Composition for forming underlayer film for lithography, underlayer film for lithography, pattern forming method and purification method

A composition with an aralkyl oligomer structure addresses the challenge of forming resist underlayer films with sufficient thickness and fine patterns, offering excellent etching resistance and solubility, enhancing lithography processes through wet application methods.

JP7589681B2Active Publication Date: 2024-11-26MITSUBISHI GAS CHEM CO INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021522753
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-05-27
Filing Date
2020-05-25
Publication Date
2024-11-26
Estimated Expiration
2040-05-25

AI Technical Summary

Technical Problem

Existing lithography processes face challenges in forming resist underlayer films that provide sufficient thickness for substrate processing while maintaining fine resist patterns, and there is a need for compositions that can be applied via wet processes like spin coating or screen printing, offering excellent etching resistance and solubility in organic solvents.

Method used

A composition for forming a resist underlayer film comprising an oligomer with an aralkyl structure, represented by specific formulas, which includes a solvent and can be applied through wet processes, providing excellent etching resistance, heat resistance, and solubility in organic solvents, with the ability to flatten the wafer surface and fill fine patterns effectively.

Benefits of technology

The composition achieves excellent flattening and filling performance, resulting in high-quality resist patterns with improved etching resistance and adhesion to resist layers, suitable for various semiconductor processing steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589681000001
    Figure 0007589681000001
  • Figure 0007589681000002
    Figure 0007589681000002
  • Figure 0007589681000003
    Figure 0007589681000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing a composition for forming a resist underlayer film for lithography, which is characterized by having excellent planarization performance on a substrate with level difference, and having good embeddability with respect to a fine hole pattern, and which is also characterized in that the wafer surface after film formation is planarized. The above-described problem is able to be solved by the composition described below. A composition for forming an underlayer film for lithography, which contains (a) an oligomer having an aralkyl structure represented by formula (1-0), and (b) a solvent. (In the formula, Ar0 represents a phenylene group, a naphthylene group, an anthrylene group, a phenanthrylene group, a pyrylene group, a fluorylene group, a biphenylene group, a diphenylmethylene group or a terphenylene group; R0 moieties are substituents of Ar0, which may be the same groups or different groups, and each of which independently represents a hydrogen atom, an optionally substituted alkyl group having 1-30 carbon atoms, an optionally substituted aryl group having 6-30 carbon atoms, an optionally substituted alkenyl group having 2-30 carbon atoms, an optionally substituted alkynyl group having 2-30 carbon atoms, an optionally substituted alkoxy group having 1-30 carbon atoms, an optionally substituted acryl group having 1-30 carbon atoms, an optionally substituted carboxyl group having 1-30 carbon atoms, an optionally substituted amino group having 0-30 carbon atoms, a halogen atom, a cyano group, a nitro group, a thiol group or a heterocyclic group; X represents a linear or branched alkylene group; n represents an integer of 1-500; r represents an integer of 1-3; p represents a positive integer; and q represents a positive integer.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for forming an underlayer film for lithography, an underlayer film for lithography, a pattern forming method, and a purification method. [Background technology]

[0002] In the manufacture of semiconductor devices, microfabrication is carried out by lithography using photoresist materials, but in recent years, with the increasing integration and speed of LSI (large-scale integrated circuits), there is a demand for even finer pattern rules. In addition, the light source for lithography used in forming resist patterns has been shortened from KrF excimer lasers (248 nm) to ArF excimer lasers (193 nm), and the introduction of extreme ultraviolet light (EUV, 13.5 nm) is also expected.

[0003] However, as the resist pattern becomes finer, problems such as resolution problems or the resist pattern collapsing after development arise, so that it is desirable to make the resist thinner. However, simply making the resist thinner makes it difficult to obtain a resist pattern with a film thickness sufficient for substrate processing. Therefore, a process is required in which not only the resist pattern but also a resist underlayer film is formed between the resist and the semiconductor substrate to be processed, and this resist underlayer film also functions as a mask during substrate processing.

[0004] Currently, various resist underlayer films for such processes are known. For example, a resist underlayer film material containing a polymer having a specific repeating unit has been proposed as a material for realizing a resist underlayer film for lithography having a selectivity of a dry etching rate smaller than that of a resist (see Patent Document 1). Furthermore, a resist underlayer film material containing a polymer obtained by copolymerizing a repeating unit of an acenaphthylene derivative with a repeating unit having a substituted or unsubstituted hydroxyl group has been proposed as a material for realizing a resist underlayer film for lithography having a selectivity of a dry etching rate smaller than that of a semiconductor substrate (see Patent Document 2).

[0005] On the other hand, as a material having high etching resistance for this type of resist underlayer film, amorphous carbon underlayer film formed by chemical vapor deposition (CVD) using methane gas, ethane gas, acetylene gas, etc. as raw materials is well known. However, from the viewpoint of process, there is a demand for a resist underlayer film material that can be formed by a wet process such as spin coating or screen printing.

[0006] The inventors have also proposed a composition for forming an underlayer film for lithography (see Patent Document 3), which contains a compound of a specific structure and an organic solvent, as a material that has excellent etching resistance, high heat resistance, is soluble in a solvent, and can be used in wet processes. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2004-271838 A [Patent Document 2] JP 2005-250434 A [Patent Document 3] International Publication No. 2013 / 024779 Summary of the Invention [Problem to be solved by the invention]

[0008] However, there is a demand for a composition for forming an underlayer film for lithography that simultaneously satisfies high levels of solubility in organic solvents, etching resistance, and resist pattern formability, while also having the characteristic of planarizing the wafer surface after film formation.

[0009] Therefore, an object of the present invention is to provide a composition for forming a resist underlayer film for lithography, which has excellent planarization performance on uneven substrates, good filling performance into fine hole patterns, and flattens the wafer surface after film formation. [Means for solving the problem]

[0010] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems and have found that a specific composition for forming an underlayer film is useful, thereby completing the present invention.

[0011] That is, the present invention is as follows. [1] a: an oligomer having an aralkyl structure represented by the following formula (1-0), and b: Solvent A composition for forming an underlayer film for lithography comprising the above compound. [ka] (In the formula, Ar 0 represents a phenylene group, a naphthylene group, an anthrylene group, a phenanthrylene group, a pyrylene group, a fluorylene group, a biphenylene group, a diphenylmethylene group, or a terphenylene group, R 0 Ar 0 and each independently represents the same or different groups, a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; X represents a linear or branched alkylene group. n represents an integer from 1 to 500; r represents an integer from 1 to 3; p represents a positive integer, q represents a positive integer.) [2] The composition for forming an underlayer film for lithography according to [1], wherein the oligomer having an aralkyl structure represented by the formula (1-0) is represented by the following formula (1-1): [ka] (In the formula, Ar 0 represents a phenylene group, a naphthylene group, an anthrylene group, a phenanthrylene group, a pyrylene group, a fluorylene group, a biphenylene group, a diphenylmethylene group, or a terphenylene group, R 0 Ar 0 and each independently represents the same or different groups, a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; n represents an integer from 1 to 500; r represents an integer from 1 to 3; p represents a positive integer, q represents a positive integer.) [3] The composition for forming an underlayer film for lithography according to [2], wherein the oligomer having an aralkyl structure represented by the formula (1-1) is represented by the following formula (1-2): [ka] (In the formula, Ar2 represents a phenylene group, a naphthylene group, or a biphenylene group, Ar 2 is a phenylene group, Ar 1 represents a naphthylene group or a biphenylene group, Ar 2 is a naphthylene group or a biphenylene group, Ar 1 represents a phenylene group, a naphthylene group, or a biphenylene group, R a Ar 1 each independently may be the same or different; R a represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group. R b Ar 2 each independently may be the same or different; R b represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group, n represents an integer from 1 to 500; r represents an integer from 1 to 3; p represents a positive integer, q represents a positive integer.) [4] Ar 2 represents a phenylene group, a naphthylene group, or a biphenylene group, Ar 2 is a phenylene group, Ar 1 represents a biphenylene group, Ar 2 is a naphthylene group or a biphenylene group, Ar 1 represents a phenylene group, a naphthylene group, or a biphenylene group, R a represents a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent. R b represents a hydrogen atom or an optionally substituted alkyl group having 1 to 30 carbon atoms, [5] The composition for forming an underlayer film for lithography according to [3] or [4], wherein the oligomer having an aralkyl structure represented by the formula (1-2) is represented by the following formula (2) or formula (3): [ka] (In formula (2), Ar 1 , R a , r, p, and n are the same as in formula (1-2). [ka] (In formula (3), Ar 1 , R a , r, p, and n are the same as in formula (1-2). [6] The composition for forming an underlayer film for lithography according to [5], wherein the oligomer having an aralkyl structure represented by the formula (2) is represented by the following formula (4): [ka] (In formula (4), R1's each independently represent a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; m1 represents an integer from 1 to 3; n represents an integer from 1 to 50. [7] The composition for forming an underlayer film for lithography according to [5], wherein the oligomer having an aralkyl structure represented by the formula (3) is represented by the following formula (5): [ka] (In formula (5), R2 each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; m2 represents an integer from 1 to 3; n represents an integer from 1 to 50. [8] The composition for forming an underlayer film for lithography according to [5], wherein the oligomer having an aralkyl structure represented by the formula (2) is represented by the following formula (6): [ka] (In formula (6), R3 each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; m3 represents an integer from 1 to 5; n represents an integer from 1 to 50. [9] The composition for forming an underlayer film for lithography according to [5], wherein the oligomer having an aralkyl structure represented by the formula (3) is represented by the following formula (7): [ka] (In formula (7), R4's each independently represent a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; m4 represents an integer from 1 to 5; n represents an integer from 1 to 50.

[10] The composition for forming an underlayer film for lithography according to any one of [1] to [9], further comprising an acid generator.

[11] The composition for forming an underlayer film for lithography according to any one of [1] to

[10] , further comprising a crosslinking agent.

[12] An underlayer film for lithography formed using the composition for forming an underlayer film for lithography according to any one of [1] to

[11] .

