Lithium secondary battery

By employing a perlithium manganese oxide with low cobalt content and a silicon-based negative electrode, the battery achieves improved energy density, rapid charging, and extended lifespan by addressing material degradation and reaction uniformity issues.

JP7590070B2Active Publication Date: 2024-11-26LG ENERGY SOLUTION LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023554046
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-07-20
Filing Date
2022-07-21
Publication Date
2024-11-26
Estimated Expiration
2042-07-21

AI Technical Summary

Technical Problem

Existing lithium secondary batteries face challenges in achieving high energy density, rapid charging performance, and maintaining longevity due to issues such as electrode material degradation and non-uniform reactions during charging and discharging.

Method used

The use of a perlithium manganese oxide with a low cobalt content as the positive electrode active material and a silicon-based negative electrode active material, which compensates for the irreversible capacity of the silicon-based negative electrode and reduces oxygen-redox reactions, thereby stabilizing the battery performance.

Benefits of technology

This configuration enhances the battery's energy density, rapid charging capability, and extends its lifespan by minimizing material deterioration and reaction non-uniformity, while also reducing production costs through lower cobalt usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590070000011
    Figure 0007590070000011
  • Figure 0007590070000012
    Figure 0007590070000012
  • Figure 0007590070000013
    Figure 0007590070000013
Patent Text Reader

Abstract

The present invention relates to a lithium secondary battery including a positive electrode, a negative electrode, a separator, and an electrolyte, in which the positive electrode includes a positive electrode active material layer including a positive electrode active material including a perlithium manganese-based oxide represented by the following Chemical Formula 1, and the negative electrode includes a negative electrode active material layer including a silicon-based negative electrode active material. [Chemical formula 1] Li a Ni b Co c Mn d M e O2 In the above Chemical Formula 1, 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0095985 filed on July 21, 2021, and No. 10-2022-0089894 filed on July 20, 2022, and all contents disclosed in the Korean patent application documents are incorporated by reference as part of this specification.

[0002] The present invention relates to a lithium secondary battery, and more particularly to a lithium secondary battery having excellent rapid charging performance, life characteristics and energy density. [Background technology]

[0003] Recently, interest in energy storage technology has been increasing, and as its application fields expand to include mobile phones, camcorders, notebook PCs, and even the energy of electric vehicles, efforts in research and development of electrochemical devices have become more and more concrete.

[0004] Among electrochemical devices, interest in the development of rechargeable secondary batteries has been growing. In particular, lithium secondary batteries, developed in the early 1990s, have been attracting attention for their advantages of high operating voltage and extremely high energy density.

[0005] Lithium secondary batteries are generally manufactured by forming an electrode assembly by interposing a separator between a positive electrode including a positive electrode active material made of a transition metal oxide containing lithium and a negative electrode including a negative electrode active material capable of storing lithium ions, inserting the electrode assembly into a battery case, injecting a non-aqueous electrolyte that serves as a medium for transferring lithium ions, and then sealing the battery case. The non-aqueous electrolyte is generally composed of a lithium salt and an organic solvent capable of dissolving the lithium salt.

[0006] Recently, as the demand for secondary batteries having high energy density, such as batteries for electric vehicles, etc., has increased, active development of high-voltage secondary batteries that are driven at high voltages has been underway. In addition, in order to realize higher capacity, research is being conducted to apply silicon-based negative electrode active materials with excellent capacity.

[0007] Lithium secondary batteries for automobiles developed to date mainly use lithium nickel-based oxides as the positive electrode active material, but when lithium nickel-based oxides are used, problems such as structural collapse of the positive electrode active material at high voltages, elution of transition metals, gas generation, etc. In addition, when silicon-based negative electrode active materials are used, sacrificial positive electrode materials are used to compensate for the high irreversible capacity of the silicon-based negative electrode active material, but in this case, there is a problem that the content of the positive electrode active material contained in the positive electrode is reduced, resulting in a decrease in battery capacity.

[0008] Meanwhile, there is an increasing demand for lithium secondary batteries with excellent fast-charging performance to shorten the charging time, which is the biggest obstacle to the commercialization of electric vehicles. However, the fast-charging batteries developed to date have not been able to demonstrate satisfactory performance in terms of life characteristics and energy density.

[0009] Therefore, there is a need to develop a lithium secondary battery that has excellent fast charging performance while minimizing the decrease in life characteristics and energy density. Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention aims to solve the above problems and to provide a lithium secondary battery having excellent fast charging performance, life characteristics, and energy density by using a perlithium manganese-based oxide having a low cobalt content and a silicon-based negative electrode active material. [Means for solving the problem]

[0011] On one side, the present invention provides a lithium secondary battery including a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode includes a positive electrode active material layer including a positive electrode active material containing a lithium-rich manganese-based oxide represented by the following Chemical Formula 1, and the negative electrode includes a negative electrode active material layer containing a silicon-based negative electrode active material.

[0012] [Chemical Formula 1] Li a Ni b Co c Mn d M e O2 In Chemical Formula 1, 1 < a, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.1, 0.5 ≤ d < 1.0, 0 ≤ e ≤ 0.2, and M is at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr. Preferably, in Chemical Formula 1, 1.1 ≤ a ≤ 1.5, 0.1 ≤ b ≤ 0.4, 0 ≤ c ≤ 0.05, 0.5 ≤ d ≤ 0.80, 0 ≤ e ≤ 0.1.

[0013] On the other hand, the lithium-rich manganese-based oxide may be a mixture of a rock-salt structure Li2MnO3 phase and a layered structure LiM'O2 phase, and can be represented, for example, by the following [Chemical Formula 2].

[0014] [Chemical Formula 2] X Li2MnO3·(1-X)Li[Ni 1-y-z-w Mn y Co z M w O2 In the [Chemical Formula 2], M is at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr, 0.1 ≤ X ≤ 0.5, 0.4 ≤ y < 1, 0 ≤ z ≤ 0.1, and 0 ≤ w ≤ 0.2.

[0015] Preferably, the positive electrode active material may have D 50 of 2 μm to 10 μm and a BET specific surface area of 3 m 2 / g to 8 m 2 / g.

[0016] The lithium secondary battery may have an energy density of 500 Wh / L or more, and may require 20 minutes or less for rapid charging to 80% SOC. Effect of the Invention

[0017] The present invention uses a perlithium manganese-based oxide in which a rock-salt structured Li2MnO3 phase and a layered structured LiMO2 phase (where M is Ni, Co, Mn) are mixed as a positive electrode active material, and a silicon-based negative electrode active material as a negative electrode active material, so that the excess lithium generated from the Li2MnO3 phase during the activation process can compensate for the irreversible capacity of the silicon-based negative electrode active material. Therefore, the lithium secondary battery of the present invention can minimize the use of a sacrificial positive electrode material for negative electrode compensation and pre-lithiation, thereby maximizing the positive electrode capacity.

