Composition for producing polyimide film and polyimide film for flexible metal foil laminate produced using the same
A composition for polyimide film production using aromatic dianhydrides, diamines, and curing catalysts enhances flexibility and stability, addressing the limitations of existing polyimide films in flexible metal clad laminates, ensuring reliable adhesion and reduced repulsion for flexible printed circuit boards.
Patent Information
- Application Number
- JP2022539365
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-13
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2042-04-13
AI Technical Summary
Existing polyimide films used in flexible metal clad laminates have high structural dimensional stability and strong repulsion characteristics, leading to reduced flexibility and increased risk of joint failure when the bonding area is minimized.
A composition for producing a polyimide film containing aromatic dianhydrides, diamines, and curing catalysts such as imidazole, quinolone, and quinoline compounds, which improves flexibility, heat resistance, and dimensional stability, resulting in a polyimide film with low repulsion properties.
The polyimide film exhibits high flexibility, dimensional stability, and low repulsion, ensuring excellent adhesion even when the bonding area is reduced, making it suitable for applications in flexible printed circuit boards with minimized bezels.
Smart Images

Figure 0007587865000003 
Figure 0007587865000004 
Figure 0007587865000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition for producing a polyimide film and a polyimide film for flexible metal foil laminates produced using the same. [Background technology]
[0002] Flexible Printed Circuit Boards (FPCBs) are PCBs that are manufactured to be used when flexibility and a thin board are required. Recently, with the trend of electronic devices becoming smaller, faster, and combining various functions, there has been an increasing demand for faster transmission, lighter weight, thinner boards, and smaller boards. This has created a demand for technological development of FPCB materials that can meet this trend.
[0003] In the current display panel industry, various attempts are being made to minimize the bezel, one of which is to minimize the bezel by folding back the FPCB located at the edge of the display panel.
[0004] However, when using this method, the FPCB at the edge of the display panel is folded back, reducing the adhesion area, and the repulsive force of the circuit material can cause the joint to come off.
[0005] Figure 1 shows a diagram of a display bezel that is reduced by folding back the FPCB at the edge of the display panel. This shows that when folding back the FPCB at the edge of the panel in a display panel, the adhesive area of the FPCB is reduced, which may cause a problem that the joint may come off due to the repulsive force of the circuit material.
[0006] For these reasons, there is a demand for flexible metal clad laminate (FMCL) materials that are not only highly flexible but also have low resilience properties and can be smoothly adhered even when the adhesion area is minimized.
[0007] However, polyimide, which is generally the insulating layer material of soft metal thin laminates, has high structural dimensional stability while at the same time having strong repulsion properties, and there is a problem that if the repulsion properties are reduced, the dimensional stability also decreases.
[0008] Therefore, there is a need for a polyimide film manufacturing technique that can simultaneously improve high flexibility, low rebound properties, and dimensional stability. The above-mentioned background art is held or acquired by the inventors in the process of arriving at the contents of the disclosure of this specification, and is not necessarily publicly known art that was disclosed to the general public prior to the filing of this application. Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a composition for producing a polyimide film, which can improve all of the flexibility, heat resistance, dimensional stability, and rebound properties of a polyimide film, and a polyimide film and a flexible metal foil laminate produced using the same. However, the problems that the present invention aims to solve are not limited to those mentioned above, and further problems not mentioned will be clearly understood by those skilled in the art from the description below. [Means for solving the problem]
[0010] One aspect of the present invention provides a composition for producing a polyimide film, comprising an aromatic dianhydride, a diamine, and a curing catalyst, the curing catalyst comprising at least one selected from the group consisting of an imidazole-based compound, a quinolone-based compound, and a quinoline-based compound.
[0011] In one embodiment, the aromatic dianhydride can include one or more selected from the group consisting of pyromellitic dianhydride (PMDA), biphenyltetracarboxylic dianhydride (BPDA), bisphenol A dianhydride (BPADA), and 4,4'-(hexafluoropropylidene)diphthalic anhydride (6FDA).
[0012] In one embodiment, the diamine can include a first diamine including p-phenylenediamine (p-PDA), m-phenylenediamine (m-PDA), or two thereof; a second diamine including 4,4'-oxydianiline (ODA), 4,4'-methylenedianiline (MDA), or two thereof; and a tertiary diamine including 2-(4-aminophenyl)-5-amino-benzimidazole (PBI).