[13] forming an underlayer film on a substrate using the composition for forming an underlayer film for lithography according to any one of [1] to

[11] ; forming at least one photoresist layer on the underlayer film; and exposing predetermined areas of the photoresist layer to radiation and developing; A method for forming a resist pattern comprising the steps of:

[14] forming an underlayer film on a substrate using the composition for forming an underlayer film for lithography according to any one of [1] to

[11] ; forming an intermediate layer film on the underlayer film using a resist intermediate layer film material containing silicon atoms; forming at least one photoresist layer on the intermediate layer film; irradiating predetermined areas of the photoresist layer with radiation and developing to form a resist pattern; a step of etching the intermediate layer film using the resist pattern as a mask; a step of etching the underlayer film using the obtained intermediate layer film pattern as an etching mask; and A step of forming a pattern on a substrate by etching the substrate using the obtained underlayer film pattern as an etching mask; A method for forming a circuit pattern comprising the steps of:

[15] A step of dissolving the oligomer having an aralkyl structure according to any one of [1] to

[11] in a solvent to obtain an organic phase; contacting the organic phase with an acidic aqueous solution to extract impurities in the oligomer; Including, The method for purification, wherein the solvent used in the step of obtaining the organic phase comprises a solvent that is optionally immiscible with water. Effect of the Invention

[0012] According to the present invention, it is possible to provide a useful composition for forming an underlayer film for lithography. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention (also referred to as "the present embodiment") will be described. Note that the following embodiment is an example for explaining the present invention, and the present invention is not limited to the embodiment.

[0014] With respect to the structural formulae described herein, for example as shown below, when the line showing the bond to C touches ring A and ring B, it means that C is bonded to either one or both of ring A and ring B. [ka]

[0015] [Composition for forming lower layer film for lithography] The composition for forming an underlayer film of this embodiment is a: an oligomer having an aralkyl structure represented by the following formula (1-0), and b: Solvent Includes.

[0016] [ka]

[0017] In the oligomer represented by the general formula (1-0), Ar 0 R represents a phenylene group, a naphthylene group, an anthrylene group, a phenanthrylene group, a pyrylene group, a fluorylene group, a biphenylene group, a diphenylmethylene group, or a terphenylene group, and preferably represents a phenylene group, a naphthylene group, an anthrylene group, a phenanthrylene group, a fluorylene group, a biphenylene group, a diphenylmethylene group, or a terphenylene group. 0 Ar 0and each independently represents the same or different groups, a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group or a heterocyclic group, and preferably represents a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent.

[0018] In the oligomer represented by the general formula (1-0), X represents a linear or branched alkylene group, specifically, a methylene group, an ethylene group, an n-propylene group, an i-propylene group, an n-butylene group, an i-butylene group, or a tert-butylene group, preferably a methylene group, an ethylene group, an n-propylene group, or an n-butylene group, more preferably a methylene group or an n-propylene group, and most preferably a methylene group.

[0019] In the oligomer represented by the general formula (1-0), n is an integer of 1 to 500, preferably an integer of 1 to 50.

[0020] In the oligomer represented by the general formula (1-0), r represents an integer of 1 to 3.

[0021] In the oligomer represented by the general formula (1-0), p represents a positive integer. 0 The time period varies depending on the type of the device.

[0022] In the oligomer represented by the general formula (1-0), q represents a positive integer. 0 The time period varies depending on the type of the device.

[0023] The oligomer represented by the general formula (1-0) is preferably an oligomer represented by the following general formula (1-1). [ka]

[0024] In the oligomer represented by the general formula (1-1), Ar 0 R represents a phenylene group, a naphthylene group, an anthrylene group, a phenanthrylene group, a pyrylene group, a fluorylene group, a biphenylene group, a diphenylmethylene group, or a terphenylene group, and preferably represents a phenylene group, a naphthylene group, an anthrylene group, a phenanthrylene group, a fluorylene group, a biphenylene group, a diphenylmethylene group, or a terphenylene group. 0 Ar 0 and each independently represents the same or different groups, a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group or a heterocyclic group, and preferably represents a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent.

[0025] In the oligomer represented by the general formula (1-1), n ​​is an integer of 1 to 500, preferably an integer of 1 to 50.

[0026] In the oligomer represented by the general formula (1-1), r represents an integer of 1 to 3.

[0027] In the oligomer represented by the general formula (1-1), p represents a positive integer. 0 The time period varies depending on the type of the device.

[0028] In the oligomer represented by the general formula (1-1), q represents a positive integer. 0 The time period varies depending on the type of the device.

[0029] The oligomer represented by the general formula (1-1) is preferably an oligomer represented by the following general formula (1-2).

[0030] [ka]

[0031] In the oligomer represented by the general formula (1-2), Ar 2 represents a phenylene group, a naphthylene group, or a biphenylene group, and Ar 2 is a phenylene group, Ar 1 represents a naphthylene group or a biphenylene group (preferably a biphenylene group), Ar 2 is a naphthylene group or a biphenylene group, Ar 1 represents a phenylene group, a naphthylene group or a biphenylene group. 1 and Ar 2 Specific examples of such alkylene groups include a 1,4-phenylene group, a 1,3-phenylene group, a 4,4'-biphenylene group, a 2,4'-biphenylene group, a 2,2'-biphenylene group, a 2,3'-biphenylene group, a 3,3'-biphenylene group, a 3,4'-biphenylene group, a 2,6-naphthylene group, a 1,5-naphthylene group, a 1,6-naphthylene group, a 1,8-naphthylene group, a 1,3-naphthylene group, and a 1,4-naphthylene group.

[0032] In the oligomer represented by the general formula (1-2), R a Ar 1 R is a substituent of the formula (I), each of which may be the same or different. aR represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group, and is preferably a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent. a Specific examples of the alkyl group include methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, tert-butyl, isomeric pentyl, isomeric hexyl, isomeric hexyl, isomeric octyl, and isomeric nonyl groups, and examples of the aryl group include phenyl, alkylphenyl, naphthyl, alkylnaphthyl, biphenyl, and alkylbiphenyl groups. Preferred are methyl, ethyl, n-propyl, n-butyl, n-octyl, and phenyl groups, more preferred are methyl, n-butyl, and n-octyl groups, and most preferred is n-octyl.

[0033] In the oligomer represented by the general formula (1-2), R b Ar 2 R is a substituent of the formula (I), each of which may be the same or different. bR represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group, and is preferably a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent. b Specific examples of the alkyl group include methyl, ethyl, n-propyl, isopropyl, n-butyl, i-butyl, tert-butyl, isomeric pentyl, isomeric hexyl, isomeric hexyl, isomeric octyl, and isomeric nonyl groups, and the aryl group includes phenyl, alkylphenyl, naphthyl, alkylnaphthyl, biphenyl, and alkylbiphenyl groups. Preferred are methyl, ethyl, n-propyl, n-butyl, n-octyl, and phenyl groups, more preferred are methyl, n-butyl, and n-octyl groups, and most preferred is n-octyl.

[0034] Among the oligomers represented by the general formula (1-2), the compounds represented by the formula (2) or (3) are preferred, and the compounds represented by the formulae (4) to (7) are more preferred.

[0035] [ka] (In formula (2), Ar 1 , R a , r, p, and n are as above.) [ka] (In formula (3), Ar 1 , R a , r, p, n are as above) [ka] (In formula (4), R1's each independently represent a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group or a heterocyclic group, preferably a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent, m1 represents an integer from 1 to 3; n represents an integer from 1 to 50. [ka] (In formula (5), R2 each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group, preferably a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent, m2 represents an integer from 1 to 3; n represents an integer from 1 to 50. [ka] (In formula (6), R3 each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group, preferably a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent, m3 represents an integer from 1 to 5; n represents an integer from 1 to 50. [ka] (In formula (7), R4 each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group, preferably a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent, m4 represents an integer from 1 to 5; n represents an integer from 1 to 50.

[0036] In the compounds of formulae (2) to (7), the substituent on the aromatic ring can be substituted at any position on the aromatic ring.

[0037] In the oligomers represented by the general formulas (4), (5), (6), and (7), R1、 R 2、 R 3、 Each R4 may be independently the same or different. 1、 R 2、 R 3、 R4 represents hydrogen, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group, and is preferably a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent. 1、 R 2、 R 3、 Specific examples of R4 include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, i-butyl, tert-butyl, isomeric pentyl, isomeric hexyl, isomeric hexyl, isomeric octyl, and isomeric nonyl, and aryl groups such as phenyl, alkylphenyl, naphthyl, alkylnaphthyl, biphenyl, and alkylbiphenyl. Preferred are methyl, ethyl, n-propyl, n-butyl, n-octyl, and phenyl, more preferred are methyl, n-butyl, and n-octyl, and most preferred is n-octyl.

[0038] In the present invention, unless otherwise defined, "substitution" means that one or more hydrogen atoms in a functional group are substituted with a substituent. The "substituent" is not particularly limited, but examples thereof include a halogen atom, a hydroxyl group, a cyano group, a nitro group, a thiol group, a heterocyclic group, an alkyl group having 1 to 30 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkoxyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, an alkynyl group having 2 to 30 carbon atoms, an acyl group having 1 to 30 carbon atoms, and an amino group having 0 to 30 carbon atoms. The alkyl group may be any of a linear aliphatic hydrocarbon group, a branched aliphatic hydrocarbon group, and a cyclic aliphatic hydrocarbon group.

[0039] Specific examples of the compound represented by the above formula (1-0) include compounds represented by the following formulas: However, the compound represented by the above formula (1-0) is not limited to the compounds represented by the following formulas.

[0040] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]

change

change

change

change

change

change

change

change

change

change

[0041] Although the oligomer represented by the above formula (1-0) has a relatively low molecular weight, it has high heat resistance due to the aromaticity of its structure, so that the composition for forming an underlayer film for lithography of this embodiment is applicable to a wet process and has excellent heat resistance and etching resistance. The composition for forming an underlayer film for lithography of this embodiment contains a resin having an aromatic structure and crosslinking properties, and even when used alone, it undergoes a crosslinking reaction by high-temperature baking to exhibit high heat resistance. As a result, deterioration of the film during high-temperature baking is suppressed, and an underlayer film having excellent etching resistance against oxygen plasma etching and the like can be formed. Furthermore, despite having an aromatic structure, the composition for forming an underlayer film for lithography of this embodiment has high solubility in organic solvents, high solubility in safe solvents, and good stability of product quality. In addition, the composition for forming an underlayer film for lithography of this embodiment has excellent adhesion to a resist layer and a resist intermediate layer film material, so that an excellent resist pattern can be obtained.

[0042] The molecular weight of the oligomer having an aralkyl structure represented by the above formula (1-0) is not particularly limited, but is preferably Mw=300 to 10000 in terms of polystyrene equivalent molecular weight, and from the viewpoint of the balance between embedding flatness and heat resistance, more preferably Mw=500 to 8000, even more preferably Mw=1000 to 6000, and particularly preferably Mw=1000 to 5000. In addition, from the viewpoint of increasing crosslinking efficiency and suppressing volatile components during baking, the compound having the structure represented by the above formula (1-0) preferably has a dispersity (weight average molecular weight Mw / number average molecular weight Mn) in the range of 1.1 to 7, more preferably in the range of 1.1 to 5. The above Mw, Mn, and dispersity can be determined by the method described in the examples below.

