Thin film forming method and memory device manufacturing method including the same
Patent Information
- Application Number
- JP2023078214
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-04-14
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-05-10
AI Technical Summary
【0043】 本発明の一実施形態によれば,ギャップフィーチャ上に底部から上方に充填されるSi又はMetal含有膜を形成することができ,サイクル毎に工程条件を調節したり,プラズマや化学的改質などの表面改質がなくても,一般的なALDを介して上部と下部の他の蒸着厚さを実現できるだけでなく,欠陥のないギャップフィルを達成して電気的特性を改善することができる。
Smart Images

Figure 0007587873000041 
Figure 0007587873000042 
Figure 0007587873000043
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for forming a thin film and a method for manufacturing a memory element including the same, and more particularly to a method for forming a thin film using an additive precursor, which is excellent in safety, and a method for manufacturing a memory element including the same. [Background technology]
[0002] Atomic layer deposition (ALD) is used as a process to fill gap features such as trenches formed in a substrate. Because atomic layer deposition utilizes surface reactions, when filling gap features using atomic layer deposition, uniform thickness can be formed and void formation can be minimized.
[0003] However, as the gap feature changes to a high aspect ratio, the size of the gap entrance may be smaller than the size of the gap interior, and the narrowing of the gap entrance may prevent sufficient diffusion of reactants to the bottom of the high aspect ratio feature.
[0004] Additionally, poor diffusion results in a deposition profile that has decreasing coverage on the sidewalls of the feature as the depth increases. Additionally, the use of atomic layer deposition can result in defects such as voids or seams, as well as the formation of films that are more porous than desired.
[0005] Furthermore, ALD for gap-filling can be repeated hundreds of times to achieve a target film thickness, which can be a disadvantage in terms of yield. Therefore, for high aspect ratio gap features, it is advantageous to have a higher growth rate at the bottom than at the top, and various growth suppression techniques have been developed for this purpose. Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a thin film formation method capable of minimizing the occurrence of defects and ensuring high production volume, and a memory element manufacturing method including the same.
[0007] Other objects of the present invention will become more apparent from the following detailed description. [Means for solving the problem]
[0008] According to one embodiment of the present invention, a method for forming a thin film using an additive precursor includes an additive precursor supplying step of supplying an additive precursor into a chamber in which a substrate having one or more gap features is placed, thereby adsorbing the additive precursor onto the substrate; a step of purging the interior of the chamber; and a thin film forming step of supplying a reactant into the chamber to react with the adsorbed additive precursor to form a thin film to fill the gap features, wherein the additive precursor is formed by mixing 1 to 5 moles of a compound represented by the following <Chemical Formula 1> or the following <Chemical Formula 2> with 1 to 5 moles of a metal compound.
[0009] [ka] In the above <Chemical Formula 1>, X is O or S, and R1 and R2 are each independently selected from an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms.
[0010] [ka] In the above <Chemical Formula 2>, X is O or S, n = 1 to 5, and R1 to R4 are each independently selected from a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms.
[0011] The adduct precursor may be formed by mixing ethyl methyl sulfide or ethyl propyl ether or tetrahydrofuran with the metal compound.
[0012] The metal compound may have at least one Group 4 element, including Zr, Hf, and Ti, as a central element.
[0013] The metal compound can be represented by the following <Chemical Formula 3>.
[0014] [ka] M is selected from the metal elements in group 4 of the periodic table, L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
[0015] The metal compound can be represented by the following <Chemical Formula 4>.
[0016] [ka] M is selected from the metal elements in group 4 of the periodic table, R1, R2, R3, R4, and R5 are each independently selected from a hydrogen atom, a linear, branched, or cyclic alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, and a phenyl group having 6 to 12 carbon atoms; L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an aralkyl group having 7 to 13 carbon atoms; When L is a dialkylamino group, they can be linked together to form a cyclic amine group having 3 to 10 carbon atoms.
[0017] The metal compound may have at least one of the Group 5 elements including Nb and Ta as a central element.
