Non-aqueous electrolyte secondary battery

The non-aqueous electrolyte secondary battery enhances electrolyte absorption in the negative electrode mixture layer by strategically placing low-porosity graphite particles and concentrated rubber binder, addressing rapid charge/discharge cycle deterioration.

JP7588581B2Active Publication Date: 2024-11-22PANASONIC ENERGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021516019
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-24
Filing Date
2020-04-14
Publication Date
2024-11-22
Estimated Expiration
2040-04-14

AI Technical Summary

Technical Problem

Existing non-aqueous electrolyte secondary batteries used in electric vehicles experience rapid charge/discharge cycle deterioration due to insufficient electrolyte absorption into the negative electrode during charging and discharging.

Method used

A non-aqueous electrolyte secondary battery design featuring a negative electrode mixture layer with a specific distribution of graphite particles and rubber binder, where graphite particles with low internal porosity are predominantly in the outer half region and the rubber binder is concentrated near the negative electrode current collector, enhancing electrolyte absorption.

Benefits of technology

The improved electrolyte absorbability in the negative electrode mixture layer effectively suppresses deterioration in rapid charge/discharge cycle characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588581000002
    Figure 0007588581000002
  • Figure 0007588581000003
    Figure 0007588581000003
  • Figure 0007588581000004
    Figure 0007588581000004
Patent Text Reader

Abstract

The purpose of the present disclosure is to provide a nonaqueous electrolyte secondary battery which is provided with a negative electrode mixture layer that exhibits excellent electrolyte absorbing properties. A nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure is characterized by being provided with a negative electrode having a negative electrode collector and a negative electrode mixture layer that is provided on the surface of the negative electrode collector, and is also characterized in that: the negative electrode mixture layer contains graphite particles A and graphite particles B, which serve as a negative electrode active material, and a rubber binder which serves as a binding agent; the graphite particles A have an internal void fraction of 5% or less; the graphite particles B have an internal void fraction of from 8% to 20%; if the negative electrode mixture layer is divided into two halves in the thickness direction, the outer surface-side half contains more graphite particles A than the negative electrode collector-side half; and from 90% to 100% of the all rubber binder contained in the negative electrode mixture layer is contained in the negative electrode collector-side half.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery. [Background technology]

[0002] The negative electrode mixture layer constituting the negative electrode of the nonaqueous electrolyte secondary battery contains a negative electrode active material and a binder such as a rubber-based binder. In recent years, carbon materials such as graphite particles having a low internal porosity have been used as the negative electrode active material for the purpose of increasing the energy density.

[0003] For example, Patent Document 1 discloses a non-aqueous electrolyte secondary battery that uses densified carbon having an internal porosity of 5% or less as a carbon material.

[0004] Patent Document 2 discloses a nonaqueous electrolyte secondary battery using carbon materials including carbon material A having an internal porosity of 1% or more and less than 23% and carbon material B having an internal porosity of 23% or more and 40% or less. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-320600 [Patent Document 2] JP 2014-67638 A Summary of the Invention [Problem to be solved by the invention]

[0006] When a non-aqueous electrolyte secondary battery is used as a power source for an electric vehicle (EV) or the like, it is often charged and discharged at a high rate, and therefore it is necessary to suppress the deterioration of the rapid charge-discharge cycle characteristics. One of the factors that deteriorate the rapid charge-discharge cycle characteristics is that the electrolyte discharged from the negative electrode that has expanded during charging is not quickly absorbed by the negative electrode during discharging. However, Patent Document 1 and Patent Document 2 do not consider the absorbability of the electrolyte into the negative electrode at all.

[0007] In view of the above, an object of the present disclosure is to provide a nonaqueous electrolyte secondary battery including a negative electrode mixture layer that has excellent electrolyte absorbency. [Means for solving the problem]

[0008] A nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a negative electrode having a negative electrode current collector and a negative electrode mixture layer provided on a surface of the negative electrode current collector. The negative electrode mixture layer includes graphite particles A and graphite particles B as negative electrode active materials, and a rubber-based binder as a binding agent, the internal porosity of the graphite particles A being 5% or less, the internal porosity of the graphite particles B being 8% to 20%, the graphite particles A being contained in a larger amount in an outer surface half region than in an anode current collector half region when the negative electrode mixture layer is divided into two equal parts in a thickness direction, and the rubber-based binder is contained in 90% to 100% of the total rubber-based binder contained in the negative electrode mixture layer in the anode current collector half region. Effect of the Invention

[0009] In the nonaqueous electrolyte secondary battery according to the present disclosure, the negative electrode mixture layer has excellent electrolyte absorbency, and therefore degradation of rapid charge / discharge cycle characteristics can be suppressed. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is an axial cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of a negative electrode according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view of a graphite particle according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] As a result of intensive investigations, the present inventors have found that in order to increase the electrolyte absorbency of the negative electrode mixture layer, it is extremely effective to arrange a larger number of graphite particles with low internal porosity on the outer surface side than on the negative electrode current collector side in a negative electrode mixture layer containing graphite particles with low internal porosity and graphite particles with high internal porosity, while arranging a rubber-based binder on the negative electrode current collector side, and have arrived at the nonaqueous electrolyte secondary battery of the embodiment shown below.

