Cleaning sponge

The cleaning sponge with a flexible polyurethane foam layer and a softer porous body layer addresses the issues of water drainage and shape followability, ensuring effective dirt scraping without damage.

JP7588561B2Active Publication Date: 2024-11-22INOAC CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021117183
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-15
Publication Date
2024-11-22
Estimated Expiration
2037-07-21

AI Technical Summary

Technical Problem

Conventional cleaning sponges with a nonwoven fabric layer for scraping off hard dirt face difficulties in water drainage and shape followability due to the nonwoven fabric being too hard to deform.

Method used

A cleaning sponge with a first layer of flexible polyurethane foam having communicating cells and a second layer of a porous body, where the first layer is compression molded to achieve a hardness of 40-85 Asker F, allowing for both hardness and deformability, and the second layer is softer to enhance water drainage.

Benefits of technology

The sponge improves shape followability and water drainage while effectively scraping off dirt without damaging the object, maintaining an appropriate balance of physical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588561000004
    Figure 0007588561000004
  • Figure 0007588561000005
    Figure 0007588561000005
  • Figure 0007588561000001
    Figure 0007588561000001
Patent Text Reader

Abstract

To provide a cleaning sponge having good shape followability.SOLUTION: A cleaning sponge 10 comprises a first layer 12 which is made of a flexible polyurethane foam having cells communicating with one another and in which Asker F hardness is set to be in the range of 40-85 degrees, and a second layer 14 which is made of a porous material having pores communicating with one another and is set more flexible than the first layer 12. In the first layer 12, the number of the cells existing on a second surface 12b along a lamination direction of the first layer 12 and second layer 14 is set larger than the number of the cells existing on a first surface 12a orthogonal to the lamination direction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cleaning sponge used for cleaning tableware, cooking utensils, etc. [Background technology]

[0002] A cleaning sponge used for cleaning tableware and cooking utensils has been proposed that has a multi-layer structure consisting of a soft polyurethane foam and a nonwoven fabric layer attached to one side of the soft polyurethane foam (see, for example, Patent Document 1). The cleaning sponge uses the soft polyurethane foam with fine cells to create a foam of detergent, and the soft polyurethane foam is used to wash the tableware. The cleaning sponge also uses the nonwoven fabric layer, which is harder than the soft polyurethane foam, to scrape off dirt stuck to cooking utensils such as frying pans and pots. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-99916 A Summary of the Invention [Problem to be solved by the invention]

[0004] In the cleaning sponge described above, if the nonwoven fabric layer is set to be hard enough to scrape off hard dirt such as burnt food adhering to a frying pan or the like, but hard enough not to cause the fibers to fluff, the nonwoven fabric layer will be difficult to deform. For this reason, a cleaning sponge having a nonwoven fabric layer has the drawbacks of being difficult to squeeze out water from and poor conformability to the shape of the object being cleaned, such as a frying pan.

[0005] The present invention has been proposed in view of the above-mentioned problems associated with the conventional technology, and aims to provide a cleaning sponge having a layer that is relatively hard but easy to squeeze and has good shape-following properties. [Means for solving the problem]

[0006] The cleaning sponge of the first embodiment comprises: A first layer made of a flexible polyurethane foam having cells communicating with each other and having an Asker F hardness set in the range of 40 degrees to 85 degrees; A second layer is made of a porous body having pores communicating with each other and is set to be softer than the first layer, The first layer has a greater number of cells on a plane perpendicular to the stacking direction between the first layer and the second layer than on a plane parallel to the stacking direction. According to the first aspect, the first layer made of soft polyurethane foam can be set to be relatively hard, and even if the first layer is made hard, bending deformation of the first layer is allowed, thereby improving the ability to conform to the shape of the object to be cleaned.

