Aluminum electroplating solution, method for producing aluminum film using same, and method for producing aluminum foil
The electrolytic aluminum plating solution with optimized ratios of aluminum halide, ammonium chloride, and tetramethylammonium chloride addresses the challenges of high conductivity, efficiency, flexibility, and low melting point, enhancing production stability and cost-effectiveness.
Patent Information
- Application Number
- JP2020202372
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-17
- Filing Date
- 2020-12-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-12-07
AI Technical Summary
Existing electrolytic aluminum plating solutions face challenges in achieving high electrical conductivity, low electrolytic voltage, high electrodeposition efficiency, flexibility of the resulting film, and a low melting point, which are essential for reducing manufacturing costs and ensuring stable production in mass production equipment.
An electrolytic aluminum plating solution is formulated with a specific ratio of aluminum halide, ammonium chloride, and tetramethylammonium chloride in dialkyl sulfone, optimizing the content to achieve high electrical conductivity, electrodeposition efficiency, flexibility, and a low melting point.
The solution results in a plating solution with high electrical conductivity, high electrodeposition efficiency, flexible aluminum film, and a low melting point, reducing production costs and ensuring stable operation in mass production.
Smart Images

Figure 0007589529000001 
Figure 0007589529000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an aluminum electroplating solution for forming an aluminum coating and an aluminum electroplating technique using the same. [Background technology]
[0002] Since the electrodeposition potential of aluminum is lower than the potential for hydrogen evolution, it is difficult to electrolytically deposit aluminum from an aqueous solution. Therefore, many studies of aluminum electroplating solutions using non-aqueous solvents have been conducted.
[0003] Patent Document 1 discloses an aluminum electroplating solution that contains 1.5 to 4.0 mol of an aluminum halide per 10.0 mol of dimethyl sulfone and that contains ammonium chloride in a molar ratio of 1 / 15 to 1 / 4 relative to the aluminum halide, or contains tetraalkylammonium chloride in a molar ratio of 1 / 15 to 1 / 2, and that is capable of performing aluminum electroplating treatment stably for a long period of time and has a long life.
[0004] Patent Document 2 discloses a method for producing a high-purity aluminum foil with excellent ductility at a high film formation rate using a plating solution containing at least one nitrogen-containing compound selected from the group consisting of (1) dialkyl sulfone, (2) aluminum halide, and (3) ammonium halide, hydrogen halide salts of primary amines, hydrogen halide salts of secondary amines, hydrogen halide salts of tertiary amines, and quaternary ammonium salts represented by the general formula: R1R2R3R4N·X (R1 to R4 are the same or different alkyl groups, and X is a counter anion for the quaternary ammonium cation).
[0005] Patent Document 3 discloses a method for preparing a plating solution for aluminum electroplating that contains at least (1) a dialkyl sulfone, (2) an aluminum halide, and (3) a nitrogen-containing compound, in which the mixing ratios of the dialkyl sulfone, aluminum halide, and nitrogen-containing compound when preparing the plating solution are 10 moles of dialkyl sulfone, 3.5+n to 4.2+n moles of the aluminum halide, and n moles of the nitrogen-containing compound (wherein n is 0.001 to 2.0 moles), thereby making the melting point of the plating solution 25°C or lower, and using this plating solution that is easy to handle, a method for producing a high-purity aluminum foil that is highly ductile at a high film formation rate is disclosed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] International Publication No. 2010 / 044305 [Patent Document 2] International Publication No. 2011 / 001932 [Patent Document 3] International Publication No. 2013 / 129479 Summary of the Invention [Problem to be solved by the invention]
[0007] In order to reduce the manufacturing cost of electrolytic aluminum plating, it is important to increase the electrical conductivity of the plating solution to lower the electrolytic voltage required to produce an aluminum film, to increase the electrodeposition efficiency, which is the ratio of the actual amount of electrodeposition to the theoretical amount of electrodeposition calculated from the amount of current applied, and to produce an aluminum film (or aluminum foil) with high ductility (flexibility) to reduce quality defects. In addition, in mass production equipment, when considering the temperature drop during the infusion of the plating solution, if the melting point is high, it is possible that the solution will solidify inside the piping and cause clogging. Therefore, an aluminum electroplating solution for reducing the production costs of aluminum electroplating needs to simultaneously satisfy the following four effects: high electrical conductivity, high electrodeposition efficiency for the applied current, flexibility of the resulting aluminum coating, and a low melting point. Patent Documents 1 to 3 do not provide a means for simultaneously satisfying the four effects of obtaining a flexible aluminum coating, having high electrical conductivity, having a high electrodeposition efficiency for the applied current, and having a low melting point.
