Metallic laminate and metallic molded body

A laminate structure with a thermoplastic resin and polyester adhesive layer addresses the corrosion issue of aluminum in automotive decorations, ensuring effective alkali resistance and maintaining the metallic appearance.

JP7588529B2Active Publication Date: 2024-11-22NIPPON CARBIDE KOGYO KK
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021041734
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-15
Publication Date
2024-11-22
Estimated Expiration
2041-03-15

AI Technical Summary

Technical Problem

Aluminum layers in metal-like molded bodies used for automotive decorations are susceptible to corrosion when exposed to alkaline substances like detergents and window washer fluids, leading to deterioration of the metallic appearance.

Method used

A laminate structure comprising a thermoplastic resin layer, an aluminum layer, and a polyester adhesive layer with a curing index of 15 or more, which enhances the adhesion and corrosion resistance of the aluminum layer.

Benefits of technology

The laminate structure effectively prevents corrosion of the aluminum layer by alkaline substances, maintaining the metallic appearance and reducing the dissolution distance, allowing for a smaller margin and improved durability in decorative applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588529000003
    Figure 0007588529000003
  • Figure 0007588529000004
    Figure 0007588529000004
  • Figure 0007588529000005
    Figure 0007588529000005
Patent Text Reader

Abstract

To provide a laminate including an aluminum layer having sufficient corrosion resistance against alkali, and a molding.SOLUTION: A metallic laminate includes a thermoplastic resin layer, an aluminum layer and an adhesive layer stacked in this order. The adhesive layer is composed of a polyester adhesive, and the curing index of the adhesive layer calculated by a specific formula is 15 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metallic laminate and a metallic molded product. [Background technology]

[0002] Metallic molded bodies are known as metallic decorative items for the exterior of automobiles, such as automobile emblems. As such metallic molded bodies, molded bodies are known that are formed by molding a laminated sheet having a transparent thermoplastic resin film, a metal layer, an adhesive layer, and a thermoplastic resin film in this order (see, for example, Patent Document 1). The transparent thermoplastic resin film in this molded body is, for example, a polyester-based polymer compound having a benzene ring and a cyclohexane ring in the main chain, and the metal of the metal layer is, for example, indium. The adhesive in the adhesive layer is, for example, a polyurethane-based adhesive.

[0003] Also, the above-mentioned metallic molded body is known to be a molded body obtained by molding a laminated sheet having, in this order, a transparent or semi-transparent surface film layer, an adhesive layer, a metal layer-retaining film layer of a polyester-based film or a polyolefin-based film having a metal layer on at least one side, a urethane-based adhesive layer, and a base film layer (see, for example, Patent Document 2). The metal layer in this molded body is formed, for example, on the surface of the metal layer-retaining film layer on the side of the base film layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2002-370311 A [Patent Document 2] JP 2004-001243 A Summary of the Invention [Problem to be solved by the invention]

[0005] Detergents used when washing cars and window washer fluids in cars are usually alkaline. This is to easily remove acidic dirt that accumulates in nature. However, when an aluminum layer is used as the metal layer of the metallic molded body, the aluminum layer may dissolve due to contact between the alkaline liquid and the molded body, and the metallic appearance of the molded body may be impaired.

[0006] An object of the present invention is to provide a laminate and a molded article in which the aluminum layer has sufficient corrosion resistance to alkali. [Means for solving the problem]

[0007] In order to solve the above problems, the metallic laminate according to the present invention has a thermoplastic resin layer, an aluminum layer, and an adhesive layer stacked in this order, the adhesive layer being made of a polyester-based adhesive, and the hardening index of the adhesive layer calculated from the following formula is 15 or more. (formula) Cure index = acid value x hydroxyl value x hydroxyl value equivalent crosslinking degree (In the above formula, "acid value" is the acid value (mgKOH / g) of the polyester-based adhesive, "hydroxyl value" is the hydroxyl value (mgKOH / g) of the polyester-based adhesive, and "degree of cross-linking by hydroxyl value equivalent" is the proportion of hydroxyl groups possessed by the polyester of the polyester-based adhesive that are subjected to cross-linking in the adhesive layer.)

[0008] In order to solve the above problems, the metallic molded product according to the present invention is a metallic molded product obtained by molding the metallic laminate of the present invention. Effect of the Invention

[0009] According to the present invention, it is possible to provide a laminate and a molded article in which the aluminum layer has sufficient corrosion resistance to alkali. [Brief description of the drawings]

[0010] [Figure 1]FIG. 1 is a cross-sectional view showing a layer structure of a laminate according to one embodiment of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view showing a layer structure of a laminate according to another embodiment of the present invention. [Diagram 3] FIG. 2 is a cross-sectional view showing a layer structure of a molded body according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Metallic laminate] Fig. 1 is a cross-sectional view showing the layer structure of a metallic laminate (hereinafter, simply referred to as "laminate") according to one embodiment of the present invention. As shown in Fig. 1, a laminate 10 of this embodiment has a thermoplastic resin layer 1, an aluminum layer 2, and a first adhesive layer 3 stacked in this order. In the laminate 10, an aluminum layer is used as the metallic layer, and a polyester-based adhesive is used as the adhesive of the first adhesive layer 3.

[0012] [Thermoplastic resin layer] The thermoplastic resin layer 1 is made of a thermoplastic resin. The thermoplastic resin layer 1 may be substantially transparent or opaque. "Substantially transparent" means that the layer has sufficient transparency so that the molded body has a metallic appearance due to the aluminum layer. The substantially transparent thermoplastic resin layer 1 can be a surface layer that constitutes the surface of the molded body.

[0013] If the thickness of the thermoplastic resin layer 1 is too thin, the thermoplastic resin layer 1 is likely to wrinkle during the aluminum deposition process, and the deposition of aluminum is likely to adhere unevenly. In addition, if the thickness of the thermoplastic resin layer 1 is too thin, the thermoplastic resin layer 1 may be likely to wrinkle when the first adhesive layer 3 is applied or when the surface resin layer described later is further laminated. If the thickness of the thermoplastic resin layer 1 is too thick, the flexibility required for molding the laminate may be insufficient, and the desired molded body may not be obtained. Alternatively, if the thickness of the thermoplastic resin layer 1 is too thick, internal stress is likely to remain during molding, and the molded body is likely to deform due to the stress when exposed to a high-temperature environment. The thickness of the thermoplastic resin layer 1 can be appropriately determined, for example, from 10 to 50 μm, more preferably from 15 to 30 μm, based on various conditions such as mechanical strength, optical function, and the desired moldability of the laminate 10.

[0014] The thermoplastic resin constituting the thermoplastic resin layer 1 may have a thermoplasticity that allows the molding of a molded article described below. The thermoplastic resin may be one or more types, and may contain additives within a range in which the effects of the present embodiment can be obtained. Furthermore, the thermoplastic resin can be appropriately selected from the viewpoint of exhibiting desired physical properties (e.g., alkali resistance, transparency, moldability, etc.) in the thermoplastic resin layer 1.

