Spherical AlN particles, their manufacturing method, and composite materials containing the same

By adding Zr to alumina powder and using a nitriding process with carbon, spherical AlN particles with smooth surfaces are produced, addressing the issue of poor fluidity and enhancing thermal conductivity in thermal interface materials.

JP7588481B2Active Publication Date: 2024-11-22NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2020139334
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-20
Publication Date
2024-11-22
Estimated Expiration
2040-08-20

AI Technical Summary

Technical Problem

Conventional methods for producing aluminum nitride (AlN) particles result in uneven surfaces, leading to poor fluidity and filling properties when incorporated into resins, which hinders the improvement of thermal conductivity in thermal interface materials.

Method used

The production of spherical AlN particles is achieved by adding Zr atoms to alumina powder in a specific molar ratio, followed by a nitriding process with carbon powder, resulting in smooth particle surfaces and enhanced fluidity.

Benefits of technology

The resulting spherical AlN particles exhibit superior fluidity and can be highly filled into resins, offering improved thermal conductivity and suitability for thermal interface materials, especially in power devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588481000003
    Figure 0007588481000003
  • Figure 0007588481000004
    Figure 0007588481000004
  • Figure 0007588481000005
    Figure 0007588481000005
Patent Text Reader

Abstract

To provide a filler which has a particle surface made to be smooth so as to increase in a filling property, in an aluminum nitride particle excellent in high heat conductivity and useful as a filler for a heat-dissipating material.SOLUTION: A spherical AlN particle contains an Al atom and a Zr atom at an amount of a mole ratio of the Zr atom to the Al atom of Zr / Al=4.0×10-4 to 4.2×10-2 and has an AlN conversion ratio of 70.0% or more and a degree of circularity of 0.85 to 1.00.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to spherical aluminum nitride (AlN) particles and a method for producing the same, as well as a composite material containing spherical AlN particles and used in thermal interface materials such as heat dissipation sheets. [Background technology]

[0002] As the power density of semiconductor devices increases in recent years, materials used in these devices are required to have more advanced heat dissipation properties. Heat dissipation materials include a series of materials called thermal interface materials (hereinafter simply referred to as "TIM"), and their usage is rapidly expanding. TIMs are materials that reduce the thermal resistance of the path that dissipates heat generated by semiconductor devices to a heat sink or housing, and are used in a variety of forms such as sheets, gels, and greases.

[0003] Generally, TIM is a composite material in which a thermally conductive filler is dispersed in a resin such as epoxy or silicone. Metal oxides such as silica and alumina are often used as such thermally conductive fillers. However, sheet-shaped molded products made of composite materials using metal oxides have a thermal conductivity in the thickness direction of about 1 to 3 W / m·K, and sheet-shaped molded products with higher thermal conductivity are required. Therefore, as the next-generation thermally conductive filler material to be used in such sheet-shaped molded products, it is expected that the practical application of nitride-based high thermal conductive fillers such as boron nitride, aluminum nitride, and silicon nitride will be promoted. Among them, aluminum nitride (AlN) is expected to be used as a heat dissipation material because it has excellent electrical insulation and high thermal conductivity. In order to improve the thermal conductivity of heat dissipation materials, it is important to highly fill the resin matrix with aluminum nitride, which has a high crystallinity and a solid structure.

[0004] Various methods for producing AlN particles have been proposed in the past. For example, Patent Document 1 proposes a method for producing spherical aluminum nitride powder, which is characterized in that spherical granules of alumina (Al2O3) powder or alumina hydrate (Al2O3·nH2O) powder are used as a starting material and fed to a reduction-nitridation step to carry out reduction-nitridation.

[0005] Patent Document 2 proposes a method for producing spherical aluminum nitride powder, which comprises reducing and nitriding a composition containing 100 parts by mass of alumina or alumina hydrate, 0.5 to 30 parts by mass of a compound containing a rare earth metal element, and 38 to 46 parts by mass of carbon powder, at a temperature of 1620 to 1900°C for 2 hours or more.

[0006] Patent Document 3 proposes spherical AlN particles and a method for producing the same, characterized in that the particles contain 0.01 to 0.5 wt% Y, calculated as Y2O3, 0.01 to 0.5 wt% Si, calculated as SiO2, and AlN, with the weight ratio of the entire particle being 100 wt%, the AlN content being 60 wt% or more, the particles have a relative density of 90% or more of the theoretical density, and a circularity of 0.85 to 1.00.

[0007] Patent Document 4 proposes spherical AlN particles and a method for producing the same, which are spherical particles containing a compound of one or more of La, Dy, and Er, a compound of Si, and AlN in a specific ratio, and are characterized by having a relative density of 90% or more of the theoretical density and a circularity of 0.85 to 1.00.

[0008] A method for obtaining AlN particles is known to be the nitriding of spherical alumina particles, but when producing AlN particles by the nitriding reduction method, previously, AlN particles with uneven surfaces were generated due to grain growth.When these AlN particles were incorporated into resin as a filler to make a composite material, the uneven surface reduced the fluidity of the filler, making it difficult to improve the filling ability of the resin. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] International Publication No. 2011 / 093488 [Patent Document 2] JP 2012-72013 A [Patent Document 3] JP 2017-178751 A [Patent Document 4] JP 2017-178752 A Summary of the Invention [Problem to be solved by the invention]

[0010] The inventors of the present invention conducted intensive research aimed at solving the above problems and discovered that, when producing AlN particles by a nitriding reduction method, spherical AlN particles with excellent surface smoothness can be produced by mixing alumina powder, alumina hydrate powder, or a mixture thereof with a raw powder of a Zr compound in a specific ratio. As a result, they discovered that when kneaded with a resin to produce a composite material, spherical AlN particles with better flowability than conventional ones and applicable as a TIM can be realized.

