Bonding Sheet
The copper-based bonding sheet with a specific solvent and protective film addresses oxidation issues, forming a dense, void-free bonding layer for strong electronic component bonding.
Patent Information
- Application Number
- JP2021011374
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-01-27
AI Technical Summary
Silver-based bonding materials face issues with ion migration and sulfidation, while copper-based materials are prone to oxidation, leading to sintering difficulties and potential short circuits in electronic components with narrow pitches and thin wiring patterns.
A bonding sheet composed of copper particles and a solvent with a boiling point of 150°C or higher, a 99:1 to 90:10 mass ratio, and a BET diameter of 40 nm to 750 nm, coated with an organic protective film, forms a dense bonding layer with reduced oxidation and voids.
The bonding sheet provides high-strength bonding with fewer voids and improved sinterability, ensuring stable bonding of electronic components.
Smart Images

Figure 0007589567000003 
Figure 0007589567000004 
Figure 0007589567000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a bonding sheet. [Background technology]
[0002] When assembling or mounting electronic components, a bonding material is generally used to bond two or more components. A known bonding material is a paste-like bonding material in which metal particles are dispersed in a solvent. When bonding components using a paste-like bonding material, the bonding material is applied to the surface of one component, the other component is brought into contact with the applied surface, and the bonding material is heated in this state to sinter the metal particles and form a bonding layer, thereby bonding the components. Patent Document 1 describes a silver particle paste.
[0003] Also, a sheet-shaped bonding material in which metal particles are partially sintered is known as a bonding material. When bonding parts using a sheet-shaped bonding material, the bonding material is placed between the parts and heated in this state to sinter the unsintered parts of the metal particles to form a bonding layer, thereby bonding the parts. Compared to a paste-shaped bonding material, a sheet-shaped bonding material is advantageous in that the solvent does not volatilize when heated, making it difficult for voids (air bubbles) to form in the bonding layer. Patent Document 2 describes a sheet-shaped bonding material in which silver particles are sintered. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6428339 [Patent Document 2] Patent No. 6245933 Summary of the Invention [Problem to be solved by the invention]
[0005] Silver is useful as a material for bonding materials for electronic components and the like because of its excellent electrical conductivity and thermal conductivity. However, silver has a problem in that ion migration and sulfurization are likely to occur. In particular, due to the recent narrowing of pitches of electronic components and the thinning of wiring patterns, when ion migration and sulfurization occur in the bonding layer, short circuits are likely to occur between the pitches of electronic components and between wiring patterns. For this reason, it is considered to use copper as a material for the bonding material. In addition, copper is cheaper than silver and is useful for reducing the manufacturing costs of electronic components. However, copper is more easily oxidized than silver. For this reason, there is a problem that a bonding sheet in which copper particles are sintered is prone to sintering due to the oxidation of the copper particles.
[0006] This invention has been made in consideration of the above-mentioned circumstances, and aims to provide a bonding sheet using copper particles, which is less susceptible to a decrease in sinterability due to oxidation of the copper particles, can form a dense bonding layer with few voids, and can bond electronic components, etc. with high strength. [Means for solving the problem]
[0007] In order to solve the above problems, the bonding sheet of the present invention contains copper particles and a solvent having a boiling point of 150°C or higher, the content ratio of the copper particles to the solvent is 99:1 to 90:10 by mass, the BET diameter of the copper particles is in the range of 40 nm or more and 750 nm or less, and the molecular weight of the solvent is 1000 or less.
[0008] The bonding sheet of the present invention contains copper particles and a solvent, and the copper particles are covered with the solvent, so that the copper particles are not easily oxidized. In addition, the solvent has a boiling point of 150°C or more, so that it is not easily volatilized. Therefore, the bonding sheet of the present invention is less likely to suffer from a decrease in sinterability due to oxidation of the copper particles, and has improved shape stability. Furthermore, the copper particles are fine, with a BET diameter in the range of 40 nm to 750 nm, so that the sinterability is high, and the content ratio of the copper particles to the solvent is in the range of 99:1 to 90:10 in mass ratio, and the content of the copper particles is 90 mass% or more, so that a dense sintered body (bonding layer) of the copper particles can be formed by heating. In addition, since the content of the solvent is 10 mass% or less, the amount of volatilized gas and decomposition gas of the solvent generated during heating is small. In addition, by setting the molecular weight of the solvent to 1000 or less, it is possible to suppress the solvent from remaining after heating. Therefore, according to the bonding sheet of the present invention, a dense bonding layer with few voids can be formed, and electronic components and the like can be bonded with high strength.
[0009] In addition, in the bonding sheet of the present invention, the molecular weight of the solvent is preferably from 200 to 600. When the molecular weight of the solvent is in this range, the solvent can be more appropriately prevented from remaining after heating.
[0010] In addition, the bonding sheet of the present invention preferably contains at least one of a diol compound and a triol compound as a solvent. In this case, the diol compound and the triol compound have high adhesion to the copper particles, so that they are unlikely to volatilize for a long period of time. Therefore, the deterioration of sinterability due to oxidation of the copper particles can be suppressed for a long period of time, and the shape stability of the bonding sheet is improved for a long period of time.
[0011] In the bonding sheet of the present invention, the copper particles are preferably coated with an organic protective film on the surface thereof, which can suppress oxidation of the copper particles.