[0008] An object of the present invention is to provide a method for producing an aluminum coating that is suitable for reducing production costs, and to provide a method for producing an aluminum foil that enables mass production of aluminum foil by peeling off the aluminum coating, i.e., is suitable for reducing production costs, and to provide an aluminum electric plating solution for achieving these. [Means for solving the problem]
[0009] In the present invention, the content ratio is 3.5 mol to 4.2 mol of aluminum halide and 0.5 mol of ammonium chloride per 10 mol of dialkyl sulfone. 2 The aluminum electroplating solution is characterized by containing 0.1 mol or more and 0.5 mol or less of tetramethylammonium chloride and 0.1 mol or more and 1.5 mol or less of tetramethylammonium chloride.
[0010] moreover, In the aluminum electroplating of the present invention, it is preferable to use 0.3 mol or less of ammonium chloride per 10 mol of dialkylsulfone. Also, The present invention is a method for producing an aluminum coating, which comprises electroplating a substrate with the aluminum electroplating solution to form an aluminum coating on the substrate surface.
[0011] The present invention also provides a method for producing an aluminum foil, comprising: a first step of electroplating a substrate with the aluminum electroplating solution to form an aluminum coating on a surface of the substrate; and a second step of peeling off the aluminum coating from the substrate. Effect of the Invention
[0012] The present invention can provide a method for producing an aluminum coating suitable for reducing production costs, a method for producing an aluminum foil suitable for reducing production costs, and an aluminum electroplating solution for achieving these. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] As described in the literature, it is known that a plating solution that can be used for aluminum electroplating can be obtained by adding an aluminum halide and a nitrogen-containing compound to a dialkyl sulfone in a certain ratio. According to the research of the present inventors, it has been found that by simultaneously adding ammonium chloride and tetramethylammonium chloride to a mixture of dialkyl sulfone and aluminum halide, it is possible to simultaneously achieve the following four effects: (1) high electrical conductivity of the plating solution; (2) high electrodeposition efficiency for the applied current; (3) flexibility of the obtained aluminum coating; and (4) low melting point of the plating solution.
[0014] An embodiment of the present invention is an aluminum electroplating solution containing, as a content ratio, 3.5 mol to 4.2 mol of aluminum halide, 0.1 mol to 0.5 mol of ammonium chloride, and 0.1 mol to 1.5 mol of tetramethylammonium chloride per 10 mol of dialkyl sulfone. With this configuration, it is possible to provide an aluminum electroplating solution having high electrical conductivity and high electrodeposition efficiency relative to the applied current as an aluminum electroplating solution for forming a flexible aluminum coating. Furthermore, with the above configuration, it is possible to lower the melting point and viscosity of the plating solution, which is also useful for managing the plating solution in mass production equipment. Here, the content ratio refers to the ratio at which each compound is mixed. Dimethyl sulfone is an example of dialkyl sulfone, and aluminum chloride is an example of aluminum halide, and the molar ratio is expressed taking into account the difference in molecular weight.
[0015] The higher the electrical conductivity of the aluminum electroplating solution, the lower the electrolysis voltage required to produce an aluminum coating, making it possible to reduce the amount of power required and therefore reducing production costs. Furthermore, by lowering the electrolysis voltage required to produce an aluminum coating, the amount of Joule heat generated is reduced, making it easier to control the temperature of the solution and making it difficult for the quality of the aluminum coating to deteriorate. For this reason, the electrical conductivity of the aluminum electroplating solution is preferably 1.8 S / m or more, more preferably 2.0 S / m or more, and even more preferably 2.5 S / m or more.
[0016] When an aluminum coating is produced using an aluminum electric plating solution, the higher the electrodeposition efficiency relative to the amount of current applied, the more efficiently the aluminum coating can be produced, and the less excess power required for producing the aluminum coating can be consumed. In order to efficiently produce an aluminum coating, the electrodeposition efficiency is preferably 70% or more, more preferably 75% or more, and even more preferably 85% or more.