[0011] An object of the present invention is to provide aluminum nitride particles which have excellent thermal conductivity and are useful as a filler for heat dissipation materials, and which have a smooth particle surface in order to improve packing properties, and to provide a method for producing the same. [Means for solving the problem]

[0012] The gist of the present invention is as follows. [1] Zr atoms per Al atom, molar ratio Zr / Al = 4.0 x 10 -4 ~4.2×10 -2 Contains in amounts of It consists of sintered particles The spherical AlN particles have an AlN conversion rate of 70.0% or more and a circularity of 0.85 to 1.00. [2] The spherical AlN particles according to [1], characterized in that the AlN conversion rate is 90.0% or more. [3] A composite material of resin and spherical AlN particles, characterized in that the spherical AlN particles according to [1] or [2] above are contained in a resin. [4] A method for producing the spherical AlN particles according to [1] or [2], comprising the steps of: a raw material mixing step of mixing an alumina raw material powder having one or both of an alumina powder and an alumina hydrate powder having an average particle size (D50) of 0.05 to 4.00 μm with a raw material powder of a Zr compound in an amount of 0.10 to 10.00 mass% calculated as a ZrO2 component, based on 100 mass% of the alumina raw material powder calculated as an alumina component; A granulation step for converting the mixture produced in the raw material mixing step into spherical granules; a carbon powder mixing step of mixing the spherical granules with carbon powder; The mixture obtained in the carbon powder mixing step is subjected to a nitrogen-containing atmosphere. Temperature: 1700℃~1800℃ Nitriding process in which heat treatment is performed A method for producing spherical AlN particles, comprising: [5] The method for producing spherical AlN particles described in [4] above, characterized in that the ratio of carbon powder to be mixed with the spherical granules in the carbon powder mixing step is 20.0 to 40.0 mass % relative to 100 mass % of the alumina raw material powder in the spherical granules, calculated as the alumina component. [6] The method for producing spherical AlN particles according to [4] or [5], characterized in that in the raw material mixing step, 0.3 to 2.1 mass% of carbon powder is further mixed into the alumina raw material powder, with the alumina raw material powder being calculated as 100 mass% of the alumina component. Effect of the Invention

[0013] Because the spherical AlN particles of the present invention have a smooth particle surface, they have better fluidity than conventional particles and can be highly loaded into resins as spherical AlN particle fillers that can be used as TIMs. They can be used as TIMs, and are particularly suitable as spherical AlN fillers in the TIM field for power devices, etc. [Brief description of the drawings]

[0014] [Figure 1] 13 is an XRD pattern of a powder made of spherical AlN particles according to the present invention in Example 10. [Diagram 2] 13 is an XRD pattern of a powder made of spherical AlN particles in Comparative Example 4. [Diagram 3] 4 is an SEM image showing the surface properties of spherical AlN particles of an example and a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The spherical AlN particles of the present invention have a molar ratio of Zr atoms to Al atoms of Zr / Al=4.0×10 -4 ~4.2×10 -2 The AlN conversion rate is 70.0% or more, and the circularity is 0.85 to 1.00.

[0016] The spherical AlN particles according to the present invention can be produced by a method including a raw material mixing step of mixing an alumina raw material powder having one or both of alumina powder and alumina hydrate powder having an average particle size (D50) of 0.05 to 4.00 μm with a raw material powder of a Zr compound in an amount of 0.10 to 10.00 mass% calculated as ZrO2 component, with the alumina raw material powder being 100 mass% calculated as the alumina component; a granulation step of converting the mixture produced in the raw material mixing step into spherical granules; a carbon powder mixing step of mixing the spherical granules with carbon powder; and a nitridation step of heat-treating the mixture produced in the carbon powder mixing step in a nitrogen-containing atmosphere.

[0017] First, a method for producing spherical AlN particles according to one embodiment of the present invention will be described. <Raw material mixing process> (Alumina raw powder) The alumina raw powder may be alumina powder alone, alumina hydrate powder alone, or a mixture of alumina powder and alumina hydrate powder. The amount of the alumina component in the alumina raw powder is 100 mass%, and the mass% of the raw powder of the Zr compound to be mixed therewith is 0.10 to 10.00 mass% in terms of ZrO2 component, so that similar spherical AlN particles can be produced regardless of which alumina raw powder is used. The alumina raw powder used has an average particle size (D50) of 0.05 to 4.00 μm. When an alumina raw powder having an average particle size (D50) smaller than 0.05 μm is used, the filling rate of the alumina raw powder in the granulated product obtained by granulation and drying in the granulation step described below tends to be low, that is, the amount of alumina raw powder in the granulated product is small, so that voids may remain in the spherical AlN particles finally obtained. When using alumina raw powder with a particle size larger than 4.00 μm, the strength of the granules is low, the spherical granules become fragile, and the circularity of the resulting AlN particles decreases. If the circularity decreases, it becomes difficult to increase the filling rate when mixing with resin.

[0018] The average particle size (D50) of the alumina raw material powder can be obtained by particle size distribution measurement using a laser diffraction method. The specific surface area of ​​the alumina raw material powder used as a raw material is 2.0 to 30.0 m. 2 It is preferable that the powder has a specific surface area of ​​2.0 m 2 When using an alumina raw material powder with a specific surface area of ​​less than 30.0 m / g, sintering of the alumina powder is difficult to occur during the heating process in the heat treatment step described below, so even if the granulated material is spherical, it is likely to become irregular in shape during the process of nitriding the alumina or sintering the AlN, and it may not be possible to obtain AlN particles with a high degree of circularity. 2When an alumina raw material powder having a specific surface area of ​​more than 1 / g is used, sintering tends to proceed during the heating process in the heat treatment step or at a temperature lower than the temperature at which nitridation occurs, so that the pores on the surface of the alumina granules are blocked, and the nitrogen required for internal nitridation is not supplied, resulting in particles with a low AlN conversion rate, which is undesirable. The specific surface area can be measured by the BET specific surface area measurement method specified in JIS-Z8830. In this way, by using powder with an average particle size (D50) of 0.05 to 4.00 μm as the alumina raw material powder, sintering of the alumina powder before nitriding also progresses, but since the AlN particles after nitriding are also fine, sintering of the AlN particles also progresses easily, and spherical AlN particles with an AlN conversion rate of 70.0% or more can be obtained.

