Lithium secondary battery, its usage method, and manufacturing method of lithium secondary battery

The lithium secondary battery design without a negative electrode active material, using Li6Mn x Co 1-x O 4, addresses the issues of energy density and cycle characteristics by suppressing dendrite growth and enhancing productivity, achieving stable and efficient lithium deposition.

JP7587888B2Active Publication Date: 2024-11-21TERAWATT TECH KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023522051
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-18
Publication Date
2024-11-21
Estimated Expiration
2041-05-18

AI Technical Summary

Technical Problem

Conventional lithium secondary batteries face challenges in achieving high energy density and sufficient cycle characteristics due to the presence of negative electrode active materials, which occupy significant volume and mass, and the formation of dendrite-like lithium metal during charging and discharging, leading to short circuits and capacitance deterioration.

Method used

A lithium secondary battery design without a negative electrode active material, utilizing a positive electrode with Li6Mn x Co 1-x O 4 (0

Benefits of technology

The battery achieves high energy density and excellent cycle characteristics by suppressing dendrite formation and improving productivity, with Li6Mn x Co 1-x O 4 acting as a sacrificial cathode material, ensuring stable operation and efficient lithium deposition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587888000004
    Figure 0007587888000004
  • Figure 0007587888000005
    Figure 0007587888000005
  • Figure 0007587888000006
    Figure 0007587888000006
Patent Text Reader

Abstract

The present invention provides, inter alia, a lithium secondary battery that has high energy density and exceptional cycle characteristics and production properties, and a method for using the lithium secondary battery. The present invention relates to a lithium secondary battery comprising a positive electrode, and a negative electrode that does not have a negative-electrode active material, the positive electrode including a positive-electrode active material and a lithium-containing compound represented by Li6MnxCo1−xO4 (where 0<x<1). The present invention also relates to a method for manufacturing a lithium secondary battery, the method including: a step for preparing a positive electrode that includes a positive-electrode active material and a lithium-containing compound represented by Li6MnxCo1−xO4 (where 0<x<1), and preparing a negative electrode that does not have a negative-electrode active material; a step for disposing the positive electrode and the negative electrode such that the two electrodes face each other; and a step for applying a voltage between the positive electrode and the negative electrode to carry out initial charging using charging conditions in which the cut-off voltage is 4.3-5.0 V.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lithium secondary battery, a method for using the same, and a method for manufacturing the lithium secondary battery. [Background technology]

[0002] In recent years, technology for converting natural energy such as solar or wind power into electrical energy has been attracting attention. Accordingly, various secondary batteries have been developed as electricity storage devices that are highly safe and capable of storing a large amount of electrical energy.

[0003] Among them, lithium secondary batteries, which charge and discharge by transferring lithium ions between a positive electrode and a negative electrode, are known to exhibit high voltage and high energy density. A typical lithium secondary battery is the lithium ion secondary battery (LIB), which has active materials capable of retaining lithium elements in the positive electrode and the negative electrode, and charges and discharges by transferring lithium ions between the positive electrode active material and the negative electrode active material.

[0004] Furthermore, in order to achieve high energy density, lithium secondary batteries (lithium metal batteries; LMBs) have been developed that use lithium metal as the negative electrode active material instead of materials that can insert lithium ions, such as carbon materials. For example, Patent Document 1 discloses a rechargeable battery that uses a lithium metal-based electrode as the negative electrode.

[0005] In addition, for the purpose of further increasing the energy density and improving productivity, lithium secondary batteries using negative electrodes that do not have negative electrode active materials such as carbon materials and lithium metal have been developed. For example, Patent Document 2 discloses a lithium secondary battery including a positive electrode, a negative electrode, a separator and an electrolyte interposed between them, in which metal particles are formed on a negative electrode current collector, and are transferred from the positive electrode by charging to form lithium metal on the negative electrode current collector in the negative electrode. Patent Document 2 discloses that such a lithium secondary battery can provide a lithium secondary battery with improved performance and life by solving problems caused by the reactivity of lithium metal and problems that occur during the assembly process. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Special Publication No. 2006-500755 [Patent Document 2] Special Publication No. 2019-505971 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the present inventors have conducted detailed studies on conventional batteries, including those described in the above patent documents, and have found that at least one of the energy density and cycle characteristics is insufficient.

[0008] For example, it is difficult to sufficiently increase the energy density of a lithium secondary battery equipped with a negative electrode having a negative electrode active material due to the volume and mass occupied by the negative electrode active material. In addition, in the case of anode-free type lithium secondary battery equipped with a negative electrode not having a negative electrode active material, dendritic lithium metal is easily formed on the surface of the negative electrode by repeated charging and discharging, and short circuits and capacity reduction are easily caused, so that the cycle characteristics are insufficient.

[0009] By the way, various studies have been conducted to improve the productivity of lithium secondary batteries. For example, the materials of each component of a lithium secondary battery, especially the material of the positive electrode, may have low stability in the atmosphere. In such a case, there is a problem that the battery must be manufactured while precisely controlling the humidity and the like more strictly than in a normal dry room used in the usual process.

[0010] The present invention has been made in view of the above problems, and an object thereof is to provide a lithium secondary battery having a high energy density, excellent cycle characteristics and productivity, a method of using the same, and a method of manufacturing a lithium secondary battery.

Means for Solving the Problems

[0011] The lithium secondary battery according to an embodiment of the present invention includes a positive electrode and a negative electrode having no negative electrode active material, and the positive electrode includes a positive electrode active material and Li6Mn x Co 1-x a lithium-containing compound represented by O4 (0 < x < 1).

[0012] Since such a lithium secondary battery has no negative electrode active material, the volume and mass of the entire battery are smaller and the energy density is higher in principle than those of a lithium secondary battery having a negative electrode active material. In such a battery, lithium metal is deposited on the surface of the negative electrode, and charge and discharge are performed by electrolytic elution of the deposited lithium metal.

[0013] Also, Li6Mn x Co 1-xThe lithium-containing compound represented by O4 (0 < x < 1) can undergo an oxidation reaction in the charge-discharge potential range of a normal cathode active material, while substantially no reduction reaction occurs. Therefore, in the lithium secondary battery containing the above lithium-containing compound, the lithium-containing compound undergoes an oxidation reaction during the initial charging of the battery (i.e., releases lithium ions). On the other hand, during subsequent discharging, substantially no reduction reaction occurs (i.e., the lithium-containing compound before discharging is not reformed), and the lithium element derived from the lithium-containing compound remains on the anode surface as metallic lithium. And in the lithium secondary battery in which metallic lithium thus remains on the anode surface after initial charging, it is considered that the residual metallic lithium serves as a scaffold when further metallic lithium deposits on the anode surface during subsequent charging, and it is considered to assist the uniform deposition of metallic lithium on the anode surface. From the above, in the lithium secondary battery according to an embodiment of the present invention, the growth of dendritic metallic lithium on the anode is suppressed, and the lithium secondary battery has excellent cycle characteristics. However, the factor for the excellent cycle characteristics of the lithium secondary battery according to an embodiment of the present invention is not limited to this. Furthermore, since the above lithium-containing compound has excellent stability against trace moisture in the air, it is possible to provide a lithium secondary battery with high energy density and excellent cycle characteristics in an economically reasonable way (with high productivity).

[0014] The above lithium secondary battery is preferably initially charged under charging conditions where the cut-off voltage is 4.3 V or more and 5.0 V or less. Li6Mn x Co 1-x The lithium-containing compound represented by O4 (0 < x < 1) begins to undergo an oxidation reaction under the condition that the voltage of the battery reaches about 4.3 V. Therefore, according to the above aspect, the function of the above lithium-containing compound as the sacrificial cathode agent detailed above is more preferably exerted, and the cycle characteristics of the lithium secondary battery tend to be further improved.

[0015] The content of the lithium-containing compound is preferably 1.0 mass% or more and 15.0 mass% or less with respect to the total mass of the positive electrode. According to this embodiment, the function of the lithium-containing compound as a sacrificial positive electrode agent is more preferably exhibited, and the cycle characteristics of the lithium secondary battery tend to be further improved.

[0016] The lithium-containing compound is preferably Li6Mn x Co 1-x O4 (0.2≦x≦0.8). According to this embodiment, the function of the lithium-containing compound as a sacrificial positive electrode agent is more favorably exhibited, and the cycle characteristics of the lithium secondary battery tend to be further improved. In addition, the productivity of the lithium secondary battery also tends to be further improved.

[0017] The negative electrode may be an electrode made of at least one selected from the group consisting of Cu, Ni, Ti, Fe, other metals that do not form an alloy with Li, and alloys thereof, and stainless steel (SUS). According to this embodiment, the lithium secondary battery tends to be even more excellent in safety and productivity.

[0018] The above-mentioned lithium secondary battery preferably has an energy density of 350 Wh / kg or more.

[0019] The lithium secondary battery according to one embodiment of the present invention is preferably used by a method for using a lithium secondary battery, which comprises charging the battery at a cutoff voltage of 4.3 V or more and 5.0 V or less, followed by a charge-discharge cycle including at least one discharge step and at least one charge step, in this order, such that the cutoff voltage of the charge step in the charge-discharge cycle is lower than the cutoff voltage of a first initial charge carried out at a cutoff voltage of 4.3 V or more and 5.0 V or less.

[0020] A method for producing a lithium secondary battery according to one embodiment of the present invention comprises the steps of: x Co 1-xA step of preparing a positive electrode containing a lithium-containing compound represented by O4 (0 < x < 1) and a negative electrode having no negative electrode active material; a step of arranging the positive electrode and the negative electrode so that they face each other; and a step of applying a voltage between the positive electrode and the negative electrode to perform initial charging under a charging condition where the cut-off voltage is 4.3 V or more and 5.0 V or less.

[0021] According to such a manufacturing method, a battery with a high energy density can be manufactured because the negative electrode has no negative electrode active material. Also, in such a manufacturing method, Li6Mn x Co 1-x The lithium-containing compound represented by O4 (0 < x < 1) effectively and surely exhibits the function as a sacrificial positive electrode agent as detailed above. Therefore, the lithium secondary battery manufactured by such a method also has excellent cycle characteristics. Furthermore, Li6Mn x Co 1-x The lithium-containing compound represented by O4 (0 < x < 1) is excellent in stability against trace moisture in the air and can be handled without strictly controlling humidity, etc. Therefore, the above manufacturing method has high productivity.

[0022] In the above manufacturing method, the content of the lithium-containing compound is preferably 1.0% by mass or more and 15.0% by mass or less based on the total mass of the positive electrode. According to this aspect, there is a tendency to manufacture a lithium secondary battery with more excellent cycle characteristics.

[0023] In the above manufacturing method, the lithium-containing compound is preferably a compound represented by Li6Mn x Co 1-x O4 (0.2 ≤ x ≤ 0.8). According to this aspect, there is a tendency to manufacture a lithium secondary battery with more excellent cycle characteristics with high productivity.

[0024] In the above-mentioned manufacturing method, the negative electrode is preferably an electrode made of at least one selected from the group consisting of Cu, Ni, Ti, Fe, other metals that do not form an alloy with Li, and alloys thereof, and stainless steel (SUS). According to this embodiment, there is a tendency that a lithium secondary battery with even greater safety and productivity can be manufactured. Effect of the Invention

[0025] According to the present invention, it is possible to provide a lithium secondary battery having high energy density and excellent cycle characteristics and productivity, a method for using the same, and a method for producing the lithium secondary battery. [Brief description of the drawings]

[0026] [Figure 1] 1 is a schematic cross-sectional view of a lithium secondary battery according to a first embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view of a lithium secondary battery according to a first embodiment of the present invention; [Diagram 3] FIG. 2 is a schematic cross-sectional view of a lithium secondary battery according to a second embodiment of the present invention. [Figure 4] 2 is a schematic cross-sectional view of a buffer function layer in a lithium secondary battery according to the second embodiment of the present invention, in which (A) shows a fibrous buffer function layer which is one embodiment of the buffer function layer, (B) shows a precipitation pattern in which lithium metal precipitates in the fibrous buffer function layer, and (C) shows one embodiment of a component constituting the fibrous buffer function layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, embodiments of the present invention (hereinafter referred to as "the present embodiment") will be described in detail with reference to the drawings as necessary. In the drawings, the same reference numerals are assigned to the same elements, and duplicate descriptions are omitted. Also, the positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings unless otherwise specified. Furthermore, the dimensional ratios in the drawings are not limited to the illustrated ratios. In addition, hereinafter, a plurality of the present embodiments will be described in detail. However, in the description of each embodiment, the content described as "the present embodiment" can also be applied to embodiments other than the relevant embodiment. For example, in the first present embodiment, if there is a description that "the negative electrode of the present embodiment does not have a negative electrode active material", this description can also be applied to other embodiments.

