Non-aqueous secondary batteries
The non-aqueous secondary battery with a lithium iron phosphate olivine structure and controlled electrolyte composition addresses capacity retention and output performance issues across temperature extremes, enhancing durability and efficiency.
Patent Information
- Application Number
- JP2020105378
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-06-18
AI Technical Summary
Existing lithium ion secondary batteries face challenges in maintaining capacity retention in high-temperature environments due to oxidative decomposition of the solvent and metal elution, and they fail to deliver sufficient output performance in low-temperature conditions due to electrolyte freezing and lithium salt precipitation.
A non-aqueous secondary battery configuration using a lithium-containing metal oxide with an olivine structure as the positive electrode active material, combined with a non-aqueous electrolyte containing acetonitrile and specific lithium salts (LiN(SO2F)2 and LiPF6) within controlled anion and propionitrile limits, to suppress interfacial resistance and enhance performance across temperature ranges.
The solution effectively suppresses battery deterioration in high-temperature environments and maintains excellent output performance in low-temperature conditions, achieving improved cycle performance and capacity retention.
Smart Images

Figure 0007590126000004 
Figure 0007590126000005 
Figure 0007590126000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-aqueous secondary battery. [Background technology]
[0002] In recent years, lithium-ion secondary batteries have been developed with the aim of being installed in electric vehicles and hybrid vehicles. Among them, there is a movement to replace lead-acid batteries used in idling stop systems and starters with lithium-ion secondary batteries. Specifications required for the above applications include long-term reliability in high-temperature environments assumed for installation in the engine compartment, as well as output performance in low-temperature environments, since the engine needs to be driven in cold regions.
[0003] However, in high-temperature environments, the solvent contained in the nonaqueous electrolyte undergoes oxidation and reduction decomposition, and the accumulation of decomposition products increases internal resistance, and gas generation reduces battery performance. In particular, when lithium cobalt oxide (LiCoO2) or ternary positive electrodes (Li(Ni / Co / Mn)O2) are used as the positive electrode active material, it is known that transition metals are eluted from the positive electrode active material by performing charge-discharge cycles in a high-temperature environment, and the eluted metals precipitate on the surface of the negative electrode, causing various types of battery deterioration. On the other hand, for power tool applications, lithium-containing compounds with an olivine structure that has excellent thermal stability have long been used as the positive electrode active material. This positive electrode active material has excellent thermal stability and high output performance because of its stable crystal structure and small primary particle size. Furthermore, since it is mainly made of iron, which is a resource in abundance, it is low cost and has a small environmental impact. On the other hand, in low-temperature environments (below -40°C), it has been difficult to satisfy the output performance required to drive the engine due to the freezing of the nonaqueous electrolyte and the precipitation of lithium salts.
[0004] Patent Document 1 reports that when a positive electrode contains a positive electrode active material, specifically olivine-type lithium iron phosphate, having an operating potential more negative than that of metallic lithium by 4 V, and a negative electrode active material, specifically graphite, having an operating potential more positive than that of metallic lithium by 1 V, and an ether compound having a specific structure and a lithium salt are used as an electrolyte, the battery shows better rate characteristics than conventional carbonate-based electrolytes.
[0005] Patent Document 2 reports that the use of a specific electrolyte solution makes it possible to exhibit excellent characteristics over a wide temperature range from high to low temperatures.
[0006] Patent Document 3 reports that by including an ester compound and methylene bissulfonate in the electrolyte, the reductive decomposition of the electrolyte is suppressed and a good coating film forming effect is achieved, thereby improving high-temperature storage characteristics.
[0007] Patent Document 4 describes M(FSO3) x It has been reported that excellent input / output performance can be obtained by using an electrolyte containing a certain ratio of fluorosulfonate represented by the formula:
[0008] Patent Document 5 reports a lithium-ion secondary battery that uses olivine-type lithium iron phosphate as a positive electrode active material on a metal foil having through holes, and uses a specific electrolyte and separator, thereby having excellent output performance in an environment of -30°C. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2010-277958 A [Patent Document 2] International Publication No. 2017 / 057588 [Patent Document 3] International Publication No. 2012 / 017999 [Patent Document 4] JP 2011-187440 A [Patent Document 5] JP 2015-215977 A Summary of the Invention [Problem to be solved by the invention]
[0010] However, although the lithium ion secondary battery described in Patent Document 1 mentions its output performance at room temperature, it makes no mention whatsoever of its output in a low-temperature environment.
[0011] The lithium-ion secondary battery described in Patent Document 2 operates over a wide temperature range from high to low temperatures. However, its ionic conductivity in a 25°C environment is no different from that of a general carbonate electrolyte, and the ionic conductivity decreases further in an extremely low temperature environment. As a result, the battery does not achieve performance sufficient to meet the output required for in-vehicle applications.
[0012] The lithium-ion secondary battery described in Patent Document 3 can improve high-temperature durability by strengthening the negative electrode protective coating, but because too much strong protective coating is formed on the negative electrode to suppress the reductive decomposition of the electrolyte, the internal resistance increases and it is not possible to achieve sufficient output performance in a low-temperature environment.
[0013] The lithium-ion battery using the electrolyte solution containing LiFSO3 as a lithium salt described in Patent Document 4 is characterized by the fact that the FSO3 anion (FSO3 - ) was reduced and decomposed at the negative electrode, which increased the internal resistance, and good cycle performance was not obtained.
[0014] A lithium ion secondary battery using a specific positive electrode, negative electrode, and separator as described in Patent Document 5 exhibits excellent output performance in a low-temperature environment, but does not mention the reductive decomposition of the electrolyte in the negative electrode in a high-temperature environment.
[0015] In view of the above problems, an object of the present invention is to provide a nonaqueous secondary battery that suppresses a decrease in capacity retention rate when subjected to charge / discharge cycles in a high-temperature environment and also has excellent output performance in a low-temperature environment. [Means for solving the problem]
[0016] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, they have found that the above-mentioned problems can be solved by using a nonaqueous electrolyte or a nonaqueous secondary battery having the following configuration, and have completed the present invention. That is, the present invention is as follows. [1] A non-aqueous secondary battery having a positive electrode having a positive electrode active material, a negative electrode having a negative electrode active material, a separator, and a non-aqueous electrolyte solution, The positive electrode contains a lithium-containing metal oxide as the positive electrode active material, The lithium-containing metal oxide has an olivine structure. x FePO4, wherein 0 <x<1.2であり、 The nonaqueous electrolyte solution contains 1 volume % to 85 volume % of acetonitrile, and LiN(SO2F)2 and LiPF6 as lithium salts, based on the total mass of the nonaqueous solvent, and the content of FSO3 anions is 100 ppm or less based on the total mass of the nonaqueous electrolyte solution. [2] 2. The nonaqueous secondary battery according to item 1, wherein the propionitrile contained in the nonaqueous electrolyte solution is less than 5.0 ppm based on the total mass of the nonaqueous electrolyte solution. Effect of the Invention
[0017] By using lithium iron phosphate with an olivine structure as the positive electrode active material, various types of battery degradation in high-temperature environments can be suppressed, and by controlling the content of FSO3 anions in the non-aqueous electrolyte containing acetonitrile, LiN(SO2F)2, and LiPF6 within a specified range, an increase in the interface resistance of the negative electrode can be suppressed, resulting in excellent output performance in low-temperature environments. [Brief description of the drawings]
[0018] [Figure 1] 1 is a plan view illustrating a schematic example of a nonaqueous secondary battery according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view taken along line AA of the nonaqueous secondary battery of FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] Hereinafter, an embodiment for carrying out the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. The present invention is not limited to the following embodiment, and various modifications are possible without departing from the gist of the present invention. In this specification, a numerical range described using "~" includes the numerical values described before and after it.
[0020] 《Nonaqueous secondary battery》 The non-aqueous secondary battery of this embodiment includes a positive electrode having a positive electrode active material, a negative electrode having a negative electrode active material, a separator, and a non-aqueous electrolyte. In addition, although not limited thereto, the non-aqueous secondary battery of this embodiment includes a lithium ion battery including a positive electrode containing a positive electrode material capable of absorbing and releasing lithium ions as a positive electrode active material, and a negative electrode containing a negative electrode material capable of absorbing and releasing lithium ions and / or metallic lithium as a negative electrode active material.
[0021] Specifically, the nonaqueous secondary battery of this embodiment may be a nonaqueous secondary battery as shown in FIGS. 1 and 2. Here, FIG. 1 is a plan view that shows a schematic representation of a nonaqueous secondary battery, and FIG. 2 is a cross-sectional view taken along the line AA in FIG. 1. The nonaqueous secondary battery 100 shown in FIGS. 1 and 2 is formed of a pouch-type cell. The nonaqueous secondary battery 100 contains a laminated electrode body formed by laminating a positive electrode 150 and a negative electrode 160 with a separator 170 interposed therebetween, and a nonaqueous electrolyte (not shown) in a space 120 of a battery exterior 110 formed of two aluminum laminate films. The battery exterior 110 is sealed at its outer periphery by heat-sealing the upper and lower aluminum laminate films. The laminate formed by laminating the positive electrode 150, the separator 170, and the negative electrode 160 in this order is impregnated with a nonaqueous electrolyte. 2, in order to avoid complicating the drawing, the layers constituting the battery exterior 110 and the layers of the positive electrode 150 and the negative electrode 160 are not shown separately. The aluminum laminate film constituting the battery exterior 110 is preferably an aluminum foil coated on both sides with a polyolefin resin.
