Film-forming composition, resist underlayer film, film-forming method, resist pattern forming method, organic underlayer film reversal pattern forming method, method for producing film-forming composition, and method for forming metal-containing film pattern

A film-forming composition with a metal and nitrogen-containing organic compound improves storage stability and embeddability, addressing cracking issues in thick films, enhancing performance in semiconductor and liquid crystal device production.

JP7589682B2Active Publication Date: 2024-11-26JSR CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021522832
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-04
Filing Date
2020-05-27
Publication Date
2024-11-26
Estimated Expiration
2040-05-27

AI Technical Summary

Technical Problem

Conventional metal alkoxide hydrolysis condensates exhibit insufficient storage stability and embeddability into patterned substrates, particularly when forming thick films, leading to issues such as cracking and poor coating properties.

Method used

A film-forming composition comprising a metal compound, a nitrogen-containing organic compound, and a solvent, where the nitrogen-containing compound has specific structural features, enhances storage stability and embeddability, suppressing film thickness changes and cracking.

Benefits of technology

The composition achieves excellent storage stability, embeddability, film thickness change suppression, etching resistance, and removability, suitable for forming thick films without cracking, particularly in semiconductor and liquid crystal device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589682000001
    Figure 0007589682000001
  • Figure 0007589682000002
    Figure 0007589682000002
  • Figure 0007589682000003
    Figure 0007589682000003
Patent Text Reader

Abstract

The objective of the present invention is to provide: a film forming composition having excellent storage stability and embedding properties; a resist underlayer film; a film formation method; a resist pattern forming method; a resist underlayer film reverse pattern forming method; a method for producing a film forming composition; and a metal-containing film pattern forming method. The present invention is a film forming composition which contains a metal compound, a nitrogen-containing organic compound, and a solvent, wherein the nitrogen-containing organic compound is: a compound having a nitrogen atom, an aliphatic hydrocarbon group, and at least two hydroxy groups; a compound having a nitrogen-containing aromatic heterocycle and at least one hydroxy group; or a mixture thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] The present invention relates to a film-forming composition, a resist underlayer film, a film-forming method, a resist pattern forming method, an organic underlayer film reversal pattern forming method, a method for producing a film-forming composition, and a method for forming a metal-containing film pattern. [Technical field]

[0002] In the manufacture of semiconductor elements and the like, it has been proposed to use a hydrolysis condensate of a metal alkoxide (JP 2014-134592 A). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-134592 A Summary of the Invention [Problem to be solved by the invention]

[0004] The above-mentioned conventional hydrolysis and condensation products of metal alkoxides are insufficient in terms of storage stability and embedding ability into a substrate on which a pattern is formed.

[0005] The present invention has been made based on the above circumstances, and an object of the present invention is to provide a film-forming composition, a resist underlayer film, a film-forming method, a resist pattern forming method, an organic underlayer film reversal pattern forming method, a method for producing a film-forming composition, and a method for forming a metal-containing film pattern, which are excellent in storage stability and embedding ability. [Means for solving the problem]

[0006] The invention made to solve the above-mentioned problems is a film-forming composition (hereinafter also referred to as "compound (A)") that contains a metal compound (hereinafter also referred to as "compound (A)"), a nitrogen-containing organic compound (hereinafter also referred to as "compound (X)"), and a solvent (hereinafter also referred to as "solvent (C)"), in which the compound (X) is a compound having a nitrogen atom, an aliphatic hydrocarbon group, and two or more hydroxy groups (hereinafter also referred to as compound (X1)), a compound having a nitrogen-containing aromatic heterocycle and one or more hydroxy groups (hereinafter also referred to as compound (X2)), or a mixture thereof.

[0007] Another invention made to solve the above-mentioned problems is a resist underlayer film formed from a film-forming composition, the film-forming composition containing a metal compound (compound [A]), a nitrogen-containing organic compound (compound [X]), and a solvent (solvent [C]), wherein the compound [X] is a compound having a nitrogen atom, an aliphatic hydrocarbon group, and two or more hydroxy groups (compound [X1]), a compound having a nitrogen-containing aromatic heterocycle and one or more hydroxy groups (compound [X2]), or a mixture thereof.

[0008] Yet another invention made to solve the above-mentioned problems is a film-forming method comprising a step of directly or indirectly applying a film-forming composition to a substrate, the film-forming composition containing a metal compound (compound [A]), a nitrogen-containing organic compound (compound [X]), and a solvent (solvent [C]), wherein the compound [X] is a compound having a nitrogen atom, an aliphatic hydrocarbon group, and two or more hydroxyl groups (compound [X1]), a compound having a nitrogen-containing aromatic heterocycle and one or more hydroxyl groups (compound [X2]), or a mixture thereof.

[0009] Still another invention made to solve the above-mentioned problems is a method for forming a resist pattern, comprising the steps of: applying a film-forming composition directly or indirectly to a substrate; applying an organic resist film-forming composition directly or indirectly to a resist underlayer film formed by the film-forming composition-applying step; exposing the organic resist film formed by the organic resist film-forming composition-applying step to radiation; and developing the exposed organic resist film, wherein the film-forming composition contains a metal compound (compound [A]), a nitrogen-containing organic compound (compound [X]), and a solvent (solvent [C]), and the compound [X] is a compound having a nitrogen atom, an aliphatic hydrocarbon group, and two or more hydroxy groups (compound [X1]), a compound having a nitrogen-containing aromatic heterocycle and one or more hydroxy groups (compound [X2]), or a mixture thereof.

[0010] Yet another invention made to solve the above problems is a method for forming an organic underlayer film reversal pattern, comprising the steps of forming an organic underlayer film directly or indirectly on a substrate, forming a resist pattern directly or indirectly on the organic underlayer film, forming a pattern on the organic underlayer film by etching using the resist pattern as a mask, forming an organic underlayer film reversal pattern forming film directly on the organic underlayer film pattern using a composition for forming an organic underlayer film reversal pattern, and forming an organic underlayer film reversal pattern by removing the organic underlayer film pattern, wherein the composition for forming an organic underlayer film reversal pattern contains a metal compound (compound [A]), a nitrogen-containing organic compound (compound [X]), and a solvent (solvent [C]), and the compound [X] is a compound having a nitrogen atom, an aliphatic hydrocarbon group, and two or more hydroxyl groups (compound [X1]), a compound having a nitrogen-containing aromatic heterocycle and one or more hydroxyl groups (compound [X2]), or a mixture thereof.

[0011] Yet another invention made to solve the above-mentioned problems is a method for producing a film-forming composition, comprising the steps of mixing a metal alkoxide with a nitrogen-containing organic compound (an [X] compound) and adding water to the mixture obtained in the above-mentioned mixing step, wherein the [X] compound is a compound having a nitrogen atom, an aliphatic hydrocarbon group, and two or more hydroxy groups (an [X1] compound), a compound having a nitrogen-containing aromatic heterocycle and one or more hydroxy groups (an [X2] compound), or a mixture thereof.

[0012] Yet another invention made to solve the above-mentioned problems is a method for forming a metal-containing film pattern, comprising the steps of: applying a composition for forming a metal-containing film directly or indirectly to a substrate; forming an organic underlayer film directly or indirectly on the metal-containing film formed by the above-mentioned step of applying the composition for forming a metal-containing film; forming a resist pattern directly or indirectly on the organic underlayer film; and forming a pattern in the metal-containing film by etching using the resist pattern as a mask, wherein the composition for forming a metal-containing film contains a metal compound (compound [A]), a nitrogen-containing organic compound (compound [X]), and a solvent (solvent [C]), and the nitrogen-containing organic compound is a compound having a nitrogen atom, an aliphatic hydrocarbon group, and two or more hydroxy groups (compound [X1]), a compound having a nitrogen-containing aromatic heterocycle and one or more hydroxy groups (compound [X2]), or a mixture thereof. Effect of the Invention

[0013] The film-forming composition of the present invention has excellent storage stability and embedding ability.

[0014] Furthermore, according to the film-forming composition of the present invention, a film having excellent film thickness change suppression properties, etching resistance, and removability can be formed. The resist underlayer film of the present invention is formed by the film-forming composition, and therefore has excellent film thickness change suppression properties, etching resistance, and removability. According to the film-forming method of the present invention, a film having excellent film thickness change suppression properties, etching resistance, and removability can be formed. According to the resist pattern forming method of the present invention, since the film-forming composition is used, a good resist pattern can be formed. According to the resist underlayer film reversal pattern forming method of the present invention, since the film-forming composition is used as a resist underlayer film reversal pattern forming composition, a good reversal pattern can be formed. According to the method for producing the film-forming composition of the present invention, a film-forming composition having excellent storage stability and embedding properties can be produced.

[0015] According to the method for forming a metal-containing film pattern of the present invention, since the film-forming composition is used as the metal-containing film-forming composition, a good metal-containing film pattern can be formed.

[0016] Therefore, they can be suitably used in lithography processes in the manufacture of various electronic devices such as semiconductor devices and liquid crystal devices, which require further miniaturization. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present inventors have found that there is a need for a film-forming composition capable of forming a thick film, for example, 50 nm or more, as a metal-containing film. However, the present inventors have newly found that the film-forming composition using the above-mentioned conventional hydrolysis condensation product of metal alkoxide does not have good coatability when forming a thick film, and when a thick film is formed, a problem occurs in that cracks occur in the film.

[0018] The inventors conducted extensive research to solve the above-mentioned problems and surprisingly found that the film-forming composition of the present invention has good coatability when forming a thick film, and can suppress the occurrence of cracks in the film even when a thick film is formed.

[0019] Therefore, the film-forming composition of the present invention has excellent coating properties when forming a thick film. Furthermore, the film-forming composition of the present invention can form a thick film in which the occurrence of cracks is suppressed. In this specification, the term "thick film" or "thick film" means a film having an average thickness of 50 nm or more. The average thickness is a value measured using a spectroscopic ellipsometer (JAWOOLLAM's "A2000D").

[0020] Furthermore, according to the method for forming a metal-containing film pattern of the present invention, by using the film-forming composition as a metal-containing film-forming composition, a thick film in which the occurrence of cracks is suppressed can be formed, and therefore a good metal-containing film pattern can be formed.

[0021] <Composition (J)> The composition (J) contains the compound [A], the compound [X], and the solvent [C]. The composition (J) may contain other optional components as long as they do not impair the effects of the present invention.

[0022] Composition (J) contains the compound [A], the compound [X], and the solvent [C], and is therefore excellent in storage stability and embeddability. The reason why composition (J) has the above-mentioned effect due to the above-mentioned configuration is not necessarily clear, but it can be inferred, for example, as follows. That is, the nitrogen atom and hydroxyl group of the compound [X] are coordinated to the metal atom of the compound [A] or are present around this metal atom, which can increase the fluidity during application, and as a result, the embeddability of the composition (J) is thought to be improved. In addition, the nitrogen atom and hydroxyl group of the compound [X] are coordinated to the metal atom of the compound [A] or are present around this metal atom, which can suppress the deterioration of the compound [A] over time, and as a result, the storage stability of the composition (J) is thought to be improved.

[0023] In addition, the film formed by the composition (J) is excellent in thickness change suppression, etching resistance, and removability. The reason why the film formed by the composition (J) has the above effects is not necessarily clear, but it can be inferred as follows, for example. That is, it is considered that the etching resistance and removability of the film formed by the composition (J) are improved by the nitrogen atom and hydroxyl group of the [X] compound being coordinated to the metal atom of the [A] compound or being present around this metal atom. In addition, it is considered that the deterioration of the [A] compound over time can be suppressed by the nitrogen atom and hydroxyl group of the [X] compound being coordinated to the metal atom of the [A] compound or being present around this metal atom, and as a result, the thickness change suppression of the film formed by the composition (J) is improved.