[0028] [First Embodiment] (Lithium Secondary Battery) FIG. 1 is a schematic cross-sectional view of a lithium secondary battery according to the first present embodiment (hereinafter referred to as "the first embodiment"). As shown in FIG. 1, the lithium secondary battery 100 of the first embodiment includes a positive electrode 110 and a negative electrode 130 that does not have a negative electrode active material. The positive electrode 110 includes a positive electrode active material and a lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1). Further, the lithium secondary battery 100 includes a separator 120 between the positive electrode 110 and the negative electrode 130, and the positive electrode 110 has a positive electrode current collector 140 on the surface opposite to the surface facing the separator 120.

[0029] Note that the lithium secondary battery of the present embodiment disclosed in this specification is typically a liquid electrolyte-based lithium secondary battery (particularly a non-aqueous electrolyte-based lithium secondary battery) including an electrolytic solution, a solid or semi-solid electrolyte-based lithium secondary battery including a polymer electrolyte, or a gel electrolyte-based lithium secondary battery including a gel electrolyte. However, as long as the problems of the present invention are solved, the lithium secondary battery of the present embodiment may be other types, for example, an all-solid battery including an inorganic solid electrolyte. Hereinafter, each component will be described in detail.

[0030] (Negative electrode) The negative electrode of this embodiment does not have a negative electrode active material. In this specification, the "negative electrode active material" is a material that causes an electrode reaction, i.e., an oxidation reaction and a reduction reaction, at the negative electrode. Specifically, the negative electrode active material in this specification includes a host material of lithium metal and lithium element (lithium ion or lithium metal). The host material of lithium element means a material provided to hold lithium ion or lithium metal at the negative electrode. The mechanism of such holding is not particularly limited, but includes, for example, intercalation, alloying, and occlusion of metal clusters, and is typically intercalation.

[0031] In the lithium secondary battery of this embodiment, since the negative electrode does not have a negative electrode active material before the initial charge of the battery, lithium metal is deposited on the negative electrode, and the deposited lithium metal is electrolytically dissolved to perform charging and discharging. Therefore, in the lithium secondary battery of this embodiment, the volume occupied by the negative electrode active material and the mass of the negative electrode active material are reduced compared to a lithium secondary battery having a negative electrode active material, and the volume and mass of the entire battery are reduced, so that the energy density is high in principle.

[0032] As described above, in the lithium secondary battery of this embodiment, the negative electrode does not have a negative electrode active material before the initial charge of the battery, lithium metal is deposited on the negative electrode by charging the battery, and the deposited lithium metal is electrolytically dissolved by discharging the battery. Therefore, in the lithium secondary battery of this embodiment, the negative electrode functions as a negative electrode current collector.

[0033] The lithium secondary battery of this embodiment differs from a lithium ion battery (LIB) and a lithium metal battery (LMB) in the following respects. In a lithium ion battery (LIB), the negative electrode has a host material of lithium element (lithium ion or lithium metal), and when the battery is charged, the material is filled with lithium element, and when the host material releases the lithium element, the battery is discharged. LIBs differ from the lithium secondary battery of this embodiment in that the negative electrode has a host material of lithium element. A lithium metal battery (LMB) is manufactured using an electrode having lithium metal on its surface or lithium metal alone as the negative electrode. That is, the LMB differs from the lithium secondary battery of this embodiment in that the negative electrode has lithium metal as the negative electrode active material immediately after the battery is assembled, i.e., before the initial charge of the battery. The LMB is manufactured using an electrode containing lithium metal, which is highly flammable and reactive, but the lithium secondary battery of this embodiment is manufactured using a negative electrode that does not contain lithium metal, and is therefore safer and more productive. Furthermore, the lithium secondary battery of this embodiment is superior in energy density and cycle characteristics to the LMB.

[0034] In this specification, the negative electrode "has no negative electrode active material" means that the negative electrode does not have or substantially does not have a negative electrode active material. The negative electrode substantially does not have a negative electrode active material means that the content of the negative electrode active material in the negative electrode is 10 mass% or less with respect to the entire negative electrode. The content of the negative electrode active material in the negative electrode is preferably 5.0 mass% or less with respect to the entire negative electrode, and may be 1.0 mass% or less, 0.1 mass% or less, or 0.0 mass% or less. When the negative electrode does not have a negative electrode active material or the content of the negative electrode active material in the negative electrode is within the above range, the energy density of the lithium secondary battery is high.

[0035] In this specification, the term "lithium secondary battery having a negative electrode that does not have a negative electrode active material" means that the negative electrode does not have a negative electrode active material before the initial charge of the battery. Therefore, the phrase "negative electrode that does not have a negative electrode active material" may be rephrased as "negative electrode that does not have a negative electrode active material before the initial charge of the battery", "negative electrode that does not have a negative electrode active material other than lithium metal regardless of the charge state of the battery and does not have lithium metal before the initial charge", or "negative electrode current collector that does not have lithium metal before the initial charge", etc. In addition, the term "lithium battery having a negative electrode that does not have a negative electrode active material" may be rephrased as an anode-free lithium battery, a zero anode lithium battery, or an anode-less lithium battery.

[0036] In this specification, the term "before initial charge" refers to the state of the battery from assembly to the first charge, and the term "at the end of discharge" refers to the state in which a discharge reaction involving the positive electrode active material does not substantially occur even if the battery voltage is further reduced, and the battery voltage at this time is, for example, 1.0 to 3.5 V, 2.0 to 3.2 V, or 2.5 to 3.0 V.

[0037] In the negative electrode of this embodiment, regardless of the charged state of the battery, the content of negative electrode active material other than lithium metal is 10 mass% or less, preferably 5.0 mass% or less, may be 1.0 mass% or less, 0.1 mass% or less, 0.0 mass% or less, or may be 0 mass% based on the entire negative electrode. In addition, the negative electrode of this embodiment has a lithium metal content of 10% by mass or less, preferably 5.0% by mass or less, more preferably 1.0% by mass or less, or 0.1% by mass or less, based on the entire negative electrode before initial charging. The negative electrode of this embodiment particularly preferably has no lithium metal before initial charging, that is, the lithium metal content is 0% by mass based on the entire negative electrode.

[0038] In the lithium secondary battery of this embodiment, when the battery voltage is 2.5 V or more and 3.5 V or less, the lithium metal content may be 10 mass % or less (preferably 5.0 mass % or less, and may be 1.0 mass % or less) relative to the entire negative electrode; or when the battery voltage is 2.5 V or more and 3.0 V or less, the lithium metal content may be 10 mass % or less (preferably 5.0 mass % or less, and may be 1.0 mass % or less) relative to the entire negative electrode.

[0039] In the lithium secondary battery of this embodiment, the mass M of lithium metal deposited on the negative electrode when the battery voltage is 4.2 V is 4.2 The mass M of lithium metal deposited on the negative electrode when the battery voltage is 3.0 V 3.0 Ratio of M 3.0 / M 4.2 is preferably 30% or less, more preferably 25% or less, and further preferably 20% or less. 3.0 / M 4.2 may be 1.0% or more, 2.0% or more, 3.0% or more, or 4.0% or more.

[0040] Examples of the negative electrode active material in this specification include lithium metal and alloys containing lithium metal, carbon-based materials, metal oxides, and metals that are alloyed with lithium and alloys containing the metals.The carbon-based materials include, but are not limited to, graphene, graphite, hard carbon, mesoporous carbon, carbon nanotubes, and carbon nanohorns.The metal oxides include, but are not limited to, titanium oxide compounds, tin oxide compounds, and cobalt oxide compounds.The metals that are alloyed with lithium include, but are not limited to, silicon, germanium, tin, lead, aluminum, and gallium.

[0041] The negative electrode of the present embodiment is not particularly limited as long as it does not have a negative electrode active material and can be used as a current collector. For example, it includes electrodes composed of at least one selected from the group consisting of Cu, Ni, Ti, Fe, other metals that do not alloy with Li, alloys thereof, and stainless steel (SUS). Preferably, electrodes composed of at least one selected from the group consisting of Cu, Ni, alloys thereof, and stainless steel (SUS) are included. When such a negative electrode is used, the energy density and productivity of the battery tend to be further improved. In addition, when SUS is used for the negative electrode, various conventionally known types of SUS can be used. The above-mentioned negative electrode materials are used alone or in combination of two or more. In this specification, the "metal that does not alloy with Li" means a metal that does not react with lithium ions or lithium metal to form an alloy under the operating conditions of a lithium secondary battery.

[0042] The average thickness of the negative electrode of the present embodiment is preferably 4 μm or more and 20 μm or less, more preferably 5 μm or more and 18 μm or less, and still more preferably 6 μm or more and 15 μm or less. According to such an aspect, since the volume occupied by the negative electrode in the lithium secondary battery decreases, the energy density of the lithium secondary battery 100 is further improved. In this specification, the "average thickness" means the arithmetic mean when the target member is magnified and observed using a scanning electron microscope or an optical microscope, and the thicknesses of three or more parts are measured.

[0043] (Positive electrode) The positive electrode of the present embodiment includes a positive electrode active material and a lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 <x <1). Since the positive electrode contains a positive electrode active material, the lithium secondary battery of the present embodiment has excellent stability and a high output voltage.

[0044] In this specification, the "positive electrode active material" refers to a material that causes an electrode reaction, i.e., an oxidation reaction and a reduction reaction, at the positive electrode. Specifically, a host material of a lithium element (typically, a lithium ion) can be mentioned. The positive electrode active material in this specification is typically a material that causes an oxidation-reduction reaction under the condition that the voltage of the lithium secondary battery of this embodiment is in the range of 3.0 to 4.2 V, or a material that causes an oxidation-reduction reaction under the condition that the voltage of the lithium secondary battery of this embodiment is in the range of 3.0 to 4.2 V (vs. Li / Li + It is a substance that undergoes an oxidation-reduction reaction in the potential range of the reference electrode. Such positive electrode active materials include, but are not limited to, metal oxides and metal phosphates. Metal oxides include, but are not limited to, cobalt oxide compounds, manganese oxide compounds, and nickel oxide compounds. Metal phosphates include, but are not limited to, iron phosphate compounds, and cobalt phosphate compounds. Typical positive electrode active materials are LiCoO2, LiNi x Co y Mn z O(x+y+z=1), LiNi x Co y Al z O(x+y+z=1), LiNi x Mn y O(x+y=1), LiNiO2, LiMn2O4, LiFePO, LiCoPO, LiFeOF, LiNiOF, and LiTiS2. The above-mentioned positive electrode active materials are used alone or in combination of two or more. The positive electrode active material of this embodiment is preferably LiCoO2, LiNi x Co y Mn z O(x+y+z=1), LiNi x Co y Al z O(x+y+z=1), LiNi x Mn y At least one selected from the group consisting of LiNiO2, LiMn2O4, and O(x+y=1).