[0019] Alumina hydrates can be converted to transition aluminas such as γ, θ, η, and δ, and further to α-alumina by heat treatment. Examples of such alumina hydrates include boehmite, diaspore, and aluminum hydroxide.

[0020] (Zr compound raw powder) The raw powder of the Zr compound used as the starting material may be zirconium oxide (ZrO2), zirconium carbide (ZrC), zirconium nitride (ZrN), zirconium hydroxide (Zr(OH)4), zirconium chloride (ZrCl4), zirconium acetate (ZrO(CH3COO)2), zirconium alkoxide, etc. Zirconium oxide (ZrO2) powder is preferably used.

[0021] In the nitriding process, in which granulated materials such as alumina powder used as raw materials are heat-treated, the powdered Zr compound suppresses grain growth when granulated materials such as alumina powder are sintered and when AlN particles after nitriding are sintered, and is effective in forming a dense, smooth surface for the resulting spherical AlN particles.

[0022] During heat treatment, the nitriding reaction of alumina and the solid-phase sintering reaction proceed. Sintering is a phenomenon in which atoms move between powder particles, changing contact from point contact to surface contact, advancing the bonding between particles, making them denser and increasing their mechanical strength. Unlike their interiors, not just in powders, the surfaces of solids and liquids are in a state where atoms, ions, and molecules have no partners to bond with. Such a state is extremely unstable for the material, and mass transfer occurs in the direction of reducing the material's surface area. In the case of ceramics, which are solids, mass transfer proceeds by diffusion. Diffusion can be mainly classified into three types depending on where it occurs: volume diffusion, grain boundary diffusion, and surface diffusion. Volume diffusion occurs within crystals. Grain boundary diffusion occurs at grain boundaries between crystals, surface diffusion occurs at the surface of a material, and interfacial diffusion occurs at the interface between different materials. It is said that the influence of grain boundary diffusion is dominant in alumina sintering. As a result of the particle cross-sectional TEM observation of the present invention, it was confirmed that most of the ZrO2 exists isolated at the grain boundaries (some is incorporated into the grains). It is believed that ZrO2 inhibits grain boundary diffusion and suppresses crystal grain growth. As a result, dense and smooth surfaces are formed on the obtained spherical AlN particles.

[0023] The amount of Zr compound added to the raw powder during mixing is 0.10 to 10.00 mass% of the raw powder of Zr compound calculated as ZrO2 component, with respect to 100 mass% of the alumina powder calculated as alumina component. If the amount of Zr compound calculated as ZrO2 component is less than 0.10 mass%, the effect of flattening the surface of the AlN particles obtained cannot be obtained. In addition, if the amount of Zr compound is more than 10.00 mass% calculated as ZrO2 component, the amount of the second phase consisting of Al-Zr-O or Al-Zr-N formed increases, which is undesirable because the relative amount of AlN with excellent heat dissipation properties decreases. When using alumina hydrate in the raw material mixing process, the amount of hydrate (n H2O) is quantified in advance by TG thermal analysis. Once the amount of hydrate is known, the alumina component value for the alumina hydrate can be calculated. In the case of a mixture of alumina powder and alumina hydrate, the alumina component value can also be obtained by measuring the amount of hydrate using TG thermal analysis.

[0024] (raw material mixture) The alumina raw material powder and the Zr compound raw material powder can be mixed by any method that can mix them uniformly, for example, dry mixing or wet mixing using a solvent such as water, alcohol, or acetone.

[0025] <Granulation process> The mixture produced in the raw material mixing step can be made into spherical granules by methods such as spray drying, rolling granulation, stirring granulation, fluidized bed granulation, etc. In the production method of the present invention, the spray drying method is preferred.

[0026] When using the spray drying method, a large amount of the raw material mixture can be efficiently granulated into a spherical shape. When performing granulation by spray drying, the raw material mixture can be uniformly dispersed by using additives such as a dispersant and a binder in a solvent such as water, and a granulated product with high strength can be obtained.

[0027] The particle size of the spherical AlN particles obtained in the subsequent nitriding step is almost the same as the particle size of the granulated material, so spherical AlN particles of the desired particle size can be obtained by controlling the particle size of the granulated material in the granulation step.

[0028] The granules formed in the granulation process are not overly dense. Therefore, the nitriding reaction in the nitriding process described below progresses not only on the surface of the spherical particles but also to the inside of the granules through the voids in the alumina powder of the primary powder. This makes it possible to obtain spherical AlN particles with an AlN conversion rate of 70.0% or more.

[0029] <Carbon powder mixing process> (carbon powder) Carbon powder is added to the granulated product obtained in the granulation process and mixed. The ratio of carbon powder to be mixed with the granulated product is preferably 20.0 to 40.0 mass% based on 100 mass% of the alumina component in the granulated product. When the raw material mixing process is performed in a batch manner and the total amount of the mixed raw material obtained in the process is treated in the granulation process to obtain the granulated product, the amount of alumina component in the total amount of the mixed raw material and the amount of alumina component in the total amount of the granulated product are approximately equal, so it can be said that the ratio of carbon powder to be mixed is preferably 20.0 to 40.0 mass% based on 100 mass% of the alumina raw material powder in the raw material mixing process converted into alumina component. Moreover, the mixing of carbon powder may be additionally carried out in the raw material mixing process prior to the granulation process. By mixing carbon powder in the raw material mixing process as well, graphite powder can be directly mixed into the granules, and AlN particles with an even higher AlN conversion rate can be obtained. The presence of carbon powder between the granules can suppress bonding between the granules due to fusion or the like. As a result, spherical particles with a higher degree of circularity can be obtained. The presence of carbon, which is a reducing agent, in close proximity to the alumina powder allows the reduction reaction to proceed quickly. This promotes the subsequent nitriding reaction, and particles with a high AlN conversion rate can be obtained.

