Separator and manufacturing method thereof
The described separator design addresses the weaknesses of carbon and metal separators by using a multi-layered structure with conductive fibers and barrier layers, resulting in improved mechanical strength and conductivity for fuel cells and batteries.
Patent Information
- Application Number
- JP2021131863
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-13
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2041-08-13
AI Technical Summary
Existing separators for fuel cells, particularly carbon material-based ones, face challenges with low mechanical strength, high electrical resistance, and inadequate conductivity, while metal-based separators have high density and poor corrosion resistance.
A separator design incorporating a carbon material-based structure with a middle layer containing graphite and resin, surface layers with conductive fibers, and a barrier layer formed by films or filled layers to enhance strength, gas barrier properties, and conductivity, manufactured through a multi-step molding process.
The solution provides a separator with improved mechanical strength, reduced electrical resistance, and enhanced conductivity, achieving better performance in fuel cells and other batteries.
Smart Images

Figure 0007588048000002 
Figure 0007588048000003 
Figure 0007588048000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a separator and a method for producing the same. [Background technology]
[0002] A fuel cell is a battery that extracts energy by utilizing the reaction between hydrogen and oxygen. Since the reaction produces only water, fuel cells are known as environmentally friendly batteries. In particular, solid polymer fuel cells are considered promising as batteries for automobiles, communication devices, electronic devices, etc., because they enable high power density and are small and lightweight, and some have been put to practical use. A fuel cell is a cell stack composed of multiple cells stacked on top of each other. A plate-shaped member called a separator is placed between the cells. The separator is a partition plate that separates the passages of hydrogen and oxygen that are adjacent to each other, and plays a role in allowing hydrogen and oxygen to flow in contact with each other uniformly over the entire surface of the ion exchange membrane. For this reason, grooves that serve as the flow paths are formed in the separator.
[0003] Separators are broadly classified into metallic and carbon-based separators based on the material of which they are made. Stainless steel, aluminum or its alloy, or titanium or its alloy are generally used for metallic separators. Metallic separators have excellent workability and can be thinned due to the strength and ductility inherent to metals. However, metallic separators have a higher specific gravity than carbon separators described below, which is contrary to the weight reduction of fuel cells. Furthermore, metallic separators have the disadvantage of low corrosion resistance and forming a passivation film depending on the material. Corrosion of metallic materials or a passivation film is undesirable because it leads to an increase in the electrical resistance of the separator. Coating metallic separators with precious metals by plating or sputtering, etc., leads to high costs, but in order to prevent such high costs, a method is known in which the convex parts of the flow paths formed on the surface of the separator are formed with a photoresist film (see Patent Document 1).
[0004] On the other hand, carbon material-based separators have the advantage of being smaller in specific gravity and more corrosion resistant than metal material-based separators. However, carbon material-based separators are inferior in processability and mechanical strength. There is also a demand for further lower electrical resistance (i.e., further higher electrical conductivity). As a method for improving mechanical strength, for example, a separator in which graphite particles are dispersed in a thermoplastic resin is known (see Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2011-090937 A [Patent Document 2] JP 2006-294407 A Summary of the Invention [Problem to be solved by the invention]
[0006] The inventors belonging to the present applicant have previously developed a separator having a resin (particularly preferably polyphenylene sulfide) film on both sides of the thickness direction of a carbon material-based separator (Patent Application No. 2020-072036). By providing the resin film, the separator has higher strength than conventional separators and also has high gas barrier performance. However, there is a demand for separators arranged between cells of batteries, including fuel cells, to have even higher electrical conductivity.
[0007] An object of the present invention is to provide a separator having excellent strength, gas barrier properties and electrical conductivity, and a method for producing the same. [Means for solving the problem]
[0008] (1) In one embodiment of a separator for achieving the above object, the separator comprises a plate having a groove on a surface thereof as a flow path, and a barrier layer including the groove and a surface of the plate other than the groove, the barrier layer being formed on both surfaces in a thickness direction of the plate and having gas barrier properties superior to that of the plate, the plate comprising a middle layer plate including graphite and resin, and a surface layer plate including graphite, resin, and conductive fibers, laminated on both surfaces in a thickness direction of the middle layer plate. (2) In the separator according to another embodiment, the barrier layer may preferably be a film-like covering layer different from the plate. (3) In the separator according to another embodiment, the barrier layer may preferably be a filled layer in which resin or rubber fills spaces between particles or fibers that constitute the plate. (4) In the separator according to another embodiment, the barrier layer may preferably include the filling layer and a film-like covering layer different from the plate. (5) In the separator according to another embodiment, preferably, the conductive fibers of the surface plate may be unevenly distributed on the barrier layer side in the thickness direction. (6) In the separator according to another embodiment, the conductive fibers may preferably be carbon fibers. (7) In the separator according to another embodiment, preferably, the surface plate may further include aramid fibers separate from the resin. (8) In the separator according to another embodiment, the surface plate may preferably contain at least one of polyether ether ketone and polyphenylene sulfide as the resin. (9) In the separator according to another embodiment, preferably, the intermediate plate may further include aramid fibers separate from the resin. (10) In the separator according to another embodiment, preferably, the intermediate plate may further include metal fibers. (11) A separator according to another embodiment may preferably be a separator for a fuel cell used between cells of a fuel cell. (12) A method for manufacturing a separator according to one embodiment for achieving the above object is a method for manufacturing a separator as described above, comprising: a first film positioning step of positioning a film for forming the barrier layer in a mold; a first workpiece positioning step of positioning a first workpiece containing at least graphite, resin, and conductive fibers on the film; a second workpiece positioning step of positioning a second workpiece containing at least graphite and resin on the first workpiece in the mold; a third workpiece positioning step of positioning the first workpiece on the second workpiece; a second film positioning step of positioning a film for forming the barrier layer on a laminate including the first workpiece, the second workpiece, and the first workpiece; and a molding step of closing the mold with the laminate sandwiched between the films to perform molding, and forming the barrier layer on both surfaces in the thickness direction of the plate. (13) In another embodiment, the method for manufacturing a separator preferably further includes a first pre-molding step of obtaining the first molded object in a semi-cured state from a first mixture containing at least the graphite, the resin, and the conductive fibers prior to the first molded object placing step and the third molded object placing step, and the first molded object placing step may include placing the first molded object in the semi-cured state on the film, and the third molded object placing step may include placing the first molded object in the semi-cured state on the second molded object. (14) In another embodiment of the method for manufacturing a separator, preferably, the first pre-molding step is for obtaining a first molded object in a semi-cured state, in which the conductive fibers are unevenly distributed on one side of the thickness direction of the first molded object, from the first mixture, and the first molded object placement step is for placing the first molded object in a semi-cured state on the film so that the surface of the first molded object on the side on which the conductive fibers are unevenly distributed contacts the film in the mold, and the third molded object placement step is for placing the first molded object in a semi-cured state on the second molded object so that the surface of the first molded object opposite the side on which the conductive fibers are unevenly distributed contacts the second molded object in the mold. (15) In another embodiment, the method for manufacturing a separator preferably further includes a second pre-molding step of obtaining the second molded object in a semi-cured state from a second mixture containing at least the graphite and the resin prior to the second molded object placement step, and the second molded object placement step may include placing the second molded object in the semi-cured state on the first molded object. (16) In another embodiment of the method for manufacturing a separator, the mold may have an inner surface with a projection and recess for transferring the groove, and the molding step may use the mold having the projection and recess to mold the laminate and form the groove. Effect of the Invention
[0009] According to the present invention, a separator having excellent electrical conductivity and a method for producing the same can be provided. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 shows a plan view of a separator according to an embodiment of the present invention. [Figure 2A] FIG. 2A shows a cross-sectional view of the separator taken along line AA in FIG. 1 and an enlarged view of a part B thereof. [Figure 2B] FIG. 2B shows enlarged views of variations a, b, and c of part C in part B of FIG. 2A. [Diagram 3]FIG. 3 shows an example of a flow of main steps in a method for producing a separator according to an embodiment of the present invention. [Figure 4] FIG. 4 shows cross-sectional views of the respective steps of the manufacturing method shown in FIG. [Diagram 5] FIG. 5 shows cross-sectional views of the process steps subsequent to FIG. [Figure 6] FIG. 6 is a cross-sectional view showing the status of each step of the manufacturing method of the separator according to the modified example. [Figure 7] FIG. 7 shows in cross section the state of each process subsequent to FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Next, an embodiment of the present invention will be described with reference to the drawings. Note that the embodiment described below does not limit the invention according to the claims, and all of the elements and combinations thereof described in the embodiment are not necessarily essential to the solution of the present invention.