[0007] In a second embodiment, the first layer is made of a flexible polyurethane foam having a structure in which the cells are mutually connected after the membrane is removed. According to the second aspect, by forming the first layer from a flexible polyurethane foam having a structure in which the membrane is removed and the cells are interconnected, water can be easily discharged from the first layer, and water drainage can be improved.

[0008] In a third aspect, the first layer has a number of cells present in a plane perpendicular to the stacking direction in a range of 7 cells / 25 mm to 40 cells / 25 mm. According to the third aspect, the scraping layer has relatively large open cells, which improve drainage.

[0009] In a fourth aspect, the first layer has a number of cells on a surface along the stacking direction in a range of 14 cells / 25 mm to 160 cells / 25 mm. According to the fourth aspect, when the scraping layer is pressed against the object to be cleaned, the scraping layer is difficult to compress and has an appropriate hardness, so that dirt can be suitably scraped off.

[0010] In a fifth embodiment, the first layer has a density of 60 kg / m 3 ~120kg / m 3 The gist of the matter is that it is within the range of. According to the fifth aspect, it becomes easy to adjust the physical properties of the first layer, such as hardness, water drainage, and ability to conform to the shape of the object to be cleaned, to an appropriate balance.

[0011] In a sixth aspect, the first layer is a compression-processed molded product of a flexible polyurethane foam, and is arranged so that the compression direction of the compression-processed molded product coincides with the lamination direction. According to the sixth aspect, when the scraping layer is pressed against the object to be cleaned, the scraping layer is difficult to compress and has an appropriate hardness, so that dirt can be suitably scraped off.

[0012] In a seventh aspect, the first layer is a compression-molded product having a thickness that is 1 / 2 to 1 / 4 of the original flexible polyurethane foam. According to the seventh aspect, it becomes easy to adjust the physical properties of the first layer, such as hardness, water drainage, and ability to conform to the shape of the object to be cleaned, to an appropriate balance.

[0013] In an eighth aspect, the porous body constituting the second layer is a non-compressed molded product of a flexible polyurethane foam having a structure in which cells as the pores are interconnected. According to the eighth aspect, appropriate softness that does not damage the object to be cleaned can be obtained. Effect of the Invention

[0014] According to the cleaning sponge of the present invention, even if it has a relatively hard layer, it is possible to improve the ability to conform to the shape of the object to be cleaned. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic perspective view showing a cleaning sponge according to a preferred embodiment of the present invention; [Diagram 2] FIG. 2 is an explanatory diagram showing an apparatus used for testing the abrasion resistance of the scraping layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Next, the cleaning sponge according to the present invention will be described below by way of preferred embodiments with reference to the accompanying drawings. The cleaning sponge according to the present invention can be used for cleaning various objects such as tableware, cooking utensils, washstands, bathrooms, and toilets. EXAMPLES

[0017] As shown in FIG. 1, the cleaning sponge 10 according to the embodiment is formed in a cubic shape composed of rectangular faces. The cleaning sponge 10 is composed of a multi-layer structure consisting of a scraping layer (first layer) 12 made of soft polyurethane foam and a cleaning layer (second layer) 14 that is placed on top of the scraping layer 12 and is set to be softer than the scraping layer 12. The cleaning sponge 10 has one cleaning surface composed of the scraping layer 12 and the other cleaning surface on the opposite side composed of the cleaning layer 14, and can be switched between the scraping layer 12 and the cleaning layer 14 by turning it over. In the cleaning sponge 10 according to the embodiment, the scraping layer 12 is set to be thinner than the cleaning layer 14, and the thickness of the scraping layer 12 is set to be about 5 mm when the total thickness is set to about 3 cm.

[0018] The scraping layer 12 is made of a flexible polyurethane foam having cells that communicate with each other. In particular, among flexible polyurethane foams, those having a structure consisting only of a resin skeleton that forms the cells, with the cell membrane being removed by melting or the like, are preferred. By forming the scraping layer 12 from a flexible polyurethane foam having a structure consisting only of such a resin skeleton, there is an advantage that the scraping layer 12 can be easily drained.