[0012] A nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure includes a negative electrode having a negative electrode current collector and a negative electrode mixture layer provided on a surface of the negative electrode current collector. The negative electrode mixture layer includes graphite particles A and graphite particles B as negative electrode active materials, and a rubber-based binder as a binding agent, the internal porosity of the graphite particles A being 5% or less, the internal porosity of the graphite particles B being 8% to 20%, the graphite particles A being contained in a larger amount in an outer surface half region than in an anode current collector half region when the negative electrode mixture layer is divided into two equal parts in a thickness direction, and the rubber-based binder is contained in 90% to 100% of the total rubber-based binder contained in the negative electrode mixture layer in the anode current collector half region.

[0013] An example of an embodiment will be described in detail below with reference to the drawings. In the following description, specific shapes, materials, numerical values, directions, etc. are examples for facilitating understanding of the present disclosure, and can be appropriately changed according to the specifications of the nonaqueous electrolyte secondary battery. In addition, when multiple embodiments and modified examples are included in the following description, it is assumed from the beginning that the characteristic parts of these embodiments and modified examples will be appropriately combined and used.

[0014] FIG. 1 is an axial cross-sectional view of a nonaqueous electrolyte secondary battery 10 according to an embodiment. In the nonaqueous electrolyte secondary battery 10 shown in FIG. 1, an electrode body 14 and a nonaqueous electrolyte (not shown) are housed in a battery case 15. The electrode body 14 has a wound structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween. The electrode body 14 may be of a form other than the wound type, such as a laminated electrode body 14 in which the positive electrode 11 and the negative electrode 12 are alternately laminated with a separator interposed therebetween. As the nonaqueous solvent (organic solvent) for the nonaqueous electrolyte, carbonates, lactones, ethers, ketones, esters, etc. can be used, and two or more of these solvents can be mixed and used. For example, cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate, chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate, and diethyl carbonate, and mixed solvents of cyclic carbonates and chain carbonates can be used. As the electrolyte salt of the non-aqueous electrolyte, LiPF6, LiBF4, LiCF3SO3, and mixtures thereof can be used. The amount of electrolyte salt dissolved in the non-aqueous solvent can be, for example, 0.5 to 2.0 mol / L. For convenience of explanation, the sealing body 17 side of the battery case 15 will be described as the "upper" side, and the bottom side of the exterior body 16 will be described as the "lower" side.

[0015] The battery case 15 is composed of an exterior body 16 and a sealing body 17 that closes the opening of the exterior body 16. Insulating plates 18 and 19 are provided above and below the electrode body 14. The positive electrode lead 20 passes through a through hole in the insulating plate 18 and extends to the sealing body 17 side, and is welded to the lower surface of a filter 23 that is the bottom plate of the sealing body 17. In the nonaqueous electrolyte secondary battery 10, a cap 27 that is the top plate of the sealing body 17 and is electrically connected to the filter 23 serves as a positive electrode terminal. On the other hand, the negative electrode lead 21 passes through a through hole in the insulating plate 19 and extends to the bottom side of the exterior body 16, and is welded to the inner bottom surface of the exterior body 16. In the nonaqueous electrolyte secondary battery 10, the exterior body 16 serves as a negative electrode terminal. When the negative electrode lead 21 is provided near the outer end of the winding, the negative electrode lead 21 passes outside the insulating plate 19, extends to the bottom side of the exterior body 16, and is welded to the inner bottom surface of the exterior body 16. Examples of battery case 15 include metallic exterior cases having a cylindrical, rectangular, coin or button shape, and pouch exterior bodies formed by laminating a resin sheet and a metal sheet.

[0016] The exterior body 16 is, for example, a cylindrical metal exterior can with a bottom. A gasket 28 is provided between the exterior body 16 and the sealing body 17 to ensure airtightness inside the battery case 15. The exterior body 16 has a protruding portion 22 that supports the sealing body 17 and is formed, for example, by pressing a side portion from the outside. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior body 16, and supports the sealing body 17 on its upper surface.

