Reconditioning of magnets to form ND-FE-B magnets with improved or restored magnetic performance
By demagnetizing, fragmenting, and mixing waste Nd-Fe-B magnets with rare earth additives, the method effectively recycles these magnets, achieving magnetic performance equivalent to or better than the original, while minimizing resource consumption.
Patent Information
- Application Number
- JP2022003692
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2013-12-30
- Filing Date
- 2022-01-13
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2034-06-17
Smart Images

Figure 0007588104000014 
Figure 0007588104000015 
Figure 0007588104000016
Abstract
Description
[Technical field]
[0001] (background) The present disclosure relates to the production of sintered neodymium iron boron (Nd-Fe-B) magnets from waste magnet materials. Regarding. [Background technology]
[0002] The global market for rare earth permanent magnets (REPM) is growing along with the range of applications for REPM. High magnetic performance characteristics and applications in the fields of electronics, energy, transportation, aerospace, defense, Advancement of highly efficient applications of advanced technologies in many industries, including medical devices and information and communications technology It is used in.
[0003] Examples of applications using Nd-Fe-B permanent magnets include: starting motors, anti-lock brakes, etc. Brake system (ABS), fuel pump, fan, loudspeaker, microphone, telephone Ringers, switches, relays, hard disk drives (HDDs), stepping motors , servo motors, magnetic resonance imaging (MRI), wind turbine generators, robotics, sensors, magnetic Examples include sorters, guidance systems, satellites, and cruise missiles.
[0004] The Nd-Fe-B type sintered magnet has a very finely adjusted elemental composition, which is In addition to d, elements such as Dy, Tb, Ga, Co, Cu, Al, and other trace transition metal element additives are included. nothing. Summary of the Invention [Means for solving the problem]
[0005] (overview) In general, one innovative aspect of the subject matter described herein is to remove magnetic material from a waste magnet assembly. The magnetic material is demagnetized by cyclic heating and cooling of the magnetic material, and the adhesive attached to the magnetic material is removed. The adhesive is fragmented, the coating layer of the magnetic material is cracked, and the magnetic material is (a) (b) removing the coating layer by at least one of a mechanical treatment or a chemical treatment; the action of degaussing the magnetic material to provide a magnetic material free of impurities; and mixing the powder with (a) a rare earth material R and (b) an elemental additive A. (a) Nd or (b) Pr to produce a homogenous powder, and the element additive A may include at least one of: (a) Nd, (b) Pr, (c) Dy, (d) Co. (e) Cu, and (f) Fe. Other embodiments of this aspect may include a method for performing the actions of the method, respectively. A corresponding computer system, device, and one or more computer storage devices configured to A computer program stored in a memory device. A system of one or more computers. is software installed on the system that causes the system to perform actions during operation. by having software, firmware, hardware, or a combination thereof One or more computers that can be configured to perform a particular operation or action. The program, when executed by a data processing device, causes the device to perform an action. It can be configured to carry out a particular operation or action by including instructions. Cut.
[0006] Each of the above and other embodiments may optionally include one or more of the following features, either alone or in combination: The method may include simultaneously fragmenting and mixing. The step of fragmenting the demagnetized magnetic material includes a step of fragmenting the demagnetized magnetic material into particles having an average particle size of 1 to 4 μm. The step of fragmenting the degaussed magnetic material may include determining an average size of particles in the degaussed magnetic material. A particle fraction having a size greater than The method may include the step of obtaining a low oxygen concentration in the degaussed magnetic material. A particle fraction of particles of a lower size is removed from the degaussed magnetic material to provide a low oxygen concentration in the degaussed magnetic material. The step of obtaining the degree may include screening.
[0007] In some implementations, the method further comprises: mixing the homogenous powder with a rare earth material R or an elemental additive A. The method includes the steps of: (a) mechanically treating the magnetic material; or (b) removing the coating layer by at least one chemical treatment to obtain a product free of impurities. The method may include providing a magnetic material. The method may include providing the magnetic material to one or more magnetic assemblages. separating the waste magnet portion from the non-magnet portion contained in the magnet assembly. and recovering the waste magnet portion by extracting the waste magnet portion from the non-magnet portion. The step of fragmenting the demagnetized magnetic material to form a powder may include fragmenting the demagnetized magnetic material. The method may include pulverizing the mixture to form a powder having an average particle size of about 1 μm to about 2 mm. The method further comprises the steps of fragmenting the powder to an average particle size of about 1 to about 4 μm, and homogenizing the powder. The step of homogenizing the powder may include homogenizing the powder to an average particle size of about 1 μm to about 2 mm. and homogenizing the powder, which may have (a) rare earth material R and (b) The step of mixing with elemental additive A to produce a homogeneous powder has an average particle size of about 1 to about 4 μm. The powder is mixed with (a) rare earth material R and (b) elemental additive A to form a homogenous powder. The powder may be mixed with (a) a rare earth material R and (b) an elemental additive A to produce a homogeneous powder. The step of producing a powder having an average particle size of about 1 μm to about 2 mm includes: (a) a rare earth material R; and (b) and mixing the powder with elemental additive A to produce a homogenous powder. The steps may include homogenizing the powder, which may have an average particle size of about 1 to about 4 μm.
[0008] In some implementations, the method includes the step of fragmenting the demagnetized magnetic material to form a powder. Separately, the rare earth material R and the elemental additive A are fractionated, where the powder is ( The step of mixing a) rare earth material R and (b) elemental additive A to form a homogenous powder comprises: The powder is mixed with (a) the fragmented rare earth material R and (b) the fragmented elemental additive A to form a homogeneous mixture. The method may include producing a high quality powder.
[0009] In some implementations, the method comprises sintering and magnetizing the homogenous powder to remove the waste magnet assembly. Remanufacturing Nd-Fe-B magnet products with remanufactured magnets that have at least the same remanence and coercivity as the original discarded magnet parts. The homogenous powder may be sintered and magnetized to form a remanufactured Nd-Fe-B magnet product. The step of forming a homogenous powder includes compressing the homogenous powder to form a green compact. sintering the green compact at about 1000°C to about 1100°C; and cooling the sintered green compact at less than 15°C. The method may further include magnetizing the regenerated Nd—Fe—B magnet in an active atmosphere to form the regenerated Nd—Fe—B magnet product. The sintered compact is heat-treated at about 490°C to about 950°C before being magnetized. The method may include exposing the powder compact to an inert magnetic field below 15°C. The atomic percentage of Co in recycled Nd-Fe-B magnet products can be 3% or less. The atomic percentage of Cu in eB magnet products can be 0.3% or less. Recycled Nd-Fe-B magnets The total atomic percentage of Fe and Co in the product can be 77% or less. Recycled Nd-Fe-B magnets The total atomic percentages of Nd, Pr, and Dy in the waste magnet parts from the waste magnet assemblies were The total atomic percentage of Nd, Pr, and Dy can be 100% or more. The total atomic percentage of Dy, Pr, and Dy may be 18 at % or less. The method may include adding a lubricant to the powder before compressing the powder to form a green compact. The coercivity of raw Nd-Fe-B magnet products is higher than that of waste magnet parts from waste magnet assemblies. It can be increased by about 0 to about 20%.
[0010] In some implementations, the method includes sintering and magnetizing the homogenous powder to obtain the final remanence and final forming a regenerated Nd—Fe—B magnet product having a final remanence of about 97% of the remaining residual magnetism of the waste magnet portion from the waste magnet assembly, and The coercivity of the waste magnet portion is at least 30% higher than the other coercivity of the waste magnet portion. Sintering and magnetization to form a remanufactured Nd-Fe-B magnet product with final remanence and final coercivity. the final residual magnetization being a separate waste magnet portion from the waste magnet assembly. about 95% of the residual magnetism of the magnet, and the final coercivity is less than another coercivity of the discarded magnet portion. This method involves sintering and magnetizing a homogeneous powder to obtain the final remanence and final forming a regenerated Nd—Fe—B magnet product having a final remanence of Approximately 5% higher than the residual magnetism of the waste magnet portion from the waste magnet assembly and the final storage The magnetic strength is at least as great as another coercivity of the waste magnet portion.
[0011] In some implementations, the method comprises sintering and magnetizing a homogenous powder to produce a substantially W-type magnet. a R b A c Composition wherein W is waste magnet assemblies. The subscripts a, b, and c represent the atomic percent of the corresponding component or element. The powder is mixed with (a) rare earth material R and (b) elemental additive A to produce a homogeneous powder. The step of distributing the rare earth material R and the element additive A homogeneously in the demagnetizing magnetic material. and sintering and magnetizing the homogenous powder to form a remanufactured Nd—Fe—B magnet product. Step 1: The primary NdFe in the regenerated Nd-Fe-B magnet product 14 The concentration of the rare earth material R around the B phase and forming a regenerated Nd—Fe—B magnet product having an average increased concentration of the elemental additive A. The step of forming a remanufactured Nd—Fe—B magnet product may include dispersing the entire remanufactured Nd—Fe—B magnet product. and restoring the concentration and elemental composition of the grain boundary phase on average in the grain boundary regions where the grain boundaries are deformed. , changing steps, and improving steps. 81×a(Co)≦c(Co)≦3-99.9×a(Co), 0.3-81×a(Cu)≦c(Cu)≦0.3-99.9×a( Cu), 77-81×(a(Fe)+a(Co))≦c(Fe)≦77-99.9×(a(Fe)+a(Co)), a( Nd)+b(Nd)+c(Nd)+a(Pr)+b(Pr)+c(Pr)>0, a(Nd)+b(Nd)+c(Nd) +a(Pr)+b(Pr)+c(Pr)+a(Dy)+b(Dy)+c(Dy)≦18, a(Co)+b(Co)+c (Co)≦3, a(Cu)+b(Cu)+c(Cu)≦0.3, a(Fe)+b(Fe)+c(Fe)+a(Co)+b (Co)+c(Co)≦77, and b(Nd)+c(Nd)+b(Pr)+c(Pr)+b(Dy)+c(Dy)≧0 Recycled Nd-Fe-B magnet products are Nd[0.1-19at%×s(Nd), x]Pr[0.1-19at%×s( Pr), y]Dy[0.1-19%×s(Dy), z]Co[0, d]Cu[0, e]Fe[0, f], where [m, n] denotes the range from the minimum m to the maximum n; s(t) is the element in the starting composition. f(t) is the atomic percentage of element t in the final composition; x=18-[81, 99.9]at%×(s(Nd)+s(Pr)+s(Dy));y=18-[81, 99.9]at%×(s(Nd)+ s(Pr)+s(Dy));z=18-[81, 99.9]at%×(s(Nd)+s(Pr)+s(Dy));d=3 -[81, 99.9]at%×s(Co);e=0.3-[81, 99.9]at%×s(Cu);and f=77-[81, 99.9]at%×(s(Fe)+s(Co)).
[0012] In some implementations, the magnetic material from the waste magnet assembly is subjected to cyclic heating and The step of demagnetizing by cooling includes demagnetizing the waste magnet portion from the waste magnet assembly. shredding the adhesive that bonds the waste magnet portion, which may contain magnetic material, to a non-magnet portion; Electrolytic black epoxy, Ni, Ni-Cu, Ni-Ni, Ni-Cu-Ni, or Zn coating of the waste magnet parts The method may include the step of cracking at least one coating layer selected from the layers. The cyclic heating and cooling step includes heating the magnetic material to the Curie temperature of the rare earth material R; After the Curie temperature of the rare earth material R is reached, the magnetic material is heated at a rate of at least 100° C. / sec. The step of mixing the powders may include a step of cooling the powder in a water bath. The element additive A may include mixing with the following elements: Pr, Nd, Dy, Co, Cu, or Fe. The elemental additive A may comprise pure Nd. The elemental additive A may comprise pure Pr. This method fragments the demagnetized magnetic material. The method may include adding a lubricant to the powder before grinding.
[0013] In general, one innovative aspect of the subject matter described herein is directed to regenerated sintered Nd—Fe—B magnets. The regenerated Nd-Fe-B sintered magnet can be regenerated using W. a R b A c wherein the waste material W may include material from waste Nd-Fe-B sintered magnets, and the rare earth material R may include a small amount of (a) Nd or (b) Pr. and the element additive A may include at least one of: (a) Nd, (b) Pr, (c) Dy, (d) Co, (e (f) Cu, or (f) Fe, and the subscripts a, b, and c represent the corresponding elements. represents the atomic percentage of the component or element, and 81≦a≦99.9, 0.1≦b≦19, 3-81×a(Co)≦c(Co )≦3-99.9×a(Co), 0.3-81×a(Cu)≦c(Cu)≦0.3-99.9×a(Cu), 77-81×(a (Fe)+a(Co))≦c(Fe)≦77-99.9×(a(Fe)+a(Co)), a(Nd)+b(Nd)+c (Nd)+a(Pr)+b(Pr)+c(Pr)>0, a(Nd)+b(Nd)+c(Nd)+a(Pr)+b(Pr )+c(Pr)+a(Dy)+b(Dy)+c(Dy)≦18, a(Co)+b(Co)+c(Co)≦3, a(Cu )+b(Cu)+c(Cu)≦0.3, a(Fe)+b(Fe)+c(Fe)+a(Co)+b(Co)+c(Co) ≦77, and b(Nd)+c(Nd)+b(Pr)+c(Pr)+b(Dy)+c(Dy)≧0. Yes.
[0014] In general, one innovative aspect of the subject matter described herein is embodied in a regenerated Nd—Fe—B sintered magnet. The regenerated Nd-Fe-B sintered magnet can be a R b A c wherein the waste material W has a composition of: The rare earth material R may include material derived from waste Nd-Fe-B sintered magnets, and the rare earth material R may include at least one of (a) Nd or (b) Pr. and the element additive A may include one of: (a) Nd, (b) Pr, (c) Dy, (d) Co, (e) Cu. or (f) Fe, and the subscripts a, b, and c denote the corresponding elements or indicates the atomic percentage of the element, and Nd[0.1-19at%×s(Nd), x]Pr[0.1-19at%×s(P r), y]Dy[0.1-19%×s(Dy), z]Co[0, d]Cu[0, e]Fe[0, f] where [m, n] represents the range from the minimum m to the maximum n; s(t) represents the starting composition. f(t) is the atomic percentage of element t in the final composition; x=1 8-[81, 99.9]at%×(s(Nd)+s(Pr)+s(Dy));y=18-[81, 99.9]at%×(s (Nd)+s(Pr)+s(Dy));z=18-[81, 99.9]at%×(s(Nd)+s(Pr)+s(Dy) );d=3-[81, 99.9]at%×s(Co);e=0.3-[81, 99.9]at%×s(Cu);and f=7 7 - [81, 99.9]at%×(s(Fe)+s(Co)).
[0015] Each of the above and other embodiments may optionally include one or more of the following features, either alone or in combination: The rare earth material R and the element additive A are homogeneously distributed in the recycled Nd-Fe-B sintered magnet. Thus, the concentration of the rare earth material R and the concentration of the element additive A can be adjusted to the regenerated state. Primary NdFe in green Nd-Fe-B sintered magnets 14 It rises on average in the mixture of waste material W around phase B. The first atomic percentage of the waste material W can be between about 99.9 at% and about 81 at%, and the rare earth material The second atomic percentage of the combination of R and the element additive A can be about 0.1 at % to about 19 at %. The recycled Nd-Fe-B sintered magnets can have an average grain size of less than 5 μm. The regenerated Nd-Fe-B sintered magnets have an average grain size of about 7.56 g / cm 3 ~Approx. 7.6g / cm 3 The density of the sintered body may be 0.01 to 0.01.
[0016] In some implementations, the recycled Nd-Fe-B sintered magnets may have an atomic percentage of Co of 3% or less. The Nd-Fe-B sintered magnet may have an atomic percentage of Cu of 0.3% or less. The regenerated Nd-Fe-B sintered magnet may have a The total atomic percentage of Fe and Co may be 7% or less. Regenerated Nd-Fe-B sintered magnets may have 18% or less Nd, The elemental additive A may have a total atomic percentage of Dy and Pr. The elemental additive A may include pure Nd. may contain pure Pr.