[0018] The metal compound may be represented by the following <Chemical Formula 5> or <Chemical Formula 6>.
[0019] [ka] [ka] M is selected from the metal elements in group 5 of the periodic table, L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
[0020] The metal compound can be represented by the following <Chemical Formula 7>.
[0021] [ka] M is selected from the metal elements in group 5 of the periodic table, R1, R2, and R3 are each independently selected from a hydrogen atom and a linear / branched / cyclic alkyl group having 1 to 5 carbon atoms; L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
[0022] The metal compound may have at least one of the Group 6 elements, including W and Mo, as a central element.
[0023] The metal compound may be represented by the following <Chemical Formula 8> or <Chemical Formula 9>.
[0024] [ka] [ka] M is selected from the metal elements in group 6 of the periodic table, L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
[0025] The metal compound may have at least one of the Group 13 elements, including Al, as a central element.
[0026] The metal compound can be represented by the following <Chemical Formula 10>.
[0027] [ka] M is selected from the metal elements in group 13 of the periodic table, L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
[0028] According to another embodiment of the present invention, a method for forming a thin film using an additive precursor includes an additive precursor supplying step of supplying an additive precursor into a chamber in which a substrate having one or more gap features is placed, thereby adsorbing the additive precursor onto the substrate; a step of purging the interior of the chamber; and a thin film forming step of supplying a reactant into the chamber to react with the adsorbed additive precursor to form a thin film to fill the gap features, wherein the additive precursor is formed by mixing 1 to 5 moles of a compound represented by the following <Chemical Formula 1> or the following <Chemical Formula 2> with 1 to 5 moles of a non-metallic compound.
[0029] [ka] In the above <Chemical Formula 1>, X is O or S, and R1 and R2 are each independently selected from an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms.
[0030] [ka] In the above <Chemical Formula 2>, X is O or S, n = 1 to 5, and R1 to R4 are each independently selected from a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms.
[0031] The adduct precursor may be formed by mixing ethyl methyl sulfide or ethyl propyl ether or tetrahydrofuran with the non-metallic compound.
[0032] The nonmetallic compound may have at least one of the Group 14 elements, including Si and Ge, as a central element.
[0033] The non-metallic compound may be represented by the following <Chemical Formula 11>.
[0034] [ka] In the above <Chemical Formula 11>, M is one of the group 14 elements including Si and Ge, R1 to R4 are each independently selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkylamine group having 1 to 10 carbon atoms, a dialkylamine group having 1 to 10 carbon atoms, an arylamine group having 6 to 12 carbon atoms, an aralkylamine group having 7 to 13 carbon atoms, a cyclic amine group having 3 to 10 carbon atoms, a heterocyclic amine group having 3 to 10 carbon atoms, a heteroarylamine group having 6 to 12 carbon atoms, an alkylsilylamine group having 2 to 10 carbon atoms, an azide group, or a halogen.
[0035] The non-metallic compound may be represented by the following <Chemical Formula 12>.
[0036] [ka] In the above <Chemical Formula 12>, M is one of the group 14 elements including Si and Ge, R1 to R6 are each independently selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkylamine group having 1 to 10 carbon atoms, a dialkylamine group having 1 to 10 carbon atoms, an arylamine group having 6 to 12 carbon atoms, an aralkylamine group having 7 to 13 carbon atoms, a cyclic amine group having 3 to 10 carbon atoms, a heterocyclic amine group having 3 to 10 carbon atoms, a heteroarylamine group having 6 to 12 carbon atoms, an alkylsilylamine group having 2 to 10 carbon atoms, an azide group, or a halogen.
[0037] The thin film can be either a metal oxide, a metal nitride, a metal sulfide or a metal.
[0038] The thin film can be either a non-metal oxide, a non-metal nitride, a non-metal sulfide, or a non-metal.
[0039] The thin film formation method can proceed at a temperature equal to or higher than the dissociation temperature of the adduct precursor.
[0040] The thin film formation method can proceed at a temperature of 50 to 700°C.
