Semiconductor device manufacturing method, semiconductor device, semiconductor module, and power conversion device

The method addresses productivity and reliability issues in manufacturing vertical semiconductor devices by using rapid annealing to form field stop layers on large-diameter wafers, reducing on-voltage and switching loss, and minimizing noise and leakage current.

JP7589879B2Active Publication Date: 2024-11-26MINEBEA POWER SEMICON DEVICE INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021008581
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-22
Publication Date
2024-11-26
Estimated Expiration
2041-01-22

AI Technical Summary

Technical Problem

Existing methods for manufacturing vertical semiconductor devices like IGBTs and PIN diodes using large-diameter wafers face issues with productivity, reliability, and increased switching noise due to long annealing times and crystal defects, leading to high on-voltage and switching losses.

Method used

A method involving ion irradiation followed by rapid annealing at 300°C to 450°C for 60 seconds or less to form a field stop layer on large-diameter wafers, using light ions like protons, and removing crystal defects to enhance productivity and reduce switching noise.

Benefits of technology

The method improves productivity, reduces on-voltage and switching loss, suppresses high-frequency oscillation, and minimizes leakage current, ensuring reliable operation of semiconductor devices and power conversion devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589879000001
    Figure 0007589879000001
  • Figure 0007589879000002
    Figure 0007589879000002
  • Figure 0007589879000003
    Figure 0007589879000003
Patent Text Reader

Abstract

To provide a semiconductor device capable of improving the manufacturability of a field stop layer (n-buffer layer) of a vertical semiconductor device such as IGBTs and PIN diodes on which it is possible to make use of a large diameter (8inch or more) wafer, and a power conversion device using the same.SOLUTION: A manufacturing method for a semiconductor device includes the steps of, after forming a pattern on a main surface of a drift layer (101) of a first conductivity type, irradiating ions to a predetermined depth from a second main surface, after ion irradiation, forming a field stop layer (108) by turning the ions to donors through an annealing process of heating at 300°C to 450°C for 60 seconds or less, and reducing the thickness of a semiconductor substrate from the second main surface to a predetermined value so as to remove crystal defects generated in the process of ion irradiation.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a semiconductor device, a semiconductor device, a semiconductor module, and a power conversion device. [Background technology]

[0002] Semiconductor devices such as IGBTs (Insulated Gate Bipolar Transistors) and PIN diodes (p-Intrinsic-n Diodes) have a vertical structure. In an IGBT, a region including an N-type drift layer, an N-type buffer layer, and a P-type collector layer has a vertical structure. In a diode, a region including an N-type drift layer, an N-type buffer layer, and a P-type collector layer has a vertical structure. + The region including the cathode layer has a vertical structure.

[0003] In vertical semiconductor devices such as IGBTs or diodes having a vertical structure region, wafers manufactured by the FZ (Floating-Zone) method are used as the Si wafers for manufacturing the semiconductor devices in order to reduce costs, instead of wafers manufactured by epitaxial growth. In addition, the diameter of Si wafers has been increasing in recent years. In order to reduce the on-voltage and switching loss of the above semiconductor devices, it has been considered to make the n-type drift layer thinner.

[0004] In order to reduce the on-state voltage and switching loss of the above-mentioned semiconductor devices, it is effective to make the n-type drift layer that constitutes the semiconductor device thinner. However, in terms of switching noise, if the current drop during switching is rapid and the natural disappearance period of the accumulated carriers, known as the tail current, is not secured, the current will disappear abruptly, resulting in a surge voltage (L·d I / d t ) and oscillate at frequencies of several MHz or more. There are concerns that this noise may have adverse effects on motor insulation, overvoltage element destruction, element malfunction, etc.

[0005] To solve the problems of reducing switching loss and switching noise, the following conventional techniques have been disclosed.

