Slide member, and compressor and refrigeration device using same

JP7588322B2Active Publication Date: 2024-11-22PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023502187
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-24
Filing Date
2022-01-26
Publication Date
2024-11-22
Estimated Expiration
2042-01-26

AI Technical Summary

Benefits of technology

【0012】 以上のように、本発明によれば、焼付きまたは異常摩耗を効果的に抑制または回避できる摺動部材と、それを用いて良好な運転効率または信頼性を実現できる圧縮機および冷凍装置とを提供することができるという効果を奏する。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588322000001
    Figure 0007588322000001
  • Figure 0007588322000002
    Figure 0007588322000002
  • Figure 0007588322000003
    Figure 0007588322000003
Patent Text Reader

Abstract

This sliding member comprises: a substrate (11d); a combination layer (41a) that is formed from at least nickel, aluminum that is a component of the substrate (11d), and phosphorus; and a nickel film layer (41b) that contains nickel as the primary component and is disposed above the combination layer (41a). Due to this configuration, the nickel film layer (41b) formed on the sliding member is capable of realizing good peeling resistance and is therefore capable of long-term, strong suppression of seizing or abrasion of the sliding member.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a sliding member, a compressor, and a refrigeration apparatus, and in particular to a sliding member used in a sliding part of a compressor, a compressor including the sliding member and used in equipment using a refrigeration cycle device such as an air conditioner, a water heater, or a refrigerator, and a refrigeration apparatus including the compressor. [Background technology]

[0002] Patent Documents 1 and 2 disclose scroll compressors used in air conditioners, etc. In these scroll compressors, a fixed spiral wrap of a fixed scroll and an orbiting spiral wrap of an orbiting scroll are meshed with each other, and a working medium such as a refrigerant is compressed by orbiting the orbiting scroll.

[0003] The fixed scroll and the orbiting scroll are sliding members that slide when compressing the working medium. When the sliding members are made of the same metal, a method is adopted in which the surface of one of the sliding members is subjected to a surface treatment such as anodizing or plating to prevent seizure.

[0004] For example, in Patent Document 1, an alloy mainly composed of aluminum is used for the fixed scroll and the orbiting scroll, and at least one of the surfaces is plated with nickel containing aluminum oxide (Al2O3) and silicon carbide (SiC)-based hard particles.In Patent Document 2, an alloy mainly composed of aluminum is also used, and at least one of the surfaces is plated with nickel having boron nitride (BN) dispersed in the film. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Utility Model Application Publication No. 3-99801 [Patent Document 2] JP 2000-64970 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present disclosure provides a sliding member capable of effectively suppressing or avoiding seizure or abnormal wear, and a compressor and a refrigeration device using the same capable of achieving good operating efficiency or reliability. [Means for solving the problem]

[0007] In order to solve the above-mentioned problems, the slide member of the present disclosure includes a substrate, a mixed layer containing at least nickel, a component of the substrate, and phosphorus and / or boron, and a nickel coating layer containing nickel provided above the mixed layer.

[0008] According to the above-mentioned configuration, the nickel coating layer formed on the sliding member can achieve good peeling resistance, so that seizure or wear of the sliding member can be effectively suppressed for a long period of time.

[0009] Moreover, in order to solve the above-mentioned problems, the compressor and refrigeration device disclosed herein include a compression mechanism that compresses a refrigerant, an electric mechanism that drives the compression mechanism, and a sealed container that houses the compression mechanism and the electric mechanism and has an oil reservoir at the bottom that retains lubricating oil, and is configured to include a sliding part using the sliding member of the above-mentioned configuration.

[0010] According to the above-described configuration, the sliding member is provided with a nickel coating layer having good peeling resistance, so that seizure or wear caused by peeling of the surface treatment can be effectively suppressed or avoided, and even better long-term reliability can be achieved.

[0011] The above and other objects, features, and advantages of the present invention will become apparent from the following detailed description of preferred embodiments, taken in conjunction with the accompanying drawings. Effect of the Invention

[0012] As described above, the present invention has an effect of providing a sliding member that can effectively suppress or avoid seizure or abnormal wear, and a compressor and a refrigeration system that can achieve good operating efficiency or reliability by using the sliding member. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a vertical sectional view of a scroll compressor according to a first embodiment. [Diagram 2] FIG. 2 is a schematic enlarged cross-sectional view of the vicinity of the base material interface of the fixed scroll of the scroll compressor in the first embodiment. [Diagram 3] 3A and 3B are cross-sectional EDS element mapping diagrams in the vicinity of the base material interface of a fixed scroll of a scroll compressor in a representative example of the first embodiment. [Figure 4] 4A and 4B are cross-sectional EDS element mapping diagrams in the vicinity of the substrate interface when a nickel coating layer having a low phosphorus concentration is used in a representative comparative example. [Diagram 5] FIG. 5 is a correlation diagram showing the relationship between the phosphorus concentration and the thickness of the mixed layer. [Figure 6] FIG. 6 is an enlarged schematic cross-sectional view of the vicinity of the base material interface of the fixed scroll of the scroll compressor in the second embodiment. [Figure 7] 7A and 7B are cross-sectional EDS element mapping diagrams in the vicinity of the base material interface of the fixed scroll of the scroll compressor in the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] (The knowledge and other information that formed the basis of this disclosure) At the time when the inventors of the present application came up with the idea of ​​the present disclosure, as described in Patent Document 1 or Patent Document 2, scroll compressors were designed to prevent seizure by applying a hard coating treatment to the surface of at least one of the fixed scroll and the orbiting scroll, whose base material was an aluminum alloy.

[0015] However, when a hard coating such as nickel plating is formed on a soft substrate such as aluminum, the difference in hardness between the aluminum substrate and the hard coating, i.e., the difference in mechanical strength, is significantly large. Therefore, when a shear force acts parallel to the interface due to frictional sliding, the hard coating may peel off at the interface or may break (e.g., tear off) along with the substrate just below the interface, exposing the aluminum substrate between the sliding surfaces.

[0016] Furthermore, if the hard coating peels off and the aluminum substrates slide against each other, aluminum is an active metal, and this can cause abnormal wear or adhesion, resulting in seizure, which makes it difficult to ensure reliability over a long period of time.

[0017] The inventors of the present application have found these problems and have come to form the subject of the present disclosure in order to solve them.

[0018] Therefore, the present disclosure provides a slide member capable of suppressing seizure or wear over a long period of time by improving the adhesion strength and peeling resistance of the hard nickel coating layer. In addition, by using the slide member of the present disclosure, seizure or wear caused by peeling of the hard coating in the sliding portion can be avoided, thereby providing a compressor and a refrigeration device having high reliability over a long period of time.

[0019] Hereinafter, the embodiments will be described in detail with reference to the drawings. However, more detailed explanation than necessary may be omitted. For example, detailed explanation of already well-known matters or duplicate explanation of substantially the same configuration may be omitted. This is to avoid the following explanation becoming more redundant than necessary and to facilitate understanding by those skilled in the art.

[0020] It should be noted that the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand the present disclosure, and are not intended to limit the subject matter described in the claims.