[0041] According to an embodiment of the present invention, a method for manufacturing a volatile memory device may include the thin film forming method.
[0042] According to an embodiment of the present invention, a method for manufacturing a non-volatile memory device may include the thin film forming method. Effect of the Invention
[0043] According to one embodiment of the present invention, a Si- or Metal-containing film can be formed on a gap feature that fills from the bottom up, and different top and bottom deposition thicknesses can be achieved through conventional ALD without adjusting process conditions for each cycle or surface modification such as plasma or chemical modification, as well as achieving defect-free gap fill and improving electrical properties. [Brief description of the drawings]
[0044] [Figure 1] FIG. 1 is a schematic diagram illustrating a cross-sectional view of a substrate having a gap feature. [Diagram 2] 1 is a 1H-NMR graph of the precursor TMA-EMS according to Example 1 of the present invention. [Diagram 3] 2 is a graph showing differential scanning calorimetry (DSC) test results and thermogravimetric analysis (TGA) test results for Example 1. [Figure 4] 2 is a graph showing differential scanning calorimetry (DSC) test results and thermogravimetric analysis (TGA) test results for Example 1. [Diagram 5] 1 is a graph showing GPC (Growth Per Cycle) of aluminum oxide films according to Comparative Example 1 and Example 1 of the present invention as a function of process temperature. [Figure 6] The aluminum oxide film according to Comparative Example 1 of the present invention was deposited on a patterned wafer at a process temperature of 400° C., and the step coverage was confirmed (aspect ratio: 20:1). [Figure 7]The aluminum oxide film according to Example 1 of the present invention was deposited on a patterned wafer at a process temperature of 400° C., and the step coverage was confirmed (aspect ratio: 20:1). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0045] Preferred embodiments of the present invention will now be described in more detail with reference to the accompanying Figures 1 to 6. The embodiments of the present invention may be modified in various forms, and the scope of the present invention should not be construed as being limited to the embodiments described below. These embodiments are provided to explain the present invention in more detail to those skilled in the art to which the invention pertains. Therefore, the shape of each element shown in the drawings may be exaggerated to emphasize a clearer description.
[0046] The precursor according to an embodiment of the present invention exists in a stable adduct state by combining with an organic substance at room temperature and pressure, but is dissociated before being adsorbed onto the surface of a substrate by thermal energy, collision, etc. in a chamber.
[0047] In addition, the adsorption density decreases at the top of the gap feature due to the increased size and blocking effect, which reduces the reactivity of the precursor, while at the bottom of the gap feature, the organic matter is dissociated and removed, and the metal and nonmetallic compounds themselves are adsorbed, increasing the adsorption density. In particular, the deposition thickness increases, enabling bottom-up filling.
[0048] In addition, different GPCs are deposited at the top and bottom depending on the depth of the gap feature, which can achieve defect-free gap filling even in high aspect ratio structures.
[0049] According to an embodiment of the present invention, a method for forming a thin film includes a step of supplying an additive precursor into a chamber in which a substrate is placed, a step of purging the inside of the chamber, and a step of forming a thin film by supplying a reactant into the chamber and reacting the reactant with the additive precursor to form a thin film, wherein the precursor supplying step and the thin film forming step are performed at a temperature of 50 to 700°C.
[0050] The substrate has one or more gap features. A gap feature can refer to an opening or cavity disposed between one or more sloping sides of a non-planar surface. A gap feature can refer to an opening or cavity disposed between opposing sloping sidewalls of two protrusions that extend perpendicularly from the surface of the substrate. A gap feature can refer to an opening or cavity disposed between one or more opposing sloping sidewalls of a recess that extends perpendicularly from the surface of the substrate.
[0051] 1 is a schematic diagram illustrating a cross-sectional view of a substrate having gap features. At least one gap feature 210 forms an opening in a substrate surface 220. The gap feature 210 extends from the substrate surface 220 to a depth D to a bottom surface 212. The gap feature 210 has a first sidewall 214 and a second sidewall 216 that define a width W of the gap feature 210. The open area formed by the sidewalls and the bottom surface is also referred to as a gap.