[0006] Patent Document 1 discloses a technique for forming a deep n-buffer layer made of oxygen thermal donors continuously over a region having a thickness of 30 μm or more adjacent to an n-type layer, thereby suppressing the oscillation phenomenon caused by a sudden decrease in tail current. Patent Document 2 discloses a technique for forming a deep n-buffer layer in which phosphorus (P) is used as a dopant for the deep n-buffer layer. Patent Document 3 discloses a technique for forming a deep n-buffer layer in which hydrogen (proton) ion irradiation and subsequent annealing are applied. Patent Document 4 discloses a technique for forming a deep n-buffer layer in which several n-buffer layers are formed by multiple proton irradiations. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2018-56220 A [Patent Document 2] JP 2014-146721 A [Patent Document 3] Special Publication No. 2003-533047 [Patent Document 4] International Publication No. 2017 / 146148 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in Patent Document 1, in order to generate oxygen thermal donors, oxygen elements must be introduced into the silicon at high temperatures of over 1000°C for a long period of time in the initial process of wafer manufacturing, which may lead to a deterioration in the economic efficiency of the wafer manufacturing process, and when large-diameter (8 inches or more) wafers are used, there are concerns that the reliability of IGBTs and diode elements may deteriorate due to slippage caused by an increase in the wafer's own weight. Furthermore, there is a problem that oxygen thermal donors are scraped off by the thin wafer processing after the formation of the IGBT gate structure and anode structure, which reduces productivity.

[0009] In addition, as described in Patent Document 2, when phosphorus (P) is used as a dopant for the n-buffer layer, long-term high-temperature annealing is required as in Patent Document 1, and there are concerns about reduced productivity and reliability degradation due to the occurrence of slips. In addition, when a deep n-buffer layer is formed by hydrogen (proton) ion irradiation and subsequent annealing at 300°C to 500°C for 30 minutes to 5 hours as in Patent Documents 3 and 4, problems arise in the characteristics variation and reduced throughput due to the deterioration of thermal uniformity in the wafer surface when a large-diameter wafer is applied. According to the study by the present inventor, when the annealing process is shortened to improve productivity, a large number of crystal defects are generated in the proton irradiation region, and excessive lifetime killers that reduce the carrier lifetime are generated, which leads to problems such as deterioration of switching noise and increased leakage current when the withstand voltage is maintained.

[0010] The present invention has been made in view of the above-mentioned problems, and has an object to provide a semiconductor device manufacturing method capable of improving the manufacturability of a field stop layer (n-buffer layer) of a vertical semiconductor device such as an IGBT or a PIN diode that can use a large-diameter (8 inches or more) wafer, a semiconductor device, and a power conversion device using the same. [Means for solving the problem]

[0011] One aspect of the present invention for solving the above-mentioned problems is a method for manufacturing a semiconductor device having a semiconductor substrate, a second conductivity type layer formed on a first main surface of the semiconductor substrate, a first conductivity type drift layer formed on a second main surface of the semiconductor substrate opposite to the first main surface, and a first conductivity type field stop layer formed on a surface of the first conductivity type drift layer on the second main surface side and having a higher impurity concentration than the first conductivity type drift layer, the method including irradiating ions to a predetermined depth from the second main surface side. to form the field stop layer. After the ion irradiation, The field stop layer The ion donor is formed by annealing at 300℃ to 450℃ for 60 seconds or less. Transform and irradiating the ions. to form the field stop layer. and reducing the thickness of the semiconductor substrate from the second main surface side to a predetermined value so as to remove crystal defects generated in the step of reducing the thickness of the semiconductor substrate.

[0012] The present invention also provides a semiconductor device, a semiconductor module, and a power conversion device manufactured using the above-described method for manufacturing a semiconductor device.

[0013] More specific configurations of the present invention are described in the claims. Effect of the Invention

[0014] According to the present invention, it is possible to provide a semiconductor device manufacturing method capable of improving the manufacturability of a field stop layer (n-buffer layer) of a vertical semiconductor device such as an IGBT or a PIN diode that can use a large diameter (8 inches or more) wafer, and a semiconductor device, a module, and a power conversion device manufactured by the manufacturing method.

[0015] Problems, configurations and effects other than those described above will become apparent from the following description of the embodiments. [Brief description of the drawings]

[0016] [Figure 1] FIG. 1 is a flow diagram showing an example of a method for manufacturing a semiconductor device according to the present invention. [Diagram 2]FIG. 1(h) is a schematic cross-sectional view of a semiconductor device after the step is completed, and a graph showing the n-type carrier concentration and the light ion concentration. [Diagram 3] Graph showing distribution of n-type carrier concentration and hydrogen concentration in the cross section along line B-B' in step (f) of FIG. [Figure 4] Graph showing recovery waveform [Diagram 5] Graph showing leakage current waveform [Figure 6] Graph showing the relationship between carrier lifetime and n-type carrier concentration [Figure 7] Graph showing the relationship between leakage current failure rate and n-type field stop layer depth [Figure 8] Graph showing the relationship between donor activation rate and temperature when annealing for 60 seconds [Figure 9] Graph showing the relationship between donor activation rate and annealing time when annealed at 300°C [Figure 10] FIG. 1 is a circuit diagram showing a schematic configuration of a power conversion device according to the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The present invention will now be described in detail with reference to the drawings.

