Method for producing particulate ceramic mixtures

Acidic treatment of FBC fly ash stabilizes its mineral composition and thermal behavior, addressing the cracking issue in ceramic mixtures, enabling the production of high-quality ceramic articles such as porcelain floor tiles.

JP7588426B2Active Publication Date: 2024-11-22VECOR IP HLDG
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022508982
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-14
Filing Date
2020-08-14
Publication Date
2024-11-22
Estimated Expiration
2040-08-14

AI Technical Summary

Technical Problem

The incorporation of fluidized bed combustion (FBC) fly ash, particularly circulating fluidized bed (CFB) fly ash, into granular ceramic mixtures results in cracking during the firing process, especially when used in high-quality ceramic articles like porcelain floor tiles, due to its high calcium and sulfur content and irregular morphology, which is not addressed by existing ceramic technologies developed for pulverized coal combustion (PCC) fly ash.

Method used

Treating FBC fly ash with an acidic aqueous solution to form a solid acid-treated fly ash, then mixing it with clay and optional feldspar to create a granular ceramic mixture that minimizes cracking by altering mineral compositions and thermal behavior.

Benefits of technology

The acid treatment of FBC fly ash allows it to be incorporated into ceramic articles without cracking, enabling the production of high-quality ceramic products like porcelain floor tiles by stabilizing the mixture and improving its firing behavior.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a method for producing a particulate ceramic mixture, the method comprising the following steps: (a) contacting fluidized bed combustion fly ash with an acidic aqueous solution to obtain an acidic fluidized bed combustion fly ash slurry; (b) removing excess acid from the slurry obtained in step (a) to obtain a solid acid-treated fluidized bed combustion fly ash; (c)(i) the solid acid-treated fluidized bed combustion fly ash obtained in step (b); (ii) clay; (iii) optionally, feldspar; (iv) optionally, other ingredients and contacting together to produce a particulate ceramic mixture.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the incorporation of fluidized bed combustion fly ash, and in particular circulating fluidized bed combustion fly ash, into a granular ceramic mixture. [Background technology]

[0002] Fluid bed combustion (FBC) power plants vs. pulverized coal combustion (PCC) power plants

[0003] Large amounts of fly ash are produced as a result of coal-fired power generation. This will continue for the foreseeable future. There is interest in how to utilize this fly ash waste. Currently, a large amount of fly ash is used in concrete as a pozzolanic or cementitious material. Other uses include brick making and use as a soil stabilization material. However, much fly ash continues to be landfilled. This is clearly costly both environmentally and economically. There is therefore continuing value and interest in developing products and processes that can use fly ash as a raw material. This would minimize the amount of fly ash that is landfilled and reduce the use of other virgin raw materials.

[0004] With the introduction of fluidized bed combustion (FBC) technology for thermal power generation and incineration, the problem of how to reuse fly ash from power generation has become more challenging. Fluidized bed combustion (FBC) plant design is quite different from pulverized coal combustion (PCC) plant design that has been the standard in power plants for many decades. Fly ash produced by FBC plants differs from PCC fly ash, which is much harder than PCC fly ash to be reused for other uses such as ceramic production.

[0005] Fluidized bed combustors burn coal in a heated fluidized bed of ash and / or sand at lower temperatures than PCC designs. Fluidized bed combustion (FBC) designs include "bubbling" fluidized bed and "circulating" fluidized bed designs. Bubbling fluidized beds are also called "boiling fluid beds." Circulating fluidized beds, known as CFBs, are the most common. The various FBC designs can be further divided based on the pressure at which they operate, either atmospheric or pressurized.

[0006] Circulating fluidized bed (CFB) furnaces operate by continuously recirculating most of the hot ash (including any fine unburned fuel) from the exhaust stream entering the combustion zone to the bottom of a fluidized bed combustion zone. A final percentage of fly ash is continuously removed from the exhaust and fresh fuel and additives are continuously added to the combustion zone. This system has many advantages including very high levels of carbon burn (due to the repeated passage of the combustion particles through the combustion zone) and in addition, the fuel does not need to be pulverized before being added to the combustion zone. The high temperatures and high levels of particle:particle interactions experienced by the ash particles in the CFB design provide an opportunity for mineral phases to form that are not normally found in PCC ash.