[0052] The substrate is exposed to an adduct precursor provided inside the chamber, and the adduct precursor is adsorbed into the gap features of the substrate.
[0053] According to one embodiment of the present invention, the adduct precursor is formed by mixing 1 to 5 moles of a compound represented by the following <Chemical Formula 1> or the following <Chemical Formula 2> and 1 to 5 moles of a metal compound.
[0054] [ka] In the above <Chemical Formula 1>, X is O or S, and R1 and R2 are each independently selected from an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms.
[0055] [ka] In the above <Chemical Formula 2>, X is O or S, n = 1 to 5, and R1 to R4 are each independently selected from a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms.
[0056] The adduct precursor may be formed by mixing ethyl methyl sulfide or ethyl propyl ether or tetrahydrofuran with the metal compound.
[0057] The metal compound may have at least one Group 4 element, including Zr, Hf, and Ti, as a central element.
[0058] The metal compound can be represented by the following <Chemical Formula 3>.
[0059] [ka] M is selected from the metal elements in group 4 of the periodic table, L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
[0060] The metal compound can be represented by the following <Chemical Formula 4>.
[0061] [ka] M is selected from the metal elements in group 4 of the periodic table, R1, R2, R3, R4, and R5 are each independently selected from a hydrogen atom, a linear, branched, or cyclic alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, and a phenyl group having 6 to 12 carbon atoms; L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, and an aralkyl group having 7 to 13 carbon atoms; When L is a dialkylamino group, they can be linked together to form a cyclic amine group having 3 to 10 carbon atoms.
[0062] The metal compound may have at least one of the Group 5 elements including Nb and Ta as a central element.
[0063] The metal compound may be represented by the following <Chemical Formula 5> or <Chemical Formula 6>.
[0064] [ka] [ka] M is selected from the metal elements in group 5 of the periodic table, L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
[0065] The metal compound can be represented by the following <Chemical Formula 7>.
[0066] [ka] M is selected from the metal elements in group 5 of the periodic table, R1, R2, and R3 are each independently selected from a hydrogen atom and a linear / branched / cyclic alkyl group having 1 to 5 carbon atoms; L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
[0067] The metal compound may have at least one of the Group 6 elements, including W and Mo, as a central element.
[0068] The metal compound may be represented by the following <Chemical Formula 8> or <Chemical Formula 9>.
[0069] [ka] [ka] M is selected from the metal elements in group 6 of the periodic table, L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
[0070] The metal compound may have at least one of the Group 13 elements, including Al, as a central element.
[0071] The metal compound can be represented by the following <Chemical Formula 10>.
[0072] [ka] M is selected from the metal elements in group 13 of the periodic table, L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
[0073] According to another embodiment of the present invention, a method for forming a thin film using an additive precursor includes an additive precursor supplying step of supplying an additive precursor into a chamber in which a substrate having one or more gap features is placed, thereby adsorbing the additive precursor onto the substrate; a step of purging the interior of the chamber; and a thin film forming step of supplying a reactant into the chamber to react with the adsorbed additive precursor to form a thin film to fill the gap features, wherein the additive precursor is formed by mixing 1 to 5 moles of a compound represented by the following <Chemical Formula 1> or the following <Chemical Formula 2> with 1 to 5 moles of a non-metallic compound.
[0074] [ka] In the above <Chemical Formula 1>, X is O or S, and R1 and R2 are each independently selected from an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms.
[0075] [ka] In the above <Chemical Formula 2>, X is O or S, n = 1 to 5, and R1 to R4 are each independently selected from a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms.
[0076] The adduct precursor may be formed by mixing ethyl methyl sulfide or ethyl propyl ether or tetrahydrofuran with the non-metallic compound.
[0077] The nonmetallic compound may have at least one of the Group 14 elements, including Si and Ge, as a central element.
[0078] The non-metallic compound may be represented by the following <Chemical Formula 11>.