[0017] If the aluminum electroplating solution has a melting point of 60° C. or less, there is little risk of the plating solution cooling and solidifying in, for example, a circulation path for the aluminum electroplating solution in an aluminum coating production facility, and production stability is excellent. The melting point of the aluminum electroplating solution is preferably 60° C. or less, more preferably 55° C. or less.
[0018] The lower the viscosity of the aluminum electroplating solution, the easier it is for ions in the solution to diffuse and the more uniform the ions in the plating solution are, so that deterioration or variation in the quality of the aluminum coating is less likely to occur. The viscosity of the aluminum electroplating solution at a temperature of 110°C is preferably 20 cP or less.
[0019] The relationship between the configuration for satisfying the four effects of the present invention, (1) high electrical conductivity of the plating solution, (2) high electrodeposition efficiency for the applied current, (3) flexibility of the obtained aluminum coating, and (4) low melting point of the plating solution, will be explained below using aluminum chloride as an example of the aluminum halide.
[0020] When ammonium chloride or tetramethylammonium chloride is added to an aluminum plating solution, it is believed to dissociate in the plating solution as follows: Here, R is H or (CH3). NR4Cl → NR4 + +Cl - ...(Formula 1) In order to investigate the effect of adding ammonium chloride or tetramethylammonium chloride to an aluminum plating solution on the ion species in the solution, nuclear magnetic resonance (NMR) measurements were performed while changing the amount of each compound added to analyze the amount of ions in the solution. 27 By adding ammonium chloride or tetramethylammonium chloride to the aluminum plating solution, the Al(DR´SO2)3 in the plating solution involved in the Al electrodeposition reaction was 3+ The amount of Al(DR´SO2)3 was found to decrease. 3+ is formed from dialkyl sulfone and aluminum halide, where R' is an alkyl group such as a methyl group. This means that the chloride ion (Cl) dissociated from ammonium chloride or tetramethylammonium chloride is - ) in the plating solution, Al(DR´SO2)3 3+ is expected to change as follows: 4Cl - +Al(DR´SO2)3 3+ → AlCl4 - +3DR´SO2···(Formula 2) Therefore, it is believed that the addition of ammonium chloride or tetramethylammonium chloride changes the ion species in the plating solution as follows: 4NR4Cl+Al(DR´SO2)3 3+ +3AlCl4 - → 4NR4 + +4AlCl4 - +3DR´SO2···(Formula 3)
[0021] The electrical conductivity of the plating solution increases in proportion to the total amount of additives (ammonium chloride or tetramethylammonium chloride) added, regardless of the type of additive. Also, when the content ratio of DR'SO2 and AlCl3 is changed, the smaller the ratio of AlCl3, the higher the electrical conductivity of the plating solution. In other words, the greater the amount of free DR'SO2 in the plating solution, the higher the electrical conductivity of the plating solution. From these facts, it can be said that the electrical conductivity of the plating solution depends on the amount of free DR'SO2, NH 4+ and N(CH3) + It is considered that it depends on the amount. Furthermore, when the amount of free DR'SO2 in the plating solution estimated from Equation 3 is plotted on the horizontal axis and the electrical conductivity of the plating solution on the vertical axis for plating solutions with different content ratios of DR'SO2 and AlCl3 and different amounts of additives, the slope is larger for plating solutions with different amounts of additives (with additives) than for plating solutions with different content ratios of DR'SO2 and AlCl3 (without additives). From the difference in the magnitude of these slopes, it is considered that adding additives is more effective than adjusting the content ratio of DR'SO2 and AlCl3 to increase the electrical conductivity of the plating solution. Furthermore, the electrical conductivity of the plating solution is inversely proportional to the viscosity of the plating solution, and when the electrical conductivity of the plating solution is high, the viscosity of the plating solution tends to decrease. By decreasing the viscosity of the plating solution, ions in the solution are more easily diffused, and the uniformity of the ions in the plating solution is easily increased, so that the quality of the aluminum coating is less likely to deteriorate or vary.
[0022] The melting point of the plating solution is DR'SO2, which is the solvent of the plating solution, and Al(DR'SO2)3 3+ , AlCl4 - NH4 dissociated from ammonium chloride and tetramethylammonium chloride +or N(CH3)4 + The ratio of ammonium chloride and tetramethylammonium chloride in the plating solution changes the ratio of ammonium chloride and tetramethylammonium chloride in the plating solution, which changes the melting point of the plating solution. + or N(CH3)4 + By making the amount of added smaller than the predetermined amount, the increase in the melting point can be suppressed.