[0007] Fluidized bed combustion (FBC) technology is becoming increasingly popular because plants using such technology are less polluting. FBC plants emit much lower levels of nitrous oxides than traditional PCC plants, sulfur oxides are easier to remove, and FBC plants can burn a wider range of fuels, such as low-rank coal, and even fuels such as tires and oil. These low-rank fuels often have high sulfur content.

[0008] The solid / solid contact with hot particles in the FBC plant design gives a very high heat exchange coefficient. This means that FBC plants can efficiently produce power at much lower temperatures, typically between 800-900°C, compared to 1400-1700°C in PCC plants. The ability to operate efficiently at lower combustion temperatures has significant advantages. In particular, nitrous oxide production is reduced in FBC plants, thereby reducing NOx pollution.

[0009] Removing sulfur oxides is also easier in FBC plants compared to PCC plants. PCC plants typically burn higher quality, lower sulfate coal, such as anthracite. PCC plants typically have wet scrubbers that treat the flue gas to chemically remove the sulfur oxides through a process called flue gas desulfurization (FGD), which is an expensive and intensive process.

[0010] In contrast to PCC plants, FBC plants typically reduce their sulfur oxide emissions by burning a mixture of fuel and limestone / chalk / dolomite. The limestone material (calcium carbonate) forms calcium oxide in a fluidized bed. This reacts with sulfur oxides from the combustion of sulfur compounds in the fuel to form calcium sulfate in situ. This allows calcium sulfate to form easily in a fluidized bed of calcium sulfate minerals such as anhydrite, where temperatures are low enough to be stable.

[0011] Such reactions cannot occur in PCC plants due to the high temperatures used, therefore a separate FGD system is required.

[0012] Adding limestone material to coal to react sulfur oxides in situ is a much simpler process than scrubbing the flue gases.

[0013] Differences between Fluidized Bed Combustion (FBC) Fly Ash and Pulverized Coal Combustion (PCC) Fly Ash

[0014] The addition of significant amounts of limestone material to the boilers in fluidized bed combustion (FBC) plants means that FBC fly ash typically contains high levels of calcium and sulfur species.

[0015] The levels of calcium species in FBC fly ash, usually reported as equivalent calcium oxide levels, are often higher than high calcium oxide (Type C) fly ash from PCC plants.

[0016] Furthermore, the levels of sulfur species in FBC fly ash, usually reported as equivalent sulfur oxide levels, are higher than the sulfur oxide levels in PCC fly ash.

[0017] The ASTM-C618 standard is commonly used to define fly ash quality suitable for use as a pozzolanic or cementitious product. The upper SO3 limit for materials conforming to ASTM-C618 is 5% by weight. FBC fly ash typically contains much higher levels of oxides of sulfur.

[0018] Physically, the fly ash from the FBC design is quite different from conventional PCC fly ash. FBC fly ash is not exposed to the extremely high temperatures encountered in the exhaust systems of conventional PCC plants. Fly ash produced in PCC plants is suspended in the very hot effluent combustion gases. The temperatures experienced are high enough to melt the particles. This means that the majority of PCC fly ash particles are spherical and formed of a glassy amorphous phase.

[0019] In contrast, fly ash from FBC plants, especially CFB combustion plants, is not melted due to the lower temperature of the FBC. As a result, FBC fly ash particles have irregular shapes and do not contain glassy phases. Another difference is that the time that the fly ash is exposed to high temperatures is typically very long in FBC plants, especially in plants where high levels of fly ash are recirculated, such as CFB combustion plants. This means, for example, that iron in PCC fly ash is often present as magnetite and hematite, while in FBC fly ash and CFB combustion fly ash it is mostly present as ferrite. This has great implications, for example, for the ease of removal of iron.

[0020] PCC and FBC fly ashes are chemically different (e.g., typically have different levels of calcium and sulfate species), physically different (e.g., typically have different morphologies, e.g., ordered / vitreous (PCC) compared to irregular / non-vitreous (FBC)), and mineralogy. FBC fly ashes also have smaller diameters (due to self-grinding) and lower residual carbon levels than PCC fly ashes.