[0015] Examples of thermoplastic resins constituting the thermoplastic resin layer 1 include polyesters such as polyethylene terephthalate (PET), modified polyesters such as glycol-modified polyethylene terephthalate (PETG), acrylic resins, polyurethanes, polycarbonates, polyolefins, vinyl chloride resins, and acrylonitrile-butadiene-styrene (ABS) resins.

[0016] From the viewpoint of suppressing deterioration of the molded body due to alkali, it is preferable that the thermoplastic resin layer 1 has sufficient alkali resistance according to the application of the molded body. In general, since it has low permeability to alkaline solutions, it is preferable that the thermoplastic resin constituting the thermoplastic resin layer 1 is polyester, and among them, PET is more preferable from the viewpoint of increasing productivity of the laminate and the molded body because it is easy to obtain in addition to having high alkali resistance.

[0017] From the viewpoint of further enhancing the moldability of the laminate, the thermoplastic resin constituting the thermoplastic resin layer 1 is preferably a polyester having a benzene ring and a cyclohexane ring in the main chain, such as PETG. PETG is a glycol-modified polyethylene terephthalate, and has a molecular structure in which some of the ethylene glycol-derived structural units in the PET monomer are replaced with structural units derived from cyclohexanedimethanol. The substitution rate of the ethylene glycol-derived structural units with the cyclohexanedimethanol-derived structural units can be appropriately determined from the viewpoint of the desired moldability, and may be, for example, 30 to 40 mol%.

[0018] [Aluminum layer] The aluminum layer 2 is a layer made of metallic aluminum. The aluminum layer 2 may contain elements other than aluminum as long as it exhibits a desired metallic appearance. For example, the aluminum layer 2 may contain a dopant other than aluminum to change the hue of the metallic appearance.

[0019] If the thickness of the aluminum layer 2 is too thin, the light transmittance of the aluminum layer 2 becomes too high, and the expression of metallic luster may become insufficient. If the thickness of the aluminum layer 2 is too thick, the expression of the metallic appearance and the concealing property of the aluminum layer 2 may reach a plateau, which may increase the cost, and cracks or whitening may easily occur during hot forming in the production of the molded product. The thickness of the aluminum layer 2 can be appropriately determined, preferably from between 20 and 100 nm, based on various conditions such as the optical effect and the desired moldability of the laminate 10.

[0020] It is preferable that the aluminum layer 2 is in close contact with the surface of the thermoplastic resin layer 1 from the viewpoint of fully exhibiting alkali resistance in the molded body. Such an aluminum layer 2 can be formed on the surface of the thermoplastic resin layer 1 using known techniques such as vacuum deposition, sputtering, and chemical vapor deposition (CVD). Aluminum can be deposited in a planar shape, and can form a layer having high reflectivity and high brightness. Therefore, the aluminum layer 2 is advantageous from the viewpoint of increasing the L value (brightness) of the molded body.

[0021] [First adhesive layer] The first adhesive layer 3 is composed of a polyester-based adhesive. The polyester-based adhesive is composed of a composition containing polyester as a main component. Here, the term "main component" means the component that is the largest in the composition. The polyester-based adhesive may be composed of one or more types of polyester.

[0022] In addition to the polyester as the main component, the polyester adhesive may further contain other resins and additives within a range that satisfies the condition of the hardening index described later. Examples of other resins include resins having polar groups that are added to increase the cohesive force in the first adhesive layer 3, and any resin that is compatible with the polyester may be used, and examples of such resins include vinyl chloride resins, epoxy resins, polystyrene, and polyvinyl ether. Examples of additives include defoamers, leveling agents, antioxidants, ultraviolet absorbers, and colorants. Compared to polyurethane-based or acrylic-based adhesives, polyester-based adhesives can increase the alkali resistance of laminates and molded products.

[0023] The cure index of the first adhesive layer 3 is equal to or greater than 15. The "cure index" is calculated from the following formula. (formula) Cure index = acid value x hydroxyl value x hydroxyl value equivalent crosslinking degree

[0024] The higher the cure index, the more the corrosion of the aluminum layer 2 in the laminate or molded body caused by an alkaline solution can be reduced (the alkali resistance can be increased). From this viewpoint, the cure index is preferably 20 or more, more preferably 25 or more, even more preferably 30 or more, and even more preferably 40 or more. The cure index may be within a range that can be realized by the structure of the polyester, and from this viewpoint, may be 350 or less. The cure index can be adjusted by the acid value, hydroxyl value, and degree of crosslinking of the hydroxyl value equivalent described in the above formula.

[0025] The "acid value" in the above formula is the acid value (mgKOH / g) of the polyester adhesive in the first adhesive layer 3. The acid value is preferably high from the viewpoint of realizing good adhesion to polar surfaces. When the acid value is high, the adhesion at the interface between the first adhesive layer 3 and the aluminum layer 2 adhered thereto is strengthened, and the generation of air bubbles at the interface between the two layers is reduced, which is effective in preventing the intrusion of an alkaline solution into the interface. In addition, when the acid value is high, the compatibility of the two resins is further improved when a resin for improving cohesive strength is mixed into the polyester adhesive.

[0026] The acid value of the polyester adhesive can be appropriately determined according to the curing index, hydroxyl value, and crosslinking degree of hydroxyl value equivalent in the above formula, and from the above viewpoint, the acid value of the polyester adhesive is preferably 0.3 mgKOH / g or more, more preferably 0.4 mgKOH / g or more. The acid value of the polyester adhesive is preferably higher from the viewpoint of increasing the curing index, but it is sufficient as long as it is within the range that can be realized by the polyester adhesive, and it is required to have sufficient stability as a coating material. From such a viewpoint, the acid value of the polyester adhesive may be, for example, 40 mgKOH / g or less, or 35 mgKOH / g or less. The acid value of the polyester adhesive may be adjusted within the above acid value range by using two or more polyester adhesives in combination.

[0027] The acid value of the polyester adhesive may be a measured value by a known method for measuring the acid value of a polyester adhesive, such as that specified in Japanese Industrial Standards (JIS) K0070:1992, or may be a catalog value. The acid value can be adjusted by the amount of free fatty acid in the polyester adhesive. When the polyester adhesive does not substantially contain any component having an acid value other than polyester, the acid value may be the acid value of the polyester in the polyester adhesive.

[0028] The "hydroxyl value" in the above formula is the hydroxyl value (mgKOH / g) of the polyester adhesive in the first adhesive layer 3. The hydroxyl value is preferably high from the viewpoint of increasing the number of hydroxyl groups that can become crosslinking points in the polyester adhesive. When the hydroxyl value is high, the hydroxyl groups of the polyester constituting the polyester adhesive are subjected to crosslinking, thereby increasing the cohesive force of the first adhesive layer 3, which is effective in strengthening the adhesion between the first adhesive layer 3 and the aluminum layer 2.

[0029] The hydroxyl value of the polyester adhesive can be appropriately determined according to the crosslinking degree of the cure index, acid value, and hydroxyl value equivalent in the above formula, similarly to the acid value, and from the above viewpoint, the hydroxyl value of the polyester adhesive is preferably 0.5 mgKOH / g or more. The hydroxyl value of the polyester adhesive is preferably as high as possible from the viewpoint of increasing the cure index, but may be within a range that can be realized by the polyester adhesive, for example, 40 mgKOH / g or less. The hydroxyl value of the polyester adhesive may be adjusted to within the above hydroxyl value range by using two or more polyester adhesives in combination.