[0018] In addition, the present invention uses a perlithium manganese-based oxide having a low Co content of 10 mol% or less as a positive electrode active material, thereby reducing the amount of expensive Co used and saving production costs, suppressing gas generation and positive electrode deterioration by reducing oxygen-redox reactions, and reducing reaction non-uniformity at the negative electrode, thereby realizing a secondary battery with excellent life characteristics, fast charging performance, and energy density.

[0019] In addition, the perlithium nickel manganese cobalt oxide can be stably operated at a relatively high voltage compared to lithium nickel cobalt manganese oxide, so that when a positive electrode active material including the perlithium manganese oxide is used together with a silicon-based negative electrode active material, the driving voltage can be increased and a high energy density can be realized.

[0020] Furthermore, the lithium secondary battery of the present invention has excellent energy density and rapid charging performance since it contains, as the negative electrode active material, a silicon-based negative electrode active material having excellent capacity and rate characteristics. [Brief description of the drawings]

[0021] [Figure 1] 1 shows the charge / discharge profile of a half-cell manufactured using a positive electrode in which Li1.143[Ni0.33Mn0.67]0.857O2 is used as the positive electrode active material. [Diagram 2] 13 is an image showing the formation of conductive paths on the surface of the negative electrode active material when single-walled carbon nanotubes are used as the conductive material. [Diagram 3] 1 is an image showing the formation of conductive paths on the surface of a negative electrode active material when multi-walled carbon nanotubes are used as a conductive material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] The terms and words used in this specification and the claims should not be interpreted in a limited manner to their ordinary or dictionary meanings, but should be interpreted in a meaning and concept that corresponds to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term in order to best describe his / her invention.

[0023] In the present invention, the term "primary particles" refers to particle units that do not appear to have grain boundaries when observed at a magnification of 5,000 to 20,000 times using a scanning electron microscope. The term "average particle size of primary particles" refers to the arithmetic mean value calculated after measuring the particle sizes of primary particles observed in a scanning electron microscope image.

[0024] In the present invention, the "secondary particles" are particles formed by agglomeration of a plurality of primary particles.

[0025] In the present invention, the "average particle size D 50 " means the particle size at 50% of the volume cumulative particle size distribution of the positive electrode active material powder. 50can be measured using the laser diffraction method. For example, after dispersing the positive electrode active material powder in a dispersion medium, it is introduced into a commercially available laser diffraction particle size analyzer (e.g., Microtrac MT 3000), irradiated with ultrasonic waves of about 28 kHz at an output of 60 W, and after obtaining a volume cumulative particle size distribution graph, it can be measured by determining the size of the particles corresponding to 50% of the volume cumulative amount.

[0026] Hereinafter, the present invention will be specifically described.

[0027] As a result of repeated research, the present inventors have found that by using a lithium-rich manganese-based oxide having a Co content of 10 mol% or less as the positive electrode active material and a silicon-based negative electrode active material as the negative electrode active material, it is possible to embody a lithium secondary battery in which the rapid charging performance is improved while minimizing the decrease in life characteristics and energy density, and thus completed the present invention.

[0028] Specifically, the lithium secondary battery according to the present invention includes a positive electrode, a negative electrode, a separator, and an electrolyte, the positive electrode includes a positive electrode active material layer containing a positive electrode active material, the positive electrode active material contains a lithium-rich manganese-based oxide represented by the following Chemical Formula 1, and the negative electrode includes a negative electrode active material layer containing a silicon-based negative electrode active material.

[0029] [Chemical Formula 1] Li a Ni b Co c Mn d M e O2 In Chemical Formula 1, 1 < a, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.1, 0.5 ≤ d < 1.0, 0 ≤ e ≤ 0.2, and M is at least one or more selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr. Preferably, in Chemical Formula 1, 1.1 ≤ a ≤ 1.5, 0.1 ≤ b ≤ 0.4, 0 ≤ c ≤ 0.05, 0.5 ≤ d ≤ 0.80, 0 ≤ e ≤ 0.1.

[0030] Hereinafter, each component of the lithium secondary battery according to the present invention will be specifically described.

[0031] Positive electrode The positive electrode according to the present invention contains a lithium-rich manganese-based oxide represented by Chemical Formula 1 as a positive electrode active material. Specifically, the positive electrode of the present invention includes a positive electrode current collector and a positive electrode active material layer formed on at least one surface of the positive electrode current collector, and the positive electrode active material layer can contain a positive electrode active material containing a lithium-rich manganese-based oxide represented by the following Chemical Formula 1.

[0032] [Chemical Formula 1] Li a Ni b Co c Mn d M e O2 In Chemical Formula 1, M can be at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr.

[0033] On the other hand, a is the molar ratio of Li in the lithium-rich manganese-based oxide, and 1 < a, 1.1 ≤ a ≤ 1.5, or 1.1 ≤ a ≤ 1.3 can be satisfied. When a is within the above range, the irreversible capacity of the Si-based negative electrode active material can be sufficiently compensated, and high-capacity characteristics can be realized.

[0034] b is the molar ratio of Ni in the lithium-rich manganese-based oxide, and 0 ≤ b ≤ 0.5, 0.1 ≤ b ≤ 0.4, or 0.2 ≤ b ≤ 0.4 can be satisfied.

[0035] c is the molar ratio of Co in the lithium-rich manganese-based oxide, and 0 ≤ c ≤ 0.1, 0 ≤ c ≤ 0.08, or 0 ≤ c ≤ 0.05 can be satisfied. When c exceeds 0.1, it is difficult to ensure high capacity, gas generation and deterioration of the positive electrode active material become severe, and the life characteristics may decrease.

[0036] The d is the molar ratio of Mn in the perlithium manganese oxide, and may be 0.5≦d<1.0, 0.50≦d≦0.80, or 0.50≦d≦0.70. If d is less than 0.5, the ratio of the rock salt phase is too small, and the irreversible compensation and capacity improvement effects of the negative electrode are insignificant.

[0037] The e is a molar ratio of the doping element M in the lithium manganese oxide, and may be 0≦e≦0.2, 0≦e≦0.1, or 0≦e≦0.05. If the content of the doping element is too high, it may adversely affect the capacity of the active material.

