Composite particles, cathodes and solid-state batteries

A composite coating film with fluorine and glass network-forming elements on positive electrode particles in all-solid-state batteries addresses the resistance increase issue, improving durability and performance.

JP7589718B2Active Publication Date: 2024-11-26TOYOTA JIDOSHA KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2022113131
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-07-14
Publication Date
2024-11-26
Estimated Expiration
2042-07-14

AI Technical Summary

Technical Problem

Existing all-solid-state batteries face an increase in resistance rate after durability tests under high voltage, particularly in sulfide-based systems, necessitating improved coating films for positive electrode active material particles.

Method used

A composite coating film is applied to the positive electrode active material particles, comprising fluorine and at least one of phosphorus and glass network-forming elements, with specific elemental concentration ratios to suppress resistance increase, including metal elements like aluminum, titanium, or zirconium.

Benefits of technology

The composite coating significantly reduces the rate of resistance increase under high voltage conditions, enhancing the durability and performance of all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589718000002
    Figure 0007589718000002
  • Figure 0007589718000003
    Figure 0007589718000003
  • Figure 0007589718000004
    Figure 0007589718000004
Patent Text Reader

Abstract

To reduce the increase rate of a resistance.SOLUTION: The present invention relates to composite particles including positive electrode active material particles and a coating film, the coating film covering at least a part of the surface of the positive electrode active material particles and the coating film including at least one type selected from the group of fluorine, phosphorus, and a glass network formation element.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a composite particle, a positive electrode, an all-solid-state battery, and a method for producing the composite particle. [Background technology]

[0002] Patent Document 1 (JP-A-2003-338321) discloses a high-voltage all-solid-state battery in which the surface of a positive electrode active material is coated with an inorganic solid electrolyte containing lithium (Li). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2003-338321 A Summary of the Invention [Problem to be solved by the invention]

[0004] It has been proposed to form a coating film on the surface of positive electrode active material particles. For example, in sulfide-based all-solid-state batteries, the coating film is expected to reduce the initial resistance by preventing direct contact between the sulfide solid electrolyte and the positive electrode active material particles. However, there is room for improvement in the rate of increase in resistance after durability tests under high voltage.

[0005] An object of the present disclosure is to reduce the rate of increase in resistance. [Means for solving the problem]

[0006] The technical configuration and effects of the present disclosure will be described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure.

[0007] [1] Positive electrode active material particles; A coating film; A composite particle comprising: the coating film covers at least a part of the surface of the positive electrode active material particle, The coating film comprises composite particles containing fluorine (F) and at least one element selected from the group consisting of phosphorus (P) and a glass network forming element.

[0008] According to the composite particle of the above [1], it is possible to provide a coating film with a suppressed rate of increase in resistance (particularly, a coating film having excellent durability under high voltage).

[0009] As a result of examining materials to be added to the coating film, the inventors found that for a coating film containing at least one element selected from the group consisting of P and glass network forming elements, the inclusion of F further reduces the rate of increase in resistance after a durability test.

[0010] [2] The composite particle according to [1], wherein the glass network forming element is at least one selected from the group consisting of boron (B), silicon (Si), nitrogen (N), sulfur (S), germanium (Ge), and hydrogen (H).

[0011] [3] The following formula (1): C F / (C P +C Z ) ≦0.2 (1) Fulfilling the relationship, In the above formula (1), C F , C P , C Z indicates the element concentration measured by X-ray photoelectron spectroscopy, C F indicates the elemental concentration of fluorine, C P indicates the elemental concentration of phosphorus, C Z indicates the element concentration of the glass network forming element. The composite particle according to [1] or [2].

[0012] [4] The coating film further contains a metal element, The composite particle according to any one of [1] to [3], wherein the metal element is at least one selected from the group consisting of aluminum (Al), titanium (Ti) and zirconium (Zr).

[0013] [5] A positive electrode comprising the composite particle according to any one of [1] to [4] and a sulfide solid electrolyte.

[0014] [6] An all-solid-state battery comprising the positive electrode according to [5]. [7] (a) preparing a mixture by mixing a coating liquid and positive electrode active material particles; and (b) drying the mixture to produce composite particles; Including, The coating liquid includes a solute and a solvent, The method for producing composite particles, wherein the solute contains F and at least one selected from the group consisting of P and a glass network forming element.

[0015] The coating liquid adhered to the surface of the positive electrode active material particles is dried to form a coating film. The coating liquid according to the above item [7] can form the coating film according to the above item [1].

