METHOD FOR EVALUATING METAL SURFACE ROUGHNESS, METHOD FOR ROUGHNING METAL SURFACE, AND METHOD FOR REMOVING COATING
The method evaluates and maintains fine irregularities on laser-roughened steel surfaces and controlled coating removal to enhance coating durability on structures.
Patent Information
- Application Number
- JP2021057140
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-03-30
AI Technical Summary
Conventional methods for evaluating the surface roughness of laser-roughened steel surfaces and post-coating film removal surfaces fail to detect fine irregularities of several micrometers, affecting the durability of coatings on structures like bridges and buildings.
A method for evaluating surface roughness using a developed area ratio (Sdr) of 0.15 or more, combined with specific laser conditions to form and maintain fine irregularities, and a method for removing coatings while preserving these irregularities using controlled laser scanning.
Ensures the durability of coatings by detecting and maintaining fine irregularities, enhancing adhesion and longevity of coatings on steel structures.
Smart Images

Figure 0007588539000001 
Figure 0007588539000002 
Figure 0007588539000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a metal surface roughness evaluation method used to evaluate the surface roughness of a metal having a base-prepared surface that has been roughened by irradiating it with laser light. The present disclosure also relates to a metal surface roughening method used to prepare the surface of a metal to obtain a prepared surface of the metal that is evaluated as good by the above-mentioned metal surface roughness evaluation method, and a coating removal method used to remove a coating applied to a prepared surface of a steel material, which is the metal of an existing structure such as a bridge or building, that is evaluated as good by the above-mentioned metal surface roughness evaluation method. [Background technology]
[0002] In order to use the above-mentioned existing structures, such as bridges and buildings, safely for a long period of time, it is necessary to prevent corrosion of the steel material, which is a structural member, by applying a coating to the surface of the steel material. When applying a coating to the steel material surface, a roughening treatment is carried out by irradiating a laser beam onto the base preparation surface, which is the steel material surface before painting, in order to increase the adhesion of the paint and improve the durability of the paint.
[0003] In order to prevent corrosion of steel, which is a structural member, over the long term, it is necessary to periodically peel off and remove the coating applied to the surface of the steel and repaint it.When peeling off the coating from the steel surface, it is required to leave as much of the base surface as possible that has been roughened by irradiation with laser light before painting in order to increase the adhesion of the paint when repainting.
[0004] Furthermore, when performing a roughening treatment in which laser light is irradiated onto the surface of steel before painting as described above, it is necessary to evaluate the surface roughness of the base-conditioned surface obtained after the treatment. On the other hand, when the coating film on the steel surface is peeled off before repainting, it is also necessary to evaluate the surface roughness of the base-conditioned surface of the steel exposed after the coating film is removed.
[0005] Conventionally, the methods for evaluating the surface roughness of a base-conditioned surface obtained after roughening treatment by laser light irradiation and the methods for evaluating the surface roughness of a base-conditioned surface of a steel material exposed after removal of a coating have been based on the maximum height Rz, which is a parameter of line roughness (JIS B 0601), and evaluation is performed based on a standard range of 25 to 80 μm for the line roughness maximum height Rz. Incidentally, Non-Patent Document 1 describes the use of maximum height Rz as an evaluation item for surface roughness. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] "Mechanical Engineering Handbook", New Edition, 3rd Printing, Edited by the Japan Society of Mechanical Engineers, September 30, 1989, Pages B2-206 to B2-207 Summary of the Invention [Problem to be solved by the invention]
[0007] However, as described above, when a roughening treatment is performed by irradiating a laser beam onto a steel surface before painting, or when a coating is peeled off by irradiating a laser beam, even if the steel surface or the exposed, pre-painted, base-conditioning surface meets the standard of 25 to 80 μm in maximum line roughness height Rz, conventional surface roughness evaluation methods measure irregularities with a maximum line roughness height Rz of about 10 μm in width, and therefore cannot measure the presence or absence of fine irregularities with a width of about a few μm.
[0008] The durability of a paint differs depending on whether or not these fine irregularities, each a few microns in width, are present on the steel surface or on the exposed, pre-painted surface. Therefore, in order to improve the durability of paint, it is desirable to develop a method for evaluating surface roughness that can detect the presence or absence of fine irregularities, each a few microns in width. Solving this problem has been a traditional challenge.