[0012] Here, in the bonding sheet of the present invention, the surface of the copper particle is detected by analyzing by time-of-flight secondary ion mass spectrometry.+ C3H3O3 vs. ion detection amount - It is preferable that the ratio of the detected amounts of ions is 0.001 or more. Cu on the surface of copper particles + C3H3O3 vs. ion detection amount - When the ratio of the detected amounts of ions is 0.001 or more, the surfaces of the copper particles are appropriately covered with an organic protective film, and oxidation of the copper particles can be more effectively suppressed. Effect of the Invention
[0013] According to the present invention, it is possible to provide a bonding sheet using copper particles, which is less susceptible to a decrease in sinterability due to oxidation of the copper particles, can form a dense bonding layer with few voids, and can bond electronic components, etc. with high strength. [Brief description of the drawings]
[0014] [Figure 1] FIG. 2 is a schematic cross-sectional view of a bonding sheet according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a flow diagram showing a method for producing a bonding sheet according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view of a bonded body produced using the bonding sheet according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, a bonding sheet according to one embodiment of the present invention will be described with reference to the attached drawings. The bonding sheet of this embodiment is used as a bonding material for forming a bonded body in which the substrate and the electronic component are bonded via a bonding layer, for example, by placing it between a substrate and an electronic component and heating it in this state to sinter the copper particles and form a bonding layer.
[0016] FIG. 1 is a schematic cross-sectional view of a bonding sheet according to one embodiment of the present invention. 1, the bonding sheet 1 contains copper particles 2 and a solvent 3. The ratio of the copper particles 2 to the solvent 3 is 99:1 to 90:10 (=copper particles:solvent) in terms of mass ratio. That is, the bonding sheet 1 has a copper particle 2 content in the range of 90 mass % to 99 mass % and a solvent 3 content in the range of 1 mass % to 10 mass %.
[0017] The bonding sheet 1 preferably has a density in the range of 50% to 90%. The density is the proportion of the copper particles 2 spatially occupying the bonding sheet 1. When the density is 60% or more, the adhesion between the copper particles 2 is high, so that it is easier to form a dense bonding layer with few voids. When the density is 90% or less, the surface of the copper particles 2 can be covered with the solvent 3, so that oxidation of the copper particles 2 is less likely to occur, and the decrease in sinterability due to oxidation of the copper particles can be more suppressed. The density is more preferably in the range of 55% to 75%, and particularly preferably in the range of 60% to 70%. The density of the bonding sheet 1 can be calculated by observing the cross section of the bonding sheet 1 with a SEM (scanning electron microscope), binarizing the obtained SEM image, and dividing it into the part of the copper particles 2 and the space part containing the solvent 3. Specifically, it can be calculated by the method described in the examples described later.
[0018] There is no particular limitation on the shape or size of the bonding sheet 1. The bonding sheet 1 may be, for example, a circular sheet with a diameter of 1 mm to 50 mm, or a rectangular sheet with one side of 1 mm to 50 mm. There is no particular limitation on the thickness of the bonding sheet 1, but it is preferably in the range of 50 μm to 1000 μm.
[0019] The copper particles 2 have a BET diameter in the range of 40 nm to 750 nm. The BET diameter is a particle diameter calculated from the BET specific surface area and true density of the copper particles obtained by the BET method, assuming that the copper particles 2 are true spheres or cubes. Specifically, it can be obtained by the method described in the examples below.
[0020] When the BET diameter of the copper particles 2 is 40 nm or more, it is difficult to form strong aggregates. Therefore, the surface of the copper particles 2 can be uniformly coated with the solvent 3. On the other hand, when the BET diameter of the copper particles 2 is 750 nm or less, the reaction area is large and the sintering property by heating is high, so that a strong bonding layer can be formed. The BET diameter of the copper particles 2 is preferably 50 nm or more and 750 nm or less, more preferably 50 nm or more and 300 nm or less, more preferably 80 nm or more and 200 nm or less, and particularly preferably 80 nm or more and 170 nm or less.
[0021] The BET specific surface area of copper particle 2 is 2.0 m 2 / g or more 8.0m 2 / g or less, and 3.5m 2 / g or more 8.0m 2 / g or less, and more preferably 4.0m 2 / g or more 8.0m 2 / g or less. The shape of the copper particles 2 is not limited to a spherical shape, and may be a needle shape or a flat plate shape.
[0022] The surfaces of the copper particles 2 are preferably coated with an organic protective film, which is a film of an organic material. By being coated with the organic protective film, oxidation of the copper particles 2 is suppressed, and a decrease in sinterability due to oxidation of the copper particles 2 is further unlikely to occur. It can be said that the organic protective film coating the copper particles 2 is not formed by the solvent 3, and is not derived from the solvent 3. It can also be said that the organic protective film coating the copper particles 2 is not a copper oxide film formed by the oxidation of copper.
[0023] The fact that the copper particles 2 are coated with an organic protective film can be confirmed by analyzing the surface of the copper particles 2 using time-of-flight secondary ion mass spectrometry (TOF-SIMS). Therefore, in this embodiment, the copper particles 2 are coated with an organic protective film, and the organic protective film is detected by analyzing the surface of the copper particles 2 using time-of-flight secondary ion mass spectrometry. + C3H3O3 vs. ion detection amount - Ratio of detected ions (C3H3O3 - / Cu + It is preferable that the ratio is 0.001 or more. C3H3O3 - / Cu + The ratio is more preferably in the range of 0.05 to 0.2. Note that the surface of the copper particles 2 in this analysis does not refer to the surface of the copper particles 2 when the organic protective film is removed from the copper particles 2, but refers to the surface of the copper particles 2 including the covering organic protective film (i.e., the surface of the organic protective film).
