Hexagonal boron nitride powder

The reductive nitriding method for hexagonal boron nitride powder addresses thermal anisotropy and high specific gravity issues by producing fine, high-purity aggregates with small pores, enhancing thermal conductivity and dielectric strength while reducing weight in resin compositions.

JP7588527B2Active Publication Date: 2024-11-22TOKUYAMA CORP

Patent Information

Application Number
JP2021032919
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-02
Publication Date
2024-11-22
Estimated Expiration
2041-03-02

AI Technical Summary

Technical Problem

Hexagonal boron nitride powders with agglomerated particles exhibit thermal anisotropy and high specific gravity, leading to reduced thermal conductivity and dielectric strength when filled into resins, and are prone to voids that affect insulation resistance and weight.

Method used

A reductive nitriding method using an oxygen-containing boron compound, carbon source, and oxygen-containing calcium compound to produce hexagonal boron nitride aggregates with fine primary particles, reducing gaps between particles and minimizing impurities, resulting in a powder with small pores and high purity.

Benefits of technology

The method produces hexagonal boron nitride powder with improved thermal conductivity, dielectric strength, and reduced weight by eliminating thermal anisotropy and void-related issues, while maintaining high purity without the need for sintering aids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588527000004
    Figure 0007588527000004
  • Figure 0007588527000005
    Figure 0007588527000005
  • Figure 0007588527000006
    Figure 0007588527000006
Patent Text Reader

Abstract

To provide a hexagonal boron nitride powder which can give an extremely high dielectric strength and heat conductivity to a resin composition obtained by filling a resin with the powder and can reduce density of the resin composition, and a production method thereof.SOLUTION: A hexagonal boron nitride powder comprises aggregated particles of hexagonal boron nitride primary particles. The hexagonal boron nitride powder shows values of: a particle diameter (D50) of a 50% cumulative volume frequency of a particle size distribution as measured by a wet laser diffraction particle size distribution technique of 5 to 150 μm; a volume standard median diameter of pores as measured by a mercury intrusion technique of 3.0 μm or less; and an impurity element content of 500 ppm or less. The hexagonal boron nitride powder preferably comprises the aggregated particles having a BET specific surface area in a range of 2 to 10 m2 / g, an oil absorption amount in a range of 50 to 190 cc / 100 g, a major axis in a range of 5 to 10 μm, a major axis / minor axis in a range of 1.0 to 1.3, and a degree of circularity in a range of 0.3 to 0.8.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel hexagonal boron nitride agglomerated particle, specifically to a hexagonal boron nitride powder which can impart extremely high dielectric strength and thermal conductivity to a resin composition obtained by filling the hexagonal boron nitride powder into a resin, and can reduce the density and weight of the resin composition. [Background technology]

[0002] Hexagonal boron nitride powder is generally a white powder having a hexagonal layered structure similar to that of graphite, and has many properties such as high thermal conductivity, high electrical insulation, high lubricity, corrosion resistance, mold releasability, high temperature stability, chemical stability, etc. Therefore, resin compositions filled with hexagonal boron nitride powder are suitably used as thermally conductive insulating sheets by molding.

[0003] Moreover, in recent years, there has been an increasing demand for insulating sheets with low dielectric constant, low dielectric tangent, and thermal conductivity for use in high-frequency devices, and the demand for hexagonal boron nitride powder, which has a lower dielectric constant than other highly thermally conductive fillers such as aluminum nitride and aluminum oxide, is also increasing.

[0004] In particular, for use as a low-density, thermally conductive insulating sheet for vehicles, hexagonal boron nitride powder, which has a lower specific gravity than other highly thermally conductive fillers such as aluminum nitride and aluminum oxide, is attracting attention.

[0005] Hexagonal boron nitride powder contains primary particles consisting of scaly particles derived from the crystal structure, and the scaly particles have thermal anisotropy. Therefore, in the case of a thermal conductive insulating sheet using boron nitride powder containing the above-mentioned scaly particles as single particles as a filler, the scaly particles are oriented in the plane direction of the thermal conductive insulating sheet, so that heat is transmitted in the c-axis direction of the scaly particles, which has low thermal conductivity, and the thermal conductivity of the thermal conductive insulating sheet in the thickness direction is low.

[0006] In order to improve the thermal anisotropy of hexagonal boron nitride particles having such a scale-like structure, a hexagonal boron nitride powder has been proposed that contains agglomerated particles in which the scale-like particles of hexagonal boron nitride are randomly oriented and aggregated.

[0007] For example, there have been proposals for agglomerated particles in which scale-like particles are randomly oriented by spray-drying amorphous boron nitride powder and reheating the powder, or for crushing a sintered body in which scale-like particles are randomly oriented after press-molding a mixed powder of amorphous boron nitride powder and an auxiliary such as an oxide, and then sintering the mixture (see Patent Document 1). These agglomerated particles have large diameters of the scale-like particles, which are the primary particles constituting the agglomeration, and most of the scale-like particles have a size exceeding 10 μm. It is said that when the boron nitride powder made of the above-mentioned agglomerated particles is filled in a resin, the resin penetrates into the gaps between the scale-like primary particles and fills the gaps, making it difficult for large air bubbles to exist in the resin composition, thereby exhibiting high insulation resistance.

[0008] However, there is still room for improvement in the insulation resistance. That is, when filled in resin, the resin easily penetrates into the large gaps, but if the gaps become smaller toward the center of the aggregated particles or if continuous long gaps are formed, there is a concern that voids that reduce the insulation resistance will remain in the resin composition. This tendency is particularly noticeable when the viscosity of the resin is high. In addition to the above problems, there is a concern that the sintered body may cause a decrease in insulation strength due to the inclusion of impurity elements as sintering aids.