[0013] In one embodiment, the third diamine may be included in an amount of 1 mol % to 30 mol % based on the total content of the diamines.
[0014] In one embodiment, the diamine may be 10 parts by weight to 200 parts by weight based on 100 parts by weight of the aromatic dianhydride.
[0015] In one embodiment, the curing catalyst may be 5 parts by weight to 40 parts by weight based on 100 parts by weight of the total content of the aromatic dianhydride and the diamine.
[0016] In one embodiment, the imidazole-based compound may include one or more selected from the group consisting of imidazole, benzimidazole, 1-methylimidazole, 1-(trimethylsilyl)-imidazole, 1,2-dimethylimidazole, 1-(3-aminopropyl)-imidazole, 2-alkylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-undecylimidazole, and 3-phenylimidazole.
[0017] In one embodiment, the quinolone compound can include one or more selected from the group consisting of quinolone, 1,2-dihydro-2,2,4-trimethylquinolone, 2-chloro-3-(chloromethyl)quinolone, 4-(4-dimethylaminostyryl)quinolone, and 6-(aminomethyl)quinolone.
[0018] In one embodiment, the quinoline-based compound may include one or more selected from the group consisting of quinoline, isoquinoline, and benzoquinoline.
[0019] In an embodiment, the composition for preparing a polyimide film may have a solid content of 5% by weight to 20% by weight and a viscosity of 10,000 cP to 30,000 cP.
[0020] In another aspect of the present invention, there is provided a method for producing a composition for producing a polyimide film, the method comprising: preparing a diamine solution by dissolving a diamine in an organic solvent; and adding an aromatic dianhydride and a curing catalyst to the diamine solution, the curing catalyst including at least one selected from the group consisting of an imidazole-based compound, a quinolone-based compound, and a quinoline-based compound.
[0021] A further aspect of the present invention provides a polyimide film for flexible metal foil laminates, which is produced from a composition for producing a polyimide film, comprising an aromatic dianhydride, a diamine, and a curing catalyst, and has a Young's modulus of 5 GPa or less and a coefficient of thermal expansion (CTE) of 15 ppm / K or less.
[0022] In one embodiment, the polyimide film for flexible metal foil laminates may be bent 10,000 times or more in an MIT bending test using the JIS C6471 method with a coverlay attached.
[0023] In one embodiment, the polyimide film for flexible metal foil laminate has a dimensional change rate of 0.1% or less when measured after heat treatment at a temperature of 150° C. for 30 minutes, and the dimensional change rate can be calculated by the following Equation (1): [Formula(1)] Dimensional change rate (%) = {(average distance between holes after heat treatment - average distance between holes before heat treatment) / average distance between holes before heat treatment} x 100
[0024] In one embodiment, the polyimide film for flexible metal foil laminates may have a rigidity of 1.0 N / m to 1.7 N / m.
[0025] Another aspect of the present invention provides a flexible metal foil laminate comprising a metal foil and a polyimide film laminated on one or both sides of the metal foil.
[0026] In one embodiment, the metal foil may include one or more selected from the group consisting of rolled copper foil (RA, Roo-Annealed), electrolytic copper foil (ED, electrodeposition), aluminum foil, and nickel foil. Effect of the Invention
[0027] The composition for producing a polyimide film according to the present invention has the effect of improving the flexibility, heat resistance, dimensional stability, and rebound properties of a polyimide film. In addition, the polyimide film according to the present invention simultaneously has high flexibility, high dimensional stability, and low resilience, and therefore can ensure excellent adhesion even when the bonding area is reduced. Furthermore, the flexible metal foil laminate according to the present invention has the advantage that it is suitable for application to raw materials of FPCBs used to minimize bezels. [Brief description of the drawings]
[0028] [Figure 1]This is a diagram showing a configuration in which the display bezel is reduced by folding back the FPCB at the edge of the display panel. [Diagram 2] FIG. 2 is a diagram showing a cross section of a soft metal foil laminate according to one embodiment of the present invention. [Diagram 3] FIG. 13 is a diagram for explaining a specific method for calculating the dimensional change rate, and is a diagram showing the positions of each hole in a test piece. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] Hereinafter, the embodiments will be described in detail with reference to the accompanying drawings. However, various modifications can be made to the embodiments, and the scope of the patent application is not limited or restricted by the embodiments. All modifications, equivalents, or alternatives to the embodiments should be understood as being included in the scope of the patent.