[0024] The copper particles 2 were analyzed by time-of-flight secondary ion mass spectrometry to determine that the surface of the particles was C3H4O2 - Cu ions and ions of C5 or higher may be detected. + C3H4O2 vs. ion detection amount - Ratio of detected ions (C3H4O2 - / Cu + The ratio is preferably 0.001 or more. + The ratio of the amount of ions detected that are C5 or more to the amount of ions detected (C5 or more ions / Cu + It is preferable that the ratio is less than 0.005.
[0025] C3H3O3 detected by time-of-flight secondary ion mass spectrometry - Ions and C3H4O2 - The ions and C5 and higher ions originate from the organic protective film that covers the surface of copper particle 2. Therefore, C3H3O3 - / Cu + Ratio and C3H4O2 - / Cu + When each of the ratios is 0.001 or more, the surface of the copper particles 2 is less likely to be oxidized, and the copper particles 2 are less likely to aggregate. - / Cu + Ratio and C3H4O2 - / Cu +When the ratio is 0.2 or less, the oxidation and aggregation of the copper particles 2 can be suppressed without excessively decreasing the sinterability of the copper particles 2, and further, the generation of decomposition gas of the organic protective film during heating can be suppressed, so that a bonding layer with fewer voids can be formed. - / Cu + Ratio and C3H4O2 - / Cu + The ratio is preferably in the range of 0.08 to 0.16. + If the ratio is 0.005 or more, the particle surface will have a large amount of organic protective film with a relatively high desorption temperature, resulting in insufficient sintering and making it difficult to obtain a strong bonding layer. + Preferably, the ratio is less than 0.003.
[0026] The organic protective film is preferably derived from citric acid. A method for producing copper particles 2 coated with an organic protective film derived from citric acid will be described later. The amount of the organic protective film on the copper particles 2 is preferably in the range of 0.5% by mass to 2.0% by mass, more preferably in the range of 0.8% by mass to 1.8% by mass, and even more preferably in the range of 0.8% by mass to 1.5% by mass, relative to 100% by mass of the copper particles. When the amount of the organic protective film is 0.5% by mass or more, the copper particles 2 can be uniformly coated with the organic protective film, and the oxidation of the copper particles 2 can be more reliably suppressed. In addition, when the amount of the organic protective film is 2.0% by mass or less, it is possible to suppress the generation of voids in the sintered body (bonding layer) of the copper particles due to gas generated by decomposition of the organic protective film by heating. The amount of the organic protective film can be measured using a commercially available device. Specifically, it can be measured by the method described in the examples described later.
[0027] It is preferable that 50% by mass or more of the organic protective film of the copper particles 2 decomposes when heated for 30 minutes at a temperature of 300° C. in an inert gas atmosphere such as argon gas. The organic protective film derived from citric acid generates carbon dioxide gas, nitrogen gas, evaporated acetone gas, and water vapor during decomposition.
[0028] Copper particles 2 coated with an organic protective film derived from citric acid can be produced, for example, as follows. First, an aqueous dispersion of copper citrate is prepared, and a pH adjuster is added to the aqueous dispersion of copper citrate to adjust the pH to 2.0 or more and 7.5 or less. Next, in an inert gas atmosphere, a hydrazine compound capable of reducing copper ions is added as a reducing agent to the aqueous dispersion of copper citrate having the pH adjusted thereto, and mixed in an amount of 1.0 to 1.2 times the equivalent. The resulting mixture is heated to a temperature of 60° C. to 80° C. in an inert gas atmosphere and held for 1.5 to 2.5 hours. As a result, the copper ions eluted from the copper citrate are reduced to produce copper particles 2, and an organic protective film derived from citric acid is formed on the surface of the copper particles 2.
[0029] The aqueous dispersion of copper citrate can be prepared by adding powdered copper citrate to pure water such as distilled water or ion-exchanged water to a concentration of 25% by mass or more and 40% by mass or less, and stirring with a stirring blade to uniformly disperse the copper citrate. Examples of pH adjusters include triammonium citrate, ammonium hydrogen citrate, and citric acid. Among these, triammonium citrate is preferred because it is easy to adjust the pH to a mild level. The reason why the pH of the aqueous dispersion of copper citrate is set to 2.0 or more is to increase the elution rate of copper ions eluted from copper citrate, to rapidly advance the generation of copper particles, and to obtain the target fine copper particles 2. The reason why the pH is set to 7.5 or less is to prevent the eluted copper ions from becoming copper hydroxide (II) and to increase the yield of the copper particles 2. The reason why the pH is set to 7.5 or less is to prevent the reducing power of the hydrazine compound from becoming excessively high, and the target copper particles 2 can be easily obtained. The pH of the aqueous dispersion of copper citrate is preferably adjusted to a range of 4 to 6.