[0022] The positive electrode 150 is connected to the positive electrode lead body 130 within the nonaqueous secondary battery 100. Although not shown, the negative electrode 160 is also connected to the negative electrode lead body 140 within the nonaqueous secondary battery 100. One end of each of the positive electrode lead body 130 and the negative electrode lead body 140 is drawn out to the outside of the battery exterior 110 so that they can be connected to an external device, and the ionomer portions of these are heat-fused to one side of the battery exterior 110.
[0023] 1 and 2, the positive electrode 150 and the negative electrode 160 each have one laminated electrode body, but the number of laminated positive electrodes 150 and negative electrodes 160 can be appropriately increased depending on the capacity design. In the case of a laminated electrode body having a plurality of positive electrodes 150 and negative electrodes 160, the tabs of the same electrode may be joined by welding or the like and then joined to a single lead body by welding or the like and taken out of the battery. The tabs of the same electrode may be formed from an exposed portion of a current collector, or may be formed by welding a metal piece to an exposed portion of a current collector.
[0024] The positive electrode 150 is composed of a positive electrode active material layer made of a positive electrode mixture and a positive electrode current collector. The negative electrode 160 is composed of a negative electrode active material layer made of a negative electrode mixture and a negative electrode current collector. The positive electrode 150 and the negative electrode 160 are arranged with the separator 170 between them so that the positive electrode active material layer and the negative electrode active material layer face each other.
[0025] As these components, materials that are used in conventional lithium ion batteries can be used as long as they satisfy the requirements of this embodiment. Each component of the nonaqueous secondary battery will be described in more detail below.
[0026] [Positive electrode] The positive electrode contains a lithium-containing metal oxide as a positive electrode active material. Typically, the positive electrode is composed of a positive electrode current collector and a positive electrode active material layer made of a positive electrode mixture on one or both sides of the positive electrode current collector. The positive electrode is not particularly limited as long as it acts as a positive electrode of a non-aqueous secondary battery.
[0027] The positive electrode active material layer preferably contains a positive electrode active material, and further contains a conductive assistant and a binder as necessary. The positive electrode active material layer preferably contains a material capable of absorbing and releasing lithium ions as a positive electrode active material. When using such a material, it is preferable because it tends to be possible to obtain high voltage and high energy density.
[0028] Examples of the positive electrode active material include a positive electrode active material containing at least one transition metal element selected from the group consisting of Ni, Mn, and Co. The following general formula (a): Li p Ni q Co r Mn s M t O u ·····(a) {In the formula, M is at least one metal selected from the group consisting of Al, Sn, In, Fe, V, Cu, Mg, Ti, Zn, Mo, Zr, Sr, and Ba, and 0 < p < 1.3, 0 < q < 1.2, 0 < r < 1.2, 0 ≤ s < 0.5, 0 ≤ t < 0.3, 0.7 ≤ q + r + s + t ≤ 1.2, 1.8 < u < 2.2. And p is a value determined by the charge and discharge state of the battery.} At least one Li-containing metal oxide selected from Li-containing metal oxides represented by the following is preferred.
[0029] Specific examples of the positive electrode active material include, for example, lithium cobalt oxide typified by LiCoO2; lithium manganese oxides typified by LiMnO2, LiMn2O4, and Li2Mn2O4; lithium nickel oxide typified by LiNiO2; LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.8 Co 0.2 O2, and lithium-containing composite metal oxides represented by Li z MO2 (M contains at least one transition metal element selected from the group consisting of Ni, Mn, and Co, and represents two or more metal elements selected from the group consisting of Ni, Mn, Co, Al, and Mg, and z represents a number greater than 0.9 and less than 1.2).
[0030] In particular, when the Ni content ratio q of the Li-containing metal oxide represented by the general formula (a) is 0.5 < q < 1.2, it is preferable because both the reduction in the amount of Co, which is a rare metal, and the increase in the energy density can be achieved. Examples of such a positive electrode active material include, for example, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.75 Co 0.15 Mn 0.15 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.85 Co 0.075 Mn 0.075 O2, LiNi 0.8 Co 0.15 Al 0.05 O2, LiNi 0.81 Co 0.1 Al 0.09 O2, LiNi 0.85 Co 0.1 Al 0.05 O2, etc., and lithium-containing composite metal oxides represented thereby can be mentioned.
[0031] On the other hand, as the Ni content ratio increases, deterioration tends to progress at a low voltage. In the positive electrode active material of the Li-containing metal oxide represented by the general formula (a), active points that oxidatively deteriorate the non-aqueous electrolyte essentially exist, but these active points may inadvertently consume the compound added to protect the negative electrode on the positive electrode side. Among them, acid anhydrides tend to be particularly susceptible to this influence. In particular, when acetonitrile is contained as the non-aqueous solvent, the addition effect of the acid anhydride is extremely large, so the consumption of the acid anhydride on the positive electrode side is a fatal problem.
[0032] In addition, the decomposition products of these additives that are taken in and deposited on the positive electrode side not only increase the internal resistance of the non-aqueous secondary battery, but also accelerate the deterioration of the lithium salt. Furthermore, the protection of the negative electrode surface, which was the original purpose, becomes insufficient. In order to deactivate the active sites that essentially cause the oxidation deterioration of the non-aqueous electrolyte, it is important to control the Jahn-Teller distortion or to coexist with a component that plays a role as a neutralizer. Therefore, it is preferable that the positive electrode active material contains at least one metal selected from the group consisting of Al, Sn, In, Fe, V, Cu, Mg, Ti, Zn, Mo, Zr, Sr, and Ba.
[0033] For the same reason, it is preferable that the surface of the positive electrode active material is coated with a compound containing at least one metal element selected from the group consisting of Zr, Ti, Al, and Nb. It is more preferable that the surface of the positive electrode active material is coated with an oxide containing at least one metal element selected from the group consisting of Zr, Ti, Al, and Nb. Furthermore, it is particularly preferable that the surface of the positive electrode active material is coated with at least one oxide selected from the group consisting of ZrO2, TiO2, Al2O3, NbO3, and LiNbO2, since this does not inhibit the permeation of lithium ions.
[0034] The positive electrode active material may be a lithium-containing compound other than the Li-containing metal oxide represented by formula (a), and is not particularly limited as long as it contains lithium. Examples of such lithium-containing compounds include composite oxides containing lithium and transition metal elements, metal chalcogenides containing lithium, metal phosphate compounds containing lithium and transition metal elements, and metal silicate compounds containing lithium and transition metal elements. From the viewpoint of obtaining a higher voltage, the lithium-containing compound is preferably a metal phosphate compound containing lithium and at least one transition metal element selected from the group consisting of Co, Ni, Mn, Fe, Cu, Zn, Cr, V, and Ti.
[0035] More specifically, the lithium-containing compound is represented by the following formula (Xa): Li v M I D2(Xa) In the formula, D represents a chalcogen element, and M I represents one or more transition metal elements, the value of v is determined depending on the charge / discharge state of the battery and represents a number from 0.05 to 1.10, and u represents a number from 0 to 2.}, The following formula (Xb): Li w M II PO4(Xb) In the formula, D represents a chalcogen element, and M II represents one or more transition metal elements, the value of w is determined depending on the charge / discharge state of the battery and represents a number from 0.05 to 1.10, and u represents a number from 0 to 2.}, and The following formula (Xc): Li t M III u SiO4(Xc) In the formula, D represents a chalcogen element, and M III represents one or more transition metal elements, the value of t is determined depending on the charge / discharge state of the battery and represents a number from 0.05 to 1.10, and u represents a number from 0 to 2.} Examples of the compounds include those represented by the following formula:
[0036] The lithium-containing compound represented by the above formula (Xa) has a layered structure, and the compounds represented by the above formulas (Xb) and (Xc) have an olivine structure. These lithium-containing compounds may be those in which a part of the transition metal element is replaced by Al, Mg, or other transition metal element, those in which these metal elements are included in the crystal grain boundary, those in which a part of the oxygen atoms is replaced by fluorine atoms, etc., and those in which at least a part of the surface of the positive electrode active material is coated with another positive electrode active material, etc., for the purpose of stabilizing the structure.
[0037] In this embodiment, the positive electrode is a positive electrode active material represented by (Xb) having an olivine structure. xIt contains a lithium-containing metal oxide represented by FePO4, where 0 < x < 1.2. Preferably, it is lithium iron phosphate (LiFePO4). The olivine-type structure has excellent thermal stability, a stable crystal structure, and a small primary particle size. Therefore, when the positive electrode active material contains a lithium-containing metal oxide having the olivine-type structure, the high-temperature durability tends to be improved. The above Li x The content of the compound represented by FePO4 is preferably 40% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and still more preferably 80% by mass to 100% by mass based on the total mass of the positive electrode active material. The positive electrode active material may use Li x FePO4 alone or may contain other positive electrode active materials.
[0038] As the positive electrode active material in this embodiment, only the above lithium-containing compound may be used, or other positive electrode active materials may be used in combination with the lithium-containing compound. Examples of such other positive electrode active materials include metal oxides or metal chalcogenides having a tunnel structure and a layered structure; sulfur; conductive polymers, etc. Examples of the metal oxide or metal chalcogenide having a tunnel structure and a layered structure include oxides, sulfides, selenides, etc. of metals other than lithium represented by MnO2, FeO2, FeS2, V2O5, V6O 13 , TiO2, TiS2, MoS2, and NbSe2. Examples of the conductive polymer include conductive polymers represented by polyaniline, polythiophene, polyacetylene, and polypyrrole.
