RTB permanent magnet
The R-T-B permanent magnet composition, with precise element ratios and additives, addresses the trade-off in magnetic properties by improving residual magnetic flux density and coercive force, ensuring stability and corrosion resistance.
Patent Information
- Application Number
- JP2022074141
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-12-06
- Filing Date
- 2022-04-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2037-12-05
AI Technical Summary
Existing R-T-B permanent magnets face challenges in achieving high residual magnetic flux density (Br) and coercive force (HcJ), particularly after grain boundary diffusion of heavy rare earth elements, which often results in a trade-off between these properties.
The R-T-B permanent magnet composition includes specific ranges of elements such as Fe, Cu, Co, Ga, and B, with controlled atomic ratios and concentrations, along with optional additives like Nd, Pr, Al, Zr, and Mn, to enhance Br and HcJ, while maintaining manufacturing stability and corrosion resistance.
The optimized composition and manufacturing process result in an R-T-B permanent magnet with improved residual magnetic flux density and coercive force, even after grain boundary diffusion, offering enhanced magnetic properties and stability.
Smart Images

Figure 0007588618000001 
Figure 0007588618000002 
Figure 0007588618000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an RTB-based permanent magnet. [Background technology]
[0002] Rare earth permanent magnets with RTB-based compositions have excellent magnetic properties, and much research is being done to further improve these properties. Residual magnetic flux density (residual magnetization) Br and coercive force HcJ are generally used as indicators of magnetic properties. Magnets with high values for these can be said to have excellent magnetic properties.
[0003] For example, Patent Document 1 describes an Nd-Fe-B rare earth permanent magnet having good magnetic properties.
[0004] Furthermore, Patent Document 2 describes a rare earth permanent magnet in which a magnet body is immersed in a slurry in which fine powders containing various rare earth elements are dispersed in water or an organic solvent, and then heated to cause grain boundary diffusion. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2006-210893 A [Patent Document 2] International Publication No. 2006 / 43348 Brochure Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide an RTB permanent magnet that has high residual magnetic flux density Br and coercive force HcJ, and further has high residual magnetic flux density Br and coercive force HcJ after grain boundary diffusion of a heavy rare earth element. [Means for solving the problem]
[0007] In order to achieve the above object, the RTB permanent magnet of the present invention is An RTB type permanent magnet in which R is a rare earth element, T is an element other than rare earth elements, B, C, O and N, and B is boron, T contains at least Fe, Cu, Co and Ga; The total mass of R, T and B is 100% by mass. The total content of R is 28.0 mass% to 30.2 mass%; The Cu content is 0.04 mass% to 0.50 mass%. The Co content is 0.5 mass% to 3.0 mass%. The Ga content is 0.08 mass% to 0.30 mass%; The content of B is 0.85% by mass to 0.95% by mass.
[0008] The RTB permanent magnet of the present invention has the above-mentioned characteristics, which allows it to improve the residual magnetic flux density Br and the coercive force HcJ. Furthermore, it can further enhance the effect of grain boundary diffusion of a heavy rare earth element. Specifically, it can also improve the residual magnetic flux density Br and the coercive force HcJ of the RTB permanent magnet obtained by diffusing a heavy rare earth element.
[0009] The total content of R may be 29.2 mass % to 30.2 mass %.
[0010] R may contain at least Nd.
[0011] R may contain at least Pr, and the Pr content may be greater than 0 and less than or equal to 10.0 mass %.
[0012] R may contain at least Nd and Pr.
[0013] T may further contain Al, The Al content may be 0.15 mass % to 0.30 mass %.
[0014] T may further contain Zr, and the content of Zr may be 0.10 mass% to 0.30 mass%.
[0015] It may further contain C, and the content of C may be 1100 ppm or less based on the total mass of the R-T-B-based permanent magnet.
[0016] It may further contain N, and the content of N may be 1000 ppm or less based on the total mass of the R-T-B-based permanent magnet.
[0017] It may further contain O, and the content of O may be 1000 ppm or less based on the total mass of the R-T-B-based permanent magnet.
[0018] When the total content of R is defined as TRE, TRE / B may be 2.2 to 2.7 in terms of atomic ratio.
[0019] 14B / (Fe + Co) may be greater than 0 and 1.01 or less in terms of atomic ratio.
[0020] The concentration distribution of the heavy rare earth element may be a concentration distribution that decreases from the outside to the inside.
Mode for Carrying Out the Invention
[0021] Hereinafter, an embodiment of the present invention will be described.
[0022] <R-T-B-based permanent magnet> The R-T-B-based permanent magnet according to this embodiment is R2T 14The magnet has grains and grain boundaries made of B crystals. By containing a plurality of specific elements in specific ranges of content, it is possible to improve the residual magnetic flux density Br, the coercive force HcJ, the corrosion resistance, and the manufacturing stability. Furthermore, it is possible to reduce the decrease in the residual magnetic flux density Br and increase the increase in the coercive force HcJ in the grain boundary diffusion described below. In other words, the RTB permanent magnet according to this embodiment has excellent characteristics even without a grain boundary diffusion process, and is an RTB permanent magnet that is also suitable for grain boundary diffusion. Furthermore, from the viewpoint of improving the coercive force HcJ, it is preferable that the element diffused by the grain boundary diffusion is a heavy rare earth element.
