Soft magnetic metal powders, dust cores and magnetic components

A soft magnetic metal powder with controlled surface texture and coating thickness addresses the challenge of achieving high voltage resistance and mechanical strength in powder magnetic cores, enhancing their performance in magnetic components.

JP7588478B2Active Publication Date: 2024-11-22TDK CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020129377
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-07-30
Publication Date
2024-11-22
Estimated Expiration
2040-07-30

AI Technical Summary

Technical Problem

Conventional methods for forming an insulating coating on soft magnetic metal particles fail to achieve both high voltage resistance and mechanical strength in powder magnetic cores, leading to issues such as decreased magnetic permeability and inductance due to low mechanical strength and increased core loss from interparticle eddy currents.

Method used

A soft magnetic metal powder with a specific surface texture is developed, where the coating portion has a maximum height Sz of 10 nm to 700 nm, arithmetic mean height Sa of 3 nm to 50 nm, and a thickness T of 3 nm to 200 nm, composed of materials like phosphorus, aluminum, and oxygen, to enhance both voltage resistance and mechanical strength.

Benefits of technology

The solution results in a powder magnetic core with improved voltage resistance and mechanical strength, suitable for use in magnetic components like power inductors, by controlling the surface roughness and coating thickness to balance both properties effectively.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588478000032
    Figure 0007588478000032
  • Figure 0007588478000033
    Figure 0007588478000033
  • Figure 0007588478000034
    Figure 0007588478000034
Patent Text Reader

Abstract

To provide a powder magnetic core with good voltage resistance and strength, a magnetic component including the same, and a soft magnetic metal powder suitable for the powder magnetic core.SOLUTION: The soft magnetic metal powder includes a plurality of coated particles 1 in which coating portions 10 are formed on surfaces of soft magnetic metal particles 2. The maximum height at surfaces of the coating portions 10 formed on the surfaces of the soft magnetic metal particles 2 is between 10 nm and 700 nm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a soft magnetic metal powder, a dust core, and a magnetic component. [Background technology]

[0002] Transformers, choke coils, inductors, and the like are known as magnetic components used in power supply circuits of various electronic devices.

[0003] Such magnetic components have a configuration in which a coil (winding), which is an electrical conductor, is disposed around or inside a magnetic core that exhibits predetermined magnetic properties.

[0004] An example of a magnetic material used for the magnetic core of a magnetic component such as an inductor is a soft magnetic metal material containing iron (Fe). The magnetic core can be obtained as a powder magnetic core by, for example, compression molding soft magnetic metal powder containing particles made of a soft magnetic metal containing Fe.

[0005] In such powder magnetic cores, the proportion of magnetic components (filling rate) is increased to improve the magnetic properties. One method for increasing the proportion of magnetic components (filling rate) is to reduce the amount of insulating resin. However, this method increases the proportion of soft magnetic metal particles that come into contact with each other, which increases the loss caused by the current that flows between the contacting particles (interparticle eddy current) when an AC voltage is applied to the magnetic component. As a result, there is a problem in that the core loss of the powder magnetic core increases.

[0006] In order to suppress such eddy currents, an insulating coating is formed on the surface of soft magnetic metal particles. For example, Patent Document 1 discloses that powder glass containing an oxide of phosphorus (P) is softened by mechanical friction to form an insulating coating layer on the surface of Fe-based amorphous alloy powder. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2015-132010 A Summary of the Invention [Problem to be solved by the invention]

[0008] In Patent Document 1, Fe-based amorphous alloy powder on which an insulating coating layer has been formed is mixed with resin and compression molded to form a dust core. If the mechanical strength of the dust core is low, cracks are likely to occur, resulting in problems of reduced permeability and reduced inductance. For this reason, dust cores are required to have high mechanical strength in addition to good magnetic properties and high insulation (voltage resistance). However, simply forming an insulating coating layer using the method of Patent Document 1 does not allow both voltage resistance and strength to be achieved.

[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a powder magnetic core having good voltage resistance and strength, a magnetic component including the same, and a soft magnetic metal powder suitable for the powder magnetic core. [Means for solving the problem]

[0010] The inventors discovered that by providing a coating portion having prescribed surface properties on soft magnetic metal particles made of a soft magnetic metal having a specific composition, both the voltage resistance and strength of a powder magnetic core can be improved, and thus completed the present invention.

[0011] That is, an aspect of the present invention is [1] A soft magnetic metal powder comprising a plurality of soft magnetic metal particles containing iron, The surface of the soft magnetic metal particle is covered with a coating portion, The soft magnetic metal powder has a maximum height Sz of 10 nm or more and 700 nm or less on the surface of the coating portion.

[0012] [2] The soft magnetic metal powder according to [1], wherein the arithmetic mean height Sa of the surface of the coating portion is 3 nm or more and 50 nm or less.

[0013] [3] The soft magnetic metal powder according to [1] or [2], in which Sz / T is 1.5 or more and 30 or less, where T [nm] is the thickness of the coating portion.

[0014] [4] A soft magnetic metal powder comprising a plurality of soft magnetic metal particles containing iron, The surface of the soft magnetic metal particle is covered with a coating portion, The soft magnetic metal powder has a maximum height Rz of 10 nm or more and 700 nm or less on the surface of the coating portion.

[0015] [5] The soft magnetic metal powder according to [4], wherein the arithmetic mean roughness Ra of the surface of the coating portion is 3 nm or more and 100 nm or less.

[0016] [6] The soft magnetic metal powder according to [4] or [5], in which Rz / T is 1.5 or more and 30 or less, where T [nm] is the thickness of the coating portion.

[0017] [7] The soft magnetic metal powder according to any one of [1] to [6], wherein T is 3 nm or more and 200 nm or less, where T is the thickness of the coating portion, T [nm].

[0018] [8] The coating portion is a soft magnetic metal powder according to any one of [1] to [7], which contains at least one selected from the group consisting of phosphorus, aluminum, calcium, barium, bismuth, silicon, chromium, sodium, zinc, and oxygen.

[0019] [9] The soft magnetic metal powder according to any one of [1] to [8], wherein the soft magnetic metal particles are composed of an amorphous alloy.

[0020]

[10] The soft magnetic metal powder according to any one of [1] to [8], wherein the soft magnetic metal particles are composed of a nanocrystalline alloy.

[0021]

[11] A dust core comprising the soft magnetic metal powder according to any one of [1] to

[10] .

[0022]

[12] A magnetic component comprising the powder magnetic core described in

[11] . Effect of the Invention

[0023] According to the present invention, it is possible to provide a powder magnetic core having good voltage resistance and strength, a magnetic component including the powder magnetic core, and a soft magnetic metal powder suitable for the powder magnetic core. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a schematic cross-sectional view of a coated particle constituting the soft magnetic metal powder according to this embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the configuration of a powder coating apparatus used to form the coating portion. [Diagram 3] FIG. 3 is an image of the composition of the coated particles in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] Since it has been difficult to achieve both strength and voltage resistance in powder magnetic cores using conventional technology, the inventors have conducted detailed investigations into the relationship between the nano-level microstructure on the surface of soft magnetic particles on which a coating portion is formed and the strength and voltage resistance of powder magnetic cores, which is a new perspective that has not been previously considered.

[0026] Among the many strength factors of powder magnetic cores that affect each other in a complex way, the inventors conducted a detailed investigation into the relationship between the nano-level surface roughness of the surfaces of soft magnetic particles on which a coating portion is formed and the strength of the powder magnetic cores.

[0027] As a result, it was found that if the surface roughness of the soft magnetic particles on which the coating portion is formed is equal to or greater than the lower limit of the range recited in the claims, it is effective in improving the strength of the powder magnetic core.

[0028] Furthermore, with regard to the withstand voltage of the powder magnetic core, the inventors conducted a detailed investigation into the relationship with the nano-level surface roughness of the soft magnetic particle surface on which the coating portion is formed, from among the many withstand voltage factors that affect each other in a complex manner.

[0029] As a result, it was found that if the surface roughness of the soft magnetic particles on which a coating portion is formed is below the upper limit of the range described in the claims, it is effective in improving the voltage resistance of the powder magnetic core, and it was discovered that if the surface roughness of the soft magnetic particles on which a coating portion is formed is within the range described in the claims, it is possible to achieve a high level of both strength and voltage resistance of the powder magnetic core, which was difficult to achieve with conventional technology.

[0030] The present invention will now be described in detail with reference to specific embodiments shown in the drawings in the following order. 1. Soft magnetic metal powder 1.1. Soft magnetic metal 1.1.1.Fe-based amorphous alloys 1.1.2.Fe-based nanocrystalline alloys 1.2. Covering 1.2.1. Composition 1.2.2.Surface texture 2.Powder magnetic core 3. Magnetic parts 4. Manufacturing method of powder magnetic core 4.1. Manufacturing method of soft magnetic metal powder 4.2. Manufacturing method of powder magnetic core

[0031] (1. Soft magnetic metal powder) 1, the soft magnetic metal powder according to this embodiment includes a plurality of coated particles 1 in which a coating portion 10 is formed on the surface of a soft magnetic metal particle 2. When the percentage of the number of particles included in the soft magnetic metal powder is taken as 100%, the percentage of the number of coated particles is preferably 90% or more, and more preferably 95% or more.