[0039] The above-mentioned other positive electrode active materials are used alone or in combination of two or more, and there is no particular limitation. However, since it is possible to reversibly and stably occlude and release lithium ions and achieve a high energy density, it is preferable that the positive electrode active material layer contains at least one transition metal element selected from Ni, Mn, and Co.
[0040] When a lithium-containing compound and another positive electrode active material are used in combination as the positive electrode active material, the ratio of the two is preferably 80 mass % or more, and more preferably 85 mass % or more, of the lithium-containing compound relative to the total positive electrode active material.
[0041] Examples of the conductive additive include carbon black, such as graphite, acetylene black, and ketjen black, and carbon fiber. The content of the conductive additive is preferably 10 parts by mass or less, and more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the positive electrode active material.
[0042] Examples of the binder include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid, styrene butadiene rubber, and fluororubber. The content of the binder is preferably 6 parts by mass or less, and more preferably 0.5 to 4 parts by mass, relative to 100 parts by mass of the positive electrode active material.
[0043] The positive electrode active material layer is formed by dispersing a positive electrode mixture, which is a mixture of a positive electrode active material and, if necessary, a conductive assistant and a binder, in a solvent to form a positive electrode mixture-containing slurry, applying the slurry to a positive electrode current collector, drying (solvent removal), and pressing if necessary. There is no particular restriction on such a solvent, and a conventionally known solvent can be used. For example, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc. can be mentioned.
[0044] The positive electrode current collector is made of a metal foil such as aluminum foil, nickel foil, stainless steel foil, etc. The positive electrode current collector may have a carbon coating on the surface, or may be processed into a mesh shape. The thickness of the positive electrode current collector is preferably 5 to 40 μm, more preferably 7 to 35 μm, and further preferably 9 to 30 μm.
[0045] [Negative electrode] The negative electrode has a negative electrode active material. The negative electrode is generally composed of a negative electrode active material layer made of a negative electrode mixture and a negative electrode current collector. The negative electrode can act as a negative electrode of a non-aqueous secondary battery. The negative electrode active material layer contains the negative electrode active material, and preferably contains a conductive assistant and a binder as necessary.
[0046] Examples of the negative electrode active material include amorphous carbon (hard carbon), artificial graphite, natural graphite, graphite, pyrolytic carbon, coke, glassy carbon, baked bodies of organic polymer compounds, mesocarbon microbeads, carbon fibers, activated carbon, graphite, carbon colloids, and carbon black, as well as metal lithium, metal oxides, metal nitrides, lithium alloys, tin alloys, silicon alloys, intermetallic compounds, organic compounds, inorganic compounds, metal complexes, organic polymer compounds, etc. The negative electrode active material may be used alone or in combination of two or more.
[0047] The negative electrode active material layer uses lithium ions as the negative electrode active material at 0.4V vs. Li / Li in order to increase the battery voltage. + It is preferable that the hydrogen-containing gas contains a material capable of absorbing at a potential lower than the hydrogen potential.
[0048] Examples of the conductive assistant include carbon black, such as graphite, acetylene black, and ketjen black, and carbon fiber. The content of the conductive assistant is preferably 20 parts by mass or less, and more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the negative electrode active material.
[0049] Examples of the binder include carboxymethyl cellulose, PVDF, PTFE, polyacrylic acid, and fluororubber. Also included are diene rubbers such as styrene-butadiene rubber. The content of the binder is preferably 10 parts by mass or less, more preferably 0.5 to 6 parts by mass, based on 100 parts by mass of the negative electrode active material.
[0050] The negative electrode active material layer is formed by dispersing a negative electrode mixture, which is a mixture of a negative electrode active material and, if necessary, a conductive assistant and a binder, in a solvent to form a negative electrode mixture-containing slurry, applying the slurry to a negative electrode current collector, drying (solvent removal), and pressing if necessary. There is no particular restriction on such a solvent, and a conventionally known solvent may be used. Examples of such a solvent include N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, and water.
[0051] The negative electrode current collector is made of a metal foil such as copper foil, nickel foil, stainless steel foil, etc. The surface of the negative electrode current collector may be carbon-coated or processed into a mesh shape. The thickness of the negative electrode current collector is preferably 5 to 40 μm, more preferably 6 to 35 μm, and further preferably 7 to 30 μm.
[0052] [Non-aqueous electrolyte] In this specification, the term "nonaqueous electrolyte" (hereinafter simply referred to as "electrolyte") refers to an electrolyte containing 1 mass % or less of water relative to the total amount of the electrolyte.
[0053] In this embodiment, the non-aqueous electrolyte preferably contains as little water as possible, but may contain a very small amount of water as long as it does not hinder the solution of the problem of the present invention. The content of such water is preferably 300 mass ppm or less, more preferably 200 mass ppm or less, based on the total amount of the non-aqueous electrolyte. As long as the non-aqueous electrolyte has a configuration for achieving the solution of the problem of the present invention, the other components can be appropriately selected and used from the constituent materials in the known non-aqueous electrolyte used in lithium ion batteries.
[0054] In this embodiment, the nonaqueous electrolyte contains acetonitrile and, as lithium salts, LiN(SO2F)2 and LiPF6.
[0055] <Non-aqueous solvent> In the present embodiment, the term "non-aqueous solvent" refers to components other than the lithium salt and various additives among the components contained in the non-aqueous electrolyte. However, when the non-aqueous electrolyte contains an electrode protection additive, the electrode protection additive that serves as a solvent for dissolving the lithium salt is also treated as a "non-aqueous solvent". Examples of non-aqueous solvents include alcohols such as methanol and ethanol; aprotic solvents, etc. Among them, aprotic solvents are preferred as non-aqueous solvents. The non-aqueous solvent may contain a solvent other than the aprotic solvent as long as it does not hinder the problem solving of the present invention.
[0056] The non-aqueous solvent for the non-aqueous electrolyte contains acetonitrile as an aprotic solvent. The non-aqueous solvent contains acetonitrile, which improves the ionic conductivity of the non-aqueous electrolyte, thereby increasing the diffusibility of lithium ions in the battery. Therefore, when the non-aqueous electrolyte contains acetonitrile, the lithium ions can be well diffused to the area near the current collector where the lithium ions are difficult to reach during high-load discharge. Therefore, it is possible to extract sufficient capacity even during high-load discharge, and a non-aqueous secondary battery with excellent load characteristics can be obtained. This effect tends to be obtained especially in a positive electrode having a thick positive electrode active material layer and a high loading amount of positive electrode active material.
[0057] Furthermore, the non-aqueous solvent contains acetonitrile, which can improve the rapid charging characteristics of the non-aqueous secondary battery. In constant current (CC)-constant voltage (CV) charging of a non-aqueous secondary battery, the capacity per unit time during the CC charging period is greater than the charge capacity per unit time during the CV charging period. When acetonitrile is used as the non-aqueous solvent of the non-aqueous electrolyte, the range in which CC charging is possible can be expanded (CC charging time can be extended) and the charging current can also be increased, so that the time from the start of charging to fully charging the non-aqueous secondary battery can be significantly shortened.
[0058] In addition, acetonitrile is easily electrochemically decomposed by reduction. Therefore, when acetonitrile is used, it is preferable to use another solvent (e.g., an aprotic solvent other than acetonitrile) together with acetonitrile as a non-aqueous solvent and / or to add an additive for protecting an electrode for forming a protective film on the electrode.
[0059] The content of acetonitrile is 1% by volume to 85% by volume based on the total mass of the non-aqueous solvent. The lower limit of the content of acetonitrile is more preferably 5% by volume or more or 10% by volume or more, and more preferably 20% by volume or more, based on the total mass of the non-aqueous solvent. The upper limit is more preferably 80% by volume or less, and more preferably 70% by volume or less. When the content of acetonitrile is 5% by volume or more based on the total amount of the non-aqueous solvent, the ion conductivity tends to increase and high output characteristics can be expressed, and further, the dissolution of the lithium salt can be promoted. Since the additive described later suppresses the increase in the internal resistance of the battery, when the content of acetonitrile in the non-aqueous solvent is within the above range, the high temperature cycle characteristics and other battery characteristics tend to be further improved while maintaining the excellent performance of acetonitrile.
[0060] Examples of aprotic solvents other than acetonitrile include cyclic carbonates, fluoroethylene carbonate, lactones, organic compounds having sulfur atoms, chain fluorinated carbonates, cyclic ethers, mononitriles other than acetonitrile, alkoxy group-substituted nitriles, dinitriles, cyclic nitriles, short-chain fatty acid esters, chain ethers, fluorinated ethers, ketones, and compounds in which some or all of the H atoms of the aprotic solvents have been substituted with halogen atoms.
[0061] Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, 1,2-butylene carbonate, trans-2,3-butylene carbonate, cis-2,3-butylene carbonate, 1,2-pentylene carbonate, trans-2,3-pentylene carbonate, cis-2,3-pentylene carbonate, vinylene carbonate, 4,5-dimethylvinylene carbonate, and vinylethylene carbonate.