[0021] (Embodiment 1) Hereinafter, the first embodiment will be described with reference to FIGS. 1 to 3B.

[0022] [1-1. Configuration] As shown in FIG. 1, the scroll compressor according to this embodiment is configured by disposing a compression mechanism unit 10 that compresses a refrigerant and an electric mechanism unit 20 that drives the compression mechanism unit 10 in a sealed container 1.

[0023] The sealed container 1 includes a body 1a, a bottom lid 1b, and a top lid 1c. The body 1a is formed in a cylindrical shape extending in the vertical direction. The bottom lid 1b is a lid member that closes the bottom opening of the body 1a. The top lid 1c is a lid member that closes the top opening of the body 1a. The bottom lid 1b and the top lid 1c are both curved toward the outer center, and in the configuration example shown in FIG. 1, they have a bowl shape that fits inside the bottom or top opening of the body 1a.

[0024] The sealed container 1 includes a refrigerant suction pipe 2 and a refrigerant discharge pipe 3. The refrigerant suction pipe 2 introduces a refrigerant into the compression mechanism 10. The refrigerant discharge pipe 3 discharges the refrigerant compressed by the compression mechanism 10 to the outside of the sealed container 1. An injection pipe 19 is connected to the top of the sealed container 1 (upper lid 1c) together with the refrigerant discharge pipe 3.

[0025] The compression mechanism 10 has a fixed scroll 11, an orbiting scroll 12, and a rotating shaft 13 that orbits the orbiting scroll 12. The electric mechanism 20 has a stator 21 fixed to the sealed container 1, and a rotor 22 arranged inside the stator 21. The rotating shaft 13 is fixed to the rotor 22.

[0026] An eccentric shaft 13a is formed at the upper end of the rotary shaft 13, which is eccentric with respect to the rotary shaft 13. An oil reservoir 12e is formed in the eccentric shaft 13a by a recess that opens to the upper surface of the eccentric shaft 13a.

[0027] A main bearing 30 that supports the fixed scroll 11 and the orbiting scroll 12 is provided below the fixed scroll 11 and the orbiting scroll 12. The main bearing 30 is formed with a bearing portion 31 that supports the rotating shaft 13, and a boss accommodating portion 32. The main bearing 30 is fixed to the sealed container 1 by welding, shrink fitting, or the like. A lower end portion 13b of the rotating shaft 13 is supported by an auxiliary bearing 18 arranged at the bottom of the sealed container 1.

[0028] The fixed scroll 11 includes a fixed scroll end plate 11a, a fixed spiral wrap 11b, and an outer peripheral wall portion 11c. The fixed scroll end plate 11a is disk-shaped, and the fixed spiral wrap 11b is spiral-shaped and stands on the fixed scroll end plate 11a. The outer peripheral wall portion 11c stands so as to surround the periphery of the fixed spiral wrap 11b. A discharge port 14 is formed in the approximate center of the fixed scroll end plate 11a.

[0029] The orbiting scroll 12 includes an orbiting scroll end plate 12a, an orbiting spiral wrap 12b, and a boss portion 12c. The orbiting scroll end plate 12a is disk-shaped, and the orbiting spiral wrap 12b is spiral-shaped and erected on the wrap side end surface of the orbiting scroll end plate 12a. The boss portion 12c is cylindrical and formed on the end surface of the orbiting scroll end plate 12a opposite the wrap side.

[0030] The fixed spiral wrap 11b of the fixed scroll 11 and the orbiting spiral wrap 12b of the orbiting scroll 12 are meshed with each other. As a result, a plurality of compression chambers 15 are formed between the fixed spiral wrap 11b and the orbiting spiral wrap 12b. The boss portion 12c is formed at approximately the center of the orbiting scroll end plate 12a. The eccentric shaft 13a is inserted into the boss portion 12c, and the boss portion 12c is accommodated in the boss accommodation portion 32.

[0031] The fixed scroll 11 is fixed to the main bearing 30 at its outer circumferential wall portion 11c by, for example, a plurality of bolts (not shown). On the other hand, the orbiting scroll 12 is supported by the fixed scroll 11 via a rotation restraint member 17 such as an Oldham ring. The rotation restraint member 17 is provided between the fixed scroll 11 and the main bearing 30. The rotation restraint member 17 restrains the rotation of the orbiting scroll 12. As a result, the orbiting scroll 12 orbits relative to the fixed scroll 11 without rotating on its own axis.

[0032] An oil reservoir 4 for storing lubricating oil is formed at the bottom of the sealed container 1. In the example shown in FIG. 1, the inside of the bottom lid 1b serves as the oil reservoir 4. A volumetric oil pump 5 is provided at the lower end of the rotating shaft 13. The oil pump 5 is arranged so that its suction port is located within the oil reservoir 4. The oil pump 5 is driven by the rotating shaft 13 and appropriately sucks up the lubricating oil in the oil reservoir 4 provided at the bottom of the sealed container 1 regardless of pressure conditions, operating speed, or the like, thereby avoiding the risk of running out of oil.

[0033] A rotating shaft oil supply hole 13c is provided in the rotating shaft 13. The rotating shaft oil supply hole 13c is formed so as to extend from the lower end portion 13b of the rotating shaft 13 to the eccentric shaft 13a. The lubricating oil sucked up by the oil pump 5 is supplied through the rotating shaft oil supply hole 13c formed in the rotating shaft 13 to the bearing of the sub-bearing 18, the bearing portion 31, and the boss portion 12c.

[0034] The refrigerant sucked through the refrigerant suction pipe 2 is guided from the suction port 15a to the compression chamber 15. The compression chamber 15 moves from the outer periphery toward the center while decreasing in volume. When the refrigerant reaches a predetermined pressure in the compression chamber 15, it is discharged from the discharge port 14 provided in the center of the fixed scroll 11 into the discharge chamber 6.

[0035] A discharge reed valve (not shown) is provided at the discharge port 14. When the refrigerant reaches a predetermined pressure in the compression chamber 15, the discharge reed valve is pushed open and the refrigerant is discharged into the discharge chamber 6. The refrigerant discharged into the discharge chamber 6 is led to the upper part of the sealed container 1 and discharged from the refrigerant discharge pipe 3.

[0036] The scroll compressor having the above-described configuration includes a plurality of sliding parts, such as a combination of sliding members including the fixed scroll 11 and the orbiting scroll 12, or the eccentric shaft 13a of the rotary shaft 13 and the eccentric bush 33.

[0037] In this embodiment, the fixed scroll 11 and the orbiting scroll 12, which are sliding members, are both formed of a non-ferrous base material (base material 11d of the fixed scroll 11 is shown in FIG. 1) having a hardness of HV50 to 200. Specific examples of non-ferrous base materials include, but are not limited to, aluminum alloys (e.g., various aluminum (Al)-silicon (Si)-based alloys of the 4000 series). The specific gravity of the aluminum alloy is 2.6 to 2.8 g / cm. 3 However, the present invention is not limited to this.