[0016] [8] The coating liquid further contains a metal element, The method for producing composite particles according to [7], wherein the metal element is at least one selected from the group consisting of Al, Ti, and Zr. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a conceptual diagram showing a composite particle in this embodiment. [Diagram 2] FIG. 2 is a conceptual diagram showing the all-solid-state battery in this embodiment. [Diagram 3] FIG. 3 is a schematic flow chart of the method for producing composite particles in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the example do not limit the technical scope of the present disclosure.

[0019] <Definitions of terms, etc.> The words "comprise," "include," "have," and variations thereof (e.g., "consisting of") are open-ended. The open-ended form may or may not include additional elements in addition to the required elements. The words "consisting of" are closed-ended. However, the closed form does not exclude additional elements that are normally associated with the technology or that are unrelated to the technology disclosed. The words "consisting essentially of..." are semi-closed. The semi-closed form allows for the addition of elements that do not substantially affect the basic and novel characteristics of the technology disclosed.

[0020] Expressions such as "may" and "may" are used in the permissive sense, meaning "to have the possibility," rather than in the obligatory sense, meaning "to have to."

[0021] Elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only "one particle" but also "an aggregate of particles (powder, powder, particle group)."

[0022] Unless otherwise specified, the order of execution of the steps, operations, and the like included in various methods is not limited to the order described. For example, the steps may proceed simultaneously. For example, the steps may be performed in sequence.

[0023] For example, a numerical range such as "m to n%" includes the upper limit and the lower limit unless otherwise specified. That is, "m to n%" indicates a numerical range of "m% or more and n% or less". Furthermore, "m% or more and n% or less" includes "more than m% and less than n%". Furthermore, a numerical value arbitrarily selected from within the numerical range may be set as a new upper limit or lower limit. For example, a new numerical range may be set by arbitrarily combining a numerical value within the numerical range with a numerical value described in another part of this specification, in a table, in a figure, or the like.

[0024] When a compound is expressed by a stoichiometric composition formula (e.g., "LiCoO2", etc.), the stoichiometric composition formula is merely a representative example of the compound. The compound may have a non-stoichiometric composition. For example, when lithium cobalt oxide is expressed as "LiCoO2", unless otherwise specified, the lithium cobalt oxide is not limited to the composition ratio of "Li / Co / O=1 / 1 / 2" and may contain Li, Co, and O in any composition ratio. Furthermore, doping, substitution, etc. with trace elements may also be allowed.

[0025] "D50" refers to the particle size at which the cumulative frequency from the small particle size side reaches 50% in the volume-based particle size distribution. D50 can be measured by a laser diffraction method. For example, a laser diffraction type particle size distribution measuring device "Product name SALD-7500" (or an equivalent product) manufactured by Shimadzu Corporation may be used.

[0026] The term "glass network forming element" refers to an element that has glass-forming ability. The term "glass-forming ability" refers to the ability of the target element to form an oxide glass having a network structure by bonding with oxygen (O).

[0027] <XPS Measurement> (composition ratio of particle surface) C in the above formula (1) F , C p , C Zcan be measured by the following procedure. An XPS instrument is prepared. For example, an XPS instrument manufactured by ULVAC-PHI, Inc., product name: PHI X-tool (or equivalent) may be used. A sample powder consisting of composite particles is set in the XPS instrument. Narrow scan analysis is performed with a pass energy of 224 eV. The measurement data is processed by analysis software. For example, an analysis software manufactured by ULVAC-PHI, Inc., product name: MulTiPak (or equivalent) may be used. The peak area (integral value) of the F1s spectrum is used as the elemental concentration of F (C F The peak area of ​​the P2p spectrum is converted to the elemental concentration of P (C P ) for Z. An appropriate spectrum is selected depending on the type of Z. For example, for B, the peak area of ​​the B1s spectrum is the element concentration of B (C Z ) is converted to C F But, C P and C Z The composition ratio of F on the particle surface (C F / (C p +C Z ) ) is obtained.

[0028] (Coverage rate) The coverage is also measured by XPS. By analyzing the above measurement data, the ratio of each element can be obtained from the peak areas of C1s, O1s, F1s, P2p, B1s, M2p3, etc.

[0029] For example, the coverage is calculated by the following formula (2). θ=(F+P+Z) / (F+P+Z+M)×100 (2) In the above formula (2), θ represents the coverage (%), and F, P, Z, and M represent the ratio of each element.

