Manufacturing method for samarium-iron-nitrogen magnets
The method for manufacturing samarium-iron-nitrogen magnets with controlled oxygen content and optimized pressurization/sintering conditions addresses the issues of low strength and coercive force loss, resulting in magnets with improved workability and processing capabilities.
Patent Information
- Application Number
- JP2021055372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-03-29
AI Technical Summary
Samarium-iron-nitrogen magnets face issues with low strength and poor workability due to sintering at high temperatures, leading to decreased coercive force and difficulty in processing, and the addition of resin binders further deteriorates magnetic properties.
A manufacturing method involving the use of Sm-Fe-N magnet powder with controlled oxygen content and aspect ratio, pressurized and sintered within specific temperature and pressure ranges to minimize strain and thermal decomposition, ensuring high coercive force and workability.
The method produces samarium-iron-nitrogen magnets with enhanced strength and workability, significantly suppressing coercive force loss, allowing for effective processing such as cutting.
Smart Images

Figure 0007589402000004 
Figure 0007589402000005 
Figure 0007589402000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a samarium-iron-nitrogen based magnet. [Background technology]
[0002] Samarium-iron-nitrogen magnets have a high theoretical coercive force and are considered promising as high-performance permanent magnets.
[0003] To manufacture a samarium-iron-nitrogen magnet, a process is required to solidify the samarium-iron-nitrogen magnet powder. However, because the thermal decomposition temperature of the samarium-iron-nitrogen magnet powder is about 600°C, there is a problem that the magnetic properties deteriorate when the powder is sintered at a temperature above 600°C.
[0004] In light of this background, Patent Document 1 describes a method of compacting samarium-iron-nitrogen based magnet powder instead of sintering it, thereby producing a magnet molding. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. WO2015 / 199096 Summary of the Invention [Problem to be solved by the invention]
[0006] The magnet molding obtained by the manufacturing method described in Patent Document 1 has a problem that the particles are not sintered together, so that the strength is low and the magnet molding is difficult to process. For example, when an attempt is made to cut or change the shape of the magnet molding, the magnet molding crumbles relatively easily.
[0007] To address this issue, it is possible to add a resin binder when molding the magnet powder to increase the bonding between the magnet particles. However, when a resin binder is added to a magnet molding, there is a problem that the effective magnet volume is reduced, and the magnetic properties of the magnet are deteriorated.
[0008] The present invention has been made in view of the above background, and an object of the present invention is to provide a method for producing a samarium-iron-nitrogen based magnet that has good processability and in which the decrease in coercivity is significantly suppressed. [Means for solving the problem]
[0009] In the present invention, A method for producing a samarium-iron-nitrogen (Sm-Fe-N) based magnet, comprising the steps of: (1) A step of preparing Sm-Fe-N based magnet powder, The magnet powder has a residual oxygen content of 1 mass% or less, a cumulative distribution of particles having an aspect ratio of 1 to 2 of 90% or more, and 17 having a crystalline structure; (2) a step of pressure sintering the magnet powder, The magnet powder is heated to a maximum temperature T max and the magnet powder is heated to the maximum temperature T max and the maximum pressure is in the range of 1.0 GPa to 1.8 GPa for at least a portion of the time period in the range of the maximum temperature T max is equal to or higher than 400° C. and lower than 600° C., and the predetermined time period is in the range of 1 minute to 10 minutes; having A method is provided, wherein substantially no pressure is applied to the magnet powder when the magnet powder is below 100°C and above 600°C. Effect of the Invention
[0010] The present invention can provide a method for producing a samarium-iron-nitrogen magnet that has good processability and in which the decrease in coercivity is significantly suppressed. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a diagram showing a schematic diagram of the expected relationship between the temperature and coercivity of magnet powder when a Sm—Fe—N magnet is manufactured through a sintering process. [Diagram 2] 2 is a diagram showing an example of a flow of a method for manufacturing a magnet according to an embodiment of the present invention; FIG. [Diagram 3] FIG. 2 is a diagram showing a schematic diagram of an example of a flow of a method for producing magnet powder in a magnet production method according to an embodiment of the present invention. [Figure 4] FIG. 3 is a diagram showing a schematic example of a temperature and pressure profile that can be used in the pressure sintering step of magnet powder in the magnet manufacturing method shown in FIG. 2. [Diagram 5] 5A to 5C are diagrams illustrating an example of a flow of a method for manufacturing a magnet according to another embodiment of the present invention. [Figure 6] FIG. 6 is a diagram showing an example of a temperature and pressure profile of magnet powder that can be applied to a compacting step with application of a magnetic field in the magnet manufacturing method shown in FIG. 5. [Figure 7] 11 is a diagram showing an example of a flow of a magnet manufacturing method according to yet another embodiment of the present invention. FIG. [Figure 8] FIG. 8 is a schematic diagram showing an example of a temperature and pressure profile that can be used in the method for producing the magnet shown in FIG. 7. [Figure 9] FIG. 2 shows the temperature and pressure profiles used in the pressure sintering process in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, one embodiment of the present invention will be described.
[0013] Samarium-iron-nitrogen (Sm-Fe-N) magnet powders include TbCu7 type and Th2Zn 17 However, in this application, the samarium-iron-nitrogen (Sm-Fe-N) magnet powder is Th2Zn 17The target is Sm-Fe-N magnet powder with a TbCu7 type crystal structure. This is Th2Zn 17 This is because this type can exhibit a higher coercive force.
[0014] As mentioned above, the magnet molding obtained by the manufacturing method described in Patent Document 1 has problems in that it has low strength and is difficult to process. Furthermore, if a resin binder is added during molding of the magnet powder to address this problem, there is also a problem that the magnetic properties of the magnet are degraded.
[0015] In order to prevent the strength of the magnet molding from decreasing, it is possible to sinter the magnet powder. However, according to the inventors of the present application, as shown in Figure 1 below, in the case of Sm-Fe-N magnets, when a magnet is manufactured by sintering Sm-Fe-N magnet powder, the coercive force decreases.
[0016] Figure 1 shows a schematic diagram of the expected relationship between the temperature and coercivity of magnetic powder when an Sm-Fe-N magnet is manufactured through a sintering process. Note that it is assumed here that the magnet manufacturing method includes a step (first step) of magnetically compacting Sm-Fe-N magnetic powder, followed by a pressure sintering step (second step). The coercivity value on the vertical axis is the value at room temperature.
[0017] In the first step, a magnetic field and pressure are applied to the magnet powder to compact it. During this process, the coercive force of the powder decreases, as shown in region I in FIG.
[0018] This first step is usually carried out at a low temperature such as room temperature, and it is believed that the application of pressure causes distortion inside each particle, which reduces the coercive force of the powder.
[0019] In particular, when the particles are fine and have a shape close to a sphere (defined in the present application as particles with an aspect ratio of 1 to 2), the particles are less likely to be crushed into fine particles when pressurized, and strain is more likely to accumulate inside the particles. Therefore, in this case, it is believed that a greater decrease in coercivity may occur in region I.