[0023] R is a rare earth element. The rare earth elements include Sc, Y, and lanthanoid elements that belong to Group 3 of the long periodic table. The lanthanoid elements include, for example, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, etc. In addition, it is preferable that R includes Nd.
[0024] Rare earth elements are generally classified into light rare earth elements and heavy rare earth elements, but the heavy rare earth elements in the RTB permanent magnet according to this embodiment are Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu.
[0025] T represents an element other than rare earth elements, B, C, O, and N. In the RTB permanent magnet according to this embodiment, T contains at least Fe, Co, Cu, and Ga. In addition, T may further contain one or more elements selected from the group consisting of Al, Mn, Zr, Ti, V, Cr, Ni, Nb, Mo, Ag, Hf, Ta, W, Si, P, Bi, and Sn.
[0026] B is boron.
[0027] The total content of R is 28.0% by mass or more and 30.2% by mass or less, with the total mass of R, T and B being 100% by mass. If the total content of R is too low, the coercive force HcJ decreases. If the total content of R is too high, the residual magnetic flux density Br decreases. The total content of R may be 29.2% by mass or more and 30.2% by mass or less. By setting the total content of R to 29.2% by mass or more, the amount of deformation during sintering is reduced, thereby improving manufacturing stability.
[0028] Furthermore, the RTB permanent magnet of this embodiment may have any Nd content. The Nd content may be 0 mass% to 30.2 mass%, 0 mass% to 29.7 mass%, 19.7 mass% to 29.7 mass%, 19.7 mass% to 24.7 mass%, or 19.7 mass% to 22.6 mass%, with the total mass of R, T, and B being 100 mass%. The Pr content may be 0.0 mass% to 10.0 mass%. In other words, Pr may not be contained. The RTB permanent magnet of this embodiment may contain at least Nd and Pr as R. The Pr content may be 5.0 mass% or more and 10.0 mass% or less. It may also be 5.0 mass% or more and 7.6 mass% or less. When the Pr content is 10.0 mass% or less, the temperature coefficient of coercivity HcJ is excellent. In particular, from the viewpoint of increasing the coercive force HcJ at high temperatures, the Pr content is preferably set to 0.0 mass % to 7.6 mass %.
[0029] The RTB permanent magnet of this embodiment may also contain a total of 0.5 mass% or less of Tb and / or Dy as R. If the total content of Tb and / or Dy is 0.5 mass% or less, it is easy to maintain good residual magnetic flux density.
[0030] The Cu content is 0.04% by mass or more and 0.50% by mass or less, with the total mass of R, T and B being 100% by mass. If the Cu content is less than 0.04% by mass, the coercive force HcJ tends to decrease. In addition, the improvement range ΔHcJ of the coercive force HcJ by heavy rare earth diffusion (application of the so-called grain boundary diffusion method) becomes insufficient, and the coercive force HcJ after the heavy rare earth diffusion also tends to decrease. If the Cu content exceeds 0.50% by mass, the coercive force HcJ tends to decrease, and further the residual magnetic flux density Br tends to decrease. In addition, the improvement range ΔHcJ of the coercive force HcJ by the heavy rare earth diffusion becomes saturated, and the residual magnetic flux density Br tends to decrease. In addition, the Cu content may be 0.10% by mass or more and 0.50% by mass or less, or 0.10% by mass or more and 0.30% by mass or less. By containing Cu at 0.10% by mass or more, the corrosion resistance tends to be improved.
[0031] The Ga content is 0.08% by mass or more and 0.30% by mass or less, with the total mass of R, T and B being 100% by mass. By including 0.08% by mass or more of Ga, the coercive force HcJ is sufficiently improved. If the Ga content exceeds 0.30% by mass, a subphase (for example, an RT-Ga phase) is easily generated, and the residual magnetic flux density Br decreases. The Ga content may be 0.10% by mass or more and 0.25% by mass or less.
[0032] The Co content is 0.5% by mass or more and 3.0% by mass or less, with the total mass of R, T and B being 100% by mass. The inclusion of Co improves corrosion resistance. If the Co content is less than 0.5% by mass, the corrosion resistance of the final RTB permanent magnet deteriorates. If the Co content exceeds 3.0% by mass, the effect of improving corrosion resistance reaches a plateau and the cost becomes high. The Co content may be 1.0% by mass or more and 3.0% by mass or less.
[0033] The Al content may be 0.15% by mass or more and 0.30% by mass or less, with the total mass of R, T and B being 100% by mass. By making the Al content 0.15% by mass or more, the coercive force HcJ before and after the heavy rare earth diffusion can be improved. Furthermore, the change in magnetic properties (particularly the coercive force HcJ) with respect to the change in the aging temperature and / or the heat treatment temperature after the heavy rare earth diffusion is reduced, and the variation in properties during mass production is reduced. That is, the manufacturing stability is improved. By making the Al content 0.30% by mass or less, the residual magnetic flux density Br before and after the heavy rare earth diffusion can be improved. Furthermore, the temperature change rate of the coercive force HcJ can be improved. The Al content may be 0.15% by mass or more and 0.25% by mass or less. By setting the Al content to 0.15 mass % or more and 0.25 mass % or less, the change in magnetic properties (particularly coercive force HcJ) with respect to the change in aging temperature and / or the heat treatment temperature after heavy rare earth diffusion is further reduced.