[0023] The amount of NH4Cl added determines whether a flexible aluminum plating film can be obtained. In other words, when the ratio of AlCl3 amount / NH4Cl added amount (molar ratio) is smaller than a certain value, a flexible aluminum plating film can be obtained. The reason why a flexible aluminum plating film can be obtained by adding NH4Cl is that NH4 + It is speculated that this suppresses the decomposition reaction of DR'SO2 and the incorporation of impurities into the plating film by adsorbing onto the cathode surface.
[0024] The electrodeposition efficiency of Al using a plating solution containing two types of additives, ammonium chloride and tetramethylammonium chloride, becomes high when the amount of AlCl3 / total amount added (molar ratio) is higher than a certain ratio. The reason for this is that the amount of Al(DR´SO2)3 in the plating solution is 3+ When a sufficient amount of Al(DR´SO2)3 exists, it is possible to form a large amount of Al(DR´SO2)3 near the cathode during Al deposition. 3+ This is thought to be because a sufficient amount of hydrogen is supplied, making it difficult for side reactions such as the decomposition of the solvent DR'SO2 to occur. On the other hand, in the case of a plating solution containing one type of NH4Cl, by increasing the amount of AlCl3 / amount of NH4Cl added (molar ratio) above a certain ratio, the amount of hydrogen gas generated simultaneously with the electrodeposition of Al can be reduced, and the decrease in electrodeposition efficiency can be suppressed.
[0025] For the reasons described above, by providing an aluminum electroplating solution characterized in that the amount of ammonium chloride and tetramethylammonium chloride added satisfies the following: amount of AlCl3 / total amount added (molar ratio) is from 1.8 to 21.0, and amount of AlCl3 / amount of NH4Cl added (molar ratio) is from 7.0 to 42.0; in other words, the content ratio of aluminum halide is from 3.5 mol to 4.2 mol, ammonium chloride is from 0.1 mol to 0.5 mol, and tetramethylammonium chloride is from 0.1 mol to 1.5 mol, per 10 mol of dialkylsulfone, it becomes possible to obtain a plating solution that simultaneously satisfies the following four effects: (1) the electrical conductivity of the plating solution is high, (2) the electrodeposition efficiency with respect to the applied current is high, (3) the obtained aluminum coating has flexibility, and (4) the melting point of the plating solution is low.
[0026] One embodiment of the method for producing an aluminum coating on the surface of a substrate using the aluminum electroplating solution of the present invention will be described below.
[0027] The content ratio of dialkylsulfone, aluminum halide, ammonium chloride, and tetramethylammonium chloride is preferably 3.5 to 4.2 mol of aluminum halide per 10 mol of dialkylsulfone. The content of ammonium chloride is preferably 0.1 to 0.5 mol, more preferably 0.2 to 0.3 mol. The content of tetramethylammonium chloride is preferably 0.1 to 1.5 mol, more preferably 0.3 to 1.5 mol.
[0028] If the content ratio of the aluminum halide is 3.5 mol or more per 10 mol of dialkyl sulfone, the increase in the melting point of the aluminum electroplating solution can be suppressed, and the solidification of the solution in the circulation path of the aluminum electroplating solution can be suppressed. On the other hand, if the content ratio is 4.2 mol or less, the increase in the solution resistance of the plating solution can be suppressed, and the decomposition and evaporation of the plating solution due to heat generation of the aluminum electroplating solution and the deterioration of the quality of the aluminum coating can be suppressed. Furthermore, if the content ratio of ammonium chloride is 0.1 mol or more per 10 mol of dialkyl sulfone, an aluminum coating having flexibility can be obtained. If the content ratio is 0.2 mol or more, an aluminum coating having more stable potential can be obtained, which is more preferable. On the other hand, if the content ratio is 0.5 mol or less, an increase in the amount of gas generated from the cathode surface during the production of the aluminum coating can be suppressed, and a decrease in the electrodeposition efficiency can be suppressed. If the content ratio is 0.3 mol or less, a decrease in the electrodeposition efficiency can be further suppressed, which is more preferable. Furthermore, if the content ratio of tetramethylammonium chloride is 0.1 mol or more per 10 mol of dialkyl sulfone, the effect of increasing the electrical conductivity of the aluminum electroplating solution can be obtained. If the amount is 0.3 mol or more, the electrical conductivity of the aluminum electroplating solution can be further increased, which is more preferable. If the amount is 1.5 mol or less, the amount of Al(DR´SO2)3 in the plating solution can be reduced. 3+ This can suppress the decrease in the amount of aluminum ions, which makes it difficult for black deposits (called burns) to occur due to an insufficient supply of aluminum ions to the cathode surface, and can suppress the decrease in electrodeposition efficiency.