[0024] Furthermore, composition (J) has excellent coatability when forming a thick film. The reason for this effect is believed to be that the nitrogen atom and hydroxyl group of compound [X] are coordinated to the metal atom of compound [A] or are present around this metal atom, thereby increasing the fluidity during coating.

[0025] In addition, the film formed by the composition (J) can suppress the occurrence of cracks even if it is a thick film. The reason for this effect is thought to be that the nitrogen atom and hydroxyl group of the compound [X] are coordinated to the metal atom of the compound [A] or are present around this metal atom, and therefore, when the film is heated, the deterioration of the film can be suppressed, and as a result, the occurrence of cracks can be suppressed.

[0026] Each component contained in the composition (J) will be described below.

[0027] [[A] compound] The [A] compound is a metal alkoxide (hereinafter also referred to as "the [M] compound"), a hydrolysis condensation product of the [M] compound, or a mixture thereof. Here, "hydrolysis condensation" refers to a reaction in which an alkoxy group of the [M] compound is hydrolyzed and converted to -OH, and one water molecule is eliminated from the two resulting -OH by dehydration condensation to form an -O- bond. The composition (J) can contain one or more [A] compounds.

[0028] In the composition (J), the [X] compound may be coordinated to a metal atom (hereinafter also referred to as "metal atom (L)") contained in the [A] compound, or may be free from the metal atom (L) contained in the [A] compound. Specifically, for example, a part of the [X] compound may be coordinated to the metal atom (L) in the [A] compound, and the rest of the [X] compound may be free from the metal atom (L) in the [A] compound. When the [X] compound is coordinated to the metal atom (L) in the [A] compound, the [X] compound may be coordinated to the metal atom (L) as a monodentate ligand or a polydentate ligand.

[0029] Examples of the metal atom (L) contained in the compound [A] include those belonging to Groups 2 to 14, Periods 3 to 7 of the periodic table.

[0030] Group 2 metal atoms (L) include magnesium, calcium, strontium, barium, etc. Examples of the Group 3 metal atom (L) include lanthanide atoms such as scandium, yttrium, and lanthanum, and actinide atoms such as actinium. Examples of the metal atom (L) in Group 4 include titanium, zirconium, and hafnium. Examples of the metal atom (L) in Group 5 include vanadium, niobium, and tantalum. Examples of the metal atom (L) in Group 6 include chromium, molybdenum, and tungsten. Group 7 metal atoms (L) include manganese, rhenium, etc. Group 8 metal atoms (L) include iron, ruthenium, osmium, etc. Examples of the metal atom (L) in Group 9 include cobalt, rhodium, and iridium. Examples of the metal atom (L) in Group 10 include nickel, palladium, and platinum. Examples of the metal atom (L) in Group 11 include copper, silver, and gold. Examples of the metal atom (L) in Group 12 include zinc, cadmium, and mercury. Examples of the metal atom (L) in Group 13 include aluminum, gallium, indium, and thallium. Examples of the metal atom (L) in Group 14 include tin and lead.

[0031] The compound [A] may have one or more kinds of metal atoms (L). The compound [M] may have one or more metal atoms (L).

[0032] Of these, the metal atom (L) is preferably one belonging to Group 3, 4 or 13 of the periodic table, and more preferably one belonging to Group 4 of the periodic table.

[0033] Examples of the alkoxy group contained in the compound [M] include a methoxy group, an ethoxy group, an n-propoxy group, an i-propoxy group, and a butoxy group.

[0034] [M] Compounds include, for example: Compounds containing titanium include diisopropoxybis(2,4-pentanedionato)titanium(IV), tetra n-butoxytitanium(IV), tetra n-propoxytitanium(IV), tetraisopropoxytitanium(IV), tri n-butoxymonostearate titanium(IV), titanium(IV) butoxide oligomer, aminopropyltrimethoxytitanium(IV), triethoxymono(2,4-pentanedionato)titanium(IV), tri-n-propoxymono(2,4-pentanedionato)titanium(IV), triisopropoxymono(2,4-pentanedionato)titanium, di-n-butoxybis(2,4-pentanedionato)titanium(IV), etc. Compounds containing zirconium include dibutoxybis(ethylacetoacetate)zirconium(IV), di-n-butoxybis(2,4-pentanedionato)zirconium(IV), tetra-n-butoxyzirconium(IV), tetra-n-propoxyzirconium(IV), tetraisopropoxyzirconium(IV), aminopropyltriethoxyzirconium(IV), 2-(3,4-epoxycyclohexyl)ethyltrimethoxyzirconium(IV), γ-glycidoxypropionate, trimethoxyzirconium(IV), 3-isocyanopropyltrimethoxyzirconium(IV), triethoxymono(2,4-pentanedionato)zirconium(IV), tri-n-propoxymono(2,4-pentanedionato)zirconium(IV), triisopropoxymono(2,4-pentanedionato)zirconium(IV), tri(3-methacryloxypropyl)methoxyzirconium(IV), tri(3-acryloxypropyl)methoxyzirconium(IV), etc. Compounds containing hafnium include diisopropoxybis(2,4-pentanedionato)hafnium(IV), tetrabutoxyhafnium(IV), tetraisopropoxyhafnium(IV), tetraethoxyhafnium(IV), and dichlorobis(cyclopentadienyl)hafnium(IV). Compounds containing tantalum include tetrabutoxytantalum(IV), pentabutoxytantalum(V), and pentaethoxytantalum(V). Compounds containing tungsten include tetrabutoxytungsten(IV), pentabutoxytungsten(V), pentamethoxytungsten(V), hexabutoxytungsten(VI), hexaethoxytungsten(VI), and dichlorobis(cyclopentadienyl)tungsten(IV). Iron-containing compounds include iron(III) chloride, Ruthenium-containing compounds include diacetato[(S)-(-)-2,2'-bis(diphenylphosphino)-1,1'-binaphthyl]ruthenium(II), Cobalt-containing compounds include dichloro[ethylenebis(diphenylphosphine)]cobalt(II), etc. Zinc-containing compounds include diisopropoxyzinc(II) and zinc acetate(II). Examples of aluminum-containing compounds include triisopropoxyaluminum(III), diisopropoxyethyl acetoacetatealuminum(III), and aluminum acetate(III). Compounds containing indium include indium acetate (III) and triisopropoxyindium (III). Compounds containing tin include tetraethyldiacetoxystannoxane, tetrabutoxytin(IV), tetraisopropoxytin(IV), and t-butyltris(diethylamido)tin(IV). An example of a compound containing germanium is tetraisopropoxygermanium(IV).

[0035] The lower limit of the content of the compound [A] is preferably 2% by mass, more preferably 4% by mass, and even more preferably 6% by mass, based on the total components contained in the composition (J).The upper limit of the content is preferably 20% by mass, more preferably 15% by mass, and even more preferably 10% by mass, based on the total components contained in the composition (J).

[0036] [[X]Compound] The [X] compound is an [X1] compound, an [X2] compound or a mixture thereof. The composition (J) may contain one or more [X] compounds.

[0037] ([X1] compound) The compound [X1] is a compound having a nitrogen atom, an aliphatic hydrocarbon group, and two or more hydroxy groups.

[0038] The compound [X1] has one or more nitrogen atoms. The number of nitrogen atoms in the compound [X1] is preferably 1 to 10, more preferably 1 to 7, and further preferably 2 to 5. In the compound [X1], the nitrogen atom is preferably bonded to a carbon atom of the aliphatic hydrocarbon group.

[0039] The compound [X1] has one or more aliphatic hydrocarbon groups. The number of aliphatic hydrocarbon groups in the compound [X1] is preferably 2 to 10, more preferably 2 to 7, and even more preferably 2 to 5. The compound [X1] preferably has an aliphatic hydrocarbon group bonded to a nitrogen atom and a hydroxyl group (i.e., interposed between a nitrogen atom and a hydroxyl group). In addition, when the compound [X1] has two or more nitrogen atoms, it is preferable that an aliphatic hydrocarbon group is bonded between each nitrogen atom (i.e., interposed between two or more nitrogen atoms). Examples of such aliphatic hydrocarbon groups include divalent aliphatic hydrocarbon groups having 1 to 10 carbon atoms.

[0040] The term "aliphatic hydrocarbon group" includes chain-like hydrocarbon groups and alicyclic hydrocarbon groups. This "hydrocarbon group" may be a saturated or unsaturated hydrocarbon group. The term "chain-like hydrocarbon group" refers to a hydrocarbon group that does not include a cyclic structure and is composed only of a chain structure, and includes both straight-chain hydrocarbon groups and branched hydrocarbon groups. The term "alicyclic hydrocarbon group" refers to a hydrocarbon group that includes only an alicyclic structure as a ring structure and does not include an aromatic ring structure, and includes both monocyclic alicyclic hydrocarbon groups and polycyclic alicyclic hydrocarbon groups. However, it is not necessary for the group to be composed only of an alicyclic structure, and it may include a chain structure as part of it.

[0041] Examples of the divalent chain hydrocarbon group having 1 to 10 carbon atoms include alkanediyl groups such as a methanediyl group, an ethanediyl group, an n-propanediyl group, an i-propanediyl group, an n-butanediyl group, an i-butanediyl group, a sec-butanediyl group, or a t-butanediyl group; alkenediyl groups such as ethenediyl, propenediyl, and butenediyl groups; Examples of the alkyl group include alkynediyl groups such as an ethynediyl group, a propynediyl group, and a butynediyl group.

[0042] Examples of the divalent alicyclic hydrocarbon group having 3 to 10 carbon atoms include monocyclic cycloalkanediyl groups such as a cyclopropanediyl group, a cyclobutanediyl group, a cyclopentanediyl group, or a cyclohexanediyl group; monocyclic cycloalkenediyl groups such as a cyclopropenediyl group, a cyclobutenediyl group, a cyclopentenediyl group, or a cyclohexenediyl group; polycyclic cycloalkanediyl groups such as a norbornanediyl group, an adamantanediyl group, or a tricyclodecanediyl group; Examples of the aryl group include polycyclic cycloalkenediyl groups such as a norbornenediyl group and a tricyclodecenediyl group.

[0043] The upper limit of the number of carbon atoms in the divalent aliphatic hydrocarbon group is preferably 10, more preferably 6, and even more preferably 4. The lower limit of the number of carbon atoms is, for example, 1.

[0044] The compound [X1] has two or more hydroxy groups. As described above, the hydroxy groups are preferably bonded to the aliphatic hydrocarbon group. The number of hydroxy groups in the compound [X1] is preferably 2 to 10, more preferably 2 to 7, and further preferably 2 to 5.

[0045] The compound [X1] may, for example, be a compound represented by the following formula (1).

[0046] [ka]

[0047] In the above formula (1), m+n is 3, m is 2 or 3, and n is 0 or 1. 1 is a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, and multiple R 1 are the same or different. R 2 is a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, or a group represented by the following formula (1-1).

[0048] [ka]

[0049] In the above formula (1-1), R 2A is a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms. p is an integer of 1 to 4. R 2B and R 2C each independently represents a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, or -R 2D -OH. 2D is a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms. When p is 2 or more, multiple R 2A are the same or different, and multiple R 2C are the same or different. * indicates the site of binding to the nitrogen atom in the above formula (1).

