Secondary battery and manufacturing method thereof
By controlling adhesive force ratios in secondary batteries, the issue of electrolyte circulation and production efficiency is addressed, resulting in improved performance and durability, especially in large-capacity models.
Patent Information
- Application Number
- JP2021567286
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-26
- Filing Date
- 2020-12-15
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2040-12-15
AI Technical Summary
The challenge in secondary batteries is the balance between maintaining adequate adhesive force to prevent electrode displacement during handling and ensuring effective electrolyte circulation, particularly in large-capacity batteries, where the adhesive strength affects liquid permeability and production efficiency.
The solution involves controlling the adhesive force ratio between the center and outer electrodes within a specific range (0.1 to 0.9) using a heat and pressure-sensitive adhesive, ensuring minimal adhesive strength at the center to enhance electrolyte circulation while maintaining structural integrity.
This approach allows for improved electrolyte distribution, reduced production time, and enhanced power generation performance and durability of secondary batteries, particularly in high-capacity models.
Smart Images

Figure 0007588094000002 
Figure 0007588094000003 
Figure 0007588094000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a secondary battery and a manufacturing method thereof. [Background technology]
[0002] In recent years, the demand for secondary batteries has been increasing in various fields. Among them, lithium ion secondary batteries using non-aqueous electrolytes have attracted attention because of their high energy density. One of the forms is a secondary battery as shown in Patent Document 1. In this form of secondary battery, a flat electrode body in which positive and negative plates are laminated in multiple layers with a separator interposed therebetween is inserted into an exterior body. The positive plate has a positive electrode active material mixture layer provided on both sides of a positive electrode core body, and the negative plate has a negative electrode active material mixture layer provided on both sides of a negative electrode core body. The positive electrode active material and the negative electrode active material each have a structure that allows the insertion and removal of lithium ions. The separator is a porous material that allows the lithium ions to pass through while preventing a short circuit caused by electrical contact between the positive and negative electrodes.
[0003] The positive and negative plates are electrically connected to the current collectors and inserted into the exterior housing. The exterior housing is sealed after the electrolyte is injected. In this secondary battery, an adhesive layer is provided on the surface of the separator to prevent direct contact between the positive and negative electrodes due to the separator shrinking, and the positive and negative plates are bonded together by thermocompression. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2014-26943 A Summary of the Invention
[0005] The present inventors have discovered the following new problem: To be more specific, when an adhesive material is provided between the electrode and the separator in order to facilitate the handling of the electrode assembly and to prevent the electrode plates from shifting from one position to another within the laminate, and in particular to prevent the electrode plates from shifting from one position to another when the laminate is inserted into the sealing body, the liquid circulation (liquid permeability) of the electrolyte depends on the strength of the adhesion.
[0006] That is, when the adhesive strength is strong, the density of the adhesive material increases and the gap between the electrode and the separator narrows, which tends to impair the liquid circulation of the electrolyte, whereas when the adhesive strength is weak, the liquid circulation is good, but the handling of the electrode assembly is impaired and the separator is likely to become misaligned relative to the electrode.
[0007] More specifically, the liquid circulation property will be described. Since the electrolyte permeates from the end of the electrode assembly in the stacking direction, the electrolyte permeates less easily and spreads over the entire electrode surface as it moves away from the electrode located at the end of the electrode assembly in the stacking direction. In other words, the electrolyte permeates less easily toward the center of the stack. This problem is particularly noticeable in large-capacity secondary batteries that have a large electrode area and require a large amount of electrolyte between each electrode, and in large-capacity secondary batteries, it takes time to spread a sufficient amount of electrolyte over the entire surface of the electrode assembly. Therefore, when an adhesive is used, there is a risk of causing a significant decrease in productivity, especially in large-capacity secondary batteries.
[0008] Therefore, it is considered that the adhesive should have a minimum adhesive strength to achieve this purpose in order to improve the liquid circulation. However, such control of adhesive strength may have a significant impact on the production takt time. Specifically, in order to make the adhesive strength of the entire laminate group uniform while keeping the adhesive strength inside the laminate to a necessary minimum, when an adhesive material whose adhesive strength depends at least on heat and pressure is used, it is necessary to make the temperature of the entire laminate uniform at a relatively low temperature in order to suppress the separator on the outside in the stacking direction from collapsing due to heat, and this requires a long time for the heat pressing process.
[0009] A secondary battery according to one embodiment of the present disclosure includes a first electrode core and a plurality of first electrodes having a first electrode active material arranged on the first electrode core, a second electrode core and a plurality of second electrodes having a second electrode active material arranged on the second electrode core, one or more separators, at least one side surface in the thickness direction of the separator, and an adhesive arranged between the first electrodes, wherein the plurality of first electrodes and the plurality of second electrodes are alternately stacked with the separators interposed therebetween, and a laminate including the plurality of first electrodes and the plurality of second electrodes has 10 or more first electrodes, and when the adhesive strength between the first electrode in the outermost layer and the separator is A0 [N / m] and the adhesive strength between the first electrode located in the center of the laminate in the stacking direction and the separator is A1 [N / m], A1 / A0 is 0.1 or more and less than 0.9.
[0010] The first electrode may be a positive electrode or a negative electrode. The laminate is composed of, for example, an electrode group or an electrode body, and when the number of stacked first electrodes is an odd number, there is only one first electrode at the center in the stacking direction, but when the number of stacked first electrodes is an even number, there are two first electrodes at the center in the stacking direction. There are two first electrodes in the outermost layer. The A1 / A0 being 0.1 or more means that the value of A1 / A0 is 0.1 or more when the outermost layer first electrode and the center first electrode in the stacking direction, which have the smallest value of A1 / A0, are selected. Similarly, when the A1 / A0 is 0.9 less than This means that the A1 / A0 value is the largest when the first pole on the outermost layer and the first pole in the center of the lamination direction are selected, and the A1 / A0 value is 0.9. less than This means that it is.
[0011] Furthermore, a secondary battery according to another aspect of the present disclosure includes a wound body in which a band-shaped first electrode having a first electrode core and a first electrode active material arranged on the first electrode core, and a band-shaped second electrode having a second electrode active material arranged on the second electrode core are wound five or more times with a band-shaped separator interposed therebetween, the wound body having an adhesive arranged between at least one side surface in the thickness direction of the separator and the first electrode, and when the adhesive strength between the first electrode located at the outermost periphery and the separator is A0 [N / m] and the adhesive strength between the first electrode located at the innermost periphery and the separator is A1 [N / m], A1 / A0 is 0.1 or greater and less than 0.9.
[0012] The first electrode may be a positive electrode or a negative electrode. Even if the secondary battery has a wound electrode body, if the electrode body is flat, the positive electrode, the negative electrode, and the separator are stacked in a local region (a region sandwiched between a pair of press plates) where the press plate that presses the electrode body flat and the electrode are parallel, with the separator disposed between the positive electrode and the negative electrode. Therefore, even if the secondary battery has a wound electrode body, the local region where the press plate and the electrode are parallel can be considered as a laminate, and in this case, the separator located on the innermost side can be considered as the separator on the inside (center) of the laminate, and the separator located on the outermost side can be considered as the separator on the outside of the laminate.
[0013] According to the secondary battery of the present disclosure, it is easy to shorten the cycle time while ensuring the necessary adhesive strength inside the laminate, and further, it is easy to improve the circulation of the electrolyte inside the laminate. Moreover, according to the secondary battery of the present disclosure, such a secondary battery is easy to manufacture. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a perspective view of a prismatic secondary battery according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a perspective view of an electrode body and a sealing plate that constitute the prismatic secondary battery. [Diagram 3] FIG. 3 is an exploded perspective view of an electrode body of the prismatic secondary battery. [Figure 4] FIG. 4 is a schematic cross-sectional view taken along line AA in FIG. [Diagram 5] FIG. 5 is an enlarged schematic cross-sectional view of a portion of the outer side in the stacking direction of the first electrode group cut along a plane approximately perpendicular to the height direction of the prismatic secondary battery, and includes a portion of a separator, a portion of a positive electrode, and an adhesive portion bonded with an adhesive described below. [Figure 6] FIG. 6 is a schematic diagram showing the relationship between the position in the stacking direction and the adhesive strength between the electrodes and the separators in a stacked electrode assembly. [Figure 7] FIG. 7 is an enlarged schematic cross-sectional view of a portion of the inside of the stacking direction of the first electrode group cut by a plane approximately perpendicular to the height direction, and similar to FIG. 5, the enlarged schematic cross-sectional view omits the illustration of the portions of the adhesive that do not exhibit adhesive strength. [Figure 8] FIG. 8 is a plan view of a wound type prismatic secondary battery according to another embodiment. [Figure 9] FIG. 9 is a front view of a wound type prismatic secondary battery. [Figure 10] 10(a) is a cross-sectional view taken along line AA in FIG. 8, FIG. 10(b) is a cross-sectional view taken along line BB in FIG. 10(a), and FIG. 10(c) is a cross-sectional view taken along line CC in FIG. 10(a). [Figure 11A] FIG. 11A is a plan view of a positive electrode included in a wound-type prismatic secondary battery. [Figure 11B] FIG. 11B is a plan view of a negative electrode included in a wound-type prismatic secondary battery. [Figure 12] FIG. 12 is a perspective view showing an expanded winding end side of a flat wound electrode body included in a wound-type prismatic secondary battery. [Figure 13] FIG. 13 is a schematic diagram of a wound electrode body corresponding to FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, the embodiments according to the present disclosure will be described in detail with reference to the accompanying drawings. In addition, when multiple embodiments and modified examples are included below, it is assumed from the beginning that new embodiments will be constructed by appropriately combining the characteristic parts of those. In addition, in the following examples, the same components are given the same symbols in the drawings, and duplicated explanations will be omitted. In addition, multiple drawings include schematic diagrams, and the dimensional ratios of length, width, height, etc. of each member between different drawings do not necessarily match. In addition, among the components described below, components that are not described in the independent claim showing the highest concept are optional components and are not essential components. In addition, in this specification, the expression "numerical value A to numerical value B" means "numerical value A or more and numerical value B or less." In addition, in the following description, the height direction of the outer can 14, 140 is the "vertical direction" of the secondary battery 10, 110, the sealing plate 15 side, 123 side is the "upper", and the bottom side of the outer can 14, 140 is the "lower". Moreover, the direction along the longitudinal direction of the sealing plates 15, 123 is defined as the “lateral direction” of the secondary batteries 10, 110.
