown in Figure 2 (2-3). At that time, a part of the polyurethane foam raw material 20a impregnates and hardens in the second layer 33 of the skin material 30, and forms an impregnation layer 34 on the boundary side with the polyurethane foam 20.

[0050] Thereafter, as shown in FIG. 3, upper mold 43 is separated from lower mold 41 to open mold 40, and soundproofing material 10 consisting of a laminate in which skin material 30 is integrally molded on one side of polyurethane foam 20 as shown in FIG. 1 is removed. EXAMPLES

[0051] A soundproofing material measuring 500 mm square and 20 mm thick was manufactured by a mold foaming method using a mold 40 shown in Figs. 2 and 3, using polyurethane foam raw material having the composition shown in Figs. 4 and 5. The numerical values ​​of each component in the composition shown in Figs. 4 and 5 indicate parts by weight. The mold was heated with warm water, and the lower mold 41 and upper mold 43 were heated to 70°C. As a mold release agent, linear hydrocarbon wax (product name: URH-520, manufactured by Konishi Co., Ltd.) was sprayed onto the mold surface at 10 to 30 g / m. 2 It was applied.

[0052] In Examples 1 to 5 and Comparative Examples 1 to 3, soundproofing materials were manufactured by attaching a skin material to the mold surface of the upper mold 43 as shown in Figures 2 and 3. In Comparative Example 4, instead of polyurethane foam, materials such as synthetic fibers and cotton were molded with thermoplastic resin, and the basis weight was 1200 g / m. 2 This is an example using felt.

[0053] The components constituting the composition of Figure 4 are as follows: Polyol-1: Polyether polyol, functionality 3.6, number average molecular weight 5500, hydroxyl value 31.5 mg KOH / g, EO ratio 8% Polyol-2: Polymer polyol, functionality 3, number average molecular weight 5000, hydroxyl value 25 mg KOH / g, EO ratio 13%, solids concentration 30% Foaming agent: Water Amine catalyst 1: Diethanolamine Amine catalyst 2: Aliphatic tertiary amine composition [bis(2-dimethylaminoethyl) ether / dipropylene glycol] Foam stabilizer: Organic modified siloxane, product name: B8715LF2, EVONIC Additives: Polyether polyol, molecular weight 5000, functionality 3, hydroxyl value 34mgKOH, EO ratio 70% Isocyanate 1 (ISO-1): Polymeric MDI, NCO% 31.5% Isocyanate 2 (ISO-2): 4,4'-MDI / urethane prepolymer = 75-85 / 15-25, NCO% 26.5%, EO rate 10%

[0054] For each Example and Comparative Example, the thickness of the impregnated layer in the second layer, the appearance of the polyurethane foam, the hardness of the soundproofing material, the density of the polyurethane foam, the air permeability of the skin material including the impregnated layer, the reverberation chamber sound absorption coefficient, the reverberation chamber sound absorption coefficient of the polyurethane foam, and the transmission loss of the soundproofing material were calculated or measured.

[0055] The thickness of the impregnated layer in the skin 30 was measured using a scanning electron microscope (SEM: manufactured by JEOL Ltd.) at a magnification of 35x on a 500 mm square x 20 mm thick soundproofing material, and the average of five points (including the maximum and minimum) was calculated. The appearance of polyurethane foam was evaluated by visually inspecting the cross section of a 500mm square x 20mm thick soundproof polyurethane foam. If the foam is composed of cells with a maximum average diameter of 5mm or less and there are no voids larger than 5mm, it was rated as "◎", if there were voids with a maximum average diameter of 5mm or more but not exceeding 18mm, it was rated as "〇", and if there were voids with a maximum average diameter of more than 18mm, it was rated as "X". The maximum average diameter is the average of the major and minor diameters. If large voids exist, the hardness of that area is greatly reduced and that area sinks more when pressure is applied.