[0017] In general, one innovative aspect of the subject matter described herein is to use waste Nd—Fe—B sintered magnets. The present invention may be embodied in a system for recovering waste products from used products, the system comprising: a recess for receiving the used product and aligning the used product with the positioning mechanism; The positioning mechanism, wherein the used product includes a waste Nd—Fe—B sintered magnet. a positioning mechanism for positioning each used product as it passes through the separation station; The portion of the used product containing the Nd-Fe-B sintered magnet is substantially separated from the remainder of the used product. and a separation station for separating the used products into a transport station and a positioning mechanism for positioning each used product into a transport station. When the used product portion including the waste Nd-Fe-B sintered magnet is moved to the positioning and the transfer station receiving the transfer signal from the mechanism.
[0018] Each of the above and other embodiments may optionally include one or more of the following features, either alone or in combination: The system may include a loading station, and a loading device for loading the used product. A loading device can be provided to insert the cartridge into the positioning mechanism of the loading station. The loading device is then separated from the rest of the used product in the separation station. Then, the orientation of the used product is aligned with the positioning mechanism to dispose of the used product including the discarded Nd-Fe-B sintered magnet. The loading device may include a robot. The loading device may include a feeder. The transport station may include At least a portion of the used product containing a discarded Nd-Fe-B sintered magnet is disposed of. A reclaim bin may be provided for receiving from the placement mechanism.
[0019] In some implementations, the transfer station is a part of a used product that contains waste Nd-Fe-B sintered magnets. and a device for completing the removal of the used product from the remaining portion of the used product. The tool may include an abrasive cutter. can.
[0020] In some implementations, the transfer station is a used magnet transport station for transporting used magnets, including waste Nd—Fe—B sintered magnets. Upon completing the removal of the portion of the product from the remainder of the used product, at least one Part of the used product waste Recycle bin that receives parts of used products containing sintered Nd-Fe-B magnets The transfer station is provided with a device for transferring a part of a used product including a waste Nd-Fe-B sintered magnet. Upon completing the removal of the used portion from the remainder of the used product, at least a portion of the used The magnets are then fed to a conveyor that receives the waste Nd-Fe-B sintered magnets from the used product. The transport station is a device for transporting used products including waste Nd-Fe-B sintered magnets. Upon completing the removal of the portion from the remainder of the used product, at least a portion End-of-life product waste A chute is provided to receive parts of end-of-life products, including sintered Nd-Fe-B magnets. It is possible to do so.
[0021] In some implementations, the system includes a base that supports the positioning mechanism, and a waste Nd—Fe—B sinter. A transport station that allows the portion of the used product that contains the magnet to fall into a recycling bin. The system includes a hole in the base of the used product. A disposal station may be provided for removing remaining portions of the used product from the positioning mechanism. The waste station may include a waste bin. The positioning mechanism may include a central axis. It pivots around the center to move used products between the separation station and the transport station. The system may include a base supporting the positioning mechanism. The system supports the positioning mechanism and reduces friction between the base and the positioning mechanism. The bearing may include a bearing disposed on the base.
[0022] In some implementations, the separation station may be a plasma cutter, a water jet, a blade, or a The positioning mechanism may include a loading cutter, a band saw, and a shears. a turntable defining a plurality of recesses each for receiving one of the used products at the service station; The system may include a filtered vent to remove waste particles from the system. The system may include an inertial selection system for removing waste particles from the system. The system may include a vehicular pump to remove contaminants from the system. The system may include a part of a used product that includes a waste Nd-Fe-B sintered magnet. a portion of the used product including the waste Nd-Fe-B sintered magnets received from a transport station; A heater may be provided to heat the component to a temperature above the Curie temperature of the magnetic material. The system rapidly cools the parts of the used products containing the waste Nd-Fe-B sintered magnets to produce the waste Nd- Each sub-area of each magnetic material in the portion of the used product containing the Fe-B sintered magnet A cooler can be provided to facilitate peeling from the assembly. The cooler is made of waste Nd-Fe-B The portion of the used product containing the sintered magnet was heated to a temperature above the Curie temperature of the magnetic material. After that, the part of the used product containing the waste Nd-Fe-B sintered magnets can be rapidly cooled to 5℃. do.
[0023] In general, one innovative aspect of the subject matter described herein is a waste disposal system that includes multiple reaction vessels. The present invention may be embodied in a gas mixing device for fragmenting and mixing magnetic materials, the plurality of antiferromagnets being Each reaction vessel may include an inner liner having a plurality of openings defined therein, the inner liner Each of the inner shells receives a magnetic material and surrounds the magnetic material through the plurality of openings. a pump and valve assembly configured to facilitate circulation of gas through the plurality of reaction vessels; a plurality of reaction vessels for controlling the introduction of gas into the reaction vessels and for controlling the transfer of gas between the reaction vessels; The reaction vessel is operably coupled to a number of reaction vessels.
[0024] Each of the above and other embodiments may optionally include one or more of the following features, either alone or in combination: Each of the plurality of reaction vessels may include a plurality of reaction vessels defined by penetrating the diffusion promoting device. The diffusion facilitator may include a pump and a valve. operatively coupled to the assembly and configured to facilitate distribution of gas throughout the reaction vessel. Each of the plurality of reaction vessels may be provided with a removable lid. The pump and valve assembly includes: a vacuum pump for exhausting the reaction vessels; a gas pump for exhausting gas from one of the reaction vessels; One or more of: venting to atmosphere; pressurizing the reaction vessel; and filling one or both reaction vessels with gas. The apparatus can be operatively coupled to a plurality of reaction vessels to enable the Pump and valve assemblies to automate the mixing process and transfer of gas between reaction vessels A controller operatively coupled thereto may be included.
[0025] In some implementations, the apparatus includes a gas storage chamber, the gas storage chamber comprising a reaction vessel. configured to store gas transferred from one of the reaction vessels prior to transfer to the other of the reaction vessels. This gas can be hydrogen or a mixture of inert gas and hydrogen. One or more The reaction vessels are configured to facilitate the flow of gas into each of the reaction vessels. A circulation promoting device may be provided. The circulation promoting device may be a stirrer, a fan, or a gas supply device. Each of the plurality of reaction vessels may include a reaction vessel and a pump and a valve. There may be a separate gas supply line connected between the assembly. The apparatus can be configured to produce powder having a particle size of 1 to 10 μm from the waste magnetic material.
[0026] In general, one innovative aspect of the subject matter described herein is a method for fragmenting and mixing waste magnets. The present invention is embodied in a hydrogen mixing device for forming an optimal powder and / or hydride blend. the apparatus includes a pair of reaction chambers, and a a gas management component interconnecting the pair of reaction chambers, the gas management component The component transfers gas between the pair of reaction chambers and maintains one of the reaction chambers at a target pressure. The device is configured to apply a force.
[0027] Each of the above and other embodiments may optionally include one or more of the following features, either alone or in combination: The gas management component may include a gas supply to the pair of reaction chambers. and a pair of reaction chambers for controlling the transfer of gas between the pair of reaction chambers. A pump and valve assembly may be operably coupled to the reaction chamber. At least one may include a thermostatically controlled heater within the chamber. The apparatus includes a carriage assembly configured to be received in one of a pair of reaction chambers. and the carriage assembly may include one or more bottles containing waste magnetic material. The cart assembly may include a removable cover. The bottle may be A removable cover may be provided, which may be removed after the hydrogen mixing process. The chute is configured to function as a funnel to allow the induction of the hydride magnet particles through the chute. One or more of the bottles is equipped with a device that promotes the diffusion of gas within the bottle. The device is adapted to allow the gas to reach the waste magnetic material contained within the bottle. A cylinder may be provided with openings in the sides to allow diffusion of the gas.
[0028] The subject matter described herein, in certain embodiments, provides one or more of the following advantages: In some implementations, the regeneration process is low energy consuming and Less consumption of virgin material. In some implementations, remanufactured Nd-Fe-B magnets are used in the final product, full density. economic and / or environmental benefits without compromising the magnetic performance and achievable values of sintered Nd-Fe-B magnets In some implementations, remanufactured Nd-Fe-B magnet products are made from virgin Nd- They can have performance equal to or better than Fe-B magnets. In some implementations, remanufactured Nd-Fe-B magnet products may contain as much as 99.9% waste starting magnetic material that is used to form regenerated magnets.
[0029] The details of one or more embodiments of the subject matter described herein are set forth in the accompanying drawings and the description below. Other features, aspects, and advantages of the subject matter will become apparent from the description, the drawings, and the claims. It will be. [Brief description of the drawings]
[0030] BRIEF DESCRIPTION OF THE DRAWINGS [Figure 1A-C] 1A to 1C show an example of a separator.
[0031] [Diagram 2] FIG. 2 shows an example of a furnace for processing a magnet or magnet assembly for demagnetization and removal of the assembly from the EOL magnet.
[0032] [Figure 3A] FIG. 3A shows an example of an abrasive jet cleaning apparatus for cleaning a magnet.
[0033] [Figure 3B] FIG. 3B shows an example of a hydrogen mixing reactor that breaks down waste magnetic material into particles and mixes the particles.
[0034] [Figure 4A-EHJ] 4A-4E, 4H, and 4J show a reaction bottle that can be mounted on a dolly so that the reaction bottle can be moved in and out of the reaction chamber.
[0035] [Fig. 4F-G] 4F-4G show another example of a hydrogen mixing reactor with a pair of reaction chambers.
[0036] [Figure 4K] FIG. 4K shows an example of a storage container for magnetic particles received from a bottle.
[0037] [Diagram 5] FIG. 5 is an example of a process for recovering waste magnets and magnetic materials from products, such as manufacturing "bulk," failed / rejected / surplus batches, and / or EOL products, to achieve target properties.
[0038] [Figure 6] FIG. 6 is a graph showing an example of the property ranges of starting materials for remanufactured magnets available as bulk and / or EOL magnets.
[0039] [Figure 7] FIG. 7 compares the composition of the original waste magnetic material, shown in the left bar, with the final reclaimed magnet product formed by the process, shown in the right bar.
[0040] [Figure 8] FIG. 8 shows various shapes and coatings of sintered magnets.
[0041] [Figure 9] FIG. 9 is a block diagram of a computer system that can be used in connection with the computer-implemented methods described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0042] Like reference numbers and designations in the various drawings indicate like elements.
[0043] (Detailed Description) According to some implementations, waste magnets, e.g., bulk magnetic materials and / or end-of-life (EOL) A method for producing full-dense Nd-Fe-B sintered magnets using a d-of-life magnet is described. A magnet is a magnetic material that has not been finished as a final product, especially one that has not been coated with any coating material. An example of bulk magnet material is the loss of material during manufacturing, shavings (swarf) ), and magnetic materials that are discarded as a result of inefficiencies. Another term used in is drop. End of life (EOL) magnets are magnets that are used in the final This refers to magnets and magnet pieces that have been given a finish, especially a coating material. EOL magnet materials Examples include magnets or magnet fragments recovered from discarded products. A magnetic material that can be separated from a circuit, assembly, or other substrate and still retain its coating. Stone. The end-of-life products are products that contain EOL magnets, such as hard disk drives.
[0044] The manufacturing method is different from conventional Nd-Fe-B manufacturing in that it involves more steps in the total value chain. The number of processes can be reduced, for example, mining, enrichment, oxide production, chloride production, alloy production, etc. No strip-casting procedure is used. The products obtained from the process described in have a remanence (Br ), coercivity (iHc), or energy product (BHmax) In some implementations, the residuals are equal to or greater than the waste starting material. To manufacture products with the following properties: retaining magnetic field (Br), coercivity (iHc), and energy product (BHmax) The new Nd-Fe-B product has an improved temperature profile compared to waste starting material. The method requires low virgin material inputs and low base operating costs. The process can suppress the generation of 81-99.9% of waste magnetic materials and / or magnets and 0.1- It is possible to combine with 19% rare earth element additive and all the rare earth elements present in the waste magnets. High recovery of elements such as Nd, Dy, Pr, Fe, Co, Cu, Al, Ti, Zr, Gd, Tb, etc. The magnetic properties, such as Br, iHc, or BHmax, may be high.
[0045] The method for producing full-dense Nd-Fe-B sintered magnets includes, but is not limited to, hard disk drive. EO from the product structure(s) including disk drives, motors, generators, or speakers L magnet part(s) extraction; as well as the method for producing a new Nd-Fe-B sintered magnet product; It includes the preparation of magnets and magnetic materials by mechanical and chemical measurements and processing. Nd-Fe-B sintered magnets The method for producing the stone product involves the direct removal of the coating from the extracted EOL magnet parts. The method may include one or more mixing steps of the resulting uncoated material. At least one of the steps may be, but is not limited to, a hydrogen mixing reactor. The method may include mixing the uncoated magnetic material with an oxygen inhibiting agent. Methods are available for the preparation of new dilute solutions ranging from 0.1 to 19% of the starting material. Further details and optional features of some implementations may include the addition of Nd -Maintaining, improving and / or imparting performance characteristics of Fe-B magnets. is the grain size, orientation, density, energy product (BHmax), coercivity (iHc), and / or remanence (B r) any desired combination.
[0046] Some implementations reduce the need for fresh rare earth supplies when producing remanufactured products with desired properties. Some implementations are being implemented to address the risks of rare earth supply and the uncertainty of rare earth prices. A more sustainable magnet supplier that reduces end-user sensitivity to stability play an important role in the formation of the chain, or any combination of two or more of these In some implementations, the input costs of the required materials can be calculated using mined virgin By utilizing waste magnetic materials instead of conventional materials, materials, waste and pollution are reduced. , and resource requirements in terms of energy can be eased with concomitant benefits.
[0047] In some implementations, the method is included or incorporated into a product structure, e.g., an EOL product. This involves the recovery of parts of Nd-Fe-B magnets that have been scrapped. In the segregation, the method includes providing an accessory assembly or This may include recovery of EOL Nd-Fe-B magnets from accessory material. Processing is done on parts containing EOL Nd-Fe-B magnets to increase the concentration of magnets in the total mass. The first processing step involves the integration of the magnets and the separation of the EOL Nd-Fe-B magnet assemblies from the material. The magnet may be attached to the magnet and / or to other materials, such as the magnetic circuit or a supporting housing. Remove, fragment, or disintegrate any coatings over any material, such as adhesives. It is possible.
[0048] After the initial recovery processing, the adhesive bond between the magnet and the magnet assembly is separated. The heating and cooling steps are adapted to effect initial or complete decomposition of the coating on the magnet. In some implementations, further steps may be followed, including: The material is placed in a furnace and subjected to a cyclic heating process. To demagnetize the stone and weaken or burn off any adhesive attached to the magnet or any part of it The Curie temperature of a Nd-Fe-B sintered magnet is, for example, the point at which the magnetic flux drops to 0, for example, 600°C. For example, the first heating cycle may be at least 400° C. or higher. A heating cycle in which the material is heated to a temperature and for a time long enough to demagnetize the magnet. The second heating cycle is performed to ensure that the adhesive is weakened or destroyed. The first or second step may be carried out at a sufficiently high temperature, e.g., 650° C., and / or for a long time. Rapid cooling at the end of the heating cycle was used to remove all of the rare earth magnets from the assembly. Assists in removal and completely or partially fragments any coating layers covering the magnet The heating and cooling process may be performed on other parts or assemblies, For example, coating of EOL magnets that have already been separated from their supporting housing, magnetic circuit, or other components This may also include demagnetizing and / or fragmenting and / or peeling.
[0049] In some implementations, the magnetic flux is transferred to another component, such as an assembly, a magnetic circuit, a support, or other component. Cyclic heating, where the attached magnet is held at 650 °C for 1 hour followed by rapid cooling to 5 °C, Remove the magnet from the assembly, weaken or destroy any adhesive, and remove all This is effective in cracking the coating layer of the
[0050] The heating process can be carried out in air, argon, or other inert atmosphere. Heat may be provided by, for example, resistive heating, radio frequency heating, convection, microwave heating, gas combustion heating, or chemical heating. This can be done using any suitable technique, including immersion in a thermal bath or other convection heating. The magnets are then separated using a separation device, collected and transported on a suitable conveyor. This can be done.