[0032] In this embodiment, the shape of the soft magnetic metal particles 2 is preferably spherical. Specifically, the average circularity of the cross section of the soft magnetic metal particles 2 contained in the soft magnetic metal powder is preferably 0.85 or more. As the circularity, for example, Wadell's circularity can be used.

[0033] The average particle size (D50) of the soft magnetic metal powder according to this embodiment may be selected according to the application and material. In this embodiment, the average particle size (D50) is preferably within the range of 0.3 to 100 μm. By setting the average particle size of the soft magnetic metal powder within the above range, it becomes easy to maintain sufficient moldability or predetermined magnetic properties. The method for measuring the average particle size is not particularly limited, but it is preferable to use a laser diffraction scattering method.

[0034] In this embodiment, the soft magnetic metal powder may contain only soft magnetic metal particles of the same material, or soft magnetic metal particles of different materials may be mixed in. The different materials include, for example, soft magnetic metal particles of different elements constituting the soft magnetic metal, and soft magnetic metal particles of the same elements but different compositions.

[0035] (1.1. Soft magnetic metal) The soft magnetic metal particles are made of a soft magnetic metal containing iron (Fe). Examples of soft magnetic metals containing iron include pure iron, Fe-based alloys, Fe-Si-based alloys, Fe-Al-based alloys, Fe-Ni-based alloys, Fe-Si-Al-based alloys, Fe-Si-Cr-based alloys, Fe-Ni-Si-Co-based alloys, and other Fe-based crystalline materials; Fe-based amorphous alloys; and Fe-based nanocrystalline alloys.

[0036] The Fe-based amorphous alloy may be composed of only an amorphous phase, or may have a structure in which primary crystallites are dispersed in an amorphous phase, that is, a nanoheterostructure.

[0037] Fe-based nanocrystalline alloys have a structure in which Fe-based nanocrystals on the nanometer order are dispersed in an amorphous phase.

[0038] In this embodiment, the soft magnetic metal containing iron is preferably an Fe-based amorphous alloy or an Fe-based nanocrystalline alloy. In the following, an Fe-based amorphous alloy and an Fe-based nanocrystalline alloy will be described.

[0039] (1.1.1.Fe-based amorphous alloy) In this embodiment, the Fe-based amorphous alloy preferably has a nanoheterostructure in which the primary microcrystals are present in the amorphous phase. Such a structure is obtained by rapidly cooling a molten metal of the raw material of the soft magnetic metal, and a large number of microcrystals are precipitated and dispersed in the amorphous alloy. Therefore, the average crystal grain size of the primary microcrystals is very small. In this embodiment, the average crystal grain size of the primary microcrystals is preferably 0.3 nm or more and 10 nm or less.

[0040] By heat treating the soft magnetic metal having a nanoheterostructure under prescribed conditions, it becomes easy to grow the primary crystallites and obtain the Fe-based nanocrystalline alloy described below.

[0041] Next, the composition of the Fe-based amorphous alloy will be described in detail.

[0042] In this embodiment, the composition of the Fe-based amorphous alloy is represented by the formula (Fe (1-(α+β)) X1 α X2 β ) (1-(a+b+c+d+e+f)) M a B b P c S d C e S f It is preferable that the formula is represented by the formula:

[0043] In the above composition formula, M is at least one element selected from the group consisting of niobium (Nb), hafnium (Hf), zirconium (Zr), tantalum (Ta), molybdenum (Mo), tungsten (W), titanium (Ti) and vanadium (V).

[0044] Moreover, “a” represents the molar ratio of M, and from the viewpoint of the voltage resistance and strength of the powder magnetic core, it is preferable that “a” satisfies 0≦a≦0.300. In other words, the soft magnetic metal does not have to contain M.

[0045] In addition to the viewpoints of the voltage resistance and strength of the powder magnetic core, from the viewpoint of soft magnetic properties, it is preferable that "a" satisfies 0≦a≦0.150. The molar ratio (a) of M is more preferably 0.040 or more, and even more preferably 0.050 or more. The molar ratio (a) of M is more preferably 0.100 or less, and even more preferably 0.080 or less. If "a" is too large, the saturation magnetization of the powder tends to be easily reduced.

[0046] In the above composition formula, "b" represents the molar ratio of boron (B), and from the viewpoint of the voltage resistance and strength of the powder magnetic core, it is preferable that "b" satisfies 0≦b≦0.400. In other words, the soft magnetic metal does not need to contain B.

[0047] In addition to the viewpoints of the voltage resistance and strength of the powder magnetic core, and also in terms of the soft magnetic properties, it is preferable that "b" satisfies 0≦b≦0.200. The molar ratio (b) of B is more preferably 0.025 or more, even more preferably 0.060 or more, and particularly preferably 0.080 or more. The molar ratio (b) of B is more preferably 0.150 or less, and even more preferably 0.120 or less. If "b" is too large, the saturation magnetization of the powder tends to be easily reduced.

[0048] In the above composition formula, "c" represents the molar ratio of phosphorus (P), and from the viewpoint of the voltage resistance and strength of the powder magnetic core, it is preferable that "c" satisfies 0≦c≦0.400. In other words, the soft magnetic metal does not need to contain P.

[0049] In addition to the viewpoint of the voltage resistance and strength of the powder magnetic core, from the viewpoint of the soft magnetic properties, it is preferable that "c" satisfies 0≦c≦0.200. The molar ratio (c) of P is more preferably 0.005 or more, and even more preferably 0.010 or more. Moreover, the molar ratio (c) of P is more preferably 0.100 or less. When "c" is within the above range, the resistivity of the soft magnetic metal tends to improve and the coercive force tends to decrease. When "c" is too large, the saturation magnetization of the powder tends to be easily reduced.

[0050] In the above composition formula, "d" indicates the molar ratio of silicon (Si), and from the viewpoint of the voltage resistance and strength of the powder magnetic core, it is preferable that "d" satisfies 0≦d≦0.400. In other words, the soft magnetic metal does not need to contain Si.

[0051] In addition to the viewpoints of the voltage resistance and strength of the powder magnetic core, from the viewpoint of the soft magnetic properties, it is preferable that "d" satisfies 0≦d≦0.200. The molar ratio (d) of Si is more preferably 0.001 or more, and even more preferably 0.005 or more. Moreover, it is more preferable that the molar ratio (d) of Si is 0.040 or less. When "d" is within the above range, the coercive force of the soft magnetic metal tends to decrease. On the other hand, when "d" is too large, the coercive force of the soft magnetic metal tends to increase.

[0052] In the above composition formula, "e" represents the molar ratio of carbon (C), and from the viewpoint of the voltage resistance and strength of the powder magnetic core, "e" preferably satisfies 0≦e≦0.400. In other words, the soft magnetic metal does not need to contain C.

[0053] In addition to the viewpoints of the voltage resistance and strength of the powder magnetic core, from the viewpoint of soft magnetic properties, it is preferable that "e" satisfies 0≦e≦0.200. The molar ratio (e) of C is more preferably 0.001 or more. Moreover, the molar ratio (e) of C is more preferably 0.035 or less, and even more preferably 0.030 or less. When "e" is within the above range, the coercive force of the soft magnetic metal tends to be particularly easily reduced. When "e" is too large, the coercive force of the soft magnetic metal tends to increase instead.

[0054] In the above composition formula, "f" represents the molar ratio of sulfur (S), and from the viewpoint of the voltage resistance and strength of the powder magnetic core, "f" preferably satisfies 0≦f≦0.040. In other words, the soft magnetic metal does not need to contain S.

[0055] In addition to the viewpoints of voltage resistance and strength of the powder magnetic core, from the viewpoint of soft magnetic properties, it is preferable that "f" satisfies 0≦f≦0.020. It is more preferable that the molar ratio (f) of S is 0.002 or more. It is more preferable that the molar ratio (f) of S is 0.010 or less. When "f" is within the above range, the coercive force of the soft magnetic metal tends to decrease. When "f" is too large, the coercive force of the soft magnetic metal tends to increase.

[0056] Furthermore, when "f" is equal to or greater than 0.001, the circularity of the soft magnetic metal particles is likely to be improved. When the circularity of the soft magnetic metal particles is improved, the density of the powder core obtained by compression molding the powder containing the soft magnetic metal particles can be improved.

[0057] In the above composition formula, "1-(a+b+c+d+e+f)" indicates the molar ratio of iron (Fe). The molar ratio of Fe is not particularly limited, but in this embodiment, from the viewpoint of the voltage resistance and strength of the powder magnetic core, the molar ratio of Fe (1-(a+b+c+d+e+f)) is preferably 0.410 or more and 0.910 or less.

[0058] From the viewpoint of the voltage resistance and strength of the powder magnetic core as well as the viewpoint of soft magnetic properties, the molar ratio of Fe (1-(a+b+c+d+e+f)) is preferably 0.700 or more and 0.850 or less. By keeping the molar ratio of Fe within the above range, it becomes even more difficult for a crystalline phase composed of crystals having a crystal grain size larger than 100 nm to occur.

[0059] As shown in the above composition formula, a portion of the iron may be compositionally substituted with X1 and / or X2.