[0034] The content of Zr may be 0.10% by mass or more and 0.30% by mass or less, where the total mass of R, T and B is 100% by mass. By containing Zr, abnormal grain growth during sintering is suppressed, and the squareness ratio Hk / HcJ and magnetization rate under a low magnetic field are improved. By making the content of Zr 0.10% by mass or more, the effect of suppressing abnormal grain growth during sintering by containing Zr is increased, and the squareness ratio Hk / HcJ and magnetization rate under a low magnetic field are improved. By making the content of Zr 0.30% by mass or less, the residual magnetic flux density Br can be improved. In addition, the content of Zr may be 0.15% by mass or more and 0.30% by mass or less, or may be 0.15% by mass or more and 0.25% by mass or less. By making the content of Zr 0.15% by mass or more, the stable sintering temperature range is widened. That is, the effect of suppressing abnormal grain growth during sintering is further increased. And, the variation in characteristics is reduced, and the manufacturing stability is improved.
[0035] The RTB permanent magnet according to this embodiment may also contain Mn. When Mn is contained, the Mn content may be 0.02% by mass to 0.10% by mass, with the total mass of R, T and B being 100% by mass. When the Mn content is 0.02% by mass or more, the residual magnetic flux density Br tends to improve, and the improvement range ΔHcJ of the coercive force HcJ after the heavy rare earth element diffusion tends to improve. When the Mn content is 0.10% by mass or less, the coercive force HcJ tends to improve, and the improvement range ΔHcJ of the coercive force HcJ after the heavy rare earth element diffusion tends to improve. The Mn content may be 0.02% by mass or more and 0.06% by mass or less.
[0036] The content of B in the RTB permanent magnet according to this embodiment is 0.85% by mass or more and 0.95% by mass or less, where the total mass of R, T, and B is 100% by mass. If the content of B is less than 0.85% by mass, it is difficult to achieve high squareness. In other words, it is difficult to improve the squareness ratio Hk / HcJ. If the content of B exceeds 0.95% by mass, the squareness ratio Hk / HcJ after grain boundary diffusion decreases. The content of B may be 0.88% by mass or more and 0.94% by mass or less. By setting the content of B to 0.88% by mass or more, the residual magnetic flux density Br tends to be further improved. By setting the content of B to 0.94% by mass or less, the coercive force HcJ tends to be further improved.
[0037] Furthermore, when the total content of R element is TRE, TRE / B may be 2.2 to 2.7 in atomic ratio. It may also be 2.29 to 2.63, 2.32 to 2.63, 2.34 to 2.59, 2.34 to 2.54, or 2.36 to 2.54. When TRE / B is within the above range, the residual magnetic flux density and the coercive force HcJ are improved.
[0038] In addition, 14B / (Fe+Co) may be an atomic ratio greater than 0 and equal to or less than 1.01. When 14B / (Fe+Co) is equal to or less than 1.01, the squareness ratio after grain boundary diffusion tends to improve. 14B / (Fe+Co) may be equal to or less than 1.00.
[0039] The carbon (C) content in the RTB permanent magnet according to this embodiment may be 1100 ppm or less, 1000 ppm or less, or 900 ppm or less, relative to the total mass of the RTB permanent magnet. It may also be 600 ppm to 1100 ppm, 600 ppm to 1000 ppm, or 600 ppm to 900 ppm. By setting the carbon content to 1100 ppm or less, the coercive force HcJ before and after the heavy rare earth diffusion tends to improve. In particular, from the viewpoint of improving the coercive force HcJ after the heavy rare earth diffusion, the carbon content can be set to 900 ppm or less. Furthermore, manufacturing an RTB permanent magnet with a carbon content of less than 600 ppm places a heavy load on the process, which is a factor in increasing costs.
[0040] In particular, from the viewpoint of improving the squareness ratio after the heavy rare earth diffusion, the carbon content may be set to 800 ppm to 1100 ppm.
[0041] In the RTB permanent magnet according to this embodiment, the nitrogen (N) content may be 1000 ppm or less, 700 ppm or less, or 600 ppm or less, relative to the total mass of the RTB permanent magnet. It may also be 250 ppm to 1000 ppm, 250 ppm to 700 ppm, or 250 ppm to 600 ppm. The lower the nitrogen content, the easier it is to improve the coercive force HcJ. Furthermore, producing an RTB permanent magnet with a nitrogen content of less than 250 ppm places a heavy burden on the process, which is a factor in increasing costs.
