Electrolyte additive for secondary battery, non-aqueous electrolyte for lithium secondary battery containing the same, and lithium secondary battery containing the same
A non-aqueous electrolyte with imidazole and pyridine groups forms a stable SEI, addressing the decomposition issues in lithium secondary batteries, enhancing high-temperature stability and performance.
Patent Information
- Application Number
- JP2023545246
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-08-17
- Filing Date
- 2022-08-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-08-25
AI Technical Summary
Lithium secondary batteries face issues with decomposition of lithium salts at high temperatures, leading to the deterioration of the solid electrolyte interfacial film (SEI), increased resistance, gas generation, and volume expansion, which affect their performance and lifespan.
Incorporation of a non-aqueous electrolyte containing imidazole and pyridine groups, particularly a compound represented by chemical formula 1, to form a stable SEI on the negative electrode, which suppresses decomposition products like HF and PF5, reducing resistance and gas generation, and maintaining battery performance at high temperatures.
The electrolyte additive enhances high-temperature stability, reduces resistance, and prevents volume expansion, thereby improving the battery's lifespan and performance under harsh conditions.
Smart Images

Figure 0007590038000001 
Figure 0007590038000002 
Figure 0007590038000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrolyte additive for secondary batteries. More specifically, the present invention relates to a non-aqueous electrolyte additive that is excellent in the effect of removing decomposition products generated from lithium salts, and a non-aqueous electrolyte for lithium secondary batteries containing the same. The present invention relates to a non-aqueous electrolyte additive that can form a strong solid electrolyte interface film (SEI) on the surface of a negative electrode, and a non-aqueous electrolyte for lithium secondary batteries containing the same. The present invention also relates to a lithium secondary battery containing such a non-aqueous electrolyte. The lithium secondary battery of the present invention includes the non-aqueous electrolyte, and thereby the high-temperature performance of the lithium secondary battery is improved. [Background technology]
[0002] Lithium secondary batteries are not only used as portable power sources for mobile phones, laptops, etc., but are also being expanded to medium and large power sources for electric bicycles, electric vehicles (EVs), etc. As the range of applications expands, there is a demand for lithium secondary batteries that can maintain excellent performance not only at room temperature but also in harsher external environments such as high and low temperature environments.
[0003] Currently widely used lithium secondary batteries are generally composed of a carbon-based negative electrode capable of inserting and extracting lithium ions, a transition metal oxide-based positive electrode containing lithium, a non-aqueous electrolyte in which lithium salt is dissolved in a mixed carbonate organic solvent, and a separator that prevents contact between the positive and negative electrodes. When charging a lithium secondary battery, lithium atoms at the positive electrode are ionized into lithium ions and electrons, the electrons move to the negative electrode through an external circuit, and the lithium ions move to the negative electrode through the non-aqueous electrolyte and separator and are inserted (intercalated) into the carbon negative electrode. When discharging, the electrons move to the positive electrode through an external circuit, and at the same time, the lithium ions are deintercalated (deintercalated) from the carbon negative electrode and move to the positive electrode through the non-aqueous electrolyte and separator, where the lithium ions and electrons meet at the positive electrode to become lithium atoms in a stable state. A lithium secondary battery generates electric energy by repeating such charging and discharging.
[0004] In lithium secondary batteries, the positive electrode active material may structurally collapse during charging and discharging, causing metal ions to leach out from the positive electrode surface. Metal ions leach out from the positive electrode may be electrodeposited on the negative electrode, causing the negative electrode to deteriorate. This deterioration of the negative electrode tends to be accelerated when the potential of the positive electrode is high or when the secondary battery is exposed to high temperatures.
[0005] To solve these problems, a method has been proposed in which a compound capable of forming a film (solid electrolyte interphase film, SEI (Solid Electrolyte Interphase)) on the surface of the negative electrode is added to the non-aqueous electrolyte. However, such electrolyte additives cause other side effects such as a decrease in the life performance of the secondary battery and a deterioration in high-temperature safety, and also cause other problems such as a decrease in various performances of the lithium secondary battery.
[0006] LiPF6 is mainly used as the lithium salt in lithium secondary batteries to achieve suitable characteristics of the secondary battery. - Anions are very vulnerable to heat, and it is known that when a secondary battery is exposed to high temperatures, they thermally decompose to generate Lewis acids such as PF5. The PF5 generated in this way not only causes the decomposition reaction of organic solvents such as ethylene carbonate, but also generates hydrofluoric acid (HF) and accelerates the dissolution of transition metals from the positive electrode active material. The dissolve-out transition metals can be electrodeposited on the positive electrode, causing an increase in the resistance of the positive electrode, or electrodeposited on the negative electrode, causing self-discharge of the negative electrode, or destroying the solid electrolyte interfacial film (SEI) on the negative electrode, causing further decomposition of the electrolyte, and thus an increase in the resistance and deterioration of the life of the secondary battery. Such decomposition reactions of the electrolyte also lead to gas generation inside the secondary battery.