[0050] R 2A Examples of the divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms represented by the following formula include the groups exemplified as the divalent aliphatic hydrocarbon group in the aliphatic hydrocarbon group contained in the compound [X1] described above.

[0051] R 2B and R 2C Examples of the monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms represented by the formula (I) include a monovalent chain hydrocarbon group having 1 to 10 carbon atoms and a monovalent alicyclic hydrocarbon group having 3 to 10 carbon atoms.

[0052] Examples of the monovalent chain hydrocarbon group having 1 to 10 carbon atoms include Alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, a sec-butyl group, and a t-butyl group; alkenyl groups such as ethenyl, propenyl, and butenyl; Examples of the alkynyl group include an ethynyl group, a propynyl group, and a butynyl group.

[0053] Examples of the monovalent alicyclic hydrocarbon group having 3 to 10 carbon atoms include monocyclic cycloalkyl groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, and a cyclooctyl group; polycyclic cycloalkyl groups such as a norbornyl group, an adamantyl group, and a tricyclodecyl group; monocyclic cycloalkenyl groups such as a cyclobutenyl group, a cyclopentenyl group, or a cyclohexenyl group; Examples of the aryl group include polycyclic cycloalkenyl groups such as norbornenyl and tricyclodecenyl.

[0054] R 2D Examples of the divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms represented by the following formula include the groups exemplified as the divalent aliphatic hydrocarbon group in the above-mentioned compound [X1].

[0055] Of these, R 2B and R 2C are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or R 2D is a divalent alkyl group having 1 to 6 carbon atoms; 2D -OH is preferred.

[0056] ([X2] compound) The compound [X2] is a compound having a nitrogen-containing aromatic heterocycle and one or more hydroxyl groups. The compound [X2] has, for example, one or more divalent aliphatic hydrocarbon groups having 1 to 10 carbon atoms bonded to the nitrogen-containing aromatic heterocycle, and one or more hydroxyl groups bonded to each of the aliphatic hydrocarbon groups.

[0057] The nitrogen-containing aromatic heterocycle may be, for example, an aromatic heterocycle having only a nitrogen atom as a heteroatom, or an aromatic heterocycle having a nitrogen atom and a heteroatom other than a nitrogen atom as a heteroatom. Examples of heteroatoms other than a nitrogen atom include an oxygen atom and a sulfur atom. The nitrogen-containing aromatic heterocycle may be, for example, an aromatic heterocycle having only a nitrogen atom as a heteroatom, such as an imidazole ring, a pyridine ring, a pyrazine ring, a pyrazole ring, or a pyridazine ring, or a polycyclic nitrogen-containing aromatic heterocycle such as a quinazoline ring or a purine ring. Among these, the nitrogen-containing aromatic heterocycle may be, for example, a monocyclic nitrogen-containing aromatic heterocycle, and more preferably a pyridine ring.

[0058] The compound [X2] has one or more hydroxy groups. The hydroxy groups are preferably bonded to the nitrogen-containing aromatic heterocycle directly or via another group, and more preferably bonded to the nitrogen-containing aromatic heterocycle via another group. When the hydroxy groups are bonded to the nitrogen-containing aromatic heterocycle via another group, examples of the other group include divalent aliphatic hydrocarbon groups having 1 to 10 carbon atoms. The number of hydroxy groups in the compound [X2] is preferably 1 to 5, more preferably 1 to 3, and even more preferably 1 or 2.

[0059] Examples of the compound [X] include compounds represented by the chemical formulas (X-1) to (X-10) described below.

[0060] The lower limit of the content of the [X] compound is preferably 0.3 mol, more preferably 0.5 mol, and even more preferably 1.0 mol, relative to 1 mol of the [M] compound.The upper limit of the content is preferably 10.0 mol, more preferably 5.0 mol, and even more preferably 3.0 mol, relative to 1 mol of the [M] compound.

[0061] By setting the content of the compound [X] within the above range, it is possible to further improve the storage stability, embedding ability, suppression of film thickness change, etching resistance, and removability.

[0062] [[C] Solvent] The solvent [C] is a solvent other than the compound [X]. The solvent [C] can be used as a solvent in the production of the composition [J] described below.

[0063] The solvent [C] may be an organic solvent. Examples of the organic solvent include alcohol solvents, ketone solvents, ether solvents, ester solvents, and nitrogen-containing solvents. The composition (J) may contain one or more organic solvents [C].

[0064] Examples of the alcohol solvent include monoalcohol solvents such as methanol, ethanol, and n-propanol, and polyhydric alcohol solvents such as ethylene glycol, 1,2-propylene glycol, triethylene glycol, and tripropylene glycol.

[0065] Examples of the ketone solvent include chain ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone, and cyclic ketone solvents such as cyclohexanone.

[0066] Examples of the ether solvent include chain ether solvents such as n-butyl ether, polyhydric alcohol ether solvents such as cyclic ether solvents such as tetrahydrofuran and 1,4-dioxane, and polyhydric alcohol partial ether solvents such as propylene glycol monoethyl ether, tripropylene glycol monomethyl ether, and tetraethylene glycol monomethyl ether.

[0067] Examples of ester-based solvents include carbonate-based solvents such as diethyl carbonate, acetate monoester-based solvents such as methyl acetate and ethyl acetate, lactone-based solvents such as γ-butyrolactone, polyhydric alcohol partial ether carboxylate-based solvents such as diethylene glycol monomethyl ether acetate and propylene glycol monomethyl ether acetate, and lactate ester-based solvents such as methyl lactate and ethyl lactate.

[0068] Examples of the nitrogen-containing solvent include chain nitrogen-containing solvents such as N,N-dimethylacetamide, and cyclic nitrogen-containing solvents such as N-methylpyrrolidone.

[0069] The solvent [C] is preferably an ether-based solvent and / or an ester-based solvent, more preferably a polyhydric alcohol partial ether-based solvent and / or a polyhydric alcohol partial ether carboxylate-based solvent, and further preferably propylene glycol monoethyl ether and / or propylene glycol monomethyl ether acetate.

[0070] The lower limit of the content of the solvent [C] in the composition (J) is preferably 300 parts by mass, more preferably 500 parts by mass, and more preferably 700 parts by mass, relative to 100 parts by mass of the compound [A]. The upper limit of the content is preferably 5,000 parts by mass, more preferably 3,000 parts by mass, and more preferably 2,000 parts by mass, relative to 100 parts by mass of the compound [A].

[0071] The lower limit of the content of the solvent [C] in the composition (J) is preferably 10% by mass, more preferably 15% by mass, and even more preferably 20% by mass, relative to the composition (J).The upper limit of the content is preferably 99% by mass, and more preferably 95% by mass, relative to the composition (J).

[0072] By setting the content of the solvent [C] within the above range, the preparation of the composition (J) can be facilitated.

[0073] Composition (J) can be suitably used as a composition for forming a resist underlayer film. By using composition (J) as a composition for forming a resist underlayer film, the formed resist underlayer film has excellent film thickness change suppression properties, etching resistance, and removability. In addition, the resist underlayer film has excellent filling properties when filling gaps in a pattern.

[0074] In addition, composition (J) can be suitably used as a composition for forming an organic underlayer film reversal pattern. Since composition (J) is for forming an organic underlayer film reversal pattern, it has excellent embedding properties when forming an organic underlayer film reversal pattern. Furthermore, the formed organic underlayer film reversal pattern has excellent film thickness (pattern thickness) change suppression properties, etching resistance, and removability. Therefore, since composition (J) is for forming an organic underlayer film reversal pattern, a good reversal pattern can be formed.

[0075] As described above, composition (J) has excellent coatability, and the film formed by composition (J) suppresses the occurrence of cracks even when a thick film is formed. Therefore, composition (J) can be suitably used as a composition for forming a thick film. In this case, composition (J) can be suitably used in processes requiring a metal-containing film with a thick average thickness in the manufacture of semiconductor elements, etc. Composition (J) can be used as a composition for forming a film with an average thickness of 50 nm or more. The lower limit of the average thickness is preferably 100 nm, more preferably 500 nm, even more preferably 1,000 nm, even more preferably 3,000 nm, and particularly preferably 4,000 nm.

[0076] [Other optional ingredients] The composition (J) may contain, as components other than the compound [A], the compound [X] and the solvent [C], for example, an acid generator, a polymer additive, a surfactant and the like.

[0077] The acid generator is a compound that generates an acid upon irradiation with radiation and / or heating. The composition (J) may contain one or more types of acid generators.

[0078] Examples of the acid generator include onium salt compounds and N-sulfonyloxyimide compounds.

[0079] The composition (J) contains a polymer additive, which can improve the coatability to a substrate or an organic underlayer film. In addition, after the film formed by the composition (J) is heated, the occurrence of cracks in the film can be further suppressed. The composition (J) can contain one or more polymer additives.

[0080] Examples of the polymer additive include (poly)oxyalkylene polymer compounds, fluorine-containing polymer compounds, and non-fluorine-containing polymer compounds.

[0081] Examples of the (poly)oxyalkylene polymer compound include polyoxyalkylenes such as (poly)oxyethylene (poly)oxypropylene adducts; (poly)oxyalkyl ethers such as diethylene glycol heptyl ether, polyoxyethylene oleyl ether, polyoxypropylene butyl ether, polyoxyethylene polyoxypropylene-2-ethylhexyl ether, and oxyethylene oxypropylene adducts to higher alcohols having 12 to 14 carbon atoms; (poly)oxyalkylene (alkyl)aryl ethers such as polyoxypropylene phenyl ether and polyoxyethylene nonyl phenyl ether; alkylene ethers to acetylene alcohols such as 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 2,5-dimethyl-3-hexyne-2,5-diol, and 3-methyl-1-butyne-3-ol; (poly)oxyalkylene fatty acid esters such as diethylene glycol oleate, diethylene glycol laurate, and ethylene glycol distearate; (poly)oxyalkylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate and polyoxyethylene sorbitan trioleate; (poly)oxyalkylene alkyl (aryl) ether sulfate salts such as polyoxypropylene methyl ether sodium sulfate and polyoxyethylene dodecylphenol ether sodium sulfate; (poly)oxyalkylene alkyl phosphates such as (poly)oxyethylene stearyl phosphate; and (poly)oxyalkylene alkyl amines such as polyoxyethylene laurylamine.

[0082] Examples of the fluorine-containing polymeric compound include compounds described in JP 2011-89090 A. Examples of the fluorine-containing polymeric compound include compounds containing a repeating unit derived from a (meth)acrylate compound having a fluorine atom and a repeating unit derived from a (meth)acrylate compound having two or more (preferably five or more) alkyleneoxy groups (preferably ethyleneoxy groups, propyleneoxy groups), and the like.

[0083] Examples of non-fluorinated polymer compounds include linear or branched alkyl (meth)acrylates such as lauryl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, isooctyl (meth)acrylate, isostearyl (meth)acrylate, and isononyl (meth)acrylate; alkoxyethyl (meth)acrylates such as methoxyethyl (meth)acrylate; alkylene glycol di(meth)acrylates such as ethylene glycol di(meth)acrylate and 1,3-butylene glycol di(meth)acrylate; hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; dicyclopentenyloxyethyl (meth)acrylate; nonylphenoxypolyethylene glycol (-(CH2CHO) n -structure, n=1 to 17) and compounds containing one or more repeating units derived from a (meth)acrylate monomer such as (meth)acrylate.