[0030] The reduction of copper citrate with a hydrazine compound is carried out under an inert gas atmosphere. This is to prevent oxidation of copper ions dissolved in the liquid. Examples of inert gases include nitrogen gas and argon gas. When reducing copper citrate under acidic conditions, hydrazine compounds have the advantages of not producing residues after the reduction reaction, being relatively safe, and being easy to handle. Examples of this hydrazine compound include hydrazine monohydrate, anhydrous hydrazine, hydrazine hydrochloride, and hydrazine sulfate. Among these hydrazine compounds, hydrazine monohydrate and anhydrous hydrazine are preferred because they do not contain components that can become impurities such as sulfur and chlorine.
[0031] Generally, copper generated in an acidic solution having a pH of less than 7 dissolves. However, in this embodiment, a hydrazine compound, which is a reducing agent, is added and mixed with an acidic solution having a pH of less than 7, and copper particles 2 are generated in the resulting mixed solution. As a result, components derived from citric acid generated from copper citrate quickly cover the surfaces of the copper particles 2, suppressing dissolution of the copper particles 2. It is preferable to set the temperature of the aqueous dispersion of copper citrate after adjusting the pH to 50° C. or more and 70° C. or less to facilitate the progress of the reduction reaction.
[0032] The mixed solution containing the hydrazine compound is heated to a temperature of 60° C. or more and 80° C. or less under an inert gas atmosphere and held for 1.5 hours or more and 2.5 hours or less in order to generate copper particles 2 and to form and coat the surfaces of the generated copper particles 2 with an organic protective film. The reason for holding the mixture under heating under an inert gas atmosphere is to prevent oxidation of the generated copper particles 2. Copper citrate, which is the starting material, usually contains about 35% by mass of copper components. By adding a hydrazine compound, which is a reducing agent, to a copper citrate aqueous dispersion containing this amount of copper components, heating it to the above temperature, and holding it for the above time, the generation of the copper particles 2 and the generation of the organic protective film on the surfaces of the copper particles 2 proceed in a well-balanced manner, and it is possible to obtain copper particles 2 in which the amount of the organic protective film covering the copper particles 2 is in the range of 0.5% by mass to 2.0% by mass relative to 100% by mass of the copper particles. If the heating temperature is less than 60°C and the holding time is less than 1.5 hours, the copper citrate may not be completely reduced, the production rate of the copper particles 2 may become too slow, and the amount of the organic protective film covering the copper particles 2 may become excessive. If the heating temperature exceeds 80°C and the holding time exceeds 2.5 hours, the production rate of the copper particles 2 may become too fast, and the amount of the organic protective film covering the copper particles 2 may become too small. The preferred heating temperature is 65°C or higher and 75°C or lower, and the preferred holding time is 2 hours or higher and 2.5 hours or lower.
[0033] The copper particles 2 produced in the mixed solution are subjected to solid-liquid separation from the mixed solution under an inert gas atmosphere, for example, using a centrifuge, and then dried by freeze-drying or vacuum drying to obtain copper particles 2 whose surfaces are coated with an organic protective film. Since the copper particles 2 have their surfaces coated with an organic protective film, they are less likely to oxidize even if stored in the air until they are used as a bonding sheet.
[0034] The solvent 3 acts as a binder for the copper particles 2. In addition, the solvent 3 acts as an antioxidant that coats the copper particles 2 to prevent the copper particles 2 from being oxidized.
[0035] The solvent 3 has a boiling point of 150°C or higher. Therefore, the solvent 3 is not easily volatilized and is retained in the bonding sheet 1 for a long period of time. The upper limit of the boiling point of the solvent 3 is lower than the temperature at which the bonding sheet 1 is heated to sinter the copper particles 2. The boiling point of the solvent 3 is preferably 200°C or lower.
[0036] The solvent 3 is preferably a liquid at room temperature. The solvent 3 preferably has a freezing point of 30° C. or higher. When the solvent 3 is a liquid at room temperature, the copper particles 2 and the solvent 3 can be easily mixed in the production of the bonding sheet 1.
[0037] The solvent 3 has a molecular weight of 1000 or less. When the solvent 3 is a polymer compound, the molecular weight is a number average molecular weight. By setting the molecular weight of the solvent 3 to 1000 or less, it is possible to suppress the solvent from remaining in the bonding layer after heating, thereby suppressing the generation of voids. In addition, the solvent 3 is preferably an organic solvent having a molecular weight of 100 to 1000. By using an organic solvent having the above molecular weight as the solvent 3, the surface of the copper particles 2 can be uniformly coated with the solvent 3 by mixing the copper particles 2 and the solvent 3, and the solvent is less likely to flow out during storage of the bonding sheet 1. In addition, since the boiling point of the organic solvent is within an appropriate range, it is possible to suppress the shape change caused by the solvent volatilizing during storage and the sheet drying, and it is possible to suppress the solvent from remaining in the bonding layer after heating. The molecular weight of the organic solvent is more preferably in the range of 200 to 800, and particularly preferably in the range of 200 to 600. The molecular weight can be measured by the following method using a size exclusion chromatography method (apparatus: LC-8020 manufactured by Tosoh Corporation). The column was Asahipac GF-310HQ (Showa Denko K.K.). The column oven was set at 40°C, the standard substance was polyethylene glycol, and the mobile phase was a methanol solvent containing 0.05M NaCl4. The mobile phase was run at a flow rate of 1 ml / min, 0.02 ml of a high molecular weight sample was injected, and the molecular weight was calculated from the obtained spectrum.