[0062] Examples of fluoroethylene carbonate include 4-fluoro-1,3-dioxolan-2-one, 4,4-difluoro-1,3-dioxolan-2-one, cis-4,5-difluoro-1,3-dioxolan-2-one, trans-4,5-difluoro-1,3-dioxolan-2-one, 4,4,5-trifluoro-1,3-dioxolan-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolan-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolan-2-one.
[0063] Lactones include gamma-butyrolactone, alpha-methyl-gamma-butyrolactone, gamma-valerolactone, gamma-caprolactone, delta-valerolactone, delta-caprolactone, and epsilon-caprolactone.
[0064] Examples of organic compounds having a sulfur atom include ethylene sulfite, propylene sulfite, butylene sulfite, pentene sulfite, sulfolane, 3-sulfolene, 3-methylsulfolane, 1,3-propane sultone, 1,4-butane sultone, 1-propene 1,3-sultone, dimethyl sulfoxide, tetramethylene sulfoxide, and ethylene glycol sulfite.
[0065] Examples of the chain carbonate include ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, methyl butyl carbonate, dibutyl carbonate, and ethyl propyl carbonate.
[0066] Cyclic ethers include, for example, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, and 1,3-dioxane.
[0067] Examples of mononitriles other than acetonitrile include propionitrile, butyronitrile, valeronitrile, benzonitrile, and acrylonitrile.
[0068] Alkoxy-substituted nitriles include, for example, methoxyacetonitrile and 3-methoxypropionitrile.
[0069] Dinitriles include, for example, malononitrile, succinonitrile, glutaronitrile, adiponitrile, 1,4-dicyanoheptane, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 2,6-dicyanoheptane, 1,8-dicyanooctane, 2,7-dicyanooctane, 1,9-dicyanononane, 2,8-dicyanononane, 1,10-dicyanodecane, 1,6-dicyanodecane, and 2,4-dimethylglutaronitrile.
[0070] Cyclic nitriles include, for example, benzonitrile.
[0071] Examples of short-chain fatty acid esters include methyl acetate, methyl propionate, methyl isobutyrate, methyl butyrate, methyl isovalerate, methyl valerate, methyl pivalate, methyl hydroangelate, methyl caproate, ethyl acetate, ethyl propionate, ethyl isobutyrate, ethyl butyrate, ethyl isovalerate, ethyl valerate, ethyl pivalate, ethyl hydroangelate, ethyl caproate, propyl acetate, propyl propionate, propyl isobutyrate, propyl butyrate, propyl isovalerate, propyl valerate, propyl pivalate, propyl hydroangelate, propyl caproate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, isopropyl valerate, and isopropyl pivalate. butyl, isopropyl hydroangelate, isopropyl caproate, butyl acetate, butyl propionate, butyl isobutyrate, butyl butyrate, butyl isovalerate, butyl valerate, butyl pivalate, butyl hydroangelate, butyl caproate, isobutyl acetate, isobutyl propionate, isobutyl isobutyrate, isobutyl butyrate, isobutyl isovalerate, isobutyl valerate, isobutyl pivalate, isobutyl hydroangelate, isobutyl caproate, tert-butyl acetate, tert-butyl propionate, tert-butyl isobutyrate, tert-butyl butyrate, tert-butyl isovalerate, tert-butyl valerate, tert-butyl pivalate, tert-butyl hydroangelate, and tert-butyl caproate.
[0072] Examples of chain ethers include dimethoxyethane, diethyl ether, 1,3-dioxolane, diglyme, triglyme, and tetraglyme.
[0073] Examples of fluorinated ethers include Rf 20 -OR 21 (Rf 20 is an alkyl group containing a fluorine atom, R 21 is an organic group which may contain a fluorine atom).
[0074] Ketones include, for example, acetone, methyl ethyl ketone, and methyl isobutyl ketone.
[0075] Examples of the aprotic solvent compound in which some or all of the H atoms have been substituted with halogen atoms include compounds in which the halogen atoms are fluorine.
[0076] Examples of fluorinated chain carbonates include methyl trifluoroethyl carbonate, trifluorodimethyl carbonate, trifluorodiethyl carbonate, trifluoroethylmethyl carbonate, methyl 2,2-difluoroethyl carbonate, methyl 2,2,2-trifluoroethyl carbonate, and methyl 2,2,3,3-tetrafluoropropyl carbonate. The above-mentioned fluorinated chain carbonates are represented by the following general formula: R 29 -OC(O)OR 30 (In the formula, R 29 and R 30 is CH3, CH2CH3, CH2CH2CH3, CH(CH3)2, and CH2Rf 31 Rf is at least one selected from the group consisting of 31 is an alkyl group having 1 to 3 carbon atoms in which a hydrogen atom is substituted with at least one fluorine atom, and R 29 and / or R 30 contains at least one fluorine atom).
[0077] In the present embodiment, the aprotic solvent other than acetonitrile may be used alone or in combination of two or more kinds.
[0078] In the present embodiment, the non-aqueous solvent is preferably used in combination with acetonitrile and one or more of a cyclic carbonate and a chain carbonate from the viewpoint of improving the stability of the non-aqueous electrolyte. From this viewpoint, the non-aqueous solvent in the present embodiment is more preferably used in combination with acetonitrile and a cyclic carbonate, and more preferably used in combination with acetonitrile and both a cyclic carbonate and a chain carbonate.
[0079] When a cyclic carbonate is used with acetonitrile, it is particularly preferred that such cyclic carbonate comprises ethylene carbonate, vinylene carbonate, and / or fluoroethylene carbonate.
[0080] <Lithium salt> In this embodiment, the non-aqueous electrolyte contains LiN(SO2F)2 and LiPF6 as lithium salts. LiN(SO2F)2 is a lithium salt included in imide salts. In this specification, imide salts are lithium salts represented by the general formula LiN(SO2C m F 2m+1 )2 {wherein m is an integer of 0 to 8.}Specific examples of the lithium salt include LiN(SO2CF3)2 in addition to LiN(SO2F)2. The non-aqueous electrolyte may contain an imide salt other than these imide salts.
[0081] Since the saturation concentration of the imide salt in acetonitrile is higher than that of LiPF6, it is preferable to include the imide salt at a molar concentration of LiPF6≦imide salt, since this can suppress association and precipitation of the lithium salt and acetonitrile at low temperatures. In addition, it is preferable that the content of the imide salt is 0.5 mol to 3 mol per 1 L of the non-aqueous solvent from the viewpoint of the amount of ions supplied. Preferably, LiN(SO2F)2 is contained at 1.0 mol or more per 1 L of the non-aqueous electrolyte, and LiPF6 is contained at 0.01 mol or more per 1 L of the non-aqueous electrolyte. The upper limit of the content of LiN(SO2F)2 is 2.5 mol or less per 1 L of the non-aqueous electrolyte, and the upper limit of the content of LiPF6 is 1.0 mol or less per 1 L of the non-aqueous electrolyte. By further including LiN(SO2F)2 and LiPF6 in the above quantitative relationship in addition to acetonitrile, the reduction in ion conductivity in a low temperature range such as −10° C. or −30° C. can be effectively suppressed, and excellent low-temperature characteristics can be obtained. By limiting the content in this manner, it is possible to more effectively suppress the increase in resistance during high-temperature heating.
[0082] The lithium salt may include fluorine-containing inorganic lithium salts other than LiPF, such as LiBF, LiAsF, LiSiF, LiSbF, LiBF, LiAs ... 12 F b H 12-b{wherein b is an integer of 0 to 3.} and the like may be included. "Inorganic lithium salt" refers to a lithium salt that does not contain a carbon atom in the anion and is soluble in acetonitrile. "Fluorine-containing inorganic lithium salt" refers to a lithium salt that does not contain a carbon atom in the anion, contains a fluorine atom in the anion, and is soluble in acetonitrile. Fluorine-containing inorganic lithium salts are excellent in that they form a passive film on the surface of the metal foil that is the positive electrode current collector, and inhibit the corrosion of the positive electrode current collector. These fluorine-containing inorganic lithium salts are used alone or in combination of two or more. As the fluorine-containing inorganic lithium salt, a compound that is a double salt of LiF and a Lewis acid is desirable, and among them, it is more preferable to use a fluorine-containing inorganic lithium salt having a phosphorus atom, since it is easy to release free fluorine atoms. A typical fluorine-containing inorganic lithium salt is LiPF6, which dissolves and releases PF6 anions. When a fluorine-containing inorganic lithium salt having a boron atom is used as the fluorine-containing inorganic lithium salt, it is preferable because it is easy to capture excess free acid components that may cause battery deterioration, and from this viewpoint, LiBF4 is particularly preferable.
[0083] The content of the fluorine-containing inorganic lithium salt in the non-aqueous electrolyte of this embodiment is not particularly limited, but is preferably 0.01 mol or more per 1 L of non-aqueous solvent, more preferably 0.1 mol or more, and even more preferably 0.25 mol or more. When the content of the fluorine-containing inorganic lithium salt is within the above-mentioned range, the ion conductivity increases and high output characteristics tend to be exhibited. In addition, it is preferably less than 2.8 mol per 1 L of non-aqueous solvent, more preferably less than 1.5 mol, and even more preferably less than 1 mol. When the content of the fluorine-containing inorganic lithium salt is within the above-mentioned range, the ion conductivity increases and high output characteristics can be exhibited, and the decrease in ion conductivity associated with the increase in viscosity at low temperatures tends to be suppressed, and the high temperature cycle characteristics and other battery characteristics tend to be further improved while maintaining the excellent performance of the non-aqueous electrolyte.