[0084] By including a surfactant, the composition (J) can improve the coatability to a substrate or an organic underlayer film. In addition, after the film formed by the composition (J) is heated, the occurrence of cracks in the film can be further suppressed. The composition (J) can include one or more surfactants.

[0085] Commercially available surfactants include, for example, "Newcol 2320", "Newcol 714-F", "Newcol 723", "Newcol 2307", and "Newcol 2303" (all from Nippon Nyukazai Co., Ltd.), "Paionin D-1107-S", "Paionin D-1007", "Paionin D-1106-DIR", "New Kalgen TG310", "New Kalgen TG310", "Paionin D-6105-W", "Paionin D-6112", "Paionin D-6512" (all from Takemoto Oil Co., Ltd.), "Surfynol 420", "Surfynol 440", "Surfynol 465", "Surfynol 2502" (all from Nippon Air Products Co., Ltd.), "Megafac F171", "Megafac F172", "Megafac F173", "Megafac F176", "Megafac F177", "Megafac F141", "Megafac F142", "Megafac F143", "Megafac F144", "Megafac F145", "Megafac F146", "Megafac F147", "Megafac F148", "Megafac F149", "Megafac F200", "Megafac F201" (all from Nippon Air Products Co., Ltd.), "Megafac F202" (all from Nippon Air Products Co., Ltd.), "Megafac F203" (all from Nippon Air Products Co., Ltd.), "Megafac F204" (all from Nippon Air Products Co., Ltd.), "Megafac F205" (all from Nippon Air Products Co., Ltd.), "Megafac F206" (all from Nippon Air Products Co., Ltd.), "Megafac F207" (all from Nippon Air Products Co., Ltd.), "Megafac F208" (all from Nippon Air Products Co., Ltd.), These include F144, F30, F437, F475, F479, F482, F562, F563, F780, R-40, DS-21, RS-56, RS-90 and RS-72-K (all from DIC Corporation), Fluorard FC430 and FC431 (all from Sumitomo 3M Limited), Asahiguard AG710, Surflon S-382, SC-101, SC-102, SC-103, SC-104, SC-105 and SC-106 (all from AGC Corporation), FTX-218 and NBX-15 (Neos Corporation).

[0086] When composition (J) contains other optional components, the content of the other optional components in composition (J) can be appropriately determined depending on the type of the other optional components used, etc. The upper limit of the content of the other optional components is preferably 30 parts by mass, more preferably 20 parts by mass, per 100 parts by mass of the total of the compound [A] and the compound [X].

[0087] <Method of producing the composition> The method for producing the composition (composition (J)) includes a step of mixing the compound [M] and the compound [X] (hereinafter also referred to as the "mixing step"), and a step of adding water to the mixture obtained in the mixing step (hereinafter also referred to as the "water addition step").

[0088] The method for producing the composition may further include a step of diluting the mixture obtained in the mixing step with solvent [B] (hereinafter, "dilution step") after the mixing step and before the water addition step. The method for producing the composition may further include a step of adding solvent [C] to the mixture obtained in the water addition step (hereinafter, also referred to as "solvent addition step") after the water addition step, and a step of removing excess water and excess solvent [B] from the mixture obtained in the solvent addition step (hereinafter, also referred to as "solvent removal step"). The method for producing the composition may further include a step of adding solvent [C] (hereinafter, also referred to as "solvent re-addition step") after the solvent removal step.

[0089] [Mixing process] In this step, the [M] compound and the [X] compound are mixed. Specifically, for example, the [X] compound is dropped into the [M] compound over a predetermined time, heated at a predetermined temperature, and then cooled to 30°C or less. The predetermined time can be set appropriately. For example, the lower limit of the predetermined dropping time is preferably 10 minutes, more preferably 20 minutes. On the other hand, the upper limit of the predetermined dropping time is preferably 60 minutes, more preferably 40 minutes. The predetermined temperature can be set appropriately. For example, the lower limit of the predetermined heating temperature is preferably 45°C, more preferably 50°C. On the other hand, the upper limit of the predetermined heating temperature is preferably 75°C, more preferably 70°C.

[0090] In the method for producing the composition, the [M] compound and the [X] compound are mixed in a mixing step, and water is added in a water addition step described below to cause the hydrolysis and condensation reaction of the [M] compound to proceed. In other words, the [M] compound and the [X] compound are mixed in advance, and the hydrolysis and condensation reaction of the [X] compound is caused to proceed in the presence of the [X] compound, whereby a composition (J) having excellent embeddability and storage stability can be prepared.

[0091] [Dilution process] In this process, after the mixing process, the mixture obtained in the mixing process is diluted with the solvent [B]. Specifically, the mixture obtained in the mixing process is diluted with the solvent [B] so that the compound [M] has a predetermined concentration. By providing the dilution process in the method for producing the composition, the concentration of the compound [M] can be adjusted, and as a result, the film thickness of the metal-containing film can be adjusted.

[0092] The [B] solvent is not particularly limited as long as it can dissolve or disperse the [M] compound, the [A] compound, and other components contained as necessary. Examples of the [B] solvent include alcohol solvents, ketone solvents, ether solvents, ester solvents, and nitrogen-containing solvents. Examples of these solvents include the same ones as those exemplified as the [C] solvent contained in the above-mentioned composition (J). In this step, one or more [B] solvents can be used.

[0093] [B] The solvent is preferably an alcohol-based solvent, such as methanol, ethanol, isopropyl alcohol, 1-propanol, or 1-butanol.

[0094] [Water addition process] In this step, water is added to the mixture. When the method for producing the composition includes the dilution step, water is added to the diluted mixture in this step. Specifically, for example, while stirring the diluted mixture, water is added dropwise to the mixture at room temperature (25°C to 30°C) over a predetermined time. The predetermined dropping time can be appropriately set. For example, the lower limit of the predetermined dropping time is preferably 5 minutes, more preferably 10 minutes. On the other hand, the upper limit of the predetermined dropping time is preferably 40 minutes, more preferably 30 minutes.

[0095] By adding water to the mixture, the hydrolysis condensation reaction of the [M] compound occurs. Depending on the progress of the hydrolysis condensation reaction of the [M] compound, the mixture may be heated after adding water. This heating can promote the hydrolysis condensation reaction of the [M] compound. When this heating is performed, the heating temperature can be appropriately set. The lower limit of the heating temperature is preferably 45°C, more preferably 50°C. The upper limit of the heating temperature is preferably 75°C, more preferably 70°C. When this heating is performed, the heating time can be appropriately set. The lower limit of the heating time is preferably 60 minutes, more preferably 90 minutes. The lower limit of the heating time is preferably 180 minutes, more preferably 150 minutes.

[0096] [Solvent addition process] In this step, the mixture obtained in the hydrolysis condensation step is added with the solvent [C]. The solvent [C] used in this step is described as the solvent [C] in the composition (J) above. As the solvent [C], an ether solvent and / or an ester solvent are preferred, a polyhydric alcohol partial ether solvent and / or a polyhydric alcohol partial ether carboxylate solvent are more preferred, and propylene glycol monoethyl ether and / or propylene glycol monomethyl ether acetate are even more preferred.

[0097] [Solvent removal process] In this step, excess water and excess [B] solvent are removed from the mixture obtained in the solvent addition step. For example, a rotary evaporator can be used to remove the excess water and excess [B] solvent. The solution obtained in the solvent removal step may be filtered through a filter having a pore size of 0.2 μm or less. The mixture obtained in this step (hereinafter also referred to as the "[Z] mixture") may be used as it is as composition (J), or may be subjected to the solvent re-addition step described below and used as composition (J).

[0098] [Solvent re-addition process] In this step, after the solvent removal step, the solvent [C] is further added. Specifically, the solvent [C] is added to the mixture [Z] obtained by the solvent removal step. By providing the method for producing the composition with this step, the concentration of components other than the solvent contained in the mixture [Z] can be adjusted.

[0099] <Resist Underlayer Film> The resist underlayer film is formed by using the composition (J) as a composition for forming the resist underlayer film. The resist underlayer film is a metal-containing film. Since the resist underlayer film is formed by using the composition (J), it has excellent film thickness change suppression properties, etching resistance, and removability.

[0100] The average thickness of the resist underlayer film is not particularly limited and can be appropriately determined. The lower limit of the average thickness of the resist underlayer film is preferably 1 nm, more preferably 5 nm, and even more preferably 10 nm. The upper limit of the average thickness is preferably 10,000 nm, more preferably 7,000 nm, and even more preferably 6,000 nm.

[0101] As described above, the resist underlayer film formed by the composition (J) suppresses the occurrence of cracks even when a thick film is formed. Therefore, the resist underlayer film can be suitably used in processes requiring a resist underlayer film with a thick average thickness in the manufacture of semiconductor elements, etc. When the resist underlayer film is used for such purposes, the lower limit of the average thickness is preferably 100 nm, more preferably 500 nm, even more preferably 1,000 nm, even more preferably 3,000 nm, and particularly preferably 4,000 nm.

[0102] <Membrane formation method> The film forming method includes a step of directly or indirectly applying a film forming composition to a substrate (hereinafter, also referred to as a "film forming composition applying step"). In the film forming composition applying step, the above-mentioned composition (J) is used as the film forming composition. According to the film forming method, a film having excellent thickness change suppression properties, etching resistance, and removability can be formed.

[0103] The film-forming composition application step included in the film-forming method will be described below.

[0104] [Film-forming composition coating process] In this process, the film-forming composition is applied directly or indirectly to a substrate. In this process, the above-mentioned composition (J) is used as the film-forming composition. In this process, a coating film is formed directly or indirectly on a substrate. The solvent [C] volatilizes from this coating film, forming a film. The film formed in this process is a metal-containing film.

[0105] Examples of the substrate include a metal substrate and a silicon wafer. The term "metal substrate" refers to a substrate containing metal atoms in at least a part of the surface layer. The metal atoms contained in the metal substrate are not particularly limited as long as they are atoms of metal elements. Silicon and boron are not included in the metal atoms. Examples of the metal atoms include copper, iron, zinc, cobalt, aluminum, tin, tungsten, zirconium, titanium, tantalum, germanium, molybdenum, ruthenium, gold, silver, platinum, palladium, nickel, and the like. Examples of the metal substrate include a metal substrate and a silicon wafer coated with a metal. A silicon nitride film, an alumina film, a silicon dioxide film, a tantalum nitride film, a titanium nitride film, and the like may be formed on a part of the metal substrate.

[0106] The substrate may be a substrate on which no pattern is formed, or a substrate on which a pattern is formed.

[0107] Examples of the pattern formed on the substrate include a line and space pattern or a trench pattern in which the line width of the space portion is 2,000 nm or less, 1,000 nm or less, 500 nm or less, or even 50 nm or less, and a hole pattern in which the diameter is 300 nm or less, 150 nm or less, 100 nm or less, or even 50 nm or less.

[0108] Furthermore, the dimensions of the pattern formed on the substrate may include fine patterns having a height of 100 nm or more, 200 nm or more, or even 300 nm or more, a width of 50 nm or less, 40 nm or less, or even 30 nm or less, and an aspect ratio (pattern height / pattern width) of 3 or more, 5 or more, or even 10 or more.

[0109] When a substrate having a pattern formed thereon is used as the substrate, it is preferable that the coating film formed by applying the composition for forming a coating film to the substrate is capable of filling recesses in the pattern.