[0017] The sealing body 17 includes a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27, which are stacked in this order from the electrode body 14 side. Each member constituting the sealing body 17 has, for example, a disk shape or a ring shape, and each member except the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, for example, the lower valve body 24 breaks, which causes the upper valve body 26 to swell toward the cap 27 and move away from the lower valve body 24, thereby cutting off the electrical connection between them. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.

[0018] The positive electrode 11, the negative electrode 12, and the separator 13 that constitute the electrode assembly 14, and in particular the negative electrode mixture layer 42 that constitutes the negative electrode 12, will be described in detail below.

[0019] [Negative electrode] FIG. 2 is a cross-sectional view of the negative electrode 12, which is an example of an embodiment. The negative electrode 12 has a negative electrode current collector 40 and a negative electrode mixture layer 42 provided on the surface of the negative electrode current collector 40. For example, a foil of a metal such as copper that is stable in the potential range of the negative electrode 12, or a film having the metal disposed on the surface layer, is used as the negative electrode current collector 40. The negative electrode mixture layer 42 has a negative electrode current collector side half region 42a located near the negative electrode current collector 40 when the negative electrode mixture layer 42 is divided in half at the middle Z of the thickness, and an outer surface side half region 42b of the negative electrode mixture layer 42 located far from the negative electrode current collector 40. The negative electrode mixture layer 42 also contains graphite particles 30 as a negative electrode active material and a rubber-based binder as a binder.

[0020] The rubber-based binder has a molecular structure in which double bonds and single bonds are repeated, and examples thereof include styrene butadiene rubber (SBR), nitrile butadiene rubber (NBR), and modified products thereof. The average primary particle diameter of the rubber-based binder is preferably 120 to 250 nm, more preferably 150 to 230 nm. The negative electrode mixture layer 42 may further contain a binder such as fluorine-containing resin such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, etc. The negative electrode mixture layer 42 may also contain carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), etc. The CMC or a salt thereof functions as a thickener that adjusts the negative electrode active material slurry to an appropriate viscosity range, and also functions as a binder. These binders may be used alone or in combination of two or more.

[0021] The rubber-based binder is contained in the negative electrode current collector side half region 42a at 90% to 100% of the total rubber-based binder contained in the negative electrode mixture layer 42. The rubber-based binder is contained in a large amount in the negative electrode current collector side half region 42a, thereby improving the adhesive strength between the negative electrode current collector 40 and the negative electrode mixture layer 42. On the other hand, since the rubber-based binder contained in the outer surface side half region 42b is small, the negative electrode mixture layer 42 can quickly absorb the electrolyte. This can suppress the deterioration of the rapid charge / discharge cycle characteristics. As described later, the rubber-based binder diffuses between the negative electrode current collector side half region 42a and the outer surface side half region 42b of the negative electrode mixture layer 42 during drying during the manufacture of the negative electrode mixture layer 42, so that the distribution of the rubber-based binder in the negative electrode mixture layer 42 after drying is different from the distribution at the time of mixing. The content of the rubber-based binder is obtained by the following procedure.

[0022] <Method of measuring rubber binder content> (1) Exposing a cross section of the negative electrode mixture layer 42. Examples of a method for exposing the cross section include a method in which a part of the negative electrode 12 is cut out and processed with an ion milling device (e.g., IM4000PLUS manufactured by Hitachi High-Technologies Corporation) to expose the cross section of the negative electrode mixture layer 42. (2) Using osmium tetroxide or the like, a marker such as osmium is reacted with the double bonds of the rubber-based binder exposed on the cross section of the negative electrode mixture layer 42 to fix it. (3) An image of a cross section of the negative electrode mixture layer 42 is obtained by mapping markers using an EDX (Energy Dispersive X-ray Spectroscopy) attached to a scanning electron microscope. (4) From the above image, the rubber-based binder contents in the negative electrode current collector side half region 42a and the outer surface side half region 42b of the negative electrode mixture layer 42 are calculated, and the proportion of the rubber-based binder contained in the negative electrode current collector side half region 42a is calculated. The rubber-based binder content is taken as the average value of 10 measured values.

[0023] Next, the graphite particle 30 will be described with reference to Fig. 3. Fig. 3 is a cross-sectional view of the graphite particle 30 contained in the negative electrode mixture layer 42. In a cross-sectional view of the graphite particle 30, the graphite particle 30 has closed voids 32 that do not connect from the inside of the particle to the particle surface (hereinafter, internal voids 32), and voids 34 that connect from the inside of the particle to the particle surface (hereinafter, external voids 34).