[0016] In addition, when the first electrode is a positive electrode or a negative electrode, if the secondary battery has a laminated electrode body, the laminate is composed of, for example, an electrode group or an electrode body, and when the number of laminated first electrodes is an odd number, there is only one first electrode at the center in the lamination direction, but when the number of laminated first electrodes is an even number, there are two first electrodes at the center in the lamination direction. In addition, there are two first electrodes at the outermost layer in the lamination direction. The above A1 / A0 being 0.1 or more means that the value of A1 / A0 is 0.1 or more when the outermost first electrode and the center first electrode in the lamination direction, which have the smallest value of A1 / A0, are selected. Similarly, the above A1 / A0 being 0.9 or less means that the value of A1 / A0 is 0.9 or less when the outermost first electrode and the center first electrode in the lamination direction, which have the largest value of A1 / A0, are selected. Hereinafter, when the term "A1 / A0 is a or more" is used, it means that the value of A1 / A0 is a or more when the first pole in the outermost layer and the first pole in the center in the stacking direction, which have the smallest value of A1 / A0, are selected. Also, when the term "A1 / A0 is b or less" is used, it means that the value of A1 / A0 is b or less when the first pole in the outermost layer and the first pole in the center in the stacking direction, which have the largest value of A1 / A0, are selected. Also, below, when the adhesive strength at the center of a laminate (e.g., an electrode group or an electrode body) is used, it means the adhesive strength of the first pole having the lower adhesive strength among one or two first poles in the center when it means the lower limit. Also, below, when the adhesive strength at the center of a laminate (e.g., an electrode group or an electrode body) is used, it means the adhesive strength of the first pole having the higher adhesive strength among one or two first poles in the center when it means the upper limit.
[0017] Fig. 1 is a perspective view of a prismatic secondary battery 10 according to an embodiment of the present disclosure, and Fig. 2 is a perspective view (showing a state in which an outer can 14 has been removed) of an electrode body 11 and a sealing plate 15 constituting the prismatic secondary battery 10. As shown in Figs. 1 and 2, the prismatic secondary battery (hereinafter simply referred to as a secondary battery) 10 has a prismatic container including an outer can 14 and a sealing plate 15 as an outer body, but the outer body is not limited thereto.
[0018] 1 and 2, a secondary battery 10 includes an electrode assembly 11, an electrolyte, a cylindrical exterior can 14 with a bottom in which the electrode assembly 11 and the electrolyte are housed, and a sealing plate 15 to which a positive electrode terminal 12 and a negative electrode terminal 13 are attached and which closes the opening of the exterior can 14. As will be described in detail later with reference to FIG. 3, the electrode assembly 11 has a structure in which positive electrodes 20 and negative electrodes 30 are alternately stacked with separators 40 interposed therebetween. The exterior can 14 is a flat, substantially rectangular parallelepiped, metallic prismatic container with one end opened in the height direction. The exterior can 14 and the sealing plate 15 are made of, for example, a metallic material mainly composed of aluminum.
[0019] The electrolyte may be an aqueous electrolyte, but is preferably a non-aqueous electrolyte, and in this embodiment, a non-aqueous electrolyte solution is used. The non-aqueous electrolyte solution includes, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous solvent may be, for example, esters, ethers, nitriles, amides, or a mixed solvent of two or more of these. The non-aqueous solvent may contain a halogen-substituted product in which at least a part of the hydrogen of these solvents is replaced with a halogen atom such as fluorine. The electrolyte salt may be, for example, a lithium salt such as LiPF6.
[0020] As described above, the positive electrode terminal 12 and the negative electrode terminal 13 are attached to the sealing plate 15. The sealing plate 15 has a long and narrow rectangular shape, with the positive electrode terminal 12 disposed at one end in the longitudinal direction and the negative electrode terminal 13 disposed at the other end in the longitudinal direction of the sealing plate 15. The positive electrode terminal 12 and the negative electrode terminal 13 are external connection terminals that are electrically connected to other secondary batteries 10 and a load, and are attached to the sealing plate 15 via insulating members.
[0021] As will be described in detail later, the positive electrode 20 includes a positive electrode tab 23 electrically connected to the positive electrode terminal 12, and the negative electrode 30 includes a negative electrode tab 33 electrically connected to the negative electrode terminal 13. The positive electrode terminal 12 is electrically connected via a positive electrode current collector 25 to a positive electrode tab group 24 formed by stacking a plurality of positive electrode tabs 23, and the negative electrode terminal 13 is electrically connected via a negative electrode current collector 35 to a negative electrode tab group 34 formed by stacking a plurality of negative electrode tabs 33.
[0022] The sealing plate 15 is provided with a current interruption device 18 as a functional component for cutting off a current path when an abnormality occurs in the battery. The functional component is, for example, a component that functions as a safety device or a control device for the secondary battery 10. The functional component is disposed adjacent to the positive electrode terminal 12 or the negative electrode terminal 13 on the inner surface of the sealing plate 15. In this embodiment, the current interruption device 18 is associated with the positive electrode terminal 12 and disposed inside the positive electrode terminal 12.
[0023] The current interruption device 18 is a pressure-sensing safety device that interrupts the current path when an abnormality occurs in the secondary battery 10 and the internal pressure of the exterior can 14 rises above a predetermined pressure. The current interruption device 18 is disposed, for example, between the positive terminal 12 and the positive current collector plate 25, and is electrically connected to the positive terminal 12 and the positive current collector plate 25 during normal use. The structure of the current interruption device 18 is not particularly limited, but one example is a device that includes a reversal plate that reverses in a direction away from the positive current collector plate 25 when the internal pressure rises, cutting off the electrical connection with the positive current collector plate 25 and interrupting the current path between the positive terminal 12 and the positive current collector plate 25.
[0024] In addition, sealing plate 15 is provided with liquid injection part 16 for injecting nonaqueous electrolyte, and gas exhaust valve 17 for opening and discharging gas when an abnormality occurs in the battery. Gas exhaust valve 17 is disposed in the center of sealing plate 15 in the longitudinal direction, and liquid injection part 16 is disposed between positive electrode terminal 12 and gas exhaust valve 17.
[0025] 2, the electrode body 11 is divided into a first electrode group 11A and a second electrode group 11B. The electrode groups 11A and 11B have, for example, the same laminated structure and dimensions, and are laminated in the thickness direction of the electrode body 11. A positive electrode tab group 24 consisting of a plurality of positive electrode tabs 23 and a negative electrode tab group 34 consisting of a plurality of negative electrode tabs 33 are formed at the upper end of each electrode group, and are connected to each current collector plate of the sealing plate 15. The outer peripheral surfaces of the electrode groups 11A and 11B are covered with a separator 40, and the electrode groups 11A and 11B are configured to cause independent battery reactions.
[0026] FIG. 3 is an exploded perspective view of the electrode body 11. As illustrated in FIG. 3, the electrode body 11 includes a plurality of positive electrodes 20 and a plurality of negative electrodes 30. For example, the electrode groups 11A and 11B constituting the electrode body 11 include one more negative electrode 30 than the positive electrode 20, and the negative electrode 30 is disposed on both sides of the electrode groups 11A and 11B in the thickness direction. FIG. 3 illustrates a plurality of separators 40 disposed one by one between the positive electrode 20 and the negative electrode 30, but the separators 40 included in the electrode groups 11A and 11B may each be one by one. In this case, the long separator 40 is folded in a zigzag manner and disposed between the positive electrode 20 and the negative electrode 30. As will be described in detail later, in this embodiment, each of the electrode groups 11A and 11B includes an adhesive and is fabricated using a heat press process. More specifically, each of the electrode groups 11A, 11B is produced by pressing a laminate formed by alternately stacking a plurality of positive electrodes 20 and a plurality of negative electrodes 30 one by one with separators 40 interposed therebetween using a pair of hot plates in the stacking direction, thereby applying heat and pressure to the laminate and causing at least a portion of the adhesive to exhibit adhesive strength.
[0027] The electrode body 11 is a laminated electrode body including the electrode group 11A and the electrode group 11B thus produced, and is formed by alternately laminating a plurality of positive electrodes 20 and a plurality of negative electrodes 30 one by one with a separator 40 interposed therebetween. The positive electrode 20 includes a positive electrode tab 23 protruding upward, and the negative electrode 30 includes a negative electrode tab 33 protruding upward. In other words, the positive electrodes 20 and the negative electrodes 30 are laminated so that the tabs face the same direction. The positive electrode tab 23 is located at one lateral end of the electrode body 11, and the negative electrode tab 33 is located at the other lateral end of the electrode body 11, and the plurality of positive electrode tabs 23 are arranged in the thickness direction of the electrode body 11, and the plurality of negative electrode tabs 33 are arranged in the thickness direction of the electrode body 11.