[0060] X1 is at least one element selected from the group consisting of cobalt (Co) and nickel (Ni). In the above composition formula, "α" indicates the molar ratio of X1, and in this embodiment, "α" is preferably 0 or more. In other words, the soft magnetic metal does not need to contain X1.

[0061] Furthermore, when the number of atoms in the entire composition is taken as 100 at%, from the viewpoint of the voltage resistance and strength of the powder magnetic core, the number of atoms of X1 is preferably 70.00 at% or less. It is preferable that 0≦α{1-(a+b+c+d+e+f)}≦0.7000 is satisfied.

[0062] From the viewpoint of the voltage resistance and strength of the powder magnetic core as well as the soft magnetic properties, the atomic number of X1 is preferably 40.00 at% or less, i.e., 0≦α{1-(a+b+c+d+e+f)}≦0.4000 is preferably satisfied.

[0063] X2 is at least one element selected from the group consisting of aluminum (Al), manganese (Mn), silver (Ag), zinc (Zn), tin (Sn), arsenic (As), antimony (Sb), copper (Cu), chromium (Cr), bismuth (Bi), nitrogen (N), oxygen (O) and rare earth elements. In the above composition formula, "β" indicates the molar ratio of X2, and in this embodiment, "β" is preferably 0 or more. In other words, the soft magnetic metal does not need to contain X2.

[0064] Furthermore, when the number of atoms in the entire composition is taken as 100 at%, from the viewpoint of the voltage resistance and strength of the powder magnetic core, the number of atoms of X2 is preferably 6.00 at% or less, i.e., it is preferable that 0≦β{1-(a+b+c+d+e+f)}≦0.0600 is satisfied.

[0065] From the viewpoint of the soft magnetic properties as well as the voltage resistance and strength of the powder magnetic core, the atomic number of X2 is preferably 3.00 at% or less, i.e., 0≦β{1−(a+b+c+d+e+f)}≦0.0300 is satisfied.

[0066] Furthermore, the range (substitution ratio) of X1 and / or X2 substituting for iron is set to 0.94 or less of the total number of Fe atoms in terms of the number of atoms, in terms of the voltage resistance and strength of the powder magnetic core, i.e., 0≦α+β≦0.94.

[0067] Furthermore, from the viewpoint of soft magnetic properties as well as voltage resistance and strength of the powder magnetic core, the range in which X1 and / or X2 substitute for iron is set to half or less of the total number of Fe atoms in terms of the number of atoms. In other words, 0≦α+β≦0.50. If α+β>0.50, it tends to be difficult to obtain a soft magnetic metal in which Fe-based nanocrystals are precipitated by heat treatment.

[0068] The Fe-based amorphous alloy may contain elements other than those mentioned above as unavoidable impurities, for example, 0.1% by mass or less in total of elements other than those mentioned above relative to 100% by mass of the Fe-based amorphous alloy.

[0069] (1.1.2.Fe-based nanocrystalline alloys) The Fe-based nanocrystalline alloy has Fe-based nanocrystals. The Fe-based nanocrystals are Fe crystals with a crystal grain size on the order of nanometers and a bcc (body-centered cubic) crystal structure. In the soft magnetic metal, a large number of Fe-based nanocrystals are precipitated and dispersed in the amorphous phase. In this embodiment, the Fe-based nanocrystals are preferably obtained by heat-treating an Fe-based amorphous alloy having a nanoheterostructure to grow initial microcrystals.

[0070] Therefore, the average crystal grain size of the Fe-based nanocrystals tends to be slightly larger than that of the primary microcrystals. In this embodiment, the average crystal grain size of the Fe-based nanocrystals is preferably 5 nm or more and 30 nm or less. A soft magnetic metal in which the Fe-based nanocrystals are dispersed in an amorphous phase is likely to have high saturation magnetization and low coercive force.

[0071] In this embodiment, the composition of the Fe-based nanocrystalline alloy is preferably the same as the composition of the Fe-based amorphous alloy described above, and therefore the above description of the composition of the Fe-based amorphous alloy applies to the description of the composition of the Fe-based nanocrystalline alloy.

[0072] (1.2. Covering part) As shown in FIG. 1, the coating 10 is formed so as to cover the surface of the soft magnetic metal particle 2. In this embodiment, the surface being coated with a substance means that the substance comes into contact with the surface and is fixed so as to cover the contacted portion. The coating that coats the soft magnetic metal particle may cover at least a part of the surface of the particle, but it is preferable that it covers about 90%, and it is preferable that it covers the entire surface. Furthermore, the coating may cover the surface of the particle continuously or intermittently.

[0073] The coverage rate can be measured for soft magnetic metal particles on which a coating portion is formed as follows. The coated particles are observed with a known scanning electron microscope to obtain a composition image. It is preferable to obtain composition images at 10 or more locations in an area of ​​about 100 μm × 100 μm. The obtained composition image is binarized using commercially available image analysis software so that the coated portion is black and the area where the uncoated soft magnetic metal is exposed is white, and the coverage rate is determined as the ratio of the area of ​​the coated portion to the total area of ​​the coated particle.

[0074] Specifically, FIG. 3 is a composition image of a coated particle. In the composition image, the parts with different compositions (soft magnetic metal and coating) are observed as parts with different contrast, so by binarizing the image, the coated particle on the composition image can be divided into an area corresponding to the coating and an area corresponding to the soft magnetic metal. As shown in FIG. 3, the composition image shows that many soft magnetic metal particles have relatively black areas (coating) and relatively white areas (soft magnetic metal). Therefore, by binarizing the image of FIG. 3, the ratio of the area of ​​the relatively black areas to the total area of ​​the relatively black areas (coating) and the relatively white areas (soft magnetic metal) (total area of ​​the coated particle), that is, the coverage rate, can be calculated.

[0075] (1.2.1.Composition) The coating portion 10 is not particularly limited as long as it is made of a material that can insulate the soft magnetic metal particles that constitute the soft magnetic metal powder from each other. That is, the coating portion 10 is insulating. In this embodiment, it is preferable that the coating portion 10 contains at least one selected from the group consisting of phosphorus (P), aluminum (Al), calcium (Ca), barium (Ba), bismuth (Bi), silicon (Si), chromium (Cr), sodium (Na), zinc (Zn), and oxygen (O). More preferably, the coating portion 10 contains a compound containing at least one selected from the group consisting of phosphorus, zinc, and sodium. The compound is more preferably an oxide, and particularly preferably an oxide glass.

[0076] When the compound is an oxide, it is preferable that an oxide of at least one element selected from the group consisting of phosphorus, aluminum, calcium, barium, bismuth, silicon, chromium, sodium, and zinc is contained as a main component in the coating portion 10. "Containing an oxide of at least one element selected from the group consisting of P, Al, Ca, Ba, Bi, Si, Cr, Na, and Zn as a main component" means that, when the total amount of elements excluding oxygen among the elements contained in the coating portion 10 is taken as 100 mass%, the total amount of at least one element selected from the group consisting of P, Al, Ca, Ba, Bi, Si, Cr, Na, and Zn is the largest. In this embodiment, the total amount of these elements is preferably 50 mass% or more, and more preferably 60 mass% or more.

[0077] The oxide glass is not particularly limited, and examples thereof include phosphate (P2O5)-based glass, bismuthate (Bi2O3)-based glass, and borosilicate (B2O3-SiO2)-based glass.

[0078] The P2O5-based glass is preferably glass containing 50 mass% or more of P2O5, and examples thereof include P2O5-ZnO-R2O-Al2O3-based glass, where "R" represents an alkali metal.

[0079] As the Bi2O3-based glass, glass containing 50 mass % or more of Bi2O3 is preferable, and examples thereof include Bi2O3-ZnO-B2O3-SiO2-based glass.

[0080] As the B2O3-SiO2-based glass, glass containing 10 mass % or more of B2O3 and 10 mass % or more of SiO2 is preferable, and examples thereof include BaO-ZnO-B2O3-SiO2-Al2O3-based glass.

[0081] By having such an insulating coating, the insulating properties of the particles are improved, and therefore the withstand voltage of a dust core made of soft magnetic metal powder containing coated particles is improved.

[0082] The components contained in the coating can be identified from information such as lattice constants obtained by elemental analysis using energy dispersive X-ray spectroscopy (EDS) with a transmission electron microscope (TEM) such as a scanning transmission electron microscope (STEM), elemental analysis using electron energy loss spectroscopy (EELS), or fast Fourier transform (FFT) analysis of TEM images.

[0083] (1.2.2.Surface texture) In this embodiment, the surface properties of the coating are controlled to a predetermined shape. Specifically, the maximum height Sz of the coating surface is 10 nm or more and 700 nm or less. Sz is one of the surface roughness parameters defined in ISO25178, and is the sum of the maximum peak height and the maximum valley depth of the measurement surface (coating surface).

[0084] When Sz is within the above range, the voltage resistance and strength of the powder magnetic core can be compatible. If Sz is too small, the surface of the coating portion becomes too smooth, and the strength of the powder magnetic core tends to decrease. On the other hand, if Sz is too large, there are very large uneven parts on the surface of the coating portion, so that in the powder magnetic core, the unevenness of the coating portion of one particle is likely to damage the coating portion of another particle, and there are many parts with very thin coating or no coating, so the voltage resistance of the powder magnetic core tends to deteriorate.

