Non-aqueous electrolyte secondary battery
By adding Sr and Al to lithium-transition metal composite oxides, the layered structure is stabilized, enhancing the charge/discharge cycle characteristics of non-aqueous electrolyte secondary batteries by forming a protective film on the negative electrode.
Patent Information
- Application Number
- JP2021545158
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-09
- Filing Date
- 2020-07-30
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2040-07-30
AI Technical Summary
Lithium-transition metal composite oxides with high Ni content experience instability in their layered structure due to excessive Li extraction during charging, leading to reduced battery capacity and poor charge/discharge cycle characteristics.
Incorporating specific amounts of Sr and Al into the lithium-transition metal composite oxide, forming a protective film on the negative electrode surface, stabilizes the layered structure and enhances cycle characteristics by modifying the particle surface.
The synergistic effect of Sr and Al improves the charge/discharge cycle characteristics of non-aqueous electrolyte secondary batteries by stabilizing the layered structure and reducing capacity loss.
Smart Images

Figure 0007588079000002 
Figure 0007588079000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery, and more particularly to a non-aqueous electrolyte secondary battery that uses a lithium transition metal composite oxide containing Ni as a positive electrode active material. [Background technology]
[0002] In recent years, lithium transition metal composite oxides with a high Ni content have been attracting attention as a positive electrode active material with high energy density. For example, Patent Document 1 describes a compound represented by the general formula Li x Ni y Co z M m and a BET specific surface area of 0.8 m or less. 2 / g or less. Patent Document 2 discloses a positive electrode active material for a nonaqueous electrolyte secondary battery, which is made of a lithium transition metal composite oxide having a layered structure and contains at least one of Ni and Co, and also contains at least one of Sr, W, and Sb, and Mo. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2003-100295 A [Patent Document 2] JP 2007-299668 A Summary of the Invention
[0004] When a lithium transition metal composite oxide with a high Ni content is used as the positive electrode active material, the amount of Li extracted during charging is large, which makes the layered structure of the composite oxide unstable and tends to cause a decrease in battery capacity during charging and discharging. Note that the techniques disclosed in Patent Documents 1 and 2 still have room for improvement in terms of charge-discharge cycle characteristics.
[0005] A nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure is a nonaqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a nonaqueous electrolyte, the positive electrode having a layered structure and including a lithium transition metal composite oxide containing at least Ni, Al, and Sr, the lithium transition metal composite oxide having a Ni content of 80 to 95 mol % relative to the total number of moles of metal elements excluding Li, an Al content of 8.0 mol % or less relative to the total number of moles of metal elements excluding Li, and a Sr content of 1.2 mol % or less relative to the total number of moles of metal elements excluding Li, the proportion of metal elements other than Li present in the Li layer being 0.5 to 2.0 mol % relative to the total number of moles of metal elements excluding Li, and the negative electrode having a negative electrode mixture layer including a negative electrode active material and a coating containing Sr formed on a surface of the negative electrode mixture layer, the content of Sr in the coating being 20 to 400 ppm relative to the total mass of the negative electrode mixture layer and the coating.
[0006] According to one aspect of the present disclosure, in a non-aqueous electrolyte secondary battery using a lithium transition metal composite oxide with a high Ni content, it is possible to suppress a decrease in capacity accompanying charge and discharge. The non-aqueous electrolyte secondary battery according to the present disclosure has excellent charge and discharge cycle characteristics. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Lithium transition metal composite oxides with a high Ni content have high particle surface activity, and when used as a positive electrode active material, side reactions with the electrolyte occur on the particle surface, damaging the particle surface of the lithium transition metal composite oxide. In addition, because a large amount of Li is extracted from the lithium transition metal composite oxide during charging, the layered structure of the lithium transition metal composite oxide collapses and becomes unstable when the charge and discharge are repeated. Therefore, it is considered that a non-aqueous electrolyte secondary battery in which the lithium transition metal composite oxide is used as a positive electrode active material is prone to a decrease in battery capacity due to charging and discharging.
[0009] Therefore, the present inventors have conducted intensive research to solve the above problems, and have found that by adding a predetermined amount of Sr to the lithium transition metal composite oxide in addition to a predetermined amount of Al, and replacing part of the Li in the Li layer with other metal elements, the layered structure of the lithium transition metal composite oxide is stabilized, and a good coating containing Sr derived from the positive electrode is formed on the surface of the negative electrode, thereby protecting the negative electrode. It is believed that the charge and discharge cycle characteristics of a battery using the lithium transition metal composite oxide are improved by the synergistic effect of the layered structure stabilization by containing a predetermined amount of Al and replacing Li in the Li layer with a predetermined amount of other metal elements, and the good negative electrode protective coating containing Sr. Note that if the amount of other metal elements present in the Li layer is too large, the diffusion of Li is hindered, leading to an increase in resistance and a decrease in discharge capacity.
[0010] In this specification, the expression "numeric value (A) to numerical value (B)" means numerical value (A) or more and numerical value (B) or less.