[0009] Furthermore, in the case of agglomerated particles in which voids are reduced by allowing resin to penetrate into the agglomerated particles, the specific gravity of the boron nitride powder in the resin composition is equal to that of the bulk body, and it is not possible to reduce the weight of the resin composition. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2017-165609 A Summary of the Invention [Problem to be solved by the invention]

[0011] Therefore, an object of the present invention is to provide a hexagonal boron nitride powder containing agglomerated particles in which scaly primary particles of hexagonal boron nitride are aggregated, which can eliminate the anisotropy of thermal conduction through aggregation to exhibit high thermal conductivity when filled into a resin, while also imparting extremely high dielectric strength when filled into a resin, and furthermore can contribute to reducing the weight of the resin composition. [Means for solving the problem]

[0012] The present inventors have conducted extensive research to solve the above problems, and as a result, have confirmed that hexagonal boron nitride obtained by employing a specific manufacturing method in which a reduction-nitridation reaction is carried out using an oxygen-containing boron compound, a carbon source, and an oxygen-containing calcium compound, which are known as raw materials for obtaining boron nitride by reduction-nitridation, has extremely small gaps formed between randomly oriented scale-like primary particles due to the generation of agglomerated particles during the reaction, and that hexagonal boron nitride powder consisting of such agglomerated particles can solve all of the above problems when filled into a resin to form a resin composition, thereby completing the present invention.

[0013] That is, according to the present invention, the hexagonal boron nitride particles are composed of aggregated particles of hexagonal boron nitride primary particles, and have a particle size (D 50 The present invention provides a hexagonal boron nitride powder having a pore size of 5 to 150 μm, a volume-based median diameter of pores measured by mercury intrusion porosimetry of 3.0 μm or less, and a content of impurity elements of 500 ppm or less.

[0014] The hexagonal boron nitride powder of the present invention has a specific surface area of ​​1 to 15 m as measured by the BET method. 2 / g, and the oil absorption is preferably 50 to 190 cc / 100 g.

[0015] Furthermore, the hexagonal boron nitride powder of the present invention preferably contains 5% or more of agglomerated particles (specific agglomerated particles) having a major axis of 5 to 10 μm, a major axis / minor axis ratio of 1.0 to 1.3, and a circularity of 0.3 to 0.8.

[0016] Furthermore, the present invention also provides a resin composition containing the above-mentioned boron nitride powder as a filler, which has excellent thermal conductivity and exhibits high dielectric strength, and a resin sheet made of the above-mentioned resin composition. Effect of the Invention

[0017] The hexagonal boron nitride powder of the present invention is composed of agglomerated particles of fine hexagonal boron nitride scale-like primary particles, and therefore exhibits the effect of eliminating the anisotropy of thermal conductivity due to agglomeration. In addition to the above characteristics, the fine hexagonal boron nitride primary particles are configured to be attached to the agglomerated particle surface, and the agglomerated particle surface has fine pores, thereby exhibiting excellent characteristics not found in conventional agglomerates. That is, the agglomerated particles of the primary particles constituting the hexagonal boron nitride powder of the present invention have extremely small gaps between the particles due to the fineness of the primary particles, and unlike the gaps between conventional plate-like particle agglomerated particles, have a structure in which plate-like particles are attached to the agglomerated particle surface, and when filled into a resin, the voids present in the gaps have almost no effect on the dielectric strength, and the resin composition filled with this can exhibit extremely high dielectric strength. In addition, the gaps present in the agglomerated particles can reduce the weight of the hexagonal boron nitride powder, and therefore the weight of the resin composition obtained by filling it.

[0018] In addition, the hexagonal boron nitride powder of the present invention can be produced without employing a sintering method that requires a sintering aid, has a low content of impurity elements, and can be highly purified, which makes it possible to minimize the decrease in the dielectric strength of the resin composition. [Brief description of the drawings]

[0019] [Figure 1] SEM photo of specific aggregate particles in the hexagonal boron nitride powder obtained in Example 1 [Diagram 2] SEM photo of the hexagonal boron nitride powder obtained in Example 1 [Diagram 3] SEM photograph of the surface of coarse aggregated particles of the hexagonal boron nitride powder obtained in Example 1 DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] (Hexagonal boron nitride powder) The hexagonal boron nitride powder of the present invention is characterized in that it is composed of agglomerated particles of hexagonal boron nitride primary particles, has a volume-based median pore diameter of 3 μm or less, and has an impurity element content of 500 ppm or less.

[0021] The hexagonal boron nitride powder was identified by confirming that the sample powder had no peaks other than those of hexagonal boron nitride in the X-ray diffraction measurement. Here, the X-ray diffraction measurement was performed using a fully automatic horizontal multipurpose X-ray diffractometer SmartLab (product name) manufactured by Rigaku Co., Ltd. The measurement conditions were a scan speed of 20 degrees / min, a step width of 0.02 degrees, and a scan range of 10 to 90 degrees. The GI value representing the crystallinity of the hexagonal boron nitride powder was calculated from the integrated intensity ratio (area ratio) of the (100), (101), and (102) diffraction lines of the X-ray diffraction spectrum of the hexagonal boron nitride powder by the formula, GI=[{(100)+(101)} / [(102)]. The GI value of the hexagonal boron nitride powder of the present invention is 2.5 or less, and this was also confirmed in the examples.

[0022] The hexagonal boron nitride powder of the present invention is composed of aggregates of scaly primary particles of hexagonal boron nitride, but such aggregates can be obtained by employing specific reaction conditions for synthesizing hexagonal boron nitride to produce aggregated particles, rather than by a manufacturing method such as conventional granulation or sintering methods in which scaly hexagonal boron nitride single particles that have already been produced are aggregated.