[0038] In the case of perlithium manganese oxide containing an excess of lithium, it has a structure in which a layered structure (LiM'O2) and a rock salt phase (Li2MnO3) are mixed, and during the initial activation process, the rock salt phase generates an excess amount of lithium ions as it is activated, which compensates for the irreversible capacity of the negative electrode, and therefore it can be balanced with a silicon-based negative electrode without a separate compensation material such as a sacrificial positive electrode material or a pre-lithiation process. However, during the activation process of the rock salt phase, an oxygen-redox reaction (oxygen-redox) occurs, which generates a large amount of gas, which causes cracks inside the active material and collapses the crystal structure, which causes deterioration of the positive electrode and reduces the life characteristics. In particular, when perlithium manganese oxide is applied to a secondary battery that uses a Si-based negative electrode active material as the negative electrode active material, the life reduction occurs seriously.

[0039] As a result of repeated research to solve these problems, the inventors have found that when the Co content in the perlithium manganese oxide is controlled to 10 mol % or less, deterioration in life characteristics can be suppressed even when used in combination with a Si-based negative electrode active material, and have completed the present invention.

[0040] The reason why the life characteristics are improved when a perlithium manganese oxide with a Co content of 10 mol% or less is used is unclear, but it is speculated that this is because when Co in the layered structure is oxidized, oxygen-redox reaction tends to increase at high voltage, and when this is minimized, gas generation and deterioration of the positive electrode active material are reduced.

[0041] Meanwhile, since the Si-based negative electrode active material has a faster reaction rate with lithium than the conventional carbon-based negative electrode active material, lithium secondary batteries using a mixture of Si-based negative electrode active material and carbon-based negative electrode active material have been proposed to improve fast charging performance. However, in the case of a negative electrode using both a Si-based negative electrode active material and a carbon-based negative electrode active material, the reaction in the negative electrode is nonuniform due to the difference in reaction rate between the carbon-based negative electrode active material and the Si-based negative electrode active material, and the increase in the reaction nonuniformity leads to a rapid decrease in the life characteristics of the secondary battery. Meanwhile, since Co is an element that promotes the formation of a layered crystal structure, when the Co content in the positive electrode active material increases, the layered crystal structure is well developed, which improves the mobility of lithium and makes the reaction rate difference between the negative electrode active materials during charging and discharging more significant. Therefore, when the Co content in the perlithium manganese oxide is controlled to 10 mol% or less as in the present invention, the increase in the nonuniformity of the reaction in the negative electrode is suppressed, thereby improving the life characteristics of the secondary battery.

[0042] Meanwhile, in the perlithium manganese oxide represented by [Chemical Formula 1], the molar ratio of Li to the total molar number of metal elements excluding Li (Li / Me) may be 1.2 to 1.5, 1.25 to 1.5, or 1.25 to 1.4. When the Li / Me ratio satisfies the above range, the rate characteristic and capacity characteristic are excellent. If the Li / Me ratio is too high, the electrical conductivity decreases and the rock salt phase (Li2MnO3) increases, which may accelerate the deterioration rate, and if the Li / Me ratio is too low, the effect of improving the energy density is insignificant.

[0043] Meanwhile, the composition of the lithium manganese oxide may be represented by the following [Chemical Formula 2].

[0044] [Chemical formula 2] X Li2MnO3·(1-X)Li[Ni 1-y-z-w Mn y Co z M w ]O2 In the formula 2, M may be at least one selected from the group consisting of metal ions Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr.

[0045] The X means a ratio of the Li2MnO3 phase in the perlithium manganese-based oxide, and may be 0.2≦X≦0.5, 0.25≦X≦0.5, or 0.25≦X≦0.4. When the ratio of the Li2MnO3 phase in the perlithium manganese-based oxide satisfies the above range, the irreversible capacity of the Si-based negative electrode active material can be sufficiently compensated, and high capacity characteristics can be realized.

[0046] The y is a molar ratio of Mn in the LiM'O2 layer, and may be 0.4≦y<1, 0.4≦y≦0.8, or 0.4≦y≦0.7.

[0047] The z is a molar ratio of Co in the LiM'O2 layer and may be 0≦z≦0.1, 0≦z≦0.08, or 0≦z≦0.05. If z exceeds 0.1, gas generation and deterioration of the positive electrode active material may become severe, resulting in reduced life characteristics.

[0048] The w is the molar ratio of the doping element M in the LiM'O2 layer, and can be 0≦w≦0.2, 0≦w≦0.1, or 0≦w≦0.05.

[0049] Meanwhile, the positive electrode active material according to the present invention may further include a coating layer on the surface of the perlithium manganese-based oxide, if necessary. When the positive electrode active material includes a coating layer, the coating layer inhibits contact between the perlithium manganese-based oxide and the electrolyte, thereby reducing electrolyte side reactions, thereby improving the life characteristics.

[0050] The coating layer is a coating element M 1 The coating element M 1may be, for example, at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr, and may be preferably Al, Co, Nb, W, and combinations thereof, and more preferably Al, Co, and combinations thereof. 1 can contain two or more kinds, for example, Al and Co.

[0051] The coating elements are in the oxide form in the coating layer, i.e., M 1 It can exist in Oz (1≦z≦4).

[0052] The coating layer may be formed by dry coating, wet coating, chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), etc. Among these, it is preferable to form the coating layer by atomic layer deposition since the coating layer can be formed over a large area.

[0053] The coating layer may have an area of ​​10 to 100%, preferably 30 to 100%, and more preferably 50 to 100% of the total surface area of ​​the perlithium manganese-based oxide particles. When the coating layer has an area within the above range, the effect of improving the life characteristics is excellent.

[0054] Meanwhile, the positive electrode active material according to the present invention may be in the form of secondary particles in which a plurality of primary particles are aggregated, and the average particle diameter D 50 The diameter of the positive electrode active material may be 2 μm to 10 μm, preferably 2 μm to 8 μm, and more preferably 4 μm to 8 μm. 50 When satisfies this range, the electrode density can be excellently realized and the deterioration of the capacity and rate characteristics can be minimized.

[0055] The positive electrode active material has a BET specific surface area of ​​1 m 2 / g~10m 2 / g, 3~8m 2 / g, or 4-6m2 If the BET specific surface area of ​​the positive electrode active material is too low, the reaction area with the electrolyte is insufficient, making it difficult to realize sufficient capacity, whereas if the specific surface area is too high, moisture absorption is rapid, accelerating side reactions with the electrolyte, making it difficult to ensure life characteristics.

[0056] The positive electrode according to the present invention preferably has an initial irreversible capacity of about 5 to 70%, 5 to 50%, or 5 to 30%. The initial irreversible capacity of the positive electrode means the percentage of the discharge capacity when charged and discharged in a voltage range of 2.5 to 4.4 V relative to the charge capacity when activated at a high voltage of 4.6 V or more, and is a value measured based on a 0.1 C standard.