[0011] An example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail below. A cylindrical battery in which a wound electrode body 14 is housed in a cylindrical exterior can 16 with a bottom will be exemplified below, but the exterior can is not limited to a cylindrical exterior can, and may be, for example, a rectangular exterior can, or may be an exterior made of a laminate sheet including a metal layer and a resin layer. The electrode body may also be a laminated type electrode body in which multiple positive electrodes and multiple negative electrodes are alternately stacked with separators interposed therebetween.
[0012] FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 according to an embodiment. As illustrated in FIG. 1, the nonaqueous electrolyte secondary battery 10 includes a wound electrode assembly 14, a nonaqueous electrolyte, and an exterior can 16 that accommodates the electrode assembly 14 and the electrolyte. The electrode assembly 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a wound structure in which the positive electrode 11 and the negative electrode 12 are wound in a spiral shape with the separator 13 interposed therebetween. The exterior can 16 is a cylindrical metal container with a bottom that is open on one axial side, and the opening of the exterior can 16 is closed by a sealing body 17. In the following description, for convenience of explanation, the sealing body 17 side of the battery is referred to as the top, and the bottom side of the exterior can 16 is referred to as the bottom.
[0013] The non-aqueous electrolyte includes a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. For example, esters, ethers, nitriles, amides, and mixed solvents of two or more of these are used as the non-aqueous solvent. The non-aqueous solvent may contain a halogen-substituted product in which at least a part of the hydrogen of these solvents is replaced with a halogen atom such as fluorine. For the electrolyte salt, for example, a lithium salt such as LiPF6 is used. The electrolyte is not limited to a liquid electrolyte, and may be a solid electrolyte using a gel-like polymer or the like.
[0014] The positive electrode 11, the negative electrode 12, and the separator 13 constituting the electrode body 14 are all long strip-shaped bodies, and are alternately stacked in the radial direction of the electrode body 14 by being wound in a spiral shape. The negative electrode 12 is formed to be slightly larger than the positive electrode 11 in order to prevent lithium deposition. That is, the negative electrode 12 is formed to be longer than the positive electrode 11 in the longitudinal direction and the width direction (short direction). The two separators 13 are formed to be at least slightly larger than the positive electrode 11, and are arranged to sandwich the positive electrode 11, for example. The electrode body 14 has a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like.
[0015] Insulating plates 18 and 19 are disposed above and below the electrode body 14. In the example shown in Fig. 1, the positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and the negative electrode lead 21 passes outside the insulating plate 19 and extends toward the bottom side of the outer casing 16. The positive electrode lead 20 is connected to the lower surface of an internal terminal plate 23 of the sealing body 17 by welding or the like, and a cap 27, which is a top plate of the sealing body 17 and is electrically connected to the internal terminal plate 23, serves as a positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom inner surface of the outer casing 16 by welding or the like, and the outer casing 16 serves as a negative electrode terminal.
[0016] A gasket 28 is provided between the exterior can 16 and the sealing body 17 to ensure airtightness inside the battery. The exterior can 16 has a grooved portion 22 formed therein, with part of the side surface protruding inward, to support the sealing body 17. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior can 16, and supports the sealing body 17 on its upper surface. The sealing body 17 is fixed to the top of the exterior can 16 by the grooved portion 22 and the open end of the exterior can 16 which is crimped against the sealing body 17.
[0017] The sealing body 17 has a structure in which an internal terminal plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are laminated in this order from the electrode body 14 side. Each member constituting the sealing body 17 has, for example, a disk shape or a ring shape, and each member except the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks so as to push the upper valve body 26 toward the cap 27, thereby cutting off the current path between the lower valve body 24 and the upper valve body 26. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0018] The positive electrode 11, negative electrode 12, and separator 13 that constitute the electrode assembly 14, and in particular the positive electrode active material that constitutes the positive electrode 11, and the coating formed on the surface of the negative electrode 12, will be described in detail below.
[0019] [Positive electrode] The positive electrode 11 has a positive electrode core and a positive electrode composite layer provided on the surface of the positive electrode core. For the positive electrode core, a foil of a metal such as aluminum that is stable in the potential range of the positive electrode 11, a film with the metal disposed on the surface layer, or the like can be used. The positive electrode composite layer contains a positive electrode active material, a binder, and a conductive material, and is preferably provided on both sides of the positive electrode core except for the part to which the positive electrode lead 20 is connected. The positive electrode 11 can be produced, for example, by applying a positive electrode composite slurry containing a positive electrode active material, a binder, a conductive material, and the like to the surface of the positive electrode core, drying the coating, and then compressing it to form a positive electrode composite layer on both sides of the positive electrode core.
[0020] Examples of the conductive material contained in the positive electrode mixture layer include carbon materials such as carbon black, acetylene black, ketjen black, and graphite. Examples of the binder contained in the positive electrode mixture layer include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. These resins may be used in combination with cellulose derivatives such as carboxymethylcellulose (CMC) or its salt, and polyethylene oxide (PEO).