[0051] A process whose primary purpose is the removal of coatings from magnets is characterized as a surface removal process. It is possible to remove the surface by mechanical surface removal techniques, e.g., by using an abrasive jet. Surface removal processes can include centrifugal drums, grinding, or immersion in a chemical bath. may include.
[0052] In some implementations of the coating removal step, 100 kg of mixed waste magnets were scrapped using 1 mm diameter steel sheets. A 15-minute abrasive jet with a 100mm shot was used to remove NiCuNi, aluminum, and black aluminium. It is sufficient to remove the protective layer on various shapes of epoxy and zinc coated magnets. This protective layer can be collected by sieving for reuse. and the extracted magnets are sent for further processing.
[0053] The atmosphere and temperature can be controlled during abrasive jet processing. In some implementations, abrasive jet processing, e.g., shot blast processing, The drying is carried out in air, argon, or other inert atmosphere, preferably at a humidity in the range of 0-35%, 5 In some cases, the mass of waste sintered Nd-Fe-B material during this process can be The decrease in was less than 1%. The duration of processing, the velocity of the granular material, e.g., shot, and / or other parameters may be selected to limit the mass loss to 1% or less. In some implementations, the parameters ensure a mass reduction of no more than 10%, and in some implementations, no more than 5%. You can choose to make it % or less.
[0054] Mechanically stripped magnets were chemically treated in 1-5% diluted HCl or HNO3. By this, all oxide layers can be further removed from the surface of the waste magnets. The options are not limited, and in some implementations, other agents may be used to remove oxides. For example, CuSO4. The mass loss during this process is 0.1-5%. Preferably, the time, temperature and concentration are maintained in the range of 10 % or less, particularly 20% or less.
[0055] During the mixing stage, the bulk magnet is mixed to achieve the desired final properties in the final product formed from the material. The mixing process can be performed by crushing, grinding, milling, or using hydrogen. In some implementations, the magnets, e.g., Nd-Fe-B or 2 :17 type magnets were processed into powder using a hydrogen mixing reactor and the powder material was added in situ. In combination with an agent to restore or improve remanence, energy product, and / or density.
[0056] In some implementations, additional magnetic material is added to the waste magnetic material to restore or improve the performance of the magnet. The additional magnetic material can be rare earth, RE, e.g., Nd, Pr, Dy, Gd, Tb, La , Ce, Yb, Ho, or Eu and transition metals such as TM, e.g., V, Cr, Mn, Fe, Co, Ni, Cu, Y For example, the regenerative magnet can be represented by the following formula (1): The formula may be satisfied by: (1)Nd[0.1~19at%×s(Nd), x]Pr[0.1~19at%×s(Pr), y]Dy[0.1~19%×s (Dy), z]Co[0, d]Cu[0, e]Fe[0, f]
[0057] [m, n] means the range from the minimum m to the maximum n, and s(t) is the number of elements t in the starting composition. where f(t) is the atomic percentage of element t in the final composition, and x=18-[81, 99.9]at%×(s(Nd)+s(Pr)+s(Dy)), y=18-[81, 99.9]at%×(s(Nd)+s (Pr)+s(Dy)), z=18-[81, 99.9]at%×(s(Nd)+s(Pr)+s(Dy)), d=3 -[81, 99.9]at%×s(Co), e=0.3-[81, 99.9]at%×s(Cu), and f=77-[81, 99.9]at%×(s(Fe)+s(Co)).
[0058] Additional requirements include one or more of the following: (a) In the range of 0.1≦p+q+r≦19at% of the final product. and T ≥ min(R,18), NdpPrqDyr, the virgin material added, , T=f(Nd)+f(Pr)+f(Dy) and R=s(Nd)+s(Pr)+s(Dy);(b)p+q+r≧X, where X is the at% of RE (Nd, Pr, Dy) removed from the original magnet; (c) T≦18%; (d ) f(Nd) + f(Pr) > 0, where f is the at% fraction of the final product; (e) f(Nd) + f(Pr )+f(Dy)≦18;(f)f(Co)≦3;(g)f(Cu)≦0.3;(h)f(Fe)+f(Co)≦77; Or (i) f(Dy) + f(Nd) + f(Pr) ≧ R.
[0059] The process of mixing is grinding, cutting, high energy ball grinding, roller grinding, sawing, grind ... These include jet milling, tumbling, vibrating, jaw crushing, and hydrogen mixing. In this study, hydrogen mixing was used to homogenize the starting materials, waste magnets and new rare earth element additives. In the hydrogen mixing process, hydrogen is mixed with the φ phase, e.g., Nd2Fe 14 B and waste magnets Hydrogen enters the rare earth-rich grain boundaries of the stone and reacts with the rare earth elements, trapping hydrogen within the crystal structure. The crystal structure expands as a result of the absorption of hydrogen and the formation of hydrides. This results in the fracturing of brittle structures. This can be beneficial for mixing and at the same time, for the disposal of waste magnets. It can also be effective in fragmenting stone and additive materials.
[0060] As used herein, the term "fragmentation" refers to mechanical, chemical, and thermal processes. solid-state processes, including any suitable process including thermal, radiation, or a combination thereof It encompasses any type of fragmentation of a material. The degree of fragmentation can range from coarse fragmentation to complete disintegration, It can be made into a fine powder.
[0061] In some implementations, the method further comprises adding 0.1 to 19 wt % of one or more rare earth element additives to the composition. or the method described herein. In another aspect, the method comprises adding about 0.1 wt.%, about 0.2 wt.% , about 0.3wt%, about 0.4wt%, about 0.5wt%, about 1wt%, about 2wt%, about 3wt%, about 4wt%, about 5wt%, About 6 wt%, about 7 wt%, or about 8 wt% of one or more rare earth element additives or one or more rare earth The addition of a combination of elemental additives to the composition or method described herein is provided. In another embodiment, the method comprises adding about 0.1-0.5 wt%, about 0.1-1 wt%, about 0.5-1 wt%, about 1-2 wt%, about 1 to 3 wt%, about 1 to 5 wt%, about 1 to 8 wt%, about 2 to 4 wt%, about 2 to 6 wt%, about 3 to 5 wt%, or about 3-8 wt% of one or more rare earth element additives or a combination of one or more rare earth element additives Addition to the compositions or methods described herein are provided.
[0062] In some implementations, the method includes adding 25 wt% Pr and 75 wt% Nd at 0.1 to 1 at% or less, preferably 1%. % rare earth element additive. Essential rare earth element additives and / or hydrides of new elements In situ production of the desired fine, impurity-free powder mixture using a hydrogen mixing reactor with the addition of The production can be effective in recovering or improving the magnetic performance from waste Nd-Fe-B type sintered magnetic materials. .1wt%~19wt%, preferably 1% additional element additives are added to improve the magnetic performance of the magnetic material. and physical properties, such as density or corrosion resistance, can be restored or improved. The discarded magnetic material was placed in a hydrogen-mixed reactor and Pr 75 Nd 25 H x (wherein x is 1 to 3 mole fraction) forming a coarse powder mixture of rare earths containing
[0063] The hydrogen mixing process is carried out under a hydrogen atmosphere at 20 to 150°C and a pressure of 1 to 60 bar (100 to 6000 kPa). The material is then heated, preferably in situ, to 550-600°C to form the mixture. The average particle size formed by the mixing step is 1 μm to If a pressure of 50 bar (5000 kPa) is used, the average particle size will be in the range of 2000 mm. The particle size present in the ferromagnetic material, for example, 2 to 8 μm, and the particles that did not react with hydrogen by oxidation The powder can be sieved to remove oxidized coarse particles ranging from 500 μm to 2000 μm. The rare earth powder can be removed.
[0064] In some implementations, the hydrogen mixing process is performed to ensure that the particles are small enough for the final magnet and A pressure high enough to allow the jet milling step to be omitted is utilized. In this example, Sieving to remove larger particles and therefore particles with higher oxygen concentrations Sieving can be advantageous because oxides constitute the hard part of the material recovered from the magnet. and is effective in preventing shrinkage to smaller particle sizes.
[0065] For further mixing and homogenization, the magnetic powder mixture is The milled material can be transferred to a roller mill during roller milling, e.g. It can be lubricated with 1% zinc stearate. After the roller grinding step, the waste magnet The powder can be sieved to further remove any remaining rare earth oxides. In the implementation of the sieving, a sieving step may be selected to remove particles larger than 500 μm. .
[0066] The lubricant used in roller milling may have a low oxygen content and / or may contain a binder. Examples of lubricants include amides, such as oleic acid amide or amides, can be other low carbon hydrogenated esters or fatty acids such as oleic acid.
[0067] The powder can be further homogenized by jet milling. The gas can be formed using air or an inert gas, such as He, Ar, or N. Jet milling is a method for homogenizing a mixture for a period of time, for example, 1 to 4 hours, to break down agglomerates into single particles of 1 to 4 μm. In some implementations, the jet milling may be performed at a rate that further breaks the particles into single particles. , can be completed in less than 24 hours.
[0068] In some implementations, compared to jet milling of Nd-Fe-B elemental additives, waste-derived Nd-Fe-B A reduction in the time for jet milling of powders by 80% can be observed. The average particle size of the waste magnets is During jet milling, the agglomerates were broken down into single particles, but The rare earth oxide powder remained coarse. By removing the rare earth oxide coarse powder, the disposal started. The amount of oxygen contained in the magnetic material can be reduced, and more preferably, the final regenerated sintered magnet This step involves homogenizing the mixture of waste magnetic powder and (RE(TM) x ) due to the new addition of elemental additives and the decomposition of isolated single grains along grain boundaries. Preferably, the reaction is carried out in an inert atmosphere without any oxygen contamination, for example using Ar gas. RE (Rare Earth) refers to any combination of Nd, Pr, Dy, Tb, Y, La, or Sm. and TM (transition element added material) is any of Co, Ni, V, Nb, Mo, Ti, Zr, Al, C It refers to a combination of U, Ga, or Fe.
[0069] After particle reduction, mixing, and sieving are complete, the powder is oriented and compressed using air or The compact can be formed in an inert atmosphere. A lubricant is added to the powder prior to compression and orientation. The powder compact can be compressed and oriented in a magnetic field. The body can be directly advanced to sintering in the range of 1050-1100 °C with a holding time of 5 hours, followed by This is followed by heat treatment at 900°C for 5 hours and at 550°C for 3 hours. The choice of sintering temperature is based on the hydrogenation / mixing step. The amount of total rare earth additive added prior to the step may depend on the amount of total rare earth additive added.
[0070] In some implementations, the present invention provides a cost-effective and scalable process for the recovery of waste magnetic materials. The method may include a mechanical, automated process for recovering the EOL magnets. The method can provide a recovery step, in which other materials of EOL waste magnets are recovered. Efficient and rapid separation from material assemblies and / or fixtures, and collection / consolidation of EOL magnets The separation aspect of the recovery process involves demagnetization and circumferential separation of the adhesive bonds. This may include periodic heating and cooling processes.
[0071] This process can be applied to EOL magnets that are capable of retaining a coating. The rings are removed by mechanical means to minimize contamination and provide a high recovery concentration of magnetic material. The high recovery concentration of the decoated magnetic material is achieved by reducing the primary CO2, CO , SO2, NO x Significantly reduced energy and material usage reduces costs This provides a greener process using the above method. will be done.
[0072] The process involves the addition of elemental additives, hydrides, or other additives in a series of mixing stages. This allows the production of recycled sintered magnets with magnetic properties equal to or better than those of the discarded starting material. The magnetic properties can be quickly restored by adding 0.1 to 19 wt. %, preferably 1wt% virgin / unused / new additives 81-99.9wt%, preferably 99wt% By using it in combination with bulk material or EOL magnets with the coating stripped The degradation or deterioration of magnetic performance relative to the starting material can be prevented.
[0073] In some implementations, the homogenization of bulk materials and / or new elemental additions to EOL magnets is facilitated. Hydrogen mixing can be advantageously used to achieve this. This jet milling is an easy process that allows for cost-effective and scalable processing. In the process, it is used for further homogenization with auxiliary materials, such as rare earth oxides or Nd / Pr. Other implementations include grinding, roller grinding, high energy ball grinding, rolling, and other mixing steps.
[0074] 1A-1C show an example of a separator 100. The separator 100 is used to separate EOL products, e.g. The separator receives the hard disks and produces a material stream having a high concentration of the desired magnetic material. The separator 100 may include a control unit 20 for controlling the operation of the separator 100. The rotating table 4 driven by the bearing 12 rotates around the center 6 of the bearing 13 supported by the base table 19. do.
[0075] In some implementations, a hard disk drive (HDD) unit 14 is mounted on a loading stage. The materials are fed into the feeder 11 and then moved by the robot positioning device 16, a feeder, a conveyor, or a human operator. The loading and loading can be done by, for example, Cutting station with plasma cutter, water jet or blade cutter This is effective for aligning the orientation of the HDD unit 14 to be cut by the plasma cutter 21. The water jet or the blade cutter is fixed to a specific point on the base 19. The gas is then pumped through a small passage shielded by inert gas delivered through a shielding gas delivery pipe 5. A pressurized gas, such as N, Ar, or O, is fed through the rotary table 4. For example, the rotary table 4 rotates around a center 6. Then, the HDD unit 14 is transferred from the loading station 11 to the cutting station 21, and the At the cutting station 21, the HDD unit is cut and the magnetic material from the HDD unit 14 is removed. A HDD corner including the HDD is formed.
[0076] In some cases, a plasma cutter is used to remove the HDD corners from the HDD unit. The HDD unit may include a nozzle 17 disposed at the 2 o'clock position for emitting plasma. The nozzle 17 receives gas from the plasma control unit via a gas line 18. can be done.
[0077] In some implementations, the separator 100 utilizes a band saw or shears at the cutting station. The shearing process can limit magnet extraction, can damage the magnets being recovered, and can D. Any combination of two or more of the above may cause the corners of the unit 14 to break. Modifications can be made to minimize clamping of the substrate which can cause irregularities.
[0078] If the cutter does not separate the material sufficiently, the bent surface, e.g. the corner reclaim bin 7, the downwardly curved surface above the hole 8 of the base 19 on the HDD unit Further force can be applied to the corner until it separates from the remainder, The corner of the HDD can then be dropped into the corner reclaim bin 7. , an abrasive cutter, or an abrasive jet cutter, e.g., a water jet Use a cutting tool or other type of cutting implement to separate the corner from the rest of the HDD unit 14. It can be separated.
[0079] For particulate management, a filtered vent 1 equipped with a filter, e.g., a HEPA filter 2, is provided. Other particle control devices, such as an inertial force separator 3, may be provided. Contaminants can be sucked in via downdraft vent 15.
[0080] The HDD unit 14 can be held by gravity in a recess 24 of the rotating table 4 shown in FIG. 1C. This is because the HDD unit 14 can be inserted into the recess 24 by engaging with the rotating base 4 in the recess 24. The recess 24 is formed so that the magnet can be accurately aligned. Modify to suit the type of assembly, e.g. motor, windmill assembly, etc. The HDD unit 14 passes through a cutting station 21, at which point it is necessary to collect it. The corners with magnets can be completely or partially isolated. The HDD unit is then dropped into the corner recycle bin 7 through the corner drop opening 8, and the remaining parts of the HDD unit are then removed. The waste falls through an opening 10 into a waste bin 9.
[0081] In some implementations, the HDD corner or other magnet assembly may be reclaimed from the corner reclaim bin 7. A chute or conveyor may be provided to transport the material to a location for further processing. In some cases, HDD corners can be collected in batches and reused for processing. It can be transported for
[0082] FIG. 2 illustrates the process of treating a magnet or magnet assembly for demagnetization to remove the assembly from the EOL magnet. For example, the corners of the HDD unit are removed by conveyor 47. The furnace 40 can be heated by a heater 43 to heat the Curie temperature of the magnetic material. The heater 43 can reach temperatures higher than 1000° C., and is a ceramic heater as shown. The heater may be electric, with a heating element 44 in a sleeve 45, or any other suitable form. Heating can be by resistance, radio frequency (RF), convection, microwave heating, gas combustion, or chemical heating. This may include immersion in a bath, other suitable heating methods, or a combination of any two or more of these. Alternatively, alternative heating methods may be used. To further inhibit the progression of oxidation of the magnets, The atmosphere around the heated HDD corners or other waste material containing magnets, e.g. inert gas A line 46 can be provided to control the
[0083] The furnace 40 may include an insulating housing 42 with an outer wall 42'. The casing 42 reduces the amount of heat escaping from the furnace 40 and / or protects objects outside the furnace 40. The internal seals 41, 41' can reduce the amount of heat that escapes from the furnace 40.