[0043] In addition, since the oligomer represented by the formula (1-0) has a relatively low molecular weight and a low viscosity, it is easy to uniformly fill every corner of the step even on a substrate having a step (particularly, a fine space or hole pattern, etc.) and improve the flatness of the film. As a result, the composition for forming an underlayer film containing the oligomer represented by the formula (1-0) has excellent filling properties and flattening properties. In addition, since the oligomer represented by the formula (1-0) is a compound having a relatively high carbon concentration, it can also exhibit high etching resistance. From the viewpoint of filling properties and flattening properties, the solution viscosity is preferably 0.01 to 1.00 Pa·s (ICI viscosity, 150°C), more preferably 0.01 to 0.10 Pa·s. From the same viewpoint, the softening point (ring and ball method) is preferably 30 to 100°C, more preferably 30 to 70°C.

[0044] The oligomer having an aralkyl structure represented by the above formula (1-0) has improved etching resistance, especially when a condensed aromatic ring-containing phenolic compound is used as a crosslinking agent. This is because a film with high hardness and high carbon density is formed due to the intermolecular interaction between the oligomer represented by the above formula (1-0), which has a high aromaticity, and the crosslinking agent, which has a high planarity.

[0045] The oligomer having an aralkyl structure represented by the above formula (1-0) has improved filling and flattening properties, especially when a methylol group-containing phenolic compound is used as a crosslinking agent. This is because the oligomer represented by the above formula (1-0) and the crosslinking agent have similar structures, which results in a higher affinity and a lower viscosity during application.

[0046] The oligomer having an aralkyl structure represented by formula (1-0) is an oligomer of an aromatic methylene compound formed by a condensation reaction between a phenolic aromatic compound and a crosslinking agent having a methylene bond, and this reaction is carried out in the presence of an acid catalyst.

[0047] The acid catalyst used in the above reaction is not particularly limited, and examples thereof include inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, hydrobromic acid, and hydrofluoric acid, organic acids such as oxalic acid, malonic acid, succinic acid, adipic acid, sebacic acid, citric acid, fumaric acid, maleic acid, formic acid, p-toluenesulfonic acid, methanesulfonic acid, trifluoroacetic acid, dichloroacetic acid, trichloroacetic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, naphthalenesulfonic acid, and naphthalenedisulfonic acid, Lewis acids such as zinc chloride, aluminum chloride, iron chloride, and boron trifluoride, and solid acids such as silicotungstic acid, phosphotungstic acid, silicomolybdic acid, and phosphomolybdic acid. These acid catalysts are used alone or in combination of two or more. Among these, from the viewpoint of production, organic acids and solid acids are preferred, and from the viewpoint of production, such as ease of availability and ease of handling, it is preferred to use hydrochloric acid or sulfuric acid. The amount of the acid catalyst used can be appropriately set depending on the raw materials and catalyst used, as well as the reaction conditions, and is not particularly limited, but is preferably 0.01 to 100 parts by mass per 100 parts by mass of the reaction raw materials.

[0048] In the above reaction, a reaction solvent may be used. The reaction solvent is not particularly limited, and examples thereof include water, methanol, ethanol, propanol, butanol, tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, etc. These solvents may be used alone or in combination of two or more.

[0049] The amount of the solvent used can be appropriately set depending on the raw materials and catalyst used, as well as the reaction conditions, and is not particularly limited, but is preferably in the range of 0 to 2000 parts by mass per 100 parts by mass of the reaction raw materials. Furthermore, the reaction temperature in the above reaction can be appropriately selected depending on the reactivity of the reaction raw materials, and is not particularly limited, but is usually in the range of 10 to 200°C.

[0050] In order to obtain the oligomer represented by formula (1-0) of this embodiment, the reaction temperature is preferably high, specifically, in the range of 60 to 200°C. The reaction method is not particularly limited, but for example, the raw materials (reactants) and the catalyst are charged at once, or the raw materials (reactants) are successively dropped in the presence of a catalyst. After the polycondensation reaction is completed, the isolation of the obtained compound can be performed according to a conventional method, and is not particularly limited. For example, in order to remove unreacted raw materials and catalysts present in the system, the temperature of the reaction vessel is increased to 130 to 230°C, and the volatile matter is removed at about 1 to 50 mmHg, and the target oligomer can be obtained by adopting a general method.

[0051] As a preferred reaction condition, it is preferable to use 1 mole to 10 moles of the phenolic aromatic compound per mole of the crosslinking agent having a methylene bond. If the ratio of the crosslinking agent and the phenolic aromatic compound is within the above range, the amount of phenols remaining after the reaction is reduced, and not only is the yield good, but the mass average molecular weight is small, and the softening point and melt viscosity are sufficiently low. On the other hand, if the ratio of the crosslinking agent is too low, it will lead to a decrease in the yield, and if the ratio of the crosslinking agent is too high, the softening point and melt viscosity may become high.

[0052] After the reaction is completed, the oligomer can be isolated by a known method. For example, the reaction solution is concentrated, pure water is added to precipitate the reaction product, and the reaction product is cooled to room temperature, filtered to separate the product, and the solid obtained is filtered and dried, and then separated and purified from the by-products by column chromatography, and the solvent is distilled off, filtered, and dried to obtain the target oligomer represented by the above formula (1-0).

[0053] Here, the phenolic aromatic compound used as the raw material of the oligomer having an aralkyl structure of this embodiment is not particularly limited, but for example, phenol, cresol, dimethylphenol, trimethylphenol, butylphenol, phenylphenol, diphenylphenol, naphthylphenol, resorcinol, methylresorcinol, catechol, butylcatechol, methoxyphenol, methoxyphenol, propylphenol, pyrogallol, thymol, biphenol, naphthol, methylnaphthol, methoxynaphthol, dihydroxynaphthalene, etc. are mentioned. Phenol, cresol, butylphenol, diphenylphenol are preferable, phenol, cresol, butylphenol are more preferable, and phenol is most preferable. Moreover, pyrene alcohol is not very preferable from the viewpoint of dissolution stability.

[0054] In addition, examples of the crosslinking agent having a methylene bond used as a raw material for the oligomer having an aralkyl structure in this embodiment include halogenated methyl aromatic compounds and alkoxymethyl aromatic compounds. Specific examples include 1,3-bis(alkoxymethyl)phenyl, 1,3-bis(halogenated methyl)phenyl, etc. (wherein the alkoxy group has 1 to 4 carbon atoms), 4,4'-bis(alkoxymethyl)biphenyl, 2,2'-bis(alkoxymethyl)biphenyl, 2,4'-bis(alkoxymethyl)biphenyl, 4,4'-bis(halogenated methyl)biphenyl, 2,2'-bis(halogenated methyl)biphenyl, 2,4'-bis(halogenated methyl)biphenyl, etc. (wherein the alkoxy group has 1 to 4 carbon atoms), 2,6-bis(alkoxymethyl)naphthalene, 2,7-bis(alkoxymethyl)naphthalene, 1,5 ... dimethyl)biphenyl, 2,6-bis(halogenated methyl)naphthalene, 2,7-bis(halogenated methyl)naphthalene, 1,8-bis(halogenated methyl)naphthalene (provided that the alkoxy group has 1 to 4 carbon atoms), paraxylylene glycol dialkyl ether, metaxylylene glycol dialkyl ether, 1,4-bis(halogenated methyl)benzene, etc. (provided that the alkyl group has 1 to 4 carbon atoms), 4,4'-bis(alkoxymethyl)diphenylmethylene, 2,2'-bis(alkoxymethyl)diphenylmethylene, 2,4'-bis(alkoxymethyl)diphenylmethylene, 4,4'-bis(halogenated methyl)diphenylmethylene, 2,2'-bis(halogenated methyl)diphenylmethylene, 2,4'-bis(halogenated methyl)diphenylmethylene, etc. (provided that the alkoxy group has 1 to 4 carbon atoms).Preferred are 1,3-bis(alkoxymethyl)phenyl, 1,3-bis(halogenated methyl)phenyl, 4,4'-bis(alkoxymethyl)biphenyl, 4,4'-bis(halogenated methyl)biphenyl, 2,6-bis(alkoxymethyl)naphthalene, 2,6-bis(halogenated methyl)naphthalene, and 4,4'-bis(alkoxymethyl)diphenylmethylene, more preferred are 1,3-bis(halogenated methyl)phenyl, 4,4'-bis(alkoxymethyl)biphenyl, 4,4'-bis(halogenated methyl)biphenyl, and 2,6-bis(halogenated methyl)naphthalene, and most preferred is 4,4'-bis(halogenated methyl)biphenyl. From the viewpoint of improving planarization, biphenyl raw materials, which have an increased molecular free volume and a decreased viscosity, are more preferred than naphthalene raw materials, which are condensed aromatic rings. These crosslinking agents may be used alone or in combination of two or more.

[0055] The oligomer represented by the above formula (1-0) is preferably highly soluble in a solvent from the viewpoint of making it easier to apply a wet process. More specifically, when 1-methoxy-2-propanol (PGME) and / or propylene glycol monomethyl ether acetate (PGMEA) is used as the solvent, the oligomer preferably has a solubility of 10% by mass or more in the solvent. Here, the solubility in PGME and / or PGMEA is defined as "mass of resin ÷ (mass of resin + mass of solvent) × 100 (mass%)". For example, 10 g of the oligomer represented by the above formula (1-0) is evaluated as soluble in 90 g of PGMEA when the solubility of the oligomer represented by the formula (1-0) in PGMEA is "10 mass % or more," and it is evaluated as insoluble when the solubility is "less than 10 mass %."

[0056] The composition of the present embodiment contains the oligomer of the present embodiment, so that the composition can be applied to a wet process and has excellent heat resistance and planarization properties. Furthermore, the composition of the present embodiment contains the oligomer of the present embodiment, so that the deterioration of the film during high-temperature baking is suppressed, and a lithography film having excellent etching resistance against oxygen plasma etching and the like can be formed. Furthermore, the composition of the present embodiment has excellent adhesion to the resist layer, so that an excellent resist pattern can be formed. Therefore, the composition of the present embodiment is preferably used for forming an underlayer film.