[0018] Fig. 1 is a flow diagram showing an example of a method for manufacturing a semiconductor device according to the present invention. Fig. 1 shows a part of a process for manufacturing a freewheel diode of a power semiconductor chip as a semiconductor device, and illustrates the manufacturing flow together with the cross-sectional structure of the semiconductor device. Note that the present invention can also be applied to semiconductor devices such as IGBTs and MOSFETs (Metal-Oxide-Semiconductor Field-Effect Transistors) that pass current in the vertical direction.

[0019] In FIG. 1(a), a Si wafer 101 is prepared as a semiconductor substrate for fabricating a diode. As described later, the present invention is suitable for manufacturing a semiconductor device having a wafer size of 8 inches or more, but can also be applied to manufacturing a semiconductor device having a smaller wafer size. The wafer size can be, for example, 8 inches with a Si wafer thickness of 725 μm and 12 inches with a Si wafer thickness of 775 μm. Here, the Si wafer can be a wafer having a resistivity according to the withstand voltage. For example, the resistivity can be about 55 Ωcm for a diode having a withstand voltage of 1200 V, and about 250 Ωcm for a diode having a withstand voltage of 3.3 kV. Hereinafter, in FIG. 1(a) to (h), the structure in which each layer is formed on the Si wafer 101 may be referred to as a "semiconductor substrate". In FIG. 1, the upper surface side of the Si wafer 101 is referred to as the first main surface, and the lower surface side is referred to as the second main surface.

[0020] In the first step not shown in FIG. 1(a), an oxide film is formed by thermally oxidizing the entire surface of the Si wafer 101 (n-drift layer of a first conductivity type). Next, a photolithography step is performed to form a region in which the anode p-type (second conductivity type) semiconductor layer 102 is to be provided. In this photolithography step, a resist material is applied to the surface of the Si wafer 101, exposed to light, and developed to form a resist having an opening in the anode p-type semiconductor layer 102 region. Then, p-type impurities are ion-implanted. An example of the p-type impurity is B (boron). Then, the resist is removed, and an annealing process is performed to activate the impurities, thereby forming the anode p-type semiconductor layer 102 as shown in FIG. 1(a).

[0021] 1(b), an oxide film is formed on a Si wafer 101 by thermal oxidation, an insulating oxide film 103 is deposited by a chemical vapor deposition (CVD) method, and a photolithography process is performed to form a contact portion connecting the anode p-type semiconductor layer 102 and the anode electrode. A resist material is applied, exposed, and developed, and the insulating oxide film 103 is etched using the formed resist as a mask, thereby forming a contact portion connecting the anode p-type semiconductor layer 102 and the anode electrode.

[0022] 1(c), an anode electrode made of aluminum (Al) or an Al alloy is formed by sputtering, and a resist is patterned by a photolithography process, followed by etching to form an anode electrode 104. In this manner, an anode p-type semiconductor layer 102 and an anode electrode 104 are formed on the first main surface side of the Si wafer 101.

[0023] 1(d), a surface protective film 105 is formed. The surface protective film 105 can be formed, for example, by applying a solution containing a polyimide precursor material and a photosensitive material, and exposing the termination region to light to convert the precursor into polyimide, thereby forming the surface protective film 105.

[0024] In Fig. 1(e), ions are irradiated from the second main surface side of the Si wafer 101 to form an ion implantation layer 106. Here, the ion irradiation position (depth from the second main surface of the Si wafer 101) determines the thickness of an n-type (first conductivity type) field stop layer (n buffer layer) described later, and since it is necessary to sufficiently prevent the depletion layer from reaching the depletion layer when the withstand voltage is maintained, the ion irradiation position is set according to the withstand voltage class of the semiconductor device. For example, for a diode with a withstand voltage of 1200V, a depth of about 100 µm from the second main surface is preferable, and for a diode with a withstand voltage of 3.3 kV, irradiation is preferably performed at a depth of about 400 µm.