[0021] The positive electrode 11 has a layered structure and contains a lithium transition metal composite oxide containing at least Ni, Al, and Sr. Hereinafter, for convenience of explanation, the lithium transition metal composite oxide is referred to as a "composite oxide (Z)". The composite oxide (Z) functions as a positive electrode active material. The composite oxide (Z) has, for example, a layered structure belonging to the space group R-3m, or a layered structure belonging to the space group C2 / m. The positive electrode active material may be mainly composed of the composite oxide (Z) and substantially composed of only the composite oxide (Z). Note that the positive electrode active material may contain a composite oxide other than the composite oxide (Z) or other compounds within a range that does not impair the object of the present disclosure.
[0022] The complex oxide (Z) is, for example, a secondary particle formed by agglomeration of a plurality of primary particles. The particle size of the primary particles is generally 0.05 μm to 1 μm. The volume-based median diameter (D50) of the complex oxide (Z) is, for example, 3 μm to 30 μm, preferably 5 μm to 25 μm. D50 means the particle size at which the cumulative frequency is 50% from the smallest particle size in the volume-based particle size distribution, and is also called the median diameter. The particle size distribution of the complex oxide (Z) can be measured using a laser diffraction type particle size distribution measuring device (for example, MT3000II manufactured by Microtrack Bell Co., Ltd.) using water as a dispersion medium.
[0023] The composite oxide (Z) contains 80 to 95 mol% of Ni relative to the total number of moles of metal elements excluding Li. By making the Ni content 80 mol% or more, a battery with high energy density can be obtained. On the other hand, if the Ni content exceeds 95 mol%, the Al and Sr contents become too small to ensure the stability of the layered structure of the composite oxide (Z). The Ni content may be 85 mol% or more, or 90 mol% or more, relative to the total number of moles of metal elements excluding Li.
[0024] In the composite oxide (Z), the Ni content is 80 to 95 moles relative to the total moles of metal elements excluding Li. %in The Al content is 8.0 mol% or less based on the total number of moles of metal elements excluding Li. The Al content may be 7.0 mol% or less, or may be 6.0 mol% or less. From the viewpoint of the stability of the layered structure of the composite oxide (Z), the lower limit of the Al content is preferably 1.0 mol%, more preferably 2.0 mol%.
[0025] The content of Sr in the composite oxide (Z) is 1.2 mol% or less, preferably 1.0 mol% or less, based on the total number of moles of metal elements excluding Li. Sr is considered to modify the particle surface of the composite oxide (Z) and to be a source of Sr for the negative electrode coating, suppressing side reactions with the electrolyte at the positive and negative electrodes. If the composite oxide (Z) contains Sr, the effect of improving the charge-discharge cycle characteristics can be obtained, but the Sr content is preferably 0.02 mol% or more. In this case, the effect of improving the charge-discharge cycle characteristics is more pronounced. If the Sr content exceeds 1.2 mol%, the resistance increases and the charge capacity decreases.
[0026] Sr is preferably present on the particle surface of the composite oxide (Z) and in its vicinity, for example, in a surface vicinity region within 30 nm from the particle surface. When the composite oxide (Z) is a secondary particle formed by agglomeration of primary particles, Sr is present on the surface of the primary particles and in its vicinity. That is, Sr is unevenly distributed in the vicinity of the surface of the primary particles of the composite oxide (Z), and the content of Sr per unit volume is higher on the surface than inside the primary particles. The distribution of Sr in the composite oxide (Z) can be analyzed by TEM-EDX or the like.
[0027] Sr exists as a compound in the layered structure or on the surface of the composite oxide (Z). As described above, the Sr contained in the composite oxide (Z) is a Sr source for the negative electrode coating, and a portion of the Sr is dissolved and deposited on the negative electrode surface upon charging and discharging, and is contained in the coating of the negative electrode.
[0028] The composite oxide (Z) may contain a metal element other than Li, Ni, Al, and Sr. Examples of the metal element include Co, Mn, Zr, Mg, Fe, Cu, Zn, Sn, Na, K, Ba, Ca, W, Mo, Si, Nb, Bi, Ti, and Mo.
[0029] When the composite oxide (Z) contains Co, the content of Co is preferably 10 mol% or less based on the total number of moles of metal elements excluding Li. Since Co is expensive, it is preferable to reduce the amount of Co used. The composite oxide (Z) may contain 5 mol% or less of Co based on the total number of moles of metal elements excluding Li, or may contain substantially no Co. "Substantially no Co" means that no Co is contained at all, or that Co is mixed in as an impurity (that is, that Co is mixed in to an extent that cannot be accurately quantified).
[0030] When the composite oxide (Z) contains Mn, the content of Mn is preferably 10 mol % or less based on the total number of moles of metal elements excluding Li. a Ni b Co c Al d Mn e Sr f O g (In the formula, 0.8≦a≦1.2, 0.80≦b≦0.95, 0≦c≦0.05, 0 <d≦0.08、0≦e≦0.10、0<f≦0.012、1≦ g It is a composite oxide represented by the formula (2).