[0030] Note that "M2p3" and M in the above formula (2) are constituent elements of the positive electrode active material particles and represent an element other than Li and oxygen (O). That is, the positive electrode active material particles may be represented by the following formula (3).

[0031] LiMO2(3) M may be composed of one element or multiple elements. M may be, for example, at least one element selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn) and aluminum (Al). When M contains multiple elements, the sum of the composition ratios of the elements may be 1.

[0032] For example, the positive electrode active material particles are "LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 When "O2", the above formula ( 2 ) can be transformed into the following formula (3'):

[0033] θ=(F+P+Z) / (F+P+Z+Ni+Co+Mn)×100 (3') In the above formula (3'), Ni represents the element ratio of nickel determined from the peak area of ​​Ni2p3, Co represents the element ratio of cobalt determined from the peak area of ​​Co2p3, and Mn represents the element ratio of manganese determined from the peak area of ​​Mn2p3.

[0034] <Film thickness measurement> The film thickness (thickness of the coating film) can be measured by the following procedure. A sample is prepared by embedding composite particles in a resin material. A cross-section is processed on the sample by an ion milling device. For example, an ion milling device "Product name Arblade (registered trademark) 5000" (or an equivalent product) manufactured by Hitachi High-Technologies Corporation may be used. The cross-section of the sample is observed by an SEM (Scanning Electron Microscope). For example, an SEM device "Product name SU8030" (or an equivalent product) manufactured by Hitachi High-Technologies Corporation may be used. The film thickness is measured in 20 fields of view for each of 10 composite particles. The arithmetic average of the film thicknesses at a total of 200 points is regarded as the film thickness.

[0035] <Composite particles> FIG. 1 is a conceptual diagram showing a composite particle in this embodiment. The composite particle 5 may be called, for example, a "coated positive electrode active material". The composite particle 5 includes a positive electrode active material particle 1 and a coating film 2. The composite particle 5 may form, for example, an aggregate. That is, one composite particle 5 may include two or more positive electrode active material particles 1. The composite particle 5 may have, for example, a D50 of 1 to 50 μm, a D50 of 1 to 20 μm, or a D50 of 5 to 15 μm.

[0036] <Coating film> The coating film 2 is a shell of the composite particle 5. The coating film 2 covers at least a part of the surface of the positive electrode active material particle 1.

[0037] Coating film 2 contains F and at least one selected from the group consisting of P and glass network forming elements. The glass network forming element may contain, for example, at least one selected from the group consisting of B, Si, N, S, Ge, and H. When coating film 2 contains F and at least one selected from the group consisting of P and glass network forming elements, the resistance increase rate can be reduced.

[0038] The coverage may be, for example, 80% or more. A coverage of 80% or more is expected to reduce battery resistance. The coverage may be, for example, 85% or more, or 90% or more. The coverage may be, for example, 100%, or 99% or less, or 95% or less. The coverage may be, for example, 80 to 100%.

[0039] The coating film 2 may have a thickness of, for example, 5 to 100 nm, 5 to 50 nm, 10 to 30 nm, or 20 to 30 nm.

[0040] The glass network forming element and O may form an oxide glass. That is, the coating film 2 may contain an oxide glass having a network structure. The oxide glass may contain, for example, a phosphate skeleton and a borate skeleton. That is, the coating film 2 may contain, for example, at least one skeleton selected from the group consisting of a phosphate skeleton and a borate skeleton. For example, in TOF-SIMS (Time-of-Flight Secondary Ion Mass Spectrometry) of the composite particle 5, PO2 - , PO3 - When a fragment such as BO2 is detected, the coating film 2 is considered to contain a phosphate skeleton. - , BO3 - When a fragment such as is detected, the coating film 2 is deemed to contain a boric acid skeleton.

[0041] The composite particle 5 may, for example, satisfy the relationship of the following formula (1). C F / (C P +C Z ) ≦0.2 (1) C F , C P , C Z indicates the element ratio measured by XPS. F indicates the element ratio of F. P indicates the element ratio of P. Z indicates the element ratio of the glass network forming element. When the coating film 2 contains a plurality of glass network forming elements, C Z C represents the total element ratio of each glass network forming element. F / (C P +C Z ) When is 0.2 or less, the resistance increase rate is expected to be reduced. F / (C P +C Z) may be, for example, 0.15 or less, or 0.1 or less.

[0042] Furthermore, the composite particle 5 may satisfy, for example, the relationship of the following formula (4). C F / C P ≦0.2 (4) C F / C P When is 0.2 or less, the resistance increase rate is expected to be reduced. F / C P may be, for example, 0.15 or less, or 0.1 or less.