[0057] [Method for purifying film-forming materials for lithography] The lithographic film-forming material (oligomer) can be purified by washing with an acidic aqueous solution. The purification method includes a step of dissolving the lithographic film-forming material in an organic solvent that is not miscible with water to obtain an organic phase, contacting the organic phase with an acidic aqueous solution to perform an extraction treatment (first extraction step), thereby transferring the metal content contained in the organic phase containing the lithographic film-forming material and the organic solvent to the aqueous phase, and then separating the organic phase from the aqueous phase. The purification can significantly reduce the content of various metals in the lithographic film-forming material of the present invention.

[0058] The organic solvent that is not miscible with water is not particularly limited, but is preferably an organic solvent that can be safely used in the semiconductor manufacturing process. The amount of the organic solvent used is usually about 1 to 100 times by mass relative to the compound used.

[0059] Specific examples of the organic solvent to be used include those described in International Publication No. 2015 / 080240. Among these, toluene, 2-heptanone, cyclohexanone, cyclopentanone, methyl isobutyl ketone, propylene glycol monomethyl ether acetate, ethyl acetate, etc. are preferred, and cyclohexanone and propylene glycol monomethyl ether acetate are particularly preferred. These organic solvents can be used alone or in combination of two or more.

[0060] The acidic aqueous solution is appropriately selected from among aqueous solutions in which a generally known organic or inorganic compound is dissolved in water. For example, those described in International Publication No. 2015 / 080240 can be mentioned. These acidic aqueous solutions can be used alone or in combination of two or more. Examples of the acidic aqueous solution include mineral acid aqueous solutions and organic acid aqueous solutions. Examples of the mineral acid aqueous solution include an aqueous solution containing one or more selected from the group consisting of hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid. Examples of the organic acid aqueous solution include an aqueous solution containing one or more selected from the group consisting of acetic acid, propionic acid, oxalic acid, malonic acid, succinic acid, fumaric acid, maleic acid, tartaric acid, citric acid, methanesulfonic acid, phenolsulfonic acid, p-toluenesulfonic acid, and trifluoroacetic acid. In addition, as the acidic aqueous solution, an aqueous solution of sulfuric acid, nitric acid, and a carboxylic acid such as acetic acid, oxalic acid, tartaric acid, or citric acid is preferable, and an aqueous solution of sulfuric acid, oxalic acid, tartaric acid, or citric acid is more preferable, and an aqueous solution of oxalic acid is particularly preferable. It is considered that polycarboxylic acids such as oxalic acid, tartaric acid, and citric acid coordinate with metal ions and generate a chelating effect, so that more metals can be removed. In addition, the water used here is preferably one with a low metal content, such as ion-exchanged water, in line with the object of the present invention.

[0061] The pH of the acidic aqueous solution is not particularly limited, but if the acidity of the aqueous solution is too high, it may adversely affect the oligomer used, which is not preferable. The pH range is usually about 0 to 5, and more preferably about 0 to 3.

[0062] The amount of the acidic aqueous solution used is not particularly limited, but if the amount is too small, it is necessary to perform extraction many times to remove the metal, and conversely, if the amount of the aqueous solution is too large, the total amount of the solution becomes large, which may cause problems in operation. The amount of the aqueous solution used is usually 10 to 200 parts by mass, preferably 20 to 100 parts by mass, based on the solution of the film-forming material for lithography.

[0063] The metal components can be extracted by contacting the acidic aqueous solution with a solution (B) containing a film-forming material for lithography and an organic solvent that is arbitrarily immiscible with water.

[0064] The temperature during the extraction treatment is usually in the range of 20 to 90°C, and preferably in the range of 30 to 80°C. The extraction operation is carried out, for example, by thoroughly mixing the mixture by stirring or the like, and then allowing it to stand. As a result, the metal content contained in the solution containing the oligomer and the organic solvent is transferred to the aqueous phase. This operation also reduces the acidity of the solution, making it possible to suppress the deterioration of the oligomer.

[0065] After the extraction treatment, the solution phase containing the oligomer and the organic solvent is separated from the aqueous phase, and the solution containing the organic solvent is recovered by decantation or the like. The time for standing is not particularly limited, but if the time for standing is too short, the separation of the solution phase containing the organic solvent and the aqueous phase becomes poor, which is not preferable. Usually, the time for standing is 1 minute or more, more preferably 10 minutes or more, and even more preferably 30 minutes or more. In addition, the extraction treatment may be performed only once, but it is also effective to repeat the operations of mixing, standing, and separation several times.

[0066] When such an extraction treatment is carried out using an acidic aqueous solution, it is preferable that the organic phase containing the organic solvent extracted and recovered from the aqueous solution after the treatment is further subjected to an extraction treatment with water (second extraction step). The extraction operation is carried out by mixing thoroughly by stirring or the like and then leaving it to stand. The resulting solution is separated into a solution phase containing the oligomer and the organic solvent and an aqueous phase, and the solution phase is recovered by decantation or the like. In addition, the water used here is preferably one with a low metal content, such as ion-exchanged water, in line with the object of the present invention. The extraction treatment may be carried out only once, but it is also effective to repeat the operations of mixing, leaving to stand, and separating several times. In addition, the ratio of both used in the extraction treatment, and the conditions such as temperature and time are not particularly limited, but may be the same as in the case of the contact treatment with the acidic aqueous solution.

[0067] Water mixed in the thus obtained solution containing the film-forming material for lithography and the organic solvent can be easily removed by performing an operation such as vacuum distillation. In addition, the concentration of the compound can be adjusted to any desired concentration by adding an organic solvent as necessary.

[0068] The method for obtaining only the film-forming material for lithography from the obtained solution containing the organic solvent can be performed by a known method such as removal under reduced pressure, separation by reprecipitation, a combination thereof, etc. If necessary, known treatments such as a concentration operation, a filtration operation, a centrifugation operation, a drying operation, etc. can be performed.

[0069] The composition for forming an underlayer film of this embodiment contains a solvent in addition to the oligomer of this embodiment. The composition for forming an underlayer film of this embodiment may also contain a crosslinking agent, a crosslinking promoter, an acid generator, a basic compound, and other components as necessary. These components will be described below.

[0070] [solvent] The composition for forming the underlayer film in this embodiment contains a solvent. The solvent is not particularly limited as long as the oligomer of this embodiment can be dissolved in the solvent. Here, since the oligomer of this embodiment has excellent solubility in organic solvents as described above, various organic solvents are preferably used. Specific examples of the solvent include those described in International Publication No. 2018 / 016614.

[0071] Among the solvents, from the viewpoint of safety, one or more selected from the group consisting of cyclohexanone, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, methyl hydroxyisobutyrate, and anisole are preferred.

[0072] The content of the solvent is not particularly limited, but from the viewpoints of solubility and film formation, it is preferably 100 to 10,000 parts by mass, more preferably 200 to 5,000 parts by mass, and even more preferably 200 to 1,000 parts by mass relative to 100 parts by mass of the oligomer of the present embodiment.

[0073] [Crosslinking agent] The composition for forming the underlayer film of this embodiment may contain a crosslinking agent from the viewpoint of suppressing intermixing, etc.

[0074] The crosslinking agent is not particularly limited, and examples thereof include phenol compounds, epoxy compounds, cyanate compounds, amino compounds, benzoxazine compounds, acrylate compounds, melamine compounds, guanamine compounds, glycoluril compounds, urea compounds, isocyanate compounds, and azide compounds. Specific examples of these crosslinking agents include those described in International Publication No. 2018 / 016614 and International Publication No. 2013 / 024779. These crosslinking agents are used alone or in combination of two or more. Among these, condensed aromatic ring-containing phenol compounds are more preferred from the viewpoint of improving etching resistance. Furthermore, methylol group-containing phenol compounds are more preferred from the viewpoint of improving planarization.

[0075] The methylol group-containing phenol compound used as the crosslinking agent is preferably one represented by the following formula (11-1) or (11-2) from the viewpoint of improving flattening properties. [ka]

[0076] In the crosslinking agent represented by the general formula (11-1) or (11-2), V is a single bond or an n-valent organic group, R2 and R4 each independently represent a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and R3 and R5 each independently represent an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms. n is an integer of 2 to 10, and each r is independently an integer of 0 to 6.

[0077] Specific examples of the general formula (11-1) or (11-2) include compounds represented by the following formulae: However, the general formula (11-1) or (11-2) is not limited to the compounds represented by the following formulae. [ka] [ka] [ka]

[0078] In the present embodiment, the content of the crosslinking agent is not particularly limited, but is preferably 0.1 to 100 parts by mass, more preferably 5 to 50 parts by mass, and even more preferably 10 to 40 parts by mass, relative to 100 parts by mass of the composition for forming the underlayer film. By having the content of the crosslinking agent within the above range, the occurrence of a mixing phenomenon with the resist layer tends to be suppressed, and the antireflection effect tends to be enhanced, and the film formability after crosslinking tends to be improved.

[0079] [Crosslinking accelerator] The underlayer film-forming composition of the present embodiment may contain a crosslinking accelerator to accelerate the crosslinking reaction (curing reaction) as necessary. Examples of the crosslinking accelerator include a radical polymerization initiator.

[0080] The radical polymerization initiator may be a photopolymerization initiator that initiates radical polymerization by light, or a thermal polymerization initiator that initiates radical polymerization by heat. Examples of the radical polymerization initiator include at least one selected from the group consisting of ketone-based photopolymerization initiators, organic peroxide-based polymerization initiators, and azo-based polymerization initiators. Such radical polymerization initiators are not particularly limited, and examples thereof include those described in WO 2018 / 016614.

[0081] In the present embodiment, the content of the crosslinking accelerator is not particularly limited, but is preferably 0.1 to 100 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 5 parts by mass, relative to 100 parts by mass of the composition for forming the underlayer film. By having the content of the crosslinking accelerator within the above range, the occurrence of a mixing phenomenon with the resist layer tends to be suppressed, and the antireflection effect tends to be enhanced, and the film formability after crosslinking tends to be improved.

[0082] [Acid generator] The composition for forming the underlayer film of this embodiment may contain an acid generator from the viewpoint of further promoting the crosslinking reaction by heat. As the acid generator, there are known ones that generate an acid by thermal decomposition, ones that generate an acid by light irradiation, and the like, and either one can be used. As the acid generator, for example, those described in International Publication No. 2013 / 024779 can be used. Among these, more preferable from the viewpoint of improving etching resistance.

[0083] The content of the acid generator in the composition for forming an underlayer film is not particularly limited, but is preferably 0.1 to 50 parts by mass, more preferably 0.5 to 40 parts by mass, relative to 100 parts by mass of the composition for forming an underlayer film. When the content of the acid generator is within the above range, the crosslinking reaction tends to be enhanced, and the occurrence of the mixing phenomenon with the resist layer tends to be suppressed.