[0024] The graphite particles 30 include graphite particles A having an internal porosity of 5% or less and graphite particles B having an internal porosity of 8% to 20%. The internal porosity of the graphite particles A may be 5% or less in order to suppress the deterioration of rapid charge / discharge cycle characteristics, but is preferably 1% to 5%, and more preferably 3% to 5%. The internal porosity of the graphite particles B may be 8% to 20%, but is preferably 10% to 18%, and more preferably 12% to 16%, in order to suppress the deterioration of rapid charge / discharge cycle characteristics. Here, the internal porosity of the graphite particles 30 is a two-dimensional value calculated from the ratio of the area of ​​the internal voids 32 of the graphite particles 30 to the cross-sectional area of ​​the graphite particles 30. The internal porosity of the graphite particles 30 is calculated by the following procedure.

[0025] <Method for measuring internal porosity> (1) In the same manner as in the method for measuring the rubber-based binder content, a cross section of the negative electrode mixture layer 42 is exposed using an ion milling device or the like. (2) Using a scanning electron microscope, a backscattered electron image is taken of the cross section of the exposed negative electrode mixture layer 42. The magnification when taking the backscattered electron image is 3,000 to 5,000 times. (3) The cross-sectional image obtained as described above is imported into a computer and binarized using image analysis software (e.g., ImageJ, manufactured by the National Institutes of Health, USA) to obtain a binary processed image in which the particle cross-sections in the cross-sectional image are colored black and voids present in the particle cross-sections are colored white. (4) From the binarized image, graphite particles A and B having a particle size of 5 μm to 50 μm are selected, and the area of ​​the graphite particle cross section and the area of ​​the internal voids 32 present in the graphite particle cross section are calculated. Here, the area of ​​the graphite particle cross section refers to the area of ​​the region surrounded by the outer periphery of the graphite particle 30, that is, the area of ​​the entire cross section of the graphite particle 30. In addition, for voids present in the graphite particle cross section that have a width of 3 μm or less, it may be difficult to distinguish whether they are internal voids 32 or external voids 34 in image analysis, so that voids with a width of 3 μm or less may be regarded as internal voids 32. Then, the internal porosity of the graphite particle 30 (area of ​​internal voids 32 in graphite particle cross section × 100 / area of ​​graphite particle cross section) is calculated from the calculated area of ​​the graphite particle cross section and the area of ​​the internal voids 32 in the graphite particle cross section. The internal porosity of the graphite particles A and B is the average value of 10 graphite particles A and B.

[0026] The graphite particles A and B are produced, for example, as follows. <Graphite particles A with internal porosity of 5% or less> For example, the coke (precursor) as the main raw material is crushed to a predetermined size, and then the crushed coagulated coke is calcined at a temperature of 2600°C or higher, graphitized, and sieved to obtain graphite particles A of a desired size. The internal porosity can be adjusted to 5% or less by adjusting the particle size of the crushed precursor or the particle size of the aggregated precursor. For example, the average particle size (median diameter D50) of the crushed precursor is preferably in the range of 12 μm to 25 μm. In addition, when the internal porosity is reduced to a range of 5% or less, it is preferable to increase the particle size of the crushed precursor. <Graphite particles B with internal porosity of 8% to 20%> For example, the coke (precursor) as the main raw material is crushed to a predetermined size, aggregated with an aggregating agent, and then pressed into a block shape, which is then fired at a temperature of 2600°C or higher to be graphitized. The graphitized block-shaped body is crushed and sieved to obtain graphite particles B of a desired size. Here, the internal porosity can be adjusted to 8% to 20% depending on the amount of volatile components added to the block-shaped body. When a part of the aggregating agent added to the coke (precursor) volatilizes during firing, the aggregating agent can be used as a volatile component. Pitch is an example of such an aggregating agent.

[0027] The graphite particles A and B used in this embodiment may be natural graphite, artificial graphite, or the like, but are not particularly limited thereto. However, in terms of ease of adjusting the internal porosity, artificial graphite is preferred. The interplanar spacing (d 002 ) is, for example, preferably 0.3354 nm or more, more preferably 0.3357 nm or more, and preferably less than 0.340 nm, more preferably 0.338 nm or less. The crystallite size (Lc(002)) of the graphite particles A and B used in this embodiment, determined by X-ray diffraction, is, for example, preferably 5 nm or more, more preferably 10 nm or more, and preferably 300 nm or less, more preferably 200 nm or less. The interplanar spacing (d 002 When the crystallite size (Lc(002)) satisfies the above range, the battery capacity of the nonaqueous electrolyte secondary battery 10 tends to be larger than when the crystallite size (Lc(002)) does not satisfy the above range.