[0085] Sz is preferably 20 nm or more, more preferably 30 nm or more, and even more preferably 40 nm or more. Sz is preferably 600 nm or less, more preferably 500 nm or less, and even more preferably 400 nm or less.

[0086] In this embodiment, the arithmetic mean height Sa of the coating surface is preferably 3 nm or more and 50 nm or less. Sa is one of the surface roughness parameters defined in ISO25178, and is the average of the absolute values ​​of the peak height and valley depth on the measurement surface (coating surface). Sa is expressed as the average surface roughness of the entire measurement surface, suppressing the influence of local irregularities such as Sz.

[0087] When Sa is within the above range in addition to Sz, both the voltage resistance and strength of the powder magnetic core are good, and the voltage resistance and strength of the powder magnetic core can be compatible at a high level. When Sa is outside the above range, only one of the voltage resistance and strength of the powder magnetic core tends to be good.

[0088] Furthermore, in this embodiment, it is preferable that Sz and the thickness of the coating satisfy a predetermined relationship. Specifically, when the thickness of the coating is T [nm], it is preferable that Sz / T is 1.5 or more and 30 or less. By controlling Sz according to the thickness of the coating, it is possible to achieve both high levels of voltage resistance and strength of the powder magnetic core.

[0089] Sz / T is more preferably 1.8 or more, and even more preferably 2.0 or more, while Sz / T is more preferably 26 or less, and even more preferably 22 or less.

[0090] In this embodiment, the surface properties of the coating are controlled to a predetermined shape from a viewpoint other than surface roughness. Specifically, the maximum height Rz of the contour curve of the coating surface is 10 nm or more and 700 nm or less. Rz is one of the line roughness parameters defined in JIS B601, and is the sum of the maximum peak height and the maximum valley depth of the contour curve of a predetermined length on the measurement surface (coated surface).

[0091] When Rz is within the above range, similarly to Sz, the voltage resistance and strength of the powder magnetic core can be achieved. If Rz is too small, the surface of the coating portion becomes too smooth, so the strength of the powder magnetic core tends to decrease. On the other hand, if Rz is too large, there are very large uneven parts on the surface of the coating portion, so that in the powder magnetic core, the unevenness of the coating portion of one particle is likely to damage the coating portion of another particle, and there are many parts with very thin coatings and no coatings, so the voltage resistance of the powder magnetic core tends to deteriorate.

[0092] Rz is preferably 20 nm or more, more preferably 30 nm or more, and even more preferably 40 nm or more, and is preferably 600 nm or less, more preferably 500 nm or less, and even more preferably 400 nm or less.

[0093] In this embodiment, the arithmetic mean height Ra of the contour curve of the coated surface is preferably 3 nm or more and 100 nm or less. Ra is one of the line roughness parameters defined in JIS B601, and is the average of the absolute values ​​of the peak heights and valley depths of the contour curve of a given length of the measurement surface (coated surface). Ra is expressed as the average line roughness over the entire contour curve, suppressing the influence of local irregularities such as Rz.

[0094] When Ra is within the above range in addition to Rz, both the voltage resistance and strength of the powder magnetic core are good, and the voltage resistance and strength of the powder magnetic core can be achieved at a high level. When Ra is outside the above range, one of the voltage resistance and strength of the powder magnetic core tends to be good.

[0095] Furthermore, in this embodiment, it is preferable that Rz and the thickness of the coating satisfy a predetermined relationship. Specifically, when the thickness of the coating is T [nm], it is preferable that Rz / T is 1.5 or more and 30 or less. By controlling Rz according to the thickness of the coating, it is possible to achieve both high levels of voltage resistance and strength of the powder magnetic core.

[0096] Rz / T is more preferably 1.8 or more, and even more preferably 2.0 or more, while Rz / T is more preferably 26 or less, and even more preferably 22 or less.

[0097] The thickness T of the covering portion 10 is not particularly limited as long as it satisfies the above-mentioned relationship. In this embodiment, T is preferably 3 nm or more and 200 nm or less. Also, T is more preferably 5 nm or more, and even more preferably 10 nm or more. Meanwhile, T is more preferably 70 nm or less, and even more preferably 50 nm or less.

[0098] The surface texture of the coating part described above can be measured as follows. When the surface of the coating part is expressed as an XY plane using mutually orthogonal X-axis and Y-axis, the surface texture of the coating part can be expressed as a displacement in the Z-axis direction perpendicular to the XY plane. In other words, the surface roughness of the coating part is expressed as a three-dimensional (X, Y, Z) shape.

[0099] Therefore, the maximum height Sz and the arithmetic mean height Sa, which are surface roughness parameters, are calculated from the measurement results of the displacement in the Z-axis direction in the measurement area. In this embodiment, when measuring the surface roughness of the coating portion formed on the soft magnetic metal particle in the soft magnetic metal powder, it is preferable to use an atomic force microscope (AFM), which is a type of scanning probe microscope.

[0100] AFM measures the unevenness of the sample surface by detecting the atomic force acting between the sample surface and the probe attached to the tip of the cantilever as the displacement of the cantilever. Because AFM has high measurement resolution, it is suitable for measuring Sz and Sa, which are on the order of nanometers.

[0101] The measurement results of the surface properties of the coated part obtained as 3D shape data mainly include factors caused by the shape of the coated part surface, factors caused by the surface roughness of the coated part surface, and factors caused by the waviness of the coated part surface. Therefore, the measurement results of the surface properties of the coated part are a contour curved surface obtained by combining these factors. These factors are distinguished by the length of the period (wavelength), with factors caused by surface roughness having a short period (shorter wavelength), factors caused by shape having a long period (longer wavelength), and factors caused by waviness having a period intermediate between the two.

[0102] In particular, since soft magnetic metal particles on which a coating is formed are usually spherical, depending on the particle diameter of the soft magnetic metal particles, the measurement results obtained are more curved than the measurement results obtained by measuring a plane.

[0103] Therefore, an operation is performed to remove factors due to shape and factors due to waviness from the obtained measurement results, and obtain a surface roughness surface consisting of factors due to surface roughness. Based on the obtained surface roughness surface, Sz and Sa are calculated in accordance with the method specified in ISO25178. That is, the measurements can be performed in the same manner as the method specified in ISO25178, but the measurements may be performed under conditions different from those described in ISO25178.

[0104] The operation of obtaining a surface roughness curve from the measurement results can be performed by known filtering, flattening, etc. For example, analysis software attached to the AFM or commercially available analysis software can be used.

[0105] In order to obtain a highly accurate surface roughness curved surface by appropriately removing factors due to shape and factors due to waviness, it is preferable to measure the surface of the coating part formed on a particle with a regular shape rather than measuring the surface of the coating part formed on a particle with an irregular or irregular shape. Therefore, in this embodiment, it is preferable to measure the surface properties of coated particles with high circularity in order to obtain highly accurate Sz and Sa.

[0106] In this embodiment, the size of the region for measuring the surface properties of the coating portion is preferably a rectangle with one side measuring 0.1 μm to 50 μm by 0.1 μm to 50 μm. The measurement of the surface properties of the coating portion is preferably performed at about 1 to 10 locations per coated particle. The measurement of the surface properties of the coating portion is preferably performed on 10 to 1000 coated particles. The average values ​​of Sz and Sa calculated from the respective measurement results are defined as the maximum height Sz and the arithmetic mean height Sa of the surface of the coating portion.

[0107] The maximum height Rz and the arithmetic mean height Ra are the line roughness. The line roughness is expressed as two-dimensional shape data (contour curve) of the surface on a specified reference length section. Therefore, Rz and Ra can be calculated from the contour curve of the coated surface.

[0108] In the three-dimensional shape data of the surface properties of the coating portion, the cross-sectional profile parallel to the Z axis represents the contour curve of the coating portion surface. Therefore, in this embodiment, the line roughness parameter of the coating portion formed on the soft magnetic metal particles in the soft magnetic metal powder may be calculated using the contour curve of the coating portion surface extracted from the three-dimensional shape data of the surface properties of the coating portion. In addition, the contour curve of the coating portion surface may be obtained using a known measuring device.

[0109] In addition, the soft magnetic metal particles in the powder core are bonded and fixed via resin. On the other hand, the surface roughness parameter needs to be measured with the measurement surface (coated surface) exposed. Therefore, when it is difficult to expose the coated surface, for example, when the coated surface is formed on the soft magnetic metal particles in the powder core, it is very difficult to measure the surface roughness of the coated surface.

[0110] Therefore, for example, the contour curve of the coating surface may be obtained in the cross section of the coated particle appearing in the cross section of the powder magnetic core, and the line roughness parameter may be calculated. Specifically, the cross section of the coated particle may be observed with a known electron microscope (scanning electron microscope: SEM, transmission electron microscope: TEM, etc.), and the coating may be identified based on, for example, the contrast difference in the observed image and the results of composition analysis. The outermost surface of the identified coating may be taken as the contour curve of the coating surface.

[0111] As with the contour surface, factors due to the shape and factors due to waviness are removed from the obtained contour curve to obtain a surface roughness curve consisting of factors due to surface roughness. Based on the obtained surface roughness curve, Rz and Ra are calculated in accordance with the method specified in JIS B601. That is, they can be measured by a method similar to the method specified in JIS B601, but they may also be measured under conditions different from those described in JIS B601.