[0038] The solvent 3 is preferably a compound having a reducing group at the end. By having a reducing group, oxidation of the copper particles 2 can be suppressed. The reducing group is preferably a hydroxyl group. In order to sinter the copper particles 2, it is necessary to remove the organic protective film on the surface of the copper particles 2 by heating or the like. On the other hand, the copper particles 2 from which the organic protective film has been removed are prone to a decrease in sinterability due to oxidation, and the bonding strength of the bonding layer (copper sintered body) obtained by sintering the copper particles 2 is prone to decrease. By using a solvent having a hydroxyl group as the solvent 3, oxidation of the copper particles 2 can be suppressed, and the decrease in the bonding strength of the bonding layer obtained by sintering the copper particles 2 can be suppressed. In addition, since solvents having a hydroxyl group generally tend to have a high boiling point, the bonding sheet 1 using a solvent having a hydroxyl group is less likely to volatilize the solvent 3, and the shape stability of the sheet is further improved.
[0039] As the solvent 3, for example, a diol compound or a triol compound can be used. Examples of the diol compound include ethylene glycol, diethylene glycol, and polyethylene glycol. Examples of the triol compound include glycerin, butanetriol, and polyoxypropylenetriol. These organic solvents and polymer solvents may be used alone or in combination of two or more.
[0040] Next, a method for producing the bonding sheet 1 of this embodiment will be described. FIG. 2 is a flow diagram showing a method for producing the bonding sheet according to one embodiment of the present invention. The bonding sheet of this embodiment can be produced by a method including a mixing step and a molding step, as shown in FIG.
[0041] The mixing step S01 is a step of mixing copper particles 2 with a solvent 3. The copper particles 2 and the solvent 3 can be mixed using a rotation-revolution mixer or a planetary mixer.
[0042] The forming step S02 is a step of forming the mixture obtained in the mixing step S01 into a sheet shape. The mixture can be formed into a sheet by a rolling method using a pressure roller or a pressing method using a mold.
[0043] The sheet-like mixture adjusted to a predetermined thickness as described above is cut into a predetermined shape, whereby the bonding sheet 1 can be obtained.
[0044] Next, a method for producing a bonded body using the bonding sheet of this embodiment will be described. Fig. 3 is a schematic cross-sectional view of a bonded body produced using the bonding sheet according to one embodiment of the present invention. 3, the bonded body 11 includes a substrate 12, a bonding layer 13, and an electronic component 14. The substrate 12 and the electronic component 14 are bonded to each other via the bonding layer 13.
[0045] For example, a printed wiring board having an insulating plate and a wiring pattern formed on the insulating plate can be used as the substrate 12. There are no particular limitations on the printed wiring board, and a flexible printed wiring board, a rigid printed wiring board, or a rigid flexible printed wiring board can be used.
[0046] For example, a semiconductor element, a resistor, a capacitor, or a crystal oscillator can be used as the electronic component 14. Examples of the semiconductor element include a Schottky Barrier Diode (SBD), a Metal-Oxide-Semiconductor Field Effect Transistor (MOSFET), an Insulated Gate Bipolar Transistor (IGBT), a Large Scale Integration (LSI), an LED chip, and an LED-CSP (LED-Chip Size Package).
[0047] The bonded body 11 can be produced by disposing the above-mentioned bonding sheet between the substrate 12 and the electronic component 14 to obtain a laminate, and heating the obtained laminate to sinter the copper particles of the bonding sheet to form the bonding layer 13. The heating temperature of the laminate is, for example, in the range of 150°C to 300°C. The heating time of the laminate is, for example, in the range of 10 minutes to 1 hour. The heating of the laminate is preferably performed in an inert gas atmosphere while pressurizing the laminate in the stacking direction of the laminate. As the inert gas, nitrogen gas or argon gas can be used. The pressurizing pressure of the laminate is preferably in the range of 0.5 MPa to 30 MPa.
[0048] The bonding sheet 1 of the present embodiment configured as described above includes copper particles 2 and a solvent 3, and the copper particles 2 are covered with the solvent 3, so that the copper particles 2 are not easily oxidized. In addition, the solvent 3 has a boiling point of 150° C. or more, so that it is not easily volatilized. Therefore, the bonding sheet 1 of the present embodiment is less likely to suffer from a decrease in sinterability due to oxidation of the copper particles 2, and has improved shape stability. In addition, the solvent 3 has a molecular weight of 1000 or less, so that the solvent 3 is prevented from remaining in the bonding layer after heating, and the generation of voids can be suppressed. Furthermore, the copper particles 2 are fine, with a BET diameter in the range of 40 nm or more and 750 nm or less, so that the sinterability is high, and the content ratio of the copper particles 2 to the solvent 3 is in the range of 99:1 to 90:10 in mass ratio, and the content of the copper particles 2 is 90 mass% or more, so that a dense sintered body (bonding layer) of the copper particles 2 can be formed by heating. In addition, the content of the solvent 3 is 10 mass% or less, so that the amount of volatilized gas and decomposed gas of the solvent generated during heating is small. Therefore, according to the bonding sheet 1 of the present embodiment, a dense bonding layer with few voids can be formed, and electronic components and the like can be bonded with high strength.
[0049] In the bonding sheet 1 of the present embodiment, the molecular weight of the solvent 3 is preferably not less than 200 and not more than 600. When the molecular weight of the solvent 3 falls within this numerical range, the generation of voids can be more suitably suppressed.