[0007] Therefore, when a lithium secondary battery is stored at high temperatures in a fully charged state, there is a problem that the solid electrolyte interfacial film (SEI) gradually breaks down over time. This breakdown of the solid electrolyte interfacial film exposes the surface of the negative electrode. The exposed surface of the negative electrode reacts with the carbonate-based solvent in the electrolyte and decomposes, causing continuous side reactions. These side reactions continuously generate gas.
[0008] Regardless of the type of gas produced in this way, it increases the internal pressure of the lithium secondary battery, acts as a resistive element to lithium movement, expands the volume (thickness) of the secondary battery, creates major problems in reducing the weight of the secondary battery, and deteriorates the performance of the secondary battery.
[0009] In recent years, as the application fields of lithium secondary batteries expand, there is a steady demand for stability and long life characteristics in high-temperature environments. This performance is greatly influenced by the solid electrolyte interfacial film (SEI film) formed by the initial reaction between the electrode and the electrolyte. Summary of the Invention [Problem to be solved by the invention]
[0010] Therefore, in order to improve the high-temperature cycle characteristics and low-temperature output of lithium secondary batteries, there is a constant demand for the development of additives that can suppress side reactions between the positive electrode and the electrolyte and form a strong solid electrolyte interface film (SEI film) on the surface of the negative electrode.
[0011] In order to solve the above problems, the present invention provides a non-aqueous electrolyte for a lithium secondary battery, which contains an additive capable of forming a stable solid electrolyte interface film (SEI) on an electrode surface, particularly on the surface of a negative electrode.
[0012] In addition, in order to solve the above problems, the present invention provides an electrolyte additive for secondary batteries that is effective in forming a strong solid electrolyte interface film (SEI) on the surface of an electrode, particularly on the surface of a negative electrode, and in removing decomposition products generated from lithium salts.
[0013] In addition, in order to solve the above-mentioned problems of the conventional art, the present invention provides a non-aqueous electrolyte for a lithium secondary battery that can improve the high-temperature stability without deteriorating the high-temperature life and performance of the lithium secondary battery, and a lithium secondary battery including the non-aqueous electrolyte for the lithium secondary battery. [Means for solving the problem]
[0014] The nonaqueous electrolyte for a lithium secondary battery according to one embodiment of the present invention is
[0015] Compounds containing imidazole and pyridine groups as additives;
[0016] Lithium salts;
[0017] Additional additives; and
[0018] Contains a non-aqueous organic solvent.
[0019] The nonaqueous electrolyte for a lithium secondary battery according to one embodiment of the present invention is
[0020] A compound containing an imidazole group and a pyridine group represented by the following chemical formula 1 as an additive;
[0021] Lithium salts;
[0022] Additional additives; and
[0023] Contains a non-aqueous organic solvent.
[0024] [C1] JPEG0007590038000001.jpg2457
[0025] In one embodiment of the present invention, there is provided a lithium secondary battery including the nonaqueous electrolyte for a lithium secondary battery of the present invention, a positive electrode, a negative electrode, and a separator.
[0026] The negative electrode may include a carbon-based negative electrode active material and a silicon-based negative electrode active material.
[0027] The negative electrode may include a carbon-based negative electrode active material and a silicon-based negative electrode active material in a weight ratio of 97:3 to 50:50.
[0028] The negative electrode may include a carbon-based negative electrode active material and a silicon-based negative electrode active material in a weight ratio of 90:10 to 60:40. Effect of the Invention
[0029] The compound containing an imidazole group and a pyridine group, particularly the compound represented by Chemical Formula 1, which is provided as an additive to the non-aqueous electrolyte of the present invention, can remove Lewis acids such as HF and PF5, which are decomposition products generated by decomposition of anions when a secondary battery is exposed to high temperatures, from the inside of the electrolyte, since the nitrogen atom of the imidazole group acts as a Lewis base. Therefore, the compound containing an imidazole group and a pyridine group, particularly the compound represented by Chemical Formula 1, which is provided as an additive to the non-aqueous electrolyte of the present invention, can suppress deterioration of the surface film (SEI) of the positive or negative electrode caused by Lewis acid, prevent further electrolyte decomposition of the secondary battery due to destruction of the film (SEI), and can also suppress self-discharge of the secondary battery. The imidazole group also helps to form a stable film (SEI) on the surface of the negative electrode.