[0020] Next, in the second step in which the magnet powder is pressure sintered, the coercivity of the powder is further reduced, as shown in region II in FIG.
[0021] The decrease in coercivity in this region II is believed to be due to iron oxide present on the surface of each particle.
[0022] That is, under high temperature and pressure, the oxygen contained in the iron oxide on the particle surface is separated, as shown in the following reaction formula (1), and the oxygen also combines with Sm inside the grain. 2Fe2O3+2Sm2Fe 17 N3 → 19Fe+2Sm2O3+3N2↑ (1) When such a decomposition reaction occurs, the amount of Sm-Fe-N composition contained in the magnet powder decreases, resulting in a decrease in coercive force.
[0023] However, when the iron oxide present on the surface of the particles is depleted, reaction (1) is thought to no longer occur. Therefore, the decrease in coercivity in region II is thought to eventually saturate. The occurrence of a plateau in coercivity in region II in Figure 1 is thought to be due to the above-mentioned reasons.
[0024] In addition, in FIG. 1, the subsequent decrease in coercivity in region III is due to thermal decomposition of the magnet powder.
[0025] Thus, when an Sm-Fe-N magnet is produced by sintering Sm-Fe-N magnet powder, there is a high possibility that the resulting magnet will not exhibit the desired coercive force.
[0026] In the above example, it is assumed that the magnetic field compaction process (first step) is carried out before the pressure sintering process (second step). However, in normal manufacturing processes, the first step is often omitted. However, even in such manufacturing processes, it is believed that the same behavior of change in coercivity as that shown in Figure 1 can be obtained. This is because, even if the manufacturing process does not include the first step, in the second step, pressure is applied when the magnet powder is at room temperature or a relatively low temperature.
[0027] The present inventors have conducted extensive research to address these problems, and have discovered that even when the manufacturing process for Sm-Fe-N magnets includes a sintering step, it is possible to significantly suppress the decrease in coercivity of the manufactured magnet by optimizing the pressure and temperature profiles applied to the magnet powder.
[0028] That is, in one embodiment of the present invention, A method for producing a samarium-iron-nitrogen (Sm-Fe-N) based magnet, comprising the steps of: (1) A step of preparing Sm-Fe-N based magnet powder, The magnet powder has a residual oxygen content of 1 mass% or less, a cumulative distribution of particles having an aspect ratio of 1 to 2 of 90% or more, and 17 having a crystalline structure; (2) a step of pressure sintering the magnet powder, The magnet powder is heated to a maximum temperature T max and the magnet powder is heated to the maximum temperature T max and the maximum pressure is in the range of 1.0 GPa to 1.8 GPa for at least a portion of the time period in the range of the maximum temperature T max is equal to or higher than 400° C. and lower than 600° C., and the predetermined time period is in the range of 1 minute to 10 minutes; having A method is provided, wherein substantially no pressure is applied to the magnet powder when the magnet powder is below 100°C and above 600°C.
[0029] In the manufacturing method according to one embodiment of the present invention, the magnet powder is 17 The Sm-Fe-N magnet powder having the Th2Zn type crystal structure is used. 17 The Sm-Fe-N magnet powder having the above-mentioned crystal structure can exhibit high coercive force.
[0030] The magnet powder is also characterized in that the residual oxygen content is 1 wt % or less, and the cumulative distribution of particles with an aspect ratio of 1 or more and 2 or less is 90% or more.
[0031] In the case of the manufacturing method of the present invention, residual oxygen in magnet powder tends to be present in large amounts on the surface of each particle. Furthermore, as described above, the oxygen present on the surface oxidizes Sm within the particles in the pressure sintering step (second step) of the powder according to reaction formula (1), which causes a decrease in the coercive force of the magnet.
[0032] However, in the manufacturing method according to one embodiment of the present invention, the residual oxygen content in the magnet powder is suppressed to 1 wt % or less, so that the decrease in coercivity in region II can be significantly suppressed.
[0033] Furthermore, the manufacturing method according to one embodiment of the present invention is characterized in that the cumulative distribution of particles with an aspect ratio of 1 to 2 inclusive is 90% or more in the magnet powder used. This means that the majority of the magnet particles are roughly spherical.
[0034] It is generally known that magnetic powders made up of spherical particles can have a higher coercive force than magnetic powders made up of non-spherical particles. Therefore, by using magnetic powders in which the majority of particles are roughly spherical with an aspect ratio of 1 or more and 2 or less, the coercive force can be further increased.
[0035] Moreover, the manufacturing method according to one embodiment of the present invention has a feature in that substantially no pressure is applied to the magnet powder when the magnet powder is in a temperature range below 100°C.
[0036] In this case, the distortion occurring within the particles in the above-mentioned first step is significantly suppressed, and therefore the decrease in coercivity of the magnet powder that may occur in region I can be significantly suppressed.
[0037] In the manufacturing method according to the embodiment of the present invention, the maximum pressure (maximum pressure P max ) is applied during at least a portion of the time when the magnet powder is at a maximum temperature T max The applied voltage is set to overlap with at least a portion of the period during which the magnet powder reaches a maximum temperature T max The holding time ranges from 1 to 10 minutes.
[0038] Thus, the magnet powder reaches a maximum temperature T max And maximum pressure P max By keeping the time for which the powder is held at this temperature relatively short, the reaction shown in reaction formula (1) can be significantly suppressed in region II shown in Fig. 1. As a result, the decrease in coercivity of the magnet powder that may occur in region II can be significantly suppressed.
[0039] In the manufacturing method according to an embodiment of the present invention, the pressure sintering step is performed at a maximum temperature T max is carried out in a temperature range of 400° C. or more and less than 600° C. Furthermore, the manufacturing method according to one embodiment of the present invention has a feature that substantially no pressure is applied to the magnet powder when the magnet powder is in a temperature range of 600° C. or more.
[0040] In this case, the thermal decomposition of the magnet powder can be significantly suppressed, and therefore the decrease in the coercive force of the magnet powder as shown in region III of FIG.
[0041] Due to these effects, in the manufacturing method according to one embodiment of the present invention, although the manufacturing method includes a step of pressure sintering the magnet powder, it is possible to significantly suppress a decrease in coercivity throughout the entire process.
[0042] Furthermore, in the manufacturing method according to one embodiment of the present invention, the magnet powder is sintered, and therefore the resulting magnet has good strength and good processability, unlike the magnet molding as described in the above-mentioned Patent Document 1.
[0043] As a result of the above-mentioned effects, one embodiment of the present invention can provide a method for producing a samarium-iron-nitrogen magnet that has good processability and in which the decrease in coercivity is significantly suppressed.
[0044] (Method of manufacturing a magnet according to one embodiment of the present invention) The method for producing a magnet according to one embodiment of the present invention will now be described in more detail with reference to FIG.