[0057] When the initial irreversible capacity of the positive electrode satisfies the above range, the irreversible capacity of the silicon-based negative electrode active material can be sufficiently compensated for without using a separate compensation material such as a sacrificial positive electrode material.

[0058] When the perlithium manganese-based oxide represented by Formula 1 is used as the positive electrode active material as in the present invention, the amount of expensive Co used can be reduced, thereby reducing the manufacturing cost and achieving high electrode density. Table 1 below compares the prices of commercially available lithium manganese oxide positive electrode active materials and NCMA positive electrode active materials.

[0059] [Table 1]

[0060] As shown in Table 1, the price of cathode active material 2 having a low Co content is lower than that of NCMA and cathode active material 1. Therefore, when a perlithium manganese-based oxide having a low Co content is used, the production cost of a lithium secondary battery can be reduced.

[0061] Meanwhile, the perlithium manganese-based oxide may be prepared by mixing a transition metal precursor and a lithium source material and then calcining the mixture.

[0062] Examples of the lithium source material include lithium-containing carbonates (e.g., lithium carbonate, etc.), hydrates (e.g., lithium hydroxide hydrate (LiOH·H2O), etc.), hydroxides (e.g., lithium hydroxide), nitrates (e.g., lithium nitrate (LiNO3), etc.), chlorides (e.g., lithium chloride (LiCl), etc.), and any one of these may be used alone or in combination of two or more.

[0063] Meanwhile, the transition metal precursor may be in the form of a hydroxide, oxide or carbonate. When a precursor in the form of a carbonate is used, it is more preferable in that a positive electrode active material having a relatively high specific surface area can be prepared.

[0064] The transition metal precursor may be prepared through a co-precipitation process. For example, the transition metal precursor may be prepared by dissolving each transition metal-containing raw material in a solvent to prepare a metal solution, and then mixing the metal solution, an ammonium cation complexing agent, and a basic compound, and then performing a co-precipitation reaction. If necessary, an oxidizing agent or oxygen gas may be further added during the co-precipitation reaction.

[0065] In this case, the transition metal-containing raw material may be acetate, carbonate, nitrate, sulfate, halide, sulfide, etc. of each transition metal. Specifically, the transition metal-containing raw material may be NiO, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, Mn2O3, MnO2, Mn3O4MnCO3, Mn(NO3)2, MnSO4H2O, manganese acetate, manganese halide, Mn2O3, MnO2, Mn3O4, MnCO3, Mn(NO3)2, MnSO4·H2O, manganese acetate, manganese halide, etc.

[0066] The ammonium cation complexing agent may be at least one selected from the group consisting of NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, and NH4(CO3)2.

[0067] The basic compound may be at least one selected from the group consisting of NaOH, Na2CO3, KOH, and Ca(OH)2. The form of the precursor may vary depending on the type of basic compound used. For example, when NaOH is used as the basic compound, a hydroxide-form precursor can be obtained, and when Na2CO3 is used as the basic compound, a carbonate-form precursor can be obtained. In addition, when a basic compound and an oxidizing agent are used together, an oxide-form precursor can be obtained.

[0068] Meanwhile, the transition metal precursor and the lithium source material may be mixed in amounts such that the total transition metal (Ni+Co+Mn):Li molar ratio is 1:1.05 to 1:2, preferably 1:1.1 to 1:1.8, and more preferably 1:1.25 to 1:1.8.

[0069] Meanwhile, the firing may be performed at a temperature of 600° C. to 1000° C. or 700° C. to 950° C., and the firing time may be 5 hours to 30 hours or 5 hours to 20 hours. The firing atmosphere may be an air atmosphere or an oxygen atmosphere, for example, an atmosphere containing 20 to 100 volume % oxygen.

[0070] Meanwhile, the positive electrode active material layer may further include a conductive material and a binder in addition to the positive electrode active material.

[0071] Examples of the conductive material include spherical or flaky graphite; carbonaceous materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, therma black, carbon fiber, single-walled carbon nanotubes, and multi-walled carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and the like. One or a mixture of two or more of these may be used. The conductive material may be included in an amount of 0.1 to 20 wt%, 1 to 20 wt%, or 1 to 10 wt%, based on the total weight of the positive electrode active material layer.

[0072] Examples of the binder include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 20 wt%, 2 to 20 wt%, or 2 to 10 wt% based on the total weight of the positive electrode active material layer.

[0073] Meanwhile, the positive electrode according to the present invention may have an electrode density of about 2.5 to 3.8 g / cc, about 2.5 to 3.5 g / cc, or about 3.0 to 3.3 g / cc. When the electrode density of the positive electrode satisfies the above range, a high energy density can be realized.

[0074] As described above, the lithium secondary battery of the present invention using the perlithium manganese-based oxide represented by Chemical Formula 1 as a positive electrode active material can stably operate the cell and realize high capacity characteristics even when the end-of-charge voltage is set high to 4.3V to 4.5V during battery operation.

[0075] The charge and discharge profile of a half-cell manufactured using a positive electrode that uses a perlithium manganese oxide as a positive electrode active material is shown in Figure 1. From Figure 1, it can be seen that a positive electrode that uses a perlithium manganese oxide as a positive electrode active material generates an excess amount of lithium at a high voltage of 4.6V or more and is stably operated at a voltage of 4.3V or more.

[0076] negative electrode The negative electrode according to the present invention may include a silicon-based negative electrode active material as a negative electrode active material. Specifically, the negative electrode according to the present invention may include a negative electrode current collector and a negative electrode active material layer formed on at least one surface of the negative electrode current collector, and the negative electrode active material layer may include a silicon-based negative electrode active material as a negative electrode active material.

[0077] Silicon-based negative electrode active materials have a higher theoretical capacity and a faster reaction rate with lithium than carbon-based negative electrode active materials, and therefore, when a silicon-based negative electrode active material is included in a negative electrode, the energy density and fast charging performance are improved. However, silicon-based negative electrode active materials have a large irreversible capacity and a large volume expansion during charging and discharging, and therefore are inferior in terms of life characteristics. In particular, when used in combination with a perlithium manganese oxide in which an oxygen-redox reaction occurs, there is a problem that the deterioration of life characteristics becomes more severe. In addition, when a silicon-based negative electrode active material is used in combination with a carbon-based negative electrode active material, there is a problem that the difference in reaction rate between the silicon-based negative electrode active material and the carbon-based negative electrode active material causes non-uniformity in the negative electrode, which causes anode deterioration. However, when a perlithium manganese oxide with a controlled Co content is used in combination with a silicon-based negative electrode active material as in the present invention, the oxygen-redox reaction is reduced, minimizing the deterioration of life characteristics, and excellent energy density and fast charging performance can be realized.