[0019] The scraping layer 12 has an Asker F hardness set in the range of 40 degrees to 85 degrees, and if the scraping layer 12 has a hardness in this range, dirt attached to the object to be cleaned can be suitably scraped off. If the scraping layer 12 has an Asker F hardness of less than 40 degrees, it may not have a hardness that can scrape off dirt attached to the object to be cleaned, and if the Asker F hardness is greater than 85 degrees, it may damage the object to be cleaned due to its hardness. It is preferable that the scraping layer 12 has an Asker F hardness set to 80 degrees or less. Some cleaning sponges made of conventional nylon nonwoven fabric with abrasive grains bonded to them exceed the Asker F hardness scale because the abrasive grains are hard. The cleaning sponge 10 of the present invention has a scraping layer 12 with a hardness set lower than that of the conventional nylon nonwoven fabric described above, so that it is less likely to damage the surface treatment of fluororesin or the like and is suitable for surface-treated cookware.

[0020] The scraping layer 12 is a compression-processed molded product obtained by uniaxially compressing a soft polyurethane foam obtained by a predetermined method such as slab foaming, and is harder than the original soft polyurethane foam due to compression molding. The scraping layer 12 is arranged so that the compression direction of the soft polyurethane foam is the lamination direction (hereinafter simply referred to as the lamination direction) of the scraping layer 12 and the cleaning layer 14 in the cleaning sponge 10. The scraping layer 12 has a larger number of cells per unit length on the second surface 12b along the lamination direction than the number of cells per unit length on the first surface 12a perpendicular to the lamination direction. The scraping layer 12 has the same number of cells on the first surface 12a as the original soft polyurethane foam, while the number of cells on the second surface 12b is greater than the original depending on the degree of compression from the original soft polyurethane foam. Moreover, in the scraping layer 12, the cells are opened larger on the first surface 12a, which constitutes one of the largest cleaning surfaces in the cleaning sponge 10, than on the second surface 12b, and the cells are opened smaller on the second surface 12b, which constitutes a side surface in the cleaning sponge 10, than on the first surface 12a. In this way, the scraping layer 12 made of soft polyurethane foam can be set relatively hard by compression molding, and bending deformation of the scraping layer 12 is permitted even if the scraping layer 12 is made hard, so that the ability of the scraping layer 12 to follow the shape of the object to be cleaned can be improved.

[0021] The scraping layer 12 is preferably set so that the number of cells present on the first surface 12a (based on JIS K6400-1) is in the range of 7 cells / 25 mm to 40 cells / 25 mm. By setting the number of cells on the first surface 12a of the scraping layer 12 in the above range, the cells can be opened relatively widely to improve drainage. In addition, the scraping layer 12 is preferably set so that the number of cells present on the second surface 12b (based on JIS K6400-1) is in the range of 14 cells / 25 mm to 160 cells / 25 mm. By setting the number of cells on the second surface 12b of the scraping layer 12 in the above range, when the first surface 12a, which is the cleaning surface, is pressed against the object to be cleaned, the scraping layer 12 is not easily compressed in the stacking direction and has an appropriate hardness, so that dirt can be suitably scraped off. Note that the number of cells does not only define the cells exposed on the surface of the scraping layer 12.

[0022] The scraping layer 12 is a compression-molded product having a thickness of 1 / 2 to 1 / 4 of the original soft polyurethane foam, and has a density (in accordance with JIS K 7222) of 60 kg / m 3 ~120kg / m 3 In this manner, when the density of the scraping layer 12 is within the above range, it becomes easy to adjust various physical properties such as hardness, water drainage, and ability to conform to the shape of the object to be cleaned to have an appropriate balance.