[0045] FIG. 2 shows an example of a flow of a method for producing a magnet according to one embodiment of the present invention (hereinafter referred to as the "first method").
[0046] As shown in FIG. 2, the first method is: A step of preparing Sm-Fe-N based magnet powder (step S110); A step of pressure sintering the magnet powder (step S120); has.
[0047] Each step will be described below.
[0048] (Step S110) First, Sm-Fe-N based magnet powder is prepared.
[0049] The magnet powder is made up of Th2Zn particles with a residual oxygen content of 1wt% or less and mostly spherical particles. 17 This is a type Sm-Fe-N magnet powder.
[0050] The method for producing the magnet powder is not particularly limited as long as such magnet powder can be obtained.
[0051] An example of a method for producing magnet powder will be described below with reference to FIG.
[0052] FIG. 3 shows a schematic flow of a method for producing Sm-Fe-N based magnetic powder.
[0053] As shown in FIG. 3, the manufacturing method of this magnet powder is as follows: A step (S10) of preparing a precursor powder of an Sm-Fe alloy; A step (S20) of reducing and diffusing the precursor powder in an inert gas atmosphere to produce a Sm-Fe based alloy powder; A step (S30) of nitriding the Sm-Fe alloy powder to produce a Sm-Fe-N alloy powder; A step (S40) of washing the Sm-Fe-N alloy powder; has.
[0054] Each step will be briefly described below.
[0055] (Process S10) First, a precursor powder of an Sm-Fe alloy is prepared.
[0056] The precursor powder may be, for example, an Sm-Fe oxide powder or an Sm-Fe hydroxide powder. Hereinafter, the Sm-Fe oxide powder and the Sm-Fe hydroxide powder are collectively referred to as Sm-Fe (hydr)oxide powder.
[0057] The precursor powder may be prepared, for example, by a coprecipitation method. In this method, a precipitant such as an alkali is first added to a solution containing a samarium salt and an iron salt to cause precipitation, and the precipitate is then collected by filtration, centrifugation, etc. Next, the precipitate is washed and dried, and then pulverized to obtain a Sm-Fe-based (hydr)oxide powder.
[0058] However, since the magnetic properties of Sm-Fe-N magnet powder deteriorate when it contains metallic iron, it is preferable to add samarium in excess of the stoichiometric ratio when producing the precursor powder.
[0059] The counter ions in the samarium salt and iron salt may be inorganic ions such as chloride ions, sulfate ions, and nitrate ions, or organic ions such as alkoxides.
[0060] As the solvent contained in the solution containing the samarium salt and the iron salt, water can be used, but an organic solvent such as ethanol can also be used.
[0061] As the alkali, hydroxides of alkali metals and alkaline earth metals, and ammonia can be used. In addition, compounds such as urea that decompose under an external action such as heat and act as a precipitant can also be used.
[0062] The obtained precursor powder may be handled in an atmosphere-tight environment such as a glove box until the Sm-Fe-N magnet powder is produced. When an inert gas atmosphere is used, the oxygen concentration is preferably 1 ppm or less.
[0063] The obtained precursor powder is preferably pre-reduced in a reducing atmosphere, which can reduce the amount of calcium used in the subsequent reduction and diffusion step (step S20) and suppress the generation of coarse Sm-Fe alloy particles.
[0064] The pre-reduction of the precursor powder may be carried out, for example, by heating the precursor powder to 400° C. or higher in a hydrogen atmosphere. The treatment temperature is preferably in the range of 500° C. to 800° C. When the pre-reduction is carried out in this temperature range, it is possible to obtain a powder of Sm-Fe alloy having a uniform particle size.
[0065] (Process S20) Next, the precursor powder is subjected to a reduction diffusion treatment under an inert gas atmosphere.
[0066] Examples of the method for reducing and diffusing the precursor powder include a method in which the precursor powder is mixed with calcium (Ca) or calcium hydride (CaH2) and then heated to a temperature equal to or higher than the melting point of Ca (approximately 850°C).
[0067] During this treatment, Sm reduced by Ca diffuses through the Ca melt and reacts with Fe to form Sm-Fe alloy powder.
[0068] There is a correlation between the temperature of the reduction diffusion treatment and the grain size of the crystals of the Sm-Fe alloy powder, and the higher the temperature of the reduction diffusion, the larger the grain size of the Sm-Fe alloy powder.
[0069] The average grain size of the crystal grains is preferably 2.0 μm or less. When the average grain size of the crystal grains is 0.0 μm or less, the coercive force of the magnet is further increased. The average grain size of the crystal grains is more preferably in the range of 0.6 μm to 2.0 μm.
[0070] In order to obtain Sm-Fe alloy powder with a uniform particle size, it is preferable to subject the precursor powder to reduction diffusion treatment in an inert gas atmosphere at 850° C. to 1050° C. for about 1 minute to 2 hours.
[0071] As the reduction and diffusion in the precursor progresses, crystallization progresses and an Sm-Fe alloy powder is formed. In the obtained Sm-Fe alloy powder, an Sm-rich phase is formed on at least a portion of the surface of each particle.
[0072] In the Sm-Fe alloy powder, the proportion of particles having an aspect ratio of 2.0 or more is preferably 10% or less, more preferably 8% or less. When the proportion of particles having an aspect ratio of 2.0 or more is 10% or less, the coercive force of the magnet powder is further increased.
[0073] The residual oxygen content in the Sm-Fe alloy powder obtained after step S20 is preferably less than 1.0 mass %. If the residual oxygen content in the Sm-Fe alloy powder is less than 1.0 mass %, the coercive force of the magnet will be further increased.
[0074] (Process S30) Next, the obtained Sm-Fe alloy powder is subjected to a nitriding treatment.
[0075] Examples of a method for nitriding the Sm-Fe alloy powder include a method of heat treating the Sm-Fe alloy powder at 300°C to 500°C in an atmosphere of ammonia, a mixed gas of ammonia and hydrogen, nitrogen, or a mixed gas of nitrogen and hydrogen.
[0076] When ammonia is used, it is possible to nitride the Sm-Fe alloy powder in a short time. However, the nitrogen content in the Sm-Fe-N magnet powder may become higher than the optimum value. In this case, it is preferable to anneal the Sm-Fe alloy powder in hydrogen after nitriding it. This allows the excess nitrogen to be expelled from the crystal lattice.
[0077] The nitriding process produces Sm-Fe-N alloy powder.
[0078] The composition of the particles contained in the Sm-Fe-N alloy powder is Sm2Fe 17 N3 is preferred.
[0079] For example, Sm-Fe alloy powder is heat-treated in an ammonia-hydrogen mixed atmosphere at 350°C to 450°C for 10 minutes to 2 hours, and then annealed in a hydrogen atmosphere at 350°C to 450°C for 30 minutes to 2 hours. This allows the nitrogen content in the Sm-Fe-N magnet powder to be optimized.
[0080] (Process S40) Next, the Sm-Fe-N alloy powder formed in step S30 is washed.