[0030] The terms used in this specification are merely used to describe certain embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise. In this specification, the terms "include" or "have" indicate the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, and should be understood as not precluding the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0031] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Commonly used predefined terms should be interpreted as having a meaning consistent with the meaning they have in the context of the relevant art, and should not be interpreted as having an ideal or overly formal meaning unless expressly defined herein.
[0032] In addition, in the description with reference to the accompanying drawings, the same components are given the same reference numerals regardless of the reference numerals, and duplicated descriptions thereof will be omitted. In the description of the embodiments, if a detailed description of related known technology is determined to unnecessarily obscure the gist of the embodiments, the detailed description thereof will be omitted.
[0033] In addition, in describing components of the embodiments, terms such as first, second, A, B, (a), (b), etc. are used. Such terms are merely used to distinguish the components from other components, and do not limit the essence, order, or sequence of the corresponding components.
[0034] Components having a common function to those included in one embodiment will be described using the same names in other embodiments. Unless otherwise stated, the description of one embodiment will be applied to other embodiments, and detailed description will be omitted to the extent that they overlap.
[0035] One aspect of the present invention provides a composition for producing a polyimide film, comprising an aromatic dianhydride, a diamine, and a curing catalyst, the curing catalyst comprising at least one selected from the group consisting of an imidazole-based compound, a quinolone-based compound, and a quinoline-based compound.
[0036] The composition for producing a polyimide film according to the present invention contains an aromatic dianhydride, a diamine and a curing catalyst, and thus has the effect of improving the heat resistance, dimensional stability, flexibility and low resilience of the polyimide film.
[0037] The composition for producing a polyimide film according to the present invention contains an aromatic dianhydride.
[0038] The aromatic dianhydride has the characteristic of being able to improve the heat resistance and dimensional stability of the polyimide film.
[0039] In one embodiment, the aromatic dianhydride may include one or more selected from the group consisting of pyromellitic dianhydride (PMDA), biphenyltetracarboxylic dianhydride (BPDA), bisphenol A dianhydride (BPADA), and 4,4'-(hexafluoropropylidene)diphthalic anhydride (6FDA).
[0040] In one embodiment, the aromatic dianhydride can include a first aromatic dianhydride comprising pyromellitic dianhydride (PMDA) and a second aromatic dianhydride comprising biphenyltetracarboxylic dianhydride (BPDA).
[0041] In one embodiment, the amount of the second aromatic dianhydride may be 10 mol to 500 mol, preferably 40 mol to 400 mol, relative to 100 mol of the first aromatic dianhydride.
[0042] In one embodiment, the molar ratio of the first aromatic dianhydride to the second aromatic dianhydride may be 9:1 to 1:9, preferably 8:2 to 2:8, and more preferably 7:3 to 3:7.
[0043] In one embodiment, the composition for producing a polyimide film contains two or more aromatic dianhydrides in a certain molar ratio, thereby more effectively improving the heat resistance and dimensional stability of the polyimide film.
[0044] The composition for producing a polyimide film according to the present invention contains a diamine. The diamine has the characteristic of being able to improve the flexibility, low resilience, and dimensional stability of the polyimide film.
[0045] In one embodiment, the diamine can include a first diamine including p-phenylenediamine (p-PDA), m-phenylenediamine (m-PDA), or two thereof; a second diamine including 4,4'-oxydianiline (ODA), 4,4'-methylenedianiline (MDA), or two thereof; and a tertiary diamine including 2-(4-aminophenyl)-5-amino-benzimidazole (PBI).
[0046] In one embodiment, the third diamine may be present in an amount of 1 mol % to 30 mol % based on the total content of the diamine. Preferably, the third diamine may be present in an amount of 5 mol % to 20 mol % based on the total content of the diamines, and more preferably, in an amount of 5 mol % to 15 mol %. The third diamine includes an imidazole-based diamine and acts as a key element for improving the low resilience and dimensional stability of the polyimide film. If the content of the tertiary diamine is less than the above range, the coefficient of thermal expansion (CTE) increases and the dimensional stability decreases. If the content exceeds the above range, the coefficient of thermal expansion (CTE) decreases too much, and the difference in the coefficient of thermal expansion with the metal foil increases, which may decrease the dimensional stability.