[0025] The depth of ion irradiation can be adjusted by adjusting the irradiation energy or by using an absorber (not shown). For example, an aluminum member can be used as the absorber. In addition, the ion-irradiated surface of the Si wafer 101 may be pre-polished within a range (for example, 600 μm thick) where the wafer does not crack due to its own weight or does not warp excessively due to the large diameter, and then ion irradiation may be performed.

[0026] The ions are preferably light ions, preferably protons or helium, although non-light ions may also be used.

[0027] In FIG. 1(f), the ion-implanted layer 106 in FIG. 1(e) is annealed to convert the ion atoms irradiated and implanted into donors, forming an n-type field stop layer (n-buffer layer) 108. Conventionally, the annealing of the ion-implanted layer 106 requires 30 minutes to 5 hours at 300° C. to 500° C. in a heating furnace, and it has been difficult to sufficiently heat the wafer uniformly as the wafer diameter increases. In the present invention, in order to shorten the annealing time and heat the wafer uniformly, the annealing is performed in a single-wafer lamp annealing apparatus that processes the wafers one by one at 300° C. to 450° C. for 60 seconds or less in an N2 atmosphere, an H2 atmosphere, or an N2 / H2 mixed gas atmosphere to convert the ion-implanted layer into a donor.

[0028] FIG. 3 is a graph showing the distribution of n-type carrier concentration and hydrogen concentration in the cross section along line BB' in process (f) of FIG. 1, and shows the state of donorization in the cross section along line BB'. Protons (hydrogen) are injected as ions, and annealing is performed at 400°C in an H2 atmosphere. In FIG. 3, annealing times of 10 min or more (10 min: dashed line, 120 min: dashed line) are the results of heat treatment using a conventional batch-type vertical heat treatment device. As shown in FIG. 3, the gradient of n-type carrier concentration is steeper when heat treatment is performed using the lamp annealing of the present invention with an annealing time of 60 sec or less than when heat treatment is performed using a conventional heating furnace with an annealing time of 10 min or more.

[0029] FIG. 4 is a graph showing a recovery waveform, and FIG. 5 is a graph showing a leakage current waveform. In FIG. 4 and FIG. 5, the solid line indicates a semiconductor device manufactured by the manufacturing method according to the embodiment of the present invention shown in FIG. 1, and the dashed line indicates a semiconductor device manufactured by the manufacturing method of the comparative example. The comparative example is a case where a large amount of lifetime killers remain as crystal defect regions 109. In the process of forming the n-type field stop layer (n buffer layer) 108, in a region shallower than the peak concentration (the concentration at which the n-type carrier concentration is highest) in the ion implantation direction, the donor activation rate decreases, a large number of crystal defects occur, and a crystal defect region 109 in which a large amount of lifetime killers that shorten the carrier lifetime exist is generated. As shown by the dashed lines in FIG. 4 and FIG. 5, it was found that when a large amount of lifetime killers remain as crystal defect regions 109 as in the comparative example, there are problems such as deterioration of switching noise (FIG. 4) and increase in leakage current when the withstand voltage is maintained (FIG. 5). On the other hand, it can be seen that the semiconductor device manufactured by the manufacturing method according to the embodiment of the present invention shown by the solid lines in Figures 4 and 5 reduces the deterioration of switching noise (Figure 4) and also prevents an increase in leakage current when the withstand voltage is maintained (Figure 5).

[0030] Thereafter, although not shown, in order to reduce switching loss, ion implantation for individual lifetime control can be performed on the main surface side of the Si wafer 101 on which the anode p-type semiconductor layer 102 is formed, on the n-type field stop layer 108, or on both, separately from the formation of the n-type field stop layer 108.

[0031] 1(g), the crystal defect region 109 formed in the region shallower than the peak concentration is removed. For example, it can be removed by back grinding and a mixture of hydrofluoric acid and nitric acid.