[0030] The additive contained in the nonaqueous electrolyte solution for a secondary battery of the present invention, i.e., the compound containing an imidazole group and a pyridine group, particularly the functional group of the compound represented by Chemical Formula 1, has the effects described above, and can realize a secondary battery with improved performance of reducing the volume expansion of the secondary battery by suppressing the increase in resistance and gas generation during storage at high temperatures without deteriorating the lifespan of the lithium secondary battery even when the battery is exposed to high temperatures, and by suppressing the increase in resistance and gas generation during storage at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The present invention will be described in more detail below with reference to examples. These examples are merely for the purpose of illustrating the present invention, and should not be construed as limiting the scope of the present invention.
[0032] As used herein, terms such as "comprise" and "have" should be understood as open-ended terms that include the possibility of including other components, unless otherwise specifically stated in the phrase or sentence in which the expression is contained.
[0033] In this specification, "%" means % by weight, unless expressly indicated otherwise.
[0034] The electrolyte additive for lithium secondary batteries, the nonaqueous electrolyte for lithium secondary batteries, and the lithium secondary battery containing the nonaqueous electrolyte of the present invention will be specifically described below.
[0035] <Electrolyte additives for lithium secondary batteries>
[0036] The present invention provides a compound containing an imidazole group and a pyridine group, particularly a compound containing an imidazole group and a pyridine group represented by the following Chemical Formula 1, as an additive for an electrolyte for a lithium secondary battery.
[0037] [C1]
[0038] JPEG0007590038000002.jpg2457
[0039] <Electrolyte for lithium secondary batteries>
[0040] The present invention
[0041] Compounds containing imidazole and pyridine groups;
[0042] Additional additives;
[0043] Lithium salts; and
[0044] An electrolyte solution for a lithium secondary battery is provided, which contains a non-aqueous organic solvent.
[0045] The present invention
[0046] A compound containing an imidazole group and a pyridine group, represented by the above chemical formula 1;
[0047] Additional additives;
[0048] Lithium salts; and
[0049] An electrolyte solution for a lithium secondary battery is provided, which contains a non-aqueous organic solvent.
[0050] The compound containing an imidazole group and a pyridine group may be included in an amount of 0.05 to 20 wt % based on the total weight of the electrolyte for a lithium secondary battery.
[0051] The compound containing an imidazole group and a pyridine group may be included in an amount of 0.05 to 10 wt % based on the total weight of the electrolyte for a lithium secondary battery.
[0052] The compound containing an imidazole group and a pyridine group may be contained in an amount of 0.05 to 5 wt %, 0.05 to 3 wt %, or 0.05 to 2 wt % based on the total weight of the electrolyte for a lithium secondary battery.
[0053] The compound containing an imidazole group and a pyridine group may be included in an amount of 0.1 to 20 wt % based on the total weight of the electrolyte for a lithium secondary battery.
[0054] The compound containing an imidazole group and a pyridine group may be preferably included in an amount of 0.1 to 10 wt % based on the total weight of the electrolyte for a lithium secondary battery.
[0055] The compound containing an imidazole group and a pyridine group may be contained in an amount of 0.1 to 5 wt %, 0.1 to 3 wt %, or 0.1 to 2 wt % based on the total weight of the electrolyte for a lithium secondary battery.
[0056] When the compound containing an imidazole group and a pyridine group is contained in an amount of less than 0.05 wt % based on the total weight of the electrolyte for a lithium secondary battery, the effect of preventing volume expansion of the lithium secondary battery and the effect of reducing the internal resistance are insufficient. Conversely, when the compound containing an imidazole group and a pyridine group is contained in an amount of more than 20 wt % based on the total weight of the electrolyte for a lithium secondary battery, the internal resistance of the secondary battery increases and the capacity decreases, resulting in problems of a decrease in high-temperature life characteristics and a decrease in high-temperature storage characteristics.
[0057] The electrolyte for lithium secondary batteries may further include at least one additional additive selected from the group consisting of halogen-substituted or unsubstituted carbonate-based compounds, nitrile-based compounds, borate-based compounds, lithium salt-based compounds, phosphate-based compounds, sulfite-based compounds, sulfone-based compounds, sulfate-based compounds, and sultone-based compounds.
[0058] Representative examples of the additional additives include lithium difluorophosphate, lithium tetrafluoro(oxalate)phosphate, lithium bis(fluorosulfonyl)imide, 1,3-propane sultone, 1,3-propene sultone, fluoroethylene carbonate, vinylene carbonate, and vinyl ethylene carbonate.
[0059] The additional additive may be included in an amount of 0.05 to 20 wt % based on the total weight of the electrolyte for a lithium secondary battery.