[0038] The hardness HV is the result of multi-point measurement based on the Vickers hardness test method specified in JIS Z2244. The same applies to the hardness HV described below. The test method specified in JIS Z2244 can be replaced by the national standards or international standards of each country.

[0039] In addition, the fixed scroll 11 and the orbiting scroll 12 of this embodiment are each subjected to a surface treatment for hardening the surface. For example, if the orbiting scroll 12 is made of an aluminum alloy, an anodized film (alumite film) having a hardness of, for example, HV200 to 300, which is harder than the base material, is formed on the surface of the orbiting scroll 12. The surface treatment for hardening is not limited to this, and a known method is used according to the material of the base material.

[0040] A surface treatment film (hard coating) including a mixed layer laminated on the surface of the substrate 11d and a nickel coating layer laminated on the mixed layer is formed on the substrate 11d of one of the fixed scrolls 11. In the present disclosure, only the nickel coating layer may be regarded as a hard coating (single-layer hard coating), or the nickel coating layer and the lower mixed layer may be regarded as a hard coating (composite hard coating), and the composite hard coating may include other known layers as necessary in addition to the nickel coating layer and the mixed layer.

[0041] A representative example of the composite hard coating is shown in Fig. 2. Fig. 2 is an enlarged schematic cross-sectional view of a mixed layer 41a and a nickel coating layer 41b formed on a base material 11d of the fixed scroll 11. The mixed layer 41a may be composed of at least nickel, a component of the base material 11d, and phosphorus (or, as described below, phosphorus and / or boron). As described below, it is believed that the mixed layer 41 formed below the nickel coating layer 41b has been revealed for the first time by this disclosure.

[0042] In this embodiment, since the base material 11d of the fixed scroll 11 is aluminum, the mixed layer 41a is composed of aluminum (Al), which is the main component of the base material 11d, nickel (Ni), and phosphorus (P). The nickel coating layer 41b formed above the mixed layer 41a (on the surface side, the same applies below) is a single-layer hard coating mainly composed of nickel. Note that the main component here means 80 wt% or more of all components. Also, the content or concentration in this specification does not include known impurities (the inclusion of known impurities can be substantially ignored).

[0043] In Fig. 2, the mixed layer 41a is shown as being alternately arranged with a "substrate component portion 41c" made of aluminum (Al), which is the main component of the substrate 11d, and a "coating layer component portion 41d" made of nickel (Ni) and (P). The illustration in Fig. 2 is a schematic illustration for making the mixed layer 41a easier to understand, and the mixed layer 41a in the present disclosure is not limited to this illustration.

[0044] The mixed layer 41a and the nickel coating layer 41b can be formed by, for example, electroless nickel-phosphorus plating. Note that in this specification, wt% (weight %) can be replaced with mass% (mass %).

[0045] The nickel coating layer 41b contains nickel and phosphorus if it is obtained by electroless nickel-phosphorus plating. The phosphorus concentration (phosphorus content) contained in the nickel coating layer 41b is 8 to 10 wt%, with the remainder being nickel (nickel content 90 to 92 wt%). As will be described later, in a representative example of this embodiment, the surface hardness of the nickel coating layer 41b was HV550 to 600.

[0046] 3A and 3B are examples of cross-sectional EDS (Energy Dispersive X-ray Spectroscopy) element mapping of the vicinity of the interface of the base material 11d of the fixed scroll 11 in a representative example of the present embodiment.

[0047] 3A, a slightly light black area (nickel coating layer 41b in the figure), a region where slightly light black areas and dark black areas are mixed (mixed layer 41a in the figure), and a dark black area below that (11d in the figure) are confirmed. Nickel (Ni) is present in the slightly light black area at the top, and aluminum (Al), an element other than nickel, is mainly present in the dark black area at the bottom.

[0048] In the EDS element mapping (phosphorus: P) shown in Figure 3B, the upper light grey area is almost the same as the slightly light black area in Figure 3B. Phosphorus (P) is present in the light grey area, and aluminum (Al) is also present mainly in the lower black area.

[0049] By performing EDS element mapping while observing the cross section of the substrate 11d of the fixed scroll 11 with a SEM (scanning electron microscope) or a TEM (transmission electron microscope) based on Figures 3A and 3B, it is possible to easily recognize that a mixed layer 41a composed of nickel (Ni), aluminum (Al) which is the main component of the substrate 11d, and phosphorus (P) is formed above the substrate 11d (mainly aluminum), and a nickel coating layer 41b mainly composed of nickel (Ni) is formed above the mixed layer 41a.

[0050] Furthermore, aluminum (Al) is hardly present in the region where nickel (Ni) and phosphorus (P) are present. From these results, it can be seen that the mixed layer 41a is not constituted as a compound of the components of the nickel coating layer 41b (nickel and phosphorus) and the components of the base material 11d (aluminum), but rather nickel (Ni), phosphorus (P), and aluminum (Al) are individually and independently constituted.

[0051] In addition, from these results, nickel (Ni) and phosphorus (P) are distributed as if they are eroding from the interface 11e of the base material 11d (aluminum alloy) into the inside of the base material 11d and spreading their roots. The thickness of the mixed layer 41a in this embodiment was about 600 nm at maximum.

[0052] That is, as is clear from the above-described representative examples, in the slide member according to the present disclosure, a mixed layer composed of at least nickel, aluminum (a component of the substrate 11d), and phosphorus is formed under the nickel coating layer, and this mixed layer can be diagrammed as a configuration in which a "substrate component portion 41c" composed of aluminum (a component of the substrate 11d) and a "coating layer component portion 41d" composed of nickel (Ni) and (P) are alternately arranged, as shown in FIG. 2.

[0053] The specific configuration of the scroll compressor having the above configuration is not particularly limited, and various known configurations can be suitably used. For example, the scroll compressor may be horizontally placed, and the base material of the orbiting scroll 12 may be iron-based. In addition, the scroll compressor is not limited to a scroll compressor, and may be a reciprocating compressor, a rotary compressor, or the like.

[0054] [1-2. Operation] The operation and function of the scroll compressor constructed as above will now be described.

[0055] In the scroll compressor having the above-described structure, a surface treatment film harder than the base material 11d is formed on the surface of the base material 11d of the fixed scroll 11, the base material 11d being made of an aluminum alloy.

[0056] In this embodiment, the surface hardness of the nickel coating layer 41b of the substrate 11d of the fixed scroll 11 is 4 to 12 times that of the substrate 11d. Here, if a hard surface treatment film is formed directly on the surface of the substrate, the difference in hardness between the aluminum substrate and the surface treatment film, that is, the difference in mechanical strength, becomes excessive, as already described. Therefore, when a shear force acts in a direction parallel to the interface due to frictional sliding, the hard surface treatment film peels off at the interface, and destruction such as "pulling" occurs involving the substrate immediately below the interface. As a result, the hard surface treatment film is chipped, and the aluminum substrate is exposed between the sliding surfaces.

[0057] In this embodiment, a configuration is adopted in which a mixed layer 41a composed of aluminum (Al), which is the main component of the substrate 11d, nickel (Ni), and phosphorus (P), and a nickel coating layer 41b composed mainly of nickel (Ni) are formed on the mixed layer 41a.