[0047] In one embodiment, the diamine may include 10 mol to 50 mol of the second diamine and 1 mol to 30 mol of the third diamine with respect to 100 mol of the first diamine. Preferably, the diamine may include 10 to 40 moles of the second diamine and 5 to 30 moles of the third diamine relative to 100 moles of the first diamine. More preferably, the diamine may include 20 to 40 moles of the second diamine and 10 to 20 moles of the third diamine relative to 100 moles of the first diamine.
[0048] In one embodiment, the diamine may have a molar ratio of the first diamine to the second diamine of 9:1 to 1:1, preferably 8:1 to 7:2.
[0049] In one embodiment, the diamine may have a molar ratio of the first diamine to the third diamine of 9:1 to 1:1, preferably 9:1 to 7:1.
[0050] In one embodiment, the diamine may have a molar ratio of the second diamine to the third diamine of 3:1 to 1:1, preferably 3:1 to 2:1.
[0051] In one embodiment, the composition for producing a polyimide film contains three or more diamines in a certain molar ratio, which has the effect of simultaneously improving the low resilience, flexibility, and dimensional stability of the polyimide film.
[0052] In one embodiment, the diamine is 2-(4-aminophenyl)benzo[di]oxazol-5-amine (PBO), 2,5-diaminotoluene, 2,6-diaminotoluene, 1,3-bis(4,4'-aminophenoxy)benzene, 4,4'-diamino-1,5-phenoxypentane, 4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane, 2,2'-diaminodiphenylpropane, bis(3,5-diethyl-4-aminophenyl)methane, diaminodiphenyl sulfone, diaminobenzophenone, diaminonaphthalene, 1,4-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenyl)benzene , 9,10-bis(4-aminophenyl)anthracene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)diphenylsulfone, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2'-trifluoromethyl-4,4'-diaminobiphenyl, 1,4-diaminocyclohexane, 1,4-cyclohexanebis(methylamine), 4,4'-diaminodicyclohexylmethane (MCA), 4,4'-methylenebis(2-methylcyclohexylamine) (MMCA), ethylenediamine (EN), 1,3-diaminopropane (13DAP), tetramethylenediamine, 1,6-hexamethylenediamine (16DAH) and 1,12-diaminododecane (112DAD).
[0053] In one embodiment, the diamine may be 10 parts by weight to 200 parts by weight based on 100 parts by weight of the aromatic dianhydride.
[0054] Preferably, the diamine may be 50 parts by weight to 150 parts by weight relative to 100 parts by weight of the aromatic dianhydride, more preferably, the diamine may be 80 parts by weight to 120 parts by weight relative to 100 parts by weight of the aromatic dianhydride, and even more preferably, the diamine may be 100 parts by weight relative to 100 parts by weight of the aromatic dianhydride, that is, the aromatic dianhydride and the diamine may be contained in a ratio of 1:1.
[0055] In one embodiment, the content ratio of the aromatic dianhydride to the diamine may be 1:10 to 10:1, preferably 1:5 to 5:1, and more preferably 1:2 to 2:1.
[0056] The composition for producing a polyimide film according to the present invention contains a curing catalyst including one or more compounds selected from the group consisting of imidazole-based compounds, quinolone-based compounds, and quinoline-based compounds. The curing catalyst can reduce the resilience of the polyimide film and improve the bending resistance and dimensional stability.
[0057] In one embodiment, the curing catalyst may be 5 parts by weight to 40 parts by weight based on 100 parts by weight of the total content of the aromatic dianhydride and the diamine. Preferably, the content may be 5 parts by weight to 30 parts by weight relative to 100 parts by weight of the total content of the aromatic dianhydride and the diamine. Here, the total content is the sum of the content of the aromatic dianhydride and the content of the diamine. If the content of the curing catalyst is less than the above range, the tensile strength and dimensional stability are decreased and the rebound characteristics are increased. On the other hand, if the content of the curing catalyst exceeds the above range, bending resistance may decrease. In particular, the content of the curing catalyst is a key factor in controlling the physical properties of the polyimide film.