[0084] [Basic compounds] The composition for forming an underlayer film of this embodiment may contain a basic compound from the viewpoint of improving storage stability, etc.

[0085] The basic compound plays a role of preventing a small amount of acid generated from the acid generator from proceeding with a crosslinking reaction, that is, plays a role of a quencher for the acid. The storage stability of the composition for forming the underlayer film is improved. Such a basic compound is not particularly limited, but may be, for example, one described in International Publication No. 2013 / 024779.

[0086] The content of the basic compound in the composition for forming an underlayer film of the present embodiment is not particularly limited, but is preferably 0.001 to 2 parts by mass, more preferably 0.01 to 1 part by mass, relative to 100 parts by mass of the composition for forming an underlayer film. When the content of the basic compound is within the above range, the storage stability tends to be improved without excessively impairing the crosslinking reaction.

[0087] [Other additives] The underlayer film-forming composition of this embodiment may contain other resins and / or compounds for the purpose of imparting curability by heat or light or controlling absorbance. Such other resins and / or compounds are not particularly limited, and examples thereof include naphthol resins, xylene resins, naphthol-modified resins, and phenol-modified resins of naphthalene resins; polyhydroxystyrene, dicyclopentadiene resins, (meth)acrylates, dimethacrylates, trimethacrylates, tetramethacrylates, vinylnaphthalene, polyacenaphthylene, and other naphthalene rings, phenanthrenequinone, fluorene, and other biphenyl rings, thiophene, indene, and other heterocyclic rings having heteroatoms or resins not containing aromatic rings; rosin-based resins, cyclodextrins, adamantane (poly)ols, tricyclodecane (poly)ols, and derivatives thereof, and other resins or compounds containing alicyclic structures. The lithography film-forming material of this embodiment may contain known additives. Examples of known additives include, but are not limited to, heat and / or light curing catalysts, polymerization inhibitors, flame retardants, fillers, coupling agents, thermosetting resins, light curing resins, dyes, pigments, thickeners, lubricants, defoamers, leveling agents, ultraviolet absorbers, surfactants, colorants, and nonionic surfactants.

[0088] [Undercoat for lithography] The underlayer film for lithography in this embodiment is formed from the composition for forming an underlayer film in this embodiment.

[0089] [Method of forming resist pattern] The method for forming a resist pattern of the present embodiment includes an underlayer film forming step of forming an underlayer film on a substrate using the composition for forming an underlayer film of the present embodiment, a photoresist layer forming step of forming at least one photoresist layer on the underlayer film formed in the underlayer film forming step, and a step of irradiating a predetermined region of the photoresist layer formed in the photoresist layer forming step with radiation and developing the same. The method for forming a resist pattern of the present embodiment can be used to form various patterns, and is preferably a method for forming an insulating film pattern.

[0090] [Circuit pattern formation method] The circuit pattern forming method of the present embodiment includes an underlayer film forming step of forming an underlayer film on a substrate using the underlayer film forming composition of the present embodiment, an intermediate layer film forming step of forming an intermediate layer film on the underlayer film formed in the underlayer film forming step, a photoresist layer forming step of forming at least one photoresist layer on the intermediate layer film formed in the intermediate layer film forming step, a resist pattern forming step of irradiating a predetermined region of the photoresist layer formed in the photoresist layer forming step with radiation and developing it to form a resist pattern, an intermediate layer film pattern forming step of etching the intermediate layer film using the resist pattern formed in the resist pattern forming step as a mask to form an intermediate layer film pattern, an underlayer film pattern forming step of etching the underlayer film using the intermediate layer film pattern formed in the intermediate layer film pattern forming step as a mask to form an underlayer film pattern, and a substrate pattern forming step of etching the substrate using the underlayer film pattern formed in the underlayer film pattern forming step as a mask to form a pattern on the substrate.

[0091] The underlayer film for lithography of the present embodiment is formed from the composition for forming the underlayer film of the present embodiment. The method for forming the underlayer film is not particularly limited, and a known method can be applied. For example, the composition for forming the underlayer film of the present embodiment is applied to a substrate by a known coating method such as spin coating or screen printing, a printing method, or the like, and then the organic solvent is removed by volatilization, or the like, to form the underlayer film.

[0092] When forming the underlayer film, it is preferable to bake the underlayer film in order to suppress the occurrence of mixing with the resist upper layer film and to promote the crosslinking reaction. In this case, the baking temperature is not particularly limited, but is preferably in the range of 80 to 450°C, more preferably 200 to 400°C. In addition, the baking time is also not particularly limited, but is preferably in the range of 10 to 300 seconds. The thickness of the underlayer film can be appropriately selected depending on the required performance, and is not particularly limited, but is preferably 30 to 20,000 nm, more preferably 50 to 15,000 nm.

[0093] The baking is preferably carried out in an inert gas environment, for example, in a nitrogen or argon atmosphere, which can increase the heat resistance and etching resistance of the underlayer film for lithography.

[0094] After preparing the underlayer film, in the case of a two-layer process, it is preferable to prepare a silicon-containing resist layer or a monolayer resist made of hydrocarbon on the underlayer film, and in the case of a three-layer process, it is preferable to prepare a silicon-containing intermediate layer on the underlayer film, and further prepare a silicon-free monolayer resist layer on the silicon-containing intermediate layer.In this case, the photoresist material for forming this resist layer can be a known one.

[0095] As a silicon-containing resist material for a two-layer process, from the viewpoint of oxygen gas etching resistance, a positive photoresist material is preferably used which uses a silicon atom-containing polymer such as a polysilsesquioxane derivative or a vinylsilane derivative as a base polymer, and further contains an organic solvent, an acid generator, and if necessary, a basic compound, etc. Here, as the silicon atom-containing polymer, a known polymer used in this type of resist material can be used.

[0096] As the silicon-containing intermediate layer for the three-layer process, a polysilsesquioxane-based intermediate layer is preferably used. By giving the intermediate layer an effect as an anti-reflection film, reflection tends to be effectively suppressed. For example, in a 193 nm exposure process, if a material containing many aromatic groups and having high substrate etching resistance is used as the underlayer film, the k value tends to be high and the substrate reflection tends to be high, but by suppressing reflection with the intermediate layer, the substrate reflection can be reduced to 0.5% or less. As the intermediate layer having such an anti-reflection effect, it is not limited to the following, but for 193 nm exposure, a polysilsesquioxane that is crosslinked by acid or heat and has a light-absorbing group having a phenyl group or a silicon-silicon bond introduced therein is preferably used.

[0097] An intermediate layer formed by a Chemical Vapour Deposition (CVD) method can also be used. As an intermediate layer produced by a CVD method and having a high effect as an anti-reflection film, for example, a SiON film is known, but is not limited to the following. In general, it is easier and more cost-effective to form an intermediate layer by a wet process such as a spin coating method or screen printing than by a CVD method. The upper layer resist in the three-layer process may be either a positive type or a negative type, and the same resist as a commonly used single layer resist can be used.

[0098] Furthermore, the underlayer film in this embodiment can be used as an anti-reflection film for a normal single-layer resist or as a base material for suppressing pattern collapse. Since the underlayer film has excellent etching resistance for base processing, it can also be expected to function as a hard mask for base processing.

[0099] When forming a resist layer using the photoresist material, a wet process such as spin coating or screen printing is preferably used, as in the case of forming the underlayer film. After applying the resist material by spin coating or the like, pre-baking is usually performed, and this pre-baking is preferably performed at 80 to 180° C. for 10 to 300 seconds. Thereafter, exposure is performed according to a conventional method, followed by post-exposure baking (PEB) and development to obtain a resist pattern. The thickness of the resist film is not particularly limited, but is generally preferably 30 to 500 nm, more preferably 50 to 400 nm.

[0100] The exposure light may be appropriately selected depending on the photoresist material used. In general, high energy rays having a wavelength of 300 nm or less, specifically, excimer lasers having wavelengths of 248 nm, 193 nm, and 157 nm, soft X-rays having wavelengths of 3 to 20 nm, electron beams, X-rays, and the like can be used.

[0101] The resist pattern formed by the above-mentioned method is one in which pattern collapse is suppressed by the underlayer film, and therefore, by using the underlayer film of this embodiment, a finer pattern can be obtained and the exposure dose required to obtain the resist pattern can be reduced.

[0102] Next, etching is performed using the obtained resist pattern as a mask. Gas etching is preferably used for etching the lower layer film in the two-layer process. Etching using oxygen gas is suitable for gas etching. In addition to oxygen gas, it is also possible to add inert gases such as He and Ar, or CO, CO2, NH3, SO2, N2, NO2, and H2 gases. Gas etching can also be performed using only CO, CO2, NH3, N2, NO2, and H2 gases without using oxygen gas. In particular, the latter gas is preferably used for sidewall protection to prevent undercutting of the pattern sidewall.

[0103] On the other hand, gas etching is also preferably used for etching the middle layer in the three-layer process. The gas etching can be the same as that described in the two-layer process. In particular, the processing of the middle layer in the three-layer process is preferably performed using a fluorocarbon-based gas and a resist pattern as a mask. Then, as described above, the processing of the lower layer film can be performed by, for example, performing oxygen gas etching using the middle layer pattern as a mask.

[0104] Here, when forming an inorganic hard mask intermediate layer film as the intermediate layer, a silicon oxide film, a silicon nitride film, or a silicon oxynitride film (SiON film) is formed by a CVD method, an ALD method, or the like. The method for forming the nitride film is not limited to the following, but for example, the methods described in JP-A-2002-334869 and WO2004 / 066377 can be used. A photoresist film can be formed directly on such an intermediate layer film, but an organic anti-reflective coating (BARC) may be formed on the intermediate layer film by spin coating, and a photoresist film may be formed on the organic anti-reflective coating (BARC).

[0105] As the intermediate layer, a polysilsesquioxane-based intermediate layer is also preferably used. By making the resist intermediate layer film have the effect of an anti-reflection film, reflection tends to be effectively suppressed. The specific material of the polysilsesquioxane-based intermediate layer is not limited to the following, but for example, those described in JP-A-2007-226170 and JP-A-2007-226204 can be used.