[0056] To measure the hardness of the soundproofing material, a sample of 500mm square x 20mm thick soundproofing material was cut to 200mm square x 20mm thick, placed with the skin material on top, and compressed using a φ80mm compression tool at a compression speed of 50mm / min until the displacement was 80% of the thickness (sample displacement 16mm, remaining sample thickness 4mm), and the loads at 25%, 50% and 75% compression were read as the measured values. The hardness of the soundproofing material was evaluated by measuring the load at 50% compression and giving a rating of "◎" if the compressive hardness was 1000N or more, "◯" if it was 500N or more but less than 1000N, and "×" if it was less than 500N.

[0057] The density of the polyurethane foam was measured in accordance with JIS K7222:2005 on a sample made of the remaining polyurethane foam, which was obtained by cutting a 500mm square x 20mm thick soundproofing material into a 100mm square x 20mm thick piece, removing the skin portion from the resulting cut piece (or the skin portion including the impregnated layer, if an impregnated layer was present).

[0058] The air permeability of the skin material including the impregnated layer was measured by cutting a 500 mm square x 20 mm thick soundproofing material into a 100 mm square x 20 mm thick piece, cutting out the skin part (if an impregnated layer is present, then the skin part including the impregnated layer) from the resulting cut piece, placing the impregnated layer underneath the sample made of the cut-out skin part (if an impregnated layer is present, then the skin part including the impregnated layer) and measuring based on JIS K6400-7B method:2012.

[0059] The sound absorption coefficient of the reverberation room was measured by placing 10 pieces of soundproofing material measuring 500 mm square and 20 mm thick in a reverberation room (approximately 30 m 3 ) and the test was performed on the surface of the skin material (surface on the non-sound source side) based on JIS A 1409. All gaps between the samples and between the sample and the jig were sealed with aluminum tape. The reverberation room sound absorption coefficient was determined by averaging the measured sound absorption coefficients at each frequency (500, 630, 800, 1000, 1250, 1600, 2000, 2500, 3150, 4000, 5000, 6300 Hz). The reverberation room sound absorption coefficient of the soundproofing material 10 is the average sound absorption coefficient for the surface of the skin material side including the impregnated layer. The reverberation chamber sound absorption rate was evaluated as "◎" if it was 65% or more, "◯" if it was 40% or more but less than 65%, and "×" if it was less than 40%.

[0060] The transmission loss was measured based on JIS A1441-1:2007. The sound source reverberation room was 36 m 3 , the anechoic chamber is 20m 3 The measurement area is 400 × 400 mm (0.16 m 2The sound source side of the soundproofing material is a 500mm square x 20mm thick polyurethane foam, and the surface is covered with a 0.8mm thick steel plate (soundproofing material). The non-sound source side is covered with a 1mm thick rubber sheet (soundproofing material) (1700g / m 2 ) was layered, the periphery of the soundproofing material was fixed with a 50mm wide frame, and the gaps were further sealed with clay, and sound was incident from the iron plate side as the sound source, and the values ​​were measured at 1600Hz at four centrally separated scattered points (100mm pitch) 100mm away from the surface of the rubber sheet. "Configuration A" of the transmission loss in Figures 4 and 5 is a configuration in which the urethane foam is attached to the iron plate, i.e. the skin material is in close contact with the rubber sheet, and "Configuration B" is a configuration in which the skin material is in close contact with the iron plate, i.e. the urethane foam is in close contact with the rubber sheet. The transmission loss was evaluated as "◎" if it was 44.2 dB or more, "◯" if it was 42.2 or more and less than 44.2 dB, and "×" if it was less than 42.2 dB.

[0061] A comprehensive evaluation was performed for each example and each comparative example. The comprehensive evaluation was determined to be the lowest evaluation among the individual evaluations. For example, if all the evaluations were "◎", the comprehensive evaluation was "◎", if at least one of the evaluations was "◯" and the rest were "◎", the comprehensive evaluation was "◯", if at least one of the evaluations was "△" and the rest were "◯" or "◎", the comprehensive evaluation was "△", and if at least one of the evaluations was "×" and the rest were "△", "◯", or "◎", the comprehensive evaluation was "×".