[0084] The furnace 40 is used to separate the waste magnets and magnets from the subassemblies and other non-magnetic materials. Any type of heater configured to directly heat the magnet assembly and the heater without substantially polluting the atmosphere. The heating combined with the subsequent rapid cooling can be a type of heater. This may help facilitate the initial cracking of any magnet coating on the assembly. Demagnetization is achieved by heating the material to at least the Curie temperature of the magnetic material, e.g., 320°C, without an applied magnetic field. This can be ensured by
[0085] The furnace 40 is in fluid communication with a sealed piping 46 which provides a controlled inert or air atmosphere. The heating space can be defined by an inner wall. The Curie temperature depends on the composition of the magnetic material. The temperature can be 310°C to 900°C. The temperature at or above the Curie temperature is maintained to Assembly, for example, of the magnets at the corners of the HDD unit including the magnetic circuit elements and / or supports The adhesive that secures the magnet to the other parts can be securely removed or destroyed. To further facilitate separation from the assembly, subsequent fracturing of the coating, or both. After heating, the mixture can be rapidly cooled, for example to 5° C. Heating and cooling can be performed in multiple steps. This can be done repeatedly in cycles or once.
[0086] FIG. 3A shows an example of an abrasive jet cleaning device 60 for cleaning a magnet 79. The laser jet cleaning apparatus 60 supports an inlet conveyor 63 which delivers magnets 79 into a rotating drum 64. As the drum 64 rotates, the surface of the magnet 79 is pulled from the jet nozzle 66. The blade is exposed to the abrasive jet that comes out.
[0087] Ensure that the magnets 79 and their separate parts are moved to remove any materials, such as adhesives and other magnet coatings. A belt grinding roll 75 may be provided to ensure that the ring is removed from the magnet 79. The treatment of the magnet 79 by the abrasive jet cleaning device 60 includes, but is not limited to, Ni Effective in removing coating layers including CuNi, Al, Zn, and electrolytically deposited black epoxy materials. The roller 75 moves in a direction opposite to the direction of the magnet adjacent surface of the drum 64. The roller 75 can rotate in the same direction as the drum 64 so as to rotate the surface material The material can be further removed from the magnet by using rollers 75 in conjunction with drum 64. This allows the surface of the magnet 79 to be more evenly exposed to the shot blasting process of the jet nozzle 66. can.
[0088] The dust / shot collection groove 57 receives the shot and fine particles from the coating and then Then, sieving or other size or density separation processes are performed on the shot and the particles. A process is then carried out to recover the removed coating material and remove the abrasive particles, e.g. The abrasive particles are then ejected from the nozzle 66. The mixture is transported by a conveyor 68 to a feeder / generator 69 which produces a axial jet.
[0089] Once the excess material has been separated from the magnets 79, the exit conveyor 70 directs the magnets to a jet washing device. 60. The air cleaner 65 is connected to an outlet conveyor 70 which removes the magnets from the jet cleaner. When this is done, any loose material that has become detached from the magnet 79 can be removed.
[0090] The abrasive jet cleaning device is adapted to be in a suitable environment for the jet cleaning device, e.g., processing A control cabinet shown at 71 is provided to control time, atmosphere, speed, etc. It is possible.
[0091] Coating of magnets is achieved by ablating part or all of the magnet surface. It can be completely removed by cleaning with an abrasive jet. In some implementations, the abrasive jet is made up of steel shot, tungsten carbide, The particles can be burrs, ceramic, or steel grit. The size of the particles is approximately 1 mm. The abrasive jet cleaning device 60 receives the waste magnet and The magnet waste is then subjected to oxygen contamination prior to further processing of the magnet waste. The surface coating or protective coating can be substantially removed from the magnet. The atmosphere may be a controlled inert atmosphere, for example, argon.
[0092] The magnet 79 is subjected to abrasive heating at a humidity level of about 1 to 35% relative humidity (RH) and a temperature of about 5°C to 600°C. The substrate can be treated with a sieve jet cleaning device 60.
[0093] In some implementations, the surface removal process is effective to remove less than 5% of the magnet's mass. In some embodiments, the surface treatment can be performed for a period of about 15 minutes to about 5 hours. This will be carried out over a period of time.
[0094] FIG. 3B shows an example of a hydrogen mixing reactor that breaks down waste magnetic material into particles and mixes the particles. In some implementations, the hydrogen mixing reactor mixes the elemental additive with the particles. The reactor is capable of forming particles having a target average diameter of about 1 μm to about 2 mm, or about 4 to about 7 μm. The hydrogen mixing reactor comprises two vessels 102 and 124 disposed in mixing chambers 122 and 124, respectively. and 104, each of which holds magnetic material and passes it through holes in the inner lining 110. The inner lining 110 facilitates the circulation of gas around the magnetic material. When one of the containers 102, 104 containing the material is filled with hydrogen gas, the hydrogen mixture causes magnetic Fragmentation of the material occurs. Exposure to hydrogen gas can last from about 1 to 40 hours. The exposure may be for shorter or longer periods and the pressure and temperature may vary depending on the process. the scientific requirements, other processing steps used to achieve the target particle size, the target homogeneity Any other processing step or steps used to achieve the blending, or any two or more of these Selection can be based on a combination.
[0095] A diffusion facilitator 112 with holes, such as a snorkel or tube, is used to facilitate diffusion by hydrogen mixing. This allows the magnets to dissolve within the reaction vessels 102, 104 and allows the accumulation of particulate matter to dissolve some of the magnets. The hydrogen gas may be exposed to the hydrogen gas without impeding the flow of the hydrogen gas. For example, an agitator, fan, or gas supply device may be used to regulate the flow of hydrogen gas within the vessels 102, 104. The magnetic material that falls through the holes in the inner lining 110 can be moved to the respective containers. Stirring can be achieved by means of stirrers disposed at the bottom of the vessels 102,104.
[0096] A removable lid 114 may be provided for introduction of magnets into the vessels 102, 104. For example, after the magnet 79 is cleaned in the abrasive jet cleaning device 60 shown in FIG. The magnets can be placed in containers 102, 104 as shown in FIG. After being cleaned with the laser jet cleaning device 60, the magnetic material is then subjected to a controlled environmental The material can be transferred into the inner lining 110 by conveyor or manually without the use of a conveyor. A rare earth transition element additive material is added to the inner lining 110 to maximize the surface area of the magnet formed therefrom. The end product can be characterized to a given specification of remanence, energy product, and / or retentivity. In some cases, additives can be milled after mixing to adjust the properties of the final product. Some examples of additive materials include Nd, Pr, Dy, Gd, Examples include Tb, La, Ce, Yb, Ho, and Eu.
[0097] The vessels 102, 104 can withstand a certain pressure. For example, the hydrogen mixing reactor can be vacuum In some implementations, the pressure can be up to 60 bar (6000 kPa). The containers 102, 104 can also withstand low pressure. , a thermostatically controlled heater 116 and a pressure adjustment knob.
[0098] The hydrogen mixing reactor is configured to pump hydrogen or other gases through a pump assembly 128 and a valve assembly 133. The pump assembly 128 includes a gas source connection 138 for introducing gas into the vessels 102, 104. The valve assembly 133, the gas management component 144, or a combination of two or more of these , gas is introduced directly into the diffusion facilitator 112 to disperse the entire volume of the magnetic material into the vessels 102, 104. In some examples, the pump assembly 128 and the valve assembly 133 may The vessels 102 and 104 can be connected, which allows, for example, degassing or the first introduction of gas. evacuating the vessels 102, 104 with a vacuum pump to regenerate hydrogen gas, Delivery of gas from one vessel to another, e.g., to the ambient air using peripheral connection 132. Evacuation, pressurizing the vessels 102, 104, filling one or both of the vessels 102, 104 with an inert gas, etc. The control device 140 can be configured to perform a regeneration process, A valve assembly 133 and a pump assembly 128 are connected to facilitate the hydrogen mixing process and the connection between the vessel 102 and the Hydrogen transfer between the 04 and the refrigerant tank can be automated.
[0099] During the hydrogen mixing process, magnetic particles are pumped from vessels 102, 104 through chute 126 into chamber 1. The magnetic particles can then be removed from chamber 102 for further processing. In some implementations, a pressure-tight valve can be utilized at the opening between the chute 126 and the vessels 102, 104. It can be used.
[0100] In some implementations, one of the vessels 102, 104 is made airtight and includes a gas management component. The selected vessel 102, 104 is then evacuated from the gas source, e.g., using a gas pump. Hydrogen is filled through pump assembly 138 to select for mixing and fragmentation of the waste magnetic material. The selected vessels 102, 104 can be prepared. After mixing and fragmentation, for example, hydrogen can be selected. By discharging hydrogen from a selected vessel 102, 104 and transferring the hydrogen to the other vessel 104, 102. The hydrogen can then be transferred to the other vessel 104, 102 by the gas management component 144. As the contents of each vessel receive the hydrogen mix, hydrogen can be recovered and pumped to the other vessel 102, 104. It can be transferred and the process of hydrogen mixing repeated with the other vessel.
[0101] In some implementations, a gas storage chamber is included in the gas management component 144; and Hydrogen discharged from one of the vessels 102, 104 may be pumped into the other vessel 10 during, for example, a hydrogen mixing cycle. 2, 104, the gas is temporarily stored in a gas storage chamber (not shown). The use of the chamber allows the hydrogen mixing reactor to have only one vessel. In an example, the hydrogen mixing reactor may include three or more vessels. The gas storage chamber may include , minimizing pressure drops or increases during transfer to the chambers and vessels 102, 104. selected to maximize the energy economy of gas transport to and from these There may be multiple chambers making up each stage of the volume.
[0102] FIG. 4A shows a set of four reaction bottles 212 on a cart 216, which is connected to a reaction chamber. For example, the reaction bottle may be inserted into and removed from one of the reaction chambers 202, 202' shown in FIG. 4F. The reaction chamber 202, 202' allows the transport of hydrogen mixing reaction fluid 212. In some cases, the reactor may be used in conjunction with or in place of the hydrogen mixing reactor. The reaction vessel 212 may be a hydrogen mixing reactor, such as the vessels 102 and 104 shown in FIG. 3B. For example, the gas management component 144 may be used in conjunction with a magnet that is subsequently filled with The bottle 212 in which the hydrogen is introduced can be filled with an inert gas, such as Ar or N. The magnet 206 to be deactivated is dropped into the reaction bottle 212 through a transfer chute 208. Place in an atmospheric reaction bottle 212 to prevent contamination of magnet 206 by, for example, oxygen. It is possible.
[0103] In some implementations, a small amount of rare earth transition element additive material is added to the reaction bottle 212. The rare earth transition element additive material is made of magnet 206 and rare earth transition element additive material. The final product is manufactured to have the desired characteristics of remanence, energy product, and retentivity. In some examples, the hydride of the rare earth transition element additive material can be selected to be After mixing and fragmenting the magnet, it is added to a hydrogenated magnet 206. This can be done.
[0104] Each of the reaction bottles 212 includes a snorkel 213 that facilitates the diffusion of gas within the reaction bottle. Or another device may be provided. For example, a snorkel 213 may be provided at the center of each bottle 212. A silicon carbide tube with openings on the sides that allow the gas to diffuse so that it can reach the magnets placed in it. This can be used as an underwriter.
[0105] The bottle 212 and the snorkel 213 are connected to each other so that hydrogen gas flows into the bottle 212 and the snorkel 213. 212 to allow access to the magnet 206 contained within the bottle 212 and / or The bottle 212 may be open at the top to allow loading into it.
[0106] Once the magnet 215 is placed within the bottle 212, the transport cover 214 is removed as shown in FIG. The cover can be attached to a dolly 216 to isolate the bottle 212 and its contents from the outside air. The container formed by the container 214 and the dolly 216 cannot tolerate gas leakage. The internal volume can maintain an atmosphere of inert gas, and ambient air is prevented from contacting the magnet 215. For example, after the bottle 212 is placed in the inert atmosphere, the bottle 212 is It can be covered by a bar 214 and the dolly 216 is stored outside the space with an inert atmosphere. For example, FIG. 4E illustrates the placement of filled bottles 212 on cart 216 and the removal of cover 214 from the filled bottles. An example of a filled bottle 212 is shown prior to placement on top of the bottle 212. The container may be filled while on the cart 216 or may be filled and then placed on the cart 216. stomach.
[0107] 4F and 4G show an example of another hydrogen mixing reactor having a pair of reaction chambers 202, 202′. The reaction chambers 202, 202' are connected to the gas management component 144 as described above. The gas sources 138 are connected to the gas management component 144. , connections for a number of gases, for example inert gas and hydrogen, can be provided. Ambient connections 132 allow for exhaust to atmosphere. Gas management components 144 include: Not between the vessels 102 and 104, but from one reaction chamber 202 to the other reaction chamber 202'. In terms of transferring gases through the casing and vice versa, it operates as described above with reference to FIG. 3B.
[0108] A covered cart 260, e.g., cart 216, enters the first one of the reaction chambers 202. Meanwhile, hydrogenation is occurring in the other reaction chamber 202'. Once inside the chamber 202, the cover 214 is removed from the carriage 260 to expose the reaction chamber 202. Hatch 252 is closed. Chamber 202 can then be filled with an inert gas.
[0109] The gas management component 144 pumps hydrogen from the hydrogen source to the reaction chamber to achieve the required pressure. For example, after hydrogenation in the reaction chamber 202' is completed, The gas management component 144 then directs hydrogen from the reaction chamber 202' into the reaction chamber 202. The gas management component 144 transfers the gas to the reaction chamber 202 to a target pressure. Hydrogen gas, e.g., pressurized hydrogen gas, may be pumped from the reaction chamber 202 to the cover 232 or other portion of the bottle 212. Hydrogenation is initiated in the reaction chamber 202 by introducing hydrogen into the bottle through the opening. It is possible.
[0110] The hydrogen mixing process, for example, when the hydrogen mixing reactor performs the first mixing process, is about 1 μm to about 2 mm, or, for example, about 4 mm when the hydrogen mixing reactor performs the second mixing process. In some examples, magnetic particles having an average diameter of about 7 μm to about 5 μm can be formed. The hydrogen mixing reactor shown in FIG. 3B and FIG. 4G can perform both processes. The hydrogen mixing reactor can perform both processes. One reactor can carry out one process and the other reactor can carry out the other process. For example, the hydrogen mixing reactor shown in FIG. 3B can perform the initial mixing process. The hydrogen mixing reactor shown in Figures 4F and 4G can perform the second mixing process. can.
[0111] The gas management component 144 may be configured to evacuate the chamber 202′, e.g., completely evacuate the chamber 202′. The gas is admitted into chamber 202 for use during processing therein. 4G, the chamber 40 may be placed in a storage chamber or container. A thermostatically controlled heater 257 in 202 is controlled by a controller to provide the desired temperature. This can be controlled.
[0112] As the hydrogenation process proceeds within the reaction chamber 202, the gas management component 144 The chamber 202' is filled with an inert gas. Then, as shown in FIG. 4G, the reaction chamber The hatch 252' to the bath 202' is opened and the cover 214' is hung on the carriage 260'. The stone material, now reduced to particles, is then removed from the reaction chamber 202' on a carriage 260'. can be.
[0113] Once hydrogenation is complete in the chamber 202, the gas management component 144 removes excess hydrogen gas. The chamber 202 is then evacuated. For example, a hydrogenation process can be performed using a hydrogen source disposed in the chamber 202′. One or more bottles 212 may be restarted.