[0030] The hydroxyl value of the polyester adhesive may be a measured value by a known method for measuring the hydroxyl value of the polyester constituting the polyester adhesive as specified in JIS K0070:1992, or may be a catalog value. The hydroxyl value can be adjusted, for example, by introducing hydroxyl groups into the polyester constituting the polyester adhesive. When the polyester adhesive does not substantially contain any component having a hydroxyl value other than polyester, the hydroxyl value may be the hydroxyl value of the polyester in the polyester adhesive.

[0031] The "degree of crosslinking by hydroxyl value equivalent" in the above formula is the ratio of hydroxyl groups of the polyester of the polyester-based adhesive that are subjected to crosslinking in the first adhesive layer 3. The degree of crosslinking can be determined according to the type and amount of the crosslinking agent. For example, when the crosslinking agent is polyisocyanate, the isocyanate group usually reacts with the hydroxyl group of the polyester substantially one-to-one. Therefore, if the crosslinking agent is polyisocyanate, the "degree of crosslinking by hydroxyl value equivalent" is expressed as the ratio of the amount of isocyanate groups to the amount of hydroxyl groups of the polyester in the first adhesive layer 3.

[0032] More specifically, the "degree of crosslinking by hydroxyl value equivalent" is the degree of crosslinking of the crosslinkable functional group per hydroxyl equivalent, and is calculated as the ratio of the NCO equivalent of the isocyanate, which is the crosslinkable functional group, to the hydroxyl equivalent of the polyester, that is, NCO equivalent / hydroxyl equivalent. Here, the NCO equivalent may be calculated from the amount of polyisocyanate used (unit: g), the NCO% of the polyisocyanate, and the mass of NCO equivalent to 1 mole (42 g). The hydroxyl equivalent may be calculated from the amount of polyester resin used (unit: g), the hydroxyl value of the polyester resin, and the mass of OH equivalent to 1 mole (17 g).

[0033] The degree of crosslinking of the hydroxyl value equivalent is preferably high from the viewpoints of strengthening the adhesion between the first adhesive layer 3 and the aluminum layer 2 and enhancing the alkali resistance of the laminate or molded body. By using hydroxyl groups derived from the polyester constituting the polyester-based adhesive as crosslinking points, bonds such as chemical bonds or hydrogen bonds are further introduced into the first adhesive layer 3, making it possible to form a denser three-dimensional structure in the first adhesive layer 3. As a result, it becomes possible to further increase the cohesive force of the first adhesive layer 3 and further suppress the penetration of an alkaline solution.

[0034] The preferred range of the crosslinking degree of the hydroxyl value equivalent may vary depending on the type of crosslinking agent or the type of polyester, and cannot be generalized; however, from the viewpoint of suppressing the influence of inactivation of crosslinkable functional groups due to moisture in the air, and from the viewpoint of suppressing the influence of uncrosslinked hydroxyl groups on the water resistance and alkali resistance of a laminate or molded body, the crosslinking degree of the hydroxyl value equivalent is preferably 0.1 or more, more preferably 0.3 or more, even more preferably 0.5 or more, and most preferably 1.

[0035] However, the degree of crosslinking of the hydroxyl value equivalent calculated when producing the polyester adhesive composition may exceed 1 as a theoretical value, for example, may be 1.2 or less, or may be 1.1 or less. For example, increasing the degree of crosslinking from 1 to a direction exceeding 1, for example, from 1 to approaching 1.2, is preferable from the viewpoint of more quickly completing the reaction between the crosslinking agent and the polyester resin. In addition, decreasing the degree of crosslinking from a side exceeding 1 toward 1, for example, from 1.2 or less to approaching 1, is preferable from the viewpoint of reducing the amount of uncrosslinked crosslinking agent contained in the first adhesive layer. In addition, the degree of crosslinking is preferable from 0.1 to approaching 1 from the viewpoint of suppressing the influence of unreacted crosslinking agent on the alkali resistance of the laminate or molded body.

[0036] The degree of crosslinking of the hydroxyl value equivalent can be appropriately determined depending on the type of crosslinking agent blended in the first adhesive layer 3 or the reactivity of the crosslinking agent with respect to hydroxyl groups under the conditions in which the first adhesive layer 3 is used for adhesion, and the amount of the crosslinking agent. As described above, if the crosslinking agent is one that normally bonds to hydroxyl groups at room temperature, such as polyisocyanate, the degree of crosslinking of the hydroxyl value equivalent can be expressed as the ratio of the amount of crosslinkable functional groups possessed by the crosslinking agent to the amount of hydroxyl groups. If the crosslinking agent has reactivity with hydroxyl groups at a predetermined ratio of less than 1 under the conditions in which the first adhesive layer 3 is used for adhesion, the degree of crosslinking of the hydroxyl value equivalent can be obtained by multiplying the ratio of the amount of the crosslinking agent to the amount of hydroxyl groups by the reactivity rate of the crosslinking agent with respect to hydroxyl groups.

[0037] The degree of crosslinking of the hydroxyl value equivalent can be adjusted by, for example, the amount of a crosslinking agent such as polyisocyanate having multiple functional groups that react with hydroxyl groups added to the polyester adhesive. The degree of crosslinking of the hydroxyl value equivalent can also be adjusted by using crosslinking agents with different reactivity with hydroxyl groups.

[0038] Examples of preferred crosslinking agents include polyisocyanates, and examples thereof include hexamethylene diisocyanate, isophorone diisocyanate, tolylene diisocyanate, xylene diisocyanate, diphenylmethane diisocyanate, isocyanurates of these polyisocyanates, trimethylolpropane (TMP) adducts of these polyisocyanates, and prepolymers having an isocyanate group at the end.

[0039] In the case of manufacturing the laminate of this embodiment, the degree of crosslinking of the hydroxyl value equivalent may be estimated according to the manufacturing conditions of the laminate and the material of the first adhesive layer. For example, it is preferable to estimate and determine the degree of crosslinking of the hydroxyl value equivalent in the laminate by estimating that the crosslinking agent reacts stoichiometrically with the polyester resin in its entirety and by estimating the degree of crosslinking of the hydroxyl value equivalent in the laminate from the amount of the polyester adhesive and the amount of the crosslinking agent used. In theory, the amount of the crosslinking agent used may be determined so that the degree of crosslinking of the hydroxyl value equivalent is higher than 1.0, but it should be determined within a range in which the effect of the present invention is not impaired by an excess of the crosslinking agent.

[0040] Alternatively, the acid value, hydroxyl value, and crosslinking degree of hydroxyl value equivalent may be estimated by hydrolysis of the first adhesive layer 3 in the laminate or molded body. For example, the first adhesive layer 3 in the laminate or molded body is treated under predetermined conditions for hydrolyzing urethane bonds. Then, the hydroxyl group and the crosslinking degree of hydroxyl value equivalent in the first adhesive layer 3 may be estimated by estimating the hydroxyl group and the substantially same amount of amino group generated by the treatment in the polymer compound derived from the polyester adhesive as the hydroxyl group before crosslinking. Similarly, the acid value in the first adhesive layer 3 may be estimated by estimating the compound having a lower molecular weight than the polymer compound among the hydrolyzates of the first adhesive layer 3 as described above.