[0112] The operation of obtaining a surface roughness curve from a contour curve can be performed by known filtering, flattening, etc., in the same manner as the operation of obtaining a surface roughness curve. For example, analysis software provided with the AFM or commercially available analysis software can be used.

[0113] Furthermore, similarly to Sz and Sa, in this embodiment, whether the coated particles are contained in a soft magnetic metal powder or fixed in a powder core, it is preferable to measure the surface properties of coated particles with high circularity in order to obtain highly accurate Rz and Ra.

[0114] In this embodiment, the reference length of the contour curve is preferably 0.1 μm to 50 μm. The contour curve of the coated portion is preferably measured at about 10 to 100 points per coated particle. The contour curve of the coated portion is preferably measured for 10 to 100 coated particles. The average values ​​of Rz and Ra calculated from the respective measurement results are defined as the maximum height Rz and the arithmetic mean height Ra on the surface of the coated portion.

[0115] The thickness T of the coating portion can be measured as follows. The cross section of the coated particle is observed with a known electron microscope (scanning electron microscope: SEM, transmission electron microscope: TEM, etc.), and the coating portion is identified based on, for example, the contrast difference in the observed image and the composition analysis results, and can be measured. In this embodiment, the thickness T of the coating portion is preferably measured at about 1 to 10 points per coated particle. In addition, the thickness T of the coating portion is preferably measured for 10 to 100 coated particles. The average thickness calculated from the respective measurement results is taken as the thickness T of the coating portion.

[0116] (2.Powder magnetic core) The dust core according to the present embodiment is not particularly limited as long as it contains the above-mentioned soft magnetic metal powder and is formed to have a predetermined shape. In the present embodiment, the dust core contains a soft magnetic metal powder and a resin as a binder, and the soft magnetic metal particles constituting the soft magnetic metal powder are fixed to a predetermined shape by being bonded to each other via the resin. The dust core may also be composed of a mixed powder of the above-mentioned soft magnetic metal powder and another magnetic powder, and formed into a predetermined shape.

[0117] (3. Magnetic parts) The magnetic component according to the present embodiment is not particularly limited as long as it includes the above-mentioned powder magnetic core. For example, it may be a magnetic component in which an air-core coil around which a wire is wound is embedded inside a powder magnetic core of a predetermined shape, or a magnetic component in which a wire is wound a predetermined number of times on the surface of a powder magnetic core of a predetermined shape. The magnetic component according to the present embodiment has good voltage resistance and is therefore suitable for a power inductor used in a power supply circuit.

[0118] (4. Manufacturing method of powder magnetic core) Next, a method for manufacturing the powder magnetic core included in the magnetic component will be described. First, a method for manufacturing the soft magnetic metal powder that constitutes the powder magnetic core will be described.

[0119] (4.1. Method for producing soft magnetic metal powder) The soft magnetic metal powder according to the present embodiment can be obtained using a method similar to that of a known method for producing soft magnetic metal powder. Specifically, it can be produced using a gas atomization method, a water atomization method, a rotating disk method, or the like. It may also be produced by mechanically pulverizing a thin ribbon obtained by a single roll method, or the like. Among these, it is preferable to use the gas atomization method from the viewpoint that a soft magnetic metal powder having the desired magnetic properties can be easily obtained.

[0120] In the gas atomization method, first, a molten metal is obtained by melting the raw material of the soft magnetic metal constituting the soft magnetic metal powder. Raw materials (pure metals, etc.) of each metal element contained in the soft magnetic metal are prepared, weighed so as to obtain the composition of the soft magnetic metal to be finally obtained, and the raw materials are melted. The method of melting the raw material of the metal elements is not particularly limited, but an example is a method of melting the raw material by high-frequency heating after evacuating the chamber of the atomization device. The temperature during melting may be determined taking into consideration the melting point of each metal element, and may be, for example, 1200 to 1500°C.

[0121] The obtained molten metal is supplied into the chamber as a linear continuous fluid through a nozzle provided at the bottom of the crucible, and high-pressure gas is sprayed onto the supplied molten metal to turn it into droplets and rapidly cool it to obtain fine powder. The gas injection temperature, pressure inside the chamber, etc. can be determined according to the composition and structure (crystalline, amorphous alloy, nanocrystalline alloy) of the soft magnetic metal. The particle size can be adjusted by sieve classification, air flow classification, etc.

[0122] The obtained powder contains soft magnetic metal particles made of a crystalline soft magnetic metal, or soft magnetic metal particles made of a soft magnetic metal that is an amorphous alloy. When the soft magnetic metal is made of a nanocrystalline alloy, it is preferable to heat-treat the powder containing soft magnetic metal particles made of an amorphous alloy in order to precipitate Fe-based nanocrystals. In this case, the powder may be made of a soft magnetic metal having a nanoheterostructure, or may be made of an amorphous alloy in which each metal element is uniformly dispersed in the amorphous.

[0123] In this embodiment, if the soft magnetic metal before heat treatment contains crystals with a crystal grain size of more than 30 nm, the soft magnetic metal is determined to be crystalline, and if the soft magnetic metal does not contain crystals with a crystal grain size of more than 30 nm, the soft magnetic metal is determined to be an amorphous alloy. Whether or not the soft magnetic metal contains crystals with a crystal grain size of more than 30 nm can be evaluated by a known method. For example, X-ray diffraction measurement, observation by TEM, etc. are exemplified. When using TEM, it can be confirmed by obtaining a selected area diffraction image or a nanobeam diffraction image. When using a selected area diffraction image or a nanobeam diffraction image, ring-shaped diffraction is formed in the diffraction pattern when the material is amorphous, whereas diffraction spots due to the crystalline structure are formed when the material is not amorphous.

[0124] The presence or absence of primary microcrystals and the average crystal grain size can be evaluated by any known method without any particular limitations. For example, a sample sliced ​​by ion milling can be confirmed by obtaining a bright field image or a high resolution image using a TEM. Specifically, the presence or absence of primary microcrystals can be confirmed by obtaining a bright field image or a high resolution image using a TEM at a magnification of 1.00×10 5 ~3.00×10 5 The presence or absence of primary microcrystals and the average crystal grain size can be evaluated by visually observing bright-field images or high-resolution images obtained at 370x magnification.

[0125] Next, the obtained powder is heat-treated as necessary. Heat treatment prevents the particles from sintering together and the powder from becoming coarse, while promoting the diffusion of the elements that make up the soft magnetic metal, allowing it to reach a thermodynamic equilibrium state in a short period of time and removing the distortion and stress that exist in the soft magnetic metal. As a result, it becomes easy to obtain a powder made of a soft magnetic metal in which Fe-based nanocrystals have precipitated.

[0126] In this embodiment, the heat treatment conditions are not particularly limited as long as they are conditions that facilitate precipitation of Fe-based nanocrystals. For example, the heat treatment temperature can be 400 to 700° C., and the holding time can be 0.5 to 10 hours.

[0127] After the heat treatment, a powder containing soft magnetic metal particles made of a soft magnetic metal in which Fe-based nanocrystals are precipitated is obtained.

[0128] Next, a coating portion is formed on the soft magnetic metal particles contained in the powder before or after the heat treatment. The method for forming the coating portion is not particularly limited, and a known method can be adopted. The coating portion may be formed by performing a wet treatment on the soft magnetic metal particles, or may be formed by performing a dry treatment on the soft magnetic metal particles. The coating portion may also be formed on the soft magnetic metal powder before the heat treatment.

[0129] In this embodiment, the coating portion can be formed by a mechanochemical coating method, a phosphate treatment method, a sol-gel method, or the like. In the mechanochemical coating method, for example, a powder coating apparatus 100 shown in FIG. 2 is used. A mixture of soft magnetic metal powder and a powdered coating material of the material constituting the coating portion (compounds of P, Al, Ca, Ba, Bi, Si, Cr, Na, Zn, etc.) is charged into a container 101 of the powder coating apparatus. After charging, the grinder 102 is rotated, whereby the mixture 50 of the soft magnetic metal powder and the powdered coating material is compressed between the grinder 102 and the inner wall of the container 101, causing friction and generating heat. The generated frictional heat softens the powdered coating material, and the powdered coating material is fixed to the surface of the soft magnetic metal particles by the compression action, forming the coating portion.

[0130] In the mechanochemical coating method, the temperature of the mixture of the soft magnetic metal powder and the powdered coating material can be controlled by adjusting the rotation speed of the container, the distance between the grinder and the inner wall of the container, etc., thereby controlling the generated frictional heat. In this embodiment, the temperature is preferably 50°C or higher and 150°C or lower. By setting the temperature within this range, the coating portion can be easily formed to cover the surface of the soft magnetic metal particles. In addition, by adjusting the coating time, it tends to be easier to control the surface roughness of the coating portion, particularly Sz and Rz. Furthermore, by adjusting the mixing ratio of the soft magnetic metal powder and the powder of the material that constitutes the coating portion, the coating can be easily controlled. PartThis tends to make it easier to control the thickness T.