[0081] The Sm-Fe-N alloy powder formed in step S30 contains calcium compounds, and the washing process is carried out to remove such calcium compounds.
[0082] The cleaning process is carried out using a cleaning solution such as water and / or alcohol. Alternatively, the cleaning solution may be an acid such as amidosulfuric acid. Alternatively, the Sm-Fe-N alloy powder may be cleaned using water and / or alcohol, and then further cleaned using amidosulfuric acid.
[0083] The cleaning step may be carried out before the nitriding treatment.
[0084] The washed Sm-Fe-N alloy powder is then preferably dried.
[0085] The drying temperature is not particularly limited, but is preferably from room temperature to 100° C. By setting the drying temperature to 100° C. or less, oxidation of the Sm—Fe—N based alloy powder can be suppressed.
[0086] The Sm-Fe-N alloy powder may be subjected to a dehydrogenation treatment, which can remove hydrogen that has entered between the crystal lattices during the cleaning treatment.
[0087] The method of dehydrogenation is not particularly limited. For example, the dehydrogenation may be performed by heating the Sm-Fe-N alloy powder under vacuum or in an inert gas atmosphere. For example, the dehydrogenation may be performed by heat-treating the Sm-Fe-N alloy powder at 150°C to 250°C for 1 hour under a vacuum atmosphere.
[0088] By the above steps, it is possible to produce an Sm-Fe-N alloy powder. The amount of residual oxygen in the alloy powder is 1 mass % or less.
[0089] The average particle size of the resulting Sm-Fe-N alloy powder is preferably in the range of 0.6 μm to 2.0 μm.
[0090] The magnet powder may also be crushed.
[0091] It should be noted that "disintegration" is a different term from "pulverization." That is, "disintegration" refers to the separation of one or more particles from an aggregate of particles that are clumped together. On the other hand, "pulverization" refers to the division of a particle into smaller pieces.
[0092] The crushing process will be described below.
[0093] (Crushing process) The crushing process may be carried out in a wet manner.
[0094] The wet crushing is carried out by crushing the Sm-Fe-N alloy powder in an organic solvent. For the wet crushing, a ball mill, a vibration mill, a media stirring mill, a bead mill, or the like can be used.
[0095] By carrying out the crushing treatment, it is possible to obtain substantially "spherical" particles more reliably.
[0096] Through the above-described processing, in step S110, Sm-Fe-N based magnet powder with a residual oxygen content of less than 1.0 mass % is prepared.
[0097] The residual oxygen amount is preferably 0.9% by mass or less, and more preferably 0.8% by mass or less.
[0098] (Process S120) Next, the magnet powder is subjected to a pressure sintering process.
[0099] The pressure sintering process may be carried out by, for example, a discharge plasma method, a hot press method, or a current pressure sintering method. Among these, the current pressure sintering method is preferred because it can realize low heat load sintering by rapid heating and short sintering time.
[0100] In the electric current pressure sintering method, the magnet powder can be heated by passing an electric current through the magnet powder under pressure.
[0101] An example of a temperature and pressure profile that can be used in the pressure sintering process in step S120 will now be described with reference to FIG.
[0102] Figure 4 shows a schematic diagram of the changes in temperature and pressure of the magnetic powder over time during the pressure sintering process. In Figure 4, the horizontal axis represents time, the left vertical axis represents the temperature of the magnetic powder, and the right vertical axis represents the pressure applied to the magnetic powder.
[0103] As shown in FIG. 4, in this example, the temperature of the magnet powder changes over time t C After reaching 100°C at t S at maximum temperature T max Furthermore, the magnet powder is heated to a temperature of t E Up to maximum temperature T max The temperature is then lowered to room temperature. max The retention time at (t E -t S ).
[0104] Maximum temperature T max The maximum temperature T is in the range of 400°C to 600°C. max If the temperature is less than 400°C, the sintering reaction will not proceed. max When the temperature exceeds 600℃, the magnet powder begins to decompose. max It is preferable that the heating temperature is 550° C. or less.
[0105] Maximum temperature T max Retention time at (t E -t S ) is, for example, in the range of 1 minute to 10 minutes.
[0106] On the other hand, the pressure applied to the magnet powder is "substantially" 0 (zero) until time t1. Here, time t1>time t C It is.
[0107] Generally, in the pressure sintering process using an electric current pressure device, the magnet powder is preliminarily charged with a maximum of 3.5 × 10 -2In some cases, a pressure of up to 100 GPa may be applied. Such pre-pressing is performed to bring the particles of the powder to contact each other and ensure current flow. The pre-pressing has a different purpose and magnitude from the pressure used to sinter the particles in the pressure sintering process. Therefore, in this application, the pressure used in the pre-pressing is distinguished from the processing pressure applied for the actual sintering in the pressure sintering process.
[0108] In other words, in the present application, the magnet powder may be pre-pressed at a temperature of less than 100°C. In other words, it should be noted that in the present application, "the applied pressure is substantially zero" includes cases where the pressure applied to the magnet powder is completely zero, as well as cases where the magnet powder is pre-pressed. In other words, "the applied pressure is substantially zero" means that the applied pressure does not exceed the pre-pressure.
[0109] Next, between time t1 and time t2, the maximum pressure P max is applied. Maximum pressure P max is in the range of 1.0GPa to 1.8GPa.
[0110] Maximum pressure P max If the pressure is less than 1.0 GPa, it becomes difficult to sinter the magnet powder. max If the pressure exceeds 1.8 GPa, the life of the mold will be shortened.
[0111] After time t2, the pressure applied to the magnet powder is released.
[0112] In the example shown in FIG. 4, time t1>time t S In addition, time t2<time t E It is as follows.
[0113] However, at time t1 and time t S The relationship is not particularly limited, and time t1≦time t S However, time t1 ≥ time t S Similarly, it is preferable that time t2 and time t EThe relationship is not particularly limited, and time t2 ≥ time t E However, time t2≦time t E It is preferable that:
[0114] When such a temperature and pressure profile is applied to the magnet powder in step S120, it is possible to suppress the decrease in coercivity in regions I and II as shown in FIG.
[0115] In the first method, the maximum temperature T max is controlled to a range of 400°C or higher and lower than 600°C. Furthermore, in the temperature range of 600°C or higher, substantially no pressure is applied to the magnet powder. Therefore, in the first method, the decrease in coercivity due to thermal decomposition as shown in the above-mentioned region III is also significantly suppressed.
[0116] As a result, the first method makes it possible to sinter the magnet powder while suppressing to some extent the decrease in the coercive force of the magnet powder, making it possible to produce a Sm-Fe-N magnet with high coercive force.
[0117] Furthermore, the Sm-Fe-N magnet produced by the first method has high strength due to having been subjected to a sintering process, and can be adequately processed, such as by cutting.