[0084] The nonaqueous electrolyte solution of the present embodiment may further contain an organic lithium salt. The term "organic lithium salt" refers to a lithium salt that contains a carbon atom in the anion and is soluble in acetonitrile.
[0085] The organic lithium salt may be an organic lithium salt having an oxalic acid group. Specific examples of the organic lithium salt having an oxalic acid group include organic lithium salts represented by LiB(C2O4)2, LiBF2(C2O4), LiPF4(C2O4), and LiPF2(C2O4)2, and among them, at least one lithium salt selected from the lithium salts represented by LiB(C2O4)2 and LiBF2(C2O4) is preferred. It is more preferred to use one or more of these together with a fluorine-containing inorganic lithium salt. The organic lithium salt having an oxalic acid group may be added to a non-aqueous electrolyte solution or may be contained in the negative electrode (negative electrode active material layer).
[0086] The amount of the organic lithium salt having an oxalic acid group added to the non-aqueous electrolyte is preferably 0.005 mol or more, more preferably 0.02 mol or more, and even more preferably 0.05 mol or more per 1L of the non-aqueous solvent of the non-aqueous electrolyte, from the viewpoint of better ensuring the effect of its use. However, if the amount of the organic lithium salt having an oxalic acid group in the non-aqueous electrolyte is too large, there is a risk of precipitation. Therefore, the amount of the organic lithium salt having an oxalic acid group added to the non-aqueous electrolyte is preferably less than 1.0 mol, more preferably less than 0.5 mol, and even more preferably less than 0.2 mol per 1L of the non-aqueous solvent of the non-aqueous electrolyte.
[0087] It is known that organic lithium salts having oxalic acid groups are poorly soluble in organic solvents with low polarity, particularly in chain carbonates. Organic lithium salts having oxalic acid groups may contain a small amount of lithium oxalate, and may react with a small amount of water contained in other raw materials when mixed to form a non-aqueous electrolyte solution, resulting in the generation of new white precipitation of lithium oxalate. Therefore, the content of lithium oxalate in the non-aqueous electrolyte solution of this embodiment is not particularly limited, but is preferably 0 to 500 ppm.
[0088] In addition to the above, lithium salts generally used for non-aqueous secondary batteries may be added supplementarily as the lithium salt in this embodiment. Specific examples of other lithium salts include LiClO4, LiAlO4, LiAlCl4, LiB 10 Cl 10 Inorganic lithium salts that do not contain fluorine atoms in the anion, such as chloroborane Li; LiCF3SO3, LiCF3CO2, Li2C2F4(SO3)2, LiC(CF3SO2)3, LiC n F (2n+1) SO3 (n≧2), organic lithium salts such as lower aliphatic carboxylic acids, Li tetraphenylborate, LiB(C3O4H2)2, etc.; LiPF such as LiPF5(CF3) n (C p F 2p+1 ) 6-n {wherein n is an integer of 1 to 5, and p is an integer of 1 to 8.}; LiBF such as LiBF3(CF3) q (C s F 2s+1 ) 4-q {wherein q is an integer of 1 to 3, and s is an integer of 1 to 8.}; a lithium salt bonded to a polyvalent anion; LiC(SO2R A )(SO2R B )(SO2R C ) (a) {where, R A , R B , and R Cmay be the same or different and represent a perfluoroalkyl group having 1 to 8 carbon atoms. The following formula (b) LiN(SO2OR D )(SO2OR E ) (b) {where, R D , and R E may be the same or different and represent a perfluoroalkyl group having 1 to 8 carbon atoms.}, and The following formula (c) LiN(SO2R F )(SO2OR G ) (c) {where, R F , and R G may be the same or different and represent a perfluoroalkyl group having 1 to 8 carbon atoms.} One or more of these can be used together with the fluorine-containing inorganic lithium salt.
[0089] <Additives for electrode protection> The electrolyte solution in this embodiment may contain an additive that protects the electrodes (referred to as an "electrode protection additive" in this specification). The electrode protection additive is not particularly limited as long as it does not impede the solution of the problems by the present invention. It may substantially overlap with a substance that plays a role as a solvent for dissolving lithium salts (i.e., the above-mentioned non-aqueous solvent). The electrode protection additive is preferably a substance that contributes to improving the performance of the electrolyte solution and the non-aqueous secondary battery in this embodiment, but also includes substances that are not directly involved in electrochemical reactions.
[0090] Specific examples of the electrode protection additive include 4-fluoro-1,3-dioxolane-2-one, 4,4-difluoro-1,3-dioxolane-2-one, cis-4,5-difluoro-1,3-dioxolane-2-one, trans-4,5-difluoro-1,3-dioxolane-2-one, 4,4,5-trifluoro-1,3-dioxolane-2-one, and 4,4,5,5-tetrafluoro-1,3-dioxolane-2-one. Fluoroethylene carbonates such as 4,4,5-trifluoro-5-methyl-1,3-dioxolan-2-one; unsaturated bond-containing cyclic carbonates such as vinylene carbonate, 4,5-dimethylvinylene carbonate, and vinylethylene carbonate; γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone, and ε-caprolactone. lactones represented by 1,4-dioxane; cyclic ethers represented by ethylene sulfite, propylene sulfite, butylene sulfite, pentene sulfite, sulfolane, 3-sulfolene, 3-methyl sulfolane, 1,3-propane sultone, 1,4-butane sultone, 1-propene 1,3-sultone, and tetramethylene sulfoxide; chain acid anhydrides represented by acetic anhydride, propionic anhydride, and benzoic anhydride; cyclic acid anhydrides represented by malonic anhydride, succinic anhydride, glutaric anhydride, maleic anhydride, phthalic anhydride, 1,2-cyclohexanedicarboxylic anhydride, 2,3-naphthalene dicarboxylic anhydride, or naphthalene-1,4,5,8-tetracarboxylic dianhydride; mixed acid anhydrides having a structure in which different types of acids, such as two different types of carboxylic acids or a carboxylic acid and a sulfonic acid, are dehydrated and condensed. These may be used alone or in combination of two or more types.
[0091] The content of the electrode protection additive in the electrolyte in this embodiment is not particularly limited, but the content of the electrode protection additive relative to the total amount of the nonaqueous electrolyte is preferably 0.01 vol.% to 30 vol.%, more preferably 0.3 vol.% to 15 vol.%, and even more preferably 0.5 vol.% to 4 vol.%.
[0092] In this embodiment, the higher the content of the additive for electrode protection, the more the deterioration of the electrolytic solution is suppressed. However, the lower the content of the additive for electrode protection, the more the high-power characteristics of the non-aqueous secondary battery in a low-temperature environment are improved. Therefore, by adjusting the content of the additive for electrode protection within the above range, it is possible to maximize the excellent performance based on the high ionic conductivity of the electrolytic solution without impairing the basic functions of the non-aqueous secondary battery. By preparing the electrolytic solution with such a composition, it tends to be possible to further improve all of the cycle performance, high-power performance in a low-temperature environment, and other battery characteristics of the non-aqueous secondary battery.
[0093] Since acetonitrile, which is one component of the non-aqueous solvent, is easily electrochemically reductively decomposed, the non-aqueous solvent containing the acetonitrile preferably contains one or more cyclic aprotic polar solvents as an additive for electrode protection for forming a protective film on the negative electrode, and more preferably contains one or more unsaturated bond-containing cyclic carbonates.
[0094] Vinylene carbonate is preferable as the unsaturated bond-containing cyclic carbonate, and the content of vinylene carbonate is preferably 0.1% by volume or more and 4% by volume or less, more preferably 0.2% by volume or more and less than 3% by volume, and still more preferably 0.5% by volume or more and less than 2.5% by volume in the non-aqueous electrolytic solution. Thereby, the low-temperature durability can be more effectively improved, and it becomes possible to provide a secondary battery excellent in low-temperature performance.
[0095] Vinylene carbonate as an additive for electrode protection can suppress the reductive decomposition reaction of acetonitrile on the negative electrode surface, so that the battery performance can be improved. On the other hand, excessive film formation causes a decrease in low-temperature performance. Therefore, when vinylene carbonate is contained, by adjusting the addition amount within the above range, it is possible to suppress the cycle deterioration at low temperature while keeping the interfacial (film) resistance low.
[0096] <FSO3 Anion Reduction Step> When LiN(SO2F)2, which is generally available commercially as a lithium salt, is used, a certain amount of FSO3 anion is contained as a raw material impurity. Although it is difficult to completely remove FSO3 anion from the electrolyte, if the content of FSO3 anion is too high, a reduction decomposition reaction occurs on the negative electrode surface in the non-aqueous secondary battery, and the accumulated decomposition products increase the interface (film) resistance and lead to a decrease in output performance. The content of FSO3 anion is in the range of 100 ppm or less based on the total mass of the non-aqueous electrolyte, preferably in the range of 50 ppm or less, and more preferably in the range of 30 ppm or less. On the other hand, since a small amount of FSO3 anion acts to strengthen the negative electrode protective film, it may be contained in an amount of 0.01 ppm or more, 0.1 ppm or more, or 1 ppm or more as long as the above upper limit is satisfied.