[0131] If necessary, the powder after the formation of the coating portion may be heat-treated. The heat treatment softens the material constituting the coating portion, and tends to facilitate control of the surface roughness of the coating portion, particularly Sa and Ra. For example, when the heat treatment temperature is increased or the heat treatment time is increased, Sa and Ra tend to decrease.

[0132] (4.2. Manufacturing method of powder core) The dust core is manufactured using the soft magnetic metal powder. The specific manufacturing method is not particularly limited, and a known method can be adopted. First, a soft magnetic metal powder containing soft magnetic metal particles having a coating portion formed thereon is mixed with a known resin as a binder to obtain a mixture. If necessary, the obtained mixture may be made into a granulated powder. Then, the mixture or the granulated powder is filled into a die and compression molded to obtain a molded body having the shape of the dust core to be manufactured. Since the soft magnetic metal particles have a high sphericity, the soft magnetic metal particles are densely packed in a die by compression molding a powder containing the soft magnetic metal particles, and a dust core with a high density can be obtained.

[0133] The obtained compact is subjected to a heat treatment at, for example, 50 to 200° C., whereby the resin hardens to obtain a powder magnetic core of a predetermined shape in which the soft magnetic metal particles are fixed via the resin. A magnetic part such as an inductor is obtained by winding a wire around the obtained powder magnetic core a predetermined number of times.

[0134] Alternatively, the mixture or granulated powder and an air-core coil formed by winding a wire a predetermined number of times may be filled into a mold and compressed to obtain a compact with the coil embedded therein. The compact thus obtained is subjected to a heat treatment to obtain a powder core of a predetermined shape with the coil embedded therein. Since such a powder core has a coil embedded therein, it functions as a magnetic part such as an inductor.

[0135] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES

[0136] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0137] (Experiment 1) First, the raw metal of the soft magnetic metal was prepared. The prepared raw metal was weighed to have a predetermined composition, and was placed in a crucible arranged in an atomizing device. Next, after the chamber was evacuated, the crucible was heated by high-frequency induction using a work coil provided outside the crucible, and the raw metal in the crucible was melted and mixed to obtain a molten metal (molten metal) at 1250°C. In Examples 1 to 35 and Comparative Examples 1 and 2, the composition of the soft magnetic metal was Fe-7.6Si-2.3B-7.3Nb-1.1Cu. In Example 36, the composition of the soft magnetic metal was Fe-6.5Si-2.6B-2.5Cr. In Example 37, the composition of the soft magnetic metal was Fe-4.5Si. Note that Fe-4.5Si indicates a composition containing 95.5 mass% Fe and 4.5 mass% Si. The other compositions are similar.

[0138] The obtained molten metal was supplied into the chamber as a linear continuous fluid through a nozzle provided at the bottom of the crucible, and gas was blown onto the supplied molten metal to obtain powder. The gas injection temperature was 1250°C, and the pressure inside the chamber was 1 hPa. The average particle size (D50) of the obtained powder was 20 μm. The average circularity of the cross section of the particles contained in the obtained powder was 0.80 to 0.90.

[0139] The obtained powder was subjected to X-ray diffraction measurement to confirm the presence or absence of crystals having a crystal grain size of more than 30 nm. If no crystals having a crystal grain size of more than 30 nm exist, it was determined that the soft magnetic metal constituting the powder was made of an amorphous alloy, and if crystals having a crystal grain size of more than 30 nm exist, it was determined that the soft magnetic metal was made of a crystalline material. The results are shown in Table 1. In Example 36, the average crystal grain size of the initial microcrystals was 2 nm.

[0140] Next, the powders of Examples 1 to 35 and Comparative Examples 1 and 2 were heat-treated. The heat treatment conditions were a heat treatment temperature of 600°C and a holding time of 1 hour. X-ray diffraction measurement and TEM observation were performed on the heat-treated powders to evaluate the presence or absence of Fe-based nanocrystals. The results are shown in Table 1. In the examples in which Fe-based nanocrystals were present, it was confirmed that the crystal structure of the Fe-based nanocrystals was a bcc structure and the average crystal grain size was 5 to 30 nm.

[0141] Next, the powders of Examples 1 to 37 and Comparative Examples 1 and 2 were charged into a container of a powder coating device together with a powder coating material having the properties shown in Table 1, and the powder coating material was coated on the surface of the particles to form a coating portion, thereby obtaining a soft magnetic metal powder. The amount of powder coating material added was set to 0.01 to 3 mass% relative to 100 mass% of the powder after the heat treatment. The coating time was 0.1 to 8 hours, and the temperature of the mixture of the powder and the powder coating material after the heat treatment was 50 to 150°C. The percentage of the number of coated particles in the powder after the coating portion was formed was 85 to 95%.

[0142] In Examples 1 to 25, 36, and 37 and Comparative Examples 1 and 2, a phosphate-based glass having a composition of P2O5-ZnO-R2O-Al2O3 was used as the powdered coating material. The specific composition was 50 mass% P2O5, 12 mass% ZnO, 20 mass% R2O, 6 mass% Al2O3, and the remainder were accessory components.

[0143] The inventors have also conducted similar experiments on glass having a composition of 60 mass % P2O5, 20 mass % ZnO, 10 mass % R2O, 5 mass % Al2O3, and the remainder being minor components, and have confirmed that similar results to those described below were obtained.

[0144] The surface properties of the soft magnetic metal particles on which the coating was formed were measured as follows. A scanning probe microscope (AFM5100N manufactured by Hitachi High-Tech Science Corporation) was used as the measuring device. The cantilever used was the SI-DF40 manufactured by the same company (spring constant: 42 N / m, resonance frequency: 250 to 390 kHz), and the radius of curvature of the tip of the probe was 10 nm.

[0145] The atomic force microscope was set to the dynamic force mode, and a square area of ​​5 μm x 5 μm was selected on the surface of the coating of a soft magnetic metal particle with a circularity of 0.98 or more, and measurements were performed on that area. Measurements were performed on 30 particles. Based on ISO25178, the obtained surface property data was subjected to third-order tilt correction using the software provided with the atomic force microscope, and then Sz and Sa for each area were calculated. The results are shown in Table 1.

[0146] The thickness T of the coating was measured for soft magnetic metal particles having a coating formed thereon as follows. The cross section of the particle was observed by TEM, and the coating was identified based on the contrast difference in the observed image. The thickness was measured at 10 points in the identified coating. The thickness was measured for 10 particles, and the average of the measured thicknesses was taken as the thickness T of the coating. The results are shown in Table 1.

[0147] Next, a dust core was produced. The epoxy resin, which is a thermosetting resin, and the imide resin, which is a curing agent, were weighed out so that the total amount was 3% by mass relative to 100% by mass of the obtained soft magnetic metal powder, and were added to acetone to form a solution, and the solution was mixed with the soft magnetic metal powder. After mixing, the acetone was evaporated to obtain granules, which were then sized using a 355 μm mesh. This was filled into a toroidal mold with an outer diameter of 11 mm and an inner diameter of 6.5 mm, and molded at a molding pressure of 3.0 t / cm. 2The resin in the resulting powder core compact was cured at 180° C. for 1 hour to obtain a powder core.

[0148] The strength of the obtained powder magnetic core was measured as follows. A strength tester (Model-1311D manufactured by Aiko Engineering) was used as the measuring device. Using the strength tester, a load was applied to the powder magnetic core in the radial direction, and the radial crushing strength of the powder magnetic core was calculated using the following formula from the load P [kgf] at which the powder magnetic core broke. If the outer diameter of the powder magnetic core is D, the thickness calculated from the difference between the outer diameter and the inner diameter is A, and the length of the powder magnetic core is L, then the radial crushing strength K [MPa] is given by K=P(DA) / LA. 2 In this example, samples with a radial crushing strength of 15 MPa or more were judged to be good. The results are shown in Table 1.

[0149] In addition, In-Ga electrodes were formed on both ends of the obtained powder core sample, and a voltage was applied to both ends using a voltage boosting breakdown tester (THK-2011ADMPT manufactured by Tama Densoku Co., Ltd.), and the withstand voltage was calculated from the voltage value at which a current of 1 mA flowed and the length L of the powder core. In this example, samples with a withstand voltage of 80 V / mm or more were determined to be good. The results are shown in Table 1.

[0150] [Table 1]

[0151] It was confirmed from Table 1 that when Sz is within the above-mentioned range, the powder magnetic core has good strength and voltage resistance.

[0152] In contrast, it was confirmed that when Sz was outside the above range, one of the strength and voltage resistance of the powder magnetic core was deteriorated.

[0153] (Experiment 2) Based on JIS B601, third-order tilt correction was performed using the software attached to the atomic force microscope from the obtained surface property data, and then Rz and Ra in each region were calculated. Except for this, soft magnetic metal powder was produced in the same manner as in Experiment 1 and evaluated in the same manner as in Experiment 1. In addition, a dust core was produced using the obtained powder in the same manner as in Experiment 1 and evaluated in the same manner as in Experiment 1. The results are shown in Table 2.

[0154] In Examples 38 to 54, 209 to 226 and Comparative Examples 3 and 4, the soft magnetic metal had a composition of Fe-7.6Si-2.3B-7.3Nb-1.1Cu. In Example 227, the soft magnetic metal had a composition of Fe-6.5Si-2.6B-2.5Cr. In Example 228, the soft magnetic metal had a composition of Fe-4.5Si.