[0023] Therefore, the agglomerated particles constituting the hexagonal boron nitride powder of the present invention are composed of fine hexagonal boron nitride scale-like primary particles, the gaps between the agglomerated particles are extremely small, and the volume-based median diameter of the pores is a characteristic value of 3.0 μm or less. Such a volume-based median diameter is preferably 2.8 μm, more preferably 2.5 μm or less. If the volume-based median diameter of the pores exceeds 3.0 μm, when the resin is filled, air bubbles that affect the insulation resistance tend to remain, making it difficult to exhibit high dielectric strength. That is, by having the volume-based median diameter of the pores of the agglomerated particles constituting the hexagonal boron nitride powder of the present invention exhibit the above value, when the resin is filled, the voids present in the gaps have almost no effect on the dielectric strength, and the resulting resin composition can exhibit extremely high dielectric strength. In addition, the presence of pores (gaps) in and on the surfaces of the agglomerated particles makes it possible to reduce the weight of the resin composition obtained by filling the hexagonal boron nitride powder. The above pores can be confirmed in the SEM photograph of FIG.

[0024] The hexagonal boron nitride powder of the present invention has a pore volume of pores having a pore diameter of 3 μm or less in addition to the volume-based median diameter of the pores of the agglomerated particles of 0.2 cm 3 / g or more, preferably 0.5 to 2.0 cm 3 / g is preferable in order to further enhance the effect of reducing the weight of the resin composition due to the remaining pores.

[0025] The pore volume-based median diameter and pore volume were calculated from the cumulative pore distribution in which pores of 0.0036 μm to 200 μm were measured by mercury intrusion porosimetry using an Autopore IV9520 manufactured by Micromeritics, and the pore diameter was plotted on the horizontal axis and the cumulative pore volume was plotted on the vertical axis.

[0026] The hexagonal boron nitride powder of the present invention is obtained by a manufacturing method described below that does not use sintering aids, so there is no decrease in purity due to sintering aids and it is highly pure. For example, when used as a filler in a resin composition that constitutes an insulating sheet, it works together with the effect of the small pores to contribute to improving voltage resistance. That is, the hexagonal boron nitride powder of the present invention is characterized by having a high purity with an impurity element content of 500 ppm or less, particularly 400 ppm or less. If the content of the above impurity elements exceeds the above range, it will have an adverse effect on the dielectric strength and the object of the present invention will not be achieved.

[0027] The impurity elements referred to here are calcium, magnesium, sodium, aluminum, lithium, strontium, iron, sulfur, nickel, chromium, manganese, silicon, phosphorus, titanium, barium, and cobalt. The content of the impurity elements refers to the total content of the impurity elements.

[0028] The impurity element content of the hexagonal boron nitride powder is a value measured by fluorescent X-ray analysis. In the examples, a ZSX Primus2 (product name) manufactured by Rigaku Corporation was used as the fluorescent X-ray analyzer.

[0029] The hexagonal boron nitride powder of the present invention has a C% of 0.04% or less and an O% of 0.4% or less, which, in combination with the low amounts of the impurity elements, is more effective in improving thermal conductivity and dielectric strength.

[0030] The O% of the hexagonal boron nitride powder was measured using an oxygen / nitrogen analyzer EMGA-620 manufactured by Horiba, Ltd. The C% of the hexagonal boron nitride powder was measured using an EMIA-110 manufactured by Horiba, Ltd.

[0031] Taking into consideration the fillability into resin, the particle size of the hexagonal boron nitride powder of the present invention is the particle size at 50% cumulative volume frequency of the particle size distribution in the wet laser diffraction particle size distribution method (D 50) is 5 to 150 μm, preferably 10 to 100 μm, particularly preferably 20 to 80 μm. In order to adjust the particle size to the above range, it is also possible to produce the hexagonal boron nitride powder of the present invention by separating coarse aggregated particles, specifically aggregated particles having a size of more than 200 μm, particularly more than 150 μm, from the coarse hexagonal boron nitride powder obtained by the production method described below using a classification means such as a sieve. It is also possible to produce the hexagonal boron nitride powder by separating the coarse particles, crushing them to an appropriate size, and then returning them to the hexagonal boron nitride powder.

[0032] In the examples, the particle size measurement by the wet laser diffraction particle size distribution method is carried out using LA-950V2 (trade name) manufactured by HORIBA Corporation.

[0033] The hexagonal boron nitride powder of the present invention has a specific surface area of ​​1 to 15 m 2 / g, and 1.5 to 14.0 m 2 / g is more preferable, and 2.0 to 13.0 m 2 / g. That is, 15.0m 2 Hexagonal boron nitride powder exceeding 1 m / g means that it contains a large amount of fine particles, and such hexagonal boron nitride powder contains a large amount of boron nitride powder with low crystallinity, which not only causes thermal resistance in the insulating and heat dissipating sheet, but is also undesirable from the viewpoint of handling, since the powder tends to fly around. 2 Hexagonal boron nitride powder with a molecular weight of less than 10000 / g is not preferred because the proportion of flat hexagonal boron nitride single particles that have grown into grains increases, and the anisotropy of their thermal conductivity may lead to a decrease in the thermal conductivity of the resin composition when filled into a resin.

[0034] The specific surface area of ​​the hexagonal boron nitride powder is a value measured by the BET single point method, and in the examples, the measurement is carried out using Macsorb HM model-1201 (product name) manufactured by Mountech Co., Ltd.