[0106] The next etching of the substrate can also be performed by a conventional method, for example, if the substrate is SiO2 or SiN, etching can be performed mainly with fluorocarbon-based gas, and if it is p-Si, Al, or W, etching can be performed mainly with chlorine- or bromine-based gas. When etching the substrate with fluorocarbon-based gas, the silicon-containing resist of the two-layer resist process and the silicon-containing intermediate layer of the three-layer process are stripped at the same time as the substrate is processed. On the other hand, when the substrate is etched with chlorine- or bromine-based gas, the silicon-containing resist layer or the silicon-containing intermediate layer is stripped separately, and generally, dry etching stripping with fluorocarbon-based gas is performed after the substrate is processed.

[0107] The underlayer film in this embodiment has a feature of being excellent in etching resistance of the substrate. The substrate can be appropriately selected from known ones and is not particularly limited, but examples thereof include Si, α-Si, p-Si, SiO2, SiN, SiON, W, TiN, Al, etc. The substrate may be a laminate having a film to be processed (substrate to be processed) on a base material (support). Examples of such a film to be processed include various low-k films and their stopper films, such as Si, SiO2, SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si, etc., and a film made of a material different from that of the base material (support) is usually used. The thickness of the substrate or film to be processed is not particularly limited, but is usually preferably about 50 to 1,000,000 nm, more preferably 75 to 50,000 nm.

[0108] [Permanent resist film] The resist permanent film of this embodiment includes the composition of this embodiment. The resist permanent film formed by applying the composition of this embodiment is suitable as a permanent film that remains in the final product after forming a resist pattern as necessary. Specific examples of permanent films include solder resist, packaging material, underfill material, package adhesive layer of circuit elements, and adhesive layer between integrated circuit elements and circuit boards in semiconductor device cans, and thin film transistor protective film, liquid crystal color filter protective film, black matrix, spacer, etc. in thin display related products. In particular, the resist permanent film containing the composition of this embodiment has the excellent advantages of being excellent in heat resistance and moisture resistance, and being less susceptible to contamination by sublimation components. In particular, in display materials, it is a material that combines high sensitivity, high heat resistance, and moisture absorption reliability with little image quality deterioration due to important contamination.

[0109] When the underlayer film forming composition of the present embodiment is used for a permanent resist film, in addition to the curing agent, various additives such as other resins, surfactants, dyes, fillers, crosslinking agents, and dissolution promoters can be added as necessary, and the composition can be dissolved in an organic solvent to form a composition for a permanent resist film.

[0110] The composition for forming an underlayer film of this embodiment can be prepared by blending the above-mentioned components and mixing them using a stirrer, etc. Furthermore, when the composition of this embodiment contains a filler or a pigment, it can be prepared by dispersing or mixing using a dispersing device such as a dissolver, a homogenizer, or a three-roll mill. EXAMPLES

[0111] Hereinafter, the present embodiment will be described in more detail with reference to Synthesis Examples and Examples, but the present embodiment is not limited to these examples in any way.

[0112] (molecular weight) The weight average molecular weight (Mw) and dispersity (Mw / Mn) of the oligomer of the present embodiment were determined in terms of polystyrene by gel permeation chromatography (GPC) analysis under the following measurement conditions. Equipment: Shodex GPC-101 type (Showa Denko K.K. product) Column: KF-80M x 3 Eluent: THF 1mL / min Temperature: 40℃

[0113] (Softening point measurement) The softening point was measured using the following equipment: Equipment used: FP83HT Dropping Point / Softening Point Measurement System manufactured by Mettler Toledo Co., Ltd. Measurement conditions: Heating rate 2°C / min Measurement method: Measure according to the FP83HT manual. Specifically, pour the molten sample into the sample cup and cool and solidify it. Insert the cartridges into the top and bottom of the cup filled with the sample and insert it into the furnace. The resin softens and flows down the orifice, and the temperature when the bottom end of the resin passes through the light path is detected by a photocell as the softening point.

[0114] (Melt Viscosity Measurement) The melt viscosity at 150°C was measured using the following equipment. Equipment used: Brookfield B-type viscometer DV2T, Eiko Seiki Co., Ltd. Measurement temperature: 150℃ Measurement method: Set the furnace temperature of the B-type viscometer to 150°C and weigh a specified amount of sample into a cup. A cup containing a weighed sample is placed in a furnace to melt the resin, and a spindle is inserted from above. The spindle is rotated, and the point at which the displayed viscosity value becomes stable is read as the melt viscosity.

[0115] (Synthesis Example 1) Synthesis of NAFP-AL Under nitrogen, 1,4-bis(chloromethyl)benzene (28.8g, 0.148mol, Tokyo Chemical Industry Co., Ltd.), 1-naphthol (30.0g, 0.1368mol, Tokyo Chemical Industry Co., Ltd.), and paratoluenesulfonic acid monohydrate (5.7g, 0.029mol, Tokyo Chemical Industry Co., Ltd.) were added to a 300mL four-neck flask, and 150.4g of propylene glycol monomethyl ether acetate (hereinafter referred to as PGMEA) was further charged, stirred, and heated until reflux was confirmed to dissolve and initiate polymerization. After 16 hours, the mixture was allowed to cool to 60°C and then reprecipitated into 1600g of methanol. The resulting precipitate was filtered and dried in a vacuum dryer at 60°C for 16 hours to obtain 38.6 g of the target oligomer having the structural unit represented by the following formula (NAFP-AL). The weight average molecular weight of the resulting oligomer measured by GPC in terms of polystyrene was 2020, and the polydispersity was 1.86. The viscosity was 0.12 Pa s, and the softening point was 68°C.

[0116] [ka]

[0117] (Synthesis Example 2) Synthesis of PBIF-AL Under nitrogen, phenol (311.9 g, 3.32 mol, Tokyo Chemical Industry Co., Ltd.) and 4,4'-dichloromethylbiphenyl (200.0 g, 0.80 mol, Tokyo Chemical Industry Co., Ltd.) were charged into a four-neck flask with an outlet at the bottom, and the temperature was raised, and the inside of the system became uniform at 80°C, and HCl began to be generated. The system was held at 100°C for 3 hours, and then heat-treated at 150°C for 1 hour. HCl generated by the reaction was evaporated directly to the outside of the system and trapped with alkaline water. At this stage, there was no unreacted 4,4'-dichloromethylbiphenyl remaining, and it was confirmed by gas chromatography that all had reacted. After the reaction was completed, the pressure was reduced to remove the HCl and unreacted phenol remaining in the system. Finally, the pressure was reduced to 30 torr and 150°C, and the remaining phenol was no longer detected by gas chromatography. While the reaction product was kept at 150°C, about 30 g of the reaction product was slowly dropped from the bottom outlet of the flask onto a stainless steel pad kept at room temperature by air cooling. After 1 minute, the reaction product was rapidly cooled to 30°C on the stainless steel pad, and a solidified polymer was obtained. The solidified material was removed and the stainless steel pad was cooled by air cooling so that the surface temperature of the stainless steel pad would not rise due to the heat of the polymer. This air cooling and solidification process was repeated nine times, and 213.3 g of an oligomer having a structural unit represented by the following formula (PBIF-AL) was obtained. The weight average molecular weight of the obtained oligomer measured by GPC in terms of polystyrene was 3100, and the polydispersity was 1.33. The viscosity was 0.06 Pa s, and the softening point was 39°C.

[0118] [ka]

[0119] (Synthesis Example 2) Synthesis of p-CBIF-AL Under nitrogen, p-cresol (359.0 g, 3.32 mol, Tokyo Chemical Industry Co., Ltd.) and 4,4'-dichloromethylbiphenyl (200.0 g, 0.80 mol, Tokyo Chemical Industry Co., Ltd.) were charged into a four-neck flask with an outlet at the bottom, and the temperature was raised, and the inside of the system became uniform at 80°C, and HCl generation began. The system was held at 100°C for 3 hours, and then heat-treated at 150°C for 1 hour. HCl generated by the reaction was evaporated directly to the outside of the system and trapped with alkaline water. At this stage, there was no unreacted 4,4'-dichloromethylbiphenyl remaining, and it was confirmed by gas chromatography that all had reacted. After the reaction was completed, the pressure was reduced to remove the HCl and unreacted phenol remaining in the system. Finally, the pressure was reduced to 30 torr and 150°C, and the remaining phenol was no longer detected by gas chromatography. While the reaction product was kept at 150°C, about 30 g of the reaction product was slowly dropped from the bottom outlet of the flask onto a stainless steel pad kept at room temperature by air cooling. After 1 minute, the product was rapidly cooled to 30°C on the stainless steel pad, and a solidified polymer was obtained. The solidified material was removed and the stainless steel pad was cooled by air cooling so that the surface temperature of the stainless steel pad would not rise due to the heat of the polymer. This air cooling and solidification process was repeated nine times, and 223.1 g of an oligomer having a structural unit represented by the following formula (p-CBIF-AL) was obtained. The weight average molecular weight of the obtained oligomer measured by GPC in terms of polystyrene was 2556, and the polydispersity was 1.21. The viscosity was 0.03 Pa s, and the softening point was 35°C. [ka]

[0120] (Synthesis Example 4) Synthesis of n-BBIF-AL Under nitrogen, 4-butylphenol (498.7 g, 3.32 mol, Tokyo Chemical Industry Co., Ltd.) and 4,4'-dichloromethylbiphenyl (200.0 g, 0.80 mol, Tokyo Chemical Industry Co., Ltd.) were charged into a four-neck flask with an outlet at the bottom, and the temperature was raised, and the inside of the system became uniform at 80°C, and HCl generation began. The system was held at 100°C for 3 hours, and then heat-treated at 150°C for 1 hour. HCl generated by the reaction was evaporated directly to the outside of the system and trapped with alkaline water. At this stage, there was no unreacted 4,4'-dichloromethylbiphenyl remaining, and it was confirmed by gas chromatography that all had reacted. After the reaction was completed, the pressure was reduced to remove the HCl and unreacted phenol remaining in the system. Finally, the pressure was reduced to 30 torr and 150°C, and the remaining phenol was no longer detected by gas chromatography. While the reaction product was kept at 150°C, about 30 g of the reaction product was slowly dropped from the bottom outlet of the flask onto a stainless steel pad kept at room temperature by air cooling. After 1 minute, the reaction product was rapidly cooled to 30°C on the stainless steel pad, and a solidified polymer was obtained. The solidified material was removed and the stainless steel pad was cooled by air cooling so that the surface temperature of the stainless steel pad would not rise due to the heat of the polymer. This air cooling and solidification process was repeated nine times, and 267.5 g of an oligomer having a structural unit represented by the following formula (n-BBIF-AL) was obtained. The weight average molecular weight of the obtained oligomer measured by GPC in terms of polystyrene was 2349, and the polydispersity was 1.19. The viscosity was 0.01 Pa s, and the softening point was 30°C. [ka]