[0045] The positive electrode of this embodiment contains, in addition to the positive electrode active material, Li6Mn xCo 1-x It contains a lithium-containing compound represented by CoO4 (0 < x < 1). Li6Mn x Co 1-x The lithium-containing compound represented by CoO4 (0 < x < 1) can undergo an oxidation reaction in the charge-discharge potential range of the positive electrode active material as described above, while substantially not undergoing a reduction reaction. Therefore, when the lithium secondary battery of this embodiment is initially charged, Li6Mn x Co 1-x The lithium-containing compound represented by CoO4 (0 < x < 1) undergoes an oxidation reaction and releases lithium ions, and releases electrons to the negative electrode through the external circuit. As a result, the lithium ions derived from the above lithium-containing compound are deposited on the surface of the negative electrode as metallic lithium. Further, when the lithium secondary battery of this embodiment is discharged after the initial charge is completed (i.e., initially discharged), although the metallic lithium deposited on the negative electrode is electrolytically eluted and electrons move from the negative electrode to the positive electrode through the external circuit, the above lithium-containing compound substantially does not undergo a reduction reaction under normal discharge conditions and it is substantially impossible to return to the state before the oxidation reaction occurs. Therefore, when the lithium secondary battery of this embodiment is discharged after the initial charge, most of the metallic lithium derived from the above lithium-containing compound remains on the negative electrode, and even after the discharge of the battery is completed, some metallic lithium remains on the negative electrode. The residual metallic lithium is considered to serve as a scaffold when further metallic lithium is deposited on the surface of the negative electrode in the charging step following the initial discharge, and is considered to assist in the uniform deposition of metallic lithium on the surface of the negative electrode. As a result, the growth of dendritic metallic lithium on the negative electrode is suppressed in the lithium secondary battery of this embodiment, and the lithium secondary battery of this embodiment has excellent cycle characteristics. However, the factor for the excellent cycle characteristics of the lithium secondary battery according to this embodiment is not limited to this.

[0046] In the field of batteries, an additive that is generally added to a positive electrode and causes an oxidation reaction in the charge-discharge potential range of the positive electrode active material and substantially does not cause a reduction reaction is called a sacrificial positive electrode agent. Various materials have been proposed as sacrificial positive electrode agents for various batteries. The inventors of the present invention have found that in a lithium secondary battery (anode-free secondary battery) including an anode having no negative electrode active material, among such sacrificial positive electrode agents, Li6Mn x Co 1-x Using a lithium-containing compound represented by O4 (0 < x < 1) further improves the cycle characteristics.

[0047] In addition, the inventors of the present invention have found at least the following as the factors. (1) In a lithium-ion battery using an anode having a negative electrode active material such as a graphite material, it is normal to perform initial charging so that the cut-off voltage does not exceed 4.3V. When charging is performed beyond this, the cycle characteristics deteriorate due to decomposition of the electrolytic solution and / or the active material. On the other hand, the inventors have found that in a lithium secondary battery (anode-free secondary battery) including an anode having no negative electrode active material, even when charging is performed until the cut-off voltage reaches about 5.0V exceeding 4.3V in the initial charging, the cycle characteristics do not deteriorate. This is considered to be contributed by the relatively low negative electrode potential in the anode-free secondary battery. (2) When a lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) is contained as a sacrificial positive electrode agent in a lithium secondary battery (anode-free secondary battery) including an anode having no negative electrode active material, it has been found that the lithium-containing compound releases lithium ions under the condition that the voltage of the battery becomes about 4.3V in the initial charging.

[0048] Further, when the present inventors use a lithium-containing compound represented by (3) Li6MnO4 as a sacrificial cathode agent, even when the cut-off voltage is about 5.0 V, the lithium release reaction does not occur sufficiently, and Li6MnO4 does not fully exhibit its function as a sacrificial cathode agent. (4) When a lithium-containing compound represented by Li6CoO4 is used as a sacrificial cathode agent, the lithium-containing compound is unstable with respect to trace amounts of moisture contained in the atmosphere. (5) Surprisingly, Li6Mn x Co 1-x It has been found that if it is a lithium-containing compound represented by O4 (0 < x < 1), the problems described in (3) and (4) above do not occur. In particular, Li6Mn x Co 1-x The lithium-containing compound represented by O4 (0 < x < 1) has higher stability in the atmosphere than the lithium-containing compound represented by Li6CoO4. Specifically, when trying to fabricate a cathode using a highly alkaline material such as Li6CoO4, when preparing a cathode composite slurry by kneading with a binder such as polyvinylidene fluoride (PVDF), Li6CoO4 absorbs moisture in the atmosphere, causing the cathode composite slurry to experience a sharp increase in viscosity and / or gelation. However, Li6Mn x Co 1-x The lithium-containing compound represented by O4 (0 < x < 1) is less likely to have such problems. Therefore, the lithium secondary battery of the present embodiment uses a lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) which has high stability in the atmosphere as a sacrificial cathode agent. Therefore, it is not necessary to strictly adjust the humidity in the atmosphere when fabricating the cathode, and it can be manufactured in a normal dry room and / or glove box, thereby improving productivity. In this specification, "high productivity" includes not only the fact that a large number of lithium secondary batteries can be manufactured per unit time, but also the fact that lithium secondary batteries can be manufactured without the need for special equipment and / or environment.

[0049] In the cathode of the present embodiment, Li6Mn x Co 1-xThe value of x in the lithium-containing compound represented by O4(0 < x < 1) is not particularly limited as long as it is greater than 0. However, from the perspective of improving the productivity of lithium secondary batteries, it is preferably 0.1 or more. From the same perspective, the value of x is more preferably 0.2 or more, still more preferably 0.3 or more, and may be 0.4 or more, 0.5 or more, or 0.6 or more. Also, the value of x is not particularly limited as long as it is less than 1. However, from the perspective of improving the cycle characteristics of lithium secondary batteries, it is preferably 0.9 or less, more preferably 0.8 or less, and still more preferably 0.7 or less. The value of x may be 0.6 or less, 0.5 or less, or 0.4 or less. The value of x may be within a range obtained by arbitrarily combining the above upper and lower limit values. For example, it may be 0.1 ≤ x ≤ 0.9, 0.2 ≤ x ≤ 0.8, or 0.3 ≤ x ≤ 0.7. The positive electrode of this embodiment may contain two or more of the above lithium-containing compounds having different compositions, or may contain only one kind of lithium-containing compound. Also, commercially available lithium-containing compounds may be used, or they may be produced by conventionally known methods. The specific production method of the above lithium-containing compound will be described later.

[0050] As described above, Li6Mn x Co 1-x The lithium-containing compound represented by O4(0 < x < 1) tends to start releasing lithium ions under the condition that the voltage of the battery becomes about 4.3 V during the initial charging. Therefore, the lithium secondary battery of this embodiment is preferably initially charged under charging conditions where the cut-off voltage is 4.3 V or more and 5.0 V or less. By performing the initial charging under such conditions, the cycle characteristics of the lithium secondary battery tend to be further improved. Here, in this specification, "initially charged under charging conditions where the cut-off voltage is value X" means that when the battery is charged for the first time after being assembled, charging is continued until the voltage of the battery reaches value X. From the viewpoint of further improving the cycle characteristics of the lithium secondary battery, the lithium secondary battery of this embodiment is more preferably initially charged under charging conditions in which the cut-off voltage is more than 4.3 V, or 4.4 V or higher. The cut-off voltage in the initial charge may be 4.5 V or higher, 4.6 V or higher, or 4.7 V or higher.

[0051] Moreover, the lithium secondary battery of this embodiment is preferably initially charged under charging conditions in which the cutoff voltage is not more than 5.0 V. By initially charging under such conditions, decomposition of the positive electrode active material and / or electrolyte is reliably suppressed, and the cycle characteristics of the lithium secondary battery tend to be further improved. From the viewpoint of further improving the cycle characteristics of the lithium secondary battery, the lithium secondary battery of this embodiment is initially charged under charging conditions in which the cut-off voltage is more preferably less than 5.0 V, or 4.9 V or less, even more preferably 4.8 V or less, and even more preferably 4.7 V or less. The cut-off voltage in the initial charge may be 4.6 V or less, or 4.5 V or less.

[0052] The cutoff voltage in the initial charge may be within a range obtained by any combination of the upper and lower limits described above, for example, more than 4.3 V and less than 5.0 V, 4.4 V or more and 4.9 V or less, or 4.4 V or more and 4.7 V or less. The lithium secondary battery of the present embodiment may be provided to a user after initial charging or before initial charging. When provided to a user before initial charging, the lithium secondary battery of the present embodiment is preferably used according to the method of using the lithium secondary battery of the present embodiment described later. Specifically, when used for the first time, it is preferably charged under charging conditions in which the cutoff voltage is 4.3V or more and 5.0V or less.

[0053] As mentioned above, Li6Mn x Co 1-xThe lithium-containing compound represented by O4 (0 < x < 1) can undergo an oxidation reaction in the charge-discharge potential range of the cathode active material as described above, while substantially not undergoing a reduction reaction. In this specification, "can undergo an oxidation reaction in the charge-discharge potential range of the cathode active material" means that in the charge-discharge potential range of the cathode active material, it is possible to undergo an oxidation reaction to release lithium ions and electrons (including being decomposed by the oxidation reaction to release lithium ions). Also, "substantially does not undergo a reduction reaction in the charge-discharge potential range of the cathode active material" means that in the charge-discharge potential range of the cathode active material, under normal reaction conditions for those skilled in the art, it is impossible or substantially impossible to undergo a reduction reaction to receive lithium ions and electrons, or to be generated through a reduction reaction. "Normal reaction conditions for those skilled in the art" means, for example, the conditions when discharging a lithium secondary battery. However, Li6Mn x Co 1-x The lithium-containing compound represented by O4 (0 < x < 1) can undergo a reduction reaction to receive lithium ions and electrons by making the voltage of the battery sufficiently lower than the operating voltage range of a normal battery. Such conditions include, for example, the condition where the voltage of the battery is 2.0 V or less.

[0054] In the initial charging of the lithium secondary battery of this embodiment, Li6Mn x Co 1-x The lithium-containing compound represented by O4 (0 < x < 1) will be in an oxidized state where, by volume ratio, for example, 50% or more, 60% or more, 70% or more, 80% or more, 90% or more, 95% or more, or 99% or more of the added amount during manufacturing has released lithium ions. In the initial discharging of the lithium secondary battery of this embodiment, the lithium-containing compound that has become oxidized during initial charging is substantially not reduced. The capacity of the initial discharge relative to the capacity of the initial charging in the lithium-containing compound is, for example, 20% or less (for example, 20% or less, 15% or less, 10% or less, 5% or less, 1% or less, or 0%).

[0055] In this specification, the "charge and discharge potential range of the positive electrode active material" means the potential range in which the oxidation reaction and reduction reaction of the positive electrode active material contained in the positive electrode can occur. Specific values depend on the type of the positive electrode active material, but typically, with respect to the Li / Li + reference electrode, it is 2.5 V or more, 2.7 V or more, 3.0 V or more, 3.2 V or more, or 3.5 V or more, and 4.6 V or less, 4.5 V or less, 4.4 V or less, 4.3 V or less, 4.2 V or less, 4.1 V or less, or 4.0 V or less. A typical range of the charge and discharge potential range of the positive electrode active material is 3.0 V or more and 4.2 V or less (vs. Li / Li + reference electrode), and the upper limit value and the lower limit value thereof can be independently replaced with any of the above-described numerical values.

[0056] Regarding the charge and discharge potential range of the positive electrode active material with respect to the above-described Li / Li + reference electrode, it may be referred to the operating voltage range of the lithium secondary battery. For example, when the operating voltage of the lithium secondary battery is 3.0 V or more and 4.2 V or less, the charge and discharge potential range of the positive electrode active material with respect to the Li / Li + reference electrode can be estimated to be 3.0 V or more and 4.2 V or less. That is, it may also be paraphrased that the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) can cause an oxidation reaction in the operating voltage range of the lithium secondary battery, while substantially no reduction reaction occurs. Typically, the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) tends to cause a main oxidation reaction on the higher voltage side than the operating voltage range of the lithium secondary battery.

[0057] The positive electrode of the present embodiment may contain components other than the positive electrode active material and the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1). Such components are not particularly limited, but for example, Li6Mn x Co 1-xExamples include a sacrificial cathode agent, a conductive aid, a binder, and an electrolyte other than the lithium-containing compound represented by O4 (0 < x < 1).