[0030] As the carbon powder to be mixed with the granulated material in the carbon powder mixing step, any form of carbon powder can be used, such as activated carbon, graphite, amorphous carbon, etc. Since the carbon powder is preferably fine particles, it is preferable to use carbon black (CB). Furthermore, when carbon powder is mixed in the raw material mixing step, it is particularly preferable that the carbon powder is fine particles, and therefore it is more preferable to use carbon black (CB).

[0031] In the carbon powder mixing step, the carbon powder is mixed with the granulated material and heat-treated, so that the carbon reduces the alumina, separates oxygen, and promotes nitridation by nitrogen gas. The spherical AlN particles according to the present invention are nitrided to the inside of the granulated material, and this is believed to be because the carbon comes into contact with the alumina to generate CO gas, and this CO gas also contributes to the reduction inside the alumina granulated material. As described above, the amount of carbon powder to be added is preferably 20.0 to 40.0 mass% based on the alumina component in the granulated material being 100 mass%. If the amount is less than 20.0 mass%, the reduction of alumina may be insufficient depending on the conditions from the raw material mixing step to the nitriding step. On the other hand, if 40.0 mass% of carbon is added, the alumina reduction can be sufficiently performed. In addition, when carbon powder is mixed in the raw material mixing process, the amount of carbon powder added is preferably 0.3% to 2.1% by mass, based on 100% by mass of the alumina raw material powder in the raw material mixing process converted into an alumina component. If it is less than 0.3% by mass, the effect of improving the AlN conversion rate may be reduced, and if it exceeds 2.1% by mass, the reduction-nitridation reaction is promoted, but when the AlN particles are formed, the areas where the carbon powder was present tend to become voids, so that the internal voids may become large spherical AlN particles. Therefore, from the viewpoint of ensuring high thermal conductivity, 2.1% by mass or less is preferable. In addition, spherical AlN particles produced by adding more than 2.1% by mass of carbon powder may have a reduced circularity due to the generation of voids.

[0032] <Nitriding process> The spherical granules produced in the granulation process are subjected to heat treatment in a nitrogen-containing atmosphere at a temperature of 1700°C to 1800°C to obtain spherical AlN particles. At temperatures below 1700°C, the reduction-nitridation reaction of alumina is difficult to occur, resulting in particles with a low AlN conversion rate, which is undesirable. Heat treatment at temperatures higher than 1800°C is undesirable because the spherical AlN particles produced by reduction-nitridation begin to adhere to each other, resulting in particle bonding, and at even higher temperatures, the AlN particles begin to decompose, which is undesirable.

[0033] As a heating method for the heat treatment, for example, the granulated material can be placed in a container such as a carbon crucible and heated from the outside of the container by resistance heating using a carbon heater or the like, or by high-frequency induction heating.

[0034] In addition, by using a microwave heating method when heating, the granulated material placed in a container such as a crucible can be heated uniformly all the way to the inside, and spherical AlN particles can be obtained at a lower temperature and in a shorter time than with conventional heat treatment using external heating.

[0035] When obtaining spherical AlN particles using microwave heating, spherical granulated material is mixed with carbon powder and then irradiated with microwaves. Carbon, which absorbs microwaves efficiently, acts as a heat source, making it possible to obtain spherical AlN particles more efficiently.

[0036] In the heat treatment, the alumina powder is sintered before the alumina is nitrided, and the primary alumina particles bond together through neck formation, forming a strong alumina skeleton while maintaining the shape of the granulated material. When nitriding is performed to produce spherical AlN particles, the particles maintain their spherical shape during the nitriding reaction. If Zr is present in the granulated material, excessive grain growth of the primary alumina particles or the nitrided AlN particles can be suppressed, resulting in spherical AlN particles with flat surfaces.

[0037] <Carbon removal treatment> When carbon powder is added to prepare spherical AlN particles, it is preferable to remove the carbon by heating at 400°C to 800°C in an oxidizing atmosphere. The easiest way to oxidize is to heat in an air atmosphere. At this time, the extreme surface layer of the spherical AlN particles is oxidized to form an oxide-rich layer. This oxide-rich layer plays a role in preventing AlN from reacting with moisture to generate NH3. The structure of the extreme surface layer of the AlN particles can be observed by cross-sectional TEM. If elemental analysis is performed with an EDS (Energy Dispersive X-ray Spectroscopy) device during TEM observation, the amount of Al, O, and N present can be quantified. In addition, if XPS (X-ray photoelectron spectroscopy) analysis is performed on multiple particles, the composition and chemical bond state of the elements that make up the surface of the AlN particles can be known. In addition, if XPS analysis is performed while Ar ion sputtering is performed, an elemental profile in the depth direction can be obtained.

[0038] Next, spherical AlN particles according to another embodiment of the present invention will be described. The spherical AlN particles obtained by the above-mentioned manufacturing method have a molar ratio of Zr atoms to Al atoms of Zr / Al=4.0×10 -4 ~4.2×10 -2 The spherical AlN particles are characterized by having an AlN conversion rate of 70.0% or more and a circularity of 0.85 to 1.00.

[0039] The spherical AlN particles of the present invention have a molar ratio of Zr atoms to Al atoms of Zr / Al=4.0×10 -4 ~4.2×10 -2 Contains in an amount of The content of Zr contained in the spherical AlN particles of the present invention is measured by atomic absorption and ICP mass spectrometry (ICP-MS). Note that the amount of Zr component added in the raw material mixing process during production does not change throughout the production process, so the number of moles of Zr component in the molar ratio specified here is the same as the amount of Zr compound raw material powder added in the raw material mixing process of the above-mentioned production method, converted into the number of moles of Zr, calculated as ZrO2 component.