[0118] It should be noted that in the temperature and pressure profile shown in FIG. 4, no processing pressure is applied to the magnet powder until time t1. However, this is merely an example and the magnet powder is C After this, pressure may be applied to the magnet powder. For example, in a temperature range of 100° C. or higher, a pressure of 0.1 GPa to a maximum pressure P max A pressure in the range of may be applied.
[0119] (Method of manufacturing a magnet according to another embodiment of the present invention) Next, a method for manufacturing a magnet according to another embodiment of the present invention will be described with reference to FIG.
[0120] FIG. 5 shows an example of the flow of a method for producing a magnet according to another embodiment of the present invention (hereinafter referred to as the "second method").
[0121] As shown in FIG. 5, the second method is A step of preparing Sm-Fe-N based magnet powder (step S210); A step (step S220) of applying a magnetic field to the magnet powder to mold the magnet powder into a molded body; A step of pressure sintering the obtained compact (step S230); has.
[0122] The second method is different from the first method in that it includes a magnetic field application molding step (step S220). That is, in the second method, steps S210 and S230 are the same as steps S110 and S120 in the first method, respectively.
[0123] Therefore, step S220 will be described in detail here.
[0124] (Process S220) In the second method, a magnetic field application compacting step is performed on the magnet powder produced in step S210.
[0125] The magnetic field application compaction step is carried out to form a compact in which the magnetism is oriented in a specific direction before sintering the magnet powder. When the magnetic field application compaction step is carried out, an anisotropic magnet with high magnetic properties is obtained after step S230.
[0126] FIG. 6 shows a schematic example of a temperature and pressure profile of magnet powder that can be applied in a compaction process under magnetic field application.
[0127] In FIG. 6, the horizontal axis represents time, the left vertical axis represents the temperature of the magnetic powder, and the right vertical axis represents the pressure applied to the magnetic powder.
[0128] As shown in FIG. 6, in this example, the temperature of the magnet powder changes over time t CAfter reaching 100°C at time t A The molding temperature T1 is reached at time t B The molding temperature T1 is maintained until the molding temperature T2 is reached, and then the temperature is lowered to room temperature. Therefore, the holding time at the molding temperature T1 is (t B -t A ).
[0129] On the other hand, compacting pressure P1 is applied to the magnet powder from time t3 to time t4. That is, the application time of compacting pressure P1 is (t4-t3).
[0130] Although not shown in FIG. 6, a magnetic field is applied to the magnet powder while the compacting pressure P1 is being applied to the magnet powder.
[0131] The applied magnetic field may be, for example, 10 kOe or greater.
[0132] This results in a compact whose magnetic properties are oriented in a specific direction.
[0133] 6, the molding temperature T1 is, for example, in the range of 100° C. to 400° C. The molding temperature T1 is preferably in the range of 100° C. to 200° C.
[0134] The molding pressure P1 is, for example, in the range of 0.1 GPa to 1.8 GPa. The molding pressure P1 is, for example, preferably in the range of 0.1 GPa to 1.2 GPa.
[0135] Here, the time t3 at which the application of the molding pressure P1 starts is t3≧t C Therefore, in the compaction process under magnetic field application, the decrease in coercive force as shown in region I in FIG.
[0136] In the example shown in FIG. A and t4 <t B However, this is just one example. For example, if t3≦t A and t4≧t B may be also possible.
[0137] Thereafter, in step S230, the magnet powder is pressure sintered as described in step S120 of the first method above, to produce a Sm-Fe-N based magnet.
[0138] With this second method as well, it is possible to obtain the same effects as with the first method described above.
[0139] That is, the second method makes it possible to sinter the magnet powder while suppressing a decrease in the coercive force of the magnet powder, and to produce a Sm-Fe-N magnet with high coercive force. Furthermore, since the Sm-Fe-N magnet produced by the second method has been through a sintering process, it has high strength and can be adequately processed, such as by cutting.
[0140] (Method of manufacturing a magnet according to yet another embodiment of the present invention) Next, a method for manufacturing a magnet according to yet another embodiment of the present invention will be described with reference to FIG.
[0141] FIG. 7 shows an example of the flow of a method for producing a magnet according to yet another embodiment of the present invention (hereinafter referred to as the "third method").
[0142] As shown in FIG. 7, the third method is: A step of preparing Sm-Fe-N based magnet powder (step S310); A step of forming a compact by molding the magnetic powder while applying a magnetic field to the magnetic powder, and then pressure sintering the compact (step S320); has.
[0143] The third method differs from the second method described above in that the magnetic field compaction step (step S220) and the pressure sintering step (step S230) in the second method described above are carried out continuously.
[0144] Therefore, step S320 will be described in detail here.
[0145] (Step S320) In the third method, the magnetic field compaction process and the pressure sintering process are successively performed on the magnet powder obtained in step S310. For example, the magnetic field compaction process and the pressure sintering process may be performed in the same device. In this case, the magnet can be rapidly manufactured.
[0146] FIG. 8 shows a schematic example of a temperature and pressure profile of the magnet powder that can be applied in step S320.
[0147] In FIG. 8, the horizontal axis represents time, the left vertical axis represents the temperature of the magnetic powder, and the right vertical axis represents the pressure applied to the magnetic powder.
[0148] As shown in FIG. 8, in this example, the temperature of the magnet powder changes over time t C After reaching 100°C at time t A The molding temperature T1 is reached at time t B The molding temperature T1 is maintained until the molding temperature T1 is reached. Therefore, the holding time at the molding temperature T1 is (t B -t A ).
[0149] Furthermore, the magnet powder is B ~time t S The temperature is increased for a period of time t S At the maximum temperature T max Furthermore, the magnet powder is heated to a temperature of t E Up to maximum temperature T max The temperature is then lowered to room temperature. max The retention time at (t E -t S ).
[0150] On the other hand, the pressure applied to the magnet powder is substantially zero until time t3. Here, time t3 ≥ time t C Therefore, the magnet powder is not compressed at a temperature below 100°C.
[0151] Thereafter, compacting pressure P1 is applied to the magnet powder from time t3 to time t4. Therefore, the pressurizing time by compacting pressure P1 is (t4-t3).
[0152] Although not shown in FIG. 8, a magnetic field is applied to the magnet powder while the compacting pressure P1 is being applied to the magnet powder.
[0153] This results in a compact that is magnetized in a specific direction.
[0154] Thereafter, during the period from time t4 to time t1, the pressure on the magnet powder is released.
[0155] Furthermore, between time t1 and time t2, the maximum pressure P max is applied. Maximum pressure P max As mentioned above, the pressure is in the range of 1.0 GPa to 1.8 GPa.
[0156] After time t2, the pressure applied to the magnet powder is released.
[0157] In the example of FIG. 8, time t3=time t A and time t4 = time t B In addition, time t1 = time t S and time t2 = time t E It is.
[0158] However, this is merely an example. As mentioned above, time t1 and time t E and the relationship between time t2 and time t E The relationship is not particularly limited.