[0023] The cleaning layer 14 is made of a porous body in which pores are interconnected, and is set to be softer than the scraping layer 12. Here, as the porous body, a non-compressed molded product of soft polyurethane foam in which cells as pores are interconnected is suitable. The cleaning layer 14 made of such a non-compressed molded product of soft polyurethane foam has an appropriate softness that does not damage the object to be cleaned. The cleaning layer 14 has the same number of cells per unit length on the first surface perpendicular to the stacking direction as the number of cells per unit length on the second surface along the stacking direction, and has a lower density than the scraping layer 12. The cleaning layer 14 may have, for example, a cell number (based on JIS K6400-1) in the range of 7 cells / 25 mm to 40 cells / 25 mm and a density (based on JIS K 7222) of 30 kg / m3 ~100kg / m 3 A flexible polyurethane foam having a viscosity in the range of 100:1 or 150:1 can be used.

[0024] The flexible polyurethane foam used in the scraping layer 12 and the cleaning layer 14 may be either an ether type or an ester type, but the ether type is preferred because of its excellent water resistance and resistance to moist heat aging.

[0025] The cleaning sponge 10 can be manufactured, for example, as follows. A soft polyurethane foam obtained by slab foaming or the like is subjected to a membrane removing process to remove the cell membrane, and a plate-shaped body of a predetermined thickness made of a soft polyurethane foam having a structure in which the cells communicate with each other is prepared for each of the scraping layer and the cleaning layer. The scraping layer plate is heated and uniaxially compressed in the thickness direction to form the scraping layer 12 of a compression processed molded product. Here, the scraping layer plate is compressed to 1 / 2 to 1 / 4 of its original thickness to form the scraping layer 12 with a compression ratio of 2 to 4 times. On the other hand, the cleaning layer plate is a non-compressed molded product. The scraping layer 12 and the cleaning layer plate are overlapped so that the compression direction of the scraping layer 12 is the lamination direction, and are pressed together with a roll coater or the like to bond them together with a hot melt adhesive such as a reactive polyurethane system to obtain the cleaning sponge 10.

[0026] The cleaning sponge 10 may have projections and recesses on the cleaning surface of the scraping layer 12 by press processing or the like, and suitable projections and recesses can be easily formed with the pattern and pitch resulting from such processing. Similarly, the cleaning surface of the cleaning layer 14 may have projections and recesses on the cleaning surface by profile processing or the like. The profile processing referred to here refers to a known processing method, for example, the processing method disclosed in JP-A-2006-14819.

[0027] (Evaluation of scraping layer) Scraping layers were prepared under various conditions shown in Table 1, and the Asker F hardness, frictional force, abrasion resistance, and wiping properties were evaluated. The product names of the materials in the table, such as "CFH-13," indicate filter foams having a structure in which cells are connected to each other by a film-removing process in ether-based soft polyurethane foams (manufactured by Inoac Corporation), and the number "13" after the English letters indicates the number of cells. The product names of the materials, such as "EPH-20," indicate ether-based soft polyurethane foams (manufactured by Inoac Corporation) before film-removal of the product name "CFH," and the number "20" after the English letters indicates the number of cells. Comparative Example 1 shown in Table 2 is a scraping layer made of a nonwoven fabric containing an abrasive. Comparative Example 1 is a scraping layer made of a nonwoven fabric containing an abrasive, and is made of two types of nylon fibers, one with a single yarn fineness of 22 decitex and the other with a single yarn fineness of 16 decitex, and has a fiber basis weight of 460 g / m 2 The material used was a nonwoven fabric of a fiber aggregate (random web). In addition, in Comparative Example 1, aluminum hydroxide with an average particle size of 11 μm was used as an abrasive, and the dry solid content was 800 g / m 2 The thickness of the nonwoven fabric is 32 mm.