[0032] 6 is a graph showing the relationship between the carrier lifetime and the n-type carrier concentration. Here, the final n-type field stop layer (n buffer layer, donor layer) 108 has a carrier concentration of 1×10 15 cm -3 It is desirable to form the GaN layer with a carrier concentration of 1×10 or less, as shown in FIG.15 cm -3 Above 1×10, the carrier lifetime becomes shorter as the carrier concentration increases. 15 cm -3 By setting it to the value below, it is possible to prevent the disappearance of excess carriers in the n-buffer layer during reverse recovery switching of the diode, and to ensure a tail current region, thereby making it possible to suppress the occurrence of ringing noise.

[0033] According to the inventor's study, the thickness of the n-type field stop layer 108 is preferably 10 μm or more. Fig. 7 is a graph showing the relationship between the leakage current defect rate and the depth of the n-type field stop layer. As shown in Fig. 7, if the depth is 7 μm or less, an increase in leakage current occurs when maintaining a withstand voltage due to scratches on the back surface occurring in the manufacturing process after the next step or in the inspection process. Also, since the processing accuracy of the back grinding and the mixed solution of hydrofluoric acid and nitric acid is approximately ±3 μm, it is preferable to set the depth to 10 μm or more in consideration of processing variations.

[0034] Therefore, as shown in Figures 2 and 3, it is necessary to remove crystal defect region 109 from the second main surface side and a portion of n-type field stop layer 108 (up to where the peak of n-type carrier concentration is removed) to a predetermined value so that there is no crystal defect region 109 and the carrier concentration (n-type carrier concentration) increases with a positive gradient from the n-drift layer (layer of Si wafer 101) toward the second main surface side.

[0035] 8 is a graph showing the relationship between the donor activation rate and temperature when annealing for 60 seconds. d and ion (proton) concentration n h Ratio to (n d / n h8 shows the annealing temperature dependency of the donor activation rate, which is the ratio of the activation rate of the donor to the activation rate of the semiconductor device. As shown in FIG. 8, the activation rate is 0.5% or more in the range of 300°C to 450°C, and the activation rate is 1% or more in the range of 350°C to 400°C, which is the highest activation rate and is stable. Therefore, the annealing temperature is preferably 300°C to 450°C, and more preferably 350°C to 400°C. By setting the annealing temperature to 300°C to 450°C, a stable n-type carrier concentration is obtained, and since the activation rate is high, the amount of ion implantation can be reduced, and a semiconductor device can be manufactured with small variations and at low manufacturing costs.

[0036] Fig. 9 is a graph showing the relationship between the donor activation rate and the annealing time when annealing at 300° C. As shown in Fig. 9, the activation rate is 0.5% or more when the annealing time is 70 seconds or less.

[0037] In view of the above, the annealing treatment is preferably carried out at a temperature in the range of 300° C. to 450° C. for 60 seconds or less, and for a time of 1 second or more.

[0038] In FIG. 1(h), n-type impurities are ion-implanted from the second main surface side of the semiconductor substrate. Examples of n-type impurities include phosphorus (P) and arsenic (As). After that, laser annealing is performed to activate the ion-implanted n-type impurities, and n + A type semiconductor layer 110 is formed. A cathode electrode 111 is formed by sputtering to have a laminated structure of, for example, AlSi alloy / titanium (Ti) / nickel (Ni) / gold (Au).

[0039] 2 is a schematic cross-sectional view of the semiconductor device after the step (h) in FIG. 1 is completed, and a graph showing the n-type carrier concentration and ion concentration. With the above-mentioned configuration, the carrier concentration of the n-type field stop layer (n buffer layer) 108 shown in FIG. 15 cm -3It is possible to manufacture a diode having an n-type field stop layer thickness of 10 μm or more, no crystal defect region 109, and in which the carrier concentration increases with a positive gradient from the n-drift layer (layer of Si wafer 101) toward the second main surface side.

[0040] According to the above-described method for manufacturing a semiconductor device of the present invention, the ions implanted into the n-type field-stop layer 108 are converted into donors by lamp annealing heat treatment, which makes it possible to uniformly heat the surface, particularly in large-diameter wafers.

[0041] According to the above-described method for manufacturing a semiconductor device of the present invention, it is possible to provide a semiconductor device which has a lower on-voltage, improved switching loss, suppresses high-frequency oscillation due to noise during switching, and reduces leakage current during voltage resistance maintenance, which is a cause of element destruction or degradation.