[0155] In Examples 38 to 54, 209 to 216, 227, and 228 and Comparative Examples 3 and 4, a phosphate-based glass having a composition of P2O5-ZnO-R2O-Al2O3 was used as the powdered coating material. The specific composition was 50 mass% P2O5, 12 mass% ZnO, 20 mass% R2O, 6 mass% Al2O3, and the remainder were accessory components.

[0156] The inventors have also conducted similar experiments on glass etc. having a composition of 60 mass % P2O5, 20 mass % ZnO, 10 mass % R2O, 5 mass % Al2O3, with the remainder being minor components, and have confirmed that the same results as those described below were obtained for Rz and Ra.

[0157] [Table 2]

[0158] From Table 2, it was confirmed that when Rz is within the above-mentioned range, the powder magnetic core has both good strength and good voltage resistance.

[0159] In contrast, it was confirmed that when Rz was outside the above range, one of the strength and voltage resistance of the powder magnetic core was deteriorated.

[0160] (Experiment 3) A soft magnetic metal powder was produced in the same manner as in Example 1 of Experiment 1, except that the proportion of the number of coated particles was set to the value shown in Table 3, and the same evaluations were performed as in Experiment 1. In addition, a dust core was produced using the obtained powder in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 3.

[0161] In addition, soft magnetic metal powder was produced in the same manner as in Example 1 of Experiment 1, except that the average circularity of the soft magnetic metal particles was set to the value shown in Table 4, and the same evaluations were performed as in Experiment 1. In addition, a dust core was produced using the obtained powder in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 4.

[0162] Furthermore, soft magnetic metal powders were produced in the same manner as in Example 1 of Experiment 1, except that the average particle diameter of the soft magnetic metal powders was set to the values ​​shown in Table 5, and the same evaluations were performed as in Experiment 1. Furthermore, using the obtained powders, dust cores were produced in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 5. In Examples 55 to 65, the composition of the soft magnetic metal and the material of the powdered coating material were the same as in Example 1.

[0163] [Table 3]

[0164] [Table 4]

[0165] [Table 5]

[0166] From Tables 3 to 5, it can be seen that when the surface roughness is within the above-mentioned range, as well as the number ratio of coated particles, the average circularity of soft magnetic metal particles, and the average particle diameter of the soft magnetic metal powder are within the above-mentioned ranges, both the strength and voltage resistance of the powder magnetic core are even better.

[0167] (Experiment 4) A soft magnetic metal powder was produced in the same manner as in Example 36 of Experiment 1, except that the average crystal grain size of the primary crystallites was set to the value shown in Table 6, and the same evaluations were performed as in Experiment 1. Furthermore, using the obtained powder, a dust core was produced in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 6. In Examples 66 to 70, the composition of the soft magnetic metal and the material of the powdered coating material were the same as in Example 36.

[0168] Furthermore, soft magnetic metal powder was produced in the same manner as in Example 1 of Experiment 1, except that the average crystal particle size of the nanocrystals was set to the value shown in Table 7, and the same evaluations were performed as in Experiment 1. Furthermore, using the obtained powder, a dust core was produced in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 7. In Examples 71 to 75, the composition of the soft magnetic metal and the material of the powdered coating material were the same as in Example 1.

[0169] [Table 6]

[0170] [Table 7]

[0171] Tables 6 and 7 confirm that when the surface roughness is within the above-mentioned range, and the average crystal grain size of the primary microcrystals and the average crystal grain size of the nanocrystals are within the above-mentioned ranges, it is possible to achieve high levels of both strength and voltage resistance of the powder magnetic core.

[0172] (Experiment 5) A soft magnetic metal powder was prepared in the same manner as in Example 1 of Experiment 1, except that the amount of P2O5 in the P2O5-ZnO-R2O-Al2O3 glass was set to the value shown in Table 8, and the same evaluations were performed as in Experiment 1. Furthermore, using the obtained powder, a dust core was prepared in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 8. In Examples 76 to 78, the composition of the soft magnetic metal was the same as in Example 1.

[0173] In addition, soft magnetic metal powder was produced in the same manner as in Example 1 of Experiment 1, except that the P2O5-ZnO-R2O-Al2O3 glass was changed to Bi2O3-ZnO-B2O3-SiO2 glass or BaO-ZnO-B2O3-SiO2-Al2O3 glass, and the same evaluation as in Experiment 1 was performed. In addition, a dust core was produced in the same manner as in Experiment 1 using the obtained powder, and the same evaluation as in Experiment 1 was performed. The results are shown in Tables 9 and 10. In Examples 79 to 84, the composition of the soft magnetic metal was the same as in Example 1. In addition, the composition of the Bi2O3-ZnO-B2O3-SiO2 glass was 40 to 60 mass% Bi2O3, 10 to 15 mass% ZnO, 15 to 25 mass% B2O3, 15 to 20 mass% SiO2, and the remainder was a secondary component. The composition of the BaO-ZnO-B2O3-SiO2-Al2O3 glass was 35-40 mass% BaO, 30-40 mass% ZnO, 5-15 mass% B2O3, 5-15 mass% SiO2, 5-10 mass% Al2O3, and the remainder were accessory components.

[0174] [Table 8]

[0175] [Table 9]

[0176] [Table 10]

[0177] Tables 8 to 10 confirm that when the surface roughness is within the above-mentioned range, and when the oxide glass is the above-mentioned glass, and when the composition of the oxide glass is within the above-mentioned range, it is possible to achieve high levels of both strength and voltage resistance of the powder magnetic core.

[0178] (Experiment 6) A soft magnetic metal powder was produced in the same manner as in Example 36 of Experiment 1, except that the composition of the soft magnetic metal was the composition shown in Tables 11 and 12, and the same evaluations were performed as in Experiment 1. In addition, a dust core was produced in the same manner as in Experiment 1 using the obtained powder, and the same evaluations were performed as in Experiment 1. The results are shown in Tables 11 and 12. In Examples 85 to 142, the soft magnetic metal was an amorphous alloy, and the average crystal grain size of the primary crystallites was 0.3 to 10 nm. In addition, the material of the powdered coating material was the same as in Example 1.

[0179] [Table 11]

[0180] [Table 12]

[0181] (Experiment 7) A soft magnetic metal powder was produced in the same manner as in Example 1 of Experiment 1, except that the composition of the soft magnetic metal was the composition shown in Tables 13 to 15, and the same evaluations were performed as in Experiment 1. Furthermore, using the obtained powder, a dust core was produced in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Tables 13 to 15. In Examples 143 to 208, the soft magnetic metal was a nanocrystalline alloy, and the average crystal grain size of the nanocrystals was 5 to 30 nm. Furthermore, the material of the powdered coating material was the same as in Example 1.

[0182] [Table 13]

[0183] [Table 14]

[0184] [Table 15]

[0185] Tables 11 to 15 confirm that when the surface roughness is within the above-mentioned range and the composition of the soft magnetic metal is within the above-mentioned range, it is possible to achieve high levels of both strength and voltage resistance of the powder magnetic core.

[0186] (Experiment 8) A soft magnetic metal powder was produced in the same manner as in Example 38 of Experiment 2, except that the number ratio of the coated particles was set to the value shown in Table 16, and the same evaluations were performed as in Experiment 2. That is, Rz and Ra were calculated. In addition, a dust core was produced using the obtained powder in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 16.

[0187] In addition, soft magnetic metal powder was produced in the same manner as in Example 38 of Experiment 2, except that the average circularity of the soft magnetic metal particles was set to the value shown in Table 17, and the same evaluations were performed as in Experiment 2. In addition, a dust core was produced using the obtained powder in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 17.

[0188] In addition, soft magnetic metal powder was produced in the same manner as in Example 38 of Experiment 2, except that the average particle diameter of the soft magnetic metal powder was set to the value shown in Table 18, and the same evaluations were performed as in Experiment 2. Furthermore, using the obtained powder, a dust core was produced in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 18. In Examples 229 to 239, the composition of the soft magnetic metal and the material of the powdered coating material were the same as in Example 38.

[0189] [Table 16]

[0190] [Table 17]

[0191] [Table 18]

[0192] From Tables 16 to 18, it can be seen that when the line roughness is within the above-mentioned range, and the number ratio of coated particles, the average circularity of soft magnetic metal particles, and the average particle diameter of the soft magnetic metal powder are within the above-mentioned ranges, both the strength and voltage resistance of the powder magnetic core are even better.

[0193] (Experiment 9) A soft magnetic metal powder was produced in the same manner as in Example 227 of Experiment 2, except that the average crystal grain size of the primary crystallites was set to the value shown in Table 19, and the same evaluations were performed as in Experiment 2. Furthermore, using the obtained powder, a dust core was produced in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 19. In Examples 240 to 244, the composition of the soft magnetic metal and the material of the powdered coating material were the same as in Example 227.

[0194] In addition, soft magnetic metal powder was produced in the same manner as in Example 38 of Experiment 2, except that the average crystal particle size of the nanocrystals was set to the value shown in Table 20, and the same evaluations were performed as in Experiment 2. Furthermore, using the obtained powder, a dust core was produced in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 20. In Examples 245 to 249, the composition of the soft magnetic metal and the material of the powdered coating material were the same as in Example 38.