[0012] 1. Separator Fig. 1 shows a plan view of a separator according to an embodiment of the present invention, and Fig. 2A shows a cross-sectional view of the separator taken along line AA in Fig. 1 and an enlarged view of a part B thereof.
[0013] The separator 1 according to this embodiment is a plate-like body having a substantially rectangular shape in a plan view. The separator 1 is a plate-like body sandwiched from both sides of a membrane electrode assembly (MEA) in which both sides of an electrolyte membrane are sandwiched between an air electrode and a hydrogen electrode in a fuel cell, for example. In this embodiment, the separator 1 is broadly interpreted to include an anode-side separator arranged on the hydrogen electrode (also called an "anode electrode") side, and a cathode-side separator arranged on the air electrode (also called a "cathode electrode") side. In this embodiment, the separator 1 is a carbon material-based separator. The separator 1 is not limited to use in fuel cells, and can also be used as a plate-like member arranged between cells of other batteries (preferably storage batteries).
[0014] The separator 1 has through holes 11, 12, 21, and 22 penetrating in the thickness direction. The through holes 11 and 21 are arranged on one end side of the separator 1. The through hole 12 is arranged on the other end side opposite the one end side of the separator 1, facing the through hole 21 when the separator 1 is viewed in plan. The through hole 22 is arranged on the other end side opposite the one end side of the separator 1 so as to face the through hole 11 when the separator 1 is viewed in plan. A groove 30 is formed as a flow path on one surface side (front surface side) of the separator 1. The surface 31 other than the groove 30 is convex with respect to the groove 30. In addition, a groove 32 is formed as a flow path on the surface (rear surface side) opposite the one surface side of the separator 1. The surface 31 other than the groove 32 is convex with respect to the groove 32.
[0015] When the separator 1 is a cathode separator, the through hole 11 is an oxidizing gas supply port. The through hole 12 is an oxidizing gas exhaust port. The through hole 21 is a hydrogen gas exhaust port. The through hole 22 is a hydrogen gas supply port. The oxidizing gas is, for example, air, but may be oxygen. The groove 30 on the front side of the separator 1 is a flow path for the oxidizing gas to flow. The groove 32 on the back side of the separator 1 is a flow path for the cooling water to flow. In FIG. 1, the flow of the oxidizing gas is indicated by white arrows.
[0016] When separator 1 is an anode separator, through-hole 11 is a hydrogen gas supply port. Through-hole 12 is a hydrogen gas exhaust port. Through-hole 21 is an oxidizing gas exhaust port. Through-hole 22 is an oxidizing gas supply port. Groove 30 on the front side of separator 1 is a flow path for hydrogen gas to flow. Groove 32 on the back side of separator 1 is a flow path for cooling water to flow.
[0017] The separator 1 includes at least a plate 2 and a barrier layer 8. The plate 2 includes surface plates 3 and 4 and an intermediate plate 4. The plate 2 includes grooves 30 and 32 on a surface 31 as flow paths.
[0018] (Middle plate) The intermediate plate 5 is a plate containing graphite and resin. The intermediate plate 5 is a molded body containing graphite and resin, and has a microstructure in which graphite is dispersed in the resin solidified after melting. The intermediate plate 5 may have fibers other than the resin in addition to graphite and resin. The fibers may be any type of nonmetallic fibers such as resin fibers, carbon fibers, and ceramic fibers, but are preferably resin fibers, and more preferably aramid fibers. The fiber diameter of the aramid fibers is preferably 5 to 20 μm, more preferably 9 to 15 μm. The fiber length of the aramid fibers is preferably 1 to 15 mm, more preferably 3 to 9 mm. The fiber diameter and fiber length refer to the fiber diameter and fiber length measured from the field of view of 20 independent fibers selected under a microscope (optical microscope and scanning electron microscope are used depending on the size). When determining the average fiber diameter or average fiber length, the diameters or lengths of the 20 fibers are averaged. The same applies to the following fiber diameter, fiber length, average fiber diameter, and average fiber length. By adding fibers to the intermediate layer plate 5, the strength of the intermediate layer plate 5 can be increased. The intermediate layer plate 5 may include metal fibers in addition to graphite and resin. The metal fibers are fibers made of metals such as copper, stainless steel, titanium, iron, aluminum, nickel, gold, silver, and chromium, and are preferably fibers made of copper, stainless steel, or titanium, and more preferably fibers made of copper. The fiber diameter of the metal fibers is preferably 5 to 100 μm, and more preferably 20 to 60 μm. The fiber length of the metal fibers is preferably 0.5 to 3.5 mm, and more preferably 1.5 to 2.5 mm. The area of the intermediate layer plate 5 in a plan view is preferably 10 to 1000 cm. 2 , more preferably 100 to 750 cm 2 The thickness of the intermediate plate 5 is preferably 0.1 to 2.0 mm, and more preferably 0.2 to 1.5 mm.