[0058] Li6Mn x Co 1-x The sacrificial cathode agent other than the lithium-containing compound represented by O4 (0 < x < 1) is not particularly limited. For example, lithium oxides such as Li2O2; lithium nitrides such as Li3N; lithium sulfide-based solid solutions such as Li2S-P2S5, Li2S-LiCl, Li2S-LiBr, and Li2S-LiI; Li 1+x (Ti 1-y Fe y ) 1-x O2 (0 < x ≤ 0.25, 0.4 < y ≤ 0.9), Li 2-x Ti 1-z Fe z O 3-y (0 ≤ x < 2, 0 ≤ y ≤ 1, 0.05 ≤ z ≤ 0.95), and iron-based lithium oxides such as Li5FeO4. The sacrificial cathode agents other than the lithium-containing compounds as described above are used alone or in combination of two or more.

[0059] The conductive aid is not particularly limited. For example, carbon black, single-walled carbon nanotubes (SWCNT), multi-walled carbon nanotubes (MWCNT), carbon nanofibers (CF), and acetylene black are included. Also, the binder is not particularly limited. For example, polyvinylidene fluoride, polytetrafluoroethylene, styrene-butadiene rubber, acrylic resin, and polyimide resin are included. The conductive aids and binders as described above are each used alone or in combination of two or more.

[0060] Examples of electrolytes that the positive electrode of the present embodiment may contain include polymer electrolytes, gel electrolytes, and inorganic solid electrolytes, etc., and typically are polymer electrolytes or gel electrolytes. As the polymer electrolyte and the gel electrolyte, those described later can be used. The electrolytes as described above are used alone or in combination of two or more.

[0061] The content of each component in the positive electrode of the present embodiment is not particularly limited. The content of each component in the positive electrode can vary depending on the charge state of the battery, but can be defined, for example, by the blending ratio of each component during manufacturing. Alternatively, it may be defined by the content of each component in the discharged state (at the end of discharge).

[0062] During the production of the positive electrode of the present embodiment, the total blending amount of the positive electrode active material and the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) may be, for example, 50% by mass or more and 100% by mass or less, or 70% by mass or more and 99% by mass or less with respect to the total mass of the positive electrode. The total blending amount of the positive electrode active material and the lithium-containing compound is preferably 60% by mass or more, more preferably 70% by mass or more, still more preferably 80% by mass or more, and even more preferably 90% by mass or more with respect to the total mass of the positive electrode. The total blending amount of the positive electrode active material and the lithium-containing compound is preferably 99% by mass or less, more preferably 98% by mass or less with respect to the total mass of the positive electrode.

[0063] At the end of discharge of the lithium secondary battery of the present embodiment, the positive electrode active material and Li6Mn x Co 1-xThe total content of the lithium-containing compound represented by O4 (0 < x < 1) may be, for example, 50% by mass or more and 100% by mass or less, or 70% by mass or more and 99% by mass or less with respect to the total mass of the positive electrode. The total content of the positive electrode active material and the lithium-containing compound is preferably 60% by mass or more, more preferably 70% by mass or more, still more preferably 80% by mass or more, and even more preferably 90% by mass or more with respect to the total mass of the positive electrode. The total content of the positive electrode active material and the lithium-containing compound is preferably 99% by mass or less, more preferably 98% by mass or less with respect to the total mass of the positive electrode.

[0064] During the production of the positive electrode of the present embodiment, Li6Mn x Co 1-x The compounding amount of the lithium-containing compound represented by O4 (0 < x < 1) may be, for example, 1.0% by mass or more and 15% by mass or less with respect to the total mass of the positive electrode. The content of the lithium-containing compound is preferably 1.0% by mass or more, more preferably 2.0% by mass or more, and still more preferably 3.0% by mass or more with respect to the total mass of the positive electrode. Also, the content of the lithium-containing compound is preferably 15% by mass or less, more preferably 12% by mass or less, still more preferably 10% by mass or less, and may be 8.0% by mass or less or 5.0% by mass or less with respect to the total mass of the positive electrode.

[0065] By the initial charging of the battery, although at least a part of the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) releases lithium ions and electrons to become an oxidized state, the sum of the oxidized state and the reduced state of the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) is constant before and after the initial charging and is also constant regardless of the charge state of the battery. Therefore, Li6Mn x Co 1-xThe total content of the oxidized state and the reduced state of the lithium-containing compound represented by O4(0 < x < 1) may be, for example, 1.0% by mass or more and 15% by mass or less with respect to the total mass of the positive electrode. The total content of the oxidized state and the reduced state is preferably 1.0% by mass or more, more preferably 2.0% by mass or more, and still more preferably 3.0% by mass or more with respect to the total mass of the positive electrode. Further, the total content of the oxidized state and the reduced state is preferably 15% by mass or less, more preferably 12% by mass or less, still more preferably 10% by mass or less, and may be 8.0% by mass or less or 5.0% by mass or less with respect to the total mass of the positive electrode.

[0066] Li6Mn x Co 1-x The total content of the oxidized state and the reduced state of the lithium-containing compound represented by O4(0 < x < 1) is equivalent to the blending amount of the lithium-containing compound during the production of the positive electrode. Further, after sweeping the battery to a lower voltage (for example, about 1.0 V) than the voltage range in a normal charge-discharge cycle to return the lithium-containing compound to the reduced state represented by Li6Mn x Co 1-x O4(0 < x < 1), it is also possible to calculate the total content of the oxidized state and the reduced state by measuring the content of Li6Mn x Co 1-x O4 by a conventionally known method. Note that the content of the positive electrode active material and the lithium-containing compound represented by Li6Mn x Co 1-x O4(0 < x < 1) in the positive electrode can be measured, for example, by a method of comparing the relative intensities of peaks by X-ray diffraction measurement (XRD) or by the Rietveld method.

[0067] Regarding the conductive assistant, the blending amount during the production of the positive electrode of the present embodiment and the content at the end of discharge of the battery may be, for example, 0.5% by mass to 30% by mass or less, 1.0% by mass to 20% by mass or less, or 1.5% by mass to 10% by mass or less with respect to the total mass of the positive electrode. Regarding the binder, the blending amount during the production of the positive electrode of the present embodiment and the content at the end of discharge of the battery may be, for example, 0.5% by mass or less, 30% by mass or less, 1.0% by mass or less, 20% by mass or less, or 1.5% by mass or less, 10% by mass or less with respect to the total mass of the positive electrode. Regarding the electrolyte, the blending amount during the production of the positive electrode of the present embodiment and the content at the end of discharge of the battery may be, for example, 0.5% by mass or less, 30% by mass or less, 1.0% by mass or less, 20% by mass or less, or 1.5% by mass or less, 10% by mass or less with respect to the total mass of the positive electrode. Li6Mn x Co 1-x Regarding the sacrificial positive electrode agent other than the lithium-containing compound represented by Li6MnCoO4 (0 < x < 1), the blending amount during the production of the positive electrode of the present embodiment may be, for example, 0.5% by mass or less, 30% by mass or less, 1.0% by mass or less, 20% by mass or less, or 1.5% by mass or less, 10% by mass or less with respect to the total mass of the positive electrode.

[0068] The average thickness of the positive electrode of the present embodiment is, for example, 10 μm or more and 300 μm or less, preferably 30 μm or more and 200 μm or less, or 50 μm or more and 150 μm or less. However, the average thickness of the positive electrode can be appropriately adjusted according to the desired capacity of the battery.

[0069] (Positive electrode current collector) On one side of the positive electrode 110, a positive electrode current collector 140 is formed. The positive electrode current collector of the present embodiment is not particularly limited as long as it is a conductor that does not react with lithium ions in the battery. Examples of such a positive electrode current collector include aluminum.

[0070] The average thickness of the positive electrode current collector of the present embodiment is preferably 4 μm or more and 20 μm or less, more preferably 5 μm or more and 18 μm or less, and still more preferably 6 μm or more and 15 μm or less. According to such an aspect, since the volume occupied by the positive electrode current collector in the lithium secondary battery decreases, the energy density of the lithium secondary battery is further improved.

[0071] (Separator) The separator of this embodiment is a member for preventing the battery from short-circuiting by isolating the positive electrode and the negative electrode, while ensuring the ionic conductivity of lithium ions that serve as charge carriers between the positive electrode and the negative electrode. That is, the separator 120 has a function of isolating the positive electrode 110 and the negative electrode 130, and a function of ensuring the ionic conductivity of lithium ions. As such a separator, a member having the above two functions may be used alone, or two or more members having the above one function may be used in combination. The separator is not particularly limited as long as it has the above-mentioned function, but examples thereof include insulating porous members, polymer electrolytes, gel electrolytes, and inorganic solid electrolytes, and is typically at least one selected from the group consisting of insulating porous members, polymer electrolytes, and gel electrolytes.

[0072] When the separator includes an insulating porous member, the pores of the member are filled with an ion-conductive substance, such that the member exhibits ion conductivity. Examples of the substance to be filled include an electrolytic solution, a polymer electrolyte, and a gel electrolyte. The separator of the present embodiment may be made of an insulating porous material, a polymer electrolyte, or a gel electrolyte, either singly or in combination of two or more of them. However, when an insulating porous material is used alone as the separator, the lithium secondary battery must further include an electrolyte to ensure ion conductivity.

[0073] The material constituting the insulating porous member is not particularly limited, but may be, for example, an insulating polymer material, specifically, polyethylene (PE) and polypropylene (PP). That is, the separator of the present embodiment may be a porous polyethylene (PE) film, a porous polypropylene (PP) film, or a laminated structure thereof.

[0074] The polymer electrolyte is not particularly limited, but examples thereof include solid polymer electrolytes mainly containing a polymer and an electrolyte, and semi-solid polymer electrolytes mainly containing a polymer, an electrolyte, and a plasticizer. The gel electrolyte is not particularly limited, but may be, for example, one that mainly contains a polymer and a liquid electrolyte (that is, a solvent and an electrolyte).

[0075] Polymers that may be included in the polymer electrolyte and gel electrolyte include, but are not limited to, polymers containing functional groups containing oxygen atoms such as ether and ester, halogen groups, and polar groups such as cyano groups.Specific examples include resins having ethylene oxide units in the main chain and / or side chain such as polyethylene oxide (PEO), resins having propylene oxide units in the main chain and / or side chain such as polypropylene oxide (PPO), acrylic resins, vinyl resins, ester resins, nylon resins, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polysiloxane, polyphosphazene, polymethyl methacrylate, polyamide, polyimide, aramid, polylactic acid, polyurethane, polyacetal, polysulfone, polyethylene carbonate, polypropylene carbonate, and polytetrafluoroethylene.The above-mentioned resins may be used alone or in combination of two or more.

[0076] Examples of electrolytes contained in the polymer electrolyte and the gel electrolyte include salts of Li, Na, K, Ca, and Mg. Typically, in this embodiment, the polymer electrolyte and the gel electrolyte contain a lithium salt. The lithium salt is not particularly limited, but examples thereof include LiI, LiCl, LiBr, LiF, LiBF4, LiPF6, LiAsF6, LiSO3CF3, LiN(SO2F)2, LiN(SO2CF3)2, LiN(SO2CF3CF3)2, LiB(O2C2H4)2, LiB(C2O4)2, LiB(O2C2H4)F2, LiB(OCOCF3)4, LiNO3, and Li2SO4, and is preferably at least one selected from the group consisting of LiN(SO2F)2, LiN(SO2CF3)2, and LiN(SO2CF3CF3)2. The above-mentioned salts or lithium salts are used alone or in combination of two or more.

[0077] The blending ratio of the polymer and the lithium salt in the polymer electrolyte and the gel electrolyte may be determined by the ratio of the polar group of the polymer to the lithium atom of the lithium salt. For example, when the polymer has oxygen atoms, the blending ratio may be determined by the ratio ([Li] / [O]) of the number of oxygen atoms of the polymer to the number of lithium atoms of the lithium salt. In the polymer electrolyte and the gel electrolyte, the blending ratio of the polymer and the lithium salt may be adjusted so that the ratio ([Li] / [O]) is, for example, 0.02 to 0.20, 0.03 to 0.15, or 0.04 to 0.12.