[0079] [ka] In the above <Chemical Formula 11>, M is one of the group 14 elements including Si and Ge, R1 to R4 are each independently selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkylamine group having 1 to 10 carbon atoms, a dialkylamine group having 1 to 10 carbon atoms, an arylamine group having 6 to 12 carbon atoms, an aralkylamine group having 7 to 13 carbon atoms, a cyclic amine group having 3 to 10 carbon atoms, a heterocyclic amine group having 3 to 10 carbon atoms, a heteroarylamine group having 6 to 12 carbon atoms, an alkylsilylamine group having 2 to 10 carbon atoms, an azide group, or a halogen.
[0080] The non-metallic compound may be represented by the following <Chemical Formula 12>.
[0081] [ka] In the above <Chemical Formula 12>, M is one of the group 14 elements including Si and Ge, R1 to R6 are each independently selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkylamine group having 1 to 10 carbon atoms, a dialkylamine group having 1 to 10 carbon atoms, an arylamine group having 6 to 12 carbon atoms, an aralkylamine group having 7 to 13 carbon atoms, a cyclic amine group having 3 to 10 carbon atoms, a heterocyclic amine group having 3 to 10 carbon atoms, a heteroarylamine group having 6 to 12 carbon atoms, an alkylsilylamine group having 2 to 10 carbon atoms, an azide group, or a halogen.
[0082] Metal / nonmetal compounds can exist in the form of dimers or oligomers at room temperature and pressure, and can maintain the dimer or oligomer form even after the formation of the adduct precursor.
[0083] Thereafter, a purge gas (eg, an inert gas such as Ar) is supplied into the interior of the chamber to remove or purify any unadsorbed adduct precursors or by-products.
[0084] The substrate is then exposed to a reactive material delivered inside the chamber, forming a thin film on the surface of the substrate to fill the gap feature. The reactive material reacts with the additive precursor layer to form a thin film, where the thin film is a metal / non-metal oxide film when the reactive material is O3, O2, or H2O gas, and the thin film is a metal / non-metal nitride film when the reactive material is one or more of ammonia (NH3), hydrazine (N2H4), nitrogen dioxide (NO2), or nitrogen (N2). Additionally, the thin film may be a metal / non-metal sulfide or a metal / non-metal.
[0085] Thereafter, a purge gas (eg, an inert gas such as Ar) is supplied into the chamber to remove or purify unreacted substances or by-products.
[0086] Example 1 In a glove box at room temperature, 10.56 g (0.139 mol) of ethyl methyl sulfide corresponding to <Chemical Formula 1> was added to a 500 ml round flask, and 5 g (0.069 mol) of trimethylaluminum corresponding to <Chemical Formula 6> was added very slowly to obtain the precursor TMA-EMS.
[0087] FIG. 2 is a 1H-NMR graph of the precursor TMA-EMS according to Example 1 of the present invention.
[0088] 1 is a 1H-NMR graph of the precursor TMA-EMS according to Example 1 of the present invention, showing the NMR spectrum of Example 1 / ethyl methyl sulfide / trimethylaluminum. Trimethyl aluminum:δ-0.36(s) Ethyl methyl sulfide: δ2.19(q), 1.76(s), 1.20(t) TMA-EMS:δ-0.37(s),δ2.05(q),1.58(s),0.85(t)
[0089] The peaks at δ=2.19 ppm, 1.76 ppm, and 1.20 ppm, which were derived from ethyl methyl sulfide, did not change in shape even after the formation of the precursor TMA-EMS, and shifted to 2.05 ppm, 1.58 ppm, and 0.85 ppm, respectively.
[0090] It can also be confirmed that the peak of chemical migration δ=-0.36 ppm derived from trimethylaluminum does not change in shape after the formation of the precursor TMA-EMS, but migrates finely to form a stable precursor.
[0091] - Thermal analysis 3 and 4 are graphs showing the results of a differential scanning calorimetry (DSC) test and a thermogravimetry (TGA) test for Example 1. A differential scanning calorimetry (DSC) test and a thermogravimetry (TGA) test were performed on the TMA-EMS obtained in Example 1, and the thermal analysis test conditions for measuring the thermal decomposition temperature in each test are as follows: Transport gas: Argon (Ar) gas Transport gas flow rate: 200ml / min Heating profile: Heat from 30℃ to 400℃ at a rate of 10℃ / min.