[0097] In the present invention, the content of FSO3 anion can be reduced by, for example, dissolving LiN(SO2F)2 in a non-aqueous solvent, adding an adsorbent capable of adsorbing FSO3 anion to the mixed solution, and leaving the mixture for a certain period of time. Examples of the adsorbent include molecular sieves. The molecular sieves may be commercially available or may be synthesized. The time required for the content of FSO3 anion to be reduced to the range of the present invention is not particularly limited, but is preferably 5 hours or more, more preferably 12 hours or more, after the addition of the molecular sieves. After the addition of the molecular sieves, heating or stirring may be applied as appropriate.
[0098] <Propionitrile> The non-aqueous electrolyte may contain propionitrile. Propionitrile reacts quickly during overcharging and contributes to alpha hydrogen abstraction. This allows the battery to swell and burst before burning. On the other hand, the addition of excessive propionitrile promotes the alpha hydrogen abstraction reaction even in the normal voltage range, causing gas accumulation in the electrodes and capacity degradation. For this reason, by making the propionitrile contained in the non-aqueous electrolyte 5 ppm or less, the safety of the battery can be improved without impairing the battery performance in the normal voltage range.
[0099] The upper limit of the propionitrile content is preferably less than 5 ppm, more preferably 4 ppm or less, relative to the non-aqueous electrolyte.The lower limit is preferably 0.001 ppm or more, more preferably 0.01 ppm or more.The propionitrile content in the present invention is, for example, a value measured by gas chromatography mass spectrometry.
[0100] <Other optional additives> In this embodiment, for the purpose of improving the charge-discharge cycle characteristics, high-temperature storage properties, and safety (e.g., preventing overcharging) of the nonaqueous secondary battery, an optional additive selected from, for example, sulfonic acid esters, diphenyl disulfide, cyclohexylbenzene, biphenyl, fluorobenzene, tert-butylbenzene, phosphate esters, nitrogen-containing cyclic compounds with no steric hindrance around the unshared electron pair, and derivatives of these compounds can be appropriately added to the nonaqueous electrolyte. Examples of the phosphate ester include ethyl diethyl phosphonoacetate (EDPA): (C2H5O)2(P=O)-CH2(C=O)OC2H5, tris(trifluoroethyl) phosphate (TFEP): (CF3CHO)3P=O, and triphenyl phosphate (TPP): (C6H5O)3P=O. Examples of the triallyl phosphate include (CH2=CHCHO)3P=O. Examples of the nitrogen-containing cyclic compounds include pyridine, 1-methyl-1H-benzotriazole, and 1-methylpyrazole. In particular, phosphoric acid esters are effective in suppressing side reactions during storage.
[0101] The content of other optional additives in this embodiment is calculated as a mass percentage relative to the total mass of all components constituting the non-aqueous electrolyte. There is no particular limitation on the content of other optional additives, but it is preferably in the range of 0.01 mass% to 10 mass%, more preferably 0.02 mass% to 5 mass%, and even more preferably 0.05 mass% to 3 mass% relative to the total amount of the non-aqueous electrolyte. By adjusting the content of other optional additives within the above range, there is a tendency that it is possible to add even better battery characteristics without impairing the basic function as a non-aqueous secondary battery.
[0102] [Separator] In the present embodiment, the non-aqueous secondary battery is preferably provided with a separator between the positive electrode and the negative electrode from the viewpoint of preventing short circuits between the positive electrode and the negative electrode, and providing safety such as shutdown. The separator is not limited, but may be the same as that provided in known non-aqueous secondary batteries, and is preferably an insulating thin film having high ion permeability and excellent mechanical strength. Examples of the separator include woven fabric, non-woven fabric, and synthetic resin microporous membrane, and among these, synthetic resin microporous membrane is preferable.
[0103] As the synthetic resin microporous film, for example, a microporous film containing polyethylene or polypropylene as a main component, or a polyolefin-based microporous film such as a microporous film containing both of these polyolefins is preferably used. As the nonwoven fabric, for example, a porous film made of a heat-resistant resin such as glass, ceramic, polyolefin, polyester, polyamide, liquid crystal polyester, or aramid can be used.
[0104] The separator may be a single layer or multiple layers of one type of microporous membrane, or a laminate of two or more types of microporous membranes.The separator may be a single layer or multiple layers of a mixed resin material obtained by melt-kneading two or more resin materials.
[0105] For the purpose of providing functions, inorganic particles may be present on the surface or inside of the separator, and other organic layers may be further coated or laminated. Also, a crosslinked structure may be included. In order to improve the safety performance of the non-aqueous secondary battery, these methods may be combined as necessary. By using such a separator, it is possible to realize good input / output characteristics and low self-discharge characteristics required for the lithium ion secondary battery for high power applications.
[0106] The thickness of the microporous membrane is not particularly limited, but is preferably 1 μm or more from the viewpoint of membrane strength, and is preferably 500 μm or less from the viewpoint of permeability. From the viewpoint of use in high-output applications such as safety tests where the amount of heat generated is relatively high and self-discharge characteristics higher than conventional ones are required, and from the viewpoint of winding properties in a large battery winding machine, it is preferably 5 μm or more and 30 μm or less, and more preferably 10 μm or more and 25 μm or less. In addition, when emphasizing both short circuit resistance and output performance, it is more preferable that it is 15 μm or more and 25 μm or less, but when emphasizing both high energy density and output performance, it is more preferable that it is 10 μm or more and less than 15 μm.
[0107] From the viewpoint of following the rapid movement of lithium ions during high output, the porosity is preferably 30% to 90%, more preferably 35% to 80%, and even more preferably 40% to 70%. When priority is given to improving output performance while ensuring safety, 50% to 70% is particularly preferable, and when emphasis is placed on achieving both short circuit resistance and output performance, 40% to less than 50% is particularly preferable.
[0108] The air permeability is set at 1 second / 100 cm from the viewpoint of the balance between the film thickness and the porosity. 3 More than 400 seconds / 100cm 3 Less than 100 seconds / 100 cm is preferable. 3 More than 350 / 100cm 3 The following is more preferable. If both short-circuit resistance and output performance are important, a maximum of 150 seconds / 100 cm is recommended. 3 More than 350 seconds / 100cm 3The following is particularly preferable. If you prioritize improving output performance while ensuring safety, 100 / 100cm 3 seconds or more 150 seconds / 100cm 3 Less than is particularly preferred.
[0109] On the other hand, when a non-aqueous electrolyte with low ionic conductivity is combined with a separator within the above range, the lithium ion migration rate is not determined by the structure of the separator, but by the high ionic conductivity of the electrolyte, and the expected input / output characteristics tend not to be obtained. Therefore, the ionic conductivity of the non-aqueous electrolyte is preferably 10 mS / cm or more, more preferably 15 mS / cm, and even more preferably 20 mS / cm. However, the thickness, air permeability and porosity of the separator, and the ionic conductivity of the non-aqueous electrolyte are not limited to the above examples.
[0110] [Battery exterior] The structure of the battery exterior of the nonaqueous secondary battery in this embodiment is not particularly limited, but for example, either a battery can or a laminate film exterior can be used. As the battery can, for example, a metal can such as a square, rectangular tube, cylinder, ellipse, flat, coin, or button made of steel, stainless steel, aluminum, clad material, etc. can be used. As the laminate film exterior, for example, a laminate film made of a three-layer structure of heat-melting resin / metal film / resin can be used.
[0111] The laminate film exterior body can be used as an exterior body by stacking two sheets with the heat-melting resin side facing inward, or by folding the laminate film exterior body so that the heat-melting resin side faces inward and sealing the ends by heat sealing. When using a laminate film exterior body, a positive electrode lead body (or a lead tab connected to a positive electrode terminal and a positive electrode terminal) may be connected to a positive electrode current collector, and a negative electrode lead body (or a lead tab connected to a negative electrode terminal and a negative electrode terminal) may be connected to a negative electrode current collector. In this case, the laminate film exterior body may be sealed with the ends of the positive electrode lead body and the negative electrode lead body (or the lead tabs connected to the positive electrode terminal and the negative electrode terminal, respectively) pulled out to the outside of the exterior body.
[0112] <Shape of non-aqueous secondary battery> The shape of the nonaqueous secondary battery of this embodiment is not particularly limited, and may be, for example, a cylindrical shape, an elliptical shape, a rectangular tube shape, a button shape, a coin shape, a flat shape, a laminate shape, or the like.
[0113] <<Method for manufacturing non-aqueous secondary battery>> The nonaqueous secondary battery in this embodiment can be manufactured using the above-mentioned nonaqueous electrolyte, a positive electrode having a positive electrode active material, a negative electrode having a negative electrode active material, a separator, and, if necessary, a battery exterior.
[0114] First, a laminate consisting of a positive electrode, a negative electrode, and a separator can be formed. For example, a method of preparing a laminate having a long positive electrode and a negative electrode with a long separator interposed between the positive electrode and the negative electrode, and winding the laminate to form a laminate having a wound structure; a method of forming a laminate having a laminate structure in which positive electrode sheets and negative electrode sheets obtained by cutting the positive electrode and the negative electrode into a plurality of sheets having a certain area and shape are alternately laminated with a separator sheet between them; a method of forming a laminate having a laminate structure in which a long separator is zigzag-folded and positive electrode sheets and negative electrode sheets are alternately inserted between the zigzag-folded separators; and the like are possible.