[0043] The coating film 2 may contain, for example, Li, carbon (C), etc. Furthermore, the coating film 2 may further contain at least one metal element selected from the group consisting of Al, Ti, and Zr.

[0044] The composite particle 5 may, for example, satisfy the relationship of the following formula (5). C Y / (C P +C Z ) ≦0.1 (5) C Y indicates the element ratio of at least one metal element selected from the group consisting of Al, Ti, and Zr, as measured by XPS. When the coating film 2 contains a plurality of metal elements, C Y indicates the total elemental ratio of each metal element. Y / (C P +C Z ) When is less than 0.1, the resistance increase rate is expected to be further reduced. Y / (C P +C Z ) may be, for example, 0.05 or less, or 0.03 or less.

[0045] C in the above formula (5) Y can be measured by the above-mentioned measurement method. For Y, an appropriate spectrum is selected depending on the type of Y. For example, in the case of Al, the peak area of ​​the Al2p spectrum represents the element concentration of Al (C Y ) is converted to C Y But, C P and C Z The composition ratio (C Y / (C P +C Z ) ) is obtained.

[0046] When the coating film 2 further contains at least one metal element selected from the group consisting of Al, Ti, and Zr, the coverage is calculated, for example, by the following formula (6): The coverage can be measured by the above-mentioned measurement method.

[0047] θ=(F+P+Z+Y) / (F+P+Z+Y+M)×100 (6) 《Cathode active material particles》 The positive electrode active material particle 1 is a core of the composite particle 5. The positive electrode active material particle 1 may be a secondary particle (aggregation of primary particles). The positive electrode active material particle 1 (secondary particle) may have a D50 of, for example, 1 to 50 μm, may have a D50 of 1 to 20 μm, or may have a D50 of 3 to 15 μm. The primary particle may have a maximum Feret diameter of, for example, 0.1 to 3 μm.

[0048] The positive electrode active material particles 1 may contain any component. 1may contain at least one selected from the group consisting of LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, Li(NiCoAl)O2, and LiFePO4. For example, "(NiCoMn)" in "Li(NiCoMn)O2" indicates that the sum of the composition ratios in the parentheses is 1. As long as the sum is 1, the amount of each component is arbitrary. Li(NiCoMn)O2 may contain at least one selected from the group consisting of LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(NiCoMn)O2, Li(NiCoAl)O2, and LiFePO4. For example, "(NiCoMn)" in "Li(NiCoMn)O2" indicates that the sum of the composition ratios in the parentheses is 1. As long as the sum is 1, the amount of each component is arbitrary. 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.8 Co 0.1 Mn 0.1 It may contain O2, etc.

[0049] <All-solid-state battery> 2 is a conceptual diagram showing an all-solid-state battery in this embodiment. The all-solid-state battery 100 may include, for example, an exterior body (not shown). The exterior body may be, for example, a pouch made of a metal foil laminate film. The exterior body may house a power generating element 50. The power generating element 50 includes a positive electrode 10, a separator layer 30, and a negative electrode 20. That is, the all-solid-state battery 100 includes a positive electrode 10, a separator layer 30, and a negative electrode 20.

[0050] 《Positive electrode》 The positive electrode 10 is layered. The positive electrode 10 may include, for example, a positive electrode active material layer and a positive electrode current collector. For example, the positive electrode active material layer may be formed by applying a positive electrode mixture to the surface of the positive electrode current collector. The positive electrode current collector may include, for example, an Al foil or the like. The positive electrode current collector may have a thickness of, for example, 5 to 50 μm.

[0051] The positive electrode active material layer may have a thickness of, for example, 10 to 200 μm. The positive electrode active material layer is in close contact with the separator layer 30. The positive electrode active material layer includes a positive electrode mixture. The positive electrode mixture includes composite particles and a sulfide solid electrolyte. That is, the positive electrode 10 includes composite particles and a sulfide solid electrolyte. Details of the composite particles are as described above.

[0052] The sulfide solid electrolyte can form an ion conduction path in the positive electrode active material layer. The amount of the sulfide solid electrolyte may be, for example, 1 to 200 parts by volume, 50 to 150 parts by volume, or 50 to 100 parts by volume, relative to 100 parts by volume of the composite particles (positive electrode active material). The sulfide solid electrolyte contains S. The sulfide solid electrolyte may contain, for example, Li, P, and S. The sulfide solid electrolyte may further contain, for example, O, Si, etc. The sulfide solid electrolyte may further contain, for example, a halogen, etc. The sulfide solid electrolyte may further contain, for example, iodine (I), bromine (Br), etc. The sulfide solid electrolyte may be, for example, glass ceramics or argyrodite. The sulfide solid electrolyte may include, for example, at least one selected from the group consisting of LiI-LiBr-Li3PS4, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2O-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-P2S5, and Li3PS4.