[0035] In addition, the hexagonal boron nitride powder of the present invention preferably has an oil absorption of 50 to 190 ml / 100 g, particularly 55 to 170 ml / 100 g, and further preferably 60 to 150 ml / 100 g. That is, the DBP absorption indicates the amount of open pores in the aggregated particles, the presence or absence of structure on the particle surface, and wettability with resin, among the properties of the hexagonal boron nitride powder, and the more open pores there are and the more developed the structure, the higher the DBP absorption. That is, if the oil absorption is too low, the open pores are large and the structure is not sufficiently developed, which is not preferable, and if it is too high, the opposite tendency occurs, and it is not preferable because it is easy to get large bubbles in the resin composition. The oil absorption of the hexagonal boron nitride powder is measured based on the procedure specified in JIS K5101-13-1:2004 ("Testing methods for pigments" - Part 13: Oil absorption - Section 1: Refined linseed oil method).

[0036] Furthermore, the hexagonal boron nitride powder of the present invention has a tapped bulk density of 0.40 g / cm 3 It is preferable that the tapped bulk density is equal to or greater than 0.40 g / cm. That is, the tapped bulk density is an index showing the particle shape and particle size distribution width among the properties of hexagonal boron nitride powder, and a high value indicates a state in which there are few large open pores, many agglomerated particles that are nearly spherical, and the particle size distribution is close to close-packed. The hexagonal boron nitride powder of the present invention can be made to have a high tapped bulk density by increasing the content of specific hexagonal boron nitride agglomerated particles described below, which makes it easier to fill gaps in the powder. The tapped bulk density of all the hexagonal boron nitride powders produced in the examples was 0.40 g / cm. 3 That was all.

[0037] The hexagonal boron nitride powder of the present invention preferably contains agglomerated particles (specific agglomerated particles) having a major axis of 5 to 10 μm, a major axis / minor axis ratio of 1.0 to 1.3, and a circularity of 0.3 to 0.8 in a proportion of 5% or more, preferably 10% or more.

[0038] The SEM observation major axis range was confirmed using an SEM observation image at a magnification of 10,000 times. The SEM observation major axis / minor axis was calculated from an SEM observation image at a magnification of 10,000 times. The circularity was calculated by calculating 4π×(area) / (perimeter) from an SEM observation image at a magnification of 10,000 times using image analysis software. 2 was calculated using the formula:

[0039] The content percentage % of the specific agglomerated particles can be measured using the following method. First, using a dry vibrating sieve KFC-500-1D manufactured by KOWA Corporation, a SUS mesh with an opening of 45 μm was used to sieve the hexagonal boron nitride powder above and below the 45 μm sieve for 30 minutes, and the weight percentage X% of the particles that fell under the 45 μm sieve was obtained. After that, the corresponding hexagonal boron nitride agglomerated particles and non-corresponding particles were selected from the SEM observation image of the collected 45 μm sieve at a magnification of 1000 times, and the SEM observation image area percentage Y% of the hexagonal boron nitride agglomerated particles that fell under the 45 μm sieve was obtained. Finally, the percentage (X×Y×0.01)% obtained by multiplying the weight percentage X% of the particles that fell under the 45 μm sieve by the SEM observation image area percentage Y% of the hexagonal boron nitride agglomerated particles that fell under the 45 μm sieve was taken as the percentage of the specific agglomerated particles in the present invention. For example, if the weight ratio X of the hexagonal boron nitride powder that falls under a 45 μm sieve is 20 wt %, and the SEM observation image area ratio Y of the specific agglomerated particles that fall under a 45 μm sieve is 60%, the ratio Z of the specific agglomerated particles is calculated as 20 × 60 × 0.01 = 12%.

[0040] In the hexagonal boron nitride powder of the present invention, the specific agglomerated particles have an appropriate size suitable for filling the gaps between other agglomerated particles, and are approximately spherical. Therefore, by having the specific agglomerated particles present in the hexagonal boron nitride powder in the above ratio, it is presumed that the filling ability of the hexagonal boron nitride powder into resin is improved and the remaining of relatively large air bubbles can be effectively suppressed, thereby contributing to improving the dielectric strength of the resin composition.

[0041] The proportion of the specific agglomerated particles in the hexagonal boron nitride powder is preferably higher than the lower limit value described above in order to promote the above-mentioned action, and it is preferable to increase the proportion by separating particles having a relatively large particle diameter by classifying the hexagonal boron nitride powder obtained by the manufacturing method described below using a sieve or the like.

[0042] The specific agglomerated particles are produced as part of a hexagonal boron nitride powder by a production method described below. The specific agglomerated particles are characterized in that the primary particles of hexagonal boron nitride constituting the specific agglomerated particles are smaller and more uniform in size than the other agglomerated particles, and most of the primary particles have a major axis of 4 μm or less. This characteristic also contributes to improving the dielectric strength of the resin composition.

[0043] (Method of manufacturing boron nitride powder) The method for producing the hexagonal boron nitride powder of the present invention is not particularly limited, but a representative example of the production method includes a method for producing a hexagonal boron nitride powder, which comprises mixing an oxygen-containing boron compound having a 425 μm sieve residue of 3 wt % or less, a carbon source, and an oxygen-containing calcium compound in a ratio of 0.63 to 0.73 in terms of B / C (element ratio) which is the ratio of the B source contained in the oxygen-containing boron compound to the C source contained in the carbon source, and 4 to 12 parts by mass of the oxygen-containing calcium compound in terms of CaO per 100 parts by mass of the total amount of the oxygen-containing boron compound and the carbon source (B2O3, C converted value), heating to a maximum temperature of 1910 to 2000°C in a nitrogen atmosphere to perform reduction-nitridation, and then removing by-products other than boron nitride present in the reaction product by acid washing.