[0042] In the RTB permanent magnet according to this embodiment, the oxygen (O) content may be 1000 ppm or less, 800 ppm or less, 700 ppm or less, or 500 ppm or less, relative to the total mass of the RTB permanent magnet. It may also be 350 ppm to 500 ppm. The lower the oxygen content, the easier it is to improve the coercive force HcJ before the heavy rare earth diffusion. Furthermore, manufacturing an RTB permanent magnet with an oxygen content of less than 350 ppm places a heavy burden on the process, which is a factor in increasing costs.
[0043] Furthermore, by reducing the oxygen content to 1000 ppm or less, 800 ppm or less, 700 ppm or less, or 500 ppm or less while setting the total content of R to 29.2 mass% or more, deformation during sintering can be suppressed and manufacturing stability can be improved.
[0044] The reason why deformation during sintering can be suppressed by reducing the oxygen content while keeping the total R content at a specified level or more is believed to be as follows. The sintering mechanism of RTB permanent magnets is liquid phase sintering, and grain boundary phase components called R-rich phases generate liquid phases during sintering, promoting densification. On the other hand, O easily reacts with the R-rich phase, and as the amount of O increases, rare earth oxide phases are formed, and the amount of R-rich phase decreases. Generally, there are very small amounts of oxidizing impurity gases in sintering furnaces. For this reason, the R-rich phase may be oxidized near the surface of the compact during the sintering process, and the amount of R-rich phase may decrease locally. In compositions with a high total R content and a low O content, the amount of R-rich phase is high, and the effect of oxidation on the shrinkage behavior during sintering is small. In compositions with a low total R content and / or a high O content, the amount of R-rich phase is low, so oxidation during the sintering process affects the shrinkage behavior during sintering. As a result, the sintered body is deformed due to partial shrinkage, i.e., changes in dimensions. Therefore, deformation during sintering can be suppressed by keeping the total R content at a specified level or more while reducing the oxygen content.
[0045] The various components contained in the RTB permanent magnet according to this embodiment can be measured by a method generally known in the art. The amounts of various elements are measured, for example, by X-ray fluorescence analysis and inductively coupled plasma emission spectrometry (ICP analysis). The oxygen content is measured, for example, by inert gas fusion-non-dispersive infrared absorption method. The carbon content is measured, for example, by combustion in an oxygen stream-infrared absorption method. The nitrogen content is measured, for example, by inert gas fusion-thermal conductivity method.
[0046] The RTB permanent magnet according to this embodiment may have any shape, such as a rectangular parallelepiped.
[0047] A method for producing an RTB permanent magnet will be described in detail below, but the method is not limited to this and other known methods may be used.
[0048] [Raw powder preparation process] The raw material powder can be prepared by a known method. In this embodiment, a one-alloy method using a single alloy will be described, but a so-called two-alloy method in which a first alloy and a second alloy having different compositions are mixed to prepare the raw material powder may also be used.
[0049] First, a raw material alloy for the RTB permanent magnet is prepared (alloy preparation step). In the alloy preparation step, raw material metals corresponding to the composition of the RTB permanent magnet according to this embodiment are melted by a known method, and then cast to produce a raw material alloy having the desired composition.
[0050] As the raw material metal, for example, rare earth metals or rare earth alloys, pure iron, ferroboron, metals such as Co and Cu, and further alloys and compounds thereof can be used. Any casting method can be used to cast the raw material alloy from the raw material metal. A strip casting method can be used to obtain an RTB permanent magnet with high magnetic properties. The obtained raw material alloy can be subjected to homogenization treatment by a known method as necessary.
[0051] After the raw alloy is prepared, it is pulverized (pulverization step). The atmosphere in each step from the pulverization step to the sintering step can have a low oxygen concentration in order to obtain high magnetic properties. For example, the oxygen concentration in each step can be 200 ppm or less. By controlling the oxygen concentration in each step, the amount of oxygen contained in the RTB permanent magnet can be controlled.
[0052] The following describes the case where the pulverization process is carried out in two stages: a coarse pulverization process in which the particles are pulverized to a particle size of several hundred μm to several mm, and a fine pulverization process in which the particles are pulverized to a particle size of approximately several μm. However, the process may be carried out in a single stage, namely, the fine pulverization process alone.
[0053] In the coarse pulverization step, the material is coarsely pulverized until the particle size is about several hundred μm to several mm. This produces a coarsely pulverized powder. The coarse pulverization may be performed by any method, and may be performed by a known method such as a method of performing hydrogen absorption pulverization or a method using a coarse pulverizer. When performing hydrogen absorption pulverization, the amount of nitrogen contained in the RTB permanent magnet can be controlled by controlling the nitrogen gas concentration in the atmosphere during the dehydrogenation process.
[0054] Next, the obtained coarsely pulverized powder is pulverized until the average particle size is about several μm (pulverization step). In this way, a finely pulverized powder (raw material powder) is obtained. The average particle size of the finely pulverized powder may be 1 μm or more and 10 μm or less, 2 μm or more and 6 μm or less, or 3 μm or more and 5 μm or less. By controlling the nitrogen gas concentration in the atmosphere during the pulverization step, the amount of nitrogen contained in the RTB permanent magnet can be controlled.