[0078] The silicon-based negative electrode active material is, for example, Si, SiOw (where 0 < w ≤ 2), Si-C composite, Si-M a alloy (M a is one or more selected from the group consisting of Al, Sn, Mg, Cu, Fe, Pb, Zn, Mn, Cr, Ti, Ni), or a combination thereof.

[0079] On the other hand, the silicon-based negative electrode active material can be doped with M b metal as needed, and at this time, the M b metal can be an alkali metal element of Group 1 and / or an alkaline earth metal element of Group 2, and can be, for example, Li, Mg, etc. Specifically, the silicon-based negative electrode active material can be Si, SiOw (where 0 < w ≤ 2), Si-C composite, etc. doped with M b metal. In the case of a silicon-based negative electrode active material doped with metal, although the active material capacity decreases due to the doping element, it has high efficiency and thus can realize a high energy density.

[0080] In addition, the silicon-based negative electrode active material can further include a carbon coating layer on the particle surface as needed. At this time, the carbon coating amount can be 20% by weight or less, preferably 0.1 - 20% by weight based on the total weight of the silicon-based negative electrode active material. When applying carbon coating, the electrical conductivity of the silicon surface is improved, the uniformity of the SEI layer is improved, and the initial efficiency and life characteristics are improved.

[0081] The carbon coating layer can be formed through methods such as dry coating, wet coating, chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), etc.

[0082] On the other hand, it is preferable that the silicon-based negative electrode active material has a capacity of 1000 - 4000 mAh / g, preferably 1000 - 3800 mAh / g, more preferably 1200 - 3800 mAh / g. Using a silicon-based negative electrode active material that satisfies the above capacity range can realize high-capacity characteristics.

[0083] In addition, the silicon-based negative electrode active material may have an initial efficiency of 60 to 95%, 70 to 95%, and preferably 75 to 95%. The initial efficiency of the silicon-based negative electrode active material means a percentage of a discharge capacity relative to a charge capacity measured by manufacturing a half cell using a negative electrode using 100% of the silicon-based negative electrode active material as a negative electrode active material and a lithium counter electrode, and then charging and discharging between 0.01 V and 1.5 V at a 0.1 C rate. When the initial efficiency of the silicon-based negative electrode active material satisfies the above range, lithium provided in the positive electrode can be reversibly used, and excellent fast charging performance can be realized.

[0084] The particle size of the silicon-based negative electrode active material is D 50 is 3 μm to 8 μm, preferably 4 μm to 7 μm, and D min ~D max When the particle size of the silicon-based negative electrode active material satisfies the above range, sufficient electrode density can be ensured when mixed with the carbon-based negative electrode or alone.

[0085] In addition, the negative electrode may further include a carbon-based negative electrode active material as a negative electrode active material, if necessary. The carbon-based negative electrode active material may be, for example, artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, soft carbon, hard carbon, etc., but is not limited thereto.

[0086] Meanwhile, the silicon-based negative electrode active material may be included in an amount of 1 to 100 wt %, 1 to 50 wt %, 1 to 30 wt %, 1 to 15 wt %, 10 to 70 wt %, or 10 to 50 wt % based on the total weight of the negative electrode active material.

[0087] The carbon-based negative electrode active material may be included in an amount of 0 to 99 wt %, 50 to 99 wt %, 70 to 99 wt %, 85 to 99 wt %, 30 to 90 wt %, or 50 to 90 wt % based on the total weight of the negative electrode active material.

[0088] Meanwhile, the lithium secondary battery of the present invention is preferably constructed with different N / P ratios, which are the ratios of the negative electrode discharge capacity to the positive electrode discharge capacity, depending on the type of negative electrode active material used.

[0089] For example, when a mixture of SiO and a carbon-based negative electrode active material is used as the negative electrode active material, the N / P ratio may be about 100% to 150%, preferably 100% to 140%, and more preferably 100% to 120%. If the negative electrode discharge capacity relative to the positive electrode discharge capacity deviates from the above range, the balance between the positive electrode and the negative electrode may not be achieved, resulting in a decrease in life characteristics or lithium precipitation.

[0090] In addition, when 100% of Si is used as the negative electrode active material, the N / P ratio may be about 150% to 300%, preferably 160% to 300%, and more preferably 180% to 300%. If the negative electrode discharge capacity relative to the positive electrode discharge capacity is out of the above range, the balance between the positive electrode and the negative electrode may not be achieved, resulting in a decrease in life characteristics or lithium precipitation.

[0091] Meanwhile, the negative electrode active material layer may further include a conductive material and a binder, if necessary.

[0092] Examples of the conductive material include spherical or flaky graphite; carbonaceous materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, therma black, carbon fiber, single-walled carbon nanotubes, and multi-walled carbon nanotubes; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and the like. One or a mixture of two or more of these may be used. The conductive material may be included in an amount of 0.1 to 30 wt%, 0.1 to 20 wt%, or 0.1 to 10 wt%, based on the total weight of the negative electrode active material layer.

[0093] Preferably, the conductive material may be a single-walled carbon nanotube. When the conductive material is a carbon nanotube, a conductive path is formed widely, which increases durability and reduces resistance, thereby realizing excellent life characteristics.

[0094] FIG. 2 shows an image illustrating the formation of conductive paths on the surface of the negative electrode active material when single-walled carbon nanotubes are used as the conductive material, and FIG. 3 shows an image illustrating the formation of conductive paths on the surface of the negative electrode active material when multi-walled carbon nanotubes are used as the conductive material.

[0095] As shown in FIGS. 2 and 3, when single-walled carbon nanotubes are used as a conductive material, conductive paths are evenly formed on the surface of the negative electrode active material, thereby improving cycle characteristics.

[0096] Examples of the binder include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylic acid, polyacrylamide, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, and various copolymers thereof, and one or more of these may be used alone or in combination. The binder may be included in an amount of 1 to 20 wt%, 2 to 20 wt%, or 2 to 10 wt% based on the total weight of the negative electrode active material layer.

[0097] Meanwhile, the negative electrode may have a single negative electrode active material layer or a multi-layer structure composed of two or more layers. For example, the negative electrode may include a first negative electrode active material layer formed on a negative electrode current collector and a second negative electrode active material layer formed on the first negative electrode active material.

[0098] When the negative electrode active material layer has a multi-layer structure composed of two or more layers, each layer may have a different type and / or content of the negative electrode active material, binder, and / or conductive material.

[0099] For example, the first negative electrode active material layer (lower layer) may have a higher content of carbon-based negative electrode active material in the entire negative electrode active material than the second negative electrode active material layer (upper layer), and the second negative electrode active material layer may have a higher content of silicon-based negative electrode active material in the entire negative electrode active material than the first negative electrode active material layer, or the second negative electrode active material layer (upper layer) may have a higher content of conductive material than the first negative electrode active material layer (upper layer).