[0114] In some implementations, as shown in FIGS. 4C, 4D, and 4J, the bottle 212 may be covered 232. The cover 232 can be closed, for example, when the bottle 212 is in an inverted position and the valve 23 4 is open, a leakage current is generated that allows the collected hydride magnet particles to be guided through the chute 237. The cover 232 functions as a funnel, for example, to allow the magnet 206 to enter the bottle 212. 212. The bottles 212 may then be attached to their respective bottles 212.
[0115] Referring to FIG. 4J, in the inert atmosphere, a cover 232 is placed over the bottle 212. The bottle can then be sealed and removed from the inert atmosphere without the need for a cover 214. The bottles 212 can be transported by cart 216 or can be transported individually. can.
[0116] FIG. 4K illustrates an example of a storage container 240 for magnetic particles received from a bottle 212. The valve 234 of the bottle 212 receives a nozzle 265 on the storage container 240 to form a manifold. The bottle 212 is sealed to the snorkel 213. A blower 266 blows inert gas. The magnetic particles are then fed into the snorkel 213 via the manifold 267 to The inert gas is removed and placed in a storage container 240. After entering one of the bottles 212, the inert gas is stored. It can be circulated back to chamber 240.
[0117] The inert gas is introduced into the bottle 212 and the snorkel 213 as shown in FIG. 4H, which is a cross-sectional view of the bottle 212 and the snorkel 213. The arrows indicate the direction of the snorkel 213. 1 shows the tangential pattern of inert gas exhausted through tangentially oriented slots. The tangential pattern of inert gas flow helps remove particles from the interior walls of the bottle 212. Complete evacuation of the magnetic particles from the bottle 212 can be facilitated.
[0118] The valve 234 may, for example, be a gate structure to allow the nozzle 265 to enter the bottle 212. When the bottle 212 is removed, the cover 268 is attached to the nozzle 265. 2, the storage container 240 can be sealed.
[0119] FIG. 5 shows how waste magnets and magnetic materials are sorted into products, e.g., “bulk” products, failed / rejected / excess bulk products, etc. FIG. 5 is an example of a process 500 for recovering from a retrieval and / or EOL product to achieve targeted characteristics. The process 500 can be performed using one or more of the systems described above.
[0120] At S10, the conveyor orients the product relative to the cutter and passes the product through the cutter. The magnet-containing or cut portion of the product is separated from the remainder of the product. The magnet-containing part is collected together with other magnet-containing parts "recovered" from the same or similar equipment. The products are then combined into one batch.
[0121] In S20, the magnet-containing parts or cut parts are first subjected to separation, demagnetization, and coating. In the first crushing step, the magnet-containing portion is heated, and in the second crushing step, the magnet-containing portion is heated. The magnets are then cooled and attached to their respective substrates, e.g., magnetic circuits or parts of an assembly. Any adhesive on the magnet-containing part that is used to attach the magnet is separated from the magnetic material. This process allows for the recovery of substantially the entire magnet from a magnet-containing part or assembly. Moreover, the recovered magnets do not need to be destroyed.
[0122] In some implementations, heating and cooling is sometimes used for coatings, e.g., Nd-Fe-B magnets. The nickel-copper-nickel coating may be effective in disrupting or partially spalling the nickel-copper-nickel coating. Some coatings, e.g. phosphates, lacquers, or polymers, are completely removed during heating. can be destroyed.
[0123] The heating and cooling cycle may be repeated multiple times or may be performed just once. The method involves heating the magnet-containing portion to a temperature of about 600° C. and then subjecting the magnet-containing portion to a temperature of about 5° C. Other target temperatures may be used. The heating temperature is determined by the temperature of the magnet-containing portion. The Curie temperature of the magnetic material to be used, e.g., the Curie temperature of the magnetic material at which the magnetization of the magnet disappears. A temperature higher than the Lee temperature can be used.
[0124] The magnet-containing portions of a single batch that the system heats simultaneously have different Curie temperatures. The magnets may be of multiple formulations. The selected heating temperature may be any of a variety of The highest Curie temperature of all magnet formulations to ensure that the magnetization of the magnetic material is erased The degree of the stenosis may be equal to or greater than the above.
[0125] In some implementations, both the heating and cooling are rapid. The temperature is maintained above the Curie temperature for a predetermined minimum time to demagnetize. The magnet-containing portion is heated to a temperature above the Curie temperature and maintained at that temperature for a predetermined minimum time. The magnet-containing portion is then rapidly cooled. It can be heated and held at a lower temperature for a shorter period of time and then rapidly cooled again If demagnetization occurs during the first heating and cooling cycle, subsequent cycles should be performed at the same temperature or holding temperature. Although it is not necessary to reach this time, this heating and cooling cycle may be used to remove the magnetic material from the adhesive. This may be advantageous for removing and / or fracturing the coating. In some implementations, the system The magnet-containing portion is heated at a rate of 10° C. / sec or more, preferably 50 to 100° C. / sec. The method involves rapidly heating the magnet-containing portion at a rate of, for example, 100° C. / sec, preferably about 200 to 1000° C. / sec. The mixture can be cooled to 30°C.
[0126] The process 500 is carried out in a furnace for about an hour to completely remove the non-magnetic material from the magnetic material. This can be done for a batch of about 50 to about 1000 kg of magnet-containing parts. The larger the mass of the batch, the longer it will take to hold in the furnace, e.g., due to convection. The hold time in the furnace can be the total time of all heating and cooling cycles, e.g. The furnace both heats and cools the magnet-containing part.
[0127] An inert atmosphere may be utilized in the furnace or heating may be performed in air. In the present application, the processing of the magnetic material is such that any coating is disrupted or removed from the magnetic material. Once removed, an inert atmosphere can be utilized to protect the magnetic material from excessive oxidation. do.
[0128] At S30, all coatings are removed from the magnetic material. The coatings can be removed by mechanical methods, chemical methods, or the like. In some cases, the coating may be removed by chemical and / or other methods. The coating is removed by shot blasting or abrasive jets. This can be done after shot blasting or abrasive jet treatment of, for example, oxide Dilute hydrochloric acid, nitric acid, or other agents effective in removing chemistry may be used. The bath is capable of removing oxides from the surface of the magnetic material.
[0129] At S40, the magnetic material is placed in a mixer after mechanical and chemical processing. The device is designed to expose the magnetic material to a pressurized hydrogen atmosphere for a given period of time, temperature, rotation speed, etc. For example, the magnetic material can be used in the hydrogen mixing reactor shown in FIG. 3B, the hydrogen mixing reactor shown in FIG. or both hydrogen mixing reactors, or another suitable mixing device. It can be processed.
[0130] In some instances, a rare earth transition element additive material may be added to the magnetic material before or after mixing. In some implementations, Nd-Fe-B magnets, e.g., waste magnets and rare earth transition element additives, Materials such as Nd 1-x Pr xare put together in a mixer in a ratio of 99.9:0.1 to 81:19, After S40, the rare earth transition element additive material is shredded separately and discarded. It can be added to the magnetic material.
[0131] The rare earth transition element additive material was used to analyze the composition of the waste magnetic material, as well as in the experiment. Therefore, extrapolation or other techniques may be used to achieve a given target formulation and magnetic performance. A database of restoration formulas determined by any suitable method. For example, the database can be used to select the sintered regenerated magnets that can be obtained. rare earth transition element additive materials that are added to the starting materials to achieve desired properties of the product; and It may include historical data indicating compositional characteristics of the waste magnet material.
[0132] The magnetic and physical properties of the starting magnetic material can be determined by mixing, e.g., subsequent processing to produce a new sintered recrystallized material. During or after the reduction of the starting magnetic material by mixing with hydride powder or crushed powder to be made into raw magnets to be restored or improved by the addition of specific rare earth transition element additive materials in predetermined proportions. An example of this formulation is 99 parts of scrap Nd-Fe-B magnets and a mixture of 25 wt% Pr and 75 wt% Nd. In the case of 2:17 type magnets, it is Sm2Co 17 , including some Sm. An example is 99 parts waste Nd-Fe-B magnets and 1 part Nd, Dy, Co, Cu, and Fe elemental additives. In some implementations, this combination is combined with a small amount of rare earth transition element additive or element. Most of the rare earth magnets are scrapped. In some implementations, rare earth transition element doped magnets are used. The additive is a combination of Nd and a lanthanide with another transition metal. In some implementations, the elemental additive The lanthanides are in less than 2% of combination with the starting magnetic material. can be replaced with
[0133] At S50, the powder is fragmented and homogenously mixed by suitable means. This is accomplished by jet milling to a target particle size of about 1 to about 4 μm. The fragmentation may be performed using any suitable fragmentation device, such as the fragmentation devices described in detail above. In some implementations, step S40 may include filtering, homogenizing, or both. and S50 can be carried out simultaneously. In some implementations, only a small amount of Rather than adding rare earth transition element additive materials, in S50, the rare earth materials are hydrogenated separately. In some cases, rare earth transition element additives are added after S50, for example, at the start of the disposal. It can be separately ground and added after the grinding of the magnetic material, during which the starting waste magnetic material is For example, high pressure of 60 bar (6000 kPa) is used to form powders in the range of about 1 to about 50 μm. Preferably, the mixture is sufficiently divided into
[0134] At S60, larger particles, for example about 1 mm, are sieved out of the fragmented material. The unoxidized portion is used to sift out larger particles, e.g., particles of about 500 μm to about 2 mm, from the fine powder. This procedure prevents the oxidized particles from fragmenting into debris. Due to the hardness of the oxides on the bulk of the recovered rare earth magnet material, it is necessary to remove the oxides. For example, hydrogenation, milling, jet milling, crushing, or another suitable method may be used to obtain the desired product. However, it is possible that the oxides tend not to decompose in a way that results in a large size distribution, and their proportion in the fine powder is It is possible to eliminate or reduce the inclusions by screening.
[0135] In S70, the powder is compressed by filling the press and generating a magnetic field in the press. The powder is then sintered and heat treated to form a green compact at S80. A green sintered magnet product is formed.
[0136] FIG. 6 shows the properties of starting materials for remanufactured magnets available as bulk magnets and / or EOL magnets. 5 is a graph showing an example of a range. The oval 302 depicted in the graph represents the range of the process 500 applied. The process 500 represents the approximate range of starting materials that can be used. It can also be applied to other starting materials.
[0137] FIG. 7 shows the composition of the original waste magnetic material shown in the left bar compared to the composition of the waste magnetic material formed by process 500. The starting magnetic material is shown in the right bar, which is a comparison of the final regenerated magnet product, which is shown in the right bar. The rare earth metal content indicated by the "R" region of the left bar is higher than 18 at% but lower. An amount "X" of rare earth metal is removed from the starting magnetic material during processing. In order to ensure that the remanufactured Nd-Fe-B product has a composition similar to that of the original magnet, new rare earths are added. Material, i.e. virgin material, must be added.
[0138] In FIG. 7, unused material is represented by the "V" area and is removed during processing. The amount of rare earth metal or metals approximately equal to "X". In the final recycled product, the final percentage of rare earth metals is The percentage of the starting magnetic material is at least 18 at %. The percentage of earth material "R" is lower as the dashed line below the two dashed lines on the left, for example, less than 18 at%. If the final rare earth atomic percentage in the final recycled magnet product shown in the right bar is less than At least equal to that percentage, as shown by the extended lower dashed line. However, even if the percentage of rare earth metal in the starting magnetic material is higher than 18 at%, the final regenerated magnetic material The atomic percentage in the stone is shown by the upper dashed line at 18% in the right bar. , limited to 18%.
[0139] In the final recycled product, the final rare earth atomic percentage is determined by the respective components of the virgin material: Nd, Pr, Dy, Gd, The percentage of Tb, La, Ce, Yb, Ho, and / or Eu is in the range of 0.1 to 19% of the percentage in the original magnet. The atomic percentage of Nd is in the range of 0 to 100, and the total atomic percentage of Nd and Pr is greater than 0.
[0140] Besides the rare earth metals, the remainder of both the starting magnetic material and the final regenerated magnet consists of Fe, Co, Cu. , aluminum, and other elements. In the final recycled product, the following constraints exist: (1) the atomic percentage of Co is 3% or less; (2) the atomic percentage of Cu is 0.3% or less; and (3) The total atomic percentage of Fe and Co is 77% or less.
[0141] FIG. 8 shows various shapes and coatings of sintered magnets 800. Each sintered magnet 800 has , which can be used during the regeneration process 500. Examples of coatings for the sintered magnet 800 include: Phosphate 802, Al 804, NiCuNi 806, Epoxy 808, and Zn 810. For example, FIG. The abrasive jet cleaning apparatus 60 shown in FIG. 3A removes the coating from the sintered magnet 800. can be removed.
[0142] The following examples are of grades and performances, e.g., remanence (Br) and coercivity (iHc), uniform. Waste magnets from single or mixed bulk and EOL sources are agglomerated and processed to obtain the original starting magnetic material. A new Nd-F having properties according to the desired magnetic performance that are equal to or better than those shown by We demonstrate that it is possible to form eB regenerative magnets. EXAMPLES
[0143] Example 1 The discarded magnets were subjected to inductively coupled plasma (ICP) analysis and oxygen / carbon elemental analysis as shown in Table 1A below. The mass percentages of the components are determined by a magnetic permeability meter as shown in Table 1B below. The magnetic properties of the mixed waste magnets, such as remanence, retentivity, etc., were determined. Tables 1A and 1B characterize the waste magnet material.
[0144] Approximately 300 kg of mixed grade EOL magnets were held in a muffle furnace and heated to a temperature higher than the Curie temperature. The EOL magnets were demagnetized by heating at 650°C for 4 hours. The demagnetized magnets were quenched in water and coated. The magnets were crushed and dried in an oven at 200°C. The specimen was shot blasted for 15 minutes for further removal of grease and then held in an inert atmosphere. The mass loss of the demagnetized magnet due to the removal of the coating was less than 5%. The magnets were chemically treated with dilute HCl.
[0145] 100 kg of decoated, impurity-free waste material was placed in a reaction tumbling mixer. The coating was peeled off and 1% Nd(0.55x+1)Pr(0.45x+1) was added. The waste material and additives that do not contain impurities are subjected to the above-mentioned treatment and are then subjected to the above-mentioned treatment at room temperature, for example, at about 20 to about 25° C. for 4 hours. A hydrogen pressure of 2 bar (2000 kPa) was maintained in the reaction rotating mixer vessel. The resulting hydrogen The hydride mixture was partially degassed in situ by heating it to 550-600°C. Zinc tearate was mixed with the degassed powder for 30 minutes using a roller mill to remove the degassed powder. The powder was lubricated. The degassed powder was further homogenized until an average particle size of about 2.5 μm or less was reached. The resulting particles were then jet milled under an argon atmosphere for 1.5 hours to obtain a homogeneous powder. The magnets were then heated, sintered, annealed, and demagnetized. The demagnetization temperature was maintained at about 1050°C to about 1100°C for 5 hours. Then, the mixture was heated at 600° C. for 3 hours.
[0146] ICP, elemental analysis, and magnetic permeability tests were performed on the new Nd-Fe-B sintered product. The composition and magnetic properties of the Nd-Fe-B sintered products are shown in Tables 2A and 2B, respectively.
[0147] In this example, the elemental composition of the rare earth additive RE, e.g. Nd / Pr, is prepared on-site and then discarded. The materials were used to form hydride powder blends. The addition of RE was described, for example, with reference to FIG. The rare earth oxides removed from the waste starting material during the steps S20, S30, S40, and S50 described above. Or compensated for the calculated reduction in grain boundary surface area phase. The addition of partially degassed rare earth hydrides selectively increases the formation of grain boundary phases. During sintering, the amount of oxygen in the hydride powder can be increased to aid in solid state diffusion and / or In other words, the microstructure of the newly formed magnet is reduced by For example, the regeneration process is changed when rare earth element additives, e.g., NdPr The recovery and improvement of grain boundaries is utilized when absorbing the H2 component of the process gas to generate H3. After absorption, the NdPrH3 is converted back to oxygen-free NdPr during sintering. Thus, Grain boundary recovery and Nd2Fe 14 The reaction with B component constitutes the newly formed microstructure and elemental composition. As a result, the obtained Nd-Fe-B sintered magnet has Br, iHc, BHmax, or two or more of these. The waste starting material may have properties equal to or greater than those of the starting material, including combinations.