[0110] In this step, the coating film may be heated to promote film formation. The atmosphere in which the coating film is heated may be air or nitrogen. The lower limit of the heating temperature is preferably 60°C. The upper limit of the heating temperature is preferably 150°C. The lower limit of the heating time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the heating time is preferably 300 seconds, more preferably 180 seconds.

[0111] The heating of the coating film may be performed as preheating, and the coating film after this preheating may be further heated. This heating is usually performed under air, but may be performed under a nitrogen atmosphere. The lower limit of the heating temperature is preferably 200°C, more preferably 250°C, and even more preferably 300°C. The upper limit of the heating temperature is preferably 600°C, more preferably 500°C, and even more preferably 400°C. The lower limit of the heating time is preferably 15 seconds, and more preferably 30 seconds. The upper limit of the heating time is preferably 1,200 seconds, and more preferably 600 seconds.

[0112] In the film forming method, exposure and heating can be combined. The radiation used for the exposure is appropriately selected from electromagnetic waves such as visible light, ultraviolet light, far ultraviolet light, X-rays, and gamma rays, and particle beams such as electron beams, molecular beams, and ion beams, depending on the type of acid generator.

[0113] The average thickness of the film formed is not particularly limited and can be appropriately determined. The lower limit of the average thickness of the film is preferably 1 nm, more preferably 5 nm, and even more preferably 10 nm. The upper limit of the average thickness is preferably 10,000 nm, more preferably 7,000 nm, and even more preferably 6,000 nm.

[0114] As described above, the film formed by the composition (J) is prevented from cracking even when a thick film is formed. Therefore, the film forming method can be suitably adopted in processes requiring a metal-containing film with a thick average thickness in the manufacture of semiconductor elements, etc. When the film forming method is adopted in such processes, the lower limit of the average thickness of the film formed is preferably 50 nm, more preferably 100 nm, even more preferably 200 nm, even more preferably 500 nm, and particularly preferably 1,000 nm.

[0115] <Method of forming resist pattern> The resist pattern forming method includes a step of directly or indirectly applying a film-forming composition to a substrate (hereinafter also referred to as a "film-forming composition applying step"), a step of directly or indirectly applying an organic resist film-forming composition to the resist underlayer film formed by the film-forming composition applying step (hereinafter also referred to as an "organic resist film-forming composition applying step"), a step of exposing the organic resist film formed by the organic resist film-forming composition applying step to radiation (hereinafter also referred to as an "exposure step"), and a step of developing the exposed organic resist film (hereinafter also referred to as a "development step").

[0116] The resist pattern forming method may further include a step of forming an organic underlayer film directly or indirectly on the substrate before the film forming composition coating step (hereinafter also referred to as an "organic underlayer film forming step"). The resist pattern forming method may further include a step of performing etching using the resist pattern formed by the developing step as a mask after the developing step (hereinafter also referred to as an "etching step"). The resist pattern forming method may, if necessary, include a step of forming a silicon-containing film on the resist underlayer film formed by the film forming composition coating step before the organic resist film forming composition coating step (hereinafter also referred to as a "silicon-containing film forming step").

[0117] According to the method for forming a resist pattern, since the composition (J) is used, a good resist pattern can be formed.

[0118] Each step of the resist pattern forming method will be described below.

[0119] [Organic lower layer film formation process] In this step, an organic underlayer film is formed on a substrate. The substrate may be the same as the substrate used in the film formation step in the film formation method described above. The organic underlayer film may be the same as the organic underlayer film formed in the organic underlayer film reverse pattern formation method described later.

[0120] [Film-forming composition coating process] In this step, the film-forming composition is applied directly or indirectly to the substrate. When the film-forming composition is applied indirectly to the substrate, for example, the film-forming composition is applied to the organic underlayer film formed on the substrate by the organic underlayer film forming step. In this step, the above-mentioned composition (J) is used as the film-forming composition. By this step, a resist underlayer film is formed directly or indirectly on the substrate. This step is the same as the film-forming composition application step in the above-mentioned film formation method.

[0121] [Silicon-containing film formation process] In this step, a silicon-containing film is formed on the resist underlayer film formed in the film-forming composition application step.

[0122] The silicon-containing film is formed by applying the silicon-containing film-forming composition to the resist underlayer film, and then curing the coating film by exposure and / or heating. Commercially available silicon-containing film-forming compositions include, for example, "NFC SOG01", "NFC SOG04", and "NFC SOG080" from JSR Corporation.

[0123] Examples of radiation used for the exposure include electromagnetic waves such as visible light, ultraviolet light, far ultraviolet light, X-rays and γ-rays, and particle beams such as electron beams, molecular beams and ion beams.

[0124] The lower limit of the temperature when the coating film is heated is preferably 90° C., more preferably 150° C., and even more preferably 180° C. The upper limit of the temperature is preferably 550° C., more preferably 450° C., and even more preferably 300° C.

[0125] [Organic resist film forming composition coating process] In this step, an organic resist film-forming composition is applied to the resist underlayer film formed in the film-forming composition application step. When the silicon-containing film-forming step is performed, the organic resist film-forming composition is applied to the silicon-containing film.

[0126] Specifically, in this process, the composition for forming an organic resist film is coated so that the resulting organic resist film has a predetermined thickness, and then the coating is heated to volatilize the solvent in the coating, thereby forming an organic resist film.

[0127] Examples of the composition for forming an organic resist film include a positive or negative chemically amplified resist composition that contains a radiation-sensitive acid generator, a positive resist composition that contains an alkali-soluble resin and a quinone diazide-based photosensitizer, and a negative resist composition that contains an alkali-soluble resin and a crosslinking agent.

[0128] The composition for forming an organic resist film is generally filtered through a filter having a pore size of 0.2 μm or less, and then used to form an organic resist film. In this step, a commercially available organic resist composition can also be used as it is.

[0129] The method of applying the organic resist film-forming composition is not particularly limited, and examples thereof include a rotary coating method. The heating temperature is appropriately adjusted depending on the type of the organic resist film-forming composition used, and the lower limit of the temperature is preferably 30°C, more preferably 50°C. The upper limit of the temperature is preferably 200°C, more preferably 150°C. The lower limit of the heating time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the time is preferably 600 seconds, more preferably 300 seconds.

[0130] [Exposure process] In this step, the organic resist film formed in the above-mentioned organic resist film-forming composition application step is exposed to radiation.

[0131] The radiation used for exposure is appropriately selected from visible light, ultraviolet light, far ultraviolet light, electromagnetic waves such as X-rays and gamma rays, and particle beams such as electron beams, molecular beams, and ion beams, depending on the types of radiation-sensitive acid generator, quinone diazide-based photosensitizer, and crosslinker used in the organic resist film-forming composition. Among these, far ultraviolet light is preferred, and KrF excimer laser light (248 nm), ArF excimer laser light (193 nm), F2 excimer laser light (wavelength 157 nm), Kr2 excimer laser light (wavelength 147 nm), ArKr excimer laser light (wavelength 134 nm) or extreme ultraviolet light (wavelength 13.5 nm, EUV) is more preferred, and KrF excimer laser light, ArF excimer laser light, EUV, or extreme ultraviolet light is even more preferred.

[0132] After the exposure, heating can be performed to improve resolution, pattern profile, developability, etc. The heating temperature is appropriately adjusted depending on the type of the organic resist film-forming composition used, etc., but the lower limit of the temperature is preferably 50°C, more preferably 70°C. The upper limit of the temperature is preferably 200°C, more preferably 150°C. The lower limit of the heating time is preferably 10 seconds, more preferably 30 seconds. The upper limit of the time is preferably 600 seconds, more preferably 300 seconds.

[0133] [Development process] In this step, the exposed organic resist film is developed. This development may be alkaline development or organic solvent development. In the case of alkaline development, examples of the developer include basic aqueous solutions of sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, ammonia, ethylamine, n-propylamine, diethylamine, di-n-propylamine, triethylamine, methyldiethylamine, dimethylethanolamine, triethanolamine, tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide, pyrrole, piperidine, choline, 1,8-diazabicyclo[5.4.0]-7-undecene, 1,5-diazabicyclo[4.3.0]-5-nonene, etc. These basic aqueous solutions may also contain an appropriate amount of water-soluble organic solvents, such as alcohols such as methanol and ethanol, surfactants, etc. In the case of organic solvent development, examples of the developer include various organic solvents exemplified as the solvent [C] of the above-mentioned composition (J).

[0134] After development with the developer, the resist is washed and dried to form a desired resist pattern.

[0135] [Etching process] In this step, etching is performed using the resist pattern formed by the above-mentioned development step as a mask. This forms a pattern on the substrate. The number of times of etching may be one or more times, that is, etching may be performed sequentially using the pattern obtained by etching as a mask, but from the viewpoint of obtaining a pattern with a better shape, multiple times is preferable. When performing multiple etchings, etching is performed sequentially in the order of the silicon-containing film, the resist underlayer film, and the substrate. Examples of the etching method include dry etching and wet etching. Among these, dry etching is preferable from the viewpoint of obtaining a better shape of the pattern on the substrate. For this dry etching, for example, gas plasma such as oxygen plasma is used. After the above-mentioned etching, a patterned substrate having a predetermined pattern is obtained.

[0136] <Method for forming organic underlayer film reverse pattern> The organic underlayer film reversal pattern forming method includes a step of forming an organic underlayer film directly or indirectly on a substrate (hereinafter also referred to as an "organic underlayer film forming step"); a step of forming a resist pattern directly or indirectly on the upper surface of the organic underlayer film (hereinafter also referred to as a "resist pattern forming step"); a step of forming a pattern on the organic underlayer film by etching using the resist pattern as a mask (hereinafter also referred to as an "organic underlayer film pattern forming step"); a step of forming a film for forming an organic underlayer film reversal pattern directly or indirectly on the organic underlayer film pattern using composition (J1) (hereinafter also referred to as an "organic underlayer film reversal pattern forming film forming step"); and a step of forming an organic underlayer film reversal pattern by removing the organic underlayer film pattern (hereinafter also referred to as an "organic underlayer film reversal pattern forming step"). The organic underlayer film reversal pattern forming method may include a step of forming a resist intermediate film on the organic underlayer film formed by the organic underlayer film forming step (hereinafter also referred to as a "resist intermediate film forming step") as necessary before the resist pattern forming step. In the organic underlayer film reversal pattern forming film forming step, the organic underlayer film reversal pattern forming film is formed using the above-mentioned composition (J).

[0137] According to the method for forming a reversal pattern on an organic underlayer film, a good reversal pattern can be formed because the composition (J) is used.

[0138] Hereinafter, each step of the organic underlayer film reversal pattern forming method will be described.

[0139] [Organic lower layer film formation process] In this step, an organic underlayer film is formed on a substrate, which may be the same as the substrate used in the film formation step described above.

[0140] The organic underlayer film can be formed from an organic compound. Commercially available organic compounds include, for example, "NFC HM8006" from JSR Corporation. The organic underlayer film can be formed by applying a composition for forming an organic underlayer film by spin coating or the like to form a coating film, and then heating the coating film.

[0141] The lower limit of the average thickness of the organic underlayer film to be formed is preferably 10 nm, more preferably 50 nm, and even more preferably 100 nm.The upper limit of the average thickness is preferably 1000 nm, and more preferably 500 nm.

[0142] [Resist intermediate film formation process] In this step, a resist intermediate film is formed on the organic underlayer film formed in the organic underlayer film forming step. Examples of the resist intermediate film include commercially available products such as "NFC SOG01", "NFC SOG04", and "NFC SOG080" (all from JSR Corporation). Polysiloxane, titanium oxide, aluminum oxide, tungsten oxide, and the like formed by a CVD method can also be used. The method for forming the intermediate layer is not particularly limited, and examples include a coating method and a CVD method. Among these, the coating method is preferred. When the coating method is used, the resist intermediate film can be formed continuously after the organic underlayer film is formed.