[0029] The plating conditions are, for example, a plating solution temperature of 60°C or higher and 110°C or lower, and an applied current density of 2 A / dm 2 More than 40A / dm 2The lower limit of the plating solution temperature is determined taking into consideration the melting point and electrical conductivity of the plating solution, and is preferably 70°C or higher, and more preferably 80°C or higher. On the other hand, if the plating solution temperature is 110°C or lower, the reaction between the formed aluminum coating and the electric aluminum plating solution is suppressed, and the possibility of impurities being taken into the aluminum coating, resulting in a decrease in the purity of the aluminum, can be reduced. In addition, when the applied current density is 2 A / dm 2 If the current density is 40 A / dm or more, the decrease in the film formation efficiency can be suppressed. 2 If the content is equal to or less than this, decomposition of the plating solution can be suppressed, and the plating process can be performed stably.
[0030] An example of the material of the anode for forming the aluminum coating is aluminum. An example of the material of the substrate (cathode) is a conductive material such as a copper plate, a stainless steel plate, a titanium plate, an aluminum plate, or a nickel plate. The aluminum coating may be peeled off from the substrate, or may be manufactured and used in a state in which the substrate and the aluminum film are integrated. When the substrate and the aluminum film are used in a state in which the substrate and the aluminum film are integrated, it is preferable that the substrate and the aluminum coating are in close contact with each other. In order to make the substrate and the aluminum coating in close contact with each other, it is preferable to degrease or pickle the substrate, and remove dirt and oxide coating from the substrate surface.
[0031] Furthermore, when an aluminum foil is produced by carrying out the first step of forming an aluminum coating on a substrate surface and the second step of peeling the aluminum coating from the substrate using the aluminum electroplating solution of the present invention, it is desirable that the substrate surface be as smooth as possible by mirror polishing, etc., and that a dense oxide coating be formed on the substrate surface. The aluminum coating may be peeled off from the substrate in a batchwise manner, or the aluminum coating may be formed and peeled off continuously using a cathode drum.
[0032] Next, an embodiment of an aluminum-dissimilar metal M composite plating solution in which a dissimilar metal M different from aluminum is dissolved in an aluminum plating solution will be described. Here, the dissimilar metal M can be, for example, an element such as titanium. Here, the term composite plating solution is used to explain the plating solution as one form, but since this difference does not affect the effects of the present invention, in other places, the term aluminum plating solution is used for simplicity. For example, coatings and foils that mainly contain aluminum at a molar ratio of 50% or more are all referred to as aluminum coatings and aluminum foils, and the plating solution used in the production of these is also referred to as aluminum plating solution. The dissimilar metal M may be eluted by immersing the dissimilar metal M in the prepared aluminum plating solution, or by electrolysis using the dissimilar metal M as an anode. In either case, the use of the plating solution of the present invention makes it possible to increase the elution rate. The conditions for dissolving the different metal M into the aluminum plating solution are, for example, in the case of the electrolytic method, a plating solution temperature of 60°C or higher and 110°C or lower, a current density of 20 mA / cm 2 More than 400mA / cm 2 The temperature of the plating solution is determined taking into consideration the melting point and electrical conductivity of the plating solution, and is preferably 70°C or higher, and more preferably 80°C or higher. On the other hand, if the temperature of the plating solution is 110°C or lower, the amount of evaporation of the plating solution can be reduced, and it is more preferably 100°C or lower. In addition, when the current density is 20 mA / cm 2 If the current is 400 mA / cm or more, the amount of dissolution of the different metal M per unit time can be increased. 2 If the content is below this range, decomposition of the plating solution can be suppressed, and the dissimilar metal M can be stably eluted. The dissimilar metal M used in the anode may be a pure metal or an alloy, and a pure metal is preferable in order to suppress elution of elements other than the desired dissimilar metal M into the plating solution. Examples of the material for the cathode include conductive materials such as copper, stainless steel, titanium, aluminum, and nickel.