[0028] In this embodiment, the graphite particles A are contained more in the outer surface half region 42b than in the negative electrode current collector half region 42a when the negative electrode mixture layer 42 shown in FIG. 2 is divided into two equal parts in the thickness direction. Since the graphite particles A with low internal porosity are contained more in the outer surface half region 42b, the gaps between the active material particles that serve as electrolyte absorption paths are increased in the outer surface half region 42b compared to when the graphite particles A are uniformly dispersed in the negative electrode mixture layer 42. As a result, the electrolyte is quickly absorbed into the negative electrode mixture layer 42. Furthermore, since the graphite particles A are contained more in the outer surface half region 42b, the graphite particles B with high internal porosity are contained more in the negative electrode current collector half region 42a. As a result, the gaps between the active material particles are reduced in the negative electrode current collector half region 42a, and the diffusion of the rubber-based binder from the negative electrode current collector half region 42a to the outer surface half region 42b is suppressed.

[0029] In this embodiment, it is sufficient that the graphite particles A are contained more in the outer surface half region 42b than in the negative electrode current collector half region 42a, but in order to further suppress the deterioration of rapid charge-discharge cycle characteristics, the ratio of the graphite particles A to the graphite particles B in the outer surface half region 42b is preferably 60:40 to 100:0 by mass, and more preferably 100:0. In order to further suppress the deterioration of rapid charge-discharge cycle characteristics, the ratio of the graphite particles A to the graphite particles B in the negative electrode current collector half region 42a is preferably 40:60 to 0:100 by mass, and more preferably 0:100.

[0030] Next, a method for manufacturing the negative electrode mixture layer 42 for making the amount of graphite particles A larger in the outer surface half region 42b than in the negative electrode current collector half region 42a will be described. For example, first, a negative electrode active material containing graphite particles B (graphite particles A as necessary), a binder, and a solvent such as water are mixed to prepare a negative electrode mixture slurry for the negative electrode current collector side. Separately, a negative electrode active material containing a larger amount of graphite particles A (graphite particles B as necessary) than the negative electrode mixture slurry for the negative electrode current collector side is mixed with a binder and a solvent such as water to prepare a negative electrode mixture slurry for the outer surface side. Then, the negative electrode mixture layer 42 can be formed by applying the negative electrode mixture slurry for the negative electrode current collector side to both sides of the coating film made of the negative electrode mixture slurry for the negative electrode current collector side and drying the entire coating film. In the above method, the negative electrode mixture slurry for the outer surface side is applied before drying of the negative electrode mixture slurry for the negative electrode current collector side, but the negative electrode mixture slurry for the outer surface side may be applied after drying of the negative electrode mixture slurry for the negative electrode current collector side. The negative electrode mixture slurry for the negative electrode current collector side and the negative electrode mixture slurry for the outer surface side are preferably applied so that the thicknesses of the coatings are equal to each other, but the thicknesses of the coatings may be different from each other. That is, a part of the negative electrode mixture slurry for the negative electrode current collector side may be included in the outer surface half region 42b, or a part of the negative electrode mixture slurry for the outer surface side may be included in the negative electrode current collector half region 42a.

[0031] The negative electrode active material may contain, in addition to the graphite particles A and B used in this embodiment, other materials capable of reversibly absorbing and releasing lithium ions, for example, a Si-based material. Examples of the Si-based material include Si, an alloy containing Si, and SiO x(x is 0.8 to 1.6), and the like. The Si-based material is a negative electrode material capable of improving the battery capacity more than the graphite particles 30, but on the other hand, it is disadvantageous in terms of rapid charge / discharge cycle characteristics due to its large volume expansion accompanying charge / discharge. The content of the Si-based material is, for example, preferably 1 mass % to 10 mass %, and more preferably 3 mass % to 7 mass %, relative to the mass of the negative electrode active material, from the viewpoints of improving the battery capacity and suppressing the deterioration of the rapid charge / discharge cycle characteristics.

[0032] Other examples of the other material capable of reversibly absorbing and releasing lithium ions include metals that are alloyed with lithium, such as tin (Sn), or alloys or oxides containing metal elements such as Sn. The negative electrode active material may contain the other materials, and the content of the other materials is desirably, for example, 10% by mass or less with respect to the mass of the negative electrode active material.

[0033] [Positive electrode] The positive electrode 11 is composed of a positive electrode current collector such as a metal foil and a positive electrode mixture layer formed on the positive electrode current collector. The positive electrode current collector may be a foil of a metal such as aluminum that is stable in the potential range of the positive electrode 11, or a film having the metal disposed on the surface layer. The positive electrode mixture layer contains, for example, a positive electrode active material, a binder, a conductive agent, etc.