[0060] The additional additive may be preferably included in an amount of 0.05 to 10 wt % based on the total weight of the electrolyte for lithium secondary batteries.
[0061] The additional additive may be contained in an amount of 0.05 to 5 wt %, more preferably 0.05 to 3 wt %, based on the total weight of the electrolyte for lithium secondary batteries.
[0062] When the additional additive is contained in an amount of less than 0.05 wt % based on the total weight of the electrolyte for lithium secondary batteries, the effect of forming a film on the electrode may be small and the effect of suppressing side reactions between the electrode and the electrolyte may be reduced. When the electrolyte additive is contained in an amount of more than 20 wt % based on the total weight of the electrolyte for lithium secondary batteries, a film that is too thick may be formed on the electrode surface, increasing interfacial resistance and causing a decrease in capacity.
[0063] The lithium salt may include at least one selected from the group consisting of LiPF6, LiClO4, LiAsF6, LiBF4, LiBF6, LiSbF6, LiAlO4, LiAlCl4, LiClO4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, and LiB(C2O4)2.
[0064] The lithium salt preferably has a large degree of lattice energy dissociation, excellent ion conductivity, thermal stability, and excellent oxidation resistance, and functions as a path for lithium ions to move within the secondary battery, enabling the basic operation of the lithium secondary battery.
[0065] The lithium salt may be contained at a concentration of 0.1 to 2.5 M (mol / L) based on the total amount of the electrolyte for the lithium secondary battery.
[0066] The concentration of the lithium salt may be preferably 0.3 to 2.5 M (mol / L) based on the total amount of the electrolyte for the lithium secondary battery, taking into consideration properties related to electrical conductivity and viscosity related to the mobility of lithium ions.
[0067] The concentration of the lithium salt may be more preferably 0.7 to 1.6 M (mol / L) in consideration of properties related to electrical conductivity and viscosity related to the mobility of lithium ions.
[0068] If the concentration of the lithium salt is less than 0.1M, the electrical conductivity of the electrolyte for lithium secondary batteries is reduced, and the performance of the non-aqueous electrolyte for transferring ions at high speed between the positive and negative electrodes of the lithium secondary batteries is reduced. If the concentration of the lithium salt exceeds 2.5M, the viscosity of the electrolyte for lithium secondary batteries is increased, and the mobility of lithium ions is reduced, resulting in a problem of a reduction in secondary battery performance at low temperatures.
[0069] The non-aqueous organic solvent may be a linear carbonate solvent, a cyclic carbonate solvent, or a mixture thereof.
[0070] The linear carbonate solvent may include at least one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (EMC), and methyl propyl carbonate (MPC).
[0071] The cyclic carbonate solvent may include at least one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate (BC), vinylene carbonate (VC) and fluoroethylene carbonate (FEC).
[0072] It may be desirable to mix and use a cyclic, high-dielectric carbonate-based organic solvent having high ionic conductivity that can improve the charge / discharge performance of a secondary battery with a linear, low-viscosity carbonate-based organic solvent that can appropriately adjust the viscosity of the high-dielectric carbonate-based organic solvent.
[0073] Specifically, a high dielectric constant carbonate organic solvent selected from the group consisting of cyclic carbonate solvents such as ethylene carbonate (EC), propylene carbonate (PC), and mixtures thereof, can be mixed with a low viscosity carbonate organic solvent selected from the group consisting of linear carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and mixtures thereof, and used.
[0074] The cyclic carbonate solvent has high polarity and can dissociate lithium ions sufficiently, but has the disadvantage of high viscosity and low ionic conductivity. Therefore, the characteristics of the lithium secondary battery can be optimized by mixing the cyclic carbonate solvent with a linear carbonate solvent, which has low polarity but low viscosity.
[0075] Therefore, it may be preferable to use a mixture of at least one solvent selected from the cyclic carbonate solvents and at least one solvent selected from the linear carbonate solvents as the non-aqueous organic solvent.
[0076] The mixed solvent of the linear carbonate solvent and the cyclic carbonate solvent can be used by mixing the linear carbonate solvent and the cyclic carbonate solvent in a volume ratio of 9:1 to 1:9.
[0077] From the viewpoint of the life characteristics and storage characteristics of the secondary battery, it may be more preferable to use a mixed solvent of the linear carbonate solvent and the cyclic carbonate solvent in a volume ratio of 2:8 to 8:2.
[0078] The non-aqueous organic solvent can include ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC).
[0079] The non-aqueous organic solvent may include 5 to 40% by weight of the ethylene carbonate (EC), 5 to 20% by weight of the propylene carbonate (PC), 10 to 70% by weight of the ethyl methyl carbonate (EMC), and 10 to 60% by weight of the diethyl carbonate (DEC).