[0053] For example, "LiI-LiBr-Li3PS4" refers to a sulfide solid electrolyte produced by mixing LiI, LiBr, and Li3PS4 in any molar ratio. For example, the sulfide solid electrolyte may be produced by a mechanochemical method. "Li2S-P2S5" includes Li3PS4. Li3PS4 can be produced, for example, by mixing Li2S and P2S5 in a molar ratio of Li2S / P2S5=75 / 25.

[0054] The positive electrode active material layer may further include, for example, a conductive material. The conductive material may form an electronic conduction path in the positive electrode active material layer. The amount of the conductive material may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the composite particles (positive electrode active material). The conductive material may include any component. The conductive material may include, for example, at least one selected from the group consisting of carbon black, vapor grown carbon fiber (VGCF), carbon nanotube (CNT), and graphene flake.

[0055] The positive electrode active material layer may further include, for example, a binder. The amount of the binder may be, for example, 0.1 to 10 parts by mass with respect to 100 parts by mass of the composite particles (positive electrode active material). The binder may include any component. The binder may include, for example, at least one selected from the group consisting of polyvinylidene fluoride (PVdF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), styrene butadiene rubber (SBR), and polytetrafluoroethylene (PTFE).

[0056] 《Negative electrode》 The negative electrode 20 is layered. The negative electrode 20 may include, for example, a negative electrode active material layer and a negative electrode current collector. For example, the negative electrode active material layer may be formed by applying a negative electrode mixture to the surface of the negative electrode current collector. The negative electrode current collector may include, for example, copper (Cu) foil, Ni foil, etc. The negative electrode current collector may have a thickness of, for example, 5 to 50 μm.

[0057] The negative electrode active material layer may have a thickness of, for example, 10 to 200 μm. The negative electrode active material layer is in close contact with the separator layer 30. The negative electrode active material layer includes a negative electrode mixture. The negative electrode mixture includes negative electrode active material particles and a sulfide solid electrolyte. The negative electrode mixture may further include a conductive material and a binder. The sulfide solid electrolyte may be the same or different between the negative electrode mixture and the positive electrode mixture. The negative electrode active material particles may include any component. The negative electrode active material particles may include, for example, graphite, Si, silicon oxide [SiO x (0 <x<2)〕、およびLi4Ti5O 12 may contain at least one selected from the group consisting of:

[0058] <Separator layer> The separator layer 30 is interposed between the positive electrode 10 and the negative electrode 20. The separator layer 30 separates the positive electrode 10 from the negative electrode 20. The separator layer 30 includes a sulfide solid electrolyte. The separator layer 30 may further include a binder. The sulfide solid electrolyte may be the same or different between the separator layer 30 and the positive electrode composite. The sulfide solid electrolyte may be the same or different between the separator layer 30 and the negative electrode composite.

[0059] <Method of manufacturing composite particles> 3 is a schematic flow chart of the method for producing composite particles in this embodiment. Hereinafter, the "method for producing composite particles in this embodiment" may be abbreviated as "this production method". This production method includes "(a) preparation of a mixture" and "(b) production of composite particles". This production method may further include, for example, "(c) heat treatment" or the like.

[0060] (a) Preparation of the mixture The present manufacturing method includes preparing a mixture by mixing a coating liquid with positive electrode active material particles. The details of the positive electrode active material particles are as described above. The mixture may be, for example, a suspension or a wet powder. For example, a suspension may be formed by dispersing positive electrode active material particles (powder) in a coating liquid. For example, a wet powder may be formed by spraying a coating liquid into a powder. In the present manufacturing method, any mixing device, granulating device, etc. may be used.

[0061] The coating liquid includes a solute and a solvent. The solute includes, as a raw material of the coating film, F and at least one selected from the group consisting of P and glass network forming elements. The coating liquid may further include, for example, a suspended solid (insoluble component), a precipitate, etc.

[0062] The amount of the solute may be, for example, 0.1 to 20 parts by mass, 1 to 15 parts by mass, or 5 to 10 parts by mass, relative to 100 parts by mass of the solvent. The solvent may contain any component as long as the solute dissolves therein. The solvent may contain, for example, water, alcohol, etc. The solvent may contain, for example, ion-exchanged water, etc.