[0143] [Resist pattern formation process] In this step, a resist pattern is formed on the organic underlayer film and the resist intermediate film. In this step, the resist pattern can be formed by a conventionally known method, such as a method using a resist composition or a method using nanoimprint lithography.

[0144] [Organic underlayer film pattern formation process] In this process, the organic underlayer film is etched using the resist pattern as a mask. Examples of the etching method include dry etching and wet etching. The dry etching can be performed using a known dry etching device. In addition, the source gas during dry etching depends on the elemental composition of the film to be etched, but for example, fluorine-based gases such as CHF3, CF4, C2F6, C3F8, and SF6, chlorine-based gases such as Cl2 and BCl3, oxygen-based gases such as O2 and O3, reducing gases such as H2, NH3, CO, CO2, CH4, C2H2, C2H4, C2H6, C3H4, C3H6, C3H8, HF, HI, HBr, HCl, NO, NH3, and BCl3, and inert gases such as He, N2, and Ar are used, and these gases can also be used in combination. When forming a resist intermediate film, a fluorine-based gas is usually used for dry etching of the resist intermediate film, and an oxygen-based gas is preferably used for dry etching of the organic underlayer film.

[0145] Examples of the pattern of the organic underlayer film include a line and space pattern or a trench pattern in which the line width of the space portion is 2,000 nm or less, 1,000 nm or less, 500 nm or less, or even 50 nm or less, and a hole pattern in which the diameter is 300 nm or less, 150 nm or less, 100 nm or less, or even 50 nm or less.

[0146] In addition, the dimensions of the organic underlayer film pattern may be, for example, a fine pattern having a height of 100 nm or more, 200 nm or more, or even 300 nm or more, a width of 50 nm or less, 40 nm or less, or even 30 nm or less, and an aspect ratio (pattern height / pattern width) of 3 or more, 5 or more, or even 10 or more.

[0147] [Organic underlayer film reversal pattern formation process] In this step, the composition (J) is filled into the gaps of the organic underlayer film pattern. Specifically, the composition (J) is applied onto the substrate on which the organic underlayer film pattern is formed by a suitable coating means such as spin coating, casting coating, roll coating, etc., and is filled into the gaps of the organic underlayer film pattern. In addition, in this step, it is preferable to provide a drying step after the composition (J) is filled into the gaps of the organic underlayer film pattern. The drying means is not particularly limited, but for example, the organic solvent in the composition can be volatilized by baking. The baking conditions are appropriately adjusted depending on the blending composition of the resin composition, and the baking temperature is usually 80 to 250°C, preferably 80 to 200°C. When the baking temperature is 80 to 180°C, the flattening step described below, particularly the flattening process by the wet etchback method, can be smoothly performed. The heating time is usually 10 to 300 seconds, preferably 30 to 180 seconds. The thickness of the organic underlayer film reversal pattern-forming film obtained after drying is not particularly limited, but is usually 10 to 1000 nm, and preferably 20 to 500 nm.

[0148] [Organic underlayer film inversion pattern formation process] In this step, the organic underlayer film pattern is removed, and a reversal pattern of the organic underlayer film is formed.

[0149] Specifically, first, a planarization process is preferably performed to expose the upper surface of the organic underlayer film pattern, and then the organic underlayer film pattern is removed by dry etching or dissolving to obtain a predetermined organic underlayer film reverse pattern.

[0150] This organic underlayer film reversal pattern formation process makes it possible to form fine patterns with high aspect ratios on a substrate, which are difficult to achieve by normal lithography processes, and thus allows the fine patterns to be transferred onto the substrate.

[0151] As the planarization method used in the above-mentioned planarization processing, etching methods such as dry etch back and wet etch back, CMP method, etc. can be used. Among these, dry etch back and wet etch back methods using fluorine-based gases, etc. are preferable because of their low cost. The processing conditions in the planarization processing are not particularly limited and can be appropriately adjusted.

[0152] In addition, dry etching is preferable for removing the organic underlayer film pattern, and specifically, oxygen-based gas etching, ozone etching, etc. are preferably used. For the dry etching, known devices such as an oxygen plasma ashing device and an ozone ashing device can be used. The etching processing conditions are not particularly limited and can be appropriately adjusted.

[0153] [Metal-containing film removal process] In this step, the organic underlayer film reversal pattern is removed with a remover (I) containing an acid or a base.

[0154] Examples of the acid-containing removal liquid (I) include a liquid containing acid and water, a liquid obtained by mixing acid, hydrogen peroxide, and water, etc. Examples of the acid include sulfuric acid, hydrofluoric acid, hydrochloric acid, phosphoric acid, etc. More specifically, examples of the acid-containing removal liquid (I) include a liquid obtained by mixing hydrofluoric acid and water, a liquid obtained by mixing sulfuric acid, hydrogen peroxide, and water, a liquid obtained by mixing hydrochloric acid, hydrogen peroxide, and water, etc.

[0155] Examples of the base-containing removal liquid (I) include a liquid containing a base and water, and a liquid obtained by mixing a base, hydrogen peroxide, and water, and the like. A liquid obtained by mixing a base, hydrogen peroxide, and water is preferred.

[0156] Examples of the base include sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, ammonia, ethylamine, n-propylamine, diethylamine, di-n-propylamine, triethylamine, methyldiethylamine, dimethylethanolamine, triethanolamine, tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide, pyrrole, piperidine, choline, 1,8-diazabicyclo[5.4.0]-7-undecene, 1,5-diazabicyclo[4.3.0]-5-nonene, etc. Among these, ammonia is preferable.

[0157] The lower limit of the temperature in the removal step is preferably 20° C., more preferably 40° C., and further preferably 50° C. The upper limit of the temperature is preferably 300° C., and more preferably 100° C.

[0158] The lower limit of the time in the removal step is preferably 5 seconds, more preferably 30 seconds, and the upper limit of the time is preferably 10 minutes, more preferably 180 seconds.

[0159] <Metal-containing film pattern forming method> The method for forming a metal-containing film pattern includes a step of directly or indirectly applying a metal-containing film-forming composition to a substrate (hereinafter also referred to as a "metal-containing film-forming composition application step"); a step of directly or indirectly forming an organic underlayer film on the metal-containing film formed by the metal-containing film-forming composition application step (hereinafter also referred to as an "organic underlayer film formation step"); a step of directly or indirectly forming a resist pattern on the organic underlayer film (hereinafter also referred to as a "resist pattern formation step"); and a step of forming a pattern on the metal-containing film by etching using the resist pattern as a mask (hereinafter also referred to as an "etching step"). In the metal-containing film-forming composition application step, the above-mentioned composition (J) is used as the metal-containing film-forming composition. The method for forming a metal-containing film pattern may include a step of forming a silicon-containing film on the organic underlayer film (hereinafter also referred to as a "silicon-containing film formation step") before the resist pattern formation step, as necessary.

[0160] According to the method for forming a metal-containing film pattern, a good metal-containing film pattern can be formed.

[0161] Hereinafter, each step of the metal-containing film pattern forming method will be described.

[0162] [Metal-containing film-forming composition coating process] In this process, the composition for forming a metal-containing film is directly or indirectly applied to a substrate. In this process, the above-mentioned composition (J) is used as the composition for forming a metal-containing film. By this process, a coating film is formed directly or indirectly on the substrate. The solvent [C] is evaporated from this coating film, thereby forming a metal-containing film.

[0163] The substrate may be the same as those exemplified as the substrate used in the film formation step in the above-mentioned film formation method. This step may be carried out in the same manner as the film formation step in the above-mentioned film formation method.

[0164] The average thickness of the metal-containing film formed by this process is not particularly limited and can be appropriately determined. The lower limit of the average thickness of the metal-containing film is preferably 1 nm, more preferably 5 nm, and even more preferably 10 nm. The upper limit of the average thickness is preferably 10,000 nm, more preferably 7,000 nm, and even more preferably 6,000 nm.

[0165] As described above, the film formed by the composition (J) is prevented from cracking even when it is thick. Therefore, the metal-containing film formed by this process may be a thick film. In this case, the lower limit of the average thickness of the metal-containing film is preferably 100 nm, more preferably 500 nm, even more preferably 1,000 nm, even more preferably 3,000 nm, and particularly preferably 4,000 nm. When the metal-containing film is thick, the height of the metal-containing film pattern formed by the metal-containing film pattern forming method becomes high. Therefore, for example, when etching is performed using this metal-containing film pattern as a mask, the film or substrate below the metal-containing film pattern can be etched deeper.

[0166] [Organic lower layer film formation process] In this step, an organic underlayer film is formed directly or indirectly on the metal-containing film formed by the metal-containing film-forming composition coating step. By this step, an organic underlayer film is formed directly or indirectly on the metal-containing film. This step is the same as the organic underlayer film formation step in the organic underlayer film reversal pattern described above.

[0167] [Silicon-containing film formation process] In this step, a silicon-containing film is formed on the organic underlayer film. This step is the same as the silicon-containing film forming step in the above-mentioned resist pattern forming method.

[0168] [Resist pattern formation process] In this step, a resist pattern is formed directly or indirectly on the organic underlayer film. This step forms a resist pattern directly or indirectly on the organic underlayer film. This step is the same as the resist pattern forming step in the organic underlayer film reversal pattern described above.

[0169] [Etching process] In this step, a pattern is formed in the metal-containing film by etching using the resist pattern as a mask. A metal-containing film pattern is formed by this step. This step is the same as the etching step in the resist pattern forming method described above. Note that, when a pattern is formed in the metal-containing film by etching, the organic underlayer film formed directly or indirectly on the metal-containing film is also etched. EXAMPLES

[0170] The following examples are provided to illustrate, but are not intended to limit the scope of the present invention.

[0171] In the present examples, the concentrations of components other than the solvent in the mixture [Z], the weight average molecular weight (Mw) of the hydrolysis condensate in the mixture [Z], and the average thickness of the film were measured by the following methods.

[0172] [[Z] Concentration of non-solvent components in the mixture] 0.5 g of the [Z] mixture was baked at 250°C for 30 minutes, and the mass of the residue was measured. The mass of this residue was divided by the mass of the [Z] mixture to calculate the concentration (mass%) of components other than the solvent in the [Z] mixture.

[0173] [[Z] Weight average molecular weight (Mw) of the hydrolysis condensate in the mixture] Measurements were performed by gel permeation chromatography (detector: differential refractometer) using monodisperse polystyrene as the standard, under the following analytical conditions: GPC columns (two "AWA-H", one "AW-H" and two "AW2500" from Tosoh Corporation), flow rate: 0.3 mL / min, elution solvent: N,N'-dimethylacetamide supplemented with LiBr (30 mM) and citric acid (30 mM), column temperature: 40°C.

[0174] [Average film thickness] The average thickness of the film was measured using a spectroscopic ellipsometer (JAWOOLLAM's "A2000D").

[0175] <Preparation of [Z] mixture> The [M] compound, [X] compound, [B] solvent, and [C] solvent are shown below. In the following synthesis examples, unless otherwise specified, "parts by mass" refers to a value when the mass of the [M] compound used is 100 parts by mass. In addition, "molar ratio" refers to a value when the substance amount of the [M] compound used is 1.