[0028] The scraping layer made of soft polyurethane foam is obtained by compressing a plate of soft polyurethane foam by hot pressing in the thickness direction at the compression ratio shown in Table 1. Here, the first surface of the scraping layer is a surface that is perpendicular to the lamination direction with the cleaning layer and perpendicular to the compression direction of the soft polyurethane foam. The second surface of the scraping layer is a surface that is parallel to the lamination direction with the cleaning layer and parallel to the compression direction of the soft polyurethane foam. The cell number and density of the material are the standard values ​​of the material manufacturer, and the cell number of the second surface of the scraping layer and the density of the scraping layer can be calculated based on the compression ratio from the standard value of the material.

[0029] The scraping layer made of the soft polyurethane foam is hot-pressed on the first surface, which is the cleaning surface of the cleaning sponge, using a press plate with holes of a predetermined pattern, so that the unevenness is formed with the pattern and pitch derived from the holes. The "round holes" shown in Table 1 are formed by hot-pressing the soft polyurethane foam using a press plate (manufactured by Taiyo Kinko Co., Ltd., No. 30, hole diameter 3.0 mm, pitch 4.0 mm, hole ratio 51.0%) in which the centers of three adjacent round holes (3φ) are arranged to form an equilateral triangle, and forming the unevenness of a predetermined pattern on the first surface of the scraping layer obtained. The "square holes" shown in Table 1 are formed by hot-pressing the soft polyurethane foam using a press plate (manufactured by Taiyo Kinko Co., Ltd., No. 188, hole diameter 3.0 mm, pitch 5.0 mm, hole ratio 45.0%) in which 3 mm square holes are arranged in a checkerboard pattern with a pitch of 5 mm, and forming the unevenness of a predetermined pattern on the first surface of the scraping layer obtained. For the "round hole + cross hole" shown in Table 1, a press plate (manufactured by Taiyo Wire Net Co., Ltd., No. 115, hole ratio 34.2%) with a cross hole at the center of four adjacent round holes (3φ) arranged in a regular square is used to heat press a soft polyurethane foam, forming a predetermined pattern of unevenness on the first surface of the resulting scraping layer. For the "pentagonal hole" shown in Table 1, a press plate with three adjacent pentagonal holes (the size of which is inscribed in an 8 mm circle) arranged so that the centers of the three pentagonal holes form an equilateral triangle is used to heat press a soft polyurethane foam, forming a predetermined pattern of unevenness on the first surface of the resulting scraping layer.

[0030] [Table 1]

[0031] (Hardness of scraping layer) The hardness of the scrape layer alone was measured for the scrape layer obtained by compressing the material to the thickness shown in Table 1. The hardness of the scrape layer alone was also measured for the scrape layer of the comparative example shown in Table 2. The hardness was measured using an Asker Rubber Hardness Tester Type F (manufactured by Kobunshi Keiki Co., Ltd.) to measure the Asker F hardness for each scrape layer shown in Table 1 and Comparative Example 1. The hardness measurement results for each scrape layer are shown in Table 2.

[0032] (Abrasion resistance of scraping layer) The wear resistance of each scraping layer was measured using a Gakushin abrasion tester (manufactured by Daiei Scientific Instruments Manufacturing Co., Ltd., product name: RT-300) 20 as shown in FIG. 2. Specifically, the scraping layer 12 was attached to the movable stage 22 of the Gakushin abrasion tester 20 with double-sided tape, and the scraping layer 12 was placed on the movable stage 22. Sandpaper (manufactured by Sankyo Rikagaku Co., Ltd., product name: LACS-360, AA (aluminum oxide) abrasive grains) 26 as a friction object was attached to the tip of the pressing rod 24 of the Gakushin abrasion tester 20 with double-sided tape, and the sandpaper 26 was placed in contact with the scraping layer 12 placed on the movable stage 22. While applying a constant load (500 g) from the pressing rod 24, the movable stage 22 was moved back and forth in the horizontal direction with a moving distance of 100 mm and a speed of 30 times / min until the number of friction times reached 100, and the scraping layer 12 was rubbed with the sandpaper 26. The weight of the scraping layer before and after the test was measured, and the wear rate (%) was calculated from the change in weight before and after the test. The smaller the wear rate of the scraping layer, the better its wear resistance. The measurement results of the wear resistance of each scraping layer are shown in Table 2.