[0100] By forming the negative electrode active material layer in a multi-layer structure and making each layer have a different composition, the performance characteristics of the battery can be improved. For example, when the content of conductive material or silicon-based negative electrode active material is higher in the upper layer than in the lower layer, the fast charging performance can be improved.

[0101] Meanwhile, the negative electrode active material layer may have a porosity of 20% to 70% or 20% to 50%. If the porosity of the negative electrode active material layer is too small, the electrolyte impregnation property may decrease, and the lithium mobility may decrease, whereas if the porosity is too large, the energy density may decrease.

[0102] Separation membrane In the lithium secondary battery of the present invention, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator generally used in lithium secondary batteries may be used without any particular restrictions. In particular, a separator having low resistance to ion movement of the electrolyte and excellent electrolyte humidification capacity is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, etc. may be used. In addition, a separator coated with a ceramic component or a polymer material to ensure heat resistance or mechanical strength may be used, and may be selectively used in a single layer or multilayer structure.

[0103] electrolyte In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, and the like that can be used in the production of lithium secondary batteries, but are not limited to these.

[0104] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0105] The organic solvent may be used without any particular limitation as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone, etc.; an ether solvent such as dibutyl ether or tetrahydrofuran, etc.; a ketone solvent such as cyclohexanone, etc.; an aromatic hydrocarbon solvent such as benzene or fluorobenzene, etc.; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), propylene carbonate (propylene carbonate), etc. Examples of solvents that can be used include carbonate-based solvents such as ethyl alcohol and isopropyl alcohol; alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a hydrocarbon group having a linear, branched or cyclic structure with 2 to 20 carbon atoms and may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes.

[0106] The lithium salt may be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the anion of the lithium salt may be F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , CF3CF2SO3 - , (CF3SO2)2N -, (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - The lithium salt may be at least one selected from the group consisting of LiPF6, LiN(FSO2)2, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, etc. The lithium salt may be used in a concentration range of 0.1 to 5.0M.

[0107] The electrolyte may contain additives for the purpose of improving the life characteristics of the battery, suppressing the capacity decrease, suppressing gas generation, etc. Examples of the additives include various additives used in the art, such as fluoroethylene carbonate (FEC), vinylene carbonate (VC), vinyl ethylene carbonate (VEC), ethylene sulfate (ESa), lithium difluorophosphate (LiPO2F2), lithium bisoxalatoborate (LiBOB), lithium tetrafluoroborate (LiBF4), lithium difluorooxalatoborate (LiDFOB), lithium difluorobisoxalatophosphate (LiDFBP), lithium tetrafluorooxalatophosphate (LiTFOP), lithium methyl sulfate (Li MS), lithium ethyl sulfate (LiES), propane sultone (PS), propene sultone (PRS), succinonitrile (SN), adiponitrile (AND), 1,3,6-hexanetricarbonitrile (HTCN), 1,4-dicyano-2-butene (DCB), fluorobenzene (FB), ethyl di(prop-2-yl)phosphate (EDP), 5-methyl-5-propargyloxycarbonyl-1,3-dioxane-2-one (MPOD), compounds represented by the following chemical formula A (e.g., cyanoethyl polyvinyl alcohol, PVA-CN), compounds represented by the following chemical formula B (e.g., heptafluorobutyl cyanoethyl polyvinyl alcohol, PF-PVA-CN), a compound represented by the following formula C (e.g., propargyl 1H-imidazole-1-carboxylate, PAC), and / or a compound represented by the following formula D (e.g., allylimidazole such as C6H8N2), etc., may be used.

[0108] [Chemical formula A] [ka]

[0109] In the above formula A, n and m each independently represent an integer of 1-100.

[0110] [Chemical formula B] [ka]

[0111] [Chemical formula C] [ka]

[0112] In the above formula C, R 16 is a linear or non-linear alkylene group having 1 to 3 carbon atoms; R 17 ~R 19 are each independently at least one selected from the group consisting of hydrogen, an alkyl group having 1 to 3 carbon atoms, and -CN, and D is CH or N.

[0113] [Chemical formula D] [ka]

[0114] In the formula D, R1, R2, R3, and R4 each independently may include hydrogen; or an alkyl group having 1 to 5 carbon atoms, a cyano group (CN), an allyl group, a propargyl group, an amine group, a phosphate group, an ether group, a benzene group, a cyclohexyl group, a silyl group, an isocyanate group (-NCO), or a fluoro group (-F).

[0115] Preferably, the additive may be a compound that acts as an oxygen scavenger, such as tristri(methylsilyl)phosphate (TMSPi), tristrimethylphosphate (TMPi), tris(2,2,2-trifluoroethyl)phosphate (TTFP), and other phosphate-based materials (see formula E), tristri(methylsilyl)phosphate (TMSPa), polyphosphate trimethylsilyl ester (PPSE), tris(pentafluorophenyl)borane (TPFPB), coumarin-3-carbonitrile (CMCN), 7-ethynylcoumarin (ECM), 3-acetylcoumarin (AcCM), and 3-[(trimethylsilyl)oxyl]-2H-1-benzopyran-2-one (TMSOCM). Compounds that act as oxygen scavengers include 3-(trimethylsilyl)coumarin (TMSCM), 3-(2-propyne-1-yloxyl)-2H-1-benzopyran-2-one (POCM), 2-propyne-1-yl-2-oxo-2H-1-benzopyran-3-carboxylate (OBCM), and other compounds containing a coumarin structure (see chemical formula F).

[0116] [Chemical formula E] [ka]

[0117] [Chemical formula F] [ka]

[0118] In the formulas E and F, R1 to R6 may each independently include a substituted or unsubstituted alkenyl group having 2 to 20 carbon atoms, and a substituted or unsubstituted alkynyl group having 2 to 20 carbon atoms, a cyano (nitrile), a fluoro (F), an ether (COC), a carboxyl (-O-(C=O)-), a trimethylsilyl (-TMS), an isocyanate (-NCO), and / or an isothiocyanate (-NCS) functional group.

[0119] The lithium secondary battery of the present invention configured as described above can perform an activation process at a high voltage of 4.6 V or more, and the irreversible capacity of the silicon-based negative electrode active material can be compensated for by lithium generated during the activation of the Li2MnO3 phase.

[0120] The lithium secondary battery of the present invention configured as described above has a high energy density and excellent rapid charging performance. Specifically, the lithium secondary battery of the present invention has an energy density of 500 Wh / L or more, preferably 500 to 1000 Wh / L, and the time required for rapid charging to ΔSOC 80% is 20 minutes or less.