[0121] (Synthesis Example 5) Synthesis of NAFBIF-AL Under nitrogen, 1-naphthol (478.0 g, 3.32 mol, Tokyo Chemical Industry Co., Ltd.) and 4,4'-dichloromethylbiphenyl (200.0 g, 0.80 mol, Tokyo Chemical Industry Co., Ltd.) were charged into a four-neck flask with an outlet at the bottom, and the temperature was raised, and the inside of the system became uniform at 80°C, and HCl generation began. The system was held at 100°C for 3 hours, and then heat-treated at 150°C for 1 hour. HCl generated by the reaction was evaporated directly to the outside of the system and trapped with alkaline water. At this stage, there was no unreacted 4,4'-dichloromethylbiphenyl remaining, and it was confirmed by gas chromatography that all had reacted. After the reaction was completed, the pressure was reduced to remove the HCl and unreacted phenol remaining in the system. Finally, the pressure was reduced to 30 torr and 140°C, and the remaining phenol was no longer detected by gas chromatography. While the reaction product was kept at 150°C, about 30 g of the product was slowly dropped from the bottom outlet of the flask onto a stainless steel pad kept at room temperature by air cooling. After 1 minute, the product was rapidly cooled to 30°C on the stainless steel pad, and a solidified polymer was obtained. The solidified material was removed and the stainless steel pad was cooled by air cooling so that the surface temperature of the stainless steel pad would not rise due to the heat of the polymer. This air cooling and solidification process was repeated nine times, and 288.3 g of an oligomer having a structural unit represented by the following formula (NAFBIF-AL) was obtained. The weight average molecular weight of the polymer measured by GPC in terms of polystyrene was 3450, and the polydispersity was 1.40. The viscosity was 0.15 Pa s, and the softening point was 60°C.

[0122] [ka]

[0123] [Examples 1 to 5, Comparative Example 1] The following solubility test and heat resistance evaluation were carried out on the above oligomer having an aralkyl structure and a phenol novolak resin (PSM4357 manufactured by Gun-ei Chemical Co., Ltd.) as Comparative Example 1. The results are shown in Table 1.

[0124] (Solubility evaluation) The oligomer of the present embodiment was dissolved in propylene glycol monomethyl ether acetate (PGMEA) to give a 10% by mass solution at 23° C. After that, the solution was left to stand at 10° C. for 30 days, and the solubility was evaluated according to the following criteria. Evaluation A: No precipitates were observed by visual inspection C: Precipitation confirmed by visual inspection

[0125] (Evaluation of heat resistance) Using an EXSTAR6000TG-DTA device manufactured by SII NanoTechnology, approximately 5 mg of the sample was placed in an aluminum non-sealed container, and the sample was heated to 500°C at a heating rate of 10°C / min in a nitrogen gas (300 ml / min) stream to measure the amount of thermal weight loss. From a practical standpoint, the following A or B rating is preferred. <Evaluation criteria> A: Thermal weight loss at 400℃ is less than 10% B: Thermal weight loss at 400℃ is 10% to 25% C: Thermal weight loss at 400℃ is more than 25%

[0126] [Examples 1-1 to 5-3, Comparative Example 1-1] Next, compositions for forming an underlayer film for lithography were prepared, each having the composition shown in Table 2. Next, these compositions for forming an underlayer film for lithography were spin-coated onto a silicon substrate, and then baked at 240° C. for 60 seconds and then at 400° C. for 120 seconds to prepare an underlayer film with a thickness of 200 nm. Next, the curability was evaluated according to the following evaluation criteria.

[0127] [Cureability test] The underlayer films obtained from the compositions for forming an underlayer film for lithography in Examples 1-1 to 5-3 and Comparative Example 1-1 were immersed in PGMEA for 120 seconds, and then dried on a hot plate at 110° C. for 60 seconds, after which the remaining film state was confirmed. The results are shown in Table 2. <Evaluation criteria> A: Visually confirm that there is residual film C: Visually confirm that there is no remaining film

[0128] The acid generator, crosslinking agent and organic solvent used were as follows. Acid generator: Midori Chemical Co., Ltd. product "Di-tert-butyldiphenyliodonium nonafluoromethanesulfonate" (listed as "DTDPI" in the table). Crosslinking agent: Sanwa Chemical Co., Ltd. product "Nicalac MX270" (listed as "Nicalac" in the table). Honshu Chemical Industry Co., Ltd. product "TMOM-BP" (listed as "TMOM" in the table) Etching resistance condensed aromatic ring crosslinking agent (listed as "condensed" in the table) Organic solvent: propylene glycol monomethyl ether acetate (referred to as "PGMEA" in the table).

[0129] For each of the obtained underlayer films, an etching test was carried out under the conditions shown below to evaluate the etching resistance. The evaluation results are shown in Table 2.

[0130] [Etching test] Etching equipment: Samco International "RIE-10NR" Output: 50W Pressure: 20Pa Time: 2 minutes Etching Gas Ar gas flow rate: CF4 gas flow rate: O2 gas flow rate = 50:5:5 (sccm)

[0131] [Evaluation of etching resistance] The etching resistance was evaluated according to the following procedure. First, an underlayer film containing a phenol novolac resin was prepared under the same conditions as in Example 1-1, except that a phenol novolac resin (PSM4357 manufactured by Gun-ei Chemical Co., Ltd.) was used instead of the oligomer used in Example 1-1. Then, the above-mentioned etching test was performed on the underlayer film containing the phenol novolac resin, and the etching rate (etching speed) was measured. Next, the above-mentioned etching test was performed on the underlayer films of each Example and Comparative Example, and the etching rate was measured. Then, the etching resistance of each Example and Comparative Example was evaluated according to the following evaluation criteria, based on the etching rate of the underlayer film containing the phenol novolac resin. <Evaluation criteria> S: Etching rate is less than -15% compared to the novolac underlayer. A: Etching rate is less than -10% compared to the novolac underlayer. B: Etching rate is -10% to +5% compared to the underlayer of novolac C: Etching rate is more than +5% compared to the underlayer of novolac

[0132] [Evaluation of filling ability of stepped substrates] The embedding ability into a stepped substrate was evaluated according to the following procedure. The composition for forming an underlayer film for lithography was applied to a SiO2 substrate with a thickness of 80 nm and a 60 nm line and space, and baked at 240°C for 60 seconds to form a 90 nm underlayer film. A cross section of the obtained film was cut out and observed with an electron microscope to evaluate the embedding ability into a stepped substrate. The results are shown in Table 3. <Evaluation criteria> A: The underlayer film is embedded without any defects in the uneven parts of the 60 nm line and space SiO2 substrate. C: There is a defect in the uneven portion of the 60 nm line and space SiO2 substrate, and the underlayer film is not filled in.

[0133] [Flatness evaluation] The film-forming compositions obtained above were applied to a SiO2 stepped substrate having a mixture of a trench (aspect ratio: 1.5) with a width of 100 nm, a pitch of 150 nm, and a depth of 150 nm, and a trench (open space) with a width of 5 μm and a depth of 180 nm. The substrate was then baked at 240° C. for 120 seconds in an air atmosphere to form a resist underlayer film with a thickness of 200 nm. The shape of the resist underlayer film was observed with a scanning electron microscope (Hitachi High-Technologies Corporation's "S-4800"), and the difference (ΔFT) between the maximum and minimum film thicknesses of the resist underlayer film on the trench or space was measured. The results are shown in Table 3. <Evaluation criteria> S: ΔFT<10nm (best flatness) A:10nm≦ΔFT<20nm (good flatness) B: 20nm≦ΔFT<40nm (flatness is good) C:40nm≦ΔFT (poor flatness) [Table 1] [Table 2] [Table 3]

[0134] [Examples 4 to 9] Each solution of the underlayer film forming material for lithography prepared in each of the above Examples 1-1 to 5-3 was applied onto a SiO2 substrate with a thickness of 300 nm, and baked at 240°C for 60 seconds and then at 400°C for 120 seconds to form an underlayer film with a thickness of 70 nm. An ArF resist solution was applied onto this underlayer film, and baked at 130°C for 60 seconds to form a photoresist layer with a thickness of 140 nm. The ArF resist solution was prepared by mixing 5 parts by mass of a compound represented by the following formula (11), 1 part by mass of triphenylsulfonium nonafluoromethanesulfonate, 2 parts by mass of tributylamine, and 92 parts by mass of PGMEA. The compound represented by the following formula (11) was prepared by dissolving 4.15 g of 2-methyl-2-methacryloyloxyadamantane, 3.00 g of methacryloyloxy-γ-butyrolactone, 2.08 g of 3-hydroxy-1-adamantyl methacrylate, and 0.38 g of azobisisobutyronitrile in 80 mL of tetrahydrofuran to obtain a reaction solution. The reaction solution was polymerized for 22 hours under a nitrogen atmosphere at a reaction temperature of 63° C., and then the reaction solution was dropped into 400 mL of n-hexane. The resin thus produced was coagulated and purified, and the resulting white powder was filtered and dried overnight at 40° C. under reduced pressure to obtain the compound.

[0135] [ka]

[0136] The numbers in the formula (11) indicate the ratio of each constituent unit.

[0137] Next, the photoresist layer was exposed to light using an electron beam lithography system (ELS-7500, 50 keV, manufactured by Elionix), baked (PEB) at 115°C for 90 seconds, and developed with a 2.38 mass% aqueous solution of tetramethylammonium hydroxide (TMAH) for 60 seconds to obtain a positive resist pattern.

[0138] The results of observing defects in the resulting resist patterns of 55 nmL / S (1:1) and 80 nmL / S (1:1) are shown in Table 4. In the table, "good" indicates that no major defects were observed in the formed resist pattern, and "poor" indicates that major defects were observed in the formed resist pattern.

[0139] [Comparative Example 2] A photoresist layer was formed directly on a SiO2 substrate in the same manner as in Example 7, except that no underlayer film was formed, to obtain a positive resist pattern. The results are shown in Table 4.

[0140] [Table 4]

[0141] As is clear from Table 1, it was confirmed that Examples 1 to 5, which used any of the oligomers having an aralkyl structure according to the present embodiment, were good in both solubility and heat resistance, whereas Comparative Example 1, which used a phenol novolac resin, had poor heat resistance.