[0031] The Li layer of the composite oxide (Z) contains metal elements other than Li. The ratio of metal elements other than Li present in the Li layer is 0.5 to 2.0 mol% with respect to the total number of moles of metal elements excluding Li. In this case, the structure of the Li layer is stabilized in a state in which Li ions in the Li layer are extracted, and the cycle characteristics are improved. On the other hand, when the ratio is less than 0.5 mol% or exceeds 2.0 mol%, the effect of improving the cycle characteristics cannot be obtained. The metal elements other than Li in the Li layer are considered to be mainly Ni, but may contain other metal elements. The ratio of metal elements other than Li present in the Li layer is obtained from Rietveld analysis of the X-ray diffraction pattern obtained by X-ray diffraction measurement of the composite oxide (Z).
[0032] The content of the elements constituting the composite oxide (Z) can be measured by an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.
[0033] The method for producing the composite oxide (Z) includes, for example, a first step of obtaining a metal composite oxide containing Ni, Al and an arbitrary metal element, a second step of mixing the metal composite oxide obtained in the first step with a Li compound to obtain a mixture, and a third step of firing the mixture. The ratio of metal elements other than Li in the Li layer of the layered structure of the composite oxide (Z) finally obtained is adjusted by controlling, for example, the mixing ratio of the raw materials in the second step and the firing temperature, time, etc. in the third step.
[0034] In the first step, for example, an alkaline solution such as sodium hydroxide is dropped into a stirred solution of a metal salt containing Ni, Al, and an arbitrary metal element (Co, Mn, Fe, etc.) to adjust the pH to the alkaline side (e.g., 8.5 to 12.5), thereby precipitating (co-precipitating) a metal composite hydroxide containing Ni, Al, and the arbitrary metal element, and then the metal composite hydroxide is calcined to produce Ni, Al, and the arbitrary metal element. Genus The calcination temperature is not particularly limited, but is, for example, in the range of 300°C to 600°C.
[0035] In the second step, the metal composite oxide obtained in the first step, a lithium compound, and a strontium compound are mixed to obtain a mixture. Examples of the lithium compound include Li2CO3, LiOH, Li2O2, Li2O, LiNO3, LiNO2, Li2SO4, LiOH·H2O, LiH, and LiF. Examples of the strontium compound include Sr(OH)2, SrO, SrCO3, SrSO4, and Sr(NO3)2. The mixing ratio of the metal composite oxide obtained in the first step and the Li compound is preferably such that the molar ratio of metal elements other than Li:Li is in the range of 1:0.98 to 1:1.1, in order to easily adjust the above parameters to the above-specified ranges. In the second step, when the metal composite oxide obtained in the first step, the Li compound, and the Sr compound are mixed, other metal raw materials may be added as necessary. The other metal raw materials are oxides, hydroxides, etc. containing metal elements other than the metal elements constituting the metal oxide obtained in the first step.
[0036] In the third step, the mixture obtained in the second step is fired at a predetermined temperature for a predetermined time to obtain the composite oxide (Z) according to this embodiment. The firing of the mixture in the third step includes a multi-stage firing process including a first firing process in which the mixture is fired in a firing furnace under an oxygen stream at a first heating rate to a first set temperature of 450°C or higher and 680°C or lower, and a second firing process in which the fired product obtained in the first firing process is fired in a firing furnace under an oxygen stream at a second heating rate to a second set temperature of more than 680°C and 800°C or lower.
[0037] Here, the first heating rate is in the range of 1.5°C / min to 5.5°C / min, and the second heating rate is slower than the first heating rate, in the range of 0.1°C / min to 3.5°C / min. By such multi-stage firing, in the composite oxide (Z) of this embodiment finally obtained, the parameters of the ratio of metal elements other than Li present in the Li layer of the layered structure can be adjusted to the above-specified range. Note that the first heating rate and the second heating rate may be set multiple times for each temperature region as long as they are within the above-specified range.
[0038] The holding time of the first set temperature in the first firing step is preferably 0 to 5 hours, more preferably 0 to 3 hours, from the viewpoint of adjusting the above parameters of the composite oxide (Z) to the above-specified ranges. The holding time of the first set temperature is the time during which the first set temperature is maintained after the first set temperature is reached. The holding time of the second set temperature in the second firing step is preferably 1 to 10 hours, more preferably 1 to 5 hours, from the viewpoint of adjusting the above parameters of the lithium transition metal composite oxide to the above-specified ranges. The holding time of the second set temperature is the time during which the second set temperature is maintained after the second set temperature is reached.
[0039] When the mixture is fired, the above parameters are adjusted to fall within the above-specified ranges, for example, in an oxygen flow with an oxygen concentration of 60% or more, and the flow rate of the oxygen flow is set at 10 cm 3 The flow rate should be in the range of 0.2mL / min to 4mL / min per kg of mixture and 0.3L / min or more per kg of mixture.