[0009] The present disclosure has been made to solve the above-mentioned problems of the conventional art, and aims to provide a method for evaluating the surface roughness of metals that can grasp not only the presence of irregularities on the steel surface having a width of about tens of μm, but also the presence or absence of fine irregularities on the steel surface having a width of about several μm, for example, when a roughening treatment is performed by irradiating a laser light onto the surface of a steel material before painting, thereby making it possible to guarantee the durability of the paint.
[0010] In addition, the present disclosure aims to provide a method for roughening a metal surface that can improve the durability of the paint, and a coating removal method that can remove a coating of paint applied to the surface of a structural component in an existing structure while minimizing changes to the shape and composition of the base preparation surface of the structural component. [Means for solving the problem]
[0011] A first aspect of the present disclosure is a method for evaluating the surface roughness of a metal having a roughened surface by irradiating laser light, wherein when a maximum height Rz, which is a parameter of line roughness (JIS B 0601) on the roughness-conditioned surface of the metal, is 25 to 80 μm, evaluation is performed based on a standard of a range in which at least a developed area ratio Sdr, which is a parameter of surface roughness (International Standard ISO 25178) on the roughness-conditioned surface, is 0.15 or more.
[0012] A second aspect of the present disclosure is a method for roughening a metal surface, which performs surface preparation of a metal to obtain a surface-prepared metal surface that satisfies the evaluation criteria in the method for evaluating surface roughness of a metal as set forth in claim 1, and is configured to irradiate the surface of the metal with laser light under laser conditions set to form irregularities on the surface of the metal such that at least the developed area ratio Sdr of parameters of surface roughness including sputter (international standard ISO 25178) is 0.15 or more.
[0013] Furthermore, a third aspect of the present disclosure is configured to use a pulsed laser beam as the laser beam.
[0014] Furthermore, in a fourth aspect of the present disclosure, the laser conditions are configured such that the pulse energy, calculated by dividing the average output of the laser light by the repetition rate, is at least 0.7 mJ, and the peak output of the laser light is at least 7.0 kW.
[0015] Furthermore, a fifth aspect of the present disclosure is configured such that, under the above laser conditions, the pulse energy is at least 0.7 mJ, and the pulse width (time width of the pulse) of the laser light is 100.0 ns or less to achieve a peak output of the laser light of at least 7.0 kW.
[0016] Furthermore, a sixth aspect of the present disclosure is a coating removal method for removing a coating applied to a base-prepared surface of a metal of an existing structure that is determined to satisfy the evaluation criteria in the metal surface roughness evaluation method described in claim 1, wherein the coating is scanned while being irradiated with a laser beam under laser conditions set to leave irregularities on the base-prepared surface of the metal that have at least an developed area ratio Sdr of 0.15 or more among the parameters of surface roughness (International Standard ISO 25178).
[0017] Furthermore, a seventh aspect of the present disclosure is configured such that the coating film is linearly scanned while being irradiated with laser light.
[0018] Furthermore, in an eighth aspect of the present disclosure, the laser conditions are that the output of the laser beam is 1000 W or less, and the fluence, which is the amount obtained by dividing the output of the laser beam by the product of the spot diameter of the laser beam and the scanning speed of the laser beam, is 0.25 J / mm 2 The configuration is as follows.
[0019] Furthermore, the ninth aspect of the present disclosure is a method for reducing the fluence to 0.25 J / mm 2 In order to achieve the above, the scanning speed of the laser light is set to 9.0 to 15.0 m / s.