[0034] The positive electrode 11 can be produced, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive agent, etc. onto a positive electrode current collector, drying it to form a positive electrode mixture layer, and then rolling this positive electrode mixture layer.

[0035] The positive electrode active material may be, for example, a lithium transition metal composite oxide containing a transition metal element such as Co, Mn, or Ni. x CoO2, Li x NiO2, Li x MnO2, Li x Co y Ni 1-y O2, Li x Co y M 1-y O z , Lix Ni 1-y M y O z 、 Li x Mn2O4, Li x Mn 2-y M y O4, LiMPO4, Li2MPO4F (M; at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3). These may be used alone or in combination of multiple kinds. In terms of achieving a higher capacity of the non-aqueous electrolyte secondary battery 10, the positive electrode active material is Li x NiO2, Li x Co y Ni 1-y O2, Li x Ni 1-y M y O z (M; at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3), etc., and preferably contains a lithium nickel composite oxide.

[0036] Examples of the conductive agent include carbon-based particles such as carbon black (CB), acetylene black (AB), ketjen black, and graphite. These may be used alone or in combination of two or more kinds.

[0037] Examples of the binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, and polyolefin-based resins. These may be used alone or in combination of two or more kinds.

[0038] [Separator] For example, a porous sheet having ion permeability and insulation is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. The material of the separator 13 is preferably an olefin resin such as polyethylene or polypropylene, or cellulose. The separator 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. The separator 13 may also be a multi-layer separator 13 including a polyethylene layer and a polypropylene layer, and a separator 13 having a surface coated with a material such as an aramid resin or ceramic may also be used. EXAMPLES

[0039] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.

[0040] <Example 1> [Preparation of positive electrode] The positive electrode active material is aluminum-containing lithium nickel cobalt oxide (LiNi 0.88 Co 0.09 Al 0.03 O2) was used. The positive electrode active material was mixed in an amount of 100 parts by mass, acetylene black (AB) as a conductive agent was mixed in an amount of 1 part by mass, and polyvinylidene fluoride (PVdF) as a binder was mixed in an amount of 0.9 parts by mass, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added to prepare a positive electrode mixture slurry. This slurry was applied to both sides of a positive electrode current collector made of aluminum foil (thickness 15 μm) by the doctor blade method, and after drying the coating, the coating was rolled with a rolling roller to prepare a positive electrode in which a positive electrode mixture layer was formed on both sides of the positive electrode current collector.

[0041] [Preparation of graphite particles A] The coke was pulverized until the average particle size (median diameter D50) was 12 μm. Pitch was added as a binder to the pulverized coke, and the coke was aggregated until the average particle size (median diameter D50) was 17 μm. The aggregate was graphitized by baking at a temperature of 2800° C., and then sieved using a 250 mesh sieve to obtain graphite particles A with an average particle size (median diameter D50) of 23 μm.

[0042] [Preparation of graphite particles B] The coke was crushed to an average particle size (median diameter D50) of 15 μm, and the crushed coke was agglomerated by adding pitch as a binder. The coke was then subjected to an isostatic pressure of 1.6 g / cm. 3 ~1.9g / cm 3 A block-shaped compact having a density of 1000 nm was produced. This block-shaped compact was graphitized by firing at a temperature of 2800° C. Next, the graphitized block-shaped compact was pulverized and sieved using a 250 mesh sieve to obtain graphite particles B having an average particle size (median size D50) of 23 μm.

[0043] [Preparation of negative electrode] Graphite particles A were mixed to 100 parts by mass and SiO was mixed to 5 parts by mass, and this was used as the negative electrode active material A contained in the outer surface side half region of the negative electrode mixture layer. The negative electrode active material A: carboxymethyl cellulose (CMC): polyacrylic acid (PAA) were mixed to a mass ratio of 100:1:1 to prepare a negative electrode mixture slurry for the outer surface side. In addition, graphite particles B were mixed to 100 parts by mass and SiO was mixed to 5 parts by mass, and this was used as the negative electrode active material B contained in the negative electrode current collector side half region of the negative electrode mixture layer. The negative electrode active material B: carboxymethyl cellulose (CMC): polyacrylic acid (PAA): styrene butadiene rubber (SBR) were mixed to a mass ratio of 100:1:1:1 to prepare a negative electrode mixture slurry for the negative electrode current collector side. Here, the average primary particle diameter of SBR was 150 nm.