[0121] The present invention will be described in detail below with reference to specific examples.

[0122] Example 1 The positive electrode active material, single-walled carbon nanotubes, and PVDF binder were mixed in a weight ratio of 96.0:1.0:3.0 in N-methylpyrrolidone to prepare a positive electrode slurry. 1.143 [Ni 0.35 Mn 0.65 ] 0.857 O2 was used.

[0123] The positive electrode slurry was applied onto an aluminum current collector sheet, dried, and then rolled to prepare a positive electrode.

[0124] A first negative electrode slurry was prepared by mixing negative electrode active materials (single-walled carbon nanotubes, styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) in a weight ratio of 96.2:0.8:2:1 in water.

[0125] In addition, a second negative electrode slurry was prepared by mixing the negative electrode active material, single-walled carbon nanotubes, styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) in a weight ratio of 93.8:1.2:4:1 in water.

[0126] As the negative electrode active material of the first negative electrode slurry and the second negative electrode slurry, graphite having an initial efficiency of 94% and SiOx having an initial efficiency of 82% were mixed so that the weight ratio of SiOx:graphite (SiOx:C) was 5:95.

[0127] The first negative electrode slurry was applied onto a copper current collector sheet and dried, and then the second negative electrode slurry was applied thereon, dried, and rolled to prepare a negative electrode having a double-layer structure.

[0128] Meanwhile, the positive and negative electrodes were prepared so that the ratio of the negative electrode discharge capacity to the positive electrode discharge capacity (N / P ratio) was 115% by adjusting the loading amount.

[0129] An electrode assembly was prepared by interposing a separator between the positive and negative electrodes prepared as described above. The electrode assembly was inserted into a battery case, and an electrolyte was injected. The battery case was charged at a constant current of 0.1 C at 45° C. to 4.6 V, and then discharged at a constant current of 0.1 C to 2.0 V to perform an activation process, thereby preparing a lithium secondary battery.

[0130] Example 2 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 Li coated with Al 1500ppm instead of O2 1.143 [Ni 0.34 Co 0.02 Mn 0.64 ] 0.857 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used.

[0131] Example 3 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 Li without Al coating instead of O2 1.143 [Ni 0.34 Co0.02 Mn 0.64 ] 0.857 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used.

[0132] Example 4 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 Li coated with Al 1500ppm instead of O2 1.130 [Ni 0.35 Mn 0.65 ] 0.870 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used.

[0133] Example 5 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 Li coated with Al 1500ppm instead of O2 1.143 [Ni 0.33 Mn 0.67 ] 0.857 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used and multi-walled carbon nanotubes were used instead of single-walled carbon nanotubes when preparing the first and second negative electrode slurries.

[0134] Example 6 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 Li coated with Al 1500ppm instead of O2 1.143 [Ni 0.33 Mn 0.67 ] 0.857 A lithium secondary battery was manufactured in the same manner as in Example 1, except that the second negative electrode slurry was applied onto a copper current collector sheet using O2, dried, and then rolled to manufacture a single-layer negative electrode.

[0135] Example 7 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 Li coated with Al 1500ppm instead of O2 1.143 [Ni 0.33 Mn 0.67 ] 0.857 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used and the loading amounts of the positive and negative electrodes were adjusted so that the ratio of the negative electrode discharge capacity to the positive electrode discharge capacity (N / P ratio) was 120%.

[0136] Example 8 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 Li coated with Al 1500ppm instead of O2 1.143 [Ni 0.33 Mn 0.67 ] 0.857 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used and the negative electrode active materials of the first and second negative electrode slurries were mixed with SiOx:graphite in a weight ratio of 10:90.

[0137] Example 9 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 Li coated with Al 1500ppm instead of O2 1.143 [Ni 0.33 Mn 0.67 ] 0.857 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used, SiC was used alone as the negative electrode active material of the first negative electrode slurry and the second negative electrode slurry, and the ratio of the negative electrode discharge capacity to the positive electrode discharge capacity (N / P ratio) was 250%.

[0138] Comparative Example 1 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 Li coated with Al 1500ppm instead of O2 1.143 [Ni 0.22 Co 0.12 Mn 0.66 ] 0.857 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used.

[0139] Comparative Example 2 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 LiNi coated with Al 1500ppm instead of O2 0.80 Co 0.10 Mn 0.10 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used.

[0140] Comparative Example 3 Li coated with 1500 ppm Al as the positive electrode active material 1.143 [Ni 0.35 Mn 0.65 ] 0.857 Li coated with Al 1500ppm instead of O2 1.143 [Ni 0.33 Mn 0.67 ] 0.857 A lithium secondary battery was manufactured in the same manner as in Example 1, except that O2 was used, graphite was used alone as the negative electrode active material of the first negative electrode slurry and the second negative electrode slurry, and the ratio of the negative electrode discharge capacity to the positive electrode discharge capacity (N / P ratio) was 112%.

[0141] [Table 2]

[0142] Experimental Example 1: The irreversible capacity of the positive electrode and the initial efficiency of the negative electrode prepared in the examples and comparative examples were measured as follows. The measurement results are shown in Table 3 below.

[0143] <Measurement of irreversible capacity of positive electrode> A half-cell was prepared using the positive electrode and the lithium counter electrode prepared in each of the examples and comparative examples, and was then charged to 4.65 V at a constant current of 0.1 C at 45° C., and then discharged to 2.0 V at a constant current of 0.1 C to perform an activation process, and the charge capacity C1 during the activation process was measured.

[0144] Next, the lithium secondary battery after the activation process was charged at a constant current of 0.1 C at 25° C. to 4.35 V, and discharged at a constant current of 0.1 C to 2.5 V to measure the cycle discharge capacity D1. The percentage of the discharge capacity D1 to the charge capacity C1 during the activation process was calculated to measure the irreversible capacity of the positive electrode.

[0145] <Measurement of negative electrode initial efficiency> A half-cell was prepared using the negative electrode and a lithium counter electrode prepared in each of the examples and comparative examples. A current was applied at a constant current of 0.1 C at 25° C. until the voltage reached 0.005 V, and the half-cell was charged at a constant potential of 0.005 V until the voltage reached 0.05 C. The half-cell was then discharged at a constant current of 0.1 C until the voltage reached 1.5 V, and the percentage of the discharge capacity relative to the charge capacity was measured.

[0146] [Table 3]

[0147] Experimental example 2: Number of times the life span reaches 80% The secondary batteries prepared in the examples and comparative examples were charged at 25° C. at a constant current of 0.33 C to 4.35 V and discharged at a constant current of 0.33 C to 2.5 V, which constitutes one cycle, and the number of cycles at which the discharge capacity reached 80% of the initial discharge capacity was measured. The measurement results are shown in Table 4 below.

