Low melting point porous ceramic material and its manufacturing method
A low melting point porous ceramic material with improved mechanical properties and simplified manufacturing process is achieved by using a specific composition and firing method, addressing the limitations of existing ceramics.
Patent Information
- Application Number
- JP2023535015
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-28
- Filing Date
- 2021-06-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-06-16
AI Technical Summary
Existing porous ceramics face challenges such as high manufacturing costs, complex processes, high calcination temperatures, low mechanical strength, poor earthquake resistance, and difficulty in forming ideal pores, limiting their applications.
A low melting point porous ceramic material composed of specific raw materials (borosilicate glass, purple sand, quartz, Na2O, ZrO2, and Li2O) is produced through a method involving mixing, vitrification, wet pulverization, and firing at 680-830°C, eliminating the need for a pore-forming agent.
The method results in a ceramic material with improved mechanical strength, porosity, and simplified sintering process, maintaining excellent compressive and flexural strength, and hardness, suitable for industrial applications.
Smart Images

Figure 0007590035000002 
Figure 0007590035000003 
Figure 0007590035000001
Abstract
Description
[Technical field]
[0001] The present invention relates to the technical field of ceramic materials, and in particular to a low melting point porous ceramic material and a method for producing the same. [Background technology]
[0002] Porous ceramics have a large specific surface area, and the properties of energy absorption, damping, etc., and specially processed porous ceramics have selective permeability to liquids, gases, and other substances, so they are widely used in various fields such as automotive environments, chemical industry, machinery, and biomedicine. Currently, commercialized porous ceramics are mainly made of Al2O3, SiC, ZrO2, and mullite as their main raw materials, but these materials have complex manufacturing processes, high firing temperatures, high energy consumption, high costs, or problems such as inconsistency between the pore-forming agent and the refractory degree of the matrix make it difficult to form holes. Conventional porous ceramic products have problems such as low mechanical strength, poor earthquake resistance and vibration damping, and difficulty in forming ideal through holes, which significantly restricts the popularization and application of porous ceramics. Therefore, finding a suitable raw material that can effectively reduce the sintering temperature and improve the porosity and specific surface area of porous ceramics will contribute positively to the wide range of applications of porous ceramics. Summary of the Invention [Problem to be solved by the invention]
[0003] An object of the present invention is to solve the above-mentioned drawbacks of the prior art and to provide a porous ceramic material having a low melting point.
[0004] Another object of the present invention is to provide a method for producing the above-mentioned low melting point porous ceramic material. [Means for solving the problem]
[0005] A low melting point porous ceramic material, The firing temperature is 680 to 830°C, and the porosity is 24 to 42%, A low melting point porous ceramic material, characterized in that the raw material consists of a binder and a raw material powder obtained by mixing the raw material components in the mass percentages listed below, followed by vitrification treatment, wet grinding, drying and sieving. Borosilicate Glass Sand 27.5~50% Purple sand powder 15~20% Quartz powder 20~50% Na2O powder 6~12% ZrO2 powder 1~2% Li2O powder 0.5~1.5%
[0006] In a preferred embodiment of the invention, the binder is dextrin.
[0007] In a preferred embodiment of the present invention, the borosilicate glass sand and Na2O powder are capable of passing through a 2000 mesh screen.
[0008] In a preferred embodiment of the present invention, the ultraviolet abrasive powder, quartz powder, and Li 2 O The powder can pass through a 1000 mesh screen.
[0009] In a preferred embodiment, the mass ratio of the raw material powder to the temporary binder is 80-90:10-20.
[0010] More preferably, the mass ratio of the raw material powder to the temporary binder is 85:15.
[0011] In a preferred embodiment of the present invention, the raw material powder is capable of passing through a 5000 mesh sieve.
[0012] A method for producing the low melting point porous ceramic material, comprising the steps of: (1) weighing based on the mass percentage to obtain raw material powder of each component; (2) Borosilicate GlassThe sand and Na2O powder are mixed uniformly, and then the first mixture is obtained through dry grinding and granulation in sequence; (3) uniformly mixing the purple sand powder, the quartz powder, the Li2O powder and the ZrO2 powder, and then sequentially dry grinding and sieving to obtain a second mixture; (4) homogeneously mixing the first mixture and the second mixture, and then sequentially subjecting the mixture to a vitrification treatment, wet grinding, drying and sieving to obtain the raw material powder; (5) uniformly mixing the raw material powder with a binder and then granulating the mixture to obtain a mixed raw material; (6) Press-molding the mixed raw material into a desired shape and thoroughly drying it to obtain a green body; (7) The method includes a step of raising the temperature of the base material to the firing temperature and firing the base material while maintaining the temperature.