[0019] The resin constituting the intermediate plate 5 is not particularly limited, but is preferably a thermoplastic resin. A resin more suitable for the intermediate plate 5 is a resin with excellent heat resistance, and specific examples thereof include polyphenylene sulfide (PPS), polyether ether ketone (PEEK), polyamide (PA), polyether ketone ether ketone ketone (PEKEKK), polyether ketone (PEK), liquid crystal polymer (LCP), polytetrafluoroethylene (PTFE), tetrafluoroethylene-ethylene copolymer (ETFE), polychlorotrifluoroethylene (PCTFE), polyimide (PI), polyamide imide (PAI), polyether sulfone (PES), polyphenyl sulfone (PPSU), polyether imide (PEI) and polysulfone (PSU). Among these, PPS or PEEK is particularly suitable. Examples of PPS include M2888 and E2180 manufactured by Toray Industries, Inc., and FZ-2140 and FZ-6600 manufactured by Dainippon Ink and Chemicals, Inc.
[0020] The average particle size of the resin used before molding the middle layer plate 5 is preferably 1 μm to 300 μm, more preferably 5 μm to 150 μm, and even more preferably 10 μm to 100 μm. Here, the average particle size refers to a particle size measured by a laser diffraction / scattering particle size distribution measurement method. The same method is used to measure the average particle size hereinafter.
[0021] The graphite constituting the intermediate layer plate 5 may be any of artificial graphite, expanded graphite, natural graphite, etc. Here, the expanded graphite refers to graphite or a graphite intercalation compound in which the graphite layers are expanded by inserting another material layer (=intercalation) into a specific surface of a structure in which regular hexagonal planes of graphite (graphite) are stacked. Examples of the expanded graphite include BSP-60A (average particle size 60 μm) and EXP-50SM manufactured by Fuji Graphite Industries Co., Ltd. Examples of the artificial graphite include 1707SJ (average particle size 125 μm), AT-No.5S (average particle size 52 μm), AT-No.10S (average particle size 26 μm), and AT-No.20S (average particle size 10 μm) manufactured by Oriental Sangyo Co., Ltd., or PAG and HAG manufactured by Nippon Graphite Industries Co., Ltd. Examples of the natural graphite include CNG-75N (average particle size 43 μm) manufactured by Fuji Graphite Industries Co., Ltd., and CPB (scale graphite powder, average particle size 19 μm) manufactured by Nippon Graphite Industries Co., Ltd. The shape of the graphite particles is not particularly limited, and can be appropriately selected from flaky, scaly, spherical, and the like. Furthermore, the graphite may partially contain non-crystalline carbon (amorphous carbon).
[0022] The average particle size of the graphite used before forming the intermediate layer plate 5 is preferably 1 μm to 500 μm, more preferably 3 μm to 300 μm, and even more preferably 10 μm to 150 μm.
[0023] The graphite and the resin may be mixed together after adjusting the particle size separately and then used to form the middle layer plate 5, or may be kneaded together first, pulverized, and the particle size adjusted before being used to form the middle layer plate 5. When the graphite and the resin are kneaded together and then pulverized to adjust the particle size, the average particle size of the mixed powder is preferably 1 μm or more and 500 μm or less, more preferably 3 μm or more and 300 μm or less, and even more preferably 10 μm or more and 150 μm or less.
[0024] The mass ratio of graphite and resin constituting the intermediate plate 5 is graphite:resin=70-95 parts by mass:30-5 parts by mass. For example, 5 parts by mass of resin can be mixed with 70 parts by mass or more and 95 parts by mass or less to form the constituent material of the separator 1. Similarly, for example, 30 parts by mass of resin can be mixed with 70 parts by mass or more and 95 parts by mass or less to form the constituent material of the separator 1. The separator 1 preferably contains more graphite than resin in terms of mass ratio. A more suitable mass ratio of graphite to resin is 10 parts by mass of graphite or 10.1 parts by mass or more and 20 parts by mass or less of graphite per 1 part by mass of resin. As described above, when the parts by mass of graphite are more than the parts by mass of resin, the number of contact points between the graphite particles is more than that of conventional separators, and thus the electrical resistance of the separator 1 can be lowered (i.e., the electrical conductivity can be increased). A representative sample of separator 1 had a contact resistance of 5 mΩ cm 2 The contact resistance value means the resistance value between a barrier layer 8 (film 6 described below) formed on one surface of the plate 2 in the thickness direction and a barrier layer 8 (film 7 described below) formed on the other surface of the plate 2 in the thickness direction.
[0025] (Surface plate) The surface plates 3, 4 are plates laminated on both surfaces of the middle plate 5 in the thickness direction, and have grooves 30, 32 as flow paths on the surfaces of the plates. The surface plates 3, 4 are plates containing graphite, resin, and conductive fibers. The surface plates 3, 4 are molded bodies containing graphite, resin, and conductive fibers, and have a fine structure in which graphite is dispersed in the resin and conductive fibers that have solidified after melting. The conductive fibers are preferably carbon fibers, polyester fibers plated with two layers of copper and nickel, and more preferably carbon fibers. The carbon fibers are not particularly limited, and examples thereof include PAN-based carbon fibers, pitch-based carbon fibers, phenol-based carbon fibers, rayon-based carbon fibers, and combinations thereof. Among these, PAN-based carbon fibers are preferred from the viewpoint of the flexibility and strength of the separator 1. As the carbon fibers, for example, HT C137 (average fiber diameter 7 μm, average fiber length 6 mm) manufactured by Teijin Limited can be used. The fiber diameter of the carbon fibers is preferably 2 to 50 μm, more preferably 5 to 15 μm. The fiber length of the carbon fibers is preferably 1 to 15 mm, more preferably 3 to 9 mm. In the surface plate 3, the conductive fibers are preferably distributed unevenly on the barrier layer 8 (film 6 described below) side in the thickness direction of the surface plate 3. In the surface plate 4, the conductive fibers are preferably distributed unevenly on the barrier layer 8 (film 7 described below) side in the thickness direction of the surface plate 4. By distributing the conductive fibers unevenly in this way, the electrical resistance (contact resistance) of the separator 1 can be made lower (i.e., the conductivity can be made higher).