[0020] In the present disclosure, a fiber laser, a semiconductor laser, or a YAG laser is generally used as the laser, but is not limited to these lasers. Effect of the Invention
[0021] According to the metal surface roughness evaluation method disclosed herein, for example, when a roughening treatment is performed by irradiating a laser light onto a steel surface before painting, it is possible to grasp not only the presence of irregularities on the steel surface having a width of about several tens of μm, but also the presence or absence of fine irregularities having a width of about several μm, resulting in the extremely advantageous effect of making it possible to guarantee the durability of the paint. [Brief description of the drawings]
[0022] [Figure 1] 1A to 1C are overall views of multiple base-prepared surfaces that are the subject of evaluation by a metal surface roughness evaluation method according to an embodiment of the present disclosure, and laser microscope analysis views shown in conjunction with the overall views. [Diagram 2] 2 is a distribution diagram showing the distribution of developed area ratios for comparing surface roughness for the first-stage base-conditioned surface and the fourth-stage base-conditioned surface in FIG. 1, together with the distributions of four other parameters. [Diagram 3] FIG. 1 is a schematic explanatory diagram showing a roughening device used in a method for roughening a metal surface according to an embodiment of the present disclosure. [Figure 4] 4 is a graph showing the change over time in the pulse laser output irradiated from the laser head of the metal surface roughening device in FIG. 3. [Diagram 5] 1 is a schematic explanatory diagram showing a coating removal device used in a coating removal method according to an embodiment of the present disclosure. FIG. [Figure 6] 6 is an enlarged perspective view illustrating a coating film being removed by the laser coating film removal device of FIG. 5. [Figure 7] 6 is a conceptual diagram of a scanning area of a laser beam for explaining a fluence, which is a laser condition, in the laser coating removal device of FIG. 5. FIG. [Figure 8] 1 is a graph showing the relationship between the output of laser light corresponding to various fluences and the scanning area of the laser light. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings. FIG. 1 shows an overall view of each of several base-prepared surfaces that have been roughened by irradiating them with laser light, and FIG. 1 also shows an analysis view taken with a laser microscope that corresponds to each overall view of the base-prepared surfaces.
[0024] In Figure 1, the first row is a general view and its analysis of the surface after base preparation when laser light with a laser output of 300 W is scanned once, and the second row is a general view and its analysis of the surface after base preparation when laser light with a laser output of 300 W is scanned five times.
[0025] On the other hand, the third row in Figure 1 is an overall view and its analysis diagram of the surface after the base preparation when laser light with a laser output of 500 W is scanned once, and the fourth row is an overall view and its analysis diagram of the surface after the base preparation when laser light with a laser output of 500 W is scanned five times. The fifth row in FIG. 1 shows an overall view of the surface after blasting and surface preparation, and an analysis thereof.
[0026] From the overall views and analysis views of the surface after base preparation in the first to fourth rows of FIG. 1, it can be seen that the more times the laser light is scanned, the more fine irregularities disappear.
[0027] In this embodiment, the surface roughness of each of the conditioned surfaces in the first row and the fourth row in FIG. 1 was evaluated by the metal surface roughness evaluation method according to the present disclosure.
[0028] Specifically, when the maximum height Rz, which is a parameter of line roughness (JIS B 0601) on a metal surface that has been subjected to surface preparation, is in the range of 25 to 80 μm, the interface developed area ratio Sdr, which is a parameter of surface roughness (international standard ISO 25178), was measured for each of the first and fourth conditioned surfaces in Figure 1, as shown in Figure 2, and the distributions of each were compared. In Figure 2, Spc is the arithmetic mean curvature of the peaks of the unevenness, Sdq is the root mean square slope of the conditioned surface, Spd is the peak density, and Sz is the maximum height, and the distributions of these four parameters are shown together with the distribution of Sdr.
[0029] The developed area ratio Sdr of the interface is distributed in a broadening manner from 0.10 to 0.30 on the surface after the base preparation when a laser beam with a laser output of 300 W is scanned once, whereas the distribution is concentrated in the range of 0.00 to 0.15 on the surface after the base preparation when a laser beam with a laser output of 500 W is scanned five times.
[0030] As a result of comparing the distribution of the parameter Sdr value in the surface roughness (international standard ISO 25178) in Figure 2, it was evaluated that the surface roughness of the surface after the base preparation was performed by scanning once with a laser beam of a laser output of 300 W was larger (having a larger flatness roughness) than the surface after the base preparation was performed by scanning five times with a laser beam of a laser output of 500 W. As a result, the surface after the base preparation was performed by scanning once with a laser beam of a laser output of 300 W was evaluated as having a larger flatness roughness than the surface after the base preparation was performed five times with a laser beam of a laser output of 500 W. The larger the surface area, the stronger the paint will adhere to it. The durability of the coating was found to be excellent.