[0050] In the bonding sheet 1 of this embodiment, the surfaces of the copper particles 3 are coated with an organic protective film. In the bonding sheet 1, the surfaces of the copper particles 2 are coated with an organic protective film, so the copper particles are not easily oxidized. When the copper particles are oxidized, the copper oxide film reduces the bonding property. Therefore, by making the copper particles less likely to be oxidized by the organic protective film as in this embodiment, the decrease in bonding property can be suppressed.
[0051] In addition, in the bonding sheet 1 of the present embodiment, the surface of the copper particle is Cu detected by analysis using time-of-flight secondary ion mass spectrometry. + C3H3O3 vs. ion detection amount - It is preferable that the ratio of the amount of detected ions is 0.001 or more. Cu + C3H3O3 vs. ion detection amount - When the ratio of the detected amounts of ions is 0.001 or more, the surfaces of the copper particles are appropriately coated with an organic protective film, and oxidation of the copper particles can be more effectively suppressed.
[0052] In the bonding sheet 1 of the present embodiment, when the solvent 3 has a reducing group, the solvent 3 has reducing properties, so that the oxidation of the copper particles 2 is less likely to occur. Therefore, the decrease in sinterability due to the oxidation of the copper particles 2 can be further suppressed.
[0053] In addition, in the bonding sheet 1 of this embodiment, when the reducing group of the solvent 3 is a hydroxyl group, the hydroxyl group has a high affinity for copper particles, so that the oxidation of the copper particles 2 is further suppressed and the solvent 3 is further suppressed from volatilizing. Therefore, the decrease in sinterability due to the oxidation of the copper particles 2 can be further suppressed and the shape stability of the bonding sheet 1 is further improved.
[0054] Furthermore, in the bonding sheet 1 of the present embodiment, when the solvent 3 contains at least one of a diol compound and a triol compound, the diol compound and the triol compound have high adhesion to the copper particles 2, and therefore are unlikely to volatilize for a long period of time. Therefore, the deterioration of sinterability due to oxidation of the copper particles can be suppressed for a long period of time, and the shape stability of the bonding sheet is improved for a long period of time.
[0055] Although the embodiment of the present invention has been described above, the present invention is not limited to this, and can be modified as appropriate without departing from the technical concept of the invention. For example, in FIG. 3, a bonded body 11 using the bonding sheet 1 of this embodiment is described in which a substrate 12 and an electronic component 14 are bonded via a bonding layer 13, but the use of the bonding sheet 1 is not limited thereto. For example, the bonding sheet 1 can be used when bonding two substrates together. Specifically, it can be used when bonding a base substrate and a substrate (submount substrate) that is relatively smaller in size than the base substrate. It can also be used in a power module when bonding a ceramic circuit substrate incorporating multiple semiconductor elements to a heat sink. The bonding sheet 1 can also be used when bonding an LED element to a submount substrate in an LED device. EXAMPLES
[0056] [Preparation of copper particles A] Copper citrate 2.5 hydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and ion-exchanged water were mixed and stirred with a stirring blade to prepare an aqueous dispersion of copper citrate with a concentration of 30% by mass. Then, an aqueous solution of ammonium citrate was added as a pH adjuster to the obtained aqueous dispersion of copper citrate to adjust the pH of the aqueous dispersion of copper citrate to 5. Next, the obtained aqueous dispersion of copper citrate was heated to 50°C, and while maintaining the temperature, an aqueous solution of hydrazine monohydrate (diluted 2-fold) was added as a reducing agent for copper ions in a nitrogen gas atmosphere at one time, and the mixture was stirred and mixed with a stirring blade. The amount of the aqueous solution of hydrazine monohydrate added was 1.2 times the amount required to reduce the total amount of copper ions. The obtained mixture was heated to 70°C in a nitrogen gas atmosphere and maintained at that temperature for 2 hours to generate copper particles. The generated copper particles were collected using a centrifuge. The collected copper particles were dried by a reduced pressure drying method to prepare copper particles A.
[0057] [Preparation of copper particles B] Copper particles B were prepared in the same manner as copper particles A, except that the pH of the copper citrate aqueous dispersion was adjusted to 2.0.
[0058] [Preparation of copper particles C] Copper particles C were prepared in the same manner as copper particles A, except that the pH of the copper citrate aqueous dispersion was adjusted to 7.5.
[0059] [Preparation of copper particles D] Copper particles D were prepared in the same manner as copper particles A, except that the pH of the copper citrate aqueous dispersion was adjusted to 1.7.
[0060] [Preparation of copper particles E] Copper particles E were prepared in the same manner as copper particles A, except that the pH of the copper citrate aqueous dispersion was adjusted to 8.0.
[0061] [Preparation of copper particles F] Copper microparticles F were prepared in the same manner as copper particles A, except that RCV11 (Type-B) manufactured by DOWA Electronics was used.
[0062] The BET diameter and the composition of the coating layer of the obtained copper particles A to F were measured by the following methods. The results are shown in Table 1 below.