[0176] As the [M] compound, the following compound was used. M-1: tetraisopropoxytitanium(IV) M-2: Triisopropoxyaluminum(III) M-3: Tetraisopropoxyhafnium(IV) M-4: Pentaethoxytantalum(V) M-5: Tetra-n-butoxyzirconium(IV)

[0177] As the compound [X], compounds represented by the following formulae (X-1) to (X-10) and (x-1) (hereinafter also referred to as "compound (X-1) to compound (X-10)" and "compound (x-1)") were used.

[0178] [ka]

[0179] [B] As the solvent, the following compound was used. B-1: Isopropyl alcohol B-2: Ethanol B-3: 1-butanol

[0180] [C] The following compounds were used as solvents. C-1: Propylene glycol monoethyl ether C-2: Propylene glycol monomethyl ether acetate C-3: Tripropylene glycol C-4: Tripropylene glycol monomethyl ether C-5: Triethylene glycol C-6: Tetraethylene glycol monomethyl ether

[0181] [Synthesis Example 1-1] (Example 1-1: Preparation of [Z] Mixture (Z-1)) Compound (M-1) was put into a reaction vessel under an N2 atmosphere, and while stirring at room temperature (25°C to 30°C), compound (X-1) (molar ratio 1) was added dropwise over 30 minutes. Then, the reaction was carried out at 60°C for 2 hours. After the reaction was completed, the reaction vessel was cooled to 30°C or lower. The cooled reaction solution was diluted with solvent (B-1) (900 parts by mass). While stirring the diluted reaction solution at room temperature (25°C to 30°C), water (molar ratio 0.75) was added dropwise over 10 minutes. Then, a hydrolysis condensation reaction was carried out at 60°C for 2 hours. After the hydrolysis condensation reaction was completed, the reaction vessel was cooled to 30°C or lower. After adding 1000 parts by mass of solvent (C-1) to the cooled reaction solution, water, solvent (B-1), alcohol produced by the hydrolysis condensation reaction, and excess solvent (C-1) were removed using an evaporator to obtain a mixture (Z-1). The Mw of the hydrolysis condensate in the mixture (Z-1) was 1800. The concentration of components other than the solvent in the mixture (Z-1) was 7.4 mass%.

[0182] [Synthesis Examples 1-2 to 1-17] (Examples 1-2 to 1-17: Preparation of [Z] Mixtures (Z-2) to (Z-17)) Mixtures (Z-2) to (Z-17) were obtained in the same manner as in Synthesis Example 1-1, except that the types and amounts of the [M] compound, [X] compound, [B] solvent, water content during condensation, and [C] solvent were used as shown in Table 1. Table 1 also shows the Mw of the hydrolysis condensate in the [Z] mixture, and the concentration (mass%) of components other than the solvent in the [Z] mixture.

[0183] [Synthesis Example 1-18] (Example 1-18: Preparation of [Z] Mixture (Z-18)) In a N2 atmosphere, the compound (M-1) was put into a reaction vessel, and while stirring at room temperature (25°C to 30°C), the compound (X-1) (molar ratio 2) was dropped over 30 minutes. Then, the reaction was carried out at 60°C for 2 hours. After the reaction was completed, the reaction vessel was cooled to 30°C or lower. The cooled reaction solution was diluted with a solvent (B-1) (330 parts by mass). While stirring the diluted reaction solution at room temperature (25°C to 30°C), water (molar ratio 0.75) was dropped over 10 minutes. Then, a hydrolysis condensation reaction was carried out at 60°C for 2 hours. After the hydrolysis condensation reaction was completed, the reaction vessel was cooled to 30°C or lower. After adding 430 parts by mass of a solvent (C-1) to the cooled reaction solution, the water, the solvent (B-1), the alcohol produced by the reaction, and the excess solvent (C-1) were removed using an evaporator to obtain a mixture (Z-18). The Mw of the hydrolysis condensate in the mixture (Z-18) was 1400. The concentration of components other than the solvent in the mixture (Z-18) was 32.1 mass%.

[0184] [Synthesis Example 1-19] (Example 1-19: Preparation of [Z] Mixture (Z-19)) In a N2 atmosphere, the compound (M-1) was put into a reaction vessel, and while stirring at room temperature (25°C to 30°C), the compound (X-1) (molar ratio 2) was dropped over 30 minutes. Then, the reaction was carried out at 60°C for 2 hours. After the reaction was completed, the reaction vessel was cooled to 30°C or lower. The cooled reaction solution was diluted with a solvent (B-1) (70 parts by mass). While stirring the diluted reaction solution at room temperature (25°C to 30°C), water (molar ratio 0.75) was dropped over 10 minutes. Then, a hydrolysis condensation reaction was carried out at 60°C for 2 hours. After the hydrolysis condensation reaction was completed, the reaction vessel was cooled to 30°C or lower. After adding 170 parts by mass of a solvent (C-1) to the cooled reaction solution, the water, the solvent (B-1), the alcohol produced by the reaction, and the excess solvent (C-1) were removed using an evaporator to obtain a mixture (Z-19). The Mw of the hydrolysis condensate in the mixture (Z-19) was 1,450. The concentration of components other than the solvent in the mixture (Z-19) was 53.2 mass%.

[0185] [Synthesis Example 1-20] (Comparative Example 1-1: [z] Preparation of Mixture (z-1)) A mixture (z-1) was obtained in the same manner as in Synthesis Example 1-1, except that the types and amounts of the compound [M], the compound [X], the solvent [B], water, and the solvent [C] shown in Table 1 below were used.

[0186] [Synthesis Example 1-21] (Comparative Example 1-2: [z] Preparation of Mixture (z-2)) In a N2 atmosphere, the compound (M-1) was put into a reaction vessel, and while stirring at room temperature (25°C to 30°C), the compound (x-1) (molar ratio 2) was dropped over 30 minutes. Then, the reaction was carried out at 60°C for 2 hours. After the reaction was completed, the reaction vessel was cooled to 30°C or lower. The cooled reaction solution was diluted with a solvent (B-1) (270 parts by mass). While stirring the diluted reaction solution at room temperature (25°C to 30°C), water (molar ratio 2.0) was dropped over 10 minutes. Then, a hydrolysis condensation reaction was carried out at 60°C for 2 hours. After the hydrolysis condensation reaction was completed, the reaction vessel was cooled to 30°C or lower. After adding 370 parts by mass of a solvent (C-1) to the cooled reaction solution, water, isopropanol, alcohol produced by the reaction, water, and excess solvent (C-1) were removed using an evaporator to obtain a mixture (z-2). The Mw of the hydrolysis condensate in the mixture (z-2) was 1650. The concentration of components other than the solvent in the mixture (z-2) was 13.0 mass%.

[0187] [Table 1]

[0188] <Preparation of film-forming composition (1)> [Example 2-1] Preparation of film-forming composition (J-1) As shown in Table 2 below, (Z-1) as the [Z] mixture and (C-1) as the [C] solvent were mixed so that the amount of the [C] solvent was 96 parts by mass (including the [C] solvent contained in the [Z] mixture) per 4 parts by mass of the components other than the solvent in the [Z] mixture. The resulting solution was filtered through a filter with a pore size of 0.2 μm to prepare a film-forming composition (J-1).

[0189] [Examples 2-2 to 2-17] Preparation of film-forming compositions (J-2) to (J-17) Film-forming compositions (J-2) to (J-17) were prepared in the same manner as in Example 2-1, except that the types and contents of each component were as shown in Table 2 below.

[0190] [Comparative Example 2-1] Preparation of film-forming composition (j-1) A film-forming composition (j-1) was prepared in the same manner as in Example 2-1, except that the types and contents of each component were as shown in Table 2 below.

[0191] [Table 2]

[0192] [Comparative Example 2-2] Preparation of film-forming composition (j-2) 1.61 g of oxalic acid was dissolved in 96.45 g of water by heating to prepare an aqueous oxalic acid solution. Then, a cooling tube and a dropping funnel containing the prepared aqueous oxalic acid solution were set in a flask containing 25.70 g (70 mol%) of tetramethoxysilane, 9.86 g (30 mol%) of methyltrimethoxysilane, and 366.39 g of propylene glycol monoethyl ether. Next, the flask was heated to 60°C in an oil bath, and the aqueous oxalic acid solution was slowly dropped and reacted at 60°C for 4 hours. After the reaction was completed, the flask containing the reaction solution was allowed to cool, then set in an evaporator and concentrated under reduced pressure to obtain 360 g of a polysiloxane solution. The concentration of components other than the solvent in the obtained polysiloxane solution was 9.8% by mass. The weight average molecular weight (Mw) of the obtained polysiloxane was 1,500. The polysiloxane solution and propylene glycol monoethyl ether were mixed to adjust the concentration of components other than the solvent in the polysiloxane solution to 4 mass %, thereby preparing a film-forming composition (j-2).

[0193] <Evaluation> The film-forming compositions prepared above were evaluated for storage stability, inhibition of change in film thickness, resistance to oxygen-based gas etching, embeddability, and removability according to the following methods. The evaluation results are shown in Table 3 below.

[0194] [Storage stability] The storage stability of the film-forming composition was evaluated based on the difference in coatability over time. The film-forming composition (T=0) immediately after preparation was applied to a silicon wafer (substrate) by a spin coater (Tokyo Electron Co., Ltd.'s "CLEAN TRACK ACT8") at 1,500 rpm for 30 seconds, and the resulting coating film was heated at 90°C for 60 seconds to form a metal-containing film. The formed metal-containing film was observed with an optical microscope for coatability, and was evaluated as "A" (good) if no coating unevenness was observed, and as "B" (bad) if coating unevenness was observed. The composition for which the coatability was evaluated was stored at 20°C for 60 days (T=60), and was evaluated for coatability in the same manner as above. The storage stability can be evaluated as good if both the coatability at T=0 and the coatability at T=60 were evaluated as "A" (good), and as poor if not.

[0195] [Suppression of film thickness change] The film-forming composition prepared above was applied onto an 8-inch silicon wafer by a rotary coating method using the spin coater under conditions of 1,500 rpm and 30 seconds, and then after a predetermined time had elapsed, the wafer was heated at 250° C. for 60 seconds and cooled at 23° C. for 30 seconds to form a metal-containing film. As the metal-containing film, a "metal-containing film (a0)" was formed when the predetermined time was 30 seconds, and a "metal-containing film (a1)" was formed when the predetermined time was 300 seconds. When the average thickness of the metal-containing film (a0) was T0 and the average thickness of the metal-containing film (a1) was T1, the film thickness change rate (%) was calculated by the following formula and used as an index of film thickness change suppression. Film thickness change rate (%) = |T1-T0| x 100 / T0 The film thickness change suppression property was evaluated as "A" (good) when the film thickness change rate was less than 1.7%, and as "B" (poor) when it was 1.7% or more.

[0196] [Oxygen-based gas etching resistance] The film-forming composition prepared above was applied onto an 8-inch silicon wafer by a rotary coating method using the spin coater described above, heated at 220°C for 60 seconds, and then cooled at 23°C for 30 seconds to form a metal-containing film with an average thickness of 100 nm. The substrate on which the metal-containing film was formed was etched using an etching device (Tokyo Electron Ltd.'s "Tactras-Vigus") under the conditions of O2 = 400sccm, PRESS. = 25mT, HF RF (high frequency power for plasma generation) = 200W, LF RF (high frequency power for bias) = ​​0W, DCS = 0V, RDC (gas center flow rate ratio) = 50%, and 60sec. The etching rate (nm / min) was calculated from the average film thickness before and after the etching, and the oxygen-based gas etching resistance was evaluated. The oxygen-based gas etching resistance was evaluated as "A" (good) when the etching rate was less than 1.0nm / min, and as "B" (poor) when the etching rate was 1.0nm / min or more.