[0026] The surface layer plates 3, 4 may be provided with a fiber other than the resin and the conductive fiber in addition to the graphite, the resin, and the conductive fiber. The fiber may be any type of fiber such as a resin fiber or a ceramic fiber, but is preferably a resin fiber, and more preferably an aramid fiber. By providing the surface layer plates 3, 4 with the fiber, the strength of the surface layer plates 3, 4 can be further increased. The surface layer plates 3, 4 are provided with grooves corresponding to the grooves 30, 32 of the separator 1. The resin constituting the surface layer plates 3, 4 is one or more of the above-mentioned preferred resins constituting the middle layer plate 5, and is more preferably at least one of PEEK and PPS. The graphite constituting the surface layer plates 3, 4 is one or more of the above-mentioned preferred graphites constituting the middle layer plate 5. The average particle size of the resin and graphite constituting the surface layer plates 3, 4 is the same as the average particle size of the resin and graphite constituting the middle layer plate 5 described above.
[0027] (Barrier layer) In this embodiment, the barrier layer 8 includes the grooves 30, 32 and the surface 31 of the plate 2 other than the grooves 30, 32, and covers both surfaces in the thickness direction of the plate 2. That is, the barrier layer 8 covers both the front and back surfaces of the plate 2, including the inner surfaces of the grooves 30, 32. The barrier layer 8 is, for example, a film-like covering layer different from the plate 2, and is formed by separating or fusing two types of films, a film 6 which is an example of the barrier layer 8 covering the front surface, and a film 7 which is an example of the barrier layer 8 covering the back surface. In this embodiment, the barrier layer 8 is divided into a film 6 and a film 7. The film 6 covers one side surface in the thickness direction of the plate 2, more specifically, the surface opposite the middle layer plate 5 in the thickness direction of the surface layer plate 3. The film 7 covers the other side surface in the thickness direction, more specifically, the surface opposite the middle layer plate 5 in the thickness direction of the surface layer plate 4. However, the barrier layer 8 may be in the shape of a bag that envelops the outer surface of the plate 2 with the film 6 and the film 7 joined together.
[0028] FIG. 2B shows enlarged views of variations a, b, and c of part C in part B of FIG. 2A.
[0029] In the form a, a film mainly made of resin or rubber is provided on the surface of the plate 2 (surface plate 3, 4). In the form a, the barrier layer 8 is a film-like covering layer F different from the plate 2. In the form b, the barrier layer 8 impregnated with resin or rubber is provided near the surface of the plate 2 (mainly the surface plate 3, 4). In the form b, the barrier layer 8 is a filling layer M in which the resin or rubber fills the spaces between the particles or fibers that constitute the plate 2. In the form c, the barrier layer 8 includes the filling layer M and the covering layer F. Thus, the barrier layer 8 preferably takes the form a, b, or c. However, the barrier layer 8 may take a form other than the form a, b, or c as long as it has a gas barrier property superior to the plate 2. In the present application, "gas barrier property" or "gas barrier performance" means a property of preventing gas permeation. Hereinafter, the barrier layer 8 of the form a will be mainly described.
[0030] The barrier layer 8 is preferably made of resin or rubber. The barrier layer 8 is mainly made of one or more of the above-mentioned preferred resin choices for the plate 2 (surface plates 3, 4 and middle plate 5), and more preferably at least one of PEEK and PPS. Here, the "main material" means a material that occupies more than 50% by mass of the barrier layer 8. The main material may be, for example, 51%, 60%, 70%, 80%, 90%, 95% or 100% by mass, as long as it exceeds 50% by mass with respect to the mass of the barrier layer 8.
[0031] The thickness of the barrier layer 8 is preferably 2 μm or more and 50 μm or less, more preferably 4 μm or more and 35 μm or less. When the thickness of the barrier layer 8 is 2 μm or more, or even 4 μm or more, the gas barrier property of the separator 1 can be improved and the strength (bending strength) can be increased, and the ease of handling can be improved. On the other hand, when the thickness of the barrier layer 8 is 50 μm or less, or even 35 μm or less, the contact resistance between the barrier layers 8 in the separator 1 can be reduced (i.e., the conductivity can be increased). In this embodiment, the strength means the bending strength measured according to JIS K7171.
[0032] The resin constituting the surface plates 3, 4 and the resin constituting the barrier layer 8 may be the same type of thermoplastic resin. In this case, the resin near the barrier layer 8 of the surface plates 3, 4 and the barrier layer 8 can be partially integrated, thereby further improving the strength of the separator 1. The thermoplastic resin is preferably PEEK or PPS.
[0033] 2. Separator manufacturing method Next, a method for producing a separator according to an embodiment of the present invention will be described.
[0034] The manufacturing method of the separator 1 (hereinafter, simply referred to as the "manufacturing method") includes a first film arranging step of arranging the film 6 in a mold, a first molded object arranging step of arranging a first molded object containing at least graphite, resin, and conductive fiber on the film 6, a second molded object arranging step of arranging a second molded object containing at least graphite and resin on the first molded object in the mold, a third molded object arranging step of arranging the first molded object on the second molded object, a second film arranging step of arranging the film 7 on a laminate including the first molded object, the second molded object, and the first molded object, and a molding step of closing the mold with the laminate sandwiched between the films 6 and 7 to perform molding. The manufacturing method of the separator 1 further includes a first pre-molding step of obtaining a first molded object in a semi-cured state from a first mixture containing at least graphite, resin, and conductive fiber prior to the first molded object arranging step and the third molded object arranging step. The method for producing the separator 1 further includes a second pre-molding step of obtaining a semi-hardened second object from a second mixture containing at least graphite and a resin prior to the second object placement step. In the following embodiment, the method for producing a separator is preferably a method for producing a fuel cell separator used between cells of a fuel cell. The separator 1 is preferably a carbon material-based separator. However, the separator 1 is not limited to use in fuel cells, and can also be used as a plate-like member disposed between cells of other batteries (preferably storage batteries).
[0035] Fig. 3 shows an example of a flow of main steps of a method for producing a separator according to an embodiment of the present invention. Fig. 4 shows, in cross-section, the status of each step of the production method shown in Fig. 3. Fig. 5 shows, in cross-section, the status of each step subsequent to Fig. 4.
[0036] The separator 1 can be manufactured through a first mixture forming step (S100), a first pre-molding step (S110), a second mixture forming step (S200), a second pre-molding step (S210), a first film arranging step (S300), a first object to be molded arranging step (S310), a second object to be molded arranging step (S320), a third object to be molded arranging step (S330), a second film arranging step (S340), and a molding step (S350). S100 to S350 will be described in detail below with reference to Figs. 3 to 5.
[0037] (1) First mixture formation step (S100) This step is a step of forming a first mixture containing at least graphite, resin, and conductive fibers. Specifically, graphite, resin, and conductive fibers are mixed and dispersed in water or an alcohol aqueous solution to prepare a slurry. In this step, a fiber other than the resin may be further added to the graphite, resin, and conductive fibers to prepare a slurry.