[0028] The positive electrode 20 has a positive electrode core and a positive electrode composite layer provided on the surface of the positive electrode core. For the positive electrode core, a foil of a metal such as aluminum or an aluminum alloy that is stable in the potential range of the positive electrode 20, or a film with the metal disposed on the surface layer, can be used. The positive electrode composite layer contains a positive electrode active material, a conductive material, and a binder, and is preferably provided on both sides of the positive electrode core. The positive electrode 20 can be produced, for example, by applying a positive electrode composite slurry containing a positive electrode active material, a conductive material, and a binder, and then drying the coating, and compressing it to form a positive electrode composite layer on both sides of the positive electrode core.
[0029] The positive electrode 20 has a structure in which a positive electrode composite layer made of a positive electrode composite is disposed on the entire surface of the positive electrode core excluding the positive electrode tab 23 (hereinafter referred to as the "base"). The thickness of the positive electrode core is, for example, 5 μm to 20 μm, and preferably 8 μm to 15 μm. The base of the positive electrode core has a rectangular shape when viewed from the front, and the positive electrode tab 23 protrudes from one side of the rectangle. Generally, a positive electrode core in which the base and the positive electrode tab 23 are integrally formed is obtained by processing a single sheet of metal foil.
[0030] A lithium transition metal composite oxide is used as the positive electrode active material. Metal elements contained in the lithium transition metal composite oxide include Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, W, etc. Among them, it is preferable to contain at least one of Ni, Co, and Mn. Examples of suitable composite oxides include lithium transition metal composite oxides containing Ni, Co, and Mn, and lithium transition metal composite oxides containing Ni, Co, and Al.
[0031] Examples of the conductive material contained in the positive electrode mixture layer include carbon materials such as carbon black, acetylene black, ketjen black, and graphite. Examples of the binder contained in the positive electrode mixture layer include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide resins, acrylic resins, and polyolefin resins. These resins may also be used in combination with cellulose derivatives such as carboxymethylcellulose (CMC) or its salts, and polyethylene oxide (PEO).
[0032] The negative electrode 30 has a negative electrode core and a negative electrode composite layer formed on the surface of the negative electrode core and composed of a negative electrode composite. For the negative electrode core, a foil of a metal such as copper that is stable in the potential range of the negative electrode 30, or a film with the metal disposed on the surface layer, can be used. The negative electrode composite layer contains a negative electrode active material and a binder, and is preferably provided on both sides of the negative electrode core. The negative electrode 30 can be produced, for example, by applying a negative electrode composite slurry containing a negative electrode active material and a binder to the surface of the negative electrode core, drying the coating, and then compressing it to form a negative electrode composite layer on both sides of the negative electrode core.
[0033] The negative electrode 30 has a structure in which a negative electrode composite layer is formed over the entire area of the base, which is the surface of the negative electrode core excluding the negative electrode tab 33. The thickness of the negative electrode core is, for example, 3 μm to 15 μm, and preferably 5 μm to 10 μm. As in the case of the positive electrode 20, the base of the negative electrode core has a rectangular shape when viewed from the front, and the negative electrode tab 33 protrudes from one side of the rectangle. Generally, a negative electrode core in which the base and the negative electrode tab 33 are integrally formed is obtained by processing a single sheet of metal foil.
[0034] As the negative electrode active material, for example, a carbon-based active material that reversibly absorbs and releases lithium ions is used. Suitable carbon-based active materials include natural graphite such as flake graphite, lump graphite, and earthy graphite, and artificial graphite such as lump artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB). In addition, as the negative electrode active material, a Si-based active material composed of at least one of Si and a Si-containing compound may be used, or a carbon-based active material and a Si-based active material may be used in combination.
[0035] The binder contained in the negative electrode mixture layer may be, as in the case of the positive electrode 20, a fluororesin, PAN, polyimide, acrylic resin, polyolefin, or the like, but is preferably styrene-butadiene rubber (SBR). The negative electrode mixture layer preferably further contains CMC or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), or the like. Among these, it is preferable to use SBR in combination with CMC or a salt thereof, or PAA or a salt thereof.
[0036] FIG. 4 is a schematic diagram showing a cross section taken along line AA in FIG. 2. Hereinafter, the configurations of the positive electrode tab group 24 and the negative electrode tab group 34 of the electrode assembly 11 will be described in detail with reference to FIGS. 2 and 4. As shown in FIGS. 2 and 4, the electrode assembly 11 has a positive electrode tab group 24 formed by stacking a plurality of positive electrode tabs 23, and a negative electrode tab group 34 formed by stacking a plurality of negative electrode tabs 33. The positive electrode tab group 24 is formed by stacking a plurality of positive electrode tabs 23 in the electrode stacking direction, one for each of the electrode groups 11A and 11B. Similarly, the negative electrode tab group 34 is formed by stacking a plurality of negative electrode tabs 33 in the electrode stacking direction, one for each of the electrode groups 11A and 11B.
[0037] The positive electrode tab group 24 is joined by welding or the like to a positive electrode current collector 25 attached to the inner surface (lower surface) of the sealing plate 15. As described above, the positive electrode current collector 25 is a plate-shaped conductive member electrically connected to the positive electrode terminal 12 via the current interrupter 18. An insulating member 26 is interposed between the sealing plate 15 and the positive electrode current collector 25 to prevent contact between the two members. Similarly, the negative electrode tab group 34 is joined by welding or the like to a negative electrode current collector 35 attached to the inner surface of the sealing plate 15 via an insulating member.
[0038] The positive electrode tab group 24 and the negative electrode tab group 34 are not particularly limited in shape as long as they function as conductive paths connecting the electrode body 11 and each terminal. In the example shown in FIG. 2 and FIG. 4, the positive electrode tabs 23 and the negative electrode tabs 33 of the electrode group 11A are stacked in a state of being curved from the outside to the inside of the secondary battery 10, respectively, to form the positive electrode tab group 24 and the negative electrode tab group 34 having a generally U-shaped cross section. Similarly, the electrode group 11B also has a tab group having a generally U-shaped cross section. Each tab group may have a U-shaped cross section curved from the inside to the outside of the secondary battery 10. And, as shown in FIG. 4, the tab groups of the two stacked electrode groups may be arranged such that the cross-sectional shape of the tab group of one electrode group is generally symmetrical to the cross-sectional shape of the tab group of the other electrode group at the boundary line of the electrode groups.
[0039] The positive electrode tab group 24 may be welded to the upper surface of the positive electrode current collector plate 25 facing the sealing plate 15 side, but is preferably welded to the lower surface of the positive electrode current collector plate 25. In this embodiment, both the positive electrode tab group 24 and the negative electrode tab group 34 are welded to the lower surface of the current collector plate, but for example, the positive electrode tab group 24 may be welded to the lower surface of the positive electrode current collector plate 25, and the negative electrode tab group 34 may be welded to the upper surface of the negative electrode current collector plate 35. Also, in this embodiment, a case has been described in which the electrode body 11 includes a divided first electrode group 11A and a second electrode group 11B, but the electrode body may have a single undivided electrode group.
[0040] After the electrode body 11 is welded to the sealing plate 15, for example, the sealing plate 15 is fitted into the opening of the exterior can 14, and the fitting portion between the sealing plate 15 to which the electrode body 11 is attached and the exterior can 14 is laser welded. Thereafter, the nonaqueous electrolyte is injected into the exterior can 14 using the injection part 16, and then the injection part 16 is sealed with a blind rivet to form the secondary battery 10.
[0041] Next, the structure of the first electrode group 11A and the separator 40 will be described in more detail. The second electrode group 11B has the same structure as the first electrode group 11A, and therefore the description of the structure will be omitted. FIG. 5 is an enlarged schematic cross-sectional view of a part of the outer side in the stacking direction of the first electrode group 11A (hereinafter, simply referred to as the electrode group 11A) cut by a plane substantially perpendicular to the height direction, and includes a part of the separator 40, a part of the positive electrode 20, and an adhesive part 50a (a part where the adhesive exerts adhesive force) that is bonded by the adhesive 50 described below. Paradoxically, FIG. 5 is an enlarged schematic cross-sectional view in which the part of the adhesive 50 that does not contribute to adhesion is omitted.
[0042] 5, the separator 40 has a resin substrate (e.g., a polyolefin substrate) 40a and a heat-resistant layer 40b provided on one side surface in the thickness direction of the substrate 40a by a conventional method such as coating. The heat-resistant layer 40b may be provided on both one side surface and the other side surface in the thickness direction of the substrate 40a, or the separator 40 may not have a heat-resistant layer at all.
[0043] The electrode group 11A further includes an adhesive 50. For example, in the example shown in FIG. 5, the adhesive 50 is applied by disposing a plurality of dots of adhesive (dot-shaped portions) by printing or the like on the entire area of one side surface of the separator 40 on which the heat-resistant layer 40b is not provided and on the entire area of the other side surface of the separator 40 on which the heat-resistant layer 40b is provided, so that the area density is approximately constant. Here, the amount of each dot of adhesive 50 is approximately the same in the plurality of dots of adhesive 50. Also, the number density of the dots of adhesive 50 is approximately constant over the entire area of one side surface of the separator 40 and the entire area of the other side surface. The adhesive 50 may be applied not in dots but over the entire surface of the separator. That is, the adhesive may be applied to at least one of the one side surface and the other side surface of the separator so that the area density is approximately constant, and an adhesive layer may be provided on at least one side surface of the separator.
[0044] To explain the separator 40 and the adhesive 50 in more detail, it is preferable that the adhesive 50 is located between the substrate 40a and the electrode (at least one of the positive electrode 20 and the negative electrode 30), and a heat-resistant layer (slurry coating layer) 40b containing alumina particles as a main component may be provided on the substrate 40a, and the adhesive 50 may be applied thereon. By providing the heat-resistant layer 40b, the separator 40 is less likely to break due to, for example, foreign matter or nail penetration, and the like, and the shrinkage of the separator 40 when the temperature rises can be suppressed.