[0041] The first adhesive layer 3 may have other physical properties besides the cure index within a range in which the effects of this embodiment are achieved. The molecular weight of the polyester in the first adhesive layer 3 can be appropriately determined according to the desired physical properties of the polyester-based adhesive. For example, the molecular weight of the polyester in the first adhesive layer 3 may be appropriately determined from the viewpoint of physical properties such as the shear strength, adhesion strength, and viscosity of the polyester-based adhesive. By appropriately determining the molecular weight of the polyester, it is possible to further improve the adhesion of the first adhesive layer 3 or the coatability of the polyester-based adhesive.

[0042] The molecular weight of the polyester in the first adhesive layer 3 is preferably, in terms of number average molecular weight, 5000 or more, and more preferably 6000 or more, from the viewpoint of, for example, enhancing the adhesion of the first adhesive layer 3. Furthermore, from the viewpoint of, for example, the coatability of a polyester-based adhesive, the molecular weight of the polyester in the first adhesive layer 3 is preferably, in terms of number average molecular weight, 50,000 or less, and more preferably 40,000 or less.

[0043] The number average molecular weight of the polyester may be a value measured by a known technique for measuring the number average molecular weight of a polyester constituting a polyester-based adhesive, such as gel permeation chromatography (GPC), or may be a catalog value.

[0044] The glass transition temperature of the polyester in the first adhesive layer 3 can be appropriately determined from the viewpoint of the handleability of the laminate. If the glass transition temperature is too low, the viscosity or storage modulus of the resin in the first adhesive layer 3 in a high-temperature environment may decrease, and the durability performance at high temperatures may become insufficient. If the glass transition temperature is too high, the deformability of the first adhesive layer 3 may be insufficient, and for example, the adhesion to the material to be laminated when laminating with the surface resin layer described later may become insufficient. Even if the deformability of the first adhesive layer 3 is insufficient, a method of laminating while heating with a heating roll is also possible as a method of sufficiently increasing the adhesion by lamination. In this method, care must be taken because wrinkles are likely to occur in the thermoplastic resin layer. From the viewpoint of fully expressing the durability and deformability at high temperatures, the glass transition temperature is preferably -10 to 30°C, and more preferably 0 to 20°C. From the viewpoint of making the first adhesive layer 3 deformable by sufficiently following the adhesive surface at room temperature (for example, 20°C), the glass transition temperature is preferably 20°C or less.

[0045] The glass transition temperature of the polyester in the first adhesive layer 3 may be a measured value obtained by a known method for measuring the glass transition temperature of the polyester constituting a polyester-based adhesive, such as that specified in JIS K7121:2012, or may be a catalog value.

[0046] The polyester-based adhesive of the first adhesive layer 3 can be appropriately selected within a range that provides the desired physical properties as described above. The polyester-based adhesive may be a synthetic product or a commercially available product.

[0047] The thickness of the first adhesive layer 3 may be appropriately determined according to various conditions required for the laminate or molded body, such as the state of the surface to which the first adhesive layer 3 is adhered and the desired adhesive strength. If the thickness of the first adhesive layer 3 is too thin, partial removal and repelling of the adhesive is likely to occur when the polyester adhesive is applied to the thermoplastic resin layer. In addition, if the thickness of the first adhesive layer 3 is too thin, the wetting of the part to be adhered (bonded) to the first adhesive layer 3 may be insufficient, resulting in insufficient adhesive strength. On the other hand, if the thickness of the first adhesive layer 3 is too thick, the stress generated in the first adhesive layer 3 when a shear force is applied to the first adhesive layer 3 becomes large, and peeling in the first adhesive layer 3 is likely to occur. The desired adhesiveness and peel resistance of the first adhesive layer 3 can be appropriately determined according to the application of the laminate, and therefore the thickness of the first adhesive layer 3 can be appropriately determined according to the application of the laminate. For example, in the case of a laminate for forming a molded body for the exterior of an automobile, the thickness of the first adhesive layer 3 may be appropriately determined within the range of 4 to 10 μm (eg, 10 μm).

[0048] [Other layers] The laminate of this embodiment may further include layers other than those described above, so long as the effects of this embodiment can be obtained. The thickness of the layers may be appropriately determined so long as the layers can exhibit their intended functions, and the layers may appropriately contain components other than the main components, such as additives.

[0049] For example, the laminate 10 may further have a surface resin layer that adheres to the first adhesive layer 3 .

[0050] The surface resin layer is a layer that constitutes the surface of the laminate 10. It is preferable that the surface resin layer has transparency from the viewpoint of obtaining a clearer metallic appearance due to the aluminum layer 2. It is also preferable that the surface resin layer has weather resistance from the viewpoint of increasing the durability of the laminate or molded body in exterior applications. Furthermore, it is preferable that the surface resin layer is composed of a thermoplastic resin from the viewpoint of ensuring the moldability of the laminate.

[0051] From the above viewpoint, the surface resin layer is preferably composed of a thermoplastic resin having transparency and weather resistance. Examples of thermoplastic resins having transparency include acrylic resins, fluororesins, polyvinyl chloride, polyolefins, polystyrene, polyurethane, polyamide, ABS resins, polyesters, polycarbonates, silicone resins, and alicyclic polyolefins. Examples of thermoplastic resins having weather resistance include acrylic resins, polyesters, polycarbonates, silicone resins, and alicyclic polyolefins. Among them, acrylic resins are preferred from the viewpoint of sufficient transparency and weather resistance.

[0052] Also, for example, the laminate 10 may further include an additional adhesive layer (hereinafter also referred to as a "second adhesive layer") and a base layer. The adhesive layer and the base layer are further arranged in this order on the side of the thermoplastic resin layer 1 opposite to the aluminum layer 2.

[0053] The second adhesive layer is a layer for bonding the thermoplastic resin layer 1 and the base material layer. The second adhesive layer is composed of an adhesive capable of bonding the thermoplastic resin layer 1 and the base material layer. The adhesive can be appropriately selected from known adhesives depending on the materials of both layers. For example, the adhesive constituting the second adhesive layer may be the same as the polyester adhesive described above, or may be different.

[0054] Examples of such adhesives other than the polyester-based adhesives mentioned above include polyurethane-based, polyethylene-based, polyamide-based, polyvinyl chloride-based, polychloroprene-based, carboxylated rubber-based, thermoplastic styrene-butadiene rubber-based, acrylic-based, styrene-based, cellulose-based, alkyd-based, polyvinyl acetate-based, ethylene-vinyl acetate copolymer-based, polyvinyl alcohol-based, epoxy-based and silicone-based adhesives, as well as natural and synthetic rubber.