[0038] (2) First preforming process (S110) This step is a step of obtaining a first molded object in a semi-cured state from the first mixture. Specifically, the first mixture is formed into a wet sheet by filtering and separating the liquid with a sheet machine having a mesh structure, and the wet sheet is pressed while being heated with a press machine. This allows a first molded object in a semi-cured state (hereinafter also referred to as a "pre-surface plate"). The pre-surface plate obtained in this step preferably has conductive fibers unevenly distributed on one side in the thickness direction. In this embodiment, two pre-surface plates, which are preforms of the surface plate 3.4, are molded at once. However, the two pre-surface plates may be molded separately. This step is sufficient as a step of manufacturing at least a preform of the surface plate 3, which is a preform. The pre-surface plate, which is a preform of the surface plate 4, may be manufactured at any stage before the third molded object arrangement step (S330). Furthermore, in the case where a plate containing at least graphite, resin, and conductive fibers is not manufactured but can be obtained by a method such as purchasing, the first mixture formation step (S100) and the first pre-molding step (S110) can be omitted.
[0039] (3) Second mixture formation step (S200) This step is a step of forming a second mixture containing at least graphite and resin. Specifically, graphite and resin are mixed and dispersed in water or an alcohol aqueous solution to prepare a slurry. In this step, a slurry may be prepared by adding fibers other than the resin and / or metal fibers to the graphite, resin, and conductive fibers.
[0040] (4) Second preforming process (S210) This step is a step of obtaining a second molded object in a semi-cured state from the second mixture. Specifically, the second mixture is formed into a wet sheet by filtering and separating the liquid using a sheet machine with a mesh structure, and the wet sheet is heated and pressed using a press machine. This allows the second molded object in a semi-cured state (hereinafter also referred to as a "pre-middle layer plate"). When a plate containing at least graphite and resin is not manufactured but can be obtained by a method such as purchasing, the second mixture forming step (S200) and the second pre-molding step (S210) can be omitted.
[0041] (5) First film placement process (S300) This step is a step of placing the film 6 for forming the barrier layer 8 in the mold 60. Specifically, the lower mold 40 constituting the mold 60 is prepared, and the film 6 is placed in the recess 41 of the lower mold 40 (see FIG. 4(a)). The lower mold 40 has projections and recesses 42 on the inner bottom surface of the recess 41 that can transfer and form the grooves 32.
[0042] (6) First molded object placement step (S310) This step is a step of placing the pre-surface plate 72, which is the first molding object in a semi-cured state, on the film 6. Specifically, the pre-surface plate 72 is placed on the film 6 laid on the lower mold 40 (see FIG. 4(b)). In this step, it is preferable to place the pre-surface plate 72 on the film 6 so that the surface of the pre-surface plate 72 on which the conductive fibers are concentrated is in contact with the film 6.
[0043] (7) Second molded object placement process (S320) This step is a step of placing the pre-middle layer plate 74, which is the second molding object in a semi-cured state, on the pre-surface layer plate 72. Specifically, the pre-middle layer plate 74 is placed on the pre-surface layer plate 72 on the film 6 placed in the recess 41 of the lower mold 40 (see FIG. 4(c)).
[0044] (8) Third molded object placement process (S330) This step is a step of placing the pre-surface plate 72, which is the first molding object in a semi-cured state, on the pre-middle layer plate 74. Specifically, the pre-surface plate 72 is placed on the pre-middle layer plate 74 in the lower mold 40 (see FIG. 4(d)). In this step, it is preferable to place the pre-surface plate 72 on the pre-middle layer plate 74 so that the surface of the pre-surface plate 72 opposite to the side on which the conductive fibers are unevenly distributed is in contact with the pre-middle layer plate 74.
[0045] (9) Second film placement process (S340) This step is a step of arranging a film 7 for forming a barrier layer 8 on the laminate 70 including the pre-surface layer plate 72, the pre-middle layer plate 74, and the pre-surface layer plate 72 in the mold 60 after the third molded object arranging step (S330). Specifically, the film 7 is arranged on the pre-surface layer plate 72 of the laminate 70 arranged in the recess 41 of the lower mold 40 (see FIG. 4(e)). At this time, the film 7 is arranged on the pre-surface layer plate 72 so that the surface of the pre-surface layer plate 72 on the side where the conductive fibers are unevenly distributed is in contact with the film 7.
[0046] (10) Molding process (S350) In this step, the laminate 70 is sandwiched between the films 6 and 7, and the mold 60 is closed to perform molding. Specifically, the upper mold 50 constituting the mold 60 is prepared and placed on the recessed portion 41 side of the lower mold 40, and the lower mold 40 and the upper mold 50 are closed (see Figs. 5(f) and (g)). The upper mold 50 has a recess 51 on the surface facing the recessed portion 41 of the lower mold 40. The recessed portion 51 has an irregularity 52 on its inner bottom surface that can transfer and form the groove 30. After the mold 60 is clamped, it is heated to form the laminate 70. As a result, the laminate 70 hardens to form the plate 2. In addition, the transfer of the irregularities 41 and 51 forms the grooves 30 and 32 covered with the barrier layer 8 (films 6 and 7) (see Fig. 5(h)).
[0047] After the molding step (S350), the mold 60 is opened and the separator 1 is completed.
[0048] Fig. 6 shows in cross section the status of each step of the manufacturing method of the separator according to the modified example, and Fig. 7 shows in cross section the status of each step subsequent to Fig. 6.
[0049] In this modification, the separator 1 is manufactured using a pre-surface plate 72a having grooves formed on one surface in the thickness direction instead of the pre-surface plate 72. Specifically, in the first pre-molding step (S110), the pre-surface plate 72a having grooves formed on one surface in the thickness direction is obtained from the first mixture formed in the first mixture forming step (S100). More specifically, the first mixture is formed into a wet sheet by filtering and separating the liquid using a sheet machine having a mesh structure, and the wet sheet is placed in a mold having an inner bottom surface formed with irregularities and is heated and pressed by a press machine. At this time, it is preferable that the wet sheet is placed in the mold so that the surface on the side where the conductive fibers of the wet sheet are unevenly distributed contacts the irregularities in the mold. As a result, the pre-surface plate 72a having grooves formed on the surface on the side where the conductive fibers are unevenly distributed can be obtained. Then, similarly to the manufacturing method described above (see FIG. 3), the second mixture formation step (S200), the second pre-molding step (S210), and the first film placement step (S300) are performed, followed by the first molding object placement step (S310) (see FIGS. 6(a) and (b)).