[0159] Also, time t3 and time t A The relationship is not particularly limited, and time t3>time t A Even if time t3<time t A Time t4 and time t B The same applies to time t3 ≥ time t C In addition, time t4≦time t1.
[0160] 8, the molding temperature T1 is, for example, in the range of 100° C. to 400° C. The molding temperature T1 is preferably in the range of 100° C. to 200° C.
[0161] The molding pressure P1 is, for example, in the range of 0.1 GPa to 1.8 GPa. The molding pressure P1 is, for example, preferably in the range of 0.1 GPa to 1.2 GPa.
[0162] Also, the maximum temperature T max The temperature ranges from 400°C to less than 600°C. E -t S The retention time (t E -t S ) is preferably 5 minutes or less.
[0163] In the example shown in Fig. 8, substantially no pressure is applied to the magnet powder between time t4 and time t1. However, aside from this, pressure may be continuously applied to the magnet powder between time t4 and time t1.
[0164] When such a temperature and pressure profile is applied to the magnet powder, it is also possible to suppress the decrease in coercivity in regions I and II as shown in FIG.
[0165] Also in the third method, the decrease in coercivity due to thermal decomposition as shown in the above-mentioned region III is significantly suppressed.
[0166] As a result, with the third method, the magnet powder can be sintered while suppressing a decrease in the coercive force of the magnet powder, making it possible to produce a Sm-Fe-N magnet with high coercive force.
[0167] Furthermore, the Sm-Fe-N magnet produced by the third method has been sintered, and therefore has high strength and can be adequately processed, such as by cutting. EXAMPLES
[0168] Examples of the present invention will now be described below, with reference to Examples 1 to 14 which are examples, and Examples 21 to 25 which are comparative examples.
[0169] (Example 1) A sintered magnet was produced by the following method.
[0170] (Magnetic powder production) First, Sm-Fe-N based magnet powder was prepared by the following method.
[0171] (Preparation of Sm-Fe-(hydr)oxide powder) 64.64g of iron nitrate nonahydrate and 12.93g of samarium nitrate hexahydrate were dissolved in 800ml of water, and then 120ml of 2mol / L potassium hydroxide aqueous solution was dropped while stirring, and the mixture was stirred overnight at room temperature to prepare a suspension. Next, the suspension was filtered, and the residue was washed, and then dried overnight at 120°C in an air atmosphere using a hot air oven. Next, the residue was coarsely ground with a blade mill, and then finely ground in ethanol with a rotary mill using stainless steel balls. Next, the finely ground residue in ethanol was centrifuged and then vacuum dried to prepare Sm-Fe-(hydr)oxide powder.
[0172] (Pre-reduction) The Sm-Fe-(hydr)oxide powder was pre-reduced by heat treatment at 600° C. for 6 hours in a hydrogen atmosphere to produce a powder (referred to as Powder A).
[0173] (Reduction and diffusion) 5 g of Powder A and 2.5 g of calcium powder were placed in an iron crucible, and then heated at 950° C. for 1 hour for reduction and diffusion to produce a powder (referred to as Powder B).
[0174] (nitriding) Powder B was cooled to room temperature, and then heated to 380° C. in a hydrogen atmosphere. Next, Powder B was nitrided by heating to 420° C. in an atmosphere of ammonia-hydrogen mixture with a volume ratio of 1:2 and maintaining the temperature for 1 hour.
[0175] Next, the powder was annealed in a hydrogen atmosphere at 420° C. for 1 hour, and then in an argon atmosphere at 420° C. for 0.5 hour to optimize the nitrogen content in the powder. Powder C was thus obtained.
[0176] (Washing) Powder C was washed five times with pure water. The washed powder C was added to an aqueous solution of amidosulfuric acid to adjust the pH to 5, and the mixture was maintained for 15 minutes to remove calcium compounds. Powder C was then washed with pure water to remove amidosulfuric acid. Powder D was thus obtained.
[0177] (vacuum drying) The water remaining in Powder D was replaced with 2-propanol, and then the powder was vacuum dried at room temperature.
[0178] The vacuum-dried powder D was dehydrogenated under vacuum at 200° C. for 3 hours.
[0179] The steps after the pre-reduction were carried out in a glove box under an argon atmosphere without exposure to the air.
[0180] Through the above steps, Sm-Fe-N based magnet powder was obtained. The produced magnet powder is referred to as "magnet powder 1."
[0181] (Magnetic manufacturing) Next, the magnet powder 1 was pressure sintered to produce a sintered magnet by the following method.
[0182] For the pressure sintering process, an electric current sintering machine equipped with a pressure mechanism using a servo-controlled press device was used. This machine has a 5.5 mm square cylindrical die made of cemented carbide that can be pulsed. Therefore, with magnet powder 1 (0.5 g) filled in the die, electricity is passed through the die and pressure is applied to the die from above and below, allowing the magnet powder 1 to be pressure sintered.
[0183] The temperature and pressure profile used in the pressure sintering process is shown in Figure 9. In Figure 9, the horizontal axis is time, the left vertical axis is temperature, and the right vertical axis is pressure.
[0184] First, the inside of the device is evacuated to a vacuum of 10 Pa or less, and then 1.4 × 10 -2 A pre-pressure of 10 GPa was applied. Note that the pre-pressure is not included in the pressure value in FIG.
[0185] In this state, the magnet powder 1 was heated.
[0186] The temperature of the magnet powder 1 was increased in three stages. The first temperature increase stage was in the temperature range of room temperature to 250°C, and the temperature increase rate was 125°C / min. The second temperature increase stage was in the range of 250°C to (maximum temperature T max The temperature range was 100°C (−30°C) and the heating rate was 66.7°C / min. The third heating stage was (maximum temperature T max -30℃)~Maximum temperature T max The temperature range was 10° C. / min. Q =2 minutes.
[0187] Maximum temperature T max After reaching the maximum temperature T, the magnet powder 1 was held at that temperature for a predetermined time and then rapidly cooled. max The time it takes to reach S The time when the temperature started to decrease is t E Then, the maximum temperature T max The retention time at (t E -t S ).
[0188] In this example, the maximum temperature T max is 500℃, and the maximum temperature T max Retention time at (t E -t S The time t R = 5.3 minutes, and time t E =9.3 minutes.
[0189] On the other hand, the pressure is maximum pressure P max After time t2, the pressure applied to the magnet powder 1 is released. Time t2=time t E It was decided.
[0190] In Example 1, the time t1 at which the application of the maximum pressure begins is the time at which the temperature of the magnet powder 1 reaches 100° C. (i.e., t C ) where time t1 = t C = 0.8 minutes. Also, the maximum pressure P max Therefore, the maximum pressure application time (t2-t1) was 8.5 minutes.
[0191] This resulted in a sintered magnet, which is referred to as "Magnet 1."
[0192] (Example 2) A sintered magnet was produced in the same manner as in Example 1. However, in Example 2, unlike Example 1, the temperature at which maximum pressure application began (the temperature at time t1; the same applies below) was set to 400° C. Therefore, the time t1 at which maximum pressure application began was 4.25 minutes, and the application time of maximum pressure (t2-t1) was approximately 5 minutes.