[0063] (BET diameter) The amount of nitrogen gas adsorbed by the copper particles was measured using a specific surface area measuring device (Quantachrome Instruments, QUANTACHROME AUTOSORB-1), and the specific surface area of the copper particles was calculated by the BET method. 2 / g) and the density of the copper particles ρ (g / cm 3 ) and the BET diameter was calculated using the following formula. BET diameter (nm) = 6000 / (ρ(g / cm 3 )×S(m 2 / g))
[0064] (Components of the coating layer) A time-of-flight secondary ion mass spectrometer (TOF-SIMS: ULVAC PHI, nanoTOFII) was used to measure Cu. + C3H3O3 for ions - Ions and C3H4O2 - The measurement sample was made by embedding copper powder on the surface of an In foil. The measurement area was 100 μm square, and the primary ions were Bi3 ++ The TOF-SIMS spectrum was obtained by measuring at 30 kV for 5 minutes. + , C3H3O3 - Ion, C3H4O2 - The amount of each ion was calculated as Cu, + Divide by the amount of ions detected, C3H3O3 - / Cu + ratio, C3H4O2 - / Cu + Ratio and C5 or higher ions / Cu + The ratio was calculated.
[0065] (Coating amount) The amount of coating on the copper particles was measured using a differential thermobalance TG8120-SL (RIGAKU). The sample used was copper particles from which moisture had been removed by freeze-drying. Measurements were performed in nitrogen (G2 grade) gas to suppress oxidation of the copper particles, with a heating rate of 10°C / min, and the weight loss rate when heated from 250°C to 300°C was defined as the amount of coating of the organic protective film. In other words, the amount of coating = (sample weight after measurement) / (sample weight before measurement) x 100 (wt%). The measurements were performed three times on copper particles from the same lot, and the arithmetic mean value was used as the amount of coating.
[0066] [Table 1]
[0067] [Example 1] Copper particles and polyethylene glycol (molecular weight: 200) as a binder were mixed in a mass ratio of 95:5. The mixture obtained was then rolled using a powder rolling machine (2RM-63K, manufactured by Ohno Roll Co., Ltd.) with a pressure roller under the condition of a gap width of the pressure roller of 500 μm to obtain a copper sheet having a thickness of 500 μm. The density of the obtained copper sheet was measured by the following method. In addition, the shear strength and void ratio of a bonded body produced using the obtained copper sheet were measured by the following method. The results are shown in Table 2.
[0068] (density) After sealing the copper sheet with epoxy resin, the copper sheet was cut horizontally to the thickness direction of the copper sheet. The cut surface of the copper sheet was subjected to mechanical polishing and cross-polishing to expose the copper sheet. The cut surface of the copper sheet was then observed at 50,000 times magnification using a SEM (scanning electron microscope). The obtained SEM image was binarized using image processing software (ImageJ, manufactured by the National Institutes of Health, USA) to separate it into a particle portion and a void portion, and the density was calculated using the following formula. Density (%) = (total area of particle parts / (total area of particle parts + total area of void parts)) x 100
[0069] The density was measured at 10 randomly taken SEM images, and the values shown in Table 2 are the average density values calculated from the 10 SEM images.
[0070] (Shear strength of joint) The copper sheet was cut using a commercially available cutter knife to prepare a copper sheet piece (2.5 mm square x 500 μm thick). The above copper sheet piece (2.5 mm square x 500 μm thick) was placed on a 30 mm square x 1 mm thick oxygen-free copper substrate. Next, a 2.5 mm square x 1 mm thick oxygen-free copper dummy element was placed on the copper sheet piece. In this way, a laminate was obtained in which the oxygen-free copper substrate and the oxygen-free copper dummy element were laminated via the copper sheet piece. The obtained laminate was held for 15 minutes under conditions of a nitrogen gas atmosphere, a pressurized pressure of 5 MPa, and a temperature of 250° C. using a die bonder (HTB-MM, manufactured by Alpha Design Co., Ltd.) to prepare a bonded body (sample A) in which a 2.5 mm square oxygen-free copper substrate and an oxygen-free copper dummy element were bonded via a copper bonding layer.
[0071] The shear strength of the resulting bonded body (sample A) was measured by a method conforming to JIS Z 3198-7 (Lead-free solder test method - Part 7: Shear test method for solder joints of chip components). Specifically, a load was applied to the oxygen-free copper dummy element using a tool of a bond tester (Nordson DAGE, SERIES 4000), and the load (maximum shear load) was measured when the oxygen-free copper dummy element peeled off from the copper bonding layer. The moving speed of the tool was 50 μm / sec, and the gap between the tip of the tool and the oxygen-free copper substrate was 50 μm. The obtained maximum shear load was converted into Newton and divided by the area (2.5 mm × 2.5 mm) of the copper bonding layer to obtain the shear strength (unit: MPa). Seven bonded bodies were produced, and the shear strength of each bonded body was measured. The values shown in Table 2 are the average shear strengths of the seven bonded bodies. A shear strength of 20 MPa or more was good, and one less than 20 MPa was unacceptable.
[0072] (Void ratio of joint) The copper sheet was cut using a commercially available cutter knife to prepare a copper sheet piece (10 mm square x 500 μm thick). The above copper sheet piece (10 mm square x 500 μm thick) was placed on a 30 mm square x 1 mm thick oxygen-free copper substrate. Next, a 10 mm square x 1 mm thick oxygen-free copper dummy element was placed on the copper sheet piece. In this way, a laminate was obtained in which the oxygen-free copper substrate and the oxygen-free copper dummy element were laminated via the copper sheet piece. The obtained laminate was held for 15 minutes under conditions of a nitrogen gas atmosphere, a pressurized pressure of 5 MPa, and a temperature of 250° C. using a die bonder (manufactured by Alpha Design Co., Ltd., HTB-MM) to prepare a bonded body (sample B) in which a 2.5 mm square oxygen-free copper substrate and an oxygen-free copper dummy element were bonded via a copper bonding layer.