[0045] The resin porous substrate 40a functions as the separator 40 by itself. A porous film having ion permeability and insulating properties is used for the substrate 40a. The thickness of the substrate 40a is, for example, 1 μm to 20 μm. Examples of the material of the substrate 40a include olefin resins such as polyethylene, polypropylene, ethylene-propylene copolymers, and copolymers with ethylene, propylene, and other α-olefins. The melting point of the resin substrate is generally 200° C. or lower.
[0046] The porous film constituting the substrate 40a has many pores for allowing lithium ions to pass therethrough, but the surface irregularities are smaller than those of the heat-resistant layer 40b, and the surface is flatter than that of the heat-resistant layer 40b. The size (maximum length) of the pores or recesses present on the surface of the substrate 40a is, for example, less than 0.5 μm, and preferably less than 0.3 μm.
[0047] The porous heat-resistant layer 40b may be made of a resin having a higher melting point or softening point than the resin constituting the base material 40a, such as aramid resin, polyimide, polyamideimide, etc., but is preferably made mainly of an inorganic compound. The heat-resistant layer 40b is preferably made of insulating inorganic compound particles and a binder that binds the particles to each other and to the base material 40a. The heat-resistant layer 40b has ion permeability and insulating properties, similar to the base material 40a. The thickness of the heat-resistant layer 40b is, for example, 1 μm to 10 μm, and preferably 1 μm to 6 μm.
[0048] The inorganic compound particles that are the main component of the heat-resistant layer 40b may be at least one selected from the group consisting of alumina, boehmite, silica, titania, and zirconia. Among these, it is preferable to use alumina or boehmite. The content of the inorganic compound particles is determined by the ratio of the amount of the inorganic compound particles in the heat-resistant layer 40b to the amount of the inorganic compound particles in the heat-resistant layer 40b. 0b The content is preferably 85% by mass to 99.9% by mass, and more preferably 90% by mass to 99.5% by mass, based on the mass of the component (I).
[0049] The shape of the inorganic compound particles is not particularly limited, and for example, spherical, square columnar, and other particles can be used. The average particle size of the spherical particles or the average length of one side of the square columnar particles is preferably 0.1 μm to 1.5 μm, and more preferably 0.5 μm to 1.2 μm. If the particle size of the inorganic compound particles is within this range, a heat-resistant layer 40b having good ion permeability and excellent durability can be formed.
[0050] The binder constituting the heat-resistant layer 40b may be the same as the binder contained in the positive electrode composite layer and the negative electrode composite layer, such as fluororesin such as PVdF, SBR, etc. The content of the binder is preferably 0.1% by mass to 15% by mass, more preferably 0.5% by mass to 10% by mass, based on the mass of the heat-resistant layer 40b. The heat-resistant layer 40b is formed, for example, by applying a slurry containing inorganic compound particles and a binder to one side of the porous film constituting the substrate 40a and drying the coating. By forming the heat-resistant layer 40b on the substrate 40a as described above, grooves and recesses are formed between adjacent inorganic compound particles on the surface of the heat-resistant layer 40b.
[0051] The adhesive 50 may be, for example, an acrylic resin adhesive, a urethane resin adhesive, an ethylene-vinyl acetate resin adhesive, or an epoxy resin adhesive. Examples of the resin constituting the adhesive 50 include acrylic polymers, diene polymers, polyurethanes, and fluororesins such as PVdF. As described above, the adhesive 50 may be in the form of a particulate polymer or a layer. The adhesive 50 may be applied to one or both sides of the separator 40, but it is preferable that the adhesive 50 be applied to both sides, since this increases the ease of handling of the electrode group 11A (electrode body 11) and suppresses misalignment of the laminate.
[0052] 5, for example, the substrate 40a may be made of a polyethylene porous film, a heat-resistant layer 40b may be formed on one side of the substrate 40a, and adhesive particles made of an acrylic polymer may be arranged in a dot pattern on both the substrate 40a constituting one side of the separator 40 and the heat-resistant layer 40b constituting the other side of the separator 40. The heat-resistant layer 40b may be bonded to the positive electrode composite layer by adhesive particles, and the substrate 40a may be bonded to the negative electrode composite layer by adhesive particles. The bonding of each composite layer to the separator 40 is performed, for example, by a heat pressing process in which a press plate heated to a predetermined temperature is brought into contact with one side and the other side of the laminate in the stacking direction to apply pressure.
[0053] Alternatively, the laminated electrode group 11A may have an adhesive layer formed between the separator 40 and each of the electrodes 20, 30 and made of adhesive particles. The thickness of the adhesive layer is, for example, 0.1 μm to 1 μm or 0.2 μm to 0.9 μm, and is determined by the amount of adhesive and, when the adhesive is particulate, the particle size, etc. The adhesive layer is formed, for example, by applying a slurry containing adhesive particles to the surface of the separator and drying it. The adhesive particle slurry can be a so-called emulsion in which minute adhesive particles are dispersed in water. In this case, a separator with an adhesive layer can be formed in which an adhesive layer made of adhesive particles is formed on both sides.
[0054] In this case, the average particle size of the adhesive particles is, for example, 0.1 μm to 1 μm, and preferably 0.5 μm to 0.7 μm. The average particle size of the adhesive particles is measured by observing the surface of the separator using a SEM, similar to the average particle size of the inorganic compound particles constituting the heat-resistant layer. The average particle size of the adhesive particles is, for example, equal to or smaller than the average particle size of the inorganic compound particles constituting the heat-resistant layer. For this reason, the adhesive particles may completely enter the recesses present on the surface of the heat-resistant layer. On the other hand, the average particle size of the adhesive particles is, for example, larger than the grooves or recesses present on the surface of the resin substrate. Therefore, the adhesive surface is wider than the heat-resistant layer, making it easier to obtain the minimum necessary adhesive force.
[0055] Negative electrode 30, separator 40, and positive electrode 2 There are various methods for bonding the separator 40 to the electrode 10, but a bonding method using a heat press machine can be used. Note that any method other than the heat press method may be used for bonding the separator and the electrode. In the bonding method using a heat press machine, for example, a method in which the laminate is placed on a metal plate heated to a predetermined temperature, and then the metal plate heated to a predetermined temperature is pressed against the laminate from above with a constant pressure is preferable. The temperatures of the upper and lower metal plates may be the same or different, and the temperature of the metal plate is preferably higher than the softening temperature of the adhesive and is preferably higher so that the time required for heat transfer to the center of the laminate is short, but if the temperature is too high, the thermal shrinkage of the separator becomes significant, so that the temperature is preferably 50°C or higher and 120°C or lower, and more preferably 70°C or higher and 110°C or lower.
[0056] If the pressing pressure of the laminate is too low, the adhesive will not adhere well, and if it is too high, the separator 40 itself will be easily deformed in the thickness direction, making it difficult to ensure ion permeability. The pressing pressure is preferably 0.5 MPa or more and 8 MPa or less, and more preferably 1 MPa or more and 4 MPa or less.
[0057] The shorter the time for pressing the laminate, the better in terms of speeding up the production takt time, but if it is too short, the adhesive strength in the center of the electrode group (electrode body) is likely to be insufficient. In addition, the thicker the electrodes (electrode plates) are and the more layers there are, the more difficult it becomes for heat to be transferred to the inside of the electrode group (electrode body), so it takes a long time to bring the inside of the electrode group (electrode body) to the specified temperature.
[0058] For example, the negative electrode may be an electrode plate having a total thickness of 165 μm, in which an active material mainly composed of graphite is formed on both sides of a Cu core material with the same thickness on both sides. The positive electrode may be an electrode plate having a total thickness of 137 μm, in which an active material mainly composed of lithium nickel cobalt manganese composite oxide is formed on both sides of an Al core material with the same thickness on both sides. An electrode body having 36 negative electrodes and 35 positive electrodes may be used, but is not limited thereto.
[0059] As a process after the heat pressing, for example, the electrode body 11 is inserted into a metal exterior can 14, covered with a sealing body, and then an electrolyte is poured from the sealing opening. The electrolyte starts to permeate from the end between the electrodes 20, 30, and the electrolyte permeates to the center of each electrode group 11A, 11B. The amount of electrolyte permeates is abundant on one side (upper surface) of each electrode group 11A, 11B in the stacking direction and on the other side (lower surface) of each electrode group 11A, 11B in the stacking direction because there are fewer electrode ends through which the electrolyte can flow, and the amount of electrolyte permeates is likely to be insufficient toward the center of each electrode group 11A, 11B in the stacking direction. In other words, the electrolyte permeates poorly toward the center of each electrode group 11A, 11B in the stacking direction, and it takes time for the electrolyte to permeate the entire electrode group 11A, 11B. For this reason, it is preferable for the liquid circulation to be such that the adhesive strength at the center of each of the electrode groups 11A, 11B in the stacking direction is weakened to the minimum necessary so as to increase the gap through which the electrolyte can penetrate.