[0063] The details of the glass network forming elements are as described above. The solute may include at least one selected from the group consisting of oxoacids of glass network forming elements and oxides of glass network forming elements. The solute may include at least one selected from the group consisting of phosphoric acid, boric acid, silicic acid, nitric acid, sulfuric acid, and germanic acid. The solute may include orthophosphoric acid, metaphosphoric acid, orthoboric acid, metaboric acid, etc.

[0064] In the above coating liquid, for example, the relationship of the following formula (7) may be satisfied.

[0065] n F / (n P +n Z ) ≦0.2 (7) In the above formula (7), n F denotes the molar concentration of F, and n P P Mole indicates the concentration, n Z indicates the molar concentration of the glass network forming element. When the coating liquid contains multiple types of glass network forming elements, n Z represents the sum of the molar concentrations of the glass network forming elements. When the molar ratio is 0.2 or less, a reduction in the rate of increase in resistance is expected. F / (n P +n Z ) may be, for example, 0.15 or less, or 0.1 or less.

[0066] In addition, in the above coating liquid, for example, the relationship of the following formula (8) may be satisfied.

[0067] n F / n P ≦0.2 (8) When the molar ratio is 0.2 or less, a reduction in the rate of increase in resistance is expected. F / n P may be, for example, 0.15 or less, or 0.1 or less.

[0068] The solute may further contain at least one metal element selected from the group consisting of Al, Ti, and Zr. In the coating liquid, for example, the relationship of the following formula (9) may be satisfied.

[0069] n Y / (n P +n Z ) ≦0.1 (9) n Y represents the molar concentration of at least one metal element selected from the group consisting of Al, Ti, and Zr. When the coating liquid contains multiple metal elements, n Y indicates the sum of the molar concentrations of the metal elements. When the molar ratio is 0.1 or less, a further reduction in the rate of increase in resistance is expected. Y / (n P +n Z ) may be, for example, 0.05 or less, or 0.03 or less.

[0070] The solute may further include a lithium compound, for example, lithium hydroxide, lithium carbonate, lithium nitrate, etc.

[0071] (b) Production of Composite Particles The present manufacturing method includes producing composite particles by drying the mixture. The coating solution attached to the surface of the positive electrode active material particles is dried to produce a coating film. In the present manufacturing method, any drying method can be used.

[0072] For example, the composite particles may be formed by a spray-drying method. That is, the suspension is sprayed from a nozzle to form droplets. The droplets contain the positive electrode active material particles and the coating liquid. For example, the droplets are dried by hot air to form the composite particles. The use of the spray-drying method is expected to improve, for example, the coverage rate.

[0073] The solid content of the suspension for spray drying may be, for example, 1 to 50% or 10 to 30% by volume. The nozzle diameter may be, for example, 0.1 to 10 mm or 0.1 to 1 mm. The hot air temperature may be, for example, 100 to 200°C.

[0074] For example, the composite particles may be produced by a tumbling fluidized bed coating apparatus. In the tumbling fluidized bed coating apparatus, "(a) preparation of the mixture" and "(b) production of the composite particles" can be carried out simultaneously.

[0075] (c) Heat Treatment The present manufacturing method may include subjecting the composite particles to a heat treatment. The coating film may be fixed by the heat treatment. The heat treatment may also be called "baking". In the present manufacturing method, any heat treatment device may be used. The heat treatment temperature may be, for example, 150 to 300°C. The heat treatment time may be, for example, 1 to 10 hours. For example, the heat treatment may be performed in air, or in an inert (nitrogen) atmosphere. EXAMPLES

[0076] The present embodiment will be described below using examples, but the present embodiment is not limited to these.

[0077] No.1 (positive electrode) 870.4 parts by mass of hydrogen peroxide solution (mass concentration 30%) were added to the container. Next, 987.4 parts by mass of ion-exchanged water and 44.2 parts by mass of niobic acid [Nb2O5·3H2O] were added to the container. Next, 87.9 parts by mass of ammonia water (mass concentration 28%) were added to the container. The contents of the container were thoroughly stirred to form a coating liquid. The coating liquid is believed to contain a peroxo complex of Nb.