[0042] In addition to the process described in FIG. 1, a process may be added in which a semiconductor device is manufactured with a large-diameter wafer mounted on a substrate, and the substrate and the semiconductor device are separated after completion. In that case, this process can also serve as the process of removing part of the n-type field-stop layer 108 and the crystal defect region 109 described above, thereby simplifying the manufacturing process.

[0043] Fig. 10 is a circuit diagram showing a schematic configuration of a power conversion device of the present invention. A second embodiment in which a semiconductor device of the present invention is applied to a power conversion device will be described with reference to Fig. 10. Fig. 10 shows an example of a circuit configuration of a power conversion device 500 of this embodiment and a connection relationship between a DC power supply and a three-phase AC motor (AC load).

[0044] In the power conversion device 500 of the present embodiment, semiconductor devices manufactured by the above-described semiconductor device manufacturing method of the present invention are used as any or all of the power switching elements 501 to 506 and the diodes 521 to 526. The power switching elements 501 to 506 are, for example, IGBTs, and the elements 521 to 526 are diodes.

[0045] As shown in FIG. 10, a power conversion device 500 of the present embodiment includes a pair of DC terminals, a P terminal 531 and an N terminal 532, and AC terminals, a U terminal 533, a V terminal 534, and a W terminal 535, the number of which is the same as the number of phases of the AC output.

[0046] It also has a switching leg consisting of a pair of power switching elements 501 and 502 connected in series, with U-terminal 533 connected to the series connection point as its output. It also has a switching leg consisting of power switching elements 503 and 504 of the same configuration connected in series, with V-terminal 534 connected to the series connection point as its output. It also has a switching leg consisting of power switching elements 505 and 506 of the same configuration connected in series, with W-terminal 535 connected to the series connection point as its output.

[0047] Three-phase switching legs consisting of power switching elements 501-506 are connected between DC terminals of P terminal 531 and N terminal 532, and DC power is supplied from a DC power source (not shown). Three-phase AC terminals of power conversion device 500, namely U terminal 533, V terminal 534, and W terminal 535, are connected to a three-phase AC motor (not shown) as a three-phase AC power source.

[0048] A power switching element 501 and a diode 521 connected in anti-parallel to the power switching element 501 are connected to form a parallel circuit. Similarly, a power switching element 502 and a diode 522, a power switching element 503 and a diode 523, a power switching element 504 and a diode 524, a power switching element 505 and a diode 525, and a power switching element 506 and a diode 526 are connected to form a parallel circuit. A parallel circuit including the power switching element 501 and a parallel circuit including the power switching element 502 are connected in series. Similarly, a parallel circuit including the power switching element 503 and a parallel circuit including the power switching element 504 are connected in series, and a parallel circuit including the power switching element 505 and a parallel circuit including the power switching element 506 are connected in series.

[0049] Gate circuits 511-516 are connected to the input terminals of the gates of the power switching elements 501-506 each made of an IGBT, and the power switching elements 501-506 are controlled by the gate circuits 511-516, respectively. The gate circuits 511-516 are generally controlled by a general control circuit (not shown).

[0050] The gate circuits 511 - 516 comprehensively and appropriately control the power switching elements 501 - 506 , and the DC power of the DC power supply is converted into three-phase AC power and output from the U terminal 533 , the V terminal 534 , and the W terminal 535 .

[0051] By applying the above-mentioned manufacturing method of the semiconductor device of the present invention to the power conversion device 500, it is possible to provide a power conversion device that achieves low on-voltage, low switching loss, suppresses high-frequency oscillation due to noise during switching, and reduces leakage current when maintaining a withstand voltage, which is a cause of element destruction and degradation.

[0052] As described above, according to the present invention, in vertical semiconductor devices such as IGBTs and PIN diodes that can use large diameter (8 inches or more) wafers, it has been shown that it is possible to provide a manufacturing method for a semiconductor device that can improve the manufacturability of the field stop layer (n buffer layer), while reducing the on-voltage, reducing switching loss, suppressing high frequency oscillation due to noise during switching, and reducing leakage current when maintaining a breakdown voltage that is a cause of element destruction or degradation, a semiconductor device manufactured using the method, and a power conversion device using the same.