[0033] The above-described configuration makes it possible to provide an aluminum electroplating solution having high electrical conductivity and high electrodeposition efficiency relative to the applied current as an electroplating solution for forming a flexible composite coating of aluminum and dissimilar metal M. Furthermore, the above configuration makes it possible to lower the melting point and viscosity of the plating solution, which is also useful for managing the plating solution in mass production facilities. EXAMPLES
[0034] (Method of Preparing Aluminum Electroplating Solution) As an example of a method for preparing an aluminum electroplating solution, Example 1 is shown below. Dimethyl sulfone (DMSO2) (Kanto Chemical, special grade) was used as the dialkyl sulfone, 300g (10mol), and aluminum chloride (AlCl3) (Kanto Chemical, special grade) was used as the aluminum halide, 161g (3.8mol). Ammonium chloride (NH4Cl) (Kanto Chemical, special grade) was prepared, 3.4g (0.2mol), and tetramethylammonium chloride (TMAC) (Kanto Chemical, special grade) were prepared, 3.5g (0.1mol). While continuously supplying nitrogen, dimethyl sulfone in a beaker was heated using a rubber heater and a hot stirrer until it was completely melted. Aluminum chloride, ammonium chloride, and tetramethylammonium chloride were added to the mixture, and the mixture was heated while stirring until it was completely dissolved, obtaining an aluminum electroplating solution.
[0035] Example 2 was the same as Example 1, except that the amount of tetramethylammonium chloride was 10.5 g (0.3 mol). Example 3 was the same as Example 1, except that the amount of tetramethylammonium chloride was 17.5 g (0.5 mol). Example 4 was the same as Example 1, except that the amount of tetramethylammonium chloride was 34.9 g (1.0 mol). Example 5 was the same as Example 1, except that the amount of tetramethylammonium chloride was 52.4 g (1.5 mol). Example 6 was the same as Example 4, except that the amount of ammonium chloride was 1.7 g (0.1 mol). Example 7 was the same as Example 4, except that the amount of ammonium chloride was 8.5 g (0.5 mol). Comparative Example 1 was the same as Example 4 except that ammonium chloride was not added. Comparative Example 2 was the same as Example 1 except that tetramethylammonium chloride was not added. Comparative Example 3 was the same as Example 1 except that the amount of tetramethylammonium chloride was 69.9 g (2.0 mol). Comparative Example 4 was the same as Example 1 except that the amount of ammonium chloride was 17.1 g (1.0 mol) and tetramethylammonium chloride was not added. Comparative Example 5 was the same as Example 1 except that the amount of aluminum chloride was 127.5 g (3.0 mol) and tetramethylammonium chloride was not added. Comparative Example 6 was the same as Example 1 except that the amount of aluminum chloride was 85.0 g (2.0 mol) and tetramethylammonium chloride was not added.
[0036] (Method of producing aluminum coating) For Example 1, the prepared aluminum electroplating solution was kept at 95°C, and an aluminum plate with a purity of 99.99% was used as the anode and titanium foil as the cathode, and the plating was conducted at a current density of 80 mA / cm. 2 A direct current was applied at 400 V to obtain an aluminum coating. For Examples 2 to 7 and Comparative Examples 1 to 6, the aluminum coatings were prepared in the same manner as in Example 1.
[0037] (Electrical conductivity evaluation) The electrical conductivity of the aluminum electroplating solution was measured using an electrical conductivity meter (CM-31P, manufactured by Toa DKK) at a plating solution temperature of 100°C.
[0038] (Electrodeposition efficiency evaluation) The electrodeposition efficiency of the aluminum film was calculated by preparing an aluminum film using an aluminum electroplating solution and using the following formula: The Al atomic weight was 26.98 (g / mol) as the Al molar mass, the Faraday constant was 96500 (s A / mol), and the Al valence was 3. Electrodeposition efficiency (%) = 100 × actual deposition amount (g) / theoretical deposition amount (g) (Equation 4) Theoretical deposition amount (g) = (current (A) × time (s) × molar mass of Al (g / mol)) / (Faraday constant (s A / mol) × Al valence) (Equation 5)
[0039] (Flexibility evaluation) The flexibility of the aluminum coating was evaluated using a 180° bending test. If the aluminum coating broke when bent, it was rated as ×, if some cracks were formed, it was rated as △, and if no cracks were formed, it was rated as ◯.