[0021] Issues Concerning the Incorporation of Fluidized Bed Combustion (FBC) Fly Ash, Particularly Circulating Fluidized Bed (CFB) Combustion Fly Ash, into Granular Ceramic Mixtures

[0022] Most of the FBC fly ash is currently sent to landfills or used as a very low value soil stabilizer. It is less effective than PCC fly ash as a pozzolana. Also, the high sulfate levels can cause problems. There is an increasing need to find alternative uses for FBC fly ash. A possible high value use is in ceramic articles such as ceramic and porcelain floor tiles.

[0023] Fly ash can be used as a partial replacement for clay in ceramic articles. Fly ash can be combined with clay and other materials, such as feldspar, to form a particulate ceramic mixture. The particulate ceramic mixture can be formed into ceramic articles, such as ceramic tiles, particularly porcelain floor tiles. Such ceramic articles can be manufactured using significant levels of fly ash, as is known in the art.

[0024] The replacement of clay with fly ash is beneficial as supplies of suitable clay are becoming limited, and it would be beneficial to maximize the available levels of clay that can be replaced by fly ash.

[0025] However, most of the fly ash used in the art is PCC fly ash. FBC, and especially CFB combustion, is a relatively recent development and was not used when previous ceramic technologies were developed. Thus, problems specifically related to the use of FBC fly ash in ceramic applications were not recognized, or, if they were, were mostly related to the bulk of the fly ash product. For example, the art describes fly ash consisting of spheres of an amorphous glass phase, which is a description of PCC fly ash, not FBC fly ash. It is clear that the art refers to PCC fly ash.

[0026] The inventors have discovered that simply replacing PCC fly ash with FBC fly ash, particularly CFB combustion fly ash, in ceramic compositions containing clay, feldspar, and optionally other ingredients can cause defects. Ceramic articles made with FBC fly ash have been observed to crack during the firing cycle. This is particularly problematic when producing high quality, large ceramic articles such as ceramic floor tiles, particularly porcelain floor tiles, where such defects are particularly unacceptable. The incorporation of fly ash into porcelain floor tiles, which require low water absorption and high bending strength, is particularly difficult.

[0027] The inventors have also determined that this problem is exacerbated when FBC fly ash is used at higher levels in ceramic applications.

[0028] Without wishing to be bound by theory, it is hypothesized that the high energy environment of typical ceramic manufacturing processes and the high levels of intense surface / surface contact between the clay and FBC fly ash particles result in the formation of high levels of certain mineral phases that alter the firing behavior of the material, resulting in cracking of the ceramic article.

[0029] The present inventors have discovered that treating the FBC fly ash with an aqueous acid solution during the preparation of a granular ceramic mixture overcomes the problems associated with incorporating the FBC fly ash, particularly CFB combustion fly ash, into a granular ceramic mixture, thereby enabling the FBC fly ash, particularly CFB combustion fly ash, to be incorporated into a granular ceramic mixture and formed into ceramic articles such as ceramic and porcelain floor tiles without cracking problems.

[0030] Without wishing to be bound by theory, it is hypothesized that the acid treatment of FBC fly ash and subsequent incorporation into the granular ceramic mixture results in the formation of different mineral compositions and phases that have different thermal behavior and do not crack as easily. Summary of the Invention [Problem to be solved by the invention]

[0031] The present invention provides a method for producing a particulate ceramic mixture, the method comprising the steps of: (a) contacting fluidized bed combustion fly ash with an acidic aqueous solution to obtain an acidic fluidized bed combustion fly ash slurry; (b) removing excess acid from the slurry obtained in step (a) and subjecting it to a solid acid treated fluidized bed combustion fryer; Ash obtaining the above compound; (c)(i) the solid acid-treated fluidized bed combustion fly ash obtained in step (b); (ii) clay; (iii) optionally, with feldspar; (iv) optionally, other ingredients contacting together to produce a particulate ceramic mixture. [Means for solving the problem]