[0062] In Example 1, polyurethane foam raw materials were used, which were 30 parts by weight of polyol-1, 70 parts by weight of polyol-2, 5.10 parts by weight of foaming agent, 2.71 parts by weight of amine catalyst-1, 0.39 parts by weight of amine catalyst-2, 0 parts by weight of foam stabilizer, 0 parts by weight of additive, isocyanate ISO-1:ISO-2=22:78, isocyanate index 105, and EO ratio of polyurethane foam 9.20%, and the first layer was made of 6d PET fiber and had a basis weight of 150g / m as a skin material. 2 , the second layer is 3D PET fiber, basis weight 100g / m 2 , acrylic acid Ester resin is 50g / m 2 Impregnated with 300g / m22 The skin material used was

[0063] The results of Example 1 were: thickness of the impregnated layer was 0.5 mm, the appearance of the polyurethane foam was "◎", the hardness of the soundproofing material at 50% compression was 1110 N, the evaluation was "◎", and the density of the polyurethane foam was 55 kg / m 3 The air permeability of the skin material including the impregnated layer is 20.8cc / cm 2 / sec, the reverberation chamber sound absorption rate of the soundproofing material was 71%, rated "◎", the transmission loss of the soundproofing material was "Configuration A" 49.2dB, rated "◎", and the overall rating was "◎", indicating good soundproofing (sound absorption) properties.

[0064] Example 2 is an example in which polyurethane foam raw materials containing 30 parts by weight of polyol-1, 70 parts by weight of polyol 2, 5.76 parts by weight of blowing agent, 3.06 parts by weight of amine catalyst-1, 0.45 parts by weight of amine catalyst-2, 0.31 parts by weight of foam stabilizer, 2.27 parts by weight of additives, isocyanate ISO-1:ISO-2=22:78, isocyanate index 105, and EO rate of polyurethane foam 9.65% were used, and a skin material having the same composition as that of Example 1 was used as the skin material.

[0065] The results of Example 2 were as follows: the thickness of the impregnated layer was 0.5 mm, the appearance of the polyurethane foam was "◎", the hardness of the soundproofing material at 50% compression was 1400 N, the evaluation was "◎", and the density of the polyurethane foam was 55 kg / m 3 The air permeability of the skin material including the impregnated layer is 11.7cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the soundproofing material was 65%, rated "◎", the soundproofing material's transmission loss was "Configuration A" 47.2dB, rated "◎", and the overall rating was "◎", indicating good soundproofing (sound absorption) properties.

[0066] Example 3 is an example in which polyurethane foam raw materials containing 30 parts by weight of polyol-1, 70 parts by weight of polyol 2, 5.88 parts by weight of blowing agent, 3.13 parts by weight of amine catalyst-1, 0.45 parts by weight of amine catalyst-2, 0 part by weight of foam stabilizer, 9.84 parts by weight of additives, isocyanate ISO-1:ISO-2=0:100, isocyanate index 105, and EO rate of polyurethane foam 12.56% were used, and a skin material having the same composition as that of Example 1 was used as the skin material.

[0067] The results of Example 3 were: thickness of the impregnated layer was 0.5 mm, the appearance of the polyurethane foam was "good", the hardness of the soundproofing material at 50% compression was 650N, the evaluation was "good", and the density of the polyurethane foam was 55 kg / m 3 The air permeability of the skin material including the impregnated layer is 72cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the soundproofing material was 73%, rated "◎", the transmission loss of the soundproofing material was "Configuration A" 50.2 dB, rated "◎", and the overall rating was "◯". The appearance of the polyurethane foam was inferior to the other examples, but the soundproofing (sound absorption) properties were good.

[0068] Example 4 is an example in which polyurethane foam raw materials containing 0 part by weight of polyol-1, 100 parts by weight of polyol-2, 6.41 parts by weight of blowing agent, 3.33 parts by weight of amine catalyst-1, 0.37 parts by weight of amine catalyst-2, 0 part by weight of foam stabilizer, 2.47 parts by weight of additives, isocyanate ISO-1:ISO-2=0:100, isocyanate index 120, and EO rate of polyurethane foam 11.26% were used, and a skin material having the same composition as that of Example 1 was used as the skin material.