[0058] As a result, even if a shear force due to sliding acts, the mixed layer 41a formed by the components (nickel, phosphorus) of the nickel coating layer 41b penetrating into the base material 11d acts like a nail or a wedge, exhibiting a so-called anchor effect. Therefore, even if there is a large difference in hardness between the base material 11d and the surface treatment film, peeling or destruction of the coating near the interface 11e of the base material 11d is avoided or suppressed, and sufficient coating adhesion can be ensured. As a result, the wear resistance of the nickel coating layer 41b is fully exhibited, thereby improving the long-term reliability of the compressor.

[0059] In this embodiment, the surface hardness of the nickel coating layer 41b of the substrate 11d is set to 4 to 12 times the hardness of the substrate 11d. From the experimental efforts made by the present inventors so far, it has become clear that if the hardness of the nickel coating layer 41b is 6 times or more the hardness of the substrate 11d, a more remarkable anchor effect can be obtained.

[0060] On the other hand, since the surface hardness of the counterpart orbiting scroll 12 is lower than that of the fixed scroll 11, the surface of the orbiting scroll 12 wears and becomes familiar with the surface during operation of the compressor. That is, the tip protrusions (peaks) of the roughness of the sliding surface are truncated and flattened, thereby reducing the local contact surface pressure and easing the sliding state. This significantly prevents wear from progressing beyond the appropriate level.

[0061] In this embodiment, the nickel coating layer 41b is formed by electroless nickel-phosphorus plating, and the phosphorus concentration in the nickel coating layer 41b is set to 8 to 10 wt %.

[0062] As a representative comparative example for this embodiment, an example of cross-sectional EDS elemental mapping of a nickel coating layer 41b formed by electroless nickel-phosphorus plating treatment with a phosphorus concentration of less than 2 wt % near the substrate interface is shown in FIGS. 4A and 4B.

[0063] In the EDS element mapping (nickel: Ni) shown in Figure 4A, there is a slightly light black area from the top (41b in the figure), and a dark black area just below it (11d in the figure). Nickel (Ni) is present in the slightly light black area at the top, and aluminum (Al), an element other than nickel, is mainly present in the dark black area at the bottom.

[0064] The EDS elemental mapping (phosphorus: P) shown in Figure 4B shows that the light grey area is almost the same as the light black area in Figure 4A. The EDS elemental mapping (phosphorus: P) shows that phosphorus (P) is present in the upper light grey area, and aluminum (Al) is also present mainly in the lower black area.

[0065] As is clear from Figures 4A and 4B, in the comparative example, the mixed layer 41a as shown in Figures 3A and 3B, as in the above-mentioned embodiment, cannot be confirmed, and it can be recognized that a nickel coating layer 41b made of nickel (Ni) and phosphorus (P) is directly formed above the substrate 11d.

[0066] From the above results, in the present disclosure, it has been clarified that, with regard to the nickel coating layer 41b formed in the electroless nickel-phosphorus plating process, if the phosphorus concentration is low, the mixed layer 41a is not formed.

[0067] FIG. 5 shows the relationship between the phosphorus concentration in the nickel coating layer 41b and the maximum thickness of the mixed layer 41a, which was obtained from the experimental efforts of the present inventors.

[0068] By increasing the phosphorus concentration in the nickel coating layer 41b to more than 3 wt%, the maximum thickness of the mixed layer 41a becomes 100 nm or more. As a result, even if a shear force acts in a direction parallel to the interface 11e due to frictional sliding, the mixed layer 41a formed by the components (nickel, phosphorus) of the nickel coating layer 41b penetrating into the base material 11d exhibits an anchor effect. Therefore, even if there is a large difference in hardness between the base material 11d and the surface treatment film, peeling or destruction of the coating near the interface 11e can be avoided or suppressed, and sufficient coating adhesion can be ensured.

[0069] According to the intensive study of the present inventors, when the phosphorus concentration in the nickel coating layer 41b is higher than 3 wt%, the nickel coating layer 41b tends to be relatively hard and has low durability, but tends to have high adhesion to the interface of the substrate 11d. On the other hand, when the phosphorus concentration in the nickel coating layer 41b is low, ie, 3 wt% or less, the nickel coating layer 41b tends to be relatively hard and has high durability, but tends to have low adhesion to the interface of the substrate 11d.

[0070] This disclosure has revealed for the first time that in electroless nickel-phosphorus plating formed on sliding members (particularly sliding members for refrigerant compressors), the minimum phosphorus concentration that can further improve the adhesion of the substrate 11d is clarified, and that a mixed layer 41a is formed between the substrate 11d and the nickel coating layer 41b, and that this mixed layer 41a can increase the adhesion of the nickel coating layer 41b.

[0071] This allows the nickel coating layer 41b formed on the slide member to achieve better adhesion to the substrate 11d, and the nickel coating layer 41b itself to maintain excellent durability. As a result, the slide member according to the present disclosure can be widely and suitably used in the field of compressors, which require long-term reliability.

[0072] As described above, in order to form the mixed layer 41a, it is sufficient to set the phosphorus concentration in the nickel coating layer 41b to 3 wt % or more. In order to form such a surface treatment film, for example, the bath make-up temperature in the electroless nickel-phosphorus plating process can be set to a range of 80 to 100°C.

[0073] If the bath make-up temperature is lower than 80°C, depending on various conditions, the plating speed may become too slow, resulting in uneven deposition (a phenomenon in which the plating film (nickel coating layer 41b) is formed only in places). On the other hand, if the bath make-up temperature is higher than 100°C, depending on various conditions, the plating speed may become too fast, resulting in large variations in the thickness of the plating film (nickel coating layer 41b), and the thickness of the mixed layer 41b may exceed 1000 nm or the component ratio of the base material 11d in the mixed layer 41b may decrease significantly.

[0074] In this way, if the plating speed is increased or decreased depending on the bath make-up temperature, it may affect the formation of a good mixed layer 41a in particular, and as a result, the obtained surface treatment film may not have sufficient peel resistance.

[0075] In particular, in fields such as compressors where long-term reliability is required, the bath make-up temperature can be set within a range of 85 to 95° C. Although it depends on various conditions, if the bath make-up temperature is within this range, a better mixed layer 41a can be easily formed, and the peeling resistance of the surface treatment film can be improved.

[0076] As described above, the preferred range of the bath make-up temperature is set primarily to achieve a good plating formation rate. Therefore, in the present disclosure, the bath make-up temperature in the electroless nickel-phosphorus plating process for forming a surface treatment film (a film having the nickel coating layer 41b and the mixed layer 41a) on the substrate 11d is not necessarily limited to the above range, and a bath make-up temperature outside the above range may be adopted depending on various conditions. Furthermore, in the present disclosure, other known conditions in the electroless nickel-phosphorus plating process may also be set within the preferred range.