[0032] Detailed Description of the Invention

[0033] Method for producing a particulate ceramic mixture - Patents.com The method for producing a particulate ceramic mixture comprises the steps of: (a) contacting fluidized bed combustion fly ash with an acidic aqueous solution to obtain an acidic fluidized bed combustion fly ash slurry; (b) removing excess acid from the slurry obtained in step (a) to produce a solid acid-treated fluidized bed combustion furnace; Ash obtaining the above compound; (c)(i) the solid acid-treated fluidized bed combustion fly ash obtained in step (b); (ii) clay; (iii) optionally, with feldspar; (iv) optionally, other ingredients contacting together Includes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] Treating the FBC fly ash with an aqueous acid prior to contacting the treated fly ash with other ceramic materials such as clay has several advantages. For example, it minimizes the amount of acid required since it is only the fly ash that actually requires acid treatment in such applications. The method of the present invention may require the removal of soluble products of the chemical reaction between the acid and the fly ash.

[0035] Furthermore, by contacting the fly ash only with acid, the solid suspension is easier to filter, since the fly ash does not swell (and therefore gel) in aqueous mixtures like many clays. The gelling and thickening associated with the washed clay, as well as the fly ash, can slow and complicate separation of the supernatant liquid unless very dilute solutions are used.

[0036] (a) obtaining an acidic fluidized bed combustion fly ash slurry; The fluidized bed combustion fly ash is contacted with an acidic aqueous solution to obtain an acidic fluidized bed combustion fly ash slurry. Preferably, the pH in step (a) is in the range of 2.0 to less than 7.0, preferably 2.0 to 6.0, or 2.0 to 5.0, or 2.3 to 4.0.

[0037] (b) obtaining a solid acid-treated fluidized bed combustion fly ash; The excess acid is removed from the slurry obtained in step (a) to prepare a solid acid-treated fluidized bed combustor. Ash get.

[0038] Typically, step (b) involves rinsing the slurry and removing the supernatant from the solids. This typical rinsing step can be repeated, for example, two or more times, or three or more times, or four or more times.

[0039] (c) forming a particulate ceramic mixture; During step (c), the following ingredients are contacted together: (i) the solid acid-treated fluidized bed combustion fly ash obtained in step (b); (ii) clay; (iii) optionally, feldspar; and (iv) optionally, other ingredients

[0040] Granular ceramic mixture The particulate ceramic mixture includes solid acid treated fluidized bed combustion fly ash, clay, feldspar, and optionally other ingredients.

[0041] Preferably, the particulate ceramic mixture comprises: (a) 10% to 60% by weight, or 20% to 50% by weight, of solid acid-treated fluidized bed combustion fly ash; (b) 15% to 55% clay by weight; (c) 0% to 35% by weight, or 5% to 25% by weight, of feldspar; and (d) optionally, other ingredients to make up 100% by weight Includes.

[0042] Preferably, the particulate ceramic mixture comprises: (a) Acid-treated fluidized bed combustion fly ash with 20% to 50% by weight solids; (b) 15% to 35% by weight clay; (c) 0% to 35% by weight, or 5% to 25% by weight, of feldspar; and (d) optionally, other ingredients to make up 100% by weight Includes.

[0043] Fluidized Bed Combustion Fly Ash Suitable fluidized bed combustion fly ash may be atmospheric fluidized bed combustion fly ash, pressurized fluidized bed combustion fly ash, or a combination thereof.

[0044] Suitable fluidized bed combustion fly ash may be a circulating fluidized bed combustion fly ash, a bubbling fluidized bed combustion fly ash, or a combination thereof.

[0045] A preferred fluidized bed combustion fly ash is a circulating fluidized bed combustion fly ash.

[0046] Typically, the fluidized bed combustion fly ash contains greater than 4.0% by weight oxides of sulfur, or greater than 5.0% by weight, or greater than 6.0% by weight, or greater than 6.5% by weight, or greater than 7.0% by weight, or greater than 10% by weight oxides of sulfur.

[0047] Typically, the fluidized bed combustion fly ash is derived from coal, typically fluidized bed combustion coal fly ash.