[0115] Next, the above-mentioned laminate is housed in a battery exterior (battery case), an electrolytic solution is poured into the battery case, and the laminate is immersed in the electrolytic solution and sealed to produce the nonaqueous secondary battery of this embodiment. Alternatively, a gelled electrolyte membrane may be produced in advance by impregnating a substrate made of a polymer material with the electrolytic solution, and a laminate having a laminated structure may be formed using a sheet-shaped positive electrode, a negative electrode, an electrolyte membrane, and a separator, and then the laminate may be housed in the battery exterior to produce the nonaqueous secondary battery.
[0116] In addition, when the arrangement of the electrodes is designed so that there is a portion where the outer peripheral edge of the negative electrode active material layer overlaps with the outer peripheral edge of the positive electrode active material layer, or there is a portion where the width is too small in the non-facing portion of the negative electrode active material layer, the position of the electrodes may be shifted during battery assembly, which may deteriorate the charge-discharge cycle characteristics of the non-aqueous secondary battery. Therefore, it is preferable that the electrode positions of the electrode body used in the non-aqueous secondary battery are fixed in advance by tapes such as polyimide tape, polyphenylene sulfide tape, and PP tape, adhesives, etc.
[0117] In this embodiment, when a non-aqueous electrolyte using acetonitrile is used, the lithium ions released from the positive electrode during the initial charge of the non-aqueous secondary battery may diffuse throughout the negative electrode due to its high ionic conductivity. In non-aqueous secondary batteries, the area of the negative electrode active material layer is generally made larger than that of the positive electrode active material layer. However, if lithium ions diffuse and are absorbed to a portion of the negative electrode active material layer that does not face the positive electrode active material layer, the lithium ions will not be released during the initial discharge and will remain in the negative electrode. Therefore, the contribution of the lithium ions that are not released becomes irreversible capacity. For these reasons, the initial charge / discharge efficiency may be low in non-aqueous secondary batteries using a non-aqueous electrolyte containing acetonitrile.
[0118] On the other hand, if the area of the positive electrode active material layer is larger than that of the negative electrode active material layer or they are the same, current concentration is likely to occur at the edge portions of the negative electrode active material layer during charging, making it easier for lithium dendrites to form.
[0119] Although there is no particular limitation on the ratio of the area of the entire negative electrode active material layer to the area of the portion where the positive electrode active material layer and the negative electrode active material layer face each other, for the reasons described above, it is preferably greater than 1.0 and less than 1.1, more preferably greater than 1.002 and less than 1.09, even more preferably greater than 1.005 and less than 1.08, and particularly preferably greater than 1.01 and less than 1.08. In a nonaqueous secondary battery using a nonaqueous electrolyte solution containing acetonitrile, the initial charge / discharge efficiency can be improved by reducing the ratio of the area of the entire negative electrode active material layer to the area of the portion where the positive electrode active material layer and the negative electrode active material layer face each other.
[0120] Reducing the ratio of the area of the entire negative electrode active material layer to the area of the portion where the positive electrode active material layer and the negative electrode active material layer face each other means limiting the ratio of the area of the portion of the negative electrode active material layer that does not face the positive electrode active material layer. This makes it possible to reduce as much as possible the amount of lithium ions absorbed in the portion of the negative electrode active material layer that does not face the positive electrode active material layer among the lithium ions released from the positive electrode during the initial charge (i.e., the amount of lithium ions that are not released from the negative electrode during the initial discharge and become irreversible capacity). Therefore, by designing the ratio of the area of the entire negative electrode active material layer to the area of the portion where the positive electrode active material layer and the negative electrode active material layer face each other within the above range, it is possible to improve the load characteristics of the battery by using acetonitrile, increase the initial charge / discharge efficiency of the battery, and further suppress the generation of lithium dendrites.
[0121] The non-aqueous secondary battery in this embodiment can function as a battery by initial charging, but is stabilized by decomposing a part of the electrolyte during the initial charging. There is no particular restriction on the method of initial charging, but the initial charging is preferably performed at 0.001 to 0.3C, more preferably at 0.002 to 0.25C, and even more preferably at 0.003 to 0.2C. The initial charging can also be performed via a constant voltage charge in the middle to give a favorable result. The constant current at which the designed capacity is discharged in one hour is 1C. By setting the voltage range in which the lithium salt is involved in the electrochemical reaction to be long, a stable and strong SEI is formed on the electrode surface, and there is an effect of suppressing an increase in internal resistance, and in addition, the reaction product is not firmly fixed only to the negative electrode, but in some way has a good effect on members other than the negative electrode, such as the positive electrode and the separator. For this reason, it is very effective to perform the initial charging in consideration of the electrochemical reaction of the lithium salt dissolved in the non-aqueous electrolyte.
[0122] The nonaqueous secondary battery of this embodiment can also be used as a battery pack in which a plurality of nonaqueous secondary batteries are connected in series or in parallel. From the viewpoint of managing the charge / discharge state of the battery pack, the operating voltage range per battery is preferably 2 to 5 V, more preferably 2.5 to 5 V, and particularly preferably 2.75 V to 5 V.
[0123] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment. The present invention can be modified in various ways without departing from the gist of the present invention. EXAMPLES
[0124] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0125] (1) Preparation of non-aqueous electrolyte In an inert atmosphere, various non-aqueous solvents and various lithium salts were added to give predetermined concentrations to prepare non-aqueous electrolyte solutions (S1) to (S4). The compositions of these non-aqueous electrolyte solutions are shown in Table 1.
[0126] The abbreviations for the non-aqueous solvents and lithium salts in Table 1 have the following meanings. (Non-aqueous solvent) AcN: Acetonitrile EMC: Ethyl methyl carbonate DFA: Difluoroacetate GBL: gamma-butyrolactone EC: Ethylene carbonate VC: Vinylene carbonate
[0127] (Lithium salts) LiPF6: Lithium hexafluorophosphate LiFSI: Lithium bis(fluorosulfonyl)imide (LiN(SO2F)2)
[0128] [Table 1]
[0129] For the non-aqueous electrolytes (S1) and (S2), 1 g of molecular sieve (5A 1 / 16 manufactured by Kanto Chemical Co., Ltd.) was added to 10 g of the non-aqueous electrolyte after preparation, and the mixture was left for 24 hours with occasional stirring. After that, the amount of FSO3 anion in the obtained non-aqueous electrolyte was 19 Measurements were performed using F-NMR.
[0130] (2) Preparation of coin-type non-aqueous secondary batteries (2-1) Preparation of positive electrode (A) Lithium iron phosphate (LiFePO4) having an olivine structure as a positive electrode active material, (B) carbon black powder as a conductive assistant, and polyvinylidene fluoride (PVDF) as a binder were mixed in a mass ratio of 84:10:6 to obtain a positive electrode mixture. N-methyl-2-pyrrolidone was added as a solvent to the obtained positive electrode mixture so that the solid content was 68 mass% and further mixed to prepare a positive electrode mixture-containing slurry. While adjusting the basis weight of this positive electrode mixture-containing slurry on one side of an aluminum foil having a thickness of 15 μm and a width of 280 mm to be a positive electrode current collector, it was applied using a three-roll transfer coater so as to have a coating pattern of 240 to 250 mm in coating width, 125 mm in coating length, and 20 mm in non-coating length, and the solvent was dried and removed in a hot air drying oven. Both sides of the obtained electrode roll were trimmed and cut, and reduced pressure drying was performed at 130 ° C for 8 hours. Then, the density of the positive electrode active material layer was adjusted to 1.9 g / cm by roll pressing. 3 A positive electrode consisting of the positive electrode active material layer and the positive electrode current collector was obtained by rolling the positive electrode active material layer so that the weight per unit area excluding the positive electrode current collector was 17.5 mg / cm. 2 It was.
[0131] (2-2) Preparation of negative electrode As the negative electrode active material, graphite powder, carbon black powder as a conductive assistant, and carboxymethyl cellulose and styrene butadiene rubber as a binder were mixed in a solid content mass ratio of 95.7:0.5:3.8 to obtain a negative electrode mixture. Water was added as a solvent to the obtained negative electrode mixture so that the solid content was 45 mass% and further mixed to prepare a negative electrode mixture-containing slurry. While adjusting the basis weight of this negative electrode mixture-containing slurry on one side of a copper foil having a thickness of 8 μm and a width of 280 mm to be a negative electrode current collector, it was coated using a three-roll transfer coater so as to have a coating pattern of a coating width of 240 to 250 mm, a coating length of 125 mm, and an uncoated length of 20 mm, and the solvent was dried and removed in a hot air drying oven. The obtained electrode roll was trimmed and cut on both sides, and dried under reduced pressure at 80 ° C for 12 hours. Thereafter, the density of the negative electrode active material layer was adjusted to 1.5 g / cm by roll pressing. 3 The negative electrode was obtained by rolling the negative electrode active material layer and the negative electrode current collector so that the coating weight excluding the negative electrode current collector was 7.5 mg / cm. 2 It was.