[0055] The substrate layer is a layer for reinforcing the laminate and the molded body. From the viewpoint of maintaining the shape of the molded body, the substrate layer preferably has a mechanical strength according to the application and shape of the molded body. In addition, from the viewpoint of ensuring the moldability of the laminate, the substrate layer is preferably composed of a thermoplastic resin. The substrate layer may or may not have transparency. Examples of the thermoplastic resin constituting the substrate layer include acrylic resin, polyurethane, polyester, polycarbonate, polyolefin, vinyl chloride resin, and ABS resin.

[0056] Fig. 2 is a cross-sectional view showing the layer structure of a laminate according to another embodiment of the present invention. As shown in Fig. 2, in the laminate 20, a surface resin layer 4 is adhered to a first adhesive layer 3 in the laminate 10. Furthermore, a second adhesive layer 5 and a base layer 6 are laminated in this order on the surface of the thermoplastic resin layer 1 in the laminate 10 opposite to the aluminum layer 2. Thus, in the laminate 20, the aluminum layer 2 is disposed on the surface side of the thermoplastic resin layer 1.

[0057] The laminate 20 may be used for the exterior of an automobile, and the second adhesive layer 5 and the base layer 6 are appropriately determined according to the application. In this case, as an example, the adhesive constituting the second adhesive layer 5 is a polyester adhesive, and the thermoplastic resin constituting the base layer 6 is an ABS resin. The adhesive constituting the second adhesive layer 5 may be the same as that of the first adhesive layer 3, or may be different. The laminate 20 may be used for decorative purposes with a metallic appearance due to the aluminum layer 2, by bonding the base layer 6 to a portion to be decorated with the surface resin layer 4 side in the lamination direction as the front side.

[0058] [Method of manufacturing laminate] The laminate of this embodiment can be manufactured by a method capable of realizing the above-mentioned layer structure, and such a method can be realized by utilizing a known method for manufacturing laminates.

[0059] For example, the laminate of this embodiment can be produced by forming an aluminum layer 2 on one surface of a thermoplastic resin layer 1, for example by vacuum deposition, and forming a first adhesive layer 3 on the surface of the aluminum layer 2, for example by laminating or coating and drying.

[0060] In the case where the laminate further includes the surface resin layer 4, the aluminum layer 2 is formed on one surface of the thermoplastic resin layer 1 by vacuum deposition, and the first adhesive layer 3 is formed on one surface of the surface resin layer 4. The aluminum layer 2 and the first adhesive layer 3 are then attached to each other and pressure-bonded. In this manner, the above-mentioned laminate can be manufactured.

[0061] Alternatively, in the case where the surface resin layer 4 is further included, the laminate of the present embodiment is formed by further attaching the surface resin layer 4 to the surface of the first adhesive layer 3 in the laminate structure of the thermoplastic resin layer 1, the aluminum layer 2, and the first adhesive layer 3, and then pressing them together. In this manner, the above-mentioned laminate can be manufactured.

[0062] Similarly, in the case where the laminate of this embodiment further includes a second adhesive layer 5 and a base layer 6, the laminate can be produced by forming a second adhesive layer 5 on the other surface of the thermoplastic resin layer 1, bonding the base layer 6 to the second adhesive layer 5, and pressing them together.

[0063] Alternatively, in the case where the laminate of this embodiment further includes a second adhesive layer 5 and a base layer 6, the laminate of this embodiment can be produced by forming the second adhesive layer 5 on one surface of the base layer 6, and bonding the second adhesive layer 5 and the thermoplastic resin layer 1 together and pressing them together.

[0064] In the above manufacturing method, when a crosslinking agent is applied to the adhesive layer, the adhesive layer can be formed by a known method. For example, in the above case, the adhesive and the crosslinking agent are blended in a liquid state and mixed. Then, the obtained adhesive is applied to the part where the adhesive layer is to be formed. In this way, the adhesive layer can be formed. The application of the adhesive can be realized by a known technique, and can be performed using, for example, a bar coater, a knife coater, a gravure coater, or a three-reverse coater. A gravure coater is more preferably used for applying the adhesive, and among them, a kiss gravure coater can be more preferably used.

[0065] [Application] The laminate according to the embodiment of the present invention is preferably used for exterior applications of moving objects such as automobiles and motorcycles. It is preferable that the laminate further has preferable physical properties from the viewpoint of such exterior applications. Examples of the preferable physical properties include weather resistance, heat resistance, and strength.

[0066] In exterior applications, the laminate and the molded product described below are prone to deterioration due to sunlight. Weather resistance is a property that suppresses and prevents deterioration of appearance or strength due to sunlight. The weather resistance of the laminate can be achieved by forming the surface of the laminate for exterior applications from a resin material having the above-mentioned weather resistance.

[0067] In exterior applications, the laminate and the molded product described below are exposed to an environment in which high temperatures during the day and low temperatures at night are repeated during use, and are particularly susceptible to deterioration in the high temperature environment during the day. Heat resistance is a property that suppresses and prevents deterioration of the appearance or reduction in strength due to the high temperature environment during use of the laminate or molded product. The heat resistance of the laminate can be achieved by using a resin material that has sufficient stability in the high temperature environment in exterior applications, or by using materials with a sufficiently small difference in thermal expansion or thermal contraction for the materials of adjacent layers in the stacking direction. The heat resistance of the laminate can be appropriately determined depending on the application of the laminate and the molded product.

[0068] In exterior applications, the laminate and the molded article described below are susceptible to forces from the external environment, and in addition to being strong enough to maintain their own shape, it is preferable that they also have sufficient strength against external forces that may be applied during use. The strength of the molded article can be calculated from the product of the tensile modulus and thickness of the laminate, and the tensile modulus of the laminate can be appropriately determined depending on the application of the laminate and the molded article and the thickness of the laminate. Therefore, the strength of the laminate and the molded article according to the application can be specified by the tensile modulus of the laminate.

[0069] [Metallic Molded Body] A metallic molded body according to one embodiment of the present invention (hereinafter, simply referred to as a "molded body") is formed by molding the metallic laminate of this embodiment described above. FIG. 3 is a cross-sectional view showing the layer structure of a molded body according to one embodiment of the present invention. As shown in FIG. 3, the molded body 100 includes a convex portion 101 and edge portions 102 located on both sides of the convex portion 101. The convex portion 101 is a portion having a trapezoidal cross-sectional shape with an upper side above the paper surface and a lower side below the upper side that is longer than the upper side. The edge portion 102 is a portion that extends further laterally from the lower side of the trapezoid.

[0070] The molded body 100 has a layer structure in which a base layer 6, a second adhesive layer 5, a thermoplastic resin layer 1, an aluminum layer 2, a first adhesive layer 3, and a surface resin layer 4 are laminated in this order. In the molded body 100, each layer is in close contact with the adjacent layer in the lamination direction, and is exposed at the edge of the edge portion 102. Furthermore, Lb in FIG. 3 represents the distance (width) from the convex portion 101 of the edge portion 102. The width Lb of the edge portion 102 is determined according to the specifications of the molded body 100, and when the molded body 100 is an exterior decorative item for an automobile, it can be set to less than 0.8 mm, for example, 0.7 mm.

[0071] The molded body of the present embodiment can be manufactured by a known method for molding a sheet-like material made of a thermoplastic resin having a metal layer, except that the laminate of the present embodiment is used as a material. Examples of the method for manufacturing the molded body of the present embodiment include vacuum molding, pressure molding, vacuum pressure molding, and press molding.