[0060] For this reason, in the secondary battery 10 of the present disclosure, for each of the electrode groups 11A and 11B, the adhesive strength at the center in the stacking direction of the electrode groups 11A and 11B is 0.1 times or more, more preferably 0.3 times or more, relative to both the adhesive strength at one side surface in the stacking direction and the other side surface in the stacking direction of the electrode groups 11A and 11B. Also, for each of the electrode groups 11A and 11B, the adhesive strength at the center in the stacking direction of the electrode groups 11A and 11B is 0.9 times or less, more preferably 0.5 times or less, relative to both the adhesive strength at one side surface in the stacking direction and the other side surface in the stacking direction of the electrode groups 11A and 11B. Note that, for each of the electrode groups 11A and 11B, if the adhesive strength at the center in the stacking direction of the electrode groups 11A and 11B is less than 0.1 times the adhesive strength at least one of the adhesive strength at one side surface in the stacking direction and the other side surface in the stacking direction of the electrode groups 11A and 11B, there is a risk that the center of the electrode body in the stacking direction will peel off when the electrode body is transported after bonding. On the other hand, with respect to each electrode group 11A, 11B, if the adhesive strength at the center in the stacking direction of the electrode groups 11A, 11B is greater than 0.9 times the adhesive strength of at least one of the adhesive strengths of one side surface in the stacking direction and the other side surface in the stacking direction of the electrode groups 11A, 11B, it is necessary to thoroughly melt the adhesive at the center in the stacking direction, which requires a long time for hot pressing and reduces productivity.
[0061] More specifically, if the heat press is performed under high temperature and pressure conditions, the separator on the outer side in the stacking direction is easily crushed, so the temperature and pressure must be lower than the specified value, and as a result, it takes a long time to perform the heat press to achieve the 0.9 times. In addition, the adhesive strength after the electrolyte is injected after the heat press and sufficient liquid circulation tends to be lower than the adhesive strength before the liquid circulation, but the adhesive strength ratio is generally maintained. The amount of liquid that has permeated into the electrode active material can be determined, for example, from the mass change of the electrode before and after the electrolyte is injected.
[0062] Hereinafter, the present disclosure will be described in further detail with reference to experimental examples using a non-aqueous electrolyte secondary battery, but the present disclosure is not limited to these experimental examples.
[0063] [Positive electrode] LiNi as the positive electrode active material 1 / 3 Co1 / 3 Mn 1 / 3 A positive electrode mixture slurry was prepared by mixing 93 parts by mass of a lithium-containing transition metal oxide represented by O2, 5 parts by mass of acetylene black (AB), and 2 parts by mass of polyvinylidene fluoride (PVdF), and then adding an appropriate amount of N-methyl-2-pyrrolidone (NMP). Next, the positive electrode mixture slurry was applied to both sides of a positive electrode current collector made of aluminum foil with a thickness of 15 μm, leaving the lead part, and the coating was dried. The coating was compressed using a roller and then cut to a predetermined electrode size. The area of one side surface in the thickness direction of the positive electrode other than the tab was 138 × 75 mm 2 It was.
[0064] [Negative electrode] 96 parts by mass of graphite powder, 2 parts by mass of carboxymethyl cellulose (CMC), and 2 parts by mass of styrene-butadiene rubber (SBR) were mixed, and an appropriate amount of water was added to prepare a negative electrode composite slurry. Next, the negative electrode composite slurry was applied to both sides of a long negative electrode current collector made of copper foil with a thickness of 8 μm, leaving the lead part, and the coating was dried. The coating was compressed using a roller and then cut to a predetermined electrode size. The area of one side surface in the thickness direction of the negative electrode other than the tab was 140 × 78 mm 2 It was.
[0065] [Separator] A separator was prepared that included a porous resin substrate and a porous heat-resistant layer formed on only one side of the resin substrate. A 15 μm thick polyethylene porous film was used as the resin substrate. A layer mainly composed of quadrangular columnar boehmite particles with an average side length of 0.5 μm was used as the heat-resistant layer. Many grooves and recesses were observed on the surface of this layer that were large enough to accommodate adhesive particles with a particle size of about 0.5 μm without significant deformation.
[0066] [Electrolyte] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. LiPF6 was dissolved in the mixed solvent at a concentration of 1.2 mol / L to prepare an electrolyte solution.
[0067] [Electrode body] A plurality of dot-shaped adhesives having a constant area density were applied by printing on both sides of the separator (long body) in the thickness direction as described above. In detail, a dispersion (emulsion) of adhesive particles mainly composed of acrylic polymer was applied to both sides of the separator (long body) prepared as described above, and dried to prepare an adhesive-attached separator. Then, a separator was placed on the bottom layer, a negative electrode plate with an electrode tab on which no active material was applied was placed on top, and the top was covered with a folded separator, and a positive electrode plate with a tab was placed on top of that, and the top was covered with a folded separator, and the negative and positive electrode plates were laminated while folding the separator nine times. After placing the 36th negative electrode plate, a separator was placed on top of it, and at the same time, the entire laminate was wrapped around the separator one and a half times, and the separator end was taped. Then, the laminate was placed on a press plate that had been heated in advance, and pressure was applied to the laminate by the upper press plate that had been heated in the same way. Five seconds after the laminate was placed on the lower press plate, the upper press plate was lowered to apply pressure to the laminate. After the application of pressure was completed, the laminate was transported from the press machine.
[0068] [Preparation of secondary battery] The 70 overlapping tabs protruding from all the positive electrodes in the electrode body are used as the positive electrodes of the sealing body. Current collector plate The 72 overlapping tabs protruding from all the negative electrodes in the electrode body are welded to the negative electrodes of the sealing body. Current collector plate The exterior can was a rectangular can made mainly of aluminum with a height of 95 mm, a horizontal length of 148 mm, a depth length of 29 mm, and a thickness of 1.5 mm. A secondary battery was formed by injecting a nonaqueous electrolyte into the exterior can using the injection part 16, and then sealing the injection part with a blind rivet.
[0069] [Evaluation Summary] Several electrode bodies were produced by changing the temperature of the hot plate used in the pressing process and the duration of pressing. The adhesive strength ratio was calculated for each electrode body, and the permeability of the electrolyte into the electrode plate and productivity were evaluated in relation to the adhesive strength ratio. The calculation of the adhesive strength ratio and the two evaluations were performed as follows.
[0070] <Calculation of adhesive strength ratio> The adhesive strength ratio was evaluated by measuring the adhesive strength between the outermost positive electrode and the separator, and the adhesive strength between the negative electrode and the separator, and measuring the adhesive strength between the electrode plate and the separator that showed the higher value, and setting the value as A0. The adhesive strength of the 9th plate (counting only the same electrode from the upper and lower negative electrode plates or the upper and lower positive electrode plates) of the electrode body, and the adhesive strength of the 18th plate (the center layer of the electrode body) (counting only the same electrode from the upper and lower negative electrode plates or the upper and lower positive electrode plates) were measured, and the ratios A9 / A0 and A18 / A0 were obtained when the adhesive strengths were set as A9 and A18, respectively. (Hereinafter referred to as Ai / A0). In this embodiment, in all examples and comparative examples, the adhesive strength between the porous film and the negative electrode mixture layer was high, and the value of Ai / A0 was used as the adhesive strength between the porous film and the negative electrode mixture layer. In addition, since the adhesive strength between the upper and lower electrode plates did not change, the adhesive strength of the lower electrode plate was set as A0. The adhesive strength was evaluated both before and after the electrolyte was added to the electrode body.
[0071] The adhesive strength between the separator and each electrode was measured as follows. That is, for each test sample (each test cell), the adhesive strength of the bonded surface (interface X) between the separator substrate and the negative electrode, and the bonded surface (interface Y) between the separator heat-resistant layer and the positive electrode were measured using a small tabletop tester (FGS-TV, manufactured by Nidec-Shimpo Corporation) equipped with a digital force gauge (FGP-0.5, manufactured by the same company). The test cell before electrolyte injection was disassembled leaving the bonded surface to measure the adhesive strength, and the disassembled test piece was cut into a strip with a width of 20 mm. Next, the surface of the strip-shaped test piece opposite the bonded surface to be measured was attached to a flat plate using double-sided tape. The flat plate was placed on a jig that restricted it to move in the plate surface direction without resistance and not in the vertical direction. Next, the end of the separator of the test piece was pinched with a clip attached to the tip of the digital force gauge and pulled up in the direction of 90° to the electrode surface, and the force applied to the digital force gauge at this time was measured. When the digital force gauge reading is 0.2 N, the adhesive strength of the joint surface to be measured is 0.2 x 1000 / 20 = 10 N / m. The adhesive strength was measured using the electrode body before and after the electrolyte was soaked in the electrode body.
[0072] <Evaluation of electrolyte circulation (permeability) to electrodes> After the electrolyte was poured from the sealing port, the battery was stored at room temperature, and the amount of electrolyte absorbed into the electrode active material was examined when the holding time was 8 hours and 24 hours. The stack was removed from the battery stored for a certain period of time, and the group was disassembled. The topmost negative electrode, the ninth negative electrode from the topmost layer, and the 18th negative electrode were cut out, cut into 5 cm squares at the center of the negative electrode, and the mass was measured to calculate the electrolyte content. The cut-out electrodes were placed in a metal-coated bag whose mass had been measured separately, and the mass was measured to prevent the electrolyte from drying out from the time of cutting to the measurement. In addition, a negative electrode single plate cut into a 5 cm square was immersed in a tray filled with electrolyte for 3 hours or more to allow the electrolyte to fully penetrate into the active material. The amount of electrolyte absorbed into the electrode was calculated from the change in mass of the negative electrode single plate before and after the electrolyte was absorbed, and the result was 130 mg. This amount of electrolyte absorbed was used as the amount of electrolyte when the active material was sufficiently absorbed, and the electrolyte content after the battery was disassembled was evaluated. The injectability was rated as x when the liquid content was 70 mg or less, △ when it was between 70 mg and 100 mg, and ◯ when it was more than 100 mg.