[0044] The negative electrode mixture slurry for the negative electrode current collector side was applied to both sides of the negative electrode current collector made of copper foil by the doctor blade method, the coating film was dried, and then the negative electrode mixture slurry for the outer surface side was applied to the coating film, dried, and then the coating film was rolled with a rolling roller to produce a negative electrode in which a negative electrode mixture layer was formed on both sides of the negative electrode current collector. That is, the graphite particles A:graphite particles B in the outer surface side half region of the negative electrode mixture layer was 100:0 in mass ratio, and the graphite particles A:graphite particles B in the negative electrode current collector side half region of the negative electrode mixture layer was 0:100 in mass ratio. In addition, when the internal porosity of the graphite particles A and B in the produced negative electrode was measured, it was 3% and 15%, respectively.

[0045] The mixing ratio of the rubber-based binder (rubber-based binder in the negative electrode mixture slurry for the outer surface side: rubber-based binder in the negative electrode mixture slurry for the negative electrode current collector side) was 0:100 by mass. The negative electrode mixture slurry for the negative electrode current collector side and the negative electrode mixture slurry for the outer surface side were applied so that the thickness of each coating film was equal. However, the rubber-based binder diffused during drying during the manufacture of the negative electrode mixture layer, and the presence ratio of the rubber-based binder after drying (rubber-based binder in the outer surface half of the negative electrode mixture layer: rubber-based binder in the negative electrode current collector half of the negative electrode mixture layer) was 7:93 by mass.

[0046] <Example 2> A negative electrode was produced in the same manner as in Example 1, except that a mixture of 60 parts by mass of graphite particles A, 40 parts by mass of graphite particles B, and 5 parts by mass of SiO was used as the negative electrode active material A, and a mixture of 40 parts by mass of graphite particles A, 60 parts by mass of graphite particles B, and 5 parts by mass of SiO was used as the negative electrode active material B. That is, the graphite particles A:graphite particles B in the outer surface half of the negative electrode mixture layer was 60:40 in mass ratio, and the graphite particles A:graphite particles B in the negative electrode current collector side half of the negative electrode mixture layer was 40:60 in mass ratio. In addition, the presence ratio of the rubber-based binder after drying (rubber-based binder in the outer surface half of the negative electrode mixture layer:rubber-based binder in the negative electrode current collector side half of the negative electrode mixture layer) was 9:91 in mass ratio.

[0047] <Comparative Example 1> Graphite particles A were mixed in an amount of 50 parts by mass, graphite particles B in an amount of 5 parts by mass, and SiO in an amount of 5 parts by mass, and this was used as the negative electrode active material C contained in the entire region of the negative electrode mixture layer. The negative electrode active material C: carboxymethyl cellulose (CMC): polyacrylic acid (PAA): styrene butadiene rubber (SBR) were mixed in an amount of 100:1:1:1 to prepare a negative electrode mixture slurry. This negative electrode mixture slurry was applied to both sides of a negative electrode current collector made of copper foil by a doctor blade method, and after drying the coating film, the coating film was rolled with a rolling roller to prepare a negative electrode in which a negative electrode active material layer was formed on both sides of the negative electrode current collector. That is, the graphite particles A: graphite particles B in the outer surface side half region of the negative electrode active material layer was 50:50 in mass ratio, and the graphite particles A: graphite particles B in the negative electrode current collector side half region of the negative electrode active material layer was also 50:50 in mass ratio. The ratio of the rubber-based binders after drying (rubber-based binder in the outer surface half of the negative electrode mixture layer:rubber-based binder in the negative electrode current collector half of the negative electrode mixture layer) was 48:52 by mass.

[0048] <Comparative Example 2> The same negative electrode active material A as in Example 1 was used, and the mass ratio of the negative electrode active material A: carboxymethylcellulose (CMC): polyacrylic acid (PAA): styrene butadiene rubber (SBR) was 100: 1: 1: 0.5, and these were mixed to prepare a negative electrode mixture slurry for the outer surface side. In addition, the same negative electrode active material B as in Example 1 was used, and the mass ratio of the negative electrode active material B: carboxymethylcellulose (CMC): polyacrylic acid (PAA): styrene butadiene rubber (SBR) was 100: 1: 1: 0.5, and these were mixed to prepare a negative electrode mixture slurry for the negative electrode current collector side. Thereafter, a negative electrode was produced in the same manner as in Example 1, using the negative electrode mixture slurry for the outer surface side and the negative electrode mixture slurry for the negative electrode current collector side. That is, the mass ratio of graphite particles A to graphite particles B in the outer surface half of the negative electrode mixture layer was 100:0, and the mass ratio of graphite particles A to graphite particles B in the negative electrode current collector side half of the negative electrode mixture layer was 0:100. In addition, the presence ratio of the rubber-based binder after drying (rubber-based binder in the outer surface half of the negative electrode mixture layer:rubber-based binder in the negative electrode current collector side half of the negative electrode mixture layer) was 43:57 in mass ratio.