[0195] [Table 19]

[0196] [Table 20]

[0197] From Tables 19 and 20, it can be seen that when the line roughness is within the above-mentioned range, and the average crystal grain size of the primary crystallites and the average crystal grain size of the nanocrystals are within the above-mentioned ranges, both the strength and voltage resistance of the powder magnetic core can be achieved at high levels.

[0198] (Experiment 10) A soft magnetic metal powder was prepared in the same manner as in Example 38 of Experiment 2, except that the amount of P2O5 in the P2O5-ZnO-R2O-Al2O3 glass was set to the value shown in Table 21, and the same evaluations were performed as in Experiment 2. Furthermore, using the obtained powder, a dust core was prepared in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 21. In Examples 250 to 252, the composition of the soft magnetic metal was the same as in Example 38.

[0199] In addition, soft magnetic metal powder was produced in the same manner as in Example 38 of Experiment 2, except that the P2O5-ZnO-R2O-Al2O3 glass was changed to Bi2O3-ZnO-B2O3-SiO2 glass or BaO-ZnO-B2O3-SiO2-Al2O3 glass, and the same evaluations were performed as in Experiment 2. In addition, a dust core was produced using the obtained powder in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Tables 22 and 23.

[0200] In Examples 253 to 258, the composition of the soft magnetic metal was the same as that of Example 38. In Examples 253 to 255, the composition of the Bi2O3-ZnO-B2O3-SiO2 glass was 40 to 60 mass% Bi2O3, 10 to 15 mass% ZnO, 15 to 25 mass% B2O3, 15 to 20 mass% SiO2, and the remainder was an auxiliary component. In Examples 256 to 258, the composition of the BaO-ZnO-B2O3-SiO2-Al2O3 glass was 35 to 40 mass% BaO, 30 to 40 mass% ZnO, 5 to 15 mass% B2O3, 5 to 15 mass% SiO2, and 5 to 10 mass% Al2O3, and the remainder was an auxiliary component.

[0201] [Table 21]

[0202] [Table 22]

[0203] [Table 23]

[0204] From Tables 21 to 23, it can be seen that when the line roughness is within the above-mentioned range, and when the oxide glass is the above-mentioned glass, and when the composition of the oxide glass is within the above-mentioned range, both the strength and voltage resistance of the powder magnetic core can be achieved at high levels.

[0205] (Experiment 11) A soft magnetic metal powder was prepared in the same manner as in Example 227 of Experiment 2, except that the composition of the soft magnetic metal was the composition shown in Tables 24 and 25, and the same evaluation as in Experiment 2 was performed. In addition, a dust core was prepared in the same manner as in Experiment 1 using the obtained powder, and the same evaluation as in Experiment 1 was performed. The results are shown in Tables 24 and 25. In Examples 259 to 316, the soft magnetic metal was an amorphous alloy, and the average crystal grain size of the primary crystallites was 0.3 to 10 nm. In addition, the material of the powdered coating material was the same as in Example 227.

[0206] [Table 24]

[0207] [Table 25]

[0208] (Experiment 12) A soft magnetic metal powder was produced in the same manner as in Example 38 of Experiment 2, except that the composition of the soft magnetic metal was the composition shown in Tables 26 to 28, and the same evaluations were performed as in Experiment 2. Furthermore, using the obtained powder, a dust core was produced in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Tables 26 to 29. In addition, in Examples 317 to 382, ​​the soft magnetic metal was a nanocrystalline alloy, and the average crystal grain size of the nanocrystals was 5 to 30 nm. Furthermore, the material of the powdered coating material was the same as in Example 38.

[0209] [Table 26]

[0210] [Table 27]

[0211] [Table 28]

[0212] Tables 24 to 28 confirm that when the line roughness is within the above-mentioned range and the composition of the soft magnetic metal is within the above-mentioned range, both the strength and voltage resistance of the powder magnetic core can be achieved at high levels.

[0213] (Experiment 13) Soft magnetic metal powder was prepared by the same method as in Example 1 of Experiment 1, and the surface roughness (Sz and Sa) and line roughness (Rz and Ra) of the soft magnetic metal particles on which the coating portion was formed were calculated using the same measuring device and under the same measuring conditions as in Experiments 1 and 2. In addition, a dust core was prepared by the same method as in Experiment 1 using the obtained powder, and the same evaluations were performed as in Experiment 1. The results are shown in Table 29.

[0214] [Table 29]

[0215] From Table 29, it can be seen that the surface roughness and line roughness correspond to each other, and that when the surface roughness is within the above-mentioned range, and when the line roughness is within the above-mentioned range, the strength and voltage resistance of the powder magnetic core can be achieved at the same time.

[0216] (Experiment 14) A soft magnetic metal powder was produced in the same manner as in Example 1 of Experiment 1, except that the coverage of the coated particles was set to the value shown in Table 30, and the same evaluations were performed as in Experiment 1. In addition, a dust core was produced using the obtained powder in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 30.

[0217] In addition, soft magnetic metal powder was produced in the same manner as in Example 38 of Experiment 2, except that the coverage of the coated particles was set to the value shown in Table 31, and the same evaluations were performed as in Experiment 2. In addition, a dust core was produced using the obtained powder in the same manner as in Experiment 1, and the same evaluations were performed as in Experiment 1. The results are shown in Table 31.

[0218] The coverage was measured as follows. The coverage of the soft magnetic metal particles on which the coating was formed was measured as follows. A scanning electron microscope (SU5000 manufactured by Hitachi High-Tech Science Corporation) was used as the measuring device. The observation mode of the scanning electron microscope was set to composition image, and a square area of ​​100 μm×100 μm was selected to obtain a composition image of the area. Composition images were obtained for 10 locations. The obtained composition image was binarized using commercially available image analysis software so that the coated area was black and the area where the uncoated metal was exposed was white, and the ratio of the area of ​​the coated area to the total area of ​​the particle was taken as the coverage.

[0219] [Table 30]

[0220] [Table 31]

[0221] From Table 30, it can be seen that when the surface roughness is within the above-mentioned range and the coverage rate of the coated particles is within the above-mentioned range, both the strength and voltage resistance of the powder magnetic core can be achieved at high levels.

[0222] Furthermore, from Table 31, it was confirmed that when the line roughness is within the above-mentioned range and the covering rate of the coated particles is within the above-mentioned range, both the strength and voltage resistance of the powder magnetic core can be achieved at high levels. [Explanation of symbols]

[0223] 1…Coated particles 10…Covering part 2...Soft magnetic metal particles

Claims

1. A soft magnetic metal powder comprising a plurality of soft magnetic metal particles containing iron, The average circularity of the cross section of the soft magnetic metal particles is 0.80 or more, The surface of the soft magnetic metal particle is covered with an insulating coating portion, the coating portion contains an oxide of at least one element selected from the group consisting of phosphorus, aluminum, calcium, barium, bismuth, silicon, chromium, sodium, and zinc, The soft magnetic metal powder has a maximum height Sz of 10 nm or more and 700 nm or less on the surface of the coating portion.

2. 2. The soft magnetic metal powder according to claim 1, wherein the arithmetic mean height Sa of the surface of the coating portion is 3 nm or more and 50 nm or less.

3. The soft magnetic metal powder according to claim 1 or 2, wherein Sz / T is 1.5 or more and 30 or less, where T [nm] is the thickness of the coating portion.

4. A soft magnetic metal powder comprising a plurality of soft magnetic metal particles containing iron, The average circularity of the cross section of the soft magnetic metal particles is 0.80 or more, The surface of the soft magnetic metal particle is covered with an insulating coating portion, the coating portion contains an oxide of at least one element selected from the group consisting of phosphorus, aluminum, calcium, barium, bismuth, silicon, chromium, sodium, and zinc, The soft magnetic metal powder has a maximum height Rz of 10 nm or more and 700 nm or less on the surface of the coating portion.

5. 5. The soft magnetic metal powder according to claim 4, wherein the arithmetic mean roughness Ra of the surface of the coating portion is 3 nm or more and 100 nm or less.

6. The soft magnetic metal powder according to claim 4 or 5, wherein Rz / T is 1.5 or more and 30 or less, where T [nm] is the thickness of the coating portion.

7. The soft magnetic metal powder according to claim 1 , wherein the thickness of the coating portion is T [nm], T is 3 nm or more and 200 nm or less.

8. The soft magnetic metal powder according to any one of claims 1 to 7, wherein the soft magnetic metal particles are made of an amorphous alloy.

9. The soft magnetic metal powder according to claim 1 , wherein the soft magnetic metal particles are made of a nanocrystalline alloy.

10. A dust core comprising the soft magnetic metal powder according to any one of claims 1 to 9.

11. A magnetic component comprising the powder magnetic core according to claim 10.

Citation Information

Patent Citations

  • Method for producing soft magnetic material, soft magnetic material and dust core

    JP2007092120A

  • Metallic glass compact and method for manufacturing the same

    JP2010138439A

  • Amorphous alloy powder for power inductor having insulation coating layer, and manufacturing method of the same

    JP2015132010A

  • Soft magnetic alloy powder, powder magnetic core, and magnetic component

    JP2019157187A