[0193] The resulting sintered magnet is referred to as "Magnet 2."
[0194] (Example 3) A sintered magnet was produced in the same manner as in Example 1. However, in Example 3, unlike Example 1, the temperature at which the application of maximum pressure began was set to 500° C. Therefore, the time t1 at which the application of maximum pressure began was 8.3 minutes, and the application time (t2-t1) of maximum pressure was 1 minute.
[0195] The resulting sintered magnet is referred to as "Magnet 3."
[0196] (Example 4) A sintered magnet was produced in the same manner as in Example 1. However, in Example 4, unlike Example 1, the maximum temperature T max The temperature was set to 550°C.
[0197] Moreover, the application start temperature of the maximum pressure was set to 550° C. Therefore, the application start time t1 of the maximum pressure was 9 minutes, and the application time of the maximum pressure (t2−t1) was 1 minute.
[0198] The resulting sintered magnet is referred to as "Magnet 4."
[0199] (Example 5) A sintered magnet was produced in the same manner as in Example 3. However, in Example 5, unlike Example 3, the maximum pressure P max was set to 1.0 GPa.
[0200] The resulting sintered magnet is referred to as "Magnet 5."
[0201] (Example 6) A sintered magnet was produced in the same manner as in Example 3. However, in Example 6, unlike Example 3, the maximum pressure P max was set to 1.8 GPa.
[0202] The resulting sintered magnet is referred to as "Magnet 6."
[0203] (Example 7) A sintered magnet was produced in the same manner as in Example 3. However, in Example 7, the sintered magnet was produced using a magnet powder different from that in Example 3 (referred to as "magnet powder 2").
[0204] The magnetic powder 2 was prepared as follows.
[0205] In the process (production of magnet powder) shown in Example 1 above, the temperature of the reduction diffusion treatment of powder A was set to 900°C to produce powder B'. Thereafter, the same process as in the case of powder B was carried out to produce Sm-Fe-N magnet powder (magnet powder 2).
[0206] The resulting sintered magnet is referred to as "Magnet 7."
[0207] (Example 8) A sintered magnet was produced in the same manner as in Example 3. However, in Example 8, a magnet powder different from that in Example 3 (referred to as "magnet powder 3") was used to produce the sintered magnet.
[0208] In the process (production of magnet powder) shown in Example 1 above, the temperature of the reduction diffusion treatment of Powder A was set to 1050°C to produce Powder B″. Thereafter, the same process as in the case of Powder B was carried out to produce Sm-Fe-N magnet powder (Magnet Powder 3).
[0209] The resulting sintered magnet is referred to as "Magnet 8."
[0210] (Example 9) A sintered magnet was produced in the same manner as in Example 1. However, unlike Example 1, in Example 9, the sintered magnet was produced by the above-mentioned third method.
[0211] That is, before pressure sintering the magnet powder 1, a magnetic field compaction process was carried out in a current sintering apparatus, and then pressure sintering process was carried out in the same apparatus.
[0212] The magnetic field compaction process used the temperature and pressure profile shown in the left part of Figure 8. Specifically, magnet powder 1 was heated to a compaction temperature T1 at a temperature increase rate of 40°C / min, and then held for a predetermined time (t B -t A The molding temperature T1 was set to 100°C, and the holding time (t B -t A After that, the next pressure sintering step was carried out without lowering the temperature.
[0213] On the other hand, the pressure profile was such that molding pressure P1 was applied at time t3 in FIG. 8 and was maintained at molding pressure P1 for time (t4-t3). Then, at time t4, the pressure was released. The molding pressure P1 was 0.1 GPa, and the time (t4-t3) was 5 minutes. Note that time t3=time t A and time t4 = time t B It is.
[0214] The conditions for the pressure sintering treatment were the same as those in Example 1.
[0215] The resulting sintered magnet is referred to as "Magnet 9."
[0216] (Example 10) A sintered magnet was produced in the same manner as in Example 9. However, in Example 10, the sintered magnet was produced using magnetic field compaction conditions different from those in Example 9. Specifically, the compaction temperature T1 in the magnetic field compaction process was set to 150°C.
[0217] Therefore, in FIG. 8, at time t A =t3=3.8 minutes, time t B =t4=8.8 minutes.
[0218] The resulting sintered magnet is referred to as "magnet 10."
[0219] (Example 11) A sintered magnet was produced in the same manner as in Example 9. However, in Example 11, the sintered magnet was produced using magnetic field compaction conditions different from those in Example 9. Specifically, the compaction temperature T1 in the magnetic field compaction process was set to 200°C.
[0220] Therefore, in FIG. A =t3=5 minutes, time t B =t4=10 minutes The resulting sintered magnet is referred to as "Magnet 11."
[0221] (Example 12) A sintered magnet was produced in the same manner as in Example 3. However, in Example 12, unlike Example 3, the maximum temperature T max Retention time (t S -t E ) was set to 2 minutes. Note that the maximum pressure P max The application end time t2 is the temperature drop start time t E It was decided.
[0222] The resulting sintered magnet is referred to as "magnet 12."
[0223] (Example 13) A sintered magnet was produced in the same manner as in Example 3. However, in Example 13, unlike Example 3, the maximum temperature T max Retention time (t S -t E ) was set to 5 minutes. Note that the maximum pressure P max The application end time t2 is the temperature drop start time t E It was decided.
[0224] The resulting sintered magnet is referred to as "magnet 13."
[0225] (Example 14) A sintered magnet was produced in the same manner as in Example 3. However, in Example 14, unlike Example 3, the maximum temperature T max Retention time (t S -t E ) was set to 10 minutes. max The application end time t2 is the temperature drop start time t E It was decided.
[0226] The resulting sintered magnet is referred to as "magnet 14."
[0227] (Example 21) A sintered magnet was produced in the same manner as in Example 1. However, in Example 21, unlike Example 1, the temperature at which the application of maximum pressure began was 25°C (room temperature). Therefore, the time t1 at which the application of maximum pressure began was 0 minutes, and the application time (t2-t1) of maximum pressure was 9.3 minutes.
[0228] The resulting sintered magnet is referred to as "magnet 21."
[0229] (Example 22) A sintered magnet was produced in the same manner as in Example 21. However, in Example 22, unlike Example 21, the maximum temperature T max was set to 600°C.
[0230] The resulting sintered magnet is referred to as "magnet 22."
[0231] (Example 23) An attempt was made to produce a sintered magnet in the same manner as in Example 1. However, in Example 23, unlike Example 1, the maximum temperature T max The temperature at which the maximum pressure was applied was set to 300°C.
[0232] Therefore, the application start time of maximum pressure t1=5.3 minutes, and the application time of maximum pressure (t2-t1) is 1 minute.