[0078] The solvent contained in the gel electrolyte is not particularly limited, but for example, the solvents that can be contained in the electrolyte solution described later can be used alone or in combination of two or more. Preferred examples of the solvent are the same as those in the electrolyte solution described later. The plasticizer contained in the semi-solid polymer electrolyte is not particularly limited, but may include, for example, components similar to the solvent that may be contained in the gel electrolyte, and various oligomers.

[0079] The separator of the present embodiment may be coated with a separator coating layer. The separator coating layer may cover both sides of the separator, or may cover only one side. The separator coating layer is not particularly limited as long as it is a member that does not react with lithium ions, but it is preferable that it is a layer that can firmly bond the separator and a layer adjacent to the separator. Examples of such separator coating layers include, but are not particularly limited to, polyvinylidene fluoride (PVDF), a mixture of styrene butadiene rubber and carboxymethyl cellulose (SBR-CMC), polyacrylic acid (PAA), lithium polyacrylate (Li-PAA), polyimide (PI), polyamideimide (PAI), and those containing binders such as aramid. The separator coating layer may be formed by adding inorganic particles such as silica, alumina, titania, zirconia, magnesium oxide, magnesium hydroxide, and lithium nitrate to the binder.

[0080] The average thickness of the separator in this embodiment is preferably 20 μm or less, more preferably 18 μm or less, and even more preferably 15 μm or less. According to such an embodiment, the volume occupied by the separator in the lithium secondary battery is reduced, and the energy density of the lithium secondary battery is further improved. In addition, the average thickness of the separator is preferably 5 μm or more, more preferably 7 μm or more, and even more preferably 10 μm or more. According to such an embodiment, the positive electrode and the negative electrode can be more reliably separated, and the battery can be further prevented from being short-circuited.

[0081] (electrolyte) The lithium secondary battery 100 preferably further comprises an electrolyte. The electrolytic solution is a liquid containing a solvent and an electrolyte, and has ion conductivity. The electrolytic solution may be called a liquid electrolyte, and acts as a conductive path for lithium ions. Therefore, when a lithium secondary battery has an electrolytic solution, the internal resistance is further reduced, and the energy density, capacity, and cycle characteristics tend to be further improved. The electrolyte may be permeated into the separator 120, or the completed lithium secondary battery 100 may be formed by sealing the electrolyte together with a laminate of the negative electrode, separator, positive electrode, and positive electrode current collector.

[0082] The electrolyte contained in the electrolytic solution may be any electrolyte that can be contained in the polymer electrolyte or gel electrolyte, particularly the above-mentioned lithium salts, which may be used alone or in combination of two or more. The preferred lithium salts are the same as those in the polymer electrolyte and gel electrolyte.

[0083] Examples of the solvent contained in the electrolytic solution include non-aqueous solvents having fluorine atoms (hereinafter referred to as "fluorinated solvents") and non-aqueous solvents not having fluorine atoms (hereinafter referred to as "non-fluorinated solvents").

[0084] The fluorinated solvent is not particularly limited, but examples thereof include 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether. The non-fluorine solvent is not particularly limited, but examples thereof include triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, 1,2-dimethoxyethane, dimethoxyethane, dimethoxypropane, dimethoxybutane, diethylene glycol dimethyl ether, acetonitrile, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, chloroethylene carbonate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, trimethyl phosphate, triethyl phosphate, and 12-crown-4.

[0085] The above fluorinated solvents and / or non-fluorinated solvents may be used alone or in any combination of two or more in any ratio. The contents of the fluorinated solvent and non-fluorinated solvent are not particularly limited, and the ratio of the fluorinated solvent to the entire solvent may be 0 to 100% by volume, or the ratio of the non-fluorinated solvent to the entire solvent may be 0 to 100% by volume.

[0086] (Use of lithium secondary batteries) 2 shows one usage mode of the lithium secondary battery of the first embodiment. In the lithium secondary battery 100, a positive electrode terminal 220 and a negative electrode terminal 210 for connecting the lithium secondary battery 100 to an external circuit are joined to a positive electrode current collector 140 and a negative electrode 130, respectively. The lithium secondary battery 100 is charged and discharged by connecting the negative electrode terminal 210 to one end of the external circuit and the positive electrode terminal 220 to the other end of the external circuit.

[0087] More specifically, when an external power source is connected to the positive electrode terminal 220 and the negative electrode terminal 210, and a voltage is applied such that a current flows from the negative electrode terminal 210 (negative electrode 130) through the external power source to the positive electrode terminal 220 (positive electrode 110), the lithium secondary battery 100 is charged, and lithium metal is precipitated on the surface of the negative electrode. When the positive electrode terminal 220 and the negative electrode terminal 210 of the charged lithium secondary battery 100 are connected via a desired external circuit, the lithium secondary battery 100 is discharged. As a result, the lithium metal precipitated on the surface of the negative electrode is electrolytically dissolved.

[0088] As described above, the lithium-containing compound contained in the positive electrode of the present embodiment releases lithium ions under conditions where the battery voltage is about 4.3 V. Therefore, the lithium secondary battery of the present embodiment is preferably used in the following manner.

[0089] That is, the method of using the lithium secondary battery of the present embodiment includes performing a charge-discharge cycle including at least one discharge step and at least one charge step after charging at a cut-off voltage of 4.3 V or more and 5.0 V or less, and the cut-off voltage of the charge step in the charge-discharge cycle is less than the cut-off voltage in the first charge performed at a cut-off voltage of 4.3 V or more and 5.0 V or less. According to such a method of use, since the lithium secondary battery of the present embodiment is surely charged at a cut-off voltage of 4.3 V or more and 5.0 V or less, Li6Mn x Co 1-x The lithium-containing compound represented by O4 (0 < x < 1) effectively and surely acts as a sacrificial positive electrode agent. Further, in the charge step in the subsequent charge-discharge cycle, by setting the cut-off voltage to be less than the cut-off voltage at the first charge, it is possible to effectively and surely suppress the decomposition of each component in the lithium secondary battery (particularly the solvent in the electrolyte when the positive electrode active material and the electrolyte are included), and the cycle characteristics can be further improved.

[0090] In the method of using the lithium secondary battery of the present embodiment, the cut-off voltage in the first charge before performing the charge-discharge cycle is preferably more than 4.3 V, more preferably 4.4 V or more, and may be 4.5 V or more, 4.6 V or more, or 4.7 V or more. Further, the cut-off voltage is preferably less than 5.0 V, more preferably 4.9 V or less, still more preferably 4.8 V or less, and even more preferably 4.7 V or less. The cut-off voltage in the first charge may be within a range obtained by arbitrarily combining the above upper and lower limit values. For example, it may be more than 4.3 V and less than 5.0 V, 4.4 V or more and 4.9 V or less, or 4.4 V or more and 4.7 V or less. By setting the cut-off voltage in the first charge before performing the charge-discharge cycle within the above range, the cycle characteristics of the lithium secondary battery tend to be further enhanced.

[0091] The number of charge-discharge cycles carried out after charging with a cut-off voltage above 4.3V and below 5.0V is not particularly limited. For example, the charge-discharge cycles may be repeated until the discharge capacity becomes 80% or less, 70% or less, or 60% or less of the discharge capacity in the discharge process of the first charge-discharge cycle performed immediately after the first charge. The above charge-discharge cycles may be carried out under any conditions as long as the cut-off voltage in the charging process is less than the cut-off voltage during the first charge. The cut-off voltage in the charging process may be, for example, a cut-off voltage 0.1V, 0.2V, or 0.3V lower than the cut-off voltage during the first charge. Also, the above charge-discharge cycles are preferably further carried out within a voltage range where no reduction reaction occurs in the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1). That is, the above charge-discharge cycles are preferably carried out within a voltage range where the cut-off voltage in the charging process is less than the cut-off voltage during the first charge and where no reduction reaction occurs in the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1). Such a voltage range is, for example, 2.5V or more and 4.6V or less, preferably 2.5V or more and 4.3V or less, and more preferably 3.0V or more and 4.2V or less.

[0092] Note that the above-described content as the method of using the lithium secondary battery of this embodiment only shows a preferred method when using the lithium secondary battery of this embodiment and does not limit the method of using the lithium secondary battery of this embodiment. For example, in the initial charging of the lithium secondary battery of this embodiment, the cut-off voltage may be outside the range of 4.3V or more and 5.0V or less, and the voltage range of the subsequent charge-discharge cycles may be equal to or higher than the cut-off voltage during the first charge.

[0093] (Method for manufacturing a lithium secondary battery) As a method for manufacturing the lithium secondary battery 100 as shown in FIG. 1, there is no particular limitation as long as it is a method capable of manufacturing a lithium secondary battery having the above-described configuration. For example, the following methods can be mentioned. Note that the lithium secondary battery of the present embodiment, particularly the positive electrode of the present embodiment, is preferably manufactured in an environment where a certain degree of humidity is excluded, such as a dry room with a dew point of -50 to -10°C.

[0094] The positive electrode 110 is formed on the positive electrode current collector 140, for example, as follows. In addition to the above-described positive electrode active material and the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1), optionally, a sacrificial positive electrode agent, a conductive assistant, a binder, and / or an electrolyte other than the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) are mixed to obtain a positive electrode mixture. The blending ratio may be appropriately adjusted so that each component is within the above-described range. The obtained positive electrode mixture is applied to one side of a metal foil (for example, an Al foil) as a positive electrode current collector having a predetermined thickness (for example, 5 μm or more and 1 mm or less), and press-molded. The obtained molded body is punched into a predetermined size by punching to obtain the positive electrode 110.

[0095] Note that the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) can be manufactured by pulverizing and mixing powders of Li2O, MnO, and CoO and firing them at, for example, 600 to 1000°C for 5 to 100 hours. The atmospheric conditions during firing are preferably an inert gas atmosphere such as argon and nitrogen gas, and a trace amount of hydrogen gas may be included. The ratio of hydrogen gas can be, for example, 0.1 to 10% by volume ratio. Commercially available powders of Li2O, MnO, and CoO may be used, and the mixing ratio (molar ratio) thereof is preferably such that Li2O:(MnO, CoO) = 3:1. Further, by appropriately adjusting the blending ratio of MnO and CoO, Li6Mn x Co 1-xThe value x in O4 can be controlled. Alternatively, Li6Mn x Co 1-x The lithium-containing compound represented by O4 (0 < x < 1) may be produced by a coprecipitation method.

[0096] Next, a separator 120 having the above-described configuration is prepared. The separator 120 may be manufactured by a conventionally known method or a commercially available one may be used.

[0097] Next, the above-described negative electrode material, for example, a metal foil of 1 μm or more and 1 mm or less (for example, an electrolytic Cu foil) is washed with a solvent containing sulfamic acid, punched into a predetermined size, and further ultrasonically washed with ethanol and then dried to obtain a negative electrode 130.

[0098] The positive electrode 110 provided with the positive electrode current collector 140 on one side, the separator 120, and the negative electrode 130 obtained as described above are laminated in this order to obtain a laminate. The obtained laminate is sealed in a sealed container together with an electrolytic solution to obtain a lithium secondary battery 100. The sealed container is not particularly limited, and examples thereof include a laminate film.

[0099] The lithium secondary battery 100 obtained as described above is used after being initially charged. The initial charging may be performed before the battery is provided to the user, or may be performed by the user after the battery is provided to the user. From the viewpoint of effectively and surely exhibiting the effects of the lithium secondary battery of the present embodiment, it is preferable that the initial charging is performed before the battery is provided to the user, that is, it is preferable that the lithium secondary battery of the present embodiment includes a step of initially charging the battery as one step of the manufacturing process.

[0100] Therefore, the method for manufacturing the lithium secondary battery 100 preferably includes a step of initially charging the battery obtained as described above. The initial charging may be CC charging (constant current charging) or CV charging (low voltage charging), or may be CC-CV charging, CV-CC charging, or CC-CV-CC charging. Further, the initial charging is preferably performed under charging conditions where the cut-off voltage is 4.3 V or more and 5.0 V or less.