[0031] FIG. 3 shows a roughening device used in the method for roughening a metal surface according to one embodiment of the present disclosure. As shown diagrammatically in FIG. 3, this roughening device 1 is for performing base preparation of the surface Wa of a steel material (metal) W constituting, for example, a bridge, and is equipped with a laser oscillator 2, a laser head 4 that collects laser light L supplied from the laser oscillator 2 via an optical fiber 5 using an incorporated optical system 3 and irradiates the surface Wa of the steel material W, a head driving mechanism 6 that moves the laser head 4 along the long side direction of the steel material W, a scanning mechanism 8 that reflects the laser light L irradiated from the laser head 4 and moves it back and forth on the surface Wa of the steel material W, and a control unit 10 that controls the output of the laser light L irradiated from the laser head 4, etc., based on the laser conditions described below. In this embodiment, a pulsed laser oscillator is used as the laser oscillator 2, which is capable of performing a roughening process with high processing accuracy and little thermal influence.
[0032] The head drive mechanism 6 includes a rail 6a arranged along the long side direction of the steel material W, and a slider 6b that reciprocates on the rail 6a. In this case, the laser head 4 is fixed to the slider 6b so that the laser light irradiation direction is aligned in a direction parallel to the surface Wa of the steel material W and perpendicular to the rail 6a.
[0033] In addition, the scanning mechanism 8 is held in a case 9 attached to the slider 6b of the head driving mechanism 6 via a support base 7, and is composed of a scanner mirror 8a that reflects the laser light L from the laser head 4, and a scanner motor 8b that rotates this scanner mirror 8a in small increments within a predetermined range.
[0034] In other words, in this roughening device 1, by operating both the head driving mechanism 6 and the scanning mechanism 8, the laser light L is moved to cover the entire surface Wa of the steel material W, thereby forming minute irregularities with a height difference of the order of several μm, including the resulting sputter, on the surface Wa of the steel material W.
[0035] More specifically, the scanner mirror 8a of the scanning mechanism 8, which reflects the laser light L, is rotated in small increments to move the laser spot S on the surface Wa of the steel material W along the short side direction of the steel material W by a predetermined amount for each pulse (1 / 4 of the diameter of the laser spot S in this embodiment), as shown in the enlarged oval in Figure 1.
[0036] On the other hand, the head driving mechanism 6 is operated each time the movement of the laser spot S along the short side direction of the steel material W is completed, and moves the laser spot S a predetermined amount (1 / 4 of the diameter of the laser spot S in this embodiment) along the long side direction of the steel material W.
[0037] The amount of movement of the laser spot S per pulse by the head driving mechanism 6 and the scanning mechanism 8 is not limited to 1 / 4 of the diameter of the laser spot S described above, but in order to avoid gaps between adjacent laser spots S, it is desirable to move the laser spot S within the range of 1 / 4 to 3 / 4 of the diameter of the laser spot S.
[0038] In this case, the control unit 10 controls the laser head 4, the head driving mechanism 6 and the scanning mechanism 8 under laser conditions set to form irregularities on the surface Wa of the steel material W, including sputter, such that at least the developed area ratio Sdr of the parameters of surface roughness (international standard ISO 25178) is 0.15 or more. In other words, the laser head 4, head drive mechanism 6 and scanning mechanism 8 are controlled under laser conditions set to obtain a metal base-conditioned surface that satisfies the evaluation criteria in the above-mentioned metal surface roughness evaluation method.
[0039] Here, Fig. 4 shows the change over time in the pulse laser output irradiated from the laser head 4 of the roughening device 1. In Fig. 4, the symbols Pa and Pp respectively indicate the average output and the peak output, and the symbols In and w respectively indicate the pulse interval and the pulse width (time width of the pulse) of the laser light L. Also in Fig. 4, the symbol PE indicates the pulse energy.
[0040] In determining the above laser conditions, first, the spot diameter is set to about 60 μm, and then the pulse energy PE obtained by dividing the average output power Pa of the laser light L by the repetition frequency represented by the reciprocal of the pulse interval In is set to at least 0.7 mJ, and the peak output power Pp of the laser light L is set to at least 7.0 kW. It is preferable to set the average output power Pa of the laser light L to at least 1.5 mJ and the peak output power Pp of the laser light L to at least 15.0 kW, and it is preferable to set the average output power Pa of the laser light L to at least 3.0 mJ and the peak output power Pp of the laser light L to at least 30.0 kW.
[0041] In order to set the pulse energy PE to at least 0.7 mJ as described above and the peak output power Pp of the laser light L to at least 7.0 kW, the pulse width w of the laser light L is set to 100.0 ns or less.