[0055] The fine grinding can be carried out by any method, for example, by using various fine grinding machines.
[0056] When the coarsely pulverized powder is pulverized, various grinding aids such as lauric acid amide and oleic acid amide can be added to obtain a finely pulverized powder with high orientation during molding. In addition, the amount of carbon contained in the RTB permanent magnet can be controlled by changing the amount of the grinding aid added.
[0057] [Molding process] In the compacting step, the finely pulverized powder is compacted into a desired shape. The compacting may be performed by any method. In this embodiment, the finely pulverized powder is filled into a die and pressurized in a magnetic field. The compact thus obtained has main phase crystals oriented in a specific direction, so that an RTB permanent magnet with a higher residual magnetic flux density can be obtained.
[0058] The pressure during molding can be 20 MPa to 300 MPa. The magnetic field applied can be 950 kA / m or more, and can be 950 kA / m to 1600 kA / m. The magnetic field applied is not limited to a static magnetic field, and can also be a pulsed magnetic field. A static magnetic field and a pulsed magnetic field can also be used in combination.
[0059] As a molding method, in addition to the dry molding in which the finely pulverized powder is molded as is as described above, wet molding in which a slurry in which the finely pulverized powder is dispersed in a solvent such as oil can also be applied.
[0060] The shape of the compact obtained by compacting the finely pulverized powder can be any shape. The density of the compact at this stage is 4.0 Mg / m 3 ~4.3Mg / m 3 It can be said that:
[0061] [Sintering process] The sintering process is a process in which the compact is sintered in a vacuum or in an inert gas atmosphere to obtain a sintered body. The sintering temperature needs to be adjusted depending on various conditions such as the composition, the crushing method, the particle size and particle size distribution, etc., but the compact is fired, for example, by heating in a vacuum or in the presence of an inert gas at 1000°C to 1200°C for 1 hour to 20 hours. This results in a high-density sintered body. In this embodiment, a minimum of 7.45 Mg / m 3 The density of the sintered body is 7.50Mg / m 3 It may be more than that.
[0062] [Aging treatment process] The aging treatment step is a step of heat treating the sintered body at a temperature lower than the sintering temperature. There is no particular restriction on whether or not aging treatment is performed, and there is also no particular restriction on the number of times aging treatment is performed, and it is performed appropriately depending on the desired magnetic properties. In addition, the grain boundary diffusion step described below may also serve as the aging treatment step. The RTB permanent magnet according to this embodiment is subjected to aging treatment twice. An embodiment in which aging treatment is performed twice will be described below.
[0063] The first aging step is called the first aging step, the second aging step is called the second aging step, the aging temperature of the first aging step is called T1, and the aging temperature of the second aging step is called T2.
[0064] There are no particular limitations on the temperature T1 and aging time in the primary aging step, but they can be 700° C. or higher and 900° C. or lower for 1 hour to 10 hours.
[0065] There are no particular limitations on the temperature T2 and the aging time in the second aging step, but they can be 450° C. or higher and 700° C. or lower for 1 hour to 10 hours.
[0066] Such an aging treatment can improve the magnetic properties, particularly the coercive force HcJ, of the finally obtained RTB permanent magnet.
[0067] Furthermore, the manufacturing stability of the RTB permanent magnet according to this embodiment can be confirmed by the magnitude of change in the magnetic properties relative to the change in the aging temperature. For example, if the change in the magnetic properties relative to the change in the aging temperature is large, the magnetic properties will change with a slight change in the aging temperature. This narrows the range of aging temperatures permitted in the aging process, and the manufacturing stability is low. Conversely, if the change in the magnetic properties relative to the change in the aging temperature is small, the magnetic properties will not change easily even if the aging temperature changes. This widens the range of aging temperatures permitted in the aging process, and the manufacturing stability is high.
[0068] The RTB permanent magnet according to this embodiment obtained in this manner has the desired characteristics. Specifically, it has high residual magnetic flux density and coercive force HcJ, and also has excellent corrosion resistance and manufacturing stability. Furthermore, when the grain boundary diffusion process described below is carried out, the decrease in residual magnetic flux density when the heavy rare earth element is diffused into the grain boundaries is small, and the increase in coercive force HcJ is large. In other words, the RTB permanent magnet according to this embodiment is a magnet suitable for grain boundary diffusion.
[0069] The RTB permanent magnet according to this embodiment obtained by the above method becomes an RTB permanent magnet product by magnetizing it.
[0070] The RTB permanent magnet according to this embodiment is suitable for use in motors, generators, and the like.
[0071] The present invention is not limited to the above-described embodiment, and various modifications can be made within the scope of the present invention.