[0233] When the obtained magnet (hereinafter referred to as "Magnet 23") was removed from the mold, it disintegrated upon demolding. Therefore, in Example 23, a sintered magnet was not obtained.
[0234] (Example 24) An attempt was made to produce a sintered magnet in the same manner as in Example 3. However, in Example 24, unlike Example 3, the maximum pressure P max was set to 2.5 GPa.
[0235] After the treatment, the mold was inspected and found to be damaged, so no sintered magnet was obtained.
[0236] The resulting treated body is hereinafter referred to as "magnet 24."
[0237] (Example 25) A sintered magnet was produced in the same manner as in Example 4. However, in Example 25, unlike Example 4, the maximum temperature T max Retention time (t S -t E ) was set to 20 minutes. max The application end time t2 is the temperature drop start time t E It was decided.
[0238] The resulting sintered magnet is referred to as "magnet 25."
[0239] Table 1 below shows the manufacturing conditions for each magnet.
[0240] [Table 1] (evaluation) Magnet Powders 1 to 14, as well as Magnet 21, Magnet 22 and Magnet 25, were used to carry out the following evaluations.
[0241] (Evaluation of magnetic powder properties) Using each of the magnet powders 1 to 3, the average particle size and aspect ratio were measured, the amount of residual oxygen was measured, and the coercive force was measured.
[0242] (Measuring average particle size and aspect ratio) The magnet powder and thermosetting epoxy resin were mixed and thermally cured, and then the cross section was exposed by etching using a focused ion beam (FIB) to prepare the sample.
[0243] Using a field emission scanning electron microscope (FE-SEM), the cross section of the sample was observed and over 200 randomly selected particles were outlined.
[0244] The contour lines correspond to the surfaces of particles and / or surfaces of touching particles, although touching particles can be distinguished by FE-SEM backscattered electron imaging or energy dispersive X-ray spectroscopy (EDS) mapping.
[0245] Next, the diameter of a circle having the same area as the region enclosed by the outline is defined as the particle diameter of the particle. The average particle diameter is calculated by arithmetically averaging the particle diameters of the particles.
[0246] For each particle, a rectangle was determined that circumscribed the outline and had the smallest area. The aspect ratio of each particle was calculated by dividing the length of the long side of the resulting rectangle by the length of the short side. Furthermore, the proportion of particles with an aspect ratio of 1 or more and 2 or less was evaluated.
[0247] (Measurement of residual oxygen) For each of magnet powders 1 to 3, the amount of residual oxygen was evaluated by inert gas fusion-non-dispersive infrared absorption method.
[0248] (Measurement of coercive force) After mixing the magnet powder with a thermoplastic resin, the mixture was oriented in a magnetic field of 20 kOe to prepare a sample for measuring the coercive force.
[0249] The coercive force P1 of each of the coercive force measurement samples was measured using a vibrating sample magnetometer (VSM).
[0250] The measurement temperature was 27° C., and the maximum applied magnetic field was 90 kOe.
[0251] The characteristics evaluation results obtained for each of the magnetic powders 1 to 3 are summarized in Table 2 below.
[0252] [Table 2] (Magnetic property evaluation) Magnets 1 to 14, 21, 22 and 25 were evaluated as follows.
[0253] (Measurement of coercive force) The coercive force P2 of each magnet was measured using a vibrating sample magnetometer (VSM).
[0254] The measurement temperature was 27° C., and the maximum applied magnetic field was 90 kOe.
[0255] From the obtained results, the coercive force reduction rate P was calculated using the following formula: Coercivity reduction rate P(%)=(1-(coercivity of magnet P2 / coercivity of sample for coercivity measurement P1))×100 (2) Here, the magnetic powder contained in the magnet with "coercive force P2" in the numerator on the right side of equation (2) corresponds to the magnetic powder contained in the measurement sample with "coercive force P1" in the denominator. In other words, when the coercive force measurement sample contains magnetic powder 1, equation (2) represents the reduction rate P of the coercive force of magnet 1 relative to magnetic powder 1. The same applies to other magnets.
[0256] Table 3 below shows the coercive force P2 and the coercive force reduction rate P of each magnet.
[0257] [Table 3] Table 3 shows that the coercivity reduction rate P for magnets 21, 22, and 25 is a minimum of 51% (magnet 21), and that the sintering process significantly reduces the coercivity. In contrast, the coercivity reduction rate P for magnets 1 to 14 is all 46% or less, and that the reduction in coercivity due to the sintering process is suppressed.
[0258] In this way, it was found that the coercive force reduction rate P can be significantly suppressed by optimizing the temperature and pressure profile of the magnet powder and performing pressure sintering or the like.
Claims
1. A method for producing a samarium-iron-nitrogen (Sm—Fe—N) based magnet, comprising the steps of: (1) A step of preparing Sm—Fe—N based magnet powder, The magnet powder has a residual oxygen content of 1 mass % or less, a cumulative distribution of particles having an aspect ratio of 1 to 2 of 90% or more, and 2 Zinc 17 having a crystalline structure; (2) A step of pressure sintering the magnet powder, The magnet powder is heated to a maximum temperature T max and the magnet powder is kept at the maximum temperature T max and the pressure is increased to a maximum pressure in the range of 1.0 GPa to 1.8 GPa for at least a portion of the time period in the range of the maximum temperature T max is equal to or higher than 400° C. and lower than 600° C., and the predetermined time period is in the range of 1 minute to 10 minutes; having In the steps (1) and (2), substantially no pressure is applied to the magnetic powder when the magnetic powder is at a temperature below 100° C. and at a temperature above 600° C.; Furthermore, after the step (1) and before the step (2), (3) applying a molding pressure to the magnet powder while applying a magnetic field in a temperature range of 100°C to 400°C; and when the temperature of the magnet powder is below 100° C., the molding pressure is not applied.
2. The step (1) comprises: A step of wet-grinding the magnet powder The method of claim 1 , comprising:
3. The method of claim 1 , wherein the magnetic field is 10 kOe or greater.
4. The method according to any one of claims 1 to 3, wherein in the step (3), a molding pressure in the range of 0.1 GPa to 1.8 GPa is applied.
5. The method according to claim 4, wherein the step (2) is carried out continuously after the step (3) in the same apparatus as that used in the step (3).
6. The temperature of the magnetic powder when the application of the maximum pressure to the magnetic powder starts is the maximum temperature T max The method according to any one of claims 1 to 5,
7. The temperature of the magnetic powder when the application of the maximum pressure to the magnetic powder starts is the maximum temperature T max The method according to claim 1 , wherein the concentration is less than 100 μm.
Citation Information
Patent Citations
Manufacture of magnetic anisotropy resin bonding type magnet and magnetic anisotropy resin type magnet
JP1996031677A
Magnetic anisotropic rubber coupling type magnet and its manufacturing method
JP1996181015A
Magnetic molded article
JP2001191387A
Polar anisotropic bonded magnet and manufacturing method therefor
JP2005286235A
Bond magnet
JP2010062326A