[0058] In one embodiment, the imidazole-based compound may include one or more selected from the group consisting of imidazole, benzimidazole, 1-methylimidazole, 1-(trimethylsilyl)-imidazole, 1,2-dimethylimidazole, 1-(3-aminopropyl)-imidazole, 2-alkylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-undecylimidazole, and 3-phenylimidazole.
[0059] In one embodiment, the quinolone compound can include one or more selected from the group consisting of quinolone, 1,2-dihydro-2,2,4-trimethylquinolone, 2-chloro-3-(chloromethyl)quinolone, 4-(4-dimethylaminostyryl)quinolone, and 6-(aminomethyl)quinolone.
[0060] In one embodiment, the quinoline-based compound may include one or more selected from the group consisting of quinoline, isoquinoline, and benzoquinoline.
[0061] In an embodiment, the composition for preparing a polyimide film may have a solid content of 5% by weight to 20% by weight and a viscosity of 10,000 cP to 30,000 cP. Preferably, the composition for producing a polyimide film may have a solid content of 8% by weight to 15% by weight. The above solid content range is a solid content range when the composition for preparing a polyimide film is a polyamic acid, and takes into consideration a molecular weight (degree of polymerization) appropriate for forming a polyimide film and workability (viscosity) when coating one side of a metal foil. The composition for producing a polyimide film may have a viscosity of 10,000 cP to 30,000 cP, which is determined in consideration of workability during coating. If the viscosity of the composition for preparing a polyimide film is less than the above range, the solution may flow onto one side of a metal foil during coating, whereas if the viscosity exceeds the above range, the solution may solidify during coating, resulting in an uneven coating of the surface.
[0062] The composition for producing a polyimide film according to the present invention may further include an organic solvent. In one embodiment, the organic solvent may include one or more selected from the group consisting of N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethylsulfoxide (DMSO), tetrahydrofuran (TFH), benzene, cresol, hexane, cyclohexane, chloroform, phenol, and halogenated phenols. Preferably, the organic solvent may include one or more selected from the group consisting of N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), and dimethyl sulfoxide (DMSO).
[0063] In another aspect of the present invention, there is provided a method for preparing a composition for producing a polyimide film, the method comprising: preparing a diamine solution by dissolving a diamine in an organic solvent; and adding an aromatic dianhydride and a curing catalyst to the diamine solution, the curing catalyst including at least one selected from the group consisting of an imidazole-based compound, a quinolone-based compound, and a quinoline-based compound. Here, the characteristics of the organic solvent, the diamine, the aromatic dianhydride, and the curing catalyst are the same as those described above.
[0064] A further aspect of the present invention provides a polyimide film for flexible metal foil laminates, which is produced from a composition for producing a polyimide film, comprising an aromatic dianhydride, a diamine, and a curing catalyst, and has a Young's modulus of 5 GPa or less and a coefficient of thermal expansion (CTE) of 15 ppm / K or less.
[0065] The polyimide film according to the present invention can have low stiffness and high flexibility by controlling the Young's modulus to 5 GPa or less, which also has an effect of increasing the MIT flexibility.
[0066] The polyimide film according to the present invention can improve the dimensional stability of a soft metal foil laminate by controlling the coefficient of thermal expansion (CTE) to 15 ppm / K or less. The coefficient of thermal expansion (CTE) was measured in the temperature range of 100°C to 250°C based on a film having a thickness of 20 μm.
[0067] In one embodiment, the polyimide film for flexible metal foil laminates has a bending resistance of 10,000 or more times in an MIT bending test using the JIS C6471 method with a coverlay attached. In one embodiment, the number of flexions may be 13,000 or more. The polyimide film for flexible metal foil laminates according to the present invention is characterized by excellent MIT bending property, that is, excellent bending resistance. The coverlay was composed of 12.5 μm thick polyimide and 15 μm thick adhesive. This is to replicate the Flexible Printed Circuit Board (FPCB) and reduce test deviations.
[0068] In one embodiment, the polyimide film for flexible metal foil laminates has a dimensional change rate of 0.1% or less measured after heat treatment at a temperature of 150° C. for 30 minutes, and the dimensional change rate is calculated by the following mathematical formula (1): [Formula(1)] Dimensional change rate (%) = {(average distance between holes after heat treatment - average distance between holes before heat treatment) / average distance between holes before heat treatment} x 100 The dimensional change rate includes both the dimensional change rate in the MD direction and the dimensional change rate in the TD direction.