[0050] In the first molding object placement step (S310), the pre-surface plate 72a is placed on the film 6 laid on the lower mold 40 so that the groove of the pre-surface plate 72a fits the unevenness 42 (see FIG. 6(b)). Then, similarly to the above-mentioned manufacturing method (see FIG. 3), the second molding object placement step (S320) is performed, and in the third molding object placement step (S330), the pre-surface plate 72a is placed on the pre-middle layer plate 74 in the lower mold 40 so that the groove of the pre-surface plate 72a is placed on the opposite side to the pre-middle layer plate 74 (see FIG. 6(c) and (d)). In the second film placement step (S340), the film 7 is placed on the laminate 70a including the pre-surface plate 72a, the pre-middle layer plate 74, and the pre-surface plate 72a placed in the recess 41 of the lower mold 40 (see FIG. 6(e)).
[0051] In the molding step (S350), the grooves of the pre-surface plate 72a are matched with the concaves and convexes 52 of the upper mold 50, the lower mold 40 and the upper mold 50 are closed, and the mold 60 is clamped (see Figs. 7(f) and (g)). After the molding step (S350), the mold 60 is opened, and the separator 1 is completed. The grooves formed in the pre-surface plate 72a may be of the same size as the grooves 30 and 32, or may be shallower than the grooves 30 and 32. If the grooves formed in the pre-surface plate 72a are shallower than the grooves 30 and 32, the previously formed shallow grooves can be deepened to change into the grooves 30 and 32 when the mold 60 is closed and molded in the molding step (S350).
[0052] <Other embodiments> As described above, the preferred embodiments of the present invention have been described, but the present invention is not limited to these and can be practiced in various modified forms.
[0053] The grooves 30 of the separator 1 may be grooves that form flow paths other than the flow paths that allow gas to flow in the direction indicated by the white arrows in Fig. 1. Moreover, the grooves 32 may be grooves that form any type of flow path. For example, the grooves 30 may be grooves that form linear flow paths from one end of the separator 1 to the other end, and the grooves 32 may be grooves that form linear flow paths in a direction approximately perpendicular to the grooves 30. Moreover, the separator 1 may not have at least one of the grooves 30 and the grooves 32.
[0054] In the above embodiment, the intermediate layer plate 5 does not have any grooves corresponding to the grooves 30 and 32, but may have grooves corresponding to the grooves 30 and 32 on at least one surface in the thickness direction. In that case, when the mold 60 is closed and molded in the molding step (S350), grooves may be formed in the pre-intermediate layer plate 74 that does not have grooves by transferring the irregularities 41 and 51, and the intermediate layer plate 5 having the grooves 30 and 32 may be manufactured. Also, the pre-intermediate layer plate 74 may have grooves corresponding to the grooves 30 and 32 formed in advance, similar to the pre-surface layer plate 72a (see FIG. 6). In that case, the pre-intermediate layer plate 72a having grooves formed on at least one surface in the thickness direction may be formed from the second mixture in the second pre-molding step (S210).
[0055] In the above embodiment, the surface layer plates 3, 4 have the grooves 30, 32 on one side in the thickness direction, but the grooves 30, 32 may be provided on both sides in the thickness direction. In that case, when the mold 60 is closed and molded in the molding step (S350), the surface layer plates 3, 4 having the grooves 30, 32 on both sides in the thickness direction may be manufactured by transferring the irregularities 41, 51. Also, in the first pre-molding step (S110), instead of the pre-surface plate 72a, a pre-surface plate having grooves formed on both sides in the thickness direction may be formed.
[0056] Prior to the first molding object arranging step (S310), a laminate 70, 70a including the pre-surface layer plate 72, 72a, the pre-middle layer plate 74, and the pre-surface layer plate 72, 72a may be formed, and the laminate 70, 70a may be arranged on the film 6 in the first molding object arranging step (S310). In that case, the second molding object arranging step (S320) and the third molding object arranging step (S330) may be omitted. In that case, the first molding object arranging step, the second molding object arranging step, and the third molding object arranging step of the present invention correspond to the first molding object arranging step (S310).
[0057] After the forming step, a trimming step may be performed in which excess areas of the films 6, 7 are trimmed.
[0058] The manufacturing method of the above embodiment is a method for manufacturing a fuel cell separator in which the barrier layer 8 is a layer of resin or rubber, but the method may also be a method for manufacturing a fuel cell separator in which the barrier layer 8 is a layer of Form b or Form c in Figure 2B. EXAMPLES
[0059] Next, examples of the present invention will be described in comparison with comparative examples. Note that the present invention is not limited to the following examples.
[0060] 1.Main raw materials for the middle plate (1) Graphite For the graphite powder used as the constituent material of the middle plate of the separator, two types of graphite powder were used: Oriental Kogyo Co., Ltd. product number: 1707SJ (artificial graphite, average particle size 125 μm) and Oriental Kogyo Co., Ltd. product number: AT-No.5S (artificial graphite, average particle size 52 μm). (2) Resin Polyphenylene sulfide (PPS) powder was used as the resin that constitutes the middle plate of the separator. The PPS used was fine PPS powder made by freezing and crushing flake-shaped PPS powder of Torelina M2888 manufactured by Toray Industries, Inc., and adjusting the average particle size to 50 μm. (3) Aramid fiber The aramid fibers used as the constituent material of the middle plate of the separator were Technora T32PNW 3-12 (average fiber length 3.2 mm, average fiber diameter 18 μm) manufactured by Teijin Limited, Twaron (registered trademark) 1094 (average fiber length 1.1 mm, specific surface area 13.6 m) manufactured by Teijin Limited. 2 Three types of aramid fibers were used: aramid fiber 1000 (average fiber length 0.8 mm), aramid fiber 1000 (average fiber length 0.5 mm), and Twaron (registered trademark) D8016 (average fiber length 0.8 mm). (4) Metal fibers The metal fibers used as the constituent material of the middle plate of the separator were copper metal fibers (average fiber length 1.88 mm, average fiber diameter 52.08 μm) manufactured by Kogi Co., Ltd.
[0061] 2. Main raw materials for the surface plate (1) Graphite Two types of graphite powder were used as the constituent material of the surface plate of the separator: Oriental Kogyo Co., Ltd. product number: 1707SJ (artificial graphite, average particle size 125 μm) and Oriental Kogyo Co., Ltd. product number: AT-No.5S (artificial graphite, average particle size 52 μm). (2) Resin Polyphenylene sulfide (PPS) powder was used as the resin that constitutes the surface plate of the separator. The PPS used was fine PPS powder made by freezing and crushing flake-shaped PPS powder of Toray Industries, Inc.'s Torelina M2888 to adjust the average particle size to 50 μm. (3) Carbon fiber The carbon fibers used as the constituent material of the surface plate of the separator were HT C137 (average fiber length 6.0 mm, average fiber diameter 7 μm) manufactured by Teijin Limited. (4) Aramid fiber The aramid fibers used as the constituent material of the surface plate of the separator were Twaron (registered trademark) D8016 (average fiber length 0.8 mm) manufactured by Teijin Limited.