[0040] <AlN conversion rate> The spherical AlN particles of the present invention are produced by mixing an alumina granulated product with carbon powder as a reducing agent as described above, heating in a nitrogen-containing atmosphere, and subjecting to reduction nitridation. In addition to AlN, the spherical AlN particles contain AlON which is a reaction intermediate product. In addition, a very small amount of unreacted alumina and further ZrON and ZrN which are obtained by nitridation reduction of the added ZrO2 particles are contained in trace amounts. Since the AlN conversion rate of the spherical AlN particles of the present invention is 70.0% or more, a high thermal conductivity can be obtained when mixed with a resin. When the AlN conversion rate is less than 70.0%, components with low thermal conductivity such as unreacted alumina or AlON which is a reaction intermediate product are contained, so that the thermal conductivity of the composite mixed with the resin decreases.

[0041] The AlN conversion rate of the spherical AlN particles of the present invention is measured by X-ray diffraction analysis. It is calculated by calculating the intensity ratio of the strongest peaks of AlN, alumina, and AlON obtained by X-ray diffraction analysis. Specifically, among the peaks of each X-ray diffraction pattern shown by AlN, Al2O3, and AlON, the peak with the highest intensity is selected respectively, and the ratio of the peak intensity of AlN when the total intensity shown by these peaks is 100% is defined as the AlN conversion rate.

[0042] In addition, the spherical AlN particles of the present invention contain a compound containing Zr in addition to the above Al compounds. Regarding the Zr compound, although the Zr content can be measured by atomic absorption and ICP mass spectrometry (ICP-MS), its existence form may not be known in some cases. In this case, it is difficult to calculate the AlN conversion rate considering the Zr compound. The spherical AlN particles of the present invention are spherical AlN particles containing Zr atoms in an amount of molar ratio Zr / Al = 4×10 -4 ~4.2×10 -2 Therefore, without considering the Zr-containing compound with a small content relative to the Al compound, the AlN conversion rate was determined assuming that the particles were composed of Al2O3, AlN, and AlON.

[0043] <Circularity> The circularity of the spherical AlN particles of the present invention is 0.85 to 1.00, and by setting it in this range, high fluidity can be obtained and it can be used as a filler with good packing properties. If the circularity is less than 0.85, it is undesirable because it contains a large number of irregular particles, making it difficult to increase the packing rate when mixed with a resin. The circularity of the spherical AlN particles of the present invention was measured using a commercially available flow-type particle image analyzer.

[0044] <Particle size> The spherical AlN particles of the present invention preferably have an average particle size (D50) of 5 to 150 μm. If the average particle size exceeds 150 μm, a long heat treatment is required to prevent AlON from remaining, which is time-consuming and costly. On the other hand, if the average particle size is less than 5 μm, a long heat treatment is required at a low heat treatment temperature to prevent agglomeration due to sintering, which is time-consuming and costly. The average particle size here was determined by particle size distribution measurement using a laser diffraction method. The average particle size is called the median diameter, and the particle size distribution is measured using a laser diffraction method, and the particle size at which the cumulative frequency of the particle size is 50% is taken as the average particle size (D50).

[0045] (Surface properties of AlN particles) The surface properties of AlN particles can be determined by observing the appearance of the particles with a SEM. In Table 2 shown below, the cases where multiple alumina primary particles have coalesced (grain grown) through sintering due to the grain boundary diffusion mechanism, and the roughness of the particle surface appears to have increased compared to the original alumina granules, are described as "grain growth," and the cases where the coalescence of the alumina primary particles has been suppressed and the surface roughness appears to be maintained at the same level as the original alumina granules are described as "grain growth suppression."

[0046] Yet another embodiment of the present invention is a composite material of resin and spherical AlN particles, characterized in that the spherical AlN particles of the present invention are contained in a resin.

[0047] As the resin used in the composite material of the present invention, known resins can be used, but epoxy resins are preferred. The epoxy resins used in this application are not particularly limited, but examples include bisphenol A type epoxy resins, bisphenol F type epoxy resins, biphenyl type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, naphthalene type epoxy resins, and phenoxy type epoxy resins. One of these can be used alone, or two or more types having different molecular weights can be used in combination. Among these, epoxy resins having two or more epoxy groups in one molecule are preferred from the viewpoints of curability, heat resistance, etc. Specifically, biphenyl type epoxy resins, phenol novolac type epoxy resins, orthocresol novolac type epoxy resins, epoxidized novolac resins of phenols and aldehydes, glycidyl ethers of bisphenol A, bisphenol F, bisphenol S, etc., glycidyl ester acid epoxy resins obtained by reacting polybasic acids such as phthalic acid and dimer acid with epochlorohydrin, linear aliphatic epoxy resins, alicyclic epoxy resins, heterocyclic epoxy resins, alkyl-modified polyfunctional epoxy resins, β-naphthol novolac type epoxy resins, 1,6-dihydroxynaphthalene type epoxy resins, 2,7-dihydroxynaphthalene type epoxy resins, bishydroxybiphenyl type epoxy resins, and epoxy resins into which halogens such as bromine have been introduced to impart flame retardancy, etc. Among these epoxy resins having two or more epoxy groups in one molecule, bisphenol A type epoxy resins are particularly preferred.

[0048] For example, resins other than epoxy resins can be used in prepregs for printed circuit boards and various engineering plastics.Specifically, in addition to epoxy resins, silicone resins, phenolic resins, melamine resins, urea resins, unsaturated polyesters, fluororesins, polyamides such as polyimide, polyamideimide, and polyetherimide, polyesters such as polybutylene terephthalate and polyethylene terephthalate, polyphenylene sulfide, aromatic polyesters, polysulfones, liquid crystal polymers, polyethersulfones, polycarbonates, maleimide-modified resins, ABS resins, AAS (acrylonitrile-acrylic rubber-styrene) resins, and AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resins can be used.