[0013] In a preferred embodiment, the vitrification temperature is 800 to 900°C.
[0014] In a preferred embodiment of the present invention, the temperature increase rate in step (7) is 4 to 6° C. / min, and the firing holding time is 1.5 to 2.5 hours. Effect of the Invention
[0015] Due to the synergistic effect of each raw material component in the present invention, the product obtained has the advantages of a simple sintering process, good mechanical strength, and the ability to form pores without a pore former, effectively solving problems such as inconsistency in the refractoriness of the binder and the pore former, reduced heat dissipation ability, and reduced gas permeability, and can improve the life and gripping force of the porous ceramic material. Under the condition that the firing temperature is only 680-780°C and no pore former is added, the porosity is a maximum of 42%, and excellent compressive strength, flexural strength, and hardness can be maintained. [Brief description of the drawings]
[0016] [Figure 1] 1 is an electron microscope photograph of a porous structure after firing of a low-melting-point porous ceramic material according to Example 1 of the present invention. [Diagram 2] 1 is an electron microscope photograph of a porous structure after firing of a low-melting-point porous ceramic material in Comparative Example 6 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. <Examples 1 to 6> (1) The raw material components constituting the raw material powder are weighed out by mass percentage. (2) Borosilicate Glass The sand and Na2O powder are mixed uniformly, then dry-ground and passed through a 2000 mesh sieve to obtain a first mixture. (3) The purple sand powder, the quartz powder, the ZrO2 powder and the Li2O powder are uniformly mixed, and then dry-ground in sequence and passed through a 1000 mesh sieve to obtain a second mixture. (4) The first and second mixtures are mixed uniformly, and then sequentially subjected to a vitrification treatment at 800° C., wet pulverization, drying, and sieving through a 5000 mesh sieve to obtain the raw material powder. (5) The raw material powder and dextrin are uniformly mixed in a mass ratio of 85:15, and then granulated to obtain a mixed raw material. (6) The mixed raw material is press-molded into a desired shape and thoroughly dried for 24 hours to obtain a green body. (7) The temperature of the above-mentioned body was raised to the firing temperature at a rate of 5°C / min and then held at that temperature for 2 hours for firing. The blending ratios of the raw material components, the firing temperatures, and the technical effects obtained in Examples 1 to 6 are shown in Table 1, and the porous structure after firing of the low-melting-point porous ceramic material obtained in Example 1 is shown in FIG.
[0018] <Comparative Examples 1 to 5> The specific preparation procedures were the same as those in Examples 1 to 6, and the compounding ratios of the raw material components, the firing temperatures, and the technical effects obtained are shown in Table 1. JPEG0007590035000001.jpg73170
[0019] As can be seen from Table 1, when the amount of purple sand powder added is less than 15%, the pores of the porous ceramics change from open pores to closed pores, the porosity of the porous ceramics drops sharply, and the advantages of the porous ceramics cannot be realized. On the other hand, when the amount of purple sand powder added exceeds 20%, the overlap of the pores of the porous ceramics increases sharply, the porosity of the porous ceramics increases sharply, and the mechanical properties of the ceramics drop sharply. Such sintered products have low strength, a significantly reduced range of use, and a sharp reduction in service life.
[0020] Borosilicate Glass If the amount of sand added is less than 20%, the sintering temperature of the porous ceramic will be as high as 1100°C, and if the sintering temperature is too high, its range of application (e.g., ceramic grinding wheels, etc.) will be narrowed and the morphology of the abrasive grains will be destroyed (see Sha X, Yue W, Zhang H, et al. Thermal stability of polycrystalline diamond compact sintered with boron-coated diamond particles [J]. Diamond and Related Materials. 2020, 104: 107753). On the other hand, Borosilicate Glass If the sand content is less than 55%, the firing temperature still requires 680°C. Borosilicate Glass The firing temperature does not decrease with the increase in the content. The temporary binder used in the vitrified bond obtained in the present invention is dextrin, but temporary binders such as commercially available water glass react with the vitrified bond during compounding, or generate pores after sintering, destroying the self-adhesive pores of the purple sand itself and densifying the vitrified bond.