[0044] (raw materials) The greatest feature of the manufacturing method of the present invention is that the raw materials, an oxygen-containing boron compound with a controlled particle size, a carbon source, and an oxygen-containing calcium compound, are mixed in a prescribed ratio as described below, and are reduced and nitrided at a high temperature of 1910° C. or higher. The role of each raw material is as follows:

[0045] (Oxygen-containing boron compound) In the above-mentioned production method of the present invention, as the oxygen-containing boron compound as the raw material, any compound containing a boron atom is used without any limitation. For example, boric acid, boric anhydride, metaboric acid, perboric acid, hypoboric acid, sodium tetraborate, sodium perborate, etc. can be used. In general, boric acid and boron oxide, which are easily available, are preferably used. In addition, it is preferable that the average particle size of the oxygen-containing boron compound used is such that the residue on a 425 μm sieve is 3% by mass or less, preferably 1.5% by mass or less. In particular, it is more preferable that the residue on a 300 μm sieve is 50% or less, and even more preferable that the residue on a 250 μm sieve is 70% or less. In other words, if the residue on the 425 μm sieve of the oxygen-containing boron compound is 3% by weight or more, coarse boron nitride agglomerated particles of 150 μm or more are likely to remain, and the remaining voids within the coarse agglomerated particles will increase, causing the median diameter of the pores in the resulting hexagonal boron nitride powder to exceed 3 μm, resulting in a decrease in dielectric strength.

[0046] (Oxygen-containing calcium compounds) The oxygen-containing calcium compound forms a composite oxide with the oxygen-containing boron compound, thereby forming a composite oxide having a high melting point, and has the role of preventing the volatilization of the oxygen-containing boron compound.

[0047] In the production method of the present invention, the oxygen-containing calcium compound used as the catalyst and the volatilization inhibitor of the oxygen-containing boron compound may be any known compound without any particular limitation, but an oxygen-containing calcium compound containing oxygen and calcium is preferably used. Examples of the oxygen-containing calcium compound include calcium carbonate, calcium bicarbonate, calcium hydroxide, calcium oxide, calcium nitrate, calcium sulfate, calcium phosphate, calcium oxalate, etc. Among them, the oxygen-containing calcium compound is preferably used. Examples of the oxygen-containing calcium compound include calcium carbonate, calcium bicarbonate, calcium hydroxide, calcium oxide, calcium nitrate, calcium sulfate, calcium phosphate, calcium oxalate, etc., and two or more of these may be mixed and used. Among them, calcium oxide and calcium carbonate are preferably used.

[0048] The oxygen-containing calcium compound may be used in combination of two or more kinds. The average particle size of the oxygen-containing calcium compound is preferably 0.01 to 200 μm, more preferably 0.05 to 120 μm, and particularly preferably 0.1 to 80 μm.

[0049] (Carbon Source) In the manufacturing method of the present invention, known carbon materials acting as reducing agents are used as the carbon source without any particular limitation. For example, in addition to amorphous carbon such as carbon black, activated carbon, and carbon fiber, crystalline carbon such as diamond, graphite, and nanocarbon, and pyrolytic carbon obtained by pyrolyzing monomers and polymers can be mentioned. Among them, highly reactive amorphous carbon is preferred, and carbon black is particularly preferred because it is industrially quality controlled. In addition, acetylene black, furnace black, thermal black, and the like can be used as the carbon black. In addition, the average particle size of the carbon source is preferably 0.01 to 5 μm, more preferably 0.02 to 4 μm, and particularly preferably 0.05 to 3 μm. That is, by making the average particle size of the carbon source 5 μm or less, the reactivity of the carbon source is increased, and by making it 0.01 μm or more, the handling becomes easy.

[0050] In the production method of the present invention, the form of the mixture containing the above-mentioned raw materials to be supplied to the reaction is not particularly limited. The mixture may be in the form of a powder or may be formed into granules.

[0051] In the production method of the present invention, the method for mixing the raw materials is not particularly limited, and a general mixer such as a vibration mill, a bead mill, a ball mill, a Henschel mixer, a drum mixer, a vibration agitator, or a V-shaped mixer can be used.

[0052] In addition, the granulation method when granulation is performed can be carried out by a known method such as extrusion granulation, rolling granulation, granulation by a compactor, etc., using a binder as necessary. In this case, the size of the granules is preferably about 5 to 10 mm.

[0053] (Preparation of raw materials) In the present invention, the reduction-nitridation reaction is carried out by supplying a carbon source and nitrogen, and in order to effectively obtain the desired hexagonal boron nitride agglomerated particles, the ratio of the B source and the carbon source contained in the oxygen-containing boron compound must be 0.63 to 0.73, preferably 0.65 to 0.72, calculated as B / C (element ratio). That is, if the molar ratio exceeds 0.73, the ratio of boron compounds that are not reduced and volatilize increases, and they tend to form a complex oxide with the Ca auxiliary, and the melting point of the complex oxide is low, and the plate-like particles tend to grow, making it difficult to obtain the desired agglomerated particles with small primary particles and pores. Also, if the molar ratio is less than 0.63, the carbon content is high, and there is a risk of impurities derived from carbon remaining.

[0054] In the present invention, in order to effectively obtain the desired hexagonal boron nitride agglomerated particles, it is necessary to mix the oxygen-containing calcium compound in a ratio of 4 to 12 parts by mass in terms of CaO with respect to 100 parts by mass of the total amount (B2O3, C conversion value) of the oxygen-containing boron compound and the carbon source. At this time, if the CaO conversion part is 4 parts by mass or less, not only the ratio of the boron compound that is not reduced and volatilized increases, and the yield decreases, but also the melting point of the CaO-B2O3 composite oxide formed with the remaining boron compound decreases, and the grain growth of the hexagonal boron nitride particles is promoted, making it difficult to form the desired agglomerated particles having pores, which is not preferable. If the CaO conversion part is 12 parts by mass or more, there is a risk of calcium-derived impurities remaining, which is not preferable.