[0073] <Productivity evaluation> The heat press tact was rated as ◯ if the holding time in the heat press process, i.e., the time required from placing the laminate on the press plate to the process of transporting the laminate after the heat press was completed, was less than 60 seconds, △ if it was 60 seconds or more but less than 90 seconds, and × if it was 90 seconds or more.
[0074] [Test Results] The test results are shown in Table 1 below.
[0075] [Table 1]
[0076] As shown in Table 1, according to the above test example, when the adhesive ratio is 0.1 or more and 0.9 or less, both before and after the electrolyte is contained in the electrode, an electrode body excellent in both productivity and liquid circulation (liquid permeability) can be produced. Furthermore, according to the above test example, when the adhesive ratio is 0.4 or less, both before and after the electrolyte is contained in the electrode, an electrode body excellent in both productivity and liquid circulation can be produced. In addition, according to multiple tests performed by the inventor of the present application, in which the temperature conditions of the hot plate in the pressing process, the pressure conditions applied by the hot plate, and the pressing time of the hot plate were changed, it was confirmed that when the adhesive ratio is 0.1 or more and 0.9 or less, an electrode body excellent in both productivity and liquid circulation can be produced, and when the adhesive ratio is 0.3 or more and 0.5 or less, an electrode body excellent in both productivity and liquid circulation can be produced.
[0077] [Preferred configurations and the effects derived from each configuration] As described above, the secondary battery 10 of the present disclosure includes the adhesive 50 disposed between at least one side surface in the thickness direction of the separator 40 and the negative electrode (first electrode) 30. In the secondary battery 10 of the present disclosure, when the adhesive strength between the outermost negative electrode 30 and the separator 40 is A0 [N / m] and the adhesive strength between the negative electrode 30 located at the center in the stacking direction in the stack group (laminated body) 11A and the separator 40 is A1 [N / m], A1 / A0 is equal to or greater than 0.1 and less than 0.9.
[0078] Therefore, the electrolyte can be permeated to the inside in the stacking direction in a short time. Therefore, the secondary battery 10 in which the amount of electrolyte held is easily made uniform regardless of the position in the stacking direction can be manufactured in a short time. Therefore, not only can the power generation performance of the secondary battery 10 be improved, but also the occurrence of a difference in reaction rate depending on the position in the stacking direction can be suppressed. As a result, the durability of the secondary battery 10 can be improved, and further, the productivity of the secondary battery can be improved.
[0079] In addition, the long side of the negative electrode 30 is 10 cm or more, and the area of one side surface in the thickness direction of the negative electrode 30 is 90 cm 2 It may be set to be more than this.
[0080] As described above, the greater the capacity of the secondary battery 10, the lower the liquid circulation (liquid permeability) of the electrolyte to the center in the stacking direction.
[0081] According to this configuration, the secondary battery 10 has a long side of the negative electrode 30 of 10 cm or more, and the area of one side surface in the thickness direction of the negative electrode 30 is 90 cm 2 Thus, due to the excellent liquid circulation of the electrolyte, which is one of the main effects of the technology of the present disclosure, the power generation performance and durability of the secondary battery 10 can be significantly improved compared to secondary batteries of a conventional configuration that use an adhesive.
[0082] A second adhesive may be provided between the other side surface in the thickness direction of the separator 40 and the positive electrode 20. When the adhesive strength between the outermost positive electrode 20 and the separator 40 is A2 [N / m] and the adhesive strength between the positive electrode 20 located at the center in the stacking direction in the laminate and the separator 40 is A3 [N / m], A3 / A2 may be 0.1 or more and less than 0.9.
[0083] According to this configuration, the electrolyte can easily permeate into the center portion in the stacking direction of the electrode group 11A, also between the positive electrode 20 and the separator 40. This can further improve the power generation performance, durability, and mass-producibility of the secondary battery 10.
[0084] Furthermore, the side surface of separator 40 to which the adhesive is applied may be included in a porous substrate (eg, a polyolefin substrate) that is ion-permeable and insulating.
[0085] According to this configuration, the adhesive force acting between the separator 40 and the electrode (at least one of the positive electrode and the negative electrode) can be increased, and displacement of the separator 40 with respect to the electrode can be significantly suppressed.
[0086] Furthermore, an adhesive may also be applied to the other side surface of separator 40 in the thickness direction, and the other side surface of separator 40 may be included in a porous substrate (eg, a polyolefin substrate) having ion permeability and insulating properties.
[0087] According to this configuration, the adhesive force acting between the separator 40 and the positive electrode 20 can be made large, and the adhesive force acting between the separator 40 and the negative electrode 30 can also be made large.
[0088] Furthermore, the adhesive is applied to at least one side surface in the thickness direction of separator 40 so that the area density is approximately constant, and the area density of the bonded portions with the adhesive may vary in the stacking direction.
[0089] Fig. 6 is a schematic diagram showing the relationship between the position in the stacking direction (indicated by arrow A) and the adhesive strength between the electrode and the separator in a stacked electrode assembly. As shown in Fig. 6(c), in the technology disclosed herein, in a two-dimensional graph with the position in the stacking direction on the vertical axis and the adhesive strength on the horizontal axis, the distribution of the adhesive strength between the electrode and the separator is a function f that is nearly linearly symmetric, with the adhesive strength being large at both side ends in the stacking direction and having a minimum value in the center of the stacking direction.
[0090] Here, such a function shows similar behavior to the function showing the distribution of the amount of heat (temperature distribution) given to the laminate from the hot plate in the pressing process in a two-dimensional graph with the position in the stacking direction as the vertical axis and the amount of heat given to the laminate from the hot plate in the pressing process as the horizontal axis. That is, the distribution of the amount of heat (temperature distribution) given to the laminate from the hot plate in the pressing process also becomes a function close to line symmetry, with the heat being large at both ends in the stacking direction and the minimum value in the center of the stacking direction, as shown in Figure 6(c).
[0091] According to this modification, the behavior of such heat distribution (temperature distribution) can be skillfully used to easily make the adhesive strength on the inside (center) in the stacking direction smaller than the adhesive strength on the outside in the stacking direction. That is, according to this modification, the adhesive is applied to at least one side surface in the thickness direction of the separator so that the area density is approximately constant, and the heat distribution (temperature distribution) is also used in the heat press process, which shows a tendency similar to the function shown by f in Fig. 6(c), to make the amount of melting in the adhesive on the inside in the stacking direction smaller than the amount of melting in the adhesive on the outside in the stacking direction, and to make the amount of adhesive part that exhibits adhesive strength on the adhesive on the inside in the stacking direction smaller than the amount of adhesive part that exhibits adhesive strength on the adhesive on the outside in the stacking direction.
[0092] Specifically, Fig. 7 is an enlarged schematic cross-sectional view of a part of the inside of the first electrode group 11A in the stacking direction cut by a plane substantially perpendicular to the height direction, and like Fig. 5, the illustration of the part of the adhesive 50 that does not exhibit adhesive force is omitted. Here, the area density of the applied adhesive 50 is the same on the outside and inside of the stacking direction, but as shown in Figs. 5 and 7, the amount of adhesive parts 50a, 50b that exhibit adhesive force in the adhesive 50 can be made smaller on the inside of the stacking direction than on the outside of the stacking direction by using a heat quantity distribution (temperature distribution) that shows a similar tendency to the function shown by f in Fig. 6(c). Therefore, the adhesive force on the inside (center side) of the stacking direction can be easily made smaller than the adhesive force on the outside of the stacking direction.
[0093] Conventionally, if physical conditions were set such that part of the adhesive applied to the separator would not melt, part of the adhesive would not be effective, leading to increased material costs, so performing the pressing process under such physical conditions was avoided.
[0094] However, when the adhesive 50 is applied to the separator 40 so that the areal density is approximately constant, a remarkable effect can be obtained that far surpasses the above-mentioned problem of significantly increasing mass productivity compared to a case in which an electrode body is produced using a plurality of different separators with different amounts of adhesive applied. Thus, according to this modified example, it is possible to produce an electrode body in which the adhesive strength on the inside (center side) in the stacking direction is smaller than the adhesive strength on the outside in the stacking direction with much greater ease, and furthermore, mass productivity can be significantly increased.
[0095] In addition, since the technology disclosed in the present application aims to make the adhesive strength on the inside (center) of the laminate in the stacking direction smaller than the adhesive strength on the outside in the stacking direction, the electrode body may be produced using multiple different separators with different amounts of adhesive applied.
[0096] The separator may also be folded zigzag.
[0097] According to this configuration, the handleability of the laminate (electrode group, electrode body) can be improved.
[0098] Furthermore, when manufacturing a secondary battery 10 having the laminated electrode body 11 of the present disclosure, the laminated electrode body 11 may be manufactured by welding at least a part of the adhesive 50 in a heat press process. According to this configuration, a secondary battery 10 having the laminated electrode body 11 of the present disclosure can be easily manufactured.
[0099] The above describes the case where the secondary battery includes a laminated electrode body. Next, the case where the secondary battery includes a wound electrode body will be described. FIG. 8 is a plan view of a wound prismatic secondary battery 110, and FIG. 9 is a front view of the prismatic secondary battery 110. FIG. 10(a) is a cross-sectional view taken along line AA in FIG. 8, FIG. 10(b) is a cross-sectional view taken along line BB in FIG. 10(a), and FIG. 10(c) is a cross-sectional view taken along line CC in FIG. 10(a). FIG. 11A is a plan view of a positive electrode included in the prismatic secondary battery 110, and FIG. 11B is a plan view of a negative electrode included in the prismatic secondary battery 110. FIG. 12 is a perspective view showing the end of the winding of a flattened wound electrode body included in the prismatic secondary battery 110. The materials of the members of the wound prismatic secondary battery 110 can be the same as those of the corresponding members of the laminated prismatic secondary battery 10 described above. Therefore, in the following description, the materials of each component will be briefly described or will not be described at all.