[0073] The ultrasonic inspection image of the copper bonding layer of the obtained bonded body (sample B) was measured using an ultrasonic inspection device (FINE-SAT, Hitachi High-Technologies Corporation). The obtained ultrasonic inspection image was binarized using image processing software (ImageJ, National Institutes of Health, USA) to separate voids (cavities) and the bonded body (copper particle sintered body), and the void ratio was calculated using the following formula. Void ratio (%) = (total area of voids / area of copper bonding layer (10 mm x 10 mm)) x 100
[0074] Seven bonded bodies were produced, and the void ratio was measured for each bonded body. The values shown in Table 2 are the average void ratios of the seven bonded bodies. A void ratio of less than 10% is acceptable, and one of 10% or more is unacceptable.
[0075] [Example 2 of the present invention ~3, Reference Example 4, Invention Examples 5-8, Reference Examples 9-12, Invention Example 13 ~16, Comparative Examples 1~4] A copper sheet was produced in the same manner as in Example 1 of the present invention, except that the type of copper particles, the type of binder, the boiling point, the number average molecular weight, and the amount of copper particles and binder were changed as shown in Table 2 below. In Table 2, PEG stands for polyethylene glycol, DEG stands for diethylene glycol, and EG stands for ethylene glycol. Then, in the same manner as in Example 1 of the present invention, the density of the obtained copper sheet was measured, and the shear strength and void ratio of the bonded body produced using the obtained copper sheet were measured. The results are shown in Table 2.
[0076] [Table 2]
[0077] Examples 1 to 3 of the present invention contain copper particles having a BET diameter in the range of 40 nm to 750 nm and a solvent having a boiling point of 150° C. or higher and a molecular weight of 1000 or less as a binder in a mass ratio of 99:1 to 90:10 (copper particles:solvent). 3、5~8、13~ All of the 16 bonded structures using copper sheets had high shear strengths of 15 MPa or more and low void ratios of less than 10%, indicating that the deterioration of sinterability due to oxidation of copper particles is unlikely to occur, and that a dense bonding layer with few voids can be formed, making it possible to bond electronic components, etc. with high strength.
[0078] In contrast, the bonded body using the copper sheet of Comparative Example 1, which contains polyethylene glycol as a binder that is solid at room temperature rather than having a molecular weight of 1000 or less, shows a large decrease in shear strength and a large increase in void ratio, and it is understood that a dense bonding layer with few voids cannot be formed. In Comparative Example 1, it is considered that the void ratio is high because the polyethylene glycol does not volatilize during heating to prepare the bonded body due to the high molecular weight and remains in the bonding layer. In addition, it is found that the bonded body using the copper sheet of Comparative Example 2, which contains ethanol with a boiling point of 80°C as a binder, shows an increase in void ratio and it is difficult to form a dense bonding layer with few voids. It is considered that the pores become large due to the ethanol volatilizing at once during heating to prepare the bonded body.
[0079] In Comparative Example 3, in which the content ratio of polyethylene glycol, a binder, exceeds the upper limit of the present invention, the copper sheet obtained by the rolling process adhered with strong adhesion to the surface of the pressure roller of the powder rolling machine. When the copper sheet was peeled off from the pressure roller, the copper sheet was damaged, and the copper sheet of the minimum dimensions required to produce a bonded body could not be recovered, so the shear strength and void ratio of the bonded body could not be evaluated. In Comparative Example 4, in which the content ratio of polyethylene glycol, a binder, falls below the lower limit of the present invention, many cracks occurred in the copper sheet obtained by the rolling process. The copper sheet was damaged by these cracks, and the copper sheet of the minimum dimensions required to produce a bonded body could not be recovered, so the shear strength and void ratio of the bonded body could not be evaluated. [Explanation of symbols]
[0080] 1. Bonding sheet 2. Copper particles 3. Solvent 11 Zygote 12 Substrate 13 Bonding layer 14 Electronic Components
Claims
1. A method for producing a solvent having a boiling point of 150° C. or higher, comprising: The content ratio of the copper particles to the solvent is 99:1 to 90:10 by mass ratio, The BET diameter of the copper particles is in the range of 40 nm or more and 750 nm or less, The molecular weight of the solvent is 200 or more and 600 or less.
2. The bonding sheet according to claim 1 , wherein the solvent contains at least one of a diol compound and a triol compound.
3. The bonding sheet according to claim 1 or 2, wherein the copper particles have surfaces covered with an organic protective film.
4. The surface of the copper particles is analyzed by time-of-flight secondary ion mass spectrometry to detect Cu. + C vs. the amount of ions detected 3 H 3 O 3 - The bonding sheet according to claim 3 , wherein a ratio of detected amounts of ions is 0.001 or more.
Citation Information
Patent Citations
Swirl controller
JP1987045933A
Aluminum casting alloy for intake manifold
JP1989028339A
Joint material and method for producing joint material
JP2019203172A
Particles for joining material and production method thereof, joining paste and preparation method thereof, and production method of joined body
JP2020059914A