[0048] Acid-treated fluidized bed combustion of solid fly ash. Typically, the solid acid treated fluidized bed combustion fly ash contains greater than 4.0% by weight oxides of sulfur, or greater than 5.0% by weight, or greater than 6.0% by weight, or greater than 6.5% by weight, or greater than 7.0% by weight, or greater than 10% by weight oxides of sulfur.

[0049] Oxides of sulfur Analysis of the elemental composition of fly ash is most commonly performed by X-ray fluorescence (XRF) techniques, which measure the levels of heavier elements such as iron, aluminum, silicon, sulfate, and calcium. By convention, these are reported as equivalent stoichiometric levels of the oxides. Sulfur is reported as SO3.

[0050] The term "sulfate" is technically SO4 2- ions, SO3 is often referred to as "sulfate" in the ceramic literature. Sometimes sulfur is reported as elemental sulfur, but how sulfur is reported makes no difference to the actual levels present. Therefore, the present invention uses the more general term "oxides of sulfur." ​​"Oxides of sulfur," SO3, and "sulfate" are interchangeable terms as used herein.

[0051] The level of oxides of sulfur present in fly ash can be determined using the following XRF method.

[0052] A suitable XRF instrument is the Epsilon 4 XRF analyzer from Malvern panalytical, with sample disks produced using an Aegon2 automatic fusion machine for sample disk preparation from Classe. The ash sample is automatically dissolved in molten lithium borate flux and formed into a disk. This is then placed in the Epsilon 4 for analysis. The instrument should be operated according to the manufacturer's instructions. When measuring SO3, the Epsilon 4 is set to a voltage of 4.5 kV, a current of 3000 μa, helium as the medium, no filter, and a measurement time of 450 seconds.

[0053] clay Suitable clays include standard clays such as Ukrainian clays and illitic clays. A preferred clay is a combination of standard clays and high plasticity clays. The weight ratio of standard clays to high plasticity clays may range from 2:1 to 5:1. A suitable clay is a high plasticity clay such as bentonite clay. Typically, high plasticity clays have an Atterburg plasticity index greater than 25.0. Typically, standard clays have an Atterburg plasticity index of 25.0 or less. The amount of high plasticity clay can be selected to provide sufficient robustness and flowability to the granular ceramic mixture.

[0054] feldspar Suitable feldspars include sodium and / or potassium feldspars.

[0055] Optional Other Ingredients Other optional ingredients include chemical additives and binders.

[0056] acidic aqueous solution The aqueous acid solution can be an organic aqueous acid solution, an inorganic aqueous acid solution, or a combination thereof. The aqueous acid solution is preferably a weak acid.

[0057] Suitable aqueous acids are selected from acetic acid (ethanoic acid), ascorbic acid ((2R)-2-[(lS)-l,2-dihydroxyethyl]-3,4-dihydroxy-2H-furan-5-one), hydrochloric acid, nitric acid, oxalic acid (ethanedioic acid), sulfuric acid, and any combination thereof.

[0058] Preferably, the acidic aqueous solution is an aqueous solution of acetic acid (ethanoic acid). A suitable source of acetic acid (ethanoic acid) is vinegar.

[0059] Typically, during step (a), the aqueous acidic solution has a molar concentration of 0.2M to 3.0M, or 0.4M to 2.0M, or 0.5M to 1.5M.

[0060] Preferably, the pH of said acidic aqueous solution during step (a) is in the range of from 2.0 to less than 7.0, preferably from 2.0 to 6.0, or from 2.0 to 5.0, or from 2.3 to 4.0.

[0061] Preferably, said acid is not sulfuric acid and said aqueous acid solution is not an aqueous solution of sulfuric acid. EXAMPLES

[0062] Examples of the present invention Acid-treated FBC fly ash was prepared by taking FBC fly ash and washing it in a 10% (volume %) aqueous solution of acetic (ethanoic) acid at a ratio of 50 g of FBC fly ash to 500 ml of the aqueous solution of acetic (ethanoic) acid. The mixture was stirred vigorously at ambient temperature for 60 minutes.

[0063] After mixing, the mixture was allowed to settle and the supernatant liquid was discarded. The mixture was then swirled and rinsed with fresh water, the solids were allowed to settle, and the supernatant liquid was decanted. The wet ash was then dried at 120° C. for 1 hour to produce dried acid-treated FBC fly ash.