[0049] The amount of the spherical AlN particles of the present invention added to the composite material is preferably large from the viewpoints of heat resistance and thermal expansion coefficient, but is usually appropriate to be 70% by mass or more and 95% by mass or less, preferably 80% by mass or more and 95% by mass or less, and more preferably 85% by mass or more and 95% by mass or less. This is because if the amount of spherical AlN particles is too small, it is difficult to obtain effects such as improving the strength of the material and suppressing thermal expansion, and conversely, if it is too large, the viscosity of the composite material becomes too high, making it difficult to put it into practical use as a material.

[0050] The composite material of the present invention may contain a curing agent, a silane coupling agent, etc., in addition to the spherical AlN particles and the resin. A known curing agent may be used as the curing agent to cure the resin, but a phenol-based curing agent may be used. As the phenol-based curing agent, a phenol novolac resin, an alkylphenol novolac resin, polyvinylphenols, etc. may be used alone or in combination of two or more. The amount of the phenol-based curing agent to be blended is preferably such that the equivalent ratio with the epoxy resin (phenolic hydroxyl group equivalent / epoxy group equivalent) is less than 1.0 and is 0.1 or more. This eliminates the residue of unreacted phenol curing agent, improving the moisture absorption and heat resistance. As for the silane coupling agent, a known coupling agent may be used, but one having an epoxy-based functional group is preferable.

[0051] As an example of a method for producing the composite material of the present invention, the composite material of the present invention was produced as follows. A powder consisting of the spherical AlN particles of the present invention was collected in a container. After that, this spherical AlN powder was kneaded under atmospheric pressure in a mixer (Awatori Rentaro) manufactured by Thinky Corporation in order to mix it with an epoxy resin, and further kneaded while evacuating from atmospheric pressure to obtain the composite material of the present invention. EXAMPLES

[0052] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention should not be construed as being limited to the following examples.

[0053] Preparation of spherical AlN particles Example 1 As shown in Table 1, 1.00% by mass of ZrO2 powder (average particle size 1.0 μm) was added to 100% by mass of alumina (Al2O3) powder with an average particle size (D50) of 1.00 μm, a PVA (polyvinyl alcohol) binder, a polycarboxylic acid dispersant, and water were added, and mixed in a ball mill. The resulting mixture was granulated by spray drying (CL-8 manufactured by Okawara Kakoki Co., Ltd.) to obtain a Zr / Al molar ratio of 4.14×10 -3 The granules were mixed with carbon powder (activated carbon with an average particle size of 5 μm) and placed in a graphite crucible, and heat-treated for 8 hours at 1750° C. in a nitrogen atmosphere. At this time, the carbon powder (activated carbon) was mixed in a ratio of 30.0% by mass to 100% by mass of the alumina component in the granules. The heat-treated powder was then subjected to a heat treatment in an electric furnace SUPER-BURN (manufactured by Motoyama Co., Ltd.) at 750° C. for 8 hours in an air atmosphere to remove residual carbon components, thereby obtaining spherical AlN particles.

[0054] Example 2 Except for adding 0.50 mass% ZrO2 powder to 100 mass% alumina powder, spherical AlN particles were produced in the same manner as in Example 1. The ratio of the mixed carbon powder (activated carbon) to 100 mass% alumina component in the granulated product was 30.0 mass%. Example 3 Except for adding 0.10 mass% ZrO2 powder to 100 mass% alumina powder, spherical AlN particles were produced in the same manner as in Example 1. The ratio of the mixed carbon powder (activated carbon) to 100 mass% alumina component in the granulated product was 30.0 mass%. Example 4 Except for adding 5.00 mass% ZrO2 powder to 100 mass% alumina powder, spherical AlN particles were produced in the same manner as in Example 1. The ratio of the mixed carbon powder (activated carbon) to 100 mass% alumina component in the granulated product was 30.0 mass%. Example 5 Except for adding 10.00 mass% ZrO2 powder to 100 mass% alumina powder, spherical AlN particles were produced in the same manner as in Example 1. The ratio of the mixed carbon powder (activated carbon) to 100 mass% alumina component in the granulated product was 30.0 mass%. Example 6 Spherical AlN particles were produced in the same manner as in Example 1, except that the heating temperature in the nitrogen atmosphere was 1700°C. Example 7 Spherical AlN particles were produced in the same manner as in Example 1, except that the heating temperature in the nitrogen atmosphere was 1800°C. Example 8 Spherical AlN particles were produced in the same manner as in Example 1, except that alumina powder with an average particle size (D50) of 0.1 μm was used. Example 9 Spherical AlN particles were produced in the same manner as in Example 1, except that alumina powder with an average particle size (D50) of 3.9 μm was used. Example 10 To the alumina powder of Example 1, 1.00 mass% ZrO2 powder (average particle size 1.0 μm), a PVA (polyvinyl alcohol) binder, a polycarboxylic acid dispersant, and water were added in an external ratio based on 100 mass% of the alumina powder, and 0.40 mass% carbon black (average particle size 20 nm) was further added. The mixture was mixed in a ball mill and granulated by spray drying to produce spherical AlN particles in the same manner as in Example 1. Example 11 To the alumina powder of Example 1, 1.00 mass% ZrO2 powder (average particle size 1.0 μm), a PVA (polyvinyl alcohol) binder, a polycarboxylic acid dispersant, and water were added in an external ratio based on 100 mass% of the alumina powder, and 2.00 mass% carbon black (average particle size 20 nm) was further added. The mixture was mixed in a ball mill and granulated by spray drying to produce spherical AlN particles in the same manner as in Example 1.