[0055] In the present invention, by adjusting the particle size and composition ratio of the raw materials, the targeted excessive particle growth is prevented, and agglomerated particles having a small primary particle size can be produced with high selectivity. (Reduction Nitridation) In the method for producing boron nitride of the present invention, the nitrogen source can be supplied to the reaction system by known means. For example, the most common method is to circulate nitrogen gas through the reaction system of the reaction device exemplified below. The nitrogen source to be used is not limited to the above-mentioned nitrogen gas, but is not particularly limited as long as it is a gas capable of nitridation in the reduction-nitridation reaction. Specifically, in addition to the above-mentioned nitrogen gas, ammonia gas can also be used. Also, a gas obtained by mixing nitrogen gas or ammonia gas with a non-oxidizing gas such as hydrogen, argon, or helium can be used.

[0056] In the above manufacturing method, in order to obtain a hexagonal boron nitride powder having high crystallinity and pores, it is necessary to adopt a heating temperature in the reduction-nitridation reaction of usually 1910°C to 2000°C, preferably 1920°C to 1980°C. By setting the heating temperature at 1910°C to 2000°C, the crystallinity of the hexagonal boron nitride particles is improved, the outer circumference of the primary particle shape becomes sharper, and the number of fine pores between the particles increases. Furthermore, if the temperature is less than 1910°C, the reduction-nitridation reaction does not proceed and it is difficult to obtain white hexagonal boron nitride with high crystallinity, and if the temperature exceeds 2000°C, the effect reaches a plateau, which is not only economically disadvantageous but also undesirably increases damage to the heating furnace.

[0057] The time for the reduction-nitridation reaction is appropriately determined, but is generally about 6 to 30 hours.

[0058] The method for producing the hexagonal boron nitride powder of the present invention can be carried out using a known reaction apparatus capable of controlling the reaction atmosphere, such as an atmosphere-controlled high-temperature furnace in which heat treatment is performed by high-frequency induction heating or heater heating, and in addition to a batch furnace, a pusher-type tunnel furnace, a vertical reaction furnace, or other continuous furnace can also be used.

[0059] (acid washing) In the production method of the present invention, the reaction product obtained by the above-mentioned reduction nitridation contains impurities such as a composite oxide consisting of boron oxide-calcium oxide in addition to the hexagonal boron nitride powder, so it is preferable to wash it with an acid. There is no particular limitation on the method of acid washing, and any known method can be used without limitation. For example, there is a method in which the by-product-containing boron nitride obtained after the nitriding treatment is crushed and placed in a container, and dilute hydrochloric acid (10 to 20 mass % HCl) is added in an amount 5 to 10 times the amount of the hexagonal boron nitride powder containing the impurities, and the mixture is allowed to come into contact for 4 to 8 hours.

[0060] As the acid used in the above-mentioned acid washing, other than hydrochloric acid, nitric acid, sulfuric acid, acetic acid, etc. can also be used.

[0061] After the acid washing, the boron nitride is washed with pure water to remove the remaining acid. The washing method involves filtering the acid, dispersing the acid-washed boron nitride in the same amount of pure water as the acid used, and filtering again.

[0062] (Dry) The conditions for drying the hydrous aggregate after the acid washing and water washing are preferably drying in the air or under reduced pressure at 50 to 250° C. The drying time is not particularly specified, but it is preferable to dry until the moisture content approaches 0%.

[0063] (classification) The dried boron nitride powder may be crushed, if necessary, and then subjected to removal of coarse particles using a sieve or the like, and removal of fine particles using air classification or the like.

[0064] (Applications of boron nitride powder) The use of the boron nitride powder of the present invention is not particularly limited, and it can be applied to known uses without any particular restrictions. An example of a suitable use is use as a filler in a resin for the purpose of improving electrical insulation and imparting thermal conductivity. In the above-mentioned use of the boron nitride powder, the obtained resin composition has high electrical insulation and thermal conductivity.

[0065] The resin composition of the present invention can be used for known applications without any restrictions, but by mixing it with a resin described later to form a thermally conductive resin composition or a thermally conductive molded body, it can be preferably used for applications such as thermal interface materials such as polymer-based heat dissipation sheets and phase change sheets, organic heat dissipation sheets such as heat dissipation tapes, heat dissipation greases, heat dissipation adhesives, and gap fillers, heat dissipation paints such as heat dissipation paints and heat dissipation coats, heat dissipation resin substrates such as PWB-based resin substrates and CCL-based resin substrates, insulating layers for metal-based substrates such as aluminum-based substrates and copper-based substrates, sealing materials for power devices, and interlayer insulating films.

[0066] Furthermore, when the boron nitride powder of the present invention is prepared into a resin composition, it can be mixed with a thermally conductive filler such as aluminum nitride or aluminum oxide, which is a common highly thermally conductive insulating filler.

[0067] Examples of the resin include thermoplastic resins such as polyolefin, vinyl chloride resin, methyl methacrylate resin, nylon, and fluororesin; thermosetting resins such as epoxy resin, phenol resin, urea resin, melamine resin, unsaturated polyester resin, silicone resin, and bismaleimide triazine resin; fluororesin, liquid crystal polymer, and synthetic rubber.