[0092] The thermal decomposition temperature in the DSC test was determined as the temperature at which the heat flow suddenly increased during heating on the DSC thermogram.
[0093] Referring to Table 1 below, it has been confirmed that TMA-EMS has excellent vaporization properties with a residual component amount of less than 0.1%, and does not leave impurities in the thin film. In addition, the decomposition temperature of TMA-EMS is about 340℃, which shows improved thermal stability compared to trimethylaluminum (TMA), which has a decomposition temperature of about 320℃. This can be seen as the effect of the organic substance effectively blocking the Al-Al interactions between TMAs, forming a stable molecule. Furthermore, the addition of the additive increases steric hindrance around the Al center, which is expected to reduce reactivity compared to TMA before the additive is added.
[0094] [Table 1]
[0095] The diameter of the TMA-EMS precursor is about 8.6 Å, which is a significant increase in size compared to the TMA diameter of 5 Å. This not only further reduces the accessibility of the Al center of the TMA-EMS precursor to the surface -OH*, but also reduces the deposition thickness per cycle due to greater steric hindrance when there are several adsorbed precursors on the surface. This can be confirmed through the deposition results using the TMA-EMS precursor in Figure 5.
[0096] Similarly, the TMA-EMS precursor has reduced reactivity with the -OH* termination group on the surface, which reduces the sticking coefficient and increases diffusion at the surface, resulting in the formation of a uniform film, ultimately improving uniformity and step coverage.
[0097] Comparative Example 1 An aluminum oxide film was formed on a silicon substrate by the ALD process, the ALD process temperature was 250-400℃, and O3 gas was used as the reactant.
[0098] The aluminum oxide film formation process by the ALD process is as follows, and the following steps were carried out as one cycle. 1) Using Ar as a carrier gas, the aluminum precursor TMA (Trimethylaluminium) was supplied to the reaction chamber at room temperature, and the aluminum precursor was adsorbed onto the substrate. 2) Supply Ar gas into the reaction chamber to remove any unadsorbed aluminum precursor or by-products. 3) O3 gas is supplied to the reaction chamber to form a monolayer. 4) Ar gas is supplied into the reaction chamber to remove unreacted materials or by-products.
[0099] The thickness of the aluminum oxide film obtained by the above process was measured, and the thickness of the aluminum oxide film obtained per cycle of the ALD process was about 0.9 Å / cycle at 250~400℃.
[0100] 5 is a graph showing the GPC (Growth Per Cycle) versus process temperature in the process of forming aluminum oxide films on flat wafers according to Comparative Example 1 and Example 1 of the present invention. As shown in FIG. 5, ideal ALD behavior was shown with almost no change in GPC with increasing substrate temperature within the substrate temperature range of 250 to 400°C. In the ZrO2 / Al2O3 / ZrO2 composite dielectric film of a DRAM, assuming that the total thickness of the dielectric film is 50 Å and that the Al2O3 of Comparative Example 1 is used for about 3 cycles, the EOT of the dielectric film is 5.93 Å.
[0101] Example 1 An aluminum oxide film was formed on a silicon substrate using the precursor TMA-EMS according to Example 1 of the present invention. The aluminum oxide film was formed in the same manner as in Comparative Example 1, except that the precursor was changed.
[0102] The thickness of the aluminum oxide film obtained by the above procedure was measured, and the thickness of the aluminum oxide film obtained per cycle of the ALD process was about 0.7 Å / cycle at 250-400°C.
[0103] 5, ideal ALD behavior is shown with almost no GPC change accompanying an increase in substrate temperature within the range of 250 to 400°C, and a reduction effect of approximately 20% is achieved compared to Comparative Example 1. Assuming that the total thickness of the dielectric film in the ZrO2 / Al2O3 / ZrO2 composite dielectric film of a DRAM is 50 Å and Al2O3 in Comparative Example 1 is used for about three cycles, the EOT of the dielectric film is 5.72 Å, and a sculling down of approximately 4% can be achieved compared to Comparative Example 1.