[0040] (Melting Point Evaluation) The melting point of the aluminum electroplating solution was measured by heating the solution to 100°C or higher, completely melting it, allowing it to cool naturally in a glass container, and observing the temperature at which the solution started to solidify. If the solution was liquid at room temperature, it was indicated as "-".
[0041] Table 1 shows the content ratios, electrical conductivity, electrodeposition efficiency, flexibility of the resulting aluminum coating, and melting points of the plating solutions in Examples 1 to 7 and Comparative Examples 1 to 6.
[0042] [Table 1]
[0043] The results in Table 1 show that, from Examples 1 to 7, the addition of 0.1 mol or more and 0.5 mol or less of ammonium chloride and the addition of 0.1 mol or more and 1.5 mol or less of tetramethylammonium chloride simultaneously achieves the following four effects: (1) the electrical conductivity of the plating solution is high; (2) the electrodeposition efficiency for the applied current is high; (3) the obtained aluminum coating has flexibility; and (4) the melting point of the plating solution is low.
[0044] From Comparative Examples 1 and 2 and Example 6, it was found that when the amount of ammonium chloride added was 0.0 mol, the aluminum coating did not have flexibility and became brittle and easily cracked, whereas when the amount of ammonium chloride added was 0.1 mol, a flexible aluminum coating was obtained. From these results, it was found that in order to obtain a flexible aluminum coating, it is necessary to add 0.1 mol or more of ammonium chloride. It was found from Comparative Example 3 and Example 5 that the electrodeposition efficiency decreased when the amount of tetramethylammonium chloride added was 2.0 mol or more. This is thought to be because the amount of aluminum complex involved in the deposition of aluminum decreases depending on the amount of tetramethylammonium chloride or ammonium chloride added, which makes the supply of aluminum ions to the cathode surface more likely to be insufficient, making it more likely that burning will occur. It was found from Comparative Example 4 and Example 7 that when the amount of ammonium chloride added was 1.0 mol or more, a flexible aluminum coating was obtained, but the electrodeposition efficiency decreased. This is thought to be because the amount of aluminum complex decreased according to the amount added, which tended to cause a shortage of aluminum ions on the cathode surface, making it easier for burnt particles to occur, and increasing the amount of gas generated from the cathode surface during electrolysis. As seen from Comparative Examples 5 and 6, when the amount of aluminum chloride is reduced, the electrical conductivity increases, but on the other hand, the melting point of the aluminum plating solution rises to more than 60° C. This may cause problems such as the plating solution solidifying during the production of the aluminum coating.
[0045] Furthermore, a similar evaluation was performed on an aluminum-dissimilar metal M composite plating solution in which a dissimilar metal M different from aluminum was dissolved in the above aluminum plating solution. Below, an example of an aluminum-dissimilar metal M composite plating solution in which a dissimilar metal M was dissolved in an aluminum plating solution will be described. Here, an example in which titanium was used as the dissimilar metal M will be described.
[0046] For Example 8, two titanium pieces (JIS H4600 equivalent, purity 99 mass%) measuring 30 mm x 30 mm x 80 μm were immersed facing each other in an aluminum electroplating solution prepared in the same ratio as in Example 4. One of the immersed titanium pieces was used as the anode and the other as the cathode, and a current of 50 mA / cm was applied to the aluminum plating solution held at 100° C. 2 After passing a current for 23 minutes at a current density of 1000 kJ / s, the plating solution was sampled and the Ti concentration of the solution was analyzed by ICP (Hitachi High-Tech Science Corporation, SPS-3520UV).
[0047] Example 9 was carried out in the same manner as Example 8, except that the electrolysis time for dissolving Ti was 47 minutes.
[0048] Example 10 was carried out in the same manner as Example 8, except that the electrolysis time for dissolving Ti was 70 minutes.
[0049] Example 11 was carried out in the same manner as Example 8, except that the electrolysis time for dissolving Ti was 94 minutes.