[0080] Specifically, in the cyclic carbonate solvent, ethylene carbonate (EC) or propylene carbonate (PC) having a high dielectric constant can be used. When artificial graphite is used as the negative electrode active material, it is preferable to use the ethylene carbonate (EC). In the linear carbonate solvent, it is preferable to use dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), or diethyl carbonate (DEC) having a low viscosity.
[0081] The non-aqueous organic solvent may be included in an amount of 5% to 80% based on the total amount of the electrolyte for the lithium secondary battery.The non-aqueous organic solvent may be included in an amount of 5% to 70% based on the total amount of the electrolyte for the lithium secondary battery.
[0082] <Lithium secondary battery>
[0083] The lithium secondary battery containing the non-aqueous electrolyte has excellent properties such as no deterioration in life characteristics at high temperatures, no increase in resistance during storage at high temperatures, and suppression of expansion of the secondary battery volume (thickness).
[0084] The lithium secondary battery of the present invention will now be described in detail.
[0085] The lithium secondary battery of the present invention is
[0086] positive electrode;
[0087] negative electrode;
[0088] Separation membrane; and
[0089] Contains a non-aqueous electrolyte.
[0090] The positive electrode is LiCoO2, LiFePO4, LiMnO2, LiMn2O4, LiNiO 2, Or LiNi 1-x-y Co x M y The positive electrode active material may include at least one selected from the group consisting of lithium metal oxides such as O2 (0≦x≦1, 0≦y≦1, 0≦x+y≦1, M is Al, Sr, Mg, Mn, or La).
[0091] The negative electrode can include at least one negative electrode active material selected from the group consisting of silicon, silicon compounds, tin, tin compounds, lithium titanate, crystalline carbon, amorphous carbon, artificial graphite, natural graphite, and a mixture of artificial graphite and natural graphite.
[0092] The separation membrane may be composed of a porous polymer film made of at least one polyolefin polymer selected from an ethylene polymer, a propylene polymer, an ethylene / butene copolymer, and an ethylene / hexene copolymer, or may be composed of a laminate thereof. The separation membrane may include a coating membrane coated with a ceramic or polymer material.
[0093] The non-aqueous electrolyte solution includes a compound containing an imidazole group and a pyridine group, in particular, a compound containing an imidazole group and a pyridine group represented by the following formula 1:
[0094] Additional additives;
[0095] Lithium salts; and
[0096] A non-aqueous organic solvent may be included.
[0097] [C1]
[0098] JPEG0007590038000003.jpg2457
[0099] Examples of the lithium secondary battery include, but are not limited to, a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery.
[0100] More specifically, the positive electrode active material is preferably a composite metal oxide of lithium and one or more materials selected from cobalt, manganese, and nickel. The composite metal oxide may have various solid solubility rates between cobalt, manganese, and nickel metals, and may further contain elements selected from the group consisting of Mg, Al, K, Na, Ca, Si, Ti, Sn, V, Ge, Ga, B, As, Zr, Cr, Fe, Sr, V, and rare earth elements in addition to the cobalt, manganese, and nickel metals.
[0101] Specifically, the positive electrode active material is LiCoO2, LiFePO4, LiMnO2, LiMn2O4, LiNiO 2, Or LiNi 1-x-y Co x M y Lithium metal oxides such as O2 (0≦x≦1, 0≦y≦1, 0≦x+y≦1, M is Al, Sr, Mg, Mn, or La) or lithium intercalation compounds such as lithium chalcozenide compounds can be used, but are not limited thereto, and any material that can be used as a positive electrode active material in a secondary battery can be used.
[0102] The positive electrode includes a current collector and a positive electrode active material layer formed on the current collector. The positive electrode active material layer may include a positive electrode active material capable of absorbing and releasing lithium, a binder, a conductive material, and the like.
[0103] The negative electrode includes a current collector and a negative electrode active material layer formed on the current collector. The negative electrode active material layer may include a negative electrode active material capable of inserting and extracting lithium, a binder, a conductive material, etc. The negative electrode active material may be, but is not limited to, crystalline carbon, amorphous carbon, a carbon composite, carbon fiber, lithium metal, a lithium alloy, or a carbon-silicon composite, and any material that can be used as a negative electrode active material in a secondary battery may be used.
[0104] The positive electrode and / or negative electrode can be manufactured by dispersing an electrode active material, a binder, a conductive material, and optionally a thickener in a solvent to prepare an electrode slurry composition, and then applying the slurry composition to an electrode current collector. Aluminum or an aluminum alloy can be often used as the positive electrode current collector, and copper or a copper alloy can be often used as the negative electrode current collector.