[0101] In the above initial charging, the cut-off voltage is preferably more than 4.3 V, more preferably 4.4 V or more, and may be 4.5 V or more, 4.6 V or more, or 4.7 V or more. Also, the cut-off voltage is preferably less than 5.0 V, more preferably 4.9 V or less, still more preferably 4.8 V or less, and even more preferably 4.7 V or less. The cut-off voltage in the above initial charging may be within a range obtained by arbitrarily combining the above upper and lower limit values, for example, more than 4.3 V and less than 5.0 V, 4.4 V or more and 4.9 V or less, or 4.4 V or more and 4.7 V or less. By setting the cut-off voltage in the initial charging before performing charge-discharge cycles within the above range, the cycle characteristics of the manufactured lithium secondary battery tend to be further improved.

[0102] [Second Embodiment] (Lithium Secondary Battery) Figure 3 is a schematic cross-sectional view of a lithium secondary battery according to the lithium secondary battery of the second embodiment (hereinafter referred to as the "second embodiment"). The lithium secondary battery 300 of the second embodiment includes a positive electrode 110 and a negative electrode 130 having no negative electrode active material, similar to the lithium secondary battery 100 of the first embodiment. The positive electrode 110 includes a positive electrode active material and a lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 <x <1). The lithium secondary battery 100 includes a separator 120 between the positive electrode 110 and the negative electrode 130, and the positive electrode 110 has a positive electrode current collector 140 on a surface opposite to the surface facing the separator 120. The lithium secondary battery 300 of the second embodiment differs from the lithium secondary battery 100 in that it is provided with a fibrous or porous buffer functional layer 310 having ionic conductivity and electrical conductivity, which is formed on the surface of the separator 120 facing the negative electrode 130.

[0103] In the lithium secondary battery 300, the configurations and preferred aspects of the positive electrode current collector, positive electrode, separator, and negative electrode are similar to those of the lithium secondary battery 100 of the first embodiment, and with respect to these configurations, the lithium secondary battery of the second embodiment exhibits the same effects as the lithium secondary battery of the first embodiment. Similarly to the lithium secondary battery 100, the lithium secondary battery of the second embodiment may contain an electrolyte solution as described above.

[0104] (buffer layer) As shown in FIG. 3, the buffer functional layer 310 is formed on the surface of the separator 120 facing the negative electrode 130. The buffer functional layer is fibrous or porous and has ionic and electrical conductivity. Here, since the buffer functional layer 310 is fibrous or porous, it has a solid portion having ionic and electrical conductivity, and a pore portion (same as "gap portion"; the same applies hereinafter in this specification) formed by the gaps in the solid portion. In this specification, the "solid portion" in the buffer functional layer includes a gel-like portion.

[0105] Since the buffer functional layer 310 is configured as described above, when the lithium secondary battery is charged, electrons from the negative electrode and lithium ions from the separator and / or electrolyte are supplied to the solid portion. As a result, the electrons and lithium ions supplied as described above react on the surface of the solid portion, and lithium metal is precipitated in the vacant portions (surface of the solid portion). Therefore, the buffer functional layer 310 has the effect of suppressing the volume expansion of the battery caused by the precipitation of lithium metal when the battery is charged. In other words, the lithium secondary battery 300 can further suppress the volume expansion or volume change caused by charging and discharging compared to the lithium secondary battery 100.

[0106] The inventors have found that in the lithium secondary battery of this embodiment, even if a buffer functional layer is introduced as in the lithium secondary battery of the second embodiment, the cycle characteristics of the battery do not decrease or can even be improved. The inventors speculate that the reason for this is that the introduction of the buffer functional layer increases the surface area of ​​the site where lithium metal can be precipitated, so that the reaction rate of the lithium metal precipitation reaction is controlled slowly and the formation of lithium metal grown in a dendritic shape is more reliably suppressed.

[0107] In the second embodiment, "lithium metal is deposited on the negative electrode" means that lithium metal is deposited on at least one of the surface of the negative electrode and the surface of the solid part of the buffer functional layer, unless otherwise specified. Therefore, in the lithium secondary battery of the second embodiment, lithium metal may be deposited, for example, on the surface of the negative electrode (the interface between the negative electrode and the buffer functional layer) or inside the buffer functional layer (the surface of the solid part of the buffer functional layer).

[0108] The buffer functional layer 310 is not particularly limited as long as it is fibrous or porous and has ion conductivity and electrical conductivity. Non-limiting examples of the buffer functional layer 310 include a fibrous or porous ion conductive layer whose surface is entirely or partially coated with an electrical conductive layer, a fibrous or porous electrical conductive layer whose surface is entirely or partially coated with an ion conductive layer, and a fibrous ion conductive layer and a fibrous electrical conductive layer intertwined with each other.

[0109] The ion-conducting layer is not limited as long as it can conduct ions, and examples thereof include the polymer electrolyte and gel electrolyte exemplified as the electrolyte in the separator of the lithium secondary battery of the first embodiment.

[0110] The electrically conductive layer may be any material capable of conducting electrons, and may be, for example, a metal film. Non-limiting examples of metals that may be contained in the electrically conductive layer include, for example, SUS, Si, Sn, Sb, Al, Ni, Cu, Sn, Bi, Ag, Au, Pt, Pb, Zn, In, Bi-Sn, and In-Sn. From the viewpoint of increasing the affinity with lithium metal, the metals contained in the electrically conductive layer are preferably Si, Sn, Zn, Bi, Ag, In, Pb, Sb, and Al. The above-mentioned metals may be used alone or in combination of two or more.

[0111] One embodiment of the buffer functional layer 310 is a fibrous buffer functional layer. Fig. 4(A) shows a schematic cross-sectional view of a fibrous buffer functional layer. The buffer functional layer 310 shown in Fig. 4(A) is made of ion-conductive fiber 410, which is a fiber having ionic conductivity and electrical conductivity. That is, in this embodiment, "the buffer functional layer is fibrous" means that the buffer functional layer includes fiber or is made of fiber, and has a solid portion and a void portion formed by the gap between the solid portion.

[0112] When a lithium secondary battery having the buffer functional layer 310 shown in Fig. 4(A) is charged, lithium metal is precipitated on the surface of the solid part of the buffer functional layer, i.e., the surface of the ion-conducting fiber 410. Therefore, according to such an embodiment, as shown in the schematic cross-sectional view of Fig. 4(B), lithium metal 420 is precipitated on the surface of the ion-conducting fiber 410, which is the solid part of the buffer functional layer, so as to fill the pores in the buffer functional layer.

[0113] An embodiment of the ionic electrically conductive fiber 410 is shown in a schematic cross-sectional view in Fig. 4(C). As shown in Fig. 4(C), in one embodiment, the ionic electrically conductive fiber 410 comprises a fibrous ion conductive layer 430 and an electrically conductive layer 440 that covers the surface of the ion conductive layer 430. The ion conductive layer 430 may have a configuration as described above for the ion conductive layer, and the electrically conductive layer 440 may have a configuration as described above for the electrically conductive layer.

[0114] The average fiber diameter of the fibrous ion conducting layer 430 is preferably 30 nm or more and 5000 nm or less, more preferably 50 nm or more and 2000 nm or less, even more preferably 70 nm or more and 1000 nm or less, and even more preferably 80 nm or more and 500 nm or less. When the average fiber diameter of the ion conducting layer is within the above range, the surface area of ​​the reaction field where lithium metal can be deposited becomes more appropriate, which tends to further improve the cycle characteristics.

[0115] The average thickness of the electrically conductive layer 440 is preferably 1 nm to 300 nm, more preferably 5 nm to 200 nm, and even more preferably 10 nm to 150 nm. When the average thickness of the electrically conductive layer is within the above range, the electrical conductivity of the ion-conducting fiber 410 can be more appropriately maintained, and the cycle characteristics tend to be further improved.

[0116] In another embodiment, the buffer functional layer 310 may be porous. The porous buffer functional layer may include, for example, an ion conductive layer having a porous shape, particularly, continuous pores, and an electric conductive layer covering the surface of the ion conductive layer.

[0117] The buffer functional layer 310 has pores because it is fibrous or porous. The porosity of the buffer functional layer is not particularly limited, but is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more, in volume percent. When the porosity of the buffer functional layer is within the above range, the surface area of ​​the reaction site where lithium metal can be precipitated is further increased, so that the cycle characteristics tend to be further improved. In addition, according to such an embodiment, the effect of suppressing cell volume expansion tends to be more effective and reliable. The porosity of the buffer functional layer is not particularly limited, but may be 99% or less, 95% or less, or 90% or less, in volume percent.

[0118] The average thickness of the buffer functional layer 310 is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 30 μm or less. When the average thickness of the buffer functional layer is within the above range, the volume occupied by the buffer functional layer 310 in the lithium secondary battery 300 is reduced, and the energy density of the battery is further improved. In addition, the average thickness of the buffer functional layer is preferably 1 μm or more, more preferably 4 μm or more, and even more preferably 7 μm or more. When the average thickness of the buffer functional layer is within the above range, the surface area of ​​the reaction field where lithium metal can be precipitated is further increased, and the cycle characteristics tend to be further improved. In addition, according to such an embodiment, the effect of suppressing cell volume expansion tends to be more effective and reliable.

[0119] The fiber diameter of the fibrous ion conductive layer, the thickness of the electrically conductive layer, the porosity of the buffer functional layer, and the thickness of the buffer functional layer can be measured by known measuring methods. For example, the thickness of the buffer functional layer can be measured by etching the surface of the buffer functional layer with a focused ion beam (FIB) to expose its cross section, and observing the thickness of the buffer functional layer at the exposed cut surface with an electron microscope.

[0120] The fiber diameter of the fibrous ion conductive layer, the thickness of the electric conductive layer, and the porosity of the buffer functional layer can be measured by observing the surface of the buffer functional layer with an electron microscope. The porosity of the buffer functional layer can be calculated by performing a binary analysis of the observed image of the surface of the buffer functional layer using image analysis software and determining the ratio of the area of ​​the buffer functional layer to the total area of ​​the image. Each of the above measured values ​​is calculated by averaging measurements taken three or more times, preferably ten or more times.

[0121] When the buffer functional layer 310 contains a metal that can react with lithium, the total capacity of the negative electrode 130 and the buffer functional layer 310 is sufficiently small relative to the capacity of the positive electrode 110, for example, 20% or less, 15% or less, 10% or less, or 5% or less. The capacities of the positive electrode 110, the negative electrode 130, and the buffer functional layer 310 can be measured by a conventionally known method.

[0122] (Lithium secondary battery manufacturing method) In the method for producing the lithium secondary battery of the second embodiment, the production of components other than the buffer function layer, the assembly of each component, and the subsequent initial charging can be carried out in the same manner as in the method for producing the lithium secondary battery of the first embodiment.

[0123] The method for producing the buffer functional layer 310 is not particularly limited as long as it can produce a fibrous or porous layer having ion conductivity and electrical conductivity. For example, the method may be as follows.

[0124] As shown in FIG. 4(C), a fibrous buffer functional layer having an ion electrically conductive fiber 410 including a fibrous ion conductive layer 430 and an electrically conductive layer 440 covering the surface of the ion conductive layer 430 can be manufactured as follows. First, a solution of the above-mentioned resin (e.g., PVDF) dissolved in an appropriate organic solvent (e.g., N-methylpyrrolidone) is applied to the surface of a separator 120 prepared in advance using a doctor blade. Next, the separator 120 to which the resin solution has been applied is immersed in a water bath and then thoroughly dried at room temperature to form a fibrous ion-conducting layer on the separator 120 (note that the ion-conducting layer may be made to exhibit ion-conducting function by, for example, injecting an electrolyte solution during assembly of the battery). Next, a fibrous buffer function layer can be obtained by depositing an appropriate metal (e.g., Ni) under vacuum conditions onto the separator on which the fibrous ion-conducting layer has been formed.

[0125] A porous buffer functional layer including a porous ion conductive layer and an electric conductive layer covering the surface of the ion conductive layer can be produced as follows. First, using a solution obtained by dissolving the above-described resin (e.g., PVDF) in an appropriate solvent (e.g., N-methylpyrrolidone), a porous ion-conductive layer having through-holes is formed on the surface of the separator 120 by a conventionally known method (e.g., a method using phase separation with a solvent, a method using a foaming agent, etc.). (Note that the ion-conductive layer may exhibit an ion-conductive function, for example, when an electrolytic solution is poured during battery assembly.) Subsequently, a porous buffer function layer can be obtained by vapor-depositing an appropriate metal (e.g., Ni) on the separator on which the porous ion-conductive layer is formed under vacuum conditions.