[0069] The results of Example 4 were: thickness of the impregnated layer was 0.5 mm, the appearance of the polyurethane foam was "◎", the hardness of the soundproofing material at 50% compression was 1024 N, the evaluation was "◎", and the density of the polyurethane foam was 55 kg / m 3 The air permeability of the skin material including the impregnated layer is 8.23cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the soundproofing material was 59%, rated "Good", the soundproofing material's transmission loss was "Configuration A" 44.2dB, rated "Excellent", and the overall rating was "Good", indicating good soundproofing (sound absorption) properties.

[0070] Example 5 is an example in which polyurethane foam raw materials containing 30 parts by weight of polyol-1, 70 parts by weight of polyol 2, 5.10 parts by weight of blowing agent, 2.71 parts by weight of amine catalyst-1, 0.39 parts by weight of amine catalyst-2, 0 part by weight of foam stabilizer, 0 part by weight of additives, isocyanate ISO-1:ISO-2=22:78, isocyanate index 105, and EO rate of polyurethane foam 9.20% were used, and a skin material having the same composition as that of Example 1 was used as the skin material.

[0071] The results of Example 5 were: thickness of the impregnated layer was 0.5 mm, the appearance of the polyurethane foam was "◎", the hardness of the soundproofing material at 50% compression was 1110 N, the evaluation was "◎", and the density of the polyurethane foam was 55 kg / m 3 The air permeability of the skin material including the impregnated layer is 20.8cc / cm 2 / sec, the reverberation chamber sound absorption rate of the soundproofing material was 71%, rated "◎". The sound source side and non-sound source side of the soundproofing material were set in opposite directions, and the sound source was placed on the skin side, and the sound transmission loss was 47.2dB (Configuration B), rated "◎". The overall rating was "◎", and the soundproofing (sound absorption) properties were good.

[0072] Comparative Example 1 had the same configuration as Example 1, except that a resin film made of polyethylene terephthalate resin and having a thickness of 0.03 mm was adhered with an acrylic urethane adhesive to the surface of the second layer of the skin material of Examples 1 to 3 that faced the polyurethane foam.

[0073] The results of Comparative Example 1 are as follows: no impregnation layer (thickness 0 mm), polyurethane foam appearance "◎", hardness of soundproofing material at 50% compression 1230N, evaluation "◎", polyurethane foam density 55kg / m 3 , the ventilation rate of the skin is 0cc / cm 2 / sec, the soundproofing material's reverberation chamber sound absorption coefficient was 30%, rated "x", the soundproofing material's transmission loss was "Configuration A" 41.2 dB, rated "x", and the overall rating was "x". In Comparative Example 1, since a resin film was laminated on the second layer of the skin material, the skin material had no impregnation layer or breathability, the skin material's reverberation chamber sound absorption coefficient was low, and the soundproofing (sound absorption) properties of the soundproofing material were inferior to those of Examples 1 to 3.

[0074] Comparative Example 2 is an example in which polyurethane foam raw materials containing 30 parts by weight of polyol-1, 70 parts by weight of polyol 2, 4.35 parts by weight of blowing agent, 2.50 parts by weight of amine catalyst-1, 0.37 parts by weight of amine catalyst-2, 0.50 parts by weight of foam stabilizer, 1.85 parts by weight of additives, isocyanate ISO-1:ISO-2=100:0, isocyanate index 105, and EO rate of polyurethane foam 6.58% were used, and a skin material having the same composition as in Example 1 was used as the skin material.

[0075] The results of Comparative Example 2 were: thickness of the impregnated layer was 0.5 mm, the appearance of the polyurethane foam was "◎", the hardness of the soundproofing material at 50% compression was 1280 N, the evaluation was "◎", and the density of the polyurethane foam was 55 kg / m 3 The air permeability of the skin material including the impregnated layer is 2.61cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the soundproofing material was 34%, rated "x", the transmission loss of the soundproofing material was "Configuration A" 39.2 dB, rated "x", and the overall rating was "x". In Comparative Example 2, the isocyanate was 100% ISO1, so the EO ratio of the polyurethane foam was low at 6.58%, and the air permeability of the skin material including the impregnated layer was 2.61 cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the skin material including the impregnated layer and the polyurethane foam and the transmission loss of the soundproofing material were small, and the soundproofing (sound absorption) properties of the soundproofing material were inferior to those of Examples 1 to 3.