[0148] In some cases, the rare earth RE additive component may be used to produce a resulting Nd-Fe-B magnet that comprises only a Nd-rich phase. The grain boundary rich phase can be recovered and formed by diffusing along the grain boundaries, as shown in Table 3B. As will be explained in more detail with reference to the accompanying drawings, the coercivity and remanence are reduced.
[0149] The rare earth ratio of RE elements from waste magnets was calculated based on the main Nd2Fe 14 New B matrix phase In some implementations, the rare earth RE additive can be replaced by a waste magnet. By sintering together with the material from The coercivity of the original waste magnet starting material can be increased to a very small value. By using small amounts of new rare earth materials, regenerated sintered magnets can be restored or improved. For example, to produce new regenerated Nd-Fe-B products that have superior properties compared to the starting waste material. It can be constructed.
[0150] Magnetic properties are tabulated as BHmax (energy product), iHc (coercivity), and Br (residual magnetization). List them. [Table 1] [Table 2] [Table 3] [Table 4]
[0151] Example 2 EOL magnet starting material was supplied in magnetized form. EOL magnets were initially made with an Fe substrate within the EOL product. The magnets were demagnetized and subjected to the cyclic heating process described in more detail above. The mixed EOL magnets were separated from the Fe substrate using the regeneration step disclosed in Example 1. The stones were processed to form new full-dense Nd-Fe-B sintered magnet products.
[0152] 1% additive, e.g. Nd x / Pr y The additives shown in Tables 3A and 3C are The waste magnets were characterized by ICP, elemental analysis, and permeability meter. The compositions and magnetic properties of the starting waste material and the new Nd-Fe-B sintered product are shown in Table 3. A and B, as well as Tables 3C and 3D.
[0153] The magnetic properties and corresponding densities are listed as BHmax (energy product), iHc (coercivity), and Br (residual). The magnetic properties are listed in Tables 3A to 5B. [Table 5] [Table 6] [Table 7] [Table 8]
[0154] Example 3 The magnets from the waste starting material were characterized by ICP and penetrometer. See Tables 4A and 4B for details. 0.5-8% Nd, Dy, Co, Cu, and Fe additives , was added to the waste magnets as shown in the Additives column of Tables 5A and 5B. Fresh Nd-Fe-B The composition and magnetic properties of the sintered products are shown in Tables 5A and 5B, respectively. [Table 9] [Table 10] [Table 11] [Table 12]
[0155] From Tables 2B and 3B, it can be seen that the Nd / Pr element additives are used to control the recovery of remanence and the obtained It can be seen that the retention of the recycled sintered magnet can be improved by adding elements. The lower the purity of Nd in the additive, the higher the retention of the resulting regenerated sintered magnet can be restored. As more Pr is added to the elemental additive - the percentage of Nd present in the elemental additive decreases. Consistently, the coercivity of the resulting regenerated sintered magnet increases, but the remanence decreases slightly.
[0156] Similarly, the coercivity and remanence of the regenerated sintered magnets are as shown in Table 5B. It can be manipulated by varying the percentages of Co, Cu, and Fe additions. For example, From Table 5B, it can be seen that as the percentage of additive increases, there is a corresponding decrease in remanence with an increase in coercivity. Therefore, a low percentage of additive, e.g., 0.5% additive, can be used to obtain a high regeneration efficiency. The remanence of sintered magnets can be fully restored, but the addition of a high percentage of additive, e.g., 8%, The additives may reduce the remanence. A high percentage of additives reduces the remanence compared to the waste starting material in Table 4B. The coercivity value increases by at least about 30% to about 80% (see Table 5B), and this increase is due to the This can be achieved with a remanufactured sintered Nd-Fe-B product.
[0157] The waste magnets that are recycled fit into a range of possible compositions. For example, the composition of the waste magnets may vary slightly. At least 72% Fe, 7-20% Nd, at least 2% Pr, at least 5.6% B, and The first magnet waste material may include at least 0.1% Al. In some implementations, the first magnet waste The materials are 0-5% Dy; 0-4% Co; 0-0.3% Cu; 0-2.07% Tb; 0-0.19% Ga; 0-1 Contains at least one of: 0.25% Gd; 0-0.14% Ti; 0-0.3% Zr; and 0-0.3% Ni. In some implementations, the first magnet waste material comprises 0-5% Dy; 0-4% Co; 0-0.3% Cu; 0-2. 0.7% Tb; 0~0.19% Ga; 0~1.25% Gd; 0~0.14% Ti; 0~0.3% Zr; and 0~0.3 In some implementations, the first magnet waste material comprises at least two of: 0-5% Dy; 0 ~4% Co; 0~0.3% Cu; 0~2.07% Tb; 0~0.19% Ga; 0~1.25% Gd; 0~0.14% The alloy contains at least three of the following elements: Ti; 0-0.3% Zr; and 0-0.3% Ni.
[0158] In some implementations, the first magnet waste material comprises 0-5% Dy; 0-4% Co; 0-0.3% Cu; 0- 2.07% Tb; 0-0.19% Ga; 0-1.25% Gd; 0-0.14% Ti; 0-0.3% Zr; and 0-0. In some implementations, the first magnet waste material contains at least 4% of Dy; 0-5% of Ni; 0-5% of Dy; ~4% Co; 0~0.3% Cu; 0~2.07% Tb; 0~0.19% Ga; 0~1.25% Gd; 0~0.14% 0-0.3% Ti; 0-0.3% Zr; and 0-0.3% Ni. In some embodiments, the first The magnet waste material is composed of 0~5% Dy; 0~4% Co; 0~0.3% Cu; 0~2.07% Tb; 0~0.19% At least six of the following: Ga; 0-1.25% Gd; 0-0.14% Ti; 0-0.3% Zr; and 0-0.3% Ni. Includes.
[0159] In some implementations, the first magnet waste material comprises 0-5% Dy; 0-4% Co; 0-0.3% Cu; 0- 2.07% Tb; 0-0.19% Ga; 0-1.25% Gd; 0-0.14% Ti; 0-0.3% Zr; and 0-0. In some implementations, the first magnet waste material contains at least 7% Dy; 3% Ni. ~4% Co; 0~0.3% Cu; 0~2.07% Tb; 0~0.19% Ga; 0~1.25% Gd; 0~0.14% 0-0.3% Ti; 0-0.3% Zr; and 0-0.3% Ni. In some embodiments, the first The magnet waste material is composed of 0~5% Dy; 0~4% Co; 0~0.3% Cu; 0~2.07% Tb; 0~0.19% At least nine of the following: Ga; 0-1.25% Gd; 0-0.14% Ti; 0-0.3% Zr; and 0-0.3% Ni. Includes.
[0160] In some implementations, some of the above implementations contain 0-5% Dy; 0-4% Co; 0-0.3% Cu; 0~2.07% Tb; 0~0.19% Ga; 0~1.25% Gd; 0~0.14% Ti; 0~0.3% Zr; and 0 In some implementations, some of the above implementations include at least one of 0-5% Dy; 0~4% Co; 0~0.3% Cu; 0~2.07% Tb; 0~0.19% Ga; 0~1.25% Gd; 0~ It contains at least one of 0.14% Ti; 0 to 0.3% Zr; and 0 to 0.3% Ni.
[0161] In some implementations, the magnet waste material is composed of 0.1-5% Dy; 0.1-4% Co; 0.1-0.3% Cu; 0. 1~2.07% Tb; 0.01~0.19% Ga; 0.01~1.25% Gd; 0.01~0.14% Ti; 0.01~0.3% and 0.01-0.3% Ni. In some implementations, the magnet waste material comprises at least one of: 0.1~5% Dy; 0.1~4% Co; 0.1~0.3% Cu; 0.1~2.07% Tb; 0.01~0.19% Ga; 0 0.01~1.25% Gd; 0.01~0.14% Ti; 0.01~0.3% Zr; and 0.01~0.3% Ni. In some implementations, the magnet waste material contains 0.1-5% Dy; 0.1-4% Co; 0.1-5% 0.3% Cu; 0.1~2.07% Tb; 0.01~0.19% Ga; 0.01~1.25% Gd; 0.01~0.14% Ti 0.01~0.3% Zr; and 0.01~0.3% Ni.
[0162] In some implementations, the magnet waste material is composed of 0.1-5% Dy; 0.1-4% Co; 0.1-0.3% Cu; 0. 1~2.07% Tb; 0.01~0.19% Ga; 0.01~1.25% Gd; 0.01~0.14% Ti; 0.01~0.3% and 0.01-0.3% Ni. In some implementations, the magnet waste material comprises at least four of the following: 0.1~5% Dy; 0.1~4% Co; 0.1~0.3% Cu; 0.1~2.07% Tb; 0.01~0.19% Ga; 0 0.01~1.25% Gd; 0.01~0.14% Ti; 0.01~0.3% Zr; and 0.01~0.3% Ni. In some implementations, the magnet waste material contains 0.1-5% Dy; 0.1-4% Co; 0.1-5% Cr; 0.3% Cu; 0.1~2.07% Tb; 0.01~0.19% Ga; 0.01~1.25% Gd; 0.01~0.14% Ti 0.01-0.3% Zr; and 0.01-0.3% Ni.
[0163] In some implementations, the magnet waste material is composed of 0.1-5% Dy; 0.1-4% Co; 0.1-0.3% Cu; 0. 1~2.07% Tb; 0.01~0.19% Ga; 0.01~1.25% Gd; 0.01~0.14% Ti; 0.01~0.3% and 0.01-0.3% Ni. In some implementations, the magnet waste material comprises at least seven of the following: 0.1~5% Dy; 0.1~4% Co; 0.1~0.3% Cu; 0.1~2.07% Tb; 0.01~0.19% Ga; 0 0.01~1.25% Gd; 0.01~0.14% Ti; 0.01~0.3% Zr; and 0.01~0.3% Ni. In some implementations, the magnet waste material contains 0.1-5% Dy; 0.1-4% Co; 0.1-5% Cr; 0.3% Cu; 0.1~2.07% Tb; 0.01~0.19% Ga; 0.01~1.25% Gd; 0.01~0.14% Ti 0.01-0.3% Zr; and 0.01-0.3% Ni.
[0164] In some implementations, the waste magnets described herein have a composition containing Dy, Co, Cu, Tb, Ga, Gd, Ti, In some embodiments, the alloy may further comprise trace amounts of one or more of Zr, Ni, or a combination thereof. The composition of the waste magnets listed above is Dy, Co, Cu, Tb, Ga, Gd, Ti, Zr, Ni, or a combination of these. In some implementations, the waste magnet compositions described herein include one or more impurities of about 0.1 %, 0.2%, 0.3%, 0.4%, 0.5%, or less than 1% of Dy, Co, Cu, Tb, Ga, Gd, Ti, Zr, Ni In some implementations, the waste magnetic material described herein may include one or more of the following: The composition of the stone is one or more of Dy, Co, Cu, Tb, Ga, Gd, Ti, Zr, Ni, or a combination of these. In some implementations, the waste magnet compositions described herein do not include Including, consisting essentially of, or consisting of any of the ranges.
[0165] Table 6 shows material combinations that define other possible regenerative magnet materials according to some implementations. is. [Table 13]
[0166] In some implementations, the waste magnet material, whose composition ranges are defined in the table above, is first mixed with During or after the addition of a certain amount of rare earth element additive, about 0. An optimal magnetic powder mixture containing 5 to about 8 at % magnetic powder can be produced. In the above, the amount of elemental additive is determined so that at least one of the elemental components of the rare earth element additive is in the first process. The elements lost during the sieving step are the same as those lost from the waste magnet starting material, and in the amounts lost. In some embodiments, the amount of elemental additive is at least as much as rare earth. At least one of the elemental components of the elemental additive is present in the first processing step and in the further processing step. The elements are the same as those lost from the waste magnet starting material during the processing step, and the amount of this loss is To determine the amount of lost material, the amount of waste magnet starting material is Samples of the material are processed and analyzed using ICP to determine changes in rare earth element composition. For example, the reduction in the concentration of element Nd can be 0.7%. In this case, the 1% added Nd (0.70)Pr(0.25)(0.05 is other substances) element additives are the original Nd-Fe-B sintered magnet products It may be effective in restoring the grain boundary rich phase. In some cases, the reduction in Nd concentration was as low as 0.7%. In some cases, the total amount of Nd, Pr, and Dy shall not exceed 18% in the resulting Nd-Fe-B sintered product. can be added at twice the amount of the elemental additive, for example 2%.
[0167] The following equation further explains some implementations: R=s(Nd)+s(Pr)+s in waste magnet starting material. (Dy); T=f(Nd)+f(Pr)+f( Dy); and added virgin material V = Nd[p] + Pr[q] + Dy[r], where 0.1 ≦p+q+r≦19 at% of the final product, and T≧minimum (R, 18 at%). Consider the following example: the atomic percentage values of Nd, Pr, and Dy in the waste magnet starting material are If the values are 9.77, 2.96, and 0.92, the corresponding values are entered into the formula R = s(Nd) + s(Pr) + s(Dy). Substituting, R = 9.77 + 2.96 + 0.92, or R = 13.65. In the same example, a new regenerated Nd-Fe- The atomic percentages of Nd, Pr, and Dy in the sintered magnet are 10.74, 3.26, and 0.91, respectively. Substituting the value of a new recycled Nd-Fe-B sintered magnet into the formula T=s(Nd)+s(Pr)+s(Dy), , T = 10.74 + 3.26 + 0.91, or T = 14.91. In the same example, if virgin material is in the regeneration process, When doped with 0.2, 0.3, and 0.4 atomic percent N, the virgin material contains 0.2, 0.3, and 0.4 atomic percent N, respectively. d, Pr, and Dy, and by the formula V=Nd[p]+Pr[q]+Dy[r], V=0.2+0.3+0.4, or The formula for the virgin material, or V, is subject to two constraints: 0.1% of the final product ≤ p+ q+r≦19% of the final product and T≧minimum (R, 18 at%). In our example, p +q+r=0.9%, which is the first constraint: the value of p+q+r must be greater than or equal to 0.1% and less than or equal to 19%. This example satisfies the second constraint of the virgin material formula: T must be within the range of R or 18 In this example, T is 14.91, which is the smallest value of the set of R or 18. The smallest value is R, which is 13.65, so T is greater than or equal to the smallest value in the series of R, or 18.
[0168] In some implementations, V = Nd[p] + Pr[q] + Dy[r], where 0.1 ≤ p + q of the final product. +r≦15at% of the final product and T≧minimum (R, 18at%). In some implementations, V=Nd [p] + Pr[q] + Dy[r], where 0.1≦p+q+r≦12at% of the final product. and T ≥ minimum (R, 18 at%). In some implementations, V = Nd[p] + Pr[q] + Dy[r] where 0.1≦p+q+r≦8at% of the final product, and T≧minimum value(R, 18at In some implementations, V=Nd[p]+Pr[q]+Dy[r], where V is the total amount of the final product. 0.1≦p+q+r≦5at% of the final product, and T≧minimum value (R, 18at%). V = Nd[p] + Pr[q] + Dy[r], where 0.1≦p+q+r≦final product 3 at%, and T ≥ minimum (R, 18 at%). In some implementations, V = Nd[p] + Pr[q] + Dy[r], where 0.1≦p+q+r≦2at% of the final product, and T≧minimum value(R In some implementations, V=Nd[p]+Pr[q]+Dy[r], where The product has a value of 0.1≦p+q+r≦1 at% of the final product, and T is greater than or equal to the minimum value (R, 18 at%).
[0169] In some implementations, X is the at% of RE (Nd, Pr, Dy) removed from the original magnet, and p+q+ r≧X. In some implementations, the additive is f(Nd)+f(P r)>0, where f is the at% percentage of the regenerated Nd-Fe-B sintered product. In some implementations, f(Nd)+f(Pr)+f(Dy)≦18. In some implementations, f(Co)≦ 3. In some implementations, f(Cu)≦0.3. In some implementations, f(Fe)+f(Co)≦7. 7. In some implementations, f(Dy)+f(Nd)+f(Pr)≧R.