[0042] In this manner, in the present embodiment, the control unit 10 controls the laser head 4, the head driving mechanism 6, and the scanning mechanism 8 so that the pulse energy PE, which is obtained by dividing the average output power Pa of the laser light L by the pulse repetition frequency, is at least 0.7 mJ, and the peak output power Pp of the laser light L is at least 7.0 kW, so that the pulse width w of the laser light L is 100.0 ns or less.
[0043] In the method for roughening a metal surface according to this embodiment, minute irregularities with height differences on the order of several μm, including sputters, can be formed on the surface Wa of the steel material (metal) W before painting, thereby making it possible to improve the durability of the paint.
[0044] FIG. 5 shows a laser coating removal device used in a coating removal method according to an embodiment of the present disclosure. As shown diagrammatically in FIG. 5, this laser coating removal device 11 is for peeling off and removing a coating Wm applied to the surface of a steel material (structural member) W that constitutes, for example, a bridge, and is equipped with a laser oscillator 12, a laser head 14 that collects the laser light L supplied from the laser oscillator 12 using an internal optical system 13 and irradiates the surface of the steel material W, an optical fiber 15 that guides the laser light L from the laser oscillator 12 to the laser head 14, a scanning mechanism 16 that scans the laser light L from the laser head 14 over the surface of the steel material W, and a control unit 20 that controls the output of the laser light L irradiated from the laser head 14, the spot diameter of the laser light L, and the scanning speed of the laser light L by the scanning mechanism 16, etc.
[0045] The scanning mechanism 16 is held in a case 19 together with the laser head 14, and is composed of a scanner mirror 16a that reflects the laser light L from the laser head 14, and a scanner motor 16b that rotates the scanner mirror 16a within a predetermined range.
[0046] In this embodiment, the laser light L from the laser head 14 is reflected toward the steel material W by the scanner mirror 16a, and by rotating this scanner mirror 16a within a predetermined range, as shown in Figure 6, the laser light L is caused to scan in a straight line (move back and forth in a zigzag manner) on the surface of the steel material W to remove the coating film Wm.
[0047] In this case, the control unit 20 controls the laser head 14 and the scanner motor 16b of the scanning mechanism 16 under laser conditions set so that even when the laser light L is irradiated onto the surface Wa of the steel material W that has been subjected to the surface preparation, the unevenness present on the surface Wa of the steel material W, i.e., the unevenness having at least the developed area ratio Sdr of 0.15 or more among the parameters of the surface roughness (international standard ISO 25178) present on the surface Wa of the steel material W, remains. In other words, the laser head 14 and the scanner motor 16b of the scanning mechanism 16 are controlled under laser conditions set to obtain a base-prepared surface Wa of the steel material W of an existing structure that is deemed to satisfy the evaluation criteria in the above-mentioned metal surface roughness evaluation method.
[0048] When determining the above laser conditions, first, if the output of the laser light L is set too high, the minute irregularities on the surface Wa that has been subjected to the preparation will disappear regardless of other conditions, so the upper limit of the output of the laser light L is set to 1000 W.
[0049] The energy density (W / mm ) is calculated by dividing the output of the laser light L by the area SA of the spot S of the laser light L shown in FIG. 2 ) The smaller the spot diameter D, the greater the heat input per unit time, so in order to ensure reliable removal of the coating, the spot diameter D is set to 0.15 mm and the energy density is set to a large value.
[0050] In addition, the product of the spot diameter D of the laser light L and the scanning speed V (m / s) of the laser light L shown in FIG. 7 (scanning area A (m 2 The fluence, which is the output of the laser light L divided by the power of the laser beam L, is 0.25 J / mm 2 It is preferable that the value is less than 0.15 J / mm 2 less than 0.13 J / mm 2 The following applies.
[0051] Here, the relationship between the output of the laser light L corresponding to various fluences and the scanning area A of the laser light L is shown in Fig. 8. As can be seen from the graph in Fig. 8, in the relationship between the output of the laser light L and the scanning area A of the laser light L, the fluence is represented as each slope of the reference lines I to III, and in this embodiment, the fluence is 0.13 J / mm 2 Using a reference line I of the slope as an index, the energy density and the scanning speed V of the laser light L are set so that the output of the laser light L and the scanning area A of the laser light L are located on or near this reference line I, respectively.