[0033] (Friction force of scraping layer) The frictional force of the scraping layer is a dynamic frictional force, and is measured based on the plastic film and sheet friction coefficient test method specified in JIS K7125, with a load cell of 100 N, test piece dimensions of approximately 80 x 200 mm, and a contact area of ​​the sliding piece of 40 cm 2 The measurement was performed under the condition of (length of one side: 63 mm). The measurement results of the frictional force of each scraping layer are shown in Table 2.

[0034] (Wipeability of scraping layer - flat surface) The flat wiping properties of each scraping layer were evaluated as follows. Ten drops of polyol (GP-3000NS, manufactured by Sanyo Chemical Industries, Ltd.) colored with blue pigment (phthalocyanine blue pigment) were dropped onto an acrylic plastic plate (plate surface size 1830 mm × 915 mm) using a commercially available dropper. The scraping layer was placed on the polyol dropped onto the plastic plate, and the scraping layer was moved 800 mm along the surface of the plastic plate while applying a certain force, in the same manner as a monitor tester washes tableware such as a cutting board, to wipe off the polyol from the plate surface. The flat wiping properties were evaluated visually based on the range and darkness of the polyol streaks remaining on the plastic plate surface. Here, the scraping layer made of the nonwoven fabric of Comparative Example 1 was used as the standard, and if less polyol remained on the plate surface than in Comparative Example 1, it was evaluated as "○", and if there was particularly little polyol remaining, it was evaluated as "◎". The results of the flat wiping properties of each scraping layer are shown in Table 2.

[0035] (Wipeability of scraping layer - curved surface) The curved surface wiping properties of each scraping layer were evaluated as follows. 30 drops of polyol (manufactured by Sanyo Chemical Industries, Ltd., GP-3000NS) colored with blue pigment (blue pigment copper compound phthalate-di-normal butyl dispersion) were dropped onto a stainless steel hemispherical ladle (size: diameter φ95 × handle length 280 mm, capacity: 200 cc) using a commercially available dropper. The scraping layer was brought into contact with the polyol dropped onto the ladle, and the monitor tester rotated the scraping layer 180° along the inner surface of the ladle in the usual manner of washing dishes, and wiped the polyol off from the ladle. The amount of polyol wiped off was calculated from the weight difference before and after wiping of the scraping layer, and the scraping layer made of the nonwoven fabric of Comparative Example 1 was used as a standard. If the amount of wiping off was greater than that of Comparative Example 1, it was evaluated as "○", and if the amount of polyol wiped off was particularly large, it was evaluated as "◎". The results of the curved surface wiping properties of each scraping layer are shown in Table 2.

[0036] [Table 2]

[0037] Scraping layers were prepared under various conditions shown in Table 3, and evaluated for Asker F hardness, frictional force, abrasion resistance, and wiping ability in the same manner as in the above-mentioned tests. The results are shown in Table 3.

[0038] [Table 3]

[0039] As shown in Tables 2 and 3, by compressing soft polyurethane at a compression ratio in the range of 2 to 4 times, a scraping layer with an appropriate hardness, with an Asker F hardness in the range of 40 degrees to 85 degrees, can be obtained. Also, as shown in Tables 1 and 3, it can be seen that the scraping layer set to an appropriate hardness by compression molding has the same number of cells on the first side as the number of cells of the material, but the number of cells on the second side is greater than that of the first side depending on the compression ratio. Also, it can be seen that the scraping layer set to an appropriate hardness by compression molding has a higher density than the material depending on the compression ratio.