[0197] [Embeddability] The film-forming composition prepared above was applied by a spin coating method using the spin coater on a silicon nitride substrate on which a trench pattern of 300 nm in depth and 30 nm in width had been formed using an organic underlayer film-forming material ("HM8006" by JSR Corporation). The rotation speed of the spin coater was the same as that in the case of forming a film of an average thickness of 100 nm on a silicon wafer in the evaluation of the oxygen-based gas etching resistance described above. Next, the substrate was heated at 250°C for 60 seconds in an air atmosphere, and then cooled at 23°C for 30 seconds to obtain a substrate on which a metal-containing film had been formed. The cross section of the obtained substrate was examined for the presence or absence of filling defects (voids) using a field emission scanning electron microscope ("S-4800" by Hitachi High-Technologies Corporation). The filling property was evaluated as "A" (good) when no filling defects were observed, and as "B" (poor) when filling defects were observed.

[0198] [Removability] <Formation of substrate with metal-containing film> The film-forming composition prepared above was applied onto an 8-inch silicon wafer by a rotary coating method using the spin coater, and then the wafer was heated at 220°C for 60 seconds and then cooled at 23°C for 30 seconds to form a metal-containing film having an average thickness of 100 nm, thereby producing a substrate with a metal-containing film formed on the surface thereof.

[0199] <Removal of metal-containing films> Each of the substrates with the metal-containing film prepared above was treated under the film removal conditions shown below. The surface of each substrate with the metal-containing film was contacted with a removal solution shown in Table 3 below by the paddle method, and then dried by rotation with a spin coater.

[0200] (Membrane removal condition-1) Each of the metal-containing film-attached substrates obtained above was immersed in a removal solution (R-1) (a mixed aqueous solution of 25% by mass ammonia solution / 30% by mass hydrogen peroxide solution / water=1 / 1 / 5 (volume ratio)) heated to 65° C. for 5 minutes.

[0201] (Membrane removal condition-2) Each of the substrates with the metal-containing film obtained above was immersed in a removal solution (R-2) (a mixed aqueous solution of 96% by mass sulfuric acid / 30% by mass hydrogen peroxide=3 / 1 (volume ratio)) heated to 50° C. for 5 minutes.

[0202] (Membrane removal condition-3) Each of the substrates with the metal-containing film obtained above was immersed in a removal solution (R-3) (aqueous solution of 85% by mass phosphoric acid) that had been heated to 50° C. for 5 minutes.

[0203] <Evaluation> The removability of the metal-containing film was evaluated by the following method. Each of the metal-containing film-attached substrates obtained above was observed by cross-section SEM, and was rated as "A" (good) when no metal-containing film remained, and as "B" (poor) when the metal-containing film remained.

[0204] [Table 3]

[0205] From the results in Table 3, it can be seen that the film-forming compositions of the examples have excellent storage stability and embedding ability. Furthermore, from the results in Table 3, it can be seen that the films formed by the film-forming compositions of the examples have excellent thickness change suppression properties, oxygen-based gas etching resistance, and removability.

[0206] <Preparation of film-forming composition (2)> The following compounds were used as [other optional components]. D-1: Surfactant (NEOS Corporation's "NBX-15") D-2: Surfactant (DIC Corporation's "F563") D-3: Poly(2-ethylhexyl acrylate)

[0207] [Example 3-1] Preparation of film-forming composition (J-18) As shown in Table 4 below, (Z-18) as the [Z] mixture and (C-1) as the [C] solvent were mixed so that the amount of the [C] solvent was 96 parts by mass (including the [C] solvent contained in the [Z] mixture) per 4 parts by mass of the components other than the solvent in the [Z] mixture. The resulting solution was filtered through a filter with a pore size of 0.2 μm to prepare a film-forming composition (J-18).

[0208] [Examples 3-2 to 3-21] Preparation of film-forming compositions (J-19) to (J-38) Film-forming compositions (J-19) to (J-38) were prepared in the same manner as in Example 3-1, except that the types and contents of each component were as shown in Table 4 below.

[0209] [Comparative Examples 3-1 to 3-2] Preparation of film-forming compositions (j-3) to (j-4) Film-forming compositions (j-3) to (j-4) were prepared in the same manner as in Example 3-1, except that the types and contents of each component were as shown in Table 4 below.

[0210] [Table 4]

[0211] <Evaluation> The film-forming compositions prepared above were used to evaluate the coatability and occurrence of cracks according to the following methods. The evaluation results are shown in Table 4 below.

[0212] [Coatability] The film-forming composition prepared above was applied onto an 8-inch silicon wafer by a rotational coating method using the spin coater, and then heated under the conditions of temperature (°C) and time (seconds) shown in Table 4 below, and cooled at 23°C for 30 seconds to form metal-containing films (Examples 3-1 to 3-26 and Comparative Examples 3-1 to 3-2) with the thicknesses shown in Table 4 below. The metal-containing films were visually observed for the presence or absence of streaky defects (striations) extending from the center to the circumferential direction. The coatability was evaluated as "A" (good) when there were no streaky defects, and "B" (poor) when there were streaky defects.

[0213] [Crack occurrence] The film-forming composition prepared above was applied onto an 8-inch silicon wafer by a rotary coating method using the spin coater, and then heated under the conditions of temperature (°C) and time (seconds) shown in Table 4 below, and cooled at 23°C for 30 seconds to form metal-containing films (Examples 3-1 to 3-26 and Comparative Examples 3-1 to 3-2) having the thicknesses shown in Table 4 below. In addition, for Examples 3-25 and 3-26, the metal-containing films were exposed to UV light in purified air for 10 minutes. The UV light source was a Xe excimer lamp (Ushio Inc., wavelength 172 nm, 10 mW / cm 2 ) was used. The surface of the formed metal-containing film was observed with an optical microscope. Regarding the occurrence of cracks, when no cracks or peeling of the metal-containing film were observed, it was rated as "A" (good), and when cracks or peeling of the metal-containing film were observed, it was rated as "B" (poor).

[0214] [Table 5]

[0215] From the results in Table 5 above, it can be seen that the film-forming compositions of the examples have excellent coatability, and the formed films are able to suppress the occurrence of cracks. Furthermore, from the results in Table 5 above, it can be seen that the film-forming compositions of the examples are able to suppress the occurrence of cracks even when thick films are formed. [Industrial Applicability]

[0216] The film-forming composition of the present invention has excellent storage stability and embedding properties. Furthermore, the film formed by the film-forming composition of the present invention is also excellent in etching resistance, film thickness change suppression, etching resistance and removability. The resist underlayer film of the present invention is formed by the film-forming composition, and therefore has excellent film thickness change suppression, etching resistance and removability. According to the film-forming method of the present invention, since the film-forming composition is used, a film having excellent film thickness change suppression, etching resistance and removability can be formed. According to the resist pattern forming method of the present invention, since the film-forming composition is used, a good resist pattern can be formed. According to the resist underlayer film reversal pattern forming method of the present invention, since the film-forming composition is used as a resist underlayer film reversal pattern forming composition, a good reversal pattern can be formed. According to the method for producing the film-forming composition of the present invention, a film-forming composition having excellent storage stability and embedding properties, and further having excellent etching resistance, film thickness change suppression, etching resistance and removability can be produced.

[0217] According to the method for forming a metal-containing film pattern of the present invention, since the film-forming composition is used as the metal-containing film-forming composition, a good metal-containing film pattern can be formed.

[0218] The film-forming composition of the present invention has excellent coatability when forming a thick film. Furthermore, the film-forming composition of the present invention can form a thick film in which the occurrence of cracks is suppressed.

[0219] Furthermore, according to the method for forming a metal-containing film pattern of the present invention, by using the film-forming composition as a metal-containing film-forming composition, a thick film in which the occurrence of cracks is suppressed can be formed, and therefore a good metal-containing film pattern can be formed.

[0220] Therefore, they can be suitably used in lithography processes in the manufacture of various electronic devices such as semiconductor devices and liquid crystal devices, which require further miniaturization.

Claims

1. The method comprises the steps of: the nitrogen-containing organic compound is a compound having a nitrogen atom, an aliphatic hydrocarbon group, and two or more hydroxy groups, a compound having a nitrogen-containing aromatic heterocycle and one or more hydroxy groups, or a mixture thereof; the metal compound is a metal alkoxide, a hydrolysis condensate of a metal alkoxide, or a mixture thereof; a metal atom contained in the metal compound belongs to Period 3 of Groups 2 to 13 of the periodic table and Periods 4 to 7 of Groups 2 to 14 of the periodic table; The compound having a nitrogen-containing aromatic heterocycle and one or more hydroxy groups is one or more divalent aliphatic hydrocarbon groups having 1 to 10 carbon atoms bonded to the nitrogen-containing aromatic heterocycle; and one or more hydroxy groups bonded to each of the aliphatic hydrocarbon groups.

2. 2. The film forming composition according to claim 1, wherein the nitrogen-containing organic compound is coordinated to a metal atom in the metal compound, or is free from a metal atom in the metal compound.

3. 3. The film forming composition according to claim 1, wherein the compound having a nitrogen atom, an aliphatic hydrocarbon group, and two or more hydroxy groups is represented by the following formula (1): 【Chemistry 1】 (In formula (1), m+n is 3, m is 2 or 3, and n is 0 or 1. R 1 is a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, and a plurality of R 1 are the same or different. 2 is a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, or a group represented by the following formula (1-1): 【Chemistry 2】 (In formula (1-1), R 2A R is a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms. 2B and R 2C are each independently a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 10 carbon atoms, or -R 2D -OH. 2D is a divalent aliphatic hydrocarbon group having 1 to 10 carbon atoms. p is an integer from 1 to 4. When p is 2 or more, multiple R 2A are the same or different, and multiple R 2C are the same or different. * indicates the site of binding to the nitrogen atom in the above formula (1).

4. 4. The film forming composition according to claim 1, wherein the metal atom belongs to Group 4 of the periodic table.

5. The film forming composition according to claim 1 , which is used for forming a resist underlayer film.

6. The film-forming composition according to any one of claims 1 to 4, which is used for forming a reverse pattern of an organic underlayer film.

7. A film forming method comprising a step of applying the film forming composition according to claim 1 directly or indirectly to a substrate.

8. applying a metal-containing film-forming composition directly or indirectly to a substrate; forming an organic underlayer film directly or indirectly on the metal-containing film formed by the metal-containing film-forming composition coating step; forming a resist pattern directly or indirectly on the organic underlayer film; forming a pattern on the metal-containing film by etching using the resist pattern as a mask; Equipped with A method for forming a metal-containing film pattern, wherein the metal-containing film-forming composition is the film-forming composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Solution material for underlayer film and pattern forming method using the same

    JP2001272788A

  • Aqueous photosensitive resin composition, method for producing aqueous photosensitive resin composition, and method for manufacturing printed wiring board

    JP2009300533A

  • Photosensitive resin composition, photosensitive element using the same, method for forming barrier rib of image display device, and method for manufacturing image display device

    JP2010066676A

  • Composition for forming titanium-containing resist underlayer film and patterning process

    JP2014134592A

  • Curable composition, production method of cured product, production method of cured film, cured film, touch panel and display device

    JP2016044212A