[0021] <Comparative Example 6> The raw material powder of Example 1 and water glass (water and water glass in a ratio of 13.6:1, instead of dextrin as a binder) solution are mixed uniformly in a mass ratio of 85:15, and then granulated to obtain a mixed raw material. The mixed raw material is pressed into a desired shape and thoroughly dried for 24 hours to obtain a green body, which is heated to 750°C at a rate of 5°C / min and sintered at high temperature for 2 hours to obtain the porous structure shown in Figure 2. Compared with Example 1, the porous structure of the ceramic body obtained in the comparative example is denser, and the advantage of the natural porous structure of purple sand is lost, and its mechanical performance is improved, with a compressive strength of 55.4MPa, a flexural strength of 50.25MPa, and a hardness of 40HRB.
[0022] The above description is merely a preferred embodiment of the present invention, and therefore the scope of the present invention cannot be limited thereby; that is, any equivalent changes and modifications based on the claims and the contents of the specification of the present invention fall within the comprehensive scope of the present invention. [Industrial Applicability]
[0023] The present invention discloses a low melting point porous ceramic material having a firing temperature of 680-830°C and a porosity of 24-42%, the raw materials of which are a temporary binder and raw material powder, and a method for producing the same. Due to the synergistic effect of each raw material component in the present invention, the obtained product has the advantages of a simple sintering process, good mechanical strength, and the ability to generate pores without a pore-forming agent, and can effectively solve problems such as inconsistency in the refractoriness of the binder and the pore-forming agent, reduced heat dissipation ability, and reduced gas permeability, and can improve the life and gripping force of the porous ceramic material. Under conditions where the firing temperature is only 680-780°C and no pore-forming agent is added, the porosity is a maximum of 42%, and excellent compressive strength, flexural strength, and hardness are maintained, making the product industrially applicable.
Claims
1. A low melting point porous ceramic material, The porosity is 24 to 42%; A low melting point porous ceramic material comprising a binder and the following raw material components in the following mass percentages: Borosilicate glass sand 27.5-50% Purple sand powder 15-20% Quartz powder 20-50% Na 2 O powder 6-12% ZrO 2 Powder 1-2% Li 2 O powder 0.5~1.5%
2. 2. The low melting point porous ceramic material according to claim 1, wherein the binder is dextrin.
3. The borosilicate glass sand and Na 2 2. The low melting point porous ceramic material according to claim 1, characterized in that the O powder can pass through a 2000 mesh sieve.
4. The purple sand powder, quartz powder and Li 2 2. The low melting point porous ceramic material according to claim 1, wherein the O powder can pass through a 1000 mesh sieve.
5. A low melting point porous ceramic material as described in any one of claims 1 to 4, characterized in that the mass ratio of the raw material components to the binder is 80-90:10-20.
6. 6. The low melting point porous ceramic material according to claim 5, wherein a mass ratio of said raw material components to said binder is 85:
15.
7. 5. The low melting point porous ceramic material according to claim 1, wherein the raw material powder of the raw material component is capable of passing through a 5000 mesh sieve.
8. A method for producing a low melting point porous ceramic material according to any one of claims 1 to 7, (1) weighing the raw material components based on the mass percentages to obtain raw material powders of the raw material components; (2) Borosilicate glass sand and Na 2 and O powder are mixed uniformly, and then the mixture is subjected to dry grinding and grinding in order to obtain a first mixture. (3) Zisha powder, quartz powder and Li 2 O powder and ZrO 2 and then, through dry grinding and sieving in order, obtaining a second mixture. (4) uniformly mixing the first mixture and the second mixture, and then sequentially subjecting the mixture to a vitrification treatment, wet grinding, drying and sieving to obtain the raw material powder; (5) uniformly mixing the raw material powder with a binder and then granulating the mixture to obtain a mixed raw material; (6) Press-molding the mixed raw material into a desired shape and thoroughly drying it to obtain a green body; (7) A method for producing a low melting point porous ceramic material, comprising the steps of heating the base material to a firing temperature and firing the base material at a temperature maintained at that temperature, wherein the firing temperature is 680 to 830°C.
9. The method according to claim 8, wherein the vitrification treatment is carried out at a temperature of 800 to 900°C.
10. 9. The method according to claim 8, wherein the heating rate in step (7) is 4 to 6° C. / min, and the holding and baking time is 1.5 to 2.5 hours.
Citation Information
Patent Citations
Industrial purple sand product materials and manufacturing method
CN102030513A
Microcrystal bamboo charcoal purple sand composite pottery material and application thereof
CN103467066A
Low temperature sinterable domestic ceramic
CN105906311A
Red stoneware mineral aggregate lightweight porous ceramsite and preparation method thereof
CN106866175A
Dehua white porcelain and purple sand combined ceramic product and preparation process thereof
CN106938911A