[0040] [Negative electrode] The negative electrode 12 has a negative electrode core and a negative electrode composite layer provided on the surface of the negative electrode core. For the negative electrode core, a foil of a metal such as copper that is stable in the potential range of the negative electrode 12, a film with the metal disposed on the surface layer, or the like can be used. The negative electrode composite layer contains a negative electrode active material and a binder, and is preferably provided on both sides of the negative electrode core except for the part to which the negative electrode lead 21 is connected. The negative electrode 12 can be produced, for example, by applying a negative electrode composite slurry containing a negative electrode active material and a binder to the surface of the negative electrode core, drying the coating, and then compressing it to form a negative electrode composite layer on both sides of the negative electrode core.
[0041] The negative electrode mixture layer contains, as the negative electrode active material, for example, a carbon-based active material that reversibly absorbs and releases lithium ions. Suitable carbon-based active materials are graphites such as natural graphite, such as flake graphite, lump graphite, and earthy graphite, and artificial graphite, such as lump artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB). In addition, the negative electrode active material may be a Si-based active material composed of at least one of Si and a Si-containing compound, or a carbon-based active material and a Si-based active material may be used in combination.
[0042] The binder contained in the negative electrode mixture layer may be, as in the case of the positive electrode 11, a fluororesin, PAN, polyimide, acrylic resin, polyolefin, or the like, but it is preferable to use styrene-butadiene rubber (SBR). The negative electrode mixture layer preferably further contains CMC or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), or the like. Among them, it is preferable to use SBR in combination with CMC or a salt thereof, or PAA or a salt thereof.
[0043] The negative electrode 12 has a coating containing Sr (hereinafter, sometimes referred to as "negative electrode coating") formed on the surface of the negative electrode mixture layer. It is considered that the negative electrode coating is formed by depositing Sr in the complex oxide (Z) dissolved by charging and discharging on the surface of the negative electrode mixture layer. That is, the negative electrode coating contains Sr derived from the complex oxide (Z). The negative electrode coating is formed, for example, by 10 or fewer cycles of charging and discharging. By using the complex oxide (Z) containing a specific amount of Sr and forming a good quality coating containing Sr derived from the positive electrode on the negative electrode surface, the capacity decrease due to charging and discharging is suppressed, and good cycle characteristics are obtained. The presence of the negative electrode coating can be confirmed, for example, by X-ray photoelectron spectroscopy (XPS).
[0044] The Sr content in the negative electrode coating is 20 to 400 ppm with respect to the total mass of the negative electrode composite layer and the coating. If the Sr content is less than 20 ppm or more than 400 ppm, the effect of improving the charge-discharge cycle characteristics cannot be obtained. The Sr content in the negative electrode coating can be controlled by the composition of the composite oxide (Z), particularly the Sr content in the composite oxide (Z), as well as by charge-discharge conditions such as the charge cut-off voltage and the charge-discharge test temperature.
[0045] The negative electrode coating may further contain Ni. It is considered that Ni in the complex oxide (Z) dissolved by charging and discharging is deposited on the surface of the negative electrode mixture layer together with Sr to form the negative electrode coating. That is, the negative electrode coating contains Ni derived from the complex oxide (Z). The mass ratio (Ni / Sr) of Sr to Ni in the coating is preferably 0.3 to 2.0. If the Ni / Sr ratio is within this range, the effect of improving cycle characteristics can be enhanced. The Ni / Sr ratio can be controlled by the composition of the complex oxide (Z), particularly the ratio of the contents of Sr and Ni, or by charge / discharge conditions such as the end-of-charge voltage and the charge / discharge test temperature.
[0046] The negative electrode coating may further contain Al. The negative electrode coating contains Al derived from the composite oxide (Z). The mass ratio (Al / Sr) of Sr to Al in the coating is preferably 0.3 to 20.0. When the Al / Sr ratio is within this range, the effect of improving cycle characteristics can be enhanced. The Al / Sr ratio can be controlled by the composition of the composite oxide (Z), particularly the ratio of the Sr and Al contents, or by charge / discharge conditions such as the end-of-charge voltage and the charge / discharge test temperature.
[0047] The negative electrode coating may contain metal elements other than Sr, Ni, and Al. The negative electrode coating contains, for example, metal elements such as Sr, Ni, and Al, and organic substances that are decomposition products of the electrolyte. The contents of Sr, Ni, and Al in the negative electrode coating, the mass ratio of Ni / Sr, and the mass ratio of Al / Sr can be determined by removing the negative electrode from the battery after charging and discharging, dissolving the negative electrode mixture layer, and analyzing the solution by ICP-AES.
[0048] [Separator] A porous sheet having ion permeability and insulating properties is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. The material of the separator 13 is preferably a polyolefin such as polyethylene or polypropylene, or cellulose. The separator 13 may have either a single-layer structure or a laminated structure. A heat-resistant layer or the like may be formed on the surface of the separator.