[0100] As shown in Figs. 8 to 10 and 12, a prismatic secondary battery (hereinafter simply referred to as secondary battery) 110 includes an outer can (prismatic outer can) 125 (see Figs. 8 to 10), a sealing plate 123 (see Fig. 8), and a flat wound electrode body 114 (see Figs. 9(a) and 12). The outer can 125 is made of, for example, aluminum or an aluminum alloy, and has an opening on one side in the height direction. As shown in Fig. 9, the outer can 125 has a bottom 140, a pair of first side faces 141, and a pair of second side faces 142, and the second side faces 142 are larger than the first side faces 141. As shown in Fig. 10(a), the sealing plate 123 is fitted into the opening of the outer can 125. A prismatic battery case 145 is formed by joining the fitting portion between the sealing plate 123 and the outer can 125. The materials of each component in the wound secondary battery 110 may be the same as those of the corresponding components in the stacked prismatic secondary battery 10. Therefore, in the following description of the wound secondary battery 110, the materials of each component will be described briefly or omitted.
[0101] As shown in FIG. 12, the wound electrode body 114 has a structure in which the positive electrode 111 and the negative electrode 112 are wound in a state in which they are insulated from each other via the separator 113. The outermost surface side of the wound electrode body 114 is covered with the separator 113, and the negative electrode 112 is disposed on the outer periphery side of the positive electrode 111. As shown in FIG. 11A, the positive electrode 111 is formed by applying a positive electrode mixture slurry to both sides of a strip-shaped positive electrode core 115 made of aluminum or aluminum alloy foil having a thickness of about 10 to 20 μm, drying and compressing the positive electrode core 115, and then cutting the positive electrode core 115 into a strip of a predetermined size. The positive electrode mixture slurry contains a positive electrode active material, a conductive agent, a binder, and the like. At this time, a positive electrode core exposed portion 115a in which the positive electrode mixture layer 111a is not formed on both sides along the longitudinal direction is formed at one end of the width direction. It is preferable that a positive electrode protective layer 111b is formed on at least one surface of the positive electrode core exposed portion 115a along the length direction of the positive electrode core exposed portion 115a so as to be adjacent to the positive electrode composite layer 111a, for example. The positive electrode protective layer 111b contains insulating inorganic particles and a binder. The positive electrode protective layer 111b has lower conductivity than the positive electrode composite layer 111a. By providing the positive electrode protective layer 111b, it is possible to prevent a short circuit between the negative electrode composite layer 112a and the positive electrode core 115 due to foreign matter or the like. In addition, the positive electrode protective layer 111b can contain conductive inorganic particles. It is not necessary to provide the positive electrode protective layer 111b.
[0102] On the other hand, as shown in FIG. 11B, the negative electrode 112 is prepared by applying a negative electrode composite slurry to both sides of a strip-shaped negative electrode core 116 made of copper or copper alloy foil having a thickness of about 5 to 15 μm, drying and compressing the negative electrode core 116, and then cutting the negative electrode core 112 into a strip of a predetermined size. The negative electrode composite slurry contains a negative electrode active material, a binder, and the like. At this time, the negative electrode core exposed portion 116a is formed on both sides along the longitudinal direction, where the negative electrode composite layer 112a is not formed. The positive electrode core exposed portion 115a to the negative electrode core exposed portion 116a may be formed along the ends of both sides in the width direction of the positive electrode 111 to the negative electrode 112, respectively.
[0103] As shown in Fig. 12, the positive electrode 111 and the negative electrode 112 are arranged with a shift in the width direction (the width direction of the positive electrode 111 and the negative electrode 112) of the wound electrode body 114 so that the positive electrode core exposed portion 115a and the negative electrode composite layer 112a do not overlap, and so that the negative electrode core exposed portion 116a and the positive electrode composite layer 111a do not overlap. Then, the positive electrode 111 and the negative electrode 112 are wound in an insulated state with a separator 113 sandwiched therebetween, the separator 113 having an adhesive applied to at least one side surface in the thickness direction with a substantially constant area density, to form a wound body. Then, the formed wound body is sandwiched between a pair of hot plates and formed into a flat shape, to produce a flat wound electrode body 114. The wound electrode body 114 has a positive electrode core exposed portion 115a made of a plurality of layers at one end in the direction in which the winding axis extends (corresponding to the width direction when the strip-shaped positive electrode 111, the strip-shaped negative electrode 112, and the strip-shaped separator 113 are expanded into a rectangular shape), and has a negative electrode core exposed portion 116a made of a plurality of layers at the other end. As the separator 113, a polyolefin porous film can be preferably used. The width of the separator 113 is preferably large enough to cover the positive electrode mixture layer 111a and the positive electrode protective layer 111b and is larger than the width of the negative electrode mixture layer 112a.
[0104] As will be described in detail later, the positive electrode core exposed portion 115a, which is made up of a plurality of stacked sheets, is electrically connected to a positive electrode terminal 118 via a positive electrode current collector 117 (see FIG. 10(a)), and the negative electrode core exposed portion 116a, which is made up of a plurality of stacked sheets, is electrically connected to a negative electrode terminal 120 via a negative electrode current collector 119 (see FIG. 10(a)). Although not described in detail, as shown in FIG. 10(a), a current interrupt mechanism 127 that is activated when the gas pressure inside the battery case 145 reaches or exceeds a predetermined value is preferably provided between the positive electrode current collector 117 and the positive electrode terminal 118.
[0105] As shown in FIG. 8, FIG. 9, and FIG. 10(a), the positive electrode terminal 118 and the negative electrode terminal 120 are fixed to a sealing plate 123 via insulating members 121 and 122, respectively. The sealing plate 123 has a gas exhaust valve 128 that is opened when the gas pressure in the battery case 145 becomes higher than the operating pressure of a current interrupt mechanism 127. The positive electrode collector 117, the positive electrode terminal 118, and the sealing plate 123 are each formed of aluminum or an aluminum alloy, and the negative electrode collector 119 and the negative electrode terminal 120 are each formed of copper or a copper alloy. As shown in FIG. 10(c), the flat wound electrode body 114 is inserted into an exterior can 125 with one side open, with an insulating sheet (resin sheet) 124 interposed around the periphery except the sealing plate 123 side.
[0106] As shown in Fig. 10(b) and Fig. 10(c), on the positive electrode 111 side, the multiple positive electrode core exposed parts 115a that are wound and stacked are converged at the center in the thickness direction and further divided into two, the positive electrode core exposed parts 115a are converged, and the positive electrode intermediate member 130 is disposed between them. The positive electrode intermediate member 130 is made of a resin material, and the positive electrode intermediate member 130 holds one or more, for example, two, conductive positive electrode conductive members 129. The positive electrode conductive member 129 is, for example, cylindrical, and a truncated cone-shaped protrusion that acts as a projection is formed on both ends that face the stacked positive electrode core exposed parts 115a.
[0107] On the negative electrode 112 side, the multiple negative electrode core exposed portions 116a that are wound and stacked are converged toward the center in the thickness direction and further divided into two, and the negative electrode core exposed portions 116a are converged, with the negative electrode intermediate member 132 disposed therebetween. The negative electrode intermediate member 132 is made of a resin material, and the negative electrode intermediate member 132 holds one or more, for example, two, negative electrode conductive members 131. The negative electrode conductive member 131 is, for example, cylindrical, and a truncated cone-shaped protrusion that acts as a projection is formed on both ends that face the stacked negative electrode core exposed portions 116a.
[0108] The conductive member 129 for the positive electrode and the converged positive electrode core exposed portion 115a disposed on both sides in the extension direction are joined and electrically connected, and the converged positive electrode core exposed portion 115a and the positive electrode current collector 117 disposed on the outside in the depth direction of the battery case 145 are also joined and electrically connected. Similarly, the conductive member 131 for the negative electrode and the converged negative electrode core exposed portion 116a disposed on both sides are joined and electrically connected, and the converged negative electrode core exposed portion 116a and the negative electrode current collector 119 disposed on the outside in the depth direction of the battery case 145 are also joined and electrically connected. The end of the positive electrode current collector 117 opposite to the positive electrode core exposed portion 115a side is electrically connected to the positive electrode terminal 118, and the end of the negative electrode current collector 119 opposite to the negative electrode core exposed portion 116a side is electrically connected to the negative electrode terminal 120. As a result, the positive electrode core exposed portion 115 a is electrically connected to the positive electrode terminal 118 , and the negative electrode core exposed portion 116 a is electrically connected to the negative electrode terminal 120 .
[0109] The wound electrode body 114, the positive and negative intermediate members 130, 132, and the positive and negative conductive members 129, 131 are connected to form an integral structure. The positive conductive member 129 is preferably made of aluminum or an aluminum alloy, which is the same material as the positive electrode core 115, and the negative conductive member 131 is preferably made of copper or a copper alloy, which is the same material as the negative electrode core 116. The positive conductive member 129 and the negative conductive member 131 may have the same or different shapes.
[0110] The connection between the positive electrode core exposed portion 115a and the positive electrode current collector 117, and the connection between the negative electrode core exposed portion 116a and the negative electrode current collector 119 may be performed by resistance welding, laser welding, ultrasonic welding, or the like. In addition, the positive electrode intermediate member 130 and the negative electrode intermediate member 132 do not need to be used.