[0142] As is clear from Tables 2 and 3, it was confirmed that the underlayer film formed using any of the compositions for forming an underlayer film for lithography (Examples 1-1 to 5-3) made of an oligomer having an aralkyl structure according to this embodiment not only has excellent curing properties and etching resistance, but also has good embedding properties and planarization properties, compared to the underlayer film made of a phenol novolac resin in Comparative Example 1-1. It is possible to achieve particularly excellent planarization by self-curing without requiring a crosslinking agent or an acid generator.

[0143] Also, as is clear from Table 4, in Examples 4 to 18 using any of the oligomers having an aralkyl structure according to the present embodiment, it was confirmed that the resist pattern shape after development was good and no major defects were observed. Furthermore, it was confirmed that each of Examples 4 to 18 was significantly superior in both resolution and sensitivity compared to Comparative Example 2 in which no underlayer film was formed. Here, the fact that the resist pattern shape after development was good indicates that the underlayer film-forming material for lithography used in Examples 4 to 18 has good adhesion to the resist material (photoresist material, etc.).

[0144] [Examples 19 to 33] A solution of the lithography underlayer film forming material of each of Examples 1-1 to 5-3 was applied onto a SiO2 substrate having a thickness of 300 nm, and baked at 240°C for 60 seconds and then at 400°C for 120 seconds to form an underlayer film having a thickness of 80 nm. A silicon-containing intermediate layer material was applied onto this underlayer film, and baked at 200°C for 60 seconds to form an intermediate layer film having a thickness of 35 nm. Furthermore, the above-mentioned ArF resist solution was applied onto this intermediate layer film, and baked at 130°C for 60 seconds to form a photoresist layer having a thickness of 150 nm. As the silicon-containing intermediate layer material, a silicon atom-containing polymer described in <Synthesis Example 1> of JP-A-2007-226170 was used. Next, the photoresist layer was exposed to light using a mask with an electron beam lithography system (ELIONIX; ELS-7500, 50 keV), baked at 115°C for 90 seconds (PEB), and developed with a 2.38 mass% tetramethylammonium hydroxide (TMAH) aqueous solution for 60 seconds to obtain a positive resist pattern of 55 nmL / S (1:1). After that, using the obtained resist pattern as a mask, dry etching of the silicon-containing intermediate layer film (SOG) was performed using RIE-10NR manufactured by Samco International, followed by dry etching of the underlayer film using the obtained silicon-containing intermediate layer film pattern as a mask, and dry etching of the SiO2 film using the obtained underlayer film pattern as a mask.

[0145] The etching conditions for each are as follows. Etching conditions for resist pattern onto resist intermediate layer film Output: 50W Pressure: 20Pa Time: 1 min Etching Gas Ar gas flow rate: CF4 gas flow rate: O2 gas flow rate = 50:8:2 (sccm) Etching conditions for resist intermediate film pattern onto resist underlayer film Output: 50W Pressure: 20Pa Time: 2 minutes Etching Gas Ar gas flow rate: CF4 gas flow rate: O2 gas flow rate = 50:5:5 (sccm) Etching conditions for resist underlayer film pattern onto SiO2 film Output: 50W Pressure: 20Pa Time: 2 minutes Etching Gas Ar gas flow rate: C5F 12 Gas flow rate: C2F6 gas flow rate: O2 gas flow rate =50:4:3:1(sccm)

[0146] [evaluation] The cross section of the pattern obtained as described above (i.e., the shape of the SiO2 film after etching) was observed using an electron microscope (S-4800) manufactured by Hitachi, Ltd. The observation results are shown in Table 5. In the table, "good" indicates that no major defects were observed in the cross section of the formed pattern, and "poor" indicates that major defects were observed in the cross section of the formed pattern.

[0147] [Table 5]

[0148] Example 34 Acid Purification of NAFBIF-AL In a 1000 mL capacity four-neck flask (bottom-opening type), 150 g of the solution (10 mass%) obtained in Synthesis Example 5 in PGMEA was charged and heated to 80 ° C. while stirring. Next, 37.5 g of an aqueous oxalic acid solution (pH 1.3) was added, stirred for 5 minutes, and then allowed to stand for 30 minutes. As a result, the oil phase and the aqueous phase were separated, and the aqueous phase was removed. After repeating this operation once, 37.5 g of ultrapure water was charged into the obtained oil phase, stirred for 5 minutes, and then allowed to stand for 30 minutes, and the aqueous phase was removed. After repeating this operation three times, the flask was heated to 80 ° C. and the pressure inside was reduced to 200 hPa or less, thereby concentrating and distilling off the residual water and PGMEA. Then, the solution was diluted with EL grade PGMEA (a reagent manufactured by Kanto Chemical Co., Ltd.) and the concentration was adjusted to 10 mass%, thereby obtaining a PGMEA solution of NAFBIF-AL with reduced metal content.

[0149] (Comparative Example 3) Purification of NAFBIF-AL with ultrapure water The same procedure as in Example 34 was carried out except that ultrapure water was used instead of the aqueous oxalic acid solution, and the concentration was adjusted to 10 mass % to obtain a PGMEA solution of NAFBIF-AL.

[0150] The contents of various metals were measured by ICP-MS for the 10 mass % PGMEA solution of NAFBIF-AL before treatment, and for the solutions obtained in Example 34 and Comparative Example 3. The measurement results are shown in Table 6.

[0151] [Table 6]

Claims

1. a: an oligomer having an aralkyl structure represented by the following formula (1-2), and b: Solvent A composition for forming an underlayer film for lithography comprising the above compound. [Case 1] (In the formula, Ar 2 represents a phenylene group, a naphthylene group, or a biphenylene group; When Ar 2 is a phenylene group, Ar 1 is a biphenylene group; When Ar 2 is a naphthylene group or a biphenylene group, Ar 1 is a phenylene group, a naphthylene group or a biphenylene group; R a is a substituent of Ar 1 and each independently may be the same or different; R a represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; R b is a substituent of Ar 2 and each R b may be the same or different; R b represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; n represents an integer from 1 to 500; r represents an integer of 1 to 3; p represents a positive integer; q represents a positive integer.

2. Ar 2 represents a phenylene group, a naphthylene group, or a biphenylene group, Ar 2 is a phenylene group, Ar 1 represents a biphenylene group, Ar 2 is a naphthylene group or a biphenylene group, Ar 1 represents a phenylene group, a naphthylene group, or a biphenylene group, R a represents a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent; R b 2. The composition for forming an underlayer film for lithography according to claim 1, wherein represents a hydrogen atom or an alkyl group having 1 to 30 carbon atoms which may have a substituent.

3. 3. The composition for forming an underlayer film for lithography according to claim 1, wherein the oligomer having an aralkyl structure represented by the formula (1-2) is represented by the following formula (2) or formula (3): [Case 2] (In formula (2), Ar 1 , R a , r, p, and n are the same as those in formula (1-2). [C3] (In formula (3), Ar 1 , R a , r, p, and n are the same as those in formula (1-2).

4. The composition for forming an underlayer film for lithography according to claim 3 , wherein the oligomer having an aralkyl structure represented by formula (2) is represented by the following formula (4): [C4] (In formula (4), R 1each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; m 1 represents an integer from 1 to 3, n represents an integer from 1 to 50.

5. The composition for forming an underlayer film for lithography according to claim 3 , wherein the oligomer having an aralkyl structure represented by formula (3) is represented by the following formula (5): [C5] (In formula (5), R 2 each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; m 2 represents an integer from 1 to 3, n represents an integer from 1 to 50.

6. The composition for forming an underlayer film for lithography according to claim 3 , wherein the oligomer having an aralkyl structure represented by the formula (2) is represented by the following formula (6): [C6] (In formula (6), R 3 each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; m 3 represents an integer from 1 to 5, n represents an integer from 1 to 50.

7. The composition for forming an underlayer film for lithography according to claim 3 , wherein the oligomer having an aralkyl structure represented by formula (3) is represented by the following formula (7): [C7] (In formula (7), R 4 each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms which may have a substituent, an aryl group having 6 to 30 carbon atoms which may have a substituent, an alkenyl group having 2 to 30 carbon atoms which may have a substituent, an alkynyl group having 2 to 30 carbon atoms which may have a substituent, an alkoxy group having 1 to 30 carbon atoms which may have a substituent, an acyl group having 1 to 30 carbon atoms which may have a substituent, a group containing a carboxyl group having 1 to 30 carbon atoms which may have a substituent, an amino group having 0 to 30 carbon atoms which may have a substituent, a halogen atom, a cyano group, a nitro group, a thiol group, or a heterocyclic group; m 4 represents an integer from 1 to 5, n represents an integer from 1 to 50.

8. The composition for forming an underlayer film for lithography according to any one of claims 1 to 7, further comprising an acid generator.

9. The composition for forming an underlayer film for lithography according to any one of claims 1 to 8, further comprising a crosslinking agent.

10. An underlayer film for lithography formed using the composition for forming an underlayer film for lithography according to any one of claims 1 to 9.

11. A step of forming an underlayer film on a substrate using the composition for forming an underlayer film for lithography according to any one of claims 1 to 9; forming at least one photoresist layer on the underlayer film; and exposing predetermined areas of the photoresist layer to radiation and developing; A method for forming a resist pattern comprising the steps of:

12. A step of forming an underlayer film on a substrate using the composition for forming an underlayer film for lithography according to any one of claims 1 to 9; forming an intermediate layer film on the underlayer film using a resist intermediate layer film material containing silicon atoms; forming at least one photoresist layer on the intermediate layer film; irradiating predetermined areas of the photoresist layer with radiation and developing to form a resist pattern; a step of etching the intermediate layer film using the resist pattern as a mask; a step of etching the underlayer film using the obtained intermediate layer film pattern as an etching mask; and a step of forming a pattern on the substrate by etching the substrate using the obtained underlayer film pattern as an etching mask; A method for forming a circuit pattern comprising the steps of:

13. A step of dissolving the oligomer having an aralkyl structure according to any one of claims 1 to 9 in a solvent to obtain an organic phase; contacting the organic phase with an acidic aqueous solution to extract impurities in the oligomer; Including, The purification method, wherein the solvent used in the step of obtaining the organic phase comprises a solvent that is immiscible with water.

Citation Information

Patent Citations

  • Resist underlayer film material and pattern forming method

    JP2004271838A

  • Resist underlayer film material and pattern forming method

    JP2005250434A

  • Composition for forming base film for lithography and method for forming multilayer resist pattern

    WO2009072465A1

  • Underlayer film-forming material for lithography, underlayer film for lithography, and pattern formation method

    WO2013024779A1

  • Resist-underlayer-film-forming composition used in multilayer resist process, resist underlayer film, method for forming same, and pattern-formation method