[0062] 3. Film A PPS film was used as the separator film. The PPS film used was a 9 μm-thick film (product number: Torelina 9-3017) manufactured by Toray Industries, Inc.
[0063] 4.Mold The mold used was a top-bottom split mold made of prehardened steel NAK80 manufactured by Daido Steel Co., Ltd. When closed, there was a space (approximately 63 cm2) inside the mold that was large enough to mold the separator. 3 In addition, the bottom of the inside of each of the upper and lower dies has projections and recesses for forming the grooves of the separator.
[0064] 5. Evaluation Methodology The contact resistance between the separators was measured by the following method. First, two separators were stacked and sandwiched between two electrodes on both sides. A certain pressure (0.8 MPa) was applied to the entire laminate including the electrodes, and a constant current was passed using a resistance meter (product number: RM3544) manufactured by HIOKI EE Corporation to measure the electrical resistance. The obtained resistance (hereinafter referred to as the "contact resistance of the laminate") is the sum of the contact resistance between one separator and one electrode in contact with the separator, the contact resistance between the other separator and the other electrode in contact with the separator, and the contact resistance between the separators. Next, with one of the separators sandwiched between the two electrodes, a certain pressure (0.8 MPa) was applied while a constant current was passed through it using a resistance meter (product number: RM3544) manufactured by HIOKI EE Corporation to measure the electrical resistance value. The resistance value obtained was the sum of the contact resistance values between both sides of the separator and the electrodes, and this was divided by 2 to obtain the contact resistance value between one side of the separator and the electrode (hereinafter referred to as "contact resistance value of one of the separators"). Next, with the other separator sandwiched between the two electrodes, a certain pressure (0.8 MPa) was applied while a constant current was passed through it using a resistance meter (product number: RM3544) manufactured by HIOKI EE Corporation to measure the electrical resistance value. The obtained resistance value was the sum of the contact resistance values between both sides of the separator and the electrodes, and this was divided by 2 to obtain the contact resistance value between one side of the separator and the electrode (hereinafter referred to as the "contact resistance value of the other separator"). The contact resistance between the separators was calculated by subtracting the contact resistance of one separator and the contact resistance of the other separator from the contact resistance of the entire stack. 2 If it was less than this, it was rated as pass.
[0065] 6. Manufacturing of separators <Example> 1083.3 parts by mass of artificial graphite particles (product number: 1707SJ), 100 parts by mass of PPS powder, 62.5 parts by mass of aramid fiber (product number: T32PNW 3-12), 4.2 parts by mass of aramid fiber (product number: Twaron (registered trademark) 1094), and 138.9 parts by mass of metal fiber were prepared, and these were mixed and dispersed in water to prepare a slurry with a solid content of 1%. 1 part by mass corresponds to 0.1 g. This is the same in the following description of the examples. This slurry was fed into a filter equipped with a 25 cm square inlet, and a sheet-like wet sheet, which is the residue obtained by filtration, was formed. The wet sheet was set in a press machine heated to 150°C and pressurized and heated at a surface pressure of 13.4 MPa for about 20 minutes, and the wet sheet was dried to remove moisture, resulting in a 1.4 mm thick, 1435 g / m2 wet sheet in which artificial graphite particles, PPS particles, aramid fibers, and metal fibers were dispersed. 2 A pre-intermediate layer plate was manufactured. 977.8 parts by mass of artificial graphite particles (product number: 1707SJ), 244.4 parts by mass of artificial graphite particles (product number: AT-No.5S), 100 parts by mass of PPS powder, 62.5 parts by mass of carbon fiber, and 4.2 parts by mass of aramid fiber (product number: Twaron (registered trademark) D8016) were prepared, and these were mixed and dispersed in water to produce a slurry with a solid content of 1%. This slurry was fed into a filter equipped with a 25 cm square mesh-structured inlet, and a sheet-like wet sheet, which was the residue obtained by filtration, was formed. The wet sheet was set in a press machine heated to 150°C and pressurized and heated for about 20 minutes at a surface pressure of 13.4 MPa, and the wet sheet was dried to remove the moisture, resulting in a sheet with carbon fiber unevenly distributed on one side of the thickness direction, with a thickness of 0.3 mm and a basis weight of 349 g / m 2 A pre-surface plate was manufactured. Next, a PPS film was laid in the recess inside the lower mold constituting the split mold, and the pre-surface plate, the pre-middle layer plate, and the pre-surface plate were laminated on the film in this order. At this time, the pre-surface plate, the pre-middle layer plate, and the pre-surface plate were laminated so that the surface opposite to the side where the carbon fibers are unevenly distributed in the pre-surface plate was in contact with the pre-middle layer plate. Then, a PPS film was placed on the pre-surface plate laminated on the pre-middle layer plate. Next, the upper mold constituting the split mold and the lower mold were closed to perform molding. The molding was performed by heating the mold to a temperature of 340°C at a surface pressure of 13.4 MPa, and then increasing the pressure to 53.7 MPa and holding for 1 minute. Then, the mold was pressurized and cooled to 30°C while maintaining the pressure. After molding, the mold was opened, the molded body was removed, and the production of the separator was completed. This separator has a five-layer structure of a film, a surface plate, a middle layer plate, a surface plate, and a film. The separator was evaluated by the above-mentioned evaluation method.