[0077] In this manner, in the present disclosure, by following the conventional electroless nickel-phosphorus plating process and adjusting the phosphorus concentration in the nickel coating layer 41b to a predetermined value (higher than 3 wt%) to form the nickel coating layer 41b, the surface treatment film according to the present disclosure (composite hard film including the mixed layer 41a and the nickel coating layer 41b) can be formed. Therefore, there is no need to add a process such as shot blasting for roughening the surface of the untreated base material 11d in advance, and a general electroless nickel-phosphorus plating process can be used, so that the surface treatment film can be formed at low cost, and the base material 11d on which the surface treatment film is formed, i.e., the slide member according to the present disclosure, is also very excellent in terms of mass productivity.

[0078] In this embodiment (this disclosure), the mixed layer 41a may have a thickness of 100 nm or more and 1000 nm or less.

[0079] If the thickness of the mixed layer 41a is less than 100 nm, it is difficult to obtain a sufficient anchor effect as described above. On the other hand, if the phosphorus concentration of the nickel coating layer 41b is increased, the thickness of the mixed layer 41a will inevitably increase. However, if the phosphorus concentration is 15 wt% or more, the hardness of the nickel coating layer 41b will decrease, and it may be difficult to ensure high wear resistance. From the viewpoint of ensuring wear resistance, the phosphorus concentration is preferably 15 wt% or less, and the thickness of the mixed layer 41a at a phosphorus concentration of 15 wt% will be approximately 1000 nm. Therefore, the thickness of the mixed layer 41a is preferably 1000 nm or less.

[0080] In this embodiment, the base material of the sliding member is an aluminum (Al)-silicon (Si) alloy, and the specific gravity of the base material is 3.0 g / cm 3 Even if a soft non-ferrous material having a hardness of HV50 to 200 is used, the same effects as those of the above-mentioned aluminum-silicon alloy can be obtained.

[0081] For example, in the case of aluminum alloys, aluminum (Al)-copper (Cu)-magnesium (Mg) system (2000 series, etc.), aluminum (Al)-magnesium (Mg) system (5000 series), aluminum (Al)-magnesium (Mg)-silicon (Si) system (6000 series), aluminum (Al)-zinc (Zn)-magnesium (Mg) system (7000 series), and lithium (Li)-added aluminum alloys (8000 series, etc.) that have aluminum (Al) as the main component can also provide the same effects as the aluminum-silicon alloys described above.

[0082] Furthermore, if the magnesium alloy contains magnesium (Mg) as the main component, for example, a magnesium (Mg)-aluminum (Al)-zinc (Zn) based alloy, the same effects as those of the above-mentioned aluminum-silicon based alloy can be obtained.

[0083] [1-3. Effects, etc.] As described above, in the present embodiment, the sliding member is configured to include the substrate 11d, the mixed layer 41a constituted of at least nickel and components of the substrate 11d, in this embodiment, aluminum and phosphorus, and the nickel coating layer 41b mainly composed of nickel provided above the mixed layer 41a.

[0084] This allows the sliding member to have sufficient coating adhesion in addition to the seizure prevention provided by the hard coating treatment, making it possible to avoid damage or peeling of the coating near the substrate interface caused by the difference in hardness between the substrate 11d and the hard coating (nickel coating layer 41b).

[0085] In the present disclosure, including the second embodiment described later, the slide member may include components other than the base material 11d, the mixed layer 41a, and the nickel coating layer 41b. That is, the slide member according to the present disclosure may have any configuration as long as it includes the base material 11d, the mixed layer 41a, and the nickel coating layer 41b.

[0086] Also, as in this embodiment, the mixed layer 41a may be configured such that the component of the nickel coating layer 41b and the component of the base material 11d exist independently.

[0087] As a result, the mixed layer 41a formed by the components (nickel, phosphorus) of the nickel coating layer 41b penetrating into the substrate 11d fully exhibits the so-called anchor effect, acting like a nail or wedge, thereby significantly improving the adhesion of the coating.

[0088] Also, like in this embodiment, the mixed layer 41a may have a thickness of 100 nm or more and 1000 nm or less.

[0089] This makes it possible to obtain a sliding member that combines the anchor effect of the mixed layer 41a formed by the components (nickel, phosphorus) of the nickel coating layer 41b penetrating into the base material 11d, with the high wear resistance of the nickel coating layer 41b.

[0090] The nickel coating layer 41b may be formed by electroless nickel-phosphorus composite plating, in which the nickel coating layer 41b may have a phosphorus concentration of more than 3 wt %.

[0091] This makes it possible to form a surface treatment film consisting of the nickel coating layer 41b and the mixed layer 41a as in this embodiment by following the conventional electroless nickel-phosphorus plating process in which the phosphorus concentration in the nickel coating layer 41b is adjusted to a predetermined value (higher than 3 wt%). Therefore, there is no need to add a process such as roughening the surface of the base material 11d in advance, and excellent mass productivity can be achieved.

[0092] The nickel coating layer 41b may have a thickness of 2 μm or more.

[0093] This allows the components (nickel, phosphorus) of the nickel coating layer 41b to penetrate into the base material 11d, forming the mixed layer 41a, which has a sufficient anchoring effect, and makes it possible to provide a sliding member with high long-term reliability. It is also possible to select an appropriate film thickness depending on various conditions such as the application, operating conditions, and operating time.

[0094] The substrate may be made of an alloy containing aluminum as a main component and having a hardness of HV50 to 200. This allows for a lightweight sliding member having both high wear resistance and high peeling resistance.

[0095] On the other hand, a compressor constructed using the above-mentioned sliding member includes a compression mechanism that compresses a refrigerant, an electric mechanism that drives the compression mechanism, and a sealed container that houses the compression mechanism and the electric mechanism and has an oil reservoir at the bottom that retains lubricating oil, and includes a sliding part using the sliding member of the above-mentioned configuration, i.e., the sliding member of the above-mentioned configuration is disposed in at least one of the sliding parts.

[0096] As a result, by having a sliding member that has both high self-wear resistance and coating adhesion, it is possible to avoid or suppress performance degradation or malfunction caused by wear or peeling in the sliding parts of the compressor, and the compressor can be operated stably over a long period of time while maintaining high performance.

[0097] Furthermore, by configuring a refrigeration device with this compressor, it is possible to not only increase the efficiency of the refrigeration device, but also significantly improve the reliability. The specific configuration of the refrigeration device according to the present disclosure is not limited, and it may be configured to include a known refrigerant circuit (refrigeration cycle) including the compressor according to the present disclosure. The specific configuration of the refrigeration device is also not particularly limited, and it may be a known refrigeration device such as an air conditioner, a water heater, or a refrigerator.

[0098] The compression mechanism may include a fixed scroll, a revolving scroll, and a rotating shaft that drives the revolving scroll to revolve, and the sliding member may be used for at least one of the fixed scroll and the revolving scroll, i.e., the sliding portion of at least one of the process scroll and the revolving scroll may include the sliding member having the above-mentioned configuration.

[0099] As a result, the long-term reliability of the scroll compressor can be improved by providing sliding members that have both high self-wear resistance and coating adhesion. Furthermore, by using aluminum, which has a low specific gravity, for the base material of the fixed scroll or the orbiting scroll, a significant weight reduction can be achieved. Therefore, a scroll compressor that can be applied to fields where weight reduction is desired, such as vehicle-mounted types, can be provided.