[0170] In some implementations, the elemental additive is Nd[0.1-19at%×s(Nd),x]Pr[0.1-19at%×s (Pr), y]Dy[0.1-19%×s(Dy), z]Co[0, d]Cu[0, e]Fe[0, f], in the formula , [m, n] means the range from the minimum m to the maximum n; s(t) is the number of elements t in the starting composition. where f(t) is the atomic percentage of element t in the final composition, and x=18-[81, 99.9]at%×(s(Nd)+s(Pr)+s(Dy));y=18-[81, 99.9]at%×(s(Nd)+s (Pr)+s(Dy));z=18-[81, 99.9]at%×(s(Nd)+s(Pr)+s(Dy));d=3 -[81, 99.9]at%×s(Co);e=0.3-[81, 99.9]at%×s(Cu);f=77-[81, 99. 9]at%×(s(Fe)+s(Co)).
[0171] In some implementations, (i) 0.1≦p+q+r≦19 at% of the final product and T ≧minimum (R, 18) virgin material, e.g., Nd p Pr q Dy r , where T=f(Nd)+f(Pr) +f(Dy) and R=s(Nd)+s(Pr)+s(Dy); (ii) p+q+r≧X, where X is the original magnet or (iii) T≦18%; (iv) f(Nd)+f(Pr) is the at% of RE (Nd, Pr, Dy) removed from the >0, where f is the at% percentage of the final product; (v) f(Nd) + f(Pr) + f(Dy) ≦ 18; ( vi) f(Co)≦3; (vii) f(Cu)≦0.3; (viii) f(Fe)+f(Co)≦77; and (ix) f( Dy)+f(Nd)+f(Pr)≧R.
[0172] In some implementations, the method further comprises adding 0.1 to 19 wt % of one or more rare earth element additives to the composition. or the method described herein. In another aspect, the method comprises adding about 0.1 wt.%, about 0.2 wt.% , about 0.3wt%, about 0.4wt%, about 0.5wt%, about 1wt%, about 2wt%, about 3wt%, about 4wt%, about 5wt%, About 6wt%, about 7wt%, about 8wt%, about 9wt%, about 10wt%, about 11wt%, about 12wt%, about 13wt%, about 14 %, about 15 wt%, about 16 wt%, about 17 wt%, about 18 wt%, or about 19 wt% of one or more elements added The addition of an elemental additive or a combination of one or more elemental additives to the composition or the method described herein. In yet another embodiment, the method comprises adding about 0.1-0.5 wt%, about 0.1-1 wt%, about 0.5-1 wt%, %, about 1-2wt%, about 1-3wt%, about 1-5wt%, about 1-8wt%, about 1-12wt%, about 1-15wt%, about 1~19wt%, about 2~4wt%, about 2~6wt%, about 2~12wt%, about 2~19wt%, about 3~5wt%, about 3~8wt % by weight, about 3-15 wt.%, and about 3-19 wt.% of one or more elemental additives or Addition of the combination to compositions or methods described herein is provided.
[0173] In some implementations, unavoidable impurities may be combined with certain substances.
[0174] The subject matter and functional process embodiments described herein are directed to the structures and methods disclosed herein. Digital electronic circuits, tangibly embodied computer software, including their structural equivalents or firmware, computer hardware, or a combination of one or more of these. Implementations of the subject matter described herein can be implemented as one or more computer program, i.e. for execution by or in a data processing apparatus A tangible non-transitory program carrier for controlling the operation of One or more modules of computer program instructions encoded in a program carrier Alternatively or additionally, the program instructions may be implemented as The resulting propagated signal, e.g., is transmitted to a suitable receiving device and executed by a data processing device. into machine-generated electrical, optical, or electromagnetic signals that are generated to encode information to be transmitted. A computer storage medium may include a machine-readable storage device, a machine-readable storage medium, a memory board, a random or serial access memory element, or a combination of one or more of these It can be said that:
[0175] The term "data processing device" refers to data processing hardware, e.g. multiprocessor, computer, or multiprocessor or multicomputer This includes all kinds of apparatus, devices and machines for processing data, including Also, dedicated logic circuits, such as FPGAs (Field Programmable Gate Arrays) may be or may further include an ASIC (Application Specific Integrated Circuit). In addition to the hardware, the device may also include a computer program execution environment. The code that generates the a database management system, an operating system, or a combination of one or more of these. The code may include code for generating a
[0176] Programs, software, software applications, modules, software Any software modules, scripts, or code may be called or described as such. A computer program may be written in a compiled or interpreted language, or in a declarative form. It can be written in any style of programming language, including verbal or procedural languages. and the computer program can be implemented as a stand-alone program or as a module. A program, component, subroutine, or other program suitable for use in a computing environment. It can be deployed in any form, including as other units. A program can correspond to a file in the file system, but it does not necessarily correspond to a file in the file system. A program need not be encoded in other programs or data, e.g. in a markup language. Documentation, either a single file dedicated to the program or several integrated files, e.g. A file that stores one or more modules, subprograms, or pieces of code. It can be saved in a part of the file that holds one or more saved scripts. A computer program may be run on one computer or at one site or across multiple on multiple computers distributed across multiple sites and interconnected by a communications network It can be expanded to run on
[0177] The processes and logic flows described herein may be implemented using one or more computer programs. A process that executes one or more processes that perform a function by manipulating input data and producing output. The process and logic flow may be implemented by a programmable processor. Special purpose logic circuits, such as FPGAs (Field Programmable Gate Arrays) or AS The device may also be implemented by an IC (application specific integrated circuit) and the device may be implemented by the dedicated logic circuitry. It can also be implemented as
[0178] A suitable computer for running a computer program is, by way of example, a general purpose microprocessor. processor, dedicated microprocessor, or both, or other type of central processing Generally, a central processing unit transmits instructions and data to a read-only memory, The essential elements of a computer are: A central processing unit for carrying out or executing instructions, and for storing instructions and data. Typically, a computer also has one or more memory elements for storing data. One or more mass storage devices, such as magnetic disks, magneto-optical disks, or optical disks receiving data from the mass storage device; operatively connected to the mass storage device to transmit or both transmit and receive. However, a computer need not necessarily have such devices. 2. The computer may communicate with another device, such as a mobile phone, a personal digital assistant, or a personal information Terminals (PDAs), portable audio or video players, game consoles, Global Positioning Systems (G A USB (Universal Serial Bus) receiver or a portable storage device, such as a Universal Serial Bus (USB) It can also be built into a flash drive.
[0179] Computer-readable medium suitable for storing computer program instructions and data Examples include semiconductor memory devices, such as EPROM, EEPROM, and flash memory devices. ;Magnetic disks, e.g. internal hard disks or removable disks;Magnetic-optical disks and all forms of non-volatile memory, media, and The processor and memory may be supplemented by special purpose logic circuitry. or may be incorporated into the dedicated logic circuitry.
[0180] To provide for interaction with a user, embodiments of the subject matter described herein may provide a user with A display device for displaying information, such as a CRT (cathode ray tube) or LCD (liquid crystal display) A monitor, and a keyboard and pointer that allow the user to enter input into the computer. The computer has a display device, such as a mouse or trackball. Other types of devices can also be used to provide user interaction. For example, the feedback provided to the user can be any form of sensory feedback. feedback, e.g. visual feedback, auditory feedback, or haptic feedback. and the input from the user includes acoustic input, voice input, or tactile input. In addition, the computer can be used by the user to by sending and receiving documents to a device that is used for Sends web pages to the web browser on the user device in response to the received request. This allows interaction with the user.
[0181] Implementations of the subject matter described herein may be implemented in a computer system, The computer system may include back-end components, such as a data server or middleware components, e.g. application servers or front-end components, e.g., implementing the subject matter described herein. A graphical user interface or window that allows a user to interact with including a client computer with a web browser or such back-end component, middleware component, or front-end component The components of this system include any combination of one or more of the following: Digital data communication in any form or medium, including networks interconnected by a communications network. An example of a communication network is a local area network (LAN). ) and wide area networks (WANs), such as the Internet.
[0182] The computer system may include clients and servers. The servers are generally remote from each other and typically interact through a communications network. The client and server relationship is that they run on different computers and communicate with each other. It is caused by a computer program that has a client-server relationship. In an embodiment, the server may, for example, transmit data to a user device acting as a client. To display to a user interacting with the device and to receive user input from the user To do so, data, e.g., an HTML page, is sent to the user device. The data generated by the user device as a result of the user interaction is processed by the server. can be received from the user device.
[0183] One example of one such type of computer is the general computer system 900. A schematic diagram is shown in FIG. 9. According to one implementation, the system 900 may be implemented using the components previously described. The present invention may be used in conjunction with any of the computer-implemented methods described herein. The system 900 includes a processor 910, a memory 920, a storage device 930, and an input / output device 940. Each of the components 910, 920, 930, and 940 is connected to each other using a system bus 950. The processor 910 is capable of processing instructions for execution within the system 900. In an implementation, the processor 910 is a single-threaded processor. The processor 910 is a multi-threaded processor. The instructions stored in the device 930 are processed to generate graphical information for a user interface. It can be displayed on the input / output device 940 .
[0184] The memory 920 stores information within the system 900. In one implementation, the memory 920 is In one implementation, the memory 920 is a volatile memory unit. In one embodiment, memory 920 is a non-volatile memory unit.
[0185] The storage device 930 is capable of providing mass storage for the system 900. The device 930 is a computer-readable medium. In various different implementations, the storage device 930 may be a The device may be a floppy disk device, a hard disk device, an optical disk device, or a tape device. This can be done.
[0186] The input / output device 940 provides input / output operations for the system 900. In one implementation, the input / output device 940 In another embodiment, the input / output device 940 may include a keyboard and / or a pointing device. A display unit for displaying a graphical user interface Includes.
[0187] Although the specification contains numerous specific implementation details, these may not limit the scope or claims of any invention. This should not be construed as a limitation on the scope that may be sought, but rather as a guide to the particular implementation of a particular invention. The description of features that may be specific to the embodiment should be interpreted as a description of the features that may be specific to the embodiment. Certain features described in the specification may also be implemented in combination in a single embodiment. Conversely, various features that are described in the context of a single embodiment may be used in different embodiments. The features may be implemented individually or in any suitable subcombination. Described above as functioning in a certain combination and first claimed as such Although one or more features of the claimed combination may, in some cases, be The claimed combination may be removed from the combination and may be a partial or partial combination. Various combinational variations are contemplated.
[0188] Similarly, although steps may be depicted in a particular order in the drawings, this is to be understood as meaning that such steps are It is not necessary to perform the steps in the particular order or sequential order illustrated to achieve desired results. It should not be construed as necessary to perform all of the steps illustrated or illustrated in any particular situation. In certain circumstances, multitasking and parallel processing may be advantageous. The separation of the various system modules and components described herein is not intended to limit the scope of such separation in all embodiments. should not be construed as requiring that the program components and systems described Generally, they are bundled together in a single software product or packaged together in multiple software products. This should be interpreted as meaning that it can be caged.
[0189] Certain embodiments of the subject matter have been described above. Other embodiments are within the scope of the following claims. For example, the actions recited in the claims may be performed in a different order and still be desirable. By way of example, the process depicted in the accompanying drawings may be used to achieve the desired results. The particular order illustrated, nor sequential order, is necessarily required to achieve the desired results. In some cases, multitasking and parallel processing may be advantageous.