[0066] <Comparative Example> (1) Comparative Example 1 977.8 parts by mass of artificial graphite particles (product number: 1707SJ), 244.4 parts by mass of artificial graphite particles (product number: AT-No.5S), 100 parts by mass of PPS powder, 62.5 parts by mass of aramid fiber (product number: T32PNW 3-12), and 4.2 parts by mass of aramid fiber (product number: Twaron (registered trademark) D8016) were prepared, and these were mixed and dispersed in water to produce a slurry with a solid content of 1%. This slurry was formed into a wet sheet using a 25 cm square sheet machine with a mesh structure, and the wet sheet was set in a press machine heated to 150°C and pressurized and heated for about 20 minutes at a surface pressure of 13.4 MPa, and the wet sheet was dried to remove moisture, resulting in a 2.0 mm thick, 2089 g / m2 sheet with dispersed artificial graphite particles, PPS particles, and aramid fibers. 2 A pre-intermediate layer plate was manufactured. Next, a PPS film was laid in the recess inside the lower mold constituting the split mold, and the pre-middle layer plate was provided on the film. Then, the PPS film was placed on the pre-middle layer plate. Next, the upper mold constituting the split mold and the lower mold were closed to perform molding. The molding was performed by heating the mold to a temperature of 340°C at a surface pressure of 13.4 MPa, increasing the surface pressure to 53.7 MPa, and holding for 1 minute. Thereafter, the mold was pressurized and cooled to 30°C while maintaining the pressure. After the molding was completed, the mold was opened, the molded body was removed, and the production of the separator was completed. Comparative Example 1 was performed without using a surface plate. That is, the separator of Comparative Example 1 has a three-layer structure of a film, a middle layer plate, and a film. Comparative Example 1 was also performed using a middle layer plate that did not contain metal fibers. The separator was evaluated by the above evaluation method. (2) Comparative Example 2 A PPS film was laid in the recess on the inside of the lower die constituting the split type die, and two pre-middle layer plates of Example 1 were laminated on the film. The pre-middle layer plate is a plate in which aramid fibers are unevenly distributed on one side in the thickness direction. At this time, two pre-middle layer plates were laminated so that the surfaces on the side on which the aramid fibers are unevenly distributed and the opposite side were in contact with each other. Then, a PPS film was placed on the pre-middle layer plate. Next, the upper die constituting the split type die and the lower die were closed to perform molding. The molding was performed by heating the die to a temperature of 340°C at a surface pressure of 13.4 MPa, increasing the surface pressure to 53.7 MPa, and holding for 1 minute. Thereafter, the die was pressurized and cooled to 30°C while maintaining the pressure. After completion of molding, the die was opened, the molded body was removed, and the production of the separator was completed. This separator has a four-layer structure of a film, a middle layer plate, a middle layer plate, and a film. The separator was evaluated by the above evaluation method.
[0067] 7.Results Table 1 shows the production conditions and evaluation results of the examples and comparative examples.
[0068] [Table 1]
[0069] The contact resistance value of Comparative Example 2 was large and the result was unacceptable, whereas the Example was accepted.
[0070] From the above results, and by comparing the Example with Comparative Examples 1 and 2, the effect of using a surface plate containing conductive fibers under the film was confirmed. [Industrial Applicability]
[0071] The separator according to the present invention can be used as a separator between cells in a battery, particularly in a storage battery. [Explanation of symbols]
[0072] DESCRIPTION OF THE REFERENCE NUMERALS 1 separator, 2 plate, 3, 4 surface plate, 5 middle plate, 6, 7 film, 8 barrier layer, 30, 32 groove, 31 surface, 40 lower mold (a component of the mold), 41, 51 recess, 42, 52 unevenness, 50 upper mold (a component of the mold), 60 mold, 70, 70a laminate, 72, 72a pre-surface plate (an example of a first molded object), 74 pre-middle plate (an example of a second molded object), F coating layer, M filling layer.
Claims
1. A plate having a groove on its surface as a flow path; a barrier layer including the groove and a surface of the plate other than the groove, the barrier layer being formed on both surfaces of the plate in the thickness direction, the barrier layer having a gas barrier property superior to that of the plate; Equipped with The plate is a middle plate including graphite and resin; a surface layer plate including graphite, resin, and conductive fibers and laminated on both surfaces of the intermediate layer plate in the thickness direction; Equipped with A separator, wherein the conductive fibers of the surface plate are unevenly distributed on the barrier layer side in the thickness direction of the surface plate.
2. 2. The separator according to claim 1, wherein the barrier layer is a film-like covering layer different from the plate.
3. 2. The separator according to claim 1, wherein the barrier layer is a filled layer in which resin or rubber fills spaces between particles or fibers that constitute the plate.
4. 4. The separator according to claim 3, wherein the barrier layer includes the filling layer and a film-like covering layer different from the plate.
5. 5. The separator according to claim 1, wherein the conductive fibers are carbon fibers.
6. 6. The separator according to claim 1, wherein the surface plate further contains aramid fibers separate from the resin.
7. 7. The separator according to claim 1, wherein the surface plate contains at least one of polyether ether ketone and polyphenylene sulfide as the resin.
8. 8. The separator according to claim 1, wherein the intermediate plate further contains aramid fibers separate from the resin.
9. The separator according to claim 1 , wherein the intermediate plate further comprises metal fibers.
10. 10. The separator according to claim 1, which is a separator for a fuel cell used between cells of a fuel cell.
11. A method for producing the separator according to any one of claims 1 to 10, comprising the steps of: a first film placement step of placing a film for forming the barrier layer in a mold; a first molding object placement step of placing a first molding object containing at least graphite, resin, and conductive fibers on the film; a second molding object arranging step of arranging a second molding object containing at least graphite and a resin on the first molding object in the die; a third molding object placement step of placing the first molding object on the second molding object; A second film placement step of placing a film for forming the barrier layer on a laminate including the first molded object, the second molded object, and the first molded object; a molding step of closing the mold to mold the laminate sandwiched between the films, thereby forming the barrier layer on both surfaces of the plate in the thickness direction; Including, The method further includes a first pre-molding step of obtaining the first molded object in a semi-cured state from a first mixture containing at least the graphite, the resin, and the conductive fiber, prior to the first molded object arranging step and the third molded object arranging step, The first molding object placement step includes placing the first molding object in a semi-cured state on the film, The third molding object placement step includes placing the first molding object in a semi-hardened state on the second molding object, The first pre-molding step is for obtaining the semi-cured first molded object from the first mixture, in which the conductive fibers are unevenly distributed on one side of the first molded object in a thickness direction, The first molding object placement step includes placing the first molding object in a semi-cured state on the film in the mold so that a surface of the first molding object on which the conductive fibers are unevenly distributed is in contact with the film in the mold; The method for manufacturing a separator is characterized in that the third molded object placement process places the first molded object in a semi-cured state on the second molded object so that the surface of the first molded object opposite the side on which the conductive fibers are concentrated is in contact with the second molded object in the mold.
12. The method further includes a second pre-molding step of obtaining the second molded object in a semi-cured state from a second mixture containing at least the graphite and the resin, prior to the second molded object placement step; 12. The method for manufacturing a separator according to claim 11, wherein the second molding object placement step includes placing the second molding object in the semi-cured state on the first molding object.
13. the die has an inner surface provided with projections and recesses for transferring the grooves; 13. The method for producing a separator according to claim 11, wherein the molding step comprises molding the laminate and forming the grooves using the die having the projections and recesses.
Citation Information
Patent Citations
Method for manufacturing separator for fuel battery
JP2001122677A
Separator for fuel cell, manufacturing method of separator for fuel cell, and fuel cell
JP2006147173A
Manufacturing method of separator for fuel cell and separator for fuel cell
JP2006294407A
Fuel cell separator, method of manufacturing fuel cell separator and fuel cell
JP2008135299A
Separator for fuel cell and method of manufacturing the same
JP2011090937A