[0100] In addition, by reducing the weight of the orbiting scroll, the centrifugal force acting on the compression mechanism is reduced, and vibration of the compressor during operation can be suppressed. This allows for increased refrigeration capacity through faster rotation. Furthermore, the radial load acting on the rotating shaft is reduced, making it possible to change the design to reduce the diameter of the rotating shaft. This makes it possible to provide a scroll compressor with high product appeal, with high efficiency due to reduced input loss, and a more compact compressor.

[0101] Furthermore, the compressor of the present invention may be configured to use a working medium such as R134a, R32, R410A, R407C, isobutane, propane, carbon dioxide, or a refrigerant having a double bond between carbon atoms.

[0102] This effectively prevents or prevents the sliding members disposed in the compressor from being altered or deformed when exposed to any of the refrigerants, and allows the compressor to stably exhibit high self-wear resistance and coating adhesion over a long period of time.

[0103] In addition, the sliding members disposed in the compressor can be effectively prevented from being altered or deformed even when exposed to substances generated by decomposition of the refrigerant during the sliding process (e.g., fluorides found in refrigerants having double bonds between carbon atoms), allowing the compressor to stably exhibit high self-wear resistance and coating adhesion over a long period of time.

[0104] (Embodiment 2) Hereinafter, the second embodiment will be described with reference to Figures 6 to 7B, with reference to Figures 1 to 5 as appropriate. Also, the same components as those described with reference to Figures 1 to 5 will be given the same reference numerals, and some of the description will be omitted.

[0105] [2-1. Configuration] In this embodiment, the fixed scroll 11 and the orbiting scroll 12, which are sliding members, are both formed, for example, from a non-ferrous material having a hardness of HV50 to 200. Specific examples of non-ferrous material substrates include, but are not limited to, aluminum alloys (for example, various aluminum (Al)-silicon (Si)-based alloys of the 4000 series). The specific gravity of the aluminum alloy is 2.6 to 2.8 g / cm. 3 However, the present invention is not limited to this.

[0106] In addition, the fixed scroll 11 and the orbiting scroll 12 of this embodiment are each subjected to a surface treatment for hardening the surface. For example, if the orbiting scroll 12 is made of an aluminum alloy, an anodized film (alumite film) having a hardness of, for example, HV200 to 300, which is harder than the base material 11d, is formed on the surface of the orbiting scroll 12. The surface treatment for hardening is not limited to this, and a known method is used according to the material of the base material 11d.

[0107] A surface treatment film including a mixed layer laminated on the surface of the base material 11d and a nickel coating layer laminated on the mixed layer is formed on the base material 11d of one of the fixed scrolls 11, as in the first embodiment. A representative example of the surface treatment film in this embodiment is shown in Fig. 6. Fig. 6 is an enlarged cross-sectional schematic diagram of a mixed layer 51a, a first nickel coating layer 51b, and a second nickel coating layer 51c formed on the base material 11d of the fixed scroll 11.

[0108] In this embodiment, since the base material 11d of the fixed scroll 11 is aluminum, the mixed layer 51a is composed of aluminum (Al), which is the main component of the base material 11d, nickel (Ni), and phosphorus (P). A first nickel coating layer 51b is formed above the mixed layer 41a, and a second nickel coating layer 51 is formed further above (on the outermost surface side of) the first nickel coating layer 51b.

[0109] The first nickel coating layer 51b and the second nickel coating layer 51c are both single-layer hard coatings mainly composed of nickel. These nickel coating layers 51b and 51c constitute a multi-layer nickel coating layer 51d. The multi-layer nickel coating layer 51d may be composed of three or more layers, and each layer may have a different component (nickel concentration, phosphorus concentration, etc.).

[0110] 6, similarly to FIG. 2 referred to in the first embodiment, the mixed layer 51a is shown as being alternately arranged with a "substrate component portion 51e" made of aluminum (Al), which is the main component of the substrate 11d, and a "coating layer component portion 51f" made of nickel (Ni) and (P). The illustration in FIG. 6 is a schematic illustration similar to FIG. 2, and the mixed layer 51a in the present disclosure is not limited to this illustration.

[0111] The first nickel coating layer 51b and the second nickel coating layer 51c are both formed by electroless nickel-phosphorus plating. In this embodiment, the first nickel coating layer 51b has a phosphorus concentration (phosphorus content) of 8 to 10 wt%, with the remainder being made up almost entirely of nickel (nickel content of 90 to 92 wt%), while the second nickel coating layer 51c has a phosphorus concentration of 1 to 3 wt%, with the remainder being made up almost entirely of nickel (nickel content of 97 to 99 wt%). This content does not include known impurities.

[0112] In a representative example of this embodiment, in order to stably form a multi-layered plating film layer, a zincate treatment was performed in advance to form a zinc film on the surface of the base material 11d. The zinc film formed in this pretreatment process was replaced with nickel in an electroless plating solution for the first nickel film layer 51b to form a first nickel film layer 51b (plating film). Subsequently, the base material was immersed in an electroless plating solution for the second nickel film layer 51c to form a second nickel film layer 51c. In this way, a multi-layered nickel film layer 51d was produced (manufactured) as shown in FIG. 6.

[0113] The hardness of the produced multi-layer nickel coating layer 51d was measured according to JIS Z2244 using a nanoindentation device TI-950 Triboindenter (product name) manufactured by Hysitron Corp. The hardness of the first nickel coating layer 51b was HV550-600, and the hardness of the second nickel coating layer 51c was HV650-700.

[0114] It is generally known that the lower the phosphorus concentration, the harder the nickel coating layer tends to be. That is, by performing plating treatments with different phosphorus concentrations multiple times, it is possible to form a multi-layered plating layer in which the hardness of each layer is controlled in stages. In this embodiment, the multi-layered nickel coating layer 51d is formed by performing two plating treatments, but as described above, it may be a multi-layered nickel coating layer of three or more layers.

[0115] 7A and 7B are examples of cross-sectional EDS element mapping of the vicinity of the interface 11e of the base material 11d of the fixed scroll 11 in a representative example of the present embodiment.

[0116] In the EDS element mapping (nickel: Ni) shown in Figure 7A, from the top there are slightly light black areas (51b and 51c in the figure), and below that there is a region where slightly light black areas and dark black areas are mixed (51a in the figure). Nickel (Ni) exists in the slightly light black areas, while aluminum (Al), an element other than nickel, mainly exists in the dark black areas.

[0117] In the EDS element mapping (phosphorus: P) shown in FIG. 7B, the area shown in light gray is almost the same as the area shown in FIG. 4A, which is a comparative example and described in the first embodiment, and which is shown in a slightly light black color.

[0118] In Figure 7B, phosphorus (P) is present in the light gray area, and aluminum (Al) is mainly present in the lower black area. Also, the upper gray area (51c in the figure) has a different color tone compared to the lower gray area (51b in the figure). This indicates the difference in phosphorus concentration, and indicates that the phosphorus concentration in the upper dark area (51c in the figure) is lower than that of the lower area (51b in the figure).