[0072] The molded article 100 is adhered to the site of use by a method known for automotive exterior applications. For example, a filler is filled into the recess on the back side of the convex portion 101, which is surrounded by the base layer 6 on three sides, the top surface and both sides connected to it when in use, and an adhesive layer for installation is formed so as to cover the filler and form the bottom surface of the molded article 100. The filler may be any resin material that can be normally used in molding, and may be, for example, a two-component curing urethane resin material.

[0073] The molded body 100 is then adhered to a desired installation location, for example, a location on the exterior surface of an automobile to be decorated, via the adhesive layer. The molded body 100 is preferably used as an emblem, badge, patch, sticker, seal, label, nameplate, or ribbon that can be deformed to follow the shape of the surface and is attached to the exterior of a vehicle such as an automobile or the surface of an object installed outdoors. The molded body 100 is particularly useful as a molded body having a three-dimensional structure such as the above-mentioned emblem.

[0074] [Action and Effect] The laminate according to the embodiment of the present invention is composed of a thermoplastic resin layer, an aluminum layer, and a first adhesive layer stacked in this order. In the laminate according to the present embodiment, the aluminum layer is sandwiched between the first adhesive layer made of a polyester adhesive and the thermoplastic resin layer. Therefore, the first adhesive layer exhibits sufficiently strong adhesion to the aluminum layer, and as a result, a strong laminate structure including the aluminum layer is formed. Therefore, the penetration of an alkaline solution from the outside into the aluminum layer is suppressed, and as a result, the dissolution of the aluminum layer by the alkaline solution is suppressed.

[0075] In addition, the first adhesive layer made of a polyester adhesive has an acid value and a hydroxyl value that allow the polyester adhesive to exhibit a sufficient hardening index. Therefore, sufficient adhesion as described above is exhibited, sufficient adhesive strength is exhibited in the laminate, and the dissolution distance in the laminate and the molded body is sufficiently small. As a result, corrosion of the aluminum layer by alkali is sufficiently suppressed. The "dissolution distance" is the distance from the edge of the laminate or molded body into which the alkali solution has penetrated to the tip of the part where the aluminum layer has dissolved, for example, the deepest part, when the alkali solution has penetrated into the inside of the laminate or molded body from the edge.

[0076] The laminate can be molded as a sheet material for molding to form a molded body. The laminate according to the embodiment of the present invention can make the above-mentioned dissolution distance shorter than that of the conventional laminate, for example, 0.7 mm or less. On the other hand, in a molded body obtained by molding the laminate, a margin corresponding to the above-mentioned dissolution distance (for example, the above-mentioned edge portion 102) is usually set on the periphery so as not to substantially impair the metallic appearance caused by alkaline corrosion. In the molded body according to the embodiment of the present invention, since the dissolution distance of the laminate is shorter, it is possible to make the margin shorter than that of the conventional molded body, for example, sufficiently small, such as 0.7 mm or less. Therefore, the embodiment of the present invention is advantageous in realizing a molded body with excellent decorativeness in which deterioration of the metallic appearance caused by alkaline corrosion is prevented and the margin of the periphery for preventing the corrosion is smaller in decorative applications.

[0077] The laminate of the embodiment of the present invention can be composed of an acrylic resin surface layer, a first adhesive layer, an aluminum layer, a transparent thermoplastic resin layer composed of a polyester having a main chain with a benzene ring and a cyclohexane ring, and a base layer composed of a second adhesive layer and a thermoplastic resin. A laminate of this structure is further advantageous as a material sheet for forming a molded body for decorative purposes, since the aluminum layer clearly expresses its metallic appearance while being protected by the surface resin layer, and the base layer enhances its mechanical strength.

[0078] [Modifications] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the different embodiments are also included in the technical scope of the present invention.

[0079] For example, in the laminates 10 and 20, the aluminum layer 2 may be laminated on the thermoplastic resin layer 1 via another layer. For example, the thermoplastic resin layer 1 and the aluminum layer 2 may be laminated on each other via a layer that has excellent adhesion to both layers, and examples of such a layer include an adhesive layer and an organic or inorganic intermediate layer.

[0080] The molded body of the present invention may be molded from the laminate 10. For example, a molded body may be formed by overlapping a release layer on the first adhesive layer 3 and molding it. Such a molded body may be installed at an installation location by the adhesive force of the first adhesive layer 3, or, similar to the above-mentioned molded body 100, may be installed by one of a filler and an adhesive layer for installation covering it, or by both. In this case, a resin that exhibits sufficient transparency, such as PETG, is used for the thermoplastic resin of the thermoplastic resin layer 1, so that a laminate and a molded body that fully exhibit a metallic appearance due to the aluminum layer 2 through the thermoplastic resin layer 1 can be obtained.

[0081] Alternatively, the laminate of the present invention may be composed of the laminate 10, the surface resin layer 4, and the second adhesive layer 5. In this case, the laminate of the present invention can be a sheet-like decorative body for exterior use, and can also be a decorative body for exterior use (molded body) having a three-dimensional shape by molding it in the same manner as the molded body 100.

[0082] 〔summary〕 As is clear from the above description, the metallic laminate (laminate 10) of the embodiment of the present invention has a thermoplastic resin layer (1), an aluminum layer (2), and an adhesive layer (first adhesive layer 3) stacked in this order, the adhesive layer being made of a polyester-based adhesive, and the hardening index of the adhesive layer being 15 or more. The metallic molded product (molded product 100) of the embodiment of the present invention is formed by molding the metallic laminate (laminate 20) as described above. Therefore, corrosion of the aluminum layer due to the intrusion of an alkaline solution from the periphery is sufficiently suppressed, and the laminate and molded product of the embodiment of the present invention can exhibit sufficient corrosion resistance of the aluminum layer against alkali.

[0083] In an embodiment of the present invention, the cure index of the adhesive layer may be equal to or greater than 30. This configuration is even more effective in terms of enhancing the alkali resistance of the laminate and the molded product.

[0084] In an embodiment of the present invention, the thermoplastic resin layer may be made of a polyester having a benzene ring and a cyclohexane ring in the main chain, which is more effective in terms of improving the moldability of the laminate.

[0085] In an embodiment of the present invention, the laminate (20) further has a surface resin layer (4) that adheres to the adhesive layer, and the surface resin layer may be made of a thermoplastic resin that has transparency and weather resistance. This configuration is more effective from the viewpoint of clarifying the metallic appearance of the aluminum layer and from the viewpoint of improving weather resistance.

[0086] In an embodiment of the present invention, the laminate further includes an additional adhesive layer (second adhesive layer 5) and a base layer (6) in this order on the side of the thermoplastic resin layer opposite to the aluminum layer, and the base layer may be made of a thermoplastic resin. This configuration is more effective in terms of the formability of the laminate and in terms of increasing the strength after forming. EXAMPLES

[0087] An embodiment of the present invention will now be described.