[0055] Comparative Example 1 As shown in Table 1, spherical AlN particles were produced in the same manner as in Example 1, except that no ZrO2 was added, and a PVA (polyvinyl alcohol)-based binder, a polycarboxylic acid-based dispersant, and water were added to 100% by mass of alumina powder, mixed in a ball mill, and then granulated by spray drying. Comparative Example 2 Spherical AlN particles were produced in the same manner as in Example 1, except that ZrO2 powder was added at 0.05 mass % relative to 100 mass % of alumina powder. Comparative Example 3 Spherical AlN particles were produced in the same manner as in Example 1, except that ZrO2 powder was added in an amount of 13.00 mass% relative to 100 mass% of alumina powder. Comparative Example 4 Spherical AlN particles were produced in the same manner as in Example 1, except that the heating temperature in the nitrogen atmosphere was 1650°C. Comparative Example 5 Spherical AlN particles were produced in the same manner as in Example 1, except that the heating temperature in the nitrogen atmosphere was 1850°C. Comparative Example 6 Spherical AlN particles were produced in the same manner as in Example 1, except that alumina powder with an average particle size (D50) of 0.02 μm was used. Comparative Example 7 Spherical AlN particles were produced in the same manner as in Example 1, except that alumina powder with an average particle size (D50) of 4.70 μm was used. Comparative Example 8 Spherical AlN particles were produced in the same manner as in Example 11, except that 19.2% by mass of carbon powder (activated carbon) was mixed with 100% by mass of the alumina component in the granulated product. ( Reference example 1 ) To the alumina powder of Example 1, 1.00 mass% ZrO2 powder (average particle size 1.0 μm), a PVA (polyvinyl alcohol) binder, a polycarboxylic acid dispersant, and water were added in an external ratio based on 100 mass% of the alumina powder, and 2.20 mass% carbon black (average particle size 20 nm) was further added. The mixture was mixed in a ball mill and granulated by spray drying to produce spherical AlN particles in the same manner as in Example 1.

[0056] [Table 1]

[0057] The evaluation results of the obtained spherical AlN particles are shown in Table 2. <Evaluation> (AlN conversion rate) The average particle size (D50) of the obtained spherical AlN particles was measured using a CILAS920 laser diffraction scattering particle size distribution analyzer manufactured by CILAS. The circularity was measured for approximately 500 particles using a Sysmex flow type particle image analyzer "FPIA-3000" (manufactured by Spectris). The AlN conversion rate was measured using an X-ray diffraction pattern measured by a Rigaku X-ray diffractometer "RINT-2500TTR." The AlN conversion rate was calculated by measuring the maximum peak intensity of AlN (PDF card No. 25-1133), alumina (PDF card No. 10-0173), and AlON (PDF card No. 48-0686), and the AlN conversion rate was calculated as a percentage from the intensity ratio. As an example, an X-ray diffraction (XRD) pattern of the powder made of AlN particles of the present invention in Example 10 is shown in Fig. 1. An XRD pattern of the powder made of AlN particles in Comparative Example 4 is shown in Fig. 2.

[0058] (Surface texture) The particle surface properties were observed by SEM. In Table 2, the cases where multiple alumina primary particles coalesced (grain growth) through sintering by the grain boundary diffusion mechanism, and the roughness of the particle surface was increased compared to the original alumina granules, were described as "grain growth", and the cases where the coalescence of the alumina primary particles was suppressed and the surface roughness was maintained at the same level as the original alumina granules were described as "grain growth suppression". The results of Examples 1 to 4 and Comparative Examples 1 to 3 are shown in SEM images. Figure 3(a) shows an SEM image of spherical AlN particles (Comparative Example 1) produced using conventional technology without adding Zr. The particle surfaces are very uneven due to the progress of grain growth. On the other hand, Figures 3(b) and (c) show SEM images of AlN particles (Examples 1 and 4) produced with the addition of 1.00 mass% (Zr / Al=4.14E-03) and 5.00 mass% (Zr / Al=2.07E-02) of ZrO2, respectively. In Examples 1 and 4, it is clear from the SEM images that the addition of Zr suppresses the irregularities on the particle surfaces, resulting in smooth particle surfaces.

[0059] Comparing Examples 1 to 5 with Comparative Examples 1 to 3, it can be seen from the comparison of the results of Example 3 and Comparative Example 2 that the amount of Zr added must be at least 0.10 mass% in terms of ZrO2. If too much ZrO2 is added, The amount of the second phase consisting of Al-Zr-O or Al-Zr-N formed increases. However, when the amount added was 10.00 mass % (Example 5), grain growth was suppressed.

[0060] (Composite material of resin and spherical AlN particles) A composite material was produced using the AlN particles of the examples and comparative examples produced as described above. 40 g of powder consisting of spherical AlN particles was collected in a container. Then, in order to mix these 40 g of spherical AlN particles with 10 g of epoxy resin (Epicoat 801N) manufactured by Mitsubishi Chemical, the mixture was kneaded at 2000 rpm for 15 seconds under atmospheric pressure using a THINKY mixer (Awatori Rentaro), and further kneaded at 2000 rpm for 90 seconds while evacuating from atmospheric pressure to 5 Torr. The kneaded material was cooled for 1 hour by leaving the container in a water bath set at 25°C to produce a composite material.

[0061] (Liquidity assessment) The effect of flattening the particle surface morphology was judged from the results of evaluating the fluidity of the composite material prepared. The results of the evaluation of the fluidity of the composite material prepared are shown in Table 2. The viscosity (unit: μ [Pa S]) of each composite material prepared as described above was measured. A rheometer, MCR-102 manufactured by Anton Paar, was used for the viscosity measurement. Parallel plates PP50 with a diameter of 50 mm were set with a plate gap of 1 mm, and measurements were made in the frequency dispersion mode in the range of 0.1 to 100 rad / s under the conditions of a shear strain of 0.1% and a measurement temperature of 28.5°C.

[0062] For the composite material consisting of spherical AlN particles and resin produced without adding ZrO2 powder shown in Comparative Example 1, the viscosity (Pa s) at a shear rate of 1 (rad / s) was evaluated as follows: those that showed a viscosity reduction of 75% or more were marked "◎", those that showed a viscosity reduction of 50% or more were marked "○", and those that showed a viscosity reduction of less than 50% were marked "×".