[0105] The positive electrode current collector and the negative electrode current collector may be in the form of a foil or a mesh.
[0106] The binder is a material that serves to make the active material into a paste, to bond the active material to each other, to bond the active material to the current collector, and to provide a buffering effect against the expansion and contraction of the active material, and may be any binder that can be used by a person skilled in the art. For example, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride (PVdF), polyhexafluoropropylene-polyvinylidene fluoride copolymer (PVdF / HFP), poly(vinyl acetate), alkylated polyethylene oxide, polyvinyl ether, poly(methyl methacrylate), poly(ethyl acrylate), polyacrylonitrile, polyvinylpyridine, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, epoxy resin, nylon, etc. may be used, but are not limited thereto.
[0107] The conductive material is used to provide the electrode with electrical conductivity, and any conductive material that does not cause a chemical change in the secondary battery can be used. The conductive material can be at least one selected from the group consisting of graphite-based conductive materials, carbon black-based conductive materials, and metal or metal compound-based conductive materials. Examples of the graphite-based conductive materials include artificial graphite and natural graphite, examples of the carbon black-based conductive materials include acetylene black, ketjen black, denka black, thermal black, channel black, and examples of the metal or metal compound-based conductive materials include tin, tin oxide, tin phosphate (SnPO4), titanium oxide, potassium titanate, LaSrCoO3, LaSrMnO3, and other perovskite materials. However, the conductive materials are not limited to the above-listed conductive materials.
[0108] The thickener is not particularly limited as long as it serves to adjust the viscosity of the active material slurry. For example, carboxymethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, etc. can be used.
[0109] The solvent in which the electrode active material, binder, conductive material, etc. are dispersed can be a non-aqueous solvent or an aqueous solvent. Examples of the non-aqueous solvent include N-methyl-2-pyrroledione (NMP), dimethylformamide, dimethylacetamide, N,N-dimethylaminopropylamine, ethylene oxide, and tetrahydrofuran. Examples of the aqueous solvent include water.
[0110] The lithium secondary battery may include a separator that prevents short circuit between the positive electrode and the negative electrode and provides a path for lithium ions to move, and the separator may be a polyolefin polymer film such as polypropylene, polyethylene, polyethylene / polypropylene, polyethylene / polypropylene / polyethylene, or polypropylene / polyethylene / polypropylene, or a multi-layer film, microporous film, woven fabric, or nonwoven fabric thereof. Alternatively, the separator may be a film in which a porous polyolefin film is coated with a resin having excellent stability.
[0111] The lithium secondary battery can be formed into various shapes, such as a square type, a cylindrical type, a pouch type, and a coin type. EXAMPLES
[0112] The present invention will now be described in more detail with reference to examples, which should not be construed as limiting the scope of the present invention.
[0113] <Method for producing the compound of Chemical Formula 1>
[0114] Synthesis Example of 2-(pyridin-2-yl)ethyl 1H-imidazole-1-carboxylate (compound of formula 1)
[0115] A 1000mL three-neck flask was equipped with an N2 purge line, a dropping funnel, and a thermometer, and then 1.23 mol of 1,1'-carbonyldiimidazole and 400 mL of dichloromethane were added and stirred. The inside of the reactor was filled with nitrogen atmosphere and the temperature was cooled from the ambient temperature to 10°C. While maintaining the temperature, 1.36 mol of 2-pyridineethanol was added dropwise for 30 minutes. After the addition of 2-pyridineethanol was completed, the temperature was changed from 10°C to room temperature, and the reaction was carried out at the same temperature for 4 hours. After the reaction was completed, 400 mL of water was added, and the organic layer was extracted, and this procedure was repeated three times. After treatment with MgSO4 to remove moisture, filtration was performed, and concentration was carried out to remove dichloromethane in the filtrate. In this way, a powder was obtained. After drying the powder in a vacuum oven, the final compound 2-(pyridin-2-yl)ethyl 1H-imidazole-1-carboxylate was obtained in 50% yield.