[0088] [Preparing the adhesive] The following adhesives 1 to 8 were prepared as adhesives for the adhesive layer. Adhesive 1 is "Byron GK-680" manufactured by Toyobo Co., Ltd. ("Byron" is a registered trademark of the company). Adhesive 2 is "Byron GK-590" manufactured by Toyobo Co., Ltd. Adhesive 3 is "TM-K76" manufactured by Toyo Morton Co., Ltd. Adhesive 4 is "TM-K51" manufactured by Toyo Morton Co., Ltd. Adhesive 5 is "Byron GK-570" manufactured by Toyobo Co., Ltd. All of adhesives 1 to 5 are polyester (PES)-based adhesives.

[0089] Adhesive 6 is "Bontator HUX-386" manufactured by ADEKA Corporation ("Bontator" is a registered trademark of the company). Adhesive 7 is "Rezamin UD-8336" manufactured by Dainichiseika Color & Chemicals Mfg. Co., Ltd. ("Rezamin" is a registered trademark of the company). Both adhesives 6 and 7 are polyurethane (PU)-based adhesives. Adhesive 6 is a water-based polyurethane-based adhesive, and adhesive 7 is a solvent-based polyurethane-based adhesive with a crosslinking agent added.

[0090] The adhesive 8 is "Nissetsu SM412" manufactured by Nippon Carbide Industries Co., Ltd. ("Nissetsu" is a registered trademark of the company). The adhesive 8 is an acrylic resin (AR)-based adhesive, and is a solvent-based acrylic resin-based adhesive.

[0091] Table 1 shows the type of resin, number average molecular weight Mn, glass transition temperature Tg, acid value, and hydroxyl value for adhesives 1 to 8. The physical property values ​​shown in Table 1 are catalog values. The Mn value of adhesive 7 was not found in the catalog, so it is not shown in Table 1.

[0092] [Table 1]

[0093] Example 1 An aluminum layer was formed by vapor deposition on one side of a sheet of PETG (a condensation polymer of ethylene glycol, 1,4-cyclohexanedimethanol, and terephthalic acid, transparent, thickness 19 μm), a transparent thermoplastic resin. The thickness of the aluminum layer was 50 nm.

[0094] Next, polyisocyanate (xylylene diisocyanate composition, concentration 75%, isocyanate amount (NCO%) 14%) was mixed into adhesive 1, and this was applied to the surface of the aluminum layer on PETG with a bar coater so that the thickness after drying would be 7 μm to form a first adhesive layer. In this way, a laminated sheet having PETG, an aluminum layer and a first adhesive layer was produced. The thickness of the first adhesive layer was 7 μm. The "degree of cross-linking of hydroxyl value equivalent" in the first adhesive layer was 1, and the cure index of the first adhesive layer was 42.

[0095] Next, the surface of the first adhesive layer was pressed against the corona-treated surface of a transparent acrylic resin sheet (thickness 75 μm, total light transmittance 93%, breaking strength 53 MPa) to bond the acrylic resin sheet that would become the surface resin layer to the laminate sheet. The "corona-treated surface" refers to one side of the transparent acrylic resin sheet that has been subjected to a corona discharge treatment to enhance adhesion with the first adhesive layer.

[0096] In this way, a laminate 1 was produced in which a thermoplastic resin layer, an aluminum layer, a first adhesive layer, and a surface resin layer were laminated in this order. When viewed from the surface resin layer side, the laminate 1 exhibits a metallic appearance with a metallic luster due to the aluminum layer.

[0097] [Examples 2 to 4] Laminates 2 to 4 were produced in the same manner as laminate 1, except that adhesives 2 to 4 were used instead of adhesive 1. The thickness of the first adhesive layer in laminates 2 to 4 was all 7 μm.

[0098] [Examples 5 and 6] Laminates 5 and 6 were produced in the same manner as Laminate 1, except that the amount of polyisocyanate added to Adhesive 1 was 0.75 and 0.5 times, respectively, and the "degree of crosslinking per hydroxyl value equivalent" in the first adhesive layer was 0.75 and 0.5, respectively. The cure index of the first adhesive layer in Laminate 5 was 31.5, and the cure index of the first adhesive layer in Laminate 6 was 21.0.

[0099] [Examples 7 and 8] Laminates 7 and 8 were produced in the same manner as Laminate 2, except that the amount of polyisocyanate added to Adhesive 2 was 0.75 and 0.5 times, respectively, and the "degree of crosslinking per hydroxyl value equivalent" in the first adhesive layer was 0.75 and 0.5, respectively. The cure index of the first adhesive layer in Laminate 7 was 25.5, and the cure index of the first adhesive layer in Laminate 8 was 17.0.

[0100] [Examples 9 and 10] Laminates 9 and 10 were produced in the same manner as Laminate 4, except that the amount of polyisocyanate added to Adhesive 4 was 0.75 and 0.5 times, respectively, and the "degree of crosslinking per hydroxyl value equivalent" in the first adhesive layer was 0.75 and 0.5, respectively. The cure index of the first adhesive layer in Laminate 9 was 26.3, and the cure index of the first adhesive layer in Laminate 10 was 17.5.

[0101] [Comparative Examples 1 to 4] Laminate C1 was produced in the same manner as laminate 1, except that adhesive 5 was used instead of adhesive 1. Moreover, laminates C2 to C4 were produced in the same manner as laminate 1, except that adhesives 6 to 8 were used instead of adhesive 1 without being mixed with polyisocyanate. The thickness of the first adhesive layer in each of laminates C1 to C4 was 7 μm.

[0102] [Evaluation of alkali resistance] For each of the laminates 1 to 10 and C1 to C4, the laminate was cut to a size of 10 mm x 10 mm to prepare a test piece. The prepared test piece was then immersed in a 0.1N aqueous sodium hydroxide solution at room temperature (25°C) for 8 hours. The test piece was then removed from the aqueous sodium hydroxide solution, and the dissolution state of the aluminum layer was visually confirmed, and the dissolution distance was measured. The "dissolution distance" is the distance from the edge of the test piece into which the aqueous sodium hydroxide solution penetrated when immersed in the aqueous sodium hydroxide solution to the tip of the part where the aluminum layer has dissolved. In this example, the dissolution distance is the distance from the edge of the laminate into which the aqueous sodium hydroxide solution penetrated to the tip (deepest part) of the part where the aluminum layer has dissolved to the innermost part.

[0103] [Weather resistance] Each of the laminates 1 to 10 and C1 to C4 was subjected to an accelerated exposure test specified in the Japanese Industrial Standards (JIS) A1415-2013 for 3000 hours. Then, the appearance of the laminates after the test was visually observed from the surface resin layer side by a number of skilled technicians to confirm any change in appearance due to the test. As a result, the appearance of each of the laminates 1 to 10 and C1 to C4 after standing did not substantially change due to the test, and it was confirmed that they have sufficient weather resistance for use in the exterior of automobiles and the like.

[0104] [Heat resistance] For each of the laminates 1 to 10 and C1 to C4, a white-painted plate was attached to the surface of the PETG sheet opposite to the aluminum layer, and the laminate was left at 80°C for 168 hours, and the appearance of the laminate was visually observed from the surface resin layer side. As a result, no whitening, cracks, or wrinkles were observed in any of the laminates 1 to 10 and C1 to C4 after leaving the laminates. Thus, it was confirmed that the appearance of the laminates 1 to 10 and C1 to C4 did not change substantially before and after the leaving, and that the laminates have sufficient heat resistance for use in the exterior of automobiles and the like.