[0049] <Example> The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.
[0050] <Example 1> [Synthesis of lithium transition metal composite oxide (positive electrode active material)] General formula Ni 0.82 Co 0.05 Al 0.03 Mn 0.10 The metal composite oxide was mixed with strontium hydroxide (Sr(OH)2) so that the Sr content was 0.08 mol% relative to the total amount of Ni, Co, Al, and Mn in the metal composite oxide represented by O2, and lithium hydroxide (LiOH) was further mixed so that the molar ratio of Li to the total amount of Ni, Co, Al, Mn, and Sr was 1:1.05. The mixture was fired under an oxygen stream with an oxygen concentration of 95% (flow rate of 5 L / min per 1 kg of the mixture) at a heating rate of 2.0°C / min from room temperature to 650°C, and then fired at a heating rate of 0.5°C / min from 650°C to 780°C. Impurities were removed from the fired product by washing with water to obtain a lithium transition metal composite oxide. The composition of the lithium transition metal composite oxide was analyzed by ICP-AES, and the results showed that Li 0.99 Ni 0.8192 Co 0.05 Al 0.03 Mn 0.10 Sr 0.0008 It was O2.
[0051] [Preparation of positive electrode] The above-mentioned lithium transition metal composite oxide was used as the positive electrode active material. The positive electrode active material, acetylene black, and polyvinylidene fluoride (PVdF) were mixed in a solid content mass ratio of 95:3:2, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added, and then the mixture was kneaded to prepare a positive electrode composite slurry. The positive electrode composite slurry was applied to both sides of a positive electrode core made of aluminum foil, and the coating film was dried. The coating film was then rolled using a roller and cut to a predetermined electrode size to obtain a positive electrode in which a positive electrode composite layer was formed on both sides of the positive electrode core. An exposed portion in which the surface of the positive electrode core was exposed was provided in a part of the positive electrode.
[0052] [Preparation of negative electrode] Natural graphite was used as the negative electrode active material. The negative electrode active material, sodium carboxymethylcellulose (CMC-Na), and styrene-butadiene rubber (SBR) were mixed in an aqueous solution at a solid content mass ratio of 100:1:1 to prepare a negative electrode composite slurry. The negative electrode composite slurry was applied to both sides of a negative electrode core made of copper foil, and the coating film was dried. The coating film was then rolled using a roller and cut to a predetermined electrode size to obtain a negative electrode in which a negative electrode composite layer was formed on both sides of the negative electrode core. An exposed portion was provided in part of the negative electrode, where the surface of the negative electrode core was exposed.
[0053] [Preparation of non-aqueous electrolyte] A non-aqueous electrolyte was prepared by dissolving lithium hexafluorophosphate (LiPF6) at a concentration of 1.2 mol / L in a mixed solvent of ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) in a volume ratio of 3:3:4.
[0054] [Preparation of test cell (non-aqueous electrolyte secondary battery)] An aluminum lead was attached to the exposed portion of the positive electrode, and a nickel lead was attached to the exposed portion of the negative electrode, and the positive and negative electrodes were spirally wound with a polyolefin separator interposed therebetween, and then pressed in the radial direction to produce a flat wound electrode body. This electrode body was housed in an exterior body made of an aluminum laminate sheet, and the nonaqueous electrolyte was injected, and the opening of the exterior body was sealed to obtain a test cell.
[0055] The ratio of metal elements other than Li in the Li layer of the lithium transition metal composite oxide was evaluated by the following method. In addition, the Sr content, Ni / Sr ratio, Al / Sr ratio, and charge / discharge cycle characteristics in the coating formed on the surface of the negative electrode of the test cell were evaluated by the following methods. The evaluation results are shown in Table 1 (the same applies to the examples and comparative examples described later).
[0056] [Ratio of metal elements other than Li in the Li layer of lithium transition metal composite oxide] The ratio of metal elements other than Li present in the Li layer is determined by Rietveld analysis of the X-ray diffraction pattern obtained by X-ray diffraction measurement of the lithium transition metal composite oxide. The X-ray diffraction pattern is obtained by the powder X-ray diffraction method under the following conditions using a powder X-ray diffractometer (manufactured by Rigaku Corporation, product name "RINT-TTR", radiation source Cu-Kα).
[0057] Measurement range: 15-120° Scan speed: 4° / min Analysis range: 30-120° Background: B-spline Profile function: Split pseudo-Voigt function Constraint condition: Li(3a)+Ni(3a)=1 Ni(3a)+Ni(3b)=y (y is the Ni content in each element) ICSD No.:98-009-4814 In addition, the Rietveld analysis software PDXL2 (Rigaku Corporation) is used for the Rietveld analysis of the X-ray diffraction patterns.
[0058] [Evaluation of negative electrode coating] The test cell after the cycle test described later was disassembled, the negative electrode was taken out, and the negative electrode mixture layer was dissolved. The Sr content, Ni / Sr ratio, and Al / Sr ratio in the coating formed on the surface of the negative electrode mixture layer were determined by ICP-AES. Negative electrode mixture layer and coating The Ni / Sr ratio was 1.0 and the Al / Sr ratio was 8.2.