[0052] This reduces the fluence to 0.25 J / mm 2 In order to achieve the above, the scanning speed V of the laser light L is set to be desirably 9.0 m / s or more, more desirably 12.0 m / s or more, and even more desirably 15.0 m / s or more.
[0053] In this manner, in this embodiment, the control unit 20 sets the upper limit of the output of the laser light L to 1000 W, the spot diameter D to 0.15 mm, and the fluence to 0.25 J / mm 2 In order to achieve the above, the scanner motor 16b of the scanning mechanism 16 is controlled so that the scanning speed of the laser light is 9.0 to 15.0 m / s.
[0054] According to the coating removal method of this embodiment, it goes without saying that it is possible to remove the coating film Wm of the paint applied to the base-prepared surface Wa of the steel material W in an existing structure, and even in cases where the base-prepared surface Wa of the steel material W is irradiated with laser light L, it is possible to minimize changes in shape and composition caused to the base-prepared surface Wa.
[0055] The configurations of the metal surface roughness evaluation method, metal surface roughening method, and coating removal method according to the present disclosure are not limited to the above-described embodiments, and may be modified in various ways without departing from the spirit of the disclosure. [Explanation of symbols]
[0056] In Pulse Interval L Laser light PE Pulse Energy Pa average power Pp Peak power W Steel (metal, structural member) Wa Steel surface (metal surface, surface with base preparation) Wm paint film w Pulse duration
Claims
1. A method for evaluating the surface roughness of a metal having a surface that has been roughened by irradiating a laser beam, comprising the steps of: A method for evaluating the surface roughness of a metal, comprising: when a maximum height Rz, which is a parameter of line roughness (JIS B 0601) on the base-prepared surface of the metal, is 25 to 80 μm, evaluating the surface roughness based on a standard of a range in which at least a developed area ratio Sdr, which is a parameter of surface roughness (International Standard ISO 25178) on the base-prepared surface, is 0.15 or more.
2. A method for roughening a metal surface, comprising the steps of: preparing a surface of a metal to obtain a surface of the metal that satisfies the evaluation criteria in the method for evaluating the surface roughness of a metal according to claim 1; A method for roughening a metal surface, comprising irradiating the surface of the metal with laser light under laser conditions set to form irregularities on the surface of the metal such that at least the developed area ratio Sdr, among parameters of surface roughness including sputter (International Standard ISO 25178), is 0.15 or more.
3. 3. The method for roughening a metal surface according to claim 2, wherein the laser beam is a pulsed laser beam.
4. 4. The method for roughening a metal surface according to claim 3, wherein the laser conditions include a pulse energy, calculated by dividing the average output of the laser beam by the repetition rate, of at least 0.7 mJ, and a peak output of the laser beam of at least 7.0 kW.
5. 5. The method for roughening a metal surface according to claim 4, wherein the laser conditions include a pulse energy of at least 0.7 mJ and a pulse width of the laser beam of 100.0 ns or less to achieve a peak output of the laser beam of at least 7.0 kW.
6. A coating film removal method for removing a coating film applied to a surface of a metal of an existing structure that has been subjected to a base preparation process and that satisfies the evaluation criteria in the metal surface roughness evaluation method according to claim 1, comprising the steps of: a coating removal method comprising scanning the coating while irradiating it with a laser beam under laser conditions set to leave unevenness on the prepared surface of the metal such that at least the developed area ratio Sdr, among parameters of surface roughness (international standard ISO 25178), is 0.15 or more.
7. The coating film removing method according to claim 6, wherein the coating film is linearly scanned while being irradiated with the laser light.
8. The laser conditions are that the output of the laser beam is 1000 W or less, and the fluence, which is the amount obtained by dividing the output of the laser beam by the product of the spot diameter of the laser beam and the scanning speed of the laser beam, is 0.25 J / mm 2 The coating film removing method according to claim 6 or 7, wherein:
9. Fluence: 0.25 J / mm 2 The coating film removal method according to claim 8, wherein the scanning speed of the laser light for achieving the above is 9.0 to 15.0 m / s.
Citation Information
Patent Citations
Method of surface treatment using pulse laser beam and device therefor
JP2000263259A
Sheet conveying roll and its manufacturing method
JP2002104686A
Surface treatment device
JP2017124418A
Roughening method of metal surface
JP2018192480A
Electrically conductive copper components and joining processes therefor
US20190036429A1