[0116] 1 H NMR(Chloroform-d, δ ppm): 1H 8.5ppm, 1H 8.0ppm, 1H 7.6ppm, 1H 7.4ppm, 2H 7.4ppm, 1H 7.0ppm, 2H 4.8ppm, 2H 3.3ppm HRMS: C 11 H 11 N3O2S(M+):217.09
[0117] <Preparation of electrolyte for lithium secondary battery containing 2-(pyridin-2-yl)ethyl 1H-imidazole-1-carboxylate (chemical formula 1)>
[0118] After dissolving LiPF6 to 1.0 M in a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (EC / EMC = 25 / 75 by volume ratio), 1.0 wt% of fluoroethylene carbonate (FEC), 1.0 wt% of lithium difluorophosphate (LiPO2F2), 0.5 wt% of propane sultone (PS), 0.5 wt% of ethylene sulfate (Esa), and 0.5 wt% of the 2-(pyridin-2-yl)ethyl 1H-imidazole-1-carboxylate compound of the synthesis example represented by Chemical Formula 1 were added to the mixed solution to produce an electrolyte for a lithium secondary battery containing the compound of Chemical Formula 1.
[0119] <Manufacture of a Lithium Secondary Battery Containing an Electrolyte Containing the Compound of Chemical Formula 1>
[0120] 94 wt% of an NCM-based positive electrode active material containing Li[NixCo1-x-yMny]O2 (0 < x < 0.5, 0 < y < 0.5), 3 wt% of a conductive material (Super-P), and 3 wt% of a binder (PVdF) were added to N-methyl-2-pyrrolidone (NMP), an organic solvent, to prepare a positive electrode active material slurry. The positive electrode active material slurry was applied to an aluminum thin film as a current collector, dried to produce a positive electrode, and then rolled by roll pressing to produce a positive electrode. Also, SiOx (0<x<2) 96 wt% of a graphite-based negative electrode active material containing SiOx, 1 wt% of a conductive material (Super-P), 1.5 wt% of a binder SBR, and 1.5 wt% of CMC were mixed to produce a negative electrode active material slurry. The negative electrode active material slurry was applied to a copper thin film as a negative electrode current collector and dried to produce a negative electrode.
[0121] The positive electrode and negative electrode manufactured as described above were prepared, and a separator was interposed therebetween. Then, an electrolyte for a lithium secondary battery containing the compound of Chemical Formula 1 was injected between the two electrodes with the separator interposed therebetween, and a lithium secondary battery containing an electrolyte containing the compound of Chemical Formula 1 in an aluminum pouch type (Al-Pouch type) was manufactured.
[0122] Comparative Example
[0123] <Production of electrolyte for lithium secondary batteries containing 1,3-propene sultone (PRS) additive>
[0124] The non-aqueous electrolyte for lithium secondary batteries may contain a sultone-based compound as necessary to prevent the non-aqueous electrolyte from decomposing to hinder high-temperature stability and to prevent the secondary battery from expanding at high temperatures. The sultone-based compound may be, for example, at least one compound selected from the group consisting of 1,3-propane sultone (PS), 1,4-butane sultone (BS), ethene sultone, 1,3-propene sultone, 1,4-butene sultone, and 1-methyl-1,3-propene sultone. In the comparative example, 1,3-propene sultone (PRS), which is currently commonly used, was used.
[0125] LiPF6 was dissolved in a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (volume ratio of EC / EMC = 25 / 75) to a concentration of 1.0 M, and then 1.0 wt% fluoroethylene carbonate (FEC), 1.0 wt% lithium difluorophosphate (LiPO2F2), 0.5 wt% propane sultone (PS), 0.5 wt% ethylene sulfate (Esa), and 0.5 wt% 1.3-propene sultone (PRS) additive as a comparative example were added to the mixed solution to prepare an electrolyte for a lithium secondary battery.
[0126] <Manufacture of a lithium secondary battery containing an electrolyte solution containing 1,3-propene sultone (PRS) additive>
[0127] A lithium secondary battery containing 1,3-propene sultone (PRS) electrolyte without the compound of Chemical Formula 1 was manufactured in the same manner as in the manufacture of the lithium secondary battery of the above example, except that the 2-(pyridin-2-yl)ethyl 1H-imidazole-1-carboxylate compound represented by the compound of Chemical Formula 1 was not added as the electrolyte, and instead a lithium secondary battery electrolyte containing 1,3-propene sultone (PRS) was used.
[0128] The compositions of the electrolyte solutions for lithium secondary batteries of the above examples and comparative examples are shown in Table 1 below.
[0129] <Composition of electrolyte for lithium secondary batteries>
[0130] [Table 1] JPEG0007590038000004.jpg79167
[0131] [Experimental Example]
[0132] <Experimental Example 1> Measurement of life capacity retention rate at high temperature (45℃)
[0133] The pouch-type lithium secondary batteries prepared using the electrolytes for lithium secondary batteries of the Examples and Comparative Examples were charged at high temperature (45°C) at 1C-rate to 4.2V, then discharged at 1C-rate to 2.7V with a 10-minute rest period, and then again with a 10-minute rest period. This process was repeated 100 times to measure the discharge capacity (mAh) and life capacity retention (%) of the battery. The measured discharge capacity and life capacity retention of the secondary battery were compared, and the results are shown in Table 2.