[0069] In one embodiment, the dimensional change rate in the MD may be 0.06% or less, and the dimensional change rate in the TD may be 0.05% or less.
[0070] In one embodiment, the polyimide film for flexible metal foil laminates may have a rigidity of 1.0 N / m to 1.7 N / m. Preferably, the rigidity of the silver polyimide film for soft metal foil laminate may be 1.4 N / m to 1.7 N / m. The polyimide film for flexible metal foil laminates according to the present invention is characterized by having low stiffness, and therefore low resilience and modulus.
[0071] The polyimide film for flexible metal foil laminates according to the present invention has reduced resilience while maintaining excellent dimensional stability, and is therefore capable of retaining its adhesive properties even when it is deformed in response to various demands and its contact area with other materials is reduced. For example, even if the area of the display terminal portion is reduced for various reasons and the FPCB bonding area at the edge of the display panel is reduced, the adhesive portion can be prevented from falling off by reducing the repulsion properties of the polyimide film layer.
[0072] Another aspect of the present invention provides a flexible metal foil laminate comprising a metal foil and the polyimide film laminated on one or both sides of the metal foil. FIG. 2 is a diagram showing a cross section of a soft metal foil laminate according to one embodiment of the present invention. Referring to FIG. 2, it can be seen that a polyimide film layer is formed by coating one or both sides of a metal foil with a composition for preparing a polyimide once or a plurality of times.
[0073] According to an embodiment, the polyimide film may be laminated by coating one or both sides of the metal foil with the composition for preparing a polyimide film according to the present invention. The coating may be performed by slot die coating, comma coating, reverse comma coating, cast coating, or dip coating. The coating may be performed multiple times, and a drying process may be performed after the coating. The drying is performed at a temperature range of 100°C to 200°C for 1 to 20 minutes, and the maximum temperature is maintained for 1 to 8 minutes, followed by cooling.
[0074] According to one embodiment, the polyimide film may be cured after coating. The curing may be carried out in a nitrogen atmosphere at a temperature range of 300°C to 400°C for 5 to 60 minutes, and is held at the maximum temperature for 1 to 15 minutes, followed by cooling. Here, the maximum temperature is reached by increasing the temperature for 5 to 30 minutes.
[0075] In one embodiment, the metal foil may include one or more selected from the group consisting of rolled copper foil (RA, Roo-Annealed), electrolytic copper foil (ED, electrodeposition), aluminum foil, and nickel foil.
[0076] As an example, the flexible metal foil laminate may be a flexible copper foil laminate (FCCL).
[0077] In one embodiment, the polyimide film may have a thickness of 5 μm to 100 μm.
[0078] The present invention will be described in more detail below with reference to examples and comparative examples. However, the following examples are merely for the purpose of illustrating the present invention, and the contents of the present invention are not limited to the following examples.
[0079] <Examples> Composition for producing polyimide film and production of soft metal foil laminate 1) Production of compositions for producing polyimide films A diamine was dissolved in an organic solvent, and then an aromatic dianhydride and a curing catalyst were mixed therewith to prepare a composition for producing a polyimide film. 2) Manufacturing of soft metal foil laminates The prepared composition for producing a polyimide film was applied to one side of a metal foil and dried at a temperature range of 100° C. to 200° C. for 10 to 20 minutes. Thereafter, the dried laminate was cured at a temperature range of 300°C to 400°C in a continuous curing device using an infrared heat supply system. Here, nitrogen was supplied into the hardener, and the temperature was raised to 300°C to 400°C at room temperature within 30 minutes, and the maximum temperature was maintained within 10 minutes, after which cooling was carried out. The polyimide film was formed to a thickness of 7.5 μm to 50 μm.
[0080] <Comparative Example> Composition for Producing Polyimide Film and Production of Soft Metal Foil Laminate A composition for producing a polyimide film and a flexible metal foil laminate were produced in the same manner as in the Examples, except that no curing catalyst was used in producing the composition for producing a polyimide film, and only one dianhydride and two diamines were used.