[0063] When the viscosity reduction was 50% or more, it was judged that the grain growth of the AlN particles was suppressed, a smooth surface was obtained, and the viscosity of the resin kneaded material was reduced. The viscosity of the kneaded material of the powder made of AlN particles and the resin shown in Comparative Example 1 at a shear rate of 1 (rad / s) was 4363 (Pa·s). Comparing Examples 1 to 5 with Comparative Examples 1 to 3, it can be seen from the results of Example 3 and Comparative Example 2 that the amount of Zr added must be at least 0.10 mass% or more in terms of the ZrO2 component. If too much ZrO2 is added, a heterogeneous phase made of Si-Zr-O is mixed in, but when the amount added was 10.00 mass% (Example 5), grain growth was suppressed in the surface properties, and the composite material was judged to be "○".

[0064] Table 2 shows the characteristic values ​​of the spherical AlN particles of the examples (inventive examples) and comparative examples. [Table 2]

[0065] (Firing temperature under nitrogen atmosphere (Examples 1, 5, 6, Comparative Examples 4, 5)) At temperatures below 1700°C (Comparative Example 4), the reduction-nitridation reaction of alumina is difficult to occur, resulting in particles with a low AlN conversion rate, which is undesirable. When heat-treated at temperatures higher than 1800°C (Comparative Example 5), the AlN particles formed by reduction-nitridation start to adhere to each other and bond together, and at even higher temperatures, the AlN particles start to decompose, which is undesirable. The firing temperature for the AlN particles of the present invention is 1700°C to 1800°C.

[0066] (Raw alumina particle size) In the examples and comparative examples, alumina powder with an average particle size (D50) of 0.02 to 4.70 μm was used as the raw material for alumina. When alumina powder with a small average particle size of 0.02 μm was used (Comparative Example 6), the filling rate of the alumina powder in the granulated product obtained by granulation and drying in the granulation process was likely to be low, and voids remained in the spherical AlN particles finally obtained. When alumina powder with a larger average particle size of 4.70 μm was used (Comparative Example 7), the strength of the granulated product was low, and the spherical granulated product was easily broken, and the circularity of the obtained AlN particles was reduced. Due to these effects, the circularity of all the particles in the comparative examples was below 0.85.

[0067] (Adding carbon powder to granulated material) In an example (Comparative Example 8) in which the amount of carbon powder relative to the granulated material was less than 20.0% by mass, the reduction-nitridation reaction of alumina was difficult to occur, resulting in particles with an AlN conversion rate lower than 70.0%. In order to increase the AlN conversion rate, measures such as increasing the heating temperature are necessary. If the amount of carbon powder is too small, the AlN conversion rate cannot be increased to 70.0% or more even if measures such as increasing the heating temperature are taken. Therefore, it is preferable that the amount of carbon powder relative to the granulated material is 20.0% by mass or more.

[0068] (Carbon addition during raw material mixing process) When carbon powder was mixed in the raw material mixing process (Examples 10 and 11), AlN particles with a high AlN conversion rate of 90% or more could be obtained. Reference example 1), the reduction-nitridation reaction was promoted, but when the AlN particles were formed, the areas where the carbon powder had been present became voids, which deteriorated both the surface morphology and circularity. Since the AlN particles had large internal voids, a carbon content of 2.1 mass% or less is preferable from the perspective of ensuring high thermal conductivity.

Claims

1. The molar ratio of Zr atoms to Al atoms was Zr / Al=4.0×10 -4 ~4.2 x 10 -2 The spherical AlN particles are characterized in that they are made of sintered particles containing in an amount of 0.85 to 1.00, have an AlN conversion rate of 70.0% or more, and have a circularity of 0.85 to 1.

00.

2. 2. The spherical AlN particles according to claim 1, characterized in that the AlN conversion rate is 90.0% or more.

3. A composite material of resin and spherical AlN particles, comprising the spherical AlN particles according to claim 1 or 2 contained in a resin.

4. A method for producing the spherical AlN particles according to claim 1 or 2, comprising the steps of: An alumina raw material powder having one or both of alumina powder and alumina hydrate powder having an average particle size (D50) of 0.05 to 4.00 μm is mixed with a raw material powder of a Zr compound, in an amount of ZrO, in terms of 100 mass % of the alumina raw material powder calculated as an alumina component. 2 A raw material mixing step of mixing 0.10 to 10.00 mass% of the components; A granulation step for converting the mixture produced in the raw material mixing step into spherical granules; a carbon powder mixing step of mixing the spherical granules with carbon powder; A nitriding step in which the mixture obtained in the carbon powder mixing step is heat-treated at a temperature of 1700° C. to 1800° C. in a nitrogen-containing atmosphere. A method for producing spherical AlN particles, comprising:

5. The method for producing spherical AlN particles as described in claim 4, characterized in that the ratio of carbon powder mixed with the spherical granules in the carbon powder mixing process is 20.0 to 40.0 mass%, based on 100 mass% of the alumina raw material powder in the spherical granules, calculated as an alumina component.

6. The method for producing spherical AlN particles as described in claim 4 or 5, characterized in that in the raw material mixing process, 0.3 to 2.1 mass% of carbon powder is further mixed into the alumina raw material powder, with the alumina raw material powder being converted into 100 mass% of the alumina component.

Citation Information

Patent Citations

  • Production of aluminum nitride based powder

    JP1987132711A

  • Aluminum nitride powder, sintered material and production thereof

    JP1992092864A

  • Aluminum nitride powder and method for producing the same

    JP1992154610A

  • Moisture-resistant aluminum nitride powder and its production

    JP1998120407A

  • High purity aluminum nitride powder and method of manufacturing the same, and high purity aluminum nitride sintered compact

    JP2004182585A