[0132] (2-3) Assembly of coin-type non-aqueous secondary batteries A polypropylene gasket was set in a CR2032 type battery case (SUS304 / Al clad), and the positive electrode obtained as described above was punched into a disk shape with a diameter of 15.958 mm and set in the center with the positive electrode active material layer facing up. A glass fiber filter paper (GA-100, manufactured by Advantec Co., Ltd.) punched into a disk shape with a diameter of 16.156 mm was set on top of it, and 150 μL of non-aqueous electrolyte was injected, and then the negative electrode obtained as described above was punched into a disk shape with a diameter of 16.156 mm and set with the negative electrode active material layer facing down. After setting the spacer and spring, the battery cap was fitted and crimped with a crimping machine. The overflowing electrolyte was wiped clean with a rag. The laminate was kept at 25 ° C for 12 hours, and the non-aqueous electrolyte was thoroughly absorbed into the laminate to obtain a coin-type non-aqueous secondary battery.
[0133] (3) Evaluation of coin-type non-aqueous secondary batteries The coin-type non-aqueous secondary batteries obtained as described above were first subjected to an initial charge process and an initial charge / discharge capacity measurement according to the procedure in (3-1) below. Next, each coin-type non-aqueous secondary battery was evaluated according to the procedure in (3-2). The charge / discharge was performed using a charge / discharge device ACD-M01A (product name) manufactured by Asuka Electronics Co., Ltd. and a programmable thermostatic chamber IN804 (product name) manufactured by Yamato Scientific Co., Ltd. Here, 1C means a current value at which a battery in a fully charged state is discharged at a constant current and discharge is expected to be completed in one hour. It means a current value at which a battery in a fully charged state is discharged at a constant current and discharge is expected to be completed in one hour.
[0134] (3-1) Initial charge / discharge treatment of coin-type non-aqueous secondary batteries The ambient temperature of the coin-type nonaqueous secondary battery was set to 25°C, and it was charged at a constant current of 4.6 mA, which corresponds to 0.1 C, until it reached 3.8 V, and then it was charged at a constant voltage of 3.8 V until the current decayed to 0.05 C. It was then discharged to 2.5 V at a constant current of 1.38 mA, which corresponds to 0.3 C.
[0135] (3-2) 25℃ cycle test The coin-type non-aqueous secondary battery that had been subjected to the initial charge-discharge treatment according to the method described in (3-1) above was charged at an ambient temperature of 25° C., reached 3.8 V at a constant current of 2.3 mA equivalent to 0.5 C, and then charged at a constant voltage of 3.8 V until the current attenuated to 0.05 C. Thereafter, it was discharged to 2.5 V at a current value of 2.3 mA equivalent to 0.5 C. This process of charging and discharging once each was counted as one cycle, and 100 cycles of charge-discharge were performed. In addition, at the 1st cycle, the 50th cycle, and the 100th cycle, it was charged at a constant current of 1.38 mA equivalent to 0.3 C, reached 3.8 V, and then charged at a constant voltage of 3.8 V until the current attenuated to 0.05 C. Thereafter, it was discharged to 2.5 V at a constant current of 1.38 mA equivalent to 0.3 C. The discharge capacity at the 99th cycle during the cycle test when the discharge capacity at the 1st cycle during the initial charge-discharge treatment was taken as 100% was calculated as the capacity retention rate.
[0136] (3-3) 50℃ cycle test The coin-type non-aqueous secondary battery that had been subjected to the initial charge-discharge treatment according to the method described in (3-1) above was charged at an ambient temperature of 50° C., and after reaching 3.8 V at a constant current of 6.9 mA corresponding to 1.5 C, it was charged at a constant voltage of 3.8 V until the current attenuated to 0.05 C. Then, it was discharged to 2.5 V at a current value of 6.9 mA corresponding to 1.5 C. This process of charging and discharging once each was considered as one cycle, and 100 cycles of charge and discharge were performed. In the 1st cycle, 50th cycle, and 100th cycle, it was charged at a constant current of 4.6 mA corresponding to 1 C, and after reaching 3.8 V, it was charged at a constant voltage of 3.8 V until the current attenuated to 0.05 C, and then it was discharged to 2.5 V at a constant current of 1.38 mA corresponding to 0.3 C. The discharge capacity at the 99th cycle during the cycle test when the discharge capacity at the 1st cycle during the initial charge-discharge treatment was taken as 100% was calculated as the capacity retention rate.
[0137] (3-4) -40℃ discharge test For the coin-type non-aqueous secondary battery that had been subjected to the initial charge-discharge treatment according to the method described in (3-1) above, the ambient temperature of the battery was set to 25°C, and the battery was charged at a constant current of 2.3mA equivalent to 0.5C until it reached 3.8V, and then charged at a constant voltage of 3.8V until the current attenuated to 0.05C, and discharged to 2.5V at a current value of 0.46mA equivalent to 0.1C. After that, the battery was charged at a constant current of 2.3mA equivalent to 0.5C until it reached 3.8V, and then charged at a constant voltage of 3.8V until the current attenuated to 0.05C. Next, the ambient temperature of the battery was set to -40°C, and after a waiting time of 3 hours, the battery was discharged to 2.5V at a current value of 0.46mA equivalent to 0.1C. The discharge capacity at -40°C when the discharge capacity in a 25°C environment was taken as 100% was calculated as the capacity retention rate.
[0138] [Examples 1-2 and Comparative Examples 1-4] A coin-type nonaqueous secondary battery was fabricated according to the method described in (2) above using the positive electrode, negative electrode, and nonaqueous electrolyte solution shown in Table 1. Next, each coin-type nonaqueous secondary battery was evaluated according to the procedures described in (3-1) to (3-4) above. The test results are shown in Tables 2 and 3.
[0139] [Table 2]
[0140] [Table 3]
[0141] As shown in Table 2, Example 1 used an electrolyte that had been subjected to the FSO3 anion reduction process, and showed a capacity retention rate of 85% or more in the 25° C. cycle test and a capacity retention rate of 58% or more in the -40° C. discharge test. On the other hand, Comparative Example 1 used an electrolyte that had not been subjected to the FSO3 anion reduction process, and showed excellent low-temperature performance with a capacity retention rate of 57% or more in the -40° C. discharge test, but the capacity retention rate in the 25° C. cycle test was reduced to 69% or less.
[0142] As shown in Table 3, Example 2 uses an electrolyte solution that has undergone an FSO3 anion reduction process, and the capacity retention rate in the 50°C cycle test is 88% or more, and the capacity retention rate in the -40°C discharge test is also 61% or more. On the other hand, Comparative Example 2 does not use LiFSI as a lithium salt, so the amount of FSO3 anions is within the range of the present invention (0 ppm) regardless of whether or not an FSO3 anion reduction process is performed. Comparative Example 2 shows excellent high-temperature durability with a capacity retention rate of 87% or more in the 50°C cycle test, but does not use LiFSI, so the capacity retention rate in the -40°C discharge test is 13% or less, which does not satisfy the low-temperature performance. Comparative Example 3 uses an electrolyte solution that does not contain acetonitrile and has not undergone an FSO3 anion reduction process, so the capacity retention rate in the 50°C cycle test is reduced to 70% or less. The capacity retention rate in the -40°C discharge test is also 27% or less, which does not satisfy the low-temperature performance, because it does not contain acetonitrile and the LiFSI content is 0.7 mol or less. In Comparative Example 4, the FSO3 anion reduction step was not performed, and an electrolyte solution containing 5.5 ppm or more of propionitrile was used, so the capacity retention rate in the 50°C cycle test was reduced to 15% or less. For Comparative Example 4, the capacity retention rate in the 50°C cycle test was significantly reduced, so a -40°C discharge test was not performed.
[0143] As shown by these results, it has become clear that the use of a non-aqueous electrolyte solution and a specific positive electrode active material within the scope of the present invention can improve cycle performance in a high-temperature environment and low-temperature performance. [Industrial Applicability]
[0144] The nonaqueous secondary battery of the present invention is expected to be used, for example, as a power source for idling stop systems; rechargeable batteries for automobiles such as hybrid automobiles, plug-in hybrid automobiles, and electric automobiles; low-voltage power sources such as 12 V class power sources, 24 V class power sources, and 48 V class power sources; and residential electricity storage systems. [Explanation of symbols]
[0145] 100 Nonaqueous secondary battery 110 Battery housing 120 Space 130 Positive electrode lead body 140 Negative electrode lead body 150 positive electrode 160 negative electrode 170 Separator
Claims
1. A non-aqueous secondary battery having a positive electrode having a positive electrode active material, a negative electrode having a negative electrode active material, a separator, and a non-aqueous electrolyte solution, The positive electrode contains a lithium-containing metal oxide as the positive electrode active material, The lithium-containing metal oxide has an olivine structure. x FePO 4 wherein 0<x<1.2; The non-aqueous electrolyte solution contains 1% by volume to 85% by volume of acetonitrile and LiN(SO) as a lithium salt based on the total volume of the non-aqueous solvent. 2 F) 2 and LiPF 6 Contains FSO 3 A non-aqueous secondary battery having an anion content of 1 ppm or more and 30 ppm or less based on the total mass of the non-aqueous electrolyte solution.
2. 2. The nonaqueous secondary battery according to claim 1, wherein the propionitrile contained in the nonaqueous electrolyte solution is 0.01 ppm or more and less than 5.0 ppm based on the total mass of the nonaqueous electrolyte solution.
Citation Information
Patent Citations
Lithium ion secondary battery
JP2010277958A
Nonaqueous electrolyte and nonaqueous electrolyte secondary battery
JP2011187440A
Lithium secondary battery
JP2015215977A
Preparation of imides containing fluorosulfonyl groups
JP2017514779A
Nonaqueous secondary battery
JP2018156803A