[0104] 6 shows the step coverage of the aluminum oxide film according to Comparative Example 1 of the present invention deposited on a patterned wafer at a process temperature of 400°C (aspect ratio 20:1). As shown in Fig. 6, the thickness of the upper part obtained by repeating a certain cycle of the process was 8.32 Å and the thickness of the lower part was 8.34 Å, confirming the step coverage of 100%.
[0105] 7 shows the step coverage of the aluminum oxide film according to Example 1 of the present invention deposited on a patterned wafer at a process temperature of 400°C (aspect ratio 20:1). As shown in Fig. 7, the thickness of the upper part obtained by repeating a certain cycle of the process was 8.28 Å and the thickness of the lower part was 9.5 Å, resulting in a step coverage of 116%, with the thickness being about 15% thicker at the lower part than at the upper part.
[0106] Unlike the ideal ALD behavior on a flatbed, the adduct precursors in the structure can easily dissociate. A high process temperature above the adduct precursor dissociation temperature can be interpreted as providing high energy that can break the bonds between the metal / nonmetallic compound and the organic matter, and the adduct precursors can also be interpreted as dissociating due to diffusion to the bottom of the structure and an increase in the number of intermolecular collisions.
[0107] As a result, the dissociated organic matter, which is relatively volatile, exists at a high density at the top, while the relatively less volatile and heavier metal / nonmetal compounds exist at a high density at the bottom. The blocking effect of the organic matter on the metal / nonmetal compounds existing at a high density at the bottom is removed, restoring their original reactivity, and they are deposited at a high growth rate, increasing their thickness.
[0108] In conclusion, the additive precursor of the present invention can be used to obtain gradient adsorption characteristics in which the deposition rate increases toward the bottom, and by performing multiple cycloprocesses repeatedly, the material fills from the bottom up, achieving defect-free gap filling even in high aspect ratio structures.
[0109] Although the present invention has been described in detail with reference to the embodiments, other embodiments are possible, and therefore the technical spirit and scope of the following claims are not limited to the embodiments.
Claims
1. providing an additive precursor inside a chamber in which a substrate having one or more gap features is disposed, thereby adsorbing the additive precursor onto the substrate; purging the interior of the chamber; and providing a reactant into the chamber to react with the adsorbed additive precursor to form a thin film to fill the gap feature; The adduct precursor is formed by mixing 1 to 5 mol of a compound represented by the following <Chemical Formula 1> or the following <Chemical Formula 2> with 1 to 5 mol of a metal compound having at least one of Group 5 elements including Nb and Ta as a central element, or a metal compound represented by the following <Chemical Formula 8> or the following <Chemical Formula 9>. In the above <Chemical Formula 1>, X is O or S, and R 1 Or R 2 are each independently selected from an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms. In the formula 2, X is O or S, n is 1 to 5, and R 1 ~R 4 are each independently selected from a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms. In the <Chemical Formula 8> and the <Chemical Formula 9>, M is selected from metal elements belonging to Group 6 of the periodic table, L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
2. 2. The method for forming a thin film using an adduct precursor according to claim 1, wherein the adduct precursor is formed by mixing ethyl methyl sulfide, ethyl propyl ether or tetrahydrofuran with the metal compound.
3. 3. The method for forming a thin film using an adduct precursor according to claim 1 or 2, wherein the metal compound is represented by the following <Chemical Formula 5> or <Chemical Formula 6>. M is selected from the metal elements belonging to Group 5 of the periodic table; L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
4. 3. The method for forming a thin film using an adduct precursor according to claim 1 or 2, wherein the metal compound is represented by the following formula 7: M is selected from the metal elements belonging to Group 5 of the periodic table; R 1 , R 2 , R 3 are each independently selected from a hydrogen atom and a linear / branched / cyclic alkyl group having 1 to 5 carbon atoms; L may be the same or different and is selected from a hydrogen atom, a linear / branched / cyclic alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group having 1 to 5 carbon atoms, a dialkylamino group having 1 to 5 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aralkyl group having 7 to 13 carbon atoms, or a halogen element.