[0078] As the positive electrode active material particles, Li(Ni 1 / 3 Co 1 / 3 Mn 1 / 3 )O2 was prepared. 50 parts by mass of a powder of positive electrode active material particles was dispersed in 53.7 parts by mass of a coating liquid to prepare a suspension. A spray dryer manufactured by BUCHI (product name: Mini Spray Dryer B-290) was prepared. The suspension was supplied to the spray dryer to produce a powder of composite particles. The supply air temperature of the spray dryer was 200°C, and the supply air volume was 0.45 m 3 / min. The composite particles were heat treated in air. The heat treatment temperature was 200°C. The heat treatment time was 5 hours. It is considered that the coating film of composite particle No. 1 contains LiNbO3. The coverage was measured by the above-mentioned procedure. The results are shown in Table 1 below. The coverage was also measured in the same manner for Nos. 2 to 6 described later.

[0079] The following materials were prepared: Sulfide solid electrolyte: 10LiI-15LiBr-75Li3PS4 Conductive material: VGCF Binder: SBR Dispersion medium: heptane Positive electrode current collector: Aluminum foil A positive electrode slurry was prepared by mixing the composite particles, the sulfide solid electrolyte, the conductive material, the binder, and the dispersion medium. The mixing ratio of the composite particles and the sulfide solid electrolyte was "composite particles / sulfide solid electrolyte = 6 / 4 (volume ratio)". The amount of the conductive material was 3 parts by mass for 100 parts by mass of the composite particles. The amount of the binder was 3 parts by mass for 100 parts by mass of the composite particles. The positive electrode slurry was thoroughly stirred using an ultrasonic homogenizer (product name "UH-50", manufactured by SMT). The positive electrode slurry was applied to the surface of the positive electrode current collector to form a coating film. The coating film was dried at 100 °C for 30 minutes using a hot plate. In this way, a positive electrode raw sheet was manufactured. A disk-shaped positive electrode was cut out from the positive electrode raw sheet. The area of ​​the positive electrode was 1 cm2. 2 It was.

[0080] (Negative electrode) The following materials were prepared:

[0081] Negative electrode active material particles: graphite Sulfide solid electrolyte: 10LiI-15LiBr-75Li3PS4 Conductive material: VGCF Binder: SBR Dispersion medium: heptane Negative electrode current collector: Cu foil A sulfide solid electrolyte, a conductive material, a binder, and a dispersion medium were mixed with a stirring device (Filmix (registered trademark) "Model 30-L", manufactured by Primix Corporation) to prepare a slurry. The stirring speed (number of revolutions) was 2000 rpm, and the stirring time was 30 minutes. After stirring for 30 minutes, negative electrode active material particles were added to the slurry, and the slurry was further stirred. The stirring speed was 15000 rpm, and the stirring time was 60 minutes.

[0082] The mixing ratio of the negative electrode active material particles and the sulfide solid electrolyte was "negative electrode active material particles / sulfide solid electrolyte = 6 / 4 (volume ratio)". The amount of the conductive material was 1 part by mass per 100 parts by mass of the negative electrode active material particles. The amount of the binder was 2 parts by mass per 100 parts by mass of the negative electrode active material particles.

[0083] The slurry was applied to the surface of the negative electrode current collector to form a coating film. The coating film was dried at 100°C for 30 minutes on a hot plate. In this way, a negative electrode blank was produced. A disk-shaped negative electrode was cut out from the negative electrode blank. The area of ​​the negative electrode was 1 cm. 2 It was.

[0084] (Separator layer) The following materials were prepared:

[0085] Sulfide solid electrolyte: LiI-Li2S-P2S5 (glass ceramic type, D50=2.5μm) As a press processing die, the inner cross-sectional area is 1 cm 2 A cylindrical ceramic of 64.8 mg was placed in a mold, smoothed, and then subjected to a pressure of 1 ton / cm. 2 The separator layer was obtained by pressing and compacting the mixture at a pressure of 1000 MPa.

[0086] (All-solid-state battery) In the mold, a positive electrode was placed on one side of the separator layer, and a negative electrode was placed on the other side. 2 The negative electrode, separator layer, and positive electrode were pressed together for one minute with a pressure of 0.5 ton / cm. A stainless steel rod was placed between the positive electrode and the negative electrode, and a pressure of 0.5 ton / cm was applied. 2 A power generating element was formed by binding the electrode with a magnet. A pouch made of aluminum laminate film was prepared as a housing. Power Generation The elements were then encapsulated in a housing, forming a solid-state battery.