[0072] Although an RTB permanent magnet is obtained by the above method, the manufacturing method of the RTB permanent magnet is not limited to the above method and may be changed as appropriate. For example, the RTB permanent magnet according to this embodiment may be manufactured by hot working. The method of manufacturing an RTB permanent magnet by hot working includes the following steps. (a) A melting and quenching process in which raw metal is melted and the resulting bath is quenched to obtain a thin strip. (b) A grinding process in which the ribbon is pulverized to obtain a flake-shaped raw powder. (c) Cold forming process in which the crushed raw powder is cold-formed (d) A preheating step of preheating the cold-formed body (e) A hot forming process in which the preheated cold-formed body is hot-formed. (f) A hot plastic working process in which the hot-formed body is plastically deformed into a desired shape. (g) Aging treatment process for aging RTB permanent magnets
[0073] A method for diffusing a heavy rare earth element into grain boundaries in the RTB permanent magnet according to this embodiment will be described below.
[0074] [Processing process (before grain boundary diffusion)] If necessary, a process may be included in which the RTB permanent magnet according to this embodiment is processed into a desired shape. Processing methods include, for example, shaping such as cutting and grinding, and chamfering such as barrel polishing.
[0075] [Grain boundary diffusion process] Grain boundary diffusion can be carried out by adhering a heavy rare earth metal, a compound or an alloy containing a heavy rare earth element, etc. to the surface of the RTB permanent magnet by coating or vapor deposition, etc., and then performing a heat treatment. The grain boundary diffusion of the heavy rare earth element can further improve the coercive force HcJ of the final RTB permanent magnet obtained.
[0076] The heavy rare earth element may be Dy or Tb, with Tb being preferred.
[0077] In the embodiment described below, a paint containing a heavy rare earth element is prepared and applied to the surface of an RTB permanent magnet.
[0078] The form of the paint is arbitrary. Any heavy rare earth metal, heavy rare earth compound or alloy, etc., and any solvent or dispersion medium may be used. The concentration of the heavy rare earth element in the paint is also arbitrary.
[0079] The diffusion treatment temperature in the grain boundary diffusion step according to this embodiment may be 800° C. to 950° C. The diffusion treatment time may be 1 hour to 50 hours. The grain boundary diffusion step may also serve as the above-mentioned aging treatment step.
[0080] Furthermore, after the diffusion treatment, a further heat treatment may be carried out. In this case, the heat treatment temperature may be 450°C to 600°C. The heat treatment time may be 1 hour to 10 hours. Such a heat treatment can improve the magnetic properties, particularly the coercive force HcJ, of the finally obtained RTB permanent magnet.
[0081] In addition, the manufacturing stability of the RTB permanent magnet according to this embodiment can be confirmed by the magnitude of change in the magnetic properties with respect to the change in the diffusion treatment temperature in the grain boundary diffusion step and / or the heat treatment temperature after the heavy rare earth diffusion. The diffusion treatment temperature in the heavy rare earth diffusion step will be described below, but the same applies to the heat treatment temperature after the heavy rare earth diffusion. For example, if the change in the magnetic properties with respect to the change in the diffusion treatment temperature is large, the magnetic properties will change with a slight change in the diffusion treatment temperature. This narrows the range of diffusion treatment temperatures allowed in the grain boundary diffusion step, and the manufacturing stability is low. Conversely, if the change in the magnetic properties with respect to the change in the diffusion treatment temperature is small, the magnetic properties will not change easily even if the diffusion treatment temperature changes. This widens the range of diffusion treatment temperatures allowed in the grain boundary diffusion step, and the manufacturing stability is high.
[0082] [Processing process (after grain boundary diffusion)] After the grain boundary diffusion step, the RTB permanent magnet may be subjected to various types of processing. There are no particular limitations on the type of processing to be performed. For example, shape processing such as cutting and grinding, and surface processing such as chamfering using barrel polishing may be performed. EXAMPLES
[0083] The present invention will be described below with reference to more detailed examples, but the present invention is not limited to these examples.
[0084] (Experimental Example 1) (Production of RTB sintered magnets) The raw metals prepared were Nd, Pr, electrolytic iron, and low carbon ferroboron alloy.In addition, Al, Ga, Cu, Co, Mn, and Zr were prepared either as pure metals or alloys with Fe.
[0085] Using the above-mentioned raw material metals, raw material alloys were produced by strip casting so that the final magnet composition would be the composition of each sample shown in Tables 1 and 3 described below. The contents (ppm) of C, N, and O shown in Tables 1 and 3 each represent the content relative to the total mass of the magnet. Although Fe is not shown in Table 3, the contents (mass %) of each element other than C, N, and O shown in Tables 1 and 3 are values when the total content of Nd, Pr, B, Al, Ga, Cu, Co, Mn, Zr, and Fe is taken as 100 mass %. The thickness of the raw material alloys was 0.2 mm to 0.4 mm.
[0086] Next, hydrogen gas was flowed through the raw alloy at room temperature for 1 hour to absorb hydrogen. Next, the atmosphere was switched to Ar gas, and dehydrogenation was performed at 600°C for 1 hour, and the raw alloy was hydrogen-absorbed and crushed. For sample numbers 74 to 76, the nitrogen gas concentration in the atmosphere during the dehydrogenation treatment was adjusted so that the nitrogen content was a predetermined amount. Furthermore, after cooling, the sample was sieved to obtain powder with a particle size of 425 μm or less. Note that, from hydrogen absorption and crushing to the sintering process described later, a low-oxygen atmosphere with an oxygen concentration of less than 200 ppm was always used. Note that, for sample numbers 67 to 71, the oxygen concentration in the atmosphere was adjusted so that the oxygen content was a predetermined amount.