[0134] [Table 2] JPEG0007590038000005.jpg40167
[0135] As shown in Table 2, the result of the life evaluation at high temperature showed that the lithium secondary batteries of the Examples exhibited a higher level of life capacity maintenance rate at high temperature than the lithium secondary batteries of the Comparative Examples.
[0136] Therefore, it was confirmed that the lithium secondary battery of the Example had a higher life capacity retention rate without deteriorating the high-temperature life performance of the secondary battery compared to the lithium secondary battery of the Comparative Example by including an electrolyte solution containing the compound represented by Chemical Formula 1. That is, the compound additive of Chemical Formula 1 improved the life capacity retention rate at high temperatures without deteriorating performance due to side reactions with other additives.
[0137] <Experimental Example 2> Measurement of storage characteristics at high temperature (60℃)
[0138] The pouch-type lithium secondary batteries prepared using the electrolytes for lithium secondary batteries of the Examples and Comparative Examples were stored at high temperature (60°C) for 4 weeks, and then the IR (internal resistance) and the volume change rate of the secondary battery were measured. The results of the internal resistance (IR) and the volume change rate of the secondary battery after 4 weeks of storage at high temperature (60°C) compared to 0 weeks are shown in Table 3 below.
[0139] [Table 3] JPEG0007590038000006.jpg53167
[0140] The increase rate of the internal resistance (IR) of the lithium secondary batteries of the Examples was lower than that of the lithium secondary batteries of the Comparative Examples, and the batteries exhibited superior performance.
[0141] The volume increase rate index showed the same performance (0.3% is at a similar level with no significant difference).
[0142] <Experimental Example 3> Measurement of AC impedance
[0143] The lithium secondary batteries of the Examples and Comparative Examples were stored at high temperature (60°C) for 4 weeks, and then charged at 1.0C CC / CV (4.2V Cut-off), and the AC impedance was measured using an impedance analyzer. The measurement results of the AC impedance are shown in Table 4.
[0144] [Table 4] JPEG0007590038000007.jpg34167
[0145] As shown in Table 4, the lithium secondary batteries of the Examples showed very small AC impedance measurements compared to the lithium secondary batteries of the Comparative Examples. The lithium secondary batteries of the Examples showed a decrease in internal resistance after being left at high temperature (60° C.) for 4 weeks compared to the lithium secondary batteries of the Comparative Examples.
Claims
1. Additives; Additional additives; Lithium salts; and A non-aqueous electrolyte for a lithium secondary battery, comprising a non-aqueous organic solvent, The additive is a compound represented by the following Chemical Formula 1: [Chemical formula 1]
2. 2. The non-aqueous electrolyte for a lithium secondary battery according to claim 1, wherein the additive is included in an amount of 0.05 to 20 wt % based on the total weight of the non-aqueous electrolyte for a lithium secondary battery.
3. 2. The nonaqueous electrolyte solution for a lithium secondary battery according to claim 1, wherein the additional additive is at least one compound selected from the group consisting of halogen-substituted or unsubstituted carbonate-based compounds, nitrile-based compounds, borate-based compounds, lithium salt-based compounds, phosphate-based compounds, sulfite-based compounds, sulfone-based compounds, sulfate-based compounds, and sultone-based compounds.
4. The nonaqueous electrolyte for a lithium secondary battery according to claim 1; positive electrode; A negative electrode; and A lithium secondary battery including a separator.
5. 5. The lithium secondary battery according to claim 4, wherein the negative electrode comprises a carbon-based negative electrode active material and a silicon-based negative electrode active material.
6. 6. The lithium secondary battery of claim 5, wherein the carbon-based negative electrode active material and the silicon-based negative electrode active material are contained in a weight ratio of 97:3 to 50:
50.
7. 7. The lithium secondary battery of claim 6, wherein the carbon-based negative electrode active material and the silicon-based negative electrode active material are contained in a weight ratio of 90:10 to 60:40.
Citation Information
Patent Citations
Non-aqueous electrolyte solution additive, non-aqueous electrolyte solution for lithium secondary battery and lithium secondary battery, comprising non-aqueous electrolyte solution additive
EP3518334A1
Non-aqueous electrolyte for lithium secondary battery and lithium secondary battery comprising same
EP4080636A1
Nonaqueous electrolytic solution and lithium secondary battery using the same
JP2003208920A
Non-aqueous electrolyte secondary battery and non-aqueous electrolyte composition
JP2009252645A
Additive agent for electrolytic solution and lithium ion secondary battery
JP2015162398A