[0049] <Comparative Example 3> A negative electrode was prepared in the same manner as in Example 1, except that the negative electrode active material C, which was the same as in Comparative Example 1, was used instead of the negative electrode active material A and the negative electrode active material B. That is, the graphite particles A:graphite particles B in the outer surface half of the negative electrode active material layer were in a mass ratio of 50:50, and the graphite particles A:graphite particles B in the negative electrode current collector half of the negative electrode active material layer were also in a mass ratio of 50:50. In addition, the presence ratio of the rubber-based binder after drying (rubber-based binder in the outer surface half of the negative electrode mixture layer:rubber-based binder in the negative electrode current collector half of the negative electrode mixture layer) was 9:91 in mass ratio.

[0050] [Measurement of absorption time] The negative electrodes of each Example and Comparative Example were dried for 10 hours in a thermostatic chamber heated to 200°C under a nitrogen atmosphere, and each negative electrode was cut into a size of 2 cm x 5 cm to prepare a sample. 1.5 μml of polypropylene carbonate (PC) was dropped vertically onto the surface of each sample, and the time until the PC was absorbed into the inside of the sample was measured visually. Measurements were performed six times for each sample, and the average value was taken as the liquid absorption time.

[0051] The results of the liquid absorption time of the nonaqueous electrolyte secondary batteries of each Example and Comparative Example are summarized in Table 1. The liquid absorption time shown in Table 1 is a relative value assuming that the liquid absorption time of Example 1 is 100. Note that the shorter the liquid absorption time, the smoother the replacement of the electrolyte in the negative electrode mixture layer can be performed, and therefore the electrolyte discharged from the negative electrode mixture layer during charging is quickly absorbed by the negative electrode mixture layer during discharging, thereby suppressing the deterioration of the rapid charge / discharge cycle characteristics.

[0052] [Table 1]

[0053] As can be seen from Table 1, both Examples 1 and 2 have a shorter liquid absorption time than Comparative Examples 1 to 3. In Comparative Examples 2 and 3, in which only one of the graphite ratio and the mass ratio of the rubber-based binder is changed from Comparative Example 1, the liquid absorption time is shortened to 80% and 76% of Comparative Example 1, respectively. On the other hand, in Example 1, in which both the graphite ratio and the mass ratio of the rubber-based binder are changed from Comparative Example 1, the liquid absorption time is shortened to 45% of Comparative Example 1. In this way, by including more graphite particles A in the outer surface half region than in the negative electrode current collector half region in the negative electrode current collector half region, and including 90 mass% or more of the rubber-based binder in the negative electrode current collector half region in the negative electrode current collector half region in the negative electrode current collector half region, the electrolyte absorption speed can be significantly increased. Therefore, the deterioration of the rapid charge / discharge cycle characteristics can be suppressed. [Explanation of symbols]

[0054] 10 nonaqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 battery case, 16 exterior body, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 protruding portion, 23 filter, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket, 30 graphite particles, 32 internal gap, 34 external gap, 40 negative electrode current collector, 42 negative electrode mixture layer, 42a negative electrode current collector side half region, 42b outer surface side half region.

Claims

1. a negative electrode having a negative electrode current collector and a negative electrode mixture layer provided on a surface of the negative electrode current collector; and a liquid nonaqueous electrolyte; The negative electrode mixture layer contains graphite particles A and graphite particles B as negative electrode active materials, and a rubber-based binder as a binding agent, the graphite particles A have an internal porosity of 5% or less, and the graphite particles B have an internal porosity of 8% to 20%, the graphite particles A are contained in a larger amount in an outer surface half region than in an outer surface half region of the negative electrode current collector side when the negative electrode mixture layer is divided into two equal parts in a thickness direction; the rubber-based binder is contained in the negative electrode mixture layer in an amount of 90% by mass to 100% by mass in the negative electrode current collector side half region.

2. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein a mass ratio of said graphite particles A to said graphite particles B in said outer surface half region is 60:40 to 100:0.

Citation Information

Patent Citations

  • Electrochemical battery fined carbon

    JP1997320600A

  • Nonaqueous secondary battery and manufacture thereof

    JP2000011997A

  • Electrode structure, battery, and method for manufacturing electrode structure

    JP2011009203A

  • Carbon material and negative electrode for nonaqueous secondary battery, and nonaqueous secondary battery

    JP2012216537A

  • Carbon material for nonaqueous secondary battery, negative electrode, and nonaqueous secondary battery

    JP2014067638A