[0087] Next, 0.1% by mass of oleic acid amide was added as a grinding aid to the raw alloy powder after hydrogen absorption crushing and sieving, and mixed in. For sample numbers 63 to 66, the amount of the grinding aid added was adjusted so that the carbon content was a predetermined amount.
[0088] Next, the mixture was pulverized in a nitrogen gas flow using a collision plate type jet mill to obtain fine powder (raw powder) having an average particle size of 3.9 μm to 4.2 μm. Samples 72 and 73 were pulverized in a mixed gas flow of Ar and nitrogen, and the nitrogen gas concentration was adjusted so that the nitrogen content was a predetermined amount. The average particle size was the average particle size D50 measured by a laser diffraction type particle size distribution analyzer.
[0089] The resulting fine powder was compacted in a magnetic field to produce a compact. The magnetic field applied was a static magnetic field of 1200 kA / m. The pressure applied during compaction was 98 MPa. The magnetic field application direction and the pressure application direction were perpendicular to each other. When the density of the compacts was measured at this point, the density of all the compacts was 4.10 Mg / m 3 ~4.25Mg / m 3 was within the range.
[0090] Next, the green body was sintered to obtain a sintered body. The optimum sintering conditions differ depending on the composition, etc., but the temperature was kept within the range of 1040°C to 1100°C for 4 hours. The sintering atmosphere was a vacuum. The sintered density was 7.45 Mg / m 3 ~7.55Mg / m 3 The magnets were then subjected to a first aging treatment at a first aging temperature T1 of 850°C for one hour in an Ar atmosphere at atmospheric pressure, and then to a second aging treatment at a second aging temperature T2 of 520°C for one hour. As a result, the RTB sintered magnets shown in Tables 1 and 3 were obtained.
[0091] The composition of the obtained RTB sintered magnets was evaluated by fluorescent X-ray analysis. B (boron) was evaluated by ICP. The oxygen content was measured by inert gas fusion - non-dispersive infrared absorption method, the carbon content by combustion in an oxygen stream - infrared absorption method, and the nitrogen content by inert gas fusion - thermal conductivity method. It was confirmed that the composition of each sample was as shown in Tables 1 and 3.
[0092] The RTB sintered magnets were also cut vertically to a size of 14 mm x 10 mm x 11 mm (the easy axis of magnetization was 11 mm), and their magnetic properties were evaluated using a BH tracer. Prior to the measurements, the magnets were magnetized using a pulsed magnetic field of 4000 kA / m.
[0093] In general, there is a trade-off between remanence and coercivity HcJ. In other words, the higher the remanence, the lower the coercivity HcJ, and vice versa. In this embodiment, a performance index PI (potential index) is set to comprehensively evaluate the remanence and coercivity HcJ. If the magnitude of the remanence measured in mT is Br (mT) and the magnitude of the coercivity measured in kA / m is HcJ (kA / m), then: PI = Br + 25 × HcJ × 4π / 2000 In this embodiment, the residual magnetic flux density and coercive force HcJ before Tb diffusion were considered to be good when PI before Tb diffusion was 1635 or more, as described later. The squareness ratio Hk / HcJ before Tb diffusion was considered to be good when it was 97% or more. In this embodiment, the squareness ratio Hk / HcJ was calculated by Hk / HcJ×100(%), where Hk (kA / m) is the magnetic field when the magnetization is 90% of Br in the second quadrant of the magnetization J-magnetic field H curve (JH demagnetization curve).
[0094] The cases where the PI before Tb diffusion was 1635 or more and the squareness ratio before Tb diffusion was 97% or more were evaluated as ◯, and the cases where either characteristic was not good were evaluated as ×.
[0095] Furthermore, a corrosion resistance test was conducted on each sample. The corrosion resistance test was conducted by a PCT test (Pressure Cooker Test) under saturated vapor pressure. Specifically, the RTB sintered magnets were placed in an environment of 2 atm and 100% RH for 1000 hours, and the mass change before and after the test was measured. The mass loss per surface area of the magnet was 3 mg / cm. 2 The corrosion resistance was judged to be good when the mass loss was 2mg / cm or less. 2 The corrosion resistance was judged to be particularly good in the following cases: Especially good corrosion resistance was marked with ⊚, good corrosion resistance was marked with ◯, and poor corrosion resistance was marked with ×. However, none of the samples that underwent the corrosion resistance test this time had poor corrosion resistance.
[0096] (Tb diffusion) Furthermore, the RTB sintered magnet obtained in the above process was processed to 14 mm × 10 mm × 4.2 mm (thickness in the easy axis direction of magnetization 4.2 mm). Then, an etching process was performed by immersing the magnet in a mixed solution of nitric acid and ethanol (100 mass % ethanol and 3 mass % nitric acid) for 3 minutes and then immersing it in ethanol for 1 minute. The etching process of immersing the magnet in the mixed solution for 3 minutes and then immersing it in ethanol for 1 minute was performed twice. Next, a slurry in which TbH2 particles (average particle size D50 = 10.0 μm) were dispersed in ethanol was applied to the entire surface of the sintered magnet after the etching process so that the mass ratio of Tb to the mass of the sintered magnet was 0.6 mass %.