[0068] The resin composition may contain, as necessary, known additives such as polymerization initiators, curing agents, polymerization inhibitors, polymerization retarders, coupling agents, plasticizers, UV absorbers, pigments, dyes, antibacterial agents, organic fillers, organic-inorganic composite fillers, etc., as compounding agents for resin compositions. In addition, other inorganic fillers may be contained within the range that does not impair the effects of the present invention.

[0069] The boron nitride powder of the present invention can also be used as a raw material for boron nitride processed products such as cubic boron nitride and boron nitride molded products, a nucleating agent for engineering plastics, a phase change material, a solid or liquid thermal interface material, a release agent for molten metal or molten glass molds, cosmetics, and a raw material for composite ceramics. EXAMPLES

[0070] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0071] In the examples, the values ​​measured were those obtained by the following methods.

[0072] [Median pore diameter based on volume (μm)] The pore volume-based median diameter of the obtained hexagonal boron nitride powder was measured by mercury intrusion porosimetry. The median diameter was calculated from the cumulative pore distribution obtained by plotting the pore diameter on the horizontal axis and the cumulative pore volume on the vertical axis when determining the pore distribution from 0.0036 μm to 200 μm. The calculation was performed using an Autopore IV9520 manufactured by Micromeritics.

[0073] [Oil absorption of hexagonal boron nitride powder according to JIS K5101-13-1:2004] The oil absorption of the obtained hexagonal boron nitride powder was determined based on the procedure specified in JIS K5101-13-1:2004 ("Testing methods for pigments" - Part 13: Oil absorption - Section 1: Refined linseed oil method).

[0074] [Specific surface area of ​​hexagonal boron nitride powder (m 2 / g)] The specific surface area of ​​the resulting hexagonal boron nitride powder was measured using Mountec's Macsorb HM model-1201.

[0075] [Particle size D1 (μm) at 50% cumulative volume frequency of particle size distribution of hexagonal boron nitride powder] The particle size (D1) at 50% cumulative volume frequency of the particle size distribution of the obtained hexagonal boron nitride powder was measured using HORIBA's LA-950V2. The particle size distribution of the hexagonal boron nitride powder was measured using a particle size distribution measuring device MT3000 manufactured by Nikkiso Co., Ltd. The measurement sample was prepared by the following method. First, 20 g of ethanol was added as a dispersion medium to a 50 mL screw tube bottle, and 1 g of hexagonal boron nitride powder was dispersed in the ethanol. The particle size at 50% cumulative volume frequency of the obtained particle size distribution was defined as (D1).

[0076] [Hexagonal boron nitride powder impurity element concentration (mass%)] The concentrations of impurity elements (calcium, magnesium, sodium, aluminum, lithium, strontium, iron, sulfur, nickel, chromium, manganese, silicon, phosphorus, titanium, barium, and cobalt) in the obtained hexagonal boron nitride powder were measured using a ZSX Primus2 (product name) manufactured by Rigaku Corporation.

[0077] Example 1 195g of boron oxide with a 425μm sieve residue of 2.1wt%, 99g of carbon black, and 55.2g of calcium carbonate were mixed using a Spartan mixer. The (B / C) element ratio of the mixture was 0.68, and the CaO-equivalent mass content of the oxygen-containing calcium compound was 10.5 parts by mass relative to 100 parts by mass of the total mass of the oxygen-containing boron compound and carbon source in terms of B2O3 and C. 1500g of the mixture was nitrided in a graphite Tammann furnace by holding it at 1500℃ for 6 hours and at 1940℃ for 4 hours under a nitrogen gas atmosphere.

[0078] Next, the by-product-containing boron nitride was crushed and placed in a container, and hydrochloric acid (7 mass% HCl) was added in an amount 5 times the amount of the by-product-containing boron nitride, and the mixture was stirred for 24 hours at a rotation speed of 350 rpm by a three-one motor. After the acid washing, the acid was filtered, and the boron nitride obtained by filtration was dispersed in pure water in the same amount as the acid used, and filtered again. This operation was repeated until the aqueous solution after filtration became neutral, and then the mixture was vacuum dried at 200°C for 12 hours.

[0079] After drying, the resulting powder was sieved through a sieve with 90 μm openings to obtain white hexagonal boron nitride powder. The physical properties of the resulting hexagonal boron nitride powder were measured by the methods described above and are shown in Tables 1 and 2.

[0080] Example 2 The same procedures as in Example 1 were carried out except that the residue on the 425 μm sieve of boron oxide was 2.9% by weight, the (B / C) element ratio was 0.72, and the mass content of the oxygen-containing calcium compound in terms of CaO was 8 parts by mass per 100 parts by mass of the total mass of the oxygen-containing boron compound and the carbon source in terms of B2O3 and C. The respective conditions and measured values ​​are shown in Tables 1 and 2.

[0081] Example 3 The same procedures as in Example 1 were carried out except that the residue on the 425 μm sieve of boron oxide was 1.0% by weight, the (B / C) element ratio was 0.65, and the mass content of the oxygen-containing calcium compound in terms of CaO was 6 parts by mass per 100 parts by mass of the total mass of the oxygen-containing boron compound and the carbon source in terms of B2O3 and C. The respective conditions and measured values ​​are shown in Tables 1 and 2.

[0082] Example 4 The same procedures were followed as in Example 1, except that the boron oxide residue on a 425 μm sieve was 0.1% by weight and the boron oxide residue on a 300 μm sieve was 15.0% by weight. The conditions and measured values ​​are shown in Tables 1 and 2.