[0076] Comparative Example 3 is an example in which polyurethane foam raw materials containing 30 parts by weight of polyol-1, 70 parts by weight of polyol 2, 6.73 parts by weight of blowing agent, 3.13 parts by weight of amine catalyst-1, 0.51 parts by weight of amine catalyst-2, 0 part by weight of foam stabilizer, 25.46 parts by weight of additives, isocyanate ISO-1:ISO-2=0:100, isocyanate index 105, and EO rate of polyurethane foam 15.5% were used, and a skin material having the same composition as in Example 1 was used as the skin material.

[0077] The results of Comparative Example 3 were: thickness of the impregnated layer was 0.5 mm, the appearance of the polyurethane foam was "x", the hardness of the soundproofing material at 50% compression was 600 N, the evaluation was "△", and the density of the polyurethane foam was 55 kg / m 3 The air permeability of the skin material including the impregnated layer is 93cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the soundproofing material was 40%, rated "good", the transmission loss of the soundproofing material was "Configuration A" 42.2 dB, rated "good", and the overall rating was "x". In Comparative Example 3, the isocyanate was 100% ISO2, so the hardness of the soundproofing material was low, while the EO ratio of the polyurethane foam was high at 15.5%, and the air permeability of the skin material including the impregnated layer was 93 cc / cm 2 / sec, the reverberation chamber sound absorption coefficient of the skin material including the impregnated layer and the polyurethane foam and the transmission loss of the soundproofing material were small, and the soundproofing (sound absorption) properties of the soundproofing material were inferior to those of Examples 1 to 3.

[0078] In Comparative Example 4, felt was used instead of polyurethane foam and was laminated onto the second layer of the same skin material as in Example 1. The results of Comparative Example 4 are as follows: there is no impregnated layer of the skin material, the hardness of the soundproofing material when compressed by 50% is 62N, the evaluation is "x", and the density of the felt is 55kg / m 3 , the ventilation capacity of the skin is 106cc / cm 2 / sec, the reverberation chamber sound absorption rate of the soundproofing material was 84%, rated as "◎", the transmission loss of the soundproofing material was "Configuration A" 48.2 dB, rated as "◎", and the overall rating was "×". In Comparative Example 4, by using felt instead of polyurethane foam, the hardness of the soundproofing material became extremely small at 62 N, and it sunk greatly when pressed, so that when used as a floor silencer or the like, the feet of the occupant became embedded in the soundproofing material, making it difficult to move and making the posture unstable.

[0079] Thus, the soundproofing material of the present invention has high soundproofing (sound absorption) properties and is suitable not only for vehicle soundproofing materials such as vehicle floor silencers, but also for soundproofing materials for buildings, industrial machinery, home appliances, etc. [Explanation of symbols]

[0080] 10. Soundproofing materials 20 Polyurethane foam (sound absorbing material) 20a polyurethane foam raw material 30 Skin material (sound absorbing material) 31 First Layer 33 Second Layer 34 Impregnated layer 40 Mold 41 Lower mold 43 Upper mold 38 Release Agent

Claims

[Claim 1] In soundproofing materials in which a skin material is integrally molded onto one side of a polyurethane foam, A sample of 200 mm square x 20 mm thick is compressed to 80% of its thickness at a test speed of 50 mm / min using a compression tool of φ80 mm. The compression hardness is measured as the load at 50% compression and is 650 N or more. The polyurethane foam has an ethylene oxide content (EO rate) of 7 to 15%; A soundproofing material characterized by satisfying the following (1) and (2). (1) The reverberation chamber sound absorption coefficient measured based on JIS A1409 is 65% or more. (2) The transmission loss at 1600 Hz measured based on JIS A1441-1:2007 is 42.2 dB or more.

Citation Information

Patent Citations

  • Floor carpet for automobile

    JP1998071884A

  • Production of sound absorbing material

    JP1998119220A

  • Floor carpet for automobile

    JP1998329596A

  • Sound insulating material

    JP1999005499A

  • Vehicular seat pad and method for manufacturing the same

    JP2012228422A