5. providing an additive precursor inside a chamber in which a substrate having one or more gap features is disposed, thereby adsorbing the additive precursor onto the substrate; purging the interior of the chamber; and providing a reactant into the chamber to react with the adsorbed additive precursor to form a thin film to fill the gap feature; The adduct precursor is formed by mixing 1 to 5 mol of a compound represented by the following <Chemical Formula 1> or <Chemical Formula 2> and 1 to 5 mol of a non-metallic compound represented by the following <Chemical Formula 11> or <Chemical Formula 12>. In the above <Chemical Formula 1>, X is O or S, and R 1 Or R 2 are each independently selected from an alkyl group having 1 to 8 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms. In the formula 2, X is O or S, n is 1 to 5, and R 1 ~R 4 are each independently selected from a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, and an aryl group having 6 to 12 carbon atoms. In the formula 11, M is one of the group 14 elements including Si and Ge; R 1 to R 4 are each independently selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkylamine group having 1 to 10 carbon atoms, a dialkylamine group having 1 to 10 carbon atoms, an arylamine group having 6 to 12 carbon atoms, an aralkylamine group having 7 to 13 carbon atoms, a cyclic amine group having 3 to 10 carbon atoms, a heterocyclic amine group having 3 to 10 carbon atoms, a heteroarylamine group having 6 to 12 carbon atoms, an alkylsilylamine group having 2 to 10 carbon atoms, an azide group, or a halogen. In the formula 12, M is one of the group 14 elements including Si and Ge; R 1 to R 6 are each independently selected from a hydrogen atom, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, an alkylamine group having 1 to 10 carbon atoms, a dialkylamine group having 1 to 10 carbon atoms, an arylamine group having 6 to 12 carbon atoms, an aralkylamine group having 7 to 13 carbon atoms, a cyclic amine group having 3 to 10 carbon atoms, a heterocyclic amine group having 3 to 10 carbon atoms, a heteroarylamine group having 6 to 12 carbon atoms, an alkylsilylamine group having 2 to 10 carbon atoms, an azide group, or a halogen atom.
6. 6. The method for forming a thin film using an adduct precursor according to claim 5, wherein the adduct precursor is formed by mixing ethyl methyl sulfide, ethyl propyl ether or tetrahydrofuran with the nonmetallic compound.
7. 3. The method for forming a thin film using an adduct precursor according to claim 1 or 2, wherein the thin film is any one of a metal oxide, a metal nitride, a metal sulfide, and a metal.
8. 7. The method for forming a thin film using an adduct precursor according to claim 5 or 6, wherein the thin film is any one of a non-metal oxide, a non-metal nitride, a non-metal sulfide, and a non-metal.
9. 7. The method for forming a thin film using an adduct precursor according to claim 1, 2, 5 or 6, wherein the method for forming a thin film proceeds at a temperature equal to or higher than the dissociation temperature of the adduct precursor.
10. 7. The method for forming a thin film using an adduct precursor according to claim 1, 2, 5 or 6, wherein the thin film forming method proceeds at a temperature of 50 to 700°C.
11. A method for manufacturing a volatile memory element, comprising the method for forming a thin film according to any one of claims 1, 2, 5 and 6.
12. 7. A method for manufacturing a non-volatile memory element, comprising the method for forming a thin film according to claim 1.
Citation Information
Patent Citations
Systems and methods for forming metal oxides using metal organic amines and metal organic oxides
JP2005537638A
Method for forming a tantalum-containing layer on a substrate
JP2011530002A
Raw material for forming thin film and manufacturing method for thin film
JP2015054853A
Selective film deposition using halogen passivation
JP2020530661A
Group 6 transition metal-containing compositions for vapor deposition of group 6 transition metal-containing films