[0050] Example 12 was carried out in the same manner as Example 8, except that the electrolysis time for dissolving Ti was 117 minutes.
[0051] Next, using the plating solutions of Examples 8 to 12, while maintaining the solution temperature at 95°C, a 99.99% pure aluminum plate was used as the anode and titanium foil as the cathode, and a current density of 80 mA / cm was applied. 2 A direct current was applied at 400 V to obtain a titanium-containing aluminum coating. The Al content and Ti content of the obtained titanium-containing aluminum coating were analyzed by ICP.
[0052] The electrodeposition efficiency of the titanium-containing aluminum coating was calculated using the following formula: In this calculation, the atomic weight of Ti was 47.87 (g / mol) as the molar mass of Ti, and 4 was used as the valence of Ti. Electrodeposition efficiency (%) = 100 × actual deposition amount (g) / theoretical deposition amount (g) (Equation 6) Theoretical deposition amount (g) = Theoretical deposition amount of Al (g) + Theoretical deposition amount of Ti (g) (Equation 7) Theoretical amount of Al electrodeposition (g) = (current (A) × time (s) × molar mass of Al (g / mol)) / (Faraday constant (s A / mol) × Al valence) × (Al content of coating (at%) / 100) (Equation 8) Theoretical amount of Ti electrodeposition (g) = (current (A) × time (s) × Ti molar mass (g / mol)) / (Faraday constant (s A / mol) × Ti valence) × (Ti content of film (at%) / 100) (Equation 9)
[0053] Table 2 shows the content ratio and Ti concentration of the plating solution in Examples 8 to 12, the electrical conductivity, the electrodeposition efficiency, the flexibility of the obtained aluminum coating, and the melting point of the plating solution.
[0054] [Table 2]
[0055] The results in Table 2 show that, in Examples 8 to 12, even when a dissimilar metal M was dissolved into an aluminum electroplating solution to which 0.1 mol or more and 0.5 mol or less of ammonium chloride and 0.1 mol or more and 1.5 mol or less of tetramethylammonium chloride were added, the following four effects were simultaneously satisfied: (1) the electrical conductivity of the plating solution was high; (2) the electrodeposition efficiency for the applied current was high; (3) the obtained aluminum coating had flexibility; and (4) the melting point of the plating solution was low. Therefore, even in an aluminum electroplating solution from which the dissimilar metal M has been eluted, so long as the aluminum electroplating solution contains, in terms of content ratios, 3.5 mol or more and 4.2 mol or less of aluminum halide, 0.1 mol or more and 0.5 mol or less of ammonium chloride, and 0.1 mol or more and 1.5 mol or less of tetramethylammonium chloride per 10 mol of dialkyl sulfone, it is possible to obtain an aluminum electroplating solution that can realize the production of an aluminum coating that is suitable for reducing production costs and the production of an aluminum foil that is suitable for reducing production costs.
Claims
1. The content ratio is as follows: For 10 mol of dialkyl sulfone, 3.5 mol or more and 4.2 mol or less of aluminum halide; Ammonium chloride in an amount of 0.2 mol or more and 0.5 mol or less; and 0.1 mol or more and 1.5 mol or less of tetramethylammonium chloride, 1. An aluminum electroplating solution comprising:
2. The electro-aluminum plating solution according to claim 1, characterized in that the amount of ammonium chloride per 10 mol of dialkyl sulfone is 0.3 mol or less.
3. 3. A method for producing an aluminum electroplating solution comprising the steps of: electroplating a substrate using the aluminum electroplating solution according to claim 1; A method for producing an aluminum coating, which forms an aluminum coating on a substrate surface.
4. 3. A method for producing an aluminum electroplating solution comprising the steps of: electroplating a substrate using the aluminum electroplating solution according to claim 1; A first step of forming an aluminum coating on a surface of a substrate; a second step of stripping the aluminum coating from the substrate; A method for producing an aluminum foil having the above structure.
Citation Information
Patent Citations
Aluminum foil
JP2019137902A
Electrolytic aluminum plating solution and method for forming aluminum plating film
WO2010044305A1
Method for manufacturing aluminum foil
WO2011001932A1
Method for preparing low-melting-point plating solution for electrical aluminum plating, plating solution for electrical aluminum plating, method for producing aluminum foil, and method for lowering melting point of plating solution for electrical aluminum plating
WO2013129479A1