[0119] 7A and 7B, by observing the cross section of the substrate 11d of the fixed scroll 11 with an SEM or TEM while performing EDS element mapping, it is possible to easily recognize that a mixed layer 51a composed of nickel (Ni) and aluminum (Al) and phosphorus (P), which are the main components of the substrate 11d, is formed above the substrate 11d (not shown), and that a first nickel coating layer 51b composed mainly of nickel (Ni) and a second nickel coating layer 51c are formed above the mixed layer 51a.

[0120] Furthermore, aluminum (Al) is not present in the region where nickel (Ni) and phosphorus (P) are present. This shows that the mixed layer 51a is not composed of the components (nickel and phosphorus) of the first nickel coating layer 51b and the second nickel coating layer 51c and the component (aluminum) of the base material 11d as a compound, but rather nickel (Ni), phosphorus (P) and aluminum (Al) are individually and independently composed.

[0121] In addition, from these results, nickel (Ni) and phosphorus (P) are seen to have penetrated into the substrate 11d (aluminum alloy) from the interface 11e and are distributed as if taking root. The thickness of the mixed layer 51a is not shown, but is approximately 600 nm at maximum.

[0122] That is, as is clear from the representative examples described above, in the slide member according to the present disclosure, a mixed layer composed of at least nickel, aluminum (a component of the substrate 11d), and phosphorus is formed under the nickel coating layer, and this mixed layer can be diagrammed as a configuration in which a "substrate component portion 51e" composed of aluminum (a component of the substrate 11d) and a "coating layer component portion 51f" composed of nickel (Ni) and (P) are alternately arranged, as shown in FIG. 6.

[0123] Here, in the present embodiment as well, in order to form the mixed layer 51a, as in the first embodiment, it is sufficient to set the phosphorus concentration in at least the first nickel coating layer 51b to 3 wt % or more, preferably 8 to 10 wt %, as described above. In this case, too, as in the first embodiment, for example, the make-up bath temperature in the electroless nickel-phosphorus plating process can be set within a suitable range.

[0124] Furthermore, in this embodiment, the phosphorus concentration of the nickel film on the top surface (or outermost surface), i.e., the second nickel film 51c, is set to 1 to 3 wt%, which is lower than that of the first nickel film 51b (the nickel film in contact with the mixed layer 51a, the nickel film on the innermost surface) in contact with the base material 11d. To form a nickel film with such a low phosphorus concentration, the make-up bath temperature in the electroless nickel-phosphorus plating process can be set within the range of 60 to 100°C.

[0125] If the bath make-up temperature is lower than 60°C, depending on various conditions, the plating speed becomes too slow, which may result in uneven deposition (a phenomenon in which the plating film (second nickel coating layer 51c) is formed only in places). On the other hand, if the bath make-up temperature is higher than 100°C, depending on various conditions, the plating speed becomes too fast, which makes it difficult to control the stable film thickness during mass production. In addition, if the second nickel coating layer 51c is not formed well, it may also affect the first nickel coating layer 51b or mixed layer 51a located below it.

[0126] Particularly in fields such as compressors where long-term reliability is required, the bath make-up temperature for forming the nickel coating that will be the outermost surface can be set within a range of 70 to 95° C. Although it depends on various conditions, if the bath make-up temperature is within this range, the physical properties of the surface treatment film including the multiple nickel coatings and the mixed layer 51a can be further improved.

[0127] [2-2. Operation] The operation and function of the scroll compressor constructed as above will now be described.

[0128] In the scroll compressor having the above-described structure, a surface treatment film harder than the base material 11d is formed on the surface of the base material 11d of the fixed scroll 11, the base material 11d being made of an aluminum alloy.

[0129] In this embodiment, the surface hardness of the first nickel coating layer 51b of the base material 11d of the fixed scroll 11 is 4 to 12 times that of the base material 11d. Here, if a hard surface treatment film is formed directly on the surface of the base material 11d, the difference in hardness between the aluminum base material and the surface treatment film, i.e., the difference in mechanical strength, becomes excessive. Therefore, when a shear force acts in a direction parallel to the interface due to frictional sliding, the hard surface treatment film peels off at the interface, or destruction such as "pulling" occurs involving the base material immediately below the interface. As a result, the hard surface treatment film is chipped, and the aluminum base material is exposed between the sliding surfaces.

[0130] In this embodiment, a configuration is adopted in which a mixed layer 51a composed of aluminum (Al), which is the main component of the base material 11d, nickel (Ni), and phosphorus (P), and a first nickel coating layer 51b composed mainly of nickel are formed above the mixed layer 51a.

[0131] As a result, even if a shear force due to frictional sliding acts, the mixed layer 51a formed by the components (nickel, phosphorus) of the first nickel coating layer 51b penetrating into the substrate 11d acts like a nail or a wedge, exhibiting a so-called anchor effect. Therefore, even if there is a large difference in hardness between the substrate 11d and the surface treatment film, peeling or destruction near the interface 11e of the substrate 11d is avoided or suppressed, and sufficient coating adhesion can be ensured.

[0132] In addition, in this embodiment, the second nickel coating layer 51c has a lower phosphorus concentration (1 to 3 wt%) than the first nickel coating layer 51b, which makes the hardness (HV) of the outermost coating layer that slides against the counter material very high, ensuring significantly excellent self-wear resistance.

[0133] On the other hand, since the surface hardness of the counterpart orbiting scroll 12 is lower than that of the fixed scroll 11, the surface of the orbiting scroll 12 wears and becomes familiar with the surface during operation of the compressor. That is, the tip protrusions (peaks) of the roughness of the sliding surface are truncated and flattened, thereby reducing the local contact surface pressure and easing the sliding state. This significantly prevents wear from progressing beyond the appropriate level.

[0134] [2-3. Effects, etc.] As described above, in the present embodiment, the slide member is configured to include the substrate 11d, the mixed layer 51a constituted of at least nickel and components of the substrate 11d, in this embodiment, aluminum and phosphorus, and the first nickel coating layer 51b and the second nickel coating layer 51c, in this embodiment, containing nickel as a main component, above the mixed layer 51a.

[0135] This allows the sliding member to have sufficient coating adhesion to avoid destruction or peeling of the coating near the substrate interface caused by the difference in hardness between the substrate and the hard coating.

[0136] In addition, the nickel coating layer has nickel as its main component, but as described above, it can be a multi-layer nickel coating layer having at least two layers, and the phosphorus concentration of the nickel coating layer on the mixed layer side can be higher than the phosphorus concentration of the nickel coating layer on the outermost surface side.

[0137] More specifically, the nickel coating layer on the mixed layer side (first nickel coating layer 51b in this embodiment) can have a phosphorus concentration higher than 3 wt%, and the nickel coating layer on the outermost surface side (second nickel coating layer 51c in this embodiment) can have a phosphorus concentration of 3 wt% or less.