[0148] Experimental example 3: Rapid charging performance The secondary batteries manufactured in the examples and comparative examples were charged using a step charging method, and the time (unit: minutes) required to charge to 80% SOC was measured. The step charging is a method of charging at a constant charging rate (C rate), and then gradually decreasing the charging rate when a constant voltage (4.35V) is reached. In the present invention, charging was performed in the following C rate conditions: 3C→2.5C→2C→1.5C→1C→0.5C→0.1C. The measurement results are shown in Table 4 below.

[0149] Experimental Example 4: Energy density (unit: Wh / L) The secondary batteries manufactured in the examples and comparative examples were charged and discharged in the voltage range of 4.35V to 2.5V at 25°C and 0.1C to measure the energy density. The energy density was calculated by multiplying the discharge capacity by the average voltage and then dividing it by the unit volume of the secondary battery, and the average voltage was calculated by dividing the curve integral value of the capacity-voltage profile by the capacity. The measurement results are shown in Table 4 below.

[0150] [Table 4]

[0151] In the lithium secondary batteries of Examples 1 to 8 in which a perlithium manganese oxide with a Co content of less than 10 mol% was used as the positive electrode active material and a mixture of SiOx and graphite was used as the negative electrode active material, the rapid charge performance was excellent within 20 minutes, and the capacity retention rate was 80% or more after 640 or more charge / discharge cycles, showing excellent life characteristics, and the energy density was also excellent at 520 Wh / L or more. In the lithium secondary battery of Example 9 in which 100% SiC was used as the negative electrode active material, the capacity and life characteristics were somewhat inferior, but the rapid charge performance was very excellent.

[0152] On the other hand, in the case of the lithium secondary battery of Comparative Example 1, which uses a perlithium manganese-based oxide having a Co content of 10 mol % or more, the rapid charging performance of 20 minutes or less was not satisfied, and the life characteristics and energy density were also lower than those of the lithium secondary batteries of the Examples.

[0153] In the case of the lithium secondary battery of Comparative Example 2, in which NCM811, not a perlithium manganese oxide, was used as the positive electrode active material, the life characteristics were excellent, but the fast charging performance and energy density were lower than those of the lithium secondary battery of the Example.

[0154] In the case of the lithium secondary battery of Comparative Example 3, in which only graphite, a carbon-based negative electrode active material, was used as the negative electrode active material, the rapid charging performance, life characteristics, and energy density were all inferior to the lithium secondary batteries of the Examples, and in particular, the life characteristics and rapid charging performance were significantly inferior.

Claims

1. A lithium secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte, The positive electrode includes a positive electrode active material layer including a positive electrode active material including a perlithium manganese-based oxide represented by the following Chemical Formula 1: the negative electrode includes a negative electrode active material layer including a negative electrode active material that is a mixture of a silicon-based negative electrode active material and a carbon-based negative electrode active material, The silicon-based negative electrode active material is included in an amount of 1 to 15 wt % based on the total weight of the negative electrode active material, The carbon-based negative electrode active material is contained in an amount of 85 to 99 wt % based on the total weight of the negative electrode active material. [Chemical formula 1] Li a Ni b Co c Mn d M e O 2 In Formula 1, 1<a, 0≦b≦0.5, 0≦c≦0.1, 0.5≦d<1.0, and 0≦e≦0.2, and M is at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr.

2. 2. The lithium secondary battery according to claim 1, wherein, in Chemical Formula 1, 1.1≦a≦1.5, 0.1≦b≦0.4, 0≦c≦0.05, 0.5≦d≦0.80, and 0≦e≦0.

1.

3. 2. The lithium secondary battery according to claim 1, wherein the perlithium manganese oxide is represented by the following formula 2: [Chemical formula 2] X Li 2 MnO 3 ・(1-X)Li[Ni 1-y-z-w Mn y Co z M w ]O 2 In the above [Chemical Formula 2], M is at least one selected from the group consisting of Al, B, Co, W, Mg, V, Ti, Zn, Ga, In, Ru, Nb, Sn, Sr, and Zr, and 0.2≦x≦0.5, 0.4≦y<1, 0≦z≦0.1, and 0≦w≦0.

2.

4. The positive electrode active material is D 50 The lithium secondary battery according to claim 1, wherein the thickness is 2 μm to 10 μm.

5. The positive electrode active material has a BET specific surface area of ​​1 to 10 m 2 The lithium secondary battery according to claim 1, wherein the capacitance is 1 / g.

6. 2. The lithium secondary battery according to claim 1, wherein the positive electrode has an initial irreversible capacity of 5% to 70%.

7. 2. The lithium secondary battery according to claim 1, wherein the positive electrode has an electrode density of 2.5 to 3.8 g / cc.

8. 2. The lithium secondary battery according to claim 1, wherein the initial efficiency of the silicon-based negative electrode active material is 60% to 95%.

9. The negative electrode active material layer further includes a conductive material and a binder, 2. The lithium secondary battery according to claim 1, wherein the conductive material comprises single-walled carbon nanotubes.

10. D of the silicon-based negative electrode active material 50 The lithium secondary battery according to claim 1, wherein the average particle diameter is 3 μm to 8 μm.

11. 2. The lithium secondary battery according to claim 1, wherein the porosity of the negative electrode active material layer is 20% to 70%.

12. The lithium secondary battery of claim 1, wherein the N / P ratio of the lithium secondary battery is 100% to 150%.

13. The lithium secondary battery according to claim 12 , wherein the negative electrode has a multi-layer structure including two or more negative electrode active material layers.

14. the negative electrode includes a negative electrode current collector, a first negative electrode active material layer disposed on the negative electrode current collector, and a second negative electrode active material layer disposed on the first negative electrode active material layer, The lithium secondary battery of claim 12 , wherein the second negative electrode active material layer has a higher conductive material content than the first negative electrode active material layer.

15. 2. The lithium secondary battery according to claim 1, wherein the lithium secondary battery has an energy density of 500 Wh / L or more and a time required for rapid charging to an SOC of 80% is 20 minutes or less.

Citation Information

Patent Citations

  • Positive electrode active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery having the same

    JP2009158415A

  • Binder composition for secondary battery positive electrode, slurry composition for secondary battery positive electrode, secondary battery positive electrode, and secondary battery

    JP2013179040A

  • Positive electrode active material for lithium secondary battery, method of manufacturing positive electrode active material, electrode for lithium secondary battery, and lithium secondary battery

    JP2014063707A

  • Lithium ion secondary battery

    JP2019061751A

  • Lithium secondary battery

    WO2018051675A1