[0053] The present invention is not limited to the above-mentioned embodiment, but includes various modified examples. For example, the above-mentioned embodiment has been described in detail to easily explain the present invention, and is not necessarily limited to those including all of the configurations described. Also, it is possible to replace a part of the configuration of one embodiment with the configuration of another embodiment, and it is also possible to add the configuration of another embodiment to the configuration of one embodiment. Also, it is possible to add, delete, or replace a part of the configuration of each embodiment with another configuration.

[0054] For example, in this specification, the "first conductivity type" has been described as the "n type" and the "second conductivity type" as the "p type", but the "first conductivity type" may also be the "p type" and the "second conductivity type" may also be the "n type". [Explanation of symbols]

[0055] 101...Si wafer (n-drift layer), 102...p-type layer, 103...insulating oxide film, 104...anode electrode, 105...surface protection film, 106...light ion implantation layer, 108...n-type field stop layer (n buffer layer), 109...crystal defect region, 110...n + type semiconductor layer, 111...cathode electrode, 500...power conversion device, 501-506...power switching elements, 511-516...gate circuits, 521-526...diodes, 531...P terminal, 532...N terminal, 533...U terminal, 534...V terminal, 535...W terminal.

Claims

1. A method for manufacturing a semiconductor device having a semiconductor substrate, a second conductivity type layer formed on a first main surface of the semiconductor substrate, a first conductivity type drift layer formed on a second main surface of the semiconductor substrate opposite to the first main surface, and a first conductivity type field stop layer formed on a surface of the first conductivity type drift layer facing the second main surface and having an impurity concentration higher than that of the first conductivity type drift layer, the method comprising the steps of: forming the field stop layer by irradiating ions from the second main surface side to a predetermined depth; a step of converting the ions into donors by annealing the field-stop layer at 300° C. to 450° C. for 60 seconds or less after the ion irradiation; and reducing a thickness of the semiconductor substrate from the second main surface side to a predetermined value so as to remove crystal defects generated in the process of irradiating ions to form the field stop layer.

2. 2. The method for manufacturing a semiconductor device according to claim 1, wherein after the step of reducing a thickness of the semiconductor substrate to a predetermined value, a carrier concentration of the field-stop layer increases with a positive gradient from the first conductivity type drift layer toward the second main surface side.

3. 2. The method for manufacturing a semiconductor device according to claim 1, wherein the annealing treatment in the step of forming the field stop layer is performed for one second or more.

4. 2. The method of claim 1, wherein the carrier concentration of the field-stop layer after the step of reducing the thickness of the semiconductor substrate to a predetermined value is 1×10 15 cm -3 1. A method for manufacturing a semiconductor device, comprising:

5. 2. The method of claim 1, wherein the thickness of the field-stop layer after the step of reducing the thickness of the semiconductor substrate to a predetermined value is 10 [mu]m or more.

6. 2. The method for manufacturing a semiconductor device according to claim 1, wherein a donor activation rate, which is a ratio of carrier concentration to ion concentration in the field stop layer after the step of reducing the thickness of the semiconductor substrate to a predetermined value, is 0.5% or more.

7. 2. The method of claim 1, wherein the semiconductor substrate has a size of 8 inches or more.

8. A method for manufacturing a semiconductor device, as claimed in claim 1, characterized in that the process of reducing the thickness of the semiconductor substrate from the second main surface side to a predetermined value comprises reducing the thickness of the semiconductor substrate until the field stop layer is exposed.

9. A semiconductor device manufactured using the method according to any one of claims 1 to 8.

10. A semiconductor module using the semiconductor device according to claim 9.

11. A pair of DC terminals; The same number of AC terminals as the number of AC output phases, a switching leg having the same number as the number of phases of the AC output, the switching leg being connected between the pair of DC terminals and having two parallel circuits connected in series, the parallel circuits being each formed of a switching element and a diode connected in anti-parallel to the switching element; A gate circuit for controlling the switching element, 9. A power conversion device, wherein at least one of the switching element and the diode is a semiconductor device manufactured by the method for manufacturing a semiconductor device according to claim 1.

Citation Information

Patent Citations

  • Method for injecting hydrogen into the buffer region of a punch-through non-epitaxial IGBT.

    JP2003533047A

  • Semiconductor module, and method of controlling the same

    JP2011086891A

  • Semiconductor device

    JP2013138172A

  • Diode and method of manufacturing the same

    JP2014146721A

  • Semiconductor device and method of manufacturing the same, and power conversion system

    JP2018056220A