[0059] [Evaluation of charge / discharge cycle characteristics (capacity retention rate after cycle test)] The above test cell was charged at a constant current of 0.2 It in a temperature environment of 25°C until the battery voltage reached 4.2 V, and then charged at a constant voltage until the current value reached 1 / 100 It at 4.2 V. Thereafter, constant current discharge was performed at a constant current of 0.2 It until the battery voltage reached 2.5 V. This charge / discharge cycle was repeated 30 times. The discharge capacity at the first cycle and the discharge capacity at the 30th cycle of the cycle test were obtained, and the capacity retention rate was calculated by the following formula.
[0060] Capacity retention rate (%) = (30th cycle discharge capacity ÷ 1st cycle discharge capacity) × 100 <Example 2> In the synthesis of the positive electrode active material, the general formula Ni 0.90 Co 0.05 Al 0.05 A test cell was produced and evaluated in the same manner as in Example 1, except that a metal composite oxide represented by O2 was used, and the metal composite oxide was mixed with Sr(OH)2 so that the Sr content was 0.05 mol %, the metal composite oxide was mixed with lithium hydroxide (LiOH) so that the molar ratio of the total amount of Ni, Co, Al, Mn, and Sr to Li was 1:1.03, and the mixture was fired from room temperature to 650°C at a heating rate of 2.0°C / min, and then fired from 650°C to 730°C at a heating rate of 0.5°C / min.
[0061] <Example 3> In the synthesis of the positive electrode active material, the metal composite oxide and LiOH were mixed with lithium hydroxide (LiOH) so that the molar ratio of the total amount of Ni, Co, Al, Mn, and Sr to Li was 1:1.05. A test cell was produced and evaluated in the same manner as in Example 2.
[0062] <Example 4> A test cell was produced and evaluated in the same manner as in Example 2, except that in the synthesis of the positive electrode active material, Sr(OH)2 was added so that the Sr content was 0.08 mol %.
[0063] <Example 5> A test cell was produced and evaluated in the same manner as in Example 2, except that in the synthesis of the positive electrode active material, Sr(OH)2 was added so that the Sr content was 0.10 mol %.
[0064] <Example 6> A test cell was prepared and evaluated in the same manner as in Example 2, except that in the synthesis of the positive electrode active material, Sr(OH)2 was added so that the Sr content was 0.50 mol %, and the mixture was fired from room temperature to 650°C at a heating rate of 4.0°C / min, and then fired from 650°C to 730°C at a heating rate of 1.0°C / min.
[0065] <Example 7> A test cell was prepared and evaluated in the same manner as in Example 2, except that in the synthesis of the positive electrode active material, Sr(OH)2 was added so that the Sr content was 1.00 mol % and the oxygen flow rate was set to 8 L / min per 1 kg of the mixture.
[0066] <Example 8> In the synthesis of the positive electrode active material, the general formula Ni 0.92 Al 0.05 Mn 0.03 A test cell was prepared and evaluated in the same manner as in Example 1, except that a metal composite oxide represented by O2 was used, the mixture was fired from room temperature to 650°C at a heating rate of 2.0°C / min, and then fired from 650°C to 700°C at a heating rate of 0.5°C / min, and the metal composite oxide and LiOH were mixed with lithium hydroxide (LiOH) so that the molar ratio of the total amount of Ni, Al, Mn, and Sr to Li was 1:1.03.
[0067] <Example 9> A test cell was prepared and evaluated in the same manner as in Example 8, except that in the synthesis of the positive electrode active material, the metal composite oxide and LiOH were mixed with lithium hydroxide (LiOH) so that the molar ratio of the total amount of Ni, Al, Mn, and Sr to Li was 1:1.01.
[0068] <Comparative Example 1> A test cell was produced and evaluated in the same manner as in Example 1, except that Sr(OH)2 was not added in the synthesis of the positive electrode active material.
[0069] <Comparative Example 2> In the synthesis of the positive electrode active material, the general formula Ni 0.90 Mn 0.10 A test cell was prepared and evaluated in the same manner as in Example 7, except that a metal composite oxide represented by O2 was used, and the metal composite oxide and LiOH were mixed with lithium hydroxide (LiOH) so that the molar ratio of the total amount of Ni, Mn, and Sr to Li was 1:1.1.
[0070] <Comparative Example 3> A test cell was produced and evaluated in the same manner as in Example 2, except that Sr(OH)2 was not added in the synthesis of the positive electrode active material.
[0071] <Comparative Example 4> A test cell was produced in the same manner as in Example 7, except that magnesium hydroxide (Mg(OH)2) was added instead of Sr(OH)2 in the synthesis of the positive electrode active material, and the performance was evaluated.