[0081] Specific component configurations of the examples and comparative examples are shown in Table 1. [Table 1]
[0082] <Test Example> Measurement of physical properties of polyimide film In the flexible metal foil laminates manufactured in Examples 1 to 6 and Comparative Examples 1 and 2, the metal was etched with a ferric chloride solution, washed with distilled water, and the polyimide film was separated. The physical properties of the separated polyimide film were measured by the following method. 1) Tensile strength Using a UTM (INSTRON-3345), the polyimide film was cut to a width of 10 mm and a length of 100 mm (effective measurement range 50 mm) and measured at a speed of 50.8 mm / min. 2) Resilience Using a Loop Stiffness Tester (TOYOSEKI-DA), a test piece of 12.5μm thick polyimide film cut to a width of 15mm and a length of over 100mm was fixed to the measurement table. The length of the test piece actually measured was 50mm, and the width when formed into a loop shape was 20mm. The measurement was performed with a force detector of 13mm. 3) Coefficient of Thermal Expansion (CTE) Using a TMA (HITACHI-7100), a 20μm thick polyimide film was cut into a width of 4mm and a length of 50mm, and a tension of 30mN was applied to measure the thermal expansion coefficient in the range of 100℃~250℃. 4) MIT flexibility Measured using MIT-DA (TOYOSEKI) according to JIS 6471 method. Coverlay (PI-12.5μm, Adhesive-15μm) was attached and measured using MIT measuring equipment. Repeated bending at 90° or 135° was performed to measure the number of bending times until the pattern broke. The coverlay was applied during the measurement to replicate the flexible printed circuit board (FPCB) and reduce the test deviation. 5) Dimensional stability A 290 x 270 mm FCCL was fully etched and naturally dried, then stored at 23°C / 50% RH for 2 hours, and the distance between the holes was measured. The holes penetrated from the center of the specimen to the apex of the 250 x 230 mm. After heating at 150°C for 30 minutes, the specimen was stored at 23°C / 50% RH for 2 hours, and the distance between the holes was measured.
[0083] FIG. 3 is used to explain a specific method for calculating the dimensional change rate, and shows the positions of each hole in the test piece. The dimensional change rate (Heating DS) was calculated by the following formula. Dimensional change rate in MD direction (%) = (L M2 -L M ) / L M ×100 Dimensional change rate in TD direction (%) = (L T2 -L T ) / L T ×100 L M = (distance between holes A and B + distance between holes C and D) / 2 L T = (distance between holes A and C + distance between holes B and D) / 2 L M : Average hole distance in the MD direction of the disk L M1 : Average hole distance in MD after etching L M2 : Average hole distance in MD after heating L T : Average hole distance in the master TD direction L T1 : Average hole distance in TD after etching L T2 : Average hole distance in TD direction after heating
[0084] The evaluated physical properties are shown in Table 2. [Table 2]
[0085] Referring to Table 2, it can be seen that the polyimide films of the Examples are superior in MIT flexibility, dimensional stability, and heat resistance, and exhibit low resilience properties, as compared with the polyimide films of the Comparative Examples. Specifically, the polyimide film of the example exhibited excellent bending resistance, being bent 13,000 times or more in the MIT bending test after the attachment of the coverlay. In addition, the Young's modulus was shown to be about 4.5 GPa to 5 GPa, and the coefficient of linear thermal expansion (CTE) measured in the range of 100°C to 250°C was shown to be about 12 ppm / k to 15 ppm / k. According to the results of the resilience test, it is confirmed that the polyimide films of the examples have a stiffness of 1.7 N / m or less, which is lower than that of the polyimide films of the comparative examples. That is, it was confirmed that the polyimide films of the examples exhibited low stiffness and thus low resilience, which indicates that they have low modulus characteristics.
[0086] Although the embodiments of the present invention have been described in detail above with reference to the drawings, the present invention is not limited to the above-described embodiments, and various technical modifications and variations can be applied based on the above if one has ordinary knowledge in the art. For example, the described techniques can be performed in a different order from the described method, and / or the components of the described system, structure, device, circuit, etc. can be combined in a different form from the described method, or replaced or substituted with other components or equivalents to achieve appropriate results. Accordingly, other implementations, other embodiments, and equivalents of the claims are within the scope of the following claims.