[0087] No.2 A phosphoric acid solution was prepared by dissolving 10.8 parts by mass of metaphosphoric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) in 166 parts by mass of ion-exchanged water. A coating solution was prepared by dissolving boric acid (manufactured by Nacalai Tesque, Inc.) in the phosphoric acid solution so that the molar ratio of B to P was 1.0. Except for these, composite particles, positive electrodes, and all-solid-state batteries were manufactured in the same manner as in No. 1. In addition, in the composite particles of No. 2, the coating film was formed of, for example, BPO X B.x PO y (x and y are arbitrary numbers), and the same applies to Nos. 3 to 6 described below.

[0088] No.3 Composite particles, a positive electrode, and an all-solid-state battery were manufactured in the same manner as in No. 1, except that the same coating solution as in No. 2 was prepared and the heat treatment of the composite particles was performed under a nitrogen atmosphere at 400°C.

[0089] No.4 Ammonium fluoride (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in the coating solution No. 2 so that the molar ratio of F to P and the glass network forming element B was 0.1, to prepare a coating solution. From this point on, composite particles, positive electrodes, and all-solid-state batteries were manufactured in the same manner as in No. 1. In addition, the composition ratio (C F / (C P +C Z ) The composition ratio (C:B) of the particle surface was also measured. The results are shown in Table 1. F / (C P +C Z ) ) was measured.

[0090] No.5 Composite particles, a positive electrode, and an all-solid-state battery were manufactured in the same manner as in No. 1, except that the same coating solution as in No. 4 was prepared and the heat treatment of the composite particles was performed under a nitrogen atmosphere at 400°C.

[0091] No.6 Aluminum nitrate nonahydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in the coating solution No. 4 so that the molar ratio of the metal element Al to P and B was 0.05, to prepare a coating solution. From this point on, composite particles, positive electrodes, and all-solid-state batteries were manufactured in the same manner as in No. 1. In addition, the composition ratio (C Y / (C P +C Z ) ) (Y:Al, Z:B) were measured. The results are shown in Table 1 below.

[0092] <Evaluation> The initial capacity of the all-solid-state battery (hereinafter also referred to as the "cell") was confirmed. The charge and discharge conditions were as follows:

[0093] Charging: constant current-constant voltage method, rate = 1 / 3C Discharge: constant current, rate = 1 / 3C After checking the initial capacity, the SOC of the cell was adjusted to 40%. The cell was discharged at a rate of 2C for 5 seconds. The initial resistance was calculated from the voltage drop after 5 seconds. The results are shown in Table 1 below.

[0094] After measuring the initial resistance, the cell was stored in a thermostatic chamber at 60°C for 14 days. During storage, the cell was trickle charged so that the positive electrode potential was maintained at 4.5V. After 14 days, the post-endurance resistance was measured under the same conditions as the initial resistance. The resistance increase ratio was calculated by dividing the post-endurance resistance by the initial resistance. The results are shown in Table 1 below.

[0095] [Table 1]

[0096] <Result> In Nos. 4 to 6 in which the coating film contains F and at least one selected from the group consisting of P and glass network forming elements, the resistance increase rate is reduced.

[0097] The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are not restrictive. The technical scope of the present disclosure includes all modifications within the meaning and scope equivalent to the description of the claims. For example, it is also intended from the beginning that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Explanation of symbols]

[0098] 1 positive electrode active material particle, 2 coating film, 5 composite particle, 10 positive electrode, 20 negative electrode, 30 separator layer, 50 power generating element, 100 all-solid-state battery.

Claims

1. Positive electrode active material particles; A coating film; A composite particle comprising: the coating film covers at least a part of the surface of the positive electrode active material particle, The coating film contains fluorine, phosphorus and a glass network forming element, the glass network forming element is boron; The following formula (1): C F / (C P +C Z )≦0.2 (1) Fulfilling the relationship, In the above formula (1), C F , C P , and C Z represent element concentrations measured by X-ray photoelectron spectroscopy; C F represents the elemental concentration of fluorine; C P represents the elemental concentration of phosphorus; C Z represents the element concentration of the glass network forming element in the composite particle.

2. The coating film further contains a metal element, The composite particle according to claim 1 , wherein the metal element is at least one selected from the group consisting of aluminum, titanium and zirconium.

3. A positive electrode comprising the composite particle according to claim 1 or 2 and a sulfide solid electrolyte.

4. An all-solid-state battery comprising the positive electrode according to claim 3.

Citation Information

Patent Citations

  • Secondary battery

    JP2003338321A

  • Nonaqueous electrolyte secondary battery

    JP2016115654A

  • Nonaqueous electrolyte electricity storage element and method for producing same

    WO2017099201A1