[0105] [Strength] The tensile modulus of Laminates 1-10 and C1-C4 is measured according to the test method specified in JIS K7127:1999 (ISO 527-3:1995). The design thickness of each laminate is 101 μm, with the thermoplastic resin (PETG) layer being 19 μm, the first adhesive layer being 7 μm, and the surface resin (acrylic resin) layer being 75 μm. The tensile modulus of each laminate is about 1700 MPa, and it is confirmed that each of the laminates has sufficient strength for use in the exterior of automobiles and the like.

[0106] Table 2 shows the composition of each laminate, the resin type and cure index of the adhesive layer, and the dissolution distance in the laminate.

[0107] [Table 2]

[0108] As shown in Table 2, the dissolution of the aluminum layer in each of the laminates 1 to 3 was so slight that it was difficult to confirm with the naked eye. Moreover, the dissolution of the aluminum layer in the laminate 4 was visible but only slightly.

[0109] These results show that sandwiching the aluminum layer between a polyester adhesive and a PETG sheet improves the alkali resistance of the laminate, and as a result, the dissolution distance in the above-mentioned alkali resistance evaluation test can be suppressed to less than 0.8 mm.

[0110] On the other hand, the dissolution of the aluminum layer in each of the laminates C1 to C3 was easily visible to the naked eye. In the case of the laminate C1, this is thought to be because the resin of the first adhesive layer is polyester, which has a low hardening index. In the case of the laminates C2 and C3, this is thought to be because the resin of the first adhesive layer is polyurethane, which has a low hardening index and a low adhesive strength of the adhesive layer.

[0111] The dissolution of the aluminum layer in the laminate C4 was more remarkable than in the other laminates, which is believed to be because the adhesive had a sufficiently large cure index but the adhesion of the first adhesive layer was weak.

[0112] As is clear from the above results, if the adhesive material is polyester and the hardening index of the adhesive is 30 or more, the dissolution distance of the aluminum layer when immersed in an alkaline aqueous solution can be suppressed to less than 0.8 mm, regardless of the acid value and hydroxyl value of the adhesive. The test conditions in the above evaluation of alkali resistance correspond to the alkaline erosion caused by car washing.

[0113] Therefore, in the case of an automobile exterior application, providing a 0.7 mm wide edge on the laminate can practically suppress the occurrence of dissolution of the aluminum layer by alkali. As a result, it is possible to prevent the metallic appearance of the aluminum layer from being damaged by alkali erosion. The width of the edge can be set according to the evaluation results of the dissolution test, and can be made smaller than 0.7 mm, for example, as long as it does not fall below the above-mentioned dissolution distance.

[0114] On the other hand, it is found that the adhesive strength of the first adhesive layer of the laminate is low when the adhesive is an acrylic resin-based adhesive even if the hardening index is greater than 30, or when the adhesive is a polyurethane-based adhesive with a small hardening index. For this reason, in the above cases, the alkaline solution penetrates into the interface between the aluminum layer and the first adhesive layer and dissolves the aluminum layer, so the effect of suppressing aluminum erosion by alkali is also low.

[0115] Example 11 Adhesive 1 was applied to the surface of laminate 1 opposite to the surface resin layer (the surface of the PETG sheet opposite to the aluminum layer) so that the thickness after drying would be 10 μm. In this way, a second adhesive layer was formed. Then, an ABS sheet (appearance: black, thickness: 200 μm) that would become a base layer was pressed onto the second adhesive layer, and laminate 1 and the ABS sheet were bonded together via the second adhesive layer. In this way, laminate 11 was produced in which the surface resin layer, first adhesive layer, aluminum layer, thermoplastic resin layer, second adhesive layer, and base layer were stacked in this order.

[0116] The laminate 11 was placed in a pair of mold assemblies including one mold having a convex portion with a trapezoidal cross-sectional shape and the other mold having a corresponding concave portion, and heated and vacuum molded to mold the laminate 11 into a shape having a trapezoidal cross-sectional shape and edges as shown in Fig. 3. Next, the tip of the edge was cut off so that the edge width Lb was a desired width (e.g., 0.7 mm) greater than 0.1 mm and less than 0.8 mm. In this way, a molded product with a metallic appearance was produced.

[0117] As described above, the molded body has an edge that is very narrow but is wider than the dissolution distance of the laminate 1. Therefore, the appearance of the molded body is hardly affected by the edge, and the aluminum layer in the part inside the edge does not undergo alkaline corrosion. Therefore, even if the molded body is used for the exterior of an automobile, the appearance is prevented from being impaired by the alkaline corrosion during use.

[0118] Furthermore, in this molded product, both the first adhesive layer and the second adhesive layer are formed by applying the adhesive 1. In this way, since the adhesives constituting both adhesive layers have the same composition, it is possible to prevent loss of material that occurs during the coating process (such as resin pooling in the coater or adhesive remaining in the resin pan). [Industrial Applicability]

[0119] The present invention is a molded article having a metallic appearance due to an aluminum layer, and can be used for both interior and exterior applications, and is excellent in alkali resistance and decorativeness, with a small margin for preventing alkali corrosion despite having an aluminum layer. In particular, the present invention is suitable for decorative articles for the exterior of moving objects such as automobiles. [Explanation of symbols]

[0120] 1 Thermoplastic resin layer 2 Aluminum layers 3 First adhesive layer (adhesive layer) 4 Surface resin layer 5 Second adhesive layer (further adhesive layer) 6 Base material layer 10, 20 laminate 100 Molded body 101 Convex 102 Edge

Claims

1. a thermoplastic resin layer, an aluminum layer, and an adhesive layer are laminated in this order; The adhesive layer is made of a polyester adhesive, The adhesive layer has a cure index of 15 or more, as calculated by the following formula: (formula) Cure index = acid value x hydroxyl value x hydroxyl value equivalent crosslinking degree (In the above formula, "acid value" is the acid value (mg KOH / g) of the polyester-based adhesive, "hydroxyl value" is the hydroxyl value (mg KOH / g) of the polyester-based adhesive, and "degree of cross-linking by hydroxyl value equivalent" is the proportion of hydroxyl groups of the polyester of the polyester-based adhesive that are used for cross-linking in the adhesive layer.)

2. The metallic laminate according to claim 1 , wherein the adhesive layer has a cure index of 30 or more.

3. 3. The metallic laminate according to claim 1, wherein the thermoplastic resin layer is made of a polyester having a benzene ring and a cyclohexane ring in its main chain.

4. A metallic molded product obtained by molding the metallic laminate according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Metal gloss sheet for three-dimensional molding

    JP2002370311A

  • Metal-like decorative sheet, its manufacturing process and metal-like decorative sheet intermediate material

    JP2004001243A

  • Metal tone film

    JP2009262501A

  • Film with metallic tone

    JP2010167648A

  • Decorative sheet and decorative resin molded article

    JP2015164794A