[0111] As shown in FIG. 8, an electrolyte injection hole 126 is provided in the sealing plate 123. The wound electrode body 114 to which the positive electrode collector 117, the negative electrode collector 119, the sealing plate 123, and the like are attached is placed in an exterior can 125. At this time, it is preferable to insert the wound electrode body 114 into the exterior can 125 in a state in which the wound electrode body 114 is placed in an insulating sheet 124 formed into a box or bag shape. Then, the fitting portion between the sealing plate 123 and the exterior can 125 is laser welded, and then a nonaqueous electrolyte is injected through the electrolyte injection hole 126. Then, the electrolyte injection hole 126 is sealed to produce the secondary battery 110. The electrolyte injection hole 126 is sealed by, for example, blind rivets, welding, or the like.
[0112] Although the above description concerns the case where the wound electrode body 114 is arranged such that its winding axis is parallel to the bottom 140 of the outer casing 125, the wound electrode body may also be configured such that its winding axis is perpendicular to the bottom 140 of the outer casing 125.
[0113] An example of a wound type secondary battery 110 has been illustrated above, but not only the above-mentioned wound type secondary battery 110, but any wound type secondary battery 110 has an issue that the electrolyte (electrolytic solution) has difficulty penetrating into the central cavity.
[0114] That is, as shown in FIG. 6 and FIG. 13, the lamination direction A (which coincides with the pressing direction with the hot plate) in the laminated electrode body 11 and the pressing direction B with the hot plate in the wound electrode body (wound electrode body) 114 correspond to each other. Then, when the wound electrode body 114 is pressed into a flat shape in a heat pressing process to melt the adhesive, the temperature on the inner periphery side is lower than the temperature on the outer periphery side. That is, the outer side of the lamination direction of the laminated electrode body 11 corresponds to the outer periphery side of the wound electrode body 114, and the inner side (center side) of the lamination direction of the laminated electrode body 11 corresponds to the inner periphery side (hollow side) of the wound electrode body 114. Therefore, if the wound electrode body 114 having the following configuration is manufactured, the power generation performance, durability, and mass productivity of the secondary battery 110 using it can be improved, similarly to the laminated electrode body 11.
[0115] Specifically, the secondary battery 110 includes a wound body in which a strip-shaped positive electrode 111 having a positive electrode active material disposed on a positive electrode core 115 and a strip-shaped negative electrode 112 having a negative electrode active material disposed on a negative electrode core 116 and a strip-shaped separator 113 are wound five or more times via a strip-shaped separator 113. The wound body of the secondary battery 110 includes an adhesive disposed between at least one side surface in the thickness direction of the separator 113 and at least one electrode (first electrode). When the adhesive strength between the at least one electrode (first electrode) located at the outermost periphery and the separator is A0 [N / m] and the adhesive strength between the at least one electrode (first electrode) located at the innermost periphery and the separator is A1 [N / m], A1 / A0 is 0.1 or more and less than 0.9.
[0116] Therefore, the secondary battery 110 has good power generation performance, durability, and mass-producibility.
[0117] The wound body may have a flat shape, the length of the wound body in the height direction of the battery 110 may be 10 cm or more, and the length of the wound body in the lateral direction of the battery 110 may be 9 cm or more.
[0118] The larger the capacity of the secondary battery 110, the lower the circulation (permeability) of the electrolyte to the inner periphery of the wound body.
[0119] According to this configuration, the secondary battery 110 is a large-capacity battery with a wound body thickness of 10 cm or more and an outermost peripheral length of 9 cm or more. Therefore, thanks to the excellent liquid circulation of the electrolyte, which is one of the main effects of the technology disclosed herein, the power generation performance and durability of the secondary battery 110 can be significantly improved.
[0120] In addition, a second adhesive is provided between the other side surface of separator 113 in the thickness direction and the other electrode, and when the adhesive strength between the other electrode located at the outermost periphery and the separator is A2 [N / m] and the adhesive strength between the other electrode located at the innermost periphery and the separator is A3 [N / m], A3 / A2 may be greater than or equal to 0.1 and less than 0.9.
[0121] This configuration can also improve the liquid circulation (liquid permeability) between the other electrode on the inner periphery side of the wound body and separator 113. As a result, the power generation performance, durability, and mass productivity of secondary battery 110 can be further improved.
[0122] Furthermore, at least one side surface of separator 113 on which the adhesive is disposed may be included in a porous base material (eg, a polyolefin base material) that is ion permeable and insulating.
[0123] According to this configuration, the adhesive force acting between the separator 113 and at least one of the electrodes (at least one of the positive electrode and the negative electrode) can be increased, and displacement of the separator 113 with respect to the electrodes can be significantly suppressed.
[0124] Furthermore, an adhesive may also be applied to the other side surface in the thickness direction of separator 113, and the other side surface of separator 113 may be included in a porous base material (eg, a polyolefin base material) having ion permeability and insulating properties.
[0125] According to this configuration, the adhesive force acting between separator 113 and positive electrode 111 can be made large, and the adhesive force acting between separator 113 and negative electrode 112 can also be made large.
[0126] The adhesive may be applied to at least one side surface in the thickness direction of separator 113 so that the area density is approximately constant. The area density of the bonded portion of the adhesive may vary for each layer of the wound body, and more specifically, the area density of the bonded portion of the inner layer may be smaller than that of the outer layer.
[0127] According to this configuration, the productivity of secondary batteries can be significantly improved.
[0128] Furthermore, when manufacturing the secondary battery 110 having the wound electrode body 114 of the present disclosure, the wound electrode body 114 may be manufactured by welding at least a part of the adhesive in a heat press process. According to this configuration, the secondary battery 110 having the wound electrode body 114 of the present disclosure can be easily manufactured. [Explanation of symbols]
[0129] 10,110 Secondary batteries 11 Electrode body 11A,11B Electrode group 20,111 Positive electrode 115 Positive electrode core 30,112 negative electrode 116 Negative electrode core 40,113 Separator 40a base material 40b heat resistant layer 50 Adhesive 50a, 50b Adhesive portion bonded with adhesive 111a Positive electrode composite layer 112a Negative electrode composite layer 114 Wound electrode body.
Claims
1. a plurality of first electrodes each having a first electrode core and a first electrode active material disposed on the first electrode core; a plurality of second electrodes each having a second electrode core and a second electrode active material disposed on the second electrode core; one or more separators; an adhesive disposed between at least one side surface of the separator in a thickness direction and the first electrode; the first electrodes and the second electrodes are alternately stacked with the separator interposed therebetween, the laminate including the plurality of first poles and the plurality of second poles has 10 or more of the first poles, a first electrode disposed in an outermost layer and a second electrode disposed in a center of the stacking direction of the stack, the first electrode being electrically connected to the first separator;
2. a first electrode having a strip-shaped first electrode and a first electrode active material disposed on the first electrode core, and a second electrode having a strip-shaped second electrode and a second electrode active material disposed on the second electrode core, the first electrode core being wound five or more times with a strip-shaped separator interposed therebetween; the wound body has an adhesive disposed between at least one side surface of the separator in a thickness direction and the first pole, a secondary battery in which, when an adhesive strength between the first electrode located at the outermost periphery and the separator is A0 [N / m] and an adhesive strength between the first electrode located at the innermost periphery and the separator is A1 [N / m], A1 / A0 is 0.1 or more and less than 0.
9.
3. The long side of the first pole is 10 cm or more, and the area of one side surface in the thickness direction of the first pole is 90 cm 2 The secondary battery according to claim 1 .
4. a second adhesive disposed between the other side surface of the separator in the thickness direction and the second electrode; 4. The secondary battery according to claim 1, wherein when an adhesive strength between the second electrode of the outermost layer and the separator is A2 [N / m] and an adhesive strength between the second electrode located at the center in the stacking direction of the laminate and the separator is A3 [N / m], A3 / A2 is 0.1 or more and less than 0.
9.
5. The wound body has a flat shape, 3. The secondary battery according to claim 2, wherein the length of the wound body in the height direction of the secondary battery is 10 cm or more, and the length of the wound body in the lateral direction of the secondary battery is 9 cm or more.
6. a second adhesive disposed between the other side surface of the separator in the thickness direction and the second electrode; 6. The secondary battery according to claim 2, wherein when an adhesive strength between the second electrode located at the outermost periphery and the separator is A2 [N / m] and an adhesive strength between the second electrode located at the innermost periphery and the separator is A3 [N / m], A3 / A2 is 0.1 or more and less than 0.
9.
7. The secondary battery according to claim 1 , wherein the one side surface is included in a porous substrate having ion permeability and insulating properties.
8. The secondary battery according to claim 4 or 6, wherein the other side surface is included in a porous substrate having ion permeability and insulating properties.
9. the adhesive is applied to the one side surface of the separator so as to have a substantially uniform area density; 5. The secondary battery according to claim 1, 3 or 4, wherein an area density of the bonded portions of the adhesive varies in the stacking direction.
10. the adhesive is applied to the one side surface of the separator so as to have a substantially uniform area density; 7. The secondary battery according to claim 2, 5 or 6, wherein the areal density of the bonded portions of the adhesive varies for each layer of the wound body.
11. The secondary battery according to claim 1 , 3 , 4 , or 9 , wherein the separator is zigzag folded.
12. The secondary battery according to claim 1 , wherein the secondary battery is a non-aqueous electrolyte secondary battery.
13. 13. A method for manufacturing a secondary battery according to claim 1, comprising the steps of: welding at least a part of the adhesive in a heat pressing step.
14. A fuel cell comprising a plurality of the separators, The secondary battery according to claim 1 , 3 , 4 , 9 , or 11 , wherein the plurality of separators include separators having different amounts of adhesive applied thereto.
Citation Information
Patent Citations
Lithium secondary cell and manufacturing method thereof
JP2011054502A
Lamination structure battery
JP2014026943A
Secondary battery
JP2014120456A
Lithium ion secondary battery