[0190] The present application provides the following invention. (Configuration 1) 1. A method for producing a remanufactured Nd—Fe—B permanent magnet, comprising: The magnetic material from the waste magnet assembly is deactivated. demagnetizing by cyclic heating and cooling in an atmosphere; fragmenting the demagnetized magnetic material to form a first or second regenerated Nd—Fe—B powder; The first or second regenerated Nd—Fe—B powder is mixed with (a) a powder of at least one rare earth material R, and (b) and mixing with a powder of at least one elemental additive A, and optionally, the resulting powder mixture. homogenizing to produce a homogenous powder mixture, wherein the rare earth material R is Nd or Pr and the element additive A contains at least one of Dy, Co, Cu, and Fe. the steps including: The homogenous powder mixture is sintered and magnetized to produce a regenerated Nd-F containing oxygen at levels below 1.98 at%. forming a permanent magnet; where The first regenerated Nd—Fe—B powder has an average particle size of about 1 μm to about 2 mm; and The second recycled Nd-Fe-B powder has an average particle size of about 1 μm to about 4 μm; and Permanent magnets: (a) reducing the remanence and coercivity of the waste magnet material from the waste magnet assembly by at least the same the remanence and coercivity being the same; or (b) a coercivity of the waste Nd—Fe—B magnet material from the waste magnet assembly that is about 0 to about 20% higher than the coercivity of the waste Nd—Fe—B magnet material from the waste magnet assembly; low coercivity; or (c) a residual magnetization of the discarded Nd-Fe-B magnet that is approximately 97% of the residual magnetization of the discarded magnet assembly; a coercivity that is at least 30% higher than the coercivity of the waste Nd—Fe—B magnet material from Brazil; or (d) a residual magnetization of the discarded Nd-Fe-B magnet that is approximately 95% of the residual magnetization of the discarded magnet assembly; a coercivity that is at least 80% higher than the coercivity of the waste Nd—Fe—B magnet material from Brazil; or (e) a residual magnetization that is about 5% higher than the residual magnetization of the discarded Nd-Fe-B magnets, and A coercivity at least equal to the coercivity of the waste Nd—Fe—B magnet material from Buri. The method according to claim 1, (Configuration 2) The recycled Nd-Fe-B is the first recycled Nd-Fe-B powder having an average particle size of about 1 μm to about 2 mm. and mixed with the powder of the rare earth material R and the powder of the element additive A to obtain a homogeneous powder mixture. The method of claim 1, further comprising: (Configuration 3) The second recycled Nd-Fe-B powder has an average particle size of about 1 μm to about 4 μm. The powder of the rare earth material R and the powder of the element additive A are mixed together to form a homogeneous powder mixture. The method of claim 1, for producing an object. (Configuration 4) The demagnetized magnetic material is shredded from the waste Nd-Fe-B magnet to obtain a first or second regenerated Nd-Fe-B powder. The forming step forms a first regenerated Nd—Fe—B powder having an average particle size of about 1 μm to about 2 mm. and further fragmenting and homogenizing the first regenerated Nd—Fe—B powder to obtain the first regenerated Nd—Fe—B powder. providing said second regenerated Nd-Fe-B powder having an oxygen content lower than that of the d-Fe-B powder; The fraction of particles larger than the average particle size of the first regenerated Nd—Fe—B powder is sieved so as to obtain a powder having a particle diameter larger than the average particle diameter of the first regenerated Nd—Fe—B powder. By removing the Nd-Fe-B powder, a second regenerated Nd-Fe-B powder having an average particle size of about 1 μm to about 4 μm is formed. The method of claim 3, further comprising the step of: (Configuration 5) Removing the fraction of particles larger than the average particle size of the first regenerated Nd—Fe—B powder is The method according to claim 4, wherein the method is carried out in a hydrogen atmosphere. (Configuration 6) 6. The method of claim 5, wherein the inert atmosphere comprises argon. (Configuration 7) The homogenous powder mixture is mixed with a powder of another element selected from the element additive A, or or a powder of another element selected from the rare earth material R, or both; The method of claim 1. (Configuration 8) The remanufactured Nd-Fe-B permanent magnet has a plurality of grain boundary regions extending throughout the remanufactured Nd-Fe-B permanent magnet. and the plurality of grain boundary regions are present in corresponding grain boundary regions of the discarded Nd—Fe—B magnet. 2. The method of claim 1, wherein the concentration of rare earth material R and elemental additive A is greater than or equal to the concentration of rare earth material R and elemental additive A. (Configuration 9) The rare earth material R is converted to oxygen-free NdPr during sintering. 3 Including, composition 1 Method of posting. (Configuration 10) The rare earth material R powder is present at a level of 0.1 atomic % to 1 atomic % relative to the entire homogeneous powder mixture. 2. The method of claim 1, wherein (Configuration 11) The powder of the rare earth material R contains Nd and Pr in a ratio of 25 wt% Nd and 75 wt% Pr. The method described. (Configuration 12) The rare earth material R powder and the element additive A powder are continuous with the recycled Nd-Fe-B powder. 2. The method of claim 1, wherein the powder mixture is mixed continuously to produce a homogenous powder mixture. (Configuration 13) The rare earth material R powder, the element additive A powder, and the recycled Nd-Fe-B powder are simultaneously to produce a homogenous powder mixture. (Configuration 14) 2. The method of claim 1, wherein the fragmentation and mixing steps are performed simultaneously. (Configuration 15) 2. The method of claim 1, wherein the homogenous powder has an average particle size of 1 to 4 μm. (Configuration 16) The first regenerated Nd-Fe-B powder has an average particle size of about 1 μm to about 2 mm; The rare earth material R powder and the element additive A powder, to produce a homogenous powder mixture having an average particle size of about 1 μm to about 4 μm. The method of claim 1, comprising: (Configuration 17) the second regenerated Nd—Fe—B powder having an average particle size of about 1 μm to about 4 μm; The rare earth material R powder and the element additive A powder, to produce a homogenous powder mixture having an average particle size of about 1 μm to about 4 μm. The method of claim 1, comprising: (Configuration 18) A lubricant is added to the homogenous powder mixture, and the homogenous powder mixture is compressed to form a green compact. forming a sintering the green compact at a temperature of about 1000°C to about 1100°C; heat treating the sintered green compact at about 490°C to about 950°C; The heat-treated compact is magnetized in an inert atmosphere at less than 15°C to obtain a regenerated Nd-Fe-B permanent magnet. 2. The method of claim 1, further comprising the step of: (Configuration 19) 2. The method of claim 1, wherein the regenerated Nd-Fe-B permanent magnet contains 1.32 to 1.98 at % oxygen. (Configuration 20) The regenerated Nd-Fe-B permanent magnet has at least the same remanence and coercivity as the discarded Nd-Fe-B magnet. The method of claim 1, further comprising: (Configuration 21) The regenerated Nd-Fe-B permanent magnet is (a) a coercivity that is about 0 to about 20% higher than the coercivity of the discarded Nd—Fe—B magnets; or (b) a residual magnetism that is about 97% of the residual magnetism of the discarded Nd-Fe-B magnets, and a coercivity at least 30% higher than that of (c) a residual magnetism that is about 95% of the residual magnetism of said discarded Nd-Fe-B magnets, and a coercivity at least 80% higher than that of (d) a residual magnetism that is about 5% higher than the residual magnetism of the discarded Nd—Fe—B magnet, and A coercivity at least equal to that of the stone The method of claim 1, (Configuration 22) 2. The method of claim 1, wherein the recycled Nd—Fe—B permanent magnets have an average grain size of less than 5 μm. (Configuration 23) 2. The method of claim 1, wherein the recycled Nd—Fe—B permanent magnets have an average grain size of less than 2.5 μm. (Configuration 24) The recycled Nd-Fe-B permanent magnet has a mass of about 7.56 g / cm 3 ~Approx. 7.6g / cm 3 2. The method according to claim 1, having a density of method. (Configuration 25) 2. The method of claim 1, wherein the regenerated Nd-Fe-B permanent magnet comprises Co at a concentration of 3 atomic % or less. (Configuration 26) 2. The method of claim 1, wherein the regenerated Nd—Fe—B permanent magnet comprises Cu at a concentration of 0.3 atomic % or less. (Configuration 27) 2. The regenerated Nd—Fe—B permanent magnet according to claim 1, wherein the regenerated Nd—Fe—B permanent magnet contains Fe and Co in a combined concentration of 77 atomic % or less. How to. (Configuration 28) The regenerated Nd-Fe-B permanent magnet comprises Nd, Dy, and Pr in a combined concentration of 18 atomic % or less. 1. The method described in claim 1. (Configuration 29) The regenerated Nd—Fe—B permanent magnet is substantially a R b A c The composition of the present invention is Here, W is the amount of Nd-Fe-B material corresponding to the demagnetized Nd-Fe-B material derived from the discarded Nd-Fe-B magnets. Includes minutes; The subscripts a, b, and c correspond to the atomic percentage of the corresponding component or element; a(t) is the atomic percentage of element t in W relative to the composition of the recycled Nd—Fe—B permanent magnet; b(t) is the atomic ratio of element t in the rare earth-containing material R to the composition of the regenerated Nd—Fe—B permanent magnet. is a percentage; c(t) is the atomic percentage of element t in the element additive A relative to the composition of the regenerated Nd—Fe—B permanent magnet. rate; and a, b, c, a(t), b(t), and c(t) are 81at%≦a≦99.9at%, 0.1at%≦b≦19at%, 3at%-99.9%×a(Co)≦c(Co)≦3at%-81%×a(Co), 0.3at%-99.9%×a(Cu)≦c(Cu)≦0.3at%-81%×a(Cu), 77at%-99.9%×(a(Fe)+a(Co))≦c(Fe)≦77at%-81%×(a(Fe)+a(Co)), a(Nd)+b(Nd)+c(Nd)+a(Pr)+b(Pr)+c(Pr)>0at%, a(Nd)+b(Nd)+c(Nd)+a(Pr)+b(Pr)+c(Pr)+a(Dy)+b(Dy)+c(Dy)≦18at%, a(Co)+b(Co)+c(Co)≦3at%, a(Cu)+b(Cu)+c(Cu)≦0.3at%, a(Fe)+b(Fe)+c(Fe)+a(Co)+b(Co)+c(Co)≦77at%, and b(Nd)+c(Nd)+b(Pr)+c(Pr)+b(Dy)+c(Dy)≧0at% 2. The method of claim 1, having a value that satisfies: (Configuration 30) The regenerated Nd—Fe—B permanent magnet is substantially a R b A c The composition of the present invention is where W includes Nd—Fe—B material from the waste Nd—Fe—B magnets, and the subscripts a, b, and c contains the atomic percentage of the corresponding component or element, and the rare earth material R and the elemental additive A are : Nd[0.1-19%×s(Nd), x], Pr[0.1-19%×s(Pr), y], Dy[0.1-19%×s(Dy), z], Co[0at%, d], Cu[0at%, e], Fe[0at%, f] Fulfilling During the ceremony: [m, n] means a range from a first value in a minimum interval m to a second value in a maximum interval n; s(t) is the atomic percentage of element t in the starting composition; x=18at%-[81, 99.9]%×(s(Nd)+s(Pr)+s(Dy)); y=18at%-[81, 99.9]%×(s(Nd)+s(Pr)+s(Dy)); z=18at%-[81, 99.9]%×(s(Nd)+s(Pr)+s(Dy)); d=3at%-[81, 99.9]%×s(Co); e=0.3at%-[81, 99.9]%×s(Cu); and 2. The method of claim 1, wherein f=77at%-[81, 99.9]%×(s(Fe)+s(Co)). (Configuration 31) Recovering demagnetized magnetic material from one or more discarded Nd-Fe-B magnet assemblies by: The method of embodiment 1, further comprising: Physically separate each waste Nd-Fe-B magnet assembly into waste Nd-Fe-B magnets and non-magnet materials. Steps; removing any residual coating or adhesive from each of the discarded Nd—Fe—B magnets; and Demagnetizing each of the waste Nd-Fe-B magnets to form a demagnetized magnetic material from the waste Nd-Fe-B magnets. P.S. (Configuration 32) The step of removing the residual coating or adhesive is performed on the waste Nd—Fe—B magnet. , mechanical fragmentation or cracking, or chemical treatment. 32. The method of claim 31, comprising: (Configuration 33) The coating is electrolytic black epoxy, Ni, Ni-Cu, Ni-Ni, Nd-Fe-B magnet waste 33. The method of claim 32, wherein the coating layer is selected from i-Cu-Ni, or Zn. (Configuration 34) The step of demagnetizing each of the discarded Nd—Fe—B magnets includes periodically demagnetizing the discarded Nd—Fe—B magnets. - temperature and cooling at a rate of at least 100°C / sec for each discarded Nd-Fe-B magnet. 32. The method of claim 31. (Configuration 35) The cyclic heating and cooling heating each waste Nd—Fe—B magnet to the Curie temperature of the waste Nd—Fe—B magnet; Then, cooling the discarded Nd—Fe—B magnets at a rate of at least 100° C. / sec. 2. The method of claim 1, comprising: (Configuration 36) The total atomic percentage of Nd, Pr, and Dy in the recycled Nd-Fe-B permanent magnet is The method of claim 1, wherein the total atomic percentage of Nd, Pr, and Dy in the stone is equal to or greater than the total atomic percentage of Nd, Pr, and Dy in the stone. (Configuration 37) (a) The powder of the rare earth material R is contained in the homogenous powder, based on the entire homogenous powder mixture. It exists at levels between 0.1 at% and 1 at%. (b) said rare earth material R is 75 wt% Nd and 25 wt% Pr; (i) Nd or (ii) Pr or (c) determining whether the residual magnetism and the coercivity are at least equal to the waste magnet portion from the waste magnet assembly; The method of claim 1, wherein the method is at least the same as the method of claim 1. (Configuration 38) 2. The method of claim 1, wherein the first or second regenerated Nd—Fe—B powder contains oxygen at a level of 1.98 at% or less. Method of posting. (Configuration 39) 17. The method of claim 16, wherein the first regenerated Nd-Fe-B powder contains oxygen at a level of 1.98 at% or less. Law. (Configuration 40) 18. The method of claim 17, wherein the second regenerated Nd-Fe-B powder contains oxygen at a level of 1.98 at% or less. Law. The claims are as follows:
Claims
1. W a R b A c A method for producing a recycled Nd-Fe-B sintered magnet comprising the composition of: comprising sintering particles of waste material W comprising Nd-Fe-B material recovered from waste Nd-Fe-B sintered magnets together with Dy and rare earth-containing material R comprising Nd and Pr in a ratio of 75 wt% Nd to 25 wt% Pr and 0.1-1 at% of the recycled Nd-Fe-B sintered magnets, and elemental additive A comprising Co, Cu, and Fe; The subscripts a, b, and c represent the atomic percentage of the corresponding component or element.
2. The rare earth-containing material R and the element additive A are such that the concentration of the rare earth-containing material R and the concentration of the element additive A are the main Nd in the recycled Nd-Fe-B sintered magnet. 2 Fe 14 2. The method of claim 1, wherein the B phase is homogeneously distributed at grain boundaries throughout the thickness of the recycled Nd—Fe—B sintered magnet so as to be on average high in the mixture of waste material W surrounding the B phase.
3. The recycled Nd-Fe-B sintered magnet has a density of 7.56 g / cm 3 ~7.6g / cm 3 2. The method of claim 1, comprising a density in the range of:
4. The waste Nd—Fe—B sintered magnet exhibits coercivity and remanence, and the regenerated Nd—Fe—B sintered magnet exhibits: (a) a remanence and coercivity at least equal to the remanence and coercivity of the waste Nd—Fe—B sintered magnets; (b) a coercivity in the range of 0% to 20% higher than that of the waste Nd—Fe—B sintered magnets; (c) a remanence that is about 97% of the remanence of the waste Nd—Fe—B sintered magnets, and a coercivity that is at least 30% higher than the coercivity of the waste Nd—Fe—B sintered magnets; (d) a remanence that is about 95% of the remanence of the waste Nd—Fe—B sintered magnets, and a coercivity that is at least 80% higher than the coercivity of the waste Nd—Fe—B sintered magnets; and (e) a remanence that is about 5% higher than that of the waste Nd—Fe—B sintered magnets, and a coercivity that is at least the same as that of the waste Nd—Fe—B sintered magnets. The method of claim 1, wherein the method exhibits at least one of the following:
5. 2. The method according to claim 1, wherein the total atomic percentage of Nd, Pr, and Dy in the recycled Nd—Fe—B sintered magnet is equal to or greater than the total atomic percentage of Nd, Pr, and Dy in the discarded Nd—Fe—B sintered magnet.
6. 2. The method of claim 1, wherein the regenerated sintered Nd-Fe-B magnet contains up to 1.98 at % oxygen.
7. 2. The method of claim 1, wherein the regenerated sintered Nd—Fe—B magnet contains 1.32 to 1.98 at % oxygen.
8. 2. The method of claim 1, wherein the elemental additive A comprises Dy.
9. The method of claim 1 , wherein the elemental additive A comprises the rare earth-containing material R.
10. W a R b A c A method for manufacturing a recycled Nd-Fe-B sintered magnet comprising the composition of a W b R c A, the method comprising sintering particles of waste material W containing Nd-Fe-B material recovered from waste Nd-Fe-B sintered magnets together with a rare earth-containing material R containing Nd and Pr in a ratio of 75 wt% Nd to 25 wt% Pr and 0.1 to 1 at% of Nd and Pr of the recycled Nd-Fe-B sintered magnet, and an element additive A containing at least one of a) Nd, b) Pr, c) Dy, d) Co, e) Cu, or f) Fe, wherein the subscripts a, b, and c represent the atomic percentages of the corresponding components or elements.
11. The rare earth-containing material R and the element additive A are such that the concentration of the rare earth-containing material R and the concentration of the element additive A are the main Nd in the recycled Nd-Fe-B sintered magnet. 2 Fe 14 11. The method of claim 10, wherein the B phase is homogeneously distributed at grain boundaries throughout the thickness of the recycled Nd—Fe—B sintered magnet so as to be on average high in the mixture of waste material W surrounding the B phase.
12. 11. The method of claim 10, wherein a first atomic percentage of the waste material W in the recycled Nd—Fe—B sintered magnet ranges from 99.9 at% to 81 at%, and a second atomic percentage of the combination of the rare earth-containing material R and the elemental additive A in the recycled Nd—Fe—B sintered magnet ranges from 0.1 at% to 19 at%.
13. The recycled Nd-Fe-B sintered magnet has a density of 7.56 g / cm 3 ~7.6g / cm 3 11. The method of claim 10, comprising a density in the range of:
14. 11. The method of claim 10, wherein the regenerated sintered Nd-Fe-B magnet comprises an atomic percentage of Co up to 3 at%.
15. 11. The method of claim 10, wherein the regenerated sintered Nd-Fe-B magnet comprises an atomic percentage of Cu equal to or less than 0.3 at%.
16. 11. The method of claim 10, wherein the regenerated sintered Nd-Fe-B magnet comprises a combined atomic percentage of Fe and Co up to 77 at%.
17. 11. The method of claim 10, wherein the regenerated sintered Nd-Fe-B magnet comprises a total atomic percentage of Nd, Dy, and Pr of less than or equal to 18 at%.
18. 11. The method of claim 10, wherein the elemental additive A comprises the rare earth-containing material R.
19. 11. The method of claim 10, wherein the elemental additive A comprises Dy.
20. 11. The method of claim 10, wherein the regenerated sintered Nd-Fe-B magnet contains up to 1.98 at% oxygen.
21. 11. The method of claim 10, wherein the regenerated sintered Nd—Fe—B magnet contains 1.32 to 1.98 at % oxygen.
22. 22. A method for manufacturing a device or system including a remanufactured Nd—Fe—B magnet, comprising manufacturing the remanufactured Nd—Fe—B magnet according to the method of any one of claims 1 to 21, wherein the device or system is a starter motor, an antilock braking system (ABS), a fuel pump, a fan, a loudspeaker, a microphone, a telephone ringer, a switch, a relay, a hard disk drive (HDD), a stepper motor, a servo motor, a magnetic resonance imaging device (MRI), a wind turbine generator, a robotic device, a sensor, a magnetic separator, a guidance system, or a satellite.
Citation Information
Patent Citations
MANUFACTURE OF MATERIAL POWDER FOR R-Fe-B MAGNET
JP2000030919A
Method of manufacturing rare-earth magnet powder
JP2005057191A
Method for producing sintered permanent magnet, and die
JP2008163466A
R-t-b-based sintered magnet
JP2013110387A
R-t-b-type sintered magnet and method for production thereof
WO2009122709A1