[0097] After the slurry was applied and dried, a diffusion treatment was carried out at 930° C. for 18 hours while flowing Ar at atmospheric pressure (1 atm), and then a heat treatment was carried out at 520° C. for 4 hours.
[0098] After the surface of the sintered magnet after the heat treatment was scraped off by 0.1 mm per side, the magnetic properties were evaluated using a BH tracer. The magnetic properties were evaluated after magnetization using a pulse magnetic field of 4000 kA / m. Since the thickness of the sintered magnet was thin, three sheets of the sintered magnet were stacked and evaluated. In this example, the change in residual magnetic flux density due to Tb diffusion is ΔBr, and the change in coercivity due to Tb diffusion is ΔHcJ. That is, ΔBr = (Br after Tb diffusion) - (Br before Tb diffusion). Similarly, ΔHcJ = (HcJ after Tb diffusion) - (HcJ before Tb diffusion). Note that a PI of 1745 or more after Tb diffusion was considered good, and a PI of 1765 or more was considered even better. A squareness ratio of 90% or more after Tb diffusion was considered good.
[0099] The cases where the PI after Tb diffusion was 1745 or more and the squareness ratio after Tb diffusion was 90% or more were evaluated as ◯, and the cases where either characteristic was not good were evaluated as ×.
[0100] [Table 1]
[0101] [Table 2]
[0102] [Table 3]
[0103] [Table 4]
[0104] In Table 1, TRE and B were changed. Also, Nd and Pr were contained so that the mass ratio of Nd to Pr was approximately 3:1. The results are shown in Table 2. In Table 3, the contents of each component other than TRE and B were changed. Also, in sample numbers 77 to 80, the TRE was fixed and the contents of Nd and Pr were changed. The results are shown in Table 4.
[0105] As shown in Tables 1 to 4, all of the Examples had good PI, squareness ratio, and corrosion resistance before Tb diffusion. Furthermore, all of the Examples had good PI and squareness ratio after Tb diffusion. In contrast, all of the Comparative Examples had poor performance in at least one of the PI before Tb diffusion, the squareness ratio before Tb diffusion, the PI after Tb diffusion, and the squareness ratio after Tb diffusion.
[0106] Furthermore, the Tb concentration distribution was measured using an electron probe microanalyzer (EPMA) for the RTB based sintered magnets after Tb diffusion shown in Tables 1 to 4. As a result, it was confirmed that the Tb concentration distribution of the RTB based sintered magnets after Tb diffusion was a concentration distribution in which Tb concentration decreased from the outside to the inside of the RTB based sintered magnet.
Claims
1. An R-T-B system permanent magnet in which R is a rare earth element, T is an element other than rare earth elements, B, C, O and N, and B is boron, T contains at least Fe, Cu, Co, Zr and Ga; The total mass of R, T and B is 100 mass%, The total content of R is 28.0 mass% to 30.2 mass%; The Cu content is 0.04% by mass to 0.50% by mass, The Co content is 0.5 mass% to 3.0 mass%; The Zr content is 0.10 mass% to 0.30 mass%; The Ga content is 0.08% by mass to 0.30% by mass, The content of B is 0.85% by mass to 0.95% by mass, R contains at least Pr, and the Pr content is greater than 0 and less than or equal to 10.0 mass%, An RTB system permanent magnet, characterized in that the C content is 800 ppm to 1100 ppm relative to the total mass of the RTB system permanent magnet.
2. 2. The RTB system permanent sintered magnet according to claim 1, wherein the total content of R is 29.2% by mass to 30.2% by mass.
3. 3. The R-T-B system permanent magnet according to claim 1, wherein R contains at least Nd.
4. 4. The RTB system permanent magnet according to claim 1, wherein when the total content of R is TRE, the atomic ratio TRE / B is 2.2 to 2.
7.
5. 5. The RTB system permanent magnet according to claim 1, wherein 14B / (Fe+Co) is an atomic ratio greater than 0 and less than or equal to 1.
01.
6. 6. The RTB system permanent magnet according to claim 1, wherein the Zr content is 0.15% by mass to 0.30% by mass.
7. An R-T-B system permanent magnet according to any one of claims 1 to 6, wherein the Al content is 0.15 mass % to 0.25 mass %.
8. An R-T-B system permanent magnet according to claim 1, wherein the total content of Tb and Dy is 0.5 mass % or less (including 0).
Citation Information
Patent Citations
Nd-fe-b based rare earth permanent magnet material
JP2006210893A
Method for manufacturing r-t-b-based sintered magnet
JP2014160760A
R-t-b based sintered magnet
JP2017073463A
Method for producing rare earth permanent magnet material
WO2006043348A1
Method of producing r-t-b sintered magnet
WO2015030231A1