Claims
1. An aromatic dianhydride, Diamine, A curing catalyst; Including, The curing catalyst includes at least one selected from the group consisting of an imidazole-based compound, a quinolone-based compound, and a quinoline-based compound; The curing catalyst is in an amount of 5 to 40 parts by weight based on 100 parts by weight of the total content of the aromatic dianhydride and the diamine; The diamine comprises a tertiary diamine comprising 2-(4-aminophenyl)-5-amino-benzimidazole (PBI); The composition for preparing a polyimide film, wherein the tertiary diamine is included in an amount of 1 mol % to 30 mol % based on the total content of the diamines.
2. 2. The composition for producing a polyimide film according to claim 1, wherein the aromatic dianhydride comprises one or more selected from the group consisting of pyromellitic dianhydride (PMDA), biphenyltetracarboxylic dianhydride (BPDA), bisphenol A dianhydride (BPADA), and 4,4'-(hexafluoropropylidene)diphthalic anhydride (6FDA).
3. The diamine is a primary diamine comprising p-phenylenediamine (p-PDA), m-phenylenediamine (m-PDA), or both; a secondary diamine comprising 4,4'-oxydianiline (ODA), 4,4'-methylenedianiline (MDA), or both of them; The composition for producing a polyimide film according to claim 1 , further comprising:
4. 2. The composition for producing a polyimide film according to claim 1, wherein the diamine is contained in an amount of 10 to 200 parts by weight based on 100 parts by weight of the aromatic dianhydride.
5. 2. The composition for producing a polyimide film according to claim 1, wherein the imidazole-based compound comprises at least one selected from the group consisting of imidazole, benzimidazole, 1-methylimidazole, 1-(trimethylsilyl)-imidazole, 1,2-dimethylimidazole, 1-(3-aminopropyl)-imidazole, 2-alkylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-undecylimidazole, and 3-phenylimidazole.
6. 2. The composition for producing a polyimide film according to claim 1, wherein the quinolone compound comprises at least one selected from the group consisting of quinolone, 1,2-dihydro-2,2,4-trimethylquinolone, 2-chloro-3-(chloromethyl)quinolone, 4-(4-dimethylaminostyryl)quinolone, and 6-(aminomethyl)quinolone.
7. The composition for producing a polyimide film according to claim 1 , wherein the quinoline-based compound comprises at least one selected from the group consisting of quinoline, isoquinoline, and benzoquinoline.
8. The solid content is 5% to 20% by weight, The composition for producing a polyimide film according to claim 1, having a viscosity of 10,000 cP to 30,000 cP.
9. preparing a diamine solution by dissolving a diamine in an organic solvent; adding an aromatic dianhydride and a curing catalyst to the diamine solution; Including, 2. The method for producing a composition for producing a polyimide film according to claim 1, wherein the curing catalyst comprises at least one selected from the group consisting of imidazole-based compounds, quinolone-based compounds, and quinoline-based compounds.
10. A polyimide film produced from the composition for producing a polyimide film according to claim 1, A polyimide film for flexible metal foil laminates having a Young's modulus of 5 GPa or less and a coefficient of thermal expansion (CTE) of 15 ppm / K or less.
11. The polyimide film for flexible metal foil laminates according to claim 10, wherein the polyimide film for flexible metal foil laminates has a bending number of 10,000 or more in an MIT bending test using a JIS C6471 method with a coverlay attached.
12. 11. The polyimide film for flexible metal foil laminates according to claim 10, wherein the dimensional change rate measured after heat treatment at a temperature of 150° C. for 30 minutes is 0.1% or less, and the dimensional change rate is calculated by the following Equation (1): [Formula (1)] Dimensional change rate (%)={(average distance between holes after heat treatment−average distance between holes before heat treatment) / average distance between holes before heat treatment}×100
13. The polyimide film for flexible metal foil laminates according to claim 10, having a rigidity of 1.0 N / m to 1.7 N / m.
14. Metal foil; A polyimide film laminated on one or both sides of the metal foil; Including, The flexible metal foil laminate, wherein the polyimide film is the polyimide film according to claim 10.
15. The metal foil is selected from the group consisting of rolled copper foil (RA, Roo-Annealed), electrolytic copper foil (ED, electrodeposition), aluminum foil, and nickel foil. The flexible metal foil laminate according to claim 14.
Citation Information
Patent Citations
Colorless transparent polyimide film containing fluorine and Cardo structure and preparation method thereof
CN110606949A
Novel polyimide copolymer and metal laminate comprising the same
WO2004018545A1
Resin composition for printed circuit board
WO2012121164A1