[0126] [Method for manufacturing a lithium secondary battery] The present invention also provides a method for manufacturing a lithium secondary battery. Hereinafter, the method for manufacturing a lithium secondary battery of the present embodiment (hereinafter referred to as "the manufacturing method of the present embodiment") will be described in detail. The manufacturing method of the present embodiment includes a step of preparing a positive electrode containing a positive electrode active material and a lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1), and a negative electrode having no negative electrode active material, a step of arranging the positive electrode and the negative electrode so that they face each other, and a step of applying a voltage between the positive electrode and the negative electrode and performing initial charging under charging conditions where the cut-off voltage is 4.3 V or more and 5.0 V or less.

[0127] As described above, the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) starts to release lithium ions under conditions where the voltage of the battery reaches about 4.3 V during initial charging and tends to act as a sacrificial positive electrode agent. Therefore, according to the manufacturing method of the present embodiment including the step of performing initial charging under charging conditions where the cut-off voltage is 4.3 V or more and 5.0 V or less, the function of the lithium-containing compound represented by Li6Mn x Co 1-x O4 (0 < x < 1) as a sacrificial positive electrode agent can be effectively and surely exhibited, and a lithium secondary battery having excellent cycle characteristics can be manufactured. Further, Li6Mn x Co 1-xThe lithium-containing compound represented by O4(0 < x < 1) has excellent stability in the atmosphere and can be handled without strictly controlling humidity and the like, so the above manufacturing method has high productivity. Hereinafter, each step will be described. Note that the manufacturing method of the present embodiment, particularly the positive electrode preparation step, is preferably carried out in an environment where a certain degree of humidity is excluded, such as a dry room with a dew point of -50 to -10°C.

[0128] (Positive electrode and negative electrode preparation step) In the manufacturing method of the present embodiment, first, a positive electrode containing a positive electrode active material and a lithium-containing compound represented by Li6Mn x Co 1-x O4(0 < x < 1), and a negative electrode having no negative electrode active material are prepared. The configurations and preferred embodiments of the positive electrode and the negative electrode are the same as those in the lithium secondary battery of the above-described present embodiment. Also, the configurations and preferred embodiments of the positive electrode active material and the lithium-containing compound represented by Li6Mn x Co 1-x O4(0 < x < 1) contained in the positive electrode are also the same as those in the lithium secondary battery of the above-described present embodiment. In this step, a positive electrode and a negative electrode having such a configuration are prepared. Such positive and negative electrodes may be obtained by purchasing commercially available ones, or may be manufactured by the method described in the description of the lithium secondary battery of the present embodiment. Also, the preparation of the positive electrode and the negative electrode may be performed simultaneously or separately. When the preparation of the positive electrode and the negative electrode is performed separately, the order is not particularly limited.

[0129] (Positive electrode and negative electrode arrangement step) In the manufacturing method of the present embodiment, after the positive electrode and negative electrode preparation step, a step of arranging the positive electrode and the negative electrode so that they face each other is performed. In this step, there is no particular limitation as long as the positive electrode and the negative electrode are arranged so that they face each other. Only the positive electrode and the negative electrode may be arranged, or the positive electrode and the negative electrode may be opposed to each other via a separator and / or a buffer function layer as in the lithium secondary batteries 100 and 300 described above. However, the positive electrode and the negative electrode shall not be physically or electrically contacted.

[0130] In the positive electrode and negative electrode arrangement step, a plurality of sets of combinations of positive electrodes and negative electrodes may be arranged. In this case, it is preferable that the positive electrodes and negative electrodes are arranged so as to be alternately stacked. When a separator and / or a buffer functional layer is arranged, the configuration and preferred aspects of the separator and buffer functional layer are the same as those in the lithium secondary battery of this embodiment described above, and can be obtained or manufactured by the method described in the explanation of the lithium secondary battery of this embodiment.

[0131] (Initial charging process) In the manufacturing method of this embodiment, after the positive electrode and negative electrode arrangement step, a step of initially charging is carried out by applying a voltage between the positive electrode and the negative electrode under charging conditions in which the cutoff voltage is 4.3 V or more and 5.0 V or less. The initial charging may be CC charging (constant current charging) or CV charging (low voltage charging), and may be CC-CV charging, CV-CC charging, or CC-CV-CC charging.

[0132] In the initial charging step, the cutoff voltage is preferably more than 4.3 V, more preferably 4.4 V or more, and may be 4.5 V or more, 4.6 V or more, or 4.7 V or more. The cutoff voltage is preferably less than 5.0 V, more preferably 4.9 V or less, even more preferably 4.8 V or less, and even more preferably 4.7 V or less. The cutoff voltage in the initial charge may be within a range obtained by any combination of the upper and lower limits, for example, more than 4.3 V and less than 5.0 V, 4.4 V or more and 4.9 V or less, or 4.4 V or more and 4.7 V or less. By setting the cutoff voltage within the above range, a lithium secondary battery having even better cycle performance tends to be manufactured.

[0133] (Other processes) The manufacturing method of this embodiment may include steps other than the positive and negative electrode preparation step, the positive and negative electrode arrangement step, and the initial charging step. Such steps include, for example, a separator preparation step and a buffer functional layer preparation step, which are performed as necessary before the positive and negative electrode arrangement step, and an electrolyte injection step, which is performed as necessary between the positive and negative electrode arrangement step and the initial charging step, and a subsequent sealing step. These steps can be performed based on the matters described in the description of the lithium secondary battery of the first or second embodiment.

[0134] Specifically, the electrolyte injection step and the subsequent sealing step may be carried out as follows. First, the laminate including the positive electrode and the negative electrode obtained in the positive electrode and negative electrode arrangement step is held in a sealed container with at least one end open. Then, the electrolyte injection step is carried out by injecting the electrolyte that may be contained in the lithium secondary battery of the present embodiment into the sealed container. Next, the sealing step is carried out to obtain a battery as a product by sealing the open portion of the sealed container.

[0135] [Variations] The above-described embodiment is an example for explaining the present invention, and is not intended to limit the present invention to only this embodiment. The present invention can be modified in various ways without departing from the gist of the invention.

[0136] The lithium secondary battery of this embodiment may or may not have a current collector arranged on the negative electrode surface so as to contact the negative electrode. Such a current collector is not particularly limited, but may be, for example, a material that can be used for a negative electrode material. In addition, the lithium secondary battery of this embodiment may not have a positive electrode current collector. In addition, when the lithium secondary battery does not have a positive electrode current collector and a negative electrode current collector, the positive electrode and the negative electrode themselves act as current collectors, respectively.

[0137] In the lithium secondary battery of this embodiment, a terminal for connecting to an external circuit may be attached to the positive electrode current collector and / or the negative electrode. For example, a metal terminal (e.g., Al, Ni, etc.) having a thickness of 10 μm to 1 mm may be bonded to one or both of the positive electrode current collector and the negative electrode. As a bonding method, a conventionally known method may be used, for example, ultrasonic welding may be used.

[0138] The separator 120 may be omitted in the lithium secondary battery 100. In that case, it is preferable to fix the positive electrode 110 and the negative electrode 130 in a state where they are sufficiently separated from each other so that they are not in physical or electrical contact with each other.

[0139] In the buffer functional layer 310 of the lithium secondary battery 300, the ion conductive layer and the electric conductive layer are not limited to being layer-shaped, and may be fibrous, blocky, or porous. Therefore, in this specification, the terms ion conductive layer and electric conductive layer may be alternatively referred to as ion conductive phase and electric conductive phase, respectively.

[0140] In this specification, "high energy density" or "having a high energy density" means that the capacity per unit total volume or total mass of the battery is high, and is preferably 700 Wh / L or more or 300 Wh / kg or more, more preferably 800 Wh / L or more or 350 Wh / kg or more, and even more preferably 900 Wh / L or more or 400 Wh / kg or more.

[0141] In addition, in this specification, "having excellent cycle characteristics" means that the capacity of the battery is reduced at a low rate before and after a number of charge / discharge cycles that can be expected in normal use. That is, when comparing the first discharge capacity after the initial charge / discharge and the capacity after a number of charge / discharge cycles that can be expected in normal use, the capacity after the charge / discharge cycle is almost not reduced compared to the first discharge capacity after the initial charge / discharge. Here, the "number of times that can be expected in normal use" is, for example, 30 times, 50 times, 70 times, 100 times, 300 times, or 500 times, depending on the application of the lithium secondary battery. In addition, "the capacity after the charge / discharge cycle is almost not reduced compared to the first discharge capacity after the initial charge / discharge" means, for example, that the capacity after the charge / discharge cycle is 60% or more, 65% or more, 70% or more, 75% or more, 80% or more, or 85% or more compared to the first discharge capacity after the initial charge / discharge, depending on the application of the lithium secondary battery.

[0142] In this specification, the numerical ranges described as preferred ranges etc. may be replaced with numerical ranges obtained by arbitrarily combining the upper and lower limit values ​​described. For example, when a certain parameter is preferably 50 or more, more preferably 60 or more, and preferably 100 or less, more preferably 90 or less, the parameter may be any of 50 or more and 100 or less, 50 or more and 90 or less, 60 or more and 100 or less, or 60 or more and 90 or less. EXAMPLES

[0143] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.

[0144] [Method for measuring irreversible capacity density of lithium-containing compounds] The irreversible capacity density of the lithium-containing compound used as the sacrificial positive electrode agent in each example, i.e., the difference between the charge capacity density and the discharge capacity density, was measured as follows. First, each lithium-containing compound was mixed with polyvinylidene fluoride, carbon black, and N-methylpyrrolidone (NMP) to prepare a slurry, which was then applied onto aluminum foil, dried, and pressed. A test cell was prepared using this electrode as the working electrode and lithium metal as the counter electrode, and a 0.2 mAh / cm 2 The battery was CC-charged at a current of 100 mAh / g with a cutoff voltage of a predetermined value, and then CC-discharged until the voltage reached 3.0 V. The irreversible capacity density (mAh / g) was calculated by calculating the difference between the measured charge capacity density and discharge capacity density.

[0145] [Production and performance evaluation of lithium secondary batteries] [Example 1] The lithium secondary battery of Example 1 was fabricated as follows.

[0146] (Preparation of the negative electrode) A 10 μm electrolytic Cu foil was washed with a solvent containing sulfamic acid, and then punched out to a specified size (45 mm×45 mm). The foil was then ultrasonically cleaned with ethanol and dried to prepare a negative electrode.

[0147] (Preparation of positive electrode) In a dry room with a dew point of -30°C, 92.7 parts by mass of LiNi 0.85 Co 0.12 Al 0.03 O2, 3.3 parts by mass of Li6Mn 0.5 Co 0.5 A positive electrode mixture was obtained by mixing O4, 2.0 parts by mass of carbon black as a conductive assistant, 2.0 parts by mass of polyvinylidene fluoride (PVDF) as a binder, and N-methylpyrrolidone (NMP) as a solvent. The obtained positive electrode mixture was applied to one side of a 12 μm Al foil as a positive electrode current collector and press-molded, and then punched out to a specified size (40 mm × 40 mm) by punching to obtain a positive electrode.

[0148] Li6Mn 0.5 Co 0.5 Li2O4 was produced as follows. First, commercially available Li2O, MnO, and CoO powders were added to a container in a molar ratio of 6:1:1, crushed, and mixed. The resulting mixture was fired at 800°C for 12 hours under a gas flow consisting of 99% argon gas and 1% hydrogen gas by volume, to produce Li6Mn 0.5 Co 0.5 Got O4.

[0149] (Preparation of separator) A separator of a given size (50 mm×50 mm) was prepared, in which both sides of a 12 μm polyethylene microporous membrane were coated with 2 μm polyvinylidene fluoride (PVDF).