[0064] The dried acid treated FBC fly ash was then mixed with clay and feldspar and made into ceramic articles according to the following process.

[0065] 100 g of acid-treated fluidized bed combustion fly ash was mixed with 50 g of illite clay and 50 g of sodium feldspar to produce a granular ceramic mixture. The mixture was crushed, sieved, and wetted. 140 g of the granular ceramic mixture was then uniaxially pressed in a rectangular mild steel mold (155×40 mm) to a pressure of 40 MPa and held for 1.5 minutes (90 seconds). The resulting compact was removed from the mold and placed in an oven at 110° C. to dry.

[0066] The dried compact was fired in an electric kiln at a ramp rate of 2.5°C / min up to 1160°C. The temperature was held at the maximum temperature for 30 minutes. The fired body was then allowed to cool naturally (and therefore slowly) to room temperature.

[0067] No cracks were observed in this fired body.

[0068] Comparative Example The fluidized bed ash was identical to the acid treated fluidized bed combustion fly ash except for the acid treatment step, however, it was not subjected to the acid wash step, but instead was mixed directly with the other ingredients, following the same procedure as above.

[0069] Cracks were observed in this fired body.

[0070] A similarly produced comparative example, but made from PCC fly ash and of the same composition as the FBC fly ash comparative example, showed no cracking at all.

Claims

1. 1. A method for producing a particulate ceramic mixture, the method comprising the steps of: (a) contacting fluidized bed combustion fly ash with an acidic aqueous solution to obtain an acidic fluidized bed combustion fly ash slurry, wherein the acidic aqueous solution is selected from an aqueous solution of acetic acid (ethanoic acid), an aqueous solution of ascorbic acid ((2R)-2-[(lS)-l,2-dihydroxyethyl]-3,4-dihydroxy-2H-furan-5-one), an aqueous solution of hydrochloric acid, an aqueous solution of nitric acid, an aqueous solution of oxalic acid (ethanedioic acid), and any combination thereof; (b) removing excess acid from the slurry obtained in step (a) to obtain a solid acid-treated fluidized bed combustion fly ash; (c)(i) the solid acid-treated fluidized bed combustion fly ash obtained in step (b); (ii) clay; (iii) optionally, feldspar; (iv) optionally, other ingredients contacting together producing a particulate ceramic mixture.

2. 2. The method of claim 1, wherein the acidic aqueous solution is an aqueous solution of acetic acid (ethanoic acid).

3. 3. The method according to claim 1 or 2, wherein the acidic aqueous solution has a molar concentration of 0.2M to 3.0M.

4. 4. The method according to any one of claims 1 to 3, wherein step (b) comprises rinsing the slurry and removing the supernatant from the solids to obtain the solid acid-treated fluidized bed combustion fly ash.

5. The particulate ceramic mixture comprises: (a) 10% to 60% by weight of fluidized bed combustion fly ash; (b) 15% to 55% by weight of clay; (c) 0% to 35% by weight feldspar; and (d) optionally, other ingredients to make up 100% by weight The method according to any one of claims 1 to 4, comprising:

6. The particulate ceramic mixture comprises: (a) 20% to 50% by weight of fluidized bed combustion fly ash; (b) 15% to 35% by weight of clay; (c) 0% to 25% by weight feldspar; and (d) optionally, other ingredients to make up 100% by weight The method according to any one of claims 1 to 5, comprising:

7. The method according to any one of claims 1 to 6, wherein the fluidized bed combustion fly ash is a circulating fluidized bed combustion fly ash.

8. 8. The method of any one of claims 1 to 7, wherein the fluidized bed combustion fly ash contains greater than 5.0 wt.% oxides of sulfur.

9. 9. The method of any one of claims 1 to 8, wherein the fluidized bed combustion fly ash contains greater than 10% by weight of oxides of sulfur.

Citation Information

Patent Citations

  • Method for utilizing fuel ash to prepare ceramic

    CN108191401A

  • Fly ash processing and manufacture of articles incorporating fly ash compositions

    US20170073274A1