[0072] <Comparative Example 5> A test cell was produced in the same manner as in Example 7, except that barium hydroxide (Ba(OH)2) was added instead of Sr(OH)2 in the synthesis of the positive electrode active material, and the performance was evaluated.
[0073] <Comparative Example 6> In the synthesis of the positive electrode active material, the metal composite oxide and LiOH were mixed with lithium hydroxide (LiOH) so that the molar ratio of the total amount of Ni, Al, Mn, and Sr to Li was 1:1.15. A test cell was prepared and evaluated in the same manner as in Example 9.
[0074] <Comparative Example 7> A test cell was prepared and evaluated in the same manner as in Example 9, except that in the synthesis of the positive electrode active material, the mixture was fired from room temperature to 650°C at a heating rate of 6.0°C / min, and then fired from 650°C to 750°C at a heating rate of 5.0°C / min.
[0075] <Comparative Example 8> A test cell was produced and evaluated in the same manner as in Example 9, except that in the synthesis of the positive electrode active material, Sr(OH)2 was added so that the Sr content was 1.50 mol %.
[0076] [Table 1]
[0077] As shown in Table 1, the test cells of the examples all have higher capacity retention rates after cycle testing and are superior in charge-discharge cycle characteristics compared to the test cells of the comparative examples. When the positive electrode active material does not contain Sr and a coating containing Sr is not formed on the negative electrode surface (Comparative Examples 1, 3 to 5), the discharge capacity is significantly reduced after the cycle testing. Similarly, when the positive electrode active material does not contain Al (Comparative Example 2), when the positive electrode active material contains Sr but the ratio of metal elements other than Li in the Li layer is out of the range of 0.5 to 2.0 mol% (Comparative Examples 6 and 7), and when the content of Sr in the negative electrode coating exceeds 400 ppm (Comparative Example 8), the discharge capacity is also significantly reduced. That is, the charge-discharge cycle characteristics of the battery are significantly improved by the synergistic effect of the positive electrode active material containing specific amounts of Al and Sr and having specific amounts of metal elements other than Li in the Li layer, and the negative electrode coating containing a specific amount of Sr derived from the positive electrode active material. [Explanation of symbols]
[0078] 10 Secondary battery 11 Positive electrode 12 Negative electrode 13 Separator 14 Electrode body 16 Outer can 17 Sealing body 18,19 Insulating plate 20 Positive lead 21 Negative lead 22 Grooved part 23 Internal terminal board 24 Lower valve body 25 Insulating materials 26 Upper valve 27 Cap 28 Gasket
Claims
1. A non-aqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte, The positive electrode has a layered structure and contains a lithium transition metal composite oxide containing at least Ni, Al, and Sr, In the lithium transition metal composite oxide, The content of Ni is 80 to 95 mol % based on the total number of moles of metal elements excluding Li, The content of Al is more than 0 mol % and 8.0 mol % or less based on the total number of moles of metal elements excluding Li, The content of Sr is more than 0 mol % and 1.2 mol % or less with respect to the total number of moles of metal elements excluding Li, the ratio of all metal elements other than Li present in the Li layer is 0.5 to 2.0 mol % with respect to the total number of moles of all metal elements other than Li contained in the entire lithium transition metal composite oxide; The negative electrode has a negative electrode mixture layer including a negative electrode active material, and a coating containing Sr formed on a surface of the negative electrode mixture layer, a nonaqueous electrolyte secondary battery in which, after assembling the nonaqueous electrolyte secondary battery, the nonaqueous electrolyte secondary battery is subjected to constant-current charging at a constant current of 0.2 It in a temperature environment of 25° C. until a battery voltage reaches 4.2 V, and then constant-voltage charging at 4.2 V until the current value reaches 1 / 100 It, and thereafter constant-current discharging at a constant current of 0.2 It until a battery voltage reaches 2.5 V; after repeating this charge-discharge cycle for 30 cycles, the Sr content in the coating relative to the total mass of the negative electrode composite layer and the coating is 20 to 400 ppm.
2. The nonaqueous electrolyte secondary battery according to claim 1 , wherein the coating further contains Ni.
3. 3. The nonaqueous electrolyte secondary battery according to claim 2, wherein a mass ratio of Sr to Ni (Ni / Sr) in the coating is 0.3 to 2.
0.
4. 4. The nonaqueous electrolyte secondary battery according to claim 1, wherein the coating further contains Al.
5. 5. The nonaqueous electrolyte secondary battery according to claim 4, wherein a mass ratio of Sr to Al (Al / Sr) in the coating is 0.3 to 20.0.
Citation Information
Patent Citations
Alkaline storage battery and its manufacture
JP1997115509A
Nonaqueous electrolyte secondary battery
JP2002313339A
Non-aqueous electrolyte secondary battery
JP2002313417A
Positive electrode material for lithium secondary battery and manufacturing method thereof
JP2003100295A
Positive electrode active material for nonaqueous electrolyte battery, and nonaqueous electrolyte battery using it
JP2007299668A
Cited By
Non-aqueous electrolyte secondary battery
JP2023003048A