[0150] (Battery Assembly) A 4.0M solution of LiN(SO2F)2 (LFSI) in dimethoxyethane (DME) was prepared as the electrolyte. Next, the positive electrode current collector, the positive electrode, the separator, and the negative electrode were stacked in this order to obtain a laminate. Furthermore, a 100 μm Al terminal and a 100 μm Ni terminal were joined to the positive electrode current collector and the negative electrode, respectively, by ultrasonic welding, and then inserted into a laminate exterior body. Next, the above-mentioned electrolyte was injected into the exterior body. The exterior body was sealed to obtain a lithium secondary battery.

[0151] (Initial charging) Then, the lithium secondary battery was charged at 2.0 mA (0.05 C; 0.125 mA / cm 2 ) and initially charged by CC charging with a cutoff voltage of 4.7 V.

[0152] [Examples 2 to 3] A lithium secondary battery was fabricated in the same manner as in Example 1, except that the composition of the lithium-containing compound was as shown in Table 1, and then the initial charge was performed. 0.7 Co 0.3 O4 is Li2O, MnO, and CoO powders added in a molar ratio of 30:7:3, and Li6Mn 0.3 Co0.7 O4 was produced by adding Li2O, MnO, and CoO powders in a molar ratio of 30:3:7.

[0153] [Comparative Example 1] A lithium secondary battery was fabricated in the same manner as in Example 1, except that Li6MnO4 was used as the lithium-containing compound, and then an initial charge was performed. The Li6MnO4 was produced by adding Li2O and MnO powders at a molar ratio of 3:1.

[0154] [Comparative Example 2] Except for using Li6CoO4 as the lithium-containing compound, an attempt was made to fabricate a lithium secondary battery in the same manner as in Example 1. However, when Li6CoO4 was used, the positive electrode mixture gelled, and a lithium secondary battery could not be fabricated under the same conditions. Li6MnO4 was produced by adding Li2O and CoO powders at a molar ratio of 3:1.

[0155] [Evaluation of cycle characteristics] The energy density and cycle characteristics of the lithium secondary batteries produced in each of the Examples and Comparative Examples were evaluated as follows.

[0156] The lithium secondary batteries of each example were initially charged as described above at 2.0 mA (0.05 C; 0.125 mA / cm 2 ) until the voltage reached 3.0 V (initial discharge). Then, the battery was discharged at 20 mA (0.5 C; 1.25 mA / cm 2 ) until the voltage reached 4.2 V, then 20 mA (0.5 C; 1.25 mA / cm 2) Then, the charge-discharge cycle of discharging until the voltage reaches 3.0 V was repeated 99 more cycles in an environment with a temperature of 25°C. The ratio of the discharge capacity obtained from the discharge in the 100th cycle to the discharge capacity obtained from the discharge in the 2nd cycle (when the initial charge-discharge cycle was counted as the 1st cycle) was calculated as the capacity retention rate (%) and used as an index of the cycle characteristics. The higher the capacity retention rate, the better the cycle characteristics. The capacity retention rates in each example are shown in Table 1.

[0157]

Table 1

[0158] In Table 1, the irreversible capacity density is the value measured by the above method with the charge cut-off voltage being 4.7 V. Also, the addition rate means the ratio of the irreversible capacity of the lithium-containing compound to the cell capacity obtained from the initial discharge of the battery. Note that in Comparative Example 2, since a lithium secondary battery could not be stably fabricated as described above, the performance evaluation of the battery was not conducted.

[0159] From Table 1, it was found that the examples using Li6Mn x Co 1-x O4 (0 < x < 1) as the sacrificial cathode agent are excellent in cycle characteristics and productivity compared to the comparative examples using Li6MnO4 or Li6CoO4.

[0160] [Evaluation of the Influence of the Cut-off Voltage during Initial Charging on Cycle Characteristics] Next, in the lithium secondary batteries fabricated in Examples 1 to 3, it was investigated how the capacity retention rate changes when the cut-off voltage of the initial charging is changed.

[0161] [Test Examples 1 to 5] First, the composition is Li6Mn 0.5 Co 0.5The lithium secondary battery of Example 1 containing the lithium-containing compound O4 was initially charged in the same manner as in Example 1, except that the cutoff voltage was 4.2 V, 4.3 V, 4.4 V, 4.7 V, or 5.0 V. The capacity retention rate was then measured in the same manner as above. The capacity retention rate in each example is shown in Table 2.

[0162] [Test Examples 6-7] The composition is Li6Mn 0.7 Co 0.3 The lithium secondary battery of Example 2 containing the lithium-containing compound O4 was initially charged in the same manner as in Example 1, except that the cutoff voltage was 4.4 V or 4.7 V. The capacity retention rate was then measured in the same manner as above. The capacity retention rates in each example are shown in Table 2.

[0163] [Test Examples 8-9] The composition is Li6Mn 0.3 Co 0.7 The lithium secondary battery of Example 3 containing the lithium-containing compound O4 was initially charged in the same manner as in Example 1, except that the cutoff voltage was 4.4 V or 4.7 V. The capacity retention rate was then measured in the same manner as above. The capacity retention rates in each example are shown in Table 2.

[0164] [Table 2]

[0165] From the results of Test Examples 1 to 5, it was found that the lithium secondary battery of this embodiment has higher cycle characteristics when initially charged with a cutoff voltage in a predetermined range. Also, from the results of Test Examples 6 to 9, it was found that the cycle characteristics are higher when initially charged with a cutoff voltage in a predetermined range, regardless of the composition of the lithium-containing compound as the sacrificial positive electrode agent.

[0166] [Introduction of a buffer layer] Next, in the lithium secondary battery of this embodiment, the change in cycle characteristics when a buffer functional layer is introduced was examined.

[0167] [Example 4] A lithium secondary battery of Example 4 was produced as follows. First, a positive electrode having a positive electrode current collector, a negative electrode, a separator, and an electrolyte were prepared in the same manner as in Example 3. Next, a buffer functional layer was formed on one side of the separator as follows.

[0168] A resin solution in which PVDF resin was dissolved in N-methylpyrrolidone (NMP) was applied to the separator using a bar coater. Next, the separator with the resin solution applied was immersed in a water bath and then thoroughly dried at room temperature to form a fiber-shaped ion-conducting layer on the separator (Note that the ion-conducting layer exhibits ion-conducting function when an electrolyte (a 4M solution of LiN(SO2F)2 (LFSI) in dimethoxyethane (DME)) described later is injected during the assembly of the battery). The average fiber diameter of the fibrous ion-conducting layer formed on the separator was measured by observation with a scanning electron microscope (SEM) and found to be 100 nm.

[0169] Next, Ni was evaporated under vacuum conditions onto the separator with the fibrous ion conductive layer formed. When the ion conductive layer after Ni evaporation was observed using an SEM equipped with an energy dispersive X-ray analyzer (EDX), it was confirmed that Ni was distributed so as to cover the fibrous ion conductive layer, and that a fibrous buffer functional layer had been obtained in which the surface of the fibrous ion conductive layer was covered with an electrical conductive layer. In addition, when a cross section of the buffer functional layer was prepared by FIB and observed by SEM, the average thickness of the buffer functional layer was 10 μm. When the buffer functional layer was observed by a transmission electron microscope, the average thickness of the Ni thin film, which is the electrically conductive layer, and the porosity of the buffer functional layer were 20 nm and 90%, respectively.

[0170] Next, the positive electrode current collector, the positive electrode, the separator with the buffer functional layer formed thereon, and the negative electrode were laminated in this order to obtain a laminate. The laminate was laminated so that the buffer functional layer faced the negative electrode. Furthermore, a 100 μm Al terminal and a 100 μm Ni terminal were joined to the positive electrode current collector and the negative electrode, respectively, by ultrasonic welding, and then inserted into the laminate exterior body. Next, an electrolyte was injected into the exterior body. The exterior body was sealed to obtain a lithium secondary battery.

[0171] Then, the lithium secondary battery was charged at 2.0 mA (0.05 C; 0.125 mA / cm 2 ) and a cutoff voltage of 4.4 V, and the initial charging was performed by CC charging. The capacity retention rate of the lithium secondary battery produced in Example 4 was measured in the same manner as above. The measured capacity retention rates are shown in Table 3 together with the results of Test Example 8.

[0172] [Table 3]

[0173] It was found from Table 3 that the capacity retention rate was maintained even when a buffer functional layer was introduced into the lithium secondary battery of this embodiment. That is, it was found that the lithium secondary battery of Example 4 had a high energy density, excellent cycle characteristics and productivity, and a low volume expansion rate due to charging and discharging the battery. [Industrial Applicability]

[0174] INDUSTRIAL APPLICABILITY The lithium secondary battery of the present invention has high energy density and excellent cycle characteristics and productivity, and is therefore industrially applicable as an electricity storage device for various applications. [Explanation of symbols]

[0175] 100, 300... lithium secondary battery, 110... positive electrode, 120... separator, 130... negative electrode, 140... positive electrode current collector, 210... negative electrode terminal, 220... positive electrode terminal, 310... buffer functional layer, 410... ion conductive fiber, 420... lithium metal, 430... ion conductive layer, 440... conductive layer.

Claims

1. A positive electrode and a negative electrode having no negative electrode active material, The positive electrode comprises a positive electrode active material and Li 6 Mn x Co 1-x O 4 and a lithium-containing compound represented by (0<x<1), Lithium secondary battery.

2. 2. The lithium secondary battery according to claim 1, which is initially charged under charging conditions in which the cut-off voltage is 4.3 V or more and 5.0 V or less.

3. 3. The lithium secondary battery according to claim 1, wherein the content of the lithium-containing compound is 1.0% by mass or more and 15.0% by mass or less with respect to the total mass of the positive electrode.

4. The lithium-containing compound is Li 6 Mn x Co 1-x O 4 4. The lithium secondary battery according to claim 1, wherein x is a compound represented by the formula (0.2≦x≦0.8).

5. The lithium secondary battery according to any one of claims 1 to 4, wherein the negative electrode is an electrode made of at least one selected from the group consisting of Cu, Ni, Ti, Fe, other metals that do not form an alloy with Li, alloys thereof, and stainless steel (SUS).

6. 6. The lithium secondary battery according to claim 1, having an energy density of 350 Wh / kg or more.

7. A method for using the lithium secondary battery according to any one of claims 1 to 6, comprising the steps of: After charging at a cutoff voltage of 4.3 V or more and 5.0 V or less, a charge-discharge cycle including at least one discharge step and at least one charge step is performed; The method of use, wherein the charge / discharge cycle is performed so that the cut-off voltage of the charging step is lower than the cut-off voltage of the first charge, which is performed at a cut-off voltage of 4.3 V or more and 5.0 V or less.

8. A positive electrode active material and Li 6 Mn x Co 1-x O 4 preparing a positive electrode including a lithium-containing compound represented by (0<x<1) and a negative electrode having no negative electrode active material; a step of arranging the positive electrode and the negative electrode so that they face each other; A step of initially charging the battery by applying a voltage between the positive electrode and the negative electrode under a charging condition in which the cut-off voltage is 4.3 V or more and 5.0 V or less; A method for producing a lithium secondary battery, comprising:

9. The method for producing a lithium secondary battery according to claim 8 , wherein the content of the lithium-containing compound is 1.0 mass % or more and 15.0 mass % or less with respect to the total mass of the positive electrode.

10. The lithium-containing compound is Li 6 Mn x Co 1-x O 4 The method for producing a lithium secondary battery according to claim 8 or 9, wherein x is a compound represented by the formula (0.2≦x≦0.8).

11. The method for producing a lithium secondary battery according to any one of claims 8 to 10, wherein the negative electrode is an electrode made of at least one selected from the group consisting of Cu, Ni, Ti, Fe, other metals that do not form an alloy with Li, alloys thereof, and stainless steel (SUS).

Citation Information

Patent Citations

  • Lithium secondary battery

    EP3605678A1

  • rechargeable lithium battery

    JP2006500755A

  • Lithium secondary battery with lithium metal formed on the positive electrode and its manufacturing method

    JP2019505971A

  • Additives for cathode, manufacturing method of the same, cathode including the same, and lithium recharegable battery including the same

    KR1020190064424A

  • Positive electrode for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery

    WO2014118834A1