[0083] Example 5 The same procedures were followed as in Example 1, except that the boron oxide residue on the 425 μm sieve was 0.5 wt%, the (B / C) element ratio was 0.70, and the mass content ratio of the oxygen-containing calcium compound in terms of CaO was 8 parts by mass relative to 100 parts by mass of the total mass of the oxygen-containing boron compound and carbon source in terms of B2O3 and C. The obtained boron nitride powder was also subjected to the above-mentioned 45 μm sieve treatment to prepare a sample in which the proportion of hexagonal boron nitride specific agglomerated particles was increased to 18.2%. The measured values ​​are shown in Tables 1 and 2.

[0084] Comparative Examples 1 to 6 The same procedure as in Example 1 was followed except for the changes in the conditions shown in Table 1. The conditions and measured values ​​are shown in Tables 1 and 2. The hexagonal boron nitride powder produced in Comparative Example 2 did not contain hexagonal boron nitride agglomerated particles corresponding to the present invention. The hexagonal boron nitride powder produced in Comparative Example 6 was not a white powder, but contained some residual carbon and black areas, and the powder properties were not analyzed.

[0085] [Resin composition] The boron nitride powder obtained in Examples 1 to 6 was filled into an epoxy resin to prepare a resin composition, and the thermal conductivity was evaluated. The epoxy resin was prepared by mixing 100 parts by mass (JER828 manufactured by Mitsubishi Chemical Corporation), 5 parts by mass of a curing agent (imidazole-based curing agent, Curesol 2E4MZ manufactured by Shikoku Kasei Co., Ltd.), and 210 parts by mass of methyl ethyl ketone as a solvent. Next, the varnish-like mixture and hexagonal boron nitride powder were mixed in a rotation-revolution mixer (MAZERUSTAR manufactured by Kurashiki Boseki Co., Ltd.) so that the base resin was 35% by volume and the specific boron nitride powder was 65% by volume, to obtain a resin composition.

[0086] The above resin composition was coated on a PET film to a thickness of about 250 to 300 μm using an automatic coater PI-1210 manufactured by Tester Sangyo Co., Ltd., dried, and cured under reduced pressure at a temperature of 200°C, a pressure of 5 MPa, and a holding time of 30 minutes to produce a sheet with a thickness of 220 μm. The sheet was analyzed using a temperature wave thermal analyzer, and the thermal conductivity was calculated, and the results are shown in Table 3. The thermal conductivity of the sheet filled with the hexagonal boron nitride powder produced in Examples 1 to 5 was 8.5 W / m·K or more, indicating high thermal conductivity. In addition, the dielectric strength was measured using a withstand voltage tester (manufactured by Tama Densoku Co., Ltd.), and the dielectric strength was high at 80 kV / mm or more, suggesting that there is little large void volume in the resin composition that may cause a decrease in dielectric strength.

[0087] In addition, the actual density was calculated from the volume and weight of the produced sheet, and the actual density / theoretical sheet density was calculated when the theoretical sheet density calculated from the filling rate of the resin and hexagonal boron nitride particles was set to 100%, and was used as the resin sheet relative density. The resin sheet produced with the hexagonal boron nitride powder of the present invention has an actual density / theoretical sheet density of 89 to 97%, and it can be seen that the resin sheet has minute voids that do not reduce the thermal conductivity and dielectric strength. Therefore, by using the hexagonal boron nitride powder of the present invention, it was possible to maintain high thermal conductivity and dielectric strength while realizing a reduction in the weight of the inorganic-filled resin sheet.

[0088] Moreover, the resin compositions were obtained in the same manner except that the boron nitride powders obtained in Comparative Examples 1 to 5 were used, and the thermal conductivity, dielectric strength, and resin sheet relative density were measured and are shown in Table 3. As is clear from the table, none of the sheets filled with the boron nitride powder obtained in Comparative Examples 1 to 5 were able to simultaneously achieve a thermal conductivity of 8.5 W / m K, a dielectric strength of 80 kV / mm or more, and a resin sheet relative density of 97.0% or less.

[0089] [Table 1]

[0090] [Table 2]

[0091] [Table 3]

Claims

1. The particle size distribution is determined by a wet laser diffraction particle size distribution method. The particle size distribution is determined by a particle size distribution method. 50 ) is 5 to 150 μm, the volume-based median diameter of pores measured by mercury intrusion porosimetry is 3.0 μm or less, and the content of impurity elements is 500 ppm or less.

2. BET specific surface area is 2 to 10 m 2 2. The hexagonal boron nitride powder according to claim 1, having a viscosity of 100 psig / g and an oil absorption of 50 to 190 cc / 100 g.

3. 3. The hexagonal boron nitride powder according to claim 1, containing 5% or more of agglomerated particles having a major axis of 5 to 10 μm, a major axis / minor axis ratio of 1.0 to 1.3, and a circularity of 0.3 to 0.

8.

4. A resin composition comprising the boron nitride powder according to any one of claims 1 to 3.

5. A resin sheet comprising the resin composition according to claim 4.

6. 6. The resin sheet according to claim 5, having a dielectric strength of 80 kV / mm or more.

7. 7. The resin sheet according to claim 5, wherein the sheet density is 89 to 97% of the theoretical density.

Citation Information

Patent Citations

  • Primary particle aggregate of hexagonal boron nitride, resin composition and application of the same

    JP2017165609A

  • Hexagonal boron nitride powder and method for producing the same

    JP2017222522A

  • Hexagonal boron nitride powder and manufacturing method therefor

    JP2019218254A

  • Process for producing boron nitride agglomerates

    JP2019521064A

  • Boron nitride powder and resin composition

    WO2020158758A1

Cited By

  • Hexagonal boron nitride powder, resin composition, resin sheet, and method for producing hexagonal boron nitride powder

    JP2026166591A