[0138] This allows the sliding member to have sufficient coating adhesion in addition to the seizure prevention provided by the hard coating treatment. This makes it possible to avoid damage or peeling of the coating near the substrate interface caused by the difference in hardness between the substrate and the hard coating. Moreover, in addition to the seizure prevention and coating adhesion, the nickel coating layer on the outermost surface side can also have sufficient self-wear resistance.

[0139] In addition, in the present embodiment and the above-described embodiment 1, the nickel coating layer is configured to contain phosphorus, but according to the inventors' efforts to date, the present disclosure is not limited to the incorporation of phosphorus, and boron may also be incorporated.

[0140] The nickel coating layer containing boron, and further the nickel coating layer containing both phosphorus and boron, can obtain excellent adhesion strength and self-wear resistance similar to the nickel coating layer containing phosphorus. Therefore, the mixed layer only needs to contain at least one of phosphorus and boron in addition to the components of nickel and the base material.

[0141] The incorporation of boron into the nickel coating layer can be carried out in the same manner as the incorporation of phosphorus into the nickel coating layer in the above-described first embodiment or this embodiment by using a known method such as electroless nickel-boron composite plating. Therefore, by replacing the incorporation of phosphorus with boron, a person skilled in the art can easily understand the configuration and formation of the nickel coating layer containing boron.

[0142] Furthermore, when the nickel coating layer contains boron instead of phosphorus, or when it contains both phosphorus and boron, the phosphorus concentration described in the first or second embodiment can be replaced with the boron concentration.

[0143] In addition, when the nickel coating layer contains boron, the conditions described in the first embodiment or the second embodiment can be applied to the electroless nickel-boron plating process as they are. Typically, the make-up bath temperature in the electroless nickel-boron plating process can be set in the range of 80 to 100°C, or in the range of 85 to 95°C. Alternatively, in the case of forming a nickel coating in multiple layers as in the second embodiment, the make-up bath temperature can be set in the range of 60 to 100°C, or in the range of 70 to 95°C when forming the nickel coating on the outermost surface side by the electroless nickel-boron plating process. This makes it possible to preferably form a surface treatment film including a mixed layer.

[0144] The nickel coating layer may contain components other than nickel, and the mixed layer may contain components other than nickel and phosphorus, or nickel and boron. The content of such other components is not particularly limited, and may be within a range that does not affect the coating adhesion and self-wear resistance. The nickel coating layer or the mixed layer may contain inevitable impurities in terms of technical common sense, but such inevitable impurities can be ignored as components of the nickel coating layer and the mixed layer. Therefore, the lower limit of the content of the other components may be an amount that exceeds the inevitable impurities.

[0145] In the above-described embodiments, the sliding member according to the present disclosure has been described as a compressor that compresses a refrigerant as a working medium, but it may be a compressor that compresses a working medium other than a refrigerant. Alternatively, the sliding member according to the present disclosure can obtain the same effect not only when used in a compressor but also in an engine of a car. Therefore, it can be applied to a compressor that does not use a refrigerant as a working medium.

[0146] In this manner, the slide member according to the present disclosure can suppress damage or peeling of the coating near the substrate interface and ensure sufficient coating adhesion, thereby improving the long-term reliability when used to configure a sliding part.

[0147] In addition, since the compressor according to the present disclosure is provided with the sliding member, reliability and efficiency are improved, and the compressor is useful for refrigeration devices using a refrigeration cycle, such as a freezer-refrigerator, a hot water heating device, an air conditioner, a water heater, or a refrigerator.

[0148] From the above description, many improvements and other embodiments of the present invention will be apparent to those skilled in the art. Therefore, the above description should be construed as merely illustrative and is provided for the purpose of teaching those skilled in the art the best mode for carrying out the present invention. Details of the structure and / or function thereof may be substantially changed without departing from the spirit of the present invention. [Industrial Applicability]

[0149] INDUSTRIAL APPLICABILITY The present invention can be suitably used widely in the field of sliding members, and in particular in the field of compressors such as refrigerant compressors, or in the field of refrigeration cycles using such compressors, and further in fields having sliding parts similar to those of compressors. [Explanation of symbols]

[0150] 1: Airtight container 4: Oil storage section 10: Compression mechanism 11: Fixed scroll 11a: Fixed scroll head 11b: Fixed spiral wrap 11d: Base material 12: Rotating Scroll 12a: Rotating scroll head plate 12b: Swirling swirl wrap 13: Rotation axis 20: Electric mechanism section 41a, 51a: Mixed layer 41b: Nickel coating layer 51b First nickel coating layer 51c Second nickel coating layer 51d: Double-layer nickel coating layer (nickel coating layer)

Claims

1. A substrate; A mixed layer composed of at least nickel, a component of the base material, and phosphorus and / or boron; a nickel coating layer containing nickel, phosphorus and / or boron on the mixed layer; It is equipped with The mixed layer is configured so that a component of the nickel coating layer and a component of the substrate exist independently. Sliding member.

2. The mixed layer is formed by the components of the nickel coating layer penetrating into the substrate. The sliding member according to claim 1 .

3. The mixed layer has a thickness of 100 nm or more and 1000 nm or less. The sliding member according to claim 1 or 2.

4. The nickel coating layer has a phosphorus concentration or a boron concentration of more than 3 wt %. The sliding member according to claim 1 .

5. When the nickel coating layer is at least two layers, The phosphorus concentration or boron concentration of the nickel coating layer on the mixed layer side is higher than the phosphorus concentration or boron concentration of the nickel coating layer on the outermost surface side. The sliding member according to claim 1 .

6. The nickel coating layer on the mixed layer side has a phosphorus concentration or a boron concentration higher than 3 wt %. The sliding member according to claim 5 .

7. The nickel coating layer on the outermost surface side has a phosphorus concentration or a boron concentration of 3 wt % or less. The sliding member according to claim 5 or 6.

8. The nickel coating layer is electroless nickel-phosphorus composite plating or electroless nickel-boron composite plating. The sliding member according to claim 1 .

9. The nickel coating layer has a thickness of 2 μm or more. The sliding member according to claim 1 .

10. The substrate is an alloy mainly composed of aluminum and has a hardness of HV50 to 200. The sliding member according to claim 1 .

11. a compression mechanism for compressing a refrigerant; an electric mechanism that drives the compression mechanism; a sealed container that houses the compression mechanism and the electric mechanism and has an oil reservoir at the bottom that stores lubricating oil; Equipped with A sliding part using the sliding member according to any one of claims 1 to 10 is included. Compressor.

12. The compression mechanism includes a fixed scroll, a rotating scroll, and a rotating shaft that drives the rotating scroll to rotate. The sliding member is used for at least one of the fixed scroll and the orbiting scroll. The compressor according to claim 11.

13. A refrigeration system using the compressor according to claim 11 or 12.

Citation Information

Patent Citations

  • JP1991099801U

  • Scroll type compressor and plating method therefor

    JP2000064970A

  • Sliding material for compressor

    JP2003161259A

  • Scroll compressor

    JP2006226210A

  • Method of producing electrical contact

    JP2010202900A