[0040] As shown in Tables 2 and 3, the scraping layer set to an appropriate hardness by compression molding exhibits abrasion resistance equivalent to or superior to that of Comparative Example 1 made of nonwoven fabric, and is sufficiently durable for scraping hard dirt. Here, it can be seen that the scraping layer tends to have improved hardness and abrasion resistance as the compression ratio increases.

[0041] As shown in Tables 2 and 3, the scraping layer made of soft polyurethane foam has a frictional force more than twice that of the nonwoven fabric in Comparative Example 1. In other words, the scraping layer made of soft polyurethane foam can scrape off dirt with a weaker force than the nonwoven fabric, preventing damage to the object to be cleaned.

[0042] As shown in Tables 2 and 3, the scraping layer made of soft polyurethane foam has superior flat surface wiping properties compared to the nonwoven fabric of Comparative Example 1. In other words, the scraping layer made of soft polyurethane foam can remove dirt with less force than the nonwoven fabric and can prevent the dirt from returning to the object to be cleaned.

[0043] As shown in Tables 2 and 3, the scraping layer made of soft polyurethane foam has better curved surface wiping properties than Comparative Example 1 made of nonwoven fabric. This is because the scraping layer made of soft polyurethane foam has better shape conformability to deform along a curved surface than nonwoven fabric. Furthermore, even if the scraping layer made of soft polyurethane foam is set to the same hardness as nonwoven fabric, it exhibits higher curved surface wiping properties than nonwoven fabric, so it can be seen that high shape conformability can be ensured even if the scraping layer is made hard enough to scrape off dirt.

[0044] The above results show that the scraping layer made of the compression-molded flexible polyurethane foam has both appropriate hardness and excellent shape conformability to the object to be cleaned, and therefore the cleaning performance of the scraping layer is improved compared to that of nonwoven fabric. In addition, the scraping layer made of the compression-molded flexible polyurethane foam is deformable even though it is hard, so it is easy to squeeze out water and easy to grip.

[0045] (Example of change) The configuration is not limited to the above, and can be modified as follows, for example. (1) In the embodiment, the cleaning layer has a single layer structure, but the cleaning layer may have a multi-layer structure of two or more layers. For example, the intermediate layer in contact with the scraping layer may have finer and softer cells than the layer constituting the cleaning surface of the cleaning layer, so that the intermediate layer can improve foaming of the detergent. (2) It is not essential that the cleaning surface of the scraping layer has projections and recesses, and the cleaning surface may be formed flat. [Explanation of symbols]

[0046] 12 scraping layer (first layer), 14 cleaning layer (second layer)

Claims

[Claim 1] A first layer made of a flexible polyurethane foam having cells that communicate with each other; A second layer is made of a flexible polyurethane foam having pores communicating with each other and is set to be softer than the first layer. the first layer has a frictional force measured based on JIS K7125 in the range of 1.33 N to 1.61 N; the number of cells present in a plane of the first layer along a direction perpendicular to a lamination direction of the first layer and the second layer as measured based on JIS K6400-1 is in the range of 7 cells / 25 mm to 40 cells / 25 mm; the number of cells present on a surface of the first layer along a lamination direction between the first layer and the second layer as measured based on JIS K6400-1 is in the range of 14 cells / 25 mm to 160 cells / 25 mm; the number of cells present in a plane of the second layer along a direction perpendicular to the lamination direction of the first layer and the second layer as measured based on JIS K6400-1 is in the range of 7 cells / 25 mm to 40 cells / 25 mm; The density of the first layer measured based on JIS K 7222 is in the range of 60 kg / m 3 to 120 kg / m 3 , The density of the second layer measured based on JIS K 7222 is in the range of 30 kg / m 3 to 100 kg / m 3 , The first layer and the second layer are bonded together with an adhesive. A cleaning sponge characterized by:

Citation Information

Patent Citations

  • Sponge cleaner

    JP2001181438A

  • Scrub sponge

    JP2008099916A

  • Washing sponge

    JP2011092370